Conjugate type nonwoven fabric and conjugate type nonwoven fabric manufacturing method
A composite nonwoven fabric with optimized basis weight, thickness, and fiber ratios ensures both wet tensile strength and softness, improving wiping performance and reducing fiber shedding.
Patent Information
- Application Number
- JP2023073685
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Conventional composite nonwoven fabrics made of pulp and spunbond nonwoven fabrics are often hard and lack softness, leading to reduced strength during wet wiping and fiber shedding during hydroentanglement.
A composite nonwoven fabric with specific basis weight, thickness, and ratio of spunbond nonwoven fabric to pulp fiber web, along with enhanced elongation and cantilever values, ensuring both wet tensile strength and softness.
The composite nonwoven fabric maintains tensile strength when wet and provides excellent softness to the touch, addressing the issues of hardness and fiber shedding.
Smart Images

Figure 2024158464000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite nonwoven fabric and a method for producing the same. [Background technology]
[0002] Paper wipers and nonwoven fabric wipers are well known as wipers for wiping off water and dirt.
[0003] However, in recent years, wipers made of so-called composite nonwoven fabrics, in which pulp fibers and synthetic fibers are laminated or mixed, have also been sold.
[0004] The characteristics of the composite nonwoven fabrics used in wipers include absorbency, usability (wiping comfort, volume in the hand), durability (strength), and low fiber shedding.
[0005] In addition, one method for producing composite nonwoven fabrics is to hydroentangle a spunbond nonwoven fabric made from pulp fibers, which have excellent absorbency for water-based and oil-based liquids, and synthetic fibers, which have excellent strength, to produce a sheet that combines strength and absorbency. In this case, the pulp fiber web can be supplied by a general wet papermaking method or dry airlaid, or can be supplied as a sheet produced by wet papermaking.
[0006] As a prior art document on such composite nonwoven fabrics, for example, Patent Document 1 describes a composite nonwoven fabric wiper in which a pulp fiber web is laminated and integrated onto a spunbond nonwoven fabric, the spunbond nonwoven fabric being formed to include a plurality of fusion points that connect spun resin fibers, and the area of each of the fusion points is 0.10 to 0.50 mm 2 and the area ratio of the fusion points is set to 7 to 20%, and the basis weight of the pulp fiber web is 30 to 70 g / m 2 A composite nonwoven fabric wiper is disclosed, characterized in that [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2020-051010 A Summary of the Invention [Problem to be solved by the invention]
[0008] Conventional composite nonwoven fabrics made of pulp and spunbonded nonwoven fabrics tend to be too stiff when used for wiping people, and there is a demand for improved softness (hand feel).
[0009] However, although the softness of the sheet is improved by reducing the blending ratio of the spunbond nonwoven fabric, the strength during wiping is reduced, which often causes problems in wiping, especially when the sheet is wet. In addition, there is a problem that the pulp fibers are more likely to fall off during water current entanglement, which deteriorates the operability.
[0010] The present invention has been made in consideration of the above circumstances, and has an object to provide a composite nonwoven fabric that maintains its tensile strength when wet and also has excellent softness to the touch, and a method for producing the composite nonwoven fabric. [Means for solving the problem]
[0011] The inventors have conducted extensive research and have found that in a composite nonwoven fabric formed by laminating and integrating a pulp fiber web onto a polypropylene spunbond nonwoven fabric, by setting both the basis weight and thickness of the composite nonwoven fabric within prescribed numerical ranges, and also setting both the ratio of the basis weight of the spunbond nonwoven fabric to the basis weight of the composite nonwoven fabric and the value obtained by dividing the cantilever value in the MD direction of the composite nonwoven fabric by the basis weight of the composite nonwoven fabric within prescribed numerical ranges, it is possible to obtain a composite nonwoven fabric that maintains its tensile strength when wet and is also excellent in softness to the touch, thereby completing the present invention. That is, the present invention provides the following.
[0012] (1) The first aspect of the present invention is a composite nonwoven fabric obtained by laminating and integrating a pulp fiber web onto a polypropylene spunbond nonwoven fabric, and the composite nonwoven fabric has a basis weight of 45 g / m 2 More than 150g / m 2 The thickness is 0.35 mm or more and 1.00 mm or less, the ratio of the basis weight of the spunbond nonwoven fabric to the basis weight of the composite nonwoven fabric is 17% or more and 26% or less, and the cantilever value (mm) in the MD direction of the composite nonwoven fabric is expressed as the basis weight (g / m 2 ) is less than 0.80.
