Method of recovering resin film

A method for recovering single resin films from mixed laminates by applying heat and pressure to reduce adhesive strength and peel off layers addresses the inefficiencies of existing methods, achieving efficient and environmentally friendly resin recovery.

JP2024158580APending Publication Date: 2024-11-08GUNZE LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023073891
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The challenge of efficiently recovering single resin materials from mixed resin films without requiring large-scale equipment and minimizing environmental impact, particularly for polyolefin resins like polypropylene and polyethylene, is not adequately addressed by existing methods.

Method used

A method involving laminating compatible resin film layers with an adhesive layer, applying heat and pressure to reduce adhesive strength, and peeling off the layers to recover individual resin films without melting, using simple equipment and without solvents.

Benefits of technology

Enables the recovery of multiple resin materials as single materials, reducing the need for virgin raw materials and minimizing quality deterioration, while avoiding environmental effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158580000001_ABST
    Figure 2024158580000001_ABST
Patent Text Reader

Abstract

To provide a method capable of individually recovering a plurality of resin materials as a single resin material obviating the need of large-scale equipment or without melting as a prerequisite for separation.SOLUTION: The present invention comprises: a first step of preparing a composite material formed by laminating a first resin film layer and a second resin film layer at least having compatibility; a second step of applying heat and pressure to the composite material to decrease bonding strength of an interface between the first resin film layer and the second resin film layer; and a third step of separating between the first resin film layer and the second resin film layer to individually recover the first resin film layer and the second resin film layer.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for recovering a resin film. [Background technology]

[0002] Although the production volume of polyolefin (PO) resins, such as polypropylene (PP) and polyethylene (PE), accounts for half of the total plastic production in the market, recycling of these resins has not progressed as much as that of PET resins. In particular, PO resins, which are a mixture of PE and PP, are the main recovered material from plastic container packaging, but due to quality constraints, cascade recycling is the norm, and securing stable demand through quality improvements such as by converting them to a single resin is a challenge. In particular, in films for certain industrial applications that require high performance and quality, the inclusion of even PO resins significantly reduces their performance and quality.

[0003] Therefore, it is necessary to provide a film with improved recyclability that can recover each individual resin from a laminated film. For example, as described in Patent Document 1, there is a method of recovering a single resin by dissolving a specific resin from a mixture containing multiple resins. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2021-160281 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the method of efficiently recovering a single resin using a resin dissolving solution requires large-scale equipment, and the dissolving solution may have an impact on the natural environment. Note that this problem is not limited to the recovery of PP and PE, but may also occur when recovering other resin materials.

[0006] The present invention has been made to solve the above-mentioned problems, and aims to provide a method capable of recovering multiple resin materials as single resin materials without requiring large-scale equipment or melting them as a prerequisite for separation. [Means for solving the problem]

[0007] Item 1. A first step of preparing a composite material in which at least a first resin film layer and a second resin film layer having compatibility are laminated; a second step of applying heat and pressure to the composite material to reduce adhesive strength at the interface between the first resin film layer and the second resin film layer; a third step of peeling the first resin film layer and the second resin film layer and recovering the first resin film layer and the second resin film layer; The method for recovering a resin film comprises:

[0008] Item 2. A first step of preparing a composite material in which at least a first resin film layer and a second resin film layer are laminated via an adhesive layer, and the adhesive layer and the first resin film layer and / or the adhesive layer and the second resin film layer are compatible with each other; a second step of applying heat and pressure to the composite material to reduce adhesive strength at an interface between the adhesive layer and the first resin film layer and / or an interface between the adhesive layer and the second resin film layer; a third step of peeling the first resin film layer and the second resin film layer and recovering the first resin film layer and the second resin film layer; The method for recovering a resin film comprises:

[0009] Item 3. The first resin film layer contains a polyethylene resin, Item 3. The method for recovering a resin film according to item 1 or 2, wherein the second resin film layer contains a polypropylene-based resin.

