Composition for thermoplastic material

A composition of rubber, polyamide, and a crosslinking agent with specific viscosity characteristics addresses the challenge of uniform crosslinking agent addition, resulting in improved thermoplastic materials with enhanced mechanical properties and oil resistance for automotive applications.

JP2024157582AInactive Publication Date: 2024-11-08OSAKA SODA CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023071980
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing thermoplastic elastomers with rubber elasticity face challenges in uniformly adding crosslinking agents, leading to inefficiencies in workability and the need for more efficient dispersibility and crosslinking agent compositions.

Method used

A composition for thermoplastic materials containing rubber, polyamide (PA), and a crosslinking agent composition with a shear viscosity of 0.1 to 10 Pa·s, which includes a crosslinking agent and plasticizer, is used to enhance dispersibility and workability, resulting in improved physical properties.

Benefits of technology

The composition achieves excellent dispersibility and workability, producing thermoplastic materials with enhanced mechanical properties and oil resistance, suitable for automotive parts such as fuel hoses and tubes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157582000001
    Figure 2024157582000001
  • Figure 2024157582000002
    Figure 2024157582000002
Patent Text Reader

Abstract

To provide a method more excellent in workability other than a method for directly adding a crosslinking agent in a powder state, since the crosslinking agent needs to be uniformly and quantitatively added, when rubber and resin are crosslinked while being kneaded by a twin screw extruder or the like.SOLUTION: A crosslinking agent composition is excellent in dispersibility and workability, and can obtain a thermoplastic material having good normal state physical property by setting shear viscosity of the crosslinking agent composition to be a constant range, though a crosslinking agent is dispersed in a plasticizer or the like and is added as a crosslinking agent composition, and thereby can be uniformly added.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for a thermoplastic material having excellent normal physical properties and oil resistance, a thermoplastic material obtained from the composition for a thermoplastic material, and a method for producing the same. [Background technology]

[0002] Epichlorohydrin rubber materials are widely used in automobiles as fuel hoses, air hoses, and tube materials, taking advantage of their heat resistance, oil resistance, low gas permeability, etc. Conventionally, epichlorohydrin rubber has been used as a crosslinked product through a vulcanization process from the viewpoint of heat resistance.

[0003] In recent years, thermoplastic elastomers with rubber elasticity have been widely used in the field of automobile parts as an alternative material to vulcanized rubber. There is an increasing demand for further weight reduction in automobile parts to improve fuel efficiency, and for materials that are recyclable and energy-saving in terms of the SDGs. If the vulcanized rubber hoses that have been used in automobiles so far could be replaced with thermoplastic elastomers that have excellent heat resistance, oil resistance, and gas permeability resistance, the demand for lightweight, recyclable, and energy-saving materials could be realized (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 11-172047 Summary of the Invention [Problem to be solved by the invention]

[0005] When crosslinking rubber and resin while kneading them in a twin-screw extruder, it is necessary to add the crosslinking agent uniformly and quantitatively. In this case, a method that is easier to work with than directly adding the powdered crosslinking agent is required. [Means for solving the problem]

[0006] The present inventors have found that, while it is possible to add a crosslinking agent uniformly by dispersing the crosslinking agent in a plasticizer or the like and adding it as a crosslinking agent composition, by setting the shear viscosity of the crosslinking agent composition within a certain range, not only can the dispersibility and workability of the crosslinking agent composition be excellent, but also the normal state physical properties of the obtained thermoplastic material can be improved.

[0007] That is, the present invention relates to the following. Item 1 (a) rubber, (b) polyamide (PA), and (c) a crosslinking agent composition are contained, and (c) the crosslinking agent composition is a crosslinking agent having a shear rate of 0.1 s at 30 ° C. -1 (a) has a shear viscosity η of 0.1 to 10 Pa s, and (c) contains 0.1 to 10 parts by mass of a crosslinking agent in a crosslinking agent composition relative to 100 parts by mass of rubber. Item 2. (b) The thermoplastic material composition according to Item 1, wherein 10 to 39 mass % of the polyamide (PA) is a polyamide elastomer. Item 3. (c) The composition for thermoplastic materials according to item 1, wherein the crosslinking agent in the crosslinking agent composition is at least one crosslinking agent selected from the group consisting of quinoxaline-based crosslinking agents, thiourea-based crosslinking agents, and triazine-based crosslinking agents. Item 4. The composition for thermoplastic materials according to item 1, wherein the (c) crosslinking agent composition contains a crosslinking agent and a plasticizer. Item 5. A thermoplastic material obtained from the composition for a thermoplastic material according to any one of items 1 to 4. Item 6. The thermoplastic material according to item 5, which is a thermoplastic elastomer. Item 7 (a) Rubber and (b) polyamide (PA) were mixed and then subjected to a shear rate of 0.1 s at 30°C. -1 A method for producing a thermoplastic material, comprising dynamically crosslinking a composition for a thermoplastic material obtained by adding a (c) crosslinker composition having a shear viscosity η of 0.1 to 10 Pa s per 100 parts by mass of the (a) rubber, so that the amount of the crosslinker in the (c) crosslinker composition is 0.1 to 10 parts by mass. Item 8 Shear rate 0.1 s at 30°C -1A crosslinking agent composition for thermoplastic materials, which has a shear viscosity η of 0.1 to 10 Pa s. Item 9. The crosslinker composition for thermoplastic materials according to item 8, comprising a crosslinker and a plasticizer. Effect of the Invention

[0008] The crosslinking agent composition for thermoplastic materials of the present invention has excellent dispersibility and workability, and the thermoplastic materials obtained from the composition for thermoplastic materials using the crosslinking agent composition have excellent normal physical properties, and are therefore useful as industrial products such as automobile parts, in particular fuel hoses, refrigerant hoses, and tube materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in detail below.

[0010] <1. Composition for thermoplastic materials> The composition for a thermoplastic material of the present invention contains at least (a) a rubber, (b) a polyamide (PA), and (c) a crosslinking agent composition.

[0011] The (a) rubber is not particularly limited as long as a thermoplastic material can be obtained using the (b) polyamide. Examples of the rubber include epichlorohydrin-based rubber, chloroprene rubber, halogen-containing rubber such as chlorinated butyl rubber and brominated butyl rubber, and acrylic rubber, with epichlorohydrin-based rubber and acrylic rubber being preferred.

