Thermoplastic resin composition for solid phase polymerization, modified thermoplastic resin using the same, molded product, and production method of them, as well as master batch for accelerating solid phase polymerization

The thermoplastic resin composition and masterbatch improve the quality and productivity of recycled resin products by optimizing catalyst distribution and polymerization conditions, addressing viscosity and contamination issues in solid-phase polymerization.

JP2024158815APending Publication Date: 2024-11-08TOYO INK MFG CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023074366
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing methods for recycling thermoplastic resins, such as PET, face challenges in reducing viscosity and equipment contamination during solid-phase polymerization, leading to reduced productivity and quality issues in molded products due to outgassing and poor moldability.

Method used

A thermoplastic resin composition and masterbatch are developed, comprising a thermoplastic resin and a polycondensation catalyst, with specific solubility parameters and flow start temperature differences, to enhance compatibility and uniform distribution of the catalyst, facilitating shorter polymerization times and improved product quality.

Benefits of technology

The solution results in high-quality molded articles with enhanced productivity by reducing outgassing and improving moldability, even when using recycled resins, by uniformly dispersing the catalyst and optimizing polymerization conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158815000001
    Figure 2024158815000001
  • Figure 2024158815000002
    Figure 2024158815000002
  • Figure 2024158815000003
    Figure 2024158815000003
Patent Text Reader

Abstract

To provide: a master batch for accelerating solid phase polymerization which is excellent in productivity and is capable of providing a high quality molded product; a thermoplastic resin composition; and a modified thermoplastic resin; and also a production method of them.SOLUTION: A thermoplastic resin composition is formed by melt-kneading a thermoplastic resin (C) which is at least one selected from a group consisting of a polyester resin (however, excluding a polyethylene terephthalate resin), a polycarbonate resin, and a polyamide resin with a master batch for accelerating solid phase polymerization. In the thermoplastic resin composition, the master batch for accelerating solid phase polymerization comprises a thermoplastic resin (A) and a polycondensation catalyst (B), and the thermoplastic resin (A) is at least one selected from a group consisting of a polyester resin (A1) having a structural unit derived from a polyhydric alcohol, a polycarbonate resin (A2), and a polyamide resin (A3).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic resin composition for solid-state polymerization, a modified thermoplastic resin using the same, a molded article, and a masterbatch for promoting solid-state polymerization, and also to methods for producing these. [Background technology]

[0002] Thermoplastic resins such as polyester resins, polyamide resins, and polycarbonate resins are excellent in heat resistance, strength, etc., and are therefore used in a wide range of fields, including synthetic fibers, films, sheets, machine parts, automobile parts, containers, electronic materials, etc. Resins with better physical properties, including recycled resins, are in demand in the market, and various proposals have been made.

[0003] As a method for modifying a polyester resin, Patent Document 1 proposes a modifier for crystalline polyester resin, which contains an amorphous polyester resin (I) and a reactive compound (II) that contains two or more glycidyl groups and / or isocyanate groups per molecule and has a weight average molecular weight of 200 or more and 500,000 or less. Patent Document 2 discloses a method in which used PET resin (polyethylene terephthalate resin) material from bottle collection is extruded into a twin-screw extruder under heating together with a sterically hindered hydroxyphenyl alkyl phosphonic acid ester or monoester, the extrudate is formed into granules, and the granules are then solid-phase condensed in a tumble dryer under vacuum. This method has been shown to significantly increase the intrinsic viscosity after solid-phase polymerization. Patent Document 3 discloses a method of melt-kneading polyethylene terephthalate (A) obtained by mixing terephthalic acid, isophthalic acid, and ethylene glycol, and carrying out an esterification reaction, followed by a polycondensation reaction, with trimethylolpropane (polymerization accelerator) to obtain a polymerization accelerator-containing master batch. It also discloses a method of adding this master batch to the polyethylene terephthalate (A) to obtain chip-shaped granulated material of modified polyethylene terephthalate containing 0.1 wt% of polymerization accelerator, followed by solid-state polymerization for 11 hours to obtain a bottle.

[0004] As a method for modifying a polycarbonate resin, Patent Document 4 discloses a method for producing a high molecular weight polycarbonate resin, which can maximize the increase in the molecular weight of the polycarbonate after solid-state polymerization and shorten the production time by lowering the molar ratio of aryl carbonate present in a mixture of a polycarbonate prepolymer, a terminal group of a reaction by-product having a degree of polymerization less than 3, and unreacted diaryl carbonate through condensation polymerization.

[0005] As a method for modifying a polyamide resin, Patent Document 5 proposes a semi-aromatic polyamide resin that contains a constituent unit obtained from hexamethylenediamine and terephthalic acid, and a constituent unit obtained from 11-aminoundecanoic acid or undecanelactam, has a relative viscosity (RV) in the range of 1.95 to 3.50, and has a relationship among the amino terminal concentration (AEG), the carboxy terminal concentration (CEG), and the terminal concentration (EC) of blocked amino terminals with monocarboxylic acid that satisfies a specific formula. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2006-045477 A [Patent Document 2] International Publication No. 96 / 11978 [Patent Document 3] JP 2005-002170 A [Patent Document 4] Special Publication No. 2005-530874 [Patent Document 5] International Publication No. 2019 / 189145 Summary of the Invention [Problem to be solved by the invention]

[0007] In the above Patent Document 2, an increase in molecular weight can be confirmed after solid-state polymerization of recycled PET resin. However, after extensive research, the inventors found that there are problems with reducing the viscosity of the recycled PET resin before solid-state polymerization, and there are also problems with productivity due to the contamination of the equipment.

[0008] Measures to deal with the plastic waste problem have become an important issue worldwide, and there is a strong demand for highly productive technology to further promote recycling technology. In addition, even for recycled products, polyester resin molded products with excellent quality that meets moldability and color are required. In Example 1 of Patent Document 3, 7.4 ppm of acetaldehyde was detected. In general, outgassing causes mold contamination of molding machines, and is a factor that causes molding defects and deterioration of physical properties of molded products.

[0009] Although the above describes the problems associated with recycling thermoplastic resins using polyester resin as an example, similar problems may occur when recycling other thermoplastic resins whose physical properties need to be improved. In the examples and comparative examples of Patent Document 5, outgassing was detected at 303-886 ppm.

[0010] The present invention has been made in view of the above problems, and aims to provide a masterbatch for promoting solid-state polymerization, a thermoplastic resin composition for solid-state polymerization, and a modified thermoplastic resin, which are capable of providing a molded product having excellent productivity and high quality and are mainly composed of a polyester resin (excluding polyethylene terephthalate resin), a polycarbonate resin, or a polyamide resin, and also aims to provide a method for producing these. An object of the present invention is to provide a molded article which is excellent in productivity and high in quality by using the masterbatch for promoting solid-state polymerization of the present invention, even when recycled resin is used. [Means for solving the problem]

[0011] As a result of extensive investigations, the present inventors have found that the problems of the present invention can be solved in the following aspect, and have thus completed the present invention. [1]: A thermoplastic resin composition obtained by melt-kneading a thermoplastic resin (C) which is at least one selected from the group consisting of a polyester resin (excluding polyethylene terephthalate resin), a polycarbonate resin, and a polyamide resin, and a masterbatch for promoting solid-state polymerization, The solid-state polymerization promoting masterbatch contains a thermoplastic resin (A) and a polycondensation catalyst (B), the thermoplastic resin (A) is at least one selected from the group consisting of a polyester resin (A1) having a structural unit derived from a polyhydric alcohol, a polycarbonate resin (A2), and a polyamide resin (A3); The polyester resin (A1) has a content of structural units derived from ethylene glycol and / or diethylene glycol of less than 50 mol % in 100 mol % of structural units derived from a polyhydric alcohol, The polycondensation catalyst (B) is at least one selected from the group consisting of phosphorus-based catalysts, titanium-based catalysts, and antimony-based catalysts; The solid-phase polymerization promoting masterbatch contains 5 to 60 mass% of a polycondensation catalyst (B) based on 100 mass% of the non-volatile content, Solubility parameter SPc (cal / cm) of thermoplastic resin (C) 3 ) 1 / 2 and the solubility parameter SPa (cal / cm 3 ) 1 / 2 The difference (SPc-SPa) is -1.0 (cal / cm 3 ) 1 / 2 More than 1.0(cal / cm 3 ) 1 / 2 is as follows: The difference (Tc-Ta) between the flow start temperature Tc (°C) of the thermoplastic resin (C) and the flow start temperature Ta (°C) of the thermoplastic resin (A) is -30°C or more and less than 50°C. Thermoplastic resin composition for solid phase polymerization. [2]: The thermoplastic resin composition for solid-state polymerization according to [1], wherein the polycondensation catalyst (B) is an acid catalyst having an aromatic ring skeleton and / or an alicyclic skeleton, and is soluble in at least 1 part by mass in 100 parts by mass of the thermoplastic resin (A). [3]: The thermoplastic resin composition for solid-state polymerization according to [1] or [2], wherein the polycondensation catalyst (B) is at least one of an alkyl phosphonic acid ester and an alkyl phosphonic acid monoester. [4]: The thermoplastic resin composition for solid-state polymerization according to any one of [1] to [3], wherein the polycondensation catalyst (B) is at least one of a sterically hindered hydroxyphenylalkyl phosphonic acid ester and a sterically hindered hydroxyphenylalkyl phosphonic acid monoester. [5]: The thermoplastic resin composition for solid-state polymerization according to any one of [1] to [4], wherein α is the molecular weight dispersity of a mixture obtained by diluting the masterbatch for solid-state polymerization promotion with a thermoplastic resin (A) so that the polycondensation catalyst (B) is 1 part by mass per 100 parts by mass of the thermoplastic resin (A), and β is the molecular weight dispersity when the mixture is solid-state polymerized for 10 hours at a temperature 40°C lower than the flow initiation temperature of the thermoplastic resin (C), and β / α is 1.00 to 1.20. [6]: A modified thermoplastic resin obtained by solid-state polymerization of the thermoplastic resin composition for solid-state polymerization according to any one of [1] to [5]. [7]: A molded article formed using the modified thermoplastic resin described in [6].

[0012] [8]: A step of obtaining a masterbatch for promoting solid-state polymerization containing a thermoplastic resin (A) and a polycondensation catalyst (B); a mixing step of adding the master batch for promoting solid-state polymerization to a thermoplastic resin (C) to be modified, which is at least one selected from the group consisting of a polyester resin (excluding polyethylene terephthalate resin), a polycarbonate resin, and a polyamide resin, mixing the mixture, and then melt-kneading the mixture to obtain a thermoplastic resin composition for solid-state polymerization according to any one of [1] to [5]; A step of solid-state polymerization is provided simultaneously with or after the mixing step. Method for producing modified thermoplastic resin. [9]: A masterbatch for promoting solid-state polymerization, used in the method for producing the modified thermoplastic resin according to [8].

[10] : A method for producing a molded article, further comprising a step of molding the modified thermoplastic resin described in [8].

[0013]

[11] : A masterbatch for promoting solid-state polymerization of polybutylene terephthalate resin, Contains a thermoplastic resin (A) and a polycondensation catalyst (B), The thermoplastic resin (A) is at least one of a polyester resin (A1) having a structural unit derived from a polyhydric alcohol and a polycarbonate resin (A2); The polyester resin (A1) has a content of structural units derived from ethylene glycol and diethylene glycol of less than 50 mol % in 100 mol % of structural units derived from a polyhydric alcohol, The polycondensation catalyst (B) is at least one selected from the group consisting of phosphorus-based catalysts, titanium-based catalysts, and antimony-based catalysts; The solid-phase polymerization promoting masterbatch contains 5 to 60 mass% of a polycondensation catalyst (B) based on 100 mass% of the non-volatile content, The haze of a sheet having a thickness of 1 mm formed from a 260°C kneaded product of a thermoplastic resin (A) / polybutylene terephthalate resin in a mass ratio of 1 / 1 is 20% or less. Masterbatch for promoting solid-state polymerization.

[12] : A masterbatch for promoting solid-state polymerization of polycyclohexylene dimethylene terephthalate resin, Contains a thermoplastic resin (A) and a polycondensation catalyst (B), The thermoplastic resin (A) is at least one of a polyester resin (A1) having a structural unit derived from a polyhydric alcohol and a polycarbonate resin (A2); The polyester resin (A1) has a content of structural units derived from ethylene glycol and diethylene glycol of less than 50 mol % in 100 mol % of structural units derived from a polyhydric alcohol, The polycondensation catalyst (B) is at least one selected from the group consisting of phosphorus-based catalysts, titanium-based catalysts, and antimony-based catalysts; The solid-phase polymerization promoting masterbatch contains 5 to 60 mass% of a polycondensation catalyst (B) based on 100 mass% of the non-volatile content, The haze of a sheet having a thickness of 1 mm formed from a 260°C kneaded product of thermoplastic resin (A) / polycyclohexylene dimethylene terephthalate resin in a mass ratio of 1 / 1 is 20% or less. Masterbatch for promoting solid-state polymerization.

