Base material film for semiconductor manufacturing tape
A multilayer base film with 1-butene homopolymer, pentene copolymer, and olefin elastomer, along with an antistatic agent, addresses the rigidity and stress relaxation issues of polyolefin films, enhancing semiconductor manufacturing by preventing static damage and ensuring uniform handling.
Patent Information
- Application Number
- JP2023072591
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
AI Technical Summary
Existing polyolefin base films for semiconductor manufacturing tapes lack sufficient rigidity, stress relaxation properties, and antistatic properties, making them inadequate substitutes for vinyl chloride-based films, especially as IC chips become thinner and more prone to static electricity.
A base film with a multilayer structure comprising a functional layer made of 1-butene homopolymer, pentene copolymer, and olefin elastomer, and a surface layer containing an antistatic agent, with specific mass content ratios to enhance rigidity, stress relaxation, and antistatic properties.
The base film provides excellent antistatic properties, rigidity, and stress relaxation, preventing damage from static electricity and ensuring uniform expansion and handling of semiconductor devices during manufacturing.
Smart Images

Figure 2024157921000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a substrate film for a tape for manufacturing semiconductors (hereinafter, sometimes simply referred to as "substrate film"). [Background technology]
[0002] As a method for manufacturing semiconductor devices such as IC chips, for example, a method is widely used in which a wafer circuit formed on a substantially disk-shaped semiconductor wafer is divided by dicing on a semiconductor manufacturing tape (dicing tape) for wafers to obtain individual semiconductor devices. After dicing, for example, the dicing tape is stretched to form gaps between the semiconductor devices (i.e., expanded), and then each semiconductor device is picked up by a robot or the like.
[0003] In addition, a dicing die attach film (DDAF), in which an adhesive layer is laminated on the adhesive layer of the above-mentioned dicing tape, is used as a semiconductor manufacturing tape for wafers. After the wafer circuits are divided by dicing on the dicing die attach film, the dicing die attach film is stretched to form gaps between the semiconductor devices, and then the adhesive layer is photocured. The semiconductor devices are then peeled off from the adhesive layer with the adhesive layer still attached and picked up.
[0004] Conventionally, vinyl chloride-based base films have been used as base films for semiconductor manufacturing tapes. However, from the viewpoints of reducing the environmental load and preventing chloride ions and plasticizers from migrating to the wafer, polyolefin-based base films have recently been used instead of vinyl chloride-based base films.
[0005] Furthermore, due to factors such as the thinning of IC chips, static electricity is more likely to be generated during the production of IC chips. To prevent problems such as damage to the wafer circuits in IC chips caused by the static electricity, there is a demand to impart antistatic properties to dicing tapes and base films.
[0006] More specifically, for example, a substrate film for a dicing tape formed from a resin composition containing an ethylene-based resin, a propylene-based resin, and a block copolymer of propylene and a polyhydric alcohol has been proposed. It is described that a polyolefin-based substrate film having antistatic properties can be obtained by using the block copolymer of propylene and a polyhydric alcohol (for example, see Patent Document 1). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2022 / 064949 Summary of the Invention [Problem to be solved by the invention]
[0008] However, although the substrate film described in Patent Document 1 is a polyolefin-based substrate film having antistatic properties, it has insufficient rigidity and stress relaxation properties, and therefore there is a problem in that it is difficult to obtain a polyolefin-based substrate film having antistatic properties and physical properties capable of replacing vinyl chloride-based substrate films.
[0009] The present invention has been made in consideration of the above problems, and has an object to provide a substrate film for a tape for manufacturing semiconductors, which has excellent antistatic properties, rigidity and stress relaxation properties. [Means for solving the problem]
[0010] In order to achieve the above-mentioned object, the base film for semiconductor manufacturing tape of the present invention has a functional layer and a surface layer provided on at least one side of the functional layer, the functional layer contains a homopolymer of 1-butene, a copolymer of pentene, and an olefin-based elastomer, the surface layer contains an antistatic agent, and the content of the olefin-based elastomer in the entire functional layer is more than 0 mass% and less than 50 mass%, and the content of the antistatic agent in the entire surface layer is more than 0 mass% and less than 40 mass%. Effect of the Invention
[0011] According to the present invention, it is possible to provide a substrate film for a tape for manufacturing a semiconductor device, which has excellent antistatic properties, rigidity and stress relaxation properties. [Brief description of the drawings]
[0012] [Figure 1] 1 is a cross-sectional view showing a substrate film for a semiconductor manufacturing tape according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The substrate film for semiconductor manufacturing tape of the present invention will be specifically described below. Note that the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention.
