Aluminum alloy foil

By controlling the composition and grain size distribution of aluminum alloy foils, the issues of uneven grain size and surface roughness are addressed, resulting in improved formability and workability.

JP2024157652APending Publication Date: 2024-11-08MA ALUMINUM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023072124
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Conventional aluminum alloy foils lack sufficient formability and workability, particularly during deformation processes like press molding, due to uneven crystal grain size and distribution, leading to surface roughness and reduced moldability.

Method used

The aluminum alloy foil composition includes specific ranges of Fe, Si, Cu, and unavoidable impurities, with controlled grain size distribution and misorientation, achieving an average Grain Size Distribution (GSD) of 3.5 or less, ensuring uniform crystal grains and enhanced elongation in multiple directions.

Benefits of technology

The solution suppresses surface roughness and stress concentration, improving formability and workability by ensuring fine and uniform crystal grains, thereby enhancing moldability and elongation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157652000001_ABST
    Figure 2024157652000001_ABST
Patent Text Reader

Abstract

To provide an aluminum alloy foil that offers superior moldability and processability while ensuring foil elongation.SOLUTION: An aluminum alloy foil contains Fe: 0.8% or more and 1.8% or less, Si: 0.01% or more and 0.15% or less, and Cu: 0.001% or more and 0.05% or less, with the balance being Al and unavoidable impurities. For crystal grains with grain boundaries with a misorientation angle of 15° or more on the surface of the aluminum alloy foil, the grain size ratios α for an individual crystal grain with its n adjacent surrounding crystal grains are calculated. The average of the calculated n grain size ratios is set as the Grain Size Distribution (GSD) value for the individual crystal grain. The average GSD calculated across all crystal grains is 3.5 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aluminum foil having excellent formability and processability. [Background technology]

[0002] Aluminum alloy foils used as packaging materials for food products, lithium-ion batteries, and the like are required to have high formability because they are subjected to large deformation during press forming and other processes. For example, in Patent Document 1, the composition range is specified, the grain size of the crystal grains is specified, and further, the area ratio of the Cube orientation is specified, thereby improving the formability. Furthermore, in Patent Document 2, it is said that moldability is improved by defining the ratios of the diffraction intensities representing the (111) plane, the (100) plane, the (110) plane, and the (311) plane. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-115376 A [Patent Document 2] JP 2012-052158 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, conventional aluminum alloy foils do not have sufficient formability. Aluminum alloy foil with high formability can be obtained by suppressing surface roughness during deformation. The size and uniformity of crystal grains are important for suppressing surface roughness, and the more uniform the grain size distribution, the more surface roughness can be suppressed.

[0005] The present invention has been made in light of the above circumstances, and one of its objects is to provide an aluminum alloy foil having good processability and high formability. [Means for solving the problem]

[0006] That is, the first embodiment of the aluminum alloy foil of the present invention is an aluminum alloy foil, Fe: 0.8% by mass or more and 1.8% by mass or less, Si: 0.01% by mass or more and 0.15% by mass or less, Cu: 0.001% by mass or more and 0.05% by mass or less, with the balance being Al and unavoidable impurities; The aluminum alloy foil has a surface where, for crystal grains having grain boundaries with an orientation difference of 15° or more, a grain size ratio α between one crystal grain and n crystal grains adjacent thereto is calculated, and the average value of the n grain size ratios calculated based on the following formula 1 is taken as the grain size distribution (hereinafter, GSD) value of one of the crystal grains, in which the average value of the GSD calculated for each crystal grain is 3.5 or less. GSD=(Σ n i=1 αi) / n … Equation 1 Here, i and n are positive integers, and the value of n is determined for each crystal grain.

[0007] In another aspect of the invention of the aluminum alloy foil, in the above-mentioned aspect, the average value of crystal grains surrounded by high-angle grain boundaries with an orientation difference of 15° or more is 20 μm or less when the average value of the GSD is more than 2.5 and 3.5 or less, and is 25 μm or less when the average value of the GSD is 2.5 or less.

[0008] The aluminum alloy foil of the present invention in another embodiment is characterized in that, in the above-mentioned embodiment, the elongation at angles of 0°, 45° and 90° to the rolling direction is 25% or more.

