Polyarylene sulfide resin composition, molded product and method for producing the same
The blending of cyclic and chain PAS oligomers in a specific ratio with optional components addresses the balance between crystallization speed and melt viscosity, enhancing processability and mechanical properties in PAS resin compositions.
Patent Information
- Application Number
- JP2023073259
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Existing polyarylene sulfide (PAS) resin compositions face challenges in achieving an optimal balance between crystallization speed and melt viscosity while effectively utilizing PAS oligomers, leading to processability issues and environmental inefficiencies due to the disposal of these by-products.
A PAS resin composition is formulated by blending cyclic and chain oligomers in a specific ratio with linear PAS, maintaining a viscosity change rate within ±20%, and incorporating optional components like thermoplastic elastomers and inorganic fillers to enhance mechanical properties.
The composition achieves an excellent balance between crystallization rate and melt viscosity, improving processability and mechanical properties while being environmentally friendly by utilizing PAS oligomers.
Smart Images

Figure 2024158233000001 
Figure 2024158233000002 
Figure 2024158233000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyarylene sulfide resin composition, a molded article, and a method for producing the same. [Background technology]
[0002] Polyarylene sulfide (PAS) resins, such as polyphenylene sulfide (PPS) resin, have excellent heat resistance and chemical resistance and are widely used in electrical and electronic components, automotive parts, water heater parts, fibers, films, etc.
[0003] PAS resins are obtained by a method of polymerizing a sulfidizing agent and a polyhalo aromatic compound in a polar organic solvent such as N-methyl-2-pyrrolidone (NMP). At this time, by-products such as oligoarylene sulfide (hereinafter sometimes referred to as PAS oligomer), residual sulfidizing agent, and sodium chloride are also generated at the same time, but these by-products are considered impurities and have not been used in the past. In particular, most of the PAS oligomers contained in the liquid phase component obtained by solid-liquid separation of the solvent slurry after polymerization are discarded as industrial waste, resulting in significant losses in production in terms of raw material costs and disposal costs. In addition, there was a lack of consideration for the global environment in that limited resources could not be used effectively.
[0004] As an attempt to blend a PAS oligomer as a raw material for a PAS resin composition, for example, Patent Document 1 discloses a resin composition blended with a PAS resin, a PAS oligomer having at least one SH terminal and a molecular weight of 2000 or less, and an alkoxysilane compound. However, cyclic PAS oligomers may thicken due to ring-opening polymerization during melt kneading, or may slow the crystallization rate of the resin composition, and there have been few examples of their use as a raw material for PAS resin compositions due to concerns about processability and mechanical properties. As techniques for controlling the reactivity of cyclic PAS oligomers during heating, a method of blending an organic carboxylic acid compound (Patent Document 2, etc.), a method of blending a low-valent iron compound (Patent Document 3, etc.), a method of blending a carboxylic acid copper compound (Patent Document 4, etc.), etc. are known, but there are problems such as limited heating conditions and side reactions with other components. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2001-172500 A [Patent Document 2] JP 2011-173953 A [Patent Document 3] JP 2012-92315 A [Patent Document 4] JP 2016-11382 A Summary of the Invention [Problem to be solved by the invention]
[0006] Therefore, the problem that the present invention aims to solve is to provide a resin composition that utilizes a PAS oligomer and has an excellent balance between crystallization rate and melt viscosity while being environmentally friendly, as well as a molded product obtained by melt molding the resin composition, and a method for producing the same. [Means for solving the problem]
[0007] As a result of extensive investigations, the inventors of the present application discovered that the above-mentioned problems could be solved by blending with PAS a mixture in a specific ratio of cyclic oligomers and linear oligomers, which are PAS oligomers produced as by-products during the polymerization of PAS, and thus completed the present invention.
[0008] That is, the present disclosure is A PAS resin composition comprising a linear PAS (A) and a PAS oligomer (B) as essential components, the mass ratio of the cyclic PAS oligomer (X) to the linear PAS oligomer (Y) in the PAS oligomer (B) is 0:100 to 66:33; The amount of the PAS oligomer (B) is 5.0 parts by mass or less per 100 parts by mass of the linear PAS (A), and This relates to a PAS resin composition whose viscosity change rate is within the range of ±20%.
[0009] The present disclosure further relates to a molded article obtained by melt molding the above-described PAS resin composition.
[0010] The present disclosure further provides: A method for producing a PAS resin composition, comprising a step of blending a linear PAS (A) and a PAS oligomer (B) as essential components, and melt-kneading the mixture at a temperature equal to or higher than the melting point of the PAS, the mass ratio of the cyclic PAS oligomer (X) to the linear PAS oligomer (Y) in the PAS oligomer (B) is 0:100 to 66:33; The present invention relates to a method for producing a PAS resin composition, wherein the blending amount of the PAS oligomer (B) is 5.0 parts by mass or less per 100 parts by mass of the linear PAS (A), and the viscosity change rate is within the range of ±20%.
[0011] The present disclosure further relates to a method for producing a PAS resin molded product, comprising the steps of producing a resin composition by the above-described method, and melt-molding the resin composition.
[0012] In the present invention, a compound having a repeat number of 2 to 40 (a mixture of dimers to 40-mers) is sometimes referred to as an "oligomer," and a compound having a repeat number of 41 or more is sometimes referred to as a "polymer." Effect of the Invention
[0013] According to the present invention, by utilizing a PAS oligomer, it is possible to provide a resin composition that has an excellent balance between crystallization rate and melt viscosity while being environmentally friendly, as well as a molded article obtained by melt molding the resin composition and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] An embodiment of the present invention will be described in detail below, but the scope of the present invention is not limited to the embodiment described here, and various modifications can be made without departing from the spirit of the present invention. In addition, when multiple upper and lower limit values are described for a specific parameter, any upper and lower limit values can be combined to form a suitable numerical range.
[0015] <Resin composition> The resin composition according to the present embodiment is a PAS resin composition comprising a linear PAS (A) and a PAS oligomer (B) as essential components, the mass ratio of the cyclic PAS oligomer (X) to the linear PAS oligomer (Y) in the PAS oligomer (B) is 0:100 to 66:33; The amount of the PAS oligomer (B) is 5.0 parts by mass or less per 100 parts by mass of the linear PAS (A), and The viscosity change rate is within the range of ±20%.
[0016] <PAS(A)> The PAS resin composition according to this embodiment contains a linear PAS (A) as an essential component. Crosslinked PAS is not applicable.
[0017] The PAS (A) applicable to the present embodiment is a polymer having a resin structure in which a repeating unit is a structure in which an aromatic ring and a sulfur atom are bonded, and specifically, a PAS (A) represented by the following general formula (1):
[0018] [ka] (In the formula, R 1 and R 2 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a nitro group, an amino group, a phenyl group, a methoxy group, or an ethoxy group.
[0019] Here, the structural portion represented by the general formula (1) is particularly R 1 and R 2 is preferably a hydrogen atom from the viewpoint of the mechanical strength of the PAS resin, and in that case, examples include those bonded at the para position represented by the following formula (2) and those bonded at the meta position represented by the following formula (3).
[0020] [ka] Among these, a structure in which the bond between the sulfur atom and the aromatic ring in the repeating unit is at the para position represented by the general formula (2) is particularly preferred in terms of the heat resistance and crystallinity of the PAS resin.
[0021] The PAS resin may contain not only the structural moieties represented by the general formulae (1) to (3) but also the structural moieties represented by the following structural formulae (4) to (7):
[0022] [ka] The structural moieties represented by the general formulae (1) to (3) may be contained in an amount of 30 mol % or less in total, based on the structural moieties represented by the general formulae (1) to (3). In particular, in the present disclosure, it is preferable that the structural moieties represented by the general formulae (4) to (7) are 10 mol % or less in terms of the heat resistance and mechanical strength of PAS (A). When the structural moieties represented by the general formulae (4) to (7) are contained in PAS (A), the bonding mode thereof may be either a random copolymer or a block copolymer.
[0023] In addition, the PAS (A) may have naphthyl sulfide bonds or the like in its molecular structure, but the amount of such bonds is preferably 3 mol % or less, and particularly preferably 1 mol % or less, based on the total number of moles including other structural portions.
[0024] The physical properties of the PAS (A) are not particularly limited as long as they do not impair the effects of the present invention, but are as follows.
[0025] (Melt Viscosity) The melt viscosity of the PAS (A) used in the present disclosure is not particularly limited, but in order to obtain a good balance between fluidity and mechanical strength, the melt viscosity (V6) measured at 300°C is preferably in the range of 2 Pa·s or more, more preferably in the range of 5 Pa·s or more, and preferably in the range of 500 Pa·s or less, more preferably in the range of 200 Pa·s or less. The most suitable range is 5 Pa·s or more to 100 Pa·s or less. However, the melt viscosity (V6) is measured using a Shimadzu flow tester, CFT-500D, at 300°C, load: 1.96×10 6 The melt viscosity is measured after holding the sample for 6 minutes at a pressure of 1 Pa and L / D = 10 (mm) / 1 (mm).
