Integrated type sealing sheet, light-emitting type electron component, and manufacturing method of the light-emitting type electron component

The integrated sealing sheet with controlled curable resin and translucent layers addresses light diffusion and edge whitening issues in mini/micro LED displays by optimizing modulus and transmittance, enhancing display quality and reducing manufacturing complexity.

JP2024158259AActive Publication Date: 2024-11-08SHIN ETSU POLYMER CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023073310
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

Conventional methods for preventing light diffusion between mini/micro LEDs in displays require time-consuming etching processes, lead to increased manufacturing costs, and fail to completely prevent light diffusion, while cutting substrates with integrated sealing sheets causes whitening phenomena due to roughened edges.

Method used

An integrated sealing sheet with a curable resin layer and a translucent layer is applied to mini/micro LED substrates, where the translucent layer faces the light-emitting surface, and the curable resin layer fills gaps between LEDs, using specific modulus and transmittance values to minimize light diffusion and edge whitening.

Benefits of technology

The solution effectively reduces light diffusion and edge whitening, improving display contrast and appearance by using a curable resin layer with controlled properties to fill gaps and smooth edges during substrate cutting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158259000001_ABST
    Figure 2024158259000001_ABST
Patent Text Reader

Abstract

To provide an integrated type sealing sheet that reduces a whitening phenomenon that an edge part of a substrate in which a light-emitting element is arranged is viewed as a white line on a display, a light-emitting type electron component, and a manufacturing method of the light-emitting type electron component.SOLUTION: The present invention provides an integrated type sealing sheet 1 that is crimped to a surface where a plurality of light-emitting elements on a substrate with an element in which a plurality of light-emitting elements 21, 22, and 23 are arranged to a substrate 20 are arranged. A black color hardening resin layer 10 and a transparent hardening resin layer 11 are laminated in this order from an order that it is contacted to each light-emitting element when crimping it to each light-emitting element. A storage elastic modulus in an unhardened state of the transparent hardening resin layer 11 is preferably 1.0×103 Pa or more and is 1.0×107 Pa or less under 100°C, and is more preferably 5.0×103 Pa or more and is 5.0×105 Pa or less.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an integrated encapsulating sheet, a light-emitting electronic component, and a method for manufacturing a light-emitting electronic component. [Background technology]

[0002] In recent years, displays using extremely small light-emitting diodes called mini-LEDs or micro-LEDs have been attracting attention. There are roughly two known methods for using such extremely small light-emitting diodes in displays. One is to arrange a large number of light-emitting diodes on a substrate to form a backlight for liquid crystal, and to locally control the brightness of the backlight. The other is to make light-emitting diodes of each color (red, green, and blue) emit light, sending each color of light to the viewer's eyes on a pixel-by-pixel basis.

[0003] Light-emitting diodes such as mini LEDs or micro LEDs are generally arranged on a substrate. When multiple light-emitting diodes (referred to as light-emitting elements) are arranged on a substrate, it is necessary to prevent light diffusion between adjacent light-emitting elements. As a method for shielding light between multiple light-emitting elements with a resin having a light diffusion prevention function, for example, a method using a dry film is known (see Patent Document 1). The dry film is a film obtained by applying and drying a light-diffusing resin composition on a protective film.

[0004] When the dry film is pressed onto a plurality of light-emitting elements on a substrate, a light-diffusing resin layer is formed not only in the gaps between the light-emitting elements but also on the upper surface (light-emitting surface) of the light-emitting elements. Under such circumstances, the resin layer may block the light from reaching the viewer of the display. To prevent this, the above-mentioned conventional technology employs a method in which the light-emitting surface of the light-emitting element is etched by plasma treatment or the like to remove the resin layer on the light-emitting surface, and the removed surface is covered with a light-transmitting sealant. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2022-22562 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the above-mentioned conventional technology requires a long time for the etching process, which leads to an increase in manufacturing costs. Also, it is difficult to completely remove the resin layer on the light-emitting surface of the light-emitting element, and as a result, it is difficult to completely prevent the diffusion of light that should reach the viewer side of the display. In addition, a step of laminating a highly transparent sealing film is required after the etching process, which increases the number of manufacturing processes.

[0007] In view of the above problems, the present inventors have developed, prior to the present invention, an integrated encapsulating sheet in which a first layer of a highly light-transmitting curable resin and a second layer of a curable resin with excellent light diffusion properties are formed in this order on one side of a film substrate. The integrated encapsulating sheet is pressure-bonded to a light-emitting element so that the second layer side faces the light-emitting surface side of the light-emitting element, and the second layer is disposed in the gaps between the light-emitting elements and the first layer is disposed on the light-emitting surface of the light-emitting element, and these layers are cured, whereby it is possible to reduce light diffusion between the light-emitting elements and realize a structure that does not block light emitted from the light-emitting elements.

[0008] However, it was found that the technology developed prior to the present invention also requires further improvement. That is, when a plurality of substrates on which an integrated encapsulating sheet is pressed from above a light emitting element are prepared and placed on the back side of a display, and then the light emitting element is emitted, the edge of the substrate may shine in a white line shape, and such a whitening phenomenon must be reduced. The substrate with the integrated encapsulating sheet pressed is cut into a predetermined size using a cutting tool such as a rotary blade. The present inventors have found that this cutting roughens the end surface of the film base material constituting the integrated encapsulating sheet, and that this rough end surface is the cause of the whitening phenomenon.

[0009] Based on the above findings, the present invention has an object to reduce the whitening phenomenon in which the edge portion of a substrate on which light-emitting elements are arranged appears as a white line on a display. [Means for solving the problem]

[0010] (1) An integrated encapsulating sheet according to one embodiment for achieving the above object is an integrated encapsulating sheet that is pressure-bonded to a surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, the surface being in contact with the element-mounted substrate, the surface being in contact with the surface of ... A curable resin layer and a semi-transparent layer are laminated in this order in order of contact with the light-emitting element when the light-emitting element is pressure-bonded to the light-emitting element, The storage modulus of the semi-transparent layer at 60° C. is 7×10 8 Pa or more 2×10 10 Pa or less. (2) In the integrated encapsulating sheet according to another embodiment, preferably, the semi-transparent layer has a support made of a resin, and the thickness of the support may be 20 μm or more and 225 μm or less. (3) In the integrated encapsulating sheet according to another embodiment, preferably, the semi-transparent layer may have at least one layer of a coating layer or a hard coat layer. (4) In the integrated encapsulating sheet according to another embodiment, preferably, the support may contain a black pigment or dye. (5) In the integrated encapsulating sheet according to another embodiment, preferably, at least one of the coating layer or the hard coat layer may contain a black pigment or dye. (6) In the integrated encapsulating sheet according to another embodiment, preferably, the total light transmittance of the semitransparent layer may be 40% or more and 90% or less. (7) In the integrated encapsulating sheet according to another embodiment, preferably, the curable resin layer has a storage modulus of 7×10 at 60° C. after heat treatment at 120° C. for 1 hour. 8 Pa or more 2×10 10 It may be less than Pa. (8) In the integrated encapsulating sheet according to another embodiment, preferably, the curable resin layer may have a black curable resin layer and a transparent curable resin layer in the order of contact with the plurality of light emitting elements. (9) In order to achieve the above object, a light-emitting electronic component according to one embodiment comprises: a substrate having a plurality of light emitting elements disposed thereon; an integrated encapsulating cured sheet in a state of being pressure-bonded to a surface of the element-mounted substrate on which the plurality of light-emitting elements are arranged; Equipped with The integrated encapsulating cured sheet has a resin layer and a semi-transparent layer laminated in this order from the side closest to the substrate, The resin layer is filled between the plurality of light emitting elements. (10) A method for producing a light-emitting electronic component according to one embodiment of the present invention for achieving the above object includes the steps of: The integrated encapsulating sheet according to claim 1 or 2 is disposed on a surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, so that the curable resin layer of the integrated encapsulating sheet is in contact with the surface of the element-mounted substrate, The curable resin layer is filled between the plurality of light emitting elements by pressing. This is a method in which the curable resin layer is cured by heating. Effect of the Invention

[0011] According to the present invention, it is possible to reduce the whitening phenomenon in which the edge portion of a substrate on which light-emitting elements are arranged appears as a white line on a display. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 shows a cross-sectional view of an integrated encapsulating sheet according to one embodiment when cut along the thickness direction. [Diagram 2] FIG. 2 shows a cross-sectional view seen in the same manner as FIG. 1 when the integrated encapsulating sheet of FIG. 1 is disposed so that the black curable resin layer thereof is in contact with the top surface of the light emitting element of the element-mounted substrate. [Diagram 3]FIG. 3 shows a cross-sectional view, as seen from FIG. 1, of a state in which the integrated encapsulating sheet has been pressure-bonded to the element-mounted substrate, proceeding from the stage shown in FIG. 2, up to a state in which the black curable resin layer and a part of the transparent curable resin layer shown in FIG. 1 are embedded between the light-emitting elements. [Figure 4] FIG. 4 shows a cross-sectional view, seen from the same angle as FIG. 1, of a light-emitting electronic component manufactured by proceeding further from the stage shown in FIG. 3, peeling off the protective sheet on the hard coat layer, and carrying out a curing treatment. [Diagram 5] FIG. 5 shows a cross-sectional view similar to FIG. 1, but with an end of the light-emitting electronic component of FIG. 4 cut off. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Next, an embodiment of the present invention will be described with reference to the drawings. Note that the embodiment described below does not limit the invention according to the claims, and not all of the elements and combinations described in the embodiment are necessarily essential to the solution of the present invention. In this specification and claims, the main component means a component that accounts for 50% by mass or more of the total solid content of the entire composition. A numerical range represented by "~" means a numerical range with the numbers before and after ~ as the lower and upper limits.

[0014] FIG. 1 shows a cross-sectional view of an integrated encapsulating sheet according to an embodiment when cut along the thickness direction. FIG. 2 shows a cross-sectional view of the integrated encapsulating sheet of FIG. 1 when the black curable resin layer is disposed in contact with the top surface of the light-emitting element of the element-attached substrate, as seen from FIG. 1. FIG. 3 shows a cross-sectional view of the integrated encapsulating sheet of FIG. 1 when the integrated encapsulating sheet is pressed against the element-attached substrate until the black curable resin layer and a part of the transparent curable resin layer of FIG. 1 are embedded between the light-emitting elements, proceeding from the stage of FIG. 2. FIG. 4 shows a cross-sectional view of the light-emitting electronic component of FIG. 1 produced by peeling off the protective sheet on the hard coat layer and performing a curing treatment, proceeding further from the stage of FIG. 3.

[0015] 1. Integrated encapsulating sheet An integrated encapsulating sheet 1 according to one embodiment of the present invention will be described with reference to Figs. 1 and 2.