[0009] The contents stipulated in the present invention will be explained below. (composition) Fe: 0.8% by mass or more and 1.8% by mass or less Fe crystallizes as an Al-Fe intermetallic compound during casting, and becomes a recrystallization site during annealing, which has the effect of refining the recrystallized grains. If the Fe content is low, the distribution density of coarse intermetallic compounds is low, the effect of refining is low, and the final crystal grain size distribution is also non-uniform. On the other hand, if the Fe content is excessive, the effect of refining the crystal grains is saturated or reduced, and further, the size of the Al-Fe compounds generated during casting becomes very large, which reduces the formability and rollability of the foil. For this reason, the Fe content is set to a lower limit of 0.8 mass% and an upper limit of 1.8 mass%. For the same reason, it is preferable to set the lower limit to 1.0 mass% and the upper limit to 1.6 mass%.

[0010] Si: 0.01 mass% or more and 0.15 mass% or less During casting, Si crystallizes into coarse intermetallic compounds. In order to prevent the formation of coarse intermetallic compounds, it is desirable to suppress the amount of Si added. However, if the content is too small, it is necessary to use high-purity ingots, which significantly increases manufacturing costs. On the other hand, if the content is excessive, it may cause the compound size to become coarse and the distribution density to decrease, which may lead to reduced rollability, elongation, and formability. For this reason, the lower limit of the Si content is set to 0.01 mass% and the upper limit to 0.15 mass%. For the same reason, it is desirable to set the lower limit to 0.01 mass% and the upper limit to 0.08 mass%.

[0011] Cu: 0.001 mass% or more and 0.05 mass% or less Cu is an element that increases the strength of aluminum foil and reduces its elongation. On the other hand, it has the effect of suppressing excessive work softening during cold rolling, which has been reported for Al-Fe alloys. If the Cu content is too low, the effect of suppressing work softening is low, and if it is too high, the elongation is clearly reduced. For this reason, the lower limit of the Cu content is set to 0.001 mass% and the upper limit to 0.05 mass%. For the same reason, it is preferable to set the lower limit to 0.005% and the upper limit to 0.01%.

[0012] Inevitable Impurities The balance of the composition is Al and unavoidable impurities. The unavoidable impurities can include Mn, Mg, Zn, Cr, Ti, B, etc. Mn, Mg, and Zn can be expected to suppress processing softening like Cu if they are present in small amounts, but if the content is high, the amount of strengthening by solid solution is large and elongation is reduced. Mn, Zn, and Cr also form fine compounds. These have the effect of suppressing the recrystallization of aluminum, and if the content is high, it becomes difficult to obtain fine and uniform crystal grains. Furthermore, Ti and B contribute to the refinement of the crystal grains of the ingot structure, so they are added in the form of TiB during casting, but if the content is excessive, the effect of refining the crystal grains will saturate, and there is a concern that coarse crystallized products will be formed and rollability and formability will decrease. Therefore, it is desirable to set the upper limit of each component as an unavoidable impurity at 0.05%.

[0013] Average GSD is less than 3.5 In aluminum foil, unevenness occurs on the material surface due to the progress of plastic processing accompanying molding, but in order to obtain good formability, it is necessary to suppress and reduce this unevenness. In order to suppress this surface roughness, the size and uniformity of the crystal grains are important. GSD (Grain Size Distribution) can be used as an index of uniformity of crystal grain size. An average GSD value of 3.5 or less indicates that the crystal grains are uniform, suppresses surface roughness on the material due to plastic processing, and further prevents stress concentration and increases formability. If the average GSD value exceeds 3.5, the surface roughness is significant, resulting in reduced formability. The GSD is calculated as follows: For crystal grains having grain boundaries with a misorientation of 15° or more, the grain size ratio α between one crystal grain (indicated by the thick line in the figure) and the n crystal grains adjacent thereto is calculated based on the following formula, as shown in Figure 1, and the average value of the calculated n grain size ratios is taken as the Grain Size Distribution (hereinafter, GSD) value of the crystal grain. The GSD calculated for each crystal grain is grasped.

[0014]

number

[0015] Specifically, for example, this can be performed by image analysis using Image J based on a grain boundary map obtained by crystal analysis using the EBSD method. However, the present invention is not limited to this method.