[0014] The substrate film of the present invention is a substrate film constituted by a laminate of a functional layer (intermediate layer) and a surface layer provided on at least one side of the functional layer.
[0015] An example of a substrate film having this multilayer structure is a substrate film 1 having a three-layer structure composed of a laminate of a functional layer 2 and a surface layer 3 laminated on both sides of the functional layer 2, laminated in the order of surface layer / functional layer / surface layer, as shown in Figure 1.
[0016] The functional layer may include a homopolymer of 1-butene, a copolymer of pentene, and an olefin-based elastomer.
[0017] <1-butene homopolymer> In the present invention, a homopolymer obtained by polymerizing 1-butene alone is used as the polybutene. This 1-butene homopolymer has a high molecular weight and bulky side chains, and the strong intermolecular forces due to these bulky side chains can improve the uniform stretchability of the base film, in the same way as in the case of amorphous polymers, despite being a crystalline polymer.
[0018] The 1-butene homopolymer used in the present invention may have a weight average molecular weight (Mw) of about 500,000 to 1,500,000.
[0019] The "weight average molecular weight" refers to that calculated in accordance with JIS K 7252-1:2016.
[0020] Furthermore, since the 1-butene homopolymer used in the present invention has a high molecular weight, it has low surface adhesion and is more rigid than amorphous polyolefins. Therefore, in the production process of the base film, it is possible to provide a base film having high rigidity that allows the base film to be unwound and made into a tape, including coating with an adhesive.
[0021] As described above, by using a homopolymer of 1-butene as the resin forming the base film, the uniform extensibility and rigidity of the base film can be improved.
[0022] In addition, from the viewpoint of improving uniform elongation and rigidity, the content of 1-butene homopolymer in the entire functional layer 2 is preferably 20% by mass or more and 70% by mass or less, and more preferably 30% by mass or more and 60% by mass or less, of 100% by mass of the functional layer.
[0023] <Pentene copolymer> In the base film 1 of the present invention, the functional layer 2 contains a pentene copolymer as polypentene from the viewpoint of improving the stress relaxation property that enables the dimensions of the semiconductor manufacturing tape to be maintained after expansion. The use of such a pentene copolymer improves the stress relaxation property of the base film 1, making it possible to hold the semiconductor manufacturing tape with a grip ring and to maintain the spacing between each semiconductor device (semiconductor chip).
[0024] The pentene copolymer is not particularly limited, but is preferably a copolymer of 4-methyl-1-pentene and an α-olefin, which has a glass transition temperature near room temperature, is excellent in stress relaxation properties, and has good flexibility due to the α-olefin as a copolymer component. Examples of the copolymer include "Absortomer (registered trademark) EP-1013" (a product name) manufactured by Mitsui Chemicals, Inc., which is a copolymer of 4-methyl-1-pentene and polypropylene, and "Absortomer (registered trademark) EP-1001" (a product name) manufactured by Mitsui Chemicals, Inc.
[0025] In addition, when a copolymer of 4-methyl-1-pentene and polypropylene is used, from the viewpoint of improving flexibility and stress relaxation properties, the content of polypropylene in the entire copolymer of 4-methyl-1-pentene and polypropylene is preferably 10 mol % or more and 30 mol % or less, based on 100 mol % of the copolymer of 4-methyl-1-pentene and polypropylene.
[0026] From the viewpoint of improving stress relaxation, the content of the pentene copolymer in the entire functional layer 2 is preferably 10% by mass or more and less than 50% by mass, with the functional layer being 100% by mass. If the content of the pentene copolymer is 50% by mass or more, the content of the 1-butene homopolymer that contributes to uniform elongation decreases, and the uniform elongation may decrease.
[0027] The content of the pentene copolymer in the entire functional layer 2 is preferably 10% by mass or more and 40% by mass or less, with the functional layer being 100% by mass.
[0028] <Olefin elastomer> In addition, in the base film 1 of the present invention, the functional layer 2 contains an olefin-based elastomer. The olefin-based elastomer is composed of an olefin-based material that conforms to the definition of the term elastomer in JIS K 6200. More specifically, a material composed of a copolymer of amorphous or low crystalline α-olefin corresponds to the olefin-based elastomer, one mainly made of polyethylene is called an ethylene-based elastomer, and one mainly made of polypropylene is called a propylene-based elastomer. For example, an example of an ethylene-based elastomer is the product name "Tafmer (registered trademark)" manufactured by Mitsui Chemicals, and an example of a propylene-based elastomer is the product name "Vistamax (registered trademark)" manufactured by ExxonMobil.
[0029] When a propylene-based elastomer is used, the content of polyethylene in the entire propylene-based elastomer is 9% or more and 30% or less, with the propylene-based elastomer being 100%, from the viewpoint of improving flexibility.