[0010] Item 4. The method for recovering a resin film according to item 1 or 2, wherein in the second step, the adhesive strength of the peeled interface is 2.0 N / cm or less.

[0011] Item 5. The method for recovering a resin film according to Item 4, wherein a temperature of 100° C. or more and a pressure of 0.5 MPa or more are applied in the third step.

[0012] Item 6. In the first step, a first roll on which the composite material is wound is prepared, In the second step, the composite material unwound from the first roll is passed between a pair of rollers to apply heat and pressure to the composite material; 3. The method for recovering a resin film according to item 1 or 2, wherein in the third step, the peeled first resin film layer and the peeled second resin film layer are recovered by winding them up on rolls.

[0013] Item 7. A step of recovering the first resin film layer and the second resin film layer by the method for recovering a resin material according to item 1 or 2; producing the composite material using at least one of the first resin film layer and the second resin film layer that have been recovered; A method for producing a composite material, comprising: Effect of the Invention

[0014] According to the present invention, a plurality of resin materials can be recovered as single resin materials without requiring large-scale equipment or melting as a prerequisite for separation. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a target composite material. [Diagram 2] FIG. 1 is a cross-sectional view showing an example of a target composite material. [Diagram 3] FIG. 1 is a schematic diagram showing an example of equipment for recovering a resin film from a composite material. [Figure 4]1 is a graph showing the relationship between the temperature, pressure, and time applied in Example 1 and the adhesive strength. [Diagram 5] 1 is a graph showing the relationship between the temperature, pressure, and time applied in Example 2 and the adhesive strength. [Figure 6] 1 is a graph showing the relationship between the temperature, pressure, and time applied in Example 3 and the adhesive strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, one embodiment of the method for recovering resin films according to the present invention will be described. This embodiment is a method for recovering resin films after peeling them from a sheet-like composite material in which multiple resin films are laminated. First, the target film will be described, and then the separation method will be described.

[0017] <1. Examples of composite materials> There are various types of composite materials that are the subject of this embodiment, but (1) a composite material laminated by adhering compatible resin films together, or (2) a composite material in which at least one of the resin films and the adhesive are compatible when laminating two resin films by adhering them together. That is, a composite material having at least one interface bonded by compatibility rather than a covalent bond between the resin films or the interface between the adhesive layer and the resin film. In such a composite material, the resin film is recovered by peeling off this interface using a method described later. The number of resin films to be laminated is not particularly limited, and for example, a resin film of another type may be adhered to both sides of the resin film. In this case, the number of peelable interfaces is two. The composite material may also include both (1) and (2).

[0018] For example, as shown in FIG. 1, a composite material 10 can be mentioned in which a second resin film layer 2 is laminated on both sides of a first resin film layer 1. In this example, the first resin film layer 1 and the second resin film layer 2 are bonded to each other by melting them. Also, as shown in FIG. 2, a composite material 20 can be mentioned in which a second resin film layer 2 is bonded to both sides of a first resin film layer 1 via an adhesive layer 3. In this example, the first resin film layer 1 and the adhesive layer 3 are bonded to each other by melting them. Note that these are examples of composite materials, and they may include those in which three or more types of resin films are laminated, or those in which the interfaces of some of the resin films are bonded by covalent bonds, and it is sufficient that at least a part of them has a peelable interface as described above.

[0019] Examples of compatible resin materials include polyolefin resins such as polyethylene resin and polypropylene resin. Also, for example, an adhesive containing a polyethylene resin and a polypropylene resin, or an adhesive containing a polypropylene resin and a polyethylene resin, are also compatible. Since polypropylene resin and polyethylene resin have similar specific gravities, separation is difficult using a method that utilizes the difference in specific gravities. In other words, this method is suitable for separating composite materials of resins with similar specific gravities.

[0020] Examples of the polyethylene resin include branched low-density polyethylene resin, linear low-density polyethylene resin, ethylene-vinyl acetate copolymer, ionomer resin, and mixtures thereof. Also, examples of the polyethylene resin include copolymers of ethylene and α-olefins. Examples of the α-olefins include 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, and 1-octene.

