Resin composition and molded product
The resin composition of polyphenylene ether and polyolefin addresses the low adhesion and heat resistance issues of polyolefins by enhancing fluidity and adhesion to metal surfaces, suitable for applications involving substrates and circuits.
Patent Information
- Application Number
- JP2023072723
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polyolefins have low glass transition temperature and poor adhesion to metals, which limits their use in applications requiring heat resistance and durability, especially in forms that come into contact with metal substrates and circuits.
A resin composition comprising polyphenylene ether and polyolefin, with specific solubility and glass transition temperature properties, enhances adhesion and maintains fluidity by optimizing the content ratio and structural components of polyphenylene ether.
The resin composition maintains fluidity while improving adhesion to metal surfaces, ensuring suitable workability and durability in applications like covers and cover films for substrates and circuits.
Smart Images

Figure 2024157987000001 
Figure 2024157987000002 
Figure 2024157987000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition and a molded article. [Background technology]
[0002] Polyolefin is an inexpensive plastic material used in a wide variety of applications. It has excellent processability. It also excels in electrical insulation, chemical resistance, and low water absorption. For example, it is used in a wide variety of applications, including packaging films, packaging materials, cable insulation, bottles, toys, and automotive interior and exterior parts.
[0003] However, polyolefins have a low glass transition temperature and are therefore insufficient for applications requiring heat resistance.In addition, although the use of inorganic fillers to improve heat resistance is widely known, the use of inorganic fillers reduces fluidity and adversely affects processability. Therefore, Patent Document 1 discloses a technology in which polyphenylene ether is added to a polyolefin such as polyethylene to improve heat distortion resistance, flexural modulus, and flame retardancy while maintaining fluidity compared to the addition of an inorganic filler. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2017-500417 Summary of the Invention [Problem to be solved by the invention]
[0005] For example, in the case of a cover or cover film that comes into contact with metal used in a circuit board or circuit, it is required that the resin does not peel off from the metal side in order to obtain favorable workability during reuse. As described above, Patent Document 1 discloses that adding polyphenylene ether to polyolefin can improve heat distortion resistance, flexural modulus, and flame retardancy while maintaining fluidity. However, even with the technology described in Patent Document 1, it was necessary to further improve adhesion to metals.
[0006] Therefore, an object of the present invention is to provide a resin composition containing polyphenylene ether and polyolefin, which maintains fluidity and has excellent resin adhesion. [Means for solving the problem]
[0007] Means for Solving the Problems of the Prior Art The present inventors have conducted intensive research to solve the problems of the prior art described above, and as a result have found that by combining a polyphenylene ether having a specific structure with a polyolefin in a specific ratio, the solubility in n-hexane at 25°C can be increased, thereby solving the problems of the prior art described above, and have thus completed the present invention.
[0008] That is, the present invention is as follows. [1] A resin composition comprising a polyphenylene ether (A) and a polyolefin (B), a content ratio of the polyphenylene ether (A) relative to the total amount of the polyphenylene ether (A) and the polyolefin (B) is 0.1 to 30.0 mass%, and a content ratio of the polyolefin (B) is 70 to 99.9 mass%, A resin composition, characterized in that the polyphenylene ether (A) has a solubility in n-hexane at 25°C of 5 mass% or more. [2] The resin composition according to [1] above, wherein the polyphenylene ether (A) has a glass transition temperature of 100 to 180°C. [3] The resin composition according to [1] or [2] above, wherein the polyphenylene ether (A) has a partial structure represented by the following formula (3): [ka] (In formula (3), R 31 each independently represents an optionally substituted linear alkyl group having 1 to 8 carbon atoms or two R 31 is a cyclic alkyl structure having 1 to 8 carbon atoms, R 32 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 33 is a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, or an optionally substituted phenyl group. [4] The polyphenylene ether (A) contains a repeating unit derived from a phenol represented by the following formula (1) and a repeating unit derived from a phenol represented by the following formula (2): the content ratio of the repeating unit derived from phenol of the formula (1) is 5 to 89 mol %, and the content ratio of the repeating unit derived from phenol of the formula (2) is 11 to 95 mol %, relative to 100 mol % in total of the repeating units derived from phenol of the formula (1); The resin composition according to any one of the above [1] to [3], characterized in that the reduced viscosity (ηsp / c) measured in a chloroform solution having a concentration of 0.5 g / dL at 30°C is 0.03 to 0.30 dL / g. [ka] (In formula (1), R 11 each independently represents an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; R 12 are each independently a hydrogen atom, an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom. [ka] (In formula (2), R 22 are each independently a hydrogen atom, an optionally substituted saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom, and two R22 are not both hydrogen atoms, R 21 is a partial structure represented by the following formula (3). [ka] In formula (3), R31 each independently represents a linear alkyl group having 1 to 8 carbon atoms which may be substituted, or two R 31 is a cyclic alkyl structure having 1 to 8 carbon atoms, R 32 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 33 is a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, or an optionally substituted phenyl group. [5] The resin composition according to any one of the above [1] to [4], wherein the partial structure represented by the formula (3) is a tert-butyl group. [6] The resin composition according to any one of the above [1] to [5], wherein the polyolefin (B) is polypropylene (B1). [7] A molded article comprising the resin composition according to any one of [1] to [6] above. Effect of the Invention
[0009] According to the present invention, it is possible to provide a resin composition which maintains fluidity and has improved adhesion to resins. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention (hereinafter simply referred to as "the present embodiment") will be described in detail. The following embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be implemented in various modifications within the scope of the gist thereof.
[0011] In this embodiment, the structural units constituting the copolymer are referred to as "monomer units", and when describing the polymer material, the "unit" is omitted and it is simply described as "monomer".
[0012] [Resin composition] The resin composition of the present embodiment is a resin composition containing a polyphenylene ether (A) and a polyolefin (B). In the present embodiment, the content of the polyphenylene ether (A) is 0.1 to 30.0 mass% and the content of the polyolefin (B) is 70 to 99.9 mass% relative to the total amount of the polyphenylene ether (A) and the polyolefin (B), The polyphenylene ether (A) has a solubility in n-hexane at 25° C. of 5% by mass or more.
[0013] <Polyphenylene ether (A)> The polyphenylene ether (A) has a solubility in n-hexane at 25° C. of 5% by mass or more. The higher the solubility of the polyphenylene ether (A) in n-hexane at 25° C., the higher the affinity and compatibility with hydrocarbon solvents and hydrocarbon resins. As a result, the resin composition of the present embodiment maintains fluidity while improving the adhesion of the resin. From the same viewpoint, the solubility of the polyphenylene ether (A) in n-hexane at 25° C. is preferably 5% by mass or more in solid content concentration, more preferably 10% by mass or more in solid content concentration, and even more preferably 20% by mass or more in solid content concentration.
