Molded fiber-reinforced resin article, artificial wood, and article
By using a tertiary amine compound with a cyclic structure and a trimerization catalyst in polyurethane foam compositions, the issues of high reactivity and delayed curing are addressed, resulting in improved surface quality and efficient production of fiber-reinforced resin molded products and artificial wood.
Patent Information
- Application Number
- JP2023073550
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
High reactivity in polyurethane foam compositions leads to issues such as surface voids, surface roughening, and delayed curing, which can cause extended demolding times and deformation, especially when fibers or fillers are used.
Incorporating a tertiary amine compound with a cyclic structure and a trimerization catalyst into the polyurethane foam composition to moderate initial reactivity and improve curing characteristics.
The solution effectively suppresses initial reactivity, reduces surface roughness, enhances impregnation of fibers, shortens demolding time, and prevents deformation, while maintaining controlled reactivity for efficient production.
Smart Images

Figure 2024158392000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to fiber-reinforced resin molded products, artificial wood, and articles. [Background technology]
[0002] Polyurethane foams are widely used in fiber-reinforced resin molded products, artificial wood, articles, etc. Polyurethane foams are obtained from compositions for polyurethane foams. Various compositions for polyurethane foams have been disclosed. For example, Patent Document 1 discloses a composition for polyurethane foams containing dibutyltin dilaurate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 48-030137 Summary of the Invention [Problem to be solved by the invention]
[0004] When the polyurethane foam composition has a high reactivity, there are problems as follows. That is, there is a risk of causing appearance problems such as surface voids and rough surfaces of the polyurethane foam. In addition, when fibers or fillers are used, there is a risk of the impregnation of the polyurethane foam composition into the fibers and the like being deteriorated. On the other hand, when the rise time, which is used to evaluate the reactivity of a polyurethane foam composition in the latter stage, is excessively decreased, the following problem occurs: the curing is delayed, which may result in an extension of the demolding time or deformation during demolding. The present disclosure is intended to solve at least a part of the above problems, and can be realized in the following forms. [Means for solving the problem]
[0005] [1] A fiber-reinforced resin molded product obtained by impregnating fibers with a polyurethane foam composition and curing the composition, The polyurethane foam composition comprises: A polyol, A tertiary amine compound having a cyclic structure, A trimerization catalyst; A fiber-reinforced resin molded product comprising: [2] A polyol, A tertiary amine compound having a cyclic structure, A trimerization catalyst; An artificial wood material comprising a polyurethane foam obtained from a composition containing an isocyanate. [3] A polyol, A tertiary amine compound having a cyclic structure, A trimerization catalyst; and an isocyanate, An article in which the outer surface of the polyurethane foam has a designed surface. Effect of the Invention
[0006] According to the present disclosure, at least a part of the above problems is solved. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a perspective view showing a fiber-reinforced plastic molded product according to one embodiment. [Diagram 2] 2 is a cross-sectional view taken along line AA in FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The present disclosure will be described in detail below. In this specification, when a numerical range is described using "-", the lower limit and the upper limit are included unless otherwise specified. For example, the description "10-20" includes both the lower limit "10" and the upper limit "20". In other words, "10-20" has the same meaning as "10 or more and 20 or less". In this specification, the upper limit and the lower limit of each numerical range can be arbitrarily combined.
[0009] 1. Fiber-reinforced plastic moldings 10 Hereinafter, a fiber-reinforced plastic molded product according to one embodiment of the present invention will be described with reference to the drawings. 1 and 2, a fiber-reinforced resin molded article 10 is produced by impregnating fibers 11 with a composition for polyurethane foam and curing the composition. The composition for polyurethane foam contains a polyol, a tertiary amine compound having a cyclic structure, a trimerization catalyst, and an isocyanate.
[0010] 1.1 Fibers 11 The type of fiber 11 is not particularly limited as long as it can reinforce the fiber-reinforced resin molded product 10. The fiber 11 may be, for example, any of inorganic fibers such as glass fiber, carbon fiber, and metal fiber, and organic fibers such as natural fibers, and synthetic fibers such as vinylon fiber and cellulose fiber. From the viewpoint of improving strength, the fiber 11 is preferably an inorganic fiber, and more preferably a glass fiber. Only one type of fiber may be used, or two or more types may be used in combination.
[0011] The glass fiber is preferably a long glass fiber. The long glass fiber has a fiber length of, for example, 50 mm or more. The upper limit of the fiber length of the long glass fiber is not particularly limited. For example, the upper limit of the fiber length of the long glass fiber may be the same as the longitudinal dimension of the fiber-reinforced resin molded product 10. The fiber length of the long glass fiber is not limited to the above range. For example, in the case of a chopped strand injection molding method described later, the fiber length of the long glass fiber is preferably 12 mm or more and 1000 mm or less. The long glass fiber may be a glass roving made by arranging monofilaments into a roving. The fiber diameter of the monofilament is not particularly limited and may be, for example, 5 μm or more and 50 μm or less. The count (g / 1000 m) of the glass roving is not particularly limited and may be, for example, 500 or more and 5000 or less.
[0012] The mass ratio of the glass fiber to the composition for polyurethane foam is not particularly limited, and is preferably 10:90-90:10, more preferably 25:75-75:25, and even more preferably 40:60-60:40.