[13] : A masterbatch for promoting solid-state polymerization of polycarbonate resin, Contains a thermoplastic resin (A) and a polycondensation catalyst (B), The thermoplastic resin (A) is at least one of a polyester resin (A1) having a structural unit derived from a polyhydric alcohol and a polycarbonate resin (A2); The polyester resin (A1) has a content of structural units derived from ethylene glycol and diethylene glycol of less than 50 mol % in 100 mol % of structural units derived from a polyhydric alcohol, The polycondensation catalyst (B) is at least one selected from the group consisting of phosphorus-based catalysts, titanium-based catalysts, and antimony-based catalysts; The solid-phase polymerization promoting masterbatch contains 5 to 60 mass% of a polycondensation catalyst (B) based on 100 mass% of the non-volatile content, The haze of a sheet having a thickness of 1 mm formed from a 260°C kneaded product of a thermoplastic resin (A) / polycarbonate resin in a mass ratio of 1 / 1 is 20% or less. Masterbatch for promoting solid-state polymerization. Effect of the Invention

[0014] According to the present invention, in the polycondensation reaction of the thermoplastic resin to be modified, the solid-phase polymerization time can be shortened, thereby reducing outgassing, and therefore, a high-quality and highly productive molded product can be provided. It is possible to provide a thermoplastic resin composition, a modified thermoplastic resin, and a method for producing these, as well as a solid-phase polymerization promoting masterbatch used in the production method. In addition, even when recycled thermoplastic resin is used as the modified thermoplastic resin, a thermoplastic resin composition capable of providing a molded body having similarly high quality and high productivity, a method for producing a modified thermoplastic resin, and a solid-phase polymerization promoting masterbatch used in the production method can be provided. It has an excellent effect of being able to provide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an example of an embodiment to which the present disclosure is applied will be described. However, the present disclosure is not limited to this embodiment, and other embodiments may fall within the scope of the present disclosure as long as they are consistent with the gist of the present disclosure. In addition, the numerical values ​​"A to B" specified in this specification refer to a range that satisfies numerical value A and a value greater than numerical value A, and numerical value B and a value smaller than numerical value B. Note that the numerical values ​​specified in this specification are values ​​obtained by the method disclosed in the embodiment or example. In addition, the test piece in this specification is synonymous with a sheet, a film, and a plate. Unless otherwise noted, the various components appearing in this specification may be used independently, either alone or in combination of two or more types. In addition, "thermoplastic resin (C) which is at least one selected from the group consisting of polyester resin (excluding polyethylene terephthalate resin), polycarbonate resin, and polyamide resin" may be referred to as "thermoplastic resin (C)" or "resin (C)", "masterbatch for promoting solid-state polymerization" may be referred to as "masterbatch", "thermoplastic resin (A)" may be referred to as "resin (A)", "polyester resin (A1) having a structural unit derived from polyhydric alcohol" may be referred to as "polyester resin (A1)" or "resin (A1)", "polycarbonate resin (A2)" may be referred to as "resin (A2)", and "polyamide resin (A3)" may be referred to as "resin (A3)", and "thermoplastic resin composition for solid-state polymerization" may be referred to as "thermoplastic resin composition".

[0016] 1. Molded body The molded article according to this embodiment is formed using a modified thermoplastic resin obtained by solid-state polymerization of a thermoplastic resin composition for solid-state polymerization, which is prepared by melt-kneading at least a masterbatch for promoting solid-state polymerization (hereinafter also referred to as this masterbatch) described later with a thermoplastic resin (C) to be modified. That is, the modified thermoplastic resin is a thermoplastic resin obtained by increasing the molecular weight of the thermoplastic resin (C) to be modified through solid-phase polymerization to give a high molecular weight. The thermoplastic resin composition before solid-phase polymerization may be used in the form of pellets, powder, granules, beads, or the like. The modified thermoplastic resin after solid-phase polymerization may be used as it is for forming a molded article after production, or may be used after being first made into a pellet, powder, granule, bead, or other shape.

[0017] The present molded article is any molded article molded according to the application, and examples thereof include a film, a sheet, a plate, a net, a container, a cylinder, a thread-like body such as a filament, a nonwoven fabric, a woven fabric, and other fibers. The surface of the molded article may be smooth or may have an uneven or complex shape. In addition, the solid-state polymerization promoting masterbatch and the thermoplastic resin composition for solid-state polymerization may contain any component other than the thermoplastic resin (C) and the polycondensation catalyst (B) within the scope of the present disclosure. In this case, the molded body is formed from the modified thermoplastic resin composition containing the modified thermoplastic resin and any component. Examples of optional components include resins other than the thermoplastic resin (A) or the thermoplastic resin (C) and / or catalysts, chain extenders, antioxidants, antistatic agents, surfactants, flame retardants, UV absorbers, fillers, and lubricants.

[0018] The masterbatch for promoting solid-state polymerization is a polycondensation catalyst-containing resin composition in which a polycondensation catalyst (B) is dispersed at a high concentration for polycondensing a thermoplastic resin (C), and serves to modify the thermoplastic resin (C) by mixing the masterbatch with the thermoplastic resin (C) as the main component at a specified ratio.

[0019] The thermoplastic resin composition for solid-phase polymerization is prepared by melt-kneading the thermoplastic resin (C) to be modified with at least a masterbatch for promoting solid-phase polymerization, and the thermoplastic resin (C) becomes a modified thermoplastic resin by solid-phase polymerization.

[0020] In addition, in the thermoplastic resin composition containing the thermoplastic resin (C) and the masterbatch for promoting solid-state polymerization, the thermoplastic resin (C) to be modified and the thermoplastic resin (A) contained in the masterbatch for promoting solid-state polymerization satisfy the following conditions (I) and (II). (I) Solubility parameter SPc (cal / cm) of thermoplastic resin (C) 3 ) 1 / 2 and the solubility parameter SPa (cal / cm 3 ) 1 / 2 The difference (SPc-SPa) is -1.0 (cal / cm 3 ) 1 / 2 More than 1.0(cal / cm 3 ) 1 / 2 The following is the result. (II) The difference (Tc-Ta) between the flow temperature Tc (°C) of the thermoplastic resin (C) and the flow temperature Ta (°C) of the thermoplastic resin (A) is -30°C or more and less than 50°C.

[0021] From the viewpoint of compatibility, a more preferable range is that (SPc-SPa) of (I) is -0.9 (cal / cm 3 ) 1 / 2 More than -0.8(cal / cm 3 ) 1 / 2 More preferably, the value is 0.9 (cal / cm 3 ) 1 / 2 Less than 0.8 (cal / cm 3 ) 1 / 2 The following is more preferred: From the viewpoint of the dispensability and heat resistance of the masterbatch, (Tc-Ta) of (II) is preferably -25°C or higher, more preferably -20°C or higher, and is preferably lower than 40°C, more preferably lower than 30°C.

[0022] The solubility parameter is a value calculated by the Fedors method [Polm. Eng. Sci. 14(2)152(1974)]. The flow initiation temperature can be determined using a flow tester. Specifically, for example, using a Shimadzu Corporation "CFT-EX Series" or the like, it is possible to measure the minimum temperature at which the melt viscosity of each of thermoplastic resin (A) and thermoplastic resin (C) becomes 4800 Pa s or less when the resins are passed through a capillary with a die hole diameter of φ1 mm and a die length of 1 mm under a pressure of 9.8 MPa.

[0023] By using thermoplastic resin (A) and thermoplastic resin (C) that satisfy the conditions (I) and (II), the compatibility between the thermoplastic resins is excellent, and the polycondensation catalyst (B) contained in the masterbatch for promoting solid-state polymerization is distributed homogeneously. When the masterbatch is kneaded with the thermoplastic resin (C) to be modified and subjected to solid-state polymerization, productivity is increased, and a high-quality molded product can be obtained.

[0024] The thermoplastic resin composition for solid-state polymerization, which is capable of forming a molded product having superior productivity and high quality as compared with the conventional techniques, as achieved in the present invention is due to the difference in the dispersion state of the polycondensation catalyst (B) brought about by the production process using the masterbatch for promoting solid-state polymerization of the present invention. However, it is impossible to specify in general terms the structure or characteristics of the thermoplastic resin composition due to the difference in the dispersion state.

[0025] Molded products made from thermoplastic resins are processed by various molding methods, including uniaxial molding and biaxial molding. However, recycled thermoplastic resins have inferior physical properties compared to virgin thermoplastic resins, which significantly reduces productivity. In addition, the quality of recycled thermoplastic resins is reduced, so their scope of use is limited.

[0026] On the other hand, according to the modified thermoplastic resin and molded body of the present invention, even when a recycled thermoplastic resin is used as the thermoplastic resin (C) to be modified, a modified thermoplastic resin and molded body having high quality and high productivity can be obtained. The main reason for this is the use of the master batch of the present disclosure. Each component will be described in detail below.

[0027] 1-1.Thermoplastic resin (C) The thermoplastic resin (C) is a resin that is the main component of the present molded body and is a resin to be modified. The thermoplastic resin (C) is at least one selected from the group consisting of polyester resins (excluding polyethylene terephthalate resins), polycarbonate resins, and polyamide resins, and may be amorphous or crystalline. The thermoplastic resin (C) may be a virgin resin or a recycled resin. The thermoplastic resin (C) may be linear or branched. In this specification, the term "main component" refers to a component that accounts for 70% by mass or more of the nonvolatile content of the composition (100% by mass), preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more. The thermoplastic resin (C) may be one type or a mixture of two or more types.

[0028] From the viewpoint of compatibility with thermoplastic resin (A), the solubility parameter SPa (cal / cm 3 ) 1 / 2 is 8.5(cal / cm 3 ) 1 / 2 More than 15(cal / cm 3 ) 1 / 2 It is preferable that the cal / cm 3 ) 1 / 2 More than 14(cal / cm 3 ) 1 / 2 It is more preferable that: From the viewpoint of the distributability and heat resistance of the masterbatch, the flow initiation temperature of the thermoplastic resin (C) is preferably 150°C or higher and 300°C or lower, and more preferably 160°C or higher and 280°C or lower.

[0029] [Polyester resin] The polyester resin to be modified in the present invention is not particularly limited, and typical examples include polyester resins derived from polyhydric alcohols such as diols and polyvalent carboxylic acids such as dicarboxylic acids or their ester-forming derivatives, polyester resins derived from polyhydric alcohols such as diols and polyvalent hydroxycarboxylic acids such as hydroxycarboxylic acids or their ester-forming derivatives, and mixtures thereof. However, polyethylene terephthalate resin is excluded.

[0030] Specific examples of polyester resins include polybutylene terephthalate resin (PBT resin), polycyclohexylene dimethylene terephthalate resin (PCT resin), polytrimethylene terephthalate resin (PTT resin), polybutylene naphthalate resin (PBN resin), polybutylene adipate terephthalate resin (PBAT resin), polybutylene succinate resin (PBS resin), and the like. From the viewpoint of productivity and quality of the present molded article, it is preferable to use a polybutylene phthalate resin or a polycyclohexylene dimethylene terephthalate resin as the polyester resin to be modified.

[0031] (Polybutylene terephthalate resin) The polybutylene terephthalate resin (PBT resin) is not limited as long as it is a resin having butylene terephthalate units, and is, for example, a polybutylene terephthalate resin obtained by polycondensation of a dicarboxylic acid component containing at least terephthalic acid or its ester-forming derivative (C1-6 alkyl ester, acid halide, etc.) and a glycol component containing at least an alkylene glycol having 4 carbon atoms (1,4-butanediol) or its ester-forming derivative (acetylated product, etc.). The polybutylene terephthalate resin is preferably a butylene terephthalate unit as a main constituent unit, and is not limited to a homopolybutylene terephthalate resin, and may be a copolymer containing 60 mol % or more (particularly 75 mol % to 95 mol %) of butylene terephthalate units.

[0032] In the preparation of polybutylene terephthalate resin, examples of dicarboxylic acid components other than terephthalic acid and its ester-forming derivatives include C8-14 aromatic dicarboxylic acids such as isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, and 4,4'-dicarboxydiphenyl ether; C4-16 alkane dicarboxylic acids such as succinic acid, adipic acid, azelaic acid, and sebacic acid; C5-10 cycloalkane dicarboxylic acids such as cyclohexane dicarboxylic acid; and ester-forming derivatives of these dicarboxylic acid components (C1-6 alkyl ester derivatives, acid halides, etc.). These dicarboxylic acid components can be used alone or in combination of two or more.

[0033] Among these dicarboxylic acid components other than terephthalic acid and its ester-forming derivatives, C8-12 aromatic dicarboxylic acids such as isophthalic acid, and C6-12 alkanedicarboxylic acids such as adipic acid, azelaic acid, and sebacic acid are more preferred.

[0034] In the preparation of polybutylene terephthalate resin, examples of glycol components other than 1,4-butanediol include C2-10 alkylene glycols such as ethylene glycol, propylene glycol, trimethylene glycol, 1,3-butylene glycol, hexamethylene glycol, neopentyl glycol, and 1,3-octanediol; polyoxyalkylene glycols such as diethylene glycol, triethylene glycol, and dipropylene glycol; alicyclic diols such as cyclohexanedimethanol and hydrogenated bisphenol A; aromatic diols such as bisphenol A and 4,4'-dihydroxybiphenyl; C2-4 alkylene oxide adducts of bisphenol A, such as 2-mol ethylene oxide adducts of bisphenol A and 3-mol propylene oxide adducts of bisphenol A; and ester-forming derivatives of these glycols (acetylated products, etc.). These glycol components can be used alone or in combination of two or more.

