Determination method of polymer component in resin
By combining FSC and DSC to control thermal history and detect glass transition signals, the method accurately quantifies PP and PE weights in PP/PE blends, addressing the limitations of existing techniques.
Patent Information
- Application Number
- JP2023074038
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
Existing methods, such as DSC and 13C NMR, are inadequate for accurately quantifying the content of polypropylene (PP) and polyethylene (PE) in blends due to overlapping melting signals and the need for solvent use, respectively, making it difficult to determine the weight fractions in recycled resin materials.
A method combining fast scanning calorimetry (FSC) and differential scanning calorimetry (DSC) is employed to amorphize the PP portion of PP/PE blends, allowing for the detection of glass transition signals and subsequent quantification of PP and PE weights through controlled thermal history and specific heat differences.
This approach enables precise determination of PP and PE weights in PP/PE blends, overcoming the limitations of previous methods by controlling crystalline and amorphous states and using thermal properties to calculate accurate weight fractions.
Smart Images

Figure 2024158671000002 
Figure 2024158671000003 
Figure 2024158671000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for quantifying the content of polypropylene and polyethylene in a resin by using a combination of fast scanning calorimetry (hereinafter sometimes referred to as FSC) and differential scanning calorimetry (hereinafter sometimes referred to as DSC), which are thermal analysis techniques. [Background technology]
[0002] FSC is a type of DSC. Conventional DSC allows heating and cooling at a rate of several to several hundred °C / min, whereas FSC allows temperature scanning at a higher speed (up to tens of thousands of °C / s), and is a method that can investigate the flow of heat during high-speed scanning (Non-Patent Document 1). For polymeric materials, it has been used as an effective method to investigate the amount of heat, temperature, and kinetics in the glass transition, crystallization, and melting of thermoplastic resins.
[0003] Furthermore, there are standards for reading the glass transition signal from a DSC curve, such as ASTM E1356-03 and JIS K7121, and standards for reading the heat absorption and heat generation from a DSC curve, such as JIS K7122.
[0004] In the material recycling of polymer materials, materials recovered from the market, waste, and processes are washed, melted, kneaded, and repelletized to be used as recycled raw materials. These recovered materials may contain additives, foreign matter, dyes, inorganic substances, carbon fiber, glass fiber, etc. as secondary components. Regarding the main resin, recycled raw materials of polypropylene (hereinafter sometimes written as PP) may contain polyethylene (hereinafter sometimes written as PE), copolymerized polyethylene, polymethylpentene, polyester (e.g., polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, etc.), polyamide (e.g., polyamide 66, polyamide 6, polyamide 610, etc.), polystyrene, polyvinyl alcohol, polyvinyl chloride, polyphenylene sulfide, polyether ether ketone, and thermosetting resin. In materials recovered from the market, waste, and processes, the content of these polymer resins may be unknown. When performing molding processing using recycled raw materials, a method for checking the content of resin is required. In particular, a method for easily quantifying the content of blends of PP and PE (hereinafter sometimes referred to as PP / PE blends), which have similar structures, is desired.