[0021] Examples of polypropylene-based resins include binary or ternary random copolymers or block copolymers with polypropylene as the main component and ethylene, butene, or α-olefin as the copolymerization components, and block or graft copolymers containing a rubber component. Specifically, the α-olefin is preferably made of ethylene, 1-butene, 1-hexene, 1-octene, etc., and may contain two or more types of α-olefins. The propylene-based resin may be a mixture of different propylene-α-olefin random copolymers. The propylene-based resin may also be an elastomeric olefin-based elastomer having a sea-island structure in which a copolymer rubber of propylene and ethylene is finely dispersed in the polypropylene-based resin (matrix phase).

[0022] The thickness of each resin film constituting the composite material is not particularly limited. For example, The thickness of the adhesive is preferably 70 to 250 μm, and more preferably 80 to 210 μm. The thickness of the adhesive is, for example, preferably 4 to 15 μm, and more preferably 6 to 11 μm.

[0023] <2. Recovery of resin film from composite materials> Next, recovery of the resin film from the composite material will be described. First, the above-mentioned composite material is prepared, and heat and pressure are applied to it. This reduces the adhesive strength of the above-mentioned peelable interface. The reduced adhesive strength is, for example, preferably 2.0 N / cm or less, more preferably 1.5 N / cm or less, even more preferably 1.0 N / cm or less, and particularly preferably 0.5 N / cm or less. In order to reduce the adhesive strength in this way, heat and pressure are applied to the composite material for a predetermined time. The adhesive strength can be measured as follows.

[0024] The resin film to which heat and pressure had been applied for a certain period of time was cut to a size of 100 mm x 10 mm so that the MD direction of the resin film was the long side, and a portion of the film edge was delaminated. The strength (N / 10 mm) when the resin film was peeled in the 180 degree direction at a pulling speed of 100 mm / min in the long side direction was measured using an Imada digital force gauge ZTS-100N. The test was performed three times to calculate the average adhesive strength.

[0025] The temperature applied is preferably equal to or higher than the softening point of at least one of the bonded resin films (or adhesive layers). However, the temperature does not have to be strictly equal to or higher than the softening point, and is preferably equal to or higher than a temperature 15°C lower than the softening point, more preferably equal to or higher than a temperature 10°C lower than the softening point, and even more preferably equal to or higher than a temperature 5°C lower than the softening point. To peel off the above-mentioned polyethylene-based resin and polypropylene-based resin, for example, the temperature is preferably equal to or higher than 80°C, more preferably equal to or higher than 100°C, and even more preferably equal to or higher than 150°C. However, in order to prevent damage to the resin film, the temperature applied is preferably equal to or lower than 170°C.

[0026] The pressure applied is, for example, preferably 0.3 MPa or more, more preferably 0.5 MPa or more, and particularly preferably 1.0 MPa or more, but in order to prevent the resin film from being damaged, the pressure applied is preferably 1.5 MPa or less.

[0027] The time for applying the above-mentioned temperature and pressure is not particularly limited, but it is sufficient that the adhesive strength of the peeled interface is equal to or less than the above-mentioned adhesive strength. For example, 0.2 seconds or more is preferable, 0.5 seconds or more is more preferable, and 1.0 second or more is even more preferable. In order to obtain the above-mentioned adhesive strength, the applied temperature, pressure, and time can be appropriately changed.

[0028] In this way, when the adhesive strength of the interface to be peeled off is reduced, the resin films sandwiching the interface are peeled off and collected. When the interface between the resin film and the adhesive layer is peeled off, for example, in the example of Fig. 2, the adhesive layer 3 is collected while still adhered to the second resin film layer 2. However, if the adhesive layer 3 is made of substantially the same material as the second resin film layer, the collected adhesive layer 3 and the second resin material are made of substantially the same material.

