Photosensitive resin composition

The photosensitive resin composition addresses low heat and chemical resistance issues in polyimide films by increasing crosslink density and immobilizing low-boiling compounds, resulting in a resin film with improved glass transition temperature and chemical resistance.

JP2024157563AInactive Publication Date: 2024-11-07ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024117958
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional polyimide resins used in semiconductor devices face issues with low heat resistance and chemical resistance, leading to cracking and peeling during solder reflow processes due to temperature changes, and low-molecular compounds remaining in the cured film affect the physical properties, making it difficult to maintain resolution and chemical resistance.

Method used

A photosensitive resin composition containing a polyimide precursor, a compound with a hydroxyl group and polymerizable unsaturated bond, a photosensitizer, and controlled amounts of free chlorine, which increases crosslink density and immobilizes low-boiling compounds, enhancing glass transition temperature and thermogravimetric loss temperature while maintaining pattern resolution.

Benefits of technology

The composition produces a resin film with high glass transition temperature and chemical resistance, preventing cracking and peeling, and improves thermogravimetric loss temperature by immobilizing low-boiling compounds, thus maintaining pattern resolution and chemical resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157563000001
    Figure 2024157563000001
  • Figure 2024157563000002
    Figure 2024157563000002
  • Figure 2024157563000003
    Figure 2024157563000003
Patent Text Reader

Abstract

To provide a photosensitive resin composition that can produce a resin film having high Tg and thermal weight loss temperature, and excellent chemical resistance, while preventing a decrease in the resolution of a relief pattern.SOLUTION: A photosensitive resin composition contains (A) a polyimide precursor, (B) compound having a hydroxyl group and a polymerizable unsaturated bond, (C) a photosensitizer, (D) a solvent, (E) free chlorine, the amount of the free chlorine being 0.0001-2 ppm relative to the total mass of the photosensitive resin composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition. [Background technology]

[0002] Polyimide resins, which have excellent heat resistance, electrical properties, and mechanical properties, have been used as insulating materials for electronic components, and as passivation films, surface protective films, interlayer insulating films, etc. for semiconductor devices. Among these polyimide resins, those provided in the form of photosensitive polyimide precursors can easily form heat-resistant relief pattern coatings by applying the precursor, exposing it to light, developing it, and subjecting it to a thermal imidization treatment by curing.

[0003] Meanwhile, there are various methods for packaging semiconductor devices. In recent years, a semiconductor packaging method called fan-out has become mainstream as a semiconductor packaging method. In a fan-out type semiconductor package, a chip sealing body larger than the chip size of the semiconductor chip is formed by covering the semiconductor chip with an encapsulant. Furthermore, a redistribution layer is formed that extends to the area of ​​the semiconductor chip and the encapsulant. The redistribution layer is formed with a thin film thickness. Furthermore, since the redistribution layer can be formed up to the area of ​​the encapsulant, the number of external connection terminals can be increased.

[0004] For example, a fan-out type semiconductor device is known from Patent Document 1 below. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 5563814 Summary of the Invention [Problem to be solved by the invention]

[0006] On the other hand, in recent years, the method of mounting semiconductor devices on printed wiring boards has changed from the viewpoint of improving integration and computing functions, and miniaturizing chip size. In structures such as SiP, which allows higher density mounting, a structure in which a polyimide film directly contacts a solder bump has come to be used. When forming such a bump structure, the polyimide film is required to have high heat resistance and chemical resistance, and in the case of a resin composition that does not have heat resistance, a cured film with low heat resistance is produced when the resin composition is mounted on a substrate together with a semiconductor chip through a solder reflow process. A cured film with low heat resistance is prone to degassing and shrinkage due to temperature changes, and is prone to cracking and peeling.

[0007] Furthermore, in recent years, there has been an increasing demand for thermosetting materials (low-temperature curing materials) that can be cured at low temperatures. Although phenolic resins have been developed as low-temperature curing materials for insulating film applications, it is desirable to use polyimide resins from the viewpoint of chemical resistance and heat resistance. In order to cure polyimide resins, which are usually processed at 300 to 400°C, at low temperatures, it is common to use chemical imidization, in which a compound that promotes imidization is added, or to use soluble polyimides.

[0008] On the other hand, when heat treatment is performed at a low temperature, a large amount of low molecular weight compounds remain in the cured film and the interaction between the resins becomes weak, making it difficult to maintain the film properties. In particular, in a heating process such as solder reflow in the processing of semiconductor devices, cracks and peeling are likely to occur due to degassing and shrinkage.

[0009] In order to prevent the resin film from peeling off from the Cu wiring during the reflow process, it is necessary to increase the glass transition point (Tg) and weight loss temperature of the resin film. However, in recent low-temperature heat curing processes, the curing process is performed at a temperature below the reflow temperature, so that the Tg is lower than the reflow temperature, and there is a problem that the low-molecular-weight compound remains without volatilization. The Tg tends to increase by decreasing the molecular weight between crosslinking points of the cured film. However, when the functional group concentration or the amount of the radical polymerizable compound that is generally used in combination with a polyimide precursor in a negative photosensitive resin composition is increased, the resolution of the relief pattern decreases, so it is difficult to improve the Tg of the resin film while maintaining the resolution. In addition, in order to increase the thermal weight loss temperature of the resin film, it was necessary to completely volatilize or fix the low-molecular-weight compound in the resin film.

[0010] The present invention has been made in consideration of such problems, and an object of the present invention is to provide a photosensitive resin composition capable of producing a resin film having a high Tg and thermal weight loss temperature and excellent chemical resistance while suppressing a decrease in the resolution of a relief pattern. [Means for solving the problem]

[0011] The present inventors have found that the above problems can be solved by a resin composition containing a compound having a hydroxyl group and a polymerizable unsaturated bond, and a specific amount of free chlorine and / or covalently bonded chlorine, and have completed the present invention. Examples of embodiments of the present invention are listed below. [1] (A) a polyimide precursor; (B) a compound having a hydroxyl group and a polymerizable unsaturated bond, (C) a photosensitizer; (D) a solvent; (E) free chlorine; A photosensitive resin composition comprising: The amount of the free chlorine is 0.0001 to 2 ppm based on the total mass of the photosensitive resin composition. [2] 2. The photosensitive resin composition according to item 1, wherein the (C) photosensitizer is a photopolymerization initiator. [3] 3. The photosensitive resin composition according to item 1 or 2, wherein the polyimide precursor (A) is represented by the following general formula (1): [ka] {In formula (1), X 1 is a tetravalent organic group having 6 to 40 carbon atoms, and Y 1 is a divalent organic group having 6 to 40 carbon atoms, n1 is an integer of 2 to 150, and R 1 and R 2 are each independently a hydrogen atom or a monovalent organic group having 1 to 40 carbon atoms. 1 and R 2 At least one of the following general formula (2): [ka] In formula (2), R 3 , R 4 and R 5 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, and m1 is an integer of 2 to 10.} [4] 4. The photosensitive resin composition according to any one of items 1 to 3, comprising 100 to 860 parts by mass of the solvent (D) relative to 100 parts by mass of the polyimide precursor (A). [5] The photosensitive resin composition according to any one of items 1 to 4, wherein the (D) solvent comprises one or more compounds selected from the group consisting of N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, dimethylsulfoxide, diethylene glycol dimethyl ether, cyclopentanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, tetramethylurea, 1,3-dimethyl-2-imidazolinone, N-cyclohexyl-2-pyrrolidone, and 2-octanone. [6] 6. The photosensitive resin composition according to any one of items 1 to 5, wherein the compound (B) having a hydroxyl group and a polymerizable unsaturated bond has two or more polymerizable unsaturated bonds. [7] 6. The photosensitive resin composition according to any one of items 1 to 5, wherein the (B) compound having a hydroxyl group and a polymerizable unsaturated bond is a reaction product of an epoxy resin and (meth)acrylic acid. [8] 6. The photosensitive resin composition according to any one of items 1 to 5, wherein the compound (B) having a hydroxyl group and a polymerizable unsaturated bond is represented by the following general formula (3) or (4): [ka] {In formula (3), R 1 is a monovalent organic group having 1 to 40 carbon atoms.} [ka] {In formula (4), R 2 is a monovalent organic group having 1 to 40 carbon atoms.} [9] 6. The photosensitive resin composition according to any one of items 1 to 5, wherein the compound (B) having a hydroxyl group and a polymerizable unsaturated bond is represented by the following general formula (5) or (6): [ka] {In formula (5), R 3 is a monovalent organic group having 1 to 40 carbon atoms.} [ka] {In formula (6), R 4 is a monovalent organic group having 1 to 40 carbon atoms.}

[10] 6. The photosensitive resin composition according to any one of items 1 to 5, wherein the compound (B) having a hydroxyl group and a polymerizable unsaturated bond includes a compound represented by the following general formula (7): [ka] {In formula (7), R 2 is a divalent organic group having 1 to 40 carbon atoms.}

[11] 6. The photosensitive resin composition according to any one of items 1 to 5, wherein the compound (B) having a hydroxyl group and a polymerizable unsaturated bond includes a compound represented by the following general formula (8): [ka] {In formula (8), R 6 is a divalent organic group having 1 to 40 carbon atoms.}

[12] (A) a polyimide precursor; (B) a compound having a hydroxyl group and a polymerizable unsaturated bond, (C) a photosensitizer; (D) a solvent; (E) Free chlorine and A photosensitive resin composition comprising: The photosensitive resin composition is applied onto a substrate by a rotation method so as to give a film thickness after curing of about 10 μm, and cured by heating on a hot plate at 110° C. for 180 seconds, wherein the amount of the free chlorine contained in the resulting coating film is 0.0001 to 5 ppm based on the total mass of the coating film.

[13] 13. The photosensitive resin composition according to any one of items 1 to 12, further comprising (G) an epoxy resin.

[14] Item 14. The photosensitive resin composition according to item 13, wherein the amount of the (G) epoxy resin is 0.1 to 10 parts by mass per 100 parts by mass of the (A) polyimide precursor.

[15] 15. The photosensitive resin composition according to any one of items 1 to 14, which is a negative photosensitive resin composition.