[0013] 1.2 Composition for polyurethane foam The composition for producing a polyurethane foam contains a polyol, a tertiary amine compound having a cyclic structure, a trimerization catalyst, and an isocyanate.
[0014] (1) Polyol The polyol is not particularly limited, and various polyols may be used alone or in combination of two or more kinds.
[0015] The functionality and hydroxyl value of the polyol are not particularly limited. The functionality of the polyol is preferably 2-8, more preferably 2.5-6, and even more preferably in the range of 3-5. The hydroxyl value of the polyol is preferably 200mgKOH / g-600mgKOH / g, more preferably 300mgKOH / g-550mgKOH / g, and even more preferably 350mgKOH / g-550mgKOH / g. When using multiple polyols with different functionality or hydroxyl values, it is preferable that the average functionality or average hydroxyl value is in the above range. The average functionality or average hydroxyl value is the average value of the functionality or hydroxyl value of each polyol according to the blending ratio.
[0016] The number average molecular weight of the polyol is not particularly limited. The number average molecular weight of the polyol is, for example, 200-3000. When using a plurality of polyols with different number average molecular weights, it is preferable that the number average molecular weights of all the polyols are within the above range. The number average molecular weight of the polyol can be measured by gel permeation chromatography (GPC). When the polyol is a commercially available product, the catalog value may be used as the number average molecular weight of the polyol.
[0017] The viscosity of the polyol is not particularly limited. In order to sufficiently impregnate the fibers with the liquid, the viscosity of the polyol is preferably 10,000 mPa·s or less, more preferably 5,000 mPa·s or less, and even more preferably 2,500 mPa·s or less. The viscosity of the polyol is usually 200 mPa·s or more. The viscosity of the polyol can be measured at 25°C and 60 rpm using a B-type rotational viscometer.
[0018] The type of polyol is not particularly limited. Examples of polyols include polyether polyols, polyester polyols, polyether ester polyols, polycarbonate diols, and polyols having a carbon-carbon bond main chain. Among these, polyether polyols are preferably used from the viewpoint of hydrolysis resistance. Examples of polyether polyols include polyoxypropylene-polyoxyethylene polyols, polymer polyols, and polyoxytetramethylene glycol. Examples of the polyester polyol include aliphatic or aromatic polycondensation polyester polyols and polycaprolactone polyols. Examples of polyols having a carbon-carbon bond-based main chain include polyolefin-based polyols such as polybutadiene polyol and isoprene polyol, plant-derived polyols, and acrylic polyols.
[0019] (1.1) Polyether polyols Examples of polyether polyols include polyether polyols obtained by adding one or more of ethylene oxide, propylene oxide, butylene oxide, tetrahydrofuran, epichlorohydrin, styrene oxide, etc., to one or more of the following initiators (compounds), or polytetramethylene ether glycol. Among the following initiators, from the viewpoint of imparting appropriate hardness to the polyurethane foam and improving durability, it is preferable to use an alcohol having 4 to 8 functionalities as at least one of the initiators.
[0020] (1.1.1) Initiator (1.1.1.1) Polyhydric alcohols and alkylene oxide adducts of polyhydric alcohols Examples of polyhydric alcohols: [Difunctional alcohol] Ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, dipropylene glycol, trimethylene glycol [Trifunctional alcohol] Glycerin, trimethylolpropane [Tetrafunctional alcohol] Pentaerythritol [Hexafunctional alcohol] Sorbitol [Octanoic alcohol] Sucrose (1.1.1.2) Alkylene oxide adducts of polyhydric phenols Examples of alkylene oxide adducts of polyhydric phenols: alkylene oxide adducts of bisphenol A (1.1.1.3) Polyhydroxy compounds Examples of polyhydroxy compounds are phosphoric acid, benzene phosphoric acid, polyphosphoric acid (e.g. tripolyphosphoric acid and tetrapolyphosphoric acid), etc. (1.1.1.4) Phenol-aniline-formaldehyde ternary condensation products (1.1.1.5) Aniline-formaldehyde condensation products (1.1.1.6) Polyamines Examples of polyamines: ethylenediamine, diethylenetriamine, triethylenetetramine, methylenebisorthochloroaniline, 4,4- and 2,4'-diphenylmethanediamine, 2,4-tolylenediamine, 2,6-tolylenediamine, etc. (1.1.1.7) Alkanolamines Examples of alkanolamines: triethanolamine, diethanolamine, etc.
[0021] (1.1.2) Polymer polyol The polymer polyol is a polyol obtained by graft-polymerizing the above-mentioned polyether polyol with an ethylenically unsaturated compound such as acrylonitrile, styrene, or alkyl methacrylate.
[0022] (1.2) Polyester polyol The polyester polyols are polyester polyols obtained by condensation of one or more compounds having at least two hydroxyl groups with one or more compounds having at least two carboxyl groups, or ring-opening polymers of cyclic esters such as caprolactone and methylvalerolactone.
