Thermal recording medium
A heat-sensitive recording material with a diphenyl sulfone compound and phenolic hydroxyl groups, combined with silica pigment and hollow particles, addresses the issues of light and moisture resistance, ensuring color density and sensitivity under harsh conditions.
Patent Information
- Application Number
- JP2023074598
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Existing heat-sensitive recording materials lack sufficient light resistance, water resistance, and moisture resistance, particularly under harsh conditions, and do not maintain color density during long-term storage.
A heat-sensitive recording material with a heat-sensitive recording layer containing a diphenyl sulfone compound as a color developer and a compound with three or more phenolic hydroxyl groups as a preservability improver, along with silica pigment and hollow particles, to enhance light resistance, water resistance, and moisture resistance.
The material exhibits excellent light resistance, water resistance, and moisture resistance, maintaining color density under harsh conditions and improving dynamic sensitivity.
Smart Images

Figure 2024158945000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosensitive recording medium. [Background technology]
[0002] Thermal recording media develop color through a chemical reaction when heated by a thermal head or the like, resulting in a recorded image. They are used for a wide range of purposes, not only as recording media for facsimiles, automatic ticket vending machines, and scientific measuring instruments, but also as thermal recording labels for POS systems in retail stores, etc., and as receipt paper.
[0003] As described above, thermal recording media are widely used. For this reason, various properties are required for thermal recording media. For example, they are required to be water-resistant and heat-resistant, that is, capable of maintaining the color density of the printed area even when stored for a long period of time in harsh environments such as exposure to water and high temperatures.
[0004] As a heat-sensitive recording material having excellent water resistance, heat resistance, etc., for example, a heat-sensitive recording material has been proposed that uses a urea urethane compound as an electron accepting compound in a heat-sensitive recording layer in combination with 4-hydroxy-4'-allyloxydiphenyl sulfone (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2004-255842 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the thermal recording material of Patent Document 1 does not disclose the resistance of non-printed areas to yellowing when exposed to light for a long time, i.e., light resistance, and the performance in question is unclear.Furthermore, there is no disclosure about the ability to maintain the color density of printed areas even when stored for a long time under high temperature and high humidity conditions, i.e., humidity and heat resistance, and the performance in question is unclear.
[0007] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a thermal recording medium which is excellent in light resistance, water resistance and moist heat resistance.
[0008] Another object of the present invention is to provide a thermal recording medium which, in addition to the above, also has excellent dynamic sensitivity. [Means for solving the problem]
[0009] As a result of intensive research into solving the above problems, the present inventors have found the following: 1. A thermal recording medium having excellent light resistance, water resistance, and moist heat resistance can be provided by containing a diphenyl sulfone compound represented by formula (1) as a developer in a thermal recording layer, further containing a compound having three or more phenolic hydroxyl groups in the molecule as a storage stability improver, and further making the mass ratio of the diphenyl sulfone compound represented by formula (1) to the developer in the thermal recording layer greater than 50 mass%. 2. In addition to the above, by incorporating silica pigment and / or hollow particles as pigments in the heat-sensitive recording layer, it is possible to provide a heat-sensitive recording medium with excellent dynamic sensitivity. The present invention was completed based on these findings.
[0010] That is, the present invention provides a thermosensitive recording medium having a thermosensitive recording layer laminated on a substrate, the thermosensitive recording layer containing a developer and a storage stability improver, the developer containing a diphenyl sulfone compound represented by the following formula (1), the storage stability improver containing a compound having three or more phenolic hydroxyl groups in its molecule, and the mass ratio of the diphenyl sulfone compound represented by the following formula (1) to the developer in the thermosensitive recording layer (mass of the diphenyl sulfone compound represented by the following formula (1) in the thermosensitive recording layer / mass of the developer in the thermosensitive recording layer) is greater than 50 mass%. [ka] (In formula (1), R 1 , R2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 R each independently represents a hydrogen atom or a substituent. 9 represents a hydrogen atom, an alkyl group, or an alkenyl group.
[0011] The heat-sensitive recording layer preferably contains an inorganic pigment and an organic pigment.
[0012] It is preferable that the inorganic pigment contains a silica pigment, and the organic pigment contains hollow particles.
[0013] The mass ratio of the silica pigment to the hollow particles in the thermosensitive recording layer (solid mass of silica pigment in thermosensitive recording layer / solid mass of hollow particles in thermosensitive recording layer) is preferably 10:90 to 90:10.
[0014] The developer preferably contains 4-hydroxy-4'-allyloxydiphenylsulfone.
[0015] The storage stability improver preferably contains a compound represented by the following formula (2). [ka] (In formula (2), R 13 R represents an alkyl group having 4 or less carbon atoms. 14 represents an alkyl group having 4 or less carbon atoms or a cyclohexyl group. 13 , R 14 may be the same or different.)
[0016] It is preferable that the preservability improving agent contains 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane.
[0017] The thermosensitive recording medium preferably comprises an intermediate layer and a topcoat layer in this order on the side of the thermosensitive recording layer opposite the substrate.
[0018] The top coat layer contains a lubricant, and the lubricant preferably contains polyethylene wax and / or paraffin wax. Effect of the Invention
[0019] According to the present invention, it is possible to provide a thermal recording medium having excellent light resistance, water resistance, and moist heat resistance. [Brief description of the drawings]
[0020] [Figure 1] 1 is a schematic cross-sectional view showing one embodiment of a thermosensitive recording medium of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] In this specification, "color development" refers to the ability of a non-printed area (plain area) to turn black when the thermal recording medium is heated. In addition, the ability of the density (color development density) of the printed area to be less likely to decrease even under various storage conditions (for example, in an environment exposed to water, moist heat, plasticizers, etc.) is sometimes called "print storage stability." In other words, in this specification, "print storage stability" is sometimes used as a term that includes the water resistance, moist heat resistance, and plasticizer resistance of the printed area.
[0022] [Thermal recording medium] The thermosensitive recording medium of the present invention has a laminated structure in which at least a thermosensitive recording layer is laminated on a substrate. In the thermosensitive recording medium of the present invention, the thermosensitive recording layer contains at least a color developer and a storage stability improving agent.
[0023] The thermal recording medium of the present invention contains a diphenylsulfone compound represented by formula (1) as the color developer.
[0024] The thermosensitive recording medium of the present invention also contains a compound having three or more phenolic hydroxyl groups in the molecule as the storage stability improving agent.
[0025] Furthermore, the thermosensitive recording medium of the present invention contains, in the thermosensitive recording layer, a mass ratio of the diphenyl sulfone compound represented by formula (1) to the developer (solid mass of the diphenyl sulfone compound represented by formula (1) in the thermosensitive recording layer / solid mass of the developer in the thermosensitive recording layer) of more than 50 mass%.
[0026] Hereinafter, an embodiment of the thermal recording medium of the present invention will be described in detail with reference to the drawings, but the present invention is not limited to the following embodiments.
[0027] FIG. 1 is a schematic cross-sectional view showing one embodiment of a thermosensitive recording medium of the present invention.
[0028] As shown in FIG. 1, the thermosensitive recording material 1 of this embodiment has a layered structure in which an undercoat layer 6, a thermosensitive recording layer 3, an intermediate layer 4, and a topcoat layer 5 are layered in this order on a sheet-like substrate 2.
[0029] (base material) In this embodiment, the substrate 2 functions as a support for the thermal recording medium 1. The substrate 2 is not particularly limited, and may be, for example, fine paper, art paper, coated paper, craft paper, laminated paper obtained by laminating a thermoplastic resin such as polyethylene on these paper substrates, synthetic paper, or porous material such as nonwoven fabric. Transparent synthetic resin films such as polypropylene film, polyethylene terephthalate film, polystyrene film, polycarbonate film, etc. may also be used.
[0030] The thickness of the substrate 2 is not particularly limited, but is preferably about 10 μm to 100 μm, which is excellent in coatability and transparency. The basis weight of the substrate 2 is not particularly limited, but is preferably about 10 g / m 2 ~200g / m 2 This is preferable because it provides excellent coatability and transparency.
[0031] (Undercoat layer) In this embodiment, the undercoat layer 6 has functions such as heat insulation to prevent the dissipation of heat applied from the thermal head, cushioning, etc. Also, it has a function of improving the adhesion between the substrate 2 and the thermosensitive recording layer 3. The undercoat layer 6 is not particularly limited, and is formed, for example, by adding hollow particles as a filler to a binder.
[0032] By providing the thermally insulating undercoat layer 6 on the thermal recording medium 1 as described above, the dissipation of heat applied from the thermal head during printing is suppressed. This allows the thermal energy during printing to be efficiently applied to the thermal recording layer, making it possible to print with less printing energy. In other words, by providing the thermally insulating undercoat layer, the printing sensitivity is improved. This makes it possible to suppress an increase in the voltage applied to the thermal head, and as a result, to suppress burn-in of the thermal head.
