Method for repairing inner face
A MMA-based repair method for drains, grease traps, and invert boxes in commercial kitchens addresses adhesion and durability issues, enabling quick, cost-effective repairs with enhanced water resistance and flexibility, reducing downtime to half a day or less.
Patent Information
- Application Number
- JP2023072889
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Existing methods for repairing the inner surfaces of drains, grease traps, and invert boxes in commercial kitchens are inefficient, requiring long construction periods, leading to significant business disruptions and high costs due to poor adhesion, water resistance, and durability issues, especially when exposed to oily components and constant water flow.
A repair method using a specific composition of methyl methacrylate (MMA) based repair liquid, including a radical polymerization initiator, thixotropy-imparting powder, and inorganic filler, which forms a durable and flexible repair structure through steps of cleaning, applying a primer layer, and a top coat layer to ensure strong adhesion and water resistance.
The method allows for rapid repair of inner surfaces with enhanced adhesion, water resistance, and durability, reducing downtime to half a day or less, preventing business interruptions and extending the lifespan of repairs to semi-permanent levels.
Smart Images

Figure 2024158049000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for repairing the inner surface of a drain, grease trap, or invert basin located on a kitchen floor. [Background technology]
[0002] On the floors of commercial kitchens, there are many devices such as "drains, which are generally covered with gratings," which drain water containing oily and other waste materials; grease traps, which are generally located at the end of drains or drain pipes and which separate and collect the oil in the wastewater; and invert manholes, which are generally installed in the middle of drain pipes made of polyvinyl chloride and allow the wastewater to flow smoothly.
[0003] In commercial kitchens, drains, grease traps, invert manholes, etc. must be repaired or replaced regularly to prevent and reduce drainage leaks (water leakage) and the accumulation of dirt. Regardless of whether it is in the kitchen or not, the inside surfaces of drains and catch basins are now usually constructed or repaired with mortar or epoxy resin.
[0004] Patent Document 1 describes a method for manufacturing a catch basin having a distinctive shape of a connecting pipe, but an epoxy adhesive is used for the bonding portion. Patent Document 2 describes a manhole socket for the outflow side that connects a drain pipe (sewer pipe) and a manhole, but an epoxy adhesive is used for the adhesive portion. Patent Document 3 describes a connection structure between a drainage pipe (sewer pipe) and an intermediate structure, but uses an epoxy adhesive for the bonding portion.
[0005] Patent documents 1 to 3 all relate to manufacturing, not repair of drain pipes, drain ditches, drainage basins, etc., but patent document 4 describes an invention relating to a method for rehabilitating sewerage faucet pipes, in which an epoxy acrylate resin liquid is also used for adhesive parts, etc. Here, epoxy acrylate resin is a type of epoxy resin, as it is polymerized and hardened by ring-opening polymerization of the epoxy ring to exhibit adhesive properties.
[0006] Furthermore, Patent Document 5 describes a method for repairing a catchment area by sucking up water from an isolated space within the catchment area and then filling the space, using a cloud of cement paste, mortar, or the like as a filler.
[0007] When drainage ditches, catch basins, etc. deteriorate over time, the mainstream practice is to replace them, but when repairing them, as mentioned above, epoxy resins and mortar are generally used as materials.
[0008] On the other hand, acrylic materials that utilize the radical polymerization and curing of the carbon-carbon double bonds of (meth)acrylates are inhibited by air (oxygen) and are thought to be insufficiently cured in air, or to have a slow curing rate and poor adhesion. In particular, methyl methacrylate (MMA) monomer has the above-mentioned properties and is also thought to be easily adversely affected by water.
[0009] On the other hand, drains, grease traps, or invert manholes on kitchen floors have a short lifespan, and there are increasing cases of previously installed or newly constructed drains, grease traps, or invert manholes deteriorating, causing drainage leaks (water leakage). In such cases, excavating the area and replacing them would be extremely costly and would take a long time to complete. With conventional repair methods, whether the repair material was epoxy resin or mortar, it would take at least one day, and usually nearly one week.
[0010] However, in kitchens, particularly commercial kitchens such as restaurants, if the time required for repairs, i.e. the period during which the kitchen is out of use, is long, the business is forced to suspend operations during that time, causing enormous losses (loss in sales) during that time.
[0011] Furthermore, even if repairs were to be made, conventional epoxy-based materials had low flexibility and poor adhesion, so that the repaired area would only last for 2 to 3 years, and did not meet the demands for kitchen repairs mentioned above. Furthermore, conventional so-called "underwater bonds" use epoxy resin as a material, which, in addition to having the above problems, has no resistance to oily components and also has low resistance to water flow. Waterproof mortar has also been used as a repair material, but although this material is resistant to still water, it has low resistance to water flow in drains, grease traps, and invert manholes.
[0012] As described above, repairing kitchen drains, grease traps, or invert manholes requires many demands and strict conditions, and known techniques have not been able to adequately meet these demands. [Prior art documents] [Patent documents]
[0013] [Patent Document 1] JP 2001-132083 A [Patent Document 2] JP 2008-297772 A [Patent Document 3] JP 2013-040477 A [Patent Document 4] Japanese Patent Application Publication No. 11-107360 [Patent Document 5] JP 2010-281049 A Summary of the Invention [Problem to be solved by the invention]
[0014] The present invention has been made in consideration of the above-mentioned background technology, and an object of the present invention is to provide an excellent method for repairing the inner surface of a drain, a grease trap, or an invert manhole, which is present on a kitchen floor and has an inner surface made of concrete or mortar. [Means for solving the problem]
[0015] The inventors of the present invention have conducted extensive research to solve the above problems and issues, and have found that by using a specific repair liquid whose main component is methyl methacrylate (MMA) and a repair method having specific steps, it is possible to avoid the adverse effects of oily stains caused by oily components on the inner surface of drains, grease traps, or invert manholes in kitchens; the repair liquid has excellent water resistance, mechanical strength, and durability over time; it has excellent adhesion, bonding, and applicability to the above inner surfaces formed of concrete or mortar, which are said to have poor adhesion and adhesion; it does not deteriorate even when exposed to running water; and, because it has good hardening performance, it can shorten the "period during which the kitchen cannot be used" and does not cause loss of business for restaurants, etc.; and these findings led to the present invention.
[0016] That is, the present invention is a method for repairing the inner surface of a drain, a grease trap, or an invert manhole, the inner surface of which is formed of concrete or mortar and is present on a kitchen floor, comprising the steps of: (2) removing oily dirt from the inner surface using a strong alkaline cleaner having a pH of 11 or higher, which contains a surfactant, a water-soluble organic solvent, and water; (4) applying a primer layer forming liquid containing methyl methacrylate and a radical polymerization initiator to form a primer layer; and (5) applying a repair liquid containing methyl methacrylate, a radical polymerization initiator, and a thixotropy-imparting powder to the inner surface to form a repair structure, and then solidifying the repair structure over time; The present invention provides an inner surface repair method, which is characterized by carrying out the steps of:
[0017] Further, the present invention relates to a method for producing a fluororesin comprising the steps of: (6) The method for repairing an inner surface as described above further comprises the step of forming a top coat layer by applying a top coat layer forming liquid containing methyl methacrylate and a radical polymerization initiator.
[0018] The present invention also provides the above-described method for repairing an inner surface, wherein the primer layer-forming liquid and / or the repair liquid further contain an inorganic filler.
