Liquid crystalline resin composition
A tailored liquid crystal resin composition with glass fibers, plate-shaped fillers, and hollow fillers addresses mechanical strength and fluidity issues, enhancing the performance of high-frequency electronic components by providing low dielectric properties and reduced warpage.
Patent Information
- Application Number
- JP2023074104
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
Conventional liquid crystal resin compositions used in high-frequency electronic components suffer from inferior mechanical strength, high warpage, and inadequate fluidity, which hinders their performance in high-frequency applications.
A liquid crystal resin composition containing a specific blend of liquid crystal resin, flat cross-section glass fibers, plate-shaped fillers, and hollow fillers, optimized for low dielectric constant, low dielectric loss tangent, and improved mechanical strength, with a balanced content of glass fibers, plate-shaped fillers, and hollow fillers to enhance fluidity and reduce warpage.
The composition achieves a low dielectric constant, low dielectric loss tangent, excellent mechanical strength, and good fluidity, resulting in molded articles with reduced warpage and improved performance in high-frequency electronic components.
Smart Images

Figure 2024158700000006 
Figure 2024158700000007 
Figure 2024158700000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid crystalline resin composition. [Background technology]
[0002] Liquid crystal resins, such as liquid crystal polyester resins, have a good balance of excellent mechanical strength, heat resistance, chemical resistance, electrical properties, and the like, and also have excellent dimensional stability, and are therefore widely used as high-performance engineering plastics. Meanwhile, in recent years, remarkable technological developments have been made in the field of information and communication, such as mobile phones, wireless LANs, and ITS technologies, such as GPS, VICS (registered trademark), and ETC. Accordingly, there is an increasing need for high-performance electronic components that can be used in high-frequency regions such as microwaves and millimeter waves. Materials constituting such electronic components are required to have appropriate dielectric properties according to the design of each electronic component.
[0003] For example, Patent Document 1 discloses a molded article of a wholly aromatic liquid crystalline polyester resin composition having a relative dielectric constant of 3.0 or less and a dielectric dissipation factor of 0.04 or less, which is obtained by injection molding a composition containing 90 to 45% by weight of a wholly aromatic liquid crystalline polyester having a melting point of 320°C or more, 10 to 40% by weight of inorganic hollow spheres having an aspect ratio of 2 or less, and 0 to 15% by weight of an inorganic filler having an aspect ratio of 4 or more. The molded article has heat resistance such as solder reflow resistance, excellent dielectric properties, and is used as a fixing or holding member for transmitting and receiving parts of information and communication devices used in high frequency bands such as microwaves and millimeter waves. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2004-27021 A Summary of the Invention [Problem to be solved by the invention]
[0005] The above-mentioned high-frequency electronic components are required to have excellent dielectric properties and low warpage. To meet such requirements, a liquid crystalline resin composition containing a hollow filler and a plate-like filler can be used, such as a composition containing a liquid crystalline polyester, hollow microspheres, and talc, as disclosed in the examples of Patent Document 1. However, according to the studies of the present inventors, it has been found that such conventional liquid crystalline resin compositions have poor mechanical strength.
[0006] In addition, when a liquid crystalline resin composition is molded to obtain a molded article, the liquid crystalline resin composition is required to have good fluidity.
[0007] The present invention has been made to solve the above problems, and an object of the present invention is to provide a liquid crystalline resin composition with good fluidity that has a low dielectric constant and a low dielectric tangent, and gives a molded article with low warpage and excellent mechanical strength. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that a liquid crystalline resin composition containing a liquid crystalline resin and a flat cross section glass fiber made of a specific low dielectric glass in a specific content has a low dielectric constant and a low dielectric tangent, is excellent in low warpage and mechanical strength, and has good flowability, and have completed the present invention. More specifically, the present invention provides the following.
[0009] (1) A liquid crystalline resin composition comprising (A) a liquid crystalline resin and (B) a glass fiber, the content of the (B) glass fiber being 10 to 100 parts by mass per 100 parts by mass of the (A) liquid crystalline resin, the (B) glass fiber having a flat cross-sectional shape with a ratio of its major axis to its minor axis being 1.5 to 6.0, the major axis of the (B) glass fiber being 10 to 40 μm, the relative dielectric constant of the glass constituting the (B) glass fiber at a measurement frequency of 1 GHz being 6 or less, and the dielectric loss tangent of the glass constituting the (B) glass fiber at a measurement frequency of 1 GHz being 0.003 or less.
[0010] (2) The liquid crystalline resin composition according to (1), wherein the (A) liquid crystalline resin is an aromatic polyester or an aromatic polyester amide having, as a constituent component, a constituent unit derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and derivatives thereof.
[0011] (3) The liquid crystalline resin composition according to (1) or (2), further comprising a plate-like filler (C), the content of the plate-like filler (C) being 2.5 to 10 parts by mass per 100 parts by mass of the liquid crystalline resin (A).
[0012] (4) The liquid crystal resin composition according to (3), wherein the (C) plate-like filler contains at least one member selected from the group consisting of talc and mica.
[0013] (5) The liquid crystalline resin composition according to any one of (1) to (4), further comprising a hollow filler (D), the content of the hollow filler (D) being 2.5 to 17.5 parts by mass per 100 parts by mass of the liquid crystalline resin (A).
