Polyarylene sulfide resin composition, molded product and method for producing the same

By extracting and incorporating cyclic PAS oligomers into the resin composition through controlled purification and blending, the method addresses the balance between crystallization speed and melt viscosity, enhancing processability and sustainability in PAS resin production.

JP2024158232APending Publication Date: 2024-11-08DIC CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023073258
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing polyarylene sulfide (PAS) resin compositions face challenges in achieving a balance between crystallization speed and melt viscosity while effectively utilizing PAS oligomers, leading to processability issues and environmental inefficiencies due to the disposal of by-products like PAS oligomers.

Method used

A method is developed to extract and utilize cyclic PAS oligomers, specifically hexamers, by purifying them from the polymerization process and blending them with PAS resin, involving steps of solid-liquid separation and controlled cooling to maintain a viscosity change within ±20%, thereby enhancing the resin composition's properties.

Benefits of technology

The resulting resin composition achieves an excellent balance between crystallization rate and melt viscosity, improving processability and environmental sustainability by recycling otherwise discarded oligomers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158232000001
    Figure 2024158232000001
  • Figure 2024158232000002
    Figure 2024158232000002
  • Figure 2024158232000003
    Figure 2024158232000003
Patent Text Reader

Abstract

To provide a resin composition having an excellent balance between crystallization speed and melt viscosity by utilizing a polyarylene sulfide (PAS) oligomer, a molded product and a method for producing the same.SOLUTION: There is provided a resin composition which is a PAS resin composition obtained by blending PAS and a cyclic PAS oligomer as essential components, wherein PAS has a linear structure in which an aromatic ring and a sulfur atom are bonded in a para position and the cyclic PAS oligomer is a hexamer and is produced by a method comprising the steps of: reacting a dihaloaromatic compound with a sulfidizing agent in an organic polar solvent to obtain a crude reaction mixture; subjecting the crude reaction mixture to solid-liquid separation to obtain a reaction mixture containing at least a cyclic PAS oligomer; subjecting the reaction mixture to solid-liquid separation to obtain a rection mixture containing a cyclic PAS oligomer; bringing the reaction mixture into contact with an organic polar solvent to obtain a liquid phase component; and gradually cooling the liquid phase component to 25°C or less to recover a crystallized solid-phase component. A molded product; and a method for producing the resin composition and molded product.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a polyarylene sulfide resin composition, a molded article, and a method for producing the same. [Background technology]

[0002] Polyarylene sulfide (PAS) resins, such as polyphenylene sulfide (PPS), have excellent heat and chemical resistance and are widely used in electrical and electronic components, automotive parts, water heater parts, fibers, films, and other applications.

[0003] PAS resins are obtained by polymerization of a sulfidizing agent and a polyhaloaromatic compound in a polar organic solvent such as N-methyl-2-pyrrolidone (NMP). This process also produces by-products such as oligoarylene sulfides (hereinafter referred to as PAS oligomers), residual sulfidizing agents, and sodium chloride. These by-products have been considered impurities and have not been utilized to date. In particular, most of the PAS oligomers contained in the liquid phase obtained by solid-liquid separation of the solvent slurry after polymerization have been discarded as industrial waste, resulting in significant losses in production due to raw material and disposal costs. Furthermore, this process lacks consideration for the global environment, as it does not effectively utilize limited resources.

[0004] As an attempt to incorporate a PAS oligomer as a raw material for a PAS resin composition, for example, Patent Document 1 discloses a resin composition comprising a PAS resin, a PAS oligomer having at least one SH terminal and a molecular weight of 2,000 or less, and an alkoxysilane compound. However, cyclic PAS oligomers can thicken during melt-kneading due to ring-opening polymerization and slow the crystallization rate of the resin composition. Due to concerns about processability and mechanical properties, their use as a raw material for PAS resin compositions has been limited. Known techniques for controlling the reactivity of cyclic PAS oligomers during heating include incorporating an organic carboxylic acid compound (e.g., Patent Document 2), incorporating a low-valent iron compound (e.g., Patent Document 3), and incorporating a copper carboxylate compound (e.g., Patent Document 4). However, these methods have limitations on heating conditions and side reactions with other components. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Laid-Open No. 2001-172500 [Patent Document 2] Japanese Patent Application Laid-Open No. 2011-173953 [Patent Document 3] Japanese Patent Application Laid-Open No. 2012-92315 [Patent Document 4] Japanese Patent Application Laid-Open No. 2016-11382 Summary of the Invention [Problem to be solved by the invention]

[0006] Therefore, the problem that the present invention aims to solve is to provide a resin composition that utilizes a PAS oligomer and has an excellent balance between crystallization rate and melt viscosity while being environmentally friendly, as well as a molded article obtained by melt-molding the resin composition, and a method for producing the same. [Means for solving the problem]

[0007] As a result of extensive investigations, the inventors of the present application discovered that the above-mentioned problems could be solved by extracting only cyclic and hexameric PAS oligomers from the PAS oligomers that are by-produced during the polymerization of PAS and blending them with PAS, thereby completing the present invention.

[0008] That is, the present disclosure: A PAS resin composition comprising a PAS (A) and a cyclic PAS oligomer (B) as essential components, the PAS (A) has, as a repeating unit, a linear structure in which an aromatic ring and a sulfur atom are bonded at the para position, The cyclic PAS oligomer (B) is a hexamer, and (1) a step of reacting a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide, in an organic polar solvent (1) to obtain a crude reaction mixture containing a PAS (a), a cyclic PAS oligomer (B), the organic polar solvent (1), and an alkali metal halide; a step (2) of subjecting the crude reaction mixture to solid-liquid separation to obtain a reaction mixture (L1) containing at least the cyclic PAS oligomer (B) and the organic polar solvent (1); a step (3) of performing solid-liquid separation of the organic polar solvent (1) from the reaction mixture (L1) to obtain a reaction mixture (S1) containing at least the cyclic PAS oligomer (B); a step (4) of contacting the reaction mixture (S1) with an organic polar solvent (2) to obtain a mixture (L2); A step (5) of subjecting the mixture (L2) to solid-liquid separation in a temperature range higher than the boiling point of the organic polar solvent (2) minus 10°C to recover a liquid phase component (L3); and The liquid phase component (L3) is gradually cooled to 25°C or less, and a crystallized solid phase component is recovered (6). The present invention relates to a PAS resin composition characterized by a viscosity change rate within the range of ±20%.

[0009] The present disclosure further relates to a molded article obtained by melt molding the above-described PAS resin composition.

[0010] Further, the present disclosure provides: A method for producing a PAS resin composition, comprising a step of blending a PAS (A) and a cyclic PAS oligomer (B) as essential components, and melt-kneading the mixture at a temperature equal to or higher than the melting point of the PAS (A), the PAS (A) has, as a repeating unit, a linear structure in which an aromatic ring and a sulfur atom are bonded at the para position, The cyclic PAS oligomer (B) is a hexamer, and (1) A step of reacting a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide, in an organic polar solvent (1) to obtain a crude reaction mixture containing PAS (a), a cyclic PAS oligomer (B), the organic polar solvent (1), and an alkali metal halide. a step (2) of subjecting the crude reaction mixture to solid-liquid separation to obtain a reaction mixture (L1) containing at least the cyclic PAS oligomer (B) and the organic polar solvent (1); a step (3) of subjecting the organic polar solvent (1) to solid-liquid separation from the reaction mixture (L1) to obtain a reaction mixture (S1) containing at least the cyclic PAS oligomer (B); a step (4) of contacting the reaction mixture (S1) with an organic polar solvent (2) to obtain a mixture (L2); A step (5) of subjecting the mixture (L2) to solid-liquid separation in a temperature range higher than the boiling point of the organic polar solvent (2) minus 10°C to recover a liquid phase component (L3); and The liquid phase component (L3) is gradually cooled to 25°C or less, and a crystallized solid phase component is recovered (6). The present invention relates to a method for producing a PAS resin composition, characterized in that the viscosity change rate is within a range of ±20%.

[0011] The present disclosure further relates to a method for producing a PAS resin molded article, comprising the steps of producing a resin composition by the above-described method and melt-molding the resin composition.

[0012] In the present invention, a compound having a repeat number of 2 to 40 (a mixture of dimers to 40-mers) may be referred to as an "oligomer," and a compound having a repeat number of 41 or more may be referred to as a "polymer." [Effects of the Invention]

[0013] According to the present invention, by utilizing a PAS oligomer, it is possible to provide a resin composition that is environmentally friendly and has an excellent balance between crystallization rate and melt viscosity, as well as a molded article obtained by melt-molding the resin composition, and a method for producing the same. DETAILED DESCRIPTION OF THE INVENTION

[0014] Hereinafter, one embodiment of the present invention will be described in detail, but the scope of the present invention is not limited to the embodiment described here, and various modifications can be made without departing from the spirit of the present invention. Furthermore, when multiple upper and lower limit values ​​are specified for a specific parameter, any upper and lower limit values ​​can be combined to form a suitable numerical range.