[0019] The present invention also provides the above-mentioned method for repairing an inner surface, wherein the radical polymerization initiator is an organic peroxide.
[0020] The present invention also provides the above-described method for repairing an inner surface, wherein the repair liquid is substantially free of a diluting solvent.
[0021] The present invention also provides a method for repairing a smeared area of the repair liquid by applying the repair liquid at a concentration of 500 g / m 2 More than 3000g / m 2 The following provides an inner surface repair method for forming the repair structure by application to the inner surface.
[0022] The present invention also provides a drain, grease trap, or invert manhole that has been repaired using the above-mentioned inner surface repair method, and has a "hardened repair structure containing at least a methyl methacrylate polymer, a thixotropy-imparting powder, and an inorganic filler" on its inner surface.
[0023] The present invention also provides a repair liquid that is used for the above-mentioned inner surface repair method. Effect of the Invention
[0024] The present invention solves the above-mentioned problems and issues of the conventional technology, and allows the inner surface of a drain, grease trap, or invert manhole in a kitchen to be repaired easily, in a short period of time, and at low cost, while ensuring adhesion to concrete and mortar (film properties, adhesive properties, etc.), water resistance, durability over time, and connection reinforcement with the drain pipe, etc.
[0025] In particular, oily waste accumulates and remains inside drains, grease traps, or invert manholes installed on kitchen floors, and often sticks strongly to the inner surfaces. In contrast, in home kitchens, oils such as frying oil are removed and disposed of separately, so the wastewater coming out of the sink is often oil-free. Therefore, in ordinary homes and apartments, there is very little oil left deposited or stuck tightly on the inside of the drainage manholes.
[0026] However, as mentioned above, in kitchens such as restaurants, oil is often poured down the drain along with the water, and as a result, oil accumulates, stays, and sticks inside drains, grease traps, or inverted manholes installed on the kitchen floor. However, since grease traps are designed to remove oil by allowing it to settle in the first place, it is natural that oil accumulates on their internal surfaces.
[0027] According to the present invention, even in the case of a "drain, grease trap, or invert manhole installed on a kitchen floor" which has a particularly high oil content compared to drain manholes and the like in other locations, the interior can be repaired easily, in a short period of time, and at low cost while ensuring adhesion (coating properties, adhesiveness, etc.), water resistance, and durability.
[0028] In general, the adhesion and bonding of organic coatings to concrete and mortar surfaces is significantly inferior to that of asphalt surfaces, metal (pipe) surfaces such as iron (pipe), and other material surfaces. Moreover, even a small amount of oily dirt (film) on the surface further reduces the adhesion and bonding to that surface. The inner surface repair method having the specific steps of the present invention and the primer layer forming liquid / repair liquid can achieve strong adhesion and bonding even on the surfaces of concrete and mortar, which generally have extremely poor adhesion and bonding properties.
[0029] When repairing the inside of a building with a repair liquid containing epoxy resin or a so-called "underwater bond" that is generally composed of epoxy resin, the repair coating on the inside of the building deteriorates in 2 to 3 years due to the oil contained in the wastewater from the kitchen. In addition, although the underwater bond has some resistance to still water, its water resistance is further reduced in the drains, grease traps, and inverted manholes with concrete or mortar surfaces in kitchens where water is constantly flowing. The cured epoxy resin formed by ring-opening polymerization of epoxy rings has no flexibility and poor adhesiveness, which is particularly poor when the substrate is concrete or mortar, and further deteriorates significantly when the drainage pipe is displaced over the years (e.g., due to an earthquake, etc.). With commonly used epoxy repair fluids, the repaired area may only last for about two or three years, but with the present invention, the repaired inner surface will last almost permanently.
[0030] Even if repaired with waterproof mortar, water will always flow through it for a long period of time, so it will have poor resistance to running water. Therefore, it will have poor durability in kitchen drains, grease traps, and inverted manholes, which are constantly exposed to running water. According to the present invention, the repaired inner surface is extremely durable against running water.
[0031] As mentioned above, the inner surfaces of kitchen drains, grease traps, and invert manholes are made of concrete or mortar, and epoxy resins and mortar / cement pastes do not adhere well to these surfaces and deteriorate rapidly over time, especially in the presence of oil or running water. Furthermore, repair fluids that simply contain methyl methacrylate rather than the specific composition of the present invention are difficult to harden due to the influence of oxygen in the air, and also have poor adhesion to the surfaces of concrete and mortar, resulting in deterioration such as peeling over time.
[0032] By using the repair liquid of the present invention, the inside of drains, grease traps, and invert manholes installed on kitchen floors can be repaired while ensuring adhesion to concrete and mortar (film properties, adhesive properties, etc.), water resistance, durability over time, and connection reinforcement with drain pipes made of polyvinyl chloride, etc.
[0033] Even if the specific repair liquid of the present invention is used, it may be difficult to obtain sufficient adhesion, water resistance, and durability by simply cleaning the inner surface with a normal cleaning liquid. However, if the specific strong alkaline cleaning agent in step (2) of the present invention is used, it becomes possible to ensure adhesion, water resistance, and durability to the inner surface using the specific repair liquid of the present invention.
[0034] When the joint 13c between the drain pipe (usually made of polyvinyl chloride) connected to the grease trap or invert manhole peels off or the vicinity of the joint 13c is damaged, the specific repair liquid of the present invention is applied to repair the joint, and since the liquid remains flexible even after hardening, the joint can be repaired well even if the materials are different.
[0035] Methyl methacrylate (hereinafter sometimes abbreviated as "MMA"), the main component of the repair liquid in this invention, is liquid at room temperature, has a carbon-carbon double bond, and polymerizes (mainly radical polymerization) by heat or light in the presence of a thermal polymerization initiator or a photopolymerization initiator to form polymethyl methacrylate. The polymerization reaction that occurs at this time determines adhesive properties (adhesion), film properties, mechanical strength, water resistance, etc., but radical polymerization reactions are generally inhibited by the oxygen in the air, so it is said that polymerization is difficult in air. In particular, in the case of thin films, the polymerization reaction may not proceed at all depending on the polymerization conditions.
[0036] However, when repairing the inner surface of a drain, grease trap, or inverted manhole, a thin film is inevitably insufficient in terms of mechanical strength and waterproofing performance, so it is necessary to apply a certain thickness. This is also one of the reasons, and the repair liquid of the present invention, which contains at least methyl methacrylate, a radical polymerization initiator, and a thixotropy-imparting powder, is less susceptible to the effects of air (oxygen), and MMA is suitably polymerized to exhibit hardening and adhesive properties.
[0037] Furthermore, by incorporating an inorganic filler, a thick film can be formed, and by forming a thick film, and / or by the very presence of the inorganic filler or the thixotropy-imparting powder, the diffusion of oxygen is suppressed and the coating is no longer affected by oxygen (deactivation by oxygen is eliminated), so that radical polymerization proceeds suitably and a suitable repair coating is formed.
[0038] Depending on the composition of the repair liquid and the conditions after application of the repair liquid (air blowing and temperature), a thin film-like substance forms on the surface of the repair liquid immediately after application (hereinafter, this may be referred to as the "paraffin phenomenon"). This paraffin phenomenon (although not limited to the mechanism of action, it is thought to inhibit the intrusion or diffusion of oxygen) causes a subsequent hardening reaction (radical polymerization) to proceed, completing a "hardened repair structure" with good adhesion.