[0005] As a method for quantifying the content of PP and PE blends, carbon-13 nuclear magnetic resonance (hereafter referred to as 13 The most common methods are those using C NMR (sometimes referred to as C NMR) and Fourier transform infrared spectroscopy (sometimes referred to as FT-IR) (Non-Patent Documents 2, 3). 13 In C NMR, the entire sample must be dissolved in a high-temperature organic solvent for analysis, which requires equipment, complicated procedures, and time for analysis. In addition, the method has a large environmental impact because it uses solvents. FT-IR is a simple method, but has issues with the need for a calibration curve and the sensitivity of the signal detection. (Patent Document 1) The method of the present application is a method for measuring the content of polypropylene and polyethylene in a resin using DSC and FSC, which are representative methods of thermal analysis. In the past, there have been reports of quantitatively determining the content of PP and PE by reading the heat of fusion from the DSC curve of a PP / PE blend (Non-Patent Document 2). However, considering the thermal properties of polymers, it is essentially impossible to quantitatively determine the content by DSC alone (Non-Patent Documents 3, 4). That is, in the process of measuring PP or PE, which have crystallinity, by raising the temperature at a constant rate using DSC, each of the PP and PE parts in the sample undergoes a thermal change called partial melting-recrystallization, so that in the DSC curve in which the melting signals of both the PP and PE parts are observed, it is not possible to separate the melting signals of each part. (Non-Patent Documents 1, 5, 6) For this reason, the method using DSC in Non-Patent Document 2 cannot accurately calculate the content of polypropylene and polyethylene in a resin. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 6574081 [Non-patent literature]
[0007] [Non-Patent Document 1] C. Schick, V. Mathot, Eds., Fast Scanning Calorimetry, Springer, Switzerland (2016). [Non-Patent Document 2] AG Larsen, K. Olafsen, B. Alcock, Determining the PE fraction in recycled PP, Polymer Testing 96(2021)107058. https: / / doi.org / 10.1016 / j.polymertesting.2021.107058 [Non-Patent Document 3] E. Karaagac, M.P. Jones, T. Koch, V.-M. Archodoulaki, Polypropylene Contamination in Post-Consumer Polyolefin Waste: Characterization, Consequences and Compatibilization, Polymers 13(16) (2021) 2618. [Non-Patent Document 4] M. Gall, P. J. Freudenthaler, J. Fischer, R. W. Lang, Characterization of Composition and Structure-Property Relationships of Commercial Post-Consumer Polyethylene and Polypropylene Recyclates, Polymers 13(10) (2021) 1574. [Non-Patent Document 5] Y. Furushima, M. Nakada, M. Murakami, T. Yamane, A. Toda, C. Schick, Method for Calculation of the Lamellar Thickness Distribution of Not-Reorganized Linear Polyethylene Using Fast Scanning Calorimetry in Heating, Macromolecules 48 (2015) 8831-8837. [Non-Patent Document 6] Y. Furushima, A. Masuda, T. Kuroda, K. Okada, N. Iwata, M. Ohkura, M. Yamaguchi, The effect of poly(4-methyl-1-pentene) on the non-isothermal crystallization kinetics of polypropylene, Polymer Crystallization 2 (2019) e10082, 1-9. [Non-Patent Document 7] B. Wunderlich, The ATHAS database on heat capacities of polymers, Pure and Applied Chemistry 67(6) (1995) 1019-1026. DOI: http: / / dx.doi.org / 10.1351 / pac199567061019, WWW URL: https: / / materials.springer.com. Summary of the Invention [Problem to be solved by the invention]
[0008] By using high-speed calorimetry and DSC in combination, the weight of PP in the PP / PE blend is quantified. Furthermore, by measuring the prepared sample, the weight of the entire PP / PE blend is quantified. The weight obtained in this way makes it possible to quantify the content of polypropylene and polyethylene in the resin. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention has the following configuration. By using high-speed calorimetry and DSC in combination to measure the temperature-time profile isothermal, nonisothermal, or a combination of both, the PP portion of the PP / PE blend is made amorphous, the glass transition signal is read, and the weight of PP in the PP / PE blend is quantified. Furthermore, the temperature-time profile is changed to give the sample different thermal histories in the device, and the samples are measured to determine the weight of the entire PP / PE blend. The content of polypropylene and polyethylene in the resin is quantified from the weight obtained in this way.