[0014] The solubility of the polyphenylene ether (A) in n-hexane at 25° C. can be improved by decreasing the molecular weight of the polyphenylene ether (A) and by introducing a branched substituent or a long-chain alkyl group containing a tertiary carbon.
[0015] The glass transition temperature of the polyphenylene ether (A) is preferably 100 to 180° C. From the viewpoint of processability in extrusion processing of the polyolefin, it is preferably 180° C. or lower, more preferably 170° C. or lower, and even more preferably 160° C. or lower. From the viewpoint of further increasing the softening point of the resin composition, it is preferably 100° C. or higher, more preferably 110° C. or higher, and even more preferably 120° C. or higher.
[0016] From the viewpoint of improving the solubility in n-hexane at 25° C., the polyphenylene ether (A) preferably has a partial structure represented by formula (3). [ka] (In formula (3), R 31 each independently represents an optionally substituted linear alkyl group having 1 to 8 carbon atoms or two R 31 is a cyclic alkyl structure having 1 to 8 carbon atoms, R 32 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 33 is a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, or an optionally substituted phenyl group.
[0017] The partial structure represented by the above formula (3) is preferably a group containing secondary and / or tertiary carbon, such as an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a tert-amyl group, a 2,2-dimethylpropyl group, a cyclohexyl group, or a structure having a phenyl group at the end of these groups, etc. From the viewpoint of adjusting the glass transition temperature of the polyphenylene ether to a range of 100 to 180°C while improving the solubility in n-hexane at 25°C, a tert-butyl group or a cyclohexyl group is more preferable, and a tert-butyl group is even more preferable. In addition, the above R 31 The substituent in the linear alkyl group having 1 to 8 carbon atoms, 32and the substituent in the alkylene group having 1 to 8 carbon atoms, 33 Examples of the substituent in the alkyl group having 1 to 8 carbon atoms and the phenyl group include a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and a halogen atom.
[0018] The polyphenylene ether (A) may contain a repeating unit derived from a phenol of the following formula (1) and a repeating unit derived from a phenol of the following formula (2), and the repeating units in the compound may consist only of the repeating units derived from a phenol of the following formula (1) and the repeating units derived from a phenol of the following formula (2). [ka] (In formula (1), R 11 each independently represents an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; R 12 are each independently a hydrogen atom, an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom.
[0019] In the above formula (1), R 11 are each independently preferably a saturated hydrocarbon group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms, and from the viewpoint of adjusting the glass transition temperature of the polyphenylene ether (A) to the range of 100 to 180° C. and improving the solubility in n-hexane at 25° C., more preferably a methyl group or a phenyl group, and further preferably a methyl group. 11 Preferably, both have the same structure. Above R 11 Examples of the substituent in the saturated hydrocarbon group having 1 to 6 carbon atoms and the aryl group having 6 to 12 carbon atoms include a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and a halogen atom.
[0020] In the above formula (1), R 12are each independently preferably a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, more preferably a hydrogen atom or a methyl group. 12 are preferably different, and from the viewpoint of adjusting the glass transition temperature of the polyphenylene ether (A) to the range of 100 to 180°C while improving the solubility in n-hexane at 25°C, it is more preferable that one is a hydrogen atom and the other is a hydrocarbon group having 1 to 6 carbon atoms (preferably a methyl group). Above R 12 Examples of the substituent in the hydrocarbon group having 1 to 6 carbon atoms and the aryl group having 6 to 12 carbon atoms include a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and a halogen atom.
[0021] [ka] (In formula (2), R 22 are each independently a hydrogen atom, an optionally substituted saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom, and two R 22 are not both hydrogen atoms, R 21 is a partial structure represented by the above formula (3).
[0022] In the above formula (2), R 22 are preferably each independently a hydrogen atom, a saturated or unsaturated hydrocarbon group having 1 to 15 carbon atoms, or an aryl group having 6 to 12 carbon atoms which may be substituted with an alkyl group having 1 to 6 carbon atoms, and from the viewpoint of adjusting the glass transition temperature of the polyphenylene ether (A) to the range of 100 to 180°C while improving the solubility in n-hexane at 25°C, are more preferably a hydrogen atom, a hydrocarbon group having 1 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms which may be substituted with an alkyl group having 1 to 6 carbon atoms, and are further preferably a hydrogen atom or a methyl group. 22 are preferably different, and it is more preferable that one is a hydrogen atom and the other is a hydrocarbon group having 1 to 6 carbon atoms (preferably a methyl group). Above R22 Examples of the substituent in the saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms and the aryl group having 6 to 12 carbon atoms include a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and a halogen atom.
[0023] In this embodiment, the polyphenylene ether (A) can be analyzed by techniques such as NMR and mass spectrometry to identify its structure. A specific method for identifying the structure of the polyphenylene ether is to carry out field desorption mass spectrometry (FD-MS), which is known to be less prone to fragmentation, and to estimate the repeating units based on the intervals between the detected ions. In addition, there is a method for estimating the structure of the polyphenylene ether by combining peak analysis of fragment ions by electron ionization (EI) and structural analysis by NMR.
[0024] In addition, in the polyphenylene ether (A), the content of the repeating unit derived from phenol of the formula (1) is preferably 5 to 89 mol % and the content of the repeating unit derived from phenol of the formula (2) is preferably 11 to 95 mol % relative to 100 mol % in total of the repeating unit derived from phenol of the formula (1) and the repeating unit derived from phenol of the formula (2). From the viewpoint of obtaining excellent heat resistance and balance of properties of the resin composition, the repeating unit derived from the phenol of the above formula (2) is preferably 18 mol % or more, more preferably 20 mol % or more. From the same viewpoint, the repeating unit derived from the phenol of the above formula (1) is preferably 82 mol % or less, more preferably 80 mol % or less. The repeating unit derived from the phenol of formula (1) contained in the polyphenylene ether (A) may be of one type or of multiple types, and the repeating unit derived from the phenol of formula (2) contained in the polyphenylene ether may be of one type or of multiple types.
[0025] Furthermore, relative to 100 mol % of monomer units contained in the polyphenylene ether (A) (e.g., all monomer units derived from phenol contained in the polyphenylene ether), the total amount of repeating units derived from phenol of the above formula (1) and repeating units derived from phenol of the above formula (2) is preferably 75 mol % or more, more preferably 90 mol % or more, and even more preferably 95 mol % or more.
[0026] The ratio of the repeating unit derived from the phenol of the above formula (1) to the repeating unit derived from the phenol of the above formula (2) is, for example, 1 H NMR, 13 It can be determined using an analytical technique such as C NMR, and more specifically, it can be measured by the method described in the Examples below.
[0027] Since the phenol of the above formula (1) does not have an unsubstituted ortho position (i.e., since no hydrogen atoms are bonded to the carbon atoms at the two ortho positions of the carbon atom to which the hydroxyl group is bonded), it can react with another phenolic monomer only at the carbon atom at the para position to the phenolic hydroxyl group. Therefore, the repeating unit derived from formula (1) includes a repeating unit having the structure of the following formula (8). [ka] (In formula (8), R 11 and R 12 is the same as equation (1).