[0039] According to the present invention, the composition is surprisingly not susceptible to the effects of oxygen (air) and is also not susceptible to the effects of water. Therefore, according to the present invention, the weaknesses of MMA are not present, and the advantage of high flexibility is exhibited, making it superior overall to general-purpose epoxy-based or mortar-based repair fluids.
[0040] Furthermore, the repair structure formed by the hardening of the repair liquid of the present invention, i.e., "a repair structure whose main component is polymethyl methacrylate formed by the polymerization of MMA", is flexible and has strong adhesive properties that conform to the respective materials, even if the grease trap or invert manhole made of concrete or mortar and the drainage pipe made of polyvinyl chloride are made of different materials.
[0041] By using the repair liquid of the present invention and further carrying out the process of the present invention using said repair liquid, the above-mentioned advantageous effects can be obtained and the total construction period (repair time) can be shortened. With repairs using epoxy resin or mortar, it takes at least one or two days, and usually nearly a week, before the kitchen can be used, but with the interior repair method of the present invention, the kitchen can be used in half a day at most. Therefore, in a restaurant kitchen, for example, if repair work is carried out at night using this invention, business can continue without interruption, thereby avoiding large losses (reduced sales) due to business suspension. [Brief description of the drawings]
[0042] [Figure 1] 1 is a flow chart showing steps of the inner surface repair method of the present invention, in which steps enclosed in a rectangular frame are essential steps. [Diagram 2] 1 is a schematic plan view showing an example of the locations of drains, grease traps, and invert manholes, which are the subject of the inner surface repair method of the present invention, on a kitchen floor. [Diagram 3] FIG. 2 is a schematic perspective view showing an example of the structure of an inverter box. [Figure 4] FIG. 2 is a schematic cross-sectional view showing an example of a primer layer, a cured repair structure, and a top coat layer formed by carrying out the steps of the inner surface repair method of the present invention. [Diagram 5] Photographs taken during or after each step of the inner surface repair method of the present invention when the method was performed on a kitchen drain. [Figure 6] These are photographs taken during or after each step of the inner surface repair method of the present invention when the method was performed on an inverted box in a kitchen. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0043] The present invention will be described below, however, the present invention is not limited to the specific embodiments below and can be modified as desired within the scope of the technical concept.
[0044] The inner surface repair method of the present invention is a method for repairing the inner surface of a drain, a grease trap, or an invert manhole, which is present on a kitchen floor and has an inner surface made of concrete or mortar, comprising the steps of: (2) removing oily dirt from the inner surface using a strong alkaline cleaner having a pH of 11 or higher, which contains a surfactant, a water-soluble organic solvent, and water; (4) applying a primer layer forming liquid containing methyl methacrylate and a radical polymerization initiator to form a primer layer; and (5) applying a repair liquid containing methyl methacrylate, a radical polymerization initiator, and a thixotropy-imparting powder to the inner surface to form a repair structure, and then solidifying the repair structure over time; The present invention is characterized by carrying out the following steps.
[0045] [Target of the inner surface repair method of the present invention] The target of repair by the inner surface repair method of the present invention is the inner surface of a drain 11, a grease trap 12, or an invert manhole 13 that is present on a kitchen floor and whose inner surface is made of concrete or mortar. Here, the "inner surface" includes not only the wall surface and bottom surface, but also the connection part with the drain pipe 14 (see Figure 3), the inside of the invert (see Figure 3), and the "concave portion of the upper edge of the drain, manhole, etc." (see Figures 5 and 6) where the edge of the grating or mesh cover covering the drain 11 or manhole is placed on (supported by) the drain 11 or manhole, etc.
[0046] <Drain> An example of the location of a drain 11 on a kitchen floor is shown in Figure 2. Normally, the drain 11 in a kitchen is covered with a grating so that the drain 11 does not get in the way of workers in the kitchen.
[0047] When repairing the inner surface of the present invention, the grating is temporarily removed and the inside of the drainage groove 11 is repaired (see FIG. 5). A drain pipe 14 from a dishwasher, sink, etc. in the kitchen is connected to the drain 11. When repairing the inner surface of the present invention, it is preferable to also reinforce and repair the connection portion.
[0048] <Grease trap> A "grease trap" is a grease separator that is required to be installed in commercial kitchens. An example of the location of a grease trap 12 on a kitchen floor is shown in Figure 2. Normally, the grease trap 12 in a kitchen is covered with a lid so that the grease trap 12 does not get in the way of workers in the kitchen. When repairing the inner surface of the present invention, the lid is temporarily removed and the interior 12a of the grease trap 12 is repaired (see FIG. 5).
[0049] Grease traps 12 may consist of three tanks: a first tank for removing large debris using a basket or the like; a second tank for separating oil and fine sludge; and a third tank for draining only the water after the oil and fine sludge have been separated. With the interior repair method of the present invention, all three tanks can be repaired.
[0050] In the kitchen of a restaurant or the like, staff may periodically remove large debris, oil, and sludge trapped inside the grease trap 12. However, even in this case, it is preferable to completely remove oil and sludge from within the grease trap 12 by high-pressure cleaning with a water jet in the first step (1) of the inner surface repair method of the present invention.
[0051] Furthermore, in the inner surface repair method of the present invention, it is essential to remove oily dirt from the inner surface 15 using a strong alkaline cleaner in step (2). By carrying out step (2), the "repair liquid containing MMA" of the present invention can be suitably adhered to the inner surface.
[0052] The above description of steps (1) and (2) applies not only to the grease trap 12, but also to the drain 11 and the invert manhole 13.
[0053] <Inverted box> An "invert manhole" refers to a drain manhole with an "invert, which is a shape / concave 13b similar to the cross section of a pipe connected from the side" formed at the bottom of the manhole, as shown in Figure 3. Half of the pipe is carved into the bottom of the manhole to prevent the drain pipe 14 from being clogged with waste such as oil and to make it easier for the waste to flow. They are installed at key points in the kitchen to prevent clogging of the pipe and to make cleaning and inspection easy (see Figure 2). An example of the location of the inverted box 13 on the kitchen floor is shown in Figure 2. Usually, the inverted box 13 in the kitchen is covered with a lid so that the inverted box 13 does not get in the way of the workers in the kitchen.
[0054] When repairing the inner surface of the present invention, the lid is temporarily removed and the inner surface 13a of the invert box 13 is repaired (see FIG. 6). A drain pipe 14 from a dishwasher, sink, etc. in the kitchen is connected to the invert manhole 13. When repairing the inner surface of the present invention, it is preferable to also reinforce and repair the connection portion (see FIG. 6).
[0055] [Inner surface repair method of the present invention] The inner surface repair method of the present invention will be described below in the order of each step, with steps (2), (4) and (5) being essential steps of the present invention, and steps (1), (3) and (6) being more preferably steps to be carried out in the present invention (see FIG. 1). In addition to the above steps (1) to (6), there are other steps that are particularly preferably performed in the present invention (some of the steps are indicated as "step (*)" in FIG. 1), and these steps will be described in the relevant sections of steps (1) to (6).
[0056] <Process (1)> Step (1) is a step of performing high-pressure cleaning using water jets on the inner surface 15 of the drain ditch 11, grease trap 12, or invert manhole 13 prior to step (2) (Figures 1, 5(b), and 6(a)). Prior to step (1), if there are large lumps of oil or other debris, such as disposable chopsticks or towels, it is preferable to remove them by hand or with a tool such as a ladle, or to perform cleaning using a scraper (FIG. 5(a)).
