Conductive resin composition

A conductive resin composition using tin powder, a specific epoxy resin, and a dicarboxylic acid compound addresses the challenge of achieving low volume resistivity and conductivity, while maintaining storage stability and cost-effectiveness, without relying on expensive silver or compromising adhesion.

JP2024157517APending Publication Date: 2024-11-07SAKATA INX

Patent Information

Application Number
JP2024017921
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-02-08
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Conductive resin compositions face challenges in achieving both excellent storage stability and conductivity while maintaining low volume resistivity, with silver-based compositions being costly and compositions using other conductive particles compromising adhesion to substrates.

Method used

A conductive resin composition comprising tin powder, a specific epoxy resin with an epoxy equivalent of 400 g/eq or more, and a dicarboxylic acid compound with 4 to 9 carbon atoms, optionally with a thiol compound, to form a conductive film with low volume resistivity and excellent conductivity.

Benefits of technology

The composition achieves low volume resistivity, excellent conductivity, and cost-effectiveness, with improved storage stability at room and refrigerated temperatures, without using thiol-based or amine-based epoxy resin curing agents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157517000001
    Figure 2024157517000001
  • Figure 2024157517000002
    Figure 2024157517000002
  • Figure 2024157517000003
    Figure 2024157517000003
Patent Text Reader

Abstract

To provide a conductive resin composition comprising a tin powder, which is cost effective and can form a conductive film having excellent room temperature (25°C) storage stability and excellent refrigeration (4°C) storage stability, low volume resistivity and excellent electrical conductivity.SOLUTION: There is provided a conductive resin composition comprising (a) a tin powder, (b) an epoxy resin and (c) a dicarboxylic acid compound, wherein the epoxy resin (b) includes an epoxy resin having an epoxy equivalent weight of 400 g / eq. or more, which is in a solid state or in a semi-solid state at 25°C and the dicarboxylic acid compound (c) includes a dicarboxylic acid compound having 4 or more and 9 or less carbon atoms.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive resin composition. The present invention also relates to a conductive film, a conductive material used when forming a circuit or the like by printing on a substrate by a screen printing method or the like, a conductive adhesive, and a circuit connecting material used when conductively connecting an electronic component to a circuit board or the like. [Background technology]

[0002] A wide variety of conductive resin compositions are known, and are used as conductive pastes, conductive films, conductive materials, conductive paints, circuit connecting materials, conductive adhesives, etc. for various applications such as the formation of electronic circuits and the adhesion of electronic components. For example, there is a demand for conductive resin compositions capable of forming conductive films having low volume resistivity and excellent conductivity in order to form conductive structures such as conductive circuits and electrodes. For example, there is a need for conductive materials that are amenable to a variety of printing methods and that are useful in the manufacture of flexible plastic substrates and the like having conductive structures such as interconnects, traces, electrodes, and the like. For example, in electronic devices such as computers and mobile phones, there is a demand for circuit connection materials that enable high-density mounting and high integration of various electronic components such as LED elements, semiconductor elements, and capacitors on the same circuit board.

[0003] As the conductive resin composition, a conductive resin composition (conductive paste) containing various resins and various conductive particles is known. However, the volume resistivity of the conductive resin composition so far has not been sufficiently low, and when it is used for applications requiring excellent conductivity (low volume resistivity), it is necessary to use silver particles as the conductive particles, which is problematic in terms of cost. In addition, when a large amount of conductive particles is contained in order to reduce the volume resistivity of the conductive film formed from the conductive resin composition, the adhesion (bonding strength) of the film to various substrates is reduced, which is not satisfactory.

[0004] Patent Document 1 discloses a conductive paste composition in which the conductive powder is a silver-based powder using at least silver, the resin component is at least one of a thermosetting resin and a thermoplastic resin, and further contains an ester-based compound having a specific molecular weight and structure or a salt thereof, or an ether / amine-based compound. Patent Document 2 discloses a conductive resin composition containing tin powder, a resin, and an organic acid compound. This conductive resin composition has a low volume resistivity when a conductive film is formed, exhibits good conductivity, can be used as a substitute for silver paste, and is considered to be a conductive resin composition useful as a conductive material, a conductive adhesive, a circuit connecting material, etc. Patent Document 3 discloses a conductive adhesive containing 85% to 92% by weight of conductive metal powder and the remainder being a binder, the binder containing an epoxy resin, an acid anhydride curing agent, an organic acid, and rubber particles having a particle size of 100 nm to 300 nm, the proportion of the rubber particles being 8% to 25% by weight relative to 100% by weight of the binder. This conductive adhesive is said to be capable of bonding metals together at a temperature lower than the melting point of the conductive metal powder, and is a conductive adhesive with reduced bleeding. Patent Document 4 discloses a conductive adhesive made of an organic resin and a conductive filler, which contains a conductive main filler made of 20 to less than 100 wt% of tin and / or a tin alloy, other conductive fillers made of powder of silver and / or a silver alloy, or gold and / or a gold alloy, or powder fillers plated with these metals, a binder, and an organic acid such as adipic acid or a derivative thereof. This conductive adhesive is said to be a conductive adhesive that is inexpensive and has excellent conductivity and repairability as a solder substitute. Patent Document 5 discloses a conductive adhesive that contains a Sn-containing conductive metal powder, a thermosetting resin, an acid anhydride curing agent, and an organic acid, and uses an organic acid metal salt generated by the reaction of the conductive metal powder and the organic acid during heating as a curing accelerator. This conductive adhesive is said to be capable of curing the thermosetting resin in a short time. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-205245 A [Patent Document 2] JP 2022-172874 A [Patent Document 3] Patent No. 6428716 [Patent Document 4] JP 2000-309773 A [Patent Document 5] International Publication No. 2015 / 019666 Summary of the Invention [Problem to be solved by the invention]

[0006] Although the conductive resin composition containing silver particles can form a conductive film with excellent conductivity, the silver particles are very expensive, so it is disadvantageous in terms of cost. On the other hand, the conductive resin composition containing conductive particles other than silver particles may result in a conductive film with high volume resistivity and insufficient conductivity. In addition, when a large amount of conductive particles is contained in order to reduce the volume resistivity, the adhesion to various substrates may be insufficient. Conductive resin compositions containing tin powder are known from Patent Documents 2 to 5, etc., but are unsatisfactory in terms of storage stability at room temperature and in a refrigerator, and in terms of volume resistivity when a conductive film is formed. No conductive resin composition has been known that satisfies the high demand for both excellent storage stability and excellent conductivity.

[0007] One of the problems that the present invention aims to solve is to provide a conductive resin composition containing tin powder, which has excellent storage stability at room temperature (25°C) and refrigerated (4°C) storage stability, is capable of forming a conductive film having low volume resistivity and excellent conductivity, and is cost-effective. One of the problems that the present invention aims to solve is to provide a conductive resin composition containing tin powder, which has excellent storage stability at room temperature (25°C) and refrigerated (4°C) storage stability, is capable of forming a conductive film having low volume resistivity and excellent conductivity, has excellent curability without using a thiol-based epoxy resin curing agent, an amine-based epoxy resin curing agent, an acid anhydride-based epoxy resin curing agent, or a phenol-based epoxy resin curing agent, and is cost-effective. One of the problems that the present invention aims to solve is to provide, at low cost, a conductive film having a low volume resistivity formed from the conductive resin composition, a conductive material containing the conductive resin composition, a conductive adhesive containing the conductive resin composition, and a circuit connecting material containing the conductive resin composition. [Means for solving the problem]

[0008] As a result of extensive investigations aimed at solving the above problems, the present inventors have found that the above problems can be solved by forming a conductive resin composition having a specific composition, and have thus completed the present invention. Specifically, it is as follows: [Section 1] (a) tin powder; (b) epoxy resin, and (c) containing a dicarboxylic acid compound, The (b) epoxy resin includes an epoxy resin having an epoxy equivalent of 400 g / eq or more and being solid or semi-solid at 25° C., The (c) dicarboxylic acid compound includes a dicarboxylic acid compound having 4 to 9 carbon atoms. Conductive resin composition. [Section 2] Item 2. The conductive resin composition according to item 1, wherein the content of the (a) tin powder is 92.01% by mass or more and 99.50% by mass or less, based on 100% by mass of the total amount of components other than the solvent in the conductive resin composition. [Section 3] 3. The conductive resin composition according to item 1 or 2, wherein the (c) dicarboxylic acid compound further includes a dicarboxylic acid compound having 10 or more carbon atoms. [Section 4] 4. The conductive resin composition according to any one of items 1 to 3, further comprising (d) a thiol compound. [Section 5] Item 5. A conductive resin composition having a volume resistivity of 4.0 × 10 -4 Conductive film with a resistance of less than Ω·cm. [Section 6] Item 5. A conductive material comprising the conductive resin composition according to any one of items 1 to 4. [Section 7] Item 5. A conductive adhesive comprising the conductive resin composition according to any one of items 1 to 4. [Section 8] Item 5. A circuit connecting material comprising the conductive resin composition according to any one of items 1 to 4. Effect of the Invention

[0009] The present invention provides a conductive resin composition containing tin powder, which has excellent storage stability at room temperature (25°C) and refrigerated (4°C) storage stability, is capable of forming a conductive film having low volume resistivity and excellent conductivity, and is cost-effective. The present invention provides a conductive resin composition containing tin powder, which has excellent storage stability at room temperature (25°C) and refrigerated (4°C) storage stability, is capable of forming a conductive film having low volume resistivity and excellent conductivity, has excellent curability without the use of a thiol-based epoxy resin curing agent, an amine-based epoxy resin curing agent, an acid anhydride-based epoxy resin curing agent, or a phenol-based epoxy resin curing agent, and is cost-effective. According to the present invention, it is possible to provide, at low cost, a conductive film having a low volume resistivity formed from the conductive resin composition, a conductive material containing the conductive resin composition, a conductive adhesive containing the conductive resin composition, and a circuit connecting material containing the conductive resin composition. INDUSTRIAL APPLICABILITY The conductive resin composition of the present invention is useful as a printed electronics material, and is extremely useful in mass production of various electronic devices such as display devices, vehicle-related parts, IoT, and mobile communication systems. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention relates to a conductive resin composition, a conductive film, a conductive material, a conductive adhesive, and a circuit connecting material, which will be described in detail below.

