Laminate for packaging

A packaging laminate with a polyethylene adhesive layer of mixed polyethylene resins addresses high-temperature processing defects and impact resistance, ensuring robustness for heavy contents.

JP2024157819APending Publication Date: 2024-11-08KYODO PRINTING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023072415
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing flexible packaging materials face issues with high-temperature processing defects and impact resistance, particularly when packaging heavy contents, leading to pinholes and breakage.

Method used

A packaging laminate comprising a base resin layer and a sealant layer bonded via a polyethylene adhesive layer containing a mixture of first and second polyethylene resins with specific densities and elastic moduli, allowing for a thin sealant layer with improved high-temperature processability and impact resistance.

Benefits of technology

The laminate provides good workability and impact resistance at high temperatures, effectively preventing bag breakage even with heavy contents, while maintaining a thin sealant layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157819000001_ABST
    Figure 2024157819000001_ABST
Patent Text Reader

Abstract

To provide a novel laminate for packaging, which can provide a packaging having a good processability at a high temperature and a good impact resistance while reducing a thickness of a sealant layer.SOLUTION: As shown in Fig.1(a), a laminate 10a for packaging of the present invention has a base resin layer 12 and a sealant layer 14. The base resin layer 12 and the sealant layer 14 are bonded to each other via a polyethylene adhesive layer 16 constituted by a polyethylene-based resin. The polyethylene adhesive layer contains at least first and second polyethylene-based resins. In a first embodiment, a density of the first polyethylene-based resin is 0.910 g / cm3 or more, and a density of the second polyethylene-based resin is 0.900 g / cm3 or less. In a second embodiment, the first polyethylene resin has a modulus of elasticity of 100 MPa or more, and the second polyethylene resin has a modulus of elasticity of 50 MPa or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a packaging laminate. [Background technology]

[0002] Various flexible packages have been proposed for packaging liquids or viscous materials. In the field of such flexible packages, there have been conventional proposals for suppressing pinholes.

[0003] Patent Document 1 discloses a packaging laminate having a first film layer, a second film layer, and an adhesive layer bonding the first film layer and the second film layer, the adhesive layer being composed of a reactive curing adhesive containing a plasticizer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2022-102584 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention provides a novel packaging laminate that can provide packaging having good processability at high temperatures and impact resistance while allowing the use of a thin sealant layer. [Means for solving the problem]

[0006] As a result of intensive research, the present inventors have found that the above problems can be solved by the following means, and have completed the present invention. That is, the present invention is as follows: <Aspect 1> Having a base resin layer and a sealant layer, the base resin layer and the sealant layer are bonded to each other via a polyethylene adhesive layer made of a polyethylene-based resin; the polyethylene adhesive layer contains at least a first and a second polyethylene resin, The density of the first polyethylene resin is 0.910 g / cm 3 And The density of the second polyethylene resin is 0.900 g / cm 3 Below is the Packaging laminates. <Aspect 2> A substrate resin layer and a sealant layer are provided, the base resin layer and the sealant layer are bonded to each other via a polyethylene adhesive layer made of a polyethylene-based resin; the polyethylene adhesive layer contains at least a first and a second polyethylene resin, The first and second polyethylene resins were formed into a film having a thickness of 200 μm, which was then punched out into a dumbbell shape No. 3 conforming to JIS K 6251. When a tensile test was carried out using this film with a support distance of 20 mm, The first polyethylene resin has an elastic modulus of 100 MPa or more; and The elastic modulus of the second polyethylene resin is 50 MPa or less. Packaging laminates. <Aspect 3> The packaging laminate according to aspect 1 or 2, wherein the ratio of the mass of the second polyethylene resin to the mass of the first polyethylene resin is 0.2 or more and 2.5 or less. <Aspect 4> The packaging laminate according to any one of Aspects 1 to 3, wherein the sealant layer is made of a polyethylene-based resin. <Aspect 5> The packaging laminate according to any one of Aspects 1 to 4, wherein the total thickness of the polyethylene adhesive layer and the sealant layer is 55 μm or less. Aspect 6: The packaging laminate according to any one of Aspects 1 to 5, having an anchor coat layer between the base resin layer and the polyethylene adhesive layer. <Aspect 7> The packaging laminate according to any one of Aspects 1 to 6, further comprising a reinforcing layer on the opposite side of the base resin layer from the sealant layer. <Aspect 8> The packaging laminate according to any one of Aspects 1 to 7, which is used for packaging a heavy item weighing 1 kg or more. A packaging bag having the packaging laminate according to any one of Aspects 1 to 8. A packaging bag containing contents, comprising the packaging bag described in Aspect 9, and contents stored in the packaging bag. Effect of the Invention

