Solder alloy, solder ball, solder preform, solder joint, and circuit

The optimized solder alloy composition with controlled Ag, Cu, Ni, and Ge content addresses void formation and oxidation issues, enhancing bonding reliability and impact resistance in BGA packages by maintaining regular bump shapes and fine intermetallic compounds.

JP2024159118AActive Publication Date: 2024-11-08SENJU METAL IND CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023074902
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

Existing solder alloys used in BGA packages suffer from void formation, shear strength deterioration, and oxidation during multiple reflow solderings, leading to poor bonding and increased failure modes, with irregularly shaped solder bumps causing bonding defects and short circuits in highly integrated electronic components.

Method used

A solder alloy composition with specific ranges of Ag (0.10-3.00%), Cu (0.80-6.00%), Ni (0.08-0.60%), Ge (0.0010-0.0150%), and the balance Sn, optimized to enhance wettability, shear strength, and drop impact resistance, while suppressing intermetallic compound growth and maintaining appropriate bump shape.

Benefits of technology

The optimized solder alloy composition ensures excellent wettability, shear strength, and drop impact resistance, with fine intermetallic compounds and regular bump shapes, reducing failure modes and bonding defects in electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159118000001_ABST
    Figure 2024159118000001_ABST
Patent Text Reader

Abstract

To provide a solder alloy which has excellent wettability and shear strength and a proper fracture mode, and in which growth of intermetallic compounds of a joint interface is suppressed even after multiple times of reflowing and which has excellent drop impact resistance, and further, which has a proper bump shape, and to provide a solder ball, a solder preform, a solder joint, and a circuit.SOLUTION: A solder alloy has an alloy composition comprising, in mass%, 0.10-3.00% Ag, 0.80-6.00% Cu, 0.08-0.60% Ni, 0.0010-0.0150% Ge, and the balance consisting of Sn. Preferably, the alloy composition also contains at least one kind out of Bi, Sb, In, Zn, Ga, Mn, Cr, Co, Si, Ti, and rare earth by 0.1% or less in total.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to solder alloys, solder balls, solder preforms, solder joints, and circuits. [Background technology]

[0002] In recent years, there has been a demand for electronic devices to be highly integrated and to be lighter, thinner, and smaller. The electronic components installed in electronic devices are also required to be smaller and thinner. The mainstream semiconductor package that meets these demands is the area array type surface mount package, the Ball Grid Array (BGA). BGA has external electrode terminals in which solder balls are arranged in a grid pattern at equal intervals on the mounting board of the package. After being placed on the electrodes, the solder balls are heated together with the mounting board in a reflow furnace, where they melt and form solder bumps.

[0003] To meet the ever-increasing demand for higher integration and lighter, thinner, shorter, and smaller electronic devices, electronic components are sometimes connected to both sides of a board. To connect electronic components to both sides of a board, a first reflow soldering is performed on one side, and then a second reflow soldering is performed on the other side. For power semiconductor boards, a third reflow soldering is performed to connect a heat sink. When multiple reflow soldering processes are performed in this way, the solder alloy used in the first or second soldering is repeatedly melted and solidified.

[0004] Conventional BGAs use Sn-Ag-Cu solder alloys, such as Sn-3.0Ag-0.5Cu. However, when multiple reflow soldering processes are performed, voids occur at the interface between the solder alloy and the electrodes that make up the solder joint. As the voids grow, the shear strength and drop impact resistance deteriorate. In addition, repeated melting and solidification of the solder alloy can cause oxidation of the solder alloy, deteriorating its wettability.

[0005] Therefore, in order to suppress the deterioration of the reliability of the solder joint due to multiple reflow soldering, Patent Document 1 discloses a Sn alloy containing 1 to 9% Cu and various optional elements. Specifically, a Sn-Cu-Ni solder alloy and a Sn-Cu-Ni-Ge solder alloy are disclosed. These solder alloys further contain P and the like. It is also disclosed that Ag may be contained as an optional element. In the same document, the tilt of the die, the growth of voids, and the shear strength after multiple reflow soldering are evaluated.

[0006] Patent Document 2 discloses a Sn-Ag-Cu-Ni solder alloy to improve drop impact resistance by reducing the hardness of the solder alloy. The invention described in the same document also describes the inclusion of P and Ge as elements that suppress discoloration of the solder alloy.

[0007] Patent Document 3 discloses a Sn-Ag-Cu-Ni-Ge solder alloy as an inexpensive 5-element solder alloy with good bonding properties. The invention described in the document is evaluated for the void generation rate and breaking elongation. The document also describes that the breaking elongation is improved by reducing the generation of voids and thinning the film thickness of Cu3Sn. The document also discloses that the reason for adding Ge is to suppress oxidation.

