Method for producing low-molecular-weight fluorine compound

By controlling temperature differences using microwave irradiation in fluororesin decomposition, the method enhances the selectivity of monomers in low-molecular-weight fluorine compounds, addressing the lack of temperature control in conventional methods.

JP2024159120APending Publication Date: 2024-11-08MICROWAVE CHEM +2

Patent Information

Application Number
JP2023074905
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Conventional chemical recycling methods for fluororesins lack control over the temperature environment of low-molecular-weight fluorine compounds generated during decomposition, leading to suboptimal selectivity of constituent monomers.

Method used

A method involving microwave irradiation to heat a microwave absorber in a reaction vessel, controlling temperature differences (Δ1 and Δ2) between the absorber and the generated gas, and carrier gas, to enhance the selectivity of monomers in the produced low-molecular-weight fluorine compounds.

Benefits of technology

Improves the selectivity of constituent monomers in the produced low-molecular-weight fluorine compounds by controlling temperature differences, resulting in a higher proportion of desired monomers in the decomposition products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159120000002
    Figure 2024159120000002
  • Figure 2024159120000003
    Figure 2024159120000003
  • Figure 2024159120000004
    Figure 2024159120000004
Patent Text Reader

Abstract

To improve selectivity of a constituent monomer of a fluororesin among the low-molecular-weight fluorine compounds produced in a fluororesin decomposition method in which a temperature difference is provided so that a temperature of product gas led out from a reaction vessel becomes lower than a temperature of a heated microwave absorber in the decomposition of the fluororesin.SOLUTION: In a method for producing a low-molecular-weight fluorine compound by decomposing a fluororesin by bringing a heated microwave absorber into contact with a material containing a fluororesin in a reaction vessel provided with a carrier gas inlet and a decomposition gas outlet, (i) a temperature difference Δ1(TR-TI), obtained by subtracting a carrier gas temperature TI(°C) from a temperature TR(°C) of the heated microwave absorber, is set to be more than 500°C and / or (ii) a temperature difference Δ2(TR-TE), obtained by subtracting the product gas temperature TE(°C) at the outlet from the temperature TR(°C), is set to be 300°C or higher.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a technique for decomposing a fluororesin. More specifically, the present invention relates to a method for producing a low molecular weight fluorine compound by thermal decomposition of a fluororesin using microwave irradiation heating. [Background technology]

[0002] Fluorine resins are widely used in coating materials for heat-resistant electric wires, semiconductor manufacturing materials, electronic components, etc., taking advantage of their excellent properties such as lubricity, heat resistance, and chemical resistance. In recent years, decomposition and reuse of synthetic resins containing fluororesins has been actively studied in general. For example, Patent Document 1 proposes a chemical recycling method for extracting low-molecular-weight tetrafluoroethylene monomers and dimers generated by thermally decomposing PTFE from a material containing PTFE, the chemical recycling method including the steps of heating a fluidized bed reactor having a fluidized bed formed of an inert granular material and having the material supplied thereto, introducing an inert gas as a fluidizing gas into the fluidized bed reactor, and extracting from the fluidized bed reactor the low-molecular-weight tetrafluoroethylene monomers and dimers generated by thermally decomposing PTFE by the heating together with the inert gas. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2004-346000 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present inventors noticed that in the conventional chemical recycling technology for fluororesin, no consideration was given to control of the temperature environment to which low molecular weight fluorine compounds such as fluorine-based monomers generated from fluororesin are exposed, and discovered a method for controlling the temperature of the generated gas discharged from the reaction vessel to be lower than the temperature in the decomposition reaction system. However, further consideration led to the problem that such a method has room for improvement in the selectivity of the constituent monomers of the fluororesin among the generated low molecular weight fluorine compounds.

[0005] Therefore, the present invention aims to improve the selectivity of constituent monomers of fluororesin among the low molecular weight fluorine compounds produced in a fluororesin decomposition method in which a temperature difference (hereinafter also referred to as "temperature TE") is provided so as to control the temperature of the product gas discharged from a reaction vessel to be lower than the temperature in the decomposition reaction system, i.e., the temperature of a heated microwave absorber (hereinafter also referred to as "temperature TR"). [Means for solving the problem]

[0006] As a result of intensive research, the present inventors have found that the selectivity of the constituent monomers of the fluororesin among the low molecular weight fluorine compounds produced can be improved by setting the temperature difference Δ1 (TR-TI) obtained by subtracting the carrier gas temperature TI (°C) at the inlet of the reaction vessel from the temperature TR (°C) of the microwave absorber heated in the reaction vessel to more than 500°C, and / or by setting the temperature difference Δ2 (TR-TE) obtained by subtracting the decomposition gas outlet TE (°C) of the product gas discharged from the reaction vessel from the temperature TR (°C) of the microwave absorber heated in the reaction vessel to 300°C or more. The present invention was completed based on this finding and through further research.