[0012] The epichlorohydrin rubber is a polymer containing at least a structural unit derived from epichlorohydrin, and examples thereof include a homopolymer of epichlorohydrin, or a copolymer of epichlorohydrin and a compound selected from alkylene oxides such as ethylene oxide, propylene oxide, and n-butylene oxide, glycidyls such as methyl glycidyl ether, ethyl glycidyl ether, n-glycidyl ether, allyl glycidyl ether, and phenyl glycidyl ether, and styrene oxide.

[0013] Specific examples of epichlorohydrin rubber include epichlorohydrin homopolymer, epichlorohydrin-ethylene oxide copolymer, epichlorohydrin-propylene oxide copolymer, epichlorohydrin-ethylene oxide-allyl glycidyl ether terpolymer, epichlorohydrin-ethylene oxide-propylene oxide-allyl glycidyl ether terpolymer, etc., and epichlorohydrin homopolymer, epichlorohydrin-ethylene oxide copolymer, epichlorohydrin-ethylene oxide-allyl glycidyl ether terpolymer are preferred, and epichlorohydrin homopolymer and epichlorohydrin-ethylene oxide copolymer are particularly preferred. The molecular weight of these homopolymers or copolymers is not particularly limited, but is about ML1+4(100°C)=30-150 in Mooney viscosity measured according to JIS K6300-1.

[0014] In the epichlorohydrin rubber, the content of structural units derived from epichlorohydrin is preferably 10 to 100 mol %, more preferably 20 to 100 mol %, and particularly preferably 25 to 100 mol %, based on all structural units.

[0015] In the epichlorohydrin rubber, the content of constituent units derived from ethylene oxide is preferably 0 to 90 mol %, more preferably 0 to 80 mol %, and particularly preferably 0 to 75 mol %, based on all constituent units.

[0016] For epichlorohydrin rubber, the total of the constituent units derived from epichlorohydrin and the constituent units derived from ethylene oxide is preferably 80 mol% or more, more preferably 85 mol% or more, and particularly preferably 90 mol% or more, based on the total constituent units. The other constituent units than the constituent units derived from epichlorohydrin and the constituent units derived from ethylene oxide may be epihalohydrins other than epichlorohydrin, alkylene oxides other than ethylene oxide, glycidyls, styrene oxide, and other epichlorohydrin and ethylene oxide copolymerizable compounds.

[0017] In the case of an epichlorohydrin-ethylene oxide copolymer, the copolymerization ratio of the epichlorohydrin-derived structural unit is preferably 5 mol% to 95 mol%, more preferably 20 mol% to 75 mol%, and particularly preferably 25 to 65 mol%, and the ethylene oxide-derived structural unit is preferably 5 mol% to 95 mol%, more preferably 25 mol% to 80 mol%, and particularly preferably 35 mol% to 75 mol%.

[0018] In the case of epichlorohydrin-ethylene oxide-allyl glycidyl ether terpolymer, the copolymerization ratio of the epichlorohydrin-derived structural unit is preferably 5 mol% to 95 mol%, more preferably 20 mol% to 75 mol%, and particularly preferably 25 mol% to 65 mol%. The ethylene oxide-derived structural unit is preferably 4 mol% to 94 mol%, more preferably 24 mol% to 79 mol%, and particularly preferably 34 mol% to 74 mol%. The allyl glycidyl ether-derived structural unit is preferably 1 mol% to 10 mol%, more preferably 1 mol% to 8 mol%, and particularly preferably 1 mol% to 7 mol%.

[0019] The copolymer composition of epichlorohydrin-ethylene oxide copolymer and epichlorohydrin-ethylene oxide-allyl glycidyl ether terpolymer is determined by the chlorine content and iodine value. The chlorine content is measured by potentiometric titration in accordance with the method described in JIS K 7229. The mole fraction of the structural unit derived from epichlorohydrin is calculated from the obtained chlorine content. The iodine value is measured according to a method in accordance with JIS K 6235. The mole fraction of the constitutional unit derived from allyl glycidyl ether is calculated from the obtained iodine value. The molar fraction of constituent units derived from ethylene oxide is calculated from the molar fraction of constituent units derived from epichlorohydrin and the molar fraction of constituent units derived from allyl glycidyl ether.

[0020] The production of epichlorohydrin rubber can be carried out by a solution polymerization method, a slurry polymerization method, or the like, using a catalyst capable of ring-opening polymerization of an oxirane compound at a temperature range of -20 to 100°C. Examples of such catalysts include a catalyst system in which organoaluminum is the main component and water, a phosphorus oxo acid compound, acetylacetone, or the like is reacted therewith, a catalyst system in which organozinc is the main component and water is reacted therewith, and an organotin-phosphate ester condensate catalyst system. For example, the organotin-phosphate ester condensate catalyst system described in U.S. Pat. No. 3,773,694 by the present applicant can be used to produce epichlorohydrin rubber. When copolymerizing by such a method, it is preferable to copolymerize these components substantially randomly.

[0021] Examples of the acrylic rubber include those having a structural unit derived from an alkyl acrylate and / or a structural unit (a) derived from an alkoxyalkyl acrylate and a structural unit (b) derived from a crosslinkable monomer, and may further contain a structural unit (c) derived from an alkyl methacrylate.

[0022] The alkyl acrylate ester is preferably one in which the alkyl group has 1 to 8 carbon atoms, and more preferably one in which the alkyl group has 2 to 4 carbon atoms. The alkoxyalkyl acrylate ester is preferably one in which the alkoxyalkyl group has 2 to 8 carbon atoms, and more preferably one in which the alkoxyalkyl group has 2 to 4 carbon atoms. The alkyl acrylate ester and the alkoxyalkyl acrylate ester may be used alone or in combination of two or more kinds.

[0023] Specific examples of structural units derived from alkyl acrylates include structural units derived from acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, n-hexyl acrylate, n-heptyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, and cyclohexyl acrylate, and structural units derived from ethyl acrylate and n-butyl acrylate are preferred. Specific examples of structural units derived from alkoxyalkyl acrylates include structural units derived from acrylic esters such as methoxymethyl acrylate, methoxyethyl acrylate, ethoxymethyl acrylate, 2-ethoxyethyl acrylate, 2-propoxyethyl acrylate, 2-butoxyethyl acrylate, 2-methoxypropyl acrylate, 2-ethoxypropyl acrylate, 3-methoxypropyl acrylate, 3-ethoxypropyl acrylate, 4-methoxybutyl acrylate, and 4-ethoxybutyl acrylate, and a structural unit derived from methoxyethyl acrylate is preferable.