[0007] According to the present invention, it is possible to provide a novel packaging laminate which can provide packaging having good processability at high temperatures and good impact resistance while reducing the thickness of the sealant layer. [Brief description of the drawings]

[0008] [Figure 1] 1(a) to (c) are side cross-sectional views of the packaging laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] <<Packaging laminate>> As shown in FIG. 1(a), the packaging laminate 10a of the present invention is A base resin layer 12 and a sealant layer 14 are included. The base resin layer 12 and the sealant layer 14 are bonded to each other via a polyethylene adhesive layer 16 made of a polyethylene resin. The polyethylene adhesive layer contains at least first and second polyethylene resins.

[0010] In a first embodiment of the packaging laminate of the present invention, the density of the first polyethylene resin is 0.910 g / cm 3 or more, and the density of the second polyethylene resin is 0.900 g / cm 3 The following is the result.

[0011] In a second embodiment of the packaging laminate of the present invention, the first and second polyethylene resins are formed into a film having a thickness of 200 μm, which is then punched out into a dumbbell shape No. 3 conforming to JIS K 6251. When a tensile test is carried out using this film with a support distance of 20 mm, The first polyethylene resin has an elastic modulus of 100 MPa or more; and The second polyethylene resin has an elastic modulus of 50 MPa or less.

[0012] In recent years, due to concerns about environmental issues, attention has been focused on reducing the amount of plastic used, and in fact, efforts are being made to reduce the thickness of materials used in rigid packaging such as PET bottles.

[0013] On the other hand, when such thinning is simply applied to conventional flexible packaging, such as the flexible packaging described in Patent Document 1, when the package containing the contents is dropped or during transportation, tiny holes (pinholes), cracks, etc. are formed in the packaging laminate, which can cause the bag to break. This breakage is particularly noticeable when the contents are heavy, for example, weighing 1 kg or more.

[0014] In addition, depending on the configuration of the packaging laminate, a manufacturing process at a high temperature significantly higher than the melting point of the polyethylene resin, particularly lamination at 300° C. or higher, may be required. When a manufacturing process is carried out at such a high temperature, depending on the type of resin, processing defects may occur.

[0015] In response to this, the present inventors have found that these problems can be solved by mixing the above-mentioned first and second polyethylene-based resins to form a polyethylene adhesive layer.

[0016] In the present invention, "bonded via a polyethylene adhesive layer" includes not only the case where the substrate resin layer 12 and the sealant layer 14 are both in direct contact with the polyethylene adhesive layer 16 as shown in FIG. 1(a), but also the case where an anchor coat layer 15 is present between the polyethylene adhesive layer 16 and at least one of these layers, for example the substrate resin layer 12, as shown in FIG. 1(b).

[0017] According to the present invention, the combined thickness of the polyethylene adhesive layer and the sealant layer can be 57 μm or less, 55 μm or less, or 53 μm or less.

[0018] The thickness of the packaging laminate of the present invention, when it does not have a reinforcing layer, may be 20 μm or more, 25 μm or more, 30 μm or more, 35 μm or more, 40 μm or more, 45 μm or more, 50 μm or more, 55 μm or more, or 60 μm or more, and may be 125 μm or less, 120 μm or less, 110 μm or less, 100 μm or less, 90 μm or less, 80 μm or less, 75 μm or less, or 70 μm or less.

[0019] 1(c), the packaging laminate 10c of the present invention may have an optional reinforcing layer 18 on the opposite side of the base resin layer 12 to the sealant layer 14. The reinforcing layer may be bonded via an adhesive layer 17 that is separate from the polyethylene adhesive layer 16.