[0028] In addition to the phenolic hydroxyl group, the phenol of formula (2) can react with another phenolic monomer at either the ortho or para position of the phenol. Thus, the repeat unit derived from the phenol of formula (2) has a monomer unit of formula (9), formula (10), or a combination thereof: [ka] [ka] (R in Equation (9) and Equation (10) 21 , R 22 is the same as equation (2).
[0029] The reduced viscosity of the polyphenylene ether measured in a chloroform solution having a concentration of 0.5 g / dL at 30° C. is preferably 0.03 to 0.30 dL / g, and more preferably 0.06 to 0.30 dL / g, from the viewpoint of obtaining an excellent heat resistance and balance of properties of the resin composition. The reduced viscosity of the polyphenylene ether can be measured by the method described in the Examples section below.
[0030] The polyphenylene ether (A) in the present embodiment may contain, in addition to the phenol of the formula (1) and the phenol of the formula (2), a terpolymer containing a structure derived from a dihydric phenol of the following formula (11) as an impurity (sometimes simply referred to as "impurity A" in this specification). The polyphenylene ether (A) may be a mixture of the polyphenylene ether and the impurity A. The molar ratio of the impurity A to 100 mol % of the polyphenylene ether is preferably 10 mol % or less, and more preferably 5 mol % or less. [ka] (In formula (11), R 11 and R 12 is the same as formula (1). z is 0 or 1, and Y is the following structure: [ka] (In the formula, R 41 each independently represents any one of an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, and a halogen atom) )
[0031] The impurity A can be synthesized, for example, as a terpolymer containing a structure derived from a dihydric phenol, where z=0 in formula (11), by reacting the following formula (12), which is generated as a by-product during the oxidative polymerization of a monohydric phenol, with a polyphenylene ether composed of a monohydric phenol. [ka] (In formula (12), R 11 and R 12 is the same as equation (1).
[0032] The polyphenylene ether (A) may be a modified polyphenylene ether in which a hydroxyl group contained in the polyphenylene ether is modified to a functional group (for example, a functional group containing an unsaturated carbon bond).
[0033] The polyphenylene ether (A) may have at least one partial structure selected from the group consisting of the following formulas (4), (5), (6) and (7). [ka] [ka] [ka] (In formula (6), R 6 is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon is R 6 may have a substituent within the range of a total carbon number of 1 to 10.) [ka] (In formula (7), R 7 is a saturated or unsaturated divalent hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated divalent hydrocarbon is R 7 may have a substituent within a range in which the total carbon number of R is 1 to 10; 8is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon is R 8 may have a substituent within the range of a total carbon number of 1 to 10.)
[0034] At least one partial structure selected from the group consisting of formula (4), formula (5), formula (6), and formula (7) may be directly bonded to a hydroxyl group contained in the polyphenylene ether.
[0035] The respective ratios of the repeating units derived from phenol of formula (1) and the repeating units derived from phenol of formula (2) contained in the modified polyphenylene ether into which at least one partial structure represented by the group consisting of the above formulas (4), (5), (6), and (7) has been introduced are, for example, 1 H NMR, 13 It can be determined using analytical techniques such as C NMR.
[0036] <Production method of polyphenylene ether> The polyphenylene ether (A) can be obtained, for example, by a method including at least a step of oxidatively polymerizing a monohydric phenol compound represented by the above formula (1) or formula (2). The step of oxidatively polymerizing the above is preferably performed by oxidatively polymerizing a raw material including at least the phenol of the above formula (1) and the phenol of the above formula (2).
[0037] Examples of the monohydric phenol compound represented by the above formula (1) include 2,6-dimethylphenol, 2-methyl-6-ethylphenol, 2,6-diethylphenol, 2-ethyl-6-n-propylphenol, 2-methyl-6-chlorophenol, 2-methyl-6-bromophenol, 2-methyl-6-n-propylphenol, 2-ethyl-6-bromophenol, 2-methyl-6-n-butylphenol, 2,6-di-n-propylphenol, 2-ethyl-6-chlorophenol, 2-methyl-6-phenylphenol, 2,6-diphenylphenol, 2-methyl-6-tolylphenol, 2,6-ditolylphenol, 2,3,6-trimethylphenol, 2,3-diethyl-6-n-propylphenol, 2,3,6-tributylphenol, 2,6-di-n-butyl-3-methylphenol, 2,6-dimethyl-3-n-butylphenol, and 2,6-dimethyl-3-tert-butylphenol. Among these, 2,6-dimethylphenol, 2,3,6-trimethylphenol, and 2,6-diphenylphenol are particularly preferable since they are inexpensive and easily available. The monohydric phenol compound represented by the above formula (1) may be used alone or in combination of two or more kinds.
[0038] Examples of the monohydric phenol compound represented by the above formula (2) include 2-isopropyl-5-methylphenol, 2-cyclohexyl-5-methylphenol, 2-tert-butyl-5-methylphenol, 2-isobutyl-5-methylphenol, etc. From the viewpoint of suppressing multi-branching and gelation, 2-tert-butyl-5-methylphenol and 2-cyclohexyl-5-methylphenol, which are bulky substituents, are more preferred. The monohydric phenol compound represented by the above formula (2) may be used alone or in combination of two or more kinds.
[0039] Normally, in the oxidative polymerization of phenols having a hydrogen atom at the ortho position (e.g., 2-methylphenol, 2,5-dimethylphenol, 2-phenylphenol), ether bonds can also be formed at the ortho position, making it difficult to control the bonding position of the phenol compound during oxidative polymerization. As a result, a high molecular weight polymer is obtained that is polymerized in a branched manner with an average of 3 or more hydroxyl groups per molecule, and ultimately a gel component that is insoluble in solvents is generated. On the other hand, when a phenol having a bulky substituent at the ortho-position on one side, as represented by the above formula (2), is used, it is possible to control the bonding position of the phenol compound during oxidative polymerization, despite the presence of a hydrogen atom at the ortho-position on the opposite side, and a polyphenylene ether having an average of less than 2.5 hydroxyl groups per molecule can be obtained.
[0040] The molecular weight of the polyphenylene ether (A) can be adjusted by the molar ratio of the repeating unit derived from the above formula (2) to the sum of the repeating unit derived from the above formula (1) and the repeating unit derived from the above formula (2). That is, when the molar ratio of the repeating unit derived from the above formula (2) is high, the molecular weight (reduced viscosity) can be lowered, and when the molar ratio of the repeating unit derived from the above formula (2) is low, the molecular weight (reduced viscosity) can be adjusted to be high. Although the reason is not clear, it is presumed that the bulky substitution at the ortho position of the above formula (2) suppresses the increase in molecular weight.