[0014] (6) The liquid crystalline resin composition according to (5), wherein the (D) hollow filler contains glass balloons. Effect of the Invention
[0015] According to the present invention, it is possible to provide a liquid crystalline resin composition having good flowability, which has a low dielectric constant and a low dielectric loss tangent, and gives a molded article having low warpage and excellent mechanical strength. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a top view showing the cutting positions of test pieces for evaluating dielectric properties in the direction perpendicular to the flow used in the examples and comparative examples. [Diagram 2] FIG. 2 is a top view showing the cutting positions of test pieces for evaluating dielectric characteristics in the flow direction used in the examples and comparative examples. [Diagram 3] 3 is a diagram showing the FPC connectors molded in the examples and comparative examples, in which the numerical values are in mm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment.
[0018] <Liquid crystal resin composition> The liquid crystal resin composition according to the present invention contains (A) a liquid crystal resin and (B) glass fibers which will be described later.
[0019] [(A) Liquid crystal resin] The liquid crystal resin (A) used in the present invention refers to a melt-processable polymer having the property of being capable of forming an optically anisotropic molten phase. The property of the anisotropic molten phase can be confirmed by a conventional polarized light inspection method using crossed polarizers. More specifically, the anisotropic molten phase can be confirmed by observing a molten sample placed on a Leitz hot stage at a magnification of 40 times under a nitrogen atmosphere using a Leitz polarizing microscope. When the liquid crystal polymer applicable to the present invention is inspected between crossed polarizers, it usually transmits polarized light even in a molten stationary state, and is optically anisotropic.
[0020] The type of the liquid crystal resin (A) as described above is not particularly limited, and is preferably an aromatic polyester and / or an aromatic polyesteramide. Also, polyesters partially containing aromatic polyester and / or aromatic polyesteramide in the same molecular chain are included in the scope. As the liquid crystal resin (A), one having an inherent viscosity (IV) of preferably at least about 2.0 dl / g, more preferably 2.0 to 10.0 dl / g when dissolved in pentafluorophenol at a concentration of 0.1 mass% at 60°C is preferably used.
[0021] The aromatic polyester or aromatic polyesteramide as the (A) liquid crystalline resin applicable to the present invention is particularly preferably an aromatic polyester or aromatic polyesteramide having, as a constituent component, a constituent unit derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and derivatives thereof.
[0022] More specifically, (1) A polyester mainly composed of structural units derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and derivatives thereof; (2) A polyester mainly composed of (a) a structural unit derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and derivatives thereof, and (b) a structural unit derived from at least one selected from the group consisting of aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and derivatives thereof; (3) A polyester mainly composed of (a) a structural unit derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and derivatives thereof, (b) a structural unit derived from at least one selected from the group consisting of aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and derivatives thereof, and (c) a structural unit derived from at least one selected from the group consisting of aromatic diols, alicyclic diols, aliphatic diols, and derivatives thereof; (4) A polyesteramide mainly composed of (a) a structural unit derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and derivatives thereof, (b) a structural unit derived from at least one selected from the group consisting of aromatic hydroxyamines, aromatic diamines, and derivatives thereof, and (c) a structural unit derived from at least one selected from the group consisting of aromatic dicarboxylic acids, alicyclic dicarboxylic acids, and derivatives thereof; (5) polyesteramides mainly consisting of (a) structural units derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and their derivatives, (b) structural units derived from at least one selected from the group consisting of aromatic hydroxyamines, aromatic diamines and their derivatives, (c) structural units derived from at least one selected from the group consisting of aromatic dicarboxylic acids, alicyclic dicarboxylic acids and their derivatives, and (d) structural units derived from at least one selected from the group consisting of aromatic diols, alicyclic diols, aliphatic diols and their derivatives. If necessary, a molecular weight modifier may be used in combination with the above structural components.
[0023] In the (A) liquid crystal resin, the content of the structural unit derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and their derivatives is preferably 45 mol% or more, more preferably 50 mol% or more, even more preferably 55 mol% or more, even more preferably 60 mol% or more, and particularly preferably 62 mol% or more, based on all structural units, from the viewpoint of suppressing fluctuations in the molecular structure of the (A) liquid crystal resin. The upper limit of the content is not particularly limited, and may be 100 mol% or less, 90 mol% or less, 80 mol% or less, 75 mol% or less, or 70 mol% or less, based on all structural units.
[0024] Preferable examples of specific compounds constituting the (A) liquid crystal resin applicable to the present invention include aromatic hydroxycarboxylic acids such as p-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid; aromatic diols such as 2,6-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 4,4'-dihydroxybiphenyl, hydroquinone, resorcin, compounds represented by the following general formula (I) and compounds represented by the following general formula (II); aromatic dicarboxylic acids such as 1,4-phenylenedicarboxylic acid, 1,3-phenylenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid and compounds represented by the following general formula (III); aromatic amines such as p-aminophenol, p-phenylenediamine and N-acetyl-p-aminophenol. As the aromatic hydroxycarboxylic acid and its derivatives, p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, or a combination thereof are preferable from the viewpoints of reactivity and stability of the molecular structure of the (A) liquid crystal resin. [ka] (X is a group selected from alkylene (C1 to C4), alkylidene, -O-, -SO-, -SO2-, -S-, and -CO-) [ka] [ka] (Y:-(CH2) n -(n=1 to 4) and -O(CH2) n O-(n=1 to 4).