[0026] (Non-Newtonian Exponents) The non-Newtonian index of the PAS (A) used in the present disclosure is not particularly limited, but is preferably in the range of 0.90 or more, more preferably 0.95 or more, and preferably 1.50 or less, more preferably 1.20 or less. Such a PAS (A) has excellent mechanical properties, fluidity, and abrasion resistance. However, the non-Newtonian index (N value) in the present disclosure is a value calculated using the following formula by measuring the shear rate (SR) and shear stress (SS) using a capillary rheometer under the conditions of melting point +20°C and a ratio of orifice length (L) to orifice diameter (D) of L / D=40. The closer the non-Newtonian index (N value) is to 1, the closer the structure is to a linear structure, and the higher the non-Newtonian index (N value), the more branched the structure is.
[0027]
number
[0028] (Manufacturing method) The method for producing the PAS (A) is not particularly limited, and examples thereof include (Production Method 1) a method in which a dihalogeno aromatic compound is polymerized in the presence of sulfur and sodium carbonate, and if necessary, a polyhalogeno aromatic compound or other copolymerization component is added, (Production Method 2) a method in which a dihalogeno aromatic compound is polymerized in a polar solvent in the presence of a sulfidizing agent or the like, and if necessary, a polyhalogeno aromatic compound or other copolymerization component is added, (Production Method 3) a method in which p-chlorothiophenol is added, and if necessary, other copolymerization components are added, and self-condensed, and (Production Method 4) a method in which a diiodo aromatic compound and elemental sulfur are melt-polymerized under reduced pressure in the presence of a polymerization inhibitor that may have a functional group such as a carboxy group or an amino group. Among these methods, (Production Method 2) is preferred because it is versatile. During the reaction, an alkali metal salt of a carboxylic acid or sulfonic acid or an alkali hydroxide may be added to adjust the degree of polymerization. Among the above-mentioned (Production Method 2) methods, there is a method for producing PAS by introducing a water-containing sulfidizing agent into a mixture containing a heated organic polar solvent and a dihalogeno aromatic compound at a rate at which water can be removed from the reaction mixture, and reacting the dihalogeno aromatic compound with the sulfidizing agent in the organic polar solvent, and optionally adding a polyhalogeno aromatic compound, and controlling the amount of water in the reaction system to within a range of 0.02 to 0.5 moles per mole of the organic polar solvent (see JP-A-07-228699). Particularly preferred is a method in which a dihalogeno-aromatic compound and, if necessary, a polyhalogeno-aromatic compound or other copolymerization component are added in the presence of potassium metal sulfide and an aprotic polar organic solvent, and an alkali metal hydrosulfide and an organic acid alkali metal salt are reacted while controlling the organic acid alkali metal salt in the range of 0.01 to 0.9 mol per mol of the sulfur source and the amount of water in the reaction system to 0.02 mol or less per mol of the aprotic polar organic solvent (see WO2010 / 058713 pamphlet).Specific examples of the dihalogenoaromatic compound include p-dihalobenzene, m-dihalobenzene, o-dihalobenzene, 2,5-dihalotoluene, 1,4-dihalonaphthalene, 1-methoxy-2,5-dihalobenzene, 4,4'-dihalobiphenyl, 3,5-dihalobenzoic acid, 2,4-dihalobenzoic acid, 2,5-dihalonitrobenzene, 2,4-dihalonitrobenzene, 2,4-dihaloanisole, p,p'-dihalodiphenyl ether, 4,4'-dihalobenzophenone, 4,4'-di Examples of the polyhalogeno aromatic compounds include 1,2,3-trihalobenzene, 1,2,4-trihalobenzene, 1,3,5-trihalobenzene, 1,2,3,5-tetrahalobenzene, 1,2,4,5-tetrahalobenzene, 1,4,6-trihalonaphthalene, etc. The halogen atoms contained in the above compounds are preferably chlorine atoms or bromine atoms.
[0029] The method for post-treating the reaction mixture containing PAS obtained by the polymerization step is not particularly limited, and examples thereof include (post-treating 1) a method in which, after the completion of the polymerization reaction, the solvent is first distilled off under reduced pressure or normal pressure, either as is or after the addition of an acid or base, and then the solid remaining after the solvent distillation is washed once or more than twice with a solvent such as water, the reaction solvent (or an organic solvent having a similar solubility to the low molecular weight polymer), acetone, methyl ethyl ketone, or alcohols, and then neutralized, washed with water, filtered, and dried; or (post-treating 2) a method in which, after the completion of the polymerization reaction, the reaction mixture is dissolved in a solvent such as water, acetone, methyl ethyl ketone, alcohols, ethers, halogenated hydrocarbons, aromatic hydrocarbons, aliphatic hydrocarbons, or the like (a solvent that is soluble in the polymerization solvent used and is a poor solvent for at least PAS). or (post-treatment 3) after the polymerization reaction is completed, the reaction mixture is added with a reaction solvent (or an organic solvent having a solubility equivalent to that of the low molecular weight polymer) and stirred, and then filtered to remove the low molecular weight polymer, followed by washing once or twice or more times with a solvent such as water, acetone, methyl ethyl ketone, or an alcohol, followed by neutralization, washing with water, filtration, and drying; (post-treatment 4) after the polymerization reaction is completed, the reaction mixture is added with water, washed with water, filtered, and if necessary, acid is added during the water washing to perform an acid treatment, and then dried; or (post-treatment 5) after the polymerization reaction is completed, the reaction mixture is filtered, and if necessary, washed once or twice or more times with the reaction solvent, followed by further washing with water, filtration, and drying.
[0030] In the post-treatment methods exemplified above in (Post-treatment 1) to (Post-treatment 5), the PAS may be dried in a vacuum, or in air or in an inert gas atmosphere such as nitrogen.
[0031] The PAS (A) used in this embodiment may be a PAS newly polymerized by the above method, or a recycled PAS. For example, a PAS recovered from a PAS resin composition or a PAS resin molded product may be used. Specifically, a PAS obtained by heating a PAS resin composition or a PAS resin molded product in an organic polar solvent to dissolve the PAS contained therein and performing the above-mentioned post-treatment on the solution may be used. In addition, a PAS resin composition or a PAS resin molded product mechanically crushed may be used as the PAS. Specifically, a sprue or runner generated during the manufacture of a molded product, a product recovered as a non-standard molded product, or a molded product once used as a product may be crushed. In this case, a crushed product of a PAS resin composition or a PAS resin molded product containing a component other than PAS may be used.
[0032] <Oligoarylene sulfide (B)> The PAS resin composition according to this embodiment further contains a PAS oligomer (B) as an essential component. The PAS oligomer (B) applicable to this embodiment has a mass ratio of the cyclic oligomer (X) to the linear oligomer (Y) of 0:100 to 66:33. The PAS oligomer (B) in this disclosure has a resin structure in which a repeating unit is a structure in which an aromatic ring and a sulfur atom are bonded, similar to the PAS (A), and can contain the above formulas (1) to (6) as constituent units.
[0033] In the present embodiment, the amount of PAS oligomer (B) is preferably 5.0 parts by mass or less, more preferably 4.5 parts by mass or less, per 100 parts by mass of PAS (A) from the viewpoint of the processability and mechanical properties of the resulting resin composition and molded article. On the other hand, the lower limit is not particularly limited as long as it does not impair the effects of the present invention, but is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, per 100 parts by mass of PAS (A) from the viewpoint of the recovery rate of the PAS oligomer.
[0034] (Manufacturing method) The method for producing the PAS oligomer (B) applicable to this embodiment is not particularly limited, but for example, a cyclic oligomer (X) produced by steps (1) to (6) and a linear oligomer (Y) produced by steps (1) to (4) and (7) as shown below can be mixed and used. The method will be explained below.
[0035] -Process (1) Step (1) is a step of reacting a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide, in an organic polar solvent (1) to obtain a crude reaction mixture containing PAS (a), PAS oligomer (b), the organic polar solvent (1), and an alkali metal halide.