[0015] <Resin composition> The resin composition according to the present embodiment is a PAS resin composition containing a PAS (A) and a cyclic PAS oligomer (B) as essential components, the PAS (A) has, as a repeating unit, a linear structure in which an aromatic ring and a sulfur atom are bonded at the para position, The cyclic PAS oligomer (B) is a hexamer, and (1) A step of reacting a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide, in an organic polar solvent (1) to obtain a crude reaction mixture containing PAS (a), a cyclic PAS oligomer (B), the organic polar solvent (1), and an alkali metal halide. a step (2) of subjecting the crude reaction mixture to solid-liquid separation to obtain a reaction mixture (L1) containing at least the cyclic PAS oligomer (B) and the organic polar solvent (1); a step (3) of subjecting the organic polar solvent (1) to solid-liquid separation from the reaction mixture (L1) to obtain a reaction mixture (S1) containing a cyclic PAS oligomer (B); and a step (4) of contacting the reaction mixture (S1) with an organic polar solvent (2) to obtain a mixture (L2); A step (5) of subjecting the mixture (L2) to solid-liquid separation in a temperature range higher than the boiling point of the organic polar solvent (2) minus 10°C to recover a liquid phase component (L3); and The liquid phase component (L3) is gradually cooled to 25°C or less, and a crystallized solid phase component is recovered (6). The melt viscosity (V6) of the resin composition is within a range of ±20% of the melt viscosity (V6) of the PAS (A).

[0016] <PAS(A)> The PAS resin composition according to this embodiment contains PAS (A) as an essential component.

[0017] The PAS (A) applicable to this embodiment is a polymer having a resin structure in which a repeating unit has a structure in which an aromatic ring and a sulfur atom are bonded at the para position, and specifically, a polymer represented by the following general formula (1):

[0018] [ka] (In the formula, R 1 and R 2 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a nitro group, an amino group, a phenyl group, a methoxy group, or an ethoxy group.

[0019] Here, the structural moiety represented by the general formula (1) is particularly R 1 and R 2 is preferably a hydrogen atom from the viewpoint of the mechanical strength of the PAS (A), and in that case, is bonded at the para position represented by the following formula (2).

[0020] [ka]

[0021] The PAS (A) may contain not only the structural moieties represented by the general formulas (1) and (2) but also the structural moieties represented by the following structural formulas (3) to (6):

[0022] [ka] The structural moieties represented by the general formula (1) and the general formula (2) may account for 30 mol % or less of the total of the structural moieties represented by the general formula (1) and the general formula (2). In particular, in the present disclosure, it is preferred that the structural moieties represented by the general formulae (3) to (6) account for 10 mol % or less from the viewpoint of the heat resistance and mechanical strength of the PAS (A). When the PAS (A) contains the structural moieties represented by the general formulae (3) to (6), the bonding mode thereof may be either a random copolymer or a block copolymer.

[0023] Furthermore, the PAS (A) may have naphthyl sulfide bonds or the like in its molecular structure, but the amount of such bonds is preferably 3 mol % or less, and particularly preferably 1 mol % or less, relative to the total number of moles including other structural moieties.

[0024] The physical properties of the PAS (A) are not particularly limited as long as they do not impair the effects of the present invention, but are as follows.

[0025] (melt viscosity) The melt viscosity of the PAS (A) used in the present disclosure is not particularly limited, but in order to obtain a good balance between fluidity and mechanical strength, the melt viscosity (V6) measured at 300°C is preferably in the range of 2 Pa·s or more, more preferably 5 Pa·s or more, and preferably 500 Pa·s or less, more preferably 200 Pa·s or less. The most suitable range is 5 Pa·s or more to 100 Pa·s or less. However, the melt viscosity (V6) is measured using a Shimadzu flow tester, CFT-500D, at 300°C with a load of 1.96×10 6The melt viscosity is measured after holding the sample at a pressure of 10 Pa and L / D=10 (mm) / 1 (mm) for 6 minutes.

[0026] (Non-Newtonian exponents) The non-Newtonian index of the PAS (A) used in the present disclosure is not particularly limited, but is preferably in the range of 0.90 or more, more preferably 0.95 or more, and preferably 1.50 or less, more preferably 1.20 or less. Such a PAS (A) has excellent mechanical properties, fluidity, and abrasion resistance. In the present disclosure, the non-Newtonian index (N value) is a value calculated using the following formula after measuring the shear rate (SR) and shear stress (SS) using a capillary rheometer under conditions of a melting point of +20°C and an orifice length (L) to orifice diameter (D) ratio of L / D = 40. The closer the non-Newtonian index (N value) is to 1, the more linear the structure is, and the higher the non-Newtonian index (N value), the more branched the structure is.

[0027]

number

[0028] (Manufacturing method) The method for producing the PAS (A) is not particularly limited, but examples include (Production Method 1) a method in which a dihalogenoaromatic compound is polymerized in the presence of sulfur and sodium carbonate, optionally with a polyhalogenoaromatic compound or other copolymerization component; (Production Method 2) a method in which a dihalogenoaromatic compound is polymerized in a polar solvent in the presence of a sulfidizing agent or the like, optionally with a polyhalogenoaromatic compound or other copolymerization component; (Production Method 3) a method in which p-chlorothiophenol is added, optionally with other copolymerization components, and then self-condensed; and (Production Method 4) a method in which a diiodoaromatic compound and elemental sulfur are melt-polymerized under reduced pressure in the presence of a polymerization inhibitor that may have a functional group such as a carboxyl group or an amino group. Among these methods, (Production Method 2) is preferred because it is versatile. During the reaction, an alkali metal salt of a carboxylic acid or sulfonic acid or an alkali hydroxide may be added to adjust the degree of polymerization. Among the above-mentioned (Production Method 2) methods, there is a method for producing PAS by introducing a water-containing sulfidizing agent into a mixture containing a heated organic polar solvent and a dihalogeno aromatic compound at a rate at which water can be removed from the reaction mixture, and then reacting the dihalogeno aromatic compound with the sulfidizing agent in the organic polar solvent, and optionally adding a polyhalogeno aromatic compound, and controlling the amount of water in the reaction system to be in the range of 0.02 to 0.5 moles per mole of the organic polar solvent (see JP-A-07-228699). Particularly preferred is a compound obtained by a method in which a dihalogenoaromatic compound and, if necessary, a polyhalogenoaromatic compound or other copolymerization component are added in the presence of potassium metal sulfide and an aprotic polar organic solvent, and an alkali metal hydrosulfide and an organic acid alkali metal salt are reacted while controlling the organic acid alkali metal salt in the range of 0.01 to 0.9 mol per mol of the sulfur source and the amount of water in the reaction system to 0.02 mol or less per mol of the aprotic polar organic solvent (see WO2010 / 058713 pamphlet).Specific examples of dihalogenoaromatic compounds include p-dihalobenzene, m-dihalobenzene, o-dihalobenzene, 2,5-dihalotoluene, 1,4-dihalonaphthalene, 1-methoxy-2,5-dihalobenzene, 4,4'-dihalobiphenyl, 3,5-dihalobenzoic acid, 2,4-dihalobenzoic acid, 2,5-dihalonitrobenzene, 2,4-dihalonitrobenzene, 2,4-dihaloanisole, p,p'-dihalodiphenyl ether, 4,4'-dihalobenzophenone, 4,4'-di Examples of the polyhalogenoaromatic compounds include 1,2,3-trihalobenzene, 1,2,4-trihalobenzene, 1,3,5-trihalobenzene, 1,2,3,5-tetrahalobenzene, 1,2,4,5-tetrahalobenzene, 1,4,6-trihalonaphthalene, etc. The halogen atoms contained in the above compounds are preferably chlorine atoms or bromine atoms.

[0029] The method for post-treating the reaction mixture containing PAS obtained by the polymerization step is not particularly limited, and examples thereof include: (post-treatment 1) after completion of the polymerization reaction, first distilling off the solvent under reduced pressure or normal pressure, either directly or after adding an acid or base, and then washing the solid remaining after solvent distillation once or twice or more times with a solvent such as water, the reaction solvent (or an organic solvent having a similar solubility to the low-molecular-weight polymer), acetone, methyl ethyl ketone, or alcohols, followed by neutralization, washing with water, filtration, and drying; or (post-treatment 2) after completion of the polymerization reaction, adding a solvent such as water, acetone, methyl ethyl ketone, alcohols, ethers, halogenated hydrocarbons, aromatic hydrocarbons, or aliphatic hydrocarbons (a solvent that is soluble in the polymerization solvent used and is a poor solvent for at least PAS) to the reaction mixture. (a solvent which is a compound selected from the group consisting of methyl methyl ketone, methyl ethyl ...

[0030] In the post-treatment methods exemplified above as (Post-treatment 1) to (Post-treatment 5), the PAS may be dried in a vacuum, in air, or in an inert gas atmosphere such as nitrogen.