[0016] Elongation at 0°, 45°, and 90° to the rolling direction is 25% or more The aluminum alloy foil used in packaging materials is subjected to three-dimensional deformation by press forming. Therefore, elongation is required in various directions, not just in the rolling direction. For this reason, it is desirable for the elongation at 0°, 45°, and 90° to the rolling direction to be 25% or more. If the elongation in any direction is less than 25%, that direction becomes the rate-limiting factor and formability decreases. Effect of the Invention

[0017] According to the present invention, it is possible to suppress the decrease in forming limit, obtain excellent formability, and further to suppress stress concentration, obtain good processability. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is a diagram for explaining an example of a method for calculating the GSD value of a crystal grain in the present invention. [Diagram 2] FIG. 2 is a diagram showing the planar shape of a square punch used in a limit forming height test in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, one embodiment of the aluminum alloy foil of the present invention will be described. In the production of the aluminum alloy foil of this embodiment, first, an ingot having a predetermined composition is melted. The composition contains Fe: 0.8% by mass to 1.8% by mass, Si: 0.01% by mass to 0.15% by mass, Cu: 0.001% by mass to 0.05% by mass, and the remainder is Al and unavoidable impurities.

[0020] The slab, which is an ingot, is subjected to a homogenization treatment, followed by hot rolling and further cold rolling. In the cold rolling, one or more intermediate annealings can be performed as desired. In the final cold rolling after the last intermediate annealing, rolling is performed at a predetermined rolling reduction to obtain an aluminum alloy foil of a predetermined thickness. The aluminum alloy foil after cold rolling is subjected to a final annealing to obtain the alloy foil of the embodiment. The aluminum alloy foil of the embodiment can be subjected to forming processing. Each step will be described below.

[0021] Casting: Slab thickness: 600mm to 750mm Casting to obtain an ingot can be performed by a conventional method, but it is desirable to set the slab to a specified thickness. The slab thickness affects the cooling rate during casting, and also affects the size and distribution of crystallized products and crystal grains generated during casting. In addition, if the slab thickness is different, the rolling ratio to the final foil also changes. It is believed that making the crystal grains fine and uniform at the time of casting contributes to making the foil fine and uniform after final annealing. In addition, changes in the rolling ratio due to changes in slab thickness also contribute to the development of texture in the final foil. The size and uniformity of the crystal grains and the degree of accumulation of the texture affect surface roughness, which in turn contributes to formability. For this reason, it is desirable to make the slab thickness 600 mm or more. However, if the slab thickness exceeds 750 mm, the cooling rate during casting decreases, making it easier for crystallized products generated during casting and for the crystal grain size to become coarse and non-uniform.

[0022] ·Predetermined composition The aluminum alloy foil has a composition containing Fe: 0.8% by mass to 1.8% by mass, Si: 0.01% by mass to 0.15% by mass, Cu: 0.001% by mass to 0.05% by mass, with the remainder being Al and other unavoidable impurities.

[0023] Homogenization: 480℃~540℃×8 hours or more The homogenization treatment is intended to eliminate microsegregation in the ingot and adjust the distribution state of intermetallic compounds, and is an important treatment for obtaining a fine and uniform crystal grain structure in the aluminum alloy foil after final annealing. If the homogenization temperature is less than 480°C, the precipitation of Fe is insufficient, resulting in a high amount of Fe in solid solution, and the density of the coarse intermetallic compounds with a grain size of 1 μm or more and less than 3 μm, which serve as nucleation sites for recrystallization, decreases, resulting in coarse grain size. On the other hand, if the temperature exceeds 540°C, the intermetallic compounds grow significantly, resulting in a large decrease in density of the intermetallic compounds, leading to coarsening of the grains. A treatment time of 8 hours or more is required to distribute the intermetallic compounds at a high density, and if the treatment time is short, the homogenization treatment will be insufficient.

[0024] Hot rolling Finishing temperature: 230℃~280℃ When hot rolling the ingot after homogenization, the finishing temperature is important. By setting the finishing temperature appropriately, recrystallization is suppressed (the hot-rolled sheet has a fibrous structure). However, if the finishing temperature exceeds 280°C, recrystallization occurs in a part of the sheet after hot rolling, making it difficult to obtain an ideal texture in the final product. In addition, a non-uniform structure in which fibrous grains and recrystallized grains are mixed will affect the non-uniformity of the crystal grain structure in the final product, which may lead to a decrease in formability. On the other hand, if the finishing rolling temperature is less than 230°C, the temperature during hot rolling will be extremely low, and there is a concern that cracks will occur on the sides of the sheet, significantly reducing productivity. For this reason, the finishing temperature of hot rolling is preferably in the above range.