[0016] As shown in FIG. 1, the integrated encapsulating sheet 1 is a multi-layer sheet that is pressure-bonded to a surface on which a plurality of light-emitting elements are arranged in an element-attached substrate on which a plurality of light-emitting elements are arranged. The integrated encapsulating sheet 1 is laminated in the order of a curable resin layer 5 and a semi-transparent layer 6 in contact with the light-emitting element when pressure-bonded to the light-emitting element. That is, the integrated encapsulating sheet 1 is a sheet in a state in which the curable resin layer 5 and the semi-transparent layer 6 are laminated in the thickness direction. In a state in which the integrated encapsulating sheet 1 is not used, the curable resin layer 5 is an uncured layer. The semi-transparent layer 6 is a cured layer. The "semi-transparent" of the semi-transparent layer 6 means a transparency between completely transparent and completely opaque, and means a property in which the total light transmittance measured in accordance with JIS K 7136 using a haze meter is 30% or more and 95% or less. The integrated encapsulating sheet 1 is preferably a laminate of a black curable resin layer 10, a transparent curable resin layer 11, a support 12, and a hard coat layer 13. The black curable resin layer 10 and the transparent curable resin layer 11 constitute the curable resin layer 5. The support 12 and the hard coat layer 13 constitute the semi-transparent layer 6. The semi-transparent layer 6 may further include a coating layer (not shown) on at least one surface in the thickness direction of the support 12. The coating layer is a layer for adjusting the total light transmittance of the semi-transparent layer 6 to an appropriate value. Note that the semi-transparent layer 6 does not need to include the coating layer and the hard coat layer 13 as long as it includes the resin support 12.

[0017] For ease of handling, the integrated encapsulating sheet 1 may further include a protective film on the outer surface of either one or both of the black curable resin layer 10 and the hard coat layer 13. Fig. 1 shows an example of the integrated encapsulating sheet 1 having protective films 14, 15 on the outer surfaces of both the black curable resin layer 10 and the hard coat layer 13. More specifically, the integrated encapsulating sheet 1 has a structure in which the protective film 15, the black curable resin layer 10, the transparent curable resin layer 11, the support 12, the hard coat layer 13, and the protective film 14 are laminated in this order.

[0018] As shown in FIG. 2, the integrated encapsulating sheet 1 is used to fill spaces between a plurality of light emitting elements 21, 22, and 23 of a substrate 2 with elements in which a plurality of light emitting elements (a light emitting element 21, a light emitting element 22, and a light emitting element 23, typified by an LED) are arranged on a substrate 20. The substrate 2 with elements will be described later in detail. The integrated encapsulating sheet 1 is used such that the black curable resin layer 10 contacts the substrate 2 with elements during pressure bonding, as shown in FIG. 2. The black curable resin layer 10 and the transparent curable resin layer 11 of the integrated encapsulating sheet 1 are in an uncured state until pressure bonding to the substrate 2 with elements is completed. A specific method for obtaining a light emitting electronic component by pressure bonding the integrated encapsulating sheet 1 to the substrate 2 with elements will be described later.

[0019] (1) Black curable resin layer The black curable resin layer 10 is a layer for preventing light diffusion between the light emitting elements 21, 22, 23 and improving the contrast of the display. The black curable resin layer 10 also serves to sufficiently fill the gaps between the multiple light emitting elements 21, 22, 23 arranged on the element-mounted substrate 2 in a pressure bonding process represented by thermocompression bonding, and to prevent poor appearance due to expansion of unfilled gaps in a hardening process represented by thermosetting, and damage to the light emitting elements 21, 22, 23 due to external factors in a later process.

[0020] [Lab value] The black curable resin layer 10 preferably has Lab values ​​in a cured state measured in accordance with JIS Z8722 using a light source of D65, a field of view of 2°, and a transmission method of L: 5 to 60, a: -3 to 7, and b: -20 to 20, and more preferably L: 10 to 50, a: -2 to 5, and b: -15 to 15. When the Lab values ​​in the cured state are within the preferred ranges, light diffusion between the light emitting elements 21, 22, and 23 can be further prevented, and the contrast of the display can be further improved.

[0021] [Total light transmittance] The total light transmittance of the black curable resin layer 10 in a cured state is lower than that of the transparent curable resin layer 11 in a cured state. Specifically, the black curable resin layer 10 is prepared so that the total light transmittance of the black curable resin layer 10 in a cured state is 0 to 50%. The black curable resin layer 10 is preferably prepared so that the total light transmittance of the black curable resin layer 10 in a cured state is 0 to 40%, more preferably 0 to 30%. When the total light transmittance of the black curable resin layer 10 in a cured state is equal to or less than an upper limit value such as 50%, 40%, or 30%, light diffusion between the light emitting elements 21, 22, and 23 can be further prevented. The total light transmittance in this specification can be measured by a haze meter in accordance with JIS K 7136. The total light transmittance of the cured state can be changed mainly by the presence or absence of carbon black or the amount of carbon black. The total light transmittance of the cured state can also be changed by the thickness of the black curable resin layer 10 and the type of resin composition.

[0022] [Storage modulus] The storage modulus of the black curable resin layer 10 in an uncured state is preferably smaller than the storage modulus of the transparent curable resin layer 11 in an uncured state. The storage modulus of the black curable resin layer 10 in an uncured state is preferably 1.0×10 5 Pa or less, and 1.0×10 2 Pa or more 1.0×10 5 Pa or less, and more preferably 1.0×10 3 Pa or more 5.0×10 4 It is even more preferable that the storage modulus at 100°C is equal to or less than 100 Pa. In an uncured state, the black curable resin layer 10 has a storage modulus at 100°C equal to or less than the preferred upper limit, so that sufficient fluidity is obtained when the layer is pressure-bonded to the element-mounted substrate 2, and the layers can be sufficiently filled between the light-emitting elements 21, 22, and 23 by following the unevenness of the element-mounted substrate 2 due to the light-emitting elements 21, 22, and 23. In an uncured state, the black curable resin layer 10 has a storage modulus at 100°C equal to or more than the preferred lower limit, so that pressure bias during thermocompression can be prevented, and a uniform appearance can be maintained. In addition, the resin can be prevented from flowing out of the range, and the film thickness after pressure bonding can be ensured.

[0023] The storage modulus of the black curable resin layer 10 at 60° C. after heat treatment at 120° C. for 1 hour is preferably 7×10 8 Pa or more 2×10 10 Pa or less. Since the storage modulus of the black curable resin layer 10 at 60°C after heat treatment at 120°C x 1 hour is equal to or less than the preferred upper limit, it is possible to prevent cracks from occurring in the cured black curable resin layer 10 when cutting the edge of the substrate 20. Furthermore, since the storage modulus of the black curable resin layer 10 at 60°C after heat treatment at 120°C x 1 hour is equal to or more than the preferred lower limit, it is possible to prevent the cured black curable resin layer 10 from deforming and expanding and contracting when cutting the edge of the substrate 20, and to prevent the integrated encapsulating sheet 1 on the edge side of the substrate 20 from becoming wavy.

[0024] [Curable resin composition] The black curable resin layer 10 includes a curable resin composition. An example of the curable resin composition is a curable resin composition containing at least one resin selected from an epoxy resin, an acrylic resin, a polyester resin, and a polyurethane resin, and a curing agent. Among the above curable resin compositions, an epoxy resin composition that can achieve curing at low temperatures and has excellent heat resistance and reliability is preferred. In this specification, the epoxy resin composition is a composition containing an epoxy resin as a main component, or a composition containing an epoxy resin and a curing agent as main components.

[0025] When the black curable resin layer 10 is made of an epoxy resin composition, it may contain a curing agent for epoxy resin other than the modified elastomer having a functional group capable of reacting with an epoxy group. Examples of the other curing agent include known curing agents such as phenol-based curing agents, acid anhydride-based curing agents, and amine-based curing agents. Two or more types of the other curing agents may be used in combination.

[0026] (Epoxy resin) In the present application, an epoxy resin is a compound having an epoxy group in the molecule. The epoxy resin used in the present invention is preferably one having two or more epoxy groups in one molecule. This is because a crosslinked structure is formed by reaction with a modified resin having a functional group capable of reacting with an epoxy group, and the cured product can exhibit high heat resistance. In addition, when an epoxy resin having two or more epoxy groups is used, the degree of crosslinking with a curing agent having a functional group capable of reacting with an epoxy group is sufficient, and sufficient heat resistance can be obtained in the cured product.

[0027] Examples of epoxy resins include bifunctional epoxy resins having two epoxy groups in a molecule, polyfunctional epoxy resins having three or more epoxy groups in a molecule, and high molecular weight epoxy resins having a weight average molecular weight of 10,000 or more. They may also be hydrogenated epoxy resins. In this application, high molecular weight epoxy resins are not classified as bifunctional epoxy resins or polyfunctional epoxy resins, but as phenoxy-type epoxy resins, regardless of the number of epoxy groups in the molecule. The weight average molecular weight of an epoxy resin is a polystyrene-equivalent molecular weight measured by gel permeation chromatography.

[0028] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, phenoxy type epoxy resins obtained by polymerizing these resins, and hydrogenated versions of these resins; glycidyl ester-based epoxy resins such as diglycidyl phthalate, diglycidyl isophthalate, diglycidyl terephthalate, glycidyl p-hydroxybenzoate, diglycidyl tetrahydrophthalate, diglycidyl succinate, diglycidyl adipic acid, diglycidyl sebacate, and triglycidyl trimellitate; ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, Examples of the epoxy resins include, but are not limited to, glycidyl ether-based epoxy resins such as 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, pentaerythritol tetraglycidyl ether, tetraphenylglycidyl ether ethane, triphenylglycidyl ether ethane, polyglycidyl ether of sorbitol, and polyglycidyl ether of polyglycerol; glycidylamine-based epoxy resins such as triglycidyl isocyanurate and tetraglycidyl diaminodiphenylmethane; and linear aliphatic epoxy resins such as epoxidized polybutadiene and epoxidized soybean oil. In addition, novolac-type epoxy resins such as xylene structure-containing novolac epoxy resins, naphthol novolac-type epoxy resins, phenol novolac epoxy resins, o-cresol novolac epoxy resins, and bisphenol A novolac epoxy resins can also be used.

[0029] Examples of epoxy resins that can be used include brominated bisphenol A type epoxy resins, phosphorus-containing epoxy resins, fluorine-containing epoxy resins, dicyclopentadiene skeleton-containing epoxy resins, naphthalene skeleton-containing epoxy resins, anthracene type epoxy resins, tertiary butyl catechol type epoxy resins, triphenylmethane type epoxy resins, tetraphenylethane type epoxy resins, biphenyl type epoxy resins, and bisphenol S type epoxy resins.

[0030] Examples of high molecular weight epoxy resins that can be used include phenoxy type epoxy resins, epoxy modified polybutadiene, copolymers of glycidyl methacrylate and methyl methacrylate, modified polymers obtained by epoxy modifying other resins, etc. These epoxy resins may be used alone or in combination of two or more.

[0031] Among the above epoxy resins, the epoxy resin used in the black curable resin layer 10 is preferably a multifunctional epoxy resin from the viewpoint of increasing the crosslink density after curing. Among the multifunctional epoxy resins, novolac-type epoxy resins are particularly preferred because they are epoxy resins that can be appropriately introduced with a flexible skeleton and can adjust the flexibility and softening point, making the cured product less susceptible to brittle fracture, improving the stability of performance over long-term use of the cured product of the epoxy resin composition, increasing the crosslink density, and improving heat resistance.

[0032] Specific examples of novolac-type epoxy resins include "YX7700" manufactured by Mitsubishi Chemical Corporation, "NC7000L", "XD1000", and "EOCN-1020" manufactured by Nippon Kayaku Co., Ltd., "ESN485" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "N-690", "N-695", and "HP-7200H" manufactured by DIC Corporation.

[0033] The blending amount of the polyfunctional epoxy resin in the black curable resin layer 10 is preferably 10 to 99% by mass, more preferably 40 to 95% by mass, and even more preferably 60 to 90% by mass, based on 100% by mass of the total resin solid content of the black curable resin layer 10. When the blending amount is equal to or greater than the lower limit, the crosslinking density can be increased to provide chemical resistance and heat resistance. When the blending amount is equal to or less than the upper limit, the storage modulus during thermocompression bonding can be adjusted, and the fluidity of the black curable resin layer 10 can be ensured.