[0007] That is, the present invention provides the following aspects. Item 1. The method includes a decomposition step of heating a microwave absorber by microwave irradiation in a reaction vessel provided with a carrier gas inlet and a decomposition gas outlet, and decomposing the fluororesin into a low molecular weight fluorine compound by contacting the heated microwave absorber with a material containing a fluororesin, (i) A method for producing a low molecular weight fluorine compound, wherein a temperature difference Δ1 (TR−TI) obtained by subtracting a carrier gas temperature TI (°C) at the inlet from a temperature TR (°C) of the heated microwave absorber is set to be more than 500°C. Item 2. The method includes a step of heating a microwave absorber by microwave irradiation in a reaction vessel provided with a carrier gas inlet and a decomposition gas outlet, and decomposing the fluororesin into a low molecular weight fluorine compound by contacting the heated microwave absorber with a material containing a fluororesin, (ii) A method for producing a low molecular weight fluorine compound, wherein a temperature difference Δ2 (TR-TE) obtained by subtracting a temperature TE (°C) of the generated gas at the outlet of the reaction vessel from a temperature TR (°C) of the heated microwave absorber is set to be 300°C or more. Item 3. The method according to item 1 or 2, wherein an introduction speed R of the carrier gas from the inlet is 0.005 to 20 m / s. Item 4. The method according to any one of Items 1 to 3, wherein the temperature TE (°C) of the generated gas discharged from the reaction vessel at the outlet is 20°C or higher and lower than 250°C. Item 5. The microwave absorber is prepared in the form of a microwave absorber-containing layer that contains particles of a material containing the microwave absorber and the fluororesin and is provided so as to pass an air flow from the carrier gas inlet to the decomposition gas outlet, 5. The manufacturing method according to any one of items 1 to 4, wherein, when a center of an opening of the outlet is defined as point Pe and an intersection point between a central axis of the microwave absorber-containing layer and a surface of the microwave absorber-containing layer opposite to the outlet is defined as point Pl, a ratio h / H of a height h of the microwave absorber-containing layer to a height H from point Pl to point Pe is 0.01 to 0.8. Item 6. The method according to any one of Items 1 to 5, wherein the microwave absorber has a particle size d of 0.1 to 25 mm. Item 7. The method according to item 5 or 6, wherein the microwave absorber-containing layer has a height h of 0.1 to 200 mm. Item 8. The manufacturing method according to any one of Items 2 to 7, wherein a temperature difference Δ1 (TR−TI) obtained by subtracting a carrier gas temperature TI (°C) at the inlet from a temperature TR (°C) of the heated microwave absorber is set to be more than 250°C. Effect of the Invention

[0008] According to the present invention, in a fluororesin decomposition method in which a temperature difference Δ2 (TR-TE) is provided so as to control the temperature TE of the generated gas discharged from a reaction vessel to be lower than the temperature in the decomposition reaction system, i.e., the temperature TR of the heated microwave absorber, the selectivity of the constituent monomers of the fluororesin can be improved among the generated low molecular weight fluorine compounds. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic diagram of an example of an apparatus (upward parallel flow type cylindrical reaction vessel) used in the production method of the present invention. [Diagram 2] FIG. 1 is a schematic diagram of an example of an apparatus (a downward parallel flow type cylindrical reaction vessel) used in the production method of the present invention. [Diagram 3] FIG. 1 is a schematic diagram of an example of an apparatus (continuous-tank reaction vessel) used in the production method of the present invention. [Figure 4] FIG. 1 is a schematic diagram of an example of an apparatus (continuous-tank reaction vessel) used in the production method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The method for producing a low molecular weight fluorine compound of the present invention includes a decomposition step of heating a microwave absorber by microwave irradiation in a reaction vessel provided with a carrier gas inlet and a decomposition gas outlet, and decomposing the fluororesin into a low molecular weight fluorine compound by bringing the heated microwave absorber into contact with a material containing a fluororesin, and is characterized in that the following settings (i) and / or (ii) are performed: (i) Set the temperature difference Δ1 (TR-TI) obtained by subtracting the carrier gas temperature TI (℃) at the inlet from the temperature TR (℃) of the heated microwave absorber to be more than 500°C. (ii) Set the temperature difference Δ2 (TR-TE) obtained by subtracting the temperature TE (°C) at the outlet of the generated gas discharged from the reaction vessel from the temperature TR (°C) of the heated microwave absorber to be 300°C or more. The method for producing a low molecular weight fluorine compound of the present invention will be described in detail below.

