Laminated film and method for separating laminated film

A laminated film design with a styrene-resin adhesive layer enables efficient separation into resin layers using solvent immersion, addressing inefficiencies in existing separation methods.

JP2024158943APending Publication Date: 2024-11-08GUNZE LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023074595
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing methods for separating laminated films are not efficient, necessitating a laminated film design and separation method that facilitates easy separation.

Method used

A laminated film with a first and second resin layer bonded by an adhesive layer containing a styrene resin that can be dissolved by a solvent, allowing for easy peeling and recovery of individual layers.

Benefits of technology

The laminated film can be easily separated into its constituent layers using a solvent-based method, maintaining interlayer strength and reducing operational costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158943000001_ABST
    Figure 2024158943000001_ABST
Patent Text Reader

Abstract

To provide a laminated film and a method for separating multiple layers, which can be easily separated.SOLUTION: A laminated film according to the present invention comprises: a first resin layer having a first surface and a second surface; and a second resin layer bonded to at least one of the first surface and the second surface via an adhesive layer, wherein the adhesive layer contains a styrene-based resin that is soluble in a solvent.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated film and a method for separating the laminated film. [Background technology]

[0002] In recent years, in response to the demand for recycling resin materials, a method has been proposed for separating a laminated film in which multiple resin layers are laminated via an adhesive layer into multiple resin layers and recovering them.For example, Patent Document 1 describes a method for separating a laminated film in which a surface layer of a laminated film made of different materials is brought into contact with a transfer material that thermally bonds the surface layer under heat and pressure, and the surface layer and the base film layer are separated. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 10-034650 Summary of the Invention [Problem to be solved by the invention]

[0004] However, even with the above-mentioned method, there is still room for improvement in terms of easily separating the laminated film, and therefore a laminated film suitable for separation and a method for separating the same have been desired.

[0005] The present invention has been made to solve the above problems, and has an object to provide a laminated film that can be easily separated, and a method for separating the same. [Means for solving the problem]

[0006] Item 1. A first resin layer having a first surface and a second surface; a second resin layer bonded to at least one of the first surface and the second surface via an adhesive layer; Equipped with The adhesive layer contains a styrene-based resin that can be dissolved by a solvent. Laminated film.

[0007] Item 2. The styrene ratio in the adhesive layer is 2 to 75% by weight. Item 1. The laminate film according to item 1.

[0008] Item 3. The styrene-based resin is at least one selected from styrene / ethylene / butylene / styrene block copolymer (SEBS), styrene / ethylene / propylene / styrene block copolymer (SEPS), styrene / isoprene / styrene block copolymer (SIS) and styrene / butadiene / styrene block copolymer (SBS), Item 3. The laminate film according to item 1 or 2.

[0009] Item 4. The thickness of the adhesive layer is 3 to 35 μm. Item 4. The laminate film according to any one of items 1 to 3.

[0010] Item 5. A step of immersing the laminated film according to any one of items 1 to 4 in a solvent; peeling the second resin layer from the laminated film immersed in a solvent; The method for separating a laminated film comprises:

[0011] Item 6. Prior to the step of immersing in the solvent, a step of unwinding the laminate film from a roll on which the laminate film is wound; winding up the peeled second resin layer and the first resin layer after the peeling of the second resin layer onto a roll; Item 6. The method for separating a laminated film according to item 5, further comprising: Effect of the Invention

[0012] According to the present invention, the laminated film can be easily separated. [Brief description of the drawings]

[0013] [Figure 1]FIG. 1 is a cross-sectional view of a laminated film according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a side view showing an example of a method for separating the laminated film of FIG. [Diagram 3] FIG. 2 illustrates the mechanism of separation of an adhesive layer. [Figure 4] 1 is a table showing compositions of Examples 1 to 8 and Comparative Examples 1 to 3. [Diagram 5] 1 is a table showing the physical properties of Examples 1 to 8 and Comparative Examples 1 to 3. [Figure 6] 1 is a table showing the peel strengths of Examples 1 to 8 and Comparative Examples 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the laminate film and the method for separating the laminate film according to the present invention will be described. In this embodiment, the laminate film will be described, and then the method for separating the laminate film will be described.