[0024] In the acrylic rubber of the present invention, the content of the structural unit derived from an alkyl acrylate and / or the structural unit (a) derived from an alkoxyalkyl acrylate is 45 to 99.5 mass%, preferably 50 to 99.5 mass%, and more preferably 60 to 99.5 mass%, or may be 45 to 89.5 mass%, 50 to 89.5 mass%, or 60 to 89.5 mass%, based on 100 mass% of the acrylic rubber. When two or more types of structural units (a) are contained, the content of the structural units (a) refers to the total content. The same applies to other descriptions.

[0025] The structural unit (b) derived from a crosslinkable monomer is not particularly limited as long as it is a structural unit derived from a crosslinkable monomer having a crosslinking group that can react with a crosslinking agent, and includes a structural unit derived from a crosslinkable monomer having any of a carboxy group, an epoxy group, and a halogen group, but is preferably a structural unit derived from a crosslinkable monomer having a carboxy group. The crosslinkable monomer having a crosslinking group that can react with a crosslinking agent may be used alone or in combination of two or more kinds.

[0026] Examples of the structural unit derived from a crosslinkable monomer having an epoxy group as a crosslinking group include structural units derived from an epoxy group-containing (meth)acrylic acid ester such as glycidyl (meth)acrylate, structural units derived from an epoxy group-containing styrene such as p-vinylbenzyl glycidyl ether, structural units derived from an epoxy group-containing ether such as allyl glycidyl ether and vinyl glycidyl ether, 3,4-epoxy-1-pentene, 3,4-epoxy-1-butene, 4,5-epoxy-2-pentene, 4-vinylcyclohexyl glycidyl ether, cyclohexenylmethyl glycidyl ether, 3,4-epoxy-1-vinylcyclohexene and allylphenyl glycidyl ether. These may be used alone or in combination of two or more.

[0027] Examples of constituent units derived from crosslinkable monomers having a halogen group as a crosslinking group include constituent units derived from 2-chloroethyl vinyl ether, 2-chloroethyl acrylate, vinylbenzyl chloride, vinyl monochloroacetate, allyl chloroacetate, etc. These can be used alone or in combination of two or more kinds.

[0028] Examples of the structural unit derived from a crosslinkable monomer having a carboxy group include structural units derived from an ethylenically unsaturated monocarboxylic acid such as (meth)acrylic acid, crotonic acid, 2-pentenoic acid, and cinnamic acid; structural units derived from an ethylenically unsaturated dicarboxylic acid such as fumaric acid, maleic acid, and itaconic acid; fumaric acid monoalkyl esters such as monomethyl fumarate, monoethyl fumarate, monopropyl fumarate, monobutyl fumarate, monohexyl fumarate, and monooctyl fumarate; maleic acid monoalkyl esters such as monomethyl maleate, monoethyl maleate, monopropyl maleate, monobutyl maleate, monopentyl maleate, and monodecyl maleate; and itaconic acid monoalkyl esters such as monomethyl itaconate, monoethyl itaconate, monopropyl itaconate, and monobutyl itaconate. These can be used alone or in combination of two or more. As the structural unit derived from a crosslinkable monomer having a carboxy group, an ethylenically unsaturated dicarboxylic acid monoester is preferable, a fumaric acid monoalkyl ester is more preferable, and a fumaric acid monoalkyl ester having an alkyl group with 1 to 4 carbon atoms is most preferable.

[0029] The content of the structural unit (b) derived from a crosslinkable monomer in the acrylic rubber of the present invention is 0.5 to 5.5 mass%, preferably 0.5 to 5 mass%, and more preferably 0.5 to 2 mass% in 100 mass% of the acrylic rubber. By having the structural unit (b) derived from a crosslinkable monomer (preferably a structural unit derived from a crosslinkable monomer having a carboxy group) in the above range, the effects of the present invention tend to be more favorably exhibited, and it is also preferable in terms of physical properties.

[0030] The structural unit (c) derived from an alkyl methacrylate ester is preferably a structural unit derived from an alkyl methacrylate ester having an alkyl group with 3 to 16 carbon atoms (preferably 4 to 16 carbon atoms). An alkyl methacrylate ester having an alkyl group with 3 to 16 carbon atoms (preferably 4 to 16 carbon atoms) means that the alkyl group of the alkyl methacrylate ester has 3 to 16 carbon atoms (preferably 4 to 16 carbon atoms). Examples of the structural unit (c) derived from an alkyl methacrylate include structural units derived from alkyl methacrylates such as n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, n-decyl methacrylate, isodecyl methacrylate, n-dodecyl methacrylate, n-lauryl methacrylate, and n-octadecyl methacrylate, and it is preferably a structural unit derived from an alkyl methacrylate selected from n-butyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, isodecyl methacrylate, and n-lauryl methacrylate. More preferably, the structural unit (c) is derived from an alkyl methacrylate ester having an alkyl group with 4 or more and 9 or less carbon atoms (more preferably 8 or less, even more preferably 7 or less, and particularly preferably 6 or less), and more preferably, for example, a structural unit derived from n-butyl methacrylate, n-hexyl methacrylate, or 2-ethylhexyl methacrylate. These may be structural units derived from a single alkyl methacrylate ester, or two or more kinds of alkyl methacrylate esters.

[0031] The content of the structural unit (c) derived from an alkyl methacrylate ester in the acrylic rubber of the present invention is 0 to 50 mass%, preferably 10 to 50 mass%, more preferably 10 to 40 mass%, and particularly preferably 10.5 to 30 mass%, based on 100 mass% of the acrylic rubber.

[0032] It is preferable that the ratio is based on 100% by mass of the entire acrylic rubber of the present invention, and the acrylic rubber may contain structural units other than the structural units (a), (b), and (c). However, in 100% by mass of the acrylic rubber, the total content of the structural units (a), (b), and (c) is, for example, 55.5% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, particularly preferably 90% by mass or more, may be 95% by mass or more, may be 98% by mass or more, or may be 100% by mass.