[0008] Patent Document 4 discloses a solder alloy containing at least one of La, Ce, Pr, Nd, Sm, and Yb, or Y, Gd, and Dy in a predetermined amount in an Sn-Ag-Cu solder alloy in order to improve the joint strength while reducing the Ag content. The same document discloses that the solder alloy may further contain Ni and Fe in order to refine the crystals of the solidification structure of the solder alloy and improve the mechanical strength. The same document also discloses that the solder alloy may contain P, Ga, and Ge as elements that are highly easily oxidized in order to suppress the generation of dross due to the oxidation of La, Ce, Pr, Nd, Sm, and Yb, or Y, Gd, and Dy, and Ni, and Fe. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2020 / 135932 [Patent Document 2] International Publication No. 2007 / 102588 [Patent Document 3] JP 2008-93701 A [Patent Document 4] JP 2013-049073 A Summary of the Invention [Problem to be solved by the invention]

[0010] In Patent Document 1, various evaluations are performed on alloy compositions containing Sn and Cu. However, the evaluations are performed using alloy compositions with different constituent elements depending on the evaluation items. For example, in the evaluation of die tilt, a solder alloy is used that has constituent elements that do not melt in the second reflow or that have a melting point that maintains a high viscosity even if melted. Similarly, the growth of voids and the shear strength after multiple reflow soldering are evaluated using solder alloys with different constituent elements.

[0011] Thus, in the invention described in Patent Document 1, although various evaluations are performed, the constituent elements other than Sn and Cu differ according to each evaluation item. Therefore, an alloy composition that satisfies all of the evaluation items disclosed in Patent Document 1 is not disclosed. Also, as mentioned above, the same document discloses that Ag may be contained. However, not a single alloy composition containing Ag has been evaluated. Therefore, the effect of adding Ag has not been proven in the invention described in Patent Document 1.

[0012] In the inventions described in Patent Documents 2 and 3, the Ni content is reduced and the properties of the bonding interface are improved to improve drop impact resistance, etc. In the invention described in Patent Document 4, the bonding interface is refined by using expensive rare metals.

[0013] Thus, in Patent Documents 1 to 4, the joint interface of the solder joint is examined. Naturally, improving the properties of the joint interface of the solder joint is an important objective in the solder alloy. However, even if the load of the solder joint increases, the fracture mode should not be such that the fracture occurs at the joint interface. In the solder joint, the physical and electrical loads are mainly applied to the joint interface, so it is desired that the joint interface is firmly joined.

[0014] Thus, evaluation of solder joints under extreme conditions is an important indicator for confirming that good solder joints have been formed. However, because Patent Documents 1 to 4 do not consider the fracture mode, it is unclear whether solder joints with good bonding interfaces have been formed.

[0015] In addition, the evaluation items discussed in Patent Documents 1 to 4 are all for the case after the solder joint is formed. As a property of the solder alloy before the solder joint is formed, excellent wettability of the molten solder is also important. Although Patent Documents 1 to 4 refer to wettability, they do not evaluate specific alloy compositions.

[0016] Furthermore, when bonding to a substrate such as a BGA, the solder bumps must have an appropriate shape before the solder joints are formed. If the solder bumps have an irregular shape, there is a high possibility that some problem will occur during soldering. However, Patent Documents 1 to 4 do not consider the shape of the solder bumps for forming the solder joints at all.

[0017] Solder bumps are formed by melting a solder ball on an electrode, solidifying it, and bonding it to the electrode. For this reason, it is considered preferable for the surface to have a roughly elliptical shape. On the other hand, there are cases where holes are formed in the solder bump, causing the surface to become uneven, needle-like intermetallic compounds protrude from the surface of the solder bump, or the solder bump has an irregular shape that is significantly different from a roughly elliptical shape. Such solder bumps are prone to poor bonding and short circuits between electronic components and substrates. In recent years, as electronic components have become smaller and thinner, bonding defects caused by irregularly shaped bumps have been increasing year by year, and therefore immediate improvement is desired.

[0018] Therefore, an object of the present invention is to provide a solder alloy, a solder ball, a solder preform, a solder joint, and a circuit that have excellent wettability and shear strength, an appropriate fracture mode, suppression of the growth of intermetallic compounds at the bonding interface even after multiple reflows, excellent drop impact resistance, and an appropriate bump shape. [Means for solving the problem]

[0019] The present inventors have investigated various alloy compositions of the solder alloys disclosed in Patent Documents 2 to 4 in order to solve the problems of the present invention. Specifically, evaluation was performed on a Ge-free Sn-1.0Ag-1.0Cu-0.1Ni solder alloy, which is the alloy composition of Example 10 in Patent Document 2. As a result, it was discovered that an abnormality occurs in the solder bump.