[0013] (2) A second aspect of the present invention is the composite nonwoven fabric according to (1), characterized in that the spunbond nonwoven fabric alone has a breaking elongation in the MD direction of 65% or more.
[0014] (3) The third aspect of the present invention is the composite nonwoven fabric according to (1), wherein the wet tensile strength (WMDT) (gf / 25 mm) of the composite nonwoven fabric according to JIS P 8135 is calculated by multiplying the basis weight (g / m 2 ) is 29 or more.
[0015] (4) A fourth aspect of the present invention is the composite nonwoven fabric according to (1), characterized in that the wet tensile strength (WMDT) of the composite nonwoven fabric in MD according to JIS P 8135 is 1900 gf / 25 mm or more.
[0016] (5) A fifth aspect of the present invention is the composite nonwoven fabric according to (1), characterized in that the cantilever value in the MD direction of the composite nonwoven fabric is less than 75.0 mm.
[0017] (6) The sixth aspect of the present invention is a method for producing a composite nonwoven fabric, comprising laminating and integrating a pulp fiber web onto a polypropylene spunbond nonwoven fabric, the spunbond nonwoven fabric having a MD breaking elongation of 65% or more, and a basis weight of the composite nonwoven fabric of 45 g / m 2More than 150g / m 2 The following is a method for producing a composite nonwoven fabric, characterized in that the thickness is 0.35 mm or more and 1.00 mm or less, and the ratio of the basis weight of the spunbond nonwoven fabric to the basis weight of the composite nonwoven fabric is 17% or more and 26% or less. Effect of the Invention
[0018] According to the present invention, it is possible to provide a composite nonwoven fabric that maintains its tensile strength when wet and also has an excellent softness to the touch, and a method for producing the composite nonwoven fabric. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.
[0020] <Composite nonwoven fabric> The composite nonwoven fabric according to this embodiment is formed by laminating and integrating a pulp fiber web onto a spunbonded nonwoven fabric made of polypropylene. The method for integrating the spunbond nonwoven fabric and the pulp fiber web will be described later.
[0021] Spunbond nonwoven fabrics are made of polypropylene and contain primarily polypropylene fibers, but may also contain one or more synthetic fibers selected from the group consisting of nylon, vinylon, polyester, acrylic, polyethylene, and polystyrene.
[0022] The pulp fiber web preferably comprises one or more bleached softwood kraft pulp (NBKP) fibers selected from the group consisting of radiata pine, slash pine, southern pine, lodgepole pine, spruce, and Douglas fir. In addition to softwood bleached kraft pulp (NBKP), general pulp fibers such as hardwood bleached kraft pulp (LBKP) may also be included, but it is preferable to include softwood bleached kraft pulp (NBKP) and hardwood bleached kraft pulp (LBKP). The content ratio of NBKP and LBKP in the pulp fibers is preferably 50:50 or more and 100:0 or less, more preferably 70:30 or more and 100:0 or less, even more preferably 90:10 or more and 100:0 or less, and most preferably 100:0.
[0023] The basis weight of the composite nonwoven fabric is 45g / m 2 More than 150g / m 2 By setting the basis weight within the above range, a composite nonwoven fabric can be obtained that maintains its tensile strength in a wet state and also has excellent softness to the touch. The basis weight of the composite nonwoven fabric is 50 g / m 2 More than 130g / m 2 It is preferable that the thickness is 55 g / m or less. 2 More than 100g / m 2 It is more preferable that: Basis weight is measured in accordance with JIS P 8124.
[0024] In addition, the ratio of the basis weight of the spunbond nonwoven fabric (before integration) to the basis weight of the composite nonwoven fabric is 17% or more and 26% or less. By setting the ratio within the above numerical range, it is possible to obtain a composite nonwoven fabric that maintains its tensile strength when wet and also has excellent softness to the touch. The ratio of the basis weight of the spunbond nonwoven fabric (before integration) to the basis weight of the composite nonwoven fabric is preferably 18% or more and 24% or less. The ratio is calculated by: basis weight of spunbond nonwoven fabric ÷ basis weight of composite nonwoven fabric × 100 (%).