[0010] In other words, this is an analytical method for determining the weights of the PP and PE portions in a sample piece of a PP / PE blend used in FSC measurement from the results of isothermal, non-isothermal, or a combination of both FSC and DSC measurements. Effect of the Invention
[0011] By applying the temperature-time profile in the FSC and DSC measurements of the present invention to a PP / PE blend, the crystalline and amorphous states of the PP and PE parts in the sample are controlled and prepared, and the total heat quantity is measured from a temperature-ramp DSC measurement in that sample state, and the total heat quantity and the specific heat difference at the glass transition of the PP part are measured from a temperature-ramp FSC measurement. The weights of the entire sample and the PP part can be calculated based on the values read, and the weight of the PE part (hereinafter sometimes referred to as M_PE) can be calculated from the difference between the weight of the entire sample piece used in the FSC measurement (hereinafter sometimes referred to as M_total) and the weight of the PP part (hereinafter sometimes referred to as M_PP). [Brief description of the drawings]
[0012] [Figure 1] TEM image of PP / PE=7 / 3 blend cooled from melt at 10℃ / min [Diagram 2] Cooling rate from melt and peak crystallization temperature of PP / PE=7 / 3 blend and its constituent PP homopolymer and PE homopolymer [Diagram 3]Heating FSC curves of PP homopolymer and PE homopolymer after quenching from the melt at 5000℃ / s [Figure 4] An example of a temperature-time profile for determining polypropylene and polyethylene content in resins using a combination of FSC and DSC. [Diagram 5] Cooling DSC curve and reheating DSC curve of a PP / PE = 7 / 3 blend from 230 °C. The reheating DSC curve corresponds to the DSC measurement result in Figure 4 (a). [Figure 6] Heating FSC curves of the PP / PE=7 / 3 blend corresponding to (b) and (c) in Figure 4 [Figure 7] Reheating DSC curves of Type 1, Type 2, Type 3, and coPP / PE corresponding to (a) in Figure 4 [Figure 8] Temperature-rising FSC curves of Type 1, Type 2, Type 3, and coPP / PE, which correspond to (b) in Figure 4 [Figure 9] Temperature-rising FSC curves of Type 1, Type 2, Type 3, and coPP / PE, which correspond to (c) in Figure 4 DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] In the present invention, when a PP / PE blend is quenched from melt to below room temperature using FSC, only the PP portion can be completely amorphous. By amorphizing the PP portion, the glass transition phenomenon exhibited by a completely amorphous material can be observed on the FSC curve, and the specific heat difference before and after the glass transition (hereinafter, sometimes referred to as ΔCp,aPP) can be read in accordance with standards such as ASTM E1356-03 and JIS K7121, and the weight M_PP of the PP in the sample piece used for FSC measurement can be determined.
[0014] M_total is determined using the results of two measurements, DSC and FSC. That is, in each measurement, the total heat is read from the heating measurement results after preparing a sample in the same crystalline state by cooling it from the melt at 10℃ / min. In this case, the total heat is obtained in units of J / g from the DSC measurement, and the total heat is obtained in units of J from the FSC measurement. Hereinafter, the total heat read from the DSC curve may be referred to as ΔH_DSC, and the total heat read from the FSC curve as ΔH_FSC. The weight of the entire sample piece used in the FSC measurement is calculated from ΔH_FSC / ΔH_DSC=M_total.
[0015] As the high-speed calorimetry, one capable of heating and cooling at 0.1 to 10,000°C / s is preferred. For example, in the case of a PP / PE blend, the set temperature is preferably between -60 and 230°C, and the scanning speed during heating and measurement is preferably 3,000°C / s. In addition, as the differential scanning calorimeter, one capable of heating and cooling at 0.1 to 100°C / min is preferred. For example, in the case of a PP / PE blend, the set temperature is preferably between -60 and 230°C, and the scanning speed during sample preparation and heating and measurement is preferably both 10°C / min.
[0016] In the present invention, it is preferable to make only the PP portion amorphous by rapidly cooling from a melt, and then reading the specific heat difference from the glass transition signal of the PP portion by measuring the temperature rise thereafter.
[0017] As long as the signal does not overlap with the glass transition temperature range of the PP part, the analysis can also be applied to polymer blends other than PE or PE copolymers, such as polyester, polyamide, polyolefin, polystyrene, polyvinyl alcohol, polyvinyl chloride, polyphenylene sulfide, polyphenylene sulfide, polyether ether ketone, and thermosetting resins. Of these, PP / PE blends are preferable. On the other hand, if the PP part is a copolymer, the glass transition signal is different from that of PP, so measurement may be difficult.