[0011] [Conductive resin composition] <(a) Tin powder> The (a) tin powder contained in the conductive resin composition of the present invention is a powder composed of 99.5% by mass or more of tin and may contain components other than tin (for example, unavoidable impurities). Examples of the tin powder include tin powder containing only unavoidable impurities and tin powder containing 0.5% by mass or less of components other than tin. (a) The tin content in tin powder can be easily measured using an X-ray fluorescence analysis (XRF) device or the like. (a) Examples of components other than tin that may be contained in the tin powder include one or more other atoms selected from the group consisting of Mn, Sb, Si, K, Na, Li, Ba, Sr, Ca, Mg, Be, Zn, Pb, Cd, Tl, V, Al, Zr, W, Mo, Ti, Co, Ag, Cu, Ni, Au, B, C, N, O, Ge, Sb, In, As, Al, Fe, etc. The content of other atoms in the (a) tin powder is preferably less than 0.3% by mass, and more preferably 0.1% by mass or less.

[0012] (a) The shape of the tin powder is not particularly limited. For example, flake-like, flat, spherical, nearly spherical (for example, with a vertical to horizontal aspect ratio of 1.5 or less), block-like, plate-like, polygonal pyramid-like, polyhedral, rod-like, fibrous, needle-like, irregular shapes, etc. can be used depending on the application. In the present invention, from the viewpoints of volume resistivity, dispersibility, handleability, etc., flake-like, spherical, nearly spherical, and flat shapes are preferred.

[0013] When the (a) tin powder is spherical, its volume average particle diameter (50% particle diameter D50 of cumulative frequency % diameter in volume-based particle size distribution) is not particularly limited. D50 is, for example, 0.5 μm or more, preferably 1.0 μm or more, more preferably 3.0 μm or more, and for example, 300 μm or less, preferably 200 μm or less, more preferably 100 μm or less. When D50 is 0.5 μm or more, the dispersibility and handleability of the (a) tin powder are improved. When D50 is 300 μm or less, the volume resistivity can be reduced, and the dispersibility and handleability are improved. The method for measuring D50 is not particularly limited, but examples thereof include a laser diffraction scattering particle size distribution measurement method.

[0014] (a) When the tin powder is flat or flaky, its average diameter, average thickness and aspect ratio (average diameter / average thickness) are not particularly limited. The average diameter is, for example, 0.5 μm or more, preferably 1.0 μm or more, more preferably 5.0 μm or more, and for example, 500.0 μm or less, preferably 300.0 μm or less, more preferably 150.0 μm or less. The average thickness is, for example, 0.1 μm or more, preferably 0.5 μm or more, more preferably 1.0 μm or more, and for example, 50.0 μm or less, preferably 20.0 μm or less, more preferably 10.0 μm or less. The aspect ratio is, for example, 2 or more, preferably 10 or more, and more preferably 50 or more. The method for measuring the average diameter and the average thickness is not particularly limited, but may be, for example, a measurement method using a scanning electron microscope.

[0015] The content of the (a) tin powder in the conductive resin composition is not particularly limited, and is, for example, 88.00 mass% or more, preferably 90.10 mass% or more, more preferably 92.01 mass% or more, and for example, 99.50 mass% or less, preferably 99.00 mass% or less, more preferably 98.00 mass% or less, based on 100 mass% of the total amount of components other than the solvent in the conductive resin composition. When the content of (a) tin powder is less than 88.00 mass%, assuming that the total amount of components other than the solvent in the conductive resin composition is 100 mass%, there is a risk that the conductivity will decrease and the volume resistivity will increase. When the content of (a) tin powder is more than 99.50 mass%, there is a risk that a film cannot be formed, the adhesion to the substrate will be low, curing will take a long time, the dispersibility of (a) tin powder will decrease so that a uniform composition cannot be formed, and storage stability will decrease.

[0016] <(b) Epoxy resin> The (b) epoxy resin contained in the conductive resin composition of the present invention is not particularly limited as long as it contains an epoxy resin which has two or more epoxy groups in the molecule, has an epoxy equivalent of 400 g / eq or more, and is solid or semi-solid at 25° C. In the present invention, an epoxy resin having an epoxy equivalent of 400 g / eq or more and being solid at 25° C. is an epoxy resin that does not exhibit fluidity at 25° C. and has a melting point or softening point of 25° C. or more. There are no particular limitations on the upper limit of the melting point or softening point, but it is preferably, for example, 150° C. or less. In the present invention, the softening point is a value measured by a softening point test (ring and ball method) method (measurement conditions: in accordance with JIS-K7234:1986). In the present invention, an epoxy resin having an epoxy equivalent of 400 g / eq or more and being semi-solid at 25°C is an epoxy resin having a Gardner viscosity standard solution symbol at 25°C of Z-Z2 (measurement conditions: concentration 60%, butyl carbitol solvent, JIS K 5600).

[0017] Examples of epoxy resins having an epoxy equivalent of 400 g / eq or more and being solid or semi-solid at 25° C. include biphenyl type epoxy resins; bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, and tetramethyl bisphenol F type epoxy resins; naphthalene type epoxy resins; alkylene oxide modified bisphenol type resins; chelate modified epoxy resins; stilbene type epoxy resins; glycol type epoxy resins; pentaerythritol type epoxy resins; novolac type epoxy resins such as phenol novolac type epoxy resins, cresol novolac type epoxy resins, and bisphenol A novolac type epoxy resins; polyfunctional epoxy resins such as trisphenol methane type epoxy resins and alkyl modified trisphenol methane type epoxy resins; phenol aralkyl type epoxy resins having a phenylene skeleton, biphenyl type epoxy resins, and bisphenol F type epoxy resins. Examples of the epoxy resin include aralkyl-type epoxy resins such as phenol aralkyl-type epoxy resins having a phenylene skeleton; naphthol-type epoxy resins such as dihydroxynaphthalene-type epoxy resins and epoxy resins obtained by glycidyl etherifying a dimer of dihydroxynaphthalene; triazine nucleus-containing epoxy resins such as triglycidyl isocyanurate and monoallyl diglycidyl isocyanurate; urethane-modified epoxy resins such as resins obtained by reacting a urethane bond-containing compound having an isocyanate group with a hydroxy group-containing epoxy compound; bridged cyclic hydrocarbon compound-modified phenol-type epoxy resins such as dicyclopentadiene-modified phenol-type epoxy resins; chelate-modified epoxy resins; dimer acid-modified epoxy resins; rubber-modified epoxy resins; polysulfide-modified epoxy resins; glycidyl amine-type epoxy resins; and glycidyl ester-type epoxy resins.Examples of epoxy resins include bisphenol compounds such as bisphenol A, bisphenol F, and biphenol, or derivatives thereof, hydrogenated bisphenol A, hydrogenated bisphenol F, hydrogenated biphenol, cyclohexanediol, cyclohexanedimethanol, cyclohexanediethanol, and other alicyclic epoxy resins, such as polydiols having an alicyclic structure, or epoxidized derivatives thereof; aliphatic epoxy resins, such as butanediol, hexanediol, octanediol, nonanediol, decanediol, and polybutadiene polyol, or epoxidized derivatives thereof; epoxy resins having a trihydroxyphenylmethane skeleton (trisphenolmethane skeleton); aminophenol-type epoxy resins; polyether-modified epoxy resins; polyfunctional aromatic epoxy resins; hydrogenated bisphenol-type epoxy resins, etc., may be used alone or in combination of two or more kinds of epoxy resins.

[0018] The epoxy resin having an epoxy equivalent of 400 g / eq or more and being in a solid or semi-solid state at 25° C. may be a synthesized product or a commercially available product. Commercially available epoxy resins that have an epoxy equivalent of 400 g / eq or more and are solid or semi-solid at 25°C include, for example: YD-011, YD-012, YD-013, YD-014, YD-017, YD-019, YD-901, YD-902, YD-903N, YD-904, YD-907, YD-7910, YDF-2001, YDF-2004 manufactured by Nippon Steel Chemical & Material Co., Ltd.; jER-4005P, jER-4007P, jER-4010P, jER-1010 manufactured by Mitsubishi Chemical Corporation; DIC manufactured EPICLON 5500, EPICLON 5800, EPICLON 1050, EPICLON 1055, EPICLON 3050, EPICLON 4050, EPICLON 7050, EPICLON AM-030-P, EPICLON AM-040-P, EPICLON HM-091, EPICLON TSR-601; Nippon Kayaku's LCE-2615; and the like.

[0019] In the present invention, the epoxy resin (b) may contain (i) an epoxy resin that is liquid at 25°C, and / or (ii) an epoxy resin that has an epoxy equivalent of less than 400 g / eq and is solid or semi-solid at 25°C. Examples of such epoxy resins include bisphenol-type epoxy resins, naphthalene-type epoxy resins, glycidyl ester-type epoxy resins, glycidyl amine-type epoxy resins, phenol novolac-type epoxy resins, alicyclic epoxy resins such as alicyclic epoxy resins having an ester skeleton, cyclohexane-type epoxy resins, cyclohexane dimethanol-type epoxy resins, glycidyl amine-type epoxy resins, and epoxy resins having a structure that is an epoxidized product of polybutadiene polyol, rubber-modified epoxy resins, chelate-modified epoxy resins, urethane-modified epoxy resins, polysulfide-modified epoxy resins, etc. Preferably, one or more selected from the group consisting of bisphenol-type epoxy resins, rubber-modified epoxy resins, alicyclic epoxy resins, glycidyl amine-type epoxy resins, urethane-modified epoxy resins, polysulfide-modified epoxy resins, chelate-modified epoxy resins, trisphenol methane-type epoxy resins, and dicyclopentadiene-modified epoxy resins are used.

[0020] The content of the epoxy resin (b) in the conductive resin composition is not particularly limited, and is, for example, 0.1% by mass or more, preferably 0.5% by mass or more, more preferably 1.0% by mass or more, and for example, 10.0% by mass or less, preferably 9.0% by mass or less, more preferably 8.0% by mass or less, based on 100% by mass of the total amount of components other than the solvent in the conductive resin composition. When the total amount of components other than the solvent in the conductive resin composition is taken as 100 mass%, if the content of (b) the epoxy resin is less than 0.1 mass%, there is a risk that a film cannot be formed, that curing takes a long time, or that the dispersibility of the tin powder decreases and a uniform composition cannot be formed. If the content exceeds 10.0 mass%, there is a risk that the conductivity decreases and the volume resistivity increases.

[0021] The content of epoxy resins in the (b) epoxy resin having an epoxy equivalent of 400 g / eq or more and in a solid or semi-solid state at 25° C., relative to the total amount of the (b) epoxy resin being 100 mass%, can be, for example, 10 mass% or more, preferably 25 mass% or more, and more preferably 50 mass% or more, and can be 100 mass% or less (only epoxy resins having an epoxy equivalent of 400 g / eq or more and in a solid or semi-solid state at 25° C. are used).