[0057] The "high pressure washing with water jets" used in step (1) may be carried out by any conventional method using any type of device (FIG. 5(b), FIG. 6(a)). Step (1) is not essential, but not performing step (1) may hinder the effective removal of oily stains using a strong alkaline detergent in the next step (2).
[0058] <Process (2)> Step (2) is an essential step of the present invention, in which oily stains are removed from the inner surface 15 of the repair object using a "strong alkaline cleaner having a pH of 11 or more, which contains a surfactant, a water-soluble organic solvent, and water" (FIG. 1, FIG. 6(c)). If step (2) is not performed, the repair structure 17 (after hardening) mainly made of MMA will not adhere or bond well to the concrete or mortar that is the material of the inner surface, and will not be durable over time. Furthermore, if an acidic or neutral cleaning agent is used, the same phenomenon will occur as if step (2) was not performed at all.
[0059] <<Strong alkaline cleaner>> << <ph>>> The pH of the strong alkaline cleaner used in step (2) is increased by the inclusion of an alkaline substance. The alkaline substance is not limited as long as it can sufficiently increase the pH with an appropriate amount, but sodium hydroxide, potassium hydroxide, etc. are preferred, and sodium hydroxide is particularly preferred. The pH of the strong alkaline cleaner must be at least 11, preferably at least 12, more preferably at least 13, and particularly preferably at least 14. The pH is adjusted by the amount of an alkaline substance such as sodium hydroxide.
[0060] <<<Surfactants>>> The surfactant contained in the strong alkaline detergent may be any of anionic, cationic, nonionic and amphoteric. In the step (2) of the present invention, however, anionic surfactants are particularly preferred since they can effectively remove oil. Specific examples of the anionic surfactant include alkyl sulfates, alkyl sulfate ester salts, polyoxyethylene alkyl ether sulfates, alkylbenzene sulfonates, etc. Here, the above-mentioned "salt" is preferably a sodium salt. Among these, sodium polyoxyethylene isotridecyl sulfate, sodium polyoxyethylene lauryl (dodecyl) sulfate, sodium polyoxyethylene tetradecyl sulfate, and the like are particularly preferred.
[0061] <<<Water-soluble organic solvents>>> The water-soluble organic solvent contained in the strong alkaline cleaner is not particularly limited as long as it dissolves (is compatible with) water and has affinity for oil, but examples thereof include ethylene glycol, diethylene glycol, methyl ethyl ketone, acetone, ethylene glycol monoalkyl ether, diethylene glycol monoalkyl ether, triethylene glycol monoalkyl ether, etc. Also included are those in which the above "ethylene" is replaced with "propylene". Examples of the above "monoalkyl" include monomethyl, monoethyl, monopropyl, monobutyl, etc.
[0062] The method for removing oily dirt from the inner surface 15 using the strong alkaline cleaner is not particularly limited, but it is preferable to use a brush or a cleaning tool held in the hand for direct cleaning (FIG. 6(c)).
[0063] <Process (3)> Step (3) is a step of filling unevenness or gaps present on the inner surface 15 with a thermosetting epoxy resin. Step (3) is not an essential step of the present invention, but is preferably performed when unevenness or gaps exist (FIGS. 1 and 6(d)). Examples of such gaps include the joint with the drain pipe 14 (FIGS. 2 and 3). Prior to step (3), it is preferable to carry out a step of rinsing off the strong alkaline cleaner used in step (2) and then drying the product (Figure 1). As the thermosetting epoxy resin, known ones can be used.
[0064] <Process (4)> Step (4) is an essential step of the present invention, and is a step of applying a primer layer forming liquid containing methyl methacrylate and a radical polymerization initiator to form a primer layer 16 (FIGS. 1, 4, 5(c), and 6(e)). The primer layer 16 is formed on a base such as concrete or mortar, or polyvinyl chloride of the drainage pipe 14, so that strong adhesion of the repair structure 17 can be obtained (FIG. 4). That is, by forming the primer layer 16 in step (4), the repair structure 17 in step (5) is formed favorably, and the adhesion of the hardened repair structure 17 to the base after the repair structure 17 is hardened is improved.
[0065] The primer layer forming liquid may contain, in addition to methyl methacrylate and a radical polymerization initiator, a thixotropy-imparting powder, an inorganic filler, and / or other components in the repair liquid described below. The (particularly) preferred components and substances contained in the primer layer forming liquid are the same as the (particularly) preferred components and substances contained in the repair liquid in step (5) described below.
[0066] The primer layer 16 is required to have direct adhesion and bonding properties to concrete or mortar; its thickness is usually thinner than the repair structure 17 (and therefore more susceptible to the effects of oxygen) (Figure 4); and coloring is not necessary. Taking these factors into consideration, the composition of the primer layer forming liquid is determined by appropriately modifying the composition of the repair liquid used to form the repair structure 17 in step (5) described below. Specifically, for example, the primer layer 16 can exert its function even if it is thin, and since the thinner the layer, the less likely it is to sag, the less thixotropy-imparting powder to prevent sagging may be contained, or may be present in small amounts.
[0067] The primer layer forming liquid is applied / applied in the same manner as the repair liquid for the repair structure 17 described later. Hand application or spray application / appliance is preferred, and hand application is particularly preferred.
[0068] The thickness of the primer layer 16 is 50 g / m on average at the joint with the drain pipe 14 and its vicinity; on the inner surfaces of the drain ditch 11, the grease trap 12, and the inverted pit 13. 2 More than 800g / m 2 It is preferable to provide a thickness of 100 g / m or less. 2 More than 500g / m 2 It is more preferable to provide it with a thickness of 130 g / m or less. 2 More than 300g / m 2 It is particularly preferable to provide the following:
[0069] Prior to the step (4), it is preferable to carry out a step of drying the inner surface (FIG. 1). After normal air drying, it is preferable to further increase the degree of drying using a torch burner or the like in order to ensure more suitable adhesion.
[0070] <Process (5)> Step (5) is an essential step of the present invention, in which a repair liquid containing methyl methacrylate, a radical polymerization initiator, and a thixotropy-imparting powder is applied to the inner surface 15 to form a repair structure 17, which is then solidified over time (FIG. 1, FIG. 5(d)(e), FIG. 6(f)).
[0071] <<Repair fluid>> The repair liquid in the present invention contains at least methyl methacrylate (sometimes abbreviated as "MMA"), a polymerization initiator, and a thixotropy-imparting powder.
[0072] <<<Methyl methacrylate (MMA)>>> There is no particular limitation on the purity of the MMA used, and general-purpose MMA (commercially available products, etc.) can be used. MMA has a carbon-carbon double bond, and in the present invention, the double bond is polymerized to form polymethyl methacrylate. However, for the reasons described above, it is rarely polymerized in an open environment, that is, without being blocked from oxygen (air), and is rarely used as an adhesive, repair material, filler (sealant), or the like. In the present invention, although the objects to be repaired are open, such as a drain 11, a grease trap 12, and an invert manhole 13, the repair structure 17 can be solidified mainly by the polymerization reaction of MMA to form a hardened repair structure 17.
[0073] By adjusting the components and composition ratio of the repair liquid, the amount applied (thickness of the repair structure), and the hardening conditions (air temperature, presence or absence of wind, etc.), it is possible to form and harden a repair structure 17 to repair the inner surface. It is preferable to set the above conditions so that a good repair structure 17 is formed and the above-mentioned paraffin phenomenon occurs.