[0020] The thickness of the packaging laminate of the present invention, when it has a reinforcing layer, may be 25 μm or more, 30 μm or more, 35 μm or more, 40 μm or more, 45 μm or more, 50 μm or more, 55 μm or more, 60 μm or more, 65 μm or more, 70 μm or more, or 80 μm or more, and may be 175 μm or less, 170 μm or less, 160 μm or less, 150 μm or less, 140 μm or less, 130 μm or less, 120 μm or less, 110 μm or less, 100 μm or less, or 90 μm or less.

[0021] Each component of the present invention will now be described.

[0022] <Base material resin layer> The base resin layer is a layer that is bonded to the sealant layer via a polyethylene adhesive layer.

[0023] From the viewpoint of preventing bag breakage, the tensile strength of the base resin layer is preferably 150 MPa or more, 180 MPa or more, 200 MPa or more, or 230 MPa or more.

[0024] In the case of an injection molded product, the tensile strength may be the higher of the tensile strength in the molding direction (MD) and the tensile strength in the transverse direction (TD).

[0025] As the resin having the above tensile strength, for example, a polyamide resin, a polyester resin, or a polypropylene resin can be used.

[0026] As the polyamide resin, for example, nylon such as Nylon (registered trademark) 6 or Nylon MXD6 can be used.

[0027] As the polyester resin, for example, polyethylene terephthalate, polybutylene terephthalate, etc. can be used.

[0028] The polypropylene-based resin is a resin containing repeating units of propylene groups in the main chain of the polymer at more than 50 mol%, 60 mol% or more, 70 mol% or more, or 80 mol% or more. Examples of the polypropylene-based resin that can be used include polypropylene (PP) homopolymer, random polypropylene (random PP), block polypropylene (block PP), chlorinated polypropylene, acid-modified polypropylene, and derivatives thereof, as well as mixtures thereof.

[0029] The thickness of the base resin layer may be 5 μm or more, 10 μm or more, or 12 μm or more, and may be 50 μm or less, 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, 25 μm or less, 20 μm or less, or 18 μm or less.

[0030] <Polyethylene adhesive layer> The polyethylene adhesive layer contains at least a first and a second polyethylene resin.

[0031] In this specification, the term "polyethylene resin" refers to a resin that contains more than 50 mol%, 60 mol% or more, 70 mol% or more, or 80 mol% or more of ethylene group repeating units in the main chain of the polymer, and is selected from the group consisting of, for example, low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), ethylene-acrylic acid copolymer (EAA), ethylene-methacrylic acid copolymer (EMAA), ethylene-ethyl acrylate copolymer (EEA), ethylene-methyl acrylate copolymer (EMA), derivatives thereof, and mixtures thereof.

[0032] The ratio of the mass of the second polyethylene resin to the mass of the first polyethylene resin may be 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, or 0.9 or more, and may be 2.5 or less, 2.4 or less, 2.3 or less, 2.2 or less, 2.1 or less, 2.0 or less, 1.8 or less, 1.5 or less, 1.3 or less, or 1.1 or less.

[0033] The density of the resin composition constituting the polyethylene adhesive layer is 0.890 g / cm 3 More than 0.895g / cm 3 or more than 0.900g / cm 3 or more, and may be 0.920 g / cm 3 Below, 0.915g / cm 3 or less than 0.912 g / cm 3 It may be the following:

[0034] The breaking strength of the resin composition constituting the polyethylene adhesive layer is 8N / mm 2 More than 10N / mm 2 More than 12N / mm 2 More than 15N / mm 2 or more than 18N / mm 2 It may be more than 50N / mm2 Below, 45N / mm 2 Below, 40N / mm 2 Below, 38N / mm 2 Below, 35N / mm 2 Below, 33N / mm 2 or less than 30N / mm 2 It may be the following:

[0035] The tensile elongation of the resin composition constituting the polyethylene adhesive layer may be 400% or more, 500% or more, 600% or more, 700% or more, 800% or more, 900% or more, 1000% or more, or 1100% or more, and may be 2000% or less, 1900% or less, 1800% or less, 1700% or less, 1600% or less, 1500% or less, or 1400% or less.