[0033] In this embodiment, the average particle diameter of the hollow particles added as a filler to the undercoat layer 6 is not particularly limited, and is preferably 0.1 μm to 100 μm, more preferably 0.2 μm to 20 μm, even more preferably 0.3 μm to 5 μm, and particularly preferably 0.5 μm to 3 μm. Within such a range, the effect of improving the heat insulating properties of the undercoat layer 6 can be sufficiently obtained, and the surface after drying can be made sufficiently smooth because it is easy to apply uniformly. Here, the average particle diameter is the weight average particle diameter measured by a laser diffraction method. The measurement of the average particle diameter by the laser diffraction method can be performed using, for example, a product name "MT3300EX-II" manufactured by Microtrack Bell Co., Ltd.
[0034] The hollow ratio of the hollow particles is not particularly limited, and is preferably 30% to 99%. Within this range, sufficient heat insulation can be obtained. Furthermore, the higher the hollow ratio of the hollow particles, the higher the heat insulation effect. Therefore, color can be effectively developed with less printing energy. In other words, it is believed that the higher the hollow ratio of the hollow particles, the more the dynamic sensitivity of the thermal recording medium 1 is improved, and thus the printing quality is improved.
[0035] Here, the hollow ratio of the hollow particles is calculated by the following formula. Hollow ratio = {(void volume) / (hollow particle volume)} x 100
[0036] In this embodiment, the content of hollow particles in the undercoat layer 6 is preferably 40% by mass to 90% by mass when the solid content mass of the undercoat layer is taken as 100% by mass. If it is 40% by mass or more, the effect of improving the heat insulating property of the undercoat layer 6 is sufficiently obtained, and the dynamic sensitivity of the thermosensitive recording medium 1 is further improved, which is preferable. Also, if it is 90% by mass or less, the adhesion between the substrate 2 and the thermosensitive recording layer 3 is sufficient, which is preferable.
[0037] In this specification, the term "mass of solid content" refers to the mass of non-volatile content (solid content) excluding solvents (volatile components) such as water contained in the coating liquid and its raw materials.
[0038] The material constituting the hollow particles is not particularly limited, and examples thereof include thermoplastic resins. Examples of the thermoplastic resins include poly(meth)acrylic acid ester-based resins such as styrene-acrylic resins and polymethyl methacrylate resins, polystyrene-based resins, urea-formaldehyde resins, polyolefin resins, polyvinyl chloride-based resins, polyvinylidene chloride-based resins, polyvinyl acetate-based resins, polyacrylonitrile-based resins, and polybutadiene-based resins. These hollow particles can be used alone or in combination of two or more.
[0039] In the present embodiment, the filler of the undercoat layer 6 may be a material other than hollow particles. Examples of the filler include calcined kaolin, aluminum oxide, aluminum silicate, calcium carbonate, titanium oxide, barium sulfate, silica gel, activated clay, talc, clay, kaolinite, diatomaceous earth, white carbon, magnesium carbonate, magnesium oxide, magnesium hydroxide, zinc oxide, polystyrene resin particles, urea-formalin resin particles, polyolefin resin particles, etc. These fillers may be used alone or in combination of two or more.
[0040] The binder contained in the undercoat layer 6 in this embodiment is not particularly limited, and examples thereof include modified styrene-butadiene latex, an acrylic-styrene copolymer, a styrene-butadiene copolymer, an acrylic-butadiene-styrene copolymer, a vinyl acetate resin, a vinyl acetate-acrylic acid copolymer, a styrene-acrylic acid ester copolymer, an acrylic acid ester-based resin, and a polyurethane-based resin.
[0041] Other binders that may be used include polyvinyl alcohol, starch and its derivatives, cellulose derivatives such as methoxycellulose, hydroxyethylcellulose, carboxymethylcellulose, methylcellulose, and ethylcellulose, water-soluble polymers such as sodium polyacrylate, polyvinylpyrrolidone, acrylamide-acrylic acid ester copolymers, acrylamide-acrylic acid ester-methacrylic acid terpolymers, alkali salts of styrene-maleic anhydride copolymers, alkali salts of isobutylene-maleic anhydride copolymers, polyacrylamide, sodium alginate, gelatin, and casein. These binders may be used alone or in combination of two or more.
[0042] The coating amount (dry weight) of the undercoat layer 6 in this embodiment is not particularly limited, but is, for example, 1 g / m 2 ~10g / m 2 and preferably 2 g / m 2 ~5g / m 2 It is.
[0043] The thickness of the undercoat layer 6 in the present embodiment is not particularly limited, but is, for example, 1 μm to 20 μm, and preferably 2 μm to 10 μm.
[0044] In the present embodiment, when the coating amount and thickness of the undercoat layer 6 are within the above ranges, the heat insulating function of the undercoat layer 6 becomes more preferable, and therefore the dynamic sensitivity is further improved, which is preferable.
[0045] (Thermal recording layer) In this embodiment, the thermosensitive recording layer 3 is a layer that develops color through a chemical reaction when heated by a thermal head or the like, and forms a recorded image on the thermosensitive recording medium 1. In this embodiment, the thermosensitive recording layer 3 contains at least a color developer and a storage stability improver. The thermosensitive recording layer preferably contains a color former and a pigment, and may further contain other components as necessary.
[0046] In this embodiment, the thermosensitive recording layer 3 contains at least a diphenylsulfone compound represented by the following formula (1) as the color developer. [ka]
[0047] In formula (1), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 R each independently represents a hydrogen atom or a substituent. 9 represents a hydrogen atom, an alkyl group, or an alkenyl group.
[0048] It is believed that when the diphenyl sulfone compound represented by the above formula (1) is heated, the phenolic hydroxyl group supplies a proton to, for example, a dye described below, to cause color development, and also forms an intermolecular hydrogen bond with the dye to maintain the color development.
[0049] The above-mentioned "substituent" can be a group other than a hydrogen atom without any particular limitation, and examples thereof include a halogen atom, a nitro group, an amino group, an alkyl group, an alkenyl group, an alkoxy group, an aryl group, an aryloxy group, an alkylcarbonyloxy group, an alkylcarbonylamino group, an arylcarbonylamino group, an alkylsulfonylamino group, an arylsulfonylamino group, a monoalkylamino group, a dialkylamino group, and an arylamino group.
[0050] The above-mentioned "halogen atom" includes a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom.
[0051] Examples of the "alkyl group" and "alkyl" include linear or branched alkyl groups having 1 to 12 carbon atoms, such as a methyl group, ethyl group, normal propyl group, isopropyl group, normal butyl group, isobutyl group, secondary butyl group, tertiary butyl group, normal pentyl group, isopentyl group, tertiary pentyl group, neopentyl group, 2,3-dimethylpropyl group, 1-ethylpropyl group, 1-methylbutyl group, 2-methylbutyl group, normal hexyl group, isohexyl group, 2-hexyl group, 3-hexyl group, 2-methylpentyl group, 3-methylpentyl group, normal heptyl group, normal octyl group, normal nonyl group, normal decyl, normal undecyl group, and normal dodecyl group.
[0052] Examples of the above-mentioned "alkenyl group" include linear or branched alkenyl groups having 2 to 6 carbon atoms, such as a vinyl group, an allyl group, an isopropenyl group, a 1-butenyl group, a 2-butenyl group, a 2-methyl-2-propenyl group, a 1-methyl-2-propenyl group, a 2-methyl-1-propenyl group, a pentenyl group, a 1-hexenyl group, and a 3,3-dimethyl-1-butenyl group.
[0053] Examples of the "alkoxy group" include straight-chain or branched-chain alkoxy groups having 1 to 8 carbon atoms, such as a methoxy group, ethoxy group, normal propoxy group, isopropoxy group, normal butoxy group, sec-butoxy group, tertiary butoxy group, normal pentyloxy group, isopentyloxy group, tertiary pentyloxy group, neopentyloxy group, 2,3-dimethylpropyloxy group, 1-ethylpropyloxy group, 1-methylbutyloxy group, normal hexyloxy group, isohexyloxy group, normal heptyloxy group, and normal octyloxy group.
[0054] The above-mentioned "aryl group" and "aryl" include, for example, aromatic hydrocarbon groups having 6 to 10 carbon atoms, such as a phenyl group, a 1-naphthyl group, and a 2-naphthyl group.
[0055] In the above "dialkylamino group", the two alkyl groups may be the same or different.
[0056] As the diphenylsulfone compound represented by formula (1), a compound represented by the following formula (1a) is preferred from the viewpoint of imparting excellent color development to the thermal recording medium 1. [ka]
[0057] In formula (1a), R 10 , R 11 , and R 12 Each independently represents a hydrogen atom, an alkyl group, or an alkenyl group. 12 If hydrogen atom, R 10 , and R 11 each independently represents an alkyl group or an alkenyl group; R 12 When R is an alkyl group or an alkenyl group, R 10 , and R 11 represents a hydrogen atom.