[0034] The black curable resin layer 10 does not contain a high molecular weight epoxy resin, or if it contains a high molecular weight epoxy resin, it preferably contains it in an amount less than that of the transparent curable resin layer 11. This makes it easier to ensure sufficient fluidity during thermocompression bonding. The amount of high molecular weight epoxy resin in the black curable resin layer 10 is preferably less than 50% by mass, more preferably less than 30% by mass, and even more preferably less than 10% by mass, relative to 100% by mass of the total resin solid content of the black curable resin layer 10.

[0035] From the viewpoint of ensuring sufficient fluidity during thermocompression bonding, the black curable resin layer 10 preferably contains an epoxy resin having a softening point or melting point of 100° C. or less. From the viewpoint of handleability and heat resistance of the cured product, it is more preferable that the black curable resin layer 10 contains an epoxy resin having a softening point or melting point of 40 to 95° C. By containing an epoxy resin having a softening point or melting point within the above range, it becomes possible to control the storage modulus.

[0036] The total amount of epoxy resin in the black curable resin layer 10 is preferably 10 to 100% by mass, more preferably 20 to 99% by mass, and even more preferably 35 to 95% by mass, based on 100% by mass of the total resin solid content of the black curable resin layer 10. Within the above range, the storage modulus can be controlled, and appropriate fluidity during thermocompression bonding can be ensured. Furthermore, if it is equal to or greater than the above lower limit, heat resistance after curing can be improved.

[0037] (Elastomer) The black curable resin layer 10 preferably contains an elastomer in addition to a resin such as an epoxy resin, etc. By containing an elastomer, it becomes easier to control the storage modulus, that is, the fluidity.

[0038] As the elastomer, a thermosetting elastomer, generally called "rubber", is preferred because it provides excellent heat resistance. Examples of thermosetting elastomers include acrylonitrile butadiene rubber (NBR), which is a random copolymer of butadiene and acrylonitrile, acrylic rubber, styrene butadiene rubber, vinyl acetate resin, silicone resin, etc. Among them, NBR is preferred because it has good compatibility with epoxy resins, allows control of the fluidity of the black curable resin layer 10 at around 100°C, and has good adhesion to the transparent curable resin layer 11 and the element-mounted substrate 2.

[0039] The weight average molecular weight of the elastomer is preferably 100,000 to 1,000,000, more preferably 120,000 to 500,000, and further preferably 150,000 to 300,000. When the weight average molecular weight of the elastomer is within the above range, the storage modulus of the black curable resin layer 10 can be controlled, and the flowability during thermocompression bonding can be ensured. When the weight average molecular weight of the elastomer is equal to or less than the above upper limit, the compatibility with the epoxy resin is improved, and the flowability during thermal curing can be more effectively controlled.

[0040] In particular, when the black curable resin layer 10 is composed of an epoxy resin composition, it is preferable to include a modified elastomer having a functional group capable of reacting with an epoxy group. A modified elastomer having a functional group capable of reacting with an epoxy group also acts as a curing agent for the epoxy resin. In addition, since it can react and bond with the epoxy resin, the heat resistance and reliability against thermal shock are improved. Furthermore, the difference in polarity between the functional group capable of reacting with the epoxy resin and the resin skeleton has a favorable effect on dispersibility, and good dispersibility can be obtained when carbon black is contained in the black curable resin layer 10.

[0041] Examples of functional groups capable of reacting with an epoxy group include acid groups such as a carboxy group, a sulfo group, a nitro group, and a phosphoric acid group, as well as their acid anhydride groups, a hydroxyl group, and an amino group. Among these, an acid group or an acid anhydride group is preferred, and a carboxy group or a carboxylic acid anhydride group is particularly preferred, since they can be cured at low temperatures and can ensure a long pot life.

[0042] That is, when the black curable resin layer 10 is composed of an epoxy resin composition, it preferably contains an acid-modified elastomer having an acid group or an acid anhydride group, more preferably contains an acid-modified elastomer having a carboxy group, and particularly preferably contains modified NBR having a carboxy group.

[0043] The modified NBR having a carboxy group is preferably a carboxylated acrylonitrile rubber into which acrylic acid, methacrylic acid, maleic anhydride, etc. are introduced. Commercially available products of the carboxylated acrylonitrile rubber include Nipol (registered trademark) NX775 and Nipol 1072CGJ manufactured by Zeon Corporation. Two or more types of modified elastomers having a functional group capable of reacting with an epoxy group may be used in combination.

[0044] The amount of elastomer in the black curable resin layer 10 is preferably greater than the amount of elastomer in the transparent curable resin layer 11. This allows the storage modulus of the black curable resin layer 10 during thermocompression bonding to be adjusted to an appropriate range lower than that of the transparent curable resin layer 11, and allows flow during thermal curing to be suppressed, when the black curable resin layer 10 contains a large amount of low molecular weight components such as polyfunctional epoxy. As a result, the black curable resin layer 10 can have sufficient flowability during thermocompression bonding and can be prevented from flowing out during thermal curing.

[0045] The blending amount of the elastomer in the black curable resin layer 10 is preferably 0.01 to 90% by mass, more preferably 1 to 80% by mass, and even more preferably 5 to 65% by mass, based on 100% by mass of the total resin solid content of the black curable resin layer 10. Within the above range, the storage modulus can be controlled, and appropriate fluidity during thermocompression bonding can be ensured. Furthermore, when the blending amount is equal to or greater than the above lower limit, the dispersibility of carbon black is improved. Furthermore, the film-forming property is improved, and the film thickness distribution can be narrowed when the epoxy resin composition is applied to form a film.

[0046] (Curing agent) When the black curable resin layer 10 is made of an epoxy resin composition, it may contain a curing agent for epoxy resin other than the modified elastomer having a functional group capable of reacting with an epoxy group. Examples of the other curing agent include known curing agents such as phenol-based curing agents, acid anhydride-based curing agents, and amine-based curing agents. Two or more of the other curing agents may be used in combination.

[0047] (curing catalyst) When the black curable resin layer 10 is composed of an epoxy resin composition, it may contain a curing catalyst that promotes the curing reaction of the epoxy resin. Examples of the curing catalyst include imidazole-based, tertiary amine-based, and phosphorus compound-based. Among them, imidazole-based catalysts are preferred because they are compatible with epoxy resins and do not easily cause yellowing. Among imidazole-based curing catalysts, those having a cyanoethyl group are particularly preferred because they are easily dissolved in epoxy resins. The blending amount of the curing catalyst is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the total resin solid content of the black curable resin layer 10. When it is within the above range, the curing can be sufficiently promoted and the usable time of the integrated encapsulating sheet 1 can be secured. Two or more types of curing catalysts may be used in combination.

[0048] (Black pigment or black dye) The black curable resin layer 10 is colored black. For coloring, it is preferable to contain a black pigment or a black dye, more preferable to contain a black pigment, and even more preferable to contain carbon black. By being colored black, light diffusion prevention properties between the multiple light emitting elements 21, 22, and 23 of the element-mounted substrate 2 can be obtained.

[0049] The particle size of the carbon black is preferably 10 to 500 nm, more preferably 10 to 300 nm, and particularly preferably 10 to 100 nm. The particle size refers to the average particle size, and can be determined by a measuring device using the dynamic light scattering method. An example of a measuring device using the dynamic light scattering method is NanotracWave II UT151 manufactured by Microtrack Bell.

[0050] As the carbon black, one or more of known carbon blacks such as gas black, channel black, furnace black, thermal black, and lamp black can be used. Resin-coated carbon black may also be used. Furthermore, carbon nanofibers and carbon nanotubes may also be used.

[0051] Among the above carbon blacks, gas black is preferred because it has a large amount of surface functional groups, has high dispersibility, and exerts a sufficient light diffusion prevention function even when added in a small amount. In addition, when the black curable resin layer 10 contains a modified elastomer having a functional group capable of reacting with an epoxy resin, the dispersibility is further increased due to the interaction between the surface functional group of the gas black and the functional group of the modified elastomer having a functional group capable of reacting with an epoxy resin, and good light diffusion prevention properties and coating liquid stability can be ensured.

[0052] The amount of carbon black is preferably 0.1 to 15 mass %, and more preferably 0.3 to 5 mass %, based on the total solid content of the black curable resin layer 10. When the amount of carbon black is equal to or greater than the above lower limit, sufficient light blocking properties are obtained. When the amount of carbon black is greater than the above upper limit, the thixotropy of the black curable resin layer 10 increases, the fluidity during thermocompression bonding decreases, and the gaps between the multiple light emitting elements 21, 22, and 23 of the element-mounted substrate 2 cannot be sufficiently filled.

[0053] (Other Components) The black curable resin layer 10 may contain an inorganic filler to improve flame retardancy and heat resistance and adjust the refractive index. The black curable resin layer 10 may further contain, as necessary, a resin other than the epoxy resin and the elastomer, a thickener, a defoamer and / or a leveling agent, an adhesion imparting agent such as a coupling agent, and a flame retardant.

[0054] (2)Transparent curable resin layer The transparent curable resin layer 11 is a layer for sufficiently pressing the black curable resin layer 10 into spaces between the plurality of light emitting elements 21, 22, 23 arranged on the element-mounted substrate 2 in the thermocompression bonding step.

[0055] [Total Light Transmittance] The transparent curable resin layer 11 is preferably prepared so that the total light transmittance in the cured state is 30 to 99%. The transparent curable resin layer 11 is more preferably prepared so that the total light transmittance in the cured state is 35 to 95%, and even more preferably 40 to 90%.

[0056] When the total light transmittance of the transparent curable resin layer 11 in a cured state is equal to or greater than the above lower limit, even if the transparent curable resin layer 11 in a cured state remains on the light emitting elements 21, 22, and 23, the light is not prevented from reaching the viewer.

[0057] [Storage modulus] The storage modulus of the transparent curable resin layer 11 in an uncured state is preferably greater than the storage modulus of the black curable resin layer 10 in an uncured state. At 100° C., the storage modulus of the transparent curable resin layer 11 in an uncured state is preferably greater than the storage modulus of the black curable resin layer 10 in an uncured state. In addition, at 150° C., the storage modulus of the transparent curable resin layer 11 in an uncured state is preferably greater than the storage modulus of the black curable resin layer 10 in an uncured state.

[0058] The storage modulus of the transparent curable resin layer 11 in an uncured state is preferably greater than that of the black curable resin layer 10 at 100° C. to 150° C. When the storage modulus of the transparent curable resin layer 11 in an uncured state is greater than that of the black curable resin layer 10 in an uncured state at 100° C. and 150° C., the storage modulus of the transparent curable resin layer 11 in an uncured state is usually greater than that of the black curable resin layer 10 in an uncured state over the entire range of 100° C. to 150° C.

[0059] The storage modulus of the transparent curable resin layer 11 in an uncured state at 100° C. is 1.0×10 3 Pa or more, 1.0×10 7 Pa or less, and 5.0×10 3 Pa or more, 5.0×10 5 It is more preferable that the pressure is 0.1 Pa or less.