[0029] The above steps can be carried out, for example, in equipment as shown in FIG. 3. In the example shown in FIG. 3, a first roll 4 on which the composite material 10 shown in FIG. 1 is wound is prepared, and the composite material 10 is unwound from the first roll 4. The unwound composite material 10 is then passed between a pair of rollers 5. These rollers 5 are for applying temperature and pressure. For example, at least one of the rollers 5 is configured to be heatable. In addition, the pair of rollers 5 are configured to press against each other, and are configured to apply pressure to the composite material 10 passing between the rollers 5.

[0030] As described above, the adhesive strength of the interface where the composite material 10 is peeled off is reduced by passing the composite material 10 between these rollers 5. Thereafter, the resin films 1, 2 are peeled off at the interface where the adhesive strength has been reduced, and each of the resin films 1, 2 is wound up and collected by collection rollers 7-9.

[0031] <3. Features> According to the above-mentioned method for recovering a resin film, in a composite material, the adhesive strength is reduced by remelting the interface that has been bonded by melting, and then the resin film is peeled off and recovered. Therefore, a resin film made of a single material can be recovered from the composite material. This reduces the amount of virgin raw material used, making it possible to recycle resources. Note that the single material does not have to be a completely single material, and may be a mixture of the same type of material, for example, a polyethylene-based resin and a polypropylene-based resin. Since the recovered resin film can be reused as a raw material for each layer of the composite material, it is possible to reduce the inclusion of different resins originating from other layers, and to minimize deterioration in quality and changes in film properties. In other words, the recovered resin film can be used for the layers that constitute the resin film.

[0032] In addition, the above-mentioned recovery method does not require special equipment, and can be achieved by simply applying heat and pressure to the composite material. In addition, since no solvent is used, it is possible to prevent any adverse effect on the environment.

[0033] When the polyethylene-based resin and polypropylene-based resin recovered from the composite material as described above are reused as a composite material, 5 to 100% by weight, more preferably 10 to 90% by weight, and even more preferably 20 to 80% by weight of the materials constituting the composite material can be composed of the recovered polyethylene-based resin and polypropylene-based resin. The present inventors have confirmed that this allows the composite material to have physical properties equivalent to those of a composite material using virgin materials. EXAMPLES

[0034] The resin film recovery method and the reuse of the recovered resin film according to the embodiments of the present invention will be described in detail below, but the present invention is not limited to these embodiments.

[0035] A. How to collect resin film <1. Target composite materials> First, as shown in Tables 1 and 2, three types of composite materials (Examples 1 to 3) were prepared as targets of the recovery method of the present invention. Examples 1 and 2 have the configuration shown in FIG. 1, and Example 3 has the configuration shown in FIG. 2. The layer configurations and physical property values ​​of each Example are as follows. The units of the configuration of each resin are % by weight. Table 2 also includes Examples 4 and 5, and a comparative example, which will be described later. [Table 1] [Table 2]

[0036] The materials of the resin films and adhesive layers constituting each composite material are as follows: [Table 3]

[0037] Heat and pressure were applied to the above Examples 1 to 3 for a predetermined period of time. As a result, the adhesive strength decreased as shown in Table 4. The adhesive strength measured here is the adhesive strength at the interface between the intermediate layer (first resin film layer) and the surface layer (second resin film layer) in Examples 1 and 2, and the adhesive strength at the interface between the adhesive layer and the intermediate layer in Example 3. The adhesive strength was measured as described in the above embodiment. [Table 4] The unit is N / cm.

[0038] 4 to 6 are graphs showing the relationship between the temperature, pressure, and time applied to Examples 1 to 3, respectively, and the adhesive strength. The values ​​before treatment are set to values ​​at 0°C for convenience. According to these graphs, it was found that the adhesive strength decreases with increasing pressure and time. Also, the adhesive strength decreases with increasing temperature, but the decrease in adhesive strength becomes gradual at 100°C or higher. Comparing Examples 1 to 3, it was found that Example 3 using an adhesive layer has a high initial adhesive strength, and therefore by setting the temperature to 150°C or higher, the adhesive strength can be decreased to the same extent as when a temperature of 100°C is applied to Examples 1 and 2. However, the present inventors have confirmed that if the adhesive strength after treatment is 2.0 N / cm or less, there is no problem with recovery.