[0011] [1. Fluorine resin] In the present invention, a fluororesin is used as a raw material for a low molecular weight fluorine compound. The fluororesin is a fluorine compound having a molecular weight of 500 or more and a fluorine content (weight basis) of 57% or more.

[0012] Examples of the fluororesin include fluorinated polyolefin and fluorinated polyether.

[0013] Fluorinated polyolefins are polymers or oligomers having repeat units derived from a fluorinated olefin.

[0014] Examples of the fluorinated olefin include tetrafluoroethylene (TFE), hexafluoropropylene (HFP), vinylidene fluoride (VDF), chlorotrifluoroethylene (CTFE), partially fluorinated or perfluorovinyl ethers, partially fluorinated or perfluoroallyl ethers, and the like.

[0015] The perfluorovinyl ether has the general formula CF2=CF-OR f A compound represented by the formula: f R represents a perfluorinated linear, cyclic, or branched aliphatic group which may contain one or more oxygen atoms. f When R contains one or more oxygen atoms, f As for -(R a f O) n (R bf O) m R c f [wherein R a f and R b f are different linear or branched or cyclic perfluoroalkylene groups having 1 to 6 carbon atoms, in particular 2 to 6 carbon atoms, m and n are independently 0 to 10, R c f R is a perfluoroalkyl group having 1 to 6 carbon atoms. f When does not contain an oxygen atom, specific examples of the perfluorovinyl ether include perfluoromethyl vinyl ether (PMVE), perfluoropropyl vinyl ether, and perfluoroisopropyl vinyl ether.

[0016] Specific examples of the perfluorovinyl ether include perfluoro(methyl vinyl) ether (PMVE), perfluoro(ethyl vinyl) ether (PEVE), perfluoro(n-propyl vinyl) ether (PPVE-1), perfluoro-2-propoxypropyl vinyl ether (PPVE-2), perfluoro-3-methoxy-n-propyl vinyl ether, perfluoro-2-methoxy-ethyl vinyl ether, CF3-(CF2)2-O-CF(CF3)-CF2-O-CF(CF3)-CF2-O-CF=CF2, CF2=CF-O-(CF2)3OCF3, and CF2=CFO(CF2)2OCF3.

[0017] The perfluoroallyl ether may be represented by the general formula CF2=CF-CF2-OR f A compound represented by the formula: f is the same as R described above for perfluorovinyl ether. f is the same as.]

[0018] The fluorinated polyolefin may be a polymer or oligomer consisting of repeating units derived from a fluorinated olefin, or may be a polymer or oligomer containing repeating units derived from a non-fluorinated olefin in addition to repeating units derived from a fluorinated olefin. The non-fluorinated olefin is not particularly limited, but may be a C2-C8 olefin, more preferably ethylene (E) and propylene (P). Among these fluorinated polyolefins, a polymer or oligomer consisting of repeating units derived from a fluorinated olefin (i.e., a fluorinated polyolefin in which the molar ratio of repeating units derived from a non-fluorinated olefin is 0%) is preferably used.

[0019] Suitable examples of the fluorinated polyolefin include homopolymers of TFE and the following copolymers: TFE and HFP; TFE, HFP and VDF; TFE and CTFE; TFE, CTFE and E or P; TFE and PMVE, PEVE, PPVE-1 or PPVE-2; TFE, E and HFP; and polymers containing repeating units derived from CTFE and E or P. Among these fluorinated polyolefins, preferred is homopolymer of TFE.

[0020] Fluorinated polyethers are polymers or oligomers that have fluorinated oxyalkylene repeating units.

[0021] The fluorinated oxyalkylene repeat unit is -C l X 2l O-, l is an integer of 1 or more, X is hydrogen or fluorine, is linear or branched, and l and X may be different in each repeat occurrence.

[0022] The fluororesin may be a fluorinated non-ionomer or a fluorinated ionomer (plural -SO3 - and / or -COO -The fluorinated ionomer may be a fluoropolymer having a group as a pendant group or a terminal group. As the fluorinated ionomer, those used for preparing membranes in fuel cells or electrochemical reactions can be used without particular limitation.