[0023] (1.2.1) Examples of compounds having at least two hydroxy groups Ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, trimethylene glycol, 1,3- and 1,4-butanediol, tetramethylene glycol, neopentyl glycol, methylpentanediol, butylethylpropanediol, hexamethylene glycol, decamethylene glycol, glycerin, trimethylolpropane, pentaerythritol, sorbitol
[0024] (1.2.2) Examples of compounds having at least two carboxyl groups Malonic acid, maleic acid, succinic acid, adipic acid, tartaric acid, pimelic acid, azelaic acid, sebacic acid, oxalic acid, phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, hemellitic acid
[0025] (1.3) Polycarbonate polyol Examples of polycarbonate polyols include those obtained by transesterification of a low molecular weight polyol such as butanediol or hexanediol with a low molecular weight carbonate such as propylene carbonate or diethyl carbonate.
[0026] (1.4) Polyolefin polyols Examples of polyolefin polyols include polybutadiene polyols, polyisoprene polyols, hydrogenated polybutadiene polyols, and hydrogenated polyisoprene polyols.
[0027] (1.5) Plant-derived polyols The polyol may contain a plant-derived polyol in addition to the above polyols. Examples of the plant-derived polyol include castor oil-based polyol, soybean oil-based polyol, palm oil-based polyol, palm kernel oil-based polyol, coconut oil-based polyol, cashew oil-based polyol, olive oil-based polyol, cottonseed oil-based polyol, safflower oil-based polyol, sesame oil-based polyol, sunflower oil-based polyol, and linseed oil-based polyol. The plant-derived polyols usually have 2 to 3 functional hydroxyl groups in one molecule. Examples of castor oil-based polyols include castor oil, a reaction product of castor oil with a polyol, an esterification reaction product of castor oil fatty acid with a polyol, etc. Examples of polyols to be reacted with castor oil or castor oil fatty acid include divalent polyols such as ethylene glycol, diethylene glycol, and propylene glycol, and trivalent or higher polyols such as glycerin, trimethylolpropane, hexanetriol, and sorbitol. The soybean oil-based polyol may be a polyol derived from soybean oil, such as a reaction product of soybean oil and a polyol, or an esterification reaction product of soybean oil fatty acid and a polyol. The polyol to be reacted with soybean oil or soybean oil fatty acid may be the same as that of castor oil. The same applies to palm oil-based polyol, cashew oil-based polyol, and the like. The various polyols exemplified as plant-derived polyols may be used alone or in combination of two or more kinds.
[0028] (2) Tertiary amine compounds having a cyclic structure Tertiary amine compounds refer to compounds in which one nitrogen atom is bonded to three different carbon atoms. Tertiary amine compounds are used as urethane catalysts (resin catalysts, foaming catalysts). Tertiary amine compounds having a cyclic structure tend to have lower foaming activity than, for example, tertiary amine compounds having a linear structure. Therefore, by using a tertiary amine compound having a cyclic structure, it is possible to suppress the initial reactivity of the polyurethane foam composition. For example, when a tertiary amine compound having a cyclic structure is used, the cream time of the polyurethane foam composition can be preferably 70 seconds or more, more preferably 2 minutes 30 seconds or more and 3 minutes 20 seconds or less (150 seconds or more and 200 seconds or less).
[0029] Examples of the cyclic structure include a cyclic structure containing nitrogen and / or a cyclic structure containing a carbon bonded to nitrogen. The cyclic structure is preferably at least one selected from a benzene ring, a morpholine ring, an imidazole ring, a piperazine ring, and a cyclohexane ring. The tertiary amine compound having a cyclic structure may be used alone or in combination of two or more.
[0030] The tertiary amine compound having a benzene ring has a structure in which, for example, one substituent having a benzene ring and two identical or different alkyl groups having 1 to 8 carbon atoms are bonded to a nitrogen atom. An example of the tertiary amine compound having a benzene ring is DMBA (N,N-dimethylbenzylamine).
[0031] The tertiary amine compound having a morpholine ring has, for example, a structure in which an alkyl group having 1 to 8 carbon atoms is bonded to a nitrogen atom constituting the morpholine ring. Examples of the tertiary amine compound having a morpholine ring include N-methyl morpholine, N-ethylmorpholine, and N-(N',N'-dimethylaminoethyl)morpholine.
[0032] The tertiary amine compound having an imidazole ring has, for example, a structure in which an alkyl group having 1 to 8 carbon atoms is bonded to a nitrogen atom constituting the imidazole ring. Examples of the tertiary amine compound having an imidazole ring include 1-isobutyl-2-methylimidazole, 1-methylimidazole, and 1,2-dimethylimidazole.
[0033] The tertiary amine compound having a piperazine ring has, for example, a structure in which at least one of the nitrogen atoms constituting the piperazine ring is bonded to an alkyl group having 1 to 8 carbon atoms. Examples of the tertiary amine compound having a piperazine ring include N,N',N'-trimethylaminoethylpiperazine, N,N'-dimethylaminoethylpiperazine, and bis(N,N-dimethylaminoethyl-piperazinyl)ethane.
[0034] The tertiary amine compound having a cyclohexane ring has a structure in which a substituent having a cyclohexane ring and two identical or different alkyl groups having 1 to 8 carbon atoms are bonded to a nitrogen atom. Examples of the tertiary amine compound having a cyclohexane ring include DMCHA (N,N-Dimethylcyclohexylamine) and MDCHA (N,N-Dicyclohexylmethylamine).