[0025] : Rolling ratio 99.2% or more It is desirable to set the rolling ratio from slab to hot rolling finish at 99.2% or more to finely break down the crystallized particles formed during casting. In addition, by increasing the rolling ratio, a fibrous structure is formed after hot rolling.

[0026] Cold rolling The hot rolling is followed by cold rolling, possibly with one or more intermediate annealing steps. Intermediate annealing softens the material that has been hardened by cold rolling (recovering rollability), and also promotes the precipitation of Fe and reduces the amount of dissolved Fe. There are two types of intermediate annealing: batch annealing, in which the coil is placed in a furnace and held there for a certain period of time, and continuous annealing line (CAL annealing), in which the material is rapidly heated and cooled. Either method is acceptable when applying intermediate annealing. For example, in batch annealing, conditions of 300 to 400° C. for 3 hours or more can be adopted, and in CAL annealing, conditions of heating rate: 100 to 250° C. / sec, heating temperature: 300 to 400° C., no holding time or holding time: 5 seconds or less, and cooling rate: 20 to 200° C. / sec can be adopted. However, in this embodiment, the presence or absence of intermediate annealing, and the conditions when intermediate annealing is performed are not limited to specific ones.

[0027] In batch annealing, if the intermediate annealing temperature is less than 300°C, there is a risk that recrystallization will not be completed and the grain structure will become non-uniform. Furthermore, if the intermediate annealing temperature is higher than 400°C, the recrystallized grains will become coarse and the final grain size will also become larger. Furthermore, at higher temperatures, the amount of Fe precipitated decreases and the amount of dissolved Fe increases. If the amount of dissolved Fe is high, recrystallization during final annealing will be suppressed. Even if the treatment time is less than 3 hours, there is a risk that recrystallization will be incomplete and Fe precipitation will be insufficient. Similarly, in CAL annealing, if the annealing temperature is less than 300°C, recrystallization is incomplete and this may lead to non-uniform crystal grain structure, while if it exceeds 400°C, there are concerns about coarsening of recrystallized grains and residual Fe solid solution. These also affect recrystallization during final annealing, and there is a risk of the final crystal grains becoming coarse and non-uniform.

[0028] Final cold rolling: rolling rate 95% or more Since the crystal grains are also refined during the cold rolling process, the higher the final cold rolling reduction ratio from the intermediate annealing to the final thickness, the more refined the crystal grains become. Therefore, a high final cold rolling reduction ratio is desirable, and specifically, a final cold rolling reduction ratio of 95% or more is desirable. If the final cold rolling reduction ratio is less than 95%, the recrystallized grain size after final annealing becomes coarse and non-uniform, causing surface roughness to worsen, making it difficult to achieve high ductility and therefore high formability.

[0029] Final cold rolled thickness A desired thickness can be achieved by final cold rolling. In this embodiment, the thickness is not particularly limited, but may be, for example, 10 to 40 μm.

[0030] Final annealing: 250℃~350℃×10 hours or more In order to completely soften the foil after the final cold rolling, final annealing is performed. The final annealing after the foil rolling may be performed at, for example, 250°C to 350°C. If the temperature of the final annealing is low, the softening is insufficient. On the other hand, if the temperature exceeds 350°C, problems such as deformation of the foil and reduced economic efficiency arise. If the time of the final annealing is less than 10 hours, the effect of the final annealing is insufficient.

[0031] The aluminum alloy foil obtained in this embodiment has an average GSD of 3.5 or less. For crystal grains having grain boundaries with an orientation difference of 15° or more, when the grain size ratio between a crystal grain and each of the n adjacent crystal grains is defined as α, the average value of the n αs is defined as the GSD value of that crystal grain, and the average value of the GSD values ​​calculated for each crystal grain is 3.5 or less. The above-mentioned requirements can be achieved by controlling the slab thickness in the manufacturing process to 600 mm to 750 mm, and by controlling the size and distribution of the crystallites and crystal grains generated during casting, as well as the rolling ratio up to the final foil, thereby optimizing the size and distribution of the crystal grains in the final foil.

