Packaging body for laminated body

A packaging material with a paper layer and heat-sealable coating layer addresses operability and sheet stability issues by optimizing peel strength and friction coefficients, ensuring stable sheet retention and recyclability.

JP2024158810APending Publication Date: 2024-11-08NIPPON PAPER CRECIA CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023074357
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing packaging materials for laminates face issues with operability, misalignment, and inability to stably hold sheets, particularly when using reduced thermoplastic resin content for recyclability, leading to potential sheet shifting and poor adhesion during manufacturing, transportation, and use.

Method used

A packaging material comprising a laminate of laminated sheets with a paper layer and a heat-sealable coating layer, optimized for peel strength, basis weight, and friction coefficients, ensuring stable holding and fixing of the laminate.

Benefits of technology

The packaging material provides good operability, stable adhesion, and effective sheet retention, while being recyclable, through specific adjustments in peel strength, basis weight, and friction coefficients.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158810000001_ABST
    Figure 2024158810000001_ABST
Patent Text Reader

Abstract

To provide a packaging body for a laminated body using a packaging material that can be subjected to heat seal processing, has satisfactory operability and can stably hold and fix the laminated body.SOLUTION: Disclosed is a packaging body for a laminated body that comprises: a laminated body obtained by laminating sheets; and a packaging material having a paper layer and heat-sealable coating layers. In the packaging material, peeling strength between the coating layers is 750 gf / 25 mm or more and basis weight is 40 or more to 60 g / m2 or less, and the coefficient of dynamic friction between the coating layers is 0.47 or more to 0.54 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a packaging body for a laminate in which a laminate of sheets is packaged in a packaging material. [Background technology]

[0002] In recent years, paper products and nonwoven fabric products for various purposes, such as paper towels, hand towels, and nonwoven fabric wipes, have been sold.

[0003] These products are sold in the form of individual sheets, either rolled up or stacked, but because there is a risk of the sheets shifting or falling off when left stacked, they are often sold wrapped in paper, plastic film, or other packaging materials.

[0004] In recent years, plastic waste has become a major issue due to concerns that plastic that has been released into the environment as garbage will not decompose for a long time and will have a negative impact on the ecosystem. As a countermeasure, it has been proposed to replace plastic with biomass-derived materials and paper, which is a biodegradable material.

[0005] On the other hand, when paper packaging materials are formed into packaging materials for foods, bags, containers, boxes, cups, lids, and the like, it has been common practice to impart heat sealing suitability to the packaging materials by laminating a thermoplastic resin, typically a polyolefin resin such as polyethylene, polypropylene, or polymethylpentene, onto the packaging materials by extrusion lamination or the like.

[0006] However, these thermoplastic resin laminates have a thickness of 10 to 30 g / m 2 The amount of thermoplastic resin used is about the same as that of conventional paper, and the reduction in the amount of plastic cannot be said to be sufficient. For this reason, currently, wrapping paper is being provided in which the coating layer is made thinner and lighter by coating a water or solvent dispersion containing a thermoplastic resin dispersion on a paper base material.

[0007] As a prior art document for such heat seal paper, for example, Patent Document 1 describes a paper substrate having a coating layer containing a thermoplastic resin on at least one side thereof, the coating layer containing at least a pigment as an antiblocking agent, the amount of pigment in the coating layer being less than 200 parts by mass per 100 parts by mass of the thermoplastic resin, and the thermoplastic resin contained in the coating layer being one or more of low density polyethylene, high density polyethylene, linear low density polyethylene, polypropylene, polyester resin, ethylene methacrylic acid copolymer resin, ethylene methyl acrylate copolymer resin, and polylactic acid resin (with the proviso that the paper substrate has a longitudinal tensile energy absorption amount X1 measured in accordance with JIS P 8113:2006, a transverse tensile energy absorption amount Y1 measured in accordance with JIS P 8113:2006, a longitudinal tensile energy absorption ratio X2 measured in accordance with JIS P 8113:2006, and a longitudinal tensile energy absorption ratio Y3 measured in accordance with JIS P 8113:2006). When the specific tensile energy absorption in the transverse direction measured in accordance with 8113:2006 is Y2, the geometric mean of X1 and Y1 is 120 J / m 2 or more, the ratio of X1 to Y1 (X1 / Y1) is 0.5 or more and 2.0 or less, and the geometric mean of X2 and Y2 is 2.0 J / g or more is excluded.