[0022] <(c) Dicarboxylic acid compound> The (c) dicarboxylic acid compound is, for example, represented by R-(COOH)2 (wherein R is hydrogen or an organic group having 1 to 50 carbon atoms. R may contain an oxygen atom, a nitrogen atom, or a sulfur atom.) In the present invention, the (c) dicarboxylic acid compound includes a dicarboxylic acid compound having 4 to 9 carbon atoms. Examples of the dicarboxylic acid compound having 4 to 9 carbon atoms include succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, maleic acid, fumaric acid, citraconic acid, glutaconic acid, itaconic acid, mesaconic acid, 2-pentenedioic acid, methylenesuccinic acid, allylmalonic acid, hexadienedioic acid, terephthalic acid, isophthalic acid, o-phthalic acid, 1,4-cyclohexyldicarboxylic acid, malic acid, tartaric acid, 2,4-diethylglutaric acid, diglycolic acid, glutamic acid, aspartic acid, and thiodiglycolic acid. Among these, aliphatic dicarboxylic acid compounds having 4 to 9 carbon atoms are preferred, aliphatic dicarboxylic acid compounds having 5 to 9 carbon atoms are more preferred, and aliphatic dicarboxylic acid compounds having 6 to 8 carbon atoms are even more preferred. In the aliphatic dicarboxylic acid having 4 to 9 carbon atoms, the aliphatic group may be linear or branched.

[0023] In the present invention, the (c) dicarboxylic acid compound may contain a dicarboxylic acid other than a dicarboxylic acid compound having 4 to 9 carbon atoms (such as a dicarboxylic acid compound having 2 to 3 carbon atoms and a dicarboxylic acid compound having 10 or more carbon atoms). Examples of the dicarboxylic acid compound having 2 to 3 carbon atoms include one or more selected from the group consisting of oxalic acid, malonic acid, and the like. Examples of dicarboxylic acid compounds having 10 or more carbon atoms include sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, eicosane diacid, nonadecanedioic acid, docosane diacid, eicosadiene diacid, isoeicosane diacid, isodocosane diacid, isodocosadiene diacid, butyloctanedioic acid, 2-methylazelaic acid, dimethylmethacrylate ... and the like).

[0024] (c) By using a dicarboxylic acid compound containing a dicarboxylic acid compound having 4 to 9 carbon atoms as the dicarboxylic acid compound, it is possible to improve the dispersibility of the tin powder, increase the content of the tin powder, and increase the electrical conductivity.

[0025] The content of the (c) dicarboxylic acid compound in the conductive resin composition is not particularly limited, and is, for example, 0.1% by mass or more, preferably 0.3% by mass or more, more preferably 0.5% by mass or more, and for example, 4.0% by mass or less, preferably 3.5% by mass or less, more preferably 3.0% by mass or less, based on 100% by mass of the total amount of components other than the solvent in the conductive resin composition. When the content of the (c) dicarboxylic acid compound is less than 0.1% by mass, assuming that the total amount of components other than the solvent in the conductive resin composition is 100% by mass, there are concerns that a film cannot be formed, that curing takes a long time, that the dispersibility of the tin powder is reduced and a uniform composition cannot be formed, and the like. When the content exceeds 4.0% by mass, there are concerns that the conductivity is reduced, the volume resistivity is increased, and that storage stability is reduced.

[0026] The content of the dicarboxylic acid compounds having 4 to 9 carbon atoms in the (c) dicarboxylic acid compounds is, for example, 10 mass% or more, preferably 25 mass% or more, and more preferably 50 mass% or more, and can be 100 mass% or less (only dicarboxylic acid compounds having 4 to 9 carbon atoms are used), relative to the total amount of the (c) dicarboxylic acid compounds being 100 mass%.

[0027] <(d) Thiol-based compounds> The conductive resin composition of the present invention may further contain (d) a thiol-based compound. The (d) thiol-based compound can act as a curing agent for the (b) epoxy resin in the conductive resin composition, and can cause the curing of the conductive resin composition to proceed more quickly and reliably.

[0028] The (d) thiol-based compound may be one or more compounds having one or more thiol groups in the molecule that can react with an epoxy group. Preferably, one or more compounds having two or more thiol groups. The (d) thiol-based compound is more preferably one having 2 to 6 (bifunctional to hexafunctional) thiol groups in one molecule, and even more preferably one having 3 to 6 (trifunctional to hexafunctional) thiol groups in one molecule.

[0029] (d) Examples of thiol compounds include trimethylolpropane tris(3-mercaptopropionate) (abbreviation: TMTP), pentaerythritol tetrakis(3-mercaptopropionate) (abbreviation: PEMP), dipentaerythritol hexakis(3-mercaptopropionate) (abbreviation: DPMP), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate (abbreviation: TEMPIC), tris(3-mercaptopropyl)isocyanurate (abbreviation: TMPIC), ethylene glycol bisthioglycolate (abbreviation: EGTG), trimethylolpropane tristhioglycolate (abbreviation: TMTG), pentaerythritol tetrakisthioglycolate (abbreviation: PETG), pentaerythritol tetrakis(3-mercaptobutylate), tris(3-mercaptobutyryloxy)butane, 1,3,5-tris(3-mercaptobutyryloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, trimethylolpropane tris(3-mercaptobutyrate) (abbreviation: TPMB), trimethylolethane tris(3-mercaptobutyrate) (abbreviation: TEMB), 1,3,4,6-tetrakis(2-mercaptoethyl)glycoluril, 1,3,4,6-tetrakis(2-mercaptopropyl)glycoluril, 4,4'-isopropylidenebis[(3-mercaptopropoxy)benzene], thiocyanuric acid (1,3,5-triazine-2,4,6-trithiol), polysulfide polymers having a thiol group, and the like can be mentioned as one or more selected from the group consisting of 1,3,5-tris(3-mercaptobutyryloxy)ethyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, trimethylolpropane tris(3-mercaptobutyrate) (abbreviation: TPMB), trimethylolethane tris(3-mercaptobutyrate) (abbreviation: TEMB), 1,3,4,6-tetrakis(2-mercaptoethyl)glycoluril, 1,3,4,6-tetrakis(2-mercaptopropyl)glycoluril, 4,4'-isopropylidenebis[(3-mercaptopropoxy)benzene], thiocyanuric acid (1,3,5-triazine-2,4,6-trithiol), polysulfide polymers having a thiol group, and the like.

[0030] Specific examples include thiol compounds manufactured by SC Organic Chemical Industry Co., Ltd. (TMMP-LV, PEMP-LV, DPMP, TEMPIC, PEMP, etc.), thiol compounds manufactured by Toray Fine Chemical Co., Ltd. (QE-340M, LP-3, LP-55, LP-31, etc.), thiol compounds manufactured by Shikoku Chemical Industry Co., Ltd. (TS-G, C3TS-G, etc.), thiol compounds manufactured by Resonaq Inc. (PE-1, BD-1, NR-1, TPMB, TEMB, etc.), thiol compounds manufactured by Yodo Chemical Industry Co., Ltd. (OTG, EGTG, TMTG, PETG, 3-MPA, TMTP, PETP, etc.), and thiol compounds manufactured by Sakai Chemical Industry Co., Ltd. (TEMP, PEMP, TEMPIC, DPMP, etc.).

[0031] The content of the thiol compound (d) in the conductive resin composition is not particularly limited. In the present invention, the conductive resin composition can be cured without using the thiol compound (d). When the (d) thiol compound is contained, the thiol group (-SH group) in the (d) thiol compound is, for example, 0.05 equivalents or more, preferably 0.10 equivalents or more, more preferably 0.15 equivalents or more, and is preferably contained in an amount of, for example, 4.00 equivalents or less, preferably 3.50 equivalents or less, more preferably 1.50 equivalents or less, relative to 1 equivalent of the epoxy group of the epoxy resin. When the (d) thiol compound content exceeds 4.00 equivalents, the coating film may be poorly cured due to the influence of the excess unreacted curing agent, and the coating film hardness may be reduced. Furthermore, when the thiol compound (d) is contained, the amount is, for example, 1.0 part by mass or more, preferably 1.5 parts by mass or more, more preferably 2.0 parts by mass or more, and can be, for example, 250 parts by mass or less, preferably 200 parts by mass or less, more preferably 180 parts by mass or less, relative to 100 parts by mass of the epoxy resin. If the amount of the thiol compound (d) exceeds 250 parts by mass relative to 100 parts by mass of the epoxy resin, the conductive resin composition may not become solid.

[0032] <(e) Solvent> The conductive resin composition of the present invention may further contain (e) a solvent. This can improve the fluidity of the conductive resin composition and contribute to improving workability. In addition, by mixing the conductive resin composition with a solvent, a conductive resin paste, a conductive material, a conductive adhesive, or a circuit connecting material can be formed.

[0033] The solvent may be any one or more selected from the group consisting of water and various organic solvents. Examples of the organic solvent include alcohol-based solvents and alcohol ether-based solvents such as ethyl alcohol, propyl alcohol, butyl alcohol, pentyl alcohol, hexyl alcohol, heptyl alcohol, octyl alcohol, nonyl alcohol, decyl alcohol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, diethylene glycol dibutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, methyl methoxybutanol, α-terpineol, β-terpineol, hexylene glycol, benzyl alcohol, 2-phenylethyl alcohol, isopalmityl alcohol, isostearyl alcohol, lauryl alcohol, ethylene glycol, propylene glycol, and glycerin; acetone, methyl ethyl ketone ... Ketone solvents such as ethyl isobutyl ketone, cyclohexanone, diacetone alcohol (4-hydroxy-4-methyl-2-pentanone), 2-octanone, isophorone (3,5,5-trimethyl-2-cyclohexen-1-one) or diisobutyl ketone (2,6-dimethyl-4-heptanone); ethyl acetate, butyl acetate, diethyl phthalate, dibutyl phthalate, acetoxyethane, methyl butyrate, methyl hexanoate, methyl octanoate, methyl decanoate, methyl cellosolve acetate, ethylene glycol monobutyrate ester-based solvents such as ethylene glycol monomethyl ether acetate, propylene glycol monomethyl ether acetate, and 1,2-diacetoxyethane; ether-based solvents such as tetrahydrofuran, dimethyl ether, diethyl ether, dipropyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, propylene glycol dimethyl ether, ethoxyethyl ether, 1,2-bis(2-diethoxy)ethane, and 1,2-bis(2-methoxyethoxy)ethane;Examples of the solvent include at least one selected from the group consisting of ester ethers such as 2-(2-butoxyethoxy)ethane acetate; ether alcohol solvents such as 2-(2-methoxyethoxy)ethanol; hydrocarbon solvents such as benzene, toluene, xylene, n-paraffin, isoparaffin, dodecylbenzene, turpentine oil, kerosene, and light oil; nitrile solvents such as acetonitrile and propionitrile; nitrogen-containing polar solvents such as dimethylacetamide, N,N-dimethylformamide, and N-methyl-2-pyrrolidone; and silicone oil solvents. Among these, one or more selected from the group consisting of alcohol solvents, alcohol ether solvents, ether solvents, ester solvents, and ketone solvents are preferred, one or more selected from the group consisting of alcohol ether solvents, ether solvents, ester solvents, and ketone solvents are more preferred, and one or more selected from the group consisting of alcohol ether solvents, ether solvents, and ester solvents are even more preferred. When an organic solvent is used, the amount used is not particularly limited, and may be appropriately adjusted so that the viscosity of the conductive resin composition is such that it can be appropriately applied, printed, etc. onto a substrate and / or such that it can be appropriately impregnated into a porous body.