[16] (A) a polyimide precursor; (B) a compound having a hydroxyl group and a plurality of polymerizable unsaturated bonds; (C) a photosensitizer; (D) a solvent; (E) free chlorine and / or covalently bound chlorine; A photosensitive resin composition comprising: A photosensitive resin composition, wherein the total amount of chlorine in the photosensitive resin composition when the photosensitive resin composition is allowed to stand for 3 days at 23°C±0.5°C and a relative humidity of 50%±10% after preparation is 0.0001 to 250 ppm based on the total mass of the photosensitive resin composition. Effect of the Invention

[0012] According to the present invention, a photosensitive resin composition can be provided that can produce a resin film having high glass transition temperature and thermal weight loss temperature and excellent chemical resistance while maintaining the resolution of the formed relief pattern. In one embodiment, the crosslink density of the polymer in the resin can be improved after the relief pattern is formed, and the glass transition temperature of the cured film tends to be high while maintaining the resolution. In one embodiment, the low boiling point compound in the film can be fixed by reaction, and the thermal weight loss temperature can be improved. Furthermore, in one embodiment, the high crosslink density and the specific amount of free chlorine prevent the intrusion of chemicals into the cured film, and therefore the chemical resistance of the relief pattern can be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the form for carrying out the present invention (hereinafter, abbreviated as "embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment, and can be carried out in various modifications within the scope of the gist. Throughout this specification, when a structure represented by the same symbol in a general formula is present in a molecule, it is independently selected and may be the same as or different from each other, unless otherwise specified. Furthermore, structures represented by a common symbol in different general formulas are also independently selected and may be the same as or different from each other, unless otherwise specified.

[0014] [Photosensitive resin composition] The photosensitive resin composition of the present embodiment includes (A) a polyimide precursor, (B) a compound having a hydroxyl group and a polymerizable unsaturated bond, (C) a photosensitizer, (D) a solvent, and (E) a specific amount of free chlorine and / or covalently bonded chlorine. If desired, the photosensitive resin composition includes other components. Each component will be described in turn below.

[0015] The photosensitive resin composition may be either a negative type or a positive type depending on the desired application, and is preferably a negative type from the viewpoint of the physical properties of the (A) polyimide precursor described below.

[0016] (A) Polyimide precursor In this embodiment, the (A) polyimide precursor is a resin component contained in the photosensitive resin composition, and is preferably a polyamide having a structural unit represented by the following general formula (1). [ka] {In formula (1), X 1 is a tetravalent organic group having 6 to 40 carbon atoms, and Y 1 is a divalent organic group having 6 to 40 carbon atoms, 1 is an integer from 2 to 150, and R 1 and R 2 are each independently a hydrogen atom or a monovalent organic group having 1 to 40 carbon atoms. 1 and R 2 At least one of the following general formula (2): [ka] In formula (2), R 3 , R 4 and R 5 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, and m 1 is an integer between 2 and 10.

[0017] (A) R of the precursor represented by the above general formula (1) contained in the polyimide precursor 1 and R 2The proportion of the monovalent organic group represented by the above general formula (2) to all of the above is preferably 50 mol % to 100 mol % from the viewpoint of high resolution, and more preferably 75 mol % to 100 mol % from the viewpoint of high chemical resistance and sensitivity.

[0018] In the above general formula (1), n1 is preferably an integer from 3 to 100, and more preferably an integer from 5 to 70, from the viewpoint of the photosensitive properties and mechanical properties of the photosensitive resin composition.

[0019] In the above general formula (1), X 1 The tetravalent organic group represented by the formula (I) is preferably an organic group having 6 to 40 carbon atoms, more preferably, -COOR 1 Group and -COOR 2 The X group and the -CONH- group are in the ortho position relative to each other, or the X group is an alicyclic aliphatic group. 1 Specific examples of the tetravalent organic group represented by the formula (20) include organic groups having 6 to 40 carbon atoms containing an aromatic ring, such as those represented by the formula (20): [ka] {In formula (20), R6 is a monovalent group selected from the group consisting of a hydrogen atom, a fluorine atom, a C1-C10 hydrocarbon group, and a C1-C10 fluorine-containing hydrocarbon group, l is an integer selected from 0 to 2, m is an integer selected from 0 to 3, and n is an integer selected from 0 to 4.} Examples of the group having a structure represented by the following formula (1) include, but are not limited to, X 1 The structure represented by the above formula (20) may be one type or a combination of two or more types. 1 The group is particularly preferred in that it has both heat resistance and photosensitive properties.

[0020] In the above general formula (1), Y 1 The divalent organic group represented by the formula (21) below is preferably an aromatic group having 6 to 40 carbon atoms in terms of achieving both heat resistance and photosensitive properties. [ka] {In formula (21), R6 is a monovalent group selected from the group consisting of a hydrogen atom, a fluorine atom, a C1 to C10 hydrocarbon group, and a C1 to C10 fluorine-containing hydrocarbon group, and n is an integer selected from 0 to 4.} Examples of the structure include, but are not limited to, those represented by the following formula: 1 The structure represented by the above formula (21) may be one type or a combination of two or more types. 1 The group is particularly preferred in that it has both heat resistance and photosensitive properties.

[0021] Y 1 As the group, among the structures represented by the above formula (21), the following formula: [ka] The structure represented by the following formula is preferable from the viewpoints of the imidization rate during low-temperature heating, degassing properties, copper adhesion, and chemical resistance.

[0022] R in the above general formula (2) 3 is preferably a hydrogen atom or a methyl group, and R 4 and R 5 From the viewpoint of photosensitive properties, it is preferable that m is a hydrogen atom. 1 is an integer of 2 or more and 10 or less, preferably an integer of 2 or more and 4 or less, from the viewpoint of photosensitive characteristics.

[0023] In one embodiment, the polyimide precursor (A) is represented by the following general formula (9): [ka] {In formula (9), R 1 , R 2 , and n 1 is defined above.} It is preferable that the polyimide precursor contains a polyimide precursor having a structural unit represented by the following formula:

[0024] In the general formula (9), R 1 and R 2At least one of them is more preferably a monovalent organic group represented by the above general formula (2).

[0025] In one embodiment, the polyimide precursor (A) is represented by the following general formula (10): [ka] {In formula (10), R 1 , R 2 , and n 1 is defined above.} It is preferable that the polyimide precursor contains a polyimide precursor having a structural unit represented by the following formula:

[0026] In the general formula (10), R 1 and R 2 At least one of them is more preferably a monovalent organic group represented by the above general formula (2).

[0027] (A) Method for preparing polyimide precursor The polyimide precursor having the structure represented by the above general formula (1) in this embodiment may be, for example, a tetravalent organic group X having 6 to 40 carbon atoms. 1 with (a) an alcohol having a structure in which a monovalent organic group represented by the above general formula (2) and a hydroxyl group are bonded, and, if desired, with (b) an alcohol having a structure other than the group represented by the above general formula (2) to prepare a partially esterified tetracarboxylic acid (hereinafter also referred to as an acid / ester body); and subsequently, reacting the obtained acid / ester body with the divalent organic group Y 1 and polycondensing the resulting product with a diamine comprising the above-mentioned formula (I).

[0028] (Preparation of Acid / Ester Forms) In this embodiment, a tetravalent organic group X having 6 to 40 carbon atoms 1Examples of tetracarboxylic dianhydrides containing the above include pyromellitic anhydride, diphenylether-3,3',4,4'-tetracarboxylic dianhydride, benzophenone-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, diphenylsulfone-3,3',4,4'-tetracarboxylic dianhydride, diphenylmethane-3,3',4,4'-tetracarboxylic dianhydride, 2,2-bis(3,4-phthalic anhydride)propane, 2,2-bis(3,4-phthalic anhydride)-1,1,1,3,3,3-hexafluoropropane, etc. These may be used alone or in combination of two or more.

[0029] (b) Examples of alcohols having a structure other than the group represented by general formula (2) above include aliphatic alcohols having 5 to 30 carbon atoms or aromatic alcohols having 6 to 30 carbon atoms, such as 1-pentanol, 2-pentanol, 3-pentanol, neopentyl alcohol, 1-heptanol, 2-heptanol, 3-heptanol, 1-octanol, 2-octanol, 3-octanol, 1-nonanol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol monomethyl ether, tetraethylene glycol monoethyl ether, and benzyl alcohol.

[0030] The content of the organic group of general formula (2) in the polyimide precursor is R 1 , R 2 , R 6 , and R 7 It is preferably 50 mol % or more with respect to the total content of the organic group of general formula (2). When the content of the organic group of general formula (2) exceeds 50 mol %, it is preferable since the desired photosensitive characteristics can be obtained. The content of the organic group of general formula (2) in the photosensitive resin composition is R 1 , R 2 , R 6 , and R 7 It is preferable that the total content of the above is 75 mol % or more.

[0031] The above tetracarboxylic dianhydride and the above (a) alcohol are dissolved and mixed in a reaction solvent in the presence of a basic catalyst such as pyridine, whereby a half-esterification reaction of the acid dianhydride proceeds to obtain the desired acid / ester. The reaction conditions are preferably a reaction temperature of 20 to 50°C and stirring for 4 to 10 hours.

[0032] The reaction solvent is preferably one that dissolves the acid / ester and the polyimide precursor, which is a polycondensation product of the acid / ester and diamine. Examples of the reaction solvent include N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethylsulfoxide, tetramethylurea, gamma butyrolactone, ketones, esters, lactones, ethers, halogenated hydrocarbons, hydrocarbons, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, methyl acetate, ethyl acetate, butyl acetate, diethyl oxalate, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, dichloromethane, 1,2-dichloroethane, 1,4-dichlorobutane, chlorobenzene, o-dichlorobenzene, hexane, heptane, benzene, toluene, and xylene. These may be used alone or in combination as needed.

[0033] (Preparation of polyimide precursor) The acid / ester compound (typically a solution in the reaction solvent) is mixed with a known dehydration condensation agent under ice cooling to convert the acid / ester compound into a polyacid anhydride, and then a divalent organic group Y having 6 to 40 carbon atoms is added to the polyacid anhydride. 1 A polyimide precursor can be obtained by adding dropwise a diamine containing the above dissolved or dispersed in a separate solvent and polycondensing it. Examples of dehydration condensation agents include dicyclohexylcarbodiimide, 1-ethoxycarbonyl-2-ethoxy-1,2-dihydroquinoline, 1,1-carbonyldioxy-di-1,2,3-benzotriazole, and N,N'-disuccinimidyl carbonate.

[0034] Divalent organic group Y having 6 to 40 carbon atoms 1Examples of diamines containing the above include p-phenylenediamine, m-phenylenediamine, 4,4-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3' -Diaminobiphenyl, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 4,4-bis(4- aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 9,10-bis(4-aminophenyl)anthracene, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2- Bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,4-bis(3-aminopropyldimethylsilyl)benzene, ortho-tolidine sulfone, 9,9-bis(4-aminophenyl)fluorene, and those in which some of the hydrogen atoms on the benzene ring are substituted with methyl groups, ethyl groups, hydroxymethyl groups, hydroxyethyl groups, halogens, etc., such as 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 2,Examples of the diamines include 2'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dimethytoxy-4,4'-diaminobiphenyl, 3,3'-dichloro-4,4'-diaminobiphenyl, and mixtures thereof. However, the diamines are not limited to these.