[0023] The fluororesin may have a functional group containing a hydrogen atom or an atom other than fluorine at the end. The functional group containing an atom other than fluorine is not particularly limited, but examples thereof include an iodine group, a bromine group, a chlorine group, a hydroxyl group and its esters, and a vinyl group.

[0024] The above fluororesins may be used alone or in combination of two or more.

[0025] [2. Materials containing fluororesin] The fluororesin is subjected to the decomposition step in the form of a material containing the fluororesin. The material may consist of only the fluororesin, or may contain other components other than the fluororesin. Examples of other components include resin additives to be mixed into the fluororesin composition, and more specifically, examples of such additives include fillers, pigments, lubricants, curing agents, curing accelerators, thermal conductive agents, and electrical conductive agents.

[0026] The properties of the material containing fluororesin in the decomposition step are determined according to the conditions in the decomposition step and are not particularly limited. When the material containing fluororesin is solid, it is used in a particulate form. The particles are obtained by processing the fluororesin material into particles by any means. Examples of such means include a milling device, a pulverizing device, and the like.

[0027] The particle size is not particularly limited, but may be, for example, 20 μm to 100 mm, preferably 100 μm to 10 mm, and more preferably 250 μm to 5 mm.

[0028] The material containing fluororesin may be obtained by a pretreatment that may be carried out prior to the decomposition step. Such pretreatment is not particularly limited as long as a material containing fluororesin can be obtained, and examples of such pretreatment include a treatment for separating and removing components not containing fluororesin and / or materials other than fluororesin from the material to be recycled, a treatment for removing oil and / or dust, and a fluorination treatment of polymer materials (a treatment for converting C-H bonds to C-F bonds by treating a polymer material with F2 gas).

[0029] The method of supplying the material containing fluororesin into the reaction vessel is not particularly limited, and may be appropriately selected by a person skilled in the art. For example, when the material containing fluororesin is in the form of particles, it is preferable to supply it into the reaction vessel by gravity, and when the material containing fluororesin is in the form of a liquid, it can be supplied into the reaction vessel by spraying, for example.

[0030] [3. Reaction vessel] The reaction vessel used is a vessel equipped with a carrier gas inlet and a cracked gas outlet for introducing and discharging a gas flow. Examples of the reaction vessel used in the present invention include a parallel flow type cylindrical reaction vessel and a continuous tank type reaction vessel.

[0031] Specific examples of parallel flow cylindrical reaction vessels are shown in Figures 1 and 2. The parallel flow cylindrical reaction vessel 1 shown in Figure 1 is provided with a carrier gas inlet 1I and a decomposition gas outlet 1E, and is configured so that the flow pattern of the carrier gas 3 is an upward parallel flow type. The parallel flow cylindrical reaction vessel 1a shown in Figure 2 is provided with a carrier gas inlet 1I and a decomposition gas outlet 1E, and is configured so that the flow pattern of the carrier gas 3 is a downward parallel flow type.

[0032] Specific examples of continuous-tank reaction vessels are shown in Figures 3 and 4. The continuous-tank reaction vessel 1b shown in Figure 3 is provided with a carrier gas inlet 1I and a decomposition gas outlet 1E, and is preferably used for small-scale reactions. The continuous-tank reaction vessel 1c shown in Figure 4 is provided with a carrier gas inlet 1I and a decomposition gas outlet 1E, and is preferably used for large-scale reactions. In addition, the continuous-tank reaction vessels 1b and 1c shown in Figures 3 and 4 can be equipped with a stirrer (not shown).

[0033] More specifically, the reaction vessel of the present invention can be incorporated into an apparatus similar to a general catalytic reactor, and in this apparatus, a microwave absorber is used instead of the catalyst in the general catalytic reactor.

[0034] Furthermore, since microwaves are used as the heating means in the present invention, the device can be equipped with a microwave generator. The microwave generator can be appropriately selected from known devices, and examples of such devices include diodes, magnetrons, gyrotrons, traveling wave tubes, klystrons, ubitrons, and amplitrons.

[0035] [4. Microwave absorbers] [4-1. Examples of microwave absorbers] The microwave absorber is not particularly limited as long as it absorbs the irradiated microwaves, generates heat to a temperature at which the fluororesin can be decomposed, and has the properties of being in a solid state and chemically inactive under the decomposition reaction conditions of the fluororesin. The temperature TR of the microwave absorber heated in the decomposition step establishes the temperature conditions for advancing the decomposition reaction of the fluororesin, and corresponds to the temperature in the reaction system of the decomposition reaction of the fluororesin.