[0008] Patent Document 2 describes a paper base material mainly made of unbleached softwood kraft pulp and a heat seal layer laminated on one side of the paper base material, in which the paper base material has a folding endurance in the machine direction of 500 to 1,000 times and a folding endurance in the width direction of 80 to 200 times, the Beck smoothness of the surface of the heat seal layer laminated surface is 3 seconds to 230 seconds, the main component of the heat seal layer is an ionomer resin, and the coating amount of the heat seal layer is 1.5 g / m 2 More than 10.0g / m 2 The following heat seal paper is disclosed: [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2023-010964 A [Patent Document 2] Patent Publication No. 2022-024906 Summary of the Invention [Problem to be solved by the invention]

[0010] Even in the case of a package in which a laminate of sheets, such as paper wipers or nonwoven wipers, is held and fixed by a paper band, in the case of automated packaging equipment for continuous packaging, extrusion laminated paper is generally used.

[0011] On the other hand, in order to reduce the amount of thermoplastic resin used and to impart recyclability, it is desirable to use a packaging material coated with a resin body.

[0012] However, with conventional packaging materials, there have been cases where operability has deteriorated and shifting has occurred in the laminate of sheets during production, transportation, or when the sheet is used by the user.

[0013] Therefore, there is a demand for a packaging material that can be recycled after use, has excellent operability, and can firmly hold a sheet stack.

[0014] The present invention has been made in consideration of the above circumstances, and has an object to provide a packaging body for laminates using a packaging material that is capable of being subjected to heat sealing processing, has good operability, and can stably hold and fix the laminate. [Means for solving the problem]

[0015] The inventors have conducted extensive research and have found that in a package for a laminate including a laminate obtained by stacking sheets and a packaging material having a paper layer and a heat-sealable coating layer, by adjusting the peel strength and basis weight of the paper layer and coating layer of the packaging material within respective predetermined numerical ranges and by adjusting the dynamic friction coefficient between the coating layers in the packaging material within predetermined numerical ranges, a package for a laminate using a packaging material that has good operability and can stably hold and fix a laminate can be obtained, and the present invention has been completed. That is, the present invention provides the following.

[0016] (1) A first aspect of the present invention is a package for a laminate, comprising a laminate obtained by laminating sheets, and a packaging material having a paper layer and a heat-sealable coating layer, the packaging material having a peel strength between the coating layers of 750 gf / 25 mm or more and a basis weight of 40 g / m 2 More than 60g / m 2 The present invention is a packaging body for laminates, characterized in that the coefficient of dynamic friction between the coating layers in the packaging material is 0.47 or more and 0.54 or less.

[0017] (2) A second aspect of the present invention is a packaging material for laminates according to (1), characterized in that the static friction coefficient between the coating layers in the packaging material is 0.14 or more.

[0018] (3) A third aspect of the present invention is a packaging material for laminates as described in (1), characterized in that the coefficient of dynamic friction between the coating layer and the paper layer in the packaging material is 0.23 or more and 0.30 or less.

[0019] (4) A fourth aspect of the present invention is the packaging material for laminates according to (1), characterized in that the cantilever stiffness value of the packaging material is 50 mm or more and 130 mm or less.

[0020] (5) A fifth aspect of the present invention is a packaging material for laminates according to (1), characterized in that the base paper used for the paper layer of the packaging material is western paper. Effect of the Invention

[0021] According to the present invention, it is possible to provide a packaging body for a laminate that uses a packaging material that can be subjected to heat sealing processing, has good operability, and can stably hold and fix the laminate. [Brief description of the drawings]

[0022] [Figure 1] 1 is a perspective view of a packaging body for a laminate according to an embodiment of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.

[0024] In the drawings, the same elements are given the same reference numerals, and duplicated explanations are omitted. Furthermore, unless otherwise specified, the positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.

[0025] <Packaging for laminate> FIG. 1 is a perspective view of a packaging body 1 for a laminate according to this embodiment (hereinafter, also simply referred to as packaging body 1). The laminate packaging body 1 according to this embodiment includes a laminate 10 formed by laminating sheets, and a packaging material 20 having a paper layer and a heat-sealable coating layer.

[0026] <Laminate> The laminate 10 according to this embodiment is formed by laminating sheets. The sheets may be made of paper or nonwoven fabric, and may be laminated one by one as they are, or may be laminated after being folded one by one in a V-shape, Z-shape, or the like.