[0033] Furthermore, the acrylic rubber of the present invention may contain, in addition to the above-mentioned structural units (a) to (c), structural units derived from other monomers copolymerizable therewith. Examples of the other structural units include structural units derived from ethylenically unsaturated nitriles, structural units derived from (meth)acrylamide monomers, structural units derived from aromatic vinyl monomers, structural units derived from conjugated diene monomers, structural units derived from non-conjugated dienes, structural units derived from other olefins, etc. These may be used alone or in combination of two or more.

[0034] In the acrylic rubber of the present invention, the content of the structural units can be determined by the nuclear magnetic resonance spectrum of the obtained polymer.

[0035] The acrylic rubber used in the present invention can be obtained by polymerizing various monomers. The monomers used may be commercially available products and are not particularly limited.

[0036] As the form of the polymerization reaction, any of emulsion polymerization, suspension polymerization, bulk polymerization, and solution polymerization can be used. From the viewpoint of ease of control of the polymerization reaction, however, it is preferable to use emulsion polymerization under normal pressure, which is generally used as a conventional method for producing acrylic rubber.

[0037] (b) Polyamide (PA) is preferably a polyamide resin, and includes all thermoplastic polyamides having an amide bond in the main chain. Polyamides can be obtained by known methods such as polycondensation of a salt obtained by reaction of adipic acid, sebacic acid, dodecanedioic acid, etc. with ethylenediamine, hexamethylenediamine, metaxylenediamine, etc., polycondensation of a diamine derivative such as diformyl with a dibasic acid, self-condensation of amino acid or its derivative, ring-opening polymerization of lactam, etc., and polyamides may be copolymers or may be used in combination of two or more different polymers.

[0038] Polyamide resins include polycaprolactam (polyamide 6), polyundecane lactam (polyamide 11), polydodecane lactam (polyamide 12), polyethylene adipamide (polyamide 26), polytetramethylene adipamide (polyamide 46), polyhexamethylene adipamide (polyamide 66), polyhexamethylene azelamide (polyamide 69), polyhexamethylene sebacamide (polyamide 610), polyhexamethylene undecamide (polyamide 611), polyhexamethylene dodecamide (polyamide 612), polyhexamethylene terephthalamide (polyamide 6T), polyhexamethylene isophthalamide (polyamide 61), polymethacrylate (polyamide 62), polymethacrylate (polyamide 63), polymethacrylate (polyamide 64), polymethacrylate (polyamide 65), polymethacrylate (polyamide 66). Examples of polyamide resins include taxylylene adipamide (polyamide MXD6), polymetaxylylene suberamide (polyamide MXD8), polymetaxylylene azelamide (polyamide MXD9), polymetaxylylene sebacamide (polyamide MXD10), polymetaxylylene dodecamide (polyamide MXD12), polymetaxylylene terephthalamide (polyamide MXDT), polymetaxylylene isophthalamide (polyamide MXDI), and polymetaxylylene naphthalamide (polyamide MXDN). Of these, polycaprolactam (polyamide 6), polyundecane lactam (polyamide 11), and polydodecane lactam (polyamide 12) are preferred.

[0039] The polyamide resin has a melting point as measured by DSC of preferably 190° C. or less, more preferably 185° C. or less, and although there is no particular lower limit, it is preferably 165° C. or more, more preferably 170° C. or more. The melting point as measured by DSC can be determined using a differential scanning calorimeter (DSC-8000 manufactured by PerkinElmer) in accordance with JIS K7121-1987.

[0040] The weight average molecular weight of the polyamide resin is preferably 10,000 to 100,000, more preferably 12,000 to 70,000, and particularly preferably 15,000 to 50,000.

[0041] The (b) polyamide (PA) of the present invention may contain a polyamide elastomer in addition to the above-mentioned polyamide resin.

[0042] The polyamide elastomer of the present invention includes a thermoplastic elastomer consisting of a hard segment made of polyamide and a soft segment made of polyether. Examples of polyamides constituting the hard segment include nylon 6, nylon 66, nylon 11, and nylon 12, among which nylon 11 or nylon 12 is preferred. Examples of polyethers constituting the soft segment include polyethylene glycol, polypropylene glycol, and polytetramethylene glycol. Commercially available polyamide elastomers can be used. The number average molecular weight of the hard segment may be 300 to 15,000, the number average molecular weight of the soft segment may be 200 to 6,000, and the hard segment / soft segment (mass ratio) may be 95 / 5 to 25 / 75. Examples of commercially available polyamide elastomers include "UBESTA" (registered trademark) XPA manufactured by Ube Industries, Ltd., "Pebax" (registered trademark) 33 series, 53 series, MV series, MH series, HD series, MP series, and Rnew series manufactured by Arkema Co., Ltd., and "Vestamid" manufactured by Polypla-Evonik Co., Ltd. The melting point of the polyamide elastomer is preferably 130°C or more and 170°C or less in terms of heat resistance and flexibility. When the (b) polyamide (PA) contains a polyamide elastomer, the content ratio of the polyamide resin is preferably 61% by mass to 90% by mass, more preferably 64% by mass to 85% by mass, and particularly preferably 64% by mass to 82% by mass, and the content ratio of the polyamide elastomer is preferably 10% by mass to 39% by mass, more preferably 15% by mass to 36% by mass, and particularly preferably 18% by mass to 36% by mass. The content ratio of the polyamide elastomer in the range of 10% by mass to 39% by mass is preferable in terms of flexibility, heat resistance, and mechanical properties.

[0043] The amount of (b) polyamide (PA) added is preferably 15 to 100 parts by mass, more preferably 20 to 80 parts by mass, and particularly preferably 25 to 75 parts by mass, per 100 parts by mass of (a) rubber.

[0044] The (c) crosslinking agent composition of the present invention has a shear rate of 0.1 s at 30° C. -1 The shear viscosity η in is preferably from 0.1 to 10 Pa·s, more preferably from 0.2 to 5 Pa·s, further preferably from 0.3 to 3 Pa·s, and particularly preferably from 0.3 to 1.5 Pa·s. The medium contained in the (c) crosslinking agent composition of the present invention is not limited as long as it has the above shear viscosity η, but it is preferable that the composition contains a crosslinking agent and a plasticizer.

[0045] In the composition for thermoplastic materials, the content of the (c) crosslinking agent composition is -1 The crosslinking agent in the (c) crosslinking agent composition may be contained in an amount of 0.1 to 10 parts by mass, and preferably 0.3 to 5 parts by mass, per 100 parts by mass of the (a) rubber, while satisfying the shear viscosity η in the above. The content of the (c) crosslinking agent composition may be, for example, 5 to 15 parts by mass, 6 to 12 parts by mass, etc., per 100 parts by mass of the (a) rubber.