[0031] The PAS (A) used in this embodiment can be a PAS newly polymerized by the above-described method, or a recycled PAS. For example, PAS recovered from a PAS resin composition or a PAS resin molded article can be used. Specifically, a PAS obtained by heating a PAS resin composition or a PAS resin molded article in an organic polar solvent to dissolve the PAS contained therein and then performing the above-described post-treatment on the resulting solution can be used. Mechanically pulverized PAS resin compositions or PAS resin molded articles can also be used. Specifically, sprues or runners generated during the production of molded articles, recovered non-standard molded articles, or pulverized molded articles once used as products can be used. In this case, pulverized PAS resin compositions or PAS resin molded articles containing components other than PAS can also be used.

[0032] <Cyclic oligoarylene sulfide (B)> The PAS resin composition according to this embodiment further contains a cyclic PAS oligomer (sometimes referred to as (B)) as an essential component. The cyclic PAS oligomer (B) applicable to this embodiment has a hexameric cyclic structure. The cyclic PAS oligomer (B) in this disclosure has a resin structure in which a repeating unit is a structure in which an aromatic ring and a sulfur atom are bonded, similar to the PAS (A), and can contain the above formulas (1) to (6) as constituent units.

[0033] (Manufacturing method) The cyclic PAS oligomer (B) applicable to this embodiment is (1) A step of reacting a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide, in an organic polar solvent (1) to obtain a crude reaction mixture containing PAS (a), a cyclic PAS oligomer (B), the organic polar solvent (1), and an alkali metal halide. a step (2) of subjecting the crude reaction mixture to solid-liquid separation to obtain a reaction mixture (L1) containing at least the cyclic PAS oligomer (B) and the organic polar solvent (1); a step (3) of subjecting the organic polar solvent (1) to solid-liquid separation from the reaction mixture (L1) to obtain a reaction mixture (S1) containing a cyclic PAS oligomer (B); and a step (4) of contacting the reaction mixture (S1) with an organic polar solvent (2) to obtain a mixture (L2); A step (5) of subjecting the mixture (L2) to solid-liquid separation in a temperature range higher than the boiling point of the organic polar solvent (2) minus 10°C to recover a liquid phase component (L3); and Step (6) of gradually cooling the liquid phase component (L3) to 25°C or less and recovering the crystallized solid phase component. The method for producing the compound can be described below.

[0034] -Process (1) Step (1) is a step of reacting a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide, in an organic polar solvent (1) to obtain a crude reaction mixture containing PAS (a), cyclic PAS oligomer (B), the organic polar solvent (1), and the alkali metal halide.

[0035] Here, in this process, the polyhaloaromatic compound is, for example, a halogenated aromatic compound having two or more halogen atoms directly bonded to aromatic ring, specifically, p-dichlorobenzene, o-dichlorobenzene, m-dichlorobenzene, trichlorobenzene, tetrachlorobenzene, dibromobenzene, diiodobenzene, tribromobenzene, dibromonaphthalene, triiodobenzene, dichlorodiphenylbenzene, dibromodiphenylbenzene, dichlorobenzophenone, dibromobenzophenone, dichlorodiphenyl ether, dibromodiphenyl ether, dichlorodiphenyl sulfide, dibromodiphenyl sulfide, dichlorobiphenyl, dibromobiphenyl and other dihaloaromatic compounds and their mixtures can be enumerated, and these compounds can be block copolymerized.Among these, dihalogenated benzenes are preferred, and those containing 80 mol% or more of p-dichlorobenzene are particularly preferred. Furthermore, in order to increase the viscosity of the PAS resin by forming a branched structure, a polyhaloaromatic compound having three or more halogen substituents per molecule may be used as a branching agent, if desired. Examples of such polyhaloaromatic compounds include 1,2,4-trichlorobenzene, 1,3,5-trichlorobenzene, and 1,4,6-trichloronaphthalene. Further examples include polyhaloaromatic compounds having functional groups with active hydrogen, such as amino groups, thiol groups, and hydroxyl groups. Specific examples include dihaloanilines such as 2,6-dichloroaniline, 2,5-dichloroaniline, 2,4-dichloroaniline, and 2,3-dichloroaniline; trihaloanilines such as 2,3,4-trichloroaniline, 2,3,5-trichloroaniline, 2,4,6-trichloroaniline, and 3,4,5-trichloroaniline; dihaloaminodiphenyl ethers such as 2,2'-diamino-4,4'-dichlorodiphenyl ether and 2,4'-diamino-2',4-dichlorodiphenyl ether; and mixtures thereof in which the amino groups are replaced with thiol groups or hydroxyl groups.In addition, active hydrogen-containing polyhaloaromatic compounds in which the hydrogen atoms bonded to the carbon atoms forming the aromatic rings in these active hydrogen-containing polyhaloaromatic compounds are substituted with other inert groups, for example, hydrocarbon groups such as alkyl groups, can also be used.

[0036] Among these various active hydrogen-containing polyhaloaromatic compounds, active hydrogen-containing dihaloaromatic compounds are preferred, and dichloroaniline is particularly preferred.

[0037] Examples of polyhaloaromatic compounds having a nitro group include mono- or dihalonitrobenzenes such as 2,4-dinitrochlorobenzene and 2,5-dichloronitrobenzene; dihalonitrodiphenyl ethers such as 2-nitro-4,4'-dichlorodiphenyl ether; dihalonitrodiphenyl sulfones such as 3,3'-dinitro-4,4'-dichlorodiphenyl sulfone; mono- or dihalonitropyridines such as 2,5-dichloro-3-nitropyridine and 2-chloro-3,5-dinitropyridine; and various dihalonitronaphthalenes.

[0038] In this step, an alkali metal sulfide or alkali hydrosulfide and an alkali metal hydroxide (hereinafter sometimes referred to as a sulfidizing agent) are used as raw materials.

[0039] In this step, the alkali metal sulfide includes lithium sulfide, sodium sulfide, rubidium sulfide, cesium sulfide, and mixtures thereof. Such alkali metal sulfides can be used as hydrates, aqueous mixtures, or anhydrides. The alkali metal sulfide can also be derived by reacting an alkali metal hydrosulfide with an alkali metal hydroxide. A small amount of alkali metal hydroxide may be added to react with the alkali metal hydrosulfide and alkali metal thiosulfate, which are usually present in trace amounts in the alkali metal sulfide.

[0040] The alkali metal hydrosulfides include lithium hydrogen sulfide, sodium hydrogen sulfide, rubidium hydrogen sulfide, cesium hydrogen sulfide, and mixtures thereof. These alkali metal hydrosulfides can be used as hydrates, aqueous mixtures, or anhydrous forms.

[0041] The alkali metal hydrosulfide is used together with an alkali metal hydroxide. Examples of the alkali metal hydroxide include lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, and cesium hydroxide. These may be used alone or in combination of two or more. Among these, lithium hydroxide, sodium hydroxide, and potassium hydroxide are preferred because of their easy availability, and sodium hydroxide is particularly preferred.

[0042] In this step, a hydrous sulfidizing agent can also be used as a raw material, and in that case, it is preferable to subject the hydrous sulfidizing agent to a polymerization reaction for the PAS resin after a step of dehydrating the agent in the presence of at least an aprotic polar solvent. Furthermore, when the amount of aprotic polar solvent charged is small, for example, less than 1 mole per mole of sulfur atoms in the sulfidizing agent, it is preferable to dehydrate the hydrous sulfidizing agent and the aprotic polar solvent in the presence of a polyhaloaromatic compound.

[0043] The dehydration step of the hydrous sulfidizing agent is carried out by charging at least an aprotic polar solvent and a hydrous alkali metal sulfide or a hydrous alkali hydrosulfide and an alkali metal hydroxide as the hydrous sulfidizing agent into a reaction vessel equipped with a distillation apparatus, heating to a temperature at which water is removed azeotropically, specifically, in the range of 300°C or less, preferably 80 to 220°C, more preferably 100 to 200°C, and discharging water by distillation to the outside of the system. In the dehydration step, dehydration is preferably carried out until the amount of water in the polymerization system is 5 moles or less, more preferably 0.01 to 2.0 moles per mole of sulfur atoms in the sulfidizing agent.

[0044] Examples of the organic polar solvent (1) used in this step include amides, ureas, and lactams such as formamide, acetamide, N-methylformamide, N,N-dimethylacetamide, tetramethylurea, N-methyl-2-pyrrolidone, 2-pyrrolidone, N-methyl-ε-caprolactam, ε-caprolactam, hexamethylphosphoramide, N-dimethylpropyleneurea, and 1,3-dimethyl-2-imidazolidinoic acid; sulfolanes such as sulfolane and dimethylsulfolane; nitriles such as benzonitrile; ketones such as methyl phenyl ketone; and mixtures thereof. Among these, amides having an aliphatic cyclic structure, such as N-methyl-2-pyrrolidone, 2-pyrrolidone, N-methyl-ε-caprolactam, ε-caprolactam, hexamethylphosphoramide, N-dimethylpropyleneurea, and 1,3-dimethyl-2-imidazolidinoic acid, are preferred, and N-methyl-2-pyrrolidone is more preferred.