[0027] The dimensions of the laminate 10 (after the sheet is folded) in each direction are not particularly limited, but it is preferable that the longitudinal dimension is 180 mm or more and 210 mm or less, the width dimension is 150 mm or more and 180 mm or less, and the thickness dimension is 90 mm or more and 150 mm or less.

[0028] <Packaging material> The packaging material 20 according to this embodiment is used to package a laminate 10 in which sheets are stacked, and has a paper layer and a heat-sealable coating layer. As for the packaging form of the laminate 10 using the packaging material 20, it is preferable to form the heat-sealed portion 21 in a strip-like form (as a strip of paper) as shown in FIG. 1 and package the laminate 10, but this is not limited thereto, and the laminate may be packaged in a form that is generally used for packaging paper products or nonwoven fabric products, such as pillow packaging or caramel packaging.

[0029] The basis weight of the packaging material 20 according to this embodiment is 40 g / m 2 More than 60g / m 2 The basis weight is 40 g / m 2 If the basis weight is less than 60 g / m, the packaging material 20 will have poor strength and will be easily torn when the heat sealing process described below is carried out. 2 If the temperature exceeds this range, the packaging material 20 becomes hard and it becomes difficult to package the laminate 10. The basis weight of the packaging material 20 is 42 g / m 2 More than 58g / m 2 The basis weight is measured in accordance with JIS P 8124.

[0030] In addition, the cantilever stiffness value of the packaging material 20 according to this embodiment is preferably 50 mm or more and 130 mm or less. By setting the cantilever stiffness value within the above numerical range, the operability during processing of the packaging material 20 is improved. The cantilever stiffness is more preferably 90 mm or more and 120 mm or less. The cantilever stiffness is measured in accordance with JIS L 1096 (2010) 8.21 Bending resistance Method A (45° cantilever method).

[0031] <Paper layer> The base paper used for the paper layer (paper substrate) included in the packaging material 20 according to this embodiment is not particularly limited and may be Japanese paper or Western paper, with Western paper being preferred. As the Western paper, any of the fine paper, coated paper, kraft paper, crepe paper, and the like that are normally used for packaging paper can be used without any particular limitation. The basis weight of the base paper used in the paper layer is not particularly limited, but is preferably 30 g / m 2 More than 57g / m 2 It is preferable that the basis weight is 30 g / m or less. 2 If the basis weight is less than 57 g / m, the packaging material 20 will have poor strength and will be easily torn during the heat sealing process described below. 2 If the temperature exceeds this range, the packaging material 20 becomes too hard, making it difficult to package the laminate 10.

[0032] <Coating layer> The coating layer is mainly made of a thermoplastic resin. The coating layer may be provided on both sides of the paper layer, but it is preferable to provide the coating layer on at least one side. The coating layer is heat-sealable, i.e., has heat-sealing suitability. Having heat-sealing suitability means that it can be attached to an object to be attached by applying heat and pressure (it can form a heat-sealed portion 21). Having heat-sealing suitability makes it easy to mold into a packaging form, maintain the shape, and ensure airtightness in packaging applications.

[0033] (thermoplastic resin) The thermoplastic resin used in this embodiment can be any resin used in the papermaking field for forming a heat seal layer, and can have a glass transition temperature of 100° C. or less. The glass transition temperature of the thermoplastic resin is preferably −20° C. or more and 85° C. or less. The melting point of the thermoplastic resin is preferably 80° C. or more and 120° C. or less. Examples of the thermoplastic resin that can be used include low density polyethylene (LDPE), high density polyethylene (HDPE), linear low density polyethylene (LLDPE), polypropylene (PP), polyvinyl acetate (PVAc), polyester resin (PET), ethylene methacrylic acid copolymer resin (EMAA), ethylene methyl acrylate copolymer resin (EMA), ethylene acrylic acid copolymer resin (EAA), ethylene vinyl acetate copolymer resin (EVA), styrene acrylic acid ester copolymer resin, polylactic acid resin, etc. Also, the thermoplastic resin can be used alone or in combination of two or more kinds. Among these, ethylene acrylic acid copolymer resin, which has high heat sealing suitability, is preferred. As a countermeasure against blocking, an anti-blocking agent such as a pigment or wax may be contained.