[0058] Specific examples of the compound represented by the above formula (1a) include 4-hydroxy-4'-allyloxydiphenyl sulfone, 4-hydroxy-4'-n-propoxydiphenyl sulfone, 4-hydroxy-4'-isopropoxydiphenyl sulfone, bis(3-allyl-4-hydroxyphenyl)sulfone, 4-hydroxy-4'-ethoxydiphenyl sulfone, 4-hydroxy-4'-n-butoxydiphenyl sulfone, etc. Among these, 4-hydroxy-4'-allyloxydiphenyl sulfone is particularly preferred.
[0059] In this embodiment, when the total mass of the color developer in the thermosensitive recording layer 3 is taken as 100 mass%, the mass of the diphenyl sulfone compound represented by the above formula (1) is greater than 50 mass%, more preferably greater than 60 mass%, even more preferably greater than 70 mass%, even more preferably greater than 80 mass%, particularly preferably greater than 90 mass%, and most preferably 100 mass%. When it is within this range, the optical density of the thermosensitive recording medium 1 after printing becomes sufficiently high, which is preferable because the print storage stability is further improved.
[0060] In this embodiment, the thermosensitive recording layer 3 may contain, as a developer, a single diphenyl sulfone compound represented by the above formula (1), or may contain two or more diphenyl sulfone compounds represented by the above formula (1).
[0061] In this embodiment, the thermosensitive recording layer 3 may contain a color developer other than the diphenyl sulfone compound represented by the above formula (1) (other color developers) as the color developer, within a range that does not impair the effects of the present invention.
[0062] Other color developers include, for example, 1,1-bis(p-hydroxyphenyl)cyclohexane, 1,1-bis(p-hydroxyphenyl)propane, 2,2-bis(p-hydroxyphenyl)propane, 2,2-bis(p-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2'-methylenebis(4-chlorophenol), 2,2-bis(4-hydroxyphenyl)-4-methylpentane, poly(4-hydroxybenzoic acid), 4-hydroxybenzoic acid benzyl, 2,4-bis(phenylsulfonyl)phenol, α-{4-[(4-hydroxyphenyl)sulfonyl]phenyl}-ω-hydroxypoly(polymerization degree n=1 to 7)(oxyethyleneoxyethyleneoxy-p-phenylenesulfonyl-p-phenylene), 3,5-bis(α-methylbenzyl)salicylic acid, bis[4-( n-Octyloxycarbonylamino)salicylate zinc], 4,4'-bis(p-tolylsulfonylaminocarbonylamino)diphenylmethane, 4-hydroxybenzenesulfonanilide, 2'-(3-phenylureido)benzenesulfonanilide, N-(2-hydroxyphenyl)-2-[(4-hydroxyphenyl)thio]acetamide, N-(4-hydroxyphenyl)-2-[(4-hydroxyphenyl)thio]acetamide, 4-[[4-[4-[[4-(1-methylethoxy)phenyl]sulfonylphenoxy]butoxy]phenyl]sulfonyl]phenol, 4-tert-butylphenol-formaldehyde polycondensate, N-(p-toluenesulfonyl)-N'-(3-p-toluenesulfonyloxyphenyl)urea, 1-phenyl-3-(4-methylphenylsulfonyl)urea, etc.
[0063] In this embodiment, when the solid content mass of the thermosensitive recording layer 3 is 100% by mass, the mass of the diphenylsulfone compound represented by the above formula (1) is preferably 10% by mass or more and 70% by mass or less, more preferably 20% by mass or more and 60% by mass or less, even more preferably 30% by mass or more and 50% by mass or less, and particularly preferably 35% by mass or more and 45% by mass or less. When the mass of the diphenylsulfone compound represented by the above formula (1) is 10% by mass or more, the content of the color developer becomes sufficient, the optical density after printing becomes sufficiently high, and the print storage stability is further improved, which is preferable. Also, when it is 70% by mass or less, the color developer can be sufficiently melted and colored even with less heat applied from the thermal head. In other words, it is preferable because the dynamic sensitivity is further improved.
[0064] In this embodiment, the thermosensitive recording layer 3 contains at least a compound having three or more phenolic hydroxyl groups in the molecule as a storage stability improving agent.
[0065] The compound having three or more phenolic hydroxyl groups in the molecule is believed to be able to prevent oxidative decomposition of the developer and the color former described below by capturing hydroperoxy radicals generated by air oxidation with the phenolic hydroxyl groups, thereby improving light resistance and print storage stability.
[0066] Of the above compounds having three or more phenolic hydroxyl groups in the molecule, the compounds represented by the following formula (2) are preferred. [ka]
[0067] In formula (2), R 13 R represents an alkyl group having 4 or less carbon atoms. 14 represents an alkyl group having 4 or less carbon atoms or a cyclohexyl group. 13 , R 14 may be the same or different.
[0068] Specific examples of the compound represented by the above formula (2) include 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane, tris(2,6-dimethyl-4-t-butyl-3-hydroxybenzyl)isocyanurate, etc. Among these, 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane is particularly preferred.
[0069] In this embodiment, the thermosensitive recording layer 3 may contain, as a storage stability improver, a single compound having three or more phenolic hydroxyl groups in the molecule, or two or more types of compounds having three or more phenolic hydroxyl groups in the molecule. In order to obtain excellent light resistance and print storage stability, it is preferable to contain a single compound having three or more phenolic hydroxyl groups.
[0070] In this embodiment, the thermosensitive recording layer 3 may contain a storage stability improver other than the compound having three or more phenolic hydroxyl groups (other storage stability improver) as long as the effect of the present invention is not impaired.
[0071] The other preservative improvers are not particularly limited, and examples thereof include sodium-2,2'-methylenebis(4,6-di-t-butylphenyl)phosphite, 4,4,butylidenebis(3-methyl-6-t-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane, tris(2,6-dimethyl 4-(2-methylglycyloxy)-4'-benzyloxydiphenylsulfone, 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), diethylthiourea, zinc dibutyldithiocarbamate, and 4,4'-thiobis(6-t-butyl-m-cresol). Also, known surfactants may be included. These preservatives may be used alone or in combination of two or more.
[0072] In this embodiment, the mass of the compound having three or more phenolic hydroxyl groups in the molecule when the mass of the entire storage stability improver contained in the thermosensitive recording layer 3 is taken as 100% by mass is not particularly limited, but from the viewpoint of improving light fastness and print storage stability, it is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. When it is within this range, it is preferable because the light fastness and print storage stability of the thermosensitive recording medium 1 are further improved.
[0073] In this embodiment, when the solid content mass of the thermosensitive recording layer 3 is 100 mass%, the mass of the compound having three or more phenolic hydroxyl groups in the molecule is preferably 0.1 mass% to 40 mass%, more preferably 0.5 mass% to 35 mass%, even more preferably 1 mass% to 30 mass%, even more preferably 3 mass% to 25 mass%, even more preferably 5 mass% to 20 mass%, and particularly preferably 10 mass% to 15 mass%. When the mass of the compound having three or more phenolic hydroxyl groups in the molecule is 0.1 mass% or more, it is preferable in that it can impart better light resistance and print storage stability to the thermosensitive recording medium 1 of this embodiment. In addition, when the mass is 40 mass% or less, it is preferable because the heat resistance and moist heat resistance are better.
[0074] In this embodiment, the light fastness, water fastness, and moist heat resistance of the thermal recording medium 1 are improved by incorporating a compound having three or more phenolic hydroxyl groups in the molecule into the thermal recording layer 3. Furthermore, the diphenyl sulfone compound represented by the above formula (1) tends to have low light fastness when used alone, but by combining it with the above compound having three or more phenolic hydroxyl groups in the molecule, the light fastness, water fastness, and moist heat resistance of the thermal recording medium 1 tend to be significantly improved.
[0075] In this embodiment, when the total mass of the color developer contained in the thermosensitive recording layer 3 is taken as 100 parts by mass, the total mass of the storage stability improver is preferably 2 parts by mass or more, more preferably 5 parts by mass or more, even more preferably 10 parts by mass or more, even more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, and particularly preferably 40 parts by mass or more. When it is in this range, the light resistance and print storage stability of the thermosensitive recording medium 1 are further improved, which is preferable. Furthermore, when the total mass of the color developer contained in the thermosensitive recording layer 3 is taken as 100 parts by mass, the total mass of the storage stability improver is preferably 100 parts by mass or less, more preferably 90 parts by mass or less, even more preferably 80 parts by mass or less, even more preferably 70 parts by mass or less, even more preferably 60 parts by mass or less, and particularly preferably 50 parts by mass or less. When it is in this range, it is preferable in terms of cost-effectiveness.