[0034] <(f) Other ingredients> In addition to the above (a) to (e), the conductive resin composition of the present invention may contain, as necessary, one or more additives selected from the group consisting of organic acid compounds, epoxy resin curing agents, epoxy resin curing accelerators, conductive powders other than tin powder, adhesion promoters, viscoelasticity modifiers, wetting and dispersing agents, reactive diluents, resins other than epoxy resins, pigments, fillers, antioxidants, corrosion inhibitors, defoamers, coupling agents, anti-settling agents, leveling agents, heavy metal deactivators, gap adjusters, and the like, as "(f) other components".

[0035] (organic acid compound) The organic acid compound is an organic acid compound other than a dicarboxylic acid compound, for example, RX n(wherein R is hydrogen or an organic group having 1 to 50 carbon atoms, X is an acid group and multiple Xs may be different from each other, and n is an integer of 1 or more). Examples of the acid group represented by X include a carboxyl group (-COOH), a sulfonic acid group (-SO3H), and a phosphoric acid group (-PO4H2). Examples of the organic acid compound include one or more selected from the group consisting of organic carboxylic acid compounds other than dicarboxylic acid compounds, organic sulfonic acid compounds, organic phosphonic acid compounds, etc. Preferred are organic carboxylic acid compounds other than dicarboxylic acid compounds.

[0036] {Organic carboxylic acid compound} The organic carboxylic acid compound is not particularly limited as long as it is a compound having one or three or more carboxyl groups (-COOH) in the molecular structure and having 1 to 50 carbon atoms. Examples of organic carboxylic acid compounds include formic acid, acetic acid, propionic acid, butanoic acid, pentanoic acid, hexanoic acid, heptanoic acid, octylic acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, 12-hydroxystearic acid, ricinoleic acid, oleic acid, vaccenic acid, linoleic acid, linolenic acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, melissic acid, behenic acid, arachidonic acid, eicosapentaenoic acid, docosahexaenoic acid, lactic acid, gluconic acid, citric acid, ascorbic acid, abietic acid, dimethylolpropionic acid, dimethylolbutanoic acid, dimethylolbutyric acid, dimethylolvaleric acid, trimethylolpropanoic acid, trimethylolpropanoic acid, trimethylolbutanoic acid, trimethylolbutanoic acid, trimethylolbutyric acid, trimethylolvaleric acid, trimethylolpropanoic acid, trimethylolbut ... Examples of the carboxylic acid include dimethylol butanoic acid, benzoic acid, salicylic acid, pyruvic acid, paramethylbenzoic acid, toluic acid, 4-ethylbenzoic acid, 4-propylbenzoic acid, 2-methylpropanoic acid, isopentanoic acid, 2-ethylhexanoic acid, acrylic acid, methacrylic acid, propiolic acid, crotonic acid, 2-ethyl-2-butenoic acid, hexanetricarboxylic acid, cyclohexylcarboxylic acid, ethylenediaminetetraacetic acid, trimellitic acid, pyromellitic acid, monomethyl glutarate, glycolic acid, isoleucine, leucine, lysine, methionine, phenylalanine, threonine, tryptophan, valine, histidine, tyrosine, cysteine, asparagine, serine, glutamine, proline, glycine, alanine, and arginine.

[0037] {Organic sulfonic acid compounds} The organic sulfonic acid compound is not particularly limited as long as it has one or more sulfonic acid groups (-SO3H) in its molecular structure. For example, benzenesulfonic acid, n-butylbenzenesulfonic acid, n-octylbenzenesulfonic acid, n-dodecylbenzenesulfonic acid, pentadecylbenzenesulfonic acid, 2,5-dimethylbenzenesulfonic acid, p-chlorobenzenesulfonic acid, 2,5-dichlorobenzenesulfonic acid, p-phenolsulfonic acid, cumenesulfonic acid, xylenesulfonic acid, o-cresolsulfonic acid, m-cresolsulfonic acid, p-cresolsulfonic acid, p-toluenesulfonic acid, 2-naphthalenesulfonic acid, 1-naphthalenesulfonic acid, styrenesulfonic acid, 4,4-biphenyldisulfonic acid, anthraquinone-2-sulfonic acid, m-benzenedisulfonic acid, Examples of the sulfonic acid compounds include aromatic sulfonic acid compounds such as aniline-2,4-disulfonic acid, anthraquinone-1,5-disulfonic acid, and polystyrene sulfonic acid; aliphatic sulfonic acid compounds such as methanesulfonic acid, ethanesulfonic acid, 1-propanesulfonic acid, n-octyl sulfonic acid, pentadecylsulfonic acid, trifluoromethanesulfonic acid, trichloromethanesulfonic acid, 1,2-ethanedisulfonic acid, 1,3-propanedisulfonic acid, aminomethanesulfonic acid, and 2-aminoethanesulfonic acid; and alicyclic sulfonic acid compounds such as cyclopentanesulfonic acid, cyclohexanesulfonic acid, and 3-cyclohexylaminopropanesulfonic acid. Preferable examples include one or more selected from the group consisting of benzenesulfonic acid, dodecylbenzenesulfonic acid, methanesulfonic acid, p-phenolsulfonic acid, p-toluenesulfonic acid, and (poly)styrenesulfonic acid.

[0038] {Organic phosphonic acid compounds} The organic phosphonic acid compound is not particularly limited as long as it has one or more phosphonic acid groups (-PO3H2) in its molecular structure. For example, 1-hydroxyethylidene-1,1-diphosphonic acid, 1-hydroxypropylidene-1,1-diphosphonic acid, 1-hydroxybutylidene-1,1-diphosphonic acid, aminotrimethylenephosphonic acid, methyldiphosphonic acid, nitrotrimethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, ethylenediaminebismethylenephosphonic acid, hexamethylenediaminetetramethylenephosphonic acid, diethylenetriaminepentamethylenephosphonic acid, cyclohexanediaminetetramethylenephosphonic acid, and the like. Examples of the phosphonic acid include one or more selected from the group consisting of phosphonic acid, carboxyethylphosphonic acid, phosphonoacetic acid, 2-phosphonobutane-1,2,4-tricarboxylic acid, 2,3-dicarboxypropane-1,1-diphosphonic acid, phosphonobutyric acid, phosphonopropionic acid, sulfonylmethylphosphonic acid, N-carboxymethyl-N,N-dimethylenephosphonic acid, N,N-dicarboxymethyl-N-methylenephosphonic acid, 2-ethylhexyl acid phosphate, stearyl acid phosphate, benzenephosphonic acid, and the like.

[0039] The organic phosphonic acid compound may be a surfactant having a phosphate group (-PO4H2) in its molecular structure. The surfactant having a phosphoric acid group is preferably one having a polyoxyethylene group or a phenyl group in the molecular structure. For example, one or more selected from the group consisting of polyoxyethylene alkylphenyl ether phosphate, polyoxyethylene alkyl ether phosphate, dipolyoxypropylene lauryl ether phosphate, dipolyoxyethylene oleyl ether phosphate, dipolyoxyethylene oxypropylene lauryl ether phosphate, dipolyoxypropylene oleyl ether phosphate, ammonium lauryl phosphate, ammonium octyl ether phosphate, ammonium cetyl ether phosphate, polyoxyethylene lauryl ether phosphate, polyoxyethylene oxypropylene lauryl ether phosphate, polyoxypropylene lauryl ether phosphate, polyoxyethylene tristyryl phenyl ether phosphate, polyoxyethylene oxypropylene tristyryl phenyl ether phosphate, polyoxypropylene tristyryl phenyl ether phosphate, etc. As the surfactant having a phosphate group, one or more types selected from the group consisting of commercially available products such as Phosphanol (trade name) manufactured by Toho Chemical Industry Co., Ltd. and DISPERBYK (trade name) manufactured by BYK-Chemie Japan KK can be used.

[0040] (Epoxy resin hardener) The conductive resin composition of the present invention may contain an epoxy resin curing agent other than (d) a thiol-based compound. This improves the curability of the conductive resin composition, which can contribute to improving the bonding strength, etc. Examples of the epoxy resin curing agent include amine-based curing agents, acid anhydride-based curing agents, and phenol-based curing agents. These may be used alone or in combination of two or more. From the viewpoint of more effectively improving workability, handling, etc., the conductive resin composition of the present invention preferably contains a curing agent that is liquid at 20°C.

[0041] {Amine-based hardener} Examples of amine curing agents include diethylenetriamine, triethylenetetramine, diethylaminopropylamine, menthanediamine, isophoronediamine, bis[4-amino-3-methyldicyclohexyl]methane, diaminodicyclohexylmethane, bis(aminomethyl)cyclohexane, m-xylylenediamine, metaphenylenediamine, diaminodiphenylmethane, diaminodiethyldiphenylmethane, and modified polyamines and polyamidoamines obtained by modifying these through epoxy adduct, Michael addition, Mannich reaction, etc. These may be used alone or in combination of two or more.

[0042] {Acid anhydride curing agent} There are no particular limitations on the acid anhydride curing agent as long as it is a compound having one or more carboxylic acid anhydride groups (-C(=O)-OC(=O)-) in the molecular structure. The acid anhydride-based curing agent is obtained by intermolecular dehydration of two organic carboxylic acid molecules and / or intramolecular dehydration of one organic carboxylic acid molecule. In the present invention, for example, among the organic carboxylic acids, one or more types selected from the group consisting of those obtained by intermolecular dehydration of organic monocarboxylic acid and those obtained by intramolecular dehydration and / or intermolecular dehydration of organic polycarboxylic acid can be mentioned. For example, one or more types selected from the group consisting of aliphatic monocarboxylic acid anhydrides, aliphatic polycarboxylic acid anhydrides, alicyclic polycarboxylic acid anhydrides, aromatic polycarboxylic acid anhydrides, etc. can be mentioned. Preferred examples of the anhydride include one or more selected from the group consisting of acetic anhydride, glutaric anhydride, propionic anhydride, oxalic anhydride, maleic anhydride, phthalic anhydride, benzoic anhydride, succinic anhydride, 2-methylsuccinic anhydride, trimellitic anhydride, pyromellitic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, (poly)adipic anhydride, (poly)azelaic anhydride, (poly)sebacic anhydride, norbornene-2,3-dicarboxylic anhydride, and methyl-5-norbornene-2,3-dicarboxylic anhydride.