[0046] As the crosslinking agent, at least one selected from the group consisting of a quinoxaline-based crosslinking agent, a thiourea-based crosslinking agent, and a triazine-based crosslinking agent is used, with a quinoxaline-based crosslinking agent and a triazine-based crosslinking agent being preferred, and a triazine-based crosslinking agent being particularly preferred.

[0047] Examples of the quinoxaline-based crosslinking agent include 2,3-dimercaptoquinoxaline, quinoxaline-2,3-dithiocarbonate, 6-methylquinoxaline-2,3-dithiocarbonate, and 5,8-dimethylquinoxaline-2,3-dithiocarbonate.

[0048] Examples of the thiourea-based crosslinking agent include 2-mercaptoimidazoline (ethylenethiourea), 1,3-diethylthiourea, 1,3-dibutylthiourea, and trimethylthiourea.

[0049] Examples of the triazine crosslinking agent include 1,3,5-triazinetrithiol, 6-anilino-1,3,5-triazine-2,4-dithiol, 6-methylamino-1,3,5-triazine-2,4-dithiol, 6-dimethylamino-1,3,5-triazine-2,4-dithiol, 6-ethylamino-1,3,5-triazine-2,4-dithiol, 6-diethylamino-1,3,5-triazine-2,4-dithiol, 6-propylamino-1,3,5-triazine Examples of such thiol groups include 6-dipropylamino-1,3,5-triazine-2,4-dithiol, 6-butylamino-1,3,5-triazine-2,4-dithiol, 6-dibutylamino-1,3,5-triazine-2,4-dithiol, 6-hexylamino-1,3,5-triazine-2,4-dithiol, 6-octylamino-1,3,5-triazine-2,4-dithiol, and 6-decylamino-1,3,5-triazine-2,4-dithiol.

[0050] Practically preferred crosslinking agents include 2-mercaptoimidazoline (ethylenethiourea), 6-methylquinoxaline-2,3-dithiocarbonate, and 1,3,5-triazinetrithiol, and a particularly preferred vulcanizing agent is 1,3,5-triazinetrithiol. These crosslinking agents may be used in combination of two or more kinds as long as they do not impair the effects of the present invention.

[0051] Examples of the plasticizer include N-butylbenzenesulfonamide-based plasticizers such as N-butylbenzenesulfonamide, N-(2-hydroxypropyl)benzenesulfonamide, N-ethyl-o-toluenesulfonamide, N-ethyl-p-toluenesulfonamide, o-toluenesulfonamide, and p-toluenesulfonamide; dibutoxyethyl adipate, di(butoxyethoxyethyl) adipate, di(methoxytetraethylene glycol) adipate, di(methoxypentaethylene glycol) adipate, and (methoxytetra) adipate; One or a mixture of two or more of adipic acid ether ester plasticizers such as (ethylene glycol) (methoxypentaethylene glycol), and trimellitic acid plasticizers such as trioctyl trimellitate, triisononyl trimellitate, triisodecyl trimellitate, and mixed alkyl trimellitates can be used; however, N-butylbenzenesulfonamide plasticizers and adipic acid ether ester plasticizers are preferred, and N-butylbenzenesulfonamide plasticizers are preferred in terms of the normal physical properties of the thermoplastic material.

[0052] The content of the plasticizer in the (c) crosslinking agent composition may be 3 to 15 parts by mass, and preferably 4 to 10 parts by mass, per 100 parts by mass of the (a) rubber.

[0053] The (c) crosslinking agent composition of the present invention may contain a crosslinking accelerator. For example, morpholine sulfides, amines, weak acid salts of amines, quaternary ammonium salts, quaternary phosphonium salts, alkali metal salts of fatty acids, thiuram sulfides, polyfunctional vinyl compounds, mercaptobenzothiazoles, sulfenamides, dimethothiocarbamates, guanidines, polyhydric alcohols, etc. are listed. Particularly preferred accelerators when a quinoxaline-based crosslinking agent is applied to the composition of the present invention include 1,8-diazabicyclo(5,4,0)undecene-7 (hereinafter abbreviated as DBU) salt and 1,5-diazabicyclo(4,3,0)nonene-5 (hereinafter abbreviated as DBN) salt. Particularly preferred accelerators when a triazine-based crosslinking agent is applied to the composition of the present invention include guanidines.

[0054] Examples of the DBU salt include DBU-carbonate, DBU-stearate, DBU-2-ethylhexyl salt, DBU-benzoate, DBU-salicylate, DBU-3-hydroxy-2-naphthoate, DBU-phenol resin salt, DBU-2-mercaptobenzothiazole salt, DBU-2-mercaptobenzimidazole salt, etc. Examples of the DBN salt include DBN-carbonate, DBN-stearate, DBN-2-ethylhexyl salt, DBN-benzoate, DBN-salicylate, DBN-3-hydroxy-2-naphthoate, DBN-phenol resin salt, DBN-2-mercaptobenzothiazole salt, DBN-2-mercaptobenzimidazole salt, etc.

[0055] Examples of the guanidines include 1,3-diphenylguanidine and 1,3-diorthotolylguanidine.

[0056] The content of the crosslinking accelerator in the (c) crosslinking agent composition may be 0.1 to 5 parts by mass, and preferably 0.5 to 3 parts by mass, per 100 parts by mass of the (a) rubber.

[0057] The composition of the (c) crosslinking agent composition of the present invention is not particularly limited, but in 100% by mass of the (c) crosslinking agent composition, the crosslinking agent is preferably contained in an amount of 10 to 30% by mass, more preferably 10 to 20% by mass, and even more preferably 12 to 18% by mass, the crosslinking accelerator is preferably contained in an amount of 0 to 12% by mass, and more preferably 5 to 10% by mass, and the plasticizer is preferably contained in an amount of 60 to 85% by mass, and more preferably 70 to 80% by mass.

[0058] In the composition for thermoplastic materials, in addition to (a) rubber, (b) polyamide (PA), and (c) crosslinking agent composition, additives such as a crosslinking retarder, an acid acceptor, an antiaging agent, a release agent, a light stabilizer, a filler, a reinforcing agent, a plasticizer, a processing aid, a pigment, a colorant, an antistatic agent, and a foaming agent can be arbitrarily added.