[0030] By using such an olefin-based elastomer, the crystallinity is reduced and the occurrence of a yield point can be suppressed, thereby improving the uniform extensibility of the base film.
[0031] From the viewpoint of improving uniform stretchability, the content of the olefin-based elastomer in the entire functional layer 2 is more than 0% by mass and less than 50% by mass, with respect to 100% by mass of the functional layer. If the content of the olefin-based elastomer is 50% by mass or more, the olefin-based elastomer component with low crystallinity becomes excessive, which may reduce rigidity and make it difficult to unwind the substrate and form it into a tape, including applying an adhesive.
[0032] The content of the olefin-based elastomer in the entire functional layer 2 is preferably 10% by mass or more and 30% by mass or less, based on 100% by mass of the functional layer.
[0033] From the viewpoint of further improving uniform elongation, the density of the olefin-based elastomer is 0.850 to 0.900 g / cm 3 It is preferable that the density is 0.860 to 0.890 g / cm 3 It is more preferable that:
[0034] Next, the surface layer 3 in the base film 1 of the present invention will be described. Examples of the surface layer 3 include those containing an antistatic agent and the above-mentioned 1-butene homopolymer or a polyolefin resin such as polyethylene or polypropylene.
[0035] Furthermore, despite its high molecular weight, the 1-butene homopolymer can be molded using a general-purpose extruder, and since the high molecular weight components give the film low surface adhesion, when used in a surface layer, it can suppress adhesion to transport rolls when the base film is transported, as well as suppress blocking when the base film is wound up and draw resonance when the base film is molded, thereby improving the processing stability of the base film.
[0036] In addition, from the viewpoint of suppressing surface adhesion, it is preferable that the content of 1-butene homopolymer in the entire surface layer 3 (i.e., each of the surface layers 3 laminated on both sides of the functional layer 2) is more than 0 mass% and not more than 30 mass% of 100 mass% of the surface layer.
[0037] In addition, examples of polypropylene include homopolymers and copolymers of polypropylene. Among these, the homopolymer of polypropylene is homopolypropylene obtained by polymerizing propylene alone, and this homopolymer of polypropylene has high stereoregularity and a high degree of crystallinity that contributes to the melting point, and therefore has excellent heat resistance. In addition, since the degree of crystallinity is high, the rigidity is high, but by mixing with linear low-density polyethylene described below, flexibility that contributes to the expandability of the base film can be obtained.
[0038] <Low density polyethylene> The surface layer 3 is made of a polyolefin resin having a density of 0.930 g / cm 3 It is preferred that the polyethylene comprises low density polyethylene (LDPE) having a density of 0.930 g / cm or less. 3 In the following cases, an excessive increase in crystallinity is suppressed and flexibility is improved, so that the isotropy of the base film can be improved. 3 If it is larger than , the degree of crystallinity increases excessively, which may reduce isotropy, and the rigidity becomes too large, which may reduce the pick-up ability of the semiconductor device and cause damage to the semiconductor device.
[0039] From the viewpoint of improving processing stability, the density of low-density polyethylene is 0.860 g / cm 3 It is preferable that the content is 0.880 g / cm or more. 3 More preferably, it is equal to or greater than this.
[0040] That is, the density is 0.860 g / cm 3 More than 0.93g / cm 3 The low-density polyethylene described below has low surface adhesion, and therefore, when used in a surface layer, can suppress adhesion to the transport roll when the base film is transported and can suppress blocking when the base film is wound up, thereby improving the processing stability of the base film.
[0041] In addition, from the viewpoint of suppressing surface adhesion, it is preferable that the ratio of the content of 1-butene homopolymer to the content of low-density polyethylene in the surface layer 3 (i.e., each of the surface layers 3 laminated on both sides of the functional layer 2) is 1-butene homopolymer:low-density polyethylene = 0:100 to 30:70.
[0042] Furthermore, among low-density polyethylenes, linear low-density polyethylene (LLDPE) has side-chain branches in the linear structure of high-density polyethylene, so compared to high-density polyethylene, its crystallinity is not too high and it has excellent flexibility.
[0043] From the viewpoint of strength, linear low-density polyethylene produced using a metallocene catalyst or a Ziegler catalyst may also be used.
[0044] The melt mass flow rate (MFR) of the linear low density polyethylene is preferably 0.5 to 7.5 g / 10 min, more preferably 1.0 to 6.0 g / 10 min, and even more preferably 2.0 to 5.0 g / 10 min. When the melt mass flow rate (MFR) is 0.5 g / 10 min or more, the molecular weight is not too large, and flexibility and processability can be improved, and when it is 7.5 g / 10 min or less, the molecular weight is not too small, and processing stability can be improved.