[0032] Elongation at 0°, 45°, and 90° to the rolling direction is 25% or more The aluminum alloy foil of the embodiment desirably has elongation of 25% or more at angles of 0°, 45°, and 90° to the rolling direction. The elongation of the aluminum alloy foil of this embodiment does not necessarily have to satisfy this condition, but it is preferable that it satisfies the condition, and it is even more preferable that the elongation in the above three directions is 30% or more. The above elongation characteristics can be obtained by appropriately controlling the slab thickness and rolling ratio in the manufacturing process, similarly to the surface roughness described above.

[0033] In this embodiment, it is desirable for the device to further have the following characteristics. The average grain size of grains surrounded by high-angle grain boundaries with a misorientation of 15° or more is below a specified value. By suppressing the surface roughness that occurs during plastic processing, it is expected that elongation and formability will be improved. One of the factors that influences this surface roughness is the crystal grain size, and to suppress surface roughness, it is desirable for the average crystal grain size to be fine. However, when the average GSD is more than 2.5 and not more than 3.5, it is desirable that the average grain size of the crystal grains surrounded by high-angle grain boundaries with a misorientation of 15° or more is 20 μm or less, and when the average GSD is 2.5 or less, it is desirable that the average grain size of the crystal grains surrounded by high-angle grain boundaries with a misorientation of 15° or more is 25 μm or less. When the average GSD is 2.5 or less, the uniformity of the crystal grain size is high, and the average crystal grain size may be 25 μm or less. The above characteristics can be obtained by appropriately controlling the slab thickness and rolling ratio in the manufacturing process, similar to the GSD described above. EXAMPLES

[0034] The following describes an embodiment of the present invention. The aluminum alloys shown in Table 1 (the balance being Al and other unavoidable impurities) were melted by a conventional method to obtain slabs having the thicknesses shown in Table 1. The slabs were subjected to a homogenization treatment at 500° C. for 8 hours or more. The slabs after the homogenization treatment were hot-rolled to a finished thickness of 5 mm or 8 mm by the hot rolling method shown in Table 1, and the hot rolling finishing temperature was 241°C to 292°C.

[0035] Next, the hot-rolled material was cold-rolled. In the cold rolling, except for specimens No. 11 to 13, intermediate annealing was performed when the plate thickness was 2.8 mm (cold rolling reduction 44.4%, specimen No. 10 was cold rolling reduction 65.0%). In specimen No. 11, intermediate annealing was performed when the plate thickness was 3.6 mm (cold rolling reduction 55.0%), and in specimen No. 12, intermediate annealing was performed when the plate thickness was 1.0 mm (cold rolling reduction 80.0%). Intermediate annealing was performed in a batch furnace under the conditions of 360 ° C x 3 hours. In specimen No. 13, CAL annealing was performed under the conditions of 350 ° C x 1 second when the plate thickness was 1.0 mm (cold rolling reduction 80.0%). Thereafter, final cold rolling was performed until the finished thickness was 40 μm. The reduction ratio of the final cold rolling was 98.6%. The aluminum alloy foils that had been subjected to the cold rolling were subjected to final annealing under the conditions of 300°C x 20 hours.

[0036] The obtained test materials were evaluated for each of the following items, and the evaluation results are shown in Table 2.

[0037] Growth rate The elongation was measured by a tensile test. The tensile test was conducted in accordance with JIS Z2241. JIS No. 5 test pieces were taken so that the elongation could be measured in the directions of 0°, 45°, and 90° to the rolling direction. The test was conducted at a tensile speed of 5 mm / min. using a universal tensile tester (Shimadzu Corporation, AGS-X 10 kN). The elongation percentage was calculated as follows. First, before the test, two lines were marked perpendicular to the longitudinal center of the test piece at intervals of 50 mm, which is the gauge length. After the test, the fracture surfaces of the aluminum alloy foils were butted together to measure the distance between the marks, and the elongation amount (mm) obtained by subtracting the gauge length (50 mm) from the distance was divided by the gauge length (50 mm) to obtain the elongation percentage (%).