[0059] The (c) crosslinking agent composition of the present invention can contain, in addition to the crosslinking agent, crosslinking accelerator and plasticizer, any of the same additives as those in the composition for thermoplastic materials.

[0060] Examples of the retarder include N-cyclohexylthiophthalimide, phthalic anhydride, and organic zinc compounds.

[0061] The content of the crosslinking retarder is preferably 0 to 5 parts by mass, and may be 0.1 to 3 parts by mass, based on 100 parts by mass of the (a) rubber.

[0062] In the thermoplastic material composition of the present invention, a metal compound and / or an inorganic microporous crystal is used as the acid acceptor.

[0063] Examples of metal compounds that can be used as acid acceptors include oxides, hydroxides, carbonates, carboxylates, silicates, borates, and phosphites of metals in Group II of the periodic table, and oxides, basic carbonates, basic carboxylates, basic phosphites, basic sulfites, and tribasic sulfates of metals in Group IVA of the periodic table.

[0064] Specific examples of metal compounds that can serve as acid acceptors include magnesia, magnesium hydroxide, barium hydroxide, magnesium carbonate, barium carbonate, sodium carbonate, quicklime, slaked lime, calcium carbonate, calcium silicate, calcium stearate, zinc stearate, calcium phthalate, calcium phosphite, zinc oxide, tin oxide, litharge, red lead, white lead, dibasic lead phthalate, dibasic lead carbonate, basic lead silicate, tin stearate, basic lead phosphite, basic tin phosphite, basic lead sulfite, and tribasic lead sulfate.

[0065] The inorganic microporous crystal means a crystalline porous body, and can be clearly distinguished from amorphous porous bodies such as silica gel and alumina. Examples of such inorganic microporous crystal include zeolites, aluminophosphate-type molecular sieves, layered silicates, synthetic hydrotalcites, and alkali metal titanates. A preferred acid acceptor is synthetic hydrotalcite, and a more preferred acid acceptor is synthetic hydrotalcite, such as calcined hydrotalcite, which has a heating weight loss of 4.5% or less at 300°C for 1 hour.

[0066] The synthetic hydrotalcite is represented by the following general formula (I). Mg X Zinc Y Al Z (OH) (2(X+Y)+3Z-2) CO3 wH2O (I) [In the formula, x and y are real numbers from 0 to 10 having a relationship of x+y=1 to 10, z is a real number from 1 to 5, and w is a real number from 0 to 10.]

[0067] Examples of hydrotalcites represented by the general formula (I) include Mg 4.5 Al2(OH) 13 CO3 3.5H2O, Mg 4.5 Al2(OH) 13 CO3, Mg4Al2(OH) 12 CO3·3.5H2O, Mg6Al2(OH) 16 CO3·4H2O, Mg5Al2(OH) 14 CO3·4H2O, Mg3Al2(OH) 10 CO3·1.7H2O, Mg3ZnAl2(OH) 12 CO3·3.5H2O, Mg3ZnAl2(OH) 12 CO3, etc.

[0068] The content of the acid acceptor is preferably 0.2 to 30 parts by mass, more preferably 0.5 to 20 parts by mass, particularly preferably 1 to 10 parts by mass, and may be 2 to 8 parts by mass, relative to 100 parts by mass of the (a) rubber. These ranges are preferable because they provide physical properties that are usually expected of a thermoplastic material.

[0069] Examples of the antioxidant include aromatic secondary amines, dithiocarbamate metal salts, benzimidazoles, phenols, phosphoric acids, and organic thioacids, with dithiocarbamate metal salts, phenols, and organic thioacids being preferred. Examples of aromatic secondary amine-based antiaging agents include N,N'-di-2-naphthyl-p-phenylenediamine, N-phenyl-1-naphthylamine, alkylated diphenylamine, octylated diphenylamine, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, p-(p-toluenesulfonylamide)diphenylamine, N,N'-di-2-naphthyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine, N-phenyl-N'-isopropyl-p-phenylenediamine, N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, and N-phenyl-N'-(3-methacryloyloxy-2-hydroxypropyl)-p-phenylenediamine. Examples of dithiocarbamate metal salt-based antiaging agents include nickel dibutyldithiocarbamate. Benzimidazole-based antioxidants include zinc salts of 2-mercaptobenzimidazole, 2-mercaptobenzimidazole, and the like.Specific examples of phenol-based antioxidants include 2,6-di-tert-butyl-4-methylphenol, monophenol, 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 4,4'-butylidenebis(3-methyl-6-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), butylated reaction product of p-cresol and dicyclopentadiene, 2,5'-di-tert-butylhydroquinone, 2,5'-di-tert-amylhydroquinone, 2,6-di-tert-butyl-p-cresol, butylated hydroxyanisole, and 2,6-di-tert-butyl-4-ethylphenol. , stearyl-β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tetrakis-(methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate)methane, bis(3,3'-bis-(4'-hydroxy-3'-tert-butylphenyl)butyric acid)glycol ester, 1,3,5-tris(3'5-di-tert-butyl-4'-hydroxybenzyl)-sec-triazine-2,4,6-(1H,3H,5H)trione are examples.Phosphate-based antioxidants include tris(nonylphenyl)phosphite, triphenyl phosphite, diphenyl isodecyl phosphite, diphenyl mono(2-ethylhexyl) phosphite, diphenyl monotridecyl phosphite, phenyl diisodecyl phosphite, 4,4'-butylidene-bis(3-methyl-6-tert-butylphenyl ditridecyl) phosphite, cyclic neopentane tetrayl bis, tris phosphite, diisodecyl pentaerythritol diphosphite, 9,10-dihydro-9-oxa-10 phosphaphenanthrene-10-oxide, 10-(3,5- Examples of the organic thioacid antioxidant include di-tert-butyl-4-hydroxybenzyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-decyloxy-9,10-dihydro-9-oxa-10-phosphaphenanthrene, tris(2,4-di-tert-butylphenyl)phosphite, cyclic neopentanetetraylbis(2,4-di-tert-butylphenyl)phosphite, cyclic neopentanetetraylbis(2,6-di-tert-butyl-4-methylphenyl)phosphite, and 2,2 methylenebis(4,6-di-tert-butylphenyl)octylphosphite. Examples of the organic thioacid antioxidant include dilauryl 3,3'-thiodipropionate, distearyl 3,3'-thiodipropionate, and dimyristyl 3,3'-thiodipropionate. Among these, tetrakis-(methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate)methane and dilauryl 3,3'-thiodipropionate are preferred. The antioxidant may be used alone or in combination of two or more thereof, but is preferably used in combination of two or more thereof.