[0035] Among these glycol components other than 1,4-butanediol, C2-6 alkylene glycols such as ethylene glycol and trimethylene glycol, polyoxyalkylene glycols such as diethylene glycol, and alicyclic diols such as cyclohexanedimethanol are more preferred.

[0036] Examples of comonomer components that can be used in addition to the dicarboxylic acid component and the glycol component include aromatic hydroxycarboxylic acids such as 4-hydroxybenzoic acid, 3-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 4-carboxy-4'-hydroxybiphenyl, etc.; aliphatic hydroxycarboxylic acids such as glycolic acid and hydroxycaproic acid; C3-12 lactones such as propiolactone, butyrolactone, valerolactone, caprolactone (ε-caprolactone, etc.); and ester-forming derivatives of these comonomer components (C1-6 alkyl ester derivatives, acid halides, acetylated products, etc.).

[0037] The intrinsic viscosity (IV) of the polybutylene terephthalate resin is not limited, but is preferably 0.5 dl / g or more, more preferably 0.6 dl / g or more. The upper limit is not particularly limited, but is usually 2.0 dl / g from the viewpoint of handling during molding processing in consideration of the melt viscosity. By making the intrinsic viscosity 0.6 dl / g or more, a more excellent effect can be obtained in terms of moldability. The intrinsic viscosity of the polybutylene terephthalate resin is a value measured by dissolving the polybutylene terephthalate resin pellets in phenol / 1,1,2,2-tetrachloroethane = 1 / 1 and using an automatic viscosity measuring device "SS-600-L2" manufactured by Shibayama Scientific Instruments Co., Ltd.

[0038] (Polycyclohexylene dimethylene terephthalate resin) The polycyclohexylene dimethylene terephthalate resin is not limited as long as it is a resin having a cyclohexylene dimethylene terephthalate unit, and is obtained, for example, by polycondensing a dicarboxylic acid component containing at least terephthalic acid or its ester-forming derivative (C1-6 alkyl ester, acid halide, etc.) and a glycol component containing at least 1,4-cyclohexanedimethanol or its ester-forming derivative (acetylated product, etc.). The polycyclohexylene dimethylene terephthalate resin preferably has a cyclohexylene dimethylene terephthalate unit as a main constituent unit, and is not limited to a homopolycyclohexylene dimethylene terephthalate resin, and may be a copolymer containing 60 mol % or more (particularly 75 mol % to 95 mol %) of cyclohexylene dimethylene terephthalate units.

[0039] In the preparation of polycyclohexylene dimethylene terephthalate resin, examples of dicarboxylic acid components other than terephthalic acid and its ester-forming derivatives include C8-14 aromatic dicarboxylic acids such as isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, and 4,4'-dicarboxydiphenyl ether; C4-16 alkane dicarboxylic acids such as succinic acid, adipic acid, azelaic acid, and sebacic acid; C5-10 cycloalkane dicarboxylic acids such as cyclohexane dicarboxylic acid; and ester-forming derivatives of these dicarboxylic acid components (C1-6 alkyl ester derivatives, acid halides, etc.). These dicarboxylic acid components can be used alone or in combination of two or more.

[0040] Among these dicarboxylic acid components other than terephthalic acid and its ester-forming derivatives, C8-12 aromatic dicarboxylic acids such as isophthalic acid, and C6-12 alkanedicarboxylic acids such as adipic acid, azelaic acid, and sebacic acid are more preferred.

[0041] In the preparation of polycyclohexylene dimethylene terephthalate resin, examples of glycol components other than cyclohexane dimethanol include C2-10 alkylene glycols such as 1,4-butanediol, ethylene glycol, propylene glycol, trimethylene glycol, 1,3-butylene glycol, hexamethylene glycol, neopentyl glycol, and 1,3-octanediol; polyoxyalkylene glycols such as diethylene glycol, triethylene glycol, and dipropylene glycol; alicyclic diols such as hydrogenated bisphenol A; aromatic diols such as bisphenol A and 4,4'-dihydroxybiphenyl; C2-4 alkylene oxide adducts of bisphenol A, such as 2-mol ethylene oxide adducts of bisphenol A and 3-mol propylene oxide adducts of bisphenol A; and ester-forming derivatives of these glycols (acetylated products, etc.). These glycol components can be used alone or in combination of two or more.

[0042] Among these glycol components other than cyclohexanedimethanol, 1,4-butanediol, C2-6 alkylene glycols such as ethylene glycol and trimethylene glycol, and alicyclic diols such as polyoxyalkylene glycols such as diethylene glycol, and the like are more preferred.

[0043] Examples of comonomer components that can be used in addition to the dicarboxylic acid component and the glycol component include aromatic hydroxycarboxylic acids such as 4-hydroxybenzoic acid, 3-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 4-carboxy-4'-hydroxybiphenyl, etc.; aliphatic hydroxycarboxylic acids such as glycolic acid and hydroxycaproic acid; C3-12 lactones such as propiolactone, butyrolactone, valerolactone, caprolactone (ε-caprolactone, etc.); and ester-forming derivatives of these comonomer components (C1-6 alkyl ester derivatives, acid halides, acetylated products, etc.).

[0044] The intrinsic viscosity (IV) of the polycyclohexylene dimethylene terephthalate resin is not limited, but is preferably 0.4 dl / g or more, more preferably 0.5 dl / g or more. The upper limit is not particularly limited, but is usually 1.5 dl / g from the viewpoint of handling during molding processing in consideration of the melt viscosity. By making the intrinsic viscosity 0.5 dl / g or more, a more excellent effect can be obtained in terms of moldability. The intrinsic viscosity of the polybutylene terephthalate resin is a value measured by dissolving the polybutylene terephthalate resin pellets in phenol / 1,1,2,2-tetrachloroethane = 1 / 1 and using an automatic viscosity measuring device "SS-600-L2" manufactured by Shibayama Scientific Instruments Manufacturing Co., Ltd.

[0045] [Polycarbonate resin] The polycarbonate resin (PC resin) is not particularly limited and may be an aliphatic polycarbonate or an aromatic polycarbonate. From the standpoint of impact resistance, heat resistance, etc., an aromatic polycarbonate resin is preferred. The aromatic polycarbonate resin is a thermoplastic polymer or copolymer, which may be branched, obtained by reacting an aromatic dihydroxy compound or a small amount of a polyhydroxy compound with phosgene or a carbonic acid diester. The method for producing the aromatic polycarbonate resin is not particularly limited, and it is possible to use a resin produced by the conventionally known phosgene method (interfacial polymerization method) or melting method (ester exchange method). In addition, when the melting method is used, it is possible to use an aromatic polycarbonate resin with an adjusted amount of OH groups in the terminal group.

[0046] Examples of the aromatic dihydroxy compound as the raw material include 2,2-bis(4-hydroxyphenyl)propane (=bisphenol A), tetramethylbisphenol A, bis(4-hydroxyphenyl)-p-diisopropylbenzene, hydroquinone, resorcinol, 4,4-dihydroxydiphenyl, etc., and preferably bisphenol A. In addition, a compound in which one or more tetraalkylphosphonium sulfonates are bonded to the above aromatic dihydroxy compound can also be used.

[0047] To obtain a branched aromatic polycarbonate resin, a part of the aromatic dihydroxy compound may be replaced with the following branching agents, namely, polyhydroxy compounds such as phloroglucin, 4,6-dimethyl-2,4,6-tri(4-hydroxyphenyl)heptene-2, 4,6-dimethyl-2,4,6-tri(4-hydroxyphenyl)heptane, 2,6-dimethyl-2,4,6-tri(4-hydroxyphenyl)heptene-3, 1,3,5-tri(4-hydroxyphenyl)benzene, 1,1,1-tri(4-hydroxyphenyl)ethane, and compounds such as 3,3-bis(4-hydroxyaryl)oxindole (=isatin bisphenol), 5-chloruisatin, 5,7-dichloruisatin, and 5-bromoisatin. The amount of these replacing compounds used is usually 0.0110 mol %, and preferably 0.12 mol %, based on the aromatic dihydroxy compound.

[0048] Among the above-mentioned aromatic polycarbonate resins, polycarbonate resins derived from 2,2-bis(4-hydroxyphenyl)propane or polycarbonate copolymers derived from 2,2-bis(4-hydroxyphenyl)propane and other aromatic dihydroxy compounds are preferred. Also, copolymers mainly made of polycarbonate resins, such as copolymers with polymers or oligomers having a siloxane structure, may be used.

[0049] The above-mentioned aromatic polycarbonate resins may be used alone or in combination of two or more.

[0050] To adjust the molecular weight of the aromatic polycarbonate resin, a monovalent aromatic hydroxy compound may be used. Examples of the monovalent aromatic hydroxy compound include m- and p-methylphenol, m- and p-propylphenol, p-tert-butylphenol, and p-long-chain alkyl-substituted phenol.

[0051] The intrinsic viscosity (IV) of the polycarbonate resin is not limited, but is preferably 0.3 dl / g or more, more preferably 0.4 dl / g or more. The upper limit is not particularly limited, but is usually 1.2 dl / g from the viewpoint of handling during molding processing in consideration of the melt viscosity. By making the intrinsic viscosity 0.4 dl / g or more, a more excellent effect can be obtained in terms of moldability. The intrinsic viscosity of the polycarbonate resin is a value measured by dissolving polycarbonate resin pellets in a methylene chloride solution and using an automatic viscosity measuring device "SS-600-L2" manufactured by Shibayama Scientific Instruments Manufacturing Co., Ltd.

[0052] [Polyamide resin] Polyamide resins (PA resins) are polyamide polymers that have acid amide groups (-CONH-) in their molecules and can be melted by heating. Specifically, they include various polyamide resins such as polycondensates of lactams, polycondensates of diamine compounds and dicarboxylic acids, and polycondensates of ω-aminocarboxylic acids, as well as copolymer polyamide resins and blends of these.

[0053] Examples of lactams that are raw materials for polycondensation of polyamide resins include ε-caprolactam and ω-laurolactam.

[0054] Examples of the diamine compound include aliphatic, alicyclic, and aromatic diamines such as tetramethylenediamine, hexamethylenediamine, undecamethylenediamine, dodecamethylenediamine, 2-methylpentamethylenediamine, (2,2,4- or 2,4,4-)trimethylhexamethylenediamine, 5-methylnonamethylenediamine, metaxylylenediamine (MXDA), paraxylylenediamine, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, bis(4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(aminopropyl)piperazine, and aminoethylpiperazine.

[0055] Examples of the dicarboxylic acid compound include aliphatic, alicyclic, and aromatic dicarboxylic acids such as adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodium sulfoisophthalic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid.

[0056] Examples of the ω-aminocarboxylic acid include amino acids such as 6-aminocaproic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, and para-aminomethylbenzoic acid.

[0057] Specific examples of polyamide resins obtained by polycondensation of these raw materials include PA4, PA6, PA11, PA12, PA46, PA66, PA610, PA612, polyhexamethylene terephthalamide (PA6T), polyhexamethylene isophthalamide (PA6I), polymetaxylylene adipamide (PAMXD6), polymetaxylylene dodecamide (PAMXD12), PA9T, PA9MT, etc. In the present invention, these polyamide homopolymers or copolymers can be used alone or in the form of a mixture. Among the polyamide resins described above, from the viewpoint of moldability, polyamide 6, polyamide 66, polyamide 11, polyamide 12, or a xylylenediamine-based polyamide resin (MX nylon) obtained by polycondensation of an α,ω-linear aliphatic dibasic acid and xylylenediamine is more preferred.

[0058] The relative viscosity (RV) of the polyamide resin is not limited, but is preferably 1.5 dl / g or more, more preferably 1.6 dl / g or more. The upper limit is not particularly limited, but is usually 5.0 dl / g from the viewpoint of handling during molding processing taking into account the melt viscosity. By making the relative viscosity 1.6 dl / g or more, more excellent effects can be obtained in terms of moldability. The intrinsic viscosity of the polyamide resin is a value measured by dissolving polyamide resin pellets in a 96 mass % sulfuric acid solution at a concentration of 1 g / dl and using an automatic viscosity measuring device "SS-600-L2" manufactured by Shibayama Scientific Instruments Manufacturing Co., Ltd.

[0059] The amount of the masterbatch for promoting solid-state polymerization of the present disclosure added to the thermoplastic resin (C) is not particularly limited and can be appropriately designed depending on the application. For example, the amount is preferably 0.2 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 1 to 10 parts by mass, relative to 100 parts by mass of the thermoplastic resin (C).