[0039] Thereafter, the surface layer and the intermediate layer sandwiching the interface with the reduced adhesive strength were peeled off and collected. In Example 3, the adhesive layer and the intermediate layer were peeled off at the interface between them, so the adhesive layer was collected while still attached to the surface layer. In this way, by collecting the surface layer and the intermediate layer separately, polyethylene and polypropylene could be collected as a single material.

[0040] B. Reusing the recovered resin film layer Next, the intermediate layer (first resin film layer) recovered in Example 3 was used as a polypropylene-based recovered resin, and the surface layer (second resin film layer) recovered in Example 3 was used as a polyethylene-based recovered resin as raw materials to manufacture a composite material by the following procedure. Note that Example 3 before separation, which was manufactured entirely from virgin raw materials, was used as a reference example.

[0041] Example 4 was prepared by replacing 50% of the polypropylene-based resin in the middle layer of Reference Example (Example 3) with polypropylene-based recovered resin recovered by the separation method of the present invention. Example 5 was prepared by replacing 10% of the polyethylene-based resin in the surface layer of Reference Example (Example 3) with polyethylene-based recovered resin recovered by the separation method of the present invention. A comparative example was prepared by replacing 50% of the polypropylene-based resin in the middle layer of Reference Example (Example 3) with the composite material of Example 3. (In other words, the composite material of Example 3 that had not been subjected to the separation method of the present invention was mixed as it was into 50% of the middle layer.) [Table 5]

[0042] The manufacturing conditions of the composite material are as follows: The five-layer materials in Table 5 were fed into an extruder with a barrel temperature of 180 to 260°C, extruded from a multi-layer die at 220 to 260°C into a five-layer sheet, cooled and solidified on a take-up roll at 25 to 30°C, and wound up on a winder to obtain a composite material. Examples 4 to 5 and the comparative example were carried out with the same compounding recipe as Example 3 (Reference Example) except for the above-mentioned changes.

[0043] The following physical properties were measured for each of the obtained composite materials.

[0044] <Haze> Haze was measured using a haze meter (NDH2000, manufactured by Nippon Denshoku Industries Co., Ltd.) according to a method conforming to JIS K7136. The haze was measured using four test pieces for each Example, Comparative Example, and Reference Example, and the average value was calculated. The sample size was 5 cm in the MD direction × 10 cm in the TD direction.

[0045] <Tensile strength, tensile elongation, 25% modulus> Each composite material was cut to a size of 40 mm interval and 10 mm width so that the long side was in the MD or TD direction to be measured, to obtain a test piece. The obtained test piece was measured using a Strograph VE-1D manufactured by Toyo Seiki Seisakusho Co., Ltd. in accordance with a method conforming to JIS K-6732. However, the measurement was performed at an atmospheric temperature of 25°C and a test speed of 200 mm / min. The 25% modulus was calculated by dividing the stress (N) when stretched 25% in the MD or TD direction by the sample width (10 mm). For Examples 4 and 5 and the Comparative Example, three test pieces were used for the measurement, and the average value was calculated.

[0046] <Young's modulus> Each composite material was cut to a size with a gauge interval of 250 mm and 5 mm so that the long side was in the MD or TD direction to be measured, to obtain a test piece. The obtained test piece was measured using a Strograph VE-1D manufactured by Toyo Seiki Seisakusho Co., Ltd. according to a method based on ASTM D882. The Young's modulus was measured using three test pieces for each Example and Comparative Example, and the average value was calculated.