[0034] (Pigments) The pigment used in this embodiment is not particularly limited, and inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, and satin white, and organic pigments such as solid, hollow, and core-shell pigments can be used. In addition, one type of pigment or a mixture of two or more types can be used. Among these, heavy calcium carbonate is preferred because it has excellent blocking resistance without impairing heat sealability.

[0035] (wax) The wax used in this embodiment is not particularly limited, and may be a paraffin wax mainly composed of an alkane compound, a natural oil-based wax derived from animals and plants such as carnauba or lanolin, a silicone-containing wax containing silicone or a silicone compound, or a fluorine-containing wax containing a fluorine compound. The wax may be used alone or in combination of two or more kinds. Among these, carnauba wax is preferred.

[0036] The coating method of the coating layer is not particularly limited, and coating can be performed using a known coating device and coating system. For example, the coating device may be a blade coater, a bar coater, an air knife coater, a curtain coater, a spray coater, a roll coater, a reverse roll coater, a size press coater, a gate roll coater, etc. In addition, the coating system may be a water-based coating using a solvent such as water, a solvent-based coating using a solvent such as an organic solvent, etc. Since the packaging material 20 according to the present embodiment may be used in applications where it comes into indirect contact with the skin of the user's hands through a sheet, it is preferable from the viewpoint of safety that the coating be a water-based coating. The viscosity, solid content, and other properties of the coating solution can be appropriately adjusted depending on the coating device and coating system used.

[0037] The coating amount (dry weight) of the coating layer is 3g / m per side. 2 More than 20g / m 2 The coating weight is preferably 3 g / m or less per side. 2 If the coating amount is less than 20 g / m per side, the heat sealability will decrease. 2 Above this value, there is little improvement in heat sealability and the cost increases. The coating layer may be one layer or may be composed of two or more layers. When the coating layer is composed of two or more layers, the total coating weight of all the coating layers is preferably within the above range.

[0038] The packaging material 20 according to the present embodiment may include other layers such as a sealing layer, a printing layer, a light-shielding layer, a water-resistant layer, an oil-resistant layer, a water vapor barrier layer, and a gas barrier layer, but it is preferable to include a sealing layer between the coating layer and the paper layer. By including a sealing layer, it is possible to reduce the occurrence of coating defects such as pinholes and streaks in the coating layer, and to improve water resistance and oil resistance.

[0039] Furthermore, the packaging material 20 according to this embodiment has a peel strength between the adhered coating layers of 750 gf / 25 mm or more. If the peel strength is less than 750 gf / 25 mm, the adhesiveness when heat-sealed is poor. The peel strength between the coating layers is preferably 750 gf / 25 mm or more and 1500 gf / 25 mm or less. The peel strength is measured by first overlapping the coating layers of the packaging material 20 with each other and sealing for about 1.3 seconds using a Fuji Impulse Polysealer 210E with the temperature set to "5". The laminated portion is then cut into a 2 mm width and a tensile test is performed using a Tensilon. The conditions are a chuck distance of 20 m and a tensile speed of 100 mm / min, and the final peel strength is measured at the maximum point load.

[0040] Furthermore, the coefficient of dynamic friction between the coating layers in the packaging material 20 is 0.47 or more and 0.54 or less. If the coefficient of dynamic friction is less than 0.47, the heat sealability (operability) of the packaging material 20 is poor. If the coefficient of dynamic friction exceeds 0.54, the packaging material 20 is poor in tightness, making it difficult to hold and fix the laminate 10. The static friction coefficient between the coating layers in the packaging material 20 is preferably 0.14 or more. If the static friction coefficient is less than 0.14, the heat sealability (operability) of the packaging material 20 is poor. It is more preferable that the static friction coefficient between the coating layers in the packaging material 20 is 0.17 or more.

[0041] In addition, the coefficient of dynamic friction between the coating layer and the paper layer in the packaging material 20 is preferably 0.23 or more and 0.30 or less. If the coefficient of dynamic friction is less than 0.23, the packaging material 20 will not be tight enough to hold and fix the laminate 10. If the coefficient of dynamic friction exceeds 0.30, the coating layer is likely to remain, resulting in poor recyclability. It is more preferable that the coefficient of dynamic friction between the coating layer and the paper layer in the packaging material 20 is 0.26 or more and 0.30 or less. The above dynamic friction coefficient and static friction coefficient are both measured using an ISO friction tester (compliant with ISO15359).