[0035] In order to improve adhesion between the photosensitive resin layer formed on a substrate by applying the photosensitive resin composition of the present embodiment onto the substrate and various substrates, diaminosiloxanes such as 1,3-bis(3-aminopropyl)tetramethyldisiloxane and 1,3-bis(3-aminopropyl)tetraphenyldisiloxane can also be copolymerized during preparation of the polyimide precursor (A).

[0036] After the polycondensation reaction is completed, the water-absorbing by-product of the dehydration condensation agent coexisting in the reaction solution may be filtered out as necessary, and then a poor solvent such as water, an aliphatic lower alcohol, or a mixture thereof may be added to the reaction solution to precipitate the polymer component. Furthermore, the polymer may be purified by repeating the above-mentioned redissolution and reprecipitation operations. The polymer may then be vacuum-dried to isolate the polyimide precursor. In order to improve the degree of purification, the polymer solution may be passed through a column packed with an anion and / or cation exchange resin swollen with a suitable organic solvent to remove ionic impurities.

[0037] The molecular weight of the polyimide precursor (A), as measured by gel permeation chromatography in terms of polystyrene equivalent weight average molecular weight, is preferably 8,000 to 150,000, more preferably 9,000 to 50,000, and particularly preferably 18,000 to 40,000. When the weight average molecular weight is 8,000 or more, it is preferable because the mechanical properties are good, while when it is 150,000 or less, it is preferable because the dispersibility in the developer and the resolution performance of the relief pattern are good. As the developing solvent for gel permeation chromatography, tetrahydrofuran and N-methyl-2-pyrrolidone are recommended. The molecular weight is determined from a calibration curve prepared using standard monodisperse polystyrene. As the standard monodisperse polystyrene, it is recommended to select from the organic solvent-based standard sample STANDARD SM-105 manufactured by Showa Denko KK.

[0038] (B) Compound having a hydroxyl group and a polymerizable unsaturated bond The compound (B) having a hydroxyl group and a polymerizable unsaturated bond (hereinafter, also simply referred to as "compound (B)") in this embodiment will be described. The compound (B) has at least one hydroxyl group and at least one polymerizable unsaturated bond in the molecule. The polymerizable unsaturated bond is not limited as long as it is a radically polymerizable functional group, and examples thereof include an acrylic group, a methacrylic group, an acryloyloxy group, a methacryloyloxy group, a vinyl group, and an allyl group, and an acryloyloxy group or a methacryloyloxy group (referred to as "(meth)acryloyloxy group" in this specification) is preferable. The compound (B) having a (meth)acryloyloxy group as a polymerizable unsaturated bond may be a reaction product of acrylic acid or a methacrylic group (referred to as "(meth)acrylic acid" in this specification) with an epoxy resin, or a reaction product of (meth)acrylic acid with a ring-opened epoxy resin. Among these, from the viewpoints of chemical resistance and thermal properties, reaction products of (meth)acrylic acid and epoxy resin, or reaction products of (meth)acrylic acid and ring-opened epoxy resin, represented by the following general formulas (3) to (6), are preferred. [ka] {In the above formulas (3) to (6), R 1 , R 2 , R 3 and R 4 is a monovalent organic group having 1 to 40 carbon atoms.}

[0039] The compound (B) may have one, two or more, or three or more polymerizable unsaturated bonds in the same molecule. When the compound (B) has two polymerizable unsaturated bonds, the compound (B) may have a polymerizable unsaturated bond represented by the following general formula: [ka] {In the above general formula, R 2 , R 3 is a divalent organic group having 1 to 40 carbon atoms.} Examples of the compound include compounds represented by the following formula:

[0040] More specifically, examples of the compound (B) having two polymerizable unsaturated bonds include, but are not limited to, the following compound groups: [ka] [ka] [ka] [ka]

[0041] The (B) compound having two or more polymerizable unsaturated bonds can be produced by reacting (meth)acrylic acid with a difunctional or higher epoxy resin. In this case, a compound having a monofunctional or higher oxacyclopropyl group in the molecule may be produced as a reaction impurity. Examples of the reaction impurity include compounds represented by the following general formula: [ka] {In the above formula, R 1 , R 2 , R 3and R 4 are each independently a divalent organic group having 1 to 40 carbon atoms. Among these, compounds represented by the following general formula: [ka] {In the above formula (8), R 6 is a divalent organic group having 1 to 40 carbon atoms.} is preferred.

[0042] When the (B) compound has one polymerizable unsaturated bond, examples of the compound include, but are not limited to, the following compounds: [ka]

[0043] (B) Method for preparing a compound having a hydroxyl group and a polymerizable unsaturated bond The method for producing the compound (B) is not particularly limited as long as a compound having at least one hydroxyl group and at least one polymerizable unsaturated bond in the molecule can be obtained. From the viewpoint of adjusting the amount of free chlorine and / or covalently bonded chlorine to a specific amount, the compound (B) is preferably a compound derived from an epoxy resin. For example, the compound (B) can be produced by reacting a compound having a polymerizable unsaturated bond with an epoxy resin or its ring-opening derivative. Preferably, the compound (B) may be produced by adding a basic catalyst and a polymerization inhibitor to an epoxy resin or its ring-opening derivative to obtain a mixed solution, adding methacrylic acid or acrylic acid to the solution, and reacting the solution. The reaction may be continued, for example, at 100° C. until the acid value becomes equal to or less than a certain value. After synthesis, the mixture is stirred in a mixed phase with an anion exchange resin for one day, and then filtered to obtain the compound (B). As the anion exchange resin, for example, IRA96SB can be used.

[0044] The epoxy resin used in the synthesis reaction of the compound (B) includes, but is not limited to, structures represented by the following general formula: [ka]

[0045] The ring-opened epoxy resin used in the synthesis reaction of the compound (B) is a ring-opened epoxy resin represented by the following general formula: [ka] {In the above formula, R 1 and R 2 are each independently a monovalent organic group having 1 to 40 carbon atoms.} It is preferable that the compound is a compound having a structure represented by the formula:

[0046] The photosensitive resin composition of the present embodiment contains the compound (B) and can provide a resin film having high glass transition temperature and thermal weight loss temperature while maintaining storage stability, and excellent chemical resistance. Without being bound by theory, the reason for the increase in glass transition temperature is believed to be that the polymerizable unsaturated bonds remaining after exposure without polymerization undergo an addition reaction with hydroxyl groups during high-temperature curing, resulting in a cured film that is crosslinked at a higher density than that of a normal polymerizable unsaturated bond-containing compound, and thus hindering the movement of the polymer that constitutes the resin. In addition, when the polymerizable unsaturated bond is a (meth)acrylic group, a Michael addition reaction proceeds. The reason for the improvement in chemical resistance is believed to be that the solubility in chemicals is reduced with a high crosslink density, and that the amount of free chlorine and / or covalently bonded chlorine is within a specific range, thereby suppressing the formation of ion pairs with a chemical solution that has a dissolution-promoting effect, thereby improving chemical resistance. The reason why the thermal weight loss temperature increases is thought to be that, in particular, a polymerizable unsaturated bond and a hydroxy group undergo an addition reaction with the side chain of the polyimide precursor, which is a factor in lowering the thermal weight loss temperature during low-temperature curing, and therefore, even when the temperature is raised above the curing temperature, the components derived from the side chain of the polyimide precursor do not volatilize but remain, preventing weight loss due to heating.

[0047] When a bifunctional or higher epoxy resin is used to synthesize the compound (B), the compound (B) may have unreacted epoxy groups. In this case, anionic polymerization proceeds with the hydroxyl groups as the initiating species during thermal curing, further increasing the crosslink density.

[0048] The blending amount of the (B) compound is 1 to 60 parts by mass relative to 100 parts by mass of the (A) polyimide precursor, preferably 1 to 30 parts by mass from the viewpoint of storage stability, and more preferably 4 to 20 parts by mass from the viewpoint of resolution.

[0049] (C) Photosensitizer The photosensitive resin composition of the present embodiment contains a photosensitizer. In one embodiment, the photosensitizer may be a photopolymerization initiator. The photopolymerization initiator is preferable because it promotes the curing of the relief pattern by light irradiation. The photopolymerization initiator is preferably a photoradical polymerization initiator, and examples of the photopolymerization initiator include benzophenone, o-benzoyl methyl benzoate, 4-benzoyl-4'-methyldiphenyl ketone, dibenzyl ketone, fluorenone and other benzophenone derivatives, 2,2'-diethoxyacetophenone, 2-hydroxy-2-methylpropiophenone, 1-hydroxycyclohexyl phenyl ketone and other acetophenone derivatives, thioxanthone, 2-methylthioxanthone, 2-isopropylthioxanthone, diethylthioxanthone and other thioxanthone derivatives, benzil, benzil dimethyl ketal, benzyl-β-methoxyethyl acetal and other benzyl derivatives, benzoin, benzoin methyl ether and other benzoin derivatives, 1-phenyl-1,2-butanedione-2-(o-methoxy)-2 ... Preferred examples of the photopolymerization initiator include, but are not limited to, oximes such as 1-phenyl-1,2-propanedione-2-(o-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-benzoyl)oxime, 1,3-diphenylpropanetrione-2-(o-ethoxycarbonyl)oxime, and 1-phenyl-3-ethoxypropanetrione-2-(o-benzoyl)oxime, N-arylglycines such as N-phenylglycine, peroxides such as benzoyl perchloride, aromatic biimidazoles, titanocenes, and photoacid generators such as α-(n-octanesulfonyloxyimino)-4-methoxybenzyl cyanide. Among the above photopolymerization initiators, oximes are more preferred, particularly in terms of photosensitivity.

[0050] The amount of the photopolymerization initiator is preferably 0.1 to 20 parts by mass, more preferably 1 to 8 parts by mass, based on 100 parts by mass of the polyimide precursor (A). The amount is preferably 0.1 parts by mass or more from the viewpoint of photosensitivity or patterning property, and is preferably 20 parts by mass or less from the viewpoint of the physical properties of the photosensitive resin layer after curing of the photosensitive resin composition.