[0025] The liquid crystal resin (A) used in the present invention can be prepared by a known method using a direct polymerization method or an ester exchange method from the above-mentioned monomer compound (or a mixture of monomers). Usually, a melt polymerization method, a solution polymerization method, a slurry polymerization method, a solid-phase polymerization method, or a combination of two or more of these methods is used, and a melt polymerization method or a combination of a melt polymerization method and a solid-phase polymerization method is preferably used. The above-mentioned compounds having an ester forming ability may be used in the polymerization in their original form, or may be modified from a precursor to a derivative having an ester forming ability in a stage before polymerization. Various catalysts can be used in these polymerizations, and representative examples include metal salt catalysts such as potassium acetate, magnesium acetate, stannous acetate, tetrabutyl titanate, lead acetate, sodium acetate, antimony trioxide, and tris(2,4-pentanedionato)cobalt(III), and organic compound catalysts such as 1-methylimidazole and 4-dimethylaminopyridine. The amount of the catalyst used is generally about 0.001 to 1 mass% relative to the total mass of the monomers, and particularly about 0.01 to 0.2 mass% is preferable. If necessary, the molecular weight of the polymer produced by these polymerization methods can be increased by a solid-phase polymerization method in which the polymer is heated under reduced pressure or in an inert gas.
[0026] The melt viscosity of the liquid crystal resin (A) obtained by the above method is not particularly limited. In general, the melt viscosity at the molding temperature is 1000 s -1 Liquid crystal resins having a viscosity of 3 Pa s or more and 500 Pa s or less can be used. However, liquid crystal resins with a viscosity that is too high in itself are not preferred because they will significantly deteriorate the flowability. The liquid crystal resin (A) may be a mixture of two or more kinds of liquid crystal resins.
[0027] [(B) Glass fiber] The (B) glass fiber is a flat cross-section glass fiber made of low dielectric glass. The composition of the (B) glass fiber is as described below. By including the (B) glass fiber in the liquid crystal resin composition according to the present invention, the liquid crystal resin composition is likely to have good fluidity, and it is easy to obtain a molded product having a low dielectric constant and a low dielectric loss tangent, and excellent in low warpage and mechanical strength. The (B) glass fiber may be used alone or in combination of two or more kinds.
[0028] The (B) glass fiber has a flat cross-sectional shape with a ratio of the major axis to the minor axis of 1.5 to 6.0, preferably 2.2 to 5.5, and more preferably 3 to 5. When the ratio of the major axis to the minor axis is within the above range, a molded article having excellent low warpage properties can be easily obtained from the obtained composition. In this specification, the "cross-sectional shape" refers to the shape of a cross section cut along a plane perpendicular to the longitudinal direction of the (B) glass fiber.
[0029] The major axis of the (B) glass fiber is 10 to 40 μm, preferably 15 to 37 μm, and more preferably 20 to 35 μm. When the major axis is within this range, the resulting composition tends to give a molded article having excellent low warpage properties.
[0030] The minor axis of the (B) glass fiber is preferably 1.7 to 27 μm, more preferably 2.7 to 17 μm, and even more preferably 4 to 12. However, the minor axis is shorter than the major axis. When the minor axis is within this range, a molded article having excellent low warpage properties can be easily obtained from the obtained composition.
[0031] In this specification, the long and short diameters of the (B) glass fibers are values measured as follows: The cross sections of 1,000 (B) glass fibers are observed with a scanning electron microscope, and the length L of the longest diameter passing through the center of the cross section and the length S of the diameter perpendicular to the longest diameter at the center are measured, and the average value of L is used as the long diameter of the (B) glass fibers, and the average value of S is used as the short diameter of the (B) glass fibers.
[0032] In this specification, the ratio of the major axis to the minor axis is calculated by the formula: major axis / minor axis, with the major axis and minor axis adopted as described above.
[0033] (B) The weight average fiber length of the glass fiber is 5 to 750 μm, preferably 7 to 700 μm, and more preferably 9 to 670 μm. When the weight average fiber length is within the above range, the liquid crystal resin composition is likely to have good fluidity, and the molded article containing the liquid crystal resin composition is likely to have improved mechanical strength. In this specification, the weight average fiber length of the glass fiber is determined by importing 10 stereomicroscope images of the glass fiber from a CCD camera into a PC, and measuring the fiber length of 100 glass fibers for each stereomicroscope image, i.e., a total of 1,000 glass fibers, using an image processing method with an image measuring device. The weight average fiber length of the glass fiber in the liquid crystal resin composition is measured by applying the above method to the glass fibers remaining after heating the liquid crystal resin composition at 600° C. for 2 hours to incinerate it.
[0034] From the viewpoint of dielectric properties, the relative dielectric constant at a measurement frequency of 1 GHz of the glass constituting the (B) glass fiber is not more than 6, preferably not more than 5.5, and more preferably not more than 5. The lower limit of the relative dielectric constant is not particularly limited, and may be more than 1.0, or may be 1.5 or more, or 2.0 or more.
[0035] The dielectric loss tangent of the glass constituting the (B) glass fiber at a measurement frequency of 1 GHz is 0.003 or less, preferably 0.0025 or less, and more preferably 0.002 or less, from the viewpoint of dielectric properties. The lower limit of the dielectric loss tangent is not particularly limited, and may be 0.0005 or more, 0.0007 or more, or 0.001 or more.
[0036] The composition of the (B) glass fiber is preferably 48.0-62.0 mass% of SiO2, 17.0-26.0 mass% of B2O3, 9.0-18.0 mass% of Al2O3, 0.1-9.0 mass% of CaO, 0-6.0 mass% of MgO, 0.05-0.5 mass% in total of Na2O, K2O, and Li2O, 0-5.0 mass% of TiO2, 0-6.0 mass% of SrO, 0-3.0 mass% in total of F2 and Cl2, and 50-6.0 mass% of P2O, based on the total amount of the glass fiber. When the (B) glass fiber has the composition as described above, the (B) glass fiber is likely to have a low dielectric constant and a low dielectric loss tangent. In addition, although the detailed mechanism is unclear, when the composition of the (B) glass fiber is as described above, the glass fiber is likely to break during the melt-kneading treatment, the weight average fiber length is likely to be within the above range, and the obtained liquid crystalline resin composition is likely to have good fluidity.