[0020] Therefore, the present inventors evaluated a Sn-1.0Ag-1.0Cu-0.1Ni-0.02Ge solder alloy, which is a Sn-1.0Ag-1.0Cu-0.1Ni solder alloy with Ge added, and found that the solder bump had abnormalities and poor wettability.

[0021] Next, the study was carried out with a focus on the Ni content. In paragraphs 0072 and 0139 of Patent Document 2, it is explained that when the Ni content exceeds 0.07%, the solder alloy before reflow is hardened to a degree that does not cause practical problems, resulting in poor drop impact resistance. On the other hand, in paragraph 0063 of the same document, it is described that Ni relaxes the distortion between the (Cu,Ni)6Sn5 intermetallic compound in which part of Cu is replaced by Ni and the adjacent Cu3Sn intermetallic compound. In view of these, it is presumed that the Sn-Ag-Cu-Ni-Ge solder alloy disclosed in the same document only has an alloy composition with a Ni content of 0.05%, which is close to 0.07%.

[0022] Patent Document 3 also discloses in Figures 3 and 4 that if the Ni content exceeds 0.05%, it is not possible to suppress the generation of voids. And, Patent Document 3 also discloses in Figure 5 that an alloy composition containing 0.03% Ni has a similar fracture elongation to an alloy composition containing 0.07% Ni, and therefore it is not necessary to contain Ni in an amount exceeding 0.05%.

[0023] In view of these findings, the present inventors evaluated an alloy composition in which the Ni content was reduced to 0.05% in a Sn-Ag-Cu-Ni-Ge solder alloy, and found that the shear strength was inferior and abnormalities occurred in the solder bumps, similar to an alloy composition with a Ni content of 0.07%.

[0024] In addition, since Patent Document 4 describes reducing the Ag content, an Sn-Ag-Cu-Ni-Ge solder alloy with an Ag content reduced to 0.05% was evaluated. As a result, it was found that although the abnormalities of the solder bumps were reduced, the wettability and shear strength were inferior.

[0025] In view of these findings, it is considered difficult to solve the problem of the present invention with a Sn-Ag-Cu-Ni-Ge solder alloy, even if the conventional alloy composition and effect trends are taken into consideration. Therefore, in order to obtain a Sn-Ag-Cu-Ni-Ge solder alloy that simultaneously satisfies all the effects listed in the problem of the present invention, the inventors decided to study an alloy composition in which the Ni content is increased to 0.08% or more, which is a different direction from the conventional one. In addition, the contents of Ag, Cu, and Ge were also examined in detail at the same time.

[0026] In addition, as described in paragraphs 0072 and 0139 of Patent Document 2, even if the characteristics are somewhat deteriorated, the characteristics are not problematic in practical use. Therefore, it is not necessary to achieve all of the problems set forth in the subject of the present invention at a higher level than necessary. For this reason, the above study was carried out so that the effect is not problematic in practical use.

[0027] As a result, it was discovered that when the Ni content is increased and each constituent element is within a specified range, the wettability and shear strength are excellent, the fracture mode is appropriate, the growth of intermetallic compounds at the bonding interface is suppressed even after multiple reflows, and the material has excellent drop impact resistance, and further, no abnormalities are observed in the shape of the bump, leading to the completion of the present invention. The present invention, which has been made based on these findings, is as follows.

[0028] (0) A solder alloy comprising, by mass%, 0.10-3.00% Ag, 0.80-6.00% Cu, 0.08-0.60% Ni, 0.0010-0.0150% Ge, and the remainder being Sn and unavoidable impurities. (1) A solder alloy having an alloy composition, in mass%, of 0.10-3.00% Ag, 0.80-6.00% Cu, 0.08-0.60% Ni, 0.0010-0.0150% Ge, and the balance being Sn.

[0029] (2) The solder alloy according to (0) or (1) above, further comprising at least one of Bi, Sb, In, Zn, Ga, Mn, Cr, Co, Si, Ti, and rare earth elements in a total amount of 0.1% or less.

[0030] (3) The solder alloy according to any one of (0) to (2) above, wherein the alloy composition satisfies the following formulae (1) and (2): 0.00043≦Cu×Ni×Ge≦0.00149 (1) 0.09≦Ag×Cu×Ni≦0.11 (2) In formulas (1) and (2), Ag, Cu, Ni, and Ge represent the contents (mass %) of the alloy composition.