[0036] Here, in this process, the polyhalo aromatic compound is, for example, a halogenated aromatic compound having two or more halogen atoms directly bonded to aromatic ring, specifically, p-dichlorobenzene, o-dichlorobenzene, m-dichlorobenzene, trichlorobenzene, tetrachlorobenzene, dibromobenzene, diiodobenzene, tribromobenzene, dibromonaphthalene, triiodobenzene, dichlorodiphenylbenzene, dibromodiphenylbenzene, dichlorobenzophenone, dibromobenzophenone, dichlorodiphenylether, dibromodiphenylether, dichlorodiphenylsulfide, dibromodiphenylsulfide, dichlorobiphenyl, dibromobiphenyl and other dihalo aromatic compounds and their mixtures can be mentioned, and these compounds can be block copolymerized.Among these, dihalogenated benzenes are preferred, and those containing 80 mol% or more of p-dichlorobenzene are particularly preferred. In addition, in order to increase the viscosity of the PAS resin by forming a branched structure, a polyhaloaromatic compound having three or more halogen substituents in one molecule may be used as a branching agent as desired. Examples of such polyhaloaromatic compounds include 1,2,4-trichlorobenzene, 1,3,5-trichlorobenzene, and 1,4,6-trichloronaphthalene. Further examples include polyhaloaromatic compounds having a functional group having active hydrogen, such as an amino group, a thiol group, or a hydroxyl group. Specific examples include dihaloanilines such as 2,6-dichloroaniline, 2,5-dichloroaniline, 2,4-dichloroaniline, and 2,3-dichloroaniline; trihaloanilines such as 2,3,4-trichloroaniline, 2,3,5-trichloroaniline, 2,4,6-trichloroaniline, and 3,4,5-trichloroaniline; dihaloaminodiphenyl ethers such as 2,2'-diamino-4,4'-dichlorodiphenyl ether and 2,4'-diamino-2',4-dichlorodiphenyl ether; and mixtures thereof in which the amino group is replaced with a thiol group or a hydroxyl group.In addition, active hydrogen-containing polyhalogenated aromatic compounds in which the hydrogen atoms bonded to the carbon atoms forming the aromatic rings in these active hydrogen-containing polyhalogenated aromatic compounds are substituted with other inert groups, for example, hydrocarbon groups such as alkyl groups, can also be used.
[0037] Among these various active hydrogen-containing polyhaloaromatic compounds, active hydrogen-containing dihaloaromatic compounds are preferred, and dichloroaniline is particularly preferred.
[0038] Examples of polyhaloaromatic compounds having a nitro group include mono- or dihalonitrobenzenes such as 2,4-dinitrochlorobenzene and 2,5-dichloronitrobenzene; dihalonitrodiphenyl ethers such as 2-nitro-4,4'-dichlorodiphenyl ether; dihalonitrodiphenyl sulfones such as 3,3'-dinitro-4,4'-dichlorodiphenyl sulfone; mono- or dihalonitropyridines such as 2,5-dichloro-3-nitropyridine and 2-chloro-3,5-dinitropyridine; and various dihalonitronaphthalenes.
[0039] In this step, an alkali metal sulfide or an alkali hydrosulfide and an alkali metal hydroxide (hereinafter sometimes referred to as a sulfidizing agent) are used as raw materials.
[0040] In this step, the alkali metal sulfide includes lithium sulfide, sodium sulfide, rubidium sulfide, cesium sulfide, and mixtures thereof. Such alkali metal sulfides can be used as hydrates, aqueous mixtures, or anhydrides. The alkali metal sulfides can also be derived by reacting an alkali metal hydrosulfide with an alkali metal hydroxide. Note that a small amount of an alkali metal hydroxide may be added to react with the alkali metal hydrosulfide and alkali metal thiosulfate that are usually present in trace amounts in the alkali metal sulfide.
[0041] The alkali metal hydrosulfides include lithium hydrogen sulfide, sodium hydrogen sulfide, rubidium hydrogen sulfide, cesium hydrogen sulfide, and mixtures thereof. The alkali metal hydrosulfides can be used as hydrates, aqueous mixtures, or anhydrous forms.
[0042] The alkali metal hydrosulfide is used together with an alkali metal hydroxide. Examples of the alkali metal hydroxide include lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, and cesium hydroxide, and these may be used alone or in combination of two or more. Among these, lithium hydroxide, sodium hydroxide, and potassium hydroxide are preferred because of their easy availability, and sodium hydroxide is particularly preferred.
[0043] In this step, a hydrous sulfidizing agent can also be used as a raw material, and in this case, it is preferable to dehydrate the hydrous sulfidizing agent in the presence of at least an aprotic polar solvent, and then subject it to the polymerization reaction of the PAS resin. In addition, when the amount of the aprotic polar solvent is small, for example, when it is less than 1 mole per mole of sulfur atom of the sulfidizing agent, it is preferable to dehydrate the hydrous sulfidizing agent and the aprotic polar solvent in the presence of a polyhalo aromatic compound.
[0044] The dehydration step of the hydrous sulfidizing agent is carried out by charging at least an aprotic polar solvent and a hydrous alkali metal sulfide or a hydrous alkali hydrosulfide and an alkali metal hydroxide as the hydrous sulfidizing agent into a reaction vessel equipped with a distillation apparatus, heating to a temperature at which water is removed by azeotropy, specifically, to a temperature in the range of 300° C. or less, preferably 80 to 220° C., more preferably 100 to 200° C., and discharging water by distillation out of the system. In the dehydration step, dehydration is preferably carried out until the amount of water in the polymerization system is 5 mol or less, more preferably 0.01 to 2.0 mol, per mol of sulfur atoms in the sulfidizing agent.
[0045] Examples of the organic polar solvent (1) in this step include amides, ureas, and lactams such as formamide, acetamide, N-methylformamide, N,N-dimethylacetamide, tetramethylurea, N-methyl-2-pyrrolidone, 2-pyrrolidone, N-methyl-ε-caprolactam, ε-caprolactam, hexamethylphosphoramide, N-dimethylpropyleneurea, and 1,3-dimethyl-2-imidazolidinoic acid; sulfolanes such as sulfolane and dimethylsulfolane; nitriles such as benzonitrile; ketones such as methylphenylketone, and mixtures thereof. Among these, amides having an aliphatic cyclic structure, such as N-methyl-2-pyrrolidone, 2-pyrrolidone, N-methyl-ε-caprolactam, ε-caprolactam, hexamethylphosphoramide, N-dimethylpropyleneurea, and 1,3-dimethyl-2-imidazolidinoic acid, are preferred, and N-methyl-2-pyrrolidone is more preferred.
[0046] In the reaction in this step, the above-mentioned alkali metal sulfide as a sulfidizing agent is reacted with a polyhaloaromatic compound in the presence of these organic polar solvents. Alternatively, in the reaction, the above-mentioned alkali metal hydrosulfide and alkali metal hydroxide as sulfidizing agents are reacted with a polyhaloaromatic compound in the presence of these organic polar solvents. The reaction conditions are generally a temperature in the range of 200 to 330°C, and a pressure in the range that substantially keeps the polymerization solvent and the polyhaloaromatic compound as a polymerization monomer in a liquid phase, and are generally selected from the range of 0.1 to 20 MPa, preferably from the range of 0.1 to 2 MPa. The amount of the polyhaloaromatic compound charged is adjusted to be in the range of 0.2 mol to 5.0 mol, preferably in the range of 0.8 to 1.3 mol, more preferably in the range of 0.9 to 1.1 mol, relative to 1 mol of sulfur atom of the sulfidizing agent. The amount of the aprotic polar solvent is adjusted to be in the range of 1.0 to 6.0 mol, preferably 2.5 to 4.5 mol, per mol of sulfur atom of the sulfidizing agent. The polymerization reaction is preferably carried out in the presence of a small amount of water, and the ratio is preferably adjusted appropriately in consideration of the polymerization method, the molecular weight of the obtained polymer, and the productivity. Specifically, the dehydration operation is carried out so that the amount of water is in the range of 2.0 mol or less, preferably 1.6 mol or less, per mol of sulfur atom of the sulfidizing agent. In addition, when the dehydration operation is carried out in the presence of a polyhalo aromatic compound (for example, the method of "5)" in the specific embodiment below), the dehydration operation may be carried out so that the amount of water is in the range of 0.9 mol or less, preferably 0.05 to 0.3 mol, more preferably 0.01 to 0.02 mol.
[0047] Specific examples of the polymerization of a sulfidizing agent and a polyhaloaromatic compound in the presence of the above-mentioned aprotic polar solvent include, for example, 1) A method using a polymerization aid such as an alkali metal carboxylate or a lithium halide, 2) A method using a branching agent such as an aromatic polyhalogen compound, 3) A method in which the polymerization reaction is carried out in the presence of a small amount of water and then water is added to further polymerize; 4) A method in which the gas phase of a reaction vessel is cooled during the reaction of an alkali metal sulfide with an aromatic dihalogen compound, and a part of the gas phase in the reaction vessel is condensed and refluxed to the liquid phase; 5) A method for producing a PAS resin, which includes, as essential production steps, a step of reacting an alkali metal sulfide or a hydrous alkali metal hydrosulfide and an alkali metal hydroxide with an amide, urea or lactam having an aliphatic cyclic structure in the presence of a polyhalo aromatic compound while dehydrating to produce a slurry containing a solid alkali metal sulfide, a step of adding a polar organic solvent such as NMP after producing the slurry and distilling off water to perform dehydration, and a step of reacting a polyhalo aromatic compound, an alkali metal hydrosulfide, and an alkali metal salt of a hydrolyzate of the amide, urea or lactam having an aliphatic cyclic structure in the slurry obtained through the dehydration step at a water content of 0.02 mol or less in the reaction system per 1 mol of the polar organic solvent such as NMP to polymerize.