[0041] (Oxidative polymerization process) In the method for producing the polyphenylene ether (A), an aromatic solvent, which is a good solvent for polyphenylene ether, can be used as the polymerization solvent in the oxidative polymerization step. Here, a good solvent for polyphenylene ether is a solvent capable of dissolving polyphenylene ether. Examples of such solvents include aromatic hydrocarbons such as benzene, toluene, xylene (including o-, m-, and p-isomers) and ethylbenzene; halogenated hydrocarbons such as chlorobenzene and dichlorobenzene; and nitro compounds such as nitrobenzene.
[0042] The polymerization catalyst used may be a known catalyst system that can be generally used for the production of polyphenylene ether.Generally known catalyst systems include those that are composed of a transition metal ion having redox ability and an amine compound that can form a complex with the transition metal ion, such as a catalyst system composed of a copper compound and an amine compound, a catalyst system composed of a manganese compound and an amine compound, or a catalyst system composed of a cobalt compound and an amine compound.Since the polymerization reaction proceeds efficiently under slightly alkaline conditions, a small amount of alkali or an additional amine compound may be added thereto.
[0043] A polymerization catalyst that is preferably used is a catalyst comprising a copper compound, a halogen compound and an amine compound as catalyst components, and more preferably a catalyst containing a diamine compound represented by the following formula (13) as the amine compound. [ka] (In formula (13), R 14 , R 15 , R 16 , R 17 are each independently a hydrogen atom or a linear or branched alkyl group having 1 to 6 carbon atoms, but are not all hydrogen atoms at the same time. 18 is a linear or methyl-branched alkylene group having 2 to 5 carbon atoms.
[0044] Examples of the copper compound of the catalyst component described herein are listed below. Suitable copper compounds include cuprous compounds, cupric compounds, and mixtures thereof. Examples of cupric compounds include, for example, cupric chloride, cupric bromide, cupric sulfate, and cupric nitrate. Examples of cuprous compounds include, for example, cuprous chloride, cuprous bromide, cuprous sulfate, and cuprous nitrate. Particularly preferred metal compounds among these are cuprous chloride, cupric chloride, cuprous bromide, and cupric bromide. These copper salts may be synthesized at the time of use from oxides (e.g., cuprous oxide), carbonates, hydroxides, and the like and corresponding halogens or acids. A method that is often used is to mix the cuprous oxide exemplified above with hydrogen halide (or a solution of hydrogen halide) to prepare the copper salt.
[0045] Examples of halogen compounds include hydrogen chloride, hydrogen bromide, hydrogen iodide, sodium chloride, sodium bromide, sodium iodide, potassium chloride, potassium bromide, potassium iodide, tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium iodide, tetraethylammonium chloride, tetraethylammonium bromide, and tetraethylammonium iodide. These compounds can be used as aqueous solutions or solutions using appropriate solvents. These halogen compounds can be used alone as components, or in combination of two or more. Preferred halogen compounds are aqueous solutions of hydrogen chloride and hydrogen bromide.
[0046] The amount of these compounds used is not particularly limited, but is preferably 2 to 20 times the molar amount of halogen atoms relative to the molar amount of copper atoms, and the amount of copper atoms used is preferably in the range of 0.02 to 0.6 moles per 100 moles of the phenol compound added to the polymerization reaction.
[0047] Next, examples of the diamine compound of the catalyst component are listed below. For example, N,N,N',N'-tetramethylethylenediamine, N,N,N'-trimethylethylenediamine, N,N'-dimethylethylenediamine, N,N-dimethylethylenediamine, N-methylethylenediamine, N,N,N',N'-tetraethylethylenediamine, N,N,N'-triethylethylenediamine, N,N'-diethylethylenediamine, N,N-diethylethylenediamine, N-ethylethylenediamine, N,N-dimethyl-N'-ethylethylenediamine, N,N'-dimethyl-N-ethylethylenediamine, Nn-propylethylenediamine, N,N'-n-propylethylenediamine, Ni-propylethylenediamine, N,N'-i-propylethylenediamine, Nn-butylethylenediamine, Examples of such amino acids include N,N'-n-butylethylenediamine, Ni-butylethylenediamine, N,N'-i-butylethylenediamine, N-tert-butylethylenediamine, N,N'-tert-butylethylenediamine, N,N,N',N'-tetramethyl-1,3-diaminopropane, N,N,N'-trimethyl-1,3-diaminopropane, N,N'-dimethyl-1,3-diaminopropane, N-methyl-1,3-diaminopropane, N,N,N',N'-tetramethyl-1,3-diamino-1-methylpropane, N,N,N',N'-tetramethyl-1,3-diamino-2-methylpropane, N,N,N',N'-tetramethyl-1,4-diaminobutane, and N,N,N',N'-tetramethyl-1,5-diaminopentane. A preferred diamine compound for this embodiment is one in which the number of carbon atoms in the alkylene group connecting the two nitrogen atoms is 2 or 3. The amount of these diamine compounds used is not particularly limited, but is preferably in the range of 0.01 mol to 10 mol per 100 mol of the phenol compound added to the polymerization reaction.
[0048] In this embodiment, the polymerization catalyst may contain a primary amine and a secondary monoamine as a component thereof. Examples of the secondary monoamine include, but are not limited to, dimethylamine, diethylamine, di-n-propylamine, di-i-propylamine, di-n-butylamine, di-i-butylamine, di-tert-butylamine, dipentylamines, dihexylamines, dioctylamines, didecylamines, dibenzylamines, methylethylamine, methylpropylamine, methylbutylamine, cyclohexylamine, N-phenylmethanolamine, N-phenylethanolamine, N-phenylpropanolamine, N-(m-methylphenyl)ethanolamine, N-(p-methylphenyl)ethanolamine, N-(2',6'-dimethylphenyl)ethanolamine, N-(p-chlorophenyl)ethanolamine, N-ethylaniline, N-butylaniline, N-methyl-2-methylaniline, N-methyl-2,6-dimethylaniline, and diphenylamine.
[0049] The polymerization catalyst of the present embodiment may also contain a tertiary monoamine compound as a component thereof. The tertiary monoamine compound is an aliphatic tertiary amine including an alicyclic tertiary amine. Examples of the tertiary monoamine compound include trimethylamine, triethylamine, tripropylamine, tributylamine, triisobutylamine, dimethylethylamine, dimethylpropylamine, allyldiethylamine, dimethyl-n-butylamine, diethylisopropylamine, and N-methylcyclohexylamine. These tertiary monoamines may be used alone or in combination of two or more. The amount of these compounds used is not particularly limited, but is preferably in the range of 15 moles or less relative to 100 moles of the phenol compound added to the polymerization reaction.
[0050] In this embodiment, there is no limitation on adding a surfactant that has been known to have an effect of improving polymerization activity. Examples of such surfactants include trioctylmethylammonium chloride, known under the trade names Aliquat 336 and Capriquat. The amount of the surfactant used is preferably within a range not exceeding 0.1% by mass relative to the total amount (100% by mass) of the polymerization reaction mixture.