[0018] The present invention has a three-step measurement and analysis procedure for PP / PE blends. Each step preferably includes a sample preparation part in which the sample is cooled from a molten state to below room temperature in the device to prepare the crystalline or amorphous state in the sample, and a measurement part in which the sample is heated to analyze the state prepared during the cooling process, and the results of the temperature rise measurement can be analyzed.
[0019] First, a sample is prepared by cooling to -60°C or lower at a constant cooling rate (preferably 10°C / min, but any cooling rate within the range of 0.1 to 100°C / min suitable for general-purpose DSC) using DSC (this is the sample preparation part), and then a DSC measurement is performed by heating to 230°C at 10°C / min. The temperature at the end of the heating is preferably 188°C (Non-Patent Document 7), which is the equilibrium melting point of PP, or higher, and preferably 230°C. The weight of the sample used in the DSC measurement is preferably 5 mg for the resin, and is preferably in the range of 5 mg to 20 mg. In the heating DSC curve, a double endothermic peak, in which the melting signals of PE and PP in the PP / PE blend overlap, is observed between 30°C and 180°C. It is preferable to read the heat quantity ΔH_DSC of the entire endothermic peak from the DSC curve in accordance with standards such as JIS K7122.
[0020] Next, FSC measurement is performed separately from DSC. A sample piece cut to a thickness of several μm to 10 μm and a length and width of about 10 × 10 to 200 × 200 μm is set in the FSC, heated to a molten state of 230 ° C, and then cooled to -60 ° C or less. The cooling rate at this time needs to be the same as that of the previous DSC measurement, and 10 ° C / min is a preferable example. After the sample preparation part of cooling to around -60 ° C at 10 ° C / min, a heating FSC measurement is performed at 3000 ° C / s. From the obtained FSC curve, the heat amount ΔH_FSC of the entire endothermic peak is read according to standards such as JIS K7122. The weight of the entire sample piece used in the FSC measurement is calculated using ΔH_FSC / ΔH_DSC × X = M_total from the heat amounts read from the previous DSC measurement and this FSC measurement. Here, X is the weight fraction of the PP / PE blend in the entire sample, and X=1 when minor components such as additives, foreign matter, dyes, inorganic matter, carbon fiber, and glass fiber are not included.
[0021] Finally, the sample piece previously measured by FSC is reheated to a molten state of 230°C, and then rapidly cooled to -60°C or less at 5000°C / s in the sample preparation part, followed by FSC measurement at a temperature rise of 3000°C / s. When rapidly cooled in this step, the PP part in the PP / PE blend becomes completely amorphous, and a glass transition signal derived from the completely amorphous nature of PP is observed between -30°C and 20°C. It is preferable to read the specific heat difference ΔCp,aPP before and after the glass transition from the FSC curve in accordance with standards such as ASTM E1356-03 and JIS K7121. The unit of ΔCp,aPP is J / K. The specific heat difference at the glass transition temperature of completely amorphous PP is reported as ΔCp,100=0.4563J / K / g, as a literature value (hereinafter referred to as ΔCp,100) normalized by weight. (Non-Patent Document 7) Finally, the weight of PP in the sample piece used for FSC measurement is calculated from ΔCp,aPP / ΔCp,100 = M_PP. M_PE is determined from the difference between M_total calculated from the previous FSC measurement and M_PP (M_total - M_PP). M_PP / M_PE gives the content ratio in the PP / PE blend. EXAMPLES
[0022] The present invention will now be described with reference to examples.
[0023] The samples used were melt-mixed so that the ratio of PP homopolymer to PE homopolymer was 70wt%:30wt% (hereinafter referred to as PP / PE=7 / 3 blend), as well as PP and PE blend pellets (Types 1-3) and PP copolymer and PE blend pellets (coPP / PE) obtained by melt-mixing materials recovered from the market and from processes. The polyethylene content of Types 1, 2, and 3 also includes copolymerized polyethylene.
