Manufacturing method of battery

The use of a rotary brush to remove foreign matter from the electrode stack cross section addresses the issues of burrs and scratches, enhancing battery manufacturing quality.

JP2024158105AInactive Publication Date: 2024-11-08TOYOTA JIDOSHA KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023072989
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing battery manufacturing methods result in the generation of metal burrs during cutting, leading to potential short circuits and scratches on the electrode stack cross section.

Method used

A method involving a rotary brush with brush portions rotated parallel to the stacking direction to remove foreign matter from the electrode stack cross section, while minimizing scratches.

Benefits of technology

Effectively removes foreign matter without causing damage to the electrode laminate, reducing the risk of short circuits and scratches.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158105000001_ABST
    Figure 2024158105000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a battery capable of removing foreign matter such as burrs while suppressing damages from generating on a cross-section of an electrode lamination body even if the foreign matter is generated at the time of integrally cutting the electrode lamination body.SOLUTION: The present disclosure relates to a manufacturing method of a battery, comprising: a preparation step of preparing an electrode lamination body in which a positive electrode layer, a solid electrolyte layer, and a negative electrode layer are laminated in this order; a cutting step of forming a cross-section by integrally cutting the electrode lamination body along a lamination direction of the electrode lamination body; and a foreign matter removing step of removing foreign matter existing on the cross-section of the electrode lamination body by bringing a plurality of brush parts provided around a shaft part into contact with the cross-section of the electrode lamination body while rotating a rotational brush having the shaft part and the brush parts, with a direction parallel to the lamination direction as a rotational axis. In the foreign matter removing step, the foreign matter is removed from the cross-section of the electrode lamination body while removing the foreign matter adhered to the brush parts.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a battery. [Background technology]

[0002] Patent Document 1 discloses a method for manufacturing a battery member for a secondary battery, which includes a step of forming a laminate by providing an electrolyte material layer between a pair of electrode material layers, and a step of cutting the laminate all at once. Patent Document 1 also describes that by including the cutting step, a substantially continuous surface is formed on the side surface of the laminate. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2019 / 221010 Summary of the Invention [Problem to be solved by the invention]

[0004] When the electrode laminate is cut in one go, burrs (protrusions) may occur at the cut portion, for example, metal burrs may occur on the current collector. In addition, since the cross section of the electrode laminate is substantially flush, the end face distance between the positive and negative electrodes is shortened. Therefore, foreign matter such as metal burrs present on the cross section of the electrode laminate is likely to cause a short circuit. For example, a brush may be used to remove the foreign matter, but when the foreign matter is removed using a brush, scratches (drag scratches caused by the foreign matter) may occur on the cross section of the electrode laminate.

[0005] The present disclosure has been made in consideration of the above problems, and has as its main object to provide a battery manufacturing method capable of removing foreign matter (such as metal burrs) generated during bulk cutting of an electrode stack while suppressing the occurrence of scratches on the cross section of the electrode stack. [Means for solving the problem]

[0006] [1] A method for manufacturing a battery, comprising: a preparation step of preparing an electrode laminate in which a positive electrode layer, a solid electrolyte layer, and a negative electrode layer are laminated in this order; a cutting step of cutting the electrode stack in one go along a stacking direction of the electrode stack to form a cross section; a foreign matter removal process for removing foreign matter present on a cross section of the electrode laminate by rotating a rotating brush having a shaft portion and a plurality of brush portions provided around the shaft portion, the brush portions being brought into contact with the cross section of the electrode laminate while rotating the rotating brush about a rotation axis parallel to the lamination direction, The method for manufacturing a battery, wherein in the foreign matter removing step, the foreign matter is removed from a cross section of the electrode stack while removing the foreign matter adhering to the brush portion. Effect of the Invention

[0007] According to the battery manufacturing method of the present disclosure, it is possible to remove foreign matter while preventing scratches from occurring on the cross section of the electrode stack, and therefore it is possible to manufacture a battery capable of preventing short circuits. [Brief description of the drawings]

[0008] [Figure 1] 4 is a schematic cross-sectional view illustrating an electrode stack after a cutting step in the present disclosure. FIG. [Diagram 2] 4 is a schematic cross-sectional view illustrating a foreign matter removing step in the present disclosure. FIG. [Diagram 3] 4 is a schematic cross-sectional view illustrating a foreign matter removing step in the present disclosure. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present disclosure will be described in detail below with reference to the drawings. The drawings are merely examples, and the size and shape of each part may be exaggerated to facilitate understanding.