[0060] A thermoplastic resin composition is produced from a mixture of only the thermoplastic resin (C) and the masterbatch, and a molded body can be obtained through a modified thermoplastic resin by solid-state polymerization. The masterbatch and the thermoplastic resin composition may also be a mixture to which any optional components have been added. As the optional additives, there can be mentioned, within the scope of the gist of the present disclosure, resins other than the thermoplastic resin (A) or the thermoplastic resin (C) and / or catalysts, chain extenders, antioxidants, antistatic agents, surfactants, flame retardants, ultraviolet absorbers, fillers, and lubricants.

[0061] 2.Masterbatches The masterbatch for promoting solid-state polymerization of the present disclosure is used to promote solid-state polymerization of a thermoplastic resin (C). The masterbatch contains a thermoplastic resin (A) and a polycondensation catalyst (B). It is preferable that the masterbatch further contains an antioxidant. From the viewpoint of obtaining a higher quality modified thermoplastic resin and molded body, the masterbatch preferably contains 50% by mass or more of the thermoplastic resin (A) and the polycondensation catalyst (B), more preferably 60% by mass or more, and even more preferably 70% by mass or more in 100% by mass of the masterbatch. The masterbatch may contain 100% by mass of the thermoplastic resin (A) and the polycondensation catalyst (B). The polycondensation catalyst (B) is a catalyst for promoting solid-phase polymerization of the thermoplastic resin (C) to be modified.

[0062] According to the present masterbatch, even when a recycled thermoplastic resin is used as the thermoplastic resin (C) to be modified, it is possible to provide a modified thermoplastic resin and a molded article that are high in quality and high in productivity. The main reason for this is that by making the polycondensation catalyst (B) into a masterbatch, the polycondensation catalyst (B) can be uniformly dispersed in the thermoplastic resin (C). And, the thermoplastic resin composition in which the polycondensation catalyst is uniformly dispersed can prevent localized polycondensation in the subsequent solid-phase polymerization step, so that a high-quality modified thermoplastic resin and a molded article can be obtained.

[0063] Each component will be described in detail below. Each component may be used independently, either alone or in combination of two or more.

[0064] 2-1. Thermoplastic resin (A) The thermoplastic resin (A) is a resin that functions as a dispersion medium for dispersing the polycondensation catalyst (B) in the masterbatch, and is at least one selected from the group consisting of polyester resin (A1), polycarbonate resin (A2), and polyamide resin (A3). The polyester resin (A1) has at least a structural unit derived from a polyhydric alcohol, and the content of structural units derived from ethylene glycol and diethylene glycol in 100 mol % of the structural units derived from the polyhydric alcohol is less than 50 mol %. The thermoplastic resin (A) plays a role of efficiently homogenizing the polycondensation catalyst (B) when kneaded with the thermoplastic resin (C) to be modified.

[0065] From the viewpoint of compatibility with thermoplastic resin (C), the solubility parameter SPa (cal / cm 3 ) 1 / 2 is 8.5(cal / cm 3 ) 1 / 2 More than 15(cal / cm 3 ) 1 / 2 It is preferable that the cal / cm 3 ) 1 / 2 More than 14(cal / cm 3) 1 / 2 It is more preferable that: From the viewpoint of the distributability and heat resistance of the masterbatch, the flow initiation temperature of the thermoplastic resin (A) is preferably 150°C or higher and 300°C or lower, and more preferably 160°C or higher and 280°C or lower.

[0066] [Resin (A1)] Resin (A1) is a polyester resin having structural units derived from a polyhydric alcohol, and the content of structural units derived from ethylene glycol and / or diethylene glycol in 100 mol % of the structural units derived from a polyhydric alcohol is less than 50 mol %. That is, the structural units derived from ethylene glycol and the structural units derived from diethylene glycol each account for less than 50 mol % of 100 mol % of the structural units derived from the polyhydric alcohol, and when both are contained, the total of the structural units derived from ethylene glycol and diethylene glycol is less than 50 mol %.

[0067] The structural units derived from ethylene glycol and diethylene glycol are more preferably less than 40 mol%, and even more preferably less than 30 mol%, relative to 100 mol% of the structural units derived from polyhydric alcohol. The content of the structural units derived from ethylene glycol is less than 50 mol%, so that the compatibility with the thermoplastic resin (C) is excellent. The lower limit is not limited, and may be 0 mol%.

[0068] Such polyester resins can be obtained by using polyhydric alcohols and polycarboxylic acids or their ester-forming derivatives, and adjusting the type and amount of polyhydric alcohol used during polymerization. Note that "polyhydric alcohol" refers to a polyol, a compound having two or more hydroxyl groups. As the polyvalent carboxylic acid or an ester-forming derivative thereof, a polyester resin containing structural units derived from terephthalic acid or an ester-forming derivative thereof and / or isophthalic acid or an ester-forming derivative thereof is preferred.

[0069] In addition, in the resin (A1), the structural units derived from terephthalic acid or its ester-forming derivatives and / or isophthalic acid or its ester-forming derivatives are preferably 50 mol% or more, more preferably 60 mol% or more, of the structural units derived from polyvalent carboxylic acid (100 mol%). By containing 50 mol% or more of the structural units derived from terephthalic acid or its ester-forming derivatives and / or isophthalic acid or its ester-forming derivatives, the compatibility with the thermoplastic resin (C) is improved. The upper limit is not limited and may be 100 mol%.

[0070] The ester-forming derivatives of polycarboxylic acids include lower alkyl esters and acid halides of dicarboxylic acids. Examples of lower alkyl esters of dicarboxylic acids include methyl esters, ethyl esters, hydroxyethyl esters, and hydroxybutyl esters. Specific examples of halides of dicarboxylic acids include acid chlorides, acid bromides, and acid iodides. Polyhydric alcohols are alcohols with two or more hydroxyl groups in the molecule, and are alcohols with a structure in which one hydroxyl group is substituted for each of two or more carbon atoms of chain aliphatic hydrocarbons, cyclic aliphatic hydrocarbons, and aromatic hydrocarbons.

[0071] Examples of the diol component include various diols. For example, aliphatic diols such as ethylene glycol, diethylene glycol, propanediol, butanediol, 2-methyl-1,3-propanediol, neopentyl glycol, and hexanediol, saturated alicyclic primary diols such as 1,4-cyclohexanedimethanol, 1,4-cyclohexylenedimethanol, decahydronaphthalenedimethanol, decahydronaphthalenediethanol, norbornanedimethanol, norbornanediethanol, tricyclodecanedimethanol, tricyclodecaneethanol, tetracyclododecanedimethanol, tetracyclododecanediethanol, decalindimethanol, and decalindiethanol, 2,6-dihydroxy-9-oxabicyclo[3,3,1]nonane, 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5 Examples of the diol include saturated heterocyclic primary diols containing cyclic ethers such as 5-methylol-5-ethyl-2-(1,1-dimethyl-2-hydroxyethyl)-1,3-dioxane and isosorbide, as well as alicyclic diols such as cyclohexanediol, bicyclohexyl-4,4'-diol, 2,2-bis(4-hydroxycyclohexylpropane), 2,2-bis(4-(2-hydroxyethoxy)cyclohexyl)propane, cyclopentanediol, 3-methyl-1,2-cyclopentadiol, 4-cyclopentene-1,3-diol and adamantanediol, and aromatic diols such as bisphenol A, bisphenol S, styrene glycol, 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene and 9,9'-bis(4-hydroxyphenyl)fluorene. Examples of trifunctional or higher polyhydric alcohols include glycerin, trimethylolpropane, and pentaerythritol.

[0072] Examples of the dicarboxylic acid include adipic acid, sebacic acid, azelaic acid, dodecanedicarboxylic acid, glutaric acid, succinic acid, and other fatty acid dicarboxylic acids, terephthalic acid, naphthalenedicarboxylic acid, isophthalic acid, and other aromatic dicarboxylic acids, 1,4-cyclohexanedicarboxylic acid, and other alicyclic dicarboxylic acids, and ester-forming derivatives thereof. Examples of trifunctional or higher polyvalent carboxylic acids include trimellitic acid, trimesic acid, pyromellitic acid, trimellitic anhydride, phthalic anhydride, p-hydroxybenzoic acid, and trimellitic acid monopotassium salt.

[0073] Specific examples of the resin (A1) include polybutylene terephthalate resin (PBT resin), polycyclohexylene dimethylene terephthalate resin (PCT resin), polytrimethylene terephthalate resin (PTT resin), polybutylene naphthalate resin (PBN resin), polybutylene adipate terephthalate resin (PBAT resin), polybutylene succinate resin (PBS resin), and the like. Polybutylene terephthalate resin or polycyclohexylene dimethylene terephthalate resin is preferred because of its excellent moldability and recyclability.

[0074] [Resin (A2)] Resin (A2) is a polycarbonate resin, and may be the same as the polycarbonate resin described as thermoplastic resin (C). From the viewpoints of compatibility with thermoplastic resin (C) and impact resistance, heat resistance, etc., aromatic polycarbonate resins are more preferred.

[0075] [Resin (A3)] Resin (A3) is a polyamide resin, and may be the same as the polyamide resin described as thermoplastic resin (C). From the viewpoints of compatibility with thermoplastic resin (C) and moldability, polyamide 6, polyamide 66, polyamide 11, polyamide 12, or xylylenediamine-based polyamide resin (MX nylon) obtained by polycondensation of α,ω-linear aliphatic dibasic acid and xylylenediamine is more preferred.

[0076] The thermoplastic resin (A) is at least one selected from the group consisting of polyester resin (A1), polycarbonate resin (A2), and polyamide resin (A3). The combination of thermoplastic resin (A) and thermoplastic resin (C) may be any combination as long as the solubility parameter and flow starting temperature satisfy the above conditions (I) and (II), and the thermoplastic resin (A) may be the same as or different from the thermoplastic resin (C). When the thermoplastic resin (A) and the thermoplastic resin (C) are the same thermoplastic resin, the compatibility between the thermoplastic resins is excellent, the processability and dispersibility of the modified thermoplastic resin after solid-state polymerization are good, and the heat resistance of the molded body is also high. This is preferable.

[0077] Specifically, for example, when the thermoplastic resin (C) is a polyester resin, the thermoplastic resin (A) is preferably a polyester resin (A1). Specifically, for example, when the plastic resin (C) is a polybutylene terephthalate resin, the polyester resin (A1) is more preferably a polybutylene terephthalate resin, and when the plastic resin (C) is a polycyclohexylene dimethylene terephthalate resin, the polyester resin (A1) is more preferably a polycyclohexylene dimethylene terephthalate resin.

[0078] When the thermoplastic resin (C) is a polycarbonate resin, the thermoplastic resin (A) is preferably a polycarbonate resin (A2).

[0079] When the thermoplastic resin (C) is a polyamide resin, the thermoplastic resin (A) is preferably a polyamide resin (A3). Specific examples of this combination include not only the combination of the same resin, but also polyamide 6 and polyamide 66, polyamide 6 and polyamide MXD6, or polyamide 11 and polyamide 12.

[0080] Combinations of thermoplastic resins in which the thermoplastic resin (A) and the thermoplastic resin (C) are different include: From the viewpoints of compatibility, distributability of the masterbatch, and heat resistance, when the thermoplastic resin (C) is a polyester resin, the thermoplastic resin (A) is preferably a polycarbonate resin (A2), and when the thermoplastic resin (C) is a polycarbonate resin, the thermoplastic resin (A) is preferably a polyester resin (A1).

[0081] 2-2. Polycondensation catalyst (B) The polycondensation catalyst (B) is at least one selected from phosphorus-based catalysts, titanium-based catalysts, and antimony-based catalysts. The master batch is a resin composition in which the polycondensation catalyst (B) is dispersed at a high concentration, and is mixed with the thermoplastic resin (C) as the main component at a specified ratio to modify the thermoplastic resin (C).

[0082] As a result of intensive research, the present inventors have found that by setting the content of the polycondensation catalyst (B) to 5-60% by mass in 100% by mass of the non-volatile content of the masterbatch and using at least one catalyst selected from phosphorus-based catalysts, titanium-based catalysts, and antimony-based catalysts, the molecular weight of the thermoplastic resin (C) to be modified can be increased to a high molecular weight in a shorter time than before. From the viewpoint of improving processability, the content of the polycondensation catalyst (B) in 100% by mass of the non-volatile content of the masterbatch is preferably 55% by mass or less, and more preferably 50% by mass or less. In addition, from the viewpoint of enhancing the polymerization promotion effect of the masterbatch during solid-phase polymerization, the lower limit is more preferably 7% by mass, and even more preferably 10% by mass.

[0083] A suitable example of the polycondensation catalyst (B) is preferably an acid catalyst. It is also preferable that the catalyst has an aromatic ring skeleton and / or an alicyclic skeleton. Furthermore, the catalyst is preferably soluble in at least 1 part by mass in 100 parts by mass of the thermoplastic resin (A). The solubility can be confirmed by the method of the examples described later. By having an aromatic ring skeleton and / or an alicyclic skeleton in the polycondensation catalyst (B), the compatibility with the thermoplastic resin (A) in the master batch can be improved. In addition, the compatibility with the thermoplastic resin (C) to be modified can be improved.