[0024] Figure 1 shows a transmission electron microscope (hereinafter sometimes referred to as TEM) image of a PP / PE = 7 / 3 blend prepared by cooling from a molten state of 230 °C to room temperature at 10 °C / min using a DSC device. The island component in Figure 1 corresponds to PE, and the sea component corresponds to PP. The area ratio of PP and PE that can be estimated from the image is PP:PE = 67%:33%, and it was confirmed that the sample was in accordance with the blend ratio.
[0025] The size of the PE islands was approximately 100 to 600 nm in diameter (the scale bar in Figure 1 is 500 nm), which was small compared to the standard size of test pieces used in FSC measurements, which are a few micrometers to 10 μm in thickness and 10 × 10 to 200 × 200 μm in length and width. Therefore, the FSC measurement obtained average information of the sample.
[0026] Figure 2 shows the relationship between the cooling rate from melting for the PP / PE=7 / 3 blend and the PP homopolymer and PE homopolymer that compose it, and the exothermic peak temperature (crystallization temperature) due to crystallization read from the FSC curve during the cooling process. It was confirmed that the PE part of the PP / PE=7 / 3 blend crystallized even at a cooling rate of 6000°C / s, but no exothermic peak due to crystallization was observed for the PP part when it was cooled at a rate faster than 1000°C / s. Furthermore, at cooling rates of 6000°C / s or less, the crystallization peak temperatures of the PE homopolymer and the PE part in the PP / PE=7 / 3 blend were the same, confirming that the same state of crystals was formed regardless of the presence or absence of PP.
[0027] FIG. 3 shows the FSC curves of the PP homopolymer and PE homopolymer constituting the PP / PE=7 / 3 blend after cooling from a molten state of 230°C at 5000°C / s. The FSC curve of the PP homopolymer showed a step-like signal due to glass transition near -20 to 10°C. In addition, the sum of heat generation and endotherm above 10°C (hereinafter sometimes referred to as total heat amount) was zero, and it was confirmed that the PP homopolymer cooled from a molten state at 5000°C / s was completely amorphous. The FSC curve of the PE homopolymer showed an endothermic peak due to crystal melting at 50°C to 130°C, but no signal was observed near -20 to 10°C where the glass transition signal was observed in the PP homopolymer. From this result, in the PP / PE=7 / 3 blend, the glass transition signal detected near -20 to 10°C is attributed only to the PP part.
[0028] Figure 4 shows the temperature-time profiles of DSC and FSC measurements to quantify the polypropylene and polyethylene contents in a resin. In Figure 4, (a) DSC and (b) and (c) FSC measurements were performed using different sample pieces. In (a), the sample was cooled from 230°C to -60°C at 10°C / min, and then a heating DSC measurement was performed at 10°C / min.
[0029] The obtained DSC curve is shown in Figure 5. The DSC curve during the temperature rise process showed endothermic peaks around 130℃ and 160℃, with the lower temperature side being mainly due to the melting of PE and the higher temperature side being mainly due to the melting of PP. The total heat amount ΔH_DSC between 80 and 170℃ on the DSC curve was read according to JIS K7122 and was found to be 149J / g.
[0030] Next, in the FSC measurement shown in Figure 4, the sample was cooled from a melt at 230°C to -60°C, and then a heating FSC measurement was performed at 3000°C / s ((b)). The sample was then re-cooled to -60°C at 5000°C / s, and then a heating FSC measurement was performed at 3000°C / s ((c)).
