Tin oxide particle-containing gel, method for producing tin oxide particle dispersion, and method for producing tin oxide particle laminated film

The tin oxide particle-containing gel addresses conductivity loss and dispersion challenges by using a solvent-based dispersion method with amines and doping, resulting in a conductive laminated film with reduced costs and improved stability.

JP2024158418APending Publication Date: 2024-11-08MITSUBISHI MATERIALS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023073606
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing methods for producing tin oxide particle dispersions face issues such as the use of non-volatile organic compounds as dispersants leading to conductivity loss, difficulty in dispersing single nano-sized particles, and high solvent concentrations that increase transportation costs and reduce particle spacing.

Method used

A tin oxide particle-containing gel is used, which allows for dispersion in a solvent without additional treatment, utilizing primary and secondary amines, and can be doped with elements like antimony, fluorine, and phosphorus to enhance conductivity, with a particle concentration range of 25-65% and particle size of 1.5-100 nm.

Benefits of technology

This method enables the formation of a tin oxide particle laminated film with excellent conductivity, reduced transportation costs, and stable film thickness, while eliminating the need for non-volatile dispersants and enhancing dispersion efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158418000002
    Figure 2024158418000002
  • Figure 2024158418000003
    Figure 2024158418000003
  • Figure 2024158418000004
    Figure 2024158418000004
Patent Text Reader

Abstract

To provide a tin oxide particle-containing gel capable of forming a tin oxide particle dispersion by adding a solvent without undergoing dispersion treatment, a method for producing the tin oxide particle dispersion using the tin oxide particle-containing gel, and a method for producing a tin oxide particle laminated film.SOLUTION: A tin oxide dispersion is formed by containing tin oxide particles and adding a solvent thereto, thereby the tin oxide particles are diffused into the solvent. One or both of primary amine and secondary amine are preferably contained. The content of the tin oxide particle is preferably 25 mass% or more and 65 mass% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a tin oxide particle-containing gel capable of producing a tin oxide particle dispersion liquid used, for example, in forming a conductive film, a method for producing a tin oxide particle dispersion liquid using this tin oxide particle-containing gel, and a method for producing a tin oxide particle laminate film. [Background technology]

[0002] Since tin oxide has relatively good electrical conductivity, tin oxide particle laminated films having a structure in which tin oxide particles are laminated are used as conductive materials for conductive layers in various devices, etc. In order to improve specific properties of the tin oxide particle laminated film, materials in which various elements are doped into tin oxide have also been proposed. The above-mentioned tin oxide particle laminated film is formed by coating and drying a tin oxide particle dispersion liquid in which tin oxide particles are dispersed, as disclosed in Patent Document 1, for example.

[0003] As methods for producing the above-mentioned tin oxide particle dispersion liquid, there have been proposed a method in which tin oxide powder is dispersed in a bead mill or the like to produce a dispersion liquid, and a method in which a tin oxide particle dispersion liquid is produced without using powder by a technique such as a solvothermal method. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 64-027667 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the method of dispersing tin oxide powder using a bead mill or the like to prepare a dispersion liquid, it is necessary to use a non-volatile organic compound as a dispersant, and the dispersant remaining after coating and drying causes a decrease in the conductivity of the tin oxide particle laminated film. In addition, there is also the issue that it is difficult to disperse single nano-sized tin oxide particles, such as those used as the electron transport layer in perovskite solar cells.

[0006] On the other hand, in the method of producing a tin oxide particle dispersion liquid without using powder, such as the solvothermal method, it is difficult to increase the concentration of tin oxide particles, and there are problems such as a high ratio of solvent and high transportation costs, etc. In particular, with single nano particles with a particle size of 10 nm or less, the decrease in particle spacing as the dispersion liquid becomes more concentrated is significant, making it very difficult to increase the concentration of the dispersion liquid.