[0031] (4) A solder ball made of the solder alloy according to any one of (0) to (3) above.

[0032] (5) A solder preform made of the solder alloy according to any one of (0) to (3) above.

[0033] (6) A solder joint comprising the solder alloy according to any one of (0) to (3) above.

[0034] (7) A circuit having the solder joint described in (6) above. [Brief description of the drawings]

[0035] [Figure 1] FIG. 1 is a SEM photograph of the surface of an intermetallic compound formed at a joint interface in a solder joint produced using the solder alloy of Example 3. [Diagram 2] FIG. 2 is a SEM photograph of the surface of an intermetallic compound formed at the joint interface of a solder joint produced using the solder alloy of Comparative Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] The present invention will be described in more detail below. In this specification, "%" relating to the solder alloy composition is "mass %" unless otherwise specified.

[0037] 1. Solder Alloy (1) Ag: 0.10-3.00% Ag contributes to improving wettability. In addition, the shear strength can be improved by the precipitation of fine Ag3Sn. If the Ag content is less than 0.10%, the wettability decreases, and the shear strength decreases due to poor bonding between the solder alloy and the electrode. The lower limit of the Ag content is 0.10% or more, preferably 0.50% or more, and more preferably 0.90% or more.

[0038] On the other hand, if the Ag content exceeds 3.00%, the shear strength decreases due to the precipitation of coarse Ag3Sn, and the drop impact resistance decreases after multiple reflows. The upper limit of the Ag content is 3.00% or less, preferably 2.50% or less, more preferably 2.00% or less, even more preferably 1.50% or less, particularly preferably 1.10% or less, and most preferably 1.00% or less.

[0039] (2) Cu: 0.80-6.00% Cu contributes to improving the shear strength by controlling the growth of intermetallic compounds that precipitate at the joint interface. Although thin and brittle compounds are formed on the molten solder surface together with Ge, which will be described later, the compounds are easily destroyed by the convection of the molten solder, and the surface of the molten solder is cleaned, so that the deformation of the solder bump is suppressed by improving the surface tension of the molten solder. Furthermore, Cu improves drop impact resistance and wettability, and can optimize the destruction mode.

[0040] If the Cu content is less than 0.80%, the effect of suppressing the growth of intermetallic compounds at the bonding interface is not exhibited, and the shear strength is reduced. In addition, a thin compound of Ge and Cu is not formed on the surface of the molten solder, and the solder bump becomes irregular. The lower limit of the Cu content is 0.80% or more, and preferably 0.95% or more.

[0041] On the other hand, if the Cu content exceeds 6.00%, the liquidus temperature rises excessively, resulting in deterioration of wettability. In addition, coarse intermetallic compounds are precipitated at the bonding interface, resulting in poor drop impact resistance and shear strength, and inappropriate fracture mode. Furthermore, a large amount of thick compounds of Ge and Cu are precipitated on the molten solder surface, resulting in a decrease in the surface tension of the molten solder and an irregular solder bump. The upper limit of the Cu content is 6.00% or less, preferably 5.00% or less, more preferably 4.00% or less, even more preferably 3.00% or less, even more preferably 2.00% or less, particularly preferably 1.20% or less, most preferably 1.05% or less, and may be 1.00% or less.

[0042] (3) Ni: 0.08-0.60% Ni, like Cu, contributes to improving the shear strength and suppressing the deformation of the solder bump. Furthermore, Ni improves drop impact resistance and wettability, and can optimize the fracture mode. If the Ni content is less than 0.08%, the effect of suppressing the growth of intermetallic compounds at the bonding interface is not exerted, and the shear strength decreases. In addition, a thin compound of Ge and Ni is not formed on the surface of the molten solder, and the solder bump becomes deformed. The lower limit of the Ni content is 0.08% or more, and preferably 0.09% or more.

[0043] On the other hand, if the Ni content exceeds 0.60%, the wettability deteriorates as with Cu, and coarse intermetallic compounds precipitate at the bonding interface, resulting in poor drop impact resistance and shear strength, and an inappropriate fracture mode. Furthermore, a large amount of Ge and Ni compounds precipitates on the molten solder surface, causing the solder bump to become irregular. The upper limit of the Ni content is 0.60% or less, preferably 0.50% or less, more preferably 0.40% or less, even more preferably 0.30% or less, even more preferably 0.20% or less, particularly preferably 0.12% or less, most preferably 0.11% or less, and may be 0.10% or less.