[0084] The aromatic ring skeleton includes a carbon ring skeleton, a heterocyclic skeleton, and a compound in which these are combined. The number of ring carbon atoms of the aromatic ring skeleton is preferably 3 to 20, more preferably 4 to 16, 5 to 14, or 6 to 10. Examples of the aromatic ring skeleton include a benzene ring skeleton, a naphthalene ring skeleton, and an anthracene ring skeleton. Examples of the alicyclic skeleton include an alicyclic hydrocarbon skeleton having 5 to 20 carbon atoms, such as a cyclopentane skeleton, a cyclohexane skeleton, a cyclooctane skeleton, a cyclodecane skeleton, an admantane skeleton, a norbornane skeleton, a dicyclopentane skeleton, and a tricyclodecane skeleton. In addition, it may be a heterocycle such as morpholine.

[0085] In order to prevent aggregation of the polycondensation catalyst (B) itself, it is preferred that the aromatic ring skeleton and / or the alicyclic skeleton have an isobutyl group, a sec-butyl group, a tert-butyl group, or the like as a substituent.

[0086] Examples of the phosphorus catalyst include phosphoric acid, trimethyl phosphate, triethyl phosphate, triphenyl phosphate, acidic methyl phosphate, and other phosphoric acids, their alkyl esters, and phenyl esters, phosphorous acid, trimethyl phosphite, triethyl phosphite, and other phosphorous acids, their alkyl esters, and phenyl esters, methylphosphonic acid, phenylphosphonic acid, benzylphosphonic acid, and phosphonic acids, such as methylphosphonic acid methyl ester, phenylphosphonic acid ethyl ester, and benzylphosphonic acid phenyl ester, their alkyl esters, and phenyl esters, etc. From the viewpoint of the molecular weight increasing effect, alkylphosphonic acid esters or alkylphosphonic acid monoesters are preferred, and sterically hindered hydroxyphenyl alkylphosphonic acid esters or sterically hindered hydroxyphenyl alkylphosphonic acid monoesters are more preferred.

[0087] A suitable example of the sterically hindered hydroxyphenylalkylphosphonic acid ester or monoester is represented by the general formula (1). Note that the term "ester" as used herein includes salts containing an ester group, as described below. [ka] In the formula, n is 1 to 6; R 1 is an isopropyl group, a tert-butyl group, a cyclohexyl group, or a group in which 1 to 3 hydrogen atoms of a cyclohexyl group are each independently substituted with an alkyl group having 1 to 4 carbon atoms; R 2 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a cyclohexyl group, or a group in which 1 to 3 hydrogen atoms of a cyclohexyl group are each independently substituted with an alkyl group having 1 to 4 carbon atoms; R 3 is a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a phenyl group or a naphthyl group which may have a substituent, the substituent being an alkyl group having 1 to 4 carbon atoms; R 4 is a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a phenyl group or a naphthyl group which may have a substituent, and the substituent is an alkyl group having 1 to 4 carbon atoms, or [ka] represents M r+ is a metal cation having a valence of r, where r is 1 to 3.

[0088] In the general formula (1), the alkyl group having 1 to 20 carbon atoms is a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, etc., and may be linear or branched. Among these, an alkyl group having 2 to 4 carbon atoms is more preferred. The alkyl group having 1 to 4 carbon atoms which is substituted with the cyclohexyl group preferably has 1 to 3 substituents, and particularly preferably has 1 or 2 substituents, and is a branched or unbranched alkyl radical. Examples of the alkyl group having 1 to 4 carbon atoms which is substituted with the cyclohexyl group include cyclopentyl, methylcyclopentyl, dimethylcyclopentyl, cyclohexyl, methylcyclohexyl, dimethylcyclohexyl, trimethylcyclohexyl, and tert-butylcyclohexyl. In addition, the number of the substituents of the phenyl group or naphthyl group, which may have an alkyl group having 1 to 4 carbon atoms as a substituent, is preferably 1 to 3, and particularly preferably 1 or 2. In addition, the preferable examples include o-methylphenyl, m-methylphenyl or p-methylphenyl, 2,3-dimethylphenyl, 2,4-dimethylphenyl, 2,5-dimethylphenyl, 2,6-dimethylphenyl, 3,4-dimethylphenyl, and 3,5-dimethylphenyl. 2-methyl-6-ethylphenyl, 4-tert-butylphenyl, 2-ethylphenyl, 2,6-diethylphenyl, 1-methylnaphthyl, and 2-methylnaphthyl. 4-methylnaphthyl, 1,6-dimethylnaphthyl, and 4-tert-butylnaphthyl can be exemplified. The monovalent to trivalent metal cation is preferably an alkali metal cation, an alkaline earth metal cation, a heavy metal cation, or an aluminum cation. + , K + , Mg 2+ , Ca 2+ , B.A. 2+ , Zn 2+ , Al 3+ Among these, Ca is particularly 2+ is preferred. R 1 or R 2 It is preferable that R has at least one tert-butyl group. 1 and R 2 is a tert-butyl group. n is preferably 1 or 2, and particularly preferably 1.

[0089] Suitable examples of the above general formula (1) include the following compounds: In the following compounds, t-Bu means a tertiary butyl group, and Et means an ethyl group. [ka]

[0090] Examples of the titanium catalyst include titanium complexes, titanium alkoxides such as tetra-i-propyl titanate, tetra-n-butyl titanate, and tetra-n-butyl titanate tetramer, titanium oxide, and titanium acetylacetonate.

[0091] Examples of antimony-based catalysts include antimony oxides such as antimony trioxide and antimony pentoxide, antimony carboxylic acids such as antimony acetate, antimony oxalate and antimony potassium tartrate, and antimony alkoxides such as antimony tri-n-butoxide and antimony triethoxide.

[0092] 2-3.Other ingredients The master batch may contain any component other than the thermoplastic resin (A) and the polycondensation catalyst (B). For example, the above-mentioned resins, chain extenders, antioxidants, antistatic agents, surfactants, flame retardants, ultraviolet absorbers, fillers, etc. are exemplified. In particular, in order to maintain the catalytic activity of the polycondensation catalyst (B) at a high level, it is very effective to use the polycondensation catalyst (B) in combination with an antioxidant.

[0093] Examples of the antioxidant include phenol-based antioxidants, phosphorus-based antioxidants, amine-based antioxidants, and sulfur-based antioxidants. In order to suppress the oxidative deterioration of the polycondensation catalyst (B) at high temperatures, phosphorus-based antioxidants are preferred.

[0094] When an antioxidant is contained, from the viewpoint of improving the heat resistance of the final molded body, the effective content of the antioxidant in the master batch is preferably 0.01 to 3 mass%, and more preferably 0.02 to 1 mass%.

[0095] 2-4. Characteristics of master batches When the thermoplastic resin (C) is a polybutylene terephthalate resin, the masterbatch contains a thermoplastic resin (A) and a polycondensation catalyst (B), The thermoplastic resin (A) is at least one of a polyester resin (A1) having a structural unit derived from a polyhydric alcohol and a polycarbonate resin (A2); The polyester resin (A1) has a content of structural units derived from ethylene glycol and diethylene glycol of less than 50 mol % in 100 mol % of structural units derived from a polyhydric alcohol, The polycondensation catalyst (B) is at least one selected from the group consisting of phosphorus-based catalysts, titanium-based catalysts, and antimony-based catalysts; The solid-phase polymerization promoting masterbatch contains 5 to 60 mass% of a polycondensation catalyst (B) based on 100 mass% of the non-volatile content, A sheet having a thickness of 1 mm formed from a mixture of thermoplastic resin (A) and polybutylene terephthalate resin in a mass ratio of 1 / 1 at 260°C has a haze of preferably 20% or less, more preferably 15% or less, and particularly preferably 10% or less.

[0096] By using a thermoplastic resin (A) that satisfies these conditions, compatibility with the polybutylene terephthalate resin, which is the thermoplastic resin (C), is excellent, and productivity is increased when the resin is kneaded with the polybutylene terephthalate resin to be modified and subjected to solid-state polymerization, thereby making it possible to obtain high-quality polybutylene terephthalate resin molded products.

[0097] More preferred examples of the thermoplastic resin (A) include resin (A1) and resin (A2). Resin (A1) is even more preferred, and polybutylene terephthalate resin is particularly preferred.

[0098] When the thermoplastic resin (C) is a polycyclohexylene dimethylene terephthalate resin, the masterbatch contains a thermoplastic resin (A) and a polycondensation catalyst (B), The thermoplastic resin (A) is at least one of a polyester resin (A1) having a structural unit derived from a polyhydric alcohol and a polycarbonate resin (A2); The polyester resin (A1) has a content of structural units derived from ethylene glycol and diethylene glycol of less than 50 mol % in 100 mol % of structural units derived from a polyhydric alcohol, The polycondensation catalyst (B) is at least one selected from the group consisting of phosphorus-based catalysts, titanium-based catalysts, and antimony-based catalysts; The solid-phase polymerization promoting masterbatch contains 5 to 60 mass% of a polycondensation catalyst (B) based on 100 mass% of the non-volatile content, A sheet having a thickness of 1 mm formed from a mixture of thermoplastic resin (A) and polycyclohexylene dimethylene terephthalate resin in a mass ratio of 1 / 1 at 260°C has a haze of preferably 20% or less, more preferably 15% or less, and particularly preferably 10% or less.

[0099] Use of a thermoplastic resin (A) that satisfies these conditions provides excellent compatibility with the polycyclohexylene dimethylene terephthalate resin, which is the thermoplastic resin (C), and increases productivity when mixed with the polycyclohexylene dimethylene terephthalate resin to be modified and subjected to solid-state polymerization, thereby enabling the production of high-quality polycyclohexylene dimethylene terephthalate resin molded products.

[0100] More preferred examples of the thermoplastic resin (A) include resin (A1) and resin (A2). Resin (A1) is even more preferred, and polycyclohexylene dimethylene terephthalate resin is particularly preferred.

[0101] When the thermoplastic resin (C) is a polycarbonate resin, the masterbatch contains a thermoplastic resin (A) and a polycondensation catalyst (B), The thermoplastic resin (A) is at least one of a polyester resin (A1) having a structural unit derived from a polyhydric alcohol and a polycarbonate resin (A2); The polyester resin (A1) has a content of structural units derived from ethylene glycol and diethylene glycol of less than 50 mol % in 100 mol % of structural units derived from a polyhydric alcohol, The polycondensation catalyst (B) is at least one selected from the group consisting of phosphorus-based catalysts, titanium-based catalysts, and antimony-based catalysts; The solid-phase polymerization promoting masterbatch contains 5 to 60 mass% of a polycondensation catalyst (B) based on 100 mass% of the non-volatile content, A sheet having a thickness of 1 mm formed from a 260°C kneaded mixture of thermoplastic resin (A) / polycarbonate resin in a mass ratio of 1 / 1 preferably has a haze of 20% or less, more preferably 15% or less, and particularly preferably 10% or less.

[0102] More preferred examples of the thermoplastic resin (A) include resin (A1) and resin (A2), and even more preferred is resin (A2).

[0103] In the present masterbatch, the molecular weight of the thermoplastic resin (A) may be increased during kneading of the thermoplastic resin (A) and the polycondensation catalyst (B).

[0104] By using this master batch, it is possible to provide a modified thermoplastic resin and a molded article of excellent quality, suppressing gelation and crosslinking and suppressing side reactions while shortening the polymerization time compared to conventional methods. The molecular weight dispersity of a mixture obtained by diluting this master batch with a thermoplastic resin (A) so that the polycondensation catalyst (B) is 1 part by mass per 100 parts by mass of the thermoplastic resin (A) is α, and the molecular weight dispersity of the mixture obtained by solid-phase polymerization for 10 hours at a temperature 40°C lower than the flow initiation temperature of the thermoplastic resin (A) is β, where β / α is preferably 1.00 to 1.20. The upper limit of β / α is more preferably 1.15, and even more preferably 1.10. The molecular weight dispersity refers to the ratio of the weight average molecular weight Mw to the number average molecular weight Mn of the mixture, Mw / Mn.

[0105] 2-5.Masterbatch manufacturing method Hereinafter, an example of a method for producing a masterbatch will be described as a process for obtaining a masterbatch for promoting solid-state polymerization containing a thermoplastic resin (A) and a polycondensation catalyst (B). However, the method for producing the masterbatch is not limited to this method.

[0106] The masterbatch for promoting solid-phase polymerization can be produced by melt-kneading a thermoplastic resin (A) and a polycondensation catalyst (B). Thermoplastic resin (A) and polycondensation catalyst (B) are weighed out and mixed in a masterbatch production device. Examples of the masterbatch production device include a single-screw extruder, a twin-screw extruder, and a kneader-ruder.

[0107] After kneading, the mixture can be extruded from a masterbatch production device such as a die, cooled with water, and cut into pellets to obtain a masterbatch. In addition to pelletization, the mixture may be pulverized to obtain a powder.

[0108] 3. Manufacturing method of molded body The method for producing a molded body includes a mixing step of adding at least the master batch to the thermoplastic resin (C) to be modified, mixing the mixture, and melt-kneading to form a thermoplastic resin composition, and a step of producing a modified thermoplastic resin by solid-phase polymerization of the thermoplastic resin composition simultaneously with or after the mixing step, and a step of molding the obtained modified thermoplastic resin to form a molded body. Note that it is not necessary to perform each step continuously, and the thermoplastic resin composition and the modified thermoplastic resin may be pelletized, powdered, granulated, etc. by a single-screw extruder, twin-screw extruder, kneader-ruder, etc. before use.