[0037] The content of the (B) component is 10 to 100 parts by mass, preferably 15 to 80 parts by mass, and more preferably 20 to 60 parts by mass, relative to 100 parts by mass of the (A) liquid crystal resin. When the content of the (B) component is 10 parts by mass or more, it is easy to obtain a molded article having a low dielectric constant and a low dielectric loss tangent, and excellent low warpage and mechanical strength from the obtained composition. When the content of the (B) component is 100 parts by mass or less, it is easy to obtain a liquid crystal resin composition having good fluidity.
[0038] [(C) Plate-like filler] The liquid crystal resin composition according to the present invention may contain a plate-like filler. By containing the plate-like filler in the liquid crystal resin composition according to the present invention, it is easy to obtain a molded product with suppressed anisotropy while maintaining excellent mechanical strength. The plate-like filler can be used alone or in combination of two or more.
[0039] The median diameter of component (C) is preferably 10 to 50 μm. When the median diameter is within the above range, it is easier to obtain a molded article having suppressed anisotropy while maintaining excellent mechanical strength from the obtained composition. The median diameter is preferably 15 to 40 μm, more preferably 20 to 30 μm. In this specification, the median diameter of component (C) refers to the volume-based median value measured by a laser diffraction / scattering particle size distribution measurement method. The median diameter of component (C) in the liquid crystal resin composition is measured by applying the above method to the component (C) remaining after heating the liquid crystal resin composition at 600° C. for 2 hours to incinerate it.
[0040] The content of the (C) plate-like filler is preferably 2.5 to 10 parts by mass relative to 100 parts by mass of the (A) liquid crystal resin. When the content of the (C) plate-like filler is within the above range, it is easier to obtain a molded article having suppressed anisotropy while maintaining excellent mechanical strength from the obtained composition. The content of the (C) plate-like filler is more preferably 3.5 to 9 parts by mass, and even more preferably 5 to 8 parts by mass relative to 100 parts by mass of the (A) liquid crystal resin.
[0041] Examples of the plate-like filler in the present invention include talc, mica, glass flakes, various metal foils, etc. From the viewpoint of suppressing the anisotropy of a molded article obtained from a liquid crystalline resin composition without deteriorating the fluidity of the liquid crystalline resin composition, one or more selected from the group consisting of talc and mica are preferred, and mica is more preferred.
[0042] 〔talc〕 The talc that can be used in the present invention preferably has a total content of Fe2O3, Al2O3, and CaO of 2.5% by mass or less, a total content of Fe2O3 and Al2O3 of more than 1.0% by mass and 2.0% by mass or less, and a CaO content of less than 0.5% by mass, relative to the total solid content of the talc. That is, the talc that can be used in the present invention may contain at least one of Fe2O3, Al2O3, and CaO in addition to SiO2 and MgO, which are the main components, and each component may be contained within the above content range.
[0043] In the talc, when the total content of Fe2O3, Al2O3 and CaO is 2.5 mass% or less, the moldability of the liquid crystal resin composition and the heat resistance of the molded article molded from the liquid crystal resin composition are not easily deteriorated. Therefore, the total content of Fe2O3, Al2O3 and CaO is preferably 1.0 mass% or more and 2.0 mass% or less.
[0044] Among the above talcs, talcs having a total content of Fe2O3 and Al2O3 of more than 1.0% by mass are easily available. In addition, in the above talc, when the total content of Fe2O3 and Al2O3 is 2.0% by mass or less, the moldability of the liquid crystal resin composition and the heat resistance of the molded body molded from the liquid crystal resin composition are unlikely to deteriorate. Therefore, the total content of Fe2O3 and Al2O3 is preferably more than 1.0% by mass and 1.7% by mass or less.
[0045] In addition, when the CaO content in the talc is less than 0.5% by mass, the moldability of the liquid crystal resin composition and the heat resistance of the molded article molded from the liquid crystal resin composition are not easily deteriorated, and therefore the CaO content is preferably 0.01% by mass or more and 0.4% by mass or less.
[0046] [Mica] Mica is a pulverized silicate mineral containing aluminum, potassium, magnesium, sodium, iron, etc. Examples of mica that can be used in the present invention include muscovite, phlogopite, biotite, and artificial mica, among which muscovite is preferred because of its good hue and low cost.
[0047] In addition, in the production of mica, wet grinding and dry grinding are known as methods for grinding minerals. In the wet grinding method, mica ore is coarsely ground in a dry grinder, water is added to the mica to form a slurry, and the mica is then ground by wet grinding, followed by dehydration and drying. Compared to the wet grinding method, the dry grinding method is a common method with low cost, but the wet grinding method makes it easier to grind minerals thinly and finely. In the present invention, it is preferable to use thin and finely ground materials because it is possible to obtain mica having the above-mentioned median diameter and a preferred thickness described later. Therefore, in the present invention, it is preferable to use mica produced by the wet grinding method.