[0051] As the oxygen-containing gas, in addition to pure oxygen, a mixture of oxygen and an inert gas such as nitrogen in any ratio, air, or a mixture of air and an inert gas such as nitrogen in any ratio can be used. Normal pressure is sufficient for the pressure in the system during the polymerization reaction, but reduced or increased pressure can be used as necessary.
[0052] The polymerization temperature is not particularly limited, but if it is too low, the reaction will not proceed easily, and if it is too high, the reaction selectivity may decrease or gel may be formed. Therefore, the temperature is preferably in the range of 0 to 60°C, and more preferably in the range of 10 to 40°C.
[0053] In the process for producing polyphenylene ether, the polymerization can also be carried out in a poor solvent such as an alcohol.
[0054] (Copper extraction and by-product removal process) In this embodiment, there is no particular restriction on the post-treatment method after the polymerization reaction is completed. Usually, an acid such as hydrochloric acid or acetic acid, or ethylenediaminetetraacetic acid (EDTA) and its salts, nitrilotriacetic acid and its salts, etc. are added to the reaction liquid to deactivate the catalyst. In addition, a method for removing and treating the dihydric phenol by-product generated by the polymerization of polyphenylene ether can be performed using a conventionally known method. If the metal ions, which are the catalyst, are substantially deactivated as described above, the mixture can be decolorized simply by heating it. Alternatively, a method of adding a required amount of a known reducing agent is also possible. Examples of known reducing agents include hydroquinone and sodium dithionite.
[0055] (Liquid-liquid separation process) In the method for producing polyphenylene ether, water may be added to extract the compound that has deactivated the copper catalyst, and then liquid-liquid separation may be performed into an organic phase and an aqueous phase, and the aqueous phase may be removed to remove the copper catalyst from the organic phase. This liquid-liquid separation step is not particularly limited, and may include methods such as static separation and separation using a centrifuge. In order to promote the liquid-liquid separation, a known surfactant or the like may be used.
[0056] (concentration / drying process) Next, in the method for producing polyphenylene ether of the present embodiment, the organic phase containing the polyphenylene ether after liquid-liquid separation may be concentrated and dried by volatilizing the solvent.
[0057] The method for volatilizing the solvent contained in the organic phase is not particularly limited, but examples thereof include a method of transferring the organic phase to a high-temperature concentration tank and distilling off the solvent to concentrate it, and a method of distilling off toluene using equipment such as a rotary evaporator to concentrate it, and the like.
[0058] The temperature of the drying treatment in the drying step is preferably at least 60° C. or higher, more preferably 80° C. or higher, even more preferably 120° C. or higher, and most preferably 140° C. or higher. When the polyphenylene ether is dried at a temperature of 60° C. or higher, the content of high-boiling-point volatile components in the polyphenylene ether powder can be efficiently reduced.
[0059] In order to obtain polyphenylene ether with high efficiency, a method of increasing the drying temperature, a method of increasing the degree of vacuum in the drying atmosphere, a method of stirring during drying, and the like are effective, but a method of increasing the drying temperature is particularly preferable from the viewpoint of production efficiency. In the drying step, it is preferable to use a dryer equipped with a mixing function. Examples of the mixing function include a stirring type dryer and a rolling type dryer. This allows the processing amount to be increased, and the productivity to be maintained at a high level.
[0060] The polyphenylene ether (A) can also be produced by a redistribution reaction in which a polyphenylene ether derived from a phenol of the above formula (1) is equilibrated with a phenolic compound of the above formula (2) in the presence of an oxidizing agent. Redistribution reactions are known in the art and are described, for example, in U.S. Patent No. 3,496,236 to Cooper et al. and U.S. Patent No. 5,880,221 to Liska et al.
[0061] (Modification reaction process) There is no limitation on the method of introducing a functional group into the hydroxyl group of the unmodified polyphenylene ether, and for example, it can be obtained by the formation of an ester bond between the hydroxyl group of the unmodified polyphenylene ether and a carboxylic acid having a carbon-carbon double bond (hereinafter referred to as carboxylic acid). The formation of the ester bond can be achieved by various known methods. For example, a. the reaction of a carboxylic acid halide with a hydroxyl group at the polymer end, b. the formation of an ester bond by reaction with a carboxylic acid anhydride, c. a direct reaction with a carboxylic acid, and d. a method using an ester exchange reaction. The reaction with a carboxylic acid halide is one of the most common methods. As the carboxylic acid halide, chlorides and bromides are generally used, but other halogens may also be used. The reaction may be either a direct reaction with a hydroxyl group or a reaction with an alkali metal salt of a hydroxyl group. Since an acid such as hydrogen halide is generated in the direct reaction of a carboxylic acid halide with a hydroxyl group, a weak base such as an amine may be coexisted in order to trap the acid. In the reaction with a carboxylic anhydride of b or the direct reaction with a carboxylic acid of c, a compound such as a carbodiimide or dimethylaminopyridine may be allowed to coexist in order to activate the reaction site and promote the reaction. In the case of the transesterification reaction of d, it is desirable to remove the generated alcohols as necessary. In addition, known metal catalysts may be allowed to coexist in order to promote the reaction. After the reaction, in order to remove by-products such as amine salts, the reaction product may be washed with water, an acidic or alkaline aqueous solution, or the polymer solution may be dropped into a poor solvent such as an alcohol to recover the target product by reprecipitation. In addition, after washing the polymer solution, the solvent may be distilled off under reduced pressure to recover the polymer.
[0062] The method for producing the modified polyphenylene ether of the present embodiment is not limited to the method for producing the polyfunctional modified polyphenylene ether described above, and the order and number of the above-mentioned oxidative polymerization step, copper extraction and by-product removal step, liquid-liquid separation step, and concentration and drying step may be appropriately adjusted.
[0063] <Polyolefin (B)> The polyolefin can be used without any particular limitation. Among them, polypropylene-based resins are preferable. The polypropylene-based resins are not particularly limited, and examples thereof include homopolymers and / or copolymers having propylene as a repeating unit structure, and crystalline propylene homopolymers, crystalline propylene-ethylene block copolymers, and mixtures of crystalline propylene homopolymers and crystalline propylene-ethylene block copolymers are preferable. The crystalline propylene-ethylene block copolymer is not particularly limited, and examples thereof include those having a crystalline propylene homopolymer portion and a propylene-ethylene random copolymer portion. The polypropylene content in the resin composition can be determined, for example, by freeze-pulverizing the resin composition to obtain a powder form, dissolving the powder in chloroform at 23°C, and further recovering a fraction of the insoluble matter that dissolves in o-dichlorobenzene at 150°C, and measuring the fraction by NMR.