[0070] The blending amount of the antioxidant may be 0.1 to 10 parts by mass, preferably 0.3 to 5 parts by mass, and particularly preferably 0.5 to 3 parts by mass, based on 100 parts by mass of the (a) rubber.

[0071] Examples of the release agent include metal soaps such as zinc stearate, calcium stearate, and magnesium stearate; higher fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, and oleic acid; higher fatty acid esters such as methyl esters, isopropyl esters, butyl esters, and octyl esters of higher fatty acids; higher alcohols such as myristyl alcohol, cetyl alcohol, and stearyl alcohol; hydrocarbon release agents such as liquid paraffin, paraffin wax, and synthetic polyethylene wax; and montan waxes such as montanic acid ethylene glycol ester and montanic acid butylene glycol ester Ca saponified product.

[0072] (a) The amount of the release agent is preferably 0 to 10 parts by mass relative to 100 parts by mass of the rubber. More specifically, the lower limit is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more. The upper limit is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 5 parts by mass or less.

[0073] The thermoplastic material composition is produced by kneading the components in a kneading machine. The kneading machine may be a batch-type melt kneader such as a kneader or a Banbury mixer, or a continuous melt kneader such as a twin-screw kneading extruder, and may be an apparatus capable of kneading the components under shear force while heating.

[0074] As a method for producing a thermoplastic material of the present invention, it is preferable to (dynamically) crosslink an epichlorohydrin-based rubber with a crosslinking agent while kneading a composition for a thermoplastic material in a kneader. Specifically, the most suitable method is to first melt-mix (a) rubber and (b) polyamide (PA) sufficiently in advance in a kneader, and then crosslink (a) rubber while kneading (c) crosslinking agent composition (dynamic crosslinking). In addition, the temperature and time for crosslinking the epichlorohydrin-based rubber while kneading are preferably in the range of 150 to 300°C (preferably 160 to 200°C) and 2 to 30 minutes in the present invention.

[0075] The thermoplastic material of the present invention may be any material that has thermoplasticity, and may be described as an injection or extrusion molding material that utilizes the properties of the material. It may also be described as a thermoplastic elastomer that softens and becomes fluid when heated, and returns to a rubbery state when cooled. In this case, the crosslinked (a) rubber is dispersed in the (b) polyamide (PA), that is, the (b) polyamide (PA) is the continuous phase, and the crosslinked (a) rubber is dispersed as the dispersed phase.

[0076] In the thermoplastic elastomer, the crosslinked (a) rubber in the thermoplastic elastomer (100 mass%) is preferably contained in an amount of 45 to 85 mass%, more preferably 50 to 85 mass%, and particularly preferably 55 to 85 mass%, or may be contained in an amount of 45 to 80 mass%, 45 to 75 mass%, 50 to 80 mass%, or 50 to 75 mass%.

[0077] The content of (b) polyamide (PA) in the thermoplastic elastomer (100 mass%) is preferably 10 to 50 mass%, more preferably 15 to 45 mass%, and particularly preferably 15 to 40 mass%, or may be 10 to 45 mass%, 20 to 45 mass%, or 20 to 40 mass%.

[0078] The total proportion of the crosslinked (a) rubber and (b) polyamide (PA) in the thermoplastic elastomer of the present invention (100% by mass) may be 85 to 99% by mass, or 90 to 98% by mass.

[0079] The thermoplastic elastomer of the present invention may contain a crosslinking agent, a crosslinking accelerator, an acid acceptor, etc., which are used when crosslinking the (a) rubber, and may also contain an antioxidant, etc. The total amount of these components other than the (a) crosslinked epichlorohydrin rubber and the (b) polyamide (PA) may be 1 to 15% by mass, or 2 to 10% by mass, in the thermoplastic elastomer composition (100% by mass).

[0080] Specific embodiments for carrying out the present invention will be described below with reference to examples. However, the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention.

[0081] A method for producing a (dynamically crosslinked) thermoplastic elastomer composition is described.

[0082] The crystalline melting point of the thermoplastic resin in the examples and comparative examples is determined using a differential scanning calorimeter (DSC-8000 manufactured by PerkinElmer Co., Ltd.) in accordance with JIS K7121-1987.

[0083] The crosslinking agent composition was evaluated by checking the dispersibility and workability by suction with a dropper and by using a rheometer (Hake Mars III manufactured by ThermoFicher Scientific) at a temperature of 30°C and a shear rate of 0.1 s -1 Viscosity measurements were performed under the conditions of shear viscosity η at 100°C and cone plate: C35 / 2. The dispersibility and workability were evaluated as follows. dispersibility ◯: The crosslinking agent composition was stirred and the dispersed state was maintained even after 1 hour. ×: The crosslinking agent composition was stirred and precipitated or solidified after 1 hour. Workability 〇: The crosslinking agent and crosslinking accelerator are dispersed in the plasticizer, making it easy to suck up with a dropper. ×: The crosslinking agent and crosslinking accelerator are not dispersed in the plasticizer, making it difficult to suck up with a dropper.

[0084] The methods for measuring physical properties are as follows. Tensile strength: Compliant with JIS K6251:2010 Elongation: Compliant with JIS K6251:2010 Hardness: Compliant with JIS K6253:2012 Volume change rate: JIS K6258:2016 compliant

[0085] "Example 1" A crosslinking agent composition was prepared by mixing a crosslinking agent, a crosslinking accelerator, and a plasticizer in the ratio shown in Table 1. Then, using a 60 cc kneader heated to 165°C, each material except for the crosslinking agent composition was added in the ratio shown in Table 1, and after kneading for 3 minutes at 100 rpm, the crosslinking agent composition was added, and dynamic crosslinking was carried out for 10 minutes at 100 rpm. Then, the mixture was preheated for 3 minutes and then heated for 3 minutes in a press set at 198°C, and then cooled to form a 2 mm thick sheet. Using the obtained sheet, a tensile test was performed in accordance with JIS K6251 using an AGS-5KNY manufactured by Shimadzu Corporation, and hardness measurements were performed in accordance with the measurement method specified in JIS K6253 using ASKER rubber hardness testers type A and type D manufactured by Kobunshi Keiki Co., Ltd. The volume change rate in the oil resistance test (IRM 903, 125°C x 72 hours) was performed in accordance with JIS K6258. The volume change rate was calculated by ((volume after test - volume before test) / volume before test) x 100. The viscosity of the crosslinking agent composition was measured using a rheometer HAAKE MARSIII manufactured by ThermoFicherScientific, and the viscosity was measured at a shear rate of 0.1 s at 30°C. -1 The shear viscosity η (Pa s) was measured.