[0076] In this embodiment, the thermosensitive recording layer 3 may contain a pigment. The pigment is not particularly limited, and examples thereof include inorganic pigments and organic pigments. Specifically, examples of inorganic pigments include silica pigments (mainly silicon dioxide), calcium carbonate, diatomaceous earth, talc, kaolin, calcined kaolin, magnesium carbonate, titanium oxide, zinc oxide, and aluminum hydroxide. Among these, the inclusion of silica pigments is preferable since dynamic sensitivity is further improved. Examples of organic pigments include hollow particles, and the inclusion of hollow particles is preferable since dynamic sensitivity is further improved. These pigments can be used alone or in combination of two or more kinds.
[0077] In this embodiment, the thermosensitive recording layer 3 preferably contains an inorganic pigment and an organic pigment. Among them, it is more preferable to contain a silica pigment and a hollow particle. By containing these, the dynamic sensitivity tends to be further improved.
[0078] The average particle size of the silica pigment is not particularly limited, and is preferably 0.01 μm to 100 μm, more preferably 0.05 μm to 20 μm, even more preferably 0.1 μm to 5 μm, and particularly preferably 0.2 μm to 2 μm. Such a range is preferable because it improves dynamic sensitivity, makes it easier to apply uniformly, and provides a sufficiently smooth surface after drying. Here, the average particle size is the weight average particle size measured by a laser diffraction method. Measurement of the average particle size by the laser diffraction method can be performed, for example, using a product name "MT3300EX-II" manufactured by Microtrack Bell Co., Ltd.
[0079] The material constituting the hollow particles is not particularly limited, and may be, for example, a thermoplastic resin. Examples of the thermoplastic resin include styrene-acrylic resin, polystyrene resin, urea-formaldehyde resin, polyolefin resin, polyvinyl chloride resin, polyvinylidene chloride resin, polyvinyl acetate resin, poly(meth)acrylic acid ester resin such as polymethyl methacrylate resin, polyacrylonitrile resin, polybutadiene resin, etc. In addition, the hollow particles made of these resins may be used alone or in combination of two or more kinds.
[0080] The average particle size of the hollow particles is not particularly limited, and is preferably 0.1 μm to 100 μm, more preferably 0.2 μm to 20 μm, and even more preferably 0.5 μm to 5 μm. Within such a range, the effect of improving heat insulation is sufficiently obtained, so that the dynamic sensitivity is improved, and the surface after drying is sufficiently smooth because it is easy to apply uniformly. Here, the average particle size is the weight average particle size measured by a laser diffraction method. The measurement of the average particle size by the laser diffraction method can be performed, for example, using a product name "MT3300EX-II" manufactured by Microtrack Bell Co., Ltd.
[0081] The hollow ratio of the hollow particles is not particularly limited, but is preferably 30% to 99%. Within this range, sufficient heat insulation can be obtained. Furthermore, the higher the hollow ratio of the hollow particles, the higher the heat insulation effect. Therefore, color can be effectively developed with less printing energy. In other words, it is believed that the higher the hollow ratio of the hollow particles, the higher the dynamic sensitivity of the thermal recording medium 1, and thus the better the printing quality.
[0082] Here, the hollow ratio of the hollow particles is calculated by the following formula. Hollow ratio = {(void volume) / (hollow particle volume)} x 100
[0083] In this embodiment, when the solid content mass of the thermosensitive recording layer 3 is taken as 100 mass%, the mass of the pigment is preferably 0.1 mass% to 40 mass% or less, more preferably 1 mass% to 30 mass% or less, even more preferably 3 mass% to 20 mass% or less, and particularly preferably 5 mass% to 10 mass% or less. By containing the pigment in this range, excellent dynamic sensitivity can be obtained.
[0084] In this embodiment, the mass ratio of silica pigment to hollow particles contained in the thermosensitive recording layer 3 is not particularly limited, but is preferably 10:90 to 90:10, more preferably 20:80 to 80:20, even more preferably 30:70 to 70:30, even more preferably 40:60 to 60:40, and particularly preferably 50:50. When the mass ratio of silica pigment to hollow particles is within this range, excellent dynamic sensitivity can be achieved while providing excellent light fastness and print storage stability.
[0085] In this embodiment, the thermosensitive recording layer 3 may contain a color former. In this specification, the color former is a color former that develops color when heated, and is a component that develops color through a chemical reaction when heated, for example, by a thermal head, and forms a recorded image on the thermosensitive recording medium 1 of this embodiment. The color former that develops color when heated is not particularly limited, and a commonly used known dye can be used. Examples of this dye include 3-(N-isobutyl-N-ethyl)amino-6-methyl-7-anilinofluoran, 3-(N-isopentyl-N-ethyl)amino-6-methyl-7-o-chloroanilinofluoran, 3-(N-methyl-Np-toluidino)-6-methyl-7-anilinofluoran, 3-(N-ethyl ...-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N-ethyl-N- 3-(N-isopentyl)amino-6-methyl-7-anilinofluoran, 3-(N-ethoxypropyl-N-ethyl)amino-6-methyl-7-anilinofluoran, 3-(N-cyclohexyl-N-methyl)amino-6-methyl-7-anilinofluoran, 3-(N-methyl-Nn-propyl)amino-6-methyl-7-anilinofluoran, 3-dibutylamino-6-methyl-7-anilino Fluoran, 3-diethylamino-6-methyl-7-p-toluidinofluoran, 3-diethylamino-6-methyl-7-anilinofluoran, 3-diethylamino-6-methyl-8-methylfluoran, 3-diethylamino-7-(m-trifluoromethylanilino)fluoran, 3-diethylamino-7-(o-chloroanilino)fluoran, 3-diethylamino-7-chlorofluoran, 3-dibutylamino-6-methyl-7-bromofluoran, 3-dibutylamino-7-(o-chloroanilino)fluoran, 3-dipentylamino-6-methyl-7-anilinofluoran, 3-dimethylamino-5-methyl-7-methylfluoran, 3-pyrrolidino-6-methyl-7-anilinofluoran, crystal violet lactone, etc. can be used alone or in combination of two or more.
[0086] The average particle diameter of the color former is preferably 0.1 μm to 1.0 μm. Since the color former melts and reacts, the reaction slows down as the particle diameter increases, and the sensitivity characteristics decrease. On the other hand, as the particle diameter decreases, the risk of coloring at an unexpected temperature due to heat when drying the paint increases. In this embodiment, the sensitivity characteristics and coloring temperature of the color former can be appropriately adjusted by setting the particle diameter of the color former to the above range. Here, the average particle diameter is the weight average particle diameter measured by the laser diffraction method. The measurement of the average particle diameter by the laser diffraction method can be performed using, for example, a product name "MT3300EX-II" manufactured by Microtrack Bell Co., Ltd.
[0087] In this embodiment, when the solid content mass of the thermosensitive recording layer 3 is 100% by mass, the mass of the color former is preferably 5% by mass or more and 50% by mass or less, more preferably 10% by mass or more and 45% by mass or less, even more preferably 15% by mass or more and 40% by mass or less, and particularly preferably 20% by mass or more and 35% by mass or less. When the color former is contained in this range, the optical density after printing becomes sufficiently high, and thus the print storage stability is further improved, which is preferable. It is preferable that the developer is contained in a ratio of 1 to 3 parts by dry weight to the color former. By containing it in this ratio, the optical density after printing becomes sufficiently high, and thus the print storage stability is further improved, which is preferable.
[0088] Furthermore, the thermosensitive recording layer 3 in this embodiment may contain additives such as a binder, a sensitizer, a lubricant, and a filler, as necessary.
[0089] The binder contained in the thermal recording layer 3 in this embodiment is not particularly limited, and examples thereof include polyvinyl alcohol, modified polyvinyl alcohol, starch, casein, gelatin, polyamide, polyacrylamide, modified polyacrylamide, hydroxyethyl cellulose, methyl cellulose, carboxymethyl cellulose, hydroxypropyl cellulose, polyvinyl acetate, polyacrylic acid ester, styrene-acrylic copolymer, styrene-maleic anhydride copolymer, isobutylene-maleic anhydride copolymer, diisobutylene-maleic anhydride copolymer, vinyl acetate-maleic anhydride copolymer, methyl vinyl-maleic anhydride copolymer, isopropylene-maleic anhydride copolymer, styrene-butadiene copolymer, polyvinyl chloride, polyvinylidene chloride, vinyl chloride-vinyl acetate copolymer, polyurethane, polystyrene, polyvinylpyrrolidone, acrylic acid ester, acrylonitrile, methyl vinyl ether, etc. These binders can be used alone or in combination of two or more.
[0090] The sensitizer contained in the thermal recording layer 3 in this embodiment is not particularly limited, and examples thereof include stearic acid, stearic acid amide, stearic acid anilide, methylol stearic acid amide, methylene bis stearic acid amide, ethylene bis stearic acid amide, 1-benzyloxynaphthalene, 2-benzyloxynaphthalene, 2,6-diisopropylnaphthalene, 1,2-diphenoxyethane, 1,2-diphenoxymethylbenzene, 1,2-bis(3,4-dimethyl Examples of sensitizers include those which are solid at room temperature and preferably have a melting point of about 70° C. or higher, such as 1,2-bis(3-methylphenoxy)ethane, 1,2-bis(4-methylphenoxy)ethane, di(p-chlorobenzyl) oxalate, di(p-methylbenzyl) oxalate, dibenzyl oxalate, p-benzylbiphenyl, m-terphenyl, diphenylsulfone, benzyl p-benzyloxybenzoate, dibenzyl terephthalate, and p-toluenesulfonamide. These sensitizers can be used alone or in combination of two or more.