[0045] In this step, the alkali metal sulfide as a sulfidizing agent is reacted with a polyhaloaromatic compound in the presence of such an organic polar solvent. Alternatively, the reaction is carried out by reacting the alkali metal hydrosulfide and alkali metal hydroxide as sulfidizing agents with a polyhaloaromatic compound in the presence of such an organic polar solvent. Reaction conditions generally involve a temperature in the range of 200 to 330°C, and a pressure in a range that maintains the polymerization solvent and the polyhaloaromatic compound (polymerizable monomer) substantially in liquid phase, generally selected from the range of 0.1 to 20 MPa, preferably 0.1 to 2 MPa. The amount of polyhaloaromatic compound charged is adjusted to 0.2 to 5.0 moles, preferably 0.8 to 1.3 moles, and more preferably 0.9 to 1.1 moles per mole of sulfur atom in the sulfidizing agent. The amount of aprotic polar solvent is adjusted to 1.0 to 6.0 moles, preferably 2.5 to 4.5 moles, per mole of sulfur atom in the sulfidizing agent. The polymerization reaction is preferably carried out in the presence of a small amount of water, the proportion of which is preferably adjusted appropriately depending on the polymerization method, the molecular weight of the resulting polymer, and productivity. Specifically, the dehydration operation is carried out so that the amount of water is 2.0 moles or less, preferably 1.6 moles or less, per mole of sulfur atom in the sulfidizing agent. Furthermore, when the dehydration operation is carried out in the presence of a polyhaloaromatic compound (for example, method "5") in the specific embodiment below), the dehydration operation may be carried out so that the amount of water is 0.9 moles or less, preferably 0.05 to 0.3 moles, more preferably 0.01 to 0.02 moles or less.

[0046] Specific embodiments of polymerizing a sulfidizing agent and a polyhaloaromatic compound in the presence of the above-mentioned aprotic polar solvent include, for example, 1) A method using a polymerization aid such as an alkali metal carboxylate or a lithium halide, 2) A method using a branching agent such as an aromatic polyhalogen compound, 3) A method in which the polymerization reaction is carried out in the presence of a small amount of water, and then water is added to carry out further polymerization. 4) A method in which the gas phase portion of the reaction vessel is cooled during the reaction of the alkali metal sulfide with the aromatic dihalogen compound, and a part of the gas phase in the reaction vessel is condensed and refluxed to the liquid phase; 5) A method for producing a PAS resin, the essential steps of which include a step of reacting an alkali metal sulfide, or a hydrous alkali metal hydrosulfide and an alkali metal hydroxide, with an amide, urea, or lactam having an aliphatic cyclic structure in the presence of a polyhalo-aromatic compound while dehydrating to produce a slurry containing a solid alkali metal sulfide; a step of adding a polar organic solvent such as NMP after producing the slurry and distilling off the water to dehydrate it; and a step of reacting the polyhalo-aromatic compound, the alkali metal hydrosulfide, and the alkali metal salt of a hydrolyzate of the amide, urea, or lactam having an aliphatic cyclic structure in the slurry obtained through the dehydration step, at a concentration of 0.02 mol or less of water present in the reaction system per 1 mol of the polar organic solvent such as NMP, to polymerize the slurry.

[0047] Thus, polymerization of a dihaloaromatic compound with (i) an alkali metal sulfide or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent produces PAS (a) and PAS oligomer (B) as products, with a chain PAS oligomer also being produced as a by-product. Furthermore, the reaction product may contain other by-products, such as alkali metal-containing inorganic salts, carboxyalkylamino group-containing compounds, and terminal SH group-containing compounds, as well as unreacted raw materials and water.

[0048] -Process (2) Step (2) is a step of subjecting the crude reaction mixture to solid-liquid separation to obtain a reaction mixture (L1) containing at least the cyclic PAS oligomer (B) and the organic polar solvent (1).

[0049] The solid-liquid separation is broadly divided into two types: the flash method and the quench method, which will be described later. In this step, the quench method is preferred because it obtains a liquid phase component.

[0050] The quench method is a method for separating and recovering particulate PAS(a) by slowly cooling a crude reaction mixture. Generally, the crude reaction mixture is gradually cooled from a high-temperature, high-pressure state to crystallize the PAS(a) in the reaction system, followed by solid-liquid separation by filtration or other methods to recover the solids containing PAS(a) as granules, thereby obtaining a liquid phase component. The cooling time is not particularly limited, but a preferred range is usually 0.1°C / min to 3°C / min. Furthermore, the cooling rate does not need to be constant throughout the entire quenching process. Preferred methods include cooling at a rate of 0.1°C / min to 1°C / min until the PAS(a) granules crystallize, followed by cooling at a rate of 1°C / min or faster. The final cooling step is preferably to 70°C or higher, preferably 100°C to 200°C, followed by solid-liquid separation to recover the solids containing the PAS resin. Solid-liquid separation in the quench method can be achieved by filtration or using a centrifuge such as a screw decanter.

[0051] -Process (3) Step (3) is a step of performing solid-liquid separation to remove the organic polar solvent (1) from the reaction mixture (L1) to obtain a reaction mixture (S1) containing at least the cyclic PAS oligomer (B).

[0052] Methods for removing the organic polar solvent (1) from the reaction mixture (L1) include, for example, a flash method in which the solvent is evaporated to recover the solvent and simultaneously recover solids, and solvent removal using a membrane. A preferred embodiment of the flash method is a method in which the high-temperature, high-pressure (usually 250°C or higher, 0.8 MPa or higher) reaction mixture (L1) obtained in the polymerization step is ejected from a nozzle into an atmosphere of nitrogen or water vapor at atmospheric pressure. In the flash method, the solvent can be efficiently recovered by utilizing the heat of vaporization of the solvent when the polymerization reaction mixture is flashed from a high-temperature, high-pressure state to an atmospheric pressure state. The higher the internal temperature during flashing, the more efficient the solvent recovery and the higher the productivity. Therefore, the temperature and pressure within the polymerization system during flashing are typically 250°C or higher, preferably in the range of 255 to 280°C, and 0.8 MPa or higher, preferably in the range of 1.0 to 5.0 MPa. The ambient temperature when flashing from this state to reduced pressure or normal pressure is usually in the range of 150 to 250°C, and if the recovery of solvent from the crude reaction mixture is insufficient, heating may be continued in an atmosphere of 150 to 250°C after flashing.

[0053] When removing the organic polar solvent (1), it is desirable to remove the organic polar solvent so that the proportion of solids (non-volatile content) is in the range of 20 to 100% by mass, preferably 20 to 99.99% by mass, and more preferably 30 to 90% by mass. The temperature at which the organic polar solvent is removed by heating cannot be uniquely limited because it depends on the properties of the organic polar solvent used, but it can usually be selected from the range of 20 to 150°C, preferably 40 to 120°C. In addition, the pressure at which the organic polar solvent is removed is preferably atmospheric pressure or less, which allows the organic polar solvent to be removed at a lower temperature.

[0054] -Process (4) Step (4) is a step of contacting the reaction mixture (S1) with an organic polar solvent (2) to obtain a mixture (L2).

[0055] The organic polar solvent (2) used in this step is preferably one that does not substantially cause undesirable side reactions such as decomposition or crosslinking of the PAS (A) and the cyclic PAS oligomer (B), and solvents similar to the organic polar solvent (1) can also be used. Examples of the organic polar solvent (2) include aromatic hydrocarbon solvents such as toluene and xylene; halogenated solvents such as chloroform, bromoform, methylene chloride, 1,2-dichloroethane, 1,1,1-trichloroethane, chlorobenzene, and 2,6-dichlorotoluene; ether solvents such as diethyl ether, tetrahydrofuran, and diisopropyl ether; amides such as formamide, acetamide, N-methylformamide, N,N-dimethylformamide, N,N-dimethylacetamide, tetramethylurea, N-methyl-2-pyrrolidone, 2-pyrrolidone, N-methyl-ε-caprolactam, ε-caprolactam, hexamethylphosphoramide, N-dimethylpropyleneurea, and 1,3-dimethyl-2-imidazolidinonic acid, ureas, and lactams; and polar solvents such as dimethyl sulfoxide, trimethylphosphate, N,N-dimethylimidazolidinone, and methyl ethyl ketone. Among these, the organic polar solvent (2) has a dipole moment μ of 1 [D] (*1D=3.3356×10 -30 C·m) or higher or a polar solvent with a dielectric constant ε(20°C) of 2 or higher is preferred.