[0015] <1. Laminated film> Fig. 1 is a cross-sectional view of a laminated film. As shown in Fig. 1, the laminated film 1 of this embodiment includes a first resin layer 2 having a first surface 21 and a second surface 22, and a second resin layer 4 disposed on at least one of the first surface 21 and the second surface 22 via an adhesive layer 3. The second resin layer 4 does not have to be disposed on both the first surface 21 and the second surface 22 of the first resin layer 2, and the second resin layer 4 may be disposed on either one of the surfaces via the adhesive layer 3.

[0016] In the laminated film thus configured, the second resin layer 4 can be peeled off from the first resin layer 2 by a method described later, and the first resin layer 2 and the second resin layer 4 can be collected separately. That is, the laminated film 1 can be separated into the first resin layer 2 and the second resin layer 4. In addition, such a laminated film 1 can be used as, for example, a label substrate for packaging of beverages, food products, daily necessities, etc., a food packaging film, a dicing substrate for semiconductor manufacturing, a back grinding substrate, etc. Furthermore, semi-finished products obtained during the manufacturing of the label substrate and packaging film are also included. Each layer will be described below.

[0017] <1-1. First resin layer and second resin layer> The first resin layer 2 and the second resin layer 4 are not particularly limited, and may be made of at least one resin material selected from polyethylene, polypropylene, ethylene-ethyl acrylate copolymer, ethylene-vinyl acetate copolymer, terpolymer of acrylonitrile monomer, diene monomer, and styrene monomer, terpolymer of (meth)acrylic acid alkyl ester monomer, diene monomer, and styrene monomer, copolymer of (meth)acrylic acid alkyl ester monomer, acrylonitrile monomer, diene monomer, and styrene monomer, polyethylene terephthalate, thermoplastic polyurethane, etc. Therefore, for example, a mixed resin of polyethylene and polypropylene can be used as the resin layer.

[0018] The thickness of the first resin layer 2 is not particularly limited, but is preferably, for example, 40 to 135 μm, and more preferably 45 to 130 μm. The thickness of the second resin layer is not particularly limited, but is preferably, for example, 5 to 35 μm, and more preferably 7 to 30 μm.

[0019] <1-2.Adhesive layer> The adhesive layer contains at least a styrene-based resin, and may contain other resin materials such as polyethylene, polypropylene, etc. The styrene-based resin may be at least one selected from, for example, styrene / butadiene / styrene block copolymer (SBS), styrene / isoprene / styrene block copolymer (SIS), styrene / ethylene / butylene / styrene block copolymer (SEBS), and styrene / ethylene / propylene / styrene block copolymer (SEPS).

[0020] The styrene ratio in the adhesive layer 3 is, for example, preferably 2 to 75% by weight, more preferably 3 to 72% by weight, and particularly preferably 5 to 70% by weight. If the amount of styrene-based resin in the adhesive layer is too small, the styrene ratio will be small, making it difficult to peel off the resin layer as described below, and if the amount of styrene-based resin is too large, the styrene ratio will be large, which may result in a decrease in Young's modulus, interlayer strength, and productivity of the laminated film, and an increase in cost. In addition, taking into account the decrease in interlayer strength as described below, it is preferable that the styrene ratio in the adhesive layer is low, and it may be, for example, 3 to 15% by weight. On the other hand, taking into account the remaining amount of the adhesive layer components after dissolution as described below, it may be, for example, 20 to 70% by weight.

[0021] The thickness of the adhesive layer 3 is not particularly limited, but is preferably, for example, 3 to 35 μm, and more preferably 5 to 30 μm, because if the adhesive layer 3 is too thin, the interlayer strength decreases, and if the adhesive layer is too thick, the cost increases.

[0022] <2. Manufacturing method of laminated film> The manufacturing method of the laminated film 1 is not particularly limited. For example, the resin compositions constituting the first resin layer, the second resin layer, and the adhesive layer are each fed into an extruder set at a predetermined temperature, extruded from a T-die in the stacking order of second resin layer / adhesive layer / first resin layer / adhesive layer / second resin layer, and taken up by a cooling roll set at a predetermined temperature to obtain a five-layer laminated film as shown in FIG. 1.