[0007] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a tin oxide particle-containing gel that can be turned into a tin oxide particle dispersion by adding a solvent without going through a dispersion treatment, a method for producing a tin oxide particle dispersion using this tin oxide particle-containing gel, and a method for producing a tin oxide particle laminate film. [Means for solving the problem]

[0008] In order to solve the above problems, the tin oxide particle-containing gel of aspect 1 of the present invention is characterized in that it contains tin oxide particles, and when a solvent is added, the tin oxide particles diffuse into the solvent to form a tin oxide dispersion. According to the tin oxide particle-containing gel of aspect 1 of the present invention, when a solvent is added, the tin oxide particles diffuse into the solvent, and therefore, a tin oxide particle dispersion liquid can be obtained by adding a solvent to the tin oxide particle-containing gel. Therefore, the tin oxide particles can be transported in the form of a tin oxide-containing gel, which reduces transportation costs. In addition, it is not necessary to use a dispersant made of a non-volatile organic compound, and a tin oxide particle laminate film with excellent electrical conductivity can be formed.

[0009] The tin oxide particle-containing gel of embodiment 2 of the present invention is characterized in that the tin oxide particle-containing gel of embodiment 1 contains one or two of primary amines or secondary amines. According to the tin oxide particle-containing gel of embodiment 2 of the present invention, in addition to tin oxide particles, it contains one or two of primary amines or secondary amines. Therefore, by adding a solvent such as water or a lower alcohol, it is possible to efficiently disperse the tin oxide particles contained in the tin oxide particle-containing gel in the solvent.

[0010] The tin oxide particle-containing gel of embodiment 3 of the present invention is the tin oxide particle-containing gel of embodiment 1 or 2, characterized in that the content of the tin oxide particles is within the range of 25 mass % or more and 65 mass % or less. According to the tin oxide particle-containing gel of aspect 3 of the present invention, the content of the tin oxide particles is within the range of 25 mass% or more and 65 mass% or less, so that the tin oxide particles are contained at a high concentration, and transportation costs can be significantly reduced.

[0011] A tin oxide particle-containing gel according to a fourth aspect of the present invention is characterized in that, in the tin oxide particle-containing gel according to any one of the first to third aspects, the primary particle diameter of the tin oxide particles is within the range of 1.5 nm or more and 100 nm or less. According to the tin oxide particle-containing gel of aspect 4 of the present invention, the primary particle diameter of the tin oxide particles is within the range of 1.5 nm or more and 100 nm or less, so that a tin oxide particle laminated film with a thickness on the nano-order can be stably formed.

[0012] A tin oxide particle-containing gel according to a fifth aspect of the present invention is the tin oxide particle-containing gel according to any one of the first to fourth aspects, characterized in that the tin oxide particles are doped with a different element. According to the tin oxide particle-containing gel of embodiment 5 of the present invention, the tin oxide particles are doped with a different element, so that the properties of the tin oxide particles can be adjusted and a tin oxide particle laminate film can be formed according to required properties.

[0013] A tin oxide particle-containing gel according to a sixth aspect of the present invention is characterized in that in the tin oxide particle-containing gel according to the fifth aspect, the different element is one or more elements selected from the group consisting of antimony, fluorine and phosphorus. According to the tin oxide particle-containing gel of aspect 6 of the present invention, the heterogeneous elements are one or more selected from antimony, fluorine and phosphorus, so that the properties of the tin oxide particles can be adjusted and a tin oxide particle laminate film can be formed according to the required properties.

[0014] The method for producing a tin oxide particle dispersion liquid according to the seventh aspect of the present invention is characterized by having a solvent addition step of adding a solvent to the tin oxide particle-containing gel according to any one of the first to fifth aspects. The method for producing a tin oxide particle dispersion liquid of aspect 7 of the present invention includes a solvent addition step of adding a solvent to the tin oxide particle-containing gel of any one of aspects 1 to 5. Therefore, the solvent addition step makes it possible to produce a tin oxide particle dispersion liquid in which the tin oxide particles are sufficiently dispersed in the solvent.

[0015] The method for producing a tin oxide particle laminate film according to aspect 8 of the present invention is characterized by comprising a solvent adding step of adding a solvent to the tin oxide particle-containing gel according to any one of aspects 1 to 5 to prepare a tin oxide particle dispersion, and a coating step of coating the obtained tin oxide particle dispersion. The method for producing a tin oxide particle laminate film according to aspect 8 of the present invention includes a solvent adding step of adding a solvent to the tin oxide particle-containing gel according to any one of aspects 1 to 5 to prepare a tin oxide particle dispersion, and a coating step of coating the obtained tin oxide particle dispersion. As a result, it is possible to form a tin oxide particle laminate film in which the tin oxide particles are uniformly arranged and which has excellent electrical conductivity. Effect of the Invention