[0048] In this way, by polymerizing a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent, PAS (a) and PAS oligomer (B) are obtained as products, and a linear PAS oligomer is also produced as a by-product. In addition, the substances remaining after the reaction may include by-products such as alkali metal-containing inorganic salts, carboxyalkylamino group-containing compounds, and terminal SH group-containing compounds, as well as unreacted raw materials and water.
[0049] -Process (2) The step (2) is a step of subjecting the crude reaction mixture to solid-liquid separation to obtain a reaction mixture (L1) containing at least the PAS oligomer (b) and the organic polar solvent (1).
[0050] The solid-liquid separation is broadly divided into two types, the flash method and the quench method, which will be described later. In this step, the quench method is preferred in order to obtain a liquid phase component.
[0051] The quench method is a method for separating and recovering particulate PAS (a) by gradually cooling the crude reaction mixture from a high-temperature, high-pressure state, and then crystallizing the PAS (a) in the reaction system, and then recovering the solid content containing PAS (a) as granules by solid-liquid separation by filtration or the like to obtain a liquid phase component. There is no particular limit to the cooling time, but the preferred range is usually 0.1°C / min to 3°C / min. In addition, it is not necessary to slowly cool at the same rate throughout the entire slow cooling process, and a method in which the rate is in the range of 0.1°C / min to 1°C / min until the granular material of PAS (a) crystallizes, and then cooling at a rate of 1°C / min or more is also preferred. It is preferable to finally cool to 70°C or higher, preferably 100°C or higher and 200°C or lower, and then recover the solid content containing the PAS resin by solid-liquid separation. Examples of solid-liquid separation in the quench method include filtration and a method using a centrifuge such as a screw decanter.
[0052] -Process (3) The step (3) is a step of performing solid-liquid separation of the organic polar solvent (1) from the reaction mixture (L1) to obtain a reaction mixture (S1) containing at least a PAS oligomer (b).
[0053] The method for removing the organic polar solvent (1) from the reaction mixture (L1) can be exemplified by a flash method in which the solvent is evaporated to recover the solvent and at the same time a solid is recovered, or by removing the solvent using a membrane. A preferred embodiment of the flash method is a method in which the high-temperature, high-pressure (usually 250°C or higher, 0.8 MPa or higher) reaction mixture (L1) obtained in the polymerization step is ejected from a nozzle into an atmosphere of nitrogen or water vapor under normal pressure. In the flash method, the solvent can be efficiently recovered by utilizing the heat of vaporization of the solvent when the polymerization reactant is flashed from a high-temperature, high-pressure state to a normal pressure state, and the higher the internal temperature during flashing, the higher the efficiency of solvent recovery and the better the productivity. Therefore, the temperature and pressure in the polymerization system during flashing are usually set to 250°C or higher, preferably in the range of 255 to 280°C, and 0.8 MPa or higher, preferably in the range of 1.0 to 5.0 MPa. The atmospheric temperature when flashing from this state to reduced pressure or normal pressure is usually in the range of 150 to 250°C. If the recovery of the solvent from the crude reaction mixture is insufficient, heating may be continued in an atmosphere of 150 to 250°C after flashing.
[0054] When removing the organic polar solvent (1), it is desirable to remove the organic polar solvent so that the ratio of solids (non-volatile content) is in the range of 20 to 100 mass%, preferably 20 to 99.99 mass%, and more preferably 30 to 90 mass%. The temperature when removing the organic polar solvent by heating depends on the properties of the organic polar solvent used and cannot be uniquely limited, but can usually be selected in the range of 20 to 150°C, preferably 40 to 120°C. In addition, the pressure at which the organic polar solvent is removed is preferably normal pressure or lower, which makes it possible to remove the organic polar solvent at a lower temperature.
[0055] -Process (4) Step (4) is a step of contacting the reaction mixture (S1) with an organic polar solvent (2) to obtain a mixture (L2).
[0056] The organic polar solvent (2) used in this step is preferably one that does not substantially cause undesirable side reactions such as decomposition or crosslinking of the PAS (A) and the PAS oligomer (b), and a solvent similar to the organic polar solvent (1) can be used. Examples of the organic polar solvent (2) include aromatic hydrocarbon solvents such as toluene and xylene; halogen-based solvents such as chloroform, bromoform, methylene chloride, 1,2-dichloroethane, 1,1,1-trichloroethane, chlorobenzene, and 2,6-dichlorotoluene; ether-based solvents such as diethyl ether, tetrahydrofuran, and diisopropyl ether; amides such as formamide, acetamide, N-methylformamide, N,N-dimethylformamide, N,N-dimethylacetamide, tetramethylurea, N-methyl-2-pyrrolidone, 2-pyrrolidone, N-methyl-ε-caprolactam, ε-caprolactam, hexamethylphosphoramide, N-dimethylpropyleneurea, and 1,3-dimethyl-2-imidazolidinoic acid, urea, and lactams; and polar solvents such as dimethylsulfoxide, trimethylphosphoric acid, N,N-dimethylimidazolidinone, and methyl ethyl ketone. Of these, the organic polar solvent (2) has a dipole moment μ of 1 [D] (※1D=3.3356×10 -30 It is preferable to use a polar solvent with a dielectric constant (ε(20°C)) of 2 or more.
[0057] The method of contacting the reaction mixture (S1) with the organic polar solvent (2) is not particularly limited, and for example, the reaction mixture (S1) is mixed with the organic polar solvent (2), and the mixture is contacted at a temperature in the range of 10 to 200°C, preferably 50 to 150°C, more preferably 80 to 130°C, and then separated into a liquid phase component containing the PAS oligomer (B) and a solid component. The pressure when the reaction mixture (S1) and the organic polar solvent (2) are contacted may be either normal pressure or pressurized, but it is preferable to carry out the contact under a pressurized condition in the range of 0.1 to 0.5 [MPa]. The atmosphere when the reaction mixture (S1) and the organic polar solvent (2) are contacted is not particularly limited, but when the PAS oligomer (b) or the organic polar solvent (2) is oxidized and deteriorated due to the conditions such as the temperature and time when the reaction mixture is contacted, it is preferable to carry out the reaction under a non-oxidizing atmosphere. A non-oxidizing atmosphere refers to an atmosphere in which the oxygen concentration in the gas phase is 5% by volume or less, preferably 2% by volume or less, and more preferably contains substantially no oxygen, i.e., an inert gas atmosphere such as nitrogen, helium, or argon.
[0058] -Process (5) The step (5) is a step of gradually cooling the mixture (L2) to 25° C. or lower and removing the solid phase component to obtain a liquid phase component (L3).
[0059] The cooling of the mixture (L2) is not particularly limited as long as it does not impair the effects of the present invention, and known devices and methods can be used. In the present disclosure, slow cooling does not mean rapid cooling, and for example, the cooling rate is preferably in the range of 1°C / min or less. In addition, it is not necessary to cool at the same rate throughout the entire slow cooling process. By cooling the mixture (L2) to 25°C, the linear PAS oligomers and hexamer cyclic PAS oligomers become contained in the mixture (L2) as solid phase components, and can be recovered as solids.
[0060] The method for removing the solid phase components and recovering the liquid phase components is not particularly limited as long as it does not impair the effects of the present invention, and known devices and methods can be used. For example, separation can be performed using a centrifuge such as a screw decanter or a filtration device.
[0061] -Process(6) The step (6) is a step of concentrating the liquid phase component (L3).
[0062] The method for concentrating the liquid phase component (L3) is not particularly limited as long as it does not impair the effects of the present invention, and known devices and methods can be used. For example, the liquid phase component (L3) is supplied into an evaporator and heated at less than 230° C. under reduced pressure or normal pressure.
[0063] The evaporator used in this step is not particularly limited as long as it is made of a material resistant to organic polar solvents and is a container that can be heated and decompressed, and any known evaporator can be used, for example, an evaporator, an autoclave, a thin-film evaporator, etc.
[0064] The temperature in the evaporator when concentrating the liquid phase component (L3) is not particularly limited, but from the viewpoint of suppressing decomposition of the contained PAS oligomer, it is preferably less than 230° C., and more preferably not more than 200° C. The pressure in the evaporator is preferably not more than normal pressure, specifically, preferably in the range of 10 to 760 mmHg.