[0091] The lubricant contained in the thermal recording layer 3 in this embodiment is not particularly limited, and examples thereof include paraffin wax, fatty acids such as oleic acid, polyolefin waxes such as polyethylene wax, metal soaps such as zinc stearate, ester waxes such as carnauba wax, silicone oil, oils such as whale oil, etc. These lubricants can be used alone or in combination of two or more kinds.
[0092] The filler contained in the thermosensitive recording layer 3 in this embodiment is not particularly limited, and examples thereof include aluminum hydroxide, magnesium hydroxide, aluminum oxide, magnesium oxide, aluminum silicate, calcium carbonate, magnesium carbonate, titanium oxide, barium sulfate, silica gel, activated clay, talc, clay, kaolin, calcined kaolin, diatomaceous earth, white carbon, zinc oxide, silicon oxide, colloidal silica, styrene-acrylic resin, polystyrene resin particles, urea-formalin resin particles, polyolefin resin particles, etc. These fillers may be used alone or in combination of two or more kinds.
[0093] The coating amount (dry weight) of the thermal recording layer 3 in this embodiment is not particularly limited, but is, for example, 1 g / m 2 ~10g / m 2 and preferably 2 g / m 2 ~5g / m 2 It is.
[0094] The thickness of the thermosensitive recording layer 3 in this embodiment is not particularly limited, but is, for example, 1 μm to 20 μm, and preferably 2 μm to 5 μm.
[0095] When the coating amount and thickness of the thermosensitive recording layer 3 in this embodiment are within the above ranges, the light resistance and print storage stability of the thermosensitive recording layer 3 become more preferable.
[0096] (Middle class) In this embodiment, the intermediate layer 4 has a function of improving the print preservability of the thermosensitive recording medium 1. Specifically, for example, if a plasticizer or the like attached to the thermosensitive recording medium 1 permeates into the thermosensitive recording layer 3, the color former may change in quality and the printed portion may disappear. In such a case, by providing the intermediate layer 4 on the top coat layer side of the thermosensitive recording layer 3, the printed portion becomes less susceptible to the effects of the attached matter, and the print preservability is improved.
[0097] The intermediate layer 4 is mainly made of a resin. For example, it may be an emulsion of an acrylic resin, a water-soluble resin such as a polyvinyl alcohol (PVA) resin, a styrene-butadiene copolymer (SBR) resin, etc. These resins may be used alone or in combination of two or more kinds.
[0098] Furthermore, the resin contained in the intermediate layer 4 may be a resin having a water-soluble portion, such as a polyvinyl alcohol (PVA) resin having a hydroxyl group as a hydrophilic structural unit, or a resin having a core-shell structure in which hydrophobic core particles are coated with a water-soluble shell polymer, such as a core-shell type acrylic resin. By using these core-shell type resins, the print storage stability and transparency of the thermal recording medium 1 can be improved.
[0099] The core-shell type resin may be, for example, a core-shell type acrylic resin commercially available under the name "Barrierstar (manufactured by Mitsui Chemicals, Inc.)." These resins may be used alone or in combination of two or more kinds.
[0100] The coating amount (dry weight) of the intermediate layer 4 in this embodiment is not particularly limited, but is, for example, 0.1 g / m 2 ~10g / m 2 and preferably 1 g / m 2 ~5g / m 2 It is.
[0101] The thickness of the intermediate layer 4 in this embodiment is not particularly limited, but is, for example, 0.5 μm to 20 μm, and preferably 1 μm to 5 μm.
[0102] In the present embodiment, when the coating amount and thickness of the intermediate layer 4 are within the above range, the print preservation stability of the thermal recording medium 1 is further improved, which is preferable.
[0103] (Topcoat layer) In this embodiment, the topcoat layer 5 has a function of improving matching (suitability) with respect to the head, that is, improving the slipperiness of the head and suppressing adhesion of residue to the head.
[0104] The material for the topcoat layer 5 is not particularly limited, and for example, a binder to which a lubricant, a filler, a crosslinking agent, etc. have been added can be used.
[0105] The binder contained in the topcoat layer 5 in this embodiment is not particularly limited, and may be, for example, a resin. Specific examples include an emulsion of an acrylic resin, a water-soluble resin such as a polyvinyl alcohol (PVA) resin, and a styrene-butadiene copolymer (SBR). These materials may be used alone or in combination of two or more kinds.
[0106] The cross-linking agent contained in the top coat layer 5 in this embodiment is not particularly limited, and examples thereof include zirconium carbonate.
[0107] The lubricant contained in the topcoat layer 5 in this embodiment is not particularly limited, and examples thereof include paraffin wax, fatty acids such as oleic acid, polyolefin waxes such as polyethylene wax, metal soaps such as zinc stearate, ester waxes such as carnauba wax, and oils such as silicone oil and whale oil. These lubricants can be used alone or in combination of two or more. Among them, polyethylene wax and paraffin wax are preferred because they further improve the dynamic sensitivity of the thermal recording medium 1 and the matching (suitability) with the head.
[0108] In this embodiment, when the solid content mass of the topcoat layer 5 is 100% by mass, the total mass of the lubricant is not particularly limited, but is, for example, 1% by mass or more, preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 13.5% by mass or more, and particularly preferably 15% by mass or more. Also, for example, it is 40% by mass or less, preferably 30% by mass or less, and even more preferably 20% by mass or less. When the lubricant is contained within this range, the dynamic sensitivity of the thermal recording medium 1 and the matching (suitability) with the head are further improved, which is preferable.
[0109] The average particle size of the polyethylene and paraffin lubricants is preferably 1.5 μm or less. Here, the average particle size is the weight average particle size measured by a laser diffraction method. The measurement of the average particle size by the laser diffraction method can be performed, for example, using a product name "MT3300EX-II" manufactured by Microtrack Bell.
[0110] The filler contained in the topcoat layer 5 in this embodiment is not particularly limited, and examples thereof include calcium carbonate, polymethyl methacrylate (PMMA), aluminum hydroxide, aluminum oxide, aluminum silicate, heavy calcium carbonate, light calcium carbonate, titanium oxide, barium sulfate, silica gel, activated clay, talc, clay, kaolinite, diatomaceous earth, white carbon, magnesium carbonate, magnesium oxide, magnesium hydroxide, zinc oxide, polystyrene resin particles, urea-formalin resin particles, polyolefin resin particles, etc. These fillers can be used alone or in combination of two or more. Among them, when calcium carbonate is blended, it is preferable because the cost performance of the thermal recording medium 1 and the matching (suitability) with the thermal head are further improved.
[0111] In particular, when the solid content mass of the topcoat layer 5 is taken as 100 mass%, the mass of the filler is preferably 5 mass% to 70 mass% or less, more preferably 10 mass% to 60 mass% or less, even more preferably 20 mass% to 50 mass% or less, and particularly preferably 30 mass% to 40 mass% or less. When the filler is contained within this range, the cost performance of the thermal recording medium 1 and the matching (suitability) with the thermal head are further improved, which is preferable.
[0112] When the filler is within the above range, the surface becomes uneven, and the contact area between the thermal recording medium 1 and the thermal head is reduced, improving the slipperiness and ultimately resulting in better color development (printing characteristics).
[0113] The average particle size of the filler is preferably 1.0 μm or less. Here, the average particle size is the weight average particle size measured by a laser diffraction method. The average particle size can be measured by using, for example, a product name "MT3300EX-II" manufactured by Microtrack Bell.
[0114] The coating amount (dry weight) of the topcoat layer 5 in this embodiment is not particularly limited, but is, for example, 0.1 g / m 2 ~10g / m 2 and preferably 0.5 g / m 2 ~5g / m 2 It is.
[0115] The thickness of the topcoat layer 5 in the present embodiment is not particularly limited, but is, for example, 0.1 μm to 20 μm, and preferably 0.5 μm to 2 μm.
[0116] In the present embodiment, when the coating amount and thickness of the topcoat layer 5 are within the above ranges, the light resistance and print storage stability of the thermal recording medium 1 are further improved, which is preferable.
[0117] In this embodiment, the undercoat layer 6, the thermosensitive recording layer 3, the intermediate layer 4, and the topcoat layer 5 are formed in this order on the substrate 2, but in other embodiments of the present invention, at least one of the undercoat layer 6, the intermediate layer 4, and the topcoat layer 5 may be omitted. Also, one or more different layers may be formed on the surface of each layer.