[0016] According to the present invention, it is possible to provide a tin oxide particle-containing gel that can be turned into a tin oxide particle dispersion by adding a solvent without going through a dispersion treatment, a method for producing a tin oxide particle dispersion using this tin oxide particle-containing gel, and a method for producing a tin oxide particle laminate film. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic explanatory diagram of a perovskite solar cell including a tin oxide particle laminate film according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a flow diagram showing an example of a method for producing a tin oxide particle-containing gel and a method for producing a tin oxide particle dispersion liquid according to an embodiment of the present invention. [Diagram 3] FIG. 1 is a flow diagram showing an example of a method for producing a tin oxide particle laminate film according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The following describes embodiments of the present invention, including a tin oxide particle-containing gel, a method for producing a tin oxide particle dispersion, and a method for producing a tin oxide particle laminate film, with reference to the accompanying drawings. Note that the following embodiments are specifically described to better understand the gist of the invention, and do not limit the present invention unless otherwise specified.

[0019] The tin oxide particle-containing gel according to an embodiment of the present invention contains a high concentration of tin oxide particles that constitute a tin oxide particle laminate film used, for example, as a conductive layer. A tin oxide particle dispersion liquid is produced by adding a solvent to this tin oxide particle-containing gel. The above-mentioned tin oxide particle laminate film is formed by coating and drying this tin oxide particle dispersion liquid.

[0020] Here, the tin oxide particle laminated film in this embodiment is used, for example, as an electron transport layer of a perovskite solar cell shown in Fig. 1. A perovskite solar cell 10 has a structure in which an ITO film 12, an electron transport layer 13, a perovskite layer 14, a hole transport layer 15, and a back electrode 16 are laminated on the surface of a glass substrate 11, as shown in Fig. 1, for example.

[0021] The tin oxide particle laminated film constituting the electron transport layer 13 has a film thickness within the range of 10 nm to 100 nm. For this reason, it is required that the tin oxide particle dispersion liquid be capable of forming a thin and precise tin oxide particle laminate film, and the tin oxide particle laminate film is required to have excellent electrical conductivity as a conductive material.

[0022] The tin oxide particle-containing gel of this embodiment contains tin oxide particles, and the tin oxide particles are diffused into the solvent by adding a solvent. That is, by adding a solvent, the tin oxide particles contained in the tin oxide particle-containing gel are diffused into the solvent, and a tin oxide particle dispersion is produced. The solvent to be added may be water, a lower alcohol (having a carbon number of 3 or less) such as ethanol, or a mixture thereof. Furthermore, whether or not the tin oxide particles contained in the tin oxide particle-containing gel are dispersed in the solvent when the solvent is added can be determined by particle size distribution measurement and observation with a transmission electron microscope. That is, the particle diameter measured by observation with a transmission electron microscope is defined as the geometric particle diameter, and the particle diameter measured by dynamic light scattering using a particle size distribution measuring device is defined as the hydrodynamic particle diameter, and the presence or absence of dispersion can be determined by the value obtained by dividing the hydrodynamic particle diameter by the geometric particle diameter.

[0023] In addition, since the dispersion state of the tin oxide particles in the tin oxide particle-containing gel changes over time after the addition of the solvent, it is preferable to evaluate the dispersion state of the tin oxide particles after a certain period of time has passed. The time from the addition of the solvent to the evaluation of the dispersion state of the tin oxide particles is not particularly limited, but is preferably within a range of 30 minutes to 1440 minutes. In this embodiment, the time from the addition of the solvent to the evaluation of the dispersion state of the tin oxide particles is set to 120 minutes.

[0024] The tin oxide particle-containing gel of this embodiment preferably contains one or two of primary amines or secondary amines. Here, for example, monomethylamine and 2-aminoethanol can be used as the primary amine, and for example, dimethylamine and diethylamine can be used as the secondary amine.

[0025] In the tin oxide particle-containing gel of this embodiment, the primary particle size of the tin oxide particles is preferably within the range of 1.5 nm or more and 100 nm or less. The primary particle size of the tin oxide particles is more preferably 1.8 nm or more, and even more preferably 2.0 nm or more, and more preferably 50 nm or less, and even more preferably 10 nm or less.