[0045] The melt mass flow rate is obtained by measurement in accordance with the standard of JIS K7210:1999.
[0046] From the above, the resin forming the base film has a density of 0.93 g / cm 3 By using a low density polyethylene having a density of 100 or less, the flexibility and isotropy of the base film can be improved.
[0047] In addition, from the viewpoint of suppressing surface adhesion, the content of low-density polyethylene in the entire surface layer 3 (i.e., each surface layer 3 laminated on both sides of the functional layer 2) is preferably 40 mass% or more and 90 mass% or less, out of 100 mass% of the surface layer.
[0048] <Antistatic agent> In the base film 1 of the present invention, from the viewpoint of imparting antistatic properties to the base film 1, the surface layer 3 contains an antistatic agent.
[0049] Examples of the antistatic agent include a block copolymer of a propylene-based resin and a polyhydric alcohol, a low molecular weight surfactant, a filler such as carbon black, etc. These antistatic agents may be used alone or in combination of two or more kinds.
[0050] Among these, from the viewpoint of imparting semi-permanent antistatic properties, it is preferable to use, as the antistatic agent, a block copolymer of a propylene-based resin and a polyhydric alcohol, which is a polymer-type antistatic agent.
[0051] The block copolymer of a propylene-based resin and a polyhydric alcohol is a block copolymer having a propylene polymer segment containing a structural unit derived from propylene and a polyhydric alcohol polymer segment containing a structural unit derived from a polyhydric alcohol.
[0052] This block copolymer of a propylene-based resin and a polyhydric alcohol has a structure in which the continuous phase (soft segment phase) of the polyether of the polyhydric alcohol contributes to the development of antistatic properties, and the hard segment phase of the propylene-based resin contributes to improving dispersibility in the resin forming the surface layer and the development of strength in the resin.
[0053] Examples of the propylene polymer segment include a homopolypropylene polymer segment obtained by polymerizing propylene alone, and a copolymer segment of propylene and an α-olefin.
[0054] Examples of the polyhydric alcohol constituting the polyhydric alcohol polymer segment include polyethylene glycol, ethylene glycol, diethylene glycol, 1,2-propanediol, 1,3-propanediol (trimethylene glycol), and polypropylene glycol.
[0055] In addition, examples of block copolymers of propylene-based resins and polyhydric alcohols that can be used include commercially available products such as Pelestat 230 (manufactured by Sanyo Chemical Industries, Ltd., a block copolymer having a propylene polymer segment and a polyethylene glycol segment) and Peletron PVL (manufactured by Sanyo Chemical Industries, Ltd., a block copolymer having a propylene polymer segment and a polyethylene glycol segment).
[0056] From the viewpoint of improving antistatic properties and rigidity, the content of the antistatic agent in the entire surface layer 3 (i.e., each of the surface layers 3 laminated on both sides of the functional layer 2) in the base film 1 of the present invention is more than 0 mass% and less than 40 mass% of 100 mass% of the surface layer. The content of the antistatic agent is preferably 5 mass% or more and 30 mass% or less, and more preferably 10 mass% or more and 30 mass% or less, of 100 mass% of the surface layer.
[0057] As described above, since the base film 1 of the present invention contains an antistatic agent in the surface layer 3, it is possible to prevent problems such as damage to wafer circuits in IC chips caused by static electricity, and therefore it is possible to improve wafer productivity.
[0058] <Base film> In the substrate film 1 of the present invention, the stress (at 20% elongation) in the mechanical axis (longitudinal) direction (hereinafter referred to as "MD") of the substrate film and the direction perpendicular thereto (hereinafter referred to as "TD") is preferably 6.5 MPa to 20 MPa, more preferably 7.5 MPa to 15 MPa, and even more preferably 8 MPa to 13 MPa. If the stress is greater than 20 MPa, the rigidity becomes too large, so that the pick-up ability of the semiconductor device decreases and the semiconductor device may be damaged, whereas if the stress is less than 6.5 MPa, the rigidity becomes low, so that in the manufacturing process of the substrate film, it becomes difficult to unwind the substrate and to form it into a tape, including coating with an adhesive.
[0059] In other words, when the stress (at 20% elongation) in MD and TD is 6.5 MPa or more and 20 MPa or less, a substrate film having excellent rigidity that can be unwound and made into a tape, including coating with an adhesive, can be provided in the substrate film manufacturing process.
[0060] Furthermore, in the case of conventional base films containing polyolefins, no necking occurs when the base film is stretched by 20%, allowing uniform expansion. However, once the base film is stretched by 40%, necking begins to occur, making uniform expansion difficult.