[0035] The content of the tertiary amine compound having a cyclic structure is not particularly limited. The content of the tertiary amine compound having a cyclic structure is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.15 parts by mass or more, relative to 100 parts by mass of polyol, from the viewpoint of sufficiently promoting the polyurethane production reaction. On the other hand, from the viewpoint of suppressing the initial reactivity of the polyurethane foam composition, it is preferably 3.0 parts by mass or less, more preferably 2.0 parts by mass or less, and even more preferably 1.0 parts by mass or less. From these viewpoints, the content of the tertiary amine compound having the cyclic structure is preferably 0.05 parts by mass or more and 3.0 parts by mass or less, more preferably 0.1 parts by mass or more and 2.0 parts by mass or less, and even more preferably 0.15 parts by mass or more and 1.0 parts by mass or less.
[0036] The tertiary amine compound having a cyclic structure is preferably at least one selected from the group consisting of DMBA (N,N-dimethylbenzylamine), N-methyl morpholine, and N-ethylmorpholine (hereinafter also referred to as tertiary amine compound A).
[0037] The content of the tertiary amine compound A is not particularly limited. The content of the tertiary amine compound A is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.15 parts by mass or more, relative to 100 parts by mass of polyol, from the viewpoint of sufficiently promoting the polyurethane production reaction. On the other hand, from the viewpoint of suppressing the initial reactivity of the polyurethane foam composition, it is preferably 3.0 parts by mass or less, more preferably 2.0 parts by mass or less, and even more preferably 1.0 parts by mass or less. From these viewpoints, the content of the tertiary amine compound A is preferably 0.05 parts by mass or more and 3.0 parts by mass or less, more preferably 0.1 parts by mass or more and 2.0 parts by mass or less, and even more preferably 0.15 parts by mass or more and 1.0 parts by mass or less.
[0038] (3) Trimerization catalyst The trimerization catalyst is a catalyst that reacts isocyanate groups contained in isocyanate to trimerize them and promote the formation of isocyanurate rings. The present inventors have newly discovered that the use of a tertiary amine compound having a cyclic structure in combination with a trimerization catalyst can suppress the initial reactivity of a polyurethane foam composition while improving the latter reactivity of the polyurethane foam composition, and have developed the technology of the present disclosure. For example, when a tertiary amine compound having a cyclic structure is used in combination with a trimerization catalyst, the cream time of the polyurethane foam composition can be set to 70 seconds or more, while the rise time can be set to a range of 3 minutes 20 seconds to 8 minutes. Preferably, the rise time can be set to 5 minutes 30 seconds to 7 minutes 10 seconds (330 seconds or more and 430 seconds or less).
[0039] Examples of the trimerization catalyst include alkali metal carboxylates such as potassium acetate, potassium 2-ethylhexanoate, and potassium octylate; nitrogen-containing aromatic compounds such as tris(dimethylaminomethyl)phenol, 2,4-bis(dimethylaminomethyl)phenol, and 2,4,6-tris(dialkylaminoalkyl)hexahydro-S-triazine; tertiary ammonium salts such as trimethylammonium salt, triethylammonium salt, and triphenylammonium salt; and quaternary ammonium salts such as tetramethylammonium salt, tetraethylammonium, and tetraphenylammonium salt. Among these, alkali metal carboxylates are preferred, and potassium carboxylate is more preferred. Only one trimerization catalyst may be used, or two or more may be used in combination.
[0040] The content of the trimerization catalyst is not particularly limited. The content of the trimerization catalyst is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.08 parts by mass or more, based on 100 parts by mass of polyol, from the viewpoint of improving the reactivity of the polyurethane foam composition in the latter stage. On the other hand, from the viewpoint of suppressing the initial reactivity of the polyurethane foam composition, it is preferably 1.0 parts by mass or less, more preferably 0.5 parts by mass or less, and even more preferably 0.3 parts by mass or less. From these viewpoints, the content of the trimerization catalyst is preferably 0.01 parts by mass or more and 1.0 parts by mass or less, more preferably 0.05 parts by mass or more and 0.5 parts by mass or less, and even more preferably 0.08 parts by mass or more and 0.3 parts by mass or less.
[0041] (4) Foaming agent (optional ingredient) The polyol composition preferably contains a blowing agent. The blowing agent is preferably one or more selected from the group consisting of water, hydrohaloolefins, and alkanes having 4 to 8 carbon atoms. Among these, water is preferable. Only one blowing agent may be used, or two or more blowing agents may be used in combination.
[0042] The content of water is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more, relative to 100 parts by mass of polyol. On the other hand, the content of water is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less. From these viewpoints, the content of water is preferably 0.1 parts by mass or more and 5 parts by mass or less, more preferably 0.3 parts by mass or more and 3 parts by mass or less, and even more preferably 0.5 parts by mass or more and 2 parts by mass or less, relative to 100 parts by mass of polyol.