[0056] The method for contacting the reaction mixture (S1) with the organic polar solvent (2) is not particularly limited. For example, the reaction mixture (S1) is mixed with the organic polar solvent (2), and the mixture is contacted at a temperature ranging from 10 to 200°C, preferably from 50 to 150°C, and more preferably from 80 to 130°C, followed by separation into a liquid phase component containing the cyclic PAS oligomer (B) and a solid component. The pressure during contact between the reaction mixture (S1) and the organic polar solvent (2) may be either normal pressure or elevated pressure, but is preferably 0.1 to 0.5 MPa. The atmosphere during contact between the reaction mixture (S1) and the organic polar solvent (2) is not particularly limited. However, if the temperature, time, or other conditions during contact may cause oxidative degradation of the cyclic PAS oligomer (B) or the organic polar solvent (2), it is desirable to contact the mixture in a non-oxidizing atmosphere. A non-oxidizing atmosphere refers to an atmosphere in which the oxygen concentration in the gas phase is 5% by volume or less, preferably 2% by volume or less, and more preferably an atmosphere containing substantially no oxygen, i.e., an inert gas atmosphere such as nitrogen, helium, or argon.

[0057] -Process (5) The step (5) is a step of subjecting the mixture (L2) to solid-liquid separation in a temperature range higher than the boiling point of the organic polar solvent (2) minus 10° C., to recover a liquid phase component (L3).

[0058] The method for recovering the solid phase component is not particularly limited as long as it does not impair the effects of the present invention, and known devices and methods can be used. For example, separation can be performed using a centrifuge such as a screw decanter or a filtration device.

[0059] -Process(6) Step (6) is a step of gradually cooling the liquid phase component (L3) to 25° C. or lower and recovering the crystallized solid phase component.

[0060] The cooling of the liquid phase component (L3) is not particularly limited as long as it does not impair the effects of the present invention, and known devices and methods can be used. In this disclosure, slow cooling does not mean rapid cooling; for example, a cooling rate of 1°C / min or less is preferred. Furthermore, it is not necessary to cool at the same rate throughout the entire slow cooling process. By cooling the liquid phase component (L3) to 25°C, only the hexamer PAS oligomer precipitates and can be recovered as a solid.

[0061] The solid phase component can be recovered in the same manner as in step (5). The recovered solid phase component can be used as PAS oligomer (B) as is, or can be used after further washing and drying.

[0062] The crude reaction mixture obtained in step (1) contains by-products such as cyclic PAS oligomers of pentamer or less, cyclic PAS oligomers of heptomer or more, and linear PAS oligomers, in addition to the hexamer cyclic oligoarylene sulfide (B). These by-products are separated from the PAS oligomer (B) in steps (2) to (6). For example, the pentamer and heptomer or more cyclic oligoarylene sulfides remain dissolved in the liquid phase component after the crystallization of the PAS oligomer (B) in step (6), and the linear PAS oligomers are contained in the solid phase component removed by solid-liquid separation in step (5).

[0063] The amount of cyclic PAS oligomer (B) in this embodiment is not particularly limited as long as it does not impair the effects of the present invention, but from the viewpoint of the recovery rate of the PAS oligomer, it is preferably 0.01 part by mass or more, more preferably 0.1 part by mass or more, per 100 parts by mass of PAS (A). From the viewpoint of the mechanical properties of the resulting resin composition and molded article, it is preferably 20 parts by mass or less, more preferably 10 parts by mass or less.

[0064] <Thermoplastic elastomer (C)> The PAS resin composition according to this embodiment may optionally contain a thermoplastic elastomer (C) as an optional component to improve mechanical properties. By further including the thermoplastic elastomer (C), the toughness and thermal shock resistance of the PAS resin composition can be further improved.

[0065] Examples of the thermoplastic elastomer (C) include polyolefin elastomers, fluorine elastomers, and silicone elastomers, with polyolefin elastomers being preferred. When these elastomers are added, their amount is not particularly limited, but is preferably at least 0.01 parts by mass, more preferably at least 0.1 parts by mass, and even more preferably at least 1 part by mass per 100 parts by mass of the PAS (A). On the other hand, the amount of the thermoplastic elastomer is preferably no more than 30 parts by mass, more preferably no more than 20 parts by mass, and even more preferably no more than 15 parts by mass. This range is preferred because it improves the flexibility of the resulting PAS resin composition. Addition in excess of this range can have adverse effects, such as a deterioration in the drollness of the resin composition and an increase in the amount of gas generated.

[0066] Examples of the polyolefin elastomer include a homopolymer of an α-olefin, a copolymer of two or more α-olefins, and a copolymer of one or more α-olefins with a vinyl polymerizable compound having a functional group. Examples of the α-olefin include α-olefins having 2 to 8 carbon atoms, such as ethylene, propylene, and 1-butene. Examples of the functional group include a carboxy group, an acid anhydride group (—C(═O)OC(═O)—), an epoxy group, an amino group, a hydroxyl group, a mercapto group, an isocyanate group, and an oxazoline group. Examples of the vinyl polymerizable compound having the functional group include one or more of vinyl acetate; α,β-unsaturated carboxylic acids such as (meth)acrylic acid; alkyl esters of α,β-unsaturated carboxylic acids such as methyl acrylate, ethyl acrylate, and butyl acrylate; metal salts of α,β-unsaturated carboxylic acids such as ionomers (metals include alkali metals such as sodium, alkaline earth metals such as calcium, and zinc); glycidyl esters of α,β-unsaturated carboxylic acids such as glycidyl methacrylate; α,β-unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid; and derivatives of the α,β-unsaturated dicarboxylic acids (monoesters, diesters, and acid anhydrides). The thermoplastic elastomers described above may be used alone or in combination of two or more.

[0067] <Inorganic filler (D)> The PAS resin composition according to this embodiment may further contain an inorganic filler (D) as an optional component. By further containing the inorganic filler (D), the mechanical strength, thermal conductivity, and the like of the PAS resin composition can be further improved.

[0068] Here, as the inorganic filler (D), known and commonly used materials can be used as long as they do not impair the effects of the present invention, including fillers of various shapes such as granular, plate-like, and fibrous ones. For example, fibrous fillers such as glass fiber, carbon fiber, silane glass fiber, ceramic fiber, aramid fiber, metal fiber, potassium titanate, silicon carbide, calcium silicate, wollastonite, and natural fibers can be used. Non-fibrous fillers such as glass beads, glass flakes, barium sulfate, clay, pyrophyllite, bentonite, sericite, mica, talc, attapulgite, ferrite, calcium silicate, calcium carbonate, magnesium carbonate, zeolite, milled fiber, and calcium sulfate can also be used. These other fillers can also be surface-treated, and if necessary, can be treated with epoxy compounds, isocyanate compounds, silane compounds, titanate compounds, borane treatment, ceramic coating, etc.

[0069] The amount of the inorganic filler (D) is not particularly limited, but from the viewpoint of better mechanical properties and dimensional stability, it is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more, per 100 parts by mass of the PAS (A). Also, from the viewpoint of obtaining better flowability and processability of the resin composition and surface smoothness of the molded product, it is more preferably 350 parts by mass or less, even more preferably 300 parts by mass or less, and particularly preferably 250 parts by mass or less, per 100 parts by mass of the PAS (A).

[0070] The content of the inorganic filler (D) in the PAS resin composition according to this embodiment is not particularly limited, but from the viewpoint of achieving excellent mechanical strength and the like of the resin composition, it is preferably 20 parts by mass or more, more preferably 25 parts by mass or more, and even more preferably 30 parts by mass or more, per 100 parts by mass of the total amount of the PAS (A) and the inorganic filler (D), because within this range, the isothermal crystallization time is shortened and good moldability is exhibited.

[0071] (Silane coupling agent) If necessary, a silane coupling agent can be blended as an optional component in the PAS resin composition according to this embodiment for the purpose of improving mechanical properties.

[0072] Here, the silane coupling agent having the functional group is not particularly limited as long as it does not impair the effects of the present invention, but preferred examples include silane coupling agents having a functional group that reacts with a carboxy group, such as an epoxy group, an isocyanato group, an amino group, or a hydroxyl group. Examples of such silane coupling agents include epoxy group-containing alkoxysilane compounds such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; isocyanato group-containing alkoxysilane compounds such as γ-isocyanatopropyltrimethoxysilane, γ-isocyanatopropyltriethoxysilane, γ-isocyanatopropylmethyldimethoxysilane, γ-isocyanatopropylmethyldiethoxysilane, γ-isocyanatopropylethyldimethoxysilane, γ-isocyanatopropylethyldiethoxysilane, and γ-isocyanatopropyltrichlorosilane; amino group-containing alkoxysilane compounds such as γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, and γ-aminopropyltrimethoxysilane; and hydroxyl group-containing alkoxysilane compounds such as γ-hydroxypropyltrimethoxysilane and γ-hydroxypropyltriethoxysilane.