[0038] Average grain size After electrolytic polishing of the foil surface, crystal orientation analysis was performed using SEM (Scanning Electron Microscope)-EBSD. Grain boundaries with an orientation difference between grains of 15° or more were defined as HAGBs (high angle grain boundaries), and the size of the grains surrounded by HAGBs was measured. Three fields of view with a field size of 90×180μm were measured at a magnification of 900x, and the average grain size was calculated. The grains in question were those in which all grain boundaries were observed within the field of view. The grain size of each grain was calculated as the equivalent circle diameter, and the average grain size was calculated using the Area method (Average by Area Fraction Method) of EBSD. For the analysis, a FE-SEM (JSM-7900F manufactured by JEOL) was used for the SEM, and OIM Analysis by TSL Solutions was used for EBSD.

[0039] GSD value The GSD value was calculated by image analysis using Image J (software name 1.52u) for the grain boundary map image of HAGBs obtained by EBSD analysis. The calculation procedure is as follows. The EBSD analysis outputs a grain boundary map image with grain boundaries having orientation differences of 15° or more (at that time, image processing is used to convert the background to black and the grain boundaries to white). The obtained grain boundary map is imported into Image J and binarized, after which the grain area is calculated as 1 μm 2 Using the above as a threshold, particle analysis is performed and the area of ​​each crystal grain is output. The equivalent circle diameter of each crystal grain is calculated from the obtained area. From the calculated equivalent circle diameters, crystal grains with the top 10% and bottom 10% equivalent circle diameters within the measurement range, as well as 15% randomly selected from the remaining equivalent circle diameters, are selected, and the GSD value of each crystal grain is calculated from the equivalent circle diameter ratio using the formula described above. The average value is calculated from the obtained GSD values ​​of each crystal grain to obtain the average GSD value. The results of elongation, average grain size, and average GSD value are shown in Table 2.

[0040] Square tube overhang height The square tube overhang height was evaluated in a square tube forming test. The test was performed using a universal sheet metal forming tester (ERICHSEN Model 142 / 20) and a square punch (length of one side L = 37 mm, chamfered diameter R of the corners = 4.5 mm) with a thickness of 40 μm as shown in Figure 2. The test conditions were: wrinkle suppression force 10 kN, scale of punch rising speed (forming speed) set to 1, and mineral oil was applied as a lubricant to one side of the foil (the side that the punch hits). The foil is formed by the punch rising from the bottom of the device hitting the foil, and the maximum punch rise height that could be formed without cracks or pinholes when forming three consecutive times was defined as the square tube overhang height (mm) of the material. The punch height was changed in 0.5 mm intervals. The measurement results are shown in Table 2.

[0041] As shown in the table, the examples of the present invention have a larger rectangular tube overhang height and superior formability compared to the comparative examples. In contrast, the comparative examples Nos. 14 to 20, which have either or both of the composition, average GSD value, and average grain size outside the range of the present invention, have a smaller rectangular tube overhang height and inferior formability.

[0042] [Table 1]

[0043] [Table 2]

Claims

1. An aluminum alloy foil, Fe: 0.8% by mass or more and 1.8% by mass or less, Si: 0.01% by mass or more and 0.15% by mass or less, Cu: 0.001% by mass or more and 0.05% by mass or less, with the balance being Al and unavoidable impurities; The aluminum alloy foil has a surface on which crystal grains having grain boundaries with an orientation difference of 15° or more are provided. When a grain size ratio α between one crystal grain and n crystal grains adjacent thereto is calculated, and an average value of the n grain size ratios calculated based on the following formula 1 is taken as a grain size distribution (hereinafter, referred to as GSD) value of the one crystal grain, the average value of the GSD calculated for each crystal grain is 3.5 or less. GSD = (Σ n i=1 α i ) / n... Equation 1 Here, i and n are positive integers, and the value of n is determined for each crystal grain.

2. 2. The aluminum alloy foil according to claim 1, wherein the average value of crystal grains surrounded by high-angle grain boundaries having an orientation difference of 15° or more is 20 μm or less when the average value of the GSD is more than 2.5 and 3.5 or less, and is 25 μm or less when the average value of the GSD is 2.5 or less.

3. 3. The aluminum alloy foil according to claim 1, wherein elongation at angles of 0°, 45°, and 90° to the rolling direction is 25% or more.

Citation Information

Patent Citations

  • Aluminum foil and container

    JP2012052158A

  • Aluminum alloy soft foil for molding

    JP2018115376A