[0060] In an uncured state, the storage modulus of the transparent curable resin layer 11 at 100°C is equal to or less than the preferred upper limit, so that sufficient fluidity is obtained that does not hinder the flow of the black curable resin layer 10 when it is pressed against the element-mounted substrate 2, and the layer can conform to the unevenness of the element-mounted substrate 2 caused by the multiple light-emitting elements 21, 22, 23 and sufficiently fill the spaces between the multiple light-emitting elements 21, 22, 23.

[0061] In an uncured state, the storage modulus of the transparent curable resin layer 11 at 100° C. is equal to or greater than the preferred lower limit, so that the fluidity of the transparent curable resin layer 11 is suppressed, and the surface of the transparent curable resin layer 11 can be made smoother after thermocompression bonding in accordance with the light emitting elements 21, 22, and 23. As a result, the appearance can be improved, and appearance defects such as repelling are less likely to occur during thermal curing.

[0062] In an uncured state, the storage modulus of the transparent curable resin layer 11 at 150° C. is 1.0×10 4 Pa or more, and 1.0×10 4 ~5.0×10 7 Pa is preferably 1.0×10 5 ~5.0×10 6 Pa. When the storage modulus of the transparent curable resin layer 11 at 150°C in an uncured state is equal to or less than the preferred upper limit, cracks due to cure shrinkage are unlikely to occur during thermal curing. When the storage modulus of the transparent curable resin layer 11 at 150°C in an uncured state is equal to or more than the preferred lower limit, flow of the transparent curable resin layer 11 during thermal curing can be suppressed, and defects in appearance after curing, such as repelling, are suppressed. Furthermore, problems are unlikely to occur when etching is performed in a later process.

[0063] In an uncured state, the storage modulus of the transparent curable resin layer 11 at 100° C. is preferably 10 to 1000 times, more preferably 30 to 500 times, that of the black curable resin layer 10. In an uncured state, the storage modulus of the transparent curable resin layer 11 at 150° C. is preferably 5 to 10,000 times, more preferably 10 to 1000 times, that of the black curable resin layer 10. When the storage modulus of the transparent curable resin layer 11 is higher than that of the black curable resin layer 10 at 100° C. and 150° C., the storage modulus of the transparent curable resin layer 11 is usually higher than that of the black curable resin layer 10 over the entire range of 100° C. to 150° C.

[0064] The storage modulus of the transparent curable resin layer 11 at 60° C. after heat treatment at 120° C. for 1 hour is preferably 7×10 8 Pa or more 2×10 10 Pa or less. Since the storage modulus of the transparent curable resin layer 11 at 60°C after heat treatment at 120°C x 1 hour is equal to or less than the preferred upper limit, it is possible to prevent cracks from occurring in the cured transparent curable resin layer 11 when cutting the edge of the substrate 20. Furthermore, since the storage modulus of the transparent curable resin layer 11 at 60°C after heat treatment at 120°C x 1 hour is equal to or more than the preferred lower limit, it is possible to prevent the cured transparent curable resin layer 11 from deforming and expanding and contracting when cutting the edge of the substrate 20, and to prevent the integrated encapsulating sheet 1 on the edge side of the substrate 20 from becoming wavy.

[0065] [Curable resin composition] The transparent curable resin layer 11 is composed of a curable resin composition. As with the black curable resin layer 10, the curable resin composition may be a curable resin composition containing at least one resin selected from an epoxy resin, an acrylic resin, a polyester resin, and a polyurethane resin, and a curing agent. Among these, an epoxy resin composition is preferred because it can be cured at low temperatures and has excellent heat resistance and reliability.

[0066] (Epoxy Resin) Examples of epoxy resins used in the transparent curable resin layer 11 include the same types as those in the black curable resin layer 10. From the viewpoint of imparting an appropriate viscosity during compression to the transparent curable resin layer 11, the transparent curable resin layer 11 preferably contains a high molecular weight epoxy resin having a weight average molecular weight of 10,000 to 100,000. From the viewpoint of having good compatibility with other resin components and being able to dissolve without mixing with a high boiling point solvent that may remain in the dry film even after drying, it is more preferable to contain a high molecular weight epoxy resin having a weight average molecular weight of 10,000 to 35,000.

[0067] By including a high molecular weight epoxy resin having a weight average molecular weight of 10,000 to 100,000 as the epoxy resin used in the transparent curable resin layer 11, the transparent curable resin layer 11 has an appropriate viscosity when heated, and therefore the storage modulus of the transparent curable resin layer 11 can be adjusted to a preferred range within a temperature range of 100° C. to 150° C. The high molecular weight epoxy resin used in the transparent curable resin layer 11 is preferably a phenoxy type epoxy resin, since it has good compatibility with other epoxy resins.

[0068] The phenoxy type epoxy resin has a relatively large molecular weight among epoxy resins and has an appropriate viscosity when heated, so that the storage modulus of the transparent curable resin layer 11 can be adjusted to a preferred range in the range of 100°C to 150°C. In addition, unlike other thermoplastic resins such as polyester, the phenoxy type epoxy resin can be cured as an epoxy resin, so that the crosslinking density can be increased and the heat resistance of the cured product and the reliability of performance for long-term use are not impaired. From the viewpoint of ensuring a storage modulus that presses the black curable resin layer 10 during thermocompression bonding, the glass transition temperature of the phenoxy type epoxy resin used in the transparent curable resin layer 11 is preferably 100°C or higher.

[0069] Specific examples of phenoxy type epoxy resins include "1256", "YX7200", "YX8100", and "YX7180" manufactured by Mitsubishi Chemical Corporation, "YP-50", "YP-50S", and "YP-70" manufactured by Nippon Steel Chemical & Material Co., Ltd., "N-690" manufactured by DIC Corporation, and "H-157" and "EXA-192" manufactured by DIC Corporation.

[0070] The blending amount of the high molecular weight epoxy resin in the transparent curable resin layer 11 is preferably 30 to 80 mass%, more preferably 40 to 70 mass%, and even more preferably 45 to 60 mass%, relative to 100 mass% of the total resin solid content of the transparent curable resin layer 11. The same is true for the preferred blending amount of the phenoxy type epoxy resin in the transparent curable resin layer 11.

[0071] When the blending amount is within the above range, the storage modulus can be controlled, and the storage modulus can be secured to press the transparent curable resin layer 11 during thermocompression bonding. In addition, flow during thermosetting can be suppressed, and poor appearance after curing such as repelling can be suppressed, and further, problems are less likely to occur when etching is performed in a later process. In addition, toughness is improved, and crack-like defects are less likely to occur during thermocompression bonding. In addition, when the blending amount is equal to or less than the above upper limit, the crosslink density of the transparent curable resin layer 11 in the cured state can be increased, and the heat resistance and chemical resistance can be improved.

[0072] Furthermore, it is preferable that the epoxy resin used in the transparent curable resin layer 11 contains a polyfunctional epoxy resin. The polyfunctional epoxy resin can increase the crosslink density, thereby further improving the stability of the performance of the cured product of the epoxy resin composition for long-term use and also improving the heat resistance. In addition, since the viscosity in the range of 100°C to 150°C is lower than that of the phenoxy type epoxy resin, the storage modulus of the transparent curable resin layer 11 can be adjusted by combining it with the phenoxy type epoxy resin.

[0073] Specific examples of polyfunctional epoxy resins include "YX7700", "157S70", and "1032S60" manufactured by Mitsubishi Chemical Corporation, "NC7000L", "XD1000", and "EOCN-1020" manufactured by Nippon Kayaku Co., Ltd., "ESN485" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "N-690", "N-695", and "HP-7200H" manufactured by DIC Corporation.

[0074] The blending amount of the polyfunctional epoxy resin in the transparent curable resin layer 11 is preferably 90% by mass or less, more preferably 10 to 80% by mass, and even more preferably 25 to 60% by mass, relative to 100% by mass of the total resin solid content of the transparent curable resin layer 11. Within the above range, the storage modulus of the transparent curable resin layer 11 during thermocompression bonding can be controlled, and heat resistance and chemical resistance can be imparted in the cured state.

[0075] From the viewpoint of ensuring sufficient fluidity during thermocompression bonding, the transparent curable resin layer 11 preferably contains an epoxy resin having a softening point or melting point of 120° C. or less. From the viewpoint of handleability and heat resistance of the cured product, it is more preferable that the transparent curable resin layer 11 contains an epoxy resin having a softening point or melting point of 50 to 105° C. By containing an epoxy resin having a softening point or melting point within the above range, it becomes possible to control the storage modulus.

[0076] The total amount of epoxy resin in the transparent curable resin layer 11 is preferably 10 to 100% by mass, more preferably 30 to 99% by mass, and even more preferably 50 to 95% by mass, relative to 100% by mass of the total resin solid content of the transparent curable resin layer 11. Within the above range, the storage modulus can be controlled, and the storage modulus sufficient to press the black curable resin layer 10 during thermocompression bonding can be ensured. Furthermore, within the above range, flow during thermal curing can be suppressed, and poor appearance after curing such as repelling can be suppressed, and further, problems are unlikely to occur when etching is performed in a subsequent process. Furthermore, when the amount is equal to or greater than the above lower limit, heat resistance is improved in the cured state.

[0077] (Elastomer) The transparent curable resin layer 11 preferably contains an elastomer in addition to a resin such as an epoxy resin. By containing an elastomer, it becomes easier to control the storage modulus. As the elastomer, the same types as those of the black curable resin layer 10 can be mentioned. Among them, NBR is preferred because it has good compatibility with epoxy resin, can increase the storage modulus of the transparent curable resin layer 10 at about 150°C, and has good adhesion with the black curable resin layer 10. The preferred weight average molecular weight of the elastomer is also the same as that of the black curable resin layer 10.

[0078] In particular, when the transparent curable resin layer 11 is composed of an epoxy resin composition, it is preferable that the transparent curable resin layer 11 contains a modified elastomer having a functional group capable of reacting with an epoxy group. A modified elastomer having a functional group capable of reacting with an epoxy group also acts as a curing agent for the epoxy resin. In addition, since the elastomer reacts with and bonds to the epoxy resin, the heat resistance and reliability against thermal shock are improved. Furthermore, the difference in polarity between the functional group capable of reacting with the epoxy resin and the resin skeleton has a favorable effect on dispersibility, and good dispersibility can be obtained when carbon black is contained in the transparent curable resin layer 11.

[0079] Examples of functional groups capable of reacting with an epoxy group include the same types as those in the black curable resin layer 10. Among them, an acid group or an acid anhydride group is preferred, and a carboxy group or a carboxylic acid anhydride group is particularly preferred, since they can be cured at low temperatures and can ensure a long pot life.

[0080] When the transparent curable resin layer 11 is composed of an epoxy resin composition, it is particularly preferable that the transparent curable resin layer 11 contains modified NBR having a carboxy group. The modified NBR having a carboxy group may be the same as that of the black curable resin layer 10. Two or more types of modified elastomers having a functional group capable of reacting with an epoxy group may be used in combination.

[0081] The blending amount of the elastomer in the transparent curable resin layer 11 is preferably 0 to 50% by mass, more preferably 1 to 70% by mass, and even more preferably 5 to 50% by mass, based on 100% by mass of the total resin solid content of the transparent curable resin layer 11. Within the above range, the storage modulus can be controlled. Furthermore, when the blending amount is equal to or less than the upper limit, the storage modulus can be secured to press the black curable resin layer 10 during thermocompression bonding. Furthermore, flow during thermal curing can be suppressed, and poor appearance after curing such as repelling can be suppressed, and further, problems are less likely to occur when etching is performed in a later process. Furthermore, when the blending amount is equal to or more than the lower limit, the dispersibility of the carbon black is improved. Furthermore, the film-forming property is improved, and the distribution of the film thickness can be narrowed when the epoxy resin composition is applied to form a film.