[0044] (4) Ge: 0.0010~0.0150% Ge forms compounds with Cu and Ni, which move to the surface of the molten solder, but these compounds are destroyed by the convection of the molten solder, and the surface of the molten solder is cleaned, suppressing the deformation of the solder bump. If the Ge content is less than 0.0010%, the compounds with Cu and Ni are not sufficiently precipitated on the surface of the molten solder, and the solder bump becomes deformed. The lower limit of the Ge content is 0.0010% or more, preferably 0.00020% or more, more preferably 0.0050% or more, and even more preferably 0.0060% or more.

[0045] On the other hand, if the Ge content exceeds 0.0150%, the compounds with Cu and Ni become thick on the surface of the molten solder, and these compounds remain on the surface of the solder alloy during solidification, causing the solder bump to become irregular. As a result, the wettability is also reduced. The upper limit of the Ge content is 0.0150% or less, preferably 0.0120% or less, more preferably 0.0100% or less, and particularly preferably 0.0080% or less.

[0046] (5) At least one of Bi, Sb, In, Zn, Ga, Mn, Cr, Co, Si, Ti, and rare earth elements, total amount not exceeding 0.1% The solder alloy according to the present invention may contain at least one of Bi, Sb, In, Zn, Ga, Mn, Cr, Co, Si, Ti, and rare earth elements in a total amount of 0.1% or less as optional elements, within a range that does not affect the effects of the present invention. In the present invention, the rare earth elements refer to 17 elements including Sc and Y belonging to Group 3 in the periodic table and 15 elements of the lanthanum group corresponding to atomic numbers 57 to 71. The upper limit of the content of the optional elements is not particularly limited, but is preferably 0.1% or less, more preferably 0.01% or less. The lower limit is also not particularly limited, but is preferably 0.001% or more.

[0047] (6) Equations (1) and (2) 0.00043≦Cu×Ni×Ge≦0.00149 (1) 0.09≦Ag×Cu×Ni≦0.11 (2) In formulas (1) and (2), Ag, Cu, Ni, and Ge represent the contents (mass %) of the alloy composition.

[0048] The solder alloy according to the present invention preferably satisfies formulas (1) and (2). When these formulas are satisfied, the fracture mode is more optimized, the shear strength is further improved, the drop impact resistance is further improved even after multiple reflows, the intermetallic compounds precipitated at the bonding interface become fine, and the deformation of the solder bump is suppressed. Formula (1) is a formula composed of Cu, Ni, and Ge, which are elements that suppress the deformation of the solder bump. The content of Ge is less than the content of Cu and Ni, but Ge forms a compound with Cu and Ni and greatly affects the behavior of the alloy structure in the solidification process, so that a small amount of Ge contributes greatly to the properties of the solder alloy. Therefore, the content of each constituent element can be expressed as a formula without multiplying Ge by a coefficient.

[0049] Formula (2) is composed of Ag, Cu, and Ni, which contribute to improving wettability and shear strength. A solder joint must not break at the joint interface, but the strength of the solder alloy itself must not be too weak. In this regard, Ag is a precipitation-strengthening element, and by satisfying formula (2), the strength of the solder alloy itself can be improved to a certain extent without causing an inappropriate fracture mode. In addition, Cu and Ni contribute to the formation of fine intermetallic compounds at the joint interface and the liquidus temperature, and therefore, together with Ag, affect the overall characteristics of the solder joint.

[0050] These formulas are obtained by the mutual dependence of each constituent element. This is because the alloy is an integrated combination of all the constituent elements, and each constituent element affects each other. In this way, the solder alloy according to the present invention, which adjusts the content of each constituent element to the optimum content and further satisfies formulas (1) and (2), is set to a range that fully considers the mutual dependence of each constituent element. Therefore, an alloy composition in which each constituent element is within the above-mentioned range and satisfies formulas (1) and (2) shows excellent drop impact resistance even after multiple soldering operations, and suppresses coarsening of intermetallic compounds precipitated at the joint interface. At the same time, it also has excellent wettability and shear strength, has an appropriate fracture mode, and can simultaneously exhibit a high level of suppression of deformation of the solder bump.

[0051] The lower limit of formula (1) is preferably 0.00043 or more, more preferably 0.00060 or more, even more preferably 0.00064 or more, particularly preferably 0.00072 or more, and most preferably 0.00076 or more. The upper limit of formula (1) is preferably 0.00149 or less, more preferably 0.00120 or less, even more preferably 0.00100 or less, even more preferably 0.00096 or less, particularly preferably 0.00088 or less, most preferably 0.00086 or less, and may be 0.00084 or less, or 0.00080 or less.

[0052] The lower limit of the formula (2) is preferably 0.09 or more, and the upper limit of the formula (2) is preferably 0.11 or less, and more preferably 0.10 or less.