[0065] In addition, when concentrating the liquid phase component (L3), it is desirable to adjust the amount of solvent removed so that the proportion of solids (non-volatile content) contained therein is in the range of 20 to 100 mass%, preferably 20 to 99.99 mass%, and more preferably 40 to 90 mass%.
[0066] -Process(7) In step (7), the mixture (L2) is subjected to solid-liquid separation at a temperature range equal to or higher than the boiling point of the organic polar solvent (2) minus 10° C. to recover a solid phase component (S2). By performing solid-liquid separation in such a temperature range, it is possible to efficiently recover only linear PAS oligomers without recovering cyclic PAS oligomers.
[0067] The method for recovering the solid phase component (S2) by solid-liquid separation is not particularly limited as long as it does not impair the effects of the present invention, and known devices and methods can be used, as in the above-mentioned step (3) etc.
[0068] <Thermoplastic elastomer (C)> The PAS resin composition according to the present embodiment may contain a thermoplastic elastomer (C) as an optional component, if necessary, for the purpose of improving mechanical properties. By further including the thermoplastic elastomer (C), the toughness and thermal shock resistance of the PAS resin composition can be further improved.
[0069] The thermoplastic elastomer (C) may be a polyolefin elastomer, a fluorine elastomer, or a silicone elastomer, among which polyolefin elastomers are preferred. When these elastomers are added, the amount is not particularly limited, but is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 1 part by mass or more, relative to 100 parts by mass of the PAS (A). On the other hand, the amount of the thermoplastic elastomer is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less. In this range, the flexibility of the resulting PAS resin composition is improved, which is preferable. If the amount exceeds this range, it may have adverse effects such as a deterioration in the drowning property of the resin composition or an increase in the amount of gas generated.
[0070] Examples of the polyolefin-based elastomer include homopolymers of α-olefins, copolymers of two or more α-olefins, and copolymers of one or more α-olefins and vinyl polymerizable compounds having functional groups. In this case, examples of the α-olefins include α-olefins having 2 or more to 8 or less carbon atoms, such as ethylene, propylene, and 1-butene. Examples of the functional groups include carboxy groups, acid anhydride groups (-C(=O)OC(=O)-), epoxy groups, amino groups, hydroxyl groups, mercapto groups, isocyanate groups, and oxazoline groups. Examples of the vinyl polymerizable compound having the functional group include one or more of vinyl acetate, α,β-unsaturated carboxylic acids such as (meth)acrylic acid, alkyl esters of α,β-unsaturated carboxylic acids such as methyl acrylate, ethyl acrylate, and butyl acrylate, metal salts of α,β-unsaturated carboxylic acids such as ionomers (metals include alkali metals such as sodium, alkaline earth metals such as calcium, and zinc, etc.), glycidyl esters of α,β-unsaturated carboxylic acids such as glycidyl methacrylate, α,β-unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid, and derivatives of the α,β-unsaturated dicarboxylic acids (monoesters, diesters, and acid anhydrides). The above-mentioned thermoplastic elastomers may be used alone or in combination of two or more.
[0071] <Inorganic filler (D)> The PAS resin composition according to the present embodiment may further contain an inorganic filler (D) as an optional component. By further containing the inorganic filler (D), the mechanical strength, thermal conductivity, and the like of the PAS resin composition can be further improved.
[0072] Here, as the inorganic filler (D), a known and commonly used material can be used as long as it does not impair the effect of the present invention, and examples thereof include fillers of various shapes such as granular, plate-like, and fibrous ones. For example, fibrous fillers such as glass fiber, carbon fiber, silane glass fiber, ceramic fiber, aramid fiber, metal fiber, potassium titanate, silicon carbide, calcium silicate, wollastonite, and natural fibers can be used, and non-fibrous fillers such as glass beads, glass flakes, barium sulfate, clay, pyrophyllite, bentonite, sericite, mica, talc, attapulgite, ferrite, calcium silicate, calcium carbonate, magnesium carbonate, zeolite, milled fiber, and calcium sulfate can be used. In addition, these other fillers can be surface-treated, and if necessary, epoxy compounds, isocyanate compounds, silane compounds, titanate compounds, borane treatment, ceramic coating, etc. can be applied.
[0073] The amount of the inorganic filler (D) is not particularly limited, but from the viewpoint of better mechanical properties and dimensional stability, it is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more relative to 100 parts by mass of the PAS (A). Also, from the viewpoint of obtaining better flowability and processability of the resin composition and smoothness of the surface of the molded product, it is more preferably 350 parts by mass or less, even more preferably 300 parts by mass or less, and particularly preferably 250 parts by mass or less relative to 100 parts by mass of the PAS (A).
[0074] The content of the inorganic filler (D) in the PAS resin composition according to the present embodiment is not particularly limited, but from the viewpoint of excellent mechanical strength of the resin composition, for example, it is preferably 20 parts by mass or more, more preferably 25 parts by mass or more, and even more preferably 30 parts by mass or more, relative to 100 parts by mass of the total amount of the PAS (A) and the inorganic filler (D), because within such a range, the isothermal crystallization time becomes short and good moldability is exhibited.
[0075] (Silane coupling agent) If necessary, a silane coupling agent can be blended as an optional component in the PAS resin composition according to this embodiment for the purpose of improving mechanical properties.
[0076] Here, the silane coupling agent having the functional group is not particularly limited as long as it does not impair the effects of the present invention, but preferred examples include silane coupling agents having a functional group that reacts with a carboxy group, such as an epoxy group, an isocyanato group, an amino group, or a hydroxyl group. Examples of such silane coupling agents include epoxy group-containing alkoxysilane compounds such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; isocyanato group-containing alkoxysilane compounds such as γ-isocyanatopropyltrimethoxysilane, γ-isocyanatopropyltriethoxysilane, γ-isocyanatopropylmethyldimethoxysilane, γ-isocyanatopropylmethyldiethoxysilane, γ-isocyanatopropylethyldimethoxysilane, γ-isocyanatopropylethyldiethoxysilane, and γ-isocyanatopropyltrichlorosilane; amino group-containing alkoxysilane compounds such as γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, and γ-aminopropyltrimethoxysilane; and hydroxyl group-containing alkoxysilane compounds such as γ-hydroxypropyltrimethoxysilane and γ-hydroxypropyltriethoxysilane.
[0077] In addition, the content of the silane coupling agent having the functional group in the PAS resin composition of the present invention is not particularly limited, but from the viewpoint of obtaining better moist heat resistance and mechanical strength, it is preferably 0.3 parts by mass or more per 100 parts by mass of the PAS resin, more preferably 0.4 parts by mass or more, and even more preferably 0.5 parts by mass or more.
[0078] Furthermore, in addition to the above components, the PAS resin composition according to the present embodiment may further contain synthetic resins such as polyester resin, polyamide resin, polyimide resin, polyetherimide resin, polycarbonate resin, polyphenylene ether resin, polysulfone resin, polyethersulfone resin, polyetheretherketone resin, polyetherketone resin, polyarylate resin, polyethylene resin, polypropylene resin, polyethylenetetrafluoroethylene resin, polyethylenedifluoroethylene resin, polystyrene resin, ABS resin, epoxy resin, phenol resin, urethane resin, and liquid crystal polymer as optional components depending on the application. In the present disclosure, the synthetic resin is not an essential component, but when it is added, the ratio of the synthetic resin is not particularly limited as long as it does not impair the effects of the present invention, and it differs depending on each purpose and cannot be generally defined, but the ratio of the synthetic resin to be added in the resin composition according to the present disclosure is, for example, in the range of 5 parts by mass or more and 15 parts by mass or less relative to 100 parts by mass of PAS (A). In other words, the ratio of the PAS to the total of the PAS (A) and the synthetic resin is preferably in the range of (100 / 115) or more, and more preferably in the range of (100 / 105) or more, on a mass basis.
[0079] In addition, the PAS resin composition according to the present embodiment may contain other known and commonly used additives as optional components, such as colorants, antistatic agents, antioxidants, heat stabilizers, UV stabilizers, UV absorbers, foaming agents, flame retardants, flame retardant assistants, rust inhibitors, and release agents (metal salts or esters of fatty acids having 18 to 30 carbon atoms, including stearic acid or montanic acid, polyolefin waxes such as polyethylene, etc.) as needed. These additives are not essential components, and may be used in an amount of, for example, preferably 0.01 parts by mass or more, and preferably 1000 parts by mass or less, more preferably 100 parts by mass or less, based on 100 parts by mass of PAS (A), as appropriate for the purpose or use so as not to impair the effects of the present invention.
[0080] The PAS resin composition of the present disclosure has a morphology in which PAS (A) forms a continuous phase and other essential and optional components are dispersed. After the melt-kneading, the PAS resin composition according to the present disclosure is preferably processed into pellets, chips, granules, powder, or other forms by a known method, for example, by extruding the molten resin composition into a strand shape, and then pre-dried at a temperature range of 100 to 150°C as necessary.