[0043] In the present invention, the following structural formula (1) [ka] (In structural formula (1), R 1 is a straight-chain or branched hydrocarbon group having 10 or more carbon atoms. One or more polyacid polyanhydrides represented by the formula (I) may be used as an acid anhydride-based curing agent. Such polyacid polyanhydrides are obtained by intermolecular dehydration condensation reaction of long-chain aliphatic dicarboxylic acids. Examples include SL-12AH, SL-20AH, SB-20AH, IPU-22AH, and ST-2PAH manufactured by Okamura Oil Mills. In particular, SB-20AH, IPU-22AH, and ST-2PAH, which are liquid at 25°C, are preferably used.

[0044] {Phenol-based hardener} Examples of phenol-based curing agents include compounds having one or more, preferably two or more, phenolic hydroxyl groups that can react with epoxy groups in the molecule. For example, bisphenols such as bisphenol A, bisphenol B, bisphenol F, bisphenol AD, and bisphenol S; biphenols such as biphenol and tetramethylbiphenol; phenols such as hydroxyphenol and bis(4-hydroxyphenyl)ether; alkylphenols; phenol novolacs such as 2,6-bis[(2-hydroxyphenyl)methyl]-phenol and phenol biphenylene novolac (biphenylaralkylphenol); cresol novolacs such as o-cresol novolac, m-cresol novolac, and p-cresol novolac; phenol resins; and the like. These may be used alone or in combination of two or more.

[0045] {Epoxy resin hardener content} In the conductive resin composition of the present invention, the content of the epoxy resin curing agent is not particularly limited. In the present invention, the conductive resin composition can be cured without using a curing agent. When a curing agent is contained, the group that reacts with the epoxy group in the curing agent (e.g., hydroxyl group, amino group, carboxyl group (formed from acid anhydride group)) can be, for example, 0.7 equivalents or more, preferably 0.8 equivalents or more, more preferably 0.9 equivalents or more, and for example, 1.3 equivalents or less, preferably 1.2 equivalents or less, more preferably 1.1 equivalents or less, relative to 1 equivalent of the epoxy group of the epoxy resin. If it exceeds 1.3 equivalents, the coating film may be cured poorly due to the influence of the excess unreacted curing agent, and the coating film hardness may be reduced. Most preferably, it is 1.0 equivalent.

[0046] (Epoxy resin curing accelerator) The conductive resin composition of the present invention may contain a curing accelerator (curing catalyst) for accelerating the curing of the epoxy resin. The curing accelerator is not particularly limited, but may be an amine-based curing accelerator, a guanidine-based curing accelerator, an imidazole-based curing accelerator, a phosphonium-based curing accelerator, or the like. These may be used alone or in combination of two or more. For example, ethyleneamines such as ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, and pentaethylenehexamine, aliphatic tertiary amines such as triethylamine, tripropylamine, tributylamine, dimethylbutylamine, dimethylpentylamine, and dimethylcyclohexylamine, dimethylbenzylamine, dimethylaminomethylphenol, dimethylamino-p-cresol, piperidine, α-picoline, pyridine, 2,4,6-tris(dimethylaminomethyl)phenol, 3,4,5-tris(dimethylaminomethyl)phenol, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, 2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-methylimidazole, Examples of the compound include 1-cyanoethyl-2-ethyl-4-methylimidazole, N-aminoethylpiperazine, 1,3,6-trisaminomethylhexane, m-xylenediamine, p-xylenediamine, N-(2-aminoethyl)piperazine, m-phenylenediamine, p-phenylenediamine, diaminophenylmethane, methylenedianiline, 2,4-toluenediamine, 2,4-diaminoanisole, 2,4-toluenediamine, 2,4-diaminodiphenylamine, 4,4'-methylenedianiline, 1,3-diaminocyclohexane, 3,9-bis(3-aminopropyl)-2,4,8,10-tetrapyro[5,5]undecane, 1,8-diazabicyclo[5,4,0]undecene-7, or polyamine, polyamidoamine, polyamide, modified polyamine, modified polyamidoamine, modified polyamide, etc. These may be used alone or in combination of two or more.

[0047] (Conductive powder other than tin powder) The conductive resin composition of the present invention may contain a conductive powder other than tin powder, such as lead-free solder powder, gold powder, silver powder, copper powder, silver-coated copper powder, silver-coated silica powder, silver-coated nickel powder, resin core metal-coated fine particles, nickel powder, conductive carbon powder, etc. For example, the lead-free solder powder is not particularly limited as long as it is a solder powder that does not contain more than the amount of lead that is unavoidably contained due to the influence on workers, users, the environment, etc. The melting point of the lead-free solder powder is preferably 300°C or less, more preferably 240°C or less, and even more preferably 50 to 240°C. If the melting point of the lead-free solder powder exceeds 300°C, there is a risk of thermal destruction or thermal deterioration of connected members such as circuit boards and electronic components. If the melting point is less than 50°C, there is a risk of the mechanical strength being weakened and the reliability of the conductive connection being reduced.

[0048] (Adhesion promoter) The conductive resin composition of the present invention may contain an adhesion promoter. This can improve the adhesion to the substrate when the conductive resin composition is applied to the substrate. Examples of the adhesion promoter include triazole compounds, thiazole compounds, triazine compounds, porphyrin compounds, polymers having functional groups (carboxylic acid groups, amino groups, hydroxyl groups, etc.) and salts thereof. These may be used alone or in combination of two or more. Examples of adhesion promoters include the BYK series (4509, 4510, 4512, etc.) manufactured by BYK Japan.

[0049] (Viscoelasticity modifier) The conductive resin composition of the present invention may contain a viscoelasticity modifier (rheology control agent), which can adjust the viscoelasticity (rheology) of the conductive resin composition and contribute to improving workability, etc. Examples of the viscoelasticity adjusting agent (rheology control agent) include polyamide-based, aminoplast-based, polycarboxylic acid-based, urethane-based, cellulose-based, and inorganic layered compound-based viscoelasticity adjusting agents (rheology control agents). For example, RHEOBYK series (H370, H400, H600, H600VF, 100, 405, 410, 411, 415, 430, 431, 440, 7410ET, etc.) manufactured by BYK Japan; Disparlon series (AQ-600, AQH-800, 3600N, 3900EF, etc.) manufactured by Kusumoto Chemical Industries, Ltd.; SN Thickener series (613, 617, 618, 630, 634, 636, 621N, 623N, etc.) manufactured by San Nopco; Adekanol series (UH-814N, UH-752, UH-750, UH-462, etc.) manufactured by ADEKA Corporation, HEC Daicel series (SP600N, etc.) manufactured by Daicel Corporation; BENTONE HD manufactured by Elementis Japan Co., Ltd., etc. These may be used alone or in combination of two or more.

[0050] (Wetting and dispersing agent) The conductive resin composition of the present invention may contain a dispersant, if necessary, to prevent aggregation of the tin powder. Specific examples of wetting and dispersing agents include the Solsperse series (9000, 12000, 17000, 20000, 21000, 24000, 26000, 27000, 28000, 32000, 35100, 54000, etc.) manufactured by Lubrizol Japan, and the EFKA series (4008, 4009, 4010, 4015, 4046, 4047, 4060, 4080, 7462, 4020, 4050, 4055, 4400, 4401, 4402, 4403, 4300, 4330, 4340, 6220, 6225, 6700, 6780, 6782, 8503, etc.) manufactured by EFKA Additives. ), Ajinomoto Fine-Techno Co., Ltd.'s Ajisper series (PA111, PB711, PB821, PB822, PN411, etc.), BYK-Chemie Japan's DISPERBYK series (101, 106, 108, 116, 130, 140, 145, 161, 163, 166, 168, 171, 180, 192, 2000, 2001, 2020, 2025, 2070, 2152, 2155, 2164, 220S, 300, 320, 340, 378, 380N, 410, 425, 430, etc. These may be used alone or in combination of two or more.

[0051] (Reactive diluent) The curable resin composition of the present invention may contain a reactive diluent for adjusting the viscosity or curability of the conductive resin composition. The reactive diluent is not particularly limited, and may be one or more of a compound having one epoxy group in its molecular structure, a compound having one or more oxetane groups in its molecular structure, etc. Examples of the reactive diluent include glycidyl phenyl ether, glycidyl lauryl ether, 2-phenylphenol glycidyl ether, allyl glycidyl ether, 4-tert-butylphenyl glycidyl ether, N-glycidyl phthalimide, 2-ethylhexyl glycidyl ether, 2-ethylhexyl glycidyl ether, YED111N, YED111AN, and YED188 manufactured by Mitsubishi Chemical Corporation, ADEKA Glycirol ED-502 and ADEKA Glycirol ED-502S manufactured by ADEKA Corporation, Examples of such a surfactant include ADEKA GLYCILOR ED-509E, ADEKA GLYCILOR ED-509S, ADEKA GLYCILOR ED-529, DENACOL EX-145, DENACOL EX-171, and DENACOL EX-192 manufactured by Nagase ChemteX Corporation, EPOLYTE M-1230 and EPOLYTE 100MF manufactured by Kyoeisha Chemical Co., Ltd., ARON OXETANE OXT-101, ARON OXETANE OXT-212, ARON OXETANE OXT-121, and ARON OXETANE OXT-221 manufactured by Toagosei Co., Ltd., and ETERNACOLL EHO, ETERNACOLL HBOX, ETERNACOLL OXMA, and ETERNACOLL OXBP manufactured by UBE Co., Ltd. These may be used alone or in combination of two or more.