[0082] (Curing agent) When the transparent curable resin layer 11 is composed of an epoxy resin composition, it may contain a curing agent for epoxy resin other than the modified elastomer having a functional group capable of reacting with an epoxy group. Examples of the other curing agent include the same curing agents as those for the black curable resin layer 10. Two or more kinds of the other curing agents may be used in combination.

[0083] (Curing Catalyst) When the transparent curable resin layer 11 is made of an epoxy resin composition, it may contain a curing catalyst that accelerates the curing reaction of the epoxy resin. Examples of the curing catalyst include the same curing catalysts as those for the black curable resin layer 10, and the preferred embodiments are also the same.

[0084] The blending amount of the curing catalyst is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the total resin solid content of the transparent curable resin layer 11. When it is within the above range, curing can be sufficiently promoted and the pot life of the integrated encapsulating sheet 1 can be secured. Two or more types of curing catalysts may be used in combination.

[0085] (Other Components) The transparent curable resin layer 11 may contain a black pigment or black dye in order to suppress uneven light emission or color unevenness.

[0086] From the viewpoint of increasing the total light transmittance, when the transparent curable resin layer 11 contains carbon black, the blending amount thereof is preferably less than 5 parts by mass, more preferably 1 part by mass or less, and even more preferably 0.1 part by mass or less, relative to 100 parts by mass of the total resin solid content. The transparent curable resin layer 11 may further contain, as necessary, a resin other than the epoxy resin and the elastomer, a thickener, a defoamer and / or a leveling agent, an adhesion imparting agent such as a coupling agent, and a flame retardant.

[0087] (3) Support The support 12 is a layer for protecting the light emitting elements 21, 22, and 23 from external physical impact, humidity, moisture, etc. The support 12 also serves as a support for forming layers such as the curable resin layer 5, the coating layer, and the hard coat layer 13.

[0088] [Total Light Transmittance] The support 12 is preferably prepared so that the total light transmittance is 30 to 99%, more preferably so that the total light transmittance is 35 to 95%, and even more preferably so that the total light transmittance is 40 to 95%. When the total light transmittance of the support 12 is equal to or greater than the lower limit, the light reaching the viewer side is not hindered.

[0089] [Storage modulus] The storage modulus of the support 12 at 60° C. is 7×10 8 Pa or more 2×10 10 Pa or less, and 1×10 9 Pa or more 1×10 10 Pa or less is more preferable, and 2×10 9 Pa or more 6×10 9 It is even more preferable that the storage modulus of support 12 at 60°C is equal to or greater than the preferred lower limit, thereby reducing the whitening phenomenon in which the edge portion of substrate 20 on which light-emitting elements 21, 22, and 23 are arranged appears as a white line on the display. It is even more preferable that the storage modulus of support 12 at 60°C is equal to or less than the preferred upper limit, thereby reducing cracks when light-emitting electronic component 30 is cut.

[0090] [Resin] The support 12 may be made of a thermoplastic resin or a thermosetting resin. Examples of the resin constituting the support 12 include polyethylene terephthalate resin, polybutylene terephthalate resin, polyethylene 2,6-naphthalate resin, polyamide resin, polycarbonate resin, polycarbonate copolymer resin, triacetyl cellulose resin, polymethylpentene resin, phenoxy resin, syndiotactic polystyrene resin, and polyimide resin. In terms of heat resistance, weather resistance, availability, cost, and the like, it is preferable to include at least one resin selected from polyethylene terephthalate resin, polyethylene 2,6-naphthalate resin, polycarbonate resin, polycarbonate copolymer resin, and polyamide resin. By including these resins, deformation during pressure bonding can be prevented. The support 12 may contain a black pigment or black dye to suppress uneven light emission and color unevenness.

[0091] [Film Thickness] The thickness of the support 12 is preferably 10 to 250 μm, more preferably 20 to 225 μm, and even more preferably 25 to 150 μm. When the thickness of the support 12 is equal to or greater than the preferred lower limit, the occurrence of wrinkles during thermocompression bonding of the integrated encapsulating sheet 1 to the substrate 20 can be suppressed, and handling properties can be improved. When the thickness of the support 12 is equal to or less than the preferred upper limit, visibility can be improved and costs can be reduced.

[0092] (4) Hard Coat Layer [Hardness] The hard coat layer 13 is a layer for protecting the light-emitting electronic component from scratches. The pencil hardness of the surface of the hard coat layer 13 is preferably H or more, more preferably 2H or more, and even more preferably 3H or more.

[0093] [Surface roughness] The arithmetic surface roughness (Ra) of the surface of the hard coat layer 13 is preferably 0.1 to 1 μm, more preferably 0.2 to 1 μm, and even more preferably 0.3 to 1 μm. When the Ra of the hard coat layer 13 is equal to or greater than the preferred lower limit, the reflectance of the surface of the hard coat layer 13 can be reduced. When the Ra of the hard coat layer 13 is equal to or less than the preferred upper limit, production becomes easier.

[0094] [Total Light Transmittance] The hard coat layer 13 is preferably prepared so that the total light transmittance is 30 to 99%, more preferably 50 to 99%, and even more preferably 60 to 99%. When the total light transmittance of the hard coat layer 13 is equal to or greater than the lower limit, light is not prevented from reaching the viewer side.

[0095] [resin] The hard coat layer 13 may be made of either a thermoplastic resin or a thermosetting resin, and is preferably made of a thermosetting resin. Examples of the thermosetting resin constituting the hard coat layer 13 include an acrylic resin, a urethane resin, a silicone resin, a melamine resin, and the like, and may contain one or more of these. The hard coat layer 13 may contain a black pigment or dye.

[0096] [Fine Particles] The hard coat layer 13 preferably contains fine particles. As the fine particles, one or both of inorganic fine particles and organic fine particles can be used. As inorganic fine particles, silica fine particles and titanium fine particles can be mentioned. As organic fine particles, polymethyl methacrylate resin (PMMA resin) and urethane resin can be mentioned. Among them, silica fine particles are preferable. By containing fine particles, it is possible to adjust the surface roughness of the hard coat layer 13 and improve the surface hardness.

[0097] [Film Thickness] The thickness of the hard coat layer 13 is preferably 1 to 20 μm, more preferably 2 to 10 μm, and even more preferably 3 to 8 μm. When the thickness of the hard coat layer 13 is equal to or greater than the preferred lower limit, sufficient hardness can be ensured. When the thickness of the hard coat layer 13 is equal to or less than the preferred upper limit, defects such as curling are not caused.

[0098] (5) Characteristics of the semi-transparent layer The semi-transparent layer 6 is the support 12 alone, the support 12+hard coat layer 13, the support 12+coating layer, or the support 12+hard coat layer 13+coating layer. At least one of the hard coat layer 13 and the coating layer may contain a black pigment or dye.

[0099] [Storage modulus] The storage modulus of the semi-transparent layer 6 at 60° C. is 7×10 8 Pa or more 2×10 10 Pa or less, and 1×10 9 Pa or more 1×10 10 Pa or less is more preferable, and 2×10 9 Pa or more 6×10 9 It is even more preferable that the storage modulus at 60°C is equal to or greater than the preferred lower limit, thereby reducing the whitening phenomenon in which the edge of the substrate 20 on which the light-emitting elements 21, 22, and 23 are arranged appears as a white line on the display. It is even more preferable that the storage modulus at 60°C is equal to or less than the preferred upper limit, thereby reducing cracks when the light-emitting electronic component 30 is cut.

[0100] [Total light transmittance] The total light transmittance of the semitransparent layer 6 is preferably 30% or more and 95% or less, more preferably 40% or more and 90% or less. When the total light transmittance of the semitransparent layer 6 is equal to or more than each of the above lower limits, the light is not prevented from reaching the viewer side.

[0101] (6) Optical Properties of Hard Coat Layer [Reflectance] The reflectance of the hard coat layer 13 side measured by a gloss meter (JIS-Z-8741) is preferably 1 to 50%, more preferably 3 to 30%, and even more preferably 5 to 25%. If the reflectance of the hard coat layer 13 side is equal to or higher than the lower limit, production is easy. If the reflectance of the hard coat layer 13 is equal to or lower than the preferred upper limit, the visibility of the display is improved.

[0102] (7) Protective Film The protective films 14 and 15 have a role of protecting the integrated encapsulating sheet 1, and can also be used as a film to which a coating liquid of a curable resin composition is applied when the integrated encapsulating sheet 1 is formed.

[0103] Examples of the protective films 14 and 15 that can be used include polyester films such as polyethylene terephthalate and polyethylene naphthalate, films made of thermoplastic resins such as polyimide films, polyamideimide films, polyethylene films, polytetrafluoroethylene films, polypropylene films, and polystyrene films, as well as surface-treated paper.

[0104] Among these, polyester films are preferably used from the viewpoints of heat resistance, mechanical strength, ease of handling, etc. The thickness of the protective films 14, 15 is not particularly limited and is appropriately selected from the range of about 10 to 150 μm depending on the application. The surfaces of the protective films 14, 15 on which the resin layer is to be provided may be subjected to a release treatment.

[0105] 2. Manufacturing Method of the Integrated Encapsulating Sheet In order to obtain the integrated encapsulating sheet 1, first, a protective film 15 is prepared by applying and drying a coating liquid of a curable resin composition for the black curable resin layer 10 to the protective film 15, and a support 12 is prepared by previously forming a hard coat layer 13, and a coating liquid of a curable resin composition for the transparent curable resin layer 11 is applied and dried to the surface opposite to the hard coat layer 13.

[0106] Thereafter, these are stacked and laminated so that the transparent curable resin layer 11 and the black curable resin layer 10 are in contact with each other, thereby obtaining a laminate in which the black curable resin layer 10, the transparent curable resin layer 11, the support 12, and the hard coat layer 13 are stacked in this order on the protective film 15. A protective film 14 may be laminated on the outer surface of the hard coat layer 13 as necessary.

[0107] The support 12 having the hard coat layer 13 formed thereon can be obtained by applying a coating agent for the hard coat layer 12 to the surface of the support 12 and curing the coating agent. Examples of methods for applying the coating agent include various coaters such as a die coater, gravure coater, roll coater, curtain flow coater, spin coater, bar coater, reverse coater, kiss coater, fountain coater, rod coater, air doctor coater, knife coater, blade coater, cast coater, and screen coater. Examples of methods for curing the coating agent include heat curing, ultraviolet curing, and electron beam curing.

[0108] The coating liquid of the curable resin composition of the black curable resin layer 10 and / or the coating liquid of the curable resin composition of the transparent curable resin layer 11 preferably contains an organic solvent in an amount that provides a viscosity that allows coating without hindrance. The organic solvent is not particularly limited, and examples thereof include ketones, aromatic hydrocarbons, glycol ethers, glycol ether acetates, esters, alcohols, aliphatic hydrocarbons, and petroleum-based solvents. Specific examples of the organic solvent include ketones such as methyl ethyl ketone, cyclohexanone, methyl butyl ketone, and methyl isobutyl ketone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ethyl acetate, butyl acetate, isobutyl acetate, ethyl ... Examples of the solvent include esters such as propylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, and propylene glycol butyl ether acetate; alcohols such as ethanol, propanol, 2-methoxypropanol, n-butanol, isobutyl alcohol, isopentyl alcohol, ethylene glycol, and propylene glycol; aliphatic hydrocarbons such as octane and decane; petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha, as well as N,N-dimethylformamide (DMF), tetrachloroethylene, and turpentine. When carbon black is blended into the coating liquid, carbon black powder may be added, or a liquid in which carbon black has been previously dispersed (carbon black dispersion) may be added.