[0053] (7) Remainder: Sn The balance of the solder alloy according to the present invention is Sn. In addition to the above elements, unavoidable impurities may be contained. The balance of the solder alloy according to the present invention may be Sn and unavoidable impurities. Even if unavoidable impurities are contained, the above-mentioned effects are not affected. P forms compounds with Cu, Ni, and Ge on the surface of the molten solder, which deteriorates wettability and causes the bump to deform, so it is preferable not to contain it in the solder alloy according to the present invention. Fe forms an oxide film that is difficult to remove with flux, etc., which deteriorates wettability and causes the bump to deform, so it is preferable not to contain it in the solder alloy according to the present invention. Ce increases the melting point of the solder alloy, forms an oxide film and compounds, and forms coarse intermetallic compounds at the bonding interface, so that the effects of the present invention cannot be achieved, so it is preferable not to contain it in the solder alloy according to the present invention.

[0054] 2. Solder balls The solder alloy according to the present invention can be used as a solder ball. The solder ball according to the present invention is used for forming electrodes of semiconductor packages such as BGA (ball grid array) and bumps on substrates. The diameter of the solder ball according to the present invention is preferably within a range of 1 to 1000 μm. The solder ball can be manufactured by a general solder ball manufacturing method.

[0055] 3. Solder preform The shape of the solder preform according to the present invention is not particularly limited, and it can be used in the form of a plate, a ring, a cylinder, a ribbon, a square, a disk, a washer, a chip, a wire, etc. The solder preform may contain high-melting-point metal particles (e.g., Ni particles or Cu particles, and alloy powder mainly composed of Ni or Cu) therein, which have a higher melting point than the solder alloy and are easily wetted by the molten solder.

[0056] 4. Solder joints The solder joint according to the present invention is suitable for use in joining at least two or more members to be joined. The members to be joined are not particularly limited as long as they are electrically connected using the solder alloy according to the present invention, and include, for example, elements, substrates, electronic components, printed circuit boards, insulating substrates, heat sinks, lead frames, semiconductors using electrode terminals, power modules, inverter products, and the like.

[0057] The solder alloy according to the present invention may be used for bonding in a conventional manner, for example, by using a reflow method. The melting temperature of the solder alloy when performing flow soldering may be about 20°C higher than the liquidus temperature. Furthermore, when using the solder alloy according to the present invention for bonding, the alloy structure can be made finer by taking into consideration the cooling rate during solidification. For example, the solder joint is cooled at a cooling rate of 2 to 3°C / s or more. Other bonding conditions can be appropriately adjusted depending on the alloy composition of the solder alloy.

[0058] 5. Circuit The circuit according to the present invention is an electric circuit, and since it has the above-described solder joint, it is preferably an in-vehicle electronic circuit that requires high reliability, particularly a hybrid semiconductor circuit. The present invention including the solder alloy can also be used in a power module.

[0059] 6. Other The solder alloy according to the present invention can be manufactured by using a low alpha radiation material as its raw material, and when such a low alpha radiation alloy is used to form solder bumps around a memory, it is possible to suppress soft errors. EXAMPLES

[0060] The present invention will be described with reference to the following examples, but the present invention is not limited to the following examples. In order to verify the effectiveness of the present invention, the solder alloys shown in Table 1 were used to evaluate (1) wettability, (2) shear strength, (3) fracture mode, (4) drop impact, (5) IMC grain size, and (6) irregular bumps.

[0061] (1) Wettability Solder balls with a diameter of 0.3 mm were produced from the solder alloys shown in Tables 1 and 2 below. Flux (WF-6317, manufactured by Senju Metal Industry Co., Ltd.) was applied to a substrate (S / F: Cu-OSP), and the obtained solder balls were then mounted. Next, reflow soldering (heating temperature: 220°C or higher, holding time: 40 seconds, peak temperature 245°C) was performed using a reflow device (SNR-615, manufactured by Senju Metal Industry Co., Ltd.). After reflow, the maximum length of the distance between two parallel lines sandwiching the projected image of the wetted and spread flat shape was measured using a digital microscope (VHX-7000, manufactured by Keyence Corporation). The substrate material used was a glass epoxy substrate (FR-4) with a thickness of 1.2 mm. When the wet spreading length was 900 μm or more, it was evaluated as "◎", when the wet spreading length was 800 μm or more and less than 900 μm, it was evaluated as "◯", and when the wet spreading length was less than 800 μm, it was evaluated as "×". In this example, "◯" and "◎" were evaluation results that were acceptable for practical use.