[0073] Furthermore, the content of the silane coupling agent having the functional group in the PAS resin composition of the present invention is not particularly limited, but from the viewpoint of obtaining better moist heat resistance and mechanical strength, it is preferably 0.3 parts by mass or more, more preferably 0.4 parts by mass or more, and even more preferably 0.5 parts by mass or more, per 100 parts by mass of the PAS resin.

[0074] Furthermore, in addition to the above components, the PAS resin composition according to the present embodiment may further contain, as appropriate depending on the intended use, synthetic resins (hereinafter simply referred to as synthetic resins), such as polyester resin, polyamide resin, polyimide resin, polyetherimide resin, polycarbonate resin, polyphenylene ether resin, polysulfone resin, polyethersulfone resin, polyetheretherketone resin, polyetherketone resin, polyarylate resin, polyethylene resin, polypropylene resin, polyethylenetetrafluoroethylene resin, polyethylenedifluoroethylene resin, polystyrene resin, ABS resin, epoxy resin, phenolic resin, urethane resin, and liquid crystal polymer, as optional components. While the synthetic resin is not an essential component in the present disclosure, if it is included, its proportion is not particularly limited as long as it does not impair the effects of the present invention. Furthermore, since the proportion varies depending on the intended purpose and cannot be generally defined, the proportion of the synthetic resin included in the resin composition according to the present disclosure is, for example, in the range of 5 parts by mass or more and 15 parts by mass or less per 100 parts by mass of PAS(A). In other words, the ratio of PAS to the total of PAS (A) and synthetic resin is preferably in the range of (100 / 115) or more, more preferably (100 / 105) or more, on a mass basis.

[0075] The PAS resin composition according to this embodiment may also contain other known and commonly used additives as optional components, as needed, such as colorants, antistatic agents, antioxidants, heat stabilizers, UV stabilizers, UV absorbers, foaming agents, flame retardants, flame retardant assistants, rust inhibitors, and mold release agents (metal salts or esters of fatty acids having 18 to 30 carbon atoms, including stearic acid or montanic acid, and polyolefin waxes such as polyethylene). These additives are not essential components, and may be used in amounts, for example, preferably 0.01 part by mass or more, and preferably 1000 parts by mass or less, more preferably 100 parts by mass or less, and even more preferably 10 parts by mass or less, per 100 parts by mass of PAS (A), adjusted appropriately depending on the purpose and application so as not to impair the effects of the present invention.

[0076] The PAS resin composition of the present disclosure has a morphology in which PAS (A) forms a continuous phase and other essential and optional components are dispersed. After the melt-kneading, the PAS resin composition of the present disclosure is preferably prepared by a known method, for example, by extruding the molten resin composition into a strand shape, processing it into pellets, chips, granules, powder, or the like, and then pre-drying it at a temperature in the range of 100 to 150°C as needed.

[0077] The PAS resin composition according to this embodiment has a viscosity change rate within a range of ±20%. That is, when the melt viscosity (V6) of the PAS (A) is defined as 1, the melt viscosity (V6) of the PAS resin composition is in the range of 0.8 to 1.2. When the viscosity change rate is within this range, the viscosity change rate due to the addition of the PAS oligomer (B) is small, resulting in a resin composition with excellent processability. To adjust the viscosity change rate within this range, the amount of the cyclic PAS oligomer (B) may be adjusted to 20 parts by mass or less per 100 parts by mass of the PAS (A). The viscosity change rate in this disclosure was calculated using the following formula, using the melt viscosity (V6) measured after 6 minutes using a flow tester at a temperature of 300°C, a load of 1.96 MPa, and an orifice with an orifice length to orifice diameter ratio of 10 / 1. Viscosity change rate (%) = (melt viscosity of the PAS (A) (Pa·s) - melt viscosity of the PAS resin composition (Pa·s)) / melt viscosity of the PAS (A) (Pa·s) × 100

[0078] <Molded products and manufacturing methods for molded products> The molded article according to this embodiment is obtained by melt-molding the PAS resin composition. The method for producing the molded article according to this embodiment includes a step of melt-molding the PAS resin composition obtained by the above-described method. Therefore, the molded article according to this embodiment has a morphology in which the PAS (A) forms a continuous phase and other essential and optional components are dispersed. The PAS resin composition having such a morphology allows the molded article to have excellent mechanical strength.

[0079] The PAS resin composition according to this embodiment can be subjected to various molding processes, such as injection molding, compression molding, extrusion molding (e.g., composite, sheet, pipe), pultrusion molding, blow molding, and transfer molding. However, due to its excellent mold releasability, it is particularly suited to injection molding applications. When molding by injection molding, the molding conditions are not particularly limited, and molding can be performed using conventional methods. For example, the PAS resin composition can be melted in an injection molding machine at a resin temperature in a range equal to or higher than the melting point of the PAS resin (A), preferably in a range of 10°C above the melting point, more preferably in a range of 10°C above the melting point to 100°C above the melting point, and even more preferably in a range of 20°C above the melting point to 50°C above the melting point, and then injected into a mold through a resin outlet. The mold temperature can also be set within a known temperature range, for example, from room temperature (23°C) to 300°C, preferably 130°C to 190°C.

[0080] The method for producing a molded article according to this embodiment may include a step of annealing the molded article. The optimal conditions for the annealing treatment are selected depending on the intended use or shape of the molded article. The annealing temperature is preferably in a range equal to or higher than the glass transition temperature of PAS(A), preferably in a range equal to or higher than the glass transition temperature +10°C, and more preferably in a range equal to or higher than the glass transition temperature +30°C. The annealing time is preferably in a range equal to or lower than 260°C, and more preferably in a range equal to or lower than 240°C. The annealing time is not particularly limited, but is preferably in a range equal to or higher than 0.5 hours, and more preferably in a range equal to or higher than 1 hour. The annealing time is preferably in a range equal to or lower than 10 hours, and more preferably in a range equal to or lower than 8 hours. This range is preferable because it reduces distortion in the resulting molded article, improves the crystallinity of the resin, and further improves thermal conductivity, mechanical properties, and fuel barrier properties. The annealing treatment may be performed in air, but is preferably performed in an inert gas such as nitrogen gas.

[0081] The molded article according to this embodiment includes a remolded article obtained by reusing a molded article obtained by melt-molding the PAS resin composition. Specifically, examples include sprues or runners generated during the production of molded articles, recovered non-standard molded articles, and molded articles obtained by cleaning, if necessary, pulverizing, and melt-molding the molded article again at a temperature above the melting point of PAS. When recycling, it is preferable to mix the pulverized molded article with the PAS resin composition from the viewpoint of mechanical properties. The size of the molded article to be pulverized is not particularly limited, but from the viewpoints of mixability and processability, it is preferable that the size be similar to that of the PAS resin composition to be mixed. Furthermore, the mixing ratio of the pulverized molded article to 100 parts by mass of the PAS resin composition is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 20 parts by mass or less. Within this range, recyclability can be improved without impairing the effects of the PAS resin composition of the present disclosure.

[0082] The PAS resin molded article according to this embodiment is characterized by an excellent balance between crystallization rate and melt viscosity, making it suitable for application to parts with thin-walled sections and small precision parts. Furthermore, the molded article according to this embodiment is not limited to the above, but can also be made into the following ordinary resin molded articles: For example, protective and support members for box-shaped integrated modules of electric and electronic components, multiple individual semiconductors or modules, sensors, LED lamps, resistors, relay cases, connectors, sockets, switches, coil bobbins, capacitors, variable capacitor cases, optical pickups, oscillators, various terminal boards, transformers, plugs, printed circuit boards, tuners, speakers, microphones, headphones, small motors, magnetic head bases, power modules, terminal blocks, semiconductors, liquid crystal displays, FDD carriages, FDD chassis, motor brush holders, parabolic antennas, and electric and electronic components such as computer-related parts; VTR parts, television parts, irons, headsets, etc. Home and office electrical appliance parts such as air dryers, rice cooker parts, microwave oven parts, audio parts, audio / visual equipment parts such as laser discs, compact discs, DVD discs, and Blu-ray discs, lighting parts, refrigerator parts, air conditioner parts, typewriter parts, word processor parts, and plumbing equipment parts such as water heaters, bath water volume and temperature sensors; machine-related parts such as office computer-related parts, telephone-related parts, facsimile-related parts, copier-related parts, cleaning jigs, motor parts, lighters, and typewriters; optical equipment and precision machinery-related parts such as microscopes, binoculars, cameras, and watches;Alternator terminals, alternator connectors, brush holders, slip rings, IC regulators, light dimmer potentiometer bases, relay blocks, inhibitor switches, various valves such as exhaust gas valves, various pipes for fuel, exhaust and intake systems, air intake nozzle snorkels, intake manifolds, engine coolant joints, carburetor main bodies, carburetor spacers, exhaust gas sensors, coolant sensors, oil temperature sensors, brake pad wear sensors, throttle position sensors, crankshaft position sensors, temperature sensors, air flow meters, brake pad wear sensors, air conditioner thermostat bases, heating hot air flow control valves, radiators Examples of automotive and vehicle related parts include brush holders for motors, water pump impellers, turbine vanes, wiper motor related parts, distributors, starter switches, ignition coils and bobbins, motor insulators, motor rotors, motor cores, starter relays, transmission wire harnesses, windshield washer nozzles, air conditioner panel switch boards, fuel-related electromagnetic valve coils, fuse connectors, horn terminals, electrical component insulating plates, step motor rotors, lamp sockets, lamp reflectors, lamp housings, brake pistons, solenoid bobbins, engine oil filters, ignition device cases, and many other applications. [Example]

[0083] The present invention will be specifically described below with reference to examples. These examples are illustrative and not limiting. Unless otherwise specified, "%" and "parts" are based on mass.