[0109] Examples of the method for applying the curable resin composition include various coaters such as a die coater, a gravure coater, a roll coater, a curtain flow coater, a spin coater, a bar coater, a reverse coater, a kiss coater, a fountain coater, a rod coater, an air doctor coater, a knife coater, a blade coater, a cast coater, a screen coater, etc. The drying temperature is preferably 60 to 160°C, more preferably 80 to 130°C, and even more preferably 90 to 120°C.

[0110] The temperature during lamination is preferably 20 to 120° C., more preferably 30 to 100° C., and even more preferably 40 to 80° C. By setting the temperature during lamination to a preferable lower limit or higher, it is possible to ensure adhesion between the black curable resin layer 10 and the transparent curable resin layer 11 that allows handling even when uncured. In addition, by setting the temperature during lamination to a preferable upper limit or lower, it is possible to prevent the formation of air bubbles and wrinkles. Lamination can be performed using, for example, a roll laminator, a press machine, a vacuum press machine, or the like.

[0111] 3. Substrate with elements The substrate with elements 2 has a plurality of light-emitting elements 21, 22, and 23 arranged on a substrate 20, as shown in Fig. 2. Fig. 2 etc. shows a schematic portion where three light-emitting elements (light-emitting element 21, light-emitting element 22, and light-emitting element 23) are arranged.

[0112] There is no limitation on the material of the substrate 20, but a known printed circuit board can be suitably used. Examples of known printed circuit boards include a glass epoxy board, a fluororesin board, and a ceramic board.

[0113] The light emitting elements 21, 22, and 23 are typically light emitting diodes. The present invention is particularly suitable for use when the light emitting elements 21, 22, and 23 are extremely small. For example, a light emitting diode having a height of 1000 nm to 200 μm and a side length of 0.001 to 0.5 mm can be used. For the element-mounted substrate 20 for obtaining mini LEDs or micro LEDs, the light emitting elements 21, 22, and 23 can be light emitting diodes of three colors, R, G, and B, or the light emitting elements 21, 22, and 23 can be blue light emitting diodes.

[0114] 4. Light-emitting Electronic Component and Manufacturing Method Thereof A light-emitting electronic component 30 according to one embodiment includes an element-mounted substrate 2 having a plurality of light-emitting elements 21, 22, 23 arranged on a substrate 20, and an integrated encapsulating cured sheet 50 that is pressure-bonded to the surface of the element-mounted substrate 2 on which the plurality of light-emitting elements 21, 22, 23 are arranged. The integrated encapsulating cured sheet 50 is laminated in the order of a resin layer 45 (black resin layer 40, transparent resin layer 41) and a semi-transparent layer 6 (support 12, hard coat layer 13) from the side closer to the substrate 20. The resin layer 45 is filled between the plurality of light-emitting elements 21, 22, 23.

[0115] The manufacturing method of the light-emitting electronic component according to one embodiment is a method in which the above-mentioned integrated encapsulating sheet 1 is arranged on a surface of the element-mounted substrate 2 on which the light-emitting elements 21, 22, 23 are arranged, so that the curable resin layer (in one example, the black curable resin layer 10) of the integrated encapsulating sheet 1 is in contact with the surface on which the light-emitting elements 21, 22, 23 are arranged in the element-mounted substrate 2 in which the light-emitting elements 21, 22, 23 are arranged on the substrate 20, the curable resin layer is filled between the light-emitting elements 21, 22, 23 by press bonding, and the curable resin layer is cured by heating. Hereinafter, the manufacturing method of the light-emitting electronic component according to one embodiment (also simply referred to as "the manufacturing method according to one embodiment") will be described with reference to Figs. 2 to 4.

[0116] In the manufacturing method of one embodiment, first, as shown in FIG. 2, an integrated encapsulating sheet 1 from which the protective film 15 is peeled off to expose the black curable resin layer 10 is placed on the surface of the element-mounted substrate 2 on which the light-emitting elements 21, 22, and 23 are arranged, so that the black curable resin layer 10 is in contact with the surface.

[0117] Before compression bonding, the thickness of the black curable resin layer 10 is preferably 10 to 95% of the height of the light emitting elements 21, 22, 23. The lower limit is more preferably 15% or more, and even more preferably 30% or more. The upper limit is more preferably 85% or less, and even more preferably 75% or less.

[0118] When the thickness of the black curable resin layer 10 is 10% or more of the height of the light emitting elements 21, 22, 23, the function of preventing light diffusion between the light emitting elements 21, 22, 23 is sufficient. In addition, when the storage modulus of the black curable resin layer 10 is relatively low and the layer 10 is rich in fluidity, the resin can be sufficiently filled between the light emitting elements 21, 22, 23. When the thickness of the black curable resin layer 10 is less than 15% of the height of the light emitting elements 21, 22, 23, if the fluidity of the transparent curable resin layer 11 is relatively low, crack-like defects may occur on the surface. When the thickness of the black curable resin layer 10 is 30% or more of the height of the light emitting elements 21, 22, 23, the black curable resin layer 10 having the light diffusion prevention function can be appropriately filled between the light emitting elements 21, 22, 23.

[0119] If the thickness of the black curable resin layer 10 is 95% or less of the height of the light emitting elements 21, 22, 23, leakage to the outside of the black curable resin layer 10 during thermocompression bonding can be prevented, and light from the light emitting elements 21, 22, 23 is unlikely to be hindered from reaching the viewer. If the thickness of the black curable resin layer 10 exceeds 85% of the height of the light emitting elements 21, 22, 23, black shading may be observed due to the variation in the film thickness of the black curable resin layer 10 that flows after pressing. If the thickness of the black curable resin layer 10 is 75% or less of the height of the light emitting elements 21, 22, 23, the black curable resin layer 10 having the light diffusion prevention function can be appropriately filled between the light emitting elements 21, 22, 23.

[0120] The thickness of the transparent curable resin layer 11 before compression bonding is preferably 10 to 500% of the height of the light emitting elements 21, 22, 23. The lower limit is more preferably 20% or more, and even more preferably 30% or more. The upper limit is more preferably 200% or less, and even more preferably 150% or less.

[0121] When the thickness of the transparent curable resin layer 11 is 10% or more relative to the height of the light emitting elements 21, 22, 23, it is easy to function as a sealing layer covering the light emitting elements 21, 22, 23. In addition, when the storage modulus of the transparent curable resin layer 11 is relatively high and the fluidity of the transparent curable resin layer 11 is suppressed, the transparent curable resin layer 11 can be suppressed from flowing together with the black curable resin layer 10 during thermal curing, and appearance defects are unlikely to occur on the surface. When the thickness of the transparent curable resin layer 11 is less than 20% relative to the height of the light emitting elements 21, 22, 23, the range in which the transparent curable resin layer 11 can flow is insufficient, and crack-like defects may occur on the surface. When the thickness of the transparent curable resin layer 11 is 30% or more relative to the height of the light emitting elements 21, 22, 23, the transparent curable resin layer 11 is easy to function as a sealing layer covering the light emitting elements 21, 22, 23. Furthermore, when the storage modulus of the transparent curable resin layer 11 is relatively high and the fluidity of the transparent curable resin layer 11 is suppressed, the transparent curable resin layer 11 can sufficiently press into the black curable resin layer 10.

[0122] The total thickness of the black curable resin layer 10 and the transparent curable resin layer 11 before compression bonding is preferably 110 to 550% of the height of the light emitting elements 21, 22, 23. If the total thickness of the black curable resin layer 10 and the transparent curable resin layer 11 is equal to or greater than the above lower limit value with respect to the height of the light emitting elements 21, 22, 23, the integrated encapsulating sheet 1 can be sufficiently embedded between the light emitting elements 21, 22, 23. If the total thickness of the black curable resin layer 10 and the transparent curable resin layer 11 is equal to or less than the above upper limit value with respect to the height of the light emitting elements 21, 22, 23, thickness unevenness is unlikely to occur during compression bonding, and appearance defects are unlikely to occur on the surface.

[0123] The ratio of the thickness of the black cured resin layer 10 before compression to the total thickness of the transparent cured resin layer 11 and the black cured resin layer 10 before compression is preferably 10 to 90%, and more preferably 15 to 70%. If the ratio of the thickness of the black cured resin layer 10 before compression to the total thickness of the transparent cured resin layer 11 and the black cured resin layer 10 is equal to or greater than the lower limit, the degree of blackness can be increased and the contrast of the display can be sufficiently improved. If the thickness ratio is equal to or less than the upper limit, the black cured resin layer 10 is unlikely to remain on the light emitting elements 21, 22, and 23 during compression, and the brightness can be sufficiently improved.

[0124] 2, the black curable resin layer 10 and a part of the transparent curable resin layer 11 of the integrated encapsulating sheet 1 are embedded between the light emitting elements 21, 22, and 23 as shown in Fig. 3. At this time, if the storage modulus of the black curable resin layer 10 is relatively low and the fluidity of the layer 11 is ensured, the black curable resin layer 10 is preferably easily filled between the light emitting elements 21, 22, and 23 by following the unevenness of the light emitting elements 21, 22, and 23 and is less likely to remain on the light emitting elements 21, 22, and 23.

[0125] The temperature in the thermocompression bonding is preferably 80 to 120° C., and more preferably 90 to 110° C. By setting the temperature in the thermocompression bonding to 80° C. or higher, the fluidity of the integrated encapsulating sheet 1 is easily ensured. In addition, by setting the temperature in the thermocompression bonding to 120° C. or lower, the light emitting elements 21, 22, and 23 are less likely to be damaged. By setting the temperature in the thermocompression bonding to 90 to 110° C., the fluidity can be controlled more precisely, and the occurrence of unevenness or crack-like defects can be suppressed.

[0126] The pressure in the thermocompression bonding is preferably 0.05 to 1.0 MPa, and more preferably 0.1 to 0.5 MPa. By setting the pressure in the thermocompression bonding to the preferred lower limit or more, the black curable resin layer 10 does not remain on the light emitting elements 21, 22, 23, and the light from the light emitting elements 21, 22, 23 is not prevented from reaching the viewer. By setting the pressure to the preferred upper limit or less, the light emitting elements 21, 22, 23 are less likely to be damaged. The thermocompression bonding is preferably performed using a vacuum press machine capable of molding in a vacuum state. This makes it easier to avoid defects caused by air being mixed into the obtained light emitting electronic component 30.

[0127] 4, the protective film 14 is peeled off and then thermally cured to form the black curable resin layer 10 of the integrated encapsulating sheet 1 into a black resin layer 40 (a cured layer of the black curable resin layer 10) and the transparent curable resin layer 11 into a transparent resin layer 41 (a cured layer of the transparent curable resin layer 11). In this way, a light-emitting electronic component 30 is obtained.

[0128] The curing temperature is preferably 100 to 160° C., and more preferably 110 to 150° C. By setting the curing temperature to 100° C. or higher, the integrated encapsulating sheet 1 can be reliably cured. By setting the curing temperature to 110° C. or higher, the curing time of the integrated encapsulating sheet 1 can be shortened. In addition, by setting the curing temperature to the above upper limit temperature or lower, the light emitting elements 21, 22, and 23 are less likely to be damaged.