[0062] (2) Share strength Solder balls with a diameter of 0.3 mm were prepared from the solder alloys shown in Tables 1 and 2 below. The solder balls were placed on a substrate with a thickness of 1.2 mm and an electrode size of 0.5 mm in diameter (Cu-OSP), and soldering was performed. The number of pieces to be soldered was 10. The soldering conditions were as follows: flux (WF-6400 manufactured by Senju Metal Industry Co., Ltd.) was applied onto the electrodes, and the reflow profile was set to heating temperature: 220°C or higher, holding time: 40 seconds, peak temperature: 245°C, and cooling rate: 2°C / s, and soldering was performed using a reflow device (SNR-615 manufactured by Senju Metal Industry Co., Ltd.). The prepared substrate was subjected to a shear strength test using a shear strength measuring device (SERIES4000HS manufactured by Nordson Dage) at a shear speed of 1000 mm / s. When the average bonding strength of the 10 pieces was 5.5 N or more, it was marked with "◎", when it was 4.6 N or more but less than 5.5 N, it was marked with "◯", and when it was less than 4.6 N, it was marked with "X". In this example, "◯" and "◎" were evaluation results that were acceptable for practical use.

[0063] (3) Destruction mode The samples after the shear strength test were observed using a digital microscope (Keyence Corporation: VHX-7000) to see if they were broken in the bulk or at the joint interface. If all 10 pieces were broken in the solder alloy (bulk), they were marked with "◎", if 9 out of 10 pieces were broken in the solder alloy (bulk), they were marked with "○", and if 8 or less out of 10 pieces were broken in the solder alloy (bulk), they were marked with "×". In this example, "◯" and "◎" were evaluation results that were acceptable for practical use.

[0064] (4) Drop impact Solder balls with a diameter of 0.3 mm were made from the solder alloys shown in Tables 1 and 2 below. These solder balls were soldered to a module board for CSP measuring 12 x 12 mm using flux WF-6317 manufactured by Senju Metal Industry Co., Ltd., to produce CSPs using the solder alloys of each composition as electrodes. The CSPs were mounted on a glass epoxy board (FR-4) measuring 30 x 120 mm and 0.8 mm in thickness, printed with solder paste according to the electrode pattern, and soldered using a reflow device (SNR-615 manufactured by Senju Metal Industry Co., Ltd.) with a reflow profile of a heating temperature of 220°C or higher, a holding time of 40 seconds, and a peak temperature of 245°C to produce evaluation boards.

[0065] A drop impact test was carried out on the prepared evaluation board under the following conditions. The test method was to fix both ends of the evaluation board at a position 10 mm above the base using a special jig. In accordance with the JEDEC standard, impacts with an acceleration of 1500G were repeatedly applied, and the point at which the resistance value increased 1.5 times from the initial resistance value was considered to be a break, and the number of drops was recorded. A break count of 210 or more was marked as "◎", a break count of 150 to 209 was marked as "◯", and a break count of 149 or less was marked as "×". In this example, "◯" and "◎" were evaluation results that were acceptable for practical use.

[0066] (5) IMC grain size The solder bulk remaining on the surface of the substrate after the fracture mode observation was removed using a metal stripper, exposing the crystal grains made of intermetallic compounds. Then, the exposed intermetallic compounds were photographed at 3000 times magnification using a scanning electron microscope (JSM-7000F, manufactured by JEOL Ltd.). Then, the total area of ​​each crystal grain was calculated from the photographed image using image analysis software (Scandium, manufactured by EMSIS GmbH) attached to the scanning electron microscope, and the average area (S) of the crystal grains was calculated by dividing the total area by the number of crystal grains. From this average area (S), the square root of (4S / π) was calculated to obtain the crystal grain size. When the grain size of the IMC was 3 μm or less, it was evaluated as "◎", when it was more than 3 μm and 6 μm or less, it was evaluated as "◯", and when it was more than 6 μm, it was evaluated as "×". In this example, "◯" and "◎" were evaluation results that were acceptable for practical use.

[0067] (6) Irregular Bumps Solder balls with a diameter of 0.3 mm were produced from the solder alloys shown in Tables 1 and 2 below. The solder balls were placed on a substrate with a thickness of 1.2 mm and an electrode size of 0.5 mm in diameter (Cu-OSP), and soldering was performed. The number of pieces to be soldered was 30. The soldering conditions were as follows: flux (WF-6400 manufactured by Senju Metal Industry Co., Ltd.) was applied onto the electrodes, and the reflow profile was as follows: heating temperature: 220°C or higher, holding time: 40 seconds, peak temperature: 245°C, cooling rate: 2°C / s. Soldering was performed using a reflow device (SNR-615 manufactured by Senju Metal Industry Co., Ltd.). After soldering, observation was performed using a scanning electron microscope (JSM-7000F manufactured by JEOL Ltd.). When there were zero irregular bumps among the 30, it was marked with "◎", when there were 1 to 2 bumps, it was marked with "◯", and when there were 3 or more bumps, it was marked with "X". In this example, the evaluation results of "◯" and "◎" were satisfactory for practical use. The evaluation results are shown in Tables 1 and 2.