[0084] <Reference Examples 1 to 3, Examples 1 to 4, and Comparative Examples 1 to 4> The materials were blended according to the composition and amounts listed in Tables 1 and 2. These blended materials were then fed into a vented twin-screw extruder "TEX-30α (product name)" manufactured by The Japan Steel Works, Ltd., and melt-kneaded at a resin component output rate of 30 kg / hr, a screw rotation speed of 200 rpm, and a set resin temperature of 320°C to obtain pellets of the resin composition. The glass fiber was fed through a side feeder (S / T ratio 0.5), and the other materials were pre-mixed uniformly in a tumbler and then fed through the top feeder. The resulting pellets of the resin composition were dried for 2 hours in a gear oven at 140°C and then injection-molded to prepare various test pieces, which were then subjected to the following tests.

[0085] <Evaluation>

[0086] (1) Measurement of recrystallization temperature (Tmc) The resin compositions obtained in each Example and Comparative Example were melted at 350°C and then rapidly cooled to prepare amorphous films. Approximately 4 mg of the film was taken and measured using a differential scanning calorimeter (Perkin Elmer "DSC8500"). The results are shown in Tables 1 and 2.

[0087] (2) Measurement of melt viscosity (V6) The melt viscosity (V6) of each PAS and PAS resin composition was measured using a Shimadzu flow tester "CFT-500D" at 300°C and a load of 1.96 x 10 6 The melt viscosity (V6) (Pa·s) was measured after holding for 6 minutes at a temperature of 100°C / 200°F (Pa) and an L / D ratio of 10 (mm) / 1 (mm). The melt viscosity (V6) of the PAS resin composition relative to the melt viscosity (V6) of the PAS was calculated as the viscosity change rate using the following formula. The results are shown in Tables 1 and 2. Viscosity change rate (%) = (melt viscosity of PAS (Pa s) - melt viscosity of PAS resin composition (Pa s)) / melt viscosity of PAS (Pa s) × 100

[0088] [Table 1]

[0089] [Table 2]

[0090] The blending ratios of the blending components in Tables 1 and 2 are as follows: PAS(A) A-1: PPS with a linear structure at the para position a-2: Para-Meta Copolymer PPS

[0091] PAS oligomer (B) B-1: Hexamer with a cyclic structure b-2: A mixture of 7-12 mers with a cyclic structure b-3: PAS oligomer with a chain structure

[0092] Thermoplastic elastomer (C) C-1: "Engage 8842" manufactured by Dow Chemical Company

[0093] Inorganic filler (D) D-1: Glass fiber, "T-717H" manufactured by Nippon Electric Glass Co., Ltd.

[0094] <Production Example 1> Production of PAS (A-1) [Process 1] A 150L autoclave equipped with a stirring blade and connected to a pressure gauge, thermometer, condenser, decanter, and rectification column was charged with 33.075 parts by mass (225 mol parts) of p-dichlorobenzene (hereinafter referred to as p-DCB), 3.420 parts by mass (34.5 mol parts) of NMP, 27.300 parts by mass of a 47.23% by mass NaSH aqueous solution (230 mol parts as NaSH), and 18.533 parts by mass of a 49.21% by mass NaOH aqueous solution (228 mol parts as NaOH). The mixture was heated to 173 °C over 5 hours under a nitrogen atmosphere with stirring, and 27.300 parts by mass of water was distilled off. The autoclave was then sealed. The p-DCB distilled azeotropically during dehydration was separated in a decanter and returned to the autoclave as needed. After dehydration, the autoclave contained a fine particle anhydrous sodium sulfide composition dispersed in the p-DCB. The NMP content in this composition was 0.079 parts by mass (0.8 mol parts), indicating that 98 mol% (33.7 mol parts) of the charged NMP had been hydrolyzed to the sodium salt of NMP's ring-opened derivative (4-(methylamino)butyric acid) (hereinafter abbreviated as "SMAB"). The amount of SMAB in the autoclave was 0.147 mol parts per mole of sulfur atom present in the autoclave. Since the theoretical amount of dehydration when all of the charged NaSH and NaOH is converted to anhydrous NaS is 27.921 mol parts, this indicates that of the 0.878 mol parts by mass (48.8 mol parts) of water remaining in the autoclave, 0.609 mol parts by mass (33.8 mol parts) was consumed in the hydrolysis reaction between NMP and NaOH and was not present in the autoclave as water, while the remaining 0.269 mol parts by mass (14.9 mol parts) remained in the autoclave in the form of water or crystal water. The amount of water in the autoclave was 0.065 moles per mole of sulfur atom present in the autoclave.

[0095] [Process 2] After the dehydration step was completed, the autoclave was cooled to an internal temperature of 160°C, and 46.343 parts by mass (467.5 parts by mole) of NMP was added. The temperature was then raised to 185°C. The amount of water in the autoclave was 0.025 moles per mole of NMP added in step 2. When the gauge pressure reached 0.00 MPa, the valve connecting the distillation column was opened, and the internal temperature was raised to 200°C over 1 hour. During this time, the cooling and valve opening were controlled so that the outlet temperature of the distillation column remained below 110°C. The distilled mixed vapor of p-DCB and water was condensed in a condenser and separated in a decanter. The p-DCB was returned to the autoclave. The amount of distilled water was 0.228 parts by mass (12.7 parts by mole).

[0096] [Process 3] The amount of water in the autoclave at the start of step 3 was 0.041 parts by mass (2.3 mol parts), which was 0.005 mol per mole of NMP charged in step 2 and 0.010 mol per mole of sulfur atoms present in the autoclave. The amount of SMAB in the autoclave was 0.147 mol per mole of sulfur atoms present in the autoclave, the same as in step 1. Next, the internal temperature was raised from 200°C to 230°C over 3 hours, stirred at 230°C for 1 hour, and then raised to 250°C and stirred for 1 hour. The gauge pressure at the internal temperature of 200°C was 0.03 MPa, and the final gauge pressure was 0.40 MPa. After cooling, 0.650 parts by mass of the resulting slurry was poured into 3 parts by mass (3 L) of water and stirred at 80°C for 1 hour, followed by filtration. The cake was again stirred with 3 parts by mass (3 L) of warm water for 1 hour, washed, and then filtered. This procedure was repeated four times. 3 parts by mass (3 L) of warm water and acetic acid were added to this cake, and the pH was adjusted to 4.0. The mixture was then stirred for 1 hour, washed, and filtered. This cake was then stirred for 1 hour with 3 parts by mass (3 L) of warm water, washed, and filtered. This procedure was repeated twice. The cake was then dried overnight at 120°C using a hot air dryer to obtain a white powdery PPS resin (A-1).

[0097] <Production Example 2> Production of PAS (a-2) A 150 L autoclave was charged with 19.222 kg of flaky Na2S (60.9% by mass) and 45.0 kg of NMP. The temperature was raised to 204°C with stirring under a nitrogen stream, and 4.438 kg of water was distilled off (the remaining water content was 1.14 mol per mol of Na2S). The autoclave was then sealed and cooled to 180°C, and 22.998 kg of p-DCB, 2.555 kg of m-dichlorobenzene (hereinafter referred to as m-DCB) (10 mol% relative to the total of m-DCB and p-DCB), and 18.0 kg of NMP were charged. At a liquid temperature of 150°C, nitrogen gas was used to increase the pressure to 1 kg / cm. 2 The mixture was pressurized to 220°C and the temperature began to rise. While stirring for 3 hours at a liquid temperature of 220°C, a coolant at 80°C was passed through the coil wound around the outside of the upper part of the autoclave to cool it. The temperature was then raised and the mixture was stirred for 3 hours at a liquid temperature of 260°C, after which the temperature was lowered and the cooling of the upper part of the autoclave was stopped. During the cooling of the upper part of the autoclave, the liquid temperature was kept constant so as not to drop. The maximum pressure during the reaction was 8.91 kg / cm 2 It was G. The resulting slurry was filtered and washed twice with warm water using standard methods, yielding a filter cake containing approximately 50% water by mass. Next, 60 kg of water and 100 g of acetic acid were added to the filter cake to re-slurry it, and the mixture was stirred at 50°C for 30 minutes and then filtered again. The pH of the slurry was 4.6. The filter cake was then added with 60 kg of water, stirred for 30 minutes, and filtered again, a process repeated five times. The filter cake was then dried in a hot air circulating dryer at 120°C for 4.5 hours to yield a white powdery para-PPS copolymer. The resulting para-PPS copolymer had a melting point of 230°C and a melt viscosity (V6) of 45 Pa·s.