[0051] (D) Solvent The photosensitive resin composition of the present embodiment contains a solvent. As the solvent, it is preferable to use a polar organic solvent from the viewpoint of solubility in the (A) polyimide precursor. Specific examples of the solvent include N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, dimethylsulfoxide, diethylene glycol dimethyl ether, cyclopentanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, tetramethylurea, 1,3-dimethyl-2-imidazolinone, N-cyclohexyl-2-pyrrolidone, and 2-octanone, which can be used alone or in combination of two or more.

[0052] The above-mentioned solvent can be used in an amount of, for example, 30 parts by mass to 1500 parts by mass, preferably 100 parts by mass to 1000 parts by mass, and more preferably 100 parts by mass to 860 parts by mass, relative to 100 parts by mass of the polyimide precursor (A), depending on the desired coating film thickness and viscosity of the photosensitive resin composition.

[0053] From the viewpoint of improving the storage stability of the photosensitive resin composition, a solvent containing alcohols is preferred. The alcohols that can be suitably used are typically alcohols that have an alcoholic hydroxyl group in the molecule and do not have an olefinic double bond, and specific examples thereof include alkyl alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, and tert-butyl alcohol; lactate esters such as ethyl lactate; propylene glycol monoalkyl ethers such as propylene glycol-1-methyl ether, propylene glycol-2-methyl ether, propylene glycol-1-ethyl ether, propylene glycol-2-ethyl ether, propylene glycol-1-(n-propyl) ether, and propylene glycol-2-(n-propyl) ether; monoalcohols such as ethylene glycol methyl ether, ethylene glycol ethyl ether, and ethylene glycol-n-propyl ether; 2-hydroxyisobutyric acid esters; and dialcohols such as ethylene glycol and propylene glycol. Of these, lactate esters, propylene glycol monoalkyl ethers, 2-hydroxyisobutyrate esters, and ethyl alcohol are preferred, and in particular, ethyl lactate, propylene glycol-1-methyl ether, propylene glycol-1-ethyl ether, and propylene glycol-1-(n-propyl) ether are more preferred.

[0054] When the solvent contains an alcohol having no olefinic double bond, the content of the alcohol having no olefinic double bond in the total solvent is preferably 5% by mass to 50% by mass, more preferably 10% by mass to 30% by mass, based on the mass of the total solvent. When the content of the alcohol having no olefinic double bond is 5% by mass or more, the storage stability of the photosensitive resin composition becomes good, while when it is 50% by mass or less, the solubility of the (A) polyimide precursor becomes good, which is preferable.

[0055] (E) Free chlorine and / or covalently bound chlorine The photosensitive resin composition of the present embodiment contains chlorine in the form of free chlorine and / or covalently bonded chlorine. The term "free chlorine" refers to anionized chlorine, and the term "covalently bonded chlorine" refers to chlorine that is present in a molecule by forming a covalent bond.

[0056] In one embodiment, the amount of free chlorine is 0.0001 to 10 ppm, preferably 0.0001 to 5 ppm, more preferably 0.0001 to 2.0 ppm, and even more preferably 0.0001 to 0.5 ppm based on the total mass of the photosensitive resin composition. In another embodiment, when the photosensitive resin composition is applied on a substrate by a rotation method so that the thickness of the cured resin film is about 10 μm, and the composition is cured by heating on a hot plate at 110° C. for 180 seconds, the amount of free chlorine contained in the resulting coating film is 0.0001 to 15 ppm, preferably 0.0001 to 10 ppm, more preferably 0.0001 to 5 ppm, and even more preferably 0.0001 to 0.8 ppm based on the total mass of the coating film. In still another embodiment, the total chlorine amount in the photosensitive resin composition (the total amount of free chlorine and covalently bonded chlorine) when the photosensitive resin composition is allowed to stand for 3 days at 23°C±0.5°C and a relative humidity of 50%±10% after preparation is 0.0001 to 600 ppm, preferably 0.0001 to 420 ppm, more preferably 0.0001 to 250 ppm, and even more preferably 0.0001 to 40 ppm based on the total mass of the photosensitive resin composition.

[0057] The source of chlorine is not limited, and for example, the photosensitive resin composition can adjust the amount of chlorine within the above range by including a compound capable of generating free chlorine and / or a compound having covalently bonded chlorine. Generally, epoxy resins contain a lot of chlorine in the form of free chlorine and / or covalently bonded chlorine in the resin, derived from epichlorohydrin, which is the raw material of the epoxy resin. Therefore, when the (B) compound is a compound derived from an epoxy resin, chlorine is included in the (B) compound, and as a result, chlorine is also included in the photosensitive resin composition, so it is easier to adjust the amount of chlorine within the above range. However, in the past, when the (B) compound derived from an epoxy resin was used in this way, the amount of chlorine was much greater than the above amount. Since the presence of such chlorine has been tolerated in the past, those skilled in the art have not paid attention to the amount of chlorine. However, the inventors have found that in a preferred embodiment of the present invention, when the (B) compound derived from an epoxy resin is used, it is preferable to remove the chlorine present in the compound and appropriately control the amount of chlorine.

[0058] The method for removing chlorine present in the (B) compound derived from the epoxy resin is not particularly limited. For example, chlorine can be removed by stirring the (B) compound in a mixed phase with an anion exchange resin. An anion exchange resin used for removing chlorine includes, but is not limited to, IRA96SB.

[0059] Other Ingredients The photosensitive resin composition of the present embodiment may further contain components other than the above components (A) to (E). Examples of the other components include (A) a resin component other than the polyimide precursor, a sensitizer, (F) a monomer having a photopolymerizable unsaturated bond other than the compound (B), a bonding aid, (G) an epoxy resin, a thermal polymerization inhibitor, an azole compound, a hindered phenol compound, and an organic titanium compound.

[0060] The photosensitive resin composition may further contain an epoxy resin (G) from the viewpoint of obtaining a cured film with a high degree of crosslinking. The amount of the epoxy resin (G) is preferably 0.01 to 25 parts by mass, more preferably 0.1 to 15 parts by mass, and even more preferably 0.1 to 10 parts by mass, based on 100 parts by mass of the polyimide precursor (A). When the compound (B) derived from an epoxy resin is used, the raw epoxy resin may be contained in the photosensitive resin composition, and it is easier to adjust the amount of the epoxy resin to the above range.

[0061] In one embodiment, the photosensitive resin composition may further contain a resin component other than the (A) polyimide precursor. Examples of the resin component that can be contained in the photosensitive resin composition include polyimide, polyoxazole, polyoxazole precursor, phenol resin, polyamide, epoxy resin, siloxane resin, and acrylic resin. The amount of these resin components is preferably in the range of 0.01 parts by mass to 20 parts by mass with respect to 100 parts by mass of the (A) polyimide precursor.

[0062] (A) When a positive-type photosensitive resin composition is prepared using a polyoxazole precursor together with a polyimide precursor, a compound having a quinone diazide group, such as a compound having a 1,2-benzoquinone diazide structure or a 1,2-naphthoquinone diazide structure, may be used in combination as a positive-type photosensitive material.

[0063] In one embodiment, the photosensitive resin composition may optionally contain a sensitizer to improve photosensitivity. Examples of the sensitizer include Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzal)cyclopentane, 2,6-bis(4'-diethylaminobenzal)cyclohexanone, 2,6-bis(4'-diethylaminobenzal)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, and p-dimethylaminocinnamylidene indane. Non, p-dimethylaminobenzylidene indanone, 2-(p-dimethylaminophenylbiphenylene)-benzothiazole, 2-(p-dimethylaminophenylvinylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)isonaphthothiazole, 1,3-bis(4'-dimethylaminobenzal)acetone, 1,3-bis(4'-diethylaminobenzal)acetone, 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3-acetone ethyl-7-dimethylaminocoumarin, 3-ethoxycarbonyl-7-dimethylaminocoumarin, 3-benzyloxycarbonyl-7-dimethylaminocoumarin, 3-methoxycarbonyl-7-diethylaminocoumarin, 3-ethoxycarbonyl-7-diethylaminocoumarin, N-phenyl-N'-ethylethanolamine, N-phenyldiethanolamine, Np-tolyldiethanolamine, N-phenylethanolamine, 4-morpholinobenzophenone, isoamyl dimethylaminobenzoate, isoamyl diethylaminobenzoate, 2-mercaptobenzimidazole, 1-phenyl-5-mercaptotetrazole, 2-mercaptobenzothiazole, 2-(p-dimethylaminostyryl)benzoxazole, 2-(p-dimethylaminostyryl)benzthiazole, 2-(p-dimethylaminostyryl)naphtho(1,2-d)thiazole, 2-(p-dimethylaminobenzoyl)styrene, and the like. These can be used alone or in combination of two or more (for example, two to five types).

[0064] The amount of the sensitizer to be added is preferably 0.1 to 25 parts by mass with respect to 100 parts by mass of the (A) polyimide precursor.

[0065] In one embodiment, in order to improve the resolution of the relief pattern, the photosensitive resin composition may optionally contain (F) a monomer other than the compound (B) having a photopolymerizable unsaturated bond. As such a monomer, a (meth)acrylic compound that undergoes a radical polymerization reaction with a photopolymerization initiator is preferable, and examples thereof include, but are not limited to, mono- or diacrylates and methacrylates of ethylene glycol or polyethylene glycol, including diethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate, mono- or diacrylates and methacrylates of propylene glycol or polypropylene glycol, mono-, di- or triacrylates and methacrylates of glycerol, cyclohexane diacrylate and dimethacrylate, diacrylates and dimethacrylates of 1,4-butanediol, and 1,6-hexaacrylate. Examples of suitable compounds include diacrylate and dimethacrylate of Sandiol, diacrylate and dimethacrylate of neopentyl glycol, mono- or diacrylate and methacrylate of bisphenol A, benzene trimethacrylate, isobornyl acrylate and methacrylate, acrylamide and its derivatives, methacrylamide and its derivatives, trimethylolpropane triacrylate and methacrylate, di- or triacrylate and methacrylate of glycerol, di-, tri-, or tetraacrylate and methacrylate of pentaerythritol, and ethylene oxide or propylene oxide adducts of these compounds.

[0066] The amount of the monomer having a photopolymerizable unsaturated bond blended is preferably 1 to 50 parts by mass with respect to 100 parts by mass of the (A) polyimide precursor.