[0043] (5) Isocyanate The isocyanate is not particularly limited. At least one selected from the group consisting of aromatic isocyanates, alicyclic isocyanates, and aliphatic isocyanates is preferably used as the isocyanate. At least one aliphatic isocyanate and at least one aromatic isocyanate may be used in combination. The isocyanate may be either a bifunctional isocyanate having two isocyanate groups in one molecule, or a trifunctional or higher isocyanate having three or more isocyanate groups in one molecule, and may be used alone or in combination. For example, bifunctional isocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, xylylene diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, and 3,3'-dimethoxy-4,4'-biphenylene diisocyanate. Examples of the isocyanate include aromatic isocyanates such as phenylene diisocyanate, alicyclic isocyanates such as cyclohexane-1,4-diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, and methylcyclohexane diisocyanate, and aliphatic isocyanates such as butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, and lysine isocyanate. Examples of tri- or higher functional isocyanates include 1-methylbenzene-2,4,6-triisocyanate, 1,3,5-trimethylbenzene-2,4,6-triisocyanate, biphenyl-2,4,4'-triisocyanate, diphenylmethane-2,4,4'-triisocyanate, methyldiphenylmethane-4,6,4'-triisocyanate, 4,4'-dimethyldiphenylmethane-2,2',5,5'tetraisocyanate, triphenylmethane-4,4',4"-triisocyanate, and polymeric MDI. In addition, urethane prepolymers, carbodiimide-modified isocyanates, isocyanurate-modified isocyanates, and biuret-modified isocyanates can also be used.
[0044] The blending ratio of polyol and isocyanate is not particularly limited. The blending ratio of polyol and isocyanate can be determined according to the isocyanate index. The isocyanate index is preferably 80 to 200, more preferably 90 to 150, and even more preferably 100 to 130. The isocyanate index (INDEX) is a value obtained by multiplying the number of moles of the isocyanate component per mole of active hydrogen group contained in the polyol composition by 100, and is calculated by [(isocyanate equivalent of isocyanate component / active hydrogen equivalent in polyol composition)×100].
[0045] (6) Other ingredients (optional ingredients) The polyol composition may contain, as other components, additives such as a foam stabilizer, a flame retardant, a solvent, a surfactant, a colorant, and an antioxidant. The content of these additives can be appropriately adjusted according to the desired physical properties of the resulting polyurethane foam, within a range that does not affect the foaming reaction and resinification reaction of the polyurethane foam. The total amount of the additives can be, for example, 1 part by mass or more and 30 parts by mass or less per 100 parts by mass of the polyol.
[0046] (7) Physical properties of polyurethane foam The physical properties of the polyurethane foam obtained from the polyurethane foam composition can be appropriately set depending on the application, etc. The polyurethane foam preferably has the following physical properties. (7.1) Density (apparent total density) The apparent overall density (JIS K7222:2005 compliant) is 70kg / m 3 -300kg / m 3 is preferred, and 90 kg / m 3 -250kg / m 3 More preferably, 110 kg / m 3 -200kg / m 3 The apparent density is, for example, the density at the time of free foaming. (7.2) Compressive strength Compressive strength (JIS K7220:2006 compliant) is 50N / cm2 More than 80N / cm is preferable. 2 More preferably, 100N / cm 2 More preferably, the upper limit of the compressive strength is not particularly limited. The upper limit of the compressive strength is usually 300 N / cm 2 The following is the result.
[0047] 2. Manufacturing method of fiber-reinforced plastic molded products The fiber reinforced resin molded product can be molded. The manufacturing method of the fiber reinforced resin molded product is not particularly limited. For example, the manufacturing method of the fiber reinforced resin molded product is to impregnate fibers with a polyurethane foam composition and harden the composition. Examples of the manufacturing method of the fiber reinforced resin molded product include a chopped strand injection molding method, a method of impregnating a glass nonwoven fabric, and a method of impregnating aligned fibers 11.
[0048] 2.1 Chopped strand injection molding Chopped strand injection molding is a method for producing fiber-reinforced plastic molded products by simultaneously extruding urethane raw materials and long glass fibers. For example, isocyanate and polyol are mixed, preferably in a mixing head, chopped fibers are dripped into the mixture, and then the material is sprayed onto a mold and / or support, where it is subsequently cured.
[0049] According to the chopped strand injection molding method, it is possible to obtain fiber reinforced resin molded products having the following physical properties, for example: The density of a fiber-reinforced plastic molded product is, for example, 500 kg / m 3 More than 1500kg / m 3 Below 650kg / m 3 More than 1350kg / m 3 Below 800kg / m 3 More than 1200kg / m 3 It can be as follows: The glass content of the fiber reinforced plastic molded product can be, for example, 3 mass% or more and 50 mass% or less, 5 mass% or more and 40 mass% or less, or 8 mass% or more and 35 mass% or less, when the entire fiber reinforced plastic molded product is taken as 100 mass%. The bending strength of a fiber-reinforced plastic molded product (based on JIS K7017) is, for example, 50N / mm 2 More than 200N / mm 2 Below, 60N / mm 2 More than 160N / mm 2 Below, 70N / mm 2 More than 120N / mm 2 It can be as follows: The flexural modulus of a fiber-reinforced plastic molded product (based on JIS K7017) is, for example, 1000N / mm 2 More than 10000N / mm 2 Below, 1500N / mm 2 More than 8000N / mm 2 Below, 2000N / mm 2 More than 5000N / mm 2 It can be as follows:
[0050] 2.2 Impregnation method for nonwoven glass fabric The method of impregnating the glass nonwoven fabric is, for example, a method in which a glass fiber mat is laid and the laid glass fiber mat is impregnated with the raw material. Such a method is also called a batch method.