[0036] The elastic modulus of the resin composition constituting the polyethylene adhesive layer may be 140 MPa or less, 130 MPa or less, 120 MPa or less, 110 MPa or less, or 100 MPa or less, and may be 10 MPa or more, 20 MPa or more, 30 MPa or more, 40 MPa or more, 50 MPa or more, 60 MPa or more, or 70 MPa or more.

[0037] The breaking strength, tensile elongation and elastic modulus of the resin composition constituting the polyethylene adhesive layer were obtained by molding the resin constituting the polyethylene adhesive layer into a film 200 μm thick, punching this into a dumbbell-shaped No. 3 shape conforming to JIS K 6251, and using this to perform a tensile test with a support distance of 20 mm.

[0038] The thickness of the polyethylene adhesive layer may be 30 μm or less, or 28 μm or less, and may be 5 μm or more, 10 μm or more, 15 μm or more, 20 μm or more, or 23 μm or more.

[0039] The polyethylene adhesive layer can be disposed by sandwich laminating a composition obtained by kneading at least the first and second polyethylene resins between the base resin layer and the sealant layer.

[0040] (First polyethylene resin) In the first embodiment, the first polyethylene resin has a density of 0.910 g / cm 3 The density of this polyethylene resin is 0.913 g / cm or more. 3 More than 0.915g / cm 3 or more than 0.917g / cm 3 or more, and may be 0.925 g / cm 3 Below, 0.923g / cm 3 or less than 0.920g / cm 3 It may be the following:

[0041] In the second embodiment, the first polyethylene resin is a polyethylene resin having an elastic modulus of 80 MPa or more when the above-mentioned tensile test is carried out. This elastic modulus may be 85 MPa or more, 90 MPa or more, 95 MPa or more, or 100 MPa or more, and may be 170 MPa or less, 160 MPa or less, 150 MPa or less, 145 MPa or less, 140 MPa or less, or 135 MPa or less.

[0042] By incorporating a polyethylene resin having the above physical properties into the polyethylene adhesive layer, it is possible to improve processability at high temperatures, particularly at temperatures of 300° C. or higher. Processability at this temperature promotes oxidation of the resin, thereby improving adhesion when an anchor coat layer is used.

[0043] The first polyethylene resin had a breaking strength of 8 N / mm when subjected to the above tensile test. 2 More than 10N / mm 2 More than 12N / mm 2 More than 15N / mm 2 or more than 18N / mm 2 It may be more than 50N / mm 2 Below, 45N / mm 2 Below, 40N / mm 2 Below, 38N / mm 2 Below, 35N / mm 2 Below, 33N / mm 2 or less than 30N / mm 2It may be the following:

[0044] The tensile elongation of the first polyethylene resin when subjected to the above-mentioned tensile test may be 600% or more, 700% or more, 800% or more, 900% or more, 1000% or more, or 1100% or more, and may be 2000% or less, 1900% or less, 1800% or less, 1700% or less, 1600% or less, 1500% or less, or 1400% or less.

[0045] The melt mass flow rate (MFR) of the first polyethylene resin, when measured in accordance with JIS K6922-1 and -2 and JIS K7210-1 under conditions of a temperature of 190°C and a load of 21.18 N, may be 3.0 g / 10 min or more, 4.0 g / 10 min or more, 5.0 g / 10 min or more, 5.5 g / 10 min or more, or 6.0 g / 10 min or more, and may be 10.0 g / 10 min or less, 9.0 g / 10 min or less, 8.0 g / 10 min or less, or 7.0 g / 10 min or less.

[0046] The content of the first polyethylene resin may be 25 mass% or more, 30 mass% or more, 35 mass% or more, 40 mass% or more, or 45 mass% or more, and may be 85 mass% or less, 80 mass% or less, 75 mass% or less, 70 mass% or less, 65 mass% or less, 60 mass% or less, or 55 mass% or less, relative to the mass of the polyethylene adhesive layer.