[0010] The present disclosure provides a battery manufacturing method including: a preparation step of preparing an electrode laminate having a positive electrode layer, a solid electrolyte layer, and a negative electrode layer stacked in this order; a cutting step of cutting the electrode laminate all at once along the stacking direction of the electrode laminate to form a cross section; and a foreign matter removal step of rotating a rotating brush having a shaft portion and a plurality of brush portions provided around the shaft portion around a rotation axis parallel to the stacking direction while bringing the brush portions into contact with the cross section of the electrode laminate to remove foreign matter present on the cross section of the electrode laminate, in which the foreign matter removing step removes the foreign matter from the cross section of the electrode laminate while removing the foreign matter adhering to the brush portions.

[0011] According to the present disclosure, in the foreign matter removal step, the rotating brush is rotated around a rotation axis parallel to the lamination direction while the brush part is brought into contact with the cross section of the electrode laminate, thereby removing foreign matter such as metal burrs while suppressing the occurrence of scratches. Furthermore, by performing the foreign matter removal step while removing foreign matter attached to the brush part, the electrode laminate can always be cleaned with a clean brush, thereby suppressing the re-adhesion of foreign matter. In addition, the occurrence of scratches on the cross section of the electrode laminate due to foreign matter attached to the rotating brush can be suppressed. Furthermore, in the case of performing continuous processing, the cross section of the next electrode laminate can be cleaned with a clean brush, so that the collected foreign matter is less likely to have an adverse effect. Each step will be described in detail below.

[0012] 1. Preparation process This step is a step of preparing an electrode laminate in which a positive electrode layer, a solid electrolyte layer, and a negative electrode layer are laminated in this order. The electrode laminate may include a positive electrode current collector that collects current from the positive electrode layer. The electrode laminate may include a negative electrode current collector that collects current from the negative electrode layer.

[0013] The positive electrode layer contains at least a positive electrode active material, and may contain at least one of a solid electrolyte, a conductive material, and a binder, as necessary. Examples of the positive electrode active material include lithium cobalt oxide, lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese oxide (NCM), and lithium manganese oxide. Examples of the conductive material include carbon materials. Examples of the solid electrolyte include those described below. Examples of the binder include rubber-based binders and fluoride-based binders.

[0014] The negative electrode layer contains at least a negative electrode active material, and may contain at least one of a solid electrolyte, a conductive material, and a binder, as necessary. Examples of the negative electrode active material include silicon-based active materials such as Si and Si alloys, tin and tin alloys, silicon oxide, and the like, carbon-based active materials such as graphite and hard carbon, various oxide-based active materials such as lithium titanate, metallic lithium, and lithium alloys.

[0015] The solid electrolyte layer contains at least a solid electrolyte, such as a sulfide solid electrolyte, an oxide solid electrolyte, a nitride solid electrolyte, or a halide solid electrolyte.

[0016] The material of the positive electrode current collector is not particularly limited, and may be, for example, a metal such as aluminum, SUS, or nickel. The thickness of the positive electrode current collector layer is not particularly limited, and may be, for example, in the range of 0.1 μm or more and 1 mm or less. The material of the negative electrode current collector is not particularly limited, and may be, for example, a metal such as copper, SUS, or nickel. The thickness of the negative electrode current collector layer is not particularly limited, and may be, for example, in the range of 0.1 μm or more and 1 mm or less.

[0017] The electrode laminate has a positive electrode layer, a solid electrolyte layer, and a negative electrode layer in this order in the lamination direction. When a set of a positive electrode layer, a solid electrolyte layer, and a negative electrode layer is a power generation unit, the electrode laminate may have only one power generation unit, or may have two or more power generation units. When the electrode laminate has two or more power generation units, the power generation units may be connected in series or in parallel.

[0018] 2.Cutting process This step is a step of cutting the electrode laminate in one go along the stacking direction to form a cross section of the electrode laminate. Specifically, at least the ends of the positive electrode layer, the solid electrolyte layer, and the negative electrode layer are cut in one go. FIG. 1 is a schematic cross-sectional view illustrating an example of an electrode laminate after the cutting step. The electrode laminate 10 in FIG. 1 has a substantially uniform cross section S. Metal burrs may occur on the cross section S. The metal burrs are formed so as to face the cutting direction (stacking direction).

[0019] The electrode laminate can be cut in one go using, for example, a cutting device equipped with a saw blade. The saw blade is preferably a circular saw blade, since this can suppress the generation of foreign matter during cutting. The electrode laminate may be cut in one go into any shape when viewed in plan.