[0031] Figure 6 shows the FSC curves obtained during the heating process in Figure 4 (b) and (c). The total heat amount ΔH_FSC between 70 and 190°C in the FSC curve (b) in Figure 6 was read according to JIS K7122 and was 7.29μJ. From ΔH_FSC / ΔH_DSC, the weight of the entire sample piece used in the FSC measurement, M_total, was determined to be 49ng. In the FSC curve (c) in Figure 6, a step-like signal was observed near -20 to 20°C due to the glass transition of the completely amorphous PP part. The specific heat difference ΔCp, aPP before and after the glass transition, read according to JIS K7121, was 1.54×10^-8 J / K, and the weight of the PP part in the sample piece used in the FSC measurement, M_PP, determined from ΔCp,aPP / ΔCp,100, was 34ng. The difference between M_total and M_PP, 15ng, was determined as M_PE, and the final value was determined as PP:PE=69wt%:31wt%. It can be seen from Figure 2 that the PE homopolymer and the PE portion in the PP / PE=7 / 3 blend form the same crystals when cooled at 5000°C / s. Based on this, the total heat amount between 20 and 140°C was read from the FSC curve of the PE homopolymer in Figure 3, and the value multiplied by 0.3 taking into account the feed composition of the PP / PE=7 / 3 blend was consistent with the total heat amount between 20 and 160°C on the FSC curve in Figure 6(c). From this result, it can be confirmed that the total heat amount of the PP portion in the PP / PE=7 / 3 blend cooled at 5000°C / s from the molten state is zero. In other words, it was confirmed that the PP portion in the PP / PE = 7 / 3 blend was completely amorphous upon cooling at 5000°C / s, demonstrating the validity of the weight of the PP portion, M_PP, determined by ΔCp,aPP / ΔCp,100.
[0032] The FSC measurements were performed seven times using different sample pieces of the PP / PE=7 / 3 blend, and the results of the analysis showed that the average PP weight fraction was 69.9 wt%, with a standard deviation of 1.4 wt%.
[0033] FIG. 7 shows the DSC measurement results for (a) in FIG. 4 for Type 1, Type 2, Type 3, and coPP / PE. Furthermore, FIG. 8 and FIG. 9 show the FSC measurement results for (b) and (c) in FIG. 4. From FIG. 7, 8, and 9, ΔH_DSC, ΔH_FSC, and ΔCp,aPP were read, and the content ratio M_PP / M_PE in the analyzed PP / PE blend is summarized in Table 1. Table 1 shows the results of the method and 13 The weight fractions X of the PP / PE blend in the entire samples of Type 1, Type 2, Type 3, and coPP / PE were 0.96, 0.90, 0.96, and 1, respectively. 13 The M_PP / M_PE estimated by C NMR was roughly consistent with the standard deviation range of the method of the present invention. 13 C NMR was obtained by dissolving the sample in o-dichlorobenzene-d4 heated to 135 °C.
[0034] [Table 1]
Claims
1. A method for measuring polymer components in a resin, which uses a combination of differential scanning calorimetry and high speed calorimetry to obtain an isothermal, non-isothermal, or a combination of both temperature-time measurement profiles to quantify the content of polypropylene, polyethylene, or polyethylene copolymer in the resin.
2. 2. The method for quantifying polymer components in a resin according to claim 1, wherein the profile is obtained by high-speed calorimetry in which a part for preparing a sample and a part for measuring a temperature rise for determining the weight are alternately repeated.
3. 3. The method for quantifying polymer components in a resin according to claim 1, wherein the weight of the polyethylene or polyethylene copolymer portion in the resin is determined from the difference between the weight of the resin subjected to high speed calorimetry measurement and the weight of polypropylene in the resin.
4. The method for quantifying polymer components in a resin according to claim 2, wherein the part for preparing the sample determines a set temperature, a set time, and a scanning speed.
5. 3. The method for quantifying polymer components in a resin according to claim 2, wherein in the temperature rise measurement part, the cooling rate from melting is 2000° C. / s or more, and the heating rate in the subsequent heating process is 2000° C. / s or more, and is within a temperature range of -50 to 230° C.
Citation Information
Patent Citations
Method for measuring the purity of plastics
JP6574081B1