[0074] The compound having a polymerizable double bond may be contained in addition to MMA. However, the content of MMA in the entire "compound having a polymerizable double bond" is preferably 70% by mass or more, more preferably 85% by mass or more, even more preferably 95% by mass or more, and particularly preferably substantially all (e.g., 98% by mass or more). Examples of the "compound having a polymerizable double bond other than MMA" (hereinafter, the part in parentheses may be abbreviated as "other polymerizable compounds") include (meth)acrylic acid, (meth)acrylic acid alkyl esters (the alkyl group having 6 or less carbon atoms), and polyfunctional (meth)acrylic acid esters.
[0075] <<Polymerization initiator>> In the present invention, at least radical polymerization (including living radical polymerization) of MMA mainly progresses, and the repair structure 17 formed by applying or providing the repair liquid solidifies (cures). The repair liquid in the present invention contains a polymerization initiator as an essential component. The polymerization initiator is preferably a radical polymerization initiator, and may be a thermal polymerization initiator, a photopolymerization initiator, or both. However, from the standpoint of polymerization efficiency and work efficiency (especially since light irradiation is not essential), it is more preferable that the polymerization initiator be a thermal polymerization initiator.
[0076] Among the radical polymerization initiators and thermal polymerization initiators, organic peroxides or organic bisazo compounds are more preferred, and organic peroxides are particularly preferred from the viewpoint of polymerizability (curability). Among the organic peroxides, benzoyl peroxide (hereinafter abbreviated as "BPO") is most preferable in terms of polymerizability (curability), cost, versatility, and the like.
[0077] <<Curing accelerator>> The repair liquid of the present invention can contain a curing accelerator in addition to the polymerization initiator. The curing accelerator is not necessary when the temperature is high, such as in summer, but it is preferable to add it to increase the curing speed when the temperature during repair is low. The curing accelerator is not particularly limited, but examples thereof include compounds that promote the radical generation of the polymerization initiator, RAFT agents, appropriate chain transfer agents, and sulfur (S) atom-containing compounds.
[0078] The amount of the polymerization initiator and the hardening accelerator is determined so that the time from the start of mixing the components of the repair liquid to the application to the inner surface to form the repair structure 17 falls within an appropriate range. This time is usually between 5 and 15 minutes in summer when the average temperature is 25°C or higher, and between 20 and 40 minutes in winter when the average temperature is 15°C or lower. If the time exceeds this, workability will deteriorate and the repair liquid may not harden sufficiently.
[0079] <<Thixotropic Powder>> The thixotropy-imparting powder, which is an essential component of the repair liquid in the present invention, imparts thixotropy to the repair liquid. Specifically, it imparts "the property that the viscosity is low when the repair liquid is applied when the shear rate is high, and the viscosity increases when the repair liquid is applied to the joint portion 13c, side surface, etc., and the shear rate becomes zero" (also called "structural viscosity"), and "the property that the viscosity increases with the passage of time after the shear rate becomes zero."
[0080] The inclusion of the thixotropy-imparting powder not only imparts thixotropy, but also unexpectedly imparts good hardening properties. As shown in Fig. 3, the surface to which the repair liquid is applied at and near the joint portion 13c is often oriented downward or sideways, and the thixotropy-imparting powder can prevent the repair liquid from dripping when the repair liquid is applied there, and can impart thickness to the repair structure 17 and the hardened repair structure 17 that is formed by solidifying the repair liquid.
[0081] Examples of the thixotropy-imparting powder include fibrous powder, acicular powder, flat powder, fine powder, high oil absorption powder, flame-processed silica, etc., and fibrous powder, acicular powder, and flat powder are preferred because the radical polymerization of MMA proceeds favorably to provide good curing properties and because thixotropy is good, and fibrous powder is more preferred from the above points and from the standpoint of safety. Among these, fibrous powder made from natural fibrous clay minerals is particularly preferred. Specifically, sepiolite (hydrated magnesium silicate, Mg8Si 12 O 30 (OH)4·(OH2)4·8H2O) is most preferred in terms of curability, thixotropy imparting ability, safety, etc.
[0082] The radical polymerization of MMA is inhibited by oxygen in the air, but the thixotropy-imparting powder makes it possible to increase the thickness of the repair liquid (coating); the powder itself has gas barrier properties (oxygen impermeability); and other factors prevent the diffusion of oxygen from the air into the coating film, which is thought to allow the radical polymerization of MMA to proceed smoothly without being quenched.
[0083] <<Inorganic filler>> The repair liquid in the present invention preferably contains an inorganic filler. Examples of inorganic fillers include, but are not limited to, calcium carbonate, talc, calcium sulfate, silica, glass, ferric oxide, silica sand, kaolin, clay, titanium oxide, etc. Among them, calcium carbonate, talc, silica, glass, silica sand, etc. are preferred. The average particle size of the inorganic filler is preferably 1 μm to 100 μm, particularly preferably 3 μm to 30 μm. Although inorganic fillers having a slight thixotropy-imparting effect are not excluded, those having a large thixotropy-imparting effect become the above-mentioned "thixotropy-imparting powder", and therefore the shape of the inorganic filler is not limited, but is preferably approximately spherical, amorphous, etc.
[0084] The inclusion of the inorganic filler has the effects of improving the hardening property of MMA, improving the mechanical strength of the cured repair structure 17 obtained by curing the repair structure 17, and improving the adhesion to the joint portion 13c. The curing properties of MMA are improved because, while the radical polymerization of MMA is inhibited by oxygen in the air, the inorganic filler allows the repair liquid to have a thicker (applied) film; the inorganic filler itself has gas barrier properties; and other factors prevent oxygen from the air from diffusing into the coating film, allowing the radical polymerization (chain propagation) of MMA to proceed smoothly.
[0085] <<Dilution solvent>> The repair liquid and primer layer forming liquid in the present invention preferably contain substantially no dilution solvent, which has the following effects: improved curing of MMA; improved adhesion to the inner surface; improved mechanical strength of the joint portion 13c.
[0086] <<Colorant (toner)>> The repair liquid in the present invention preferably contains a colorant (toner). If a colorant (toner) is contained, it is easy to see where the repair liquid is applied, dripping or uneven application becomes difficult to see by increasing the amount, and the appearance is improved. No colorant (toner) is particularly contained, and known pigments and dyes are suitably used. There is no particular limitation on the color as long as the above-mentioned effects are achieved.
[0087] <<Antibacterial agent>> It is also preferable that the repair liquid in the present invention contains an antibacterial agent. By containing an antibacterial agent, slippage and mold can be eliminated. The antibacterial agent is not particularly contained, and a known antibacterial agent can be used.