[0020] The electrode laminate 10 shown in FIG. 1 has two power generation units connected in parallel, and has a negative electrode current collector 1, a first negative electrode layer 2a, a first solid electrolyte layer 3a, a first positive electrode layer 4a, and a first positive electrode current collector 5a, which are arranged in this order from one surface s11 of the negative electrode current collector 1, and a second negative electrode layer 2b, a second solid electrolyte layer 3b, a second positive electrode layer 4b, and a second positive electrode current collector 5b, which are arranged in this order from the other surface s12 of the negative electrode current collector 1.

[0021] 3. Foreign matter removal process This process is a process for removing foreign matter present on the cross section of the electrode laminate by rotating a rotating brush having a shaft portion and multiple brush portions provided around the shaft portion, with the brush portions contacting the cross section of the electrode laminate, about a rotation axis parallel to the lamination direction. In the present disclosure, the foreign matter is removed from the electrode laminate while removing the foreign matter adhering to the brush portions.

[0022] 2 is a schematic cross-sectional view illustrating this step. As shown in FIG. 2, the rotating brush 30 has a shaft portion 31 and a plurality of brush portions 32 provided around the shaft portion 31. The brush portions 32 are usually provided upright around the shaft portion 31 in a direction perpendicular to the axial direction of the shaft portion 31. In this step, the rotating brush 30 is rotated in the stacking direction D of the electrode laminate 10. L The brush part 32 is brought into contact with the cross section S while rotating the electrode stack around a rotation axis R parallel to the stack direction. At this time, the brush part 32 rotates in a plane perpendicular to the stack direction. By bringing the brush part into contact with the cross section in this manner, foreign matter can be removed more easily than with conventional non-contact air blowers. In addition, by controlling the rotation direction of the rotating brush as described above, the orientation of burrs can be changed, making it easier to remove the burrs. If the rotating brush is rotated around a rotation axis in a direction that is shifted from the direction parallel to the stack direction, scratches may occur on the cross section of the electrode stack.

[0023] In this step, foreign matter adhering to the brush part is removed while foreign matter is removed from the electrode laminate. As a method for removing foreign matter adhering to the brush part, it is preferable to use a brush cleaner 40 having a comb-tooth-shaped protrusion 41 and a main body 42, which are arranged on the opposite side of the electrode laminate 10 with respect to the rotating brush 30, and a suction device 50, as shown in FIG. 2. By passing the brush part 32 of the rotating brush 30 through the brush cleaner 40 having the comb-tooth-shaped protrusion 41, it is possible to remove foreign matter entangled in the brush part 32. Furthermore, the suction device 50 can suck and collect the foreign matter collected on the brush cleaner 40.

[0024] The diameter of the brush part of the rotating brush is, for example, 30 μm or more, and may be 50 μm or more. On the other hand, it may be 80 μm or less. The material of the brush part is not particularly limited, but it is preferable that the brush part is made of an insulating material such as a resin. Examples of the resin include polypropylene.

[0025] Fig. 3(a) is an enlarged cross-sectional view showing an example of a contact portion between the rotating brush and the electrode laminate in this step. As shown in Fig. 3(a), in this step, it is preferable to bring the brush portion 32 into contact with the cross section S of the electrode laminate 10 by pressing it against the cross section S. Specifically, it is preferable to press the rotating brush 30 against the electrode laminate 10 so that the distance D between the shaft portion 31 of the rotating brush 30 and the cross section S of the electrode laminate 10 is smaller than the length of the brush portion 32. By pressing the rotating brush against the electrode laminate in this way, the distance between the brush portions becomes smaller than the size of the foreign matter, making it easier to remove the foreign matter.

[0026] The rotation speed of the rotating brush may be, for example, 70 rpm or more, or 100 rpm or more. On the other hand, the rotation speed may be, for example, 200 rpm or less, or 150 rpm or less. In this step, in order to perform continuous processing, it is preferable that the electrode laminate moves linearly. The speed of the linear movement is, for example, 50 mm / s or more. On the other hand, it is, for example, 100 mm / s or less.

[0027] Fig. 3(b) is an enlarged cross-sectional view showing an example of the contact portion between the brush cleaner and the rotating brush in this step. As shown in Fig. 3(b), it is preferable that the brush portion 32 of the rotating brush 30 is inserted into the brush cleaner 40 in a fully extended state. This is because foreign matter entangled in the brush portion 32 can be easily removed. Then, as shown in Figs. 2 and 3(c), when the suction device 50 is operated, a negative pressure is created in the suction nozzle 51 of the suction device 50, and the foreign matter X collected on the brush cleaner 40 is collected. The suction pressure is, for example, -10 kPa or less.

[0028] An example of the material for the protrusions 41 and the main body 42 of the brush cleaner is resin. The pitch of the protrusions 41 (the distance between adjacent protrusions 41) is, for example, preferably 1 mm or less, and more preferably 0.5 mm or less.