[0025] The thickness of the composite nonwoven fabric is 0.35 mm or more and 1.00 mm or less. By setting the thickness of the composite nonwoven fabric within the above numerical range, it is possible to obtain a composite nonwoven fabric that maintains its tensile strength when wet and also has excellent softness to the touch. In this case, the thickness refers to the thickness of the composite nonwoven fabric in the state of one ply. The thickness of the composite nonwoven fabric is preferably 0.42 mm or more and 0.90 mm or less. The thickness is measured using a Peacock paper thickness gauge at 37.85 gf / cm 2 The measurement is performed under a pressure of 100 MPa.
[0026] The composite nonwoven fabric preferably has a wet tensile strength in the MD direction (WMDT) of 1900 gf / 25 mm or more based on JIS P 8135. When the WMDT is within the above range, the composite nonwoven fabric has excellent wet tensile strength. In this case, the MD direction means the manufacturing direction (also called the machine direction or machine direction) during the manufacture of the composite nonwoven fabric, and the CD direction means the direction perpendicular to the MD direction (also called the width direction or transverse direction). The tensile strength in the wet MD direction (WMDT) is more preferably 2000 gf / 25 mm or more and 6000 gf / 25 mm or less. The tensile strength is measured using a tensile tester after immersing a 25 mm wide test piece cut from the composite nonwoven fabric in water for 1 second or more, leaving it on a sheet with sufficient water absorption for about 3 seconds to drain the water. The measurement conditions are a chuck distance of 100 mm, a tensile speed of 300 mm / min, and an average value of 4 measurements (n=4).
[0027] In addition, the wet tensile strength (WMDT) (gf / 25mm) of the composite nonwoven fabric based on JIS P 8135 was calculated based on the basis weight (g / m 2 ) is preferably at least 29. If the value is less than 29, the composite nonwoven fabric will have poor tensile strength in a wet state. The wet tensile strength (WMDT) (gf / 25mm) of the composite nonwoven fabric in the MD direction based on JIS P 8135 was calculated based on the basis weight (g / m 2 ) is more preferably 32 or more and 100 or less.
[0028] The cantilever value in the MD direction of the composite nonwoven fabric is preferably less than 75.0 mm. If the cantilever value is 75.0 mm or more, the composite nonwoven fabric will be inferior in softness to the touch. The cantilever value in the MD direction of the composite nonwoven fabric is more preferably 30.0 mm or more and 60.0 mm or less.
[0029] The cantilever value in the CD direction of the composite nonwoven fabric is preferably less than 32.0 mm. If the cantilever value is 32.0 mm or more, the composite nonwoven fabric will be inferior in softness to the touch. The cantilever value in the CD direction of the composite nonwoven fabric is more preferably 20.0 mm or more and 30.0 mm or less. The cantilever values in each direction are measured on the front and back of samples (n=7 each) cut from the composite nonwoven fabric according to the JIS L 1096 cantilever method, and the average is calculated. Measurements are also performed in both the MD direction (machine direction) and the CD direction (horizontal direction).
[0030] Furthermore, the cantilever value (mm) in the MD direction of the composite nonwoven fabric was calculated based on the basis weight (g / m 2 ) is less than 0.80. If the value is 0.80 or more, the composite nonwoven fabric will have poor tensile strength in a wet state and poor softness to the touch. The cantilever value (mm) in the MD direction of the composite nonwoven fabric was calculated based on the basis weight (g / m 2 ) is preferably 0.20 or more and 0.78 or less.
[0031] Furthermore, the cantilever value (mm) in the CD direction of the composite nonwoven fabric was calculated based on the basis weight (g / m 2 ) is preferably less than 0.80. If the value is 0.80 or more, the composite nonwoven fabric will have poor tensile strength in a wet state and poor softness to the touch. The cantilever value (mm) in the CD direction of the composite nonwoven fabric is expressed as the basis weight (g / m 2 ) is more preferably 0.15 or more and 0.50 or less.
[0032] The spunbond nonwoven fabric itself preferably has a breaking elongation in the MD direction of 65% or more. If the breaking elongation is less than 65%, the composite nonwoven fabric will have poor tensile strength in a wet state. The breaking elongation in the MD direction of the spunbond nonwoven fabric alone is more preferably 68% to 100%, and even more preferably 72% to 90%. If the breaking elongation exceeds 100%, the strength of the composite nonwoven fabric decreases and the wiping properties become poor. The breaking elongation is measured using a tensile tester with a test piece width of 25 mm cut out from the composite nonwoven fabric. The measurement conditions are a chuck distance of 100 mm, a tensile speed of 300 mm / min, and n=4.