[0026] Furthermore, in the tin oxide particle-containing gel of this embodiment, the content of tin oxide particles is preferably within the range of 25 mass % or more and 65 mass % or less. The content of tin oxide particles in the tin oxide particle-containing gel is more preferably 28 mass% or more, and even more preferably 30 mass% or more.The content of tin oxide particles in the tin oxide particle-containing gel is more preferably 52 mass% or less, and even more preferably 45 mass% or less.

[0027] In the tin oxide particle-containing gel of this embodiment, the tin oxide particles may be doped with a different element other than Sn and O. The content of the different element is preferably within a range of 10,000 massppm to 100,000 massppm. As the different doping elements, it is preferable to use one or more elements selected from antimony, fluorine and phosphorus.

[0028] Next, an example of a method for producing a tin oxide particle-containing gel according to this embodiment and a method for producing a tin oxide particle dispersion will be described with reference to the flow diagram of FIG.

[0029] (Raw material suspension production process S01) An aqueous solution of ammonium bicarbonate is dropped into the aqueous solution of tin chloride and allowed to stand until the foaming subsides to produce a raw material suspension. In this raw suspension producing step S01, the dropping speed is preferably set within the range of 0.2 mL / min to 1.6 mL / min.

[0030] (Tin oxide particle-containing gel generation step S02) Next, the solid matter is removed from the raw material suspension by decantation, and an aqueous amine solution is added to the solid matter and allowed to stand for a predetermined period of time, thereby producing a gel-like material containing tin oxide particles (the tin oxide particle-containing gel of this embodiment). In this tin oxide particle-containing gel generating step S02, the amine concentration in the amine or amine solution to be added is preferably within the range of 20 mass % to 70 mass %.

[0031] (Solvent addition step S03) Next, a solvent is added to the tin oxide particle-containing gel of this embodiment and allowed to stand for a predetermined period of time, whereby the tin oxide particles in the gel diffuse into the solvent, producing a tin oxide particle dispersion liquid.

[0032] Next, an example of a method for producing a tin oxide particle laminated film using a gel containing tin oxide particles will be described with reference to the flow diagram of FIG.

[0033] (Solvent addition step S11) First, a solvent is added to the tin oxide particle-containing gel of this embodiment and the mixture is left for a predetermined period of time to obtain a tin oxide particle dispersion liquid.

[0034] (Solid concentration adjustment step S12) Next, the obtained tin oxide particle dispersion liquid is prepared, and the solid content concentration in the tin oxide particle dispersion liquid is adjusted using ion-exchanged water so as to be within the range of 2 mass % or more and 20 mass % or less. The solid content concentration in the tin oxide particle dispersion liquid is preferably 5 mass% or more, more preferably 8 mass% or more, and is preferably 18 mass% or less, more preferably 15 mass% or less.

[0035] (Coating process S13) Next, the tin oxide particle dispersion liquid with the adjusted solid content concentration is applied onto a substrate by a spin coater. The conditions for the spin coating in the coating step S12 are preferably a rotation speed in the range of 500 rpm to 3000 rpm, a coating time in the range of 5 seconds to 60 seconds, and a thickness of the coating film in the range of 20 nm to 100 nm.

[0036] (Heating process S14) Next, the coating film (the coated tin oxide particle dispersion liquid) is heated to remove the solvent, thereby forming a tin oxide particle laminate film. The heating conditions in this heating step S13 are preferably a heating temperature in the range of 100° C. to 400° C. and a heating time in the range of 1 minute to 10 minutes.

[0037] Through the above-described steps, the tin oxide particle laminate film of this embodiment is formed. Here, in the tin oxide particle laminate film of this embodiment, the average film thickness is in the range of 10 nm to 100 nm, the standard deviation of the film thickness is in the range of 3 nm to 40 nm, and the coefficient of variation of the film thickness CV is 50% or less.

[0038] According to the tin oxide particle-containing gel of the present embodiment configured as described above, by adding a solvent, the tin oxide particles diffuse into the solvent, making it possible to obtain a tin oxide particle dispersion liquid. Therefore, the tin oxide particles can be transported in the form of a tin oxide-containing gel, which reduces transportation costs. In addition, it is not necessary to use a dispersant made of a non-volatile organic compound, and a tin oxide particle laminate film with excellent electrical conductivity can be formed.