[0064] In the resin composition of the present embodiment, from the viewpoint of the performance balance of the resin composition and the adhesiveness of the resin, the content ratio of the polyphenylene ether (A) is 0.1 to 30.0 mass%, and the content ratio of the polyolefin (B) is 70.0 to 99.9 mass% with respect to the amount of the polyphenylene ether (A) and the polyolefin (B). From the viewpoint of the adhesiveness of the resin, it is preferable that the content ratio of the polyphenylene ether (A) is 0.1 to 28.0 mass%, and the content ratio of the polyolefin (B) is 72.0 to 99.9 mass%. From the same viewpoint, it is more preferable that the content ratio of the polyphenylene ether (A) is 1.0 to 26.0 mass%, the content ratio of the polyolefin (B) is 74.0 to 99.0 mass%, and it is further preferable that the content ratio of the polyphenylene ether (A) is 3.0 to 25.0 mass%, and the content ratio of the polyolefin (B) is 75.0 to 97.0 mass%.
[0065] <Thermoplastic resin> Thermoplastic resins other than components (A) and (B) that are optionally used in the resin composition of this embodiment are not particularly limited, and examples thereof include polystyrene, syndiotactic polystyrene, and high impact polystyrene.
[0066] <Additives> The resin composition of the present embodiment may contain any additives as necessary. The type of additive is not particularly limited as long as it is one that is generally used in thermoplastic resins. For example, inorganic fillers such as calcium carbonate, magnesium carbonate, magnesium hydroxide, calcium sulfate, barium sulfate, silica, clay, talc, mica, wollastonite, montmorillonite, zeolite, alumina, titanium oxide, magnesium oxide, zinc oxide, slug wool, and glass fiber; pigments such as carbon black and iron oxide; lubricants such as stearic acid, behenic acid, zinc stearate, calcium stearate, magnesium stearate, and ethylene bisstearamide; release agents, paraffinic process oil, and naphthenic process oil. , aromatic process oil, paraffin, organic polysiloxane, softeners such as mineral oil, plasticizers such as polyethylene glycol and fatty acid esters; antioxidants such as hindered phenol antioxidants and phosphorus-based heat stabilizers; hindered amine light stabilizers, benzotriazole ultraviolet absorbers, flame retardants, antistatic agents; reinforcing agents such as organic fibers, glass fibers, carbon fibers, and metal whiskers; colorants, and other additives and mixtures thereof, which are described in "Rubber and Plastic Compounding Chemicals" (edited by Nippon Rubber Digest Co., Ltd.) and the like. The amount of additives to be added is not particularly limited, and is usually 50 parts by mass or less per 100 parts by mass of the resin composition.
[0067] [Method of producing resin composition] The resin composition of the present embodiment can be produced by melt-kneading the above-mentioned components (A) and (B) and further other components.
[0068] Examples of the melt kneader for melt kneading include, but are not limited to, a single screw extruder, a multi-screw extruder including a twin screw extruder, a roll, a kneader, a Brabender plastograph, a Banbury mixer, etc., and from the viewpoint of kneading properties, a twin screw extruder is particularly preferred. Specific examples include the ZSK series manufactured by COPERION, the TEM series manufactured by Toshiba Machine Co., Ltd., and the TEX series manufactured by The Japan Steel Works, Ltd.
[0069] A preferred production method using an extruder is described below. The L / D (effective barrel length / inner barrel diameter) of the extruder is preferably in the range of 20 or more and 60 or less, and more preferably 30 or more and 60 or less.
[0070] The configuration of the extruder is not particularly limited, and for example, the extruder may be provided with a first raw material supply port on the upstream side in the direction in which the raw material flows, a first vacuum vent or an open vent downstream of the first raw material supply port, and a second vacuum vent or an open vent downstream of the first vacuum vent.
[0071] [Molded body] The molded article of the present embodiment is made of the resin composition of the present embodiment described above. The molded article of the present embodiment is not particularly limited, and examples thereof include automobile parts, interior and exterior parts of electrical equipment, and other parts. The automobile parts are not particularly limited, and examples thereof include exterior parts such as bumpers, fenders, door panels, various moldings, emblems, engine hoods, wheel caps, roofs, spoilers, and various aero parts; interior parts such as instrument panels, console boxes, and trims; secondary battery container parts mounted on automobiles, electric vehicles, hybrid electric vehicles, and the like; lithium ion secondary battery parts, and the like. The interior and exterior parts of electrical equipment are not particularly limited, and examples thereof include various computers and their peripherals, junction boxes, various connectors, other OA equipment, cabinets such as televisions, videos, and various disc players, chassis, and parts used in refrigerators, air conditioners, and liquid crystal projectors. Other examples of parts include electric wires and cables obtained by applying a coating to metal conductors or optical fibers, fuel cases for solid methanol batteries, fuel cell water pipes, water cooling tanks, boiler exterior cases, ink-related parts and components for inkjet printers, furniture (chairs, etc.), chassis, water piping, joints, and shapes such as sheets and films. Among these, preferred are molded articles such as covers and cover films that come into contact with metals used in circuit boards and circuits. EXAMPLES
[0072] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples. The measurement methods for the polyphenylene ether (A) and polyolefin (B) resin compositions in the examples and comparative examples are shown below.
[0073] (Production of polyphenylene ether (A)) (1) Manufacturing Example 1 A 40-liter jacketed polymerization tank equipped with a sparger, stirring turbine blades and baffles for introducing oxygen-containing gas at the bottom of the polymerization tank and a reflux condenser on the vent gas line at the top of the polymerization tank was charged with 2.4 g of cupric oxide, 18.1 g of 47% by mass aqueous hydrogen bromide solution, 5.8 g of di-tert-butylethylenediamine, 28.1 g of di-n-butylamine, 85.6 g of butyldimethylamine, 17.9 kg of toluene, 853 g of 2,6-dimethylphenol, and 1147 g of 2-tert-butyl-5-methylphenol to obtain a homogeneous solution while blowing nitrogen gas at a flow rate of 30.9 L / min. Next, dry air was introduced into the polymerization tank from the sparger at a rate of 21.0 L / min to start polymerization. Dry air was aerated for 120 minutes to obtain a polymerization mixture. The internal temperature was controlled to be 40°C during polymerization. The polymerization mixture (polymerization liquid) at the end of polymerization was in a homogeneous solution state. The dry air flow was stopped, and 25.9 g of tetrasodium ethylenediaminetetraacetate (a reagent manufactured by Dojindo Laboratories) was added to the polymerization mixture as an aqueous solution in 2 kg of water. The polymerization mixture was stirred at 70° C. for 150 minutes, then allowed to stand for 20 minutes, and the organic phase and the aqueous phase were separated by liquid-liquid separation. The organic phase was concentrated by a rotary evaporator until the polymer concentration was 30% by mass. The above solution was mixed with methanol such that the ratio of methanol to polymer solution was 4, and polymer precipitation was performed. Wet polyphenylene ether was obtained by filtration under reduced pressure using a glass filter. The wet polyphenylene ether was further washed with an amount of methanol such that the ratio of methanol to wet polyphenylene ether was 3. The above washing operation was performed three times. Next, the wet polyphenylene ether was kept at 120°C and 1 mmHg for 120 minutes, and dry polyphenylene ether was obtained.