[0061] Therefore, from the viewpoint of improving the uniform extensibility of the base film, in the base film 1 of the present invention, the ratio of the stress (at 40% elongation) to the stress (at 20% elongation) in the MD and TD (i.e., the elongation percentage of the base film) is preferably from 0.95 to 2. If the elongation percentage of the base film is greater than 2, the expansion ring may become difficult to hold due to an excessive increase in stress, and if the elongation percentage of the base film is less than 0.95, necking may occur, making uniform expansion difficult.
[0062] That is, if the elongation percentage of the base film is 0.95 or more and 2 or less, necking does not occur and uniform expansion becomes possible.
[0063] The elongation percentage of the base film is more preferably 1.05 or more and 1.8 or less, and from the viewpoint of preventing necking and ensuring uniform expansion, the elongation percentage of the base film is even more preferably 1.1 or more and 1.7 or less.
[0064] In the base film 1 of the present invention, from the viewpoint of further improving the uniform extensibility of the base film, the ratio of stress (at 5% elongation) to stress (at 40% elongation) in MD and TD is preferably less than 1.05. If the ratio of stress (at 5% elongation) to stress (at 40% elongation) is less than 1.05, the occurrence of the later-described yield point (the yield point during the elongation rate from 0% to 100% under the condition of a tensile speed of 300 mm / min) can be suppressed, thereby suppressing the occurrence of necking and enabling uniform expansion.
[0065] It is more preferable that the ratio of the stress (at 5% elongation) to the stress (at 40% elongation) is 0.40 or more and less than 1.05, and from the viewpoint of preventing the occurrence of necking and ensuring uniform expansion, it is even more preferable that the ratio of the stress (at 5% elongation) to the stress (at 40% elongation) is 0.50 or more and less than 0.90.
[0066] In addition, the base film 1 of the present invention preferably has a stress relaxation rate of 25% or more, more preferably 30% or more, and even more preferably 35% or more. If the stress relaxation rate is less than 25%, the stress absorption performance is poor, and it may become difficult to maintain the dimensions of the tape for semiconductor production.
[0067] That is, when the stress relaxation rate is 25% or more, the dimensions of the tape for semiconductor production can be maintained, and a substrate film for a tape for semiconductor production having excellent stress relaxation properties can be provided.
[0068] The "stress relaxation rate" referred to here can be determined by the method described in the Examples section below.
[0069] In addition, from the viewpoint of suppressing the occurrence of sagging due to the isotropy of the base film during expansion, the ratio of the stress in MD (at 20% elongation) to the stress in TD (at 20% elongation) (i.e., the stress ratio of the base film at 20% elongation) is preferably 0.8 or more and 1.3 or less, more preferably 0.85 or more and 1.15 or less, and even more preferably 0.9 or more and 1.1 or less.
[0070] In addition, the substrate film 1 of the present invention has a surface resistivity of 1.00×10 13 It is preferable that the resistance is Ω / □ or less, and 1.00×10 11 More preferably, it is 1.00×10 10 It is more preferable that the surface resistivity is 1.00×10 13If it is larger than Ω / □, the static electricity carried by the base film may damage the wafer circuits in the IC chips when the wafer is diced.
[0071] That is, the surface resistivity is 1.00 x 10 13 When the resistance is Ω / □ or less, it is possible to prevent the inconvenience of damage to the wafer circuit in the IC chip due to static electricity.
[0072] The "surface resistivity" referred to here is obtained by measurement in accordance with the provisions of JIS K6911:2006, and can be determined by the method described in the Examples section below.
[0073] The thickness of the base film 1 of the present invention is preferably 50 to 300 μm, and more preferably 80 to 150 μm. If the thickness of the base film is 50 μm or more, the handleability is improved, and if the thickness is 300 μm or less, the flexibility (expandability) can be improved. In the case of a base film for a wafer, the thickness of the base film is preferably 50 to 150 μm, and more preferably 70 to 110 μm.
[0074] For example, in the case of a substrate film having a three-layer structure in which a surface layer / functional layer / surface layer are laminated in this order, the thickness of the surface layer is not particularly limited, but is preferably 2 to 60 μm, more preferably 4 to 40 μm, and the thickness of the functional layer is not particularly limited, but is preferably 40 to 120 μm, more preferably 50 to 80 μm.
[0075] For example, in the case of a base film having a three-layer structure in which surface layer / functional layer / surface layer are laminated in that order, from the viewpoints of processability and low cost, the ratio of the functional layer to the entire base film is preferably 40 to 95%, and more preferably 50 to 90%.