[0048] In addition, in the wet grinding method, since a step of dispersing the ground material in water is necessary, it is common to add a flocculating sedimentation agent and / or a sedimentation aid to the ground material in order to increase the dispersion efficiency of the ground material. Examples of flocculating sedimentation agents and sedimentation aids that can be used in the present invention include polyaluminum chloride, aluminum sulfate, ferrous sulfate, ferric sulfate, copper chloride, polyferric sulfate, polyferric chloride, iron-silica inorganic polymer flocculant, ferric chloride-silica inorganic polymer flocculant, hydrated lime (Ca(OH)2), caustic soda (NaOH), soda ash (Na2CO3), etc. These flocculating sedimentation agents and sedimentation aids have an alkaline or acidic pH. The mica used in the present invention is preferably one that has not been treated with a flocculating sedimentation agent and / or a sedimentation aid during wet grinding. When mica that has not been treated with a flocculating sedimentation agent and / or a sedimentation aid is used, decomposition of the polymer in the liquid crystal resin composition is unlikely to occur, and large amounts of gas generation and a decrease in the molecular weight of the polymer are unlikely to occur, so that it is easy to maintain the performance of the obtained molded body better.
[0049] The thickness of the mica usable in the present invention is preferably 0.01 to 1 μm, particularly preferably 0.03 to 0.3 μm, as measured by observation with an electron microscope. If the thickness of the mica is 0.01 μm or more, the mica is less likely to crack during melt processing of the liquid crystal resin composition, which is preferable since the rigidity of the molded article may be easily improved. If the thickness of the mica is 1 μm or less, the effect of improving the rigidity of the molded article is likely to be sufficient, which is preferable.
[0050] The mica that can be used in the present invention may be surface-treated with a silane coupling agent or the like, and / or may be granulated with a binder to form granules.
[0051] [(D) Hollow filler] The liquid crystalline resin composition according to the present invention may contain a hollow filler (D). When the liquid crystalline resin composition according to the present invention contains a hollow filler (D), a molded article made of the liquid crystalline resin composition tends to have a low dielectric constant and a low dielectric loss tangent.
[0052] (D) hollow filler is generally called balloon, and examples of materials for hollow spheres include inorganic materials such as alumina, silica, and glass; and organic materials such as urea resin and phenol resin. Among them, glass is preferred from the viewpoint of heat resistance and strength. That is, glass balloons are preferably used as hollow filler. (D) component may be used alone or in combination of two or more kinds.
[0053] The aspect ratio of the (D) hollow filler is preferably 1.15 or more, more preferably 1.20 or more and 2.00 or less, even more preferably 1.22 or more and 1.50 or less, and even more preferably 1.25 or more and less than 1.30, from the viewpoints of suppressing an increase in melt viscosity and a deterioration in fluidity, and moldability, etc. In this specification, the aspect ratio is determined by measuring the maximum length L, which is the length of the longest part in the particle projection plane, and the maximum perpendicular length S, which is the length of the longest part in the direction perpendicular to the maximum length L, for 3,000 particles using a dynamic image analysis method / particle state analyzer, and repeating the measurement several times to obtain the average value of the ratio L / S calculated for each particle.
[0054] From the viewpoint of moldability, the median diameter of component (D) is preferably 5 μm or more, more preferably 10 μm or more, and from the viewpoint of suppressing breakage of component (D) and moldability, it is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less. In this specification, the median diameter refers to the volume-based median value measured by a laser diffraction / scattering particle size distribution measurement method.
[0055] The content of the (D) component is 2.5 to 17.5 parts by mass, preferably 8 to 17 parts by mass, and more preferably 12 to 16 parts by mass, based on 100 parts by mass of the (A) liquid crystal resin. When the content of the (D) component is 20 parts by mass or more, a liquid crystal resin composition having excellent dielectric properties is easily obtained. When the content of the (D) component is 75 parts by mass or less, a liquid crystal resin composition having good fluidity is easily obtained.
[0056] [Other ingredients] To the liquid crystalline resin composition according to the present invention, other polymers, other fillers, and known substances generally added to synthetic resins, i.e., stabilizers such as antioxidants and ultraviolet absorbers, antistatic agents, flame retardants, colorants such as dyes and pigments, lubricants, release agents, crystallization accelerators, crystal nucleating agents, etc., may be appropriately added depending on the required performance, within the range not impairing the effects of the present invention.
[0057] The other polymers refer to polymers other than the (A) liquid crystal resin, such as an epoxy group-containing copolymer. The other fillers refer to fillers other than the (B) glass fiber, (C) plate-like filler, and (D) hollow filler, such as granular fillers such as silica; fibrous fillers other than the (B) glass fiber; carbon black; etc.
[0058] [Preparation of Liquid Crystalline Resin Composition] The preparation of the liquid crystal resin composition according to the present invention is not particularly limited. For example, the liquid crystal resin composition is prepared by blending the (A) component, the (B) component, optionally the (C) component, optionally the (D) component, and optionally other components, and melt-kneading the mixture using a single-screw or twin-screw extruder.
[0059] [Liquid crystal resin composition] The melt viscosity of the liquid crystal resin composition according to the present invention obtained as described above is preferably 100 Pa·sec or less, more preferably 90 Pa·sec or less, and even more preferably 85 Pa·sec or less, from the viewpoint of fluidity. The lower limit of the melt viscosity is not particularly limited, and may be 5 Pa·sec or more, 10 Pa·sec or more, or 20 Pa·sec or more. In this specification, the melt viscosity is defined as the maximum melt viscosity at a cylinder temperature 10 to 30°C higher than the melting point of the liquid crystal resin, a shear rate of 1000 sec -1 The value obtained using a measurement method conforming to ISO 11443 under the above conditions is used.
[0060] The liquid crystal resin composition according to the present invention has a relative dielectric constant at a measurement frequency of 5 GHz of preferably 3.5 or less, more preferably 3.4 or less, and even more preferably 3.3 or less, from the viewpoint of dielectric properties. The lower limit of the relative dielectric constant is not particularly limited, and may be more than 1.0, or may be 1.5 or more, or 2.0 or more.