[0118] The thermosensitive recording medium of the above embodiment has the above-mentioned configuration and is therefore excellent in light resistance and print storage stability (particularly water resistance, plasticizer resistance, and moist heat resistance).
[0119] When the thermal recording medium of the above embodiment is subjected to a water resistance test using the method and conditions described in the examples, the optical density (OD value) of the printed area after the test is, for example, 1.0 or more, preferably 1.1 or more, more preferably 1.2 or more, even more preferably 1.3 or more, and particularly preferably 1.4 or more.
[0120] When the thermosensitive recording medium of the above embodiment is subjected to a plasticizer resistance test according to the method and conditions described in the Examples, the optical density (OD value) of the printed portion after the test is, for example, 1.5 or more, and preferably 1.6 or more.
[0121] When the thermal recording medium of the above embodiment is subjected to a moist heat resistance test at 40°C using the method and conditions described in the examples, the optical density (OD value) of the printed area after the test is, for example, 1.3 or more, preferably 1.4 or more, and more preferably 1.5 or more.
[0122] When the thermal recording medium of the above embodiment is subjected to a moist heat resistance test at 50°C using the method and conditions described in the examples, the optical density (OD value) of the printed area after the test is, for example, 0.8 or more, preferably 0.9 or more, more preferably 1.0 or more, even more preferably 1.1 or more, even more preferably 1.2 or more, even more preferably 1.3 or more, and particularly preferably 1.4 or more.
[0123] When the thermal recording medium of the above embodiment is subjected to a light resistance test using the method and conditions described in the examples, the b value of the non-printed area after the test is, for example, 2.4 or less, preferably 2.3 or less, more preferably 2.2 or less, and even more preferably 2.1 or less.
[0124] When the thermal recording medium of the above embodiment is subjected to a light resistance test using the method and conditions described in the examples, the Δb value of the non-printed area before and after the test is, for example, 1.0 or less, preferably 0.9 or less, more preferably 0.8 or less, and even more preferably 0.7 or less.
[0125] [Method of manufacturing the thermal recording medium] The method for producing the thermal recording medium of the present invention is not particularly limited. For example, the components to be contained in each layer are dispersed in a solvent such as water to prepare a coating liquid for each layer by a known or conventional method, and the coating liquid is then applied and dried by a known or conventional method to produce the thermal recording medium.
[0126] The coating liquid may be prepared by dispersing all of the components in the same solvent in advance. Alternatively, the color former and the developer, which react with each other, may be prepared as separate dispersions and then mixed to prepare the coating liquid. In this case, the other components may be added to either the dispersion containing the color former or the dispersion containing the developer, or to both. The method for preparing the coating liquid is not particularly limited, and examples of the method include ultrasonic treatment, or a crushing treatment using a ball mill, a bead mill, a sand mill, a high-pressure homogenizer, etc.
[0127] The method for applying the coating liquid is not particularly limited, and examples thereof include air knife coating, barber blade coating, pure blade coating, rod blade coating, short dwell coating, curtain coating, die coating, and gravure coating.
[0128] In this embodiment, the layers may be simultaneously coated in multiple layers by, for example, a curtain coater, or may be formed individually and sequentially. Also, some layers may be simultaneously coated and some layers may be formed individually and sequentially. EXAMPLES
[0129] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to these examples, and is limited only by the claims.
[0130] A thermosensitive recording medium having an undercoat layer, a thermosensitive recording layer, an intermediate layer, and a topcoat layer laminated in this order on a substrate was prepared by the following steps, and was used for evaluation in the tests described below. (Examples 1 to 12, Comparative Examples 1 and 2) (Preparation of thermal recording medium) <Undercoat layer> The coating liquid for the undercoat layer was prepared by mixing and stirring 70 parts by mass of hollow particles (product name "Ropeake HP-1055", solid content concentration 26.5 mass%, hollow ratio 55 volume%, manufactured by Rohm and Haas Japan Co., Ltd.) as a filler, 10 parts by mass of modified styrene butadiene latex (solid content concentration 49 mass%) as a binder, and 20 parts by mass of water. The coating liquid was then applied to the substrate with a basis weight of 70 g / m 2 This was applied onto high-quality paper (thickness: 80 μm) and dried to give a coating weight of 3.0 g / m 2 A 5 μm-thick undercoat layer was formed.
[0131] <Thermal recording layer> A coating solution for the thermal recording layer having the composition shown in Table 1 was prepared, coated on the above undercoat layer, and dried to give a coating weight of 4.0 g / m 2 A thermosensitive recording layer having a thickness of 3.5 μm was formed. In Table 1, the numerical values of each compounded material indicate the mass ratio when dry.
[0132] As blending materials, 3-dibutylamino-6-methyl-7-anilinofluoran with a particle size of 0.6 to 0.7 μm was used as the dye, 4-hydroxy-4'-allyloxydiphenylsulfone (trade name "BPS-MAE", manufactured by Nicca Chemical Co., Ltd.) was used as the color developer 1, and urea urethane compound (trade name "UU", manufactured by Chemipro Chemical Co., Ltd.) was used as the color developer 2. Furthermore, 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane (trade name "DH43", manufactured by ADEKA Corporation) was used as the storage improver 1.
[0133] Pigment 1 was calcium carbonate (dispersed in a 5% aqueous solution of sodium hexametaphosphate to give a dispersion with a solids concentration of 30%), pigment 2 was a silica pigment (trade name "Mizukasil P-527", average particle size 0.2-2.0 μm, manufactured by Mizusawa Kogyo Co., Ltd.), and pigment 3 was hollow particles (trade name "Ropeake HP-1055", solids concentration 26.5 mass%, hollow ratio 55 volume%, manufactured by Rohm and Haas Japan Co., Ltd.). In addition, a zinc stearate emulsion was used as the lubricant, and a styrene-acrylic copolymer emulsion was used as the binder.
[0134] <Middle Class> An acrylic emulsion (solid content concentration 30% by mass) was applied as a resin onto the above-mentioned thermal recording layer and dried to give a coating weight of 1.6 g / m 2 Thus, an intermediate layer having a thickness of 1.5 μm was formed.
[0135] <Topcoat layer> A coating liquid for forming a topcoat layer was prepared containing 41.5 mass % of an acrylic emulsion (solid content concentration 30 mass %) as a binder, as the solid content in the topcoat layer, 5 mass % of zirconium carbonate as a crosslinking agent, 13.5 mass % of polyethylene wax (average particle size: 1.3 μm, softening point: 110° C.) as a lubricant, 40 mass % of polymethyl methacrylate (PMMA) as a filler, and water. The coating liquid for forming the topcoat layer thus prepared was applied onto the intermediate layer and dried to obtain a coating amount of 1.0 g / m2 when dried. 2A top coat layer having a thickness of 0.9 μm was formed. The numerical values of each compounding material (excluding water) indicate the mass ratio when dry.
[0136] By the above-mentioned method, the thermosensitive recording media of Examples 1 to 12 and Comparative Examples 1 and 2 were prepared.
[0137] [Table 1]
[0138] (Water resistance rating) In the water resistance evaluation, the optical density (OD value of the printed part / OD value of the non-printed part) was measured before and after the water resistance test for each thermal recording medium in each Example and Comparative Example. The procedure for evaluating water resistance is explained below. Note that the above optical density includes the meaning of color development density. The same applies to the optical density in the water resistance test, plasticizer resistance test, moist heat resistance test, light resistance test, and dynamic sensitivity test.
[0139] The prepared thermal recording medium was printed using a thermal paper printing test device (manufactured by Okura Engineering Co., Ltd., product name: Pulse Simulator TH-M2 / PP) under conditions of a printing speed of 50 mm / sec, an applied voltage of 17.0 V, a head resistance of 870 Ω, a pulse width of 0.488 to 1.394 ms, and a printing energy of 0.40 mJ / dot.
[0140] <Water resistance test> A sample of the printed thermosensitive recording medium was immersed in water at 23° C. for 24 hours, and then the sample was taken out and dried.
[0141] For samples of thermal recording media before the water resistance test (before immersion) and after the water resistance test (after immersion), the optical density (OD value of printed area / OD value of non-printed area) of the printed and non-printed areas was measured using a spectrophotometer (product name: eXact, manufactured by Videojet X-Rite Inc.).
[0142] The results of the measurements before and after the water resistance test are shown in Table 2. Here, if the change in the optical density (OD value) of the printed part before and after the water resistance test is small, that is, if the optical density (OD value) value after the water resistance test is the same as before the water resistance test (if the light reflectance is kept low), it indicates that the printed part of the thermal recording medium maintains its color density (black coloring). On the other hand, if the change before and after the water resistance test is large, that is, if the optical density (OD value) value after the water resistance test is smaller than before the test (if the light reflectance increases), it indicates that the printed part of the thermal recording medium has a decreased color density. In other words, the test result indicates the degree of decrease in the color density of the printed part when the thermal recording medium is immersed in water. For this reason, the water resistance evaluation of the printed part can be confirmed by the fact that the printed part (colored part) does not disappear when immersed in water. Specifically, the closer the optical density (OD value) of the printed portion after the water resistance test is to the value before the water resistance test, the more water resistance the printed portion of the thermosensitive recording medium has.