[0023] <3. How to separate the laminated film> The laminated film 1 can be separated into the first resin layer and the second resin layer as follows: As an example, separation is performed using an apparatus shown in FIG.

[0024] 2, this device has a first roll 51 on which the laminate film 1 is wound, and downstream of the first roll 51 is disposed a solvent tank 52 in which the laminate film 1 unwound from the first roll 51 is immersed. The solvent used here is not particularly limited as long as it can dissolve the styrene resin, and may be, for example, a solvent containing at least one of an aromatic solvent, a cyclic terpene solvent, a cyclic ether solvent, and a cyclic aliphatic solvent.

[0025] Examples of aromatic solvents include xylene, toluene, benzene, and mesitylene. Examples of cyclic terpene solvents include limonene, pinene, and cymene. Examples of cyclic ether solvents include tetrahydrofuran (THF) and 2-methyltetrahydrofuran. Examples of cyclic aliphatic solvents include cyclohexane, methylcyclohexane, and ethylcyclohexane.

[0026] 3, in the laminated film 1 immersed in a solvent, the styrene-based resin 31 contained in the adhesive layer 3 is dissolved by the solvent, and a large number of voids 32 are formed in the adhesive layer 3. As a result, when a force is applied to separate the second resin layer 4 from the first resin layer 2, the force is propagated through the formed voids 32, and the second resin layer 4 can be easily peeled off from the first resin layer 2.

[0027] A first separator 53 and a first driven roller 54 are arranged in this order on the downstream side of the tank 52, and a part of the second resin layer 4 on the first surface 21 side is peeled off from the first resin layer 2 by the first separator 53. Then, as the second resin layer 4 is transported upward by the first driven roller 54, the second resin layer 4 is continuously peeled off from the first resin layer 2 and taken up by the second roller 55.

[0028] Further, a second separator 56 and a second driven roller 57 are disposed in this order downstream of the first driven roller 54, and a part of the second resin layer 4 on the second surface 22 side is peeled off from the first resin layer 2 by the second separator 56. Then, as the second resin layer 4 is transported downward by the second driven roller 57, the second resin layer 4 is continuously peeled off from the first resin layer 1 and taken up by the third roller 58.

[0029] Furthermore, the first resin layer 2 from which the second resin layer 4 on the second surface 22 side has been peeled off travels straight and is taken up by the fourth roller 59. In this way, the second resin layer 4 on the first surface 21 side, the first resin layer 2, and the second resin layer 4 on the second surface 22 side are taken up and collected by the second to fourth rollers 55, 58, 59, respectively.

[0030] The first and second separators 53, 56 are not particularly limited as long as they act on the laminated film 1 to trigger peeling of the second resin layer 4 from the first resin layer 2. For example, a peeling blade or a knife edge used in a separator peeling mechanism can be used.

[0031] The above separation method is one example, and any method may be used as long as it involves at least a process of immersing the laminated film 1 in a solvent and then applying a force to separate the first resin layer 2 and the second resin layer 4.

[0032] <4. Features> As described above, according to this embodiment, the following effects can be obtained.

[0033] 3, in the laminated film 1 according to this embodiment, the adhesive layer 3 that bonds the first resin layer 2 and the second resin layer 4 contains a styrene-based resin 31. When the laminated film 1 is immersed in a solvent, the styrene-based resin 31 can be dissolved, thereby forming voids 32 in the adhesive layer 3. As a result, when a force is applied to separate the second resin layer 2 from the first resin layer 1, the force can be propagated through the voids 31, and the first resin layer 2 and the second resin layer 4 can be easily separated.

[0034] By setting the styrene ratio in the adhesive layer 3 to, for example, 2 to 75 weight %, the first resin layer 2 and the second resin layer 4 can be easily separated while the Young's modulus and interlayer strength of the laminated film 1 can be maintained at an appropriate level. EXAMPLES

[0035] Examples of the present invention will be described in detail below, but the present invention is not limited to these examples.