[0033] <Method of manufacturing composite nonwoven fabric> The method for producing the composite nonwoven fabric according to the present embodiment is not particularly limited, and the composite nonwoven fabric can be produced by any known method for producing a composite nonwoven fabric. In the manufacturing method of such a composite nonwoven fabric, the method of laminating and integrating the pulp fiber web on the polypropylene spunbond nonwoven fabric may be a general method such as a spunlace method, but from the viewpoint of water absorption performance and abrasion resistance, hydroentanglement is preferable. The integration process by hydroentanglement is described in detail in, for example, Japanese Patent No. 6758116. EXAMPLES
[0034] The present invention will be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples in any way.
[0035] Composite nonwoven fabrics of Examples 1 to 3 and Comparative Examples 1 to 4 were produced under the conditions shown in Table 1, and the following evaluations were carried out. Measurements of each parameter other than the following evaluations were carried out according to the standards or measurement methods described above. All measurements according to the standards or measurement methods described above were carried out indoors at a temperature of 23°C and a humidity of 50% RH.
[0036] (Sheet softness) The sheet softness of the composite nonwoven fabric was evaluated using the cantilever value in the MD direction and the cantilever value in the MD direction / basis weight. The measured basis weight and cantilever value in the MD direction of the composite nonwoven fabric were evaluated according to the following criteria. 1: Cantilever value in MD direction / grammage is 0.80 or more 2: The cantilever value in the MD direction / grammage is less than 0.80 and the cantilever value in the MD direction is 75.0 mm or more 3: MD cantilever value / grammage is less than 0.80 and MD cantilever value is less than 75.0 mm
[0037] (Wet tensile strength) The wet tensile strength of the composite nonwoven fabric was evaluated using WMDT and WMDT / basis weight. The measured basis weight and WMDT values of the composite nonwoven fabric were evaluated according to the following criteria. 1:WMDT / grammage less than 31 2: WMDT / grammage is 31 or more and WMDT is less than 2000gf / 25mm 3: WMDT / grammage is 31 or more and WMDT is 2000gf / 25mm or more
[0038] The conditions and evaluation results for each Example and Comparative Example are shown in Table 1. In addition, a sample was deemed to pass when all evaluations were scored as "2" or higher.
[0039] [Table 1]
[0040] From the above, it was confirmed that this example provides a composite nonwoven fabric that maintains its tensile strength when wet and also has an excellent softness to the touch.
Claims
1. A composite nonwoven fabric in which a pulp fiber web is laminated and integrated onto a polypropylene spunbond nonwoven fabric, The basis weight of the composite nonwoven fabric is 45 g / m 2 150g / m or more 2 The thickness is 0.35 mm or more and 1.00 mm or less, The ratio of the basis weight of the spunbond nonwoven fabric to the basis weight of the composite nonwoven fabric is 17% or more and 26% or less; The cantilever value (mm) in the MD direction of the composite nonwoven fabric was calculated based on the basis weight (g / m 2 ) is less than 0.
80.
2. 2. The composite nonwoven fabric according to claim 1, wherein the spunbond nonwoven fabric itself has a breaking elongation in the MD direction of 65% or more.
3. The wet tensile strength (WMDT) (gf / 25 mm) of the composite nonwoven fabric in the MD direction based on JIS P 8135 was calculated based on the basis weight (g / m 2 2. The composite nonwoven fabric according to claim 1, wherein the value obtained by dividing the elastic modulus by the elastic modulus is 29 or more.
4. 2. The composite nonwoven fabric according to claim 1, wherein the composite nonwoven fabric has a wet tensile strength (WMDT) in the machine direction of 1900 gf / 25 mm or more according to JIS P 8135.
5. 2. The composite nonwoven fabric according to claim 1, wherein the cantilever value in the MD direction of the composite nonwoven fabric is less than 75.0 mm.
6. A method for producing a composite nonwoven fabric, comprising laminating and integrating a pulp fiber web onto a spunbonded nonwoven fabric made of polypropylene, The spunbond nonwoven fabric has a breaking elongation in the MD direction of 65% or more; The basis weight of the composite nonwoven fabric is 45 g / m 2 150g / m or more 2 The thickness is 0.35 mm or more and 1.00 mm or less, A method for producing a composite nonwoven fabric, characterized in that the ratio of the basis weight of the spunbonded nonwoven fabric to the basis weight of the composite nonwoven fabric is 17% or more and 26% or less.
Citation Information
Patent Citations
Complex nonwoven fabric wiper and manufacturing method thereof
JP2020051010A