[0143] In addition, in the measurement results in Table 2, if the change in the optical density (OD value) of the non-printed part before and after the water resistance test is small, that is, if the optical density (OD value) of the non-printed part before and after the water resistance test is both small (if the light reflectance is maintained at a high level), it indicates that the non-printed part of the thermal recording medium has not discolored (the white color of the background is maintained). On the other hand, if the change before and after the water resistance test is large, that is, if the optical density (OD value) value after the water resistance test is larger than before the test (if the light reflectance has decreased), it indicates that the non-printed part of the thermal recording medium has discolored. In other words, the test result also indicates the degree of discoloration of the non-printed part when the thermal recording medium is immersed in water. Therefore, the water resistance evaluation of the non-printed part can be confirmed by the fact that the non-printed part does not discolor when immersed in water. Specifically, the closer the optical density (OD value) value of the non-printed part after the water resistance test is to the value before the water resistance test, the more excellent the water resistance of the non-printed part of the thermal recording medium.
[0144] In Table 2, the optical density (OD value) of the printed and non-printed areas is shown separated by " / ". The same applies to the plasticizer resistance test and moist heat resistance test below.
[0145] (Plasticizer resistance evaluation) In the evaluation of plasticizer resistance, the optical density (OD value of the printed part / OD value of the non-printed part) was measured before and after the plasticizer resistance test for each thermosensitive recording medium in each Example and Comparative Example. The procedure for evaluating plasticizer resistance is described below.
[0146] Printing was carried out on the prepared thermosensitive recording medium under the same conditions as those for the water resistance evaluation described above.
[0147] <Plasticizer resistance test> The printed sample of the thermal recording medium was attached to a vinyl chloride wrap, and then another vinyl chloride wrap was placed on top of it. 2 After applying a load of 150 kgf / cm2 and leaving it at 40°C for 15 hours, the sample was taken out.
[0148] For samples of thermal recording media before and after the plasticizer resistance test, the optical density (OD value of printed area / OD value of non-printed area) of the printed and non-printed areas was measured using a spectrophotometer (product name: eXact, manufactured by Videojet X-Rite Inc.).
[0149] The measurement results from the above test are shown in Table 2. The measurement results in Table 2 were judged in the same manner as in the water resistance test. That is, for the printed part, the closer the optical density (OD value) value of the printed part after the plasticizer resistance test is to the value before the plasticizer resistance test, the more excellent the plasticizer resistance of the printed part of the thermal recording medium.
[0150] Furthermore, with regard to the non-printed areas, the closer the optical density (OD value) of the non-printed areas after the plasticizer resistance test is to the value before the plasticizer resistance test, the better the plasticizer resistance of the non-printed areas of the thermal recording material.
[0151] (Heat and humidity resistance evaluation) In the evaluation of the moist heat resistance, the optical density (OD value of the printed part / OD value of the non-printed part) was measured before and after the moist heat resistance test for each thermal recording medium in each Example and Comparative Example. The procedure for evaluating the moist heat resistance will be described below.
[0152] Printing was carried out on the prepared thermosensitive recording medium under the same conditions as those for the water resistance evaluation described above.
[0153] <Moisture and heat resistance test> The printed thermosensitive recording medium samples were left to stand for 24 hours under conditions of 40° C. and 100% RH, or 50° C. and 100% RH.
[0154] The optical density (OD value of printed area / OD value of non-printed area) of the thermal recording medium samples before and after the moist heat resistance test was measured using a spectrophotometer (product name: eXact, manufactured by Videojet X-Rite Inc.).
[0155] The measurement results from the above test are shown in Table 2. The measurement results in Table 2 were judged in the same manner as the water resistance test. That is, for the printed part, the closer the optical density (OD value) value after the moist heat resistance test is to the value before the moist heat resistance test, the more excellent the moist heat resistance of the printed part of the thermal recording medium.
[0156] In addition, for non-printed areas, the closer the optical density (OD value) of the non-printed areas after the moist heat resistance test is to the value before the moist heat resistance test, the better the moist heat resistance of the non-printed areas of the thermal recording medium.
[0157] (Lightfastness evaluation) In the light fastness evaluation, the color tone (b value) of the non-printed portion was measured before and after the light fastness test for each thermosensitive recording medium in each Example and Comparative Example. The procedure for the light fastness evaluation will be described below.
[0158] <Light resistance test> Using an illuminometer, the distance from the fluorescent lamp was confirmed to be 5000 Lux, and the prepared thermal recording medium was placed at that position and left for 100 hours.
[0159] The color tone (b value) of the non-printed areas of the thermal recording medium samples before and after the light fastness test was measured using a color difference meter (product name: SpectroEye, manufactured by Videojet X-Rite Inc.).
[0160] The measurement results from the above test are shown in Table 2. In the measurement results in Table 2, the b value, which is an index of the color tone of the non-printed parts, is an index showing the change from blue to yellow, and the larger the positive b value, the more yellowish it becomes (the degree of yellowing is strong), and the larger the negative b value, the more blueish it becomes. Based on this index, the Δb value was calculated as an index of lightfastness using the following formula (1). Δb value = (b value after test) - (b value before test) (1)
[0161] That is, when the change (Δb value) in the color tone (b value) of the non-printed part before and after the lightfastness test is small, it indicates that the non-printed part of the thermal recording medium is less likely to yellow (the white color of the background is maintained). On the other hand, when the change (Δb value) before and after the lightfastness test is large, it indicates that the non-printed part of the thermal recording medium is more likely to yellow. In other words, the Δb value represents the degree of yellowing of the non-printed part when the thermal recording medium is exposed to light. Therefore, the lightfastness evaluation of the non-printed part can be confirmed by checking whether the non-printed part does not yellow in the above test. Specifically, the closer the Δb value is to 0, the better the lightfastness of the non-printed part of the thermal recording medium.
[0162] It is also possible to qualitatively evaluate the color tone of the non-printed parts of the thermosensitive recording medium by the magnitude of the b-value itself, rather than the rate of change in the b-value. In other words, the closer the b-value of the non-printed parts of the thermosensitive recording medium is to 0, the less yellow the non-printed parts of the thermosensitive recording medium are (the closer it is to white).
[0163] [Table 2]
[0164] The following can be confirmed from Table 2.
[0165] As for water resistance, as shown in Examples 1 to 7, as the blending ratio of the storage stability improver 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane increases, the OD value after the water resistance test increases, and it is understood that the water resistance of the printed part is improved. In addition, there is no particular tendency for the non-printed part after the water resistance test, and it is understood that no discoloration occurs in either the Examples or the Comparative Examples.
[0166] Regarding plasticizer resistance, it can be seen that both the printed areas of the Examples and Comparative Examples maintained a high optical density (OD value) after the plasticizer resistance test, and no discoloration occurred in the non-printed areas after the plasticizer resistance test.
[0167] As for the moisture and heat resistance, as shown in Examples 1 to 7, as the blending ratio of the storage stability improver 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane increases, the OD value after the moisture and heat resistance test increases, and it is understood that the water resistance of the printed part is improved. In addition, there is no particular tendency for the non-printed part after the moisture and heat resistance test, and it is understood that no discoloration occurs in either the Examples or the Comparative Examples.
[0168] As described above, it is seen that all of the Examples and Comparative Examples show excellent color development. In addition, although there are differences in the degree, it is seen that the print storage stability is excellent because the water resistance, plasticizer resistance, and moist heat resistance are excellent. Regarding the above water resistance evaluation and plasticizer resistance evaluation, if the optical density (OD value) of the printed part after the test is 1.20 or more and the optical density (OD value) of the non-printed part is 0.05 or less, it can be evaluated as having sufficiently excellent water resistance and plasticizer resistance. Regarding the above moist heat resistance evaluation, if the optical density (OD value) of the printed part after the test is 1.00 or more and the optical density (OD value) of the non-printed part is 0.05 or less, it can be evaluated as having sufficiently excellent moist heat resistance.
[0169] With regard to lightfastness, as in Examples 1 to 7, as the blending ratio of 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane, which is a storage stability improver, increases, the Δb value decreases, and it is understood that the lightfastness of the non-printed parts improves. On the other hand, in Comparative Example 1, which does not contain a storage stability improver, the Δb value is larger than in each Example, and it is understood that the non-printed parts have yellowed. Also, it is understood that Comparative Example 2, which contains a urea urethane compound, which is a color developer, has the most severe yellowing in Table 2. In other words, it is understood that the urea urethane compound is effective in improving print storage stability, but the lightfastness in this embodiment is inferior to the case where no compound is used.