[0086] "Example 2" Except for changing the plasticizer from Example 1 in the proportions shown in Table 1, a sheet was molded in the same manner as in Example 1, and then a tensile test was carried out in accordance with JIS K6251, the hardness was measured according to the measurement method specified in JIS K6253, and the volume change rate in an oil resistance test (IRM 903, 125°C x 72 hours) was measured in accordance with JIS K6258. The volume change rate was calculated by ((volume after test - volume before test) / volume before test) x 100. The viscosity of the crosslinking agent composition was measured using a rheometer HAAKE MARSIII manufactured by ThermoFicherScientific, and the viscosity was measured at a shear rate of 0.1 s at 30°C. -1 The shear viscosity η (Pa s) was measured.

[0087] "Example 3" Except for changing the plasticizer from Example 1 in the proportions shown in Table 1, a sheet was molded in the same manner as in Example 1, and then a tensile test was carried out in accordance with JIS K6251 in the same manner as in Example 1, the hardness was measured according to the measurement method specified in JIS K6253, and the volume change rate in an oil resistance test (IRM 903, 125°C x 72 hours) was measured in accordance with JIS K6258. The volume change rate was calculated as ((volume after test - volume before test) / volume before test) x 100. The viscosity of the crosslinking agent composition was measured using a rheometer HAAKE MARSIII manufactured by ThermoFicherScientific, and the viscosity was measured at a shear rate of 0.1 s at 30°C. -1 The shear viscosity η (Pa s) was measured.

[0088] "Comparative Example 1" Except for changing the plasticizer from Example 1 in the proportions shown in Table 1, a sheet was molded in the same manner as in Example 1, and then a tensile test was carried out in accordance with JIS K6251 in the same manner as in Example 1, the hardness was measured according to the measurement method specified in JIS K6253, and the volume change rate in an oil resistance test (IRM 903, 125°C x 72 hours) was measured in accordance with JIS K6258. The volume change rate was calculated as ((volume after test - volume before test) / volume before test) x 100. The viscosity of the crosslinking agent composition was measured using a rheometer HAAKE MARSIII manufactured by ThermoFicherScientific, and the viscosity was measured at a shear rate of 0.1 s at 30°C. -1 The shear viscosity η (Pa s) was measured.

[0089] [Table 1] *1 "Epichromer H (epichlorohydrin homopolymer)" manufactured by Osaka Soda Co., Ltd. *2 Polypla-Evonik Co., Ltd. "Diamid L1600" (melting point 178°C) *3 MP GOKYO FOOD & CHEMICAL CO., LTD. "WARADUR OP" *4 SONGWON "SONGNOX1010" *5 "Nocrac 400" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. *6 "DHT-4C" manufactured by Kyowa Chemical Industry Co., Ltd. *7 "Nocrac NBC" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. *8 "Actor TSH" manufactured by Kawaguchi Chemical Industry Co., Ltd. *9 "Noccela D" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. *10 "BBSA" manufactured by Toray Fine Chemicals Co., Ltd. *11 ADEKA CORPORATION "ADEKA CIZER RS-107" *12 "TOTM" by JPlus Corporation *13 "Polyethylene glycol 400" manufactured by Tokyo Chemical Industry Co., Ltd.

[0090] The test results obtained by each test method are shown in Table 2. In each table, Tb means tensile strength as determined in the tensile test, Eb means elongation as determined in the tensile test, and Hs means hardness as determined in the hardness test of JIS K6253.

[0091] [Table 2]

[0092] Table 2 shows that Examples 1 to 3 have better normal physical properties than Comparative Example 1. The crosslinking agent compositions of Examples 1 to 3 could be sucked up with a dropper, but it was difficult to suck up with a dropper in Comparative Example 1. In addition, the crosslinking agent composition of Comparative Example 1 solidified after about one hour.

[0093] The thermoplastic material of the present invention has excellent mechanical properties and oil resistance, and is therefore useful for industrial products such as automobile parts, and in particular for fuel hoses, refrigerant hoses, and tube materials.

Claims

1. (a) rubber, (b) polyamide (PA), and (c) a crosslinking agent composition, -1 the shear viscosity η in the crosslinking agent composition satisfies 0.1 to 10 Pa·s, and (c) the crosslinking agent in the crosslinking agent composition is contained in an amount of 0.1 to 10 parts by mass per 100 parts by mass of the rubber.

2. 2. The thermoplastic material composition according to claim 1, wherein 10 to 39% by mass of the (b) polyamide (PA) is a polyamide elastomer.

3. The composition for thermoplastic materials according to claim 1, wherein the crosslinking agent in the crosslinking agent composition (c) is at least one crosslinking agent selected from the group consisting of quinoxaline-based crosslinking agents, thiourea-based crosslinking agents, and triazine-based crosslinking agents.

4. The composition for thermoplastic materials according to claim 1, wherein (c) the crosslinking agent composition comprises a crosslinking agent and a plasticizer.

5. A thermoplastic material obtained from the composition for thermoplastic materials according to any one of claims 1 to 4.

6. The thermoplastic material of claim 5 which is a thermoplastic elastomer.

7. (a) Rubber and (b) polyamide (PA) were mixed and then subjected to a shear rate of 0.1 s at 30°C. -1 A method for producing a thermoplastic material, comprising dynamically crosslinking a composition for a thermoplastic material obtained by adding a (c) crosslinker composition having a shear viscosity η of 0.1 to 10 Pa·s to 100 parts by mass of (a) rubber, in such an amount that the amount of the crosslinker in the (c) crosslinker composition is 0.1 to 10 parts by mass.

8. Shear rate 0.1 s at 30 °C -1 The crosslinking agent composition for thermoplastic materials has a shear viscosity η of 0.1 to 10 Pa·s.

9. The crosslinking agent composition for thermoplastic materials according to claim 8, comprising a crosslinking agent and a plasticizer.