[0067] In one embodiment, the photosensitive resin composition may optionally contain an adhesion promoter in order to improve the adhesion between the film formed using the photosensitive resin composition and the substrate. Examples of the adhesion promoter include γ-aminopropyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, 3-methacryloxypropyldimethoxymethylsilane, 3-methacryloxypropyltrimethoxysilane, dimethoxymethyl-3-piperidinopropylsilane, diethoxy-3-glycidoxypropylmethylsilane, N-(3-diethoxymethylsilylpropyl)succinimide, N-[3-(triethoxysilyl)propyl]phthala. Examples of the adhesive agent include silane coupling agents such as amido acid, benzophenone-3,3'-bis(N-[3-triethoxysilyl]propylamido)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-[3-triethoxysilyl]propylamido)-2,5-dicarboxylic acid, 3-(triethoxysilyl)propyl succinic anhydride, and N-phenylaminopropyltrimethoxysilane, and aluminum-based adhesion aids such as aluminum tris(ethylacetoacetate), aluminum tris(acetylacetonate), and ethylacetoacetate aluminum diisopropylate.

[0068] Among these adhesion aids, it is more preferable to use a silane coupling agent from the viewpoint of adhesive strength. The amount of the adhesion aid to be added is preferably within a range of 0.5 to 25 parts by mass with respect to 100 parts by mass of the (A) polyimide precursor.

[0069] In one embodiment, in order to improve the stability of the viscosity and photosensitivity of the photosensitive resin composition during storage, particularly in the form of a solution containing a solvent, the photosensitive resin composition may optionally contain a thermal polymerization inhibitor. Examples of the thermal polymerization inhibitor include hydroquinone, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt, and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt.

[0070] The amount of the thermal polymerization inhibitor to be added is preferably within a range of 0.005 parts by mass to 12 parts by mass per 100 parts by mass of the (A) polyimide precursor.

[0071] For example, when a substrate made of copper or a copper alloy is used, the photosensitive resin composition may optionally contain an azole compound in order to suppress discoloration of the substrate. Examples of the azole compound include 1H-triazole, 5-methyl-1H-triazole, 5-ethyl-1H-triazole, 4,5-dimethyl-1H-triazole, 5-phenyl-1H-triazole, 4-t-butyl-5-phenyl-1H-triazole, 5-hydroxyphenyl-1H-triazole, phenyltriazole, p-ethoxyphenyltriazole, 5-phenyl-1-(2-dimethylaminoethyl)triazole, 5-benzyl-1H-triazole, hydroxyphenyltriazole, 1,5-dimethyltriazole, 4,5-diethyl-1H-triazole, 1H-benzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-benzotriazole, and the like. benzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-benzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, hydroxyphenylbenzotriazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 4-carboxy-1H-benzotriazole, 5-carboxy-1H-benzotriazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, 1-methyl-1H-tetrazole, etc. Particularly preferred are tolyltriazole, 5-methyl-1H-benzotriazole, and 4-methyl-1H-benzotriazole. These azole compounds may be used alone or in combination of two or more.

[0072] The amount of the azole compound is preferably 0.1 to 20 parts by mass relative to 100 parts by mass of the polyimide precursor (A), and more preferably 0.5 to 5 parts by mass from the viewpoint of photosensitivity characteristics. When the amount of the azole compound is 0.1 part by mass or more relative to 100 parts by mass of the polyimide precursor (A), discoloration of the copper or copper alloy surface is suppressed when the photosensitive resin composition is formed on copper or a copper alloy, while when the amount is 20 parts by mass or less, photosensitivity is excellent, which is preferable.

[0073] In this embodiment, in order to suppress discoloration on copper, the photosensitive resin composition may contain a hindered phenol compound. Examples of the hindered phenol compound include 2,6-di-t-butyl-4-methylphenol, 2,5-di-t-butyl-hydroquinone, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-thio-bis(3-methyl-6-t-butylphenol), 4,4'-butylidene-bis(3-methyl-6-t-butyl phenol), triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylene bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylene bis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 2,2'-methylene-bis(4-methyl-6-t-butylfuran phenol), 2,2'-methylene-bis(4-ethyl-6-t-butylphenol), pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], tris-(3,5-di-t-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-isopropylbenzyl)-1,3,5-triazine-2, 4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-s-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-(1-ethylpropyl)-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-triethylmethyl-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-phenylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5,6-trimethylbenzyl)- 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3, 5-Tris(4-t-butyl-6-ethyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5,6-diethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine Examples of the triazine-2,4,6-(1H,3H,5H)-trione include 1,3,5-tris(4-t-butyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, and 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, but are not limited thereto. Among these, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione is particularly preferred.

[0074] The amount of the hindered phenol compound is preferably 0.1 to 20 parts by mass relative to 100 parts by mass of the polyimide precursor (A), and more preferably 0.5 to 10 parts by mass from the viewpoint of photosensitivity characteristics. When the amount of the hindered phenol compound is 0.1 part by mass or more relative to 100 parts by mass of the polyimide precursor (A), for example, when the photosensitive resin composition is formed on copper or a copper alloy, discoloration and corrosion of the copper or copper alloy are prevented, while when the amount is 20 parts by mass or less, photosensitivity is excellent, which is preferable.

[0075] In one embodiment, the photosensitive resin composition may contain an organotitanium compound. By containing an organotitanium compound, a photosensitive resin layer having excellent chemical resistance can be formed even when cured at a low temperature of about 250°C.

[0076] Examples of organotitanium compounds that can be used include those in which an organic chemical is bonded to a titanium atom via a covalent or ionic bond.

[0077] Specific examples of the organotitanium compound are shown below in I) to VII): I) As the titanium chelate compound, a titanium chelate having two or more alkoxy groups is more preferable because it provides the storage stability of the photosensitive resin composition and a good pattern. Specific examples of the titanium chelate compound include titanium bis(triethanolamine) diisopropoxide, titanium di(n-butoxide) bis(2,4-pentanedionate), titanium diisopropoxide bis(2,4-pentanedionate), titanium diisopropoxide bis(tetramethylheptanedionate), titanium diisopropoxide bis(ethylacetoacetate), etc.

[0078] II) Examples of tetraalkoxytitanium compounds include titanium tetra(n-butoxide), titanium tetraethoxide, titanium tetra(2-ethylhexoxide), titanium tetraisobutoxide, titanium tetraisopropoxide, titanium tetramethoxide, titanium tetramethoxypropoxide, titanium tetramethylphenoxide, titanium tetra(n-nonyloxide), titanium tetra(n-propoxide), titanium tetrastearyloxide, and titanium tetrakis[bis{2,2-(allyloxymethyl)butoxide}].

[0079] III) Titanocene compounds include, for example, pentamethylcyclopentadienyltitanium trimethoxide, bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluorophenyl)titanium, bis(η 5 -2,4-cyclopentadiene-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, and the like.

[0080] IV) Examples of monoalkoxytitanium compounds include titanium tris(dioctylphosphate) isopropoxide, titanium tris(dodecylbenzenesulfonate) isopropoxide, and the like.

[0081] V) Examples of titanium oxide compounds include titanium oxide bis(pentanedionate), titanium oxide bis(tetramethylheptanedionate), and phthalocyanine titanium oxide.

[0082] VI) Titanium tetraacetylacetonate compounds include, for example, titanium tetraacetylacetonate.

[0083] VII) Titanate coupling agents include, for example, isopropyl tridodecylbenzenesulfonyl titanate.

[0084] Among the above I) to VII), it is preferable that the organic titanium compound is at least one compound selected from the group consisting of the above I) titanium chelate compounds, II) tetraalkoxytitanium compounds, and III) titanocene compounds, from the viewpoint of exhibiting better chemical resistance. In particular, titanium diisopropoxide bis(ethylacetoacetate), titanium tetra(n-butoxide), and bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium is preferred.

[0085] When an organic titanium compound is blended, the blending amount is preferably 0.05 parts by mass to 10 parts by mass, more preferably 0.1 parts by mass to 2 parts by mass, relative to 100 parts by mass of the (A) resin. When the blending amount is 0.05 parts by mass or more, good heat resistance and chemical resistance are exhibited, while when the blending amount is 10 parts by mass or less, excellent storage stability is obtained, which is preferable.

[0086] A compound having a similar structure to the imidization accelerator (a compound exhibiting basicity) may be introduced into the polymer side chain. In this way, a higher imidization rate can be obtained than in the case where the imidization accelerator is used as an additive, and a photosensitive resin composition that has both storage stability and chemical resistance can be obtained.

[0087] The photosensitive resin composition preferably has a viscosity change rate of 5% or less compared to the initial viscosity when the resin composition is stored at a temperature of 23°C and a humidity of 50%Rh for 4 weeks. Furthermore, the photosensitive resin composition preferably has an imidization rate of 70% or more, and more preferably has an imidization rate of 85% or more, when the resin composition is heated at 170°C for 2 hours to obtain a cured coating film. Thus, in one embodiment, the photosensitive resin composition can provide a polyimide having a high imidization rate and excellent storage stability and chemical resistance.

[0088] [Polyimide] The structure of the polyimide contained in the cured relief pattern formed from the polyimide precursor composition is preferably represented by the following general formula (11). [ka] {In general formula (11), X 1 and Y 1 is X in general formula (1). 1 and Y 1 where m is a positive integer. Preferred X in formula (1) 1 and Y 1 For the same reason, is also preferred in the polyimide of general formula (11). The number m of repeating units in general formula (11) is not particularly limited, but may be an integer of 2 to 150. According to the present invention, there can also be provided a method for producing a polyimide, which includes a step of converting the above-described photosensitive resin composition into a polyimide.

[0089] [Hardened relief pattern] According to the present invention, it is possible to provide a cured relief pattern using the above-described photosensitive resin composition, and a method for producing the same. In one embodiment, the method for producing a cured relief pattern includes the following steps (1) to (4): (1) applying the photosensitive resin composition according to the present embodiment onto a substrate to form a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer to light; (3) developing the exposed photosensitive resin layer to form a relief pattern; and (4) heat treating the relief pattern to form a hardened relief pattern; The method includes:

[0090] Each step will be described below. (1) A step of applying the photosensitive resin composition of the present embodiment onto a substrate to form a photosensitive resin layer on the substrate. In this step, the photosensitive resin composition according to this embodiment is applied onto a substrate, and then dried as necessary to form a photosensitive resin layer. As the application method, a method that has been conventionally used for applying a photosensitive resin composition, such as a method of applying using a spin coater, a bar coater, a blade coater, a curtain coater, a screen printer, or the like, or a method of spray application using a spray coater, can be used.

[0091] If necessary, the coating film made of the photosensitive resin composition can be dried, and examples of the drying method include air drying, heat drying using an oven or a hot plate, and vacuum drying. It is preferable to dry the coating film under conditions that do not cause imidization of the (A) polyimide precursor in the photosensitive resin composition. Specifically, when air drying or heat drying is performed, drying can be performed under conditions of 20°C to 140°C for 1 minute to 1 hour. In this manner, a photosensitive resin layer can be formed on the substrate.