[0081] The PAS resin composition according to the present embodiment has a viscosity change rate in the range of ±20%. That is, when the melt viscosity (V6) of the PAS (A) is set to 1, the melt viscosity (V6) of the PAS resin composition is in the range of 0.8 to 1.2. When the viscosity change rate is in this range, the viscosity change rate due to the addition of the PAS oligomer (B) is small, so that the resulting resin composition has excellent processability. In order to adjust the viscosity change rate to this range, the blending amount of the PAS oligomer (B) may be set to a range of 20 parts by mass or less relative to 100 parts by mass of the PAS (A). The viscosity change rate in the present disclosure is calculated from the following formula using the melt viscosity (V6) measured using a flow tester at a temperature of 300°C, a load of 1.96 MPa, and an orifice with a ratio of the orifice length to the orifice diameter of 10 / 1, after holding for 6 minutes. Viscosity change rate (%)=(melt viscosity of the PAS (A) (Pa s)−melt viscosity of the PAS resin composition (Pa s)) / melt viscosity of the PAS (A) (Pa s)×100
[0082] <Molded products and manufacturing methods for molded products> The molded article according to this embodiment is produced by melt molding the PAS resin composition. The manufacturing method of the molded article according to this embodiment includes a step of melt molding the PAS resin composition obtained by the manufacturing method described above. Therefore, the molded article according to this embodiment has a morphology in which the PAS (A) forms a continuous phase and other essential components and optional components are dispersed. The PAS resin composition having such a morphology allows the production of a molded article having excellent mechanical strength.
[0083] The PAS resin composition according to the present embodiment can be subjected to various molding processes such as injection molding, compression molding, extrusion molding of composites, sheets, pipes, pultrusion molding, blow molding, and transfer molding, but is particularly suitable for injection molding because of its excellent releasability. When molding by injection molding, various molding conditions are not particularly limited, and molding can be performed by a normal general method. For example, in an injection molding machine, the PAS resin composition is melted at a resin temperature in a temperature range of the melting point of the PAS resin (A) or higher, preferably in a temperature range of the melting point +10°C or higher, more preferably in a temperature range of the melting point +10°C to the melting point +100°C, and even more preferably in a temperature range of the melting point +20 to the melting point +50°C, and then the resin is injected into a mold from a resin discharge port and molded. At that time, the mold temperature may also be set to a known temperature range, for example, room temperature (23°C) to 300°C, preferably 130 to 190°C.
[0084] The method for producing a molded article according to this embodiment may include a step of annealing the molded article. The optimum conditions for the annealing treatment are selected depending on the application or shape of the molded article, and the annealing temperature is in a temperature range of the glass transition temperature of PAS(A) or higher, preferably in a temperature range of the glass transition temperature +10°C or higher, and more preferably in a temperature range of the glass transition temperature +30°C or higher. On the other hand, it is preferably in a range of 260°C or lower, and more preferably in a range of 240°C or lower. The annealing time is not particularly limited, but is preferably in a range of 0.5 hours or higher, and more preferably in a range of 1 hour or higher. On the other hand, it is preferably in a range of 10 hours or lower, and more preferably in a range of 8 hours or lower. In such a range, not only the distortion of the molded article obtained is reduced and the crystallinity of the resin is improved, but also the thermal conductivity, mechanical properties, and fuel barrier properties are further improved, which is preferable. The annealing treatment may be performed in air, but is preferably performed in an inert gas such as nitrogen gas.
[0085] The molded article according to the present embodiment includes a remolded article obtained by reusing a molded article obtained by melt-molding the PAS resin composition. Specifically, for example, the molded article includes a sprue or runner generated during the manufacture of a molded article, a molded article recovered as a non-standard molded article, or a molded article once used as a product, which is washed as necessary, crushed, and melt-molded again at a temperature equal to or higher than the melting point of PAS. When reusing, it is preferable from the viewpoint of mechanical properties to mix the crushed molded article with the PAS resin composition. The size of the molded article when crushed is not particularly limited, but from the viewpoint of mixability and processability, it is preferable that the size is about the same as that of the PAS resin composition to be mixed. In addition, the mixing ratio is preferably 50 parts by mass or less of the crushed molded article relative to 100 parts by mass of the PAS resin composition, more preferably 40 parts by mass or less, and even more preferably 20 parts by mass or less. In such a range, the recyclability can be improved without impairing the effect exhibited by the PAS resin composition of the present disclosure.
[0086] The PAS resin molded product according to this embodiment is characterized by an excellent balance between crystallization speed and melt viscosity, and is therefore suitable for application to parts having thin-walled parts and small precision parts. The molded product according to this embodiment can be not only the above-mentioned, but also the following ordinary resin molded products. For example, protective and supporting members for box-shaped electric and electronic component integrated modules, multiple individual semiconductors or modules, sensors, LED lamps, resistors, relay cases, connectors, sockets, switches, coil bobbins, capacitors, variable capacitor cases, optical pickups, oscillators, various terminal boards, transformers, plugs, printed circuit boards, tuners, speakers, microphones, headphones, small motors, magnetic head bases, power modules, terminal blocks, semiconductors, liquid crystal displays, FDD carriages, FDD chassis, motor brush holders, parabolic antennas, computer-related parts, and other typical electric and electronic parts; VTR parts, television parts, irons, headsets, etc. Home and office electrical appliance parts such as air dryers, rice cooker parts, microwave oven parts, audio parts, audio / visual equipment parts such as laser discs, compact discs, DVD discs, and Blu-ray discs, lighting parts, refrigerator parts, air conditioner parts, typewriter parts, word processor parts, and water-related equipment parts such as water heaters, bath water volume and temperature sensors; office computer related parts, telephone related parts, facsimile related parts, copier related parts, cleaning jigs, motor parts, lighters, typewriters, and other machine related parts; optical equipment and precision machinery related parts such as microscopes, binoculars, cameras, and watches;Alternator terminals, alternator connectors, brush holders, slip rings, IC regulators, potentiometer bases for light dimmers, relay blocks, inhibitor switches, various valves such as exhaust gas valves, various pipes for fuel, exhaust and intake systems, air intake nozzle snorkels, intake manifolds, engine coolant joints, carburetor main bodies, carburetor spacers, exhaust gas sensors, coolant sensors, oil temperature sensors, brake pad wear sensors, throttle position sensors, crankshaft position sensors, temperature sensors, air flow meters, brake pad wear sensors, thermostat bases for air conditioners, heating hot air flow control valves, radiators Examples of automotive and vehicle related parts include brush holders for motors, water pump impellers, turbine vanes, wiper motor related parts, distributors, starter switches, ignition coils and bobbins, motor insulators, motor rotors, motor cores, starter relays, transmission wire harnesses, windshield washer nozzles, air conditioner panel switch boards, coils for fuel-related electromagnetic valves, fuse connectors, horn terminals, electrical component insulating plates, step motor rotors, lamp sockets, lamp reflectors, lamp housings, brake pistons, solenoid bobbins, engine oil filters, ignition device cases, and other various applications. EXAMPLES
[0087] The present invention will be specifically described below with reference to examples. These examples are illustrative and not limiting. In the following, unless otherwise specified, "%" and "parts" are based on mass.
[0088] <Reference Examples 1 to 3, Examples 1 to 11, and Comparative Examples 1 to 6> Each material was mixed according to the composition and mixing amounts shown in Tables 1 and 2. Then, these mixed materials were fed into a vented twin-screw extruder "TEX-30α (product name)" manufactured by Japan Steel Works, Ltd., and melt-kneaded at a resin component discharge rate of 30 kg / hr, a screw rotation speed of 200 rpm, and a set resin temperature of 320°C to obtain pellets of the resin composition. The glass fiber was fed from a side feeder (S / T ratio 0.5), and the other materials were mixed uniformly in a tumbler in advance and fed from the top feeder. The pellets of the obtained resin composition were dried in a gear oven at 140°C for 2 hours, and then injection molded to prepare various test pieces, and the following tests were performed.
[0089] <Evaluation>
[0090] (1) Measurement of recrystallization temperature (Tmc) The resin compositions obtained in each of the Examples and Comparative Examples were melted at 350°C and then rapidly cooled to prepare amorphous films. Approximately 4 mg of the film was taken and measured using a differential scanning calorimeter (Perkin Elmer's DSC8500). The results are shown in Tables 1 to 4.