[0042] <Method for manufacturing laminate packaging> The method for producing the laminate packaging body 1 according to this embodiment is not particularly limited, and it can be produced by a known method for producing a laminated thin paper product. Such a manufacturing method may include, for example, the steps of (1) producing a sheet, (2) cutting and folding, (3) lamination, and (4) wrapping in a wrapping material, although some of the steps may be reversed. EXAMPLES

[0043] The present invention will be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples in any way.

[0044] Each of the packages for laminates of Examples 1 to 4 and Comparative Examples 1 to 6 was produced under the conditions shown in Table 1, and then the following evaluations were carried out. In each of the examples and comparative examples, the laminate sheet was made by laminating four sheets of base paper made mainly of NBKP by pin embossing (basis weight of base paper: 23.4 g / m 2 The sheet was folded in four and four sheets were stacked to form a laminate. The wrapping material was in a strip shape and both ends were heat sealed to wrap the laminate.

[0045] (Heat sealability (operability)) The operability was confirmed using a packaging machine that automatically forms packages using heat sealing processing. ◎: Stable heat sealing processing and good operability ○: Heat sealing can be performed without any problems, and there is no problem with operability. △: During heat sealing, the thick paper causes poor thermal conductivity and adhesion failure, resulting in slightly poor operability. ×: During heat sealing, the paper may break at the strip, resulting in poor operability.

[0046] (Adhesiveness) The adhesiveness was evaluated based on the measured peel strength between the paper layer and the coating layer. ○: Adhesion is good, and the heat-sealed portion does not peel off easily. ×: The adhesiveness is weak and the heat seal part peels off easily.

[0047] (Tightness) The packaging material of the package was held and the whole package was shook from side to side, and the state of the laminate was evaluated. ◎: The laminate of overlapping sheets is sufficiently fixed, with almost no misalignment. ○: Misalignment of the laminated body of overlapping sheets occurs, but is not a problem in normal handling. △: A somewhat large misalignment occurs in the laminate where the sheets are overlapped. ×: The laminate of overlapping sheets easily and significantly shifts

[0048] (Recyclability) A disintegration test was performed using a TAPPI disintegrator, and it was visually confirmed whether the heat seal layer dissolved without any problems (whether or not the heat seal layer remained). Those without any heat seal layer remaining were marked with "○", and those with some remaining heat seal layer were marked with "×".

[0049] (comprehensive evaluation) The above evaluations were combined and rated on a 5-point scale as follows. Packages with a score of 3 or more were considered to pass. 5 points: Packaging with excellent results in all evaluations (2 ◎ in the evaluation items) 4 points: Generally good packaging (1 item in the evaluation category was given a ◎) 3 points: Packaging that passes the standard with no particular shortcomings (only evaluation items marked with ○) 2 points: Package with poor quality (evaluation item has △) 1 point: The packaging has some items that are not suitable for solving the current problem (there is an × in the evaluation items)

[0050] Table 1 shows the conditions and evaluation results for Examples 1 to 4 and Comparative Examples 1 to 6. [Table 1]

[0051] From the above, it was confirmed that this embodiment makes it possible to perform heat sealing processing, has good operability, and provides a laminate packaging body using a packaging material that can stably hold and fix the laminate. [Explanation of symbols]

[0052] 1 (For laminate) Packaging 10 Laminate 20 Packaging materials 21 Heat seal section

Claims

1. A laminate packaging body comprising a laminate obtained by laminating sheets and a packaging material having a paper layer and a heat-sealable coating layer, The packaging material has a peel strength between the coating layers of 750 gf / 25 mm or more and a basis weight of 40 g / m 2 60g / m or more 2 is as follows: A packaging body for laminates, characterized in that the coefficient of dynamic friction between the coating layers in the packaging material is 0.47 or more and 0.54 or less.

2. 2. The packaging body for laminates according to claim 1, wherein the coating layers in the packaging material have a static friction coefficient of 0.14 or more.

3. 2. The packaging body for laminates according to claim 1, wherein the coefficient of dynamic friction between the coating layer and the paper layer in the packaging material is 0.23 or more and 0.30 or less.

4. 2. The packaging body for laminates according to claim 1, wherein the packaging material has a cantilever stiffness value of 50 mm or more and 130 mm or less.

5. 2. The packaging body for laminates according to claim 1, wherein the base paper used for the paper layer of the packaging material is western paper.

Citation Information

Patent Citations

  • Heat seal paper and packaging material

    JP2022024906A

  • heat seal paper

    JP2023010964A