[0092] (2) A step of exposing the photosensitive resin layer to light In this process, the photosensitive resin layer formed in the above process (1) is exposed to an ultraviolet light source or the like through a patterned photomask or reticle or directly using an exposure device such as a contact aligner, mirror projection, or stepper.

[0093] Thereafter, post-exposure baking (PEB) and / or pre-development baking may be performed at any combination of temperature and time as necessary for the purpose of improving photosensitivity, etc. The range of baking conditions is preferably a temperature of 40° C. to 120° C. and a time of 10 seconds to 240 seconds, but is not limited to this range as long as it does not impair the various properties of the negative photosensitive resin composition.

[0094] (3) A step of developing the exposed photosensitive resin layer to form a relief pattern. In this step, when the photosensitive resin composition is a negative type, the unexposed portion of the photosensitive resin layer after exposure is developed and removed. As a development method for developing the photosensitive resin layer after exposure (irradiation), any method can be selected from conventionally known photoresist development methods, such as a rotary spray method, a paddle method, and a dipping method accompanied by ultrasonic treatment. In addition, after development, for the purpose of adjusting the shape of the relief pattern, etc., post-development baking may be performed at any combination of temperature and time as necessary. As the developer used for development, for example, a good solvent for the negative type photosensitive resin composition, or a combination of the good solvent and a poor solvent is preferable. As the good solvent, for example, N-methyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, etc. are preferable. As the poor solvent, for example, toluene, xylene, methanol, ethanol, isopropyl alcohol, ethyl lactate, propylene glycol methyl ether acetate, water, etc. are preferable. When a good solvent and a poor solvent are used in combination, it is preferable to adjust the ratio of the poor solvent to the good solvent according to the solubility of the polymer in the negative photosensitive resin composition. In addition, two or more kinds of each solvent, for example, several kinds, can be used in combination.

[0095] (4) heat treating the relief pattern to form a hardened relief pattern; In this step, the relief pattern obtained by the above development is heated to disperse the photosensitive component and imidize the polyimide precursor (A), thereby converting it into a cured relief pattern made of polyimide. As a method for heat curing, various methods can be selected, such as a method using a hot plate, an oven, or a method using a temperature-elevating oven that can set a temperature program. Heating can be performed, for example, under conditions of 170°C to 400°C for 30 minutes to 5 hours. As the atmospheric gas during heat curing, air may be used, or an inert gas such as nitrogen or argon may also be used.

[0096] [Semiconductor Devices] The photosensitive resin composition of the present embodiment can also provide a semiconductor device having a cured relief pattern obtained by the above-mentioned method for producing a cured relief pattern. Thus, a semiconductor device can be provided having a substrate that is a semiconductor element and a cured relief pattern of polyimide formed on the substrate by the above-mentioned method for producing a cured relief pattern. The present invention can also be applied to a method for producing a semiconductor device that uses a semiconductor element as the substrate and includes the above-mentioned method for producing a cured relief pattern as part of the process. The semiconductor device of the present invention can be produced by forming the cured relief pattern formed by the above-mentioned method for producing a cured relief pattern as a surface protective film, an interlayer insulating film, an insulating film for rewiring, a protective film for a flip chip device, or a protective film for a semiconductor device having a bump structure, and combining the method with a known method for producing a semiconductor device.

[0097] [Display device] The photosensitive resin composition of the present embodiment can also provide a display device comprising a display element and a cured film provided on the upper portion of the display element, the cured film being the above-mentioned cured relief pattern. Here, the cured relief pattern may be laminated in direct contact with the display element, or may be laminated with another layer sandwiched therebetween. For example, the cured film can be a surface protective film, an insulating film, and a planarizing film for a TFT liquid crystal display element and a color filter element, a protrusion for an MVA type liquid crystal display device, and a partition wall for a cathode of an organic EL element.

[0098] The photosensitive resin composition of the present invention is useful not only for application to the above-mentioned semiconductor devices, but also for applications such as interlayer insulation in multilayer circuits, cover coats for flexible copper-clad boards, solder resist films, and liquid crystal alignment films. EXAMPLES

[0099] The present embodiment will be described in detail below with reference to examples, but the present embodiment is not limited thereto. In the examples, comparative examples, and production examples, the physical properties of the photosensitive resin composition were measured and evaluated according to the following methods.

[0100] [Measurement and evaluation methods] (1) Weight average molecular weight The weight average molecular weight (Mw) of each resin was measured by gel permeation chromatography (standard polystyrene equivalent). The column used in the measurement was "Shodex 805M / 806M in series" manufactured by Showa Denko K.K., the standard monodisperse polystyrene was "Shodex STANDARD SM-105" manufactured by Showa Denko K.K., the developing solvent was N-methyl-2-pyrrolidone, and the detector was "Shodex RI-930" manufactured by Showa Denko K.K.

[0101] (2) Measurement of free chlorine content in resin composition After preparing the photosensitive resin composition, the composition was left to stand at room temperature (23.0°C ± 0.5°C, relative humidity 50% ± 10%) for 3 days, and then the amount of free chlorine in the resin composition was measured. The ion concentration was measured at 23.0°C using ThermoFicher ICS-3000. Based on the measurement results, the content of chlorine ions in the resin composition was calculated under the following measurement conditions. 2 g of the photosensitive resin composition was weighed out, added to 4 mL of NMP, and stirred for 10 minutes on a shaker to dissolve. 30 mL of ion-exchanged water was added, stirred for 10 minutes on a shaker, and the insoluble matter was removed using a centrifuge (CF15RN manufactured by Himac). The solution was filtered through a disk filter (JP050AN manufactured by DISMIC) and used. 1 mL of the treated sample solution was automatically inserted into the column by the autosampler. Guard column for anion analysis: IonPac AS4A-SC (4mm x 250mm) Guard column pump flow rate: 0.500mL / min - Separation column for anion analysis: IonPac AS4A-SZ (4mm x 50mm) Sample introduction line pump flow rate: 0.500mL / min Negative ion chemical suppressor: ACRS-500 (for 4mm)

[0102] (3) Measurement of free chlorine content in cured polyimide coatings The photosensitive resin composition was spin-coated on a 6-inch silicon wafer so that the film thickness after curing was about 10 μm, and heated on a hot plate at 110° C. for 180 seconds to obtain a cured polyimide coating film. The film thickness was measured using a film thickness measuring device, Lambda Ace (manufactured by Dainippon Screen Co., Ltd.). The amount of free chlorine in the obtained polyimide coating film was measured under the following measurement conditions. 2 g of polyimide coating was weighed, added to 4 mL of NMP, and stirred for 10 minutes on a shaker to dissolve. 30 mL of ion-exchanged water was added, stirred for 10 minutes on a shaker, and insoluble matter was removed using a centrifuge (CF15RN, manufactured by Himac). The solution was filtered through a disk filter (JP050AN, manufactured by DISMIC) and used. 1 mL of the treated sample solution was automatically inserted into the column by the autosampler. Guard column for anion analysis: IonPac AS4A-SC (4mm x 250mm) Guard column pump flow rate: 0.500mL / min - Separation column for anion analysis: IonPac AS4A-SZ (4mm x 50mm) Sample introduction line pump flow rate: 0.500mL / min Negative ion chemical suppressor: ACRS-500 (for 4mm)

[0103] (4) Measurement of glass transition temperature of cured polyimide coating The photosensitive resin composition was spin-coated on a 6-inch silicon wafer so that the film thickness after curing would be approximately 10 μm, and the wafer was pre-baked on a hot plate at 110° C. for 180 seconds. The wafer was then heated at 170° C. for 2 hours in a nitrogen atmosphere using a temperature-programmable cure oven (VF-000 model, manufactured by Koyo Lindberg Co., Ltd.) to obtain a cured polyimide coating film. The film thickness was measured using a film thickness measuring device, Lambda Ace (manufactured by Dainippon Screen Co., Ltd.). The resulting polyimide coating film was taken out in the form of a strip and measured under a load of 200 g / mm 2 The measurements were performed using a thermomechanical testing device (TMA-50, manufactured by Shimadzu Corporation) at a heating rate of 10°C / min in the range of 20 to 500°C. The glass transition temperature (Tg) was determined as the intersection of tangents to the thermal yield point of the polyimide film in the measurement chart, which has temperature on the horizontal axis and displacement on the vertical axis.

[0104] (5) Measurement of thermal weight loss temperature (5% weight loss temperature) of cured polyimide coating film A photosensitive resin composition was spin-coated on a 6-inch silicon wafer so that the film thickness after curing was about 10 μm, and the wafer was pre-baked on a hot plate at 110° C. for 180 seconds. The wafer was then heated at 170° C. for 2 hours in a nitrogen atmosphere using a temperature-programmable curing oven (VF-2000 model, manufactured by Koyo Lindberg Co., Ltd.) to obtain a cured polyimide coating film. The film thickness was measured using a film thickness measuring device, Lambda Ace (manufactured by Dainippon Screen Co., Ltd.). The obtained polyimide coating film was scraped off, and the temperature at which the weight of the film was reduced by 5% (5% weight reduction temperature) was measured using a thermogravimetric measuring device (manufactured by Shimadzu Corporation, TGA-50) when the temperature was raised from room temperature at 10° C. / min, with the weight of the film at 170° C. being taken as 100%.

[0105] (6) Chemical resistance test of hardened relief pattern on Cu A 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) was sputtered with 200 nm of Ti and 400 nm of Cu, in that order, using a sputtering device (L-440S-FHL model, manufactured by Canon Anelva Corporation). Next, a photosensitive resin composition prepared by the method described below was spin-coated on this wafer using a coater developer (D-Spin60A model, manufactured by SOKUDO Co., Ltd.), and dried to form a coating film with a thickness of 10 μm. A test pattern mask was used to apply 500 mJ / cm2 to this coating film using Prisma GHI (manufactured by Ultratech Co., Ltd.). 2 The coating was then spray-developed with a coater developer (D-Spin60A, manufactured by SOKUDO Co., Ltd.) using cyclopentanone as a developer, and rinsed with propylene glycol methyl ether acetate to obtain a relief pattern on Cu. The wafer with the relief pattern formed on Cu was heat-treated in a temperature-programmed curing furnace (VF-2000 type, manufactured by Koyo Lindberg) under a nitrogen atmosphere at 170°C for 2 hours to obtain a cured relief pattern made of resin approximately 6 to 7 μm thick on Cu. The prepared relief pattern was immersed in a resist peeling film (manufactured by ATMI, product name ST-44, main components are 2-(2-aminoethoxy)ethanol, 1-cyclohexyl-2-pyrrolidone) heated to 50°C for 5 minutes, washed with running water for 30 minutes, and air-dried. Thereafter, the film surface was visually observed with an optical microscope, and the chemical resistance was evaluated based on the presence or absence of damage caused by the chemical solution, such as cracks, and the rate of change in film thickness after chemical treatment. Chemical resistance was evaluated based on the following criteria. Film thickness change rate (%) = (film thickness after chemical treatment) - (film thickness before chemical treatment) / (film thickness before chemical treatment) × 100 "Excellent": The change in film thickness is less than 5% based on the film thickness before immersion in the chemical solution. "Good": The rate of change in film thickness is between 5% and 10% based on the film thickness before immersion in the chemical solution. "Acceptable": The rate of change in film thickness is between 10% and 15% based on the film thickness before immersion in the chemical solution. "Not acceptable": The change in film thickness is 15% or more based on the film thickness before immersion in the chemical solution.