[0047] (Second polyethylene resin) In the first embodiment, the second polyethylene resin has a density of 0.900 g / cm 3 It is a polyethylene resin with a density of 0.895 g / cm 3 or less than 0.890g / cm 3 or less and may be 0.860 g / cm 3 or more than 0.865g / cm 3 It may be more than that.

[0048] In the second embodiment, the second polyethylene resin is a polyethylene resin having an elastic modulus of 50 MPa or less when the above-mentioned tensile test is carried out. This elastic modulus may be 45 MPa or less, 40 MPa or less, or 35 MPa or less, and may be 5 MPa or more, 7 MPa or more, 10 MPa or more, 15 MPa or more, or 20 MPa or more.

[0049] By incorporating a polyethylene resin having the above physical properties into the polyethylene adhesive layer, the physical strength, particularly the impact resistance, of the sealant layer can be improved.

[0050] This physical strength can prevent the bag from breaking when dropped when a heavy object, for example, an object weighing 1 kg or more, is packaged in the bag. Without wishing to be bound by theory, this is believed to be because the above elastic modulus of the second polyethylene resin allows the bag to withstand impact when dropped while packaging the contents.

[0051] The second polyethylene resin had a breaking strength of 8N / mm 2 More than 10N / mm 2 More than 12N / mm 2 More than 15N / mm 2 or more than 18N / mm 2 It may be more than 50N / mm 2 Below, 45N / mm 2 Below, 40N / mm 2 Below, 38N / mm 2 Below, 35N / mm 2 Below, 33N / mm 2 or less than 30N / mm 2 It may be the following:

[0052] The tensile elongation of the second polyethylene resin when subjected to the above-mentioned tensile test may be 900% or more, 1000% or more, 1100% or more, or 1200% or more, and may be 2000% or less, 1900% or less, 1800% or less, 1700% or less, 1600% or less, 1500% or less, or 1400% or less.

[0053] The melt mass flow rate (MFR) of the second polyethylene resin, when measured in accordance with JIS K6922-1 and -2 and JIS K7210-1 under conditions of a temperature of 190°C and a load of 21.18N, may be 2.0 g / 10 min or more, 3.0 g / 10 min or more, 4.0 g / 10 min or more, 5.0 g / 10 min or more, 5.5 g / 10 min or more, or 6.0 g / 10 min or more, and may be 25.0 g / 10 min or less, 22.0 g / 10 min or less, 20.0 g / 10 min or less, 18.0 g / 10 min or less, 15.0 g / 10 min or less, 12.0 g / 10 min or less, 10.0 g / 10 min or less, 9.0 g / 10 min or less, 8.0 g / 10 min or less, or 7.0 g / 10 min or less.

[0054] The content of the second polyethylene resin may be 15 mass% or more, 20 mass% or more, 25 mass% or more, 30 mass% or more, 35 mass% or more, 40 mass% or more, or 45 mass% or more, and may be 75 mass% or less, 70 mass% or less, 65 mass% or less, 60 mass% or less, or 55 mass% or less, relative to the mass of the polyethylene adhesive layer.

[0055] <Sealant layer> The sealant layer is a layer for heat sealing to an opposing resin layer, for example, a layer for heat sealing to an opposing resin layer, or a layer for heat sealing the packaging laminate to another film. This layer can be located on the content side when a packaging bag is obtained using the packaging laminate.

[0056] The resin constituting the sealant layer may be a polyethylene-based resin. As the polyethylene-based resin, those mentioned in relation to the polyethylene adhesive layer may be used. The sealant layer may be a single-layer polyethylene film, or a polyethylene laminated film composed of multiple layers of polyethylene-based resin.

[0057] The thickness of the sealant layer may be 45 μm or less, 40 μm or less, 35 μm or less, 33 μm or less, 30 μm or less, or 28 μm or less, and may be 10 μm or more, 15 μm or more, 20 μm or more, or 22 μm or more.

[0058] <Anchor coat layer> The anchor coat layer is generally a layer provided on the surface of an object to be bonded to modify the surface, thereby promoting adhesion. In particular, when laminating an anchor coat layer having a polar group onto a resin layer, the anchor coat layer is generally treated at a high temperature, for example, at a temperature of 300°C or higher, 310°C or higher, 320°C or higher, or 330°C or higher, in order to promote oxidation of the surface of the resin layer, thereby promoting polar adhesion between the surface and the anchor coat layer.