[0109] In the mixing step for preparing the thermoplastic resin composition, the master batch can be mixed homogeneously at a temperature 0 to 30°C higher than the flow initiation temperature of the thermoplastic resin (C). The mixing time is not particularly limited as long as the mixture can be homogeneously mixed. For example, it is 1 to 20 minutes.

[0110] When the thermoplastic resin (C) to be modified is a polyester resin or a polycarbonate resin, the IV value of the thermoplastic resin (C) pellet before solid-state polymerization (IV x ) and the IV value (IV0) of the thermoplastic resin (C) before processing used as a raw material. xThe ratio IV / IV0 is preferably 0.8 or more, more preferably 0.85 or more, and further preferably 0.90 or more. x The upper limit of / IV0 is not particularly limited, but is usually 1.00. When the thermoplastic resin (C) to be modified is a polyamide resin, the RV value of the thermoplastic resin (C) pellet before solid-state polymerization (RV x ) to the RV value (RV0) of the thermoplastic resin (C) used as the raw material before processing. RV x The ratio RV / RV0 is preferably 0.8 or more, more preferably 0.85 or more, and further preferably 0.90 or more. x The upper limit of / RV0 is not particularly limited, but is usually 1.00.

[0111] In the solid-phase polymerization step, a polycondensation step is carried out in a solid phase under vacuum conditions at a temperature 5 to 50°C lower than the flow initiation temperature of the thermoplastic resin (C). For example, the recycled thermoplastic resin and the master batch are pelletized at 280°C using a twin-screw extruder, and then solid-phase polymerization is carried out in a tumble dryer at 220°C under a vacuum of about 1 mbar for 5 to 10 hours. The molecular weight of the thermoplastic resin (C) increases and the viscosity increases due to the solid-phase polymerization.

[0112] When the thermoplastic resin (C) to be modified is a polyester resin or a polycarbonate resin, the IV value of the thermoplastic resin (C) pellet after solid-state polymerization (IV y ) and the aforementioned IV x Ratio IV y / IV x is preferably 1.05 or more, more preferably 1.10 or more, and further preferably 1.15 or more. y / IV x The upper limit of is not particularly limited, but is usually about 1.20. When the thermoplastic resin (C) to be modified is a polyamide resin, the RV value of the thermoplastic resin (C) pellets after solid-state polymerization (RV y ) and the aforementioned RV x Ratio of RV y / RV xis preferably 1.05 or more, more preferably 1.10 or more, and further preferably 1.15 or more. y / RV x The upper limit of is not particularly limited, but is usually about 1.20.

[0113] The solid-state polymerization time can increase the molecular weight of the thermoplastic resin (C) in a shorter time than when the polycondensation catalyst (B) is added directly to the thermoplastic resin (C) in powder or pellet form without using this master batch. The reason for this is believed to be that the polycondensation catalyst (B) is uniformly dispersed in the thermoplastic resin (C), suppressing local thickening. In addition, the presence of the thermoplastic resin (A) is believed to improve the compatibility between the polycondensation catalyst (B) and the thermoplastic resin (C). Therefore, the reaction between the polycondensation catalyst (B) and the thermoplastic resin (C) is promoted in the solid-state polymerization process, and the thickening of the thermoplastic resin (C) is promoted. As a result, a high-quality thermoplastic resin can be obtained. In addition, the productivity can be significantly improved.

[0114] The degree of increase in the melt viscosity of the thermoplastic resin (C) is preferably 5 to 40% relative to the melt viscosity of the thermoplastic resin (C) before processing, more preferably 7 to 30%, and even more preferably 10 to 25%. When the rate of increase in the melt viscosity is within the above range, the physical properties of the thermoplastic resin (C) can be improved without affecting the moldability.

[0115] Furthermore, according to the present modified thermoplastic resin and the method for producing a molded body, the amount of outgassing generated in the manufacturing process of the molded body can be significantly improved. This is because the molecular weight of the thermoplastic resin increases and decomposition products of the low molecular weight thermoplastic resin that generates outgassing are not generated.

[0116] The modified thermoplastic resin can be molded into various shapes by known methods, such as single-screw extrusion, twin-screw extrusion, injection molding, blow molding, and the like. EXAMPLES

[0117] The present disclosure will be described in more detail below based on examples, but the present disclosure is not limited to the examples. Unless otherwise specified, in the examples, "parts" and "%" represent "parts by mass" and "% by mass", respectively.

[0118] <Method for measuring the solubility parameter of thermoplastic resin> The solubility parameters were calculated by the Fedors method [Polm. Eng. Sci. 14(2)152(1974)].

[0119] <Method for measuring flow temperature of thermoplastic resin> The flow initiation temperature was determined by measuring the minimum temperature at which the melt viscosity of the thermoplastic resin became 4800 Pa s or less when the resin was passed through a capillary with a die hole diameter of φ1 mm and a die length of 1 mm under a pressure of 9.8 MPa using a Shimadzu Corporation "CFT-EX series" flow tester.

[0120] <Method of measuring intrinsic viscosity (IV) or relative viscosity (RV) of thermoplastic resin> The resin pellets were dissolved under the following conditions, and the viscosity was measured using an automatic viscosity measuring device "SS-600-L2" manufactured by Shibayama Scientific Instruments Manufacturing Co., Ltd. Polyester resin The polyester resin pellets were dissolved in phenol / 1,1,2,2-tetrachloroethane=1 / 1 to calculate the intrinsic viscosity (IV). Polycarbonate resin The polycarbonate resin pellets were dissolved in a methylene chloride solution to calculate the intrinsic viscosity (IV). Polyamide resin The polyamide resin pellets were dissolved in a 96% by mass sulfuric acid solution at a concentration of 1 g / dl, and the relative viscosity (RV) was calculated.

[0121] ≪Thermoplastic resin (A), etc.≫ [Resin (A1)] A1-1: Novaduran 5010 (Mitsubishi Engineering Plastics Corporation, polybutylene terephthalate resin (PBT resin)) A1-2: Synthesis example 1 (PBT resin) A1-3: EASTER DN011 (Eastman Chemical Company, polycyclohexylene dimethylene terephthalate resin (PCT resin)) [Resin (A2)] A2-1: Iupilon S-3000 (Mitsubishi Engineering Plastics, polycarbonate resin (PC resin)) A2-2: Iupilon H-2000 (Mitsubishi Engineering Plastics, PC resin) [Resin (A3)] A3-1: UBE Nylon 6 1022 (UBE, PA6) A3-2: Aramin CM3001-N (Toray, PA66) A3-3: Lilsan BMN O TLD (Arkema, PA11) A3-4: Lilsan AMNO TLD (Arkema, PA12) A3-5: MX nylon S6007 (Mitsubishi Engineering Plastics, PAMXD6) [Other resins (A')] A'-1: Synthesis Example 2 (Polyethylene terephthalate resin (PET resin)) A'-2: Synthesis example 3 (PET resin)

[0122] <Polyester resin (A1-2): Synthesis example 1> 100 parts by mass of dimethyl terephthalate, 83.5 parts by mass of butylene glycol, 0.06 parts by mass of magnesium acetate, and 0.03 parts by mass of antimony trioxide were melted at 150°C under a nitrogen atmosphere. Then, the mixture was heated to 230°C over 3 hours while stirring, and methanol was distilled off to terminate the transesterification reaction. After the transesterification reaction was completed, an ethylene glycol solution (PH 5.0) in which 0.019 parts by mass of phosphoric acid and 0.027 parts by mass of sodium dihydrogen phosphate dihydrate were dissolved in 0.5 parts by mass of ethylene glycol was added to the reaction product. Then, the polymerization reaction was carried out at a final temperature of 285°C and a vacuum degree of 0.1 Torr to obtain a polyester resin with an intrinsic viscosity of 0.53. The obtained polyester resin was dried and crystallized at 140°C for 5 hours. Then, solid-phase polymerization was carried out at 200°C, a vacuum degree of 0.3 Torr, and 8 hours to obtain a polyester resin (A1-2) with an intrinsic viscosity of 0.85 dl / g and a melting point of 225°C.

[0123] <Polyester resin (A'-1): Synthesis example 2> 100 parts by mass of dimethyl terephthalate, 57.5 parts by mass of ethylene glycol, 0.06 parts by mass of magnesium acetate, and 0.03 parts by mass of antimony trioxide were melted at 150°C under a nitrogen atmosphere. Then, the temperature was raised to 230°C over 3 hours while stirring, methanol was distilled off, and the transesterification reaction was terminated. After the transesterification reaction was terminated, an ethylene glycol solution (pH 5.0) in which 0.019 parts by mass of phosphoric acid and 0.027 parts by mass of sodium dihydrogen phosphate dihydrate were dissolved in 0.5 parts by mass of ethylene glycol was added to the reaction product. Then, the polymerization reaction was carried out at a final temperature of 285°C and a vacuum degree of 0.1 Torr to obtain a polyester resin with an intrinsic viscosity of 0.55. Then, the obtained polyester resin was dried and crystallized at 160°C for 5 hours. Next, solid-phase polymerization was carried out at 210°C, a vacuum degree of 0.3 Torr, and 6 hours to obtain a polyester resin (A'-1) with an intrinsic viscosity of 0.80 dl / g and a melting point of 250°C.

[0124] <Polyester resin (A'-2): Synthesis example 3> 90 parts by mass of dimethyl terephthalate, 10 parts by mass of dimethyl isophthalate, 57.5 parts by mass of ethylene glycol, 0.06 parts by mass of magnesium acetate, and 0.03 parts by mass of antimony trioxide were melted at 150°C under a nitrogen atmosphere. Then, the temperature was raised to 230°C over 3 hours while stirring, methanol was distilled off, and the transesterification reaction was terminated. After the transesterification reaction was terminated, an ethylene glycol solution (PH 5.0) in which 0.019 parts by mass of phosphoric acid and 0.027 parts by mass of sodium dihydrogen phosphate dihydrate were dissolved in 0.5 parts by mass of ethylene glycol was added to the reaction product. Then, the polymerization reaction was carried out at a final temperature of 285°C and a vacuum degree of 0.1 Torr to obtain a polyester resin with an intrinsic viscosity of 0.50. Then, the obtained polyester resin was dried and crystallized at 160°C for 5 hours. Next, solid-phase polymerization was carried out at 180°C and a vacuum degree of 0.3 Torr for 6 hours to obtain a polyester resin (A'-2) having an intrinsic viscosity of 0.75 dl / g and a melting point of 224°C.

[0125] Haze evaluation of thermoplastic resin (A) etc. Polybutylene terephthalate resin sheet (Sheet haze / PBT) Resin (A1), resin (A2) and other resin (A') were mixed with polybutylene terephthalate resin (PBT resin, flow start temperature 224°C, IV 1.10) in a mass ratio of 1 / 1, and the mixture was injected into a mold at a mold temperature of 20°C using an injection molding machine (manufactured by Toshiba Machine Co., Ltd.) with an injection pressure of 60t to form a sheet with a thickness of 1 mm. The haze of the obtained sheet was measured using a Haze Guard Plus (manufactured by Gardner Co., Ltd.) in accordance with JIS K7136:2000. The haze (H x The criteria for the evaluation were as follows: [Judgment criteria] +++: H x <= 10 ++ :10 <H x <= 15 + :15 <H x <= 20 NG:20 <H x

[0126] ·Polycyclohexylene dimethylene terephthalate resin sheet (Sheet haze / PCT) Resin (A1), resin (A2) and other resin (A') were mixed with polycyclohexylene dimethylene terephthalate resin (PCT resin, flow start temperature 240°C, IV 0.72) in a mass ratio of 1 / 1, and the mixture was injected into a mold at a mold temperature of 20°C using an injection molding machine (manufactured by Toshiba Machine Co., Ltd.) with an injection pressure of 60t to form a sheet with a thickness of 1 mm. The haze of the obtained sheet was measured using a Haze Guard Plus (manufactured by Gardner Co., Ltd.) in accordance with JIS K7136:2000. The haze (H x The criteria for the evaluation were as follows: [Judgment criteria] +++: H x <= 10 ++ :10 <H x <= 15 + :15 <H x <= 20 NG:20 <H x

[0127] · Polycarbonate resin sheet (sheet haze / PC) Resin (A1), resin (A2) and other resin (A') were mixed with polycarbonate resin (PC resin, flow start temperature 245°C, IV 0.5) in a mass ratio of 1 / 1, and the mixture was injected into a mold at a mold temperature of 20°C using an injection molding machine (manufactured by Toshiba Machine Co., Ltd.) with an injection pressure of 60t to mold a sheet with a thickness of 1 mm. The haze of the obtained sheet was measured using a Haze Guard Plus (manufactured by Gardner Co., Ltd.) in accordance with JIS K7136:2000. The haze (H x The criteria for the evaluation were as follows: [Judgment criteria] +++: H x <= 10 ++ :10 <H x <= 15 + :15 <H x <= 20 NG:20 <H x

[0128] Table 1 shows the intrinsic viscosity (IV) or relative viscosity (RV), solubility parameter (SPa), flow initiation temperature (Ta), and sheet haze of the thermoplastic resin (A) and the like. The content (mol %) of structural units derived from ethylene glycol (EG) and / or diethylene glycol (DEG) in 100 mol % of structural units derived from polyhydric alcohol constituting the polyester resin is also shown. These were determined by measuring the polyester resin with GC / MS.