[0106] (7) Resolution of hardened relief patterns on Cu A 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) was sputtered with 200 nm of Ti and 400 nm of Cu, in that order, using a sputtering device (L-440S-FHL model, manufactured by Canon Anelva Corporation). Next, a photosensitive resin composition prepared by the method described below was spin-coated on this wafer using a coater developer (D-Spin60A model, manufactured by SOKUDO Co., Ltd.), and dried to form a coating film with a thickness of 10 μm. A test pattern mask was used to apply 500 mJ / cm2 to this coating film using Prisma GHI (manufactured by Ultratech Co., Ltd.). 2 The coating was then spray-developed with a coater developer (D-Spin60A, manufactured by SOKUDO Co., Ltd.) using cyclopentanone as a developer, and rinsed with propylene glycol methyl ether acetate to obtain a relief pattern on Cu. The wafer with the relief pattern formed on Cu was heat-treated in a temperature-programmed curing furnace (VF-2000 type, manufactured by Koyo Lindberg) under a nitrogen atmosphere at 170°C for 2 hours to obtain a cured relief pattern made of resin approximately 6 to 7 μm thick on Cu. The relief pattern thus produced was observed under an optical microscope to determine the size of the minimum opening pattern. If the area of ​​the opening of the obtained pattern was at least half the area of ​​the corresponding pattern mask opening, it was deemed to be resolved, and the length of the mask opening side corresponding to the opening with the smallest area among the resolved openings was taken as the resolution. "Excellent": The minimum opening pattern size is less than 10 μm "Good": The minimum opening pattern size is 10 μm or more and less than 14 μm "Acceptable": The minimum opening pattern size is 14 μm or more and less than 18 μm "Not acceptable": The minimum opening pattern size is 18 μm or more.

[0107] (8) Measurement of total chlorine content in resin composition After preparing the photosensitive resin composition, it was left to stand for 3 days at room temperature (23.0°C ± 0.5°C, relative humidity 50% ± 10%), and then the total chlorine content of the resin composition (total amount of free chlorine and covalently bonded chlorine) was measured. The photosensitive resin composition was burned and decomposed at 800°C, and the decomposition gas was absorbed in ultrapure water, and the total chlorine content in the resin composition was determined by ion chromatography. The ion chromatography consisted of a Dionex IC-1000 and an IonPac AS12A (4 mm) column, and the eluent was 0.3 mM NaHCO 3 / 2.7mM Na 2 CO 3 The measurements were performed in aqueous solution at a flow rate of 1.5 mL / min.

[0108] [(A) Preparation of polyimide precursor] <Production Example 1> Synthesis of polyimide precursor A-1 155.1 g of 4,4'-oxydiphthalic dianhydride (ODPA) was placed in a 2 L separable flask, 131.2 g of 2-hydroxyethyl methacrylate (HEMA) and 400 mL of γ-butyrolactone were added and stirred at room temperature, and 81.5 g of pyridine was added while stirring to obtain a reaction mixture. After the heat generated by the reaction had ceased, the reaction mixture was allowed to cool to room temperature and left to stand for 16 hours. Next, under ice cooling, a solution of 206.3 g of dicyclohexylcarbodiimide (DCC) dissolved in 180 mL of γ-butyrolactone was added to the reaction mixture over 40 minutes while stirring, followed by the addition of 93.0 g of 4,4'-oxydianiline (ODA) suspended in 350 mL of γ-butyrolactone over 60 minutes while stirring. After further stirring at room temperature for 2 hours, 30 mL of ethyl alcohol was added and stirred for 1 hour, and then 400 mL of γ-butyrolactone was added. The precipitate formed in the reaction mixture was removed by filtration to obtain a reaction liquid. The reaction solution obtained was added to 3 L of ethyl alcohol to produce a precipitate consisting of a crude polymer. The produced crude polymer was filtered off and dissolved in 1.5 L of tetrahydrofuran to obtain a crude polymer solution. The obtained crude polymer solution was dropped into 28 L of water to precipitate the polymer, and the resulting precipitate was filtered off and then vacuum dried to obtain a powdered polymer (polymer A-1). The molecular weight of polymer (A-1) was measured by gel permeation chromatography (standard polystyrene equivalent) to find that the weight average molecular weight (Mw) was 20,000.

[0109] The weight average molecular weight of the resin obtained in each production example was measured by gel permeation chromatography (GPC) under the following conditions, and the weight average molecular weight was calculated in terms of standard polystyrene. Pump: JASCO PU-980 Detector: JASCO RI-930 Column oven: JASCO CO-965 40℃ Column: Shodex KD-806M, 2 in series Mobile phase: 0.1mol / L LiBr / NMP Flow rate: 1mL / min.

[0110] <Production Example 2> Synthesis of polyimide precursor A-2 Polymer (A-2) was obtained by carrying out a reaction in the same manner as in the above-mentioned Production Example 1, except that 147.1 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) was used instead of 155.1 g of 4,4'-oxydiphthalic dianhydride (ODPA) in Production Example 1. The molecular weight of polymer (A-2) was measured by gel permeation chromatography (standard polystyrene equivalent) and found to have a weight average molecular weight (Mw) of 26,000.

[0111] <Production Example 3> Synthesis of polyimide precursor A-3 Polymer (A-3) was obtained by carrying out a reaction in the same manner as in the above-mentioned Production Example 1, except that 48.7 g of p-phenylenediamine was used instead of 93.0 g of 4,4'-oxydianiline (ODA) in Production Example 1. The molecular weight of polymer (A-3) was measured by gel permeation chromatography (standard polystyrene equivalent) and found to have a weight average molecular weight (Mw) of 24,000.

[0112] <Production Example 4> Synthesis of polyimide precursor A-4 Polymer (A-4) was obtained by carrying out a reaction in the same manner as in the above-mentioned Production Example 1, except that 98.6 g of 4,4'-diamino-2,2'-dimethylbiphenyl was used instead of 93.0 g of 4,4'-oxydianiline (ODA) in Production Example 1. The molecular weight of polymer (A-4) was measured by gel permeation chromatography (standard polystyrene equivalent) and found to have a weight average molecular weight (Mw) of 26,000.

[0113] [(B) Preparation of Compound] <Production Example 5> Synthesis of epoxy (meth)acrylate compound B-1 34.0 g of bisphenol A diglycidyl ether was placed in a 1 L separable flask, 0.4 g of dimethylaniline, 0.04 g of p-methoxyphenol, and 15.5 g of methacrylic acid were added, and the mixture was reacted at 100 ° C. After confirming that the reaction had progressed by measuring the acid value, the mixture was mixed with 40.5 g of ion exchange resin IRA96SB, stirred overnight, and the ion exchange resin was filtered and removed. This process was repeated three times to obtain B-1, the main component of which was {[propane-2,2-diylbis(4,1-phenylene)]bis(oxy)}bis(2-hydroxypropane-3,1-diyl)=dimethacrylate.

[0114] <Production Example 6> Synthesis of epoxy (meth)acrylate compound B-2 Except for using 13.0 g of acrylic acid instead of 15.5 g of methacrylic acid, the reaction was carried out in the same manner as in the above-mentioned Production Example 5, to obtain B-2 containing {[propane-2,2-diylbis(4,1-phenylene)]bis(oxy)}bis(2-hydroxypropane-3,1-diyl)=diacrylate as the main component.

[0115] <Production Example 7> Synthesis of epoxy (meth)acrylate compound B-3 Except for using 17.42 g of ethylene glycol diglycidyl ether instead of 34.0 g of bisphenol A diglycidyl ether, the reaction was carried out in the same manner as described in the above Production Example 5, to obtain B-3 containing 1,2-bis(3-methacryloyloxy-2-hydroxypropyloxy)ethane as the main component.

[0116] <Production Example 8> Synthesis of epoxy (meth)acrylate compound B-4 Except for using 17.42 g of ethylene glycol diglycidyl ether instead of 34.0 g of bisphenol A diglycidyl ether and using 13.0 g of acrylic acid instead of 15.5 g of methacrylic acid, the reaction was carried out in the same manner as in the above-mentioned Production Example 5, to obtain B-4 containing 1,2-bis(3-acryloyloxy-2-hydroxypropoxy)ethane as a main component.

[0117] <Production Example 9> Synthesis of epoxy (meth)acrylate compound B-5 Except for using 23.23 g of glycerin diglycidyl ether instead of 34.0 g of bisphenol A diglycidyl ether, the reaction was carried out in the same manner as in the above-mentioned Production Example 5, to obtain B-5 containing glycerol 1,3-diglycerolate dimethacrylate as the main component.

[0118] <Production Example 10> Synthesis of epoxy (meth)acrylate compound B-6 Except for using 23.23 g of glycerin diglycidyl ether instead of 34.0 g of bisphenol A diglycidyl ether and using 13.0 g of acrylic acid instead of 15.5 g of methacrylic acid, the reaction was carried out in the same manner as in the above-mentioned Production Example 5, to obtain B-6 containing glycerol 1,3-diglycerolate diacrylate as the main component.

[0119] <Production Example 11> Synthesis of epoxy (meth)acrylate compound B-7 Except for using 31.24 g of bisphenol F type epoxy instead of 34.0 g of bisphenol A diglycidyl ether, the reaction was carried out in the same manner as described in the above-mentioned Production Example 5, to obtain B-7 containing bis[p-(3-methacryloxy-2-hydroxypropoxy)phenyl)]methane as the main component.