[0088] <<Component composition of repair fluid>> The composition of each component in the repair liquid or primer layer forming liquid is more preferably as follows when the temperature (base temperature) of the inner surface of the drain ditch 11, grease trap 12, or invert manhole 13 is 10°C to 20°C. For 100 parts by mass of MMA, Other polymerizable compounds 0 to 15 parts by mass Polymerization initiator 0.5 to 10 parts by mass Curing accelerator 0 to 10 parts by mass Thixotropy imparting powder: 2 to 10 parts by mass Inorganic filler: 30 to 160 parts by weight Colorant 0 to 40 parts by weight
[0089] When the substrate temperature of the inner surface is the same as above, it is particularly preferable that the composition of each component of the repair liquid is as follows. For 100 parts by mass of MMA, Other polymerizable compounds 0 to 10 parts by mass Polymerization initiator 1 to 5 parts by mass Curing accelerator 2 to 8 parts by mass Thixotropic powder: 4 to 8 parts by mass Inorganic filler: 50 to 140 parts by weight Colorant: 15 to 30 parts by weight
[0090] When the inner substrate temperature is between 6°C and 10°C, it is desirable to mix twice the amount of polymerization initiator and / or hardening accelerator, and when it is below 6°C, it is desirable to mix three times the amount. When the temperature of the inner surface base is 20°C to 30°C, it is desirable to set the blending amount of the polymerization initiator and / or the hardening accelerator to the above-mentioned 40% to 70%.
[0091] <<How repair fluid is produced>> Each component of the repair liquid is mixed in a mixing container by hand stirring, mixing with a mixer, etc. It is preferable to obtain the repair liquid by mixing with a mixer. There is no particular limit to the order in which each component is added. In this case, taking into account the season, it is preferable to measure the air temperature, the liquid temperature, and the "temperature of the joint part, the inner surface base, etc." and (finely) adjust the amount of each component (especially the content of the polymerization initiator and hardening accelerator).
[0092] The repair liquid used in the inner surface repair method of the present invention may be sold or transferred separately, with each component being divided into one or more types, for mixing on-site for use in the present invention.
[0093] <<Repair method>> It is preferable that the inside of the item to be repaired is appropriately washed with water and that the base surface of the inner surface including the joint portion 13c is dried by blowing air therethrough using a blower or the like. Although the repair liquid of the present invention is mainly composed of MMA and utilizes the polymerization reaction of MMA, it was unexpectedly found that the presence of a small amount of water (such as moisture on the substrate surface) does not inhibit the hardening, solidification, and repair. However, it is preferable to further increase the degree of drying using a torch burner or the like in order to ensure even better adhesion.
[0094] Prior to repair, it is preferable to insert balloons or the like through holes in the drain ditch 11, grease trap 12, and invert manhole 13 leading to the drain pipe 14 to block the upstream and downstream sides of the drain pipe 14.
[0095] <<Repair structure formed by applying repair liquid>> The method for applying the repair liquid is not particularly limited, but examples include a method of applying it using a brush or spray device, and a method of splashing the required amount of repair liquid from a container onto the inner seam portion 13c, etc. The method of applying with a brush is particularly preferred because it allows a large amount to be applied before hardening, it can be applied suitably to the joint portion 13c and its vicinity, and it allows the thickness, amount, etc. to be uniform from place to place.
[0096] The average amount of repair liquid to be applied to the inner surface, including the joints and their surroundings, is 500 g / m 2 More than 3000g / m 2 The amount is preferably less than or equal to 100. The amount may be applied in one go, or may be applied in, for example, 2 to 5 times (preferably 3 times or less) to form the repair structure 17. When applied in multiple goes, the lower layer may be applied first and then allowed to age (even partway) to allow solidification to proceed, and then the upper layer may be applied, or the upper layer may be applied continuously without intentionally allowing it to age.
[0097] The amount of repair liquid applied per unit area is 700g / m 2 More than 2500g / m 2 Less than 1000g / m is more preferable. 2 More than 2000g / m 2 The following are particularly preferred: Within this range, the inner surface 15 can be suitably repaired, and the above-mentioned effects of the present invention can be suitably achieved.
[0098] When applying in multiple times, the number of times and the amount are not limited. For example, the first time is 200 to 1000 g / m 2 The second to fifth times are 150 to 600 g / m 2 In this case, it is preferable that the total amount of the applied liquid in a plurality of times is within the above range. In this case, when the amount of thixotropy-imparting powder applied is reduced, the powder is less likely to drip, reducing the need for thixotropy. Therefore, it is also preferable to reduce the amount of thixotropy-imparting powder to within the range of 0 / 10 to 5 / 10 of the above content.
[0099] The solidification time after applying the repair liquid to form the repair structure 17 is preferably 5 to 20 minutes, and particularly preferably 7 to 15 minutes, if the substrate temperature is 22° C. or higher. Also, if the substrate temperature is 15 to 22° C., it is preferably 7 to 25 minutes, and particularly preferably 10 to 20 minutes. Also, if the substrate temperature is 15° C. or lower, it is preferably 10 to 30 minutes, and particularly preferably 15 to 25 minutes. Here, "solidification time" refers to the time from when the repair liquid is applied to form the repair structure 17 (or from when the topcoat layer forming liquid is applied, if a topcoat layer 18 is to be formed) until when drainage can begin or the kitchen can be used.
[0100] The repair method of the present invention is extremely advantageous for commercial kitchens such as restaurants because it can significantly reduce the hardening time, curing time, and time the kitchen is out of service. When conventional repair fluids are used to repair the inside of drainage pits in condominiums and apartments, or the inside of equipment installed on the floor of bathrooms, hallways, toilets, etc., residents often tolerate the use of the fluid even if it means the equipment cannot be used for long periods of time.
[0101] However, if a commercial kitchen in a restaurant or the like is unavailable for a long period of time, the resulting loss in sales becomes a major problem and is unacceptable. Therefore, the inner surface repair method of the present invention using MMA is particularly effective when repairing the inner surfaces of drains 11, grease traps 12, or invert manholes 13 in commercial kitchens, providing the aforementioned effect of "short repair time, including solidification time and curing time."
[0102] <Process (6)> <<Topcoat layer>> After the repair structure 17 is solidified (cured) using the repair liquid of the present invention, it is preferable to form a topcoat layer 18 thereon in order to protect the cured repair structure 17. The top coat layer 18 is preferably formed by applying a top coat layer forming liquid containing at least methyl methacrylate and a radical polymerization initiator. The topcoat layer forming liquid may be the same as the repair liquid, but since the topcoat layer 18 can perform its function even when it is thin, and since a thin layer makes it less likely to sag, it does not need to contain a thixotropy-imparting powder to prevent sagging.
[0103] The (preferable) composition of the topcoat layer forming liquid is similar to that of the repair liquid described above, except that the thixotropy-imparting powder is not an essential component. In addition, coloring (containing a coloring agent) and flexibility are less necessary than in the repair liquid described above, and the topcoat layer forming liquid may be colorless or hard. In addition, the topcoat layer forming liquid preferably contains a thixotropy-imparting powder. Furthermore, it is preferable to include a polyfunctional (meth)acrylic acid ester as another polymerizable compound in order to harden (make the topcoat layer 18 stiff). The (preferable) method of application is the same as the method of application of the repair liquid described above.
[0104] The topcoat layer 18 is applied on the repair structure 17 at an average thickness of 100 g / m 2 More than 1000g / m 2 It is preferable to provide the material with a thickness of 150 g / m 2 More than 800g / m 2 It is more preferable to provide it with a thickness of 200 g / m 2 More than 600g / m 2 It is particularly preferable to provide the topcoat layer 18 by applying the topcoat layer forming liquid once or in two or more portions, and it is particularly preferable to apply the topcoat layer 18 by applying the topcoat layer forming liquid once or in two or more portions. When applying the topcoat layer in two or more portions, the above-mentioned adhesion amount is the total value of the applied liquid.