[0039] Here, in the case where the tin oxide particle-containing gel of this embodiment contains one or two of primary amines or secondary amines, by adding a solvent such as water or a lower alcohol, it is possible to efficiently disperse the tin oxide particles contained in the tin oxide particle-containing gel in the solvent.

[0040] Furthermore, in the tin oxide particle-containing gel of this embodiment, when the tin oxide particle content is within the range of 25 mass% or more and 65 mass% or less, the tin oxide particles are contained at a high concentration, and transportation costs can be significantly reduced.

[0041] Furthermore, in the tin oxide particle-containing gel of this embodiment, when the primary particle diameter of the tin oxide particles is within the range of 1.5 nm or more and 100 nm or less, a tin oxide particle laminate film with a nano-order thickness can be stably formed.

[0042] Furthermore, in the tin oxide particle-containing gel of this embodiment, when the tin oxide particles are doped with a different element, it is possible to form a tin oxide particle laminate film according to the required characteristics depending on the type and content of the different element to be doped. Here, when the different element is one or more elements selected from antimony, fluorine and phosphorus, it is possible to form a tin oxide particle laminated film having particularly excellent electrical conductivity.

[0043] The method for producing a tin oxide particle dispersion liquid of this embodiment includes a solvent addition step S03 in which a solvent is added to the tin oxide particle-containing gel of this embodiment. This solvent addition step S03 makes it possible to produce a tin oxide particle dispersion liquid in which tin oxide particles are sufficiently dispersed in the solvent.

[0044] The method for producing a tin oxide particle laminate film of the present embodiment includes a solvent adding step S11 of adding a solvent to the tin oxide particle-containing gel of the present embodiment to prepare a tin oxide particle dispersion, and a coating step S13 of coating the obtained tin oxide particle dispersion. As a result, it is possible to form a tin oxide particle laminate film in which the tin oxide particles are uniformly arranged and which has excellent electrical conductivity.

[0045] Although one embodiment of the present invention has been described above, the present invention is not limited to this embodiment, and can be modified as appropriate without departing from the technical concept of the invention. In this embodiment, the tin oxide particle laminated film has been described as constituting the electron transport layer of the perovskite solar cell shown in FIG. 1, but it may be used for other purposes without being limited thereto. EXAMPLES

[0046] A confirmation experiment conducted to confirm the effectiveness of the present invention will be described.

[0047] Tin chloride pentahydrate was dissolved in ion-exchanged water to obtain solution A. Ammonium bicarbonate was dissolved in ion-exchanged water to obtain solution B. Solution B was added dropwise to solution A at a rate of 1 mL / min, and the solution was left to stand until the foaming subsided to obtain a raw suspension. The raw material suspension was decanted to remove the solid content, and an amine or amine solution shown in Table 1 was added to 1 g of this solid content and allowed to stand for 1 hour to obtain a gel containing tin oxide particles.

[0048] In addition, for Inventive Examples 6 to 17, the tin oxide particles were doped with a different element as shown in Table 1 by the procedure described below. Sb-doped: Antimony(III) chloride was added to solution A, and then solution B was added dropwise to solution A. P-doped: Phosphorus trichloride was added to solution A, and then solution B was added dropwise to solution A. F-doped: Tin(IV) fluoride was added to solution A, and then solution B was added dropwise to solution A. Sb,P co-doped: Antimony(III) chloride was added to solution A, followed by phosphorus trichloride, and then solution B was added dropwise to solution A.

[0049] The obtained gel containing tin oxide particles was evaluated as follows.

[0050] (Dispersion state of tin oxide particles after adding solvent) To 0.5 g of the obtained gel containing tin oxide particles, ion-exchanged water was added as a solvent in such an amount that the tin oxide concentration after addition would be 8 mass %. Then, a transmission electron microscope (JEOL Ltd., model name: JEM-2010F) was used to take an image at a magnification of 200,000 times. The particle diameters of 100 particles were measured from the image taken using software (product name: Image J), ​​and the average was calculated. The particle diameter thus measured was taken as the geometric particle diameter. In addition, the gel containing tin oxide particles to which the solvent had been added was diluted to 0.5 mass% with the same solvent as the dispersion medium, and then the pH was adjusted to 8.0 with 1 mol / L aqueous sodium hydroxide solution or 1 mol / L hydrochloric acid. The number distribution of particle diameters was measured by dynamic light scattering using a particle size distribution measuring device (Malvern Zetasizer nano). The average value was calculated from the number distribution to obtain the hydrodynamic particle size value. Particles with a value of 2.5 or less obtained by dividing the hydrodynamic particle diameter by the geometric particle diameter were determined to be dispersed.