[0051] 2.3 Impregnation method for aligned fibers 11 1 and 2, a plurality of fibers 11 are aligned at a predetermined interval. When continuously producing a fiber-reinforced plastic molded product 10 that is long in one direction, it is preferable to advance the fibers 11 in the length direction while aligning the plurality of fibers 11.
[0052] Next, the polyurethane foam composition is applied to the aligned fibers 11. For example, the polyurethane foam composition is applied by pouring a liquid polyurethane foam composition from above onto the aligned fibers 11 or by immersing the aligned fibers 11 in the polyurethane foam composition. In order to spread the polyurethane foam composition between the fibers 11, the fibers 11 to which the polyurethane foam composition is applied may be sandwiched between members or swung.
[0053] Next, the fibers 11 to which the polyurethane foam composition is attached are heated while being molded. For example, when continuously producing a fiber-reinforced plastic molded article 10 that is long in one direction, the bundle of fibers 11 to which the polyurethane foam composition is attached may be heated while being molded by passing it through a molding passage having a predetermined cross-sectional shape. The heated polyurethane foam composition then foams and hardens to obtain the fiber-reinforced plastic molded article 10.
[0054] The density of the fiber-reinforced article thus produced is, for example, 500 kg / m 3 More than 1500kg / m 3 Below 600kg / m 3 More than 1350kg / m 3 Below 700kg / m 3 More than 900kg / m 3 It can be as follows: The glass content of the fiber reinforced plastic molded product can be, for example, 10% by mass or more and 80% by mass or less, 20% by mass or more and 70% by mass or less, or 30% by mass or more and 60% by mass or less, when the entire fiber reinforced plastic molded product is taken as 100% by mass. The bending strength of a fiber-reinforced plastic molded product (based on JIS K7017) is, for example, 50N / mm 2 More than 300N / mm 2 Below, 100N / mm 2 More than 250N / mm 2 Below, 150N / mm 2 More than 200N / mm 2 It can be as follows: The flexural modulus of a fiber-reinforced plastic molded product (based on JIS K7017) is, for example, 5000N / mm 2 More than 15000N / mm 2 Below, 6000N / mm 2 More than 13000N / mm 2 Below, 7000N / mm 2 More than 11000N / mm 2 It can be as follows:
[0055] There is no particular limitation on the use of the fiber reinforced resin molded product 10. The fiber reinforced resin molded product 10 has excellent physical properties such as mechanical strength, durability, and light weight, and is suitable for use as a sleeper, a building material, a simple bridge, and the like.
[0056] 3.Artificial wood The artificial wood of the present disclosure includes a polyurethane foam obtained from a composition (a polyurethane foam composition) containing a polyol, a tertiary amine compound having a cyclic structure, a trimerization catalyst, and an isocyanate. The artificial wood is, for example, a molded article of polyurethane foam having a wood grain pattern on the surface.
[0057] For artificial wood, the explanations in the section "Fiber-reinforced plastic molded product 10" for "polyol," "tertiary amine compound having a cyclic structure," "trimerization catalyst," "isocyanate," and "physical properties of polyurethane foam" apply as is, and the description is omitted. In other words, the explanations in the section "Fiber-reinforced plastic molded product 10" for "polyol," "tertiary amine compound having a cyclic structure," "trimerization catalyst," "isocyanate," and "physical properties of polyurethane foam" apply as is. The composition may further contain a filler such as fiber, wood chips, etc. The composition may contain the components described in "Foaming agent (optional component)" and "Other components (optional components)" in the "Fiber-reinforced resin molded product 10" section.
[0058] 4. Manufacturing method of artificial wood An example of a method for producing artificial wood will be described. In the method for producing artificial wood, for example, unevenness is imparted to the surface of a molded polyurethane foam to form a wood grain pattern. Such artificial wood can be produced, for example, by using a molding die. The mold surface of this molding die has a shape that is an inversion of the unevenness of the grain of natural wood. In the method for producing artificial wood, a composition is foamed and cured while in contact with the mold surface. The unevenness of the mold surface is transferred to the surface of the molded polyurethane foam to impart unevenness. Since the initial reactivity of the polyurethane foam composition of the present disclosure is suppressed, the composition can be sufficiently brought into contact with the mold surface before curing, and the unevenness of the mold surface can be suitably transferred.
[0059] The uses of the artificial wood are not particularly limited. For example, the artificial wood is suitable as a building material such as a wood deck.
[0060] 5. Articles with a decorative outer surface of polyurethane foam The article of the present disclosure includes a polyurethane foam obtained from a composition (polyurethane foam composition) containing a polyol, a tertiary amine compound having a cyclic structure, a trimerization catalyst, and an isocyanate. In the article, the outer surface of the polyurethane foam has a design surface. The article is, for example, made of a molded polyurethane foam. That is, the surface of the molded polyurethane foam that was in contact with the molding surface of the mold may be the design surface. The shape of the design surface is not particularly limited. The design surface may have an uneven shape such as a grain pattern, a wood grain pattern, or a geometric pattern, or may be a smooth surface.