[0105] <<Full-thickness formation>> When repairs are made using the repair method of the present invention, a repair structure 17 is ultimately formed, but as described above, it is preferable that a primer layer 16 is further formed under the structure and / or a topcoat layer 18 is further formed on top of the structure. Particularly preferably, the primer layer 16, the repair structure 17, and the top coat layer 18 are formed in this order from the bottom. In this case, the total coating weight of the primer layer 16, the repair structure 17, and the top coat layer 18 is 700 g / m 2 More than 5000g / m 2 The total coating weight of the three layers is preferably 1000 g / m or less. 2 More than 4000g / m 2 or less, and particularly preferably 1500 g / m 2 More than 3000g / m 2 The following is the result.
[0106] As described above, when forming the three layers of primer layer 16, repair structure 17, and topcoat layer 18, if a conventional liquid other than the repair liquid of the present invention is used, it takes time for the liquid to solidify, and the repair work may take, for example, about three days from start to finish. When repairing using the repair liquid of the present invention, even when forming three layers, that is, the primer layer 16, the repair structure 17, and the topcoat layer 18, it is sufficient to have a solidification time about three times longer (for three layers) than the above-mentioned repair structure 17 alone. That is, the period during which sewage cannot be used is, for example, about 30 minutes to about 60 minutes.
[0107] Even taking into account the time it takes to mix the various components on-site to prepare the repair solution, the time it takes to insert the balloons to block the upstream side of the sewer pipe, and other preparation time, the process can be completed in less than half a day, making it ideal for repairing commercial kitchens. Restaurants are usually not open at night. Therefore, commercial kitchens are not used at night. Therefore, the present invention is preferably the above-mentioned inner surface repair method in which the repair is completed any time between 21:00 and 9:00 the following day. This is possible by using the above-mentioned repair liquid in the present invention. Since this is an inner surface repair method in which the repair is completed any time between 21:00 and 9:00 the following day, the repair may be completed, for example, between 23:00 and 7:00 the following day. This is possible if the repair liquid of the present invention is used.
[0108] <Drains, grease traps, inverted manholes> The drain ditch 11, grease trap 12, or inverted pit 13 repaired using the inner surface repair method of the present invention has excellent performance as described above. The present invention also relates to a drain ditch 11, a grease trap 12, or an inverted manhole 13 that has been repaired using the above-mentioned "internal surface repair method of the present invention." By being repaired using the inner surface repair method of the present invention, a drain 11, grease trap 12, or invert manhole 13 having a "hardened repair structure 17 containing at least methyl methacrylate polymer, thixotropy-imparting powder, and inorganic filler" on the inner surface 15 of the drain 11, grease trap 12, or invert manhole 13 has excellent performance properties such as water resistance and durability.
[0109] <Repair fluid> The present invention also relates to a repair fluid that is intended to be used in the above-mentioned "inner surface repair method of the present invention." The composition of the repair liquid is as described above. The repair solution may be sold or transferred in multiple liquid or solid forms. The scope of the present invention includes cases where the repair solution is sold or transferred in multiple liquid or solid forms, or where the repair solution is mixed on-site.
[0110] In this specification, the liquids used in each step are classified by different names, such as primer layer forming liquid, repair liquid, and topcoat layer forming liquid, but the embodiment also includes a case where the primer layer forming liquid, repair liquid, or topcoat layer forming liquid is applied multiple times. In addition, when applying multiple times, the repair liquid applied first may be the primer layer forming liquid, and the repair liquid applied last may be the topcoat layer forming liquid. In addition, the primer layer forming liquid applied last or the topcoat layer forming liquid applied first may be called the repair liquid. However, as long as the steps of the present invention are carried out, the liquid used in each step is included within the scope of the present invention, regardless of the name of the liquid. EXAMPLES
[0111] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to these examples as long as it does not depart from the gist of the present invention.
[0112] Example 1 <Drain> As shown in the example in Figure 2 (left), the grating covering the 25 cm wide drain 11 that runs through the floor of a commercial kitchen was removed (Figure 5 (a)). A drain pipe 14 made of polyvinyl chloride and with a diameter of 75 mm was connected to the drain 11 on both sides (Figure 2 (left)). In order to prevent the kitchen area (countertop, refrigerator, sink, etc.) from getting dirty, we used masking sheets and tape to protect the area (Figure 5(a)).
[0113] <<Process (1)>> First, the "waste containing oil" in the drain 11 was removed with hands and a ladle, and then the drain was cleaned with a scraper. A balloon was inserted into the drain pipe 14 connected to the drain 11 to block the drain pipe 14 (a ball was attached). Next, the inner surface 11a of the drainage groove 11 was subjected to high-pressure cleaning using a water jet (FIG. 5(b)).
[0114] <<Process (2)>> The oily dirt on the inner surface 11a of the drain 11 was removed using a strong alkaline cleaner having a pH of 14, which contained an anionic alkyl sulfate surfactant, propylene glycol monoethyl ether, sodium hydroxide, and water.
[0115] Thereafter, air was blown by a blower to dry it, and the inner surface 11a of the drainage groove 11 was further dried by a torch burner.
[0116] <<Process (3)>> Any unevenness or gaps present on the inner surface 11a of the drainage groove 11 were filled using a thermosetting epoxy resin. The joint with the drain pipe 14 was reinforced with the thermosetting epoxy resin.
[0117] <<Process (4)>> <<<Composition of primer layer forming solution>>> Each component of the primer layer forming liquid was put into a container and mixed uniformly with a mixer. The composition of the primer layer forming liquid was the same as that of the repair liquid described below, except that the thixotropy imparting powder and colorant were removed and the amount of BPO (polymerization initiator) was doubled.
[0118] The temperature of the inner surface 11a of the drain 11 to be repaired was measured and found to be 22°C. Immediately after preparation of the primer layer forming liquid, the liquid was applied to the drainage groove 11 using a brush to form a primer layer 16 (FIG. 5(c)). The adhesion weight of the primer layer 16 is 200 g / m 2 Although it did not contain any thixotropy-imparting powder, the coating film was thin and the liquid did not drip.
[0119] <<Process (5)>> Next, the "repair liquid components" shown below were placed in a container and mixed uniformly using a mixer. No solvent was used.
[0120] <<<Repair fluid composition>>> MMA 100 parts by mass BPO (polymerization initiator) 2 parts by mass Curing accelerator 2 parts by weight Sepiolite (hydrated magnesium silicate) (thixotropic powder) 5 parts by weight Silica sand (inorganic filler) 100 parts by weight Colorant 15 parts by weight
[0121] Immediately after preparation, the repair liquid was applied using a brush onto the primer layer 16 (FIG. 5(d)). The repair liquid was also applied to the "recesses on the edges of both ends of the upper part of the drainage ditch" for placing the grating.
[0122] The repair structure 17 was formed by applying the repair liquid four times. The first coat weight is 400g / m 2 The deposition weights for the second to fourth coats were 300 g / m 2 In total, 1300g / m 2 A repair structure 17 was formed (FIG. 5(e)). The paint was applied as thickly as possible using a brush without dripping. After the repair liquid was applied, the above-mentioned paraffin phenomenon was observed on the surface of the repair structure 17 during hardening.
[0123] <<Process (6)>> <<<Topcoat layer formation liquid composition>>> Next, each component of the topcoat layer forming solution was placed in a container and stirred with a mixer to mix uniformly. The composition of the topcoat layer forming liquid was the same as that of the repair liquid, but with the addition of a polyfunctional (meth)acrylic acid ester as an additional polymerizable compound, to increase the surface hardness (to make it hard) after curing.