[0036] <1. Preparation of laminated film> First, as shown in FIG. 4, laminated films having compositions according to Examples 1 to 6 and Comparative Examples 1 to 2 were prepared. All of them used five-layer laminated films as shown in FIG. 1. The thickness of the laminated films in Examples 1 to 6 and Comparative Example 2 was 200 μm. Specifically, the laminated films had thicknesses of 30 μm (second resin layer) / 10 μm (adhesive layer) / 120 μm (first resin layer) / 10 μm (adhesive layer) / 30 μm (second resin layer). On the other hand, the thickness of the laminated film in Comparative Example 1 was 150 μm. Specifically, the laminated film had thicknesses of 22 μm (second resin layer) / 8 μm (adhesive layer) / 90 μm (first resin layer) / 8 μm (adhesive layer) / 22 μm (second resin layer).

[0037] The materials constituting each component of the laminated film shown in FIG. 4 are as follows: ·PE-1(LDPE) specific gravity 0.934, MFR5.3g / 10min ·PE-2 (LDPE) specific gravity 0.922, MFR 0.5g / 10min ·PE-3 (LLDPE) specific gravity 0.931, MFR4g / 10min ·Amorphous PO specific gravity 0.89, MFR11g / 10min SEBS-1 (Asahi Kasei Corporation, H1221) Styrene content: 12.5% ​​by weight SEPS (Kraton Polymers, G1730) Styrene content of SEPS is 20% by weight SEBS-2 (Asahi Kasei Corporation, H1063) Styrene content 67% by weight The styrene ratio in Fig. 4 is calculated by multiplying the weight percent of each styrene-based resin material in the adhesive layer by the styrene content of each styrene-based resin material. For example, the adhesive layer in Example 1 uses 30 weight percent SEBS-1, which has a styrene content of 12.5 weight percent, as the styrene-based resin, so the styrene ratio in the adhesive layer is 3.8 weight percent (12.5 x 30 / 100 = 3.75 ≒ 3.8).

[0038] First, the laminated films of Examples 1 to 6 and Comparative Examples 1 and 2 were subjected to the following tests.

[0039] <2. Tensile strength, tensile elongation, 25% modulus> Each laminated film was cut to a size of 40 mm interval and 10 mm width so that the long side was in the MD or TD direction to be measured, to obtain a test piece. The obtained test piece was measured using a Strograph VE-1D manufactured by Toyo Seiki Seisakusho Co., Ltd. in accordance with a method conforming to JIS K-6732. However, the measurement was performed at an atmospheric temperature of 25°C and a test speed of 200 mm / min. The tensile strength and tensile elongation were measured using three test pieces for each example and each comparative example, and the average value was calculated. In addition, the 25% modulus (MPa) was read as the stress value at an elongation rate of 25%.

[0040] <3.Young's modulus> Each laminate film was cut to a size with a gauge interval of 250 mm and 5 mm so that the long side was in the MD or TD direction to be measured, to obtain a test piece. The obtained test piece was measured using a Strograph VE-1D manufactured by Toyo Seiki Seisakusho Co., Ltd. according to a method conforming to ASTM D882. The Young's modulus was measured using three test pieces for each Example and Comparative Example, and the average value was calculated.

[0041] <4. Haze rate> The haze ratio was measured using NDH-2000 manufactured by Nippon Denshoku Industries Co., Ltd.

[0042] <5. Dry heat shrinkage rate> Each laminate film was cut to a size of 150 mm x 20 mm so that the long side was in the MD or TD direction to be measured, and a mark was drawn so that the mark interval was 100 mm to obtain a test piece. Next, one end of the obtained test piece was fixed and placed in a thermostatic chamber PHH-102 manufactured by ESPEC Co., Ltd., whose temperature was set to 100°C. 60 seconds after the insertion, the laminate film was removed, the mark interval was measured, and the shrinkage rate was calculated from the following formula. Dry heat shrinkage rate = {(100 - gauge length after shrinkage (mm)) / 100} x 100 The dry heat shrinkage was calculated by averaging the results of three samples, and values ​​that deviated from the average by 2% or more were not counted.

[0043] The results are shown in Figure 5. Comparing Examples 1 to 4, which use the same type of styrene resin, the breaking strength, breaking elongation, and 25% modulus did not change much even when the styrene ratio in the adhesive layer increased, but Young's modulus showed a tendency to decrease. Comparing Examples 4, 5, and 6, which use different types of styrene resin, the breaking strength, breaking elongation, 25% modulus, and Young's modulus did not change much even when the styrene ratio in the adhesive layer increased.