[0061] Regarding the article, the explanations in the column "Fiber-reinforced plastic molded product 10" for "polyol," "tertiary amine compound having a cyclic structure," "trimerization catalyst," "isocyanate," and "physical properties of polyurethane foam" apply as is, and the description is omitted. In other words, the explanations in the column "Fiber-reinforced plastic molded product 10" for "polyol," "tertiary amine compound having a cyclic structure," "trimerization catalyst," "isocyanate," and "physical properties of polyurethane foam" apply as is. The composition may further contain a filler such as fiber, etc. The composition may contain the components described in the "foaming agent (optional component)" and "other components (optional components)" in the "fiber-reinforced resin molded product 10" section.
[0062] 6. Manufacturing method of the above-mentioned article An example of a method for manufacturing the above article will be described. The above article can be manufactured, for example, using a mold. The mold surface of this mold has a shape corresponding to the design surface. Specifically, when the design surface is uneven, the mold surface of the mold has a shape that is an inversion of the uneven shape of the design surface. When the design surface is a smooth surface, the mold surface of the mold is made smooth. In the method for manufacturing the above article, the composition is foamed and cured in a state in contact with the mold surface. The shape of the mold surface is transferred to the surface of the molded polyurethane foam to form the design surface. Since the initial reactivity of the polyurethane foam composition of the present disclosure is suppressed, the composition can be sufficiently brought into contact with the mold surface before curing, and the shape of the mold surface can be suitably transferred.
[0063] The uses of the above-mentioned articles are not particularly limited. For example, the above-mentioned articles are suitable as building materials such as exterior parts, exterior materials for vehicles, interior materials for vehicles, substitutes for wood, and the like. EXAMPLES
[0064] 1. Preparation of polyol composition (liquid A) for polyurethane foam composition Polyol compositions (liquid A) for polyurethane foam compositions of Experimental Example 1-23 in Table 1-4 were prepared. Experimental Examples 1-6, 10-13, and 17-23 are working examples. Experimental Examples 7-9 and 14-16 are comparative examples. In Table 1-4, when an "*" is added, such as "7*", it indicates that it is a comparative example.
[0065] The following polyol 1 and polyol 2 were mixed at 40 / 60 (parts by mass). When the total amount of this polyol was 100 parts by mass, 0.75% by mass of a blowing agent (water) and 3% by mass of a foam stabilizer were added. To this mixed solution, the cyclic tertiary amine compound 1-7, the linear tertiary amine compound 1-3, and the trimerization catalysts 1 and 2 shown in each sample in Table 1-4 were added in the blending ratios shown in Table 1-4 to obtain a polyol composition (liquid A). In Table 1-4, the cyclic tertiary amine compound 1-7 represents a tertiary amine compound having a cyclic structure. The blending ratios in Table 1-4 are the blending amounts (parts by mass) of each compound when the entire polyol is 100 parts by mass. "-" indicates that the corresponding component was not added.
[0066] The details of each raw material are as follows: Polyol 1: Polyether polyol using pentaerythritol as an initiator, hydroxyl value 400mgKOH / g Polyol 2: Polyether polyol using glycerin as an initiator, hydroxyl value 400mgKOH / g Foaming agent: Water Foam stabilizer: Silicone surfactant, Dow Toray, SF2945 Cyclic tertiary amine compound 1: DMBA (N,N-dimethylbenzylamine) ·Cyclic tertiary amine compound 2:N-methyl morpholine Cyclic tertiary amine compound 3: N-ethylmorpholine Cyclic tertiary amine compounds 4: 1-isobutyl-2-methylimidazole Cyclic tertiary amine compounds 5: 1-Methylimidazole Cyclic tertiary amine compound 6: N,N',N'-trimethylaminoethylpiperazine Cyclic tertiary amine compound 7: DMCHA (N,N-Dimethylcyclohexylamine) Linear tertiary amine compound 1: TMHMDA (N,N,N',N'-Tetramethyl-1,6-hexanediamine) Linear tertiary amine compound 2: PMDETA (N,N,N',N'',N''-Pentamethyldiethylenetriamine) Linear tertiary amine compound 3: 70% bis(2-dimethylaminoethyl) ether, 30% DPG Trimerization catalyst 1: Potassium acetate Trimerization catalyst 2: Potassium octylate
[0067] [Table 1]
[0068] [Table 2]
[0069] [Table 3]
[0070] [Table 4]
[0071] 2. Preparation of Polyurethane Foam The following raw materials were used as the isocyanate (liquid B). Isocyanate: Polymeric MDI, Formlite 200B, BASF INOAC Polyurethanes
[0072] The above polyol composition (liquid A) and the above isocyanate (liquid B) were mixed to prepare a polyurethane foam composition. Liquid A and liquid B were mixed at a ratio of 100 / 165 (liquid A / liquid B, mass ratio). A polyurethane foam was obtained from the polyurethane foam composition by free foaming.
[0073] The free foaming was carried out according to the following procedure. The polyol composition (liquid A) and the isocyanate (liquid B) were adjusted to a liquid temperature of 25° C. A plastic box measuring 100 mm×100 mm×200 mm was used as a mold for free foaming. The polyurethane foam composition was allowed to freely foam in the mold to obtain a polyurethane foam.