[0068] [Table 1]

[0069] [Table 2]

[0070] As is clear from Tables 1 and 2, all of Examples 1 to 40 had appropriate contents of Ag, Cu, Ni, and Ge, and were therefore rated as "good" or "good" in all evaluation items. Furthermore, Examples 2 to 4, 8, 9, 17, 18, 26, 27, and 29 to 40, which satisfied formulas (1) and (2), were rated as "good" in all evaluation items for solder joints, including fracture mode, shear strength, drop impact, and irregular shaped bumps, demonstrating excellent effects.

[0071] On the other hand, Comparative Example 1 had poor wettability and shear strength due to its low Ag content. Comparative Example 2 had poor shear strength and drop impact resistance due to its high Ag content. Comparative Example 3 had poor shear strength and many irregularly shaped bumps due to its low Cu content. Comparative Example 4 had poor results in all evaluations due to its high Cu content.

[0072] In Comparative Example 5, since it did not contain Ni, the fracture mode was inappropriate and the shear strength was poor. In Comparative Example 6 and Comparative Example 7, since the Ni content was low, the shear strength was poor and many irregularly shaped bumps were generated. In Comparative Example 8, since the Ni content was high, all the evaluations were poor. In Comparative Example 9 and Comparative Example 10, since the Ge content was low, many irregularly shaped bumps were generated. In Comparative Example 11, since the Ge content was high, the wettability was poor and many irregularly shaped bumps were generated. In Comparative Example 12 and Comparative Example 13, since they each contained P and Fe, the wettability was poor and many irregularly shaped bumps were generated. In Comparative Examples 14 to 16, since they contained Ce, all the evaluations were poor.

[0073] FIG. 1 is a surface SEM photograph of an intermetallic compound formed at a joint interface of a solder joint produced using the solder alloy of Example 3. FIG. 2 is a surface SEM photograph of an intermetallic compound formed at a joint interface of a solder joint produced using the solder alloy of Comparative Example 4. The particles shown in FIG. 1 and FIG. 2 are IMCs (intermetallic compounds), and are images of SEM photographs taken in the above-mentioned "(5) IMC grain size". As is clear from FIG. 1 and FIG. 2, the IMC of Example 3 was finer than the IMC of Comparative Example 4. In addition, the IMC of Example 3 had a rounded crystal grain shape and small surface irregularities in the IMC compared to the IMC of Comparative Example 4. Therefore, Example 3 had an appropriate fracture mode, high shear strength, and excellent drop impact resistance. This was the same in other Examples, and particularly, Examples 2, 4, 8, 9, 17, 18, 26, 27, 29 to 40 showed excellent results.

Claims

1. A solder alloy characterized by having an alloy composition consisting of, in mass%, Ag: 0.10 to 3.00%, Cu: 0.80 to 6.00%, Ni: 0.08 to 0.60%, Ge: 0.0010 to 0.0150%, and the balance being Sn.

2. 2. The solder alloy of claim 1, wherein the alloy composition further contains 0.1% or less in total of at least one of Bi, Sb, In, Zn, Ga, Mn, Cr, Co, Si, Ti, and rare earth elements.

3. The solder alloy according to claim 1 or 2, wherein the alloy composition satisfies the following formulas (1) and (2): 0.00043≦Cu×Ni×Ge≦0.00149 (1) 0.09≦Ag×Cu×Ni≦0.11 (2) In the above formulas (1) and (2), Ag, Cu, Ni, and Ge represent the contents (mass %) of the alloy composition.

4. A solder ball made of the solder alloy according to claim 1 or 2.

5. A solder preform made of the solder alloy according to claim 1 or 2.

6. A solder joint comprising the solder alloy of claim 1 or 2.

7. A circuit having the solder joint of claim 6.

Citation Information

Patent Citations

  • Solder

    JP1999077366A

  • Lead-free solder alloy for electronic member to be mounted on automobile, solder ball and electronic member

    JP2007237252A

  • Solder alloy for lead-free and antimony-free, solder ball, ball grid array, and solder joint

    JP2021028078A

  • Lead-free and antimony-free solder alloy, solder ball, and solder joint

    JP2021126685A

  • Lead-free and antimony-free solder alloy, solder ball, and solder joint

    JP2021126704A