[0129] [Table 1-1]

[0130] [Table 1-2]

[0131] [Table 1-3]

[0132] ≪Polycondensation catalyst (B)≫ B-1: Irganox 1222 (BASF, diethyl [[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate) B-2: Irganox 1425 (BASF, calcium diethyl bis[[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate) B-3: diethyl hydroxyphenylmethylenephosphonate B-4: 2,6-dimethylbenzenesulfonic acid (Kishida Chemical Co., Ltd.) B-5: Antimony trioxide (manufactured by Nihon Seiko Co., Ltd.) B-6: SPC-124 (Sakai Chemical Industry, titanium catalyst)

[0133] The solubility of the polycondensation catalyst (B) is shown in Table 2. When 1 part by mass of the polycondensation catalyst (B) was added to 100 parts by mass of the thermoplastic resin (A) and the like, and the mixture was heated to the flow initiation temperature while stirring with a mechanical stirrer, if the polycondensation catalyst (B) could not be visually confirmed, it was judged to have dissolved in the thermoplastic resin (A) and the like. Dissolved catalysts were marked with ○, and insoluble catalysts were marked with ×. The results are shown in Table 2.

[0134] [Table 2]

[0135] ≪Thermoplastic resin (C)≫ [Polyester resin] C1-1: Novaduran 5010 (Mitsubishi Engineering Plastics, PBT resin) C1-2: Recycled PBT resin (intrinsic viscosity 0.9 dl / g, flow start temperature 224℃, solubility parameter 10 (cal / cm) 3 ) 1 / 2 ) C1-3: EASTER DN011 (Eastman Chemical Company, PCT resin) [Polycarbonate resin] C2-1: Iupilon S-3000 (Mitsubishi Engineering Plastics, PC resin) C2-2: Recycled PC resin (intrinsic viscosity 0.45 dl / g, flow start temperature 250°C, solubility parameter 9.9 (cal / cm 3 ) 1 / 2 ) [Polyamide resin] C3-1: UBE Nylon 6 1022 (UBE, PA6) C3-2: Aramin CM3001-N (Toray, PA66) C3-3: Lilsan BMN O TLD (Arkema, PA11) C3-4: Rilsan AMNO TLD (Arkema, PA12) C3-5: MX nylon S6007 (Mitsubishi Engineering Plastics, PAMXD6)

[0136] Table 3 shows the intrinsic viscosity (IV) or relative viscosity (RV), solubility parameter (SPc), and flow start temperature (Tc) of the thermoplastic resin (C).

[0137] [Table 3-1]

[0138] [Table 3-2]

[0139] [Table 3-3]

[0140] <Antioxidants> D-1: Irgafos 168 (BASF, phosphorus-based antioxidant) D-2: Irganox B225 (BASF, phosphorus / phenolic antioxidant)

[0141] <Production of thermoplastic resin composition> (Example 1-1) [Masterbatch manufacturing] 90 parts of thermoplastic resin (A1-1) and 10 parts of polymerization catalyst (B-1) were weighed out and mixed in a co-rotating twin screw extruder "TEX-54α3" (L / D=52.5, discharge rate: 350 kg / hr, 3 vent holes) manufactured by Japan Steel Works, Ltd. Then, while sucking and degassing under high vacuum from the vent holes, the mixture was extruded at 234°C, which is 10°C higher than the flow initiation temperature of the thermoplastic resin (A1-1), and cut with a pelletizer to obtain a master batch (MB1-1).

[0142] [Production of Thermoplastic Resin Composition (Thermoplastic Resin Composition Pellet)] Next, 98 parts of the thermoplastic resin (C1-1) "Novaduran 5010 (Mitsubishi Engineering Plastics, PBT)" and 2 parts of the obtained master batch (MB1-1) were extruded in a single-screw extruder (Dalmage screw) having a screw diameter of 40 mm manufactured by Nippon Placon Co., Ltd. at a screw rotation speed of 90 rpm, a processing temperature of 244°C, which is 20°C higher than the flow initiation temperature of the thermoplastic resin (C1-1), 224°C, and a discharge rate of 20 kg / h, to obtain a pellet-shaped thermoplastic resin composition for solid-phase polymerization (PE1-1).

[0143] (Examples 1-2 to 39, Comparative Examples 1-1 to 13, Examples 2-1 to 18, Comparative Examples 2-1 to 7, Examples 3-1 to 29, Comparative Examples 3-1 to 19) Masterbatches (MB1-2 to 27, MB2-1 to 13, MB3-1 to 16, MB4-1 to 10) according to the examples and comparative examples were obtained in the same manner as in Example 1-1, except that the materials and amounts (parts by mass) shown in Table 4 and the extrusion temperature were changed to a temperature 10°C higher than the flow initiation temperature of the thermoplastic resin (A). When an antioxidant was contained, the thermoplastic resin (A), the polycondensation catalyst (B) and the antioxidant were weighed out, and a master batch was obtained in the same manner as in Example 1-1.

[0144] Next, pellet-shaped thermoplastic resin compositions for solid-phase polymerization (PE1-2 to 52, PE2-1 to 25, PE3-1 to 44) were obtained in the same manner as in Example 1-1, except that the materials and amounts (parts by mass) shown in Table 5 and the extrusion temperature were changed to a temperature 20°C higher than the flow initiation temperature of the thermoplastic resin (C).

[0145] (Comparative Examples 4-1 to 10) Pellet-shaped thermoplastic resin compositions (PE4-1 to 10) were obtained in the same manner as in Example 1-1, except that a powdered polycondensation catalyst (B) was used instead of the master batch, the materials and amounts (parts by mass) shown in Table 5-4 were changed, and the extrusion temperature was changed to a temperature 20°C higher than the flow initiation temperature of the thermoplastic resin (C).

[0146] <Masterbatch evaluation> The masterbatches were evaluated by the methods described below, and the results are shown in Table 4. In all evaluation criteria, "NG" means "not practical," "+" means "practical," "++" means "good," and "+++" means "excellent." <Processability evaluation> The masterbatches of the Examples and the like were produced continuously for 1 hour using a twin-screw extruder, and strand breakage was confirmed, and the productivity (processability) was evaluated according to the following criteria. The results are shown in Table 4. Strand breakage refers to a state in which a strand breaks and cannot be pulled. [Evaluation Criteria] +++: No strand breakage occurs. ++: Strand breakage occurred 1 or more times and 5 or less times. +: Strand breakage occurred more than 5 times but less than 10 times. NG: None of the above evaluations apply, or the masterbatch cannot be produced.

[0147] <Evaluation of the increase rate of molecular weight dispersity> The master batches of each Example and Comparative Example were diluted with the thermoplastic resin (A) used so that the polycondensation catalyst (B) was 1 part by mass per 100 parts by mass of the thermoplastic resin (A) to obtain a mixture. The molecular weight dispersity α of the obtained mixture was determined. Then, the mixture was solid-phase polymerized for 10 hours at a temperature 40°C lower than the flow start temperature, and the molecular weight dispersity β after solid-phase polymerization was determined. These results and the value of β / α are shown in Table 4. The number average molecular weight Mn and weight average molecular weight Mw were measured by gel permeation chromatography (GPC) using a Shodex GPC LF-404 column after dissolving the recycled thermoplastic resin pellets in a 10 mmol / L sodium trifluoroacetate / hexafluoroisopropanol (HFIP) mixed solution as a solvent and filtering the sample solution through a membrane filter. Note that Mn and Mw are relative values ​​to the molecular weight of standard polystyrene. That is, for example, in the case of MB1-1, this is the result of diluting it with the thermoplastic resin (A1-1) to obtain a mixture.

[0148] <Evaluation of thermoplastic resin composition, modified thermoplastic resin, and molded body> The thermoplastic resin composition, modified thermoplastic resin, and molded article were evaluated by the methods described below. The results are shown in Table 5. In all evaluation criteria, "NG" means "not practical," "+" means "practical," "++" means "good," and "+++" means "excellent."

[0149] <Production of modified thermoplastic resin> The thermoplastic resin composition pellets of each Example and Comparative Example were used to carry out solid-state polymerization to obtain modified thermoplastic resin pellets. The solid-state polymerization conditions were a temperature 40°C lower than the flow initiation temperature of the thermoplastic resin (C), a vacuum degree of 0.3 Torr, and 10 hours.

[0150] <Method for measuring intrinsic viscosity (IV) and relative viscosity (RV) of thermoplastic resin composition> The intrinsic viscosity and relative viscosity of the thermoplastic resin composition pellets of each of the Examples and Comparative Examples were measured by the following methods in accordance with the type of thermoplastic resin (C). For polyester resin: Intrinsic viscosity (IV) The polyester resin composition pellets were dissolved in phenol / 1,1,2,2-tetrachloroethane (1 / 1), and the viscosity was measured using an automatic viscosity measuring device "SS-600-L2" manufactured by Shibayama Scientific Instruments Manufacturing Co., Ltd. In the case of polycarbonate resin: Intrinsic viscosity (IV) The polycarbonate resin composition pellets were dissolved in a methylene chloride solution, and the viscosity was measured using an automatic viscosity measuring device "SS-600-L2" manufactured by Shibayama Scientific Instruments Manufacturing Co., Ltd. For polyamide resins: Relative viscosity (RV) The polyamide resin composition pellets were dissolved in a 96% by mass sulfuric acid solution at a concentration of 1 g / dl, and the viscosity was measured using an automatic viscosity measuring device "SS-600-L2" manufactured by Shibayama Scientific Instruments Manufacturing Co., Ltd.

[0151] <Evaluation of intrinsic viscosity (IV) and relative viscosity (RV) before solid-state polymerization> The intrinsic viscosity (IV x ) or relative viscosity (RV x ) and the ratio of the intrinsic viscosity (IV0) or relative viscosity (RV0) of the thermoplastic resin (C) used for each x / IV0 or RV x / RV0 was evaluated according to the following criteria in accordance with the type of thermoplastic resin (C) to be modified used in each Example and Comparative Example. [Evaluation criteria for polyester resin and polycarbonate resin] ++++:0.95≦IV x / IV0 +++: 0.90≦IV x / IV0<0.95 ++: 0.85≦IV x / IV0<0.90 +: 0.80≦IV x / IV0<0.85 NG: IV x / IV0<0.80 [Evaluation criteria for polyamide resins] ++++:0.95≦RV x / RV0 +++: 0.90≦RV x / RV0<0.95 ++: 0.85≦RV x / RV0<0.90 +: 0.80≦RV x / RV0<0.85 NG: RV x / RV0<0.80

[0152] <Evaluation of intrinsic viscosity (IV) and relative viscosity (RV) after solid-state polymerization> The intrinsic viscosity (IV x ) or relative viscosity (RV x ) and the intrinsic viscosity (IV y ), or relative viscosity (RV y ) and evaluated according to the following criteria in accordance with the type of modified thermoplastic resin (C) used in each Example and Comparative Example. [Evaluation criteria for polyester resin and polycarbonate resin] ++++:1.15≦IV y / IV x +++: 1.10≦IV y / IV x <1.15 ++: 1.08≦IV y / IV x <1.10 +: 1.05≦IV y / IV x <1.08 NG: IVy / IV x <1.05 [Evaluation criteria for polyamide resins] ++++:1.15≦RV y / RV x +++: 1.10≦RV y / RV x <1.15 ++: 1.08≦RV y / RV x <1.10 +: 1.05≦RV y / RV x <1.08 NG: RV y / RV x <1.05

[0153] <Evaluation of outgassing amount> The modified thermoplastic resin pellets after solid-state polymerization in each Example and Comparative Example were held under nitrogen for 1 hour at a temperature 20°C higher than the flow initiation temperature of the thermoplastic resin (C) in about 10 mg of sample, and the weight loss rate was measured using a Hitachi High-Tech Science STA7200. The weight loss rate after solid-state polymerization of the thermoplastic resin composition pellets in each Example and Comparative Example was set to TG1, and the weight loss rate after solid-state polymerization of the thermoplastic resin composition pellets in each Comparative Example, in which no polycondensation catalyst was added to the thermoplastic resin (C) used in each Example and Comparative Example, was set to TG0, and the evaluation was performed according to the following criteria. That is, for example, in the case of Example 1-1, the evaluation was performed based on the weight loss rate TG1 measured using the thermoplastic resin composition pellets (PE1-1) and the weight loss rate TG0 measured using the resin pellets (PE1-29) of the thermoplastic resin (C1-1). [Evaluation Criteria] +++: TG1 / TG0<0.8 ++:0.8≦TG1 / TG0<0.9 +: 0.9≦TG1 / TG0<1.0 NG:1.0≦TG1 / TG0