[0061] The dielectric loss tangent of the liquid crystal resin composition according to the present invention at a measurement frequency of 5 GHz is preferably 0.0047 or less, more preferably 0.0044 or less, and even more preferably 0.004 or less, from the viewpoint of dielectric properties. The lower limit of the dielectric loss tangent is not particularly limited, and may be 0.001 or more, 0.0015 or more, or 0.0017 or more. EXAMPLES
[0062] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0063] <Liquid crystal resin> Aromatic polyester After the following raw materials were charged into the polymerization vessel, the temperature of the reaction system was raised to 140°C and reacted at 140°C for 1 hour. Thereafter, the temperature was further raised to 360°C over 5.5 hours, and the pressure was reduced to 5 Torr (i.e., 667 Pa) over 30 minutes, and melt polymerization was carried out while distilling off acetic acid, excess acetic anhydride, and other low boiling points. After the stirring torque reached a predetermined value, nitrogen was introduced to change from a reduced pressure state to a normal pressure state and then to a pressurized state, the polymer was discharged from the bottom of the polymerization vessel, and the strands were pelletized to obtain pellets. The obtained pellets were heat-treated at 300°C for 3 hours under a nitrogen stream to obtain the target polymer. The melting point of the obtained polymer was 348°C, and the melt viscosity at 370°C was 9 Pa·s. The melting point of the above polymer was measured according to the melting point measurement method described later, and the melt viscosity of the above polymer was measured in the same manner as the melt viscosity measurement method described later. 6-Hydroxy-2-naphthoic acid (HNA); 1218 g (48 mol%) 4-Hydroxybenzoic acid (HBA); 37g (2 mol%) 1,4-Phenylenedicarboxylic acid: 560 g (TA); (25 mol%) 4,4'-dihydroxybiphenyl (BP); 628 g (25 mol%) Metal catalyst (potassium acetate catalyst); 165mg Acylating agent (acetic anhydride); 1432g
[0064] Aromatic polyester amide After the following raw materials were charged into the polymerization vessel, the temperature of the reaction system was raised to 140°C and reacted at 140°C for 1 hour. Thereafter, the temperature was further raised to 340°C over 4.5 hours, and then the pressure was reduced to 10 Torr (i.e. 1330 Pa) over 15 minutes, and melt polymerization was carried out while distilling off acetic acid, excess acetic anhydride, and other low boiling points. After the stirring torque reached a predetermined value, nitrogen was introduced to change from a reduced pressure state to a normal pressure state and then to a pressurized state, the polymer was discharged from the bottom of the polymerization vessel, and the strands were pelletized to obtain pellets. The obtained pellets were heat-treated at 300°C for 2 hours under a nitrogen stream to obtain the target polymer. The melting point of the obtained polymer was 336°C, and the melt viscosity at 350°C was 19.0 Pa·s. The melting point of the above polymer was measured according to the melting point measurement method described later, and the melt viscosity of the above polymer was measured in the same manner as the melt viscosity measurement method described later. 4-Hydroxybenzoic acid (HBA); 1380g (60 mol%) 2-Hydroxy-6-naphthoic acid (HNA); 157 g (5 mol%) 1,4-Phenylenedicarboxylic acid (TA); 484 g (17.5 mol%) 4,4'-dihydroxybiphenyl (BP); 388 g (12.5 mol%) N-acetyl-p-aminophenol (APAP); 126 g (5 mol%) Metal catalyst (potassium acetate catalyst); 110mg Acylating agent (acetic anhydride); 1659g
[0065] [Melt point measurement method] Using a TA Instruments DSC, the liquid crystalline resin was heated from room temperature at a temperature increase rate of 20°C / min to measure the endothermic peak temperature (Tm1), and then held at a temperature of (Tm1+40)°C for 2 minutes. The resin was then cooled to room temperature at a temperature decrease rate of 20°C / min, and then heated again at a temperature increase rate of 20°C / min to measure the endothermic peak temperature (Tm2), which was determined as the melting point of the polymer.
[0066] [Melt viscosity measurement method] The melt viscosity of the liquid crystal resin was measured in accordance with ISO 11443 using a Capillograph 1B model manufactured by Toyo Seiki Seisakusho Co., Ltd. at a temperature 10 to 30°C higher than the melting point of the liquid crystal resin, using an orifice with an inner diameter of 1 mm and a length of 20 mm, and at a shear rate of 1000 / sec. The specific measurement temperatures were 370°C for aromatic polyester and 350°C for aromatic polyesteramide.
[0067] <Materials other than liquid crystal resin> Glass fiber 1: Product name CNG3PA-830 (manufactured by Nitto Boseki Co., Ltd., low dielectric glass fiber, long diameter 28 μm, short diameter 7 μm, long diameter / short diameter = 4, length 3 mm) Glass fiber 2: Product name CN3J-941 (manufactured by Nitto Boseki Co., Ltd., low dielectric glass fiber, long diameter 11 μm, short diameter 11 μm, long diameter / short diameter = 1, length 3 mm) Glass fiber 3: Product name CSG3PA-830 (manufactured by Nitto Boseki Co., Ltd., general-purpose glass fiber, long diameter 28 μm, short diameter 7 μm, long diameter / short diameter = 4, length 3 mm) Glass fiber 4: Product name CS3J-257 (manufactured by Nitto Boseki Co., Ltd., general-purpose glass fiber, long diameter 11 μm, short diameter 11 μm, long diameter / short diameter = 1, length 3 mm) Talc: Crown Talc PP (Matsumura Sangyo Co., Ltd., talc, median diameter 14.6 μm) Mica: AB-25S (Made by Yamaguchi Mica Co., Ltd., mica, median diameter 25.0 μm) Glass balloon: Y12000 (manufactured by Seishin Enterprise Co., Ltd., aspect ratio (average) 1.264, median diameter 35 μm, true specific gravity 0.6)
[0068] [Dielectric constant and dielectric loss tangent of low dielectric glass] The relative permittivity and dielectric loss tangent of the glass (i.e., low dielectric glass) constituting the low dielectric glass glass fiber are 4.8 and 0.0015, respectively, at a measurement frequency of 1 GHz. The composition of the glass fiber is 48.0-62.0 mass% of SiO2, 17.0-26.0 mass% of B2O3, 9.0-18.0 mass% of Al2O3, 0.1-9.0 mass% of CaO, 0-6.0 mass% of MgO, 0.05-0.5 mass% in total of Na2O, K2O, and Li2O, 0-5.0 mass% of TiO2, 0-6.0 mass% of SrO, 0-3.0 mass% in total of F2 and Cl2, and 50-6.0 mass% of P2O, based on the total amount of the glass fiber.