[0129] The curing time varies depending on the curing temperature, but is preferably 30 to 360 minutes, and more preferably 45 to 180 minutes. At the curing temperature, if the storage modulus of the transparent curable resin layer 11 is relatively high and the fluidity of the layer 11 is suppressed, poor appearance after curing is suppressed, which is preferable.

[0130] 2 to 4, a light-emitting electronic component 30 is obtained in which an integrated sealing cured sheet 50 is pressure-bonded to the surface of the element-mounted substrate 2 on which the light-emitting elements 21, 22, and 23 are arranged, the surface being formed by the element-mounted substrate 2 having the light-emitting elements 21, 22, and 23 arranged on the substrate 20. In the light-emitting electronic component 30 thus obtained, the black curable resin layer 10 and the transparent curable resin layer 11 are cured. Parts of the black resin layer 40 and the transparent resin layer 41 are filled between the light-emitting elements 21, 22, and 23.

[0131] 5.Cutting of circuit boards for light-emitting electronic components FIG. 5 shows a cross-sectional view similar to FIG. 1, but with an end of the light-emitting electronic component of FIG. 4 cut off.

[0132] When the light-emitting electronic components 30 are arranged on the back side of the display, the light-emitting electronic components 30 are cut to a predetermined size. The light-emitting electronic components 30 cut to a predetermined size are arranged on the back side of the display with their end faces aligned. Prior to the present invention, there was a problem of whitening phenomenon in which white lines originating from the end faces are visible from the display side when the light-emitting element is made to emit light. However, by making the support 12 of the integrated encapsulating sheet 1 a layer having a specific range of storage elastic modulus, the white lines are no longer visible from the display side. It was found that the end face 6a of the semi-transparent layer 6 does not become a rough surface compared to the conventional case by cutting, and becomes a relatively smooth surface. It is considered that the so-called whitening phenomenon, which has been a problem in the past, has been solved by making it difficult for light to diffuse at the end face 6a of the semi-transparent layer 6 located on the display side from the light-emitting surfaces of the light-emitting elements 21, 22, and 23. EXAMPLES

[0133] The present invention will be specifically described below with reference to examples, although the present invention is not limited to these examples.

[0134] <Raw Materials> The raw materials used in each Example and Comparative Example are as follows. [Epoxy resin] ·EOCN-1020-55 (manufactured by Nippon Kayaku Co., Ltd., o-cresol novolac type epoxy resin, solid, softening point 55℃, epoxy equivalent 194g / eq.) ·YX7200B35 (manufactured by Mitsubishi Chemical Co., Ltd., phenoxy type epoxy resin, non-volatile content 35wt%, MEK solution, epoxy equivalent 8781g / eq., weight average molecular weight 35000) ·HP7200H (manufactured by DIC Corporation, cyclopentadiene novolac type multifunctional epoxy resin, solid, softening point 82℃, epoxy equivalent 227g / eq.) [Elastomer] ·NX775 (manufactured by Nippon Zeon Co., Ltd., carboxy-modified nitrile rubber, weight average molecular weight 208000) [Hardening agent] ·2PZ-CN (manufactured by Shikoku Kasei Co., Ltd., imidazole type hardener, 1-cyanoethyl-2-phenylimidazole) [Carbon black] ·Special Black#4 (ORION ENGINEERED CARBONS, gas black) [Acrylic resin material] ·8KX-078 (Taisei Fine Chemical, non-volatile content 40wt%) ·MX-500L (Soken Chemical, cross-linked acrylic particles, average particle size 5μm) [Photoradical generator] ·Irgacure TPO H (BASF, photoradical generator) ·Omnirad 127 (GM Resins BV, photoradical generator) [Solvent] ·MEK (Junsei Chemical, methyl ethyl ketone) ·PGM (Junsei Chemical, propylene glycol monomethyl ether) [Support] PET ·PET film 1 (Shin-Etsu Polymer, thickness 75μm) ·PET film 2 (Shin-Etsu Polymer, thickness 188μm) ·PET film 3 (Shin-Etsu Polymer, thickness 250μm) ·PC film 4 (Shin-Etsu Polymer, thickness 75μm, for 100 parts by mass of PC resin Special Black #4 (containing 0.075 parts by mass) ·PC Film 5 (manufactured by Shin-Etsu Polymer Co., Ltd., thickness 75 μm) Glass ·G-Leaf (manufactured by Nippon Electric Glass Co., Ltd., thickness 75 μm) [Protective film] ·1-E (manufactured by Nippa Corporation, release film, thickness 50 μm) <Constituent materials of each layer> The constituent materials of each layer are shown below in terms of the mass part ratio to the amount of non-volatile components.[Materials for the hard code layer] · Hard code layer 1: 8KX-078 (100 parts by weight) MX-500L (15 parts by weight) Irgacure TPO H (1 part by weight) Omnirad 127 (1 part by weight) · Hard code layer 2: 8KX-078 (100 parts by weight) MX-500L (15 parts by weight) Irgacure TPO H (1 part by weight) Omnirad 127 (1 part by weight) Special Black #4 (1 part by weight) [Materials for the code layer] · Code layer 1: EOCN-1020-55 (70 parts by weight) NX775 (30 parts by weight) Special Black#4 (0.5 parts by mass) [Material for transparent curable resin layer A] · Transparent curable resin layer A1 EOCN 1020-55 (30 parts by mass) YH7200B35 (50 parts by mass) NX775 (20 parts by mass) 2PZ-CN (1 part by mass) · Transparent curable resin layer A2 EOCN 1020-55 (50 parts by mass) YH7200B35 (30 parts by mass) NX775 (20 parts by mass) 2PZ-CN (1 part by mass) · Transparent curable resin layer A3 HP7200H (85 parts by mass) NX775 (15 parts by mass) [Material for black curable resin layer B] · Black curable resin layer B1 HP7200H (70 parts by mass) NX775 (30 parts by mass) Special Black#4 (0.5 parts by mass) 2PZ-CN(1 Quality Department).

[0135] <Evaluation> [Total light transmittance] The total light transmittance was measured in accordance with JIS K 7136 using a haze meter (NDH5000) manufactured by Nippon Denshoku Industries Co., Ltd. [Storage modulus] The storage modulus of each semi-transparent layer at 60°C was measured in accordance with JIS K7244 using a viscoelasticity measuring device (RSA-G2 manufactured by TA Instruments) under conditions of a measurement frequency of 1 Hz and a temperature rise rate of 5°C / min. The storage modulus of the transparent curable resin layer and the black curable resin layer (collectively referred to as the curable resin layer) at 60°C was measured by applying the layers to 1-E (Nippa Corporation, release film, thickness 50 μm) so that the film thickness after drying was 30 μm, and heat-treating at 120°C for 1 hour, peeling off the heat-treated curable resin layer from 1-E, and using the viscoelasticity measuring device under the same conditions as above in accordance with JIS K7244. [Brightness] Using a luminance meter CA-410 [product name] (Konica Minolta) and a φ10 mm probe CA-P410H [product name] (Konica Minolta), measure the luminance Acd / m of the element-mounted substrate to which the integrated encapsulating sheet is not thermocompression bonded. 2 and the luminance Bcd / m of the substrate with the element after the integrated encapsulating sheet is thermocompression bonded. 2 were measured and evaluated on a two-level scale based on the results calculated using B / A. ○: B / A is 0.5 or more △: B / A is less than 0.5 [Pencil hardness] The pencil hardness of the surface of the one-piece encapsulant cured sheet was measured using a pencil hardness tester (JIS-K5600-5-4). The outer periphery of five element-mounted substrates was cut using a cutter K-210 [product name] (manufactured by Hozan Corporation), and the results were evaluated on the following three-level scale according to the percentage of whitening that occurred. "◎" and "◯" were considered to be acceptable. ⊚: Of the 5 sheets, 0 / 5 sheets showed whitening. ◯: Of the 5 sheets, whitening occurred in 1 / 5 sheets. ×: Among the five sheets, whitening occurred in 2 / 5 or more sheets. [Cracks when cutting] The outer periphery of each of the five element-mounted substrates was cut and evaluated on the following three-level scale according to the percentage of cracks in the support. "A" and "◯" were deemed acceptable. ⊚: Of the 5 sheets, 0 / 5 sheets had cracks in the support. ◯: Of the five sheets, cracks occurred in the support in one of the five sheets. ×: Of the five sheets, cracks occurred in the support of 2 / 5 or more sheets.

[0136] <Example 1> [Preparation of film] Each material for the hard coat layer 1 was mixed with MEK solvent to prepare a coating liquid 1 for the hard coat layer having a solid content concentration of 30 wt %. The obtained coating liquid 1 for the hard coat layer was applied to one side of the above-mentioned PET film 1, dried at 100°C for 4 minutes, and then subjected to a 2000 mJ / cm 2 The coating layer was cured by irradiating it with ultraviolet light of 1000 nm to form a hard coat layer 1 with a thickness of 4 μm. Next, each material of the coating layer 1 was mixed with MEK solvent to prepare a coating layer liquid 1 with a solid content concentration of 20 wt %. The obtained coating layer liquid 1 was applied to the surface of the PET film 1 opposite to the hard coat layer 1, and dried at 100° C. for 4 minutes to form a coating layer 1 with a thickness of 5 μm. Then, it was aged at 60° C. for 72 hours. In this way, a semi-transparent layer 1 with a hard coat layer and a coating layer was obtained.

[0137] [Formation of transparent curable resin layer] Each material of the transparent curable resin layer A1 was mixed in a solvent of MEK / PGM=80 / 20 to prepare a coating liquid 1 for the transparent curable resin layer with a solid concentration of 35 wt%. Next, the coating liquid 1 for the transparent curable resin layer was applied to the coating layer 1 side of the semi-transparent layer 1 using a bar coater so that the dry film thickness was 30 μm, and dried at 120° C. for 4 minutes to obtain a laminated sheet 1 in which the transparent curable resin layer A1 was supported by the semi-transparent layer 1. The storage modulus at 60° C. of the transparent curable resin layer A1 after heat treatment at 120° C. for 1 hour was 2.0×10 9 The storage modulus at 60° C. after heat treatment at 120° C. for 1 hour of the transparent curable resin layer A1 in each of the following Examples and Comparative Examples is also the same.

[0138] [Formation of black curable resin layer] Each material of the black curable resin layer B1 was mixed with MEK solvent to prepare a coating liquid for the black curable resin layer with a solid content concentration of 45 mass %. Next, the coating liquid for the black curable resin layer was applied to the release-treated surface of the protective film using a bar coater so that the dry film thickness was 50 μm, and dried at 100 ° C for 4 minutes to obtain a laminated sheet 2 in which the black curable resin layer B1 was supported by the protective film. The storage modulus at 60 ° C after heat treatment at 120 ° C for 1 hour of the black curable resin layer B1 was 9.5 × 10 8 The storage modulus at 60° C. after heat treatment at 120° C. for 1 hour of the black curable resin layer B1 in each of the following Examples and Comparative Examples is also the same.

[0139] [Preparation of integrated encapsulating sheet] The laminate sheet 1 and the laminate sheet 2 were stacked so that the transparent curable resin layer A1 and the black curable resin layer B1 were in contact with each other, and laminated with a roll laminator at 60°C to prepare an integrated encapsulating sheet in which the protective film, the black curable resin layer B1, the transparent curable resin layer A1, the coating layer 1, the PET film 1, and the hard coat layer 1 were stacked in this order.