[0059] In particular, in the present invention, the anchor coat layer may be present between the substrate resin layer and the polyethylene adhesive layer. In particular, in the manufacturing stage, the anchor coat layer may be laminated in advance on the side of the substrate resin layer on which the polyethylene adhesive layer is to be provided, prior to sand lamination. In this case, the sand lamination may be performed in the above-mentioned high temperature environment.

[0060] For the anchor coat layer, for example, an anchor coat agent such as an aliphatic ester-based, urethane-based, polyethyleneimine-based, titanate-based, or butadiene-based agent can be used.

[0061] <Reinforcing layer> The reinforcing layer is an optional layer that is present on the opposite side of the base resin layer from the sealant layer.

[0062] As the resin constituting the reinforcing layer, the resins listed for the base resin layer can be used.

[0063] The thickness of the reinforcing layer may be 5 μm or more, 10 μm or more, 12 μm or more, or 15 μm or more, and may be 50 μm or less, 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, 25 μm or less, 22 μm or less, or 20 μm or less.

[0064] Other Layers The packaging laminate of the present invention may have other optional layers, such as an adhesive layer between the reinforcing layer and the base resin layer, and a barrier layer.

[0065] As the adhesive layer, for example, a dry lamination adhesive, a hot lamination adhesive, or the like can be used.

[0066] The barrier layer may be made of a material capable of preventing moisture, organic gases, and inorganic gases from penetrating into the gas absorbing layer from the outside. Examples of the barrier layer include a single metal foil layer such as copper foil or aluminum foil, an alloy foil layer such as stainless steel foil, an inorganic vapor deposition film such as a silica vapor deposition film, an alumina vapor deposition film, or a silica-alumina binary vapor deposition film, or an organic coating film such as a polyvinylidene chloride coating film, a polychlorotrifluoroethylene coating film, or a polyvinylidene fluoride coating film.

[0067] When an inorganic vapor deposition film or an organic coating film is used as the barrier layer, the thickness of the barrier layer is preferably 100 nm or more, 200 nm or more, 300 nm or more, 500 nm or more, 700 nm or more, or 1 μm or more from the viewpoint of ensuring strength and barrier properties, and is preferably 5 μm or less, 4 μm or less, 3 μm or less, or 2 μm or less from the viewpoint of reducing the thickness of the entire packaging laminate.

[0068] When a metal foil layer or a barrier resin layer is used as the barrier layer, the thickness of the barrier layer is preferably 7 μm or more, 10 μm or more, or 15 μm or more from the viewpoint of ensuring strength and barrier properties, and is preferably 50 μm or less, 45 μm or less, 40 μm or less, or 35 μm or less from the viewpoint of reducing the thickness of the entire packaging laminate.

[0069] 《Packaging bag》 The packaging bag of the present invention is a packaging bag having the above-mentioned packaging laminate.

[0070] In particular, the packaging bag of the present invention comprises one or more of the above-mentioned packaging laminates, A part of one or more sheets of the packaging laminate is heat-sealed to another part of the packaging laminate or to another film to form a bag, where the other film may be another packaging laminate or may be a film other than the packaging laminate.

[0071] The packaging bag of the present invention can be a content-containing packaging bag having the above-mentioned packaging bag and the content stored in the packaging bag.

[0072] The packaging bag of the present invention may be in the form of, for example, a three-side sealed bag, a four-side sealed bag, a pillow bag, a gusset bag, a standing pouch, or the like.

[0073] <Contents> The contents are the contents stored in the packaging bag. The contents are not limited as long as they can deteriorate when exposed to the outside air, and examples of the contents include medicines, food, cosmetics, medical instruments, medical equipment, electronic parts, precision machinery, recording materials, etc. Furthermore, medicines include pharmaceutical preparations, cleaning agents, agricultural chemicals, etc.