[0069] [Dielectric constant and dielectric loss tangent of general-purpose glass] The relative dielectric constant and dielectric loss tangent of the glass constituting the general-purpose glass fiber (i.e., general-purpose glass) are 6.8 and 0.0035, respectively, at a measurement frequency of 1 GHz. The composition of the glass fiber is 52.0-56.0 mass% of SiO2, 12.0-16.0 mass% of Al2O3, 20.0-25.0 mass% in total of MgO and CaO, and 5.0-10.0 mass% of B2O3, based on the total amount of the glass fiber.
[0070] <Production of Liquid Crystalline Resin Composition> The above components were melt-kneaded in the ratios shown in Table 1 or Table 2 using a twin-screw extruder (TEX30α type, manufactured by The Japan Steel Works, Ltd.) at the cylinder temperatures shown below to obtain liquid crystal resin composition pellets. [Manufacturing conditions] Cylinder Temperature: 370°C: In the case of a liquid crystal resin composition containing an aromatic polyester 350°C: In the case of a liquid crystal resin composition containing an aromatic polyester amide
[0071] <Deflection temperature under load> The pellets of the examples and comparative examples were molded under the following molding conditions using a molding machine (Sumitomo Heavy Industries, Ltd., "SE100DU") to obtain ISO test specimens type A. These test specimens were cut out to obtain test specimens for measurement (80 mm x 10 mm x 4 mm). Using these test specimens for measurement, the deflection temperature under load was measured in accordance with ISO75-1 and 2. The deflection temperature under load was used as an index of the heat resistance of the molded body. The results are shown in Tables 1 and 2. [Molding conditions] Cylinder Temperature: 370°C (Examples 1 to 3 and 7 and Comparative Examples 2 to 4) 350°C (Examples 4 to 6 and Comparative Examples 1 and 5) Mold temperature: 90℃ Injection speed: 33mm / sec
[0072] <Bending test> The pellets of the examples and comparative examples were molded under the following molding conditions using a molding machine (Sumitomo Heavy Industries, Ltd., "SE100DU") to obtain ISO test specimens type A. These test specimens were cut out to obtain test specimens for measurement (80 mm x 10 mm x 4 mm). Using these test specimens for measurement, bending strength, bending modulus, and bending strain were measured in accordance with ISO 178. The results are shown in Tables 1 and 2. [Molding conditions] Cylinder Temperature: 370°C (Examples 1 to 3 and 7 and Comparative Examples 2 to 4) 350°C (Examples 4 to 6 and Comparative Examples 1 and 5) Mold temperature: 90℃ Injection speed: 33mm / sec
[0073] <Dielectric properties> The pellets of the examples and comparative examples were molded under the following molding conditions using a molding machine ("SE100DU" manufactured by Sumitomo Heavy Industries, Ltd.) to prepare flat test pieces of 80 mm x 80 mm x 1 mm. As shown in FIG. 1, a test piece of 80 mm x 1 mm x 1 mm was cut out from a position 10 mm inward from one side along the flow direction of the flat test piece on the opposite gate side, so that the flow direction was the longitudinal direction, and this was used as a test piece for evaluating dielectric properties in the flow direction. Also, as shown in FIG. 2, a test piece of 80 mm x 1 mm x 1 mm was cut out from a position 10 mm inward from one side along the flow direction of the flat test piece, so that the flow direction was the longitudinal direction, and this was used as a test piece for evaluating dielectric properties in the flow direction. For these test pieces, the relative dielectric constant and dielectric loss tangent were measured at a measurement frequency of 5 GHz using a cavity resonator perturbation method complex dielectric constant evaluation device of the following configuration manufactured by Kanto Electronics Application Development Co., Ltd. The relative dielectric constant and the dielectric loss tangent of the flat test piece were determined by averaging the values in the direction perpendicular to the flow and the flow direction, respectively. The results are shown in Tables 1 and 2. Scalar network analyzer: Agilent Technologies 8757D Frequency synthesizer: Agilent Technologies 83650L Sweep CW Generator Fixed attenuator: Agilent Technologies 85025D detector Cavity resonator: Kanto Electronics Application Development CP431 Measurement program: Kanto Electronics Application Development CPMA-S2 / V2 [Molding conditions] Cylinder Temperature: 370°C (Examples 1 to 3 and 7 and Comparative Examples 2 to 4) 350°C (Examples 4 to 6 and Comparative Examples 1 and 5) Mold temperature: 80℃ Injection speed: 33mm / sec Holding pressure: 60MPa