[0029] In the present disclosure, for example, the electrode laminate after the foreign matter removal step is housed inside an exterior body, and the exterior body is sealed to manufacture a battery. The battery may be an all-solid-state battery. The type of the battery is not particularly limited, and may be, for example, a lithium ion secondary battery.

[0030] The present disclosure is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any configuration that is substantially the same as the technical idea described in the claims of the present disclosure and that exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES

[0031] Comparative Example 1 An electrode laminate was prepared by laminating a positive electrode layer, a solid electrolyte layer, and a negative electrode layer in this order. Next, the electrode laminate was cut all at once along the lamination direction to form a cross section. Next, a brush having a brush part was pressed against the cross section of the electrode laminate so that the brush part was in contact with the cross section of the electrode laminate, while the electrode laminate was moved linearly at a speed of 50 mm / s, thereby cleaning the cross section of the electrode laminate.

[0032] Comparative Example 2 An electrode laminate was prepared and cut in one go along the lamination direction in the same manner as in Comparative Example 1. Next, a rotating brush having a shaft part and a brush part was rotated at 100 rpm with a direction parallel to the lamination direction as the rotation axis, while the brush part was brought into contact with the cross section of the electrode laminate, and the electrode laminate was moved linearly at a speed of 50 mm / s to clean the cross section of the electrode laminate.

[0033] Comparative Example 3 The electrode laminate was prepared in the same manner as in Comparative Example 1, and cut in one go along the lamination direction. Next, a rotating brush having a shaft part and a brush part was rotated at 100 rpm with a direction parallel to the lamination direction as a rotation axis, and the electrode laminate was moved linearly at a speed of 50 mm / s while the brush part was in contact with the cross section of the electrode laminate, thereby cleaning the cross section of the electrode laminate. At this time, a suction device was placed on the opposite side of the rotating brush from the electrode laminate side, and the rotating brush was sucked.

[0034] (Example) The electrode laminate was prepared in the same manner as in Comparative Example 1, and the electrode laminate was cut in one go along the stacking direction to form a cross section. L The electrode laminate was rotated at 100 rpm with a rotation axis R parallel to the direction of rotation, and the electrode laminate was moved linearly at a speed of 50 mm / s while the brush portion 32 was in contact with the cross section of the electrode laminate 10. In this manner, the cross section of the electrode laminate was cleaned. At this time, as shown in Fig. 2, a brush cleaner 40 and a suction device 50 were placed on the opposite side of the electrode laminate 10 side with respect to the rotating brush 30, and the suction pressure of the suction device was set to -20 kPa, and the cross section of the electrode laminate was cleaned while removing foreign matter adhering to the brush portion.

[0035] (evaluation) In Comparative Examples 1 to 3 and Example 1, after cleaning, an evaluation was made as to whether or not foreign matter had been removed from the cross section of the electrode laminate, and whether or not scratches had occurred on the cross section of the electrode. The results are shown in Table 1.

[0036] [Table 1]

[0037] It was confirmed that the foreign matter on the cross section of the electrode laminate was removed in Comparative Examples 1 to 3 and the Example. In the Example, no scratches were generated on the cross section of the electrode laminate (evaluation ◯). On the other hand, in Comparative Example 1, the brush dragged the foreign matter, causing scratches on the cross section of the electrode laminate (evaluation ×). In Comparative Example 2, scratches were generated partially due to foreign matter attached to the rotating brush (evaluation △). In Comparative Example 3, foreign matter entangled in the brush could not be removed, causing partial scratches similar to Comparative Example 2 (evaluation △). [Explanation of symbols]

[0038] 10...Electrode laminate 30...Rotary brush 40…Brush cleaner 50...Suction device

Claims

[Claim 1] A method for manufacturing a battery, comprising: a preparation step of preparing an electrode laminate in which a positive electrode layer, a solid electrolyte layer, and a negative electrode layer are laminated in this order; a cutting step of cutting the electrode stack in one go along a stacking direction of the electrode stack to form a cross section; a foreign matter removal process for removing foreign matter present on a cross section of the electrode laminate by rotating a rotating brush having a shaft portion and a plurality of brush portions provided around the shaft portion, the brush portions being brought into contact with the cross section of the electrode laminate while rotating the rotating brush about a rotation axis parallel to the lamination direction, The method for manufacturing a battery, wherein in the foreign matter removing step, the foreign matter is removed from a cross section of the electrode stack while removing the foreign matter adhering to the brush portion.

Citation Information

Patent Citations

  • Method for manufacturing battery member for secondary battery, and secondary battery

    WO2019221010A1