[0074] In particular, when the contents are heavy, particularly when the contents are 1 kg or more in weight, the bag is generally more likely to break when dropped, and therefore the packaging laminate of the present invention is more beneficial. In particular, when the contents, particularly the heavy contents, are in a liquid, viscous, or other state, the packaging laminate of the present invention is more beneficial from the viewpoint of preventing leakage. EXAMPLES

[0075] The present invention will be specifically described with reference to examples and comparative examples, but the present invention is not limited to these.

[0076] <<Making packaging bags>> Example 1 An aliphatic ester anchor coating agent was applied to one side of a nylon film (Ny1, thickness 15 μm, MD tensile strength 250 MPa, TD tensile strength 350 MPa) as a base resin layer at a coating weight of 0.5 g / m 2 The coating was performed using a 100% aqueous solution of 100% ethyl alcohol.

[0077] Next, the surface of the nylon film coated with the anchor coating agent and a polyethylene film (LLDPE, Unilux LS711C, Idemitsu Unitech Co., Ltd.) as a sealant layer were sandwiched together by an extrusion laminator so that the total thickness of the polyethylene adhesive layer and the sealant layer was 50 μm, thereby producing a packaging laminate of Example 1. In Example 1, an LLDPE film with a thickness of 30 μm was used. The temperature setting of the extrusion laminator was 340° C.

[0078] The resin composition constituting the polyethylene adhesive layer in Example 1 was a dry blend of 50 parts by mass each of PE2 and PE4 shown in Table 1.

[0079] The prepared packaging laminate was cut into pieces measuring 430 mm x 380 mm, which were heat sealed with the top and bottom seals at a width of 10 mm and the back seal at a width of 15 mm. 2 kg of water was then filled into the pieces to prepare pillow bags with outer dimensions of 200 mm x 380 mm, in sufficient numbers to carry out the following evaluations.

[0080] Examples 2 to 8 and Comparative Examples 1 to 8 Except for changing the type and content of the polyethylene resin used and the thickness of the sealant layer to those shown in Tables 1 and 2, multiple packaging laminates and pillow bags containing contents using the same were produced in the same manner as in Example 1 for Examples 2 to 8 and Comparative Examples 1 to 8.

[0081] <Physical properties of the resin that makes up the adhesive layer> Each polyethylene resin and each resin composition constituting the polyethylene adhesive layer of Examples 1 to 8 was molded into a film having a thickness of 200 μm, which was then punched out into a dumbbell-shaped No. 3 shape conforming to JIS K 6251. Tensile tests were performed using these films with a support distance of 20 mm to measure their breaking strength, tensile elongation and elastic modulus.

[0082] The density of the polyethylene adhesive layer in Examples 1 to 8 was calculated as a weighted average from the density and content of each polyethylene resin.

[0083] For each polyethylene resin, the melt mass flow rate (MFR) was measured using a melt indexer (Techno Seven Co., Ltd.) under conditions of a temperature of 190°C and a load of 21.18 N in accordance with JIS K6922-1 and -2 and JIS K7210-1.

[0084] Details of the polyethylene resins used in the examples and comparative examples are shown in Table 1.

[0085] [Table 1]

[0086] The term "dry lamination" in Table 2 refers to a two-component dry lamination adhesive (Dic Dry LX500 / KR90S, DIC Graphics Corporation) applied at a coating weight of 3.5 g / m instead of sand lamination with a polyethylene adhesive layer. 2 By using the expression "dry laminate" in the above, it is meant that the base resin layer is dry laminated with the sealant layer.

[0087] "evaluation" <Suitability for high-temperature processing> The appearance of the resulting packaging laminate constituting the packaging bag was visually confirmed and evaluated according to the following criteria. A: A smooth packaging laminate was obtained. B: Folded edges of the packaging laminate and unevenness of the film were visible. C: Edge folding of the packaging laminate occurred to such an extent that it significantly affected bag making.

[0088] Drop Test Two pillow bags containing contents obtained using the packaging laminate of Example 1 were stacked and packed in a cardboard box with inner dimensions of 293 mm x 176 mm x 118 mm, and a drop test was conducted using this. The drop test was conducted 10 times (once on a corner, three times on an edge, and six times on a face) in one set, with the drop position being changed, and the number of sets until the bag broke was recorded. The same test was conducted three times, and the average value was calculated. The same evaluation was conducted for Examples 2 to 8 and Comparative Examples 1 to 5 and 7 to 8. This evaluation could not be conducted for Comparative Example 6, since its high-temperature processing suitability was extremely poor.