[0124] The topcoat layer forming liquid was applied in two separate applications to form the topcoat layer 18 (FIG. 5(f)). The total amount of the topcoat layer applied in the first and second applications was 300 g / m 2 The second top coat layer forming liquid did not contain a colorant.
[0125] All layers including the repair structure 17 were allowed to solidify over time. The time required for solidification (curing time) was 10 minutes since the temperature of the substrate was 22°C. The total adhesion weight of the three layers was 1800 g / m 2 The solidification of the repair structure 17 (polymerization (hardening) of MMA) proceeded smoothly without being affected by the water in the base or the oxygen in the air. The balloon was then removed, a water flow test was conducted, and a grating was placed on drain 11 to complete the repair.
[0126] <<Time required for the entire process>> As mentioned above, all of steps (1) to (6) were carried out, and at the same time, the grease trap 12 and the inverted manhole 13 were also repaired. Furthermore, curing, cleaning with a scraper, inserting a balloon to block the drain pipe 14, drying with a torch burner, mixing each liquid, allowing time for solidification, running water tests, removing the curing, etc. were all completed between 22:00 and 6:00. The restaurant was able to operate as usual the next day.
[0127] <<Condition after process>> The structure in which MMA was polymerized (the structure in which the repaired structure had solidified) had good adhesion to both concrete (mortar) and polyvinyl chloride, so the joints between them bonded well, and after the repair, the inside of the drain 11 had excellent waterproofing, durability, etc.
[0128] On the other hand, when epoxy resin was used, the workability was good because the base dried easily, but the drain pipe 14 made of polyvinyl chloride easily came out of the drain 11 made of concrete. Also, the repaired parts of the inner surface of the drain only lasted about three years, and the repairs were only temporary. Furthermore, when using a urethane-based resin, it takes three days to form the three layers of the primer layer, main layer (middle coat), and top coat layer, making it unsuitable for repairing a kitchen drain 11.
[0129] Example 2 <Grease trap> As shown in the example of FIG. 2, the inner surface 12a of a grease trap 12 connected to a drain 11 or an inverted manhole 13 in a floor of a commercial kitchen was repaired. Each step was the same as that of the drain ditch 11 of Example 1. Except for using a grease trap 12 instead of the drain ditch 11 of Example 1, the inner surface 12a of the grease trap 12 was repaired in the same manner as in Example 1.
[0130] The time required for the entire process, including repairs to the drain ditch 11 and the invert manhole 13, was completed within the time described in Example 1. As for the condition after the process, as described in Example 1, after the repair, the inside of the grease trap 12 had excellent waterproofing, durability, etc.
[0131] Example 3 <Inverted box> As an example shown in Figure 2 (right), the inner surface 13a of an inverted box 13 in the floor of a commercial kitchen was repaired. Each step was the same as that of the drain ditch 11 of Example 1. Except for using an inverted manhole 13 instead of the drain ditch 11 of Example 1, the inner surface 13a of the inverted manhole 13 was repaired in the same manner as in Example 1. 6(a) to (g) show photographs taken during or after each step.
[0132] The time required for the entire process, including repairs to the drain 11 and the grease trap 12, was completed within the time described in Example 1. As for the condition after the process, as described in Example 1, after the repair, the inside of the inverter box 13 had excellent waterproofing, durability, etc. [Industrial Applicability]
[0133] The interior surface repair method of the present invention, the repaired drains, grease traps and invert manholes, and the repair liquid used therein are widely used in the construction industry; the installation, management, inspection, repair and cleaning of kitchens, sewers, etc.; the business industry, such as cafeterias and restaurants; and the manufacturing industry of construction materials such as adhesives, paints and sealants. [Explanation of symbols]
[0134] 11. Drain 11a Inner surface of drain 12 Grease trap 12a Inside of grease trap 13 Inverted box 13a Inner surface of inverted box 13b Drain passage recess 13c Seam 14 Drain pipe 15 Inner surface (formed of concrete or mortar) 16 Primer layer 17 Repair structure (after hardening) 18 Topcoat layer< / ph>
Claims
1. A method for repairing the inner surface of a drain, grease trap, or invert manhole that is present on a kitchen floor and whose inner surface is made of concrete or mortar, comprising the steps of: (2) removing oily dirt from the inner surface using a strong alkaline cleaner having a pH of 11 or more, which contains a surfactant, a water-soluble organic solvent, and water; (4) applying a primer layer forming liquid containing methyl methacrylate and a radical polymerization initiator to form a primer layer; and (5) applying a repair liquid containing methyl methacrylate, a radical polymerization initiator, and a thixotropy-imparting powder to the inner surface to form a repair structure, and then solidifying the repair liquid over time; An inner surface repair method comprising the steps of:
2. Prior to the step (2), (1) performing high-pressure cleaning of the inner surface by jetting water; The method for repairing an inner surface according to claim 1, further comprising the steps of:
3. Prior to the step (4), (3) filling any irregularities and / or gaps present on the inner surface with a thermosetting epoxy resin; The method for repairing an inner surface according to claim 1, further comprising the steps of:
4. After the step (5), (6) applying a topcoat layer forming liquid containing methyl methacrylate and a radical polymerization initiator to form a topcoat layer; The method for repairing an inner surface according to claim 1, further comprising the steps of:
5. The method for repairing an inner surface according to claim 1 , wherein the primer layer forming liquid and / or the repair liquid further contains an inorganic filler.
6. The inner surface repair method according to claim 5, wherein the primer layer forming liquid and / or the repair liquid contains the inorganic filler in an amount of 30 parts by mass or more and 160 parts by mass or less per 100 parts by mass of methyl methacrylate in the primer layer forming liquid or per 100 parts by mass of methyl methacrylate in the repair liquid.
7. 2. The method for repairing an inner surface according to claim 1, wherein the radical polymerization initiator is an organic peroxide.
8. 2. The method of claim 1, wherein the repair fluid is substantially free of diluting solvents.
9. The repair liquid is 500 g / m 2 More than 3000g / m 2 The method of claim 1 , further comprising forming the repair structure by applying to the interior surface:
10. The method for repairing an inner surface according to claim 1 , wherein the repair liquid is applied to the inner surface using a brush or a spray device.
11. When the primer layer, the repair structure, and the topcoat layer are formed, the total adhesion amount of the primer layer, the repair structure, and the topcoat layer is 700 g / m 2 More than 5000g / m 2 The method for repairing an inner surface according to claim 4, wherein:
12. 2. The method for repairing an inner surface according to claim 1, wherein the repair is completed in any time period between 9:00 p.m. and 9:00 a.m. the following day.
13. A drain, grease trap, or invert manhole after repair using the inner surface repair method described in any one of claims 1 to 12, wherein the inner surface of the drain, grease trap, or invert manhole has a "hardened repair structure containing at least a methyl methacrylate polymer, a thixotropy-imparting powder, and an inorganic filler."
14. A repair fluid for use in the inner surface repair method according to any one of claims 1 to 12.
Citation Information
Patent Citations
Regeneration method for sewage attaching pipe and repairing apparatus
JP1999107360A
Method for manufacturing catch basin
JP2001132083A
Socket for gully
JP2008297772A
Method and basin for repairing catch basin
JP2010281049A
Connection structure of sewer pipe and intermediate structure
JP2013040477A