[0076] <Manufacturing method> For example, when producing a base film 1 having a three-layer structure in which a surface layer / functional layer / surface layer are laminated in this order as shown in Figure 1, first, a resin material for forming the surface layer and a resin material for forming the functional layer are prepared.
[0077] Next, a three-kind, three-layer co-extruder equipped with a T-die is used to simultaneously extrude and mold the resin material for forming the surface layer and the resin material for forming the functional layer at a predetermined temperature to produce the base film 1 having the multilayer structure of the present invention, which is composed of a laminate of the functional layer 2 and the surface layers 3 laminated on both sides of the functional layer 2. The base film of the present invention may also be produced by a known calendar method or inflation method.
[0078] <Other forms> The substrate film 1 of the present invention may contain various additives. As the additives, known additives that are usually used in semiconductor manufacturing tapes can be used, such as crosslinking aids, heat stabilizers, antioxidants, UV absorbers, lubricants, antiblocking agents, colorants, crystal nucleating agents, processing aids, etc. These additives may be used alone or in combination of two or more.
[0079] Furthermore, examples of the crosslinking aid include triallyl isocyanurate. When the base film contains a crosslinking aid, the content of the crosslinking aid in the base film is preferably 0.05 to 5 parts by mass, and more preferably 1 to 3 parts by mass, relative to 100 parts by mass of the resin forming the base film.
[0080] In addition, the above description has been given using as an example a substrate film having a three-layer structure in which surface layer / functional layer / surface layer is laminated in that order; however, the substrate film having a multilayer structure of the present invention is not limited to a three-layer structure as long as it has the above-mentioned functional layer, and may be, for example, a substrate film having a five-layer structure in which surface layer / functional layer / functional layer / functional layer / surface layer is laminated in that order. EXAMPLES
[0081] The present invention will be described below based on examples. Note that the present invention is not limited to these examples, and these examples can be modified or changed based on the spirit of the present invention, and they are not excluded from the scope of the present invention.
[0082] The materials used to prepare the base film are shown below. (1) LLDPE: Linear low-density polyethylene, melting point: 121°C, density: 0.922g / cm 3 , MFR: 1.6g / 10min (2) 1-Bu: homopolymer of 1-butene, melting point: 128°C, density: 0.920g / cm 3 , MFR: 0.5g / 10min (3) Antistatic agent 1: Block copolymer having a propylene polymer segment and a polyethylene glycol segment, melting point: 135°C, density: 1.1 g / cm 3 , MFR: 15.0g / 10min (4) Antistatic agent 2: Block copolymer having a propylene polymer segment and a polyethylene glycol segment, melting point: 163°C, density: 1.1 g / cm 3 , MFR: 12.0g / 10min (5) Antistatic agent 3: Block copolymer having a propylene polymer segment and a polyethylene glycol segment, melting point: 150°C, density: 1.1 g / cm 3 , MFR: 8.0g / 10min, (Sanyo Chemical Industries, Ltd., product name: Pelektron PVH) (6) PP elastomer: propylene-based elastomer, density: 0.862 g / cm 3 , MFR: 3.0 g / 10 min (230° C.), polyethylene content: 16% (manufactured by Exxon Mobil Corporation, product name: Vistamax (registered trademark) 6102FL) (7) Pentene copolymer: copolymer of 4-methyl-1-pentene and polypropylene, melting point: 130°C, density: 0.838g / cm 3 , MFR: 10.0g / 10min, 4-methyl-1-pentene content 85mol%, polypropylene content 15mol% (8) EVA: Ethylene-vinyl acetate copolymer, melting point: 100°C, density: 0.925g / cm 3 , MFR: 2.5g / 10min (Tosoh Corporation, product name: Ultrasen 515)
[0083] Example 1 <Production of Base Film> First, each material shown in Table 1 was blended to prepare a resin material for forming a surface layer and a resin material for forming a functional layer having the compositions (parts by mass) shown in Table 1.
[0084] Next, using a co-extrusion machine for three-layer with a T-die, the resin material for forming a surface layer and the resin material for forming a functional layer were simultaneously extruded and molded under the conditions that the die temperature was 180 to 230 °C and the chill roll temperature was 30 °C, thereby obtaining a base film having the thickness shown in Table 1 and having a three-layer structure laminated in the order of surface layer / functional layer / surface layer.
[0085] <Evaluation of Presence or Absence of Yield Point> Using the produced base film, in accordance with JIS K7161-2:2014, a sample for measurement was obtained. Next, the obtained sample for measurement was set in a tensile testing machine (manufactured by Shimadzu Corporation, product name: AG-5000A) so that the distance between the gripping tools was 40 mm, and in accordance with JIS K7161-2:2014, a tensile test was conducted at a tensile speed of 300 mm / min in an environment where the temperature was 23 °C and the relative humidity was 40%.