[0089] The configurations and evaluation results of the examples and comparative examples are shown in Tables 1 and 2.

[0090] [Table 2]

[0091] From Table 2, the density is 0.910 g / cm 3 and / or a modulus of elasticity of 100 MPa or more, and a density of 0.900 g / cm 3 It can be seen that the packaging laminates of Examples 1 to 8, which contain a second polyethylene resin having a modulus of elasticity of 50 MPa or less, exhibited good high-temperature processability and good drop test results.

[0092] In particular, the results of the drop test were comparable to or better than those of Comparative Example 1, in which a sealant layer was used instead of a polyethylene adhesive layer, in the packaging laminates of Examples 1 to 8, while the thickness of the sealant layer was made thinner. Moreover, Comparative Example 2, in which the sealant layer of Comparative Example 1 was simply made thinner, showed worse results in the drop test.

[0093] On the other hand, the packaging laminate of Comparative Example 3, which used the first polyethylene resin alone, did not show good results in the drop test, and the packaging laminates of Comparative Examples 5 to 8, which used the second polyethylene resin alone, did not show good suitability for high-temperature processing.

[0094] The density of the packaging laminate of the embodiment is 0.897 g / cm 3 More than 0.912g / cm 3 However, Comparative Example 4, which used PE3 alone, which had a density within this range, did not have good high-temperature processability. From this, it can be understood that in order to improve both the high-temperature processability and the drop test results, it is necessary to use a resin composition in which the above-mentioned first and second polyethylene resins are mixed as the polyethylene adhesive layer. [Explanation of symbols]

[0095] 10a, 10b Packaging laminate 12 Base resin layer 14 Sealant layer 15 Anchor coat layer 16 Polyethylene adhesive layer 17 Adhesive layer 18 Reinforcement layer

Claims

1. A substrate resin layer and a sealant layer are included. the base resin layer and the sealant layer are bonded to each other via a polyethylene adhesive layer made of a polyethylene-based resin; the polyethylene adhesive layer contains at least a first and a second polyethylene resin, The density of the first polyethylene resin is 0.910 g / cm 3 And The density of the second polyethylene resin is 0.900 g / cm 3 Below is the Packaging laminates.

2. A substrate resin layer and a sealant layer are included. the base resin layer and the sealant layer are bonded to each other via a polyethylene adhesive layer made of a polyethylene-based resin; the polyethylene adhesive layer contains at least a first and a second polyethylene resin, The first and second polyethylene resins were molded into a film having a thickness of 200 μm, which was then punched into a dumbbell shape No. 3 in accordance with JIS K 6251. A tensile test was carried out using this film with a support distance of 20 mm. The first polyethylene resin has an elastic modulus of 100 MPa or more, and The elastic modulus of the second polyethylene resin is 50 MPa or less. Packaging laminates.

3. 3. The packaging laminate according to claim 1, wherein a ratio of the mass of the second polyethylene resin to the mass of the first polyethylene resin is 0.2 or more and 2.5 or less.

4. 3. The packaging laminate according to claim 1, wherein the sealant layer is made of a polyethylene resin.

5. 3. The packaging laminate according to claim 1, wherein the sum of the thicknesses of the polyethylene adhesive layer and the sealant layer is 55 μm or less.

6. 3. The packaging laminate according to claim 1, further comprising an anchor coat layer between the base resin layer and the polyethylene adhesive layer.

7. The packaging laminate according to claim 1 or 2, further comprising a reinforcing layer on the opposite side of the base resin layer to the sealant layer.

8. 3. The packaging laminate according to claim 1, which is for packaging a heavy object weighing 1 kg or more.

9. A packaging bag comprising the packaging laminate according to claim 1 or 2.

10. A packaging bag containing a content, comprising the packaging bag according to claim 9 and a content stored in the packaging bag.

Citation Information

Patent Citations

  • Packaging laminate

    JP2022102584A