[0074] (Production Example 2) In a 4.1-liter jacketed reactor equipped with a sparger for introducing oxygen-containing gas at the bottom of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor, 0.88 g of cupric chloride dihydrate, 3.76 g of 35% hydrochloric acid, 33.57 g of N,N,N',N'-tetramethylpropanediamine, 850 g of n-butanol, 1982 g of methanol, and 630 g of 2,6-dimethylphenol were placed. The composition weight ratio of the solvent used was n-butanol:methanol=30:70. Next, oxygen was introduced into the reactor from the sparger at a rate of 410 mL / min while vigorously stirring, and at the same time, the polymerization temperature was adjusted by passing a heat medium through the jacket to maintain it at 40°C. The polymerization liquid gradually took on the form of a slurry. 200 minutes after the start of oxygen introduction, the aeration of the oxygen-containing gas was stopped, and a 50% aqueous solution of 4.56 g of ethylenediaminetetraacetic acid tripotassium salt (a reagent manufactured by Dojindo Laboratories) was added to the polymerization mixture, followed by the addition of a 20% methanol solution of 8.52 g of hydroquinone (a reagent manufactured by Wako Pure Chemical Industries) little by little. The obtained polymerization liquid was transferred to a 4.1-liter jacketed reactor equipped with stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor, and reacted at 60°C for 3 hours. After the reaction was completed, the mixture was filtered and washed three times with a washing liquid (b) in an amount such that the mass ratio (b / a) of the methanol washing liquid (b) to the polyphenylene ether (a) to be washed was 4, to obtain wet polyphenylene ether. The mixture was then vacuum-dried at 120°C for 4 hours to obtain dry polyphenylene ether.
[0075] (Production Example 3) A 1.5-liter jacketed reactor equipped with a sparger for introducing an oxygen-containing gas at the bottom of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor was charged with a mixture of 0.092 g of cuprous oxide and 0.69 g of 47% hydrogen bromide, which had been previously prepared, 0.22 g of N,N'-di-tert-butylethylenediamine, 3.27 g of dimethyl-n-butylamine, 1.07 g of di-n-butylamine, 714.65 g of toluene, 66.53 g of 2,6-dimethylphenol, and 13.47 g of 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane. Then, air was introduced into the reactor from the sparger at a rate of 0.84 L / min while vigorously stirring, and the polymerization temperature was adjusted by passing a heat medium through the jacket to maintain it at 20°C. 150 minutes after the start of air introduction, the air flow was stopped, and the inside of the reactor was replaced with nitrogen gas. Then, 0.99 g of tetrasodium ethylenediaminetetraacetate tetrahydrate (a reagent manufactured by Dojindo Laboratories) was added to the polymerization mixture as an aqueous solution of 160 g of water. The mixture was then heated to 70°C, and copper extraction was carried out at 70°C for 2 hours. After that, the unmodified polyphenylene ether solution (organic phase) and the aqueous phase to which the catalyst metal had been transferred were separated by standing separation. The organic phase was concentrated by a rotary evaporator until the polymer concentration reached 30% by mass. The above solution was mixed with methanol such that the ratio of methanol to polymer solution was 4, and polymer precipitation was performed. Wet polyphenylene ether was obtained by filtration under reduced pressure using a glass filter. The wet polyphenylene ether was further washed with an amount of methanol such that the ratio of methanol to wet polyphenylene ether was 3. The above washing operation was performed three times. Next, the wet polyphenylene ether was kept at 120°C and 1 mmHg for 120 minutes, and dry polyphenylene ether was obtained.
[0076] [Analysis of polyphenylene ether] The polyphenylene ethers obtained in the above-mentioned respective production examples were subjected to the following analyses. The results of the analyses are shown in Table 1.
[0077] (1) The content ratio of the repeating unit derived from phenol of formula (1) or formula (2) to the total of the repeating unit derived from phenol of formula (1) and the repeating unit derived from phenol of formula (2) contained in the polyphenylene ether The unmodified polyphenylene ether obtained in the above-mentioned Production Example was dissolved in deuterated chloroform, and the resulting solution was analyzed using tetramethylsilane as an internal standard. 1 H-NMR measurement (JEOL 500MHz) was performed. Prior to the measurement, the polyphenylene ether was kept at 140°C and 1mmHg for 8 hours to remove volatile components such as toluene and water, and the measurement was performed as dry unmodified polyphenylene ether. The signals of the units derived from phenol in formula (1) and formula (2) were identified, and their respective ratios were calculated. For example, in the obtained unmodified polyphenylene ether, the signal derived from the repeating unit derived from phenol in the above formula (1), i.e., the 2,6-dimethylphenol-derived structure (2,6-dimethylphenylene unit), and the signal derived from the repeating unit derived from phenol in the above formula (2), i.e., the 2-tert-butyl-5-methylphenol-derived structure (2-tert-butyl-5-methylphenylene unit), were assigned as follows. The peaks of the repeating units derived from each phenol appear in the following regions. Peaks derived from hydrogen atoms of the methyl groups of the 2,6-dimethylphenylene unit and the 2-tert-butyl-5-methylphenylene unit (6H and 3H, respectively): 1.60 to 2.50 ppm (excluding peaks derived from hydrogen atoms of the methyl group of toluene) Peaks (9H) derived from hydrogen atoms of the tert-butyl group of the 2-tert-butyl-5-methylphenylene unit: 1.00 to 1.52 ppm (excluding peaks derived from hydrogen atoms of water) The integral value of the above signal is examined, and the integral value per proton of the peak derived from the hydrogen atom of the methyl group of the 2,6-dimethylphenylene unit can be calculated using the following formula (1). E = {C - 3 × (D / 9)} / 6 Formula (1) C: Integration value of the peaks derived from the methyl of the 2,6-dimethylphenylene unit and the 2-tert-butyl-5-methylphenylene unit D: Integration value of the peak derived from the tert-butyl of the 2-tert-butyl-5-methylphenylene unit E: integral per proton of the peak derived from the methyl of the 2,6-dimethylphenylene unit Furthermore, the proportion (mol %) of the repeating units derived from the phenol of the above formula (1) or (2) can be calculated using the following mathematical formulas (2) and (3). Proportion of repeating units derived from phenol in formula (1) (mol%) = E / {(D / 9) + E} × 100 ··· Formula (2) Proportion (mol%) of repeating units derived from phenol in formula (2) = (D / 9) / {(D / 9)+E}×100 Formula (3)
[0078] (2) Reduced viscosity of polyphenylene ether (ηsp / c) A 0.5 g / dL chloroform solution of the obtained polyphenylene ether was prepared, and the reduced viscosity (ηsp / c) (dL / g) at 30° C. was determined using an Ubbelohde viscosity tube.