[0154] <Yellowness index (YI value)> The thermoplastic resin composition pellets before solid-state polymerization and the modified thermoplastic resin pellets after solid-state polymerization of each Example and Comparative Example were injection molded at a temperature 20 ° C. higher than the flow initiation temperature of the thermoplastic resin (C) using an injection molding machine (Toshiba Machine Co., Ltd., IS-100F type), and a rectangular parallelepiped molded body (test piece) of 30 mm length × 40 mm width × 3 mm height was produced. Then, using an image spectrophotometer AU Color COLOR7x manufactured by Kurabo Co., Ltd., the L value (brightness), a * value, and b * value of the test piece were measured with a standard light source of D-65 (10), and the YI value was measured according to JIS K7373. The YI value of the test piece prepared using the modified thermoplastic resin pellets after solid-state polymerization was YI1, and the test piece prepared using the thermoplastic resin composition pellets before solid-state polymerization was YI0, and the evaluation was performed according to the following criteria. [Evaluation Criteria] +++: YI1 / YI0<1.1 ++ :1.1≦YI1 / YI0<1.3 + :1.3≦YI1 / YI0<1.5 NG: 1.5≦YI1 / YI0

[0155] <Number of items> The modified thermoplastic resin pellets after solid-state polymerization in each of the Examples and Comparative Examples were injection-molded at a temperature 20°C higher than the flow initiation temperature of the thermoplastic resin (C) using an injection molding machine (Toshiba Machine Co., Ltd., IS-100F type) to produce a rectangular molded body (test piece) with dimensions of 30 mm length x 40 mm width x 3 mm height. The number of bumps larger than 100 μm was visually counted and evaluated according to the following criteria. [Evaluation Criteria] +++:No items ++ :1~2 pieces + :3~5 pieces NG: 6 or more

[0156] <Charpy impact strength before solid-state polymerization> Charpy impact test pieces (notched) were prepared using pellets of the thermoplastic resin composition before solid-state polymerization in each of the Examples and Comparative Examples. The Charpy impact strength (notched) of the prepared plate test pieces was measured at 23°C. The Charpy impact strength (notched) of the thermoplastic resin composition before solid-state polymerization in each of the Examples and Comparative Examples was measured using S x The Charpy impact strength (with notch) of the thermoplastic resin (C) was defined as S0, and the evaluation was performed according to the following criteria. [Evaluation Criteria] +++:0.95≦S X / S0 ++:0.90≦S X / S0<0.95 + :0.80≦S X / S0<0.90 NG:S X / S0<0.80

[0157] <Charpy impact strength after solid-state polymerization> Charpy impact test pieces (notched) were prepared using the modified thermoplastic resin pellets after solid-state polymerization in each Example and Comparative Example. The Charpy impact strength (notched) of the prepared plate test pieces was measured at 23°C. The Charpy impact strength (notched) of the modified thermoplastic resin pellets after solid-state polymerization in each Example and Comparative Example was S y The evaluation was based on the following criteria. [Evaluation Criteria] +++:1.15≦S Y / S X ++:1.10≦S Y / S X <1.15 + :1.05≦S Y / S X <1.10 NG:S Y / S X <1.05

[0158] [Table 4-1-1]

[0159] [Table 4-1-2]

[0160] [Table 4-2]

[0161] [Table 4-3]

[0162] [Table 4-4]

[0163] The masterbatches MB1-1 to MB2-1 to MB3-16, which contain a thermoplastic resin (A) and a polycondensation catalyst (B) and contain 5 to 60 mass% of the polycondensation catalyst (B) in 100 mass% of the non-volatile content of the masterbatch, all showed excellent results in terms of processability. In addition, it was confirmed that the increase rate β / α of the molecular weight dispersity was 1 to 1.2.

[0164] [Table 5-1-1]

[0165] [Table 5-1-2]

[0166] [Table 5-2]

[0167] [Table 5-3]

[0168] [Table 5-4]

[0169] In the thermoplastic resin composition of the comparative example not using the master batch, it was confirmed that the IVx relative to IV0 before solid-state polymerization, or the RVx relative to RV0, decreased significantly. The reason for this is believed to be that the polymerization catalyst was not uniformly and finely dispersed in the thermoplastic resin (C) because it was not master-batched. The thermoplastic resin composition of the comparative example in which the difference in solubility parameters between the thermoplastic resin (A) and the thermoplastic resin (C) did not satisfy the requirement (I), did not have good compatibility, even when using a master batch, and therefore could not obtain a molded product of good quality. In addition, the thermoplastic resin composition of the comparative example in which the difference in flow initiation temperature between the thermoplastic resin (A) and the thermoplastic resin (C) did not satisfy the requirement (II), deteriorated the thermoplastic resin during processing and poor distribution of the master batch occurred, and a molded product of good quality could not be obtained. In these examples, it is believed that the amount of outgassing was also large because the solid-state polymerization did not proceed sufficiently and there were many low molecular weight components.

[0170] [Industrial Applicability] The present masterbatch and the present thermoplastic resin composition have excellent moldability and can provide high-quality molded articles by general-purpose processing methods, and are therefore suitable for recycling plastic products whose main component is polybutylene terephthalate resin, polycarbonate resin, or polyamide resin, such as containers, cards, films, sheets, and fibers, which have been used or are generated during the production process. Furthermore, because the molded product has excellent quality, it can be suitably used as a high-performance resin material in a wide range of applications, including fibers, films, sheets, foams, containers, electronic materials, building materials, automobile parts, and various industrial parts and products.

Claims

1. A thermoplastic resin composition obtained by melt-kneading a thermoplastic resin (C) which is at least one selected from the group consisting of a polyester resin (excluding polyethylene terephthalate resin), a polycarbonate resin, and a polyamide resin, and a masterbatch for promoting solid-phase polymerization, The solid-phase polymerization promoting masterbatch contains a thermoplastic resin (A) and a polycondensation catalyst (B), the thermoplastic resin (A) is at least one selected from the group consisting of a polyester resin (A1) having a structural unit derived from a polyhydric alcohol, a polycarbonate resin (A2), and a polyamide resin (A3); The polyester resin (A1) has a content of structural units derived from ethylene glycol and / or diethylene glycol of less than 50 mol % based on 100 mol % of structural units derived from a polyhydric alcohol, The polycondensation catalyst (B) is at least one selected from the group consisting of phosphorus-based catalysts, titanium-based catalysts, and antimony-based catalysts; The solid-phase polymerization promoting masterbatch contains 5 to 60% by mass of a polycondensation catalyst (B) based on 100% by mass of the non-volatile content thereof, Solubility parameter SPc (cal / cm) of thermoplastic resin (C) 3 ) 1/2 and the solubility parameter SPa (cal / cm) of the thermoplastic resin (A). 3 ) 1/2 The difference (SPc-SPa) is -1.0 (cal / cm 3 ) 1/2 More than 1.0 (cal / cm 3 ) 1/2 is as follows: The difference (Tc-Ta) between the flow start temperature Tc (°C) of the thermoplastic resin (C) and the flow start temperature Ta (°C) of the thermoplastic resin (A) is -30°C or more and less than 50°C. Thermoplastic resin composition for solid phase polymerization.

2. The thermoplastic resin composition for solid-state polymerization according to claim 1, characterized in that the polycondensation catalyst (B) is an acid catalyst having an aromatic ring skeleton and / or an alicyclic skeleton, and is soluble in an amount of at least 1 part by mass in 100 parts by mass of the thermoplastic resin (A).

3. 2. The thermoplastic resin composition for solid-state polymerization according to claim 1, wherein the polycondensation catalyst (B) is at least one of an alkyl phosphonic acid ester and an alkyl phosphonic acid monoester.

4. 2. The thermoplastic resin composition for solid-state polymerization according to claim 1, wherein the polycondensation catalyst (B) is at least one of a sterically hindered hydroxyphenylalkylphosphonic acid ester and a sterically hindered hydroxyphenylalkylphosphonic acid monoester.

5. The thermoplastic resin composition for solid-state polymerization according to claim 1, wherein the molecular weight dispersity of a mixture obtained by diluting the masterbatch for solid-state polymerization promotion with a thermoplastic resin (A) so that the polycondensation catalyst (B) is 1 part by mass per 100 parts by mass of the thermoplastic resin (A) is α, and the molecular weight dispersity of the mixture obtained by solid-state polymerization for 10 hours at a temperature 40° C. lower than the flow initiation temperature of the thermoplastic resin (A) is β, the ratio β / α being 1.00 to 1.

20.

6. A modified thermoplastic resin obtained by solid-state polymerization of the thermoplastic resin composition for solid-state polymerization according to any one of claims 1 to 5.

7. A molded article formed using the modified thermoplastic resin according to claim 6.

8. A step of obtaining a masterbatch for promoting solid-state polymerization, comprising a thermoplastic resin (A) and a polycondensation catalyst (B); A mixing step of adding the master batch for promoting solid-state polymerization to a thermoplastic resin (C) to be modified, which is at least one selected from the group consisting of a polyester resin (excluding polyethylene terephthalate resin), a polycarbonate resin, and a polyamide resin, mixing the master batch, and then melt-kneading the mixture to obtain a thermoplastic resin composition for solid-state polymerization according to any one of claims 1 to 5; A step of solid-state polymerization is provided simultaneously with or after the mixing step. Method for producing modified thermoplastic resin.

9. A masterbatch for promoting solid-phase polymerization, used in the method for producing a modified thermoplastic resin according to claim 8.

10. A method for producing a molded body, further comprising a step of molding the modified thermoplastic resin according to claim 8.

11. A masterbatch for promoting solid-state polymerization of a polybutylene terephthalate resin, comprising: Contains a thermoplastic resin (A) and a polycondensation catalyst (B), The thermoplastic resin (A) is at least one of a polyester resin (A1) having a structural unit derived from a polyhydric alcohol and a polycarbonate resin (A2), The polyester resin (A1) has a content of structural units derived from ethylene glycol and diethylene glycol of less than 50 mol % based on 100 mol % of structural units derived from a polyhydric alcohol, The polycondensation catalyst (B) is at least one selected from the group consisting of phosphorus-based catalysts, titanium-based catalysts, and antimony-based catalysts; The solid-phase polymerization promoting masterbatch contains 5 to 60% by mass of a polycondensation catalyst (B) based on 100% by mass of the non-volatile content thereof, The haze of a sheet having a thickness of 1 mm formed from a 260°C kneaded product of a thermoplastic resin (A) / polybutylene terephthalate resin in a mass ratio of 1 / 1 is 20% or less. Masterbatch for promoting solid-state polymerization.

12. A masterbatch for promoting solid-state polymerization of a polycyclohexylene dimethylene terephthalate resin, comprising: Contains a thermoplastic resin (A) and a polycondensation catalyst (B), The thermoplastic resin (A) is at least one of a polyester resin (A1) having a structural unit derived from a polyhydric alcohol and a polycarbonate resin (A2), The polyester resin (A1) has a content of structural units derived from ethylene glycol and diethylene glycol of less than 50 mol % based on 100 mol % of structural units derived from a polyhydric alcohol, The polycondensation catalyst (B) is at least one selected from the group consisting of phosphorus-based catalysts, titanium-based catalysts, and antimony-based catalysts; The solid-phase polymerization promoting masterbatch contains 5 to 60% by mass of a polycondensation catalyst (B) based on 100% by mass of the non-volatile content thereof, The haze of a sheet having a thickness of 1 mm formed from a 260°C kneaded product of a thermoplastic resin (A) / polycyclohexylene dimethylene terephthalate resin in a mass ratio of 1 / 1 is 20% or less. Masterbatch for promoting solid-state polymerization.

13. A masterbatch for promoting solid-state polymerization of a polycarbonate resin, comprising: Contains a thermoplastic resin (A) and a polycondensation catalyst (B), The thermoplastic resin (A) is at least one of a polyester resin (A1) having a structural unit derived from a polyhydric alcohol and a polycarbonate resin (A2), The polyester resin (A1) has a content of structural units derived from ethylene glycol and diethylene glycol of less than 50 mol % based on 100 mol % of structural units derived from a polyhydric alcohol, The polycondensation catalyst (B) is at least one selected from the group consisting of phosphorus-based catalysts, titanium-based catalysts, and antimony-based catalysts; The solid-phase polymerization promoting masterbatch contains 5 to 60% by mass of a polycondensation catalyst (B) based on 100% by mass of the non-volatile content thereof, The haze of a sheet having a thickness of 1 mm formed from a 260°C kneaded product of a thermoplastic resin (A) / polycarbonate resin in a mass ratio of 1 / 1 is 20% or less. Masterbatch for promoting solid-state polymerization.

Citation Information

Patent Citations

  • Modified polyethylene terephthalate and its manufacturing method

    JP2005002170A

  • Method for producing high molecular weight polycarbonate resin

    JP2005530874A

  • Modifier for crystalline polyester resin and molded article using the same

    JP2006045477A

  • Increasing the molecular weight of polycondensates

    WO1996011978A1

  • Semi-aromatic polyamide resin and method for manufacturing same

    WO2019189145A1