[0170] Furthermore, a comparison of the Δb values of Example 1 and Comparative Example 1 and the b value before the test shows that by incorporating just 1% of 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane, a storage stability improver, the yellowing of the non-printed areas after the lightfastness test and the yellow tinge before the lightfastness test can be effectively suppressed.
[0171] As described above, it can be seen that all of the examples show excellent lightfastness and suppress the yellowing of the non-printed parts. Regarding the above lightfastness test, if the Δb value of the non-printed parts before and after the test is 0.80 or less, it can be evaluated as having sufficiently excellent lightfastness. Also, if the b value of the non-printed parts before the test is 1.50 or less, it can be evaluated as having very little yellowing of the non-printed parts.
[0172] (Dynamic sensitivity evaluation) In the dynamic sensitivity test, printing was performed with different printing energies on each thermosensitive recording medium in each Example and Comparative Example, and the optical density (OD value of the printed portion) at each printing energy was measured. From the measurement results, the dynamic sensitivity of each thermosensitive recording medium in each Example and Comparative Example was evaluated. The procedure of the dynamic sensitivity test is described below.
[0173] <Dynamic Sensitivity Test> The prepared thermal recording medium was printed using a thermal paper printing test device (manufactured by Okura Engineering, product name: Pulse Simulator TH-M2 / PP) at a printing speed of 50 mm / sec, an applied voltage of 17.0 V, a head resistance of 870 Ω, a pulse width of 0.488 to 1.394 ms, and printing energies of 0.20 mJ / dot and 0.24 mJ / dot. The optical density (OD value) under these printing energy conditions was measured using a spectrophotometer (manufactured by X-rite, product name: eXact).
[0174] The measurement results of each optical density (OD value) in the dynamic sensitivity test are shown in Table 3. In the measurement results in Table 3, the higher the optical density (OD value) value, the clearer the color development, and the lower the value, the more insufficient the color development. In other words, when the optical density (OD value) value is high despite the low printing energy, it indicates high dynamic sensitivity and excellent thermal response. On the other hand, when the optical density (OD value) value is small despite the high printing energy, it indicates low dynamic sensitivity and poor thermal response. In addition, since a higher dynamic sensitivity means that clearer printing can be achieved even with a lower printing energy, a thermosensitive recording medium with a higher dynamic sensitivity can be evaluated as having excellent color development.
[0175] [Table 3]
[0176] The following can be confirmed from Table 3.
[0177] Comparing Example 6, in which calcium carbonate was used as a pigment, with Examples 8 to 12, in which calcium carbonate was replaced with silica pigment and / or hollow particles, it can be seen that the cases in which silica pigment and / or hollow particles were used showed higher dynamic sensitivity and tended to have superior thermal responsiveness.
[0178] In addition, the dynamic sensitivity also changes depending on the ratio of silica pigment to hollow particles, and it is found that extremely excellent dynamic sensitivity is exhibited in particular when the mass ratio of silica pigment to hollow particles is 50:50, i.e., in the case of Example 10, where the mass ratio of silica pigment is 50 mass% when the sum of silica pigment and hollow particles is 100 mass%.
[0179] As mentioned above, all the examples show excellent dynamic sensitivity, but it can be seen that extremely excellent dynamic sensitivity can be achieved by blending silica pigment and hollow particles in a specific ratio. Regarding the above test, if the optical density (OD value) of the printed area when printed at 0.24 mJ / dot is 1.30 or more, it can be evaluated as having sufficiently excellent dynamic sensitivity.
[0180] In summary, the configuration of the present invention and its variations are described below. [Appendix 1] A thermal recording medium in which a thermal recording layer is laminated on a substrate, The thermal recording layer contains a color developer and a storage stability improving agent, The color developer contains a diphenyl sulfone compound represented by the following formula (1): [ka] (In formula (1), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 R each independently represents a hydrogen atom or a substituent. 9 represents a hydrogen atom, an alkyl group, or an alkenyl group. The storage stability improver contains a compound having three or more phenolic hydroxyl groups in the molecule, A thermosensitive recording medium, in which the mass ratio of the diphenyl sulfone compound represented by the following formula (1) to the developer in the thermosensitive recording layer (mass of the diphenyl sulfone compound represented by the following formula (1) in the thermosensitive recording layer / mass of the developer in the thermosensitive recording layer) is greater than 50 mass%. [Appendix 2] The thermosensitive recording material according to claim 1, wherein the thermosensitive recording layer contains an inorganic pigment and an organic pigment. [Appendix 3] The thermal recording material according to claim 2, wherein the inorganic pigment comprises a silica pigment, and the organic pigment comprises hollow particles. [Appendix 4] The thermosensitive recording material according to claim 3, wherein the mass ratio of the silica pigment to the hollow particles in the thermosensitive recording layer (solid mass of the silica pigment in the thermosensitive recording layer / solid mass of the hollow particles in the thermosensitive recording layer) is 10:90 to 90:10. [Appendix 5] The thermosensitive recording medium according to any one of claims 1 to 4, wherein the developer is 4-hydroxy-4'-allyloxydiphenylsulfone. [Appendix 6] The thermosensitive recording medium according to any one of claims 1 to 5, comprising a compound represented by the following formula (2) as the storage stability improving agent: [ka] (In formula (2), R 13 R represents an alkyl group having 4 or less carbon atoms. 14 represents an alkyl group having 4 or less carbon atoms or a cyclohexyl group. 13 , R 14 may be the same or different.) [Appendix 7] The thermosensitive recording medium according to any one of claims 1 to 6, comprising 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane as the storage stability improving agent. [Appendix 8] The thermosensitive recording medium according to any one of claims 1 to 7, further comprising an intermediate layer and a topcoat layer, in that order, on the side of the thermosensitive recording layer opposite the substrate. [Appendix 9] The thermosensitive recording material according to claim 8, wherein the top coat layer contains a lubricant, and the lubricant contains polyethylene wax and / or paraffin wax. [Industrial Applicability]
[0181] The thermal recording medium of the present invention has excellent light resistance, water resistance, and moist heat resistance, and therefore can be suitably used even in harsh environments, such as outdoors exposed to light and rain, or stored for long periods at high temperatures and high humidity. [Explanation of symbols]
[0182] 1 Thermal recording medium 2 Base material 3. Thermal recording layer 4. Middle Tier 5 Topcoat layer 6 Undercoat layer
Claims
1. A thermal recording medium in which a thermal recording layer is laminated on a substrate, The thermal recording layer contains a color developer and a storage stability improving agent, The color developer contains a diphenyl sulfone compound represented by the following formula (1): 【Chemistry 1】 (In formula (1), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 R each independently represents a hydrogen atom or a substituent. 9 represents a hydrogen atom, an alkyl group, or an alkenyl group. The storage stability improver contains a compound having three or more phenolic hydroxyl groups in the molecule, A thermosensitive recording medium, in which the mass ratio of the diphenyl sulfone compound represented by the following formula (1) to the color developer in the thermosensitive recording layer (mass of the diphenyl sulfone compound represented by the following formula (1) in the thermosensitive recording layer / mass of the color developer in the thermosensitive recording layer) is greater than 50 mass%.
2. 2. The heat-sensitive recording medium according to claim 1, wherein the heat-sensitive recording layer contains an inorganic pigment and an organic pigment.
3. 3. The heat-sensitive recording material according to claim 2, wherein the inorganic pigment comprises a silica pigment, and the organic pigment comprises hollow particles.
4. 4. The thermosensitive recording medium according to claim 3, wherein a mass ratio of the silica pigment to the hollow particles in the thermosensitive recording layer (solid content mass of the silica pigment in the thermosensitive recording layer / solid content mass of the hollow particles in the thermosensitive recording layer) is 10:90 to 90:
10.
5. 5. The thermosensitive recording medium according to claim 1, wherein the developer is 4-hydroxy-4'-allyloxydiphenylsulfone.
6. 5. The thermosensitive recording medium according to claim 1, further comprising a compound represented by the following formula (2) as the storage stability improving agent: 【Chemistry 2】 (In formula (2), R 13 represents an alkyl group having 4 or less carbon atoms, R 14 Each of R represents an alkyl group having 4 or less carbon atoms or a cyclohexyl group. 13 , R 14 may be the same or different.)
7. 5. The thermosensitive recording medium according to claim 1, further comprising 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane as the storage stability improving agent.
8. The thermosensitive recording medium according to claim 1 , further comprising an intermediate layer and a topcoat layer in this order on the side of the thermosensitive recording layer opposite to the substrate.
9. 9. The thermal recording material according to claim 8, wherein the top coat layer contains a lubricant, and the lubricant contains polyethylene wax and / or paraffin wax.
Citation Information
Patent Citations
Heat-sensitive recording material
JP1999157220A
Two-color thermosensitive recording medium and manufacture thereof
JP2001018531A
Thermosensitive recording body
JP2007125744A
Heat-sensitive recording material
JP2010094986A
Material and paper of thermal recording
JP2013237234A