[0091] (2) Measurement of melt viscosity (V6) The melt viscosity (V6) of each PAS and PAS resin composition was measured using a Shimadzu flow tester "CFT-500D" at 300°C and a load of 1.96×10 6 The melt viscosity (V6) (Pa·s) after holding for 6 minutes was measured at 10 Pa and L / D = 10 (mm) / 1 (mm). The melt viscosity (V6) of the PAS resin composition relative to the melt viscosity (V6) of the PAS was calculated as the viscosity change rate from the following formula. The results are shown in Tables 1 to 4. Viscosity change rate (%) = (melt viscosity of PAS (Pa s) - melt viscosity of PAS resin composition (Pa s)) / melt viscosity of PAS (Pa s) × 100
[0092] [Table 1]
[0093] [Table 2]
[0094] [Table 3]
[0095] [Table 4]
[0096] The blending ratios of the blended components in Tables 1 to 4 are as follows. · PAS(A) A-1: PPS with a linear structure A-2: Para-meta copolymer PPS a-3: PPS with cross-linked structure
[0097] PAS Oligomer (B) X: PAS oligomer with chain structure Y: PAS oligomer with a cyclic structure
[0098] Thermoplastic elastomer (C) C-1: Engage 8842 manufactured by Dow Chemical Company
[0099] Inorganic filler (D) D-1: Glass fiber, "T-717H" manufactured by Nippon Electric Glass Co., Ltd.
[0100] ·Silane coupling agent (E) E-1: Trimethoxyepoxysilane "KBM-403" manufactured by Shin-Etsu Chemical Co., Ltd.
[0101] <Production Example 1> Production of PAS (A-1) [Process 1] A 150L autoclave with an agitator connected to a pressure gauge, a thermometer, a condenser, a decanter, and a rectification column was charged with 33.075 parts by mass (225 mol parts) of p-dichlorobenzene (hereinafter referred to as p-DCB), 3.420 parts by mass (34.5 mol parts) of NMP, 27.300 parts by mass of 47.23% by mass NaSH aqueous solution (230 mol parts as NaSH), and 18.533 parts by mass of 49.21% by mass NaOH aqueous solution (228 mol parts as NaOH), and the mixture was heated to 173°C over 5 hours under a nitrogen atmosphere while stirring, and 27.300 parts by mass of water were distilled out, after which the autoclave was sealed. The p-DCB distilled by azeotropy during dehydration was separated in a decanter and returned to the autoclave as needed. After completion of dehydration, the autoclave was in a state in which the fine particles of anhydrous sodium sulfide composition were dispersed in the p-DCB. The NMP content in this composition was 0.079 parts by mass (0.8 parts by mole), which indicated that 98 mol% (33.7 parts by mole) of the charged NMP was hydrolyzed to the sodium salt of NMP ring-opening (4-(methylamino)butyric acid) (hereinafter abbreviated as "SMAB"). The amount of SMAB in the autoclave was 0.147 parts by mole per mole of sulfur atom present in the autoclave. Since the theoretical amount of dehydration when the charged NaSH and NaOH are all converted to anhydrous Na2S is 27.921 parts by mass, it was shown that of the remaining water amount of 0.878 parts by mass (48.8 parts by mole) in the autoclave, 0.609 parts by mass (33.8 parts by mole) was consumed in the hydrolysis reaction of NMP and NaOH and was not present in the autoclave as water, and the remaining 0.269 parts by mass (14.9 parts by mole) remained in the autoclave in the form of water or crystal water. The amount of water in the autoclave was 0.065 mole per mole of sulfur atom present in the autoclave.
[0102] [Process 2] After the dehydration step, the inside temperature was cooled to 160°C, 46.343 parts by mass (467.5 parts by mole) of NMP was charged, and the temperature was raised to 185°C. The amount of water in the autoclave was 0.025 moles per mole of NMP charged in step 2. When the gauge pressure reached 0.00 MPa, the valve connected to the distillation tower was opened, and the inside temperature was raised to 200°C over one hour. At this time, the cooling and valve opening were controlled so that the outlet temperature of the distillation tower was 110°C or less. The mixed vapor of p-DCB and water distilled was condensed in a condenser and separated in a decanter, and p-DCB was returned to the autoclave. The amount of distilled water was 0.228 parts by mass (12.7 parts by mole).
[0103] [Process 3] The amount of water in the autoclave at the start of step 3 was 0.041 parts by mass (2.3 mol parts), 0.005 mol per mol of NMP charged in step 2, and 0.010 mol per mol of sulfur atoms present in the autoclave. The amount of SMAB in the autoclave was 0.147 mol per mol of sulfur atoms present in the autoclave, the same as in step 1. Next, the internal temperature was raised from 200°C to 230°C over 3 hours, stirred at 230°C for 1 hour, and then heated to 250°C and stirred for 1 hour. The gauge pressure at the internal temperature of 200°C was 0.03 MPa, and the final gauge pressure was 0.40 MPa. After cooling, 0.650 parts by mass of the obtained slurry was poured into 3 parts by mass (3 L parts) of water and stirred at 80°C for 1 hour, and then filtered. This cake was again stirred with 3 parts by mass (3 L parts) of warm water for 1 hour, washed, and then filtered. This operation was repeated four times. 3 parts by mass (3 L parts) of warm water and acetic acid were added to this cake again, and the pH was adjusted to 4.0, then the cake was stirred for 1 hour, washed, and filtered. This cake was again stirred with 3 parts by mass (3 L parts) of warm water for 1 hour, washed, and filtered. This operation was repeated two times. The cake was dried overnight at 120°C using a hot air dryer to obtain a white powdery PPS resin (A-1). The melt viscosity (V6) of this PPS resin (A-1) was 150 Pa s.
[0104] <Production Example 2> Production of PAS (A-2) In a 150 L autoclave, 19.222 kg of flaky Na2S (60.9% by mass) and 45.0 kg of N-methyl-2-pyrrolidone (hereinafter, NMP) were charged. The temperature was raised to 204°C while stirring under a nitrogen stream, and 4.438 kg of water was distilled off (the remaining water content was 1.14 moles per mole of Na2S). The autoclave was then sealed and cooled to 180°C, and 22.998 kg of p-dichlorobenzene (hereinafter, p-DCB), 2.555 kg of m-dichlorobenzene (hereinafter, m-DCB) (10 mole% relative to the total of m-DCB and p-DCB), and 18.0 kg of NMP were charged. At a liquid temperature of 150°C, nitrogen gas was used to increase the temperature by 1 kg / cm. 2 The mixture was pressurized to 3.5 G and the temperature increase started. While stirring for 3 hours at a liquid temperature of 220°C, a coolant at 80°C was passed through the coil wound around the outside of the upper part of the autoclave to cool it. The temperature was then increased and the mixture was stirred for 3 hours at a liquid temperature of 260°C, after which the temperature was decreased and the cooling of the upper part of the autoclave was stopped. During cooling of the upper part of the autoclave, the liquid temperature was kept constant so as not to decrease. The maximum pressure during the reaction was 8.91 kg / cm 2 It was G. The obtained slurry was filtered and washed twice with warm water in a conventional manner to obtain a filter cake containing about 50% by mass of water. Next, 60 kg of water and 100 g of acetic acid were added to the filter cake to reslurry it, and the mixture was stirred at 50°C for 30 minutes and filtered again. At this time, the pH of the slurry was 4.6. The filter cake thus obtained was added with 60 kg of water, stirred for 30 minutes, and filtered again. This operation was repeated five times. The filter cake thus obtained was then dried in a hot air circulation dryer at 120°C for 4.5 hours to obtain a white powdery para-PPS copolymer. The obtained para-PPS copolymer had a melt viscosity (V6) of 45 Pa·s.
[0105] <Production Example 3> Production of PAS (a-3) The PPS resin (A-1) obtained in Production Example 1 was heat-treated in a hot air dryer at 260°C for 8.0 hours to obtain a crosslinked PPS resin (a-3). The melt viscosity (V6) of this PPS resin (a-3) was 220 Pa s.
[0106] <Production Example 4> Production of PAS oligomer (B-1) -Process (1) 19.413 kg (150 mol) of flake sodium sulfide (60.3 wt% Na2S) and 45.0 kg (454 mol) of NMP were charged into a 150 L autoclave equipped with a stirring blade and a bottom valve connected to a pressure gauge, a thermometer, and a condenser. The temperature was raised to 209°C while stirring under a nitrogen stream, and 4.644 kg of water was distilled off (the remaining water content was 1.13 mol per mol of sodium sulfide). The autoclave was then sealed and cooled to 180°C, and 21.631 kg (147 mol) of p-DCB and 18.0 kg (182 mol) of NMP were charged. At a liquid temperature of 150°C, the liquid was pressurized to 0.1 MPa at a gauge pressure using nitrogen gas, and the temperature was raised. The liquid was heated to 240°C over 135 minutes and held for 30 minutes. The liquid temperature was then raised to 250° C. over 40 minutes and maintained at that temperature for 73 minutes to complete the reaction. The autoclave was then cooled.