[0079] (3) Glass transition temperature of polyphenylene ether The glass transition temperature of the obtained polyphenylene ether was measured using a differential scanning calorimeter DSC (PerkinElmer-Pyrisl). In a nitrogen atmosphere, the material was heated from room temperature to 230°C at a heating rate of 20°C per minute, then cooled to 50°C at a heating rate of 20°C per minute, and the glass transition temperature was measured at a heating rate of 20°C per minute.
[0080] (4) Solubility of polyphenylene ether in n-hexane at 25°C The solubility of the resulting polyphenylene ether in hexane was measured. The measurement was carried out as follows: First, 400 mg of polyphenylene ether was placed in a sample tube, and n-hexane at 25°C was gradually added while gently stirring with a magnetic stirrer in a 25°C environment, and the state inside the sample tube was observed. The concentration of polyphenylene ether (A) when completely dissolved was taken as the solubility at 25°C.
[0081] [Table 1]
[0082] Next, the raw materials used in the examples and comparative examples described later are shown below. (A) Polyphenylene ether (A-1) Polyphenylene ether synthesized by Production Example 1 (A-2) Polyphenylene ether synthesized in Production Example 2 (A-3) Polyphenylene ether synthesized in Production Example 3
[0083] (B) Polyolefin (B-1) Polypropylene MFR=14, bending strength 63MPa (B-2) Polypropylene MFR=66, bending strength 46MPa
[0084] [Examples 1 to 5, Comparative Examples 1 to 7] Each example and comparative example will be described in detail below. A twin-screw extruder (ZSK-25, manufactured by Coperion) was used as a melt kneader for producing the resin compositions of each of the Examples and Comparative Examples. The L / D of the extruder was set to 35. The twin-screw extruder was configured to have a first raw material supply port on the upstream side in the direction in which the raw materials flow, a first open vent downstream of the first raw material supply port, and a second vacuum vent downstream of the first vacuum vent. The barrel temperature of the twin-screw extruder was set to 210°C from the first raw material supply port to the die port and 220°C at the die port. Pellets of the resin composition were produced under conditions of a screw rotation speed of 300 rpm and an extrusion rate of 15 kg / h.
[0085] 〔evaluation〕 The obtained resin composition samples were subjected to the following evaluations. The evaluation results of the resin composition samples obtained in Examples 1 to 5 are shown in Table 1, and the evaluation results of the resin composition samples obtained in Comparative Examples 1 to 7 are shown in Table 2. (1) Bending strength The obtained resin composition pellets were fed to a small injection molding machine (product name: IS-100GN, manufactured by Toshiba Machine Co., Ltd.) with a cylinder temperature set at 230°C, and molded under the conditions of a mold temperature of 40°C, an injection pressure of 60 MPa, an injection time of 20 seconds, and a cooling time of 15 seconds to produce an ISO dumbbell for evaluation. The bending strength (MPa) of this ISO dumbbell was measured according to ISO 178. The measured values were deemed to be excellent if they were equal to or better than the values obtained using the polyolefin alone.
[0086] (2)MFR The obtained resin composition pellets were measured at a temperature of 190° C. and a load of 10 kg in accordance with ISO 1133. Note that the larger the measured value, the better the fluidity, which is preferable.
[0087] (3) Peel test The obtained resin composition pellets were fed into a small injection molding machine (product name: IS-100GN, manufactured by Toshiba Machine Co., Ltd.) with a cylinder temperature set to 230°C, and molded under conditions of a mold temperature of 40°C, injection pressure of 60 MPa, injection time of 20 seconds, and cooling time of 20 seconds to produce a flat plate for evaluation measuring 60 mm in length and width and 2 mm in thickness. A flat plate was cut with a cutter knife, with 11 cuts each measuring 1 mm lengthwise and 1 mm width, creating 100 grid-like cuts. A copper plate was placed on the grid and the grid was placed in a hot air oven at 150°C for 168 hours. After removal, the number of squares where a thin skin-like peeling occurred when the copper plate was peeled off was counted. Note that the fewer the number of peeled sheets, the better the adhesion between the resins was judged to be.
[0088] [Table 2]
[0089] [Table 3] [Industrial Applicability]
[0090] INDUSTRIAL APPLICABILITY The resin composition of the present invention has industrial applicability in various fields as a PO alloy resin having excellent flowability and mechanical strength.
Claims
1. A resin composition comprising a polyphenylene ether (A) and a polyolefin (B), a content ratio of the polyphenylene ether (A) relative to a total amount of the polyphenylene ether (A) and the polyolefin (B) is 0.1 to 30.0 mass%, and a content ratio of the polyolefin (B) is 70 to 99.9 mass%, A resin composition, characterized in that the polyphenylene ether (A) has a solubility in n-hexane at 25°C of 5 mass% or more.
2. 2. The resin composition according to claim 1, wherein the polyphenylene ether (A) has a glass transition temperature of 100 to 180° C.
3. The resin composition according to claim 1 , wherein the polyphenylene ether (A) has a partial structure represented by the following formula (3): [Formula 1] (In formula (3), R 31 each independently represents an optionally substituted linear alkyl group having 1 to 8 carbon atoms or two R 31 is a cyclic alkyl structure having 1 to 8 carbon atoms bonded to R 32 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 33 is a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, or an optionally substituted phenyl group.
4. The polyphenylene ether (A) contains a repeating unit derived from a phenol represented by the following formula (1) and a repeating unit derived from a phenol represented by the following formula (2): the content ratio of the repeating unit derived from phenol of the formula (1) is 5 to 89 mol %, and the content ratio of the repeating unit derived from phenol of the formula (2) is 11 to 95 mol %, relative to 100 mol % in total of the repeating units derived from phenol of the formula (1); The resin composition according to claim 3, characterized in that the reduced viscosity (ηsp / c) measured in a chloroform solution having a concentration of 0.5 g / dL at 30° C. is 0.03 to 0.30 dL / g. [chemical 2] (In formula (1), R 11 are each independently an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; R 12 are each independently a hydrogen atom, an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom. [C3] (In formula (2), R 22 are each independently a hydrogen atom, an optionally substituted saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; 22 are not both hydrogen atoms, R 21 is a partial structure represented by the following formula (3). [C4] In formula (3), R31 is independently a linear alkyl group having 1 to 8 carbon atoms which may be substituted, or two R 31 is a cyclic alkyl structure having 1 to 8 carbon atoms bonded to R 32 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 33 is a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, or an optionally substituted phenyl group.
5. The resin composition according to claim 3, wherein the partial structure represented by the formula (3) is a tert-butyl group.
6. The resin composition according to claim 3, wherein the polyolefin (B) is polypropylene (B1).
7. A molded article comprising the resin composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Polyolefin compositions containing poly(phenylene ether) fillers and articles thereof
JP2017500417A