[0074] <Flatness> The pellets of the examples and comparative examples were molded under the following molding conditions using a molding machine ("SE100DU" manufactured by Sumitomo Heavy Industries, Ltd.) to prepare five flat test pieces of 80 mm x 80 mm x 1 mm. The first flat test piece obtained was placed on a horizontal surface, and the height from the horizontal surface was measured at nine points on the flat test piece using a CNC image measuring machine (Quick Vision 404PRO) manufactured by Mitutoyo Corporation, and the average height was calculated from the measured values. The positions at which the height was measured were the positions corresponding to the vertices of the square, the midpoints of each side of the square, and the intersection of the two diagonals of the square when a square with a side of 74 mm was placed on the main plane of the flat test piece so that the distance from each side of the main plane was 3 mm. The height from the horizontal plane was the same as the average height, and the plane parallel to the horizontal plane was used as the reference plane. From the heights measured at the nine locations, the maximum height and the minimum height from the reference plane were selected, and the difference between the two was calculated. In the same manner, the above differences were calculated for the other four flat test pieces, and the five values obtained were averaged to obtain the flatness value. The results are shown in Tables 1 and 2. [Molding conditions] Cylinder Temperature: 370°C (Examples 1 to 3 and 7 and Comparative Examples 2 to 4) 350°C (Examples 4 to 6 and Comparative Examples 1 and 5) Mold temperature: 80℃ Injection speed: 33mm / sec Holding pressure: 60MPa
[0075] <Weight average fiber length> The weight average fiber length of the glass fibers in the liquid crystal resin composition was measured by the following method. 5 g of the liquid crystal resin composition pellets were heated at 600°C for 2 hours and incinerated. The incineration residue was thoroughly dispersed in a 5% by mass aqueous polyethylene glycol solution, and then transferred to a petri dish with a dropper, and the glass fibers were observed under a stereomicroscope. Ten stereomicroscope images of the glass fibers were imported from a CCD camera to a PC, and the fiber lengths of 100 glass fibers per stereomicroscope image, that is, a total of 1000 glass fibers, were measured by an image processing method using an image measuring device (LUZEXFS, manufactured by Nireco Corporation), and the average of the measured values was adopted as the weight-average fiber length of the glass fibers. The results are shown in Tables 1 and 2.
[0076] [Minimum Connector Filling Pressure] The liquid crystal resin composition was injection molded under the following molding conditions (gate: tunnel gate, gate size: φ0.4mm) to obtain an FPC connector with an overall size of 17.6mm×4.00mm×1.16mm, pitch distance of 0.5mm, number of pin holes 30×2 pins, and minimum thickness of 0.12mm as shown in Fig. 3. The minimum injection filling pressure at which a good molded product could be obtained when injection molding the connector in Fig. 3 was measured as the minimum filling pressure, and was evaluated according to the following criteria. The results are shown in Tables 1 and 2. ○ (Good): The minimum filling pressure was 130 MPa or less. × (bad): The minimum filling pressure was more than 130 MPa. [Molding conditions] Molding machine: SE30DUZ manufactured by Sumitomo Heavy Industries, Ltd. Cylinder Temperature: 370°C (Example 1 and Comparative Examples 2 to 4) Mold temperature: 90℃ Injection speed: 33mm / sec
[0077] [Table 1]
[0078] [Table 2]
[0079] As is clear from the results shown in Tables 1 and 2, the liquid crystalline resin compositions of the examples had good fluidity, and the molded articles produced from the liquid crystalline resin compositions had low dielectric constants and low dielectric tangents, and were excellent in low warpage and mechanical strength.
Claims
1. (A) a liquid crystalline resin, and (B) Glass fiber Contains The content of the (B) glass fiber is 10 to 100 parts by mass with respect to 100 parts by mass of the (A) liquid crystalline resin, The (B) glass fiber has a flat cross-sectional shape with a ratio of the major axis to the minor axis of 1.5 to 6.0, The major axis of the (B) glass fiber is 10 to 40 μm, The glass constituting the (B) glass fiber has a relative dielectric constant of 6 or less at a measurement frequency of 1 GHz, The liquid crystalline resin composition (B) has a dielectric loss tangent of 0.003 or less at a measurement frequency of 1 GHz of glass constituting the glass fiber.
2. 2. The liquid crystalline resin composition according to claim 1, wherein the liquid crystalline resin (A) is an aromatic polyester or aromatic polyester amide having, as a constituent component, a constituent unit derived from at least one selected from the group consisting of aromatic hydroxycarboxylic acids and derivatives thereof.
3. Further contains (C) a plate-like filler, 3. The liquid crystal resin composition according to claim 1, wherein the content of the plate-like filler (C) is 2.5 to 10 parts by mass based on 100 parts by mass of the liquid crystal resin (A).
4. The liquid crystal resin composition according to claim 3 , wherein the plate-like filler (C) comprises at least one member selected from the group consisting of talc and mica.
5. Further containing (D) a hollow filler, 3. The liquid crystal resin composition according to claim 1, wherein the content of the hollow filler (D) is 2.5 to 17.5 parts by mass based on 100 parts by mass of the liquid crystal resin (A).
6. The liquid crystal resin composition according to claim 5 , wherein the hollow filler (D) contains glass balloons.
Citation Information
Patent Citations
Electrical connectors formed from polymer compositions having low dielectric constants and dissipation factors
JP2022547419A
5G system containing polymer composition
JP2022547816A
RF filters for use with 5G frequencies
JP2022548865A
Resin composition and molded article thereof
WO2022014663A1
Wholly aromatic liquid crystalline polyester resin molded product
JP2004027021A