[0107] -Process (2) At 100°C, the bottom valve of the autoclave was opened, and the reaction slurry was transferred to a 150L plate filter and pressure filtered at 120°C. 48.0kg of NMP was added, and the cake was washed and filtered again under pressure. The weight of the recovered NMP filtrate was 80.0kg.
[0108] -Process (3) Water was added to the obtained NMP filtrate to form a water slurry, after which solid-liquid separation and water washing were repeated twice, and then the mixture was dried in a hot air dryer at 120°C for 4 hours to obtain a powder.
[0109] -Process (4) Chloroform was added to the obtained powder, and the mixture was stirred at 65° C. for 1 hour and then filtered.
[0110] -Process (5) The residue after filtration was vacuum dried at 40° C. for 4 hours to obtain 392 g of a linear PAS oligomer (B-1).
[0111] <Production Example 5> Production of PAS oligomer (b-2) Up to the step (4), the same operations as in Production Example 1 were carried out. The filtrate was evaporated at 150 Torr and 40° C. to remove chloroform, and 764 g of a cyclic PAS oligomer (B-2) was obtained.
[0112] A comparison of Reference Example 1, Examples 1 and 2, and Comparative Example 1 in Table 1 shows that when a specific amount of a PAS oligomer having a chain structure is blended, a resin composition having an excellent balance between crystallization rate and melt viscosity can be obtained. This effect is also shown in a comparison of Reference Example 2 and Example 3. Reference Example 3 and Comparative Example 2 show that when a crosslinked PAS is used, the viscosity changes significantly even when the blending amount of PAS oligomer (B) is within a specific range. Comparing Examples 4 to 10 with Comparative Examples 3 to 5 from Tables 2 and 3, it was shown that the resin compositions of the Examples were excellent in the balance between the crystallization rate and the melt viscosity. Table 4 shows that the effect is also exhibited when a thermoplastic elastomer and an inorganic filler are blended as optional components.
Claims
1. A polyarylene sulfide resin composition comprising a linear polyarylene sulfide (A) and an oligoarylene sulfide (B) as essential components, the mass ratio of the cyclic oligoarylene sulfide (X) to the chain oligoarylene sulfide (Y) in the oligoarylene sulfide (B) is 0:100 to 66:33; The amount of the oligoarylene sulfide (B) is 5.0 parts by mass or less based on 100 parts by mass of the linear polyarylene sulfide (A), and A polyarylene sulfide resin composition having a viscosity change rate in the range of ±20%. (The viscosity change rate is calculated from the melt viscosity (V6) measured after holding the material for 6 minutes at a temperature of 300°C, a load of 1.96 MPa, and an orifice with an orifice length to orifice diameter ratio of 10 / 1 using a flow tester, using the following formula.) Viscosity change rate (%)=(melt viscosity of the polyarylene sulfide (A) (Pa·s)−melt viscosity of the polyarylene sulfide resin composition (Pa·s)) / melt viscosity of the polyarylene sulfide (A) (Pa·s)×100
2. The cyclic oligoarylene sulfide (X) is A step (1) of reacting a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent (1) to obtain a crude reaction mixture containing a polyarylene sulfide (a), an oligoarylene sulfide (b), the organic polar solvent (1), and an alkali metal halide; (2) subjecting the crude reaction mixture to solid-liquid separation to obtain a reaction mixture (L1) containing at least the oligoarylene sulfide (b) and the organic polar solvent (1); A step (3) of subjecting the organic polar solvent (1) to solid-liquid separation from the reaction mixture (L1) to obtain a reaction mixture (S1) containing at least an oligoarylene sulfide (b); A step (4) of contacting the reaction mixture (S1) with an organic polar solvent (2) to obtain a mixture (L2); (5) gradually cooling the mixture (L2) to 25° C. or less and removing the solid phase component to obtain a liquid phase component (L3); and The polyarylene sulfide resin composition according to claim 1, which is produced by a process comprising a step (6) of concentrating the liquid phase component (L3).
3. The chain oligoarylene sulfide (Y) A step (1) of reacting a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent (1) to obtain a crude reaction mixture containing a polyarylene sulfide, an oligoarylene sulfide (b), the organic polar solvent (1), and an alkali metal halide. (2) subjecting the crude reaction mixture to solid-liquid separation to obtain a reaction mixture (L1) containing at least the oligoarylene sulfide (b) and the organic polar solvent (1); A step (3) of obtaining a reaction mixture (S1) containing an oligoarylene sulfide (b) by performing solid-liquid separation of the organic polar solvent (1) from the reaction mixture (L1); A step (4) of contacting the reaction mixture (S1) with an organic polar solvent (2) to obtain a mixture (L2); and The polyarylene sulfide resin composition according to claim 1 or 2, which is produced by a method including a step (7) of subjecting the mixture (L2) to solid-liquid separation in a temperature range of the boiling point of the organic polar solvent (2) minus 10°C or more to recover a solid phase component (S2).
4. The polyarylene sulfide resin composition according to claim 1, further comprising a thermoplastic elastomer.
5. The polyarylene sulfide resin composition according to claim 1 or 2, further comprising an inorganic filler.
6. A molded article obtained by melt molding the polyarylene sulfide resin composition according to claim 1 or 2.
7. A method for producing a polyarylene sulfide resin composition, comprising a step of blending a linear polyarylene sulfide (A) and an oligoarylene sulfide (B) as essential components, and melt-kneading the blended components at a temperature equal to or higher than the melting point of the polyarylene sulfide, the mass ratio of the cyclic oligoarylene sulfide (X) to the chain oligoarylene sulfide (Y) in the oligoarylene sulfide (B) is 0:100 to 66:33; a mixing amount of the oligoarylene sulfide (B) is 5.0 parts by mass or less per 100 parts by mass of the linear polyarylene sulfide (A), and a viscosity change rate is within a range of ±20%. (Note that the viscosity change rate is calculated from the following formula using the melt viscosity (V6) measured after holding for 6 minutes using a flow tester at a temperature of 300° C., a load of 1.96 MPa, and an orifice having an orifice length / orifice diameter ratio of 10 / 1.) Viscosity change rate (%)=(melt viscosity (Pa·s) of the polyarylene sulfide (A)−melt viscosity (Pa·s) of the polyarylene sulfide resin composition) / melt viscosity (Pa·s) of the polyarylene sulfide (A)×100.
8. The cyclic oligoarylene sulfide (X) is A step (1) of reacting a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent (1) to obtain a crude reaction mixture containing a polyarylene sulfide (a), an oligoarylene sulfide (b), the organic polar solvent (1), and an alkali metal halide; (2) subjecting the crude reaction mixture to solid-liquid separation to obtain a reaction mixture (L1) containing at least the oligoarylene sulfide (b) and the organic polar solvent (1); A step (3) of subjecting the organic polar solvent (1) to solid-liquid separation from the reaction mixture (L1) to obtain a reaction mixture (S1) containing at least an oligoarylene sulfide (b); A step (4) of contacting the reaction mixture (S1) with an organic polar solvent (2) to obtain a mixture (L2); (5) gradually cooling the mixture (L2) to 25° C. or less and removing the solid phase component to obtain a liquid phase component (L3); and The method for producing a polyarylene sulfide resin composition according to claim 7, characterized in that the polyarylene sulfide resin composition is produced by a method comprising a step (6) of concentrating the liquid phase component (L3).
9. The chain oligoarylene sulfide (Y) A step (1) of reacting a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent (1) to obtain a crude reaction mixture containing a polyarylene sulfide, an oligoarylene sulfide (b), the organic polar solvent (1), and an alkali metal halide. (2) subjecting the crude reaction mixture to solid-liquid separation to obtain a reaction mixture (L1) containing at least the oligoarylene sulfide (b) and the organic polar solvent (1); A step (3) of obtaining a reaction mixture (S1) containing an oligoarylene sulfide (b) by performing solid-liquid separation of the organic polar solvent (1) from the reaction mixture (L1); A step (4) of contacting the reaction mixture (S1) with an organic polar solvent (2) to obtain a mixture (L2); and The method for producing a polyarylene sulfide resin composition according to claim 7, characterized in that the polyarylene sulfide resin composition is produced by a method including a step (7) of subjecting the mixture (L2) to solid-liquid separation in a temperature range of not less than the boiling point of the organic polar solvent (2) −10° C. to recover a solid phase component (S2).
10. The method for producing a polyarylene sulfide resin composition according to claim 7, further comprising blending a thermoplastic elastomer.
11. The method for producing a polyarylene sulfide resin composition according to claim 7, further comprising blending an inorganic filler.
12. A method for producing a polyarylene sulfide resin molded article, comprising the steps of producing a resin composition according to claim 7 or 8, and melt-molding the resin composition.
Citation Information
Patent Citations
Polyarylene sulfide resin composition
JP2001172500A
Method for producing polyarylene sulfide
JP2011173953A
Method for producing polyarylene sulfide