[0044] Next, the laminated films of Examples 1 to 6 and Comparative Examples 1 and 2 were immersed in a solvent (limonene) at room temperature for 40 minutes, and the interlaminar strength was measured before and after the immersion. The method for measuring the interlaminar strength is as follows.

[0045] Each laminate film was cut to a size of 100 mm x 10 mm so that the MD direction was the long side, and a part of the film edge was peeled off. The strength (N / 10 mm) when each laminate film was peeled off in the 180 degree direction at a pulling speed of 100 mm / min in the long side direction was measured using an Imada digital force gauge ZTS-100N. The test was performed three times to calculate the average interlayer strength. The interlayer strength after solvent immersion was evaluated in the same manner after immersing the laminate film in the solvent for 40 minutes.

[0046] In addition, the solvent immersion time at which the peel strength of the laminated film became 1 N / cm or less after immersion in the solvent was evaluated using the same evaluation method as for the peel strength described above. The results are shown in FIG.

[0047] 6, before immersion in the solvent, the peel strength (interlaminar strength) was roughly the same even if the styrene ratio of the adhesive layer changed. However, as shown in Examples 4 to 6, when the styrene ratio exceeded 10% by weight, the peel strength decreased. However, even if the styrene ratio increased significantly as in Example 6, the peel strength was roughly the same at a content of 10% by weight or more.

[0048] After immersion in the solvent, the peel strength after 40 minutes is greater, since the higher the styrene ratio in the adhesive layer, the longer it takes to dissolve, and for example, in Example 1, which has a low styrene ratio, dissolution of styrene is considered to have progressed, and the peel strength reduction rate is the largest (the ratio of the peel strength after 40 minutes to the original peel strength is lower). On the other hand, in Example 6, which has a high styrene ratio, dissolution of styrene is considered to have progressed less, and the peel strength reduction rate is the smallest.

[0049] The above tendency is reflected in the time required for the peel strength to reach 1 N / cm or less. In Example 1, which had the lowest styrene ratio, the peel strength reached 1 N / cm or less in 1 hour, whereas in Example 6, which had the highest styrene ratio, it took as long as 7.5 hours.

[0050] As described above, an adhesive layer with a low styrene ratio has the advantage of being able to reduce the peel strength in a short time, but the components in the adhesive layer other than styrene remain without dissolving, so that the peeled resin material is recovered with part of the adhesive layer still attached thereto. Therefore, the purity of the recovered material may be somewhat reduced.

[0051] On the other hand, the interlaminar strength of Comparative Examples 1 and 2 was the same as that before immersion even after immersion in the solvent. [Explanation of symbols]

[0052] 1. Laminated film 2 1st resin layer 3 Adhesion layer 4 Second resin layer

Claims

1. a first resin layer having a first surface and a second surface; a second resin layer bonded to at least one of the first surface and the second surface via an adhesive layer; Equipped with The adhesive layer contains a styrene-based resin that can be dissolved by a solvent. Laminated film.

2. The styrene ratio in the adhesive layer is 2 to 75% by weight. The laminated film according to claim 1 .

3. The styrene-based resin is at least one selected from styrene / ethylene / butylene / styrene block copolymer (SEBS), styrene / ethylene / propylene / styrene block copolymer (SEPS), styrene / isoprene / styrene block copolymer (SIS) and styrene / butadiene / styrene block copolymer (SBS). The laminated film according to claim 1 or 2.

4. The thickness of the adhesive layer is 3 to 35 μm. The laminated film according to claim 1 or 2.

5. A step of immersing the laminated film according to claim 1 or 2 in a solvent; peeling the second resin layer from the laminated film immersed in a solvent; The method for separating a laminated film comprises:

6. Prior to the step of immersing in the solvent, a step of unwinding the laminate film from a roll on which the laminate film is wound; winding up the peeled second resin layer and the first resin layer after the peeling of the second resin layer onto a roll; The method for separating a laminated film according to claim 5, further comprising:

Citation Information