[0086] Then, in the S-S curves (stress-strain curves) in MD and TD, those in which no yield point was confirmed during the elongation from an elongation ratio of 0% to 100% (no necking occurred and uniform expansion was surely possible) were rated as ◎, those in which almost no yield point was confirmed during the elongation from an elongation ratio of 0% to 100% (occurrence of necking was suppressed and almost uniform expansion was possible) were rated as 〇, and those in which a yield point was confirmed (necking occurred and uniform expansion was impossible) were rated as ×. The above results are shown in Table 1.
[0087] <Measurement of Stress in MD and TD> Using the prepared base film, a measurement sample was obtained in accordance with JIS K7161-2: 2014. Next, the obtained measurement sample was set in a tensile tester (manufactured by Shimadzu Corporation, product name: AG-5000A) so that the distance between the grippers was 40 mm, and a tensile test was performed in accordance with JIS K7161-2: 2014 at a temperature of 23°C and a relative humidity of 40% at a tensile speed of 300 mm / min.
[0088] The stress (20% stress) at 20% elongation in the MD and TD of the substrate film was measured, and the ratio of the stress (at 20% elongation) in the MD to the stress (at 20% elongation) in the TD (i.e., the stress ratio of the substrate film at 20% elongation) was calculated. The results are shown in Table 1.
[0089] Similarly, the stress at 40% elongation (40% stress) was measured in the MD and TD of the substrate film, and the ratio of the stress (at 40% elongation) to the stress (at 20% elongation) in the MD (i.e., the elongation rate of the substrate film in the MD) and the ratio of the stress (at 40% elongation) to the stress (at 20% elongation) in the TD (i.e., the elongation rate of the substrate film in the TD) were calculated. The results are shown in Table 1.
[0090] Similarly, the stress at 5% elongation (5% stress) was measured in the MD and TD of the substrate film, and the ratio of the stress (at 5% elongation) to the stress (at 40% elongation) in the MD and the ratio of the stress (at 5% elongation) to the stress (at 40% elongation) in the TD were calculated. The results are shown in Table 1.
[0091] <Calculation of stress relaxation rate> Using the prepared base film, a measurement sample having a No. 1 dumbbell shape (width 10 mm, length 120 mm) was obtained. Next, the obtained measurement sample was set in a tensile tester (manufactured by Shimadzu Corporation, product name: AG-5000A) so that the distance between the grippers was 80 mm, and the sample was stretched by 25% in the MD (or TD) at a tensile speed of 300 mm / min in an environment of a temperature of 23°C and a relative humidity of 40%.
[0092] The stress (initial stress S0) was measured when the specimen was stretched by 25%, and the specimen was held stretched for 60 seconds, after which the stress (stress after relaxation S1) was measured. The stress relaxation rate [%] of the substrate film in MD and TD was calculated from the difference between the initial stress S0 and the stress after relaxation S1 using the following formula (1). The results are shown in Table 1.
[0093] [Number 1] Stress relaxation rate [%] = [(initial stress S0 - stress after relaxation S1) / initial stress S0] × 100 (1)
[0094] <Measurement of surface resistivity> The surface resistivity of the prepared substrate film was measured in accordance with the provisions of JIS K6911:2006. More specifically, first, a measurement sample of A4 size (width 210 mm, length 297 mm) was obtained using the prepared substrate film. Next, the surface resistivity of the obtained measurement sample was measured using a high resistivity meter (manufactured by Nitto Seiko Analytech Co., Ltd., product name: Hiresta UX). In addition, with the probe pressed against the sample, an applied voltage of 1000 V was applied, and the surface resistivity was measured when the voltage was held for 10 seconds. The above results are shown in Table 1.
[0095] (Examples 2 to 9, Comparative Examples 2 to 4) Except for changing the composition of the resin component to the composition (parts by mass) shown in Tables 1 and 2, a substrate film having the thickness shown in Tables 1 and 2 and a three-layer structure laminated in the order of surface layer / functional layer / surface layer was produced in the same manner as in Example 1 described above.
[0096] Then, the presence or absence of a yield point was evaluated, the stress in MD and TD was measured, the stress relaxation rate was calculated, and the surface resistivity was measured in the same manner as in Example 1. The results are shown in Tables 1 and 2.
[0097] Comparative Example 1 First, the materials shown in Table 2 were blended to prepare a resin material for forming a surface layer having the composition (parts by mass) shown in Table 2.
[0098] Next, using a three-type, three-layer co-extruder equipped with a T-die, the resin material for forming the surface layer was extruded and molded under conditions of a die temperature of 180 to 230°C and a chill roll temperature of 30°C, thereby obtaining a substrate film having the thickness shown in Table 2 and a single-layer structure consisting of only the surface layer.