[0052] (Resins other than epoxy resins) The conductive resin composition of the present invention may contain a resin other than the epoxy resin. Such a resin may be either a thermoplastic resin or a thermosetting resin, and one or more kinds of such a resin may be used. Examples of the thermoplastic resin include one or more selected from the group consisting of polyvinyl acetal resins, acrylic resins, polyester resins, phenoxy resins, polyimide resins, polyolefin resins, thermoplastic polyurethane resins, polyamide resins, polycarbonate resins, polyphenylene ether resins, polyvinyl ether resins, polyvinyl alcohol resins, polyvinyl acetate resins, ionomer resins, and block urethane resins. Examples of the thermosetting resin include one or more resins selected from the group consisting of resol-type phenolic resins, polyimide resins, xylene resins, polyurethane resins, melamine resins, urea resins, and furan resins. In the present invention, the resin preferably contains at least one selected from the group consisting of polyvinyl acetal resins, resol-type phenolic resins, acrylic resins, polyester resins, phenoxy resins, polyimide resins, and xylene resins. Among these, polyvinyl acetal resins are preferably used from the viewpoints of film formation state, connection reliability, adhesion to substrates, etc.

[0053] (Coupling Agent) The epoxy resin composition of the present invention may contain a coupling agent. This can improve the short-time heating bonding strength of the epoxy resin composition. Examples of the coupling agent include a silane coupling agent, a titanium coupling agent, an aluminum coupling agent, and a zirconium coupling agent. Examples of the silane coupling agent include amino group-containing silane compounds such as aminoethylaminopropyltrimethoxysilane, aminoethylaminopropylmethyldimethoxysilane, and aminoethylaminopropylmethylmethoxysilane; vinyl group-containing silane compounds such as vinyltrimethoxysilane; epoxy group-containing silane compounds such as γ-glycidoxypropyltrimethoxysilane; (meth)acryloyl group-containing silane compounds such as γ-methacryloxypropyltrimethoxysilane; mercaptosilanes such as γ-mercaptopropyltrimethoxysilane, and isocyanate group-containing silane compounds such as γ-isocyanatepropyltrimethoxysilane; and the like. Examples of titanium coupling agents include tetraisopropyl titanate, tetranormalbutyl titanate, butyl titanate, tetraoctyl titanate, titanium acetylacetonate, titanium tetraacetylacetonate, titanium ethylacetoacetate, dodecylbenzenesulfonic acid titanium compound, titanium octylene glycolate, titanium ethylacetoacetate, titanium lactate ammonium salt, titanium lactate, titanium triethanolamine, tetraisopropyl titanate, tetratertiarybutyl titanate, tetrastearyl titanate, titanium acetylacetonate, titanium octylene glycolate, titanium isostearate, titanium diethanolamine, titanium aminoethylaminoethanolate, titanium oligomer, etc. Examples of aluminum coupling agents include aluminate compounds having an alkoxide group such as alkylacetoacetate aluminum diisopropylate, and aluminate compounds having an acetylacetonate group such as aluminum trisacetylacetonate.Examples of zirconium coupling agents include tetra-n-propoxyzirconium, tetra-butoxyzirconium, zirconium tetraacetylacetonate, zirconium dibutoxybis(acetylacetonate), zirconium tributoxyethylacetoacetate, zirconium butoxyacetylacetonate bis(ethylacetoacetate), and tetrakis(2,4-pentanedionate)zirconium. The coupling agent may be used alone or in combination of two or more kinds.

[0054] <Properties of the conductive resin composition> The conductive resin composition of the present invention may be in any form, such as a powder, solid, paste, liquid (varnish), etc. When used as a conductive material, conductive adhesive, or circuit connecting material, it is preferable that the composition is in a paste or liquid (varnish) form at room temperature (25° C.).

[0055] <Characteristics of the conductive resin composition> The conductive resin composition of the present invention has excellent conductivity. For example, the conductive film obtained by casting or applying the conductive resin composition onto a peelable substrate, drying it, and peeling it off has a volume resistivity of 3.0×10 -4 The volume resistivity of the conductive film is preferably less than 2.0×10 -4 The volume resistivity is less than Ω·cm. Here, the volume resistivity is obtained by the method described in the examples. The conductive resin composition of the present invention has excellent adhesion to various substrates, for example, glass, metal, or plastic (e.g., polyester, etc.). The conductive resin composition of the present invention does not solidify, develop a skin on the surface, or separate from the liquid, whether it is left to stand at room temperature (25°C) for 24 hours (storage at room temperature (25°C) for 24 hours) or left to stand in a refrigerator (4°C) for one week (storage refrigerated (4°C) for one week), and there is only a small increase in viscosity before and after storage at room temperature for 24 hours and storage refrigerated for one week, demonstrating excellent storage stability.

[0056] <Method for preparing conductive resin composition> In preparing the conductive resin composition of the present invention, the essential components are tin powder, a specific epoxy resin, and a specific dicarboxylic acid compound, and if necessary, a thiol compound, a solvent, and other components can be added to a mixing vessel in any order and mixed to produce the composition. For example, a method of mixing using a centrifugal mixer, a ball mill, a roll mill, a bead mill, a planetary mixer, a tumbler, a stirrer, a mixer, a mechanical homogenizer, an ultrasonic homogenizer, a high-pressure homogenizer, a paint shaker, a V-type blender, a Nauta mixer, a Banbury mixer, a kneading roll, or a single-screw or twin-screw extruder can be appropriately used for mixing.

[0057] The temperature at which the conductive resin composition is prepared (the temperature at which each component is mixed) is not particularly limited. If necessary, heating or the like may be performed, and the conductive resin composition can be prepared at, for example, 10 to 100°C. The atmosphere in which the conductive resin composition is prepared is not particularly limited, and the preparation can be performed in air or in an inert atmosphere.

[0058] <Applications of the conductive resin composition> The conductive resin composition of the present invention is used in the manufacture of a conductive object. The conductive object may contain other members in addition to the conductive resin composition. Examples of the conductive object include one or more selected from the group consisting of conductive materials, circuit connection materials, conductive pastes, conductive films, conductive fibers, conductive paints, conductive materials for semiconductor packages, conductive materials for microelectronic devices, antistatic materials, electromagnetic wave shielding materials, conductive adhesives (such as die attachment adhesives), die attach pastes, actuators, sensors, and conductive resin molded bodies.

[0059] For example, by using the solvent as a component of the conductive resin composition, it is possible to form a conductive material, a circuit connecting material, a conductive paste, a conductive paint, a conductive adhesive, etc. The viscosity of the composition is not particularly limited, and the composition can be in the form of a low-viscosity varnish to a high-viscosity paste, etc., depending on the application. For example, a conductive resin composition containing a solvent or the like as necessary can be applied to various substrates by casting, dipping, bar coating, dispenser, roll coating, gravure coating, screen printing, flexographic printing, spray coating, spin coating, inkjet, or the like, and then dried by heating at a temperature of 300° C. or less to form a conductive film. The atmosphere during drying can be one or more selected from the group consisting of air, inert gas, vacuum, reduced pressure, and the like. In particular, from the viewpoint of suppressing deterioration of the conductive film (preventing oxidation of tin powder, etc.), an inert gas atmosphere such as nitrogen or argon is preferred.

[0060] The conductive resin composition of the present invention can be molded into a molded article by a molding method such as extrusion molding, injection molding, compression molding, etc. Examples of the molded article include electronic device parts, automobile parts, machine mechanism parts, food containers, films, sheets, fibers, etc.

[0061] [Conductive film] The conductive film of the present invention can be formed from the conductive resin composition. -4 The volume resistivity of the conductive film is preferably less than 2.0×10 -4 Less than Ω cm, more preferably less than 1.0×10 -4 The conductive film of the present invention has a resistivity of less than 1.0×10 -4 Less than Ω cm (10 -5 It is also possible to achieve a volume resistivity of the order of Ω·cm, which is comparable to that of a conductive film formed from silver paste. Here, the volume resistivity is obtained by the method described in the examples.

[0062] The method for forming a conductive film from the conductive resin composition is not particularly limited. For example, the conductive resin composition is made to contain a solvent, and the conductive film can be formed by applying or printing the conductive resin composition onto any substrate and drying the conductive film. Alternatively, the conductive resin composition can be cast or applied onto a peelable substrate, dried, and then peeled off. The conditions for forming the conductive film are not particularly limited and can be appropriately set depending on the substrate, etc. The temperature during drying, etc. after coating the conductive resin composition is, for example, 50° C. or higher, preferably 90° C. or higher, and, for example, 250° C. or lower, preferably 220° C. or lower. The time for drying, etc. is, for example, 5 minutes or higher, preferably 7 minutes or higher, and, for example, 300 minutes or lower, preferably 200 minutes or lower. In the present invention, when forming a conductive film, either the wet film thickness and / or the dry film thickness can be adjusted depending on the application, coating / printing method, and the like to form the conductive film. The wet film thickness of the conductive film (the wet film thickness of the conductive resin composition) is not particularly limited and can be appropriately adjusted depending on the application, etc. For example, it is 5 μm or more, preferably 10 μm or more, and for example, 1000 μm or less, preferably 500 μm or less. The dry thickness of the conductive film is not particularly limited and can be appropriately adjusted depending on the application, etc. For example, it is 1 μm or more, preferably 5 μm or more, and for example, 1000 μm or less, preferably 500 μm or less.

[0063] [Conductive materials] The conductive material of the present invention contains the conductive resin composition, and can be obtained, for example, by dissolving and / or dispersing the conductive resin composition in the solvent as necessary. In addition to the tin powder, a specific epoxy resin, and a specific dicarboxylic acid compound, the conductive material may further contain various additives for forming the conductive material (e.g., conductive powders other than tin powder, various curing agents, surfactants, pH adjusters (amine compounds, etc.), adhesion promoters, viscoelasticity adjusters, wetting and dispersing agents, leveling agents, pigments, UV absorbers, antioxidants, flame retardants, etc.). The conductive material can be obtained by placing the above-mentioned components in a mixing vessel, mixing them using one or more mixers selected from the group consisting of a rotation-revolution mixer, a ball mill, a roll mill, a bead mill, a planetary mixer, a tumbler, a stirrer, an agitator, a mechanical homogenizer, an ultrasonic homogenizer, a high-pressure homogenizer, a paint shaker, and the like, to form a varnish or paste.

[0064] The conductive material can be used, for example, as a conductive ink for printing to form wiring, a circuit forming material, or a material for forming internal and external electrodes of passive components. When the conductive material is used as a conductive ink for printing, the printing method may be, for example, one or more methods selected from the group consisting of screen printing, metal mask printing, inkjet printing, flexographic printing, gravure printing, dispenser method, etc. In the present invention, it is preferable to use one or more printing methods selected from the group consisting of screen printing, inkjet printing, etc., because they have excellent printability and shape retention. Here, the mesh used in the screen printing method can be appropriately selected, and it is preferable to employ a mesh that does not remove excessive amounts of conductive powder and lead-free solder powder from the conductive material.