[0047] <Dry heat shrinkage rate> The composite material was cut to a size of 150 mm x 20 mm so that the long side was in the MD or TD direction to be measured, and a mark was drawn so that the mark interval was 100 mm to obtain a test piece. Next, one end of the obtained test piece was fixed and placed in a thermostatic chamber PHH-102 manufactured by ESPEC Co., Ltd., whose temperature was set to 100°C. 60 seconds after the insertion, the laminated film was removed, the mark interval was measured, and the shrinkage rate was calculated from the following formula. Dry heat shrinkage rate = {(100 - gauge length after shrinkage (mm)) / 100} x 100 The dry heat shrinkage was calculated by averaging the results of three samples, and values ​​that deviated from the average by 2% or more were not counted.

[0048] <Adhesion strength> The resin film to which heat and pressure had been applied for a certain period of time was cut to a size of 100 mm x 10 mm so that the MD direction of the resin film was the long side, and a portion of the film edge was delaminated. The strength (N / 10 mm) when the resin film was peeled in the 180 degree direction at a pulling speed of 100 mm / min in the long side direction was measured using an Imada digital force gauge ZTS-100N. The test was performed three times to calculate the average adhesive strength.

[0049] <Total light transmittance> A sample was cut to 40 mm in the MD direction × 20 mm in the TD direction and measured using a V-670 manufactured by Nippon Denko Co., Ltd. The measurement conditions were a measurement wavelength range of 200 to 800 nm and a scanning speed of 100 nm / min.

[0050] The results were as follows: [Table 6]

[0051] From the results in Table 6, it was found that although the adhesive strength was slightly lower in the composite material made of virgin material (Reference Example) and the composite material using recycled material (Example 4.5), there was no significant change in other physical properties, and the composite material using recycled material can be used in the same way as the composite material using virgin material. In addition, it was found that the comparative example was inferior to Examples 4 and 5, for example, in terms of 25% modulus and Young's modulus. Therefore, it was found that when a composite material is formed using a material that has not been subjected to the separation method of the present invention, as in the comparative example, the physical properties are deteriorated compared to Examples 4 and 5. [Explanation of symbols]

[0052] 1. First resin film layer 2 Second resin film layer 3 Adhesive layer 10,20 Composite materials

Claims

1. A first step of preparing a composite material including at least a first resin film layer and a second resin film layer having compatibility therewith; a second step of applying heat and pressure to the composite material to reduce adhesive strength at the interface between the first resin film layer and the second resin film layer; a third step of peeling the first resin film layer and the second resin film layer and recovering the first resin film layer and the second resin film layer; The method for recovering a resin film comprises:

2. A first step of preparing a composite material, in which at least a first resin film layer and a second resin film layer are laminated via an adhesive layer, and the adhesive layer and the first resin film layer and / or the adhesive layer and the second resin film layer are compatible with each other; a second step of applying heat and pressure to the composite material to reduce adhesive strength at an interface between the adhesive layer and the first resin film layer and / or an interface between the adhesive layer and the second resin film layer; a third step of peeling the first resin film layer and the second resin film layer and recovering the first resin film layer and the second resin film layer; The method for recovering a resin film comprises:

3. The first resin film layer contains a polyethylene resin, The method for recovering a resin film according to claim 1 or 2, wherein the second resin film layer contains a polypropylene-based resin.

4. The method for recovering a resin film according to claim 1 or 2, wherein in the second step, an adhesive strength at the peeling interface is 2.0 N / cm or less.

5. The method for recovering a resin film according to claim 4 , wherein in the third step, a temperature of 100° C. or more and a pressure of 0.5 MPa or more are applied.

6. In the first step, a first roll around which the composite material is wound is prepared; In the second step, the composite material unwound from the first roll is passed between a pair of rollers to apply heat and pressure to the composite material; The method for recovering a resin film according to claim 1 or 2, wherein in the third step, the peeled first resin film layer and the peeled second resin film layer are recovered by being wound up on rolls.

7. A method for recovering a resin material according to claim 1 or 2, comprising recovering the first resin film layer and the second resin film layer; producing the composite material using at least one of the first resin film layer and the second resin film layer that are recovered; A method for producing a composite material, comprising:

Citation Information

Patent Citations

  • Dissolution method of resin and manufacturing method of resin solution

    JP2021160281A