[0051] (Primary particle size of tin oxide particles) The tin oxide particles contained in the tin oxide particle-containing gel were photographed at a magnification of 200,000 times using a transmission electron microscope (JEOL Ltd., model name: JEM-2010F). The particle diameters of 100 particles were measured from the photographed image using software (product name: Image J), ​​and the average was calculated.

[0052] (Tin oxide particle content) 1 g of the gel containing tin oxide particles was placed on an aluminum dish and heated for 2 hours in a 200°C air dryer. The weight change before and after heating was divided by the weight of the gel containing tin oxide particles to calculate the volatile content (%) of the gel containing tin oxide particles. The content of tin oxide particles was then calculated using the following formula. Tin oxide particle content (%) = 100 - volatile content (%)

[0053] (Conductivity of tin oxide particle laminated film) The above-mentioned tin oxide particle dispersion liquid was diluted with ion-exchanged water to a solid content concentration of 8 mass %. The diluted tin oxide particle dispersion liquid was spin-coated on a 50 mm×50 mm glass substrate using a spin coater (Mikasa Co., Ltd., model number: MS-A150) at 500 rpm for 60 seconds to form a coating film. The glass substrate on which the coating film was formed was heated on a hot plate at 100° C. for 3 minutes to form a tin oxide particle laminate film. The resistance of the tin oxide particle laminated film obtained as described above was measured using a surface resistance measuring device (product number: Loresta AP MCP-T400, probe: ASP probe (four-needle), manufactured by Mitsubishi Chemical Corporation).

[0054] [Table 1]

[0055] In Comparative Examples 1 and 2, even when a solvent was added, the tin oxide particles in the gel did not diffuse into the solvent, and a tin oxide particle dispersion liquid could not be formed. Therefore, coating was not possible, and a tin oxide particle laminate film could not be formed. In contrast, in Examples 1 to 10 of the present invention, the tin oxide particles in the gel were dispersed in the solvent by adding a solvent, and a tin oxide particle dispersion liquid was formed. This tin oxide particle dispersion liquid was applied to form a tin oxide particle laminate film.

[0056] As described above, it has been confirmed that the present invention can provide a tin oxide particle-containing gel that can be turned into a tin oxide particle dispersion by adding a solvent without going through a dispersion treatment, a method for producing a tin oxide particle dispersion using this tin oxide particle-containing gel, and a method for producing a tin oxide particle laminate film.

Claims

1. A tin oxide particle-containing gel comprising tin oxide particles, the tin oxide particles being dispersed in a solvent by the addition of the solvent, to form a tin oxide dispersion.

2. The tin oxide particle-containing gel according to claim 1, characterized in that it contains one or two of primary amines or secondary amines.

3. 2. The tin oxide particle-containing gel according to claim 1, wherein the content of the tin oxide particles is within the range of 25 mass % or more and 65 mass % or less.

4. 2. The gel containing tin oxide particles according to claim 1, wherein the primary particle diameter of the tin oxide particles is within a range of 1.5 nm or more and 100 nm or less.

5. 2. The gel containing tin oxide particles according to claim 1, wherein the tin oxide particles are doped with a different element.

6. 6. The gel containing tin oxide particles according to claim 5, wherein the different element is one or more elements selected from the group consisting of antimony, fluorine and phosphorus.

7. A method for producing a tin oxide particle dispersion liquid, comprising the steps of: A method for producing a tin oxide particle dispersion liquid, comprising: a solvent addition step of adding a solvent to the tin oxide particle-containing gel according to claim 1 .

8. A method for producing a tin oxide particle laminate film, comprising the steps of:

6. A method for producing a tin oxide particle laminate film, comprising: a solvent adding step of adding a solvent to the tin oxide particle-containing gel according to claim 1 to prepare a tin oxide particle dispersion; and a coating step of coating the obtained tin oxide particle dispersion.

Citation Information

Patent Citations

  • Abrasive and abrasion

    JP2000007334A

  • Preparation and use of tin (IV) oxide dispersion

    US4946820A

  • Spin coating

    JP1989027667A