[0065] The coating method for coating the conductive material on an article or the like is not particularly limited. Any coating method can be adopted depending on the shape and use form of the article or the like. For example, one or more coating methods selected from the group consisting of spin coating, dip coating, immersion, die coating, air spray, airless spray, electrostatic coating, brush coating, roller coating, roll coater, curtain flow coater, roller curtain coater, die coater, inkjet, and coating by a dispenser can be used.

[0066] The thickness of the coating film formed by coating the conductive material is not particularly limited and can be an appropriate thickness depending on various applications, for example, 1 μm or more, preferably 2 μm or more, more preferably 5 μm or more, and 400 μm or less, preferably 200 μm or less, more preferably 100 μm or less. The conductive material has excellent storage stability under refrigeration and room temperature, electrical conductivity, and at least one property selected from the group consisting of adhesion to various substrates, leveling (surface smoothness), printability, etc.

[0067] [Conductive adhesive] The conductive adhesive of the present invention contains the conductive resin composition. For example, the conductive adhesive can be obtained by dissolving and / or dispersing the conductive resin composition in the solvent as necessary. Conductive adhesives are used to bond parts to be bonded so that they have electrical conductivity. For example, they are used when performing adhesion that requires electrical conductivity in the manufacture of batteries and electrical and electronic devices. The conductive adhesive may further contain at least one selected from the group consisting of a solvent, a curing agent for curing an epoxy resin, an adhesion imparting agent, a viscoelasticity modifier, a wetting and dispersing agent, a curing accelerator (curing catalyst), a reactive diluent, a conductive powder other than tin powder, a resin other than an epoxy resin, an antioxidant, a pigment, a filler, a corrosion inhibitor, an antifoaming agent, a coupling agent, an antisettling agent, a leveling agent, a heavy metal deactivator, a surfactant, a pH adjuster, an ultraviolet absorber, a flame retardant, an adhesion imparting agent, and the like, as necessary. The conductive adhesive can be obtained by placing the above-mentioned components in a mixing container, mixing them using one or more mixers selected from the group consisting of a rotation-revolution mixer, a ball mill, a roll mill, a bead mill, a planetary mixer, a tumbler, a stirrer, an agitator, a mechanical homogenizer, an ultrasonic homogenizer, a high-pressure homogenizer, a paint shaker, a V-type blender, a Nauter mixer, a Banbury mixer, a kneading roll, a single-screw extruder, a twin-screw extruder, and the like, to form a varnish or paste.

[0068] The conductive adhesive of the present invention can be used as an anisotropic conductive adhesive, which can form highly reliable conductive connections in miniaturized IC chips, electronic components such as light-emitting diodes, and electrode connections on circuit boards. Examples of adhesive structures in which adherends are bonded together via the conductive adhesive of the present invention include RFID-related products such as IC cards and IC tags in which an IC chip is bonded to a substrate having an electrode, and light-emitting electronic components in which a light-emitting diode is bonded to a substrate having an electrode. For example, an adhesive structure using the conductive adhesive can be formed by forming a large number of electrodes on at least one surface of a substrate, applying the conductive adhesive of the present invention so that each electrode is at least covered to form an adhesive film, and then pressing the electrode parts of each electronic component against each electrode part and curing the adhesive layer.

[0069] The means for applying the conductive adhesive of the present invention to a substrate is not particularly limited. For example, the conductive resin composition may be applied to a substrate. In the present invention, the conductive adhesive may be applied by printing, discharging, or the like. The printing method is preferably at least one selected from the group consisting of screen printing, metal mask printing, inkjet printing, flexographic printing, gravure printing, dispenser method, and the like, and is preferably at least one selected from the group consisting of screen printing, inkjet printing, and the like, because of its excellent printability and shape retention. Here, the mesh used in the screen printing can be appropriately selected, and it is preferable to employ a mesh that does not remove excessive amounts of the conductive powder from the conductive adhesive. The thickness of the adhesive film formed by applying the conductive adhesive can be appropriately adjusted depending on the application, and is, for example, 1 μm or more, preferably 2 μm or more, more preferably 5 μm or more, and 200 μm or less.

[0070] The conductive adhesive of the present invention may be formed into a film for use. The film-like conductive adhesive can be obtained, for example, by adding a solvent or the like to a conductive adhesive composition as necessary, coating the conductive adhesive solution on a peelable support, and removing the solvent or the like. The film-like conductive adhesive is more convenient in terms of handling, etc. One or more layers of the film-like conductive adhesive can also be used as a multilayer structure together with one or more insulating adhesive layers, one or more peelable material layers, etc., as necessary. The conductive adhesive of the present invention can usually be used to bond adherends together by applying heat and pressure in combination. The heating temperature is not particularly limited as long as it is within a range that does not damage the adherends, and is, for example, 70°C or higher and 250°C or lower. The pressure is not particularly limited as long as it is within a range that does not damage the adherends, and is, for example, 0.1 MPa or higher and 10 MPa or lower. Heating and pressure are preferably performed for, for example, 0.5 seconds or higher and 120 seconds or lower.

[0071] The conductive adhesive of the present invention is used to electrically bond adherends to each other. For example, it can be used as an adhesive for heterogeneous adherends to bond and electrically connect adherends made of different materials and having different thermal expansion coefficients to each other. Furthermore, the conductive adhesive of the present invention can be used as a circuit connection material such as anisotropic conductive adhesive, conductive paste, conductive adhesive film, underfill material, LOC tape, and other semiconductor element adhesive materials.

[0072] [Circuit connecting materials] The circuit connecting material of the present invention contains the conductive resin composition and is used for conductive connections between various electronic components and circuit boards and for connections (bonding) between electric and electronic circuits. The shape of the circuit connecting material is not particularly limited, but it is preferably in the form of a liquid or film. The liquid circuit connecting material can be obtained, for example, by mixing the conductive resin composition of the present invention with a solvent such as an organic solvent to liquefy it. A film-like circuit connecting material can be obtained, for example, by directly casting and applying the liquefied conductive resin composition of the present invention onto a release substrate to form a film, drying the composition to remove the solvent, forming a film, and then peeling the film off from the release substrate. Furthermore, a film-like circuit connecting material can be obtained, for example, by impregnating a nonwoven fabric or the like with the liquefied conductive resin composition of the present invention, forming the same on a release substrate, drying to remove the solvent, and then peeling the same off from the release substrate.

[0073] The electrical connection method using the circuit connection material is not particularly limited. For example, a circuit connection material is provided between an electrode of an electronic component or circuit and an electrode on a substrate facing the electrode, and heated to electrically connect and bond the electrodes. When heating, pressure can be applied as necessary. The method for providing the circuit connecting material between the opposing electrodes is not particularly limited, and examples thereof include a method of applying a liquid circuit connecting material and a method of sandwiching a film-like circuit connecting material. In addition, when electrically connecting a pin of an electronic component or the like to a circuit, a method of providing a circuit connection material at the base of the pin and butt-jointing the pin to form an electrically conductive connection can be used.

[0074] The circuit connecting material can be used substantially as an anisotropic conductive material, and can also be used in an electrode connecting method in which a circuit connecting material with excellent adhesiveness is formed between electrodes facing each other on a substrate, and the electrodes are brought into contact with each other and the substrates are bonded together by heating and pressurization. As the substrate for forming the electrodes, inorganic materials such as semiconductors, glass, and ceramics, organic materials such as polyimide resins and polycarbonate resins, and composite combinations of these materials such as glass / epoxy can be used. When the circuit connecting material contains solder powder that melts at a low temperature as a component, conductive connection can be achieved at a low temperature of 250° C. or less, for example, 200° C. or less. EXAMPLES

[0075] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to these examples. Unless otherwise specified, "parts" means "parts by mass".

[0076] [Ingredients used] The components used in the examples are as follows. ·Tin powder 1: Spherical tin powder (D50=5.5μm, Sn≧99.5% by mass) Epoxy resin 1: Solid bisphenol A type epoxy resin (Nippon Steel Chemical & Material Co., Ltd. "YD-014"; epoxy equivalent 900-1000g / eq; softening point 100℃) Epoxy resin 2: Solid bisphenol A type epoxy resin ("YD-011" manufactured by Nippon Steel Chemical & Material Co., Ltd.; epoxy equivalent: 440-510g / eq; softening point: 66°C) Epoxy resin 3: Solid bisphenol A type epoxy resin ("YD-019" manufactured by Nippon Steel Chemical & Material Co., Ltd.; epoxy equivalent: 2200-2900g / eq; softening point: 138°C) Epoxy resin 4: Solid epoxy resin ("LCE-2615" manufactured by Nippon Kayaku Co., Ltd.; epoxy equivalent 494g / eq; softening point 93°C) Epoxy resin 5: Solid bisphenol F type epoxy resin ("YDF-2004" manufactured by Nippon Steel Chemical & Material Co., Ltd.; epoxy equivalent 850-1050g / eq; softening point 85°C) Epoxy resin 6: Solid bisphenol F type epoxy resin ("jER-4005P" manufactured by Mitsubishi Chemical Corporation; epoxy equivalent: 950-1200g / eq; softening point: 87°C) Epoxy resin 7: Semi-solid rubber-modified epoxy resin (DIC "TSR-601"; epoxy equivalent 450-500g / eq) Epoxy resin 8: Solid dicyclopentadiene type epoxy resin (DIC "HP-7200"; epoxy equivalent 254-264g / eq; softening point 57-68°C) Epoxy resin 9: Solid phenol novolac type epoxy resin (DIC Corporation "N-770"; epoxy equivalent 183-193g / eq; softening point 65-75°C) Epoxy resin 10: Solid biphenyl aralkyl type epoxy resin ("NC-3000" manufactured by Nippon Kayaku Co., Ltd.; epoxy equivalent 276g / eq; softening point 57°C) Epoxy resin 11: Solid naphthol-cresol novolac type epoxy resin ("NC-7000L" manufactured by Nippon Kayaku Co., Ltd.; epoxy equivalent 232g / eq; softening point 90°C) Epoxy resin 12: Liquid bisphenol A type epoxy resin (ADEKA "EP-4100G"; epoxy equivalent 190g / eq; softening point less than 25°C) Epoxy resin 13: Liquid propylene oxide-added bisphenol A type epoxy resin (ADEKA "EP-4000S"; epoxy equivalent 260g / eq; softening point less than 25°C) Epoxy resin 14: Liquid phenol novolac type epoxy resin (Nippon Kayaku Co., Ltd. "RE-305S"; epoxy equivalent 173g / eq; softening point less than 25°C) · Linear dicarboxylic acid compound 1: Adipic acid (HOOC-(CH2)4-COOH) · Linear dicarboxylic acid compound 2: Pimelic acid (HOOC-(CH2)5-COOH) · Linear dicarboxylic acid compound 3: Sebacic acid (HOOC-(CH2)8-COOH) · Linear dicarboxylic acid compound 4: Succinic acid (HOOC-(CH2)2-COOH) Linear dicarboxylic acid compound 5: Glutaric acid (HOOC-(CH2)3-COOH) Linear dicarboxylic acid compound 6: Diglycolic acid (HOOC-CH2-O-CH2-COOH) Branched dicarboxylic acid compound 1: Long-chain branched dibasic acid ("MMA-10R" manufactured by Okamura Oil Mills) Branched dicarboxylic acid compound 2: Long-chain branched dibasic acid ("SB-12" manufactured by Okamura Oil Mills) Thiol Compound 1: Thiocyanuric Acid (1,3,5-Triazine-2,4,6-Trithiol) Solvent 1: Diethylene glycol monobutyl ether (butyl carbitol) Solvent 2: Diethylene glycol dibutyl ether (dibutyl carbitol)

[0077] <Conductivity evaluation> For the conductive film (dried coating film) formed from the conductive resin composition, the volume resistivity was determined by the following method, and the conductivity was evaluated by the following method.