[0120] <Production Example 12> Synthesis of epoxy (meth)acrylate compound B-8 Except for using 15.02 g of glycidyl phenyl ether instead of 34.0 g of bisphenol A diglycidyl ether, the reaction was carried out in the same manner as in the above-mentioned Production Example 5, to obtain B-8 containing 2-hydroxy-3-phenoxypropyl methacrylate as the main component.

[0121] <Production Example 13> Synthesis of epoxy (meth)acrylate compound B-9 Except for using 15.02 g of glycidyl phenyl ether instead of 34.0 g of bisphenol A diglycidyl ether and using 13.0 g of acrylic acid instead of 15.5 g of methacrylic acid, the reaction was carried out in the same manner as in the above-mentioned Production Example 5, to obtain B-9 containing 2-hydroxy-3-phenoxypropyl acrylate as a main component.

[0122] <Production Example 14> Synthesis of epoxy (meth)acrylate compound B-10 Except for using 35.3 g of bisphenol A diglycidyl ether hydrogenated product instead of 34.0 g of bisphenol A diglycidyl ether, the reaction was carried out in the same manner as in the above-mentioned Production Example 5, to obtain B-10 containing 2,2-bis[4-(2-hydroxy-3-methacryloxy-1-propoxy)phenyl]propane as the main component.

[0123] <Production Example 15> Synthesis of epoxy (meth)acrylate compound B-11 Except for using 46.25 g of 9,9-bis[4-(2-glycidylethoxy)phenyl]fluorene instead of 34.0 g of bisphenol A diglycidyl ether, the reaction was carried out in the same manner as described in the above Production Example 5, to obtain B-11 containing 4,4'-(9-fluorenylidene)bis(2-hydroxy-3-phenoxypropyl methacrylate) as the main component.

[0124] <Production Example 16> Synthesis of epoxy (meth)acrylate compound B-12 Except for using 24.30 g of 1,6-bis(glycidyloxy)naphthalene instead of 34.0 g of bisphenol A diglycidyl ether, the reaction was carried out in the same manner as described in the above Production Example 5, to obtain B-12 containing 1,6-bis(3-methacryloyloxy-2-hydroxypropyloxy)naphthalene as the main component.

[0125] <Production Example 17> Synthesis of epoxy (meth)acrylate compound B-13 34.0 g of bisphenol A diglycidyl ether was placed in a 1 L separable flask, and 0.4 g of dimethylaniline, 0.04 g of p-methoxyphenol, and 17.4 g of methacrylic acid were added and reacted at 100 ° C. The progress of the reaction was confirmed by measuring the acid value, and B-13, mainly composed of {[propane-2,2-diylbis(4,1-phenylene)]bis(oxy)}bis(2-hydroxypropane-3,1-diyl)=dimethacrylate, was obtained without removing free chlorine with an ion exchange resin.

[0126] [Production of photosensitive resin composition] <Example 1> A negative photosensitive resin composition was prepared using polyimide precursor A-1 by the following method, and the prepared composition was evaluated. (A) 100 g of A-1 as a polyimide precursor, (B) 10 g of B-1 as an epoxy (meth)acrylate compound, (C) 5 g of 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)-oxime (hereinafter referred to as PDO) as a photopolymerization initiator, (F) 5 g of tetraethylene glycol dimethacrylate (hereinafter referred to as M4G) as a monomer, and (D) 100 g of γ-butyrolactone (hereinafter referred to as GBL) were dissolved. The viscosity of the obtained solution was adjusted to about 40 poise by further adding a small amount of GBL to obtain a negative photosensitive resin composition. From the above procedure, the amount of free chlorine and the amount of total chlorine in (E) the photosensitive resin composition, and the amount of free chlorine contained in the cured film were adjusted. The composition was evaluated according to the above method. The results are shown in Table 1.

[0127] <Examples 2 to 18 and Comparative Examples 1 to 4> A negative type photosensitive resin composition was prepared similarly to Example 1, except that it was prepared in the blending ratio shown in Table 1, and evaluations were carried out similarly to Example 1. The results are shown in Tables 1 and 2.

[0128] [Table 1]

[0129] [Table 2]

[0130] As is clear from Tables 1 and 2, the photosensitive resin composition of Example 1 had a glass transition temperature of 210° C., a 5% weight loss temperature of 300° C., a resolution of "excellent," and a chemical resistance test result of "excellent." Similarly, the photosensitive resin compositions of Examples 2 to 10 all had glass transition temperatures of 195° C. or higher, 5% weight loss temperatures of 290° C. or higher, a resolution result of "fair" or higher, and a chemical resistance test result of "fair" or higher.

[0131] In contrast, in Comparative Example 1, the resolution was "excellent", but the glass transition temperature was 170°C, and the 5% weight loss temperature was 260°C. As a result of the chemical resistance test, the film thickness change rate changed by 20% based on the film thickness before immersion, and the evaluation was "unacceptable". In Comparative Example 2, the glass transition temperature was 210°C, the 5% weight loss temperature was 300°C, and the resolution was "good", but the chemical resistance changed by 15%, and the evaluation was "unacceptable". In Comparative Example 3, the glass transition temperature was 200°C, and the 5% weight loss temperature was 300°C, but the resolution was "unacceptable". In Comparative Example 4, the chemical resistance was "unacceptable".

[0132] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the spirit of the invention. [Industrial Applicability]

[0133] By using the photosensitive resin composition according to the present invention, it is possible to improve the glass transition temperature and 5% weight loss temperature, and to improve chemical resistance, while maintaining high resolution in a cured film processed at low temperature. Therefore, the photosensitive resin composition according to the present invention can be suitably used in the field of photosensitive materials useful for producing electric and electronic materials such as semiconductor devices and multilayer wiring boards.

Claims

1. (A) a polyimide precursor; (B) a compound having a hydroxyl group and a polymerizable unsaturated bond; (C) a photosensitizer; and (D) a solvent; (E) free chlorine; A photosensitive resin composition comprising: The amount of the free chlorine is 0.0001 to 2 ppm based on the total mass of the photosensitive resin composition.

2. The photosensitive resin composition according to claim 1 , wherein the photosensitizer (C) is a photopolymerization initiator.

3. The photosensitive resin composition according to claim 1 or 2, wherein the polyimide precursor (A) is represented by the following general formula (1): 【Chemistry 1】 {In formula (1), X 1 is a tetravalent organic group having 6 to 40 carbon atoms; Y 1 is a divalent organic group having 6 to 40 carbon atoms, n 1 is an integer from 2 to 150; R 1 and R 2 are each independently a hydrogen atom or a monovalent organic group having 1 to 40 carbon atoms. 1 and R 2 At least one of the following general formula (2): 【Chemistry 2】 In formula (2), R 3 , R 4 and R 5 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, and m 1 is an integer from 2 to 10.

4. The photosensitive resin composition according to any one of claims 1 to 3, comprising 100 to 860 parts by mass of the solvent (D) relative to 100 parts by mass of the polyimide precursor (A).

5. The photosensitive resin composition according to any one of claims 1 to 4, wherein the solvent (D) comprises one or more compounds selected from the group consisting of N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, dimethylsulfoxide, diethylene glycol dimethyl ether, cyclopentanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, tetramethylurea, 1,3-dimethyl-2-imidazolinone, N-cyclohexyl-2-pyrrolidone, and 2-octanone.

6. The photosensitive resin composition according to any one of claims 1 to 5, wherein the compound (B) having a hydroxyl group and a polymerizable unsaturated bond has two or more polymerizable unsaturated bonds.

7. The photosensitive resin composition according to any one of claims 1 to 5, wherein the (B) compound having a hydroxyl group and a polymerizable unsaturated bond is a reaction product of an epoxy resin and (meth)acrylic acid.

8. The photosensitive resin composition according to any one of claims 1 to 5, wherein the compound (B) having a hydroxyl group and a polymerizable unsaturated bond is represented by the following general formula (3) or (4): 【Chemistry 3】 {In formula (3), R 1 is a monovalent organic group having 1 to 40 carbon atoms. 【Chemistry 4】 {In formula (4), R 2 is a monovalent organic group having 1 to 40 carbon atoms.

9. The photosensitive resin composition according to any one of claims 1 to 5, wherein the compound (B) having a hydroxyl group and a polymerizable unsaturated bond is represented by the following general formula (5) or (6): 【Chemistry 5】 {In formula (5), R 3 is a monovalent organic group having 1 to 40 carbon atoms. 【Chemistry 6】 {In formula (6), R 4 is a monovalent organic group having 1 to 40 carbon atoms.

10. The photosensitive resin composition according to any one of claims 1 to 5, wherein the compound (B) having a hydroxyl group and a polymerizable unsaturated bond includes a compound represented by the following general formula (7): 【Chemistry 7】 {In formula (7), R 2 is a divalent organic group having 1 to 40 carbon atoms.

11. The photosensitive resin composition according to any one of claims 1 to 5, wherein the compound (B) having a hydroxyl group and a polymerizable unsaturated bond includes a compound represented by the following general formula (8): 【Chemistry 8】 {In formula (8), R 6 is a divalent organic group having 1 to 40 carbon atoms.

12. (A) a polyimide precursor; (B) a compound having a hydroxyl group and a polymerizable unsaturated bond; (C) a photosensitizer; and (D) a solvent; (E) Free chlorine and A photosensitive resin composition comprising: The photosensitive resin composition is applied onto a substrate by a rotation method so that the film thickness after curing is about 10 μm, and when the composition is cured by heating on a hot plate at 110° C. for 180 seconds, the amount of free chlorine contained in the resulting coating film is 0.0001 to 5 ppm based on the total mass of the coating film.

13. The photosensitive resin composition according to any one of claims 1 to 12, further comprising (G) an epoxy resin.

14. The photosensitive resin composition according to claim 13, wherein the amount of the epoxy resin (G) is 0.1 to 10 parts by mass per 100 parts by mass of the polyimide precursor (A).

15. The photosensitive resin composition according to any one of claims 1 to 14, which is a negative type photosensitive resin composition.

16. (A) a polyimide precursor; (B) a compound having a hydroxyl group and a plurality of polymerizable unsaturated bonds; (C) a photosensitizer; and (D) a solvent; (E) free chlorine and / or covalently bound chlorine; A photosensitive resin composition comprising: A photosensitive resin composition, wherein after the photosensitive resin composition is prepared, the photosensitive resin composition is allowed to stand for 3 days at 23°C±0.5°C and a relative humidity of 50%±10%, and the total amount of chlorine in the photosensitive resin composition is 0.0001 to 250 ppm based on the total mass of the photosensitive resin composition.

Citation Information

Patent Citations

  • Tap switch for transformer

    JP1980063814A