[0140] [Manufacture of light-emitting electronic component] The obtained integrated encapsulating sheet was placed on a substrate having light-emitting elements (height 70 μm, length 100 μm, width 200 μm) mounted thereon, so that the black curable resin layer 1 from which the protective film had been peeled off was in contact with the substrate. In this state, lamination was performed at a temperature of 80 to 110° C. and a pressure of 0.3 MPa using a vacuum laminator MVLP-500 (manufactured by Meiki Seisakusho). Next, the curable resin layer was cured in a hot air circulation drying oven at 120° C. for 1 hour to obtain a light-emitting electronic component.

[0141] <Example 2> A semi-transparent layer 2 was formed that was the same as the semi-transparent layer 1 except that the thickness of the coating layer 1 was set to 7.5 μm, and an integrated encapsulating sheet was produced under the same manufacturing conditions as in Example 1 after the formation of the semi-transparent layer, thereby obtaining a light-emitting electronic component.

[0142] <Example 3> A semi-transparent layer 3 was formed in the same manner as the semi-transparent layer 1 except that the thickness of the coating layer 1 was set to 10 μm, and an integrated encapsulating sheet was produced under the same manufacturing conditions as in Example 1 after the formation of the semi-transparent layer, thereby obtaining a light-emitting electronic component.

[0143] <Example 4> Each material for the hard coat layer 2 was mixed with MEK solvent to prepare a coating liquid 2 for the hard coat layer having a solid content concentration of 30 wt %. The obtained coating liquid 2 for the hard coat layer was applied to one side of the above-mentioned PET film 1, dried at 100°C for 4 minutes, and then subjected to 2000 mJ / cm 2 The sheet was cured by irradiating it with ultraviolet light of 100 .mu.m to form a hard coat layer 2 having a thickness of 4 μm. Thus, a semi-transparent layer 4 with a hard coat layer was obtained. Thereafter, an integrated encapsulating sheet was produced under the same production conditions as in Example 1 after the formation of the semi-transparent layer, and a light-emitting electronic component was obtained.

[0144] <Example 5> A translucent layer 5 was formed in the same manner as the translucent layer 1 except that the support was changed to a PET film 2, and an integrated encapsulating sheet was produced under the same manufacturing conditions as in Example 1 after the formation of the translucent layer, thereby obtaining a light-emitting electronic component.

[0145] <Example 6> A translucent layer 6 was formed in the same manner as the translucent layer 1 except that the support was a PET film 3, and an integrated encapsulating sheet was produced under the same manufacturing conditions as in Example 1 after the formation of the translucent layer, thereby obtaining a light-emitting electronic component.

[0146] <Example 7> Each material for the hard coat layer 1 was mixed with an MEK solvent to prepare a coating liquid 1 for the hard coat layer having a solid content concentration of 30 wt %. The obtained coating liquid 1 for the hard coat layer was applied to one side of the above-mentioned PC film 4, dried at 100°C for 4 minutes, and then subjected to 2000 mJ / cm 2 The hard coat layer 1 was cured by irradiating ultraviolet light of 1000 ohms to form a hard coat layer 1 having a thickness of 4 μm. Thus, a semi-transparent layer 7 with a hard coat layer was obtained. Thereafter, an integrated encapsulating sheet was produced under the same production conditions as in Example 1 after the formation of the semi-transparent layer, and a light-emitting electronic component was obtained.

[0147] <Example 8> [Preparation of integrated encapsulating sheet] A semi-transparent layer 1 was obtained under the same conditions as in Example 1. Next, each material of the transparent curable resin layer A2 was mixed in a solvent of MEK / PGM=80 / 20 to prepare a coating liquid 2 for a transparent curable resin layer having a solid content concentration of 35 mass%. Next, the coating liquid 2 for a transparent curable resin layer was applied to the coating layer 1 side of the semi-transparent layer 1 using a bar coater so that the dry film thickness was 80 μm, and dried at 120 ° C. for 5 minutes to prepare an integrated encapsulating sheet in which the transparent curable resin layer A2 was supported by the semi-transparent layer 1. The storage modulus at 60 ° C. after heat treatment at 120 ° C. for 1 hour of the transparent curable resin layer A2 was 1.0 × 10 9 The storage modulus at 60° C. after heat treatment at 120° C. for 1 hour of the transparent curable resin layer A2 in the subsequent comparative examples was also the same.

[0148] [Manufacture of light-emitting electronic component] The obtained integrated encapsulating sheet was placed on a substrate with a light-emitting element (height 70 μm, length 100 μm, width 200 μm) mounted on the substrate so that the transparent curable resin layer A2 was in contact with the substrate. In this state, lamination was performed at a temperature of 80 to 110°C and a pressure of 0.3 MPa using a vacuum laminator MVLP-500 (manufactured by Meiki Seisakusho). Next, the transparent curable resin layer A2 was cured in a hot air circulation drying oven at 120°C for 1 hour to obtain a light-emitting electronic component.

[0149] <Example 9> A semi-transparent layer 1 was obtained under the same conditions as in Example 1. Next, each material of the transparent curable resin layer A3 was mixed in a solvent of MEK / PGM=80 / 20 to prepare a 35% by mass coating liquid 3 for the transparent curable resin layer. Next, the coating liquid 3 for the transparent curable resin layer was applied to the coating layer 1 side of the semi-transparent layer 1 using a bar coater so that the dry film thickness was 80 μm, and dried at 120° C. for 5 minutes to prepare an integrated encapsulating sheet in which the transparent curable resin layer A3 was supported by the semi-transparent layer 1. Thereafter, a light-emitting electronic component was obtained in the same manner as in Example 8. The storage modulus at 60° C. after heat treatment at 120° C. for 1 hour of the transparent curable resin layer A3 was 2.0×10 8 It was Pa.

[0150] <Comparative Example 1> A translucent layer 8 was formed in the same manner as the translucent layer 1 except that the support was a PC film 5, and an integrated encapsulating sheet was produced under the same manufacturing conditions as in Example 1 after the formation of the translucent layer, thereby obtaining a light-emitting electronic component.

[0151] Comparative Example 2 A semitransparent layer 8 was obtained under the same conditions as in Comparative Example 1. The manufacturing conditions after the formation of the semitransparent layer were the same as in Example 8 to prepare an integrated encapsulating sheet, and a light-emitting electronic component was obtained.

[0152] <Comparative Example 3> Each material of the coating layer 1 was mixed with an MEK solvent to prepare a coating layer liquid 1 having a solid content concentration of 20 wt %. The obtained coating layer liquid 1 was applied to one side of the above-mentioned thin glass plate and dried at 120°C for 5 minutes to form a coating layer 1 with a thickness of 5 μm. In this way, a semi-transparent layer 9 with a coating layer was obtained. An integrated encapsulating sheet was produced under the same manufacturing conditions as in Example 1 after the formation of the semi-transparent layer, and a light-emitting electronic component was obtained.

[0153] <Configuration and Various Properties of Semitransparent Layer> Table 1 shows the configuration of the semitransparent layer produced in each of the examples and comparative examples.

[0154] [Table 1]

[0155] Table 2 shows various properties of the semi-transparent layers produced in each of the Examples and Comparative Examples. The storage modulus in Table 2 means the storage modulus at 60°C.

[0156] [Table 2]

[0157] Table 3 shows the configurations and evaluation results of each of the examples and comparative examples.

[0158] [Table 3]

[0159] As shown in Tables 2 and 3, the semi-transparent layers 1 to 7 (storage modulus at 60°C: 2.3 × 10 9 Pa~4.1×10 9 In Examples 1 to 9 having a semi-transparent layer 8 (storage modulus at 60° C.: 5.0×10 Pa), almost no whitening of the cut surface or cracking at the time of cutting was observed, and the luminance was also at an acceptable level. 8 In Comparative Examples 1 and 2, which were provided with a semi-transparent layer 9 (storage modulus at 60° C.: 7.0×10 Pa), whitening of the cut surface was observed and did not meet the acceptable standard. 10 In Comparative Example 3 having a tensile strength of 1000 mm / s, no whitening of the cut surface was observed, but cracks were observed when cutting, and the cut surface did not meet the acceptable standard. [Industrial Applicability]

[0160] The integrated encapsulating sheet according to the present invention can be used, for example, as a sheet for encapsulating a substrate on which a plurality of light emitting elements are arranged. [Explanation of symbols]

[0161] DESCRIPTION OF SYMBOLS 1...integrated encapsulating sheet, 2...substrate with element, 5...curable resin layer, 6...semi-transparent layer, 6a...end surface, 10...black curable resin layer, 11...transparent curable resin layer, 12...support, 13...hard coat layer, 14, 15...protective film, 20...substrate, 21, 22, 23...light-emitting element, 30...light-emitting electronic component, 40...black resin layer, 41...transparent resin layer, 45...resin layer, 50...integrated encapsulating curable sheet.

Claims

1. An integrated encapsulating sheet that is pressure-bonded to a surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, the surface being formed with the plurality of light-emitting elements, A curable resin layer and a semi-transparent layer are laminated in this order in order of contact with the light-emitting element when the light-emitting element is pressure-bonded to the light-emitting element, The storage modulus of the semi-transparent layer at 60° C. is 7×10 8 Pa or more 2×10 10 The integrated encapsulating sheet has a compressive strength of 0.1 Pa or less.

2. the semi-transparent layer has a resin support, The integrated encapsulating sheet according to claim 1, wherein the support has a thickness of 20 μm or more and 225 μm or less.

3. The integrated encapsulating sheet according to claim 1 , wherein the semi-transparent layer has at least one of a coating layer and a hard coat layer.

4. The integrated encapsulating sheet according to claim 2 , characterized in that the support contains a black pigment or dye.

5. The integrated encapsulating sheet according to claim 3 , wherein at least one of the coating layer or the hard coat layer contains a black pigment or dye.

6. The integrated encapsulating sheet according to any one of claims 3 to 5, wherein the translucent layer has a total light transmittance of 40% or more and 90% or less.

7. The curable resin layer has a storage modulus of 7×10 at 60° C. after heat treatment at 120° C. for 1 hour. 8 Pa or more 2×10 10 The integrated encapsulating sheet according to claim 1, characterized in that the elastic modulus is 0.05 Pa or less.

8. The integrated encapsulating sheet according to claim 1 , wherein the curable resin layer has, in the order of contact with the plurality of light-emitting elements, a black curable resin layer and a transparent curable resin layer.

9. a substrate having a plurality of light emitting elements disposed thereon; an integrated encapsulating cured sheet in a state of being pressure-bonded to a surface of the element-mounted substrate on which the plurality of light-emitting elements are arranged; Equipped with The integrated encapsulating cured sheet has a resin layer and a semi-transparent layer laminated in this order from the side closest to the substrate, The light-emitting electronic component is characterized in that the resin layer is filled between the plurality of light-emitting elements.

10. The integrated encapsulating sheet according to claim 1 or 2 is disposed on a surface of an element-mounted substrate on which a plurality of light-emitting elements are arranged, so that the curable resin layer of the integrated encapsulating sheet is in contact with the surface of the element-mounted substrate, The curable resin layer is filled between the plurality of light emitting elements by pressing. The method for producing a light-emitting electronic component further comprises curing the curable resin layer by heating.

Citation Information

Patent Citations

  • Sheet for sealing optical semiconductors

    JP2010141119A

  • Light-emitting device and manufacturing method of light-emitting device

    JP2020035910A

  • Optical semiconductor element encapsulation sheet

    JP2022129764A

  • Thermosetting resin composition

    JP2023012051A