[0099] Then, the presence or absence of a yield point was evaluated, the stress in MD and TD was measured, the stress relaxation rate was calculated, and the surface resistivity was measured in the same manner as in Example 1. The results are shown in Tables 1 and 2.
[0100] [Table 1]
[0101] [Table 2]
[0102] As shown in Table 1, in the substrate films of Examples 1 to 9 in which the functional layer contains a 1-butene homopolymer, a pentene copolymer, and an olefin-based elastomer, and the content of the olefin-based elastomer in the entire functional layer is more than 0% by mass and less than 50% by mass (20% by mass or more and 30% by mass or less), the stress in MD and TD (at 20% elongation) is 6.5 MPa or more and 20 MPa or less, and therefore the rigidity is excellent. In addition, the stress relaxation rate is 25% or more, and therefore the stress relaxation property is excellent.
[0103] Furthermore, as shown in Table 1, in the substrate films of Examples 1 to 9 in which the surface layer includes an antistatic layer and the content of the antistatic agent in the entire surface layer is more than 0 mass% and less than 40 mass% (5 mass% or more and 25 mass% or less), the surface resistivity is 1.00 × 10 13 Since the resistance is Ω / □ or less, it is clear that the antistatic properties are excellent.
[0104] On the other hand, as shown in Table 2, in the substrate film of Comparative Example 1, since the functional layer does not contain a 1-butene homopolymer, a pentene copolymer, and an olefin-based elastomer, the stress in MD and TD (at 20% elongation) is less than 6.5 MPa, indicating poor rigidity. In addition, the stress relaxation rate is less than 25%, indicating poor stress relaxation property.
[0105] Furthermore, as shown in Table 2, in the base film of Comparative Example 2, the content of the antistatic agent in the entire surface layer was 40 mass %, and the content of the soft antistatic agent was excessively large, so that the stress in TD (at 20% elongation) was less than 6.5 MPa, indicating poor rigidity.
[0106] Furthermore, as shown in Table 2, in the base film of Comparative Example 3, the content of the olefin-based elastomer in the entire functional layer was 50 mass %, so the stress in MD and TD (at 20% elongation) was less than 6.5 MPa, indicating poor rigidity.
[0107] As shown in Table 2, the substrate film of Comparative Example 4 did not contain an antistatic agent in the surface layer, and therefore the surface resistivity was 1.00×10 13 It is found that the antistatic property is poor because the value is larger than Ω / □. [Industrial Applicability]
[0108] As described above, the present invention is suitable for use as a base film for a tape for manufacturing semiconductors. [Explanation of symbols]
[0109] 1. Base film 2. Functional Layer 3 Surface layer
Claims
1. A substrate film for a semiconductor manufacturing tape having a functional layer and a surface layer provided on at least one side of the functional layer, the functional layer comprises a homopolymer of 1-butene, a copolymer of pentene, and an olefin-based elastomer; the surface layer comprises an antistatic agent; The content of the olefin-based elastomer in the entire functional layer is more than 0 mass% and less than 50 mass%, The content of the antistatic agent in the entire surface layer is more than 0 mass % and less than 40 mass %.
1. A substrate film for a tape for semiconductor manufacturing.
2. 2. The substrate film for a tape for semiconductor manufacturing according to claim 1, wherein the antistatic agent is a block copolymer of a propylene-based resin and a polyhydric alcohol.
3. 3. The substrate film for a tape for manufacturing semiconductor devices according to claim 1, wherein the antistatic agent is a block copolymer of polypropylene and polyethylene glycol.
4. 2. The substrate film for a tape for semiconductor manufacturing according to claim 1, wherein the olefin-based elastomer is a propylene-based elastomer.
5. The surface layer has a density of 0.93 g / cm 3 2. The substrate film for a tape for semiconductor manufacturing according to claim 1, further comprising at least a low-density polyethylene having a density of 100% or less.
6. 2. The substrate film for a semiconductor manufacturing tape according to claim 1, wherein the surface layer contains a homopolymer of 1-butene.
Citation Information
Patent Citations
Surface protective film
JP2015034215A
Base material film for dicing film and dicing film
JP2016162787A
Dicing substrate film
JP2022051746A
Work-machining sheet
JP2022158902A
Laminate film and film roll
WO2021193223A1
Cited By
Antistatic resin composition, resin film, and antistatic substrate film for dicing tape
JP7796658B2
Antistatic resin composition, resin film, and base film for antistatic dicing tape
JPWO2022064949A1
Polyolefin resin film
WO2026168129A1