[0074] The reactivities (cream time, gel time, rise time) of the polyurethane foam composition were measured by the following methods. Cream time: The time it took for the above mixture to become cloudy and creamy was measured as the cream time (seconds). Gel time: The time from when the mixture thickened to when it started to gel was measured as the gel time (seconds). Rise time: The time until the foam stopped rising due to foaming in the above mixed liquid was measured as the rise time (seconds). In the above measurement, the time when mixing of the polyol composition (liquid A) and the isocyanate (liquid B) was started was set as zero seconds. The evaluation was performed by visual observation.
[0075] 3. Evaluation Methodology (1) Density (apparent overall density) The apparent overall density of the resulting polyurethane foam was measured in accordance with JIS K7222:2005. (2) Compressive strength The compressive strength of the obtained polyurethane foam was measured in accordance with JIS K7220:2006. (3) Maximum surface temperature, time to reach maximum surface temperature, presence or absence of tack (stickiness of the surface) The maximum surface temperature (°C) during the reaction of the polyurethane foam composition and the time required to reach the maximum surface temperature were measured for Experimental Examples 1, 2, 17-23, and Experimental Examples 7 and 8. In addition, the surfaces of the obtained polyurethane foams of Experimental Examples 1, 2, 17-23, and Experimental Examples 7 and 8 were touched with the hand to check for the presence or absence of tack.
[0076] 4. Results The results are shown in Table 1-4. In the columns of density, compressive strength, maximum surface temperature, time to reach maximum surface temperature, and presence or absence of tack (surface stickiness) in Table 1-4, "-" indicates that no evaluation was performed.
[0077] Experimental Examples 1-6, 10-13, and 17-23 satisfy the following requirements (a) and (b). Requirement (a): The composition for a polyurethane foam contains a tertiary amine compound having a cyclic structure. Requirement (b): The composition for a polyurethane foam contains a trimerization catalyst.
[0078] In contrast, Experimental Examples 7-9 do not satisfy requirement (b), and Experimental Examples 14-16 do not satisfy requirement (a). Experimental Examples 1-6, 10-13, and 17-23, which satisfied the requirements (a) and (b), had a longer cream time than Experimental Example 14-16, which did not satisfy the requirement (a). In addition, Experimental Examples 1-6, 10-13, and 17-23, which satisfied the requirements (a) and (b), had a rise time of 3 minutes 23 seconds to 7 minutes 49 seconds. This suggests that by satisfying the requirements (a) and (b), the reactivity of the polyurethane foam composition can be appropriately suppressed while improving the latter reactivity (e.g., rise time).
[0079] It is believed that suppressing the reactivity of the polyurethane foam composition can contribute to improving the roughness of the polyurethane foam surface, and also that suppressing the reactivity of the polyurethane foam composition can contribute to improving the wettability of the polyurethane foam composition to fibers or fillers when the polyurethane foam composition is used. It is believed that if the reactivity in the latter half of the process (e.g., rise time) can be improved, it can contribute to shortening the demolding time. It is also believed that if the reactivity in the latter half of the process (e.g., rise time) can be improved, it can contribute to suppressing deformation during demolding.
[0080] Experimental Examples 1, 2, and 17-23, which satisfied the requirements (a) and (b), had a higher maximum surface temperature and also reached the maximum surface temperature sooner than Experimental Examples 7 and 8, which did not satisfy the requirement (b). Experimental Examples 1, 2, and 17-23, which satisfied the requirements (a) and (b), did not have tack. On the other hand, Experimental Examples 7 and 8, which did not satisfy the requirement (b), had tack. This suggests that by satisfying the requirements (a) and (b), it is possible to reduce tack while adjusting the reactivity of the polyurethane foam composition.
[0081] Furthermore, if the tackiness can be reduced, it is believed that this will contribute to improving the design of polyurethane foams. It is also expected to improve the production cycle.
[0082] According to the above examples, at least some of the problems related to the deterioration of the surface properties of the polyurethane foam, the deterioration of the impregnation of the polyurethane foam composition into the fibers, etc. when fibers or fillers are used, the long demolding time, and the deformation during demolding have been resolved.
[0083] The present disclosure is not limited to the embodiments described above in detail, and various modifications and variations are possible within the scope of the present disclosure. [Explanation of symbols]
[0084] 10...Fiber reinforced plastic molded products 11. Fiber
Claims
1. A fiber-reinforced resin molded product obtained by impregnating fibers with a polyurethane foam composition and curing the composition, The polyurethane foam composition comprises: A polyol, A tertiary amine compound having a cyclic structure, A trimerization catalyst; A fiber-reinforced resin molded product comprising:
2. A polyol, A tertiary amine compound having a cyclic structure, A trimerization catalyst; An artificial wood material comprising a polyurethane foam obtained from a composition containing an isocyanate.
3. A polyol, A tertiary amine compound having a cyclic structure, A trimerization catalyst; and an isocyanate, An article in which the outer surface of the polyurethane foam has a designed surface.
Citation Information
Patent Citations
JP1973030137A
Cited By
Molded article, soundproof material, and disposer cover
WO2026105246A1
Molded article, soundproofing material, garbage disposal cover, sound insulating material, and sound insulating material for vehicle
WO2026105383A1