[0078] (Preparation of conductive film (dried coating film) for measurement) Using a metal mask with a pattern of 2 cm x 2 cm and a thickness of 100 microns, the conductive resin composition was hand-printed to produce a 2 cm x 2 cm coating film on a 5 cm x 5 cm glass substrate. It was then heat-cured at 160°C for 60 minutes to produce a conductive film (dried coating film) for measuring volume resistivity.

[0079] (Volume resistivity) The volume resistivity of the obtained conductive film (dried coating film) was measured in two directions (a direction passing through the center of the coating film, parallel to the upper side of the coating film, and a direction perpendicular to the direction) by a four-terminal method using a resistivity meter "Loresta GP-MCP T610" (manufactured by Nitto Seiko Analytech Co., Ltd.), and the average volume resistivity was calculated. Furthermore, two conductive films (dried coating films) were prepared for each conductive resin composition, and the average volume resistivity of the two conductive films (dried coating films) was calculated and used as the volume resistivity. The calculated volume resistivities are also shown in Tables 1 to 6. In addition, when the volume resistivity was too high to measure (volume resistivity measurement impossible), it was indicated as "UM" in Tables 1 to 6, and when the coating performance of the conductive resin composition was low and it was impossible to apply it uniformly (bad coating), it was indicated as "UC" in Tables 1 to 6.

[0080] (Conductivity evaluation) The volume resistivity and were evaluated according to the following criteria. In this evaluation, A is pass and D is fail. A: Volume resistivity is 3.0×10 -4 Less than (Ω cm) D: Volume resistivity is 3.0×10 -4 (Ω·cm) or more, volume resistivity measurement impossible (UM) or coating failure (UC)

[0081] The viscosity measurement and storage stability evaluation of the conductive resin composition were carried out by the methods described below. <Viscosity measurement> The viscosity of the conductive resin composition was measured using a rheometer (Rheometer DHR-2 manufactured by TA Instruments). 20 mm cone plate, 25° C., shear rate 10 s -1 The measurement was started at this time, and the viscosity was recorded 180 seconds after the start of the measurement.

[0082] <Storage stability> The prepared conductive resin compositions were placed in a container and left to stand for 24 hours at room temperature (25°C) (room temperature (25°C) 24 hour storage) and for one week in a refrigerator (4°C) (refrigerated (4°C) 1 week storage), after which the storage stability of each conductive resin composition was evaluated according to the following evaluation items and criteria. Furthermore, based on each evaluation, an overall evaluation of the storage at room temperature (25°C) for 24 hours and the storage in a refrigerator (4°C) for one week was performed according to the following criteria. In this evaluation, A is pass and D is fail. The evaluation results are also shown in Tables 1 to 6. A: All four evaluations of solidification, skin formation, liquid separation and thickening rate were passed. D: There is one or more failures in the four evaluations of solidification, skinning, liquid separation and thickening rate.

[0083] (solidification) After storage under the specified conditions, each conductive resin composition was touched with a spatula. If the conductive resin composition could be scooped up with the spatula, it was deemed not solidified and given an A, and if it had no fluidity and could not be scooped up with the spatula, it was deemed solidified and given a D. In this evaluation, A is a pass and D is a fail. In addition, if the volume resistivity was "UC (poor application)", solidification was not checked and this is indicated by a diagonal line in the table.

[0084] (Leather) After storage under the specified conditions, the appearance of each conductive resin composition was checked, and if there was no skinning on the surface of the conductive resin composition, it was rated as A, and if there was skinning, it was rated as D. Here, "skinning" refers to a state in which a film is formed on the surface of the conductive resin composition that comes into contact with air. In this evaluation, A is a pass and D is a fail. Note that if the volume resistivity was "UC (poor application)" or if solidification was confirmed, skinning was not checked, and this is indicated by a diagonal line in the table.

[0085] (Liquid Separation) After storage under the specified conditions, the appearance of each conductive resin composition was checked, and if the liquid did not separate and float on the surface of the conductive resin composition, it was rated as A, and if the liquid separated and floated, it was rated as D. In this evaluation, A is a pass, and D is a fail. Note that if the volume resistivity was "UC (poor application)" or if solidification or skinning was confirmed, separation of the liquid was not checked, and this is indicated by a diagonal line in the table.

[0086] (viscosity) After storage under the specified conditions, the viscosity of each conductive resin composition was measured using a rheometer (Rheometer DHR-2 manufactured by TA Instruments). 20 mm cone plate, 25° C., shear rate 10 s -1 The measurement was started at 0°C, and the viscosity value was the viscosity 180 seconds after the start of the measurement. In addition, when the viscosity could not be measured (viscosity measurement impossible) due to the occurrence of solidification, skinning, or liquid separation after storage, this is indicated as "UM" in Tables 1 to 6. In addition, when the volume resistivity was "UC (poor application)", the viscosity was not measured, and this is indicated by a diagonal line in the table.

[0087] (Thickening rate) The viscosity of each conductive resin composition was measured after storage under the specified conditions, and the viscosity was measured immediately after preparation of the conductive resin composition to calculate the viscosity increase rate, and the composition was evaluated according to the following criteria: A and B are pass, and D is fail. Viscosity increase rate [%] = {(viscosity after storage under specified conditions / viscosity immediately after preparation) - 1} x 100 A: Viscosity increase rate is less than 50% B: Viscosity increase rate is 50% or more but less than 100% D: Viscosity increase rate is 100% or more or viscosity measurement is not possible

[0088] [Example 1] 15.00 parts of tin powder 1, 0.84 parts of epoxy resin 1, 0.40 parts of linear dicarboxylic acid compound 1, and 1.00 parts of solvent 1 were mixed and stirred using a centrifugal mixer (Thinky Corporation, "Thinker Mixer AR-100") to obtain a conductive resin composition. In the obtained conductive resin composition, the amount of tin powder in the amount of all components other than the solvent (in Example 1, the total amount of tin powder 1, epoxy resin 1, and linear dicarboxylic acid compound 1) (amount of tin powder in the total amount of non-solvent components) was 92.36 mass%. The viscosity of the obtained conductive resin composition was measured. A conductive film (dried coating film) was prepared from the obtained conductive resin composition, and the volume resistivity was measured and evaluated. The obtained conductive resin composition was evaluated for storage stability (storage at room temperature (25° C.) for 24 hours and storage in a refrigerator (4° C.) for 1 week). These results are also shown in Table 1.

[0089] [Examples 2 to 32, Comparative Examples 1 to 13] Conductive resin compositions were prepared in the same manner as in Example 1, except that the components and the contents (parts) of the conductive resin compositions were as shown in Tables 1 to 6, respectively. The viscosity of the obtained conductive resin composition was measured. A conductive film (dried coating film) was prepared from the obtained conductive resin composition, and the volume resistivity was measured and evaluated. The obtained conductive resin composition was evaluated for storage stability (storage at room temperature (25° C.) for 24 hours and storage in a refrigerator (4° C.) for 1 week). These results are shown in Tables 1 to 6.

[0090] [Table 1]

[0091] [Table 2]

[0092] [Table 3]

[0093] [Table 4]

[0094] [Table 5]

[0095] [Table 6]

[0096] The conductive films formed from the conductive resin compositions according to Examples 1 to 32 all had a volume resistivity of 3.0×10 -4 Less than Ω cm, in some cases 1.0×10 -4 The electrical conductivity was less than Ω·cm, which was equal to or greater than that of silver paste, and it had excellent electrical conductivity. This shows that a conductive resin composition was formed that was lower cost than silver paste and had high electrical conductivity equal to that of silver paste. Furthermore, the conductive resin compositions of Examples 1 to 32 did not solidify, skin on the surface, or separate from the liquid when stored at room temperature (25°C) for 24 hours or in a refrigerator (4°C) for 1 week, and the increase in viscosity was small before and after storage at room temperature for 24 hours and in a refrigerator for 1 week, demonstrating excellent storage stability.

Claims

1. (a) tin powder, (b) an epoxy resin, and (c) containing a dicarboxylic acid compound, The (b) epoxy resin includes an epoxy resin having an epoxy equivalent of 400 g / eq or more and being solid or semi-solid at 25° C., The (c) dicarboxylic acid compound includes a dicarboxylic acid compound having 4 to 9 carbon atoms. Conductive resin composition.

2. 2. The conductive resin composition according to claim 1, wherein the content of the tin powder (a) is 92.01% by mass or more and 99.50% by mass or less, based on 100% by mass of the total amount of components other than the solvent in the conductive resin composition.

3. The conductive resin composition according to claim 1 , wherein the dicarboxylic acid compound (c) further comprises a dicarboxylic acid compound having 10 or more carbon atoms.

4. The conductive resin composition according to claim 1 or 2, further comprising (d) a thiol compound.

5. A conductive resin composition according to claim 1 or 2, which has a volume resistivity of 4.0×10 -4 A conductive film having a resistivity of less than Ω·cm.

6. A conductive material comprising the conductive resin composition according to claim 1 or 2.

7. A conductive adhesive comprising the conductive resin composition according to claim 1 or 2.

8. A circuit connecting material comprising the conductive resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Interactive processing system

    JP1989028716A

  • Conductive adhesive and bonding method using same

    JP2000309773A

  • Conductive paste composition

    JP2020205245A

  • Electroconductive resin composition

    JP2022172874A

  • Electrically conductive adhesive agent, joined body, and joint

    WO2015019666A1

Cited By

  • Conductive resin composition

    JP2026148453A