[0098] <Production Example 2> Production of PAS oligomer (B-1) -Process (1) A 150-L autoclave equipped with a stirring blade, a thermometer, a condenser, a bottom valve, and a pressure gauge was charged with 19.413 kg (150 mol) of flaky sodium sulfide (60.3 wt % NaS) and 45.0 kg (454 mol) of NMP. The temperature was raised to 209°C with stirring under a nitrogen stream, and 4.644 kg of water was distilled off (the remaining water content was 1.13 mol per mol of sodium sulfide). The autoclave was then sealed and cooled to 180°C, and 21.631 kg (147 mol) of p-DCB and 18.0 kg (182 mol) of NMP were charged. At a liquid temperature of 150°C, the pressure was increased to 0.1 MPa using nitrogen gas, and the temperature was raised to 240°C over 135 minutes and maintained at that temperature for 30 minutes. The liquid temperature was then raised to 250°C over 40 minutes and maintained at that temperature for 73 minutes to complete the reaction, after which the autoclave was cooled.

[0099] -Process (2) The bottom valve of the autoclave was opened at 100°C, and the reaction slurry was transferred to a 150L plate filter and pressure filtered at 120°C. 48.0 kg of NMP was added, and the cake was washed and filtered again under pressure. The weight of the recovered NMP filtrate was 80.0 kg.

[0100] -Process (3) Water was added to the obtained NMP filtrate to form a water slurry, after which solid-liquid separation and water washing were repeated twice, and then the mixture was dried in a hot air dryer at 120°C for 4 hours to obtain a powder.

[0101] Steps (4) and (5) Chloroform was added to the obtained powder, and the mixture was stirred at 65°C for 1 hour and then filtered.

[0102] -Process(6) The filtered filtrate was gradually cooled to room temperature and then filtered again, and the residue after filtration was dried in vacuo at 40° C. for 4 hours to obtain 45 g of PAS oligomer (B-1) consisting only of hexamers.

[0103] <Production Example 3> Production of PAS oligomer (b-2) The same operations as in Production Example 1 were carried out up to step (4). The filtered filtrate was gradually cooled to room temperature and then filtered again to separate out PAS oligomers containing only hexamers. The filtrate obtained was evaporated at 150 Torr and 40°C to remove chloroform, yielding 719 g of a mixture of heptamers to dodecamers.

[0104] <Production Example 4> Production of PAS oligomer (b-3) Up to the step (5), the same operations as in Production Example 1 were carried out. The residue after filtration was dried in vacuo at 40° C. for 4 hours to obtain 392 g of a linear oligomer (b-3).

[0105] Comparing the Example and Comparative Example 1 in Table 1 shows that when a mixture of hepta-dodecamers having a cyclic structure was blended as the PAS oligomer (B), even a small amount of addition changed the crystallization temperature and increased the rate of viscosity change, limiting the amount of PAS oligomer that could be used. Comparing the Example and Comparative Examples 2 and 3 also shows that the resin composition of the Example had a Tmc closer to that of Reference Example 1 and exhibited a smaller rate of viscosity change, demonstrating that it was a resin composition that could suppress thickening and delay in crystallization behavior and had excellent processability. Furthermore, Example 4 in Table 2 shows that this effect is also achieved when the resin composition contains a thermoplastic elastomer and glass fiber. Furthermore, Comparative Example 4 shows that when PAS (a-2) having a structure other than the para position is used, the viscosity change rate when PAS oligomer (B) is added is large, resulting in poor processability.

Claims

1. A polyarylene sulfide resin composition comprising a polyarylene sulfide (A) and a cyclic oligoarylene sulfide (B) as essential components, The polyarylene sulfide (A) has, as a repeating unit, a linear structure in which an aromatic ring and a sulfur atom are bonded at a para position, The cyclic oligoarylene sulfide (B) is a hexamer, and A step (1) of reacting a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent (1) to obtain a crude reaction mixture containing a polyarylene sulfide (a), a cyclic oligoarylene sulfide (B), an organic polar solvent (1), and an alkali metal halide; A step (2) of subjecting the crude reaction mixture to solid-liquid separation to obtain a reaction mixture (L1) containing at least a cyclic oligoarylene sulfide (B) and the organic polar solvent (1); A step (3) of subjecting the organic polar solvent (1) to solid-liquid separation from the reaction mixture (L1) to obtain a reaction mixture (S1) containing at least a cyclic oligoarylene sulfide (B); A step (4) of contacting the reaction mixture (S1) with an organic polar solvent (2) to obtain a mixture (L2); A step (5) of subjecting the mixture (L2) to solid-liquid separation at a temperature range higher than the boiling point of the organic polar solvent (2) minus 10° C. to recover a liquid phase component (L3); and A step (6) of gradually cooling the liquid phase component (L3) to 25° C. or less and recovering the crystallized solid phase component. The method comprises the steps of: A polyarylene sulfide resin composition, characterized in that the viscosity change rate is within the range of ±20%. (Note that the viscosity change rate is calculated from the following formula using the melt viscosity (V6) measured after holding for 6 minutes using a flow tester at a temperature of 300° C., a load of 1.96 MPa, and an orifice having an orifice length / orifice diameter ratio of 10 / 1.) Viscosity change rate (%)=(melt viscosity (Pa·s) of the polyarylene sulfide (A)−melt viscosity (Pa·s) of the polyarylene sulfide resin composition) / melt viscosity (Pa·s) of the polyarylene sulfide (A)×100.

2. The polyarylene sulfide resin composition according to claim 1, further comprising a thermoplastic elastomer (C).

3. The polyarylene sulfide resin composition according to claim 1 or 2, further comprising an inorganic filler (D).

4. A molded article obtained by melt molding the polyarylene sulfide resin composition according to claim 1 or 2.

5. A method for producing a polyarylene sulfide resin composition, comprising a step of blending a polyarylene sulfide (A) and a cyclic oligoarylene sulfide (B) as essential components, and melt-kneading the blend at a temperature equal to or higher than the melting point of the polyarylene sulfide (A), The polyarylene sulfide (A) has, as a repeating unit, a linear structure in which an aromatic ring and a sulfur atom are bonded at a para position, The cyclic oligoarylene sulfide (B) is a hexamer, and A step (1) of reacting a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent (1) to obtain a crude reaction mixture containing a polyarylene sulfide (a), a cyclic oligoarylene sulfide (B), an organic polar solvent (1), and an alkali metal halide; A step (2) of subjecting the crude reaction mixture to solid-liquid separation to obtain a reaction mixture (L1) containing at least a cyclic oligoarylene sulfide (B) and the organic polar solvent (1); A step (3) of subjecting the organic polar solvent (1) to solid-liquid separation from the reaction mixture (L1) to obtain a reaction mixture (S1) containing at least a cyclic oligoarylene sulfide (B); A step (4) of contacting the reaction mixture (S1) with an organic polar solvent (2) to obtain a mixture (L2); A step (5) of subjecting the mixture (L2) to solid-liquid separation at a temperature range higher than the boiling point of the organic polar solvent (2) minus 10° C. to recover a liquid phase component (L3); and The liquid phase component (L3) is gradually cooled to 25° C. or less, and a crystallized solid phase component is recovered (6). A method for producing a polyarylene sulfide resin composition, characterized in that the viscosity change rate is within a range of ±20%. (Note that the viscosity change rate is calculated from the following formula using the melt viscosity (V6) measured after holding for 6 minutes using a flow tester at a temperature of 300° C., a load of 1.96 MPa, and an orifice having an orifice length / orifice diameter ratio of 10 / 1.) Viscosity change rate (%)=(melt viscosity (Pa·s) of the polyarylene sulfide (A)−melt viscosity (Pa·s) of the polyarylene sulfide resin composition) / melt viscosity (Pa·s) of the polyarylene sulfide (A)×100.

6. The method for producing a polyarylene sulfide resin composition according to claim 5, further comprising blending a thermoplastic elastomer (C).

7. The method for producing a polyarylene sulfide resin composition according to claim 5 or 6, further comprising blending an inorganic filler (D).

8. A method for producing a polyarylene sulfide resin molded article, comprising the steps of producing a resin composition by the method according to claim 5 or 6, and melt molding the resin composition.

Citation Information

Patent Citations

  • Polyarylene sulfide resin composition

    JP2001172500A

  • Method for producing polyarylene sulfide

    JP2011173953A

  • Method for producing polyarylene sulfide

    JP2012092315A

  • Cyclic polyarylene sulfide composition

    JP2016011382A