[0036] Specific examples of microwave absorbers include metals, metal salts, intermetallic compounds, carbon, carbides, etc., having the above-mentioned characteristics. Preferably, the microwave absorber has a density of, for example, 1 to 10 g / cm. 3 , preferably 1.5 to 7 g / cm 3Preferably, as the microwave absorber, a substance having a microwave absorbing ability with a dielectric loss of, for example, 0.01 to 30, preferably 0.1 to 11, can be used.

[0037] More specific examples of microwave absorbers include metals such as single metals such as Ni, Pt, Co, and Pt, and alloys such as Pt / Cu and Pt / Re. Metal salts include metal oxides, metal hydroxides, metal halides, and silicides. Intermetallic compounds include molybdenum silicide and titanium boride. Carbon includes graphite such as expanded graphite, activated carbon, carbon fiber, carbon nanotubes, and carbon black. Carbides include silicon carbide, boron carbide, titanium carbide, and zirconium carbide. These microwave absorbers may be used alone or in combination. Among these microwave absorbers, carbides are preferred, and silicon carbide is more preferred.

[0038] [4-2. Microwave absorber particle size d] In the present invention, the microwave absorber is preferably used in the form of particles. The particle size of the microwave absorber particles (hereinafter also referred to as "particle size d") is not particularly limited, but may be, for example, 0.1 to 25 mm. In addition, when the microwave absorber-containing layer described later is in the form of a fixed bed, the particle size d is preferably 0.1 to 25 mm, more preferably 1 to 25 mm, even more preferably 2.8 to 25 mm, and even more preferably 4.8 to 25 mm, from the viewpoint of further increasing the temperature difference Δ2 (TR-TE) and further improving the selectivity of the constituent monomer of the fluororesin, and further, the upper limit of the range of the particle size d may be 10 mm or less or 8 mm or less. When the microwave absorber-containing layer described later is in the form of a fluidized bed, the particle size d is preferably 0.5 to 25 mm, more preferably 1 to 25 mm, even more preferably 2 to 10 mm, even more preferably 2.8 to 25 mm, and even more preferably 4.8 to 25 mm, from the viewpoint of further increasing the temperature difference Δ2 (TR-TE) and further improving the selectivity of the constituent monomer of the fluororesin, and the upper limit of the range of the particle size d may be 15 mm or less, 10 mm or less, 5 mm or less, 2.5 mm or less, 2 mm or less, or 1.5 mm or less. In the present invention, the particle size d is the average of the measured values ​​obtained by measuring the maximum diameter in a certain direction of 20 randomly selected particles with a gauge. For the gauge measurement, visual observation, an optical microscope, or an electron microscope is used depending on the size of the particles.

[0039] In order to control (i) above, the upper limit of the particle size d of the microwave absorber can be set to preferably 2.5 mm or less, more preferably 2 mm or less, and further preferably 1.5 mm or less.

[0040] [4-3. Aspects of microwave absorber-containing layer] As a more specific embodiment of the microwave absorber during the decomposition reaction, it may be either a fixed bed or a fluidized bed.

[0041] The microwave absorber can be prepared in the reaction vessel prior to the decomposition step in the form of a microwave absorber-containing layer of a mixture containing the microwave absorber and particles of the material containing the fluororesin.

[0042] The microwave absorber-containing layer is provided in the reaction vessel so as to pass the airflow from the carrier gas inlet to the decomposition gas outlet. Specifically, in the parallel flow type cylindrical reaction vessels 1 and 1a shown in Fig. 1 and Fig. 2, the microwave absorber-containing layer 2 is provided between the carrier gas inlet and the decomposition gas outlet, and in the continuous tank type reaction vessels 1b and 1c shown in Fig. 3 and Fig. 4, the microwave absorber-containing layer 2 is provided at the bottom of the reaction vessel.

[0043] The amount of microwave absorber used relative to the amount of particles of the fluororesin-containing material is not particularly limited, but may be, for example, 0.1 to 1000 parts by weight, preferably 1 to 100 parts by weight, more preferably 10 to 50 parts by weight, and even more preferably 15 to 45 parts by weight, relative to 1 part by weight of the particles of the fluororesin-containing material.

[0044] The microwave absorber-containing layer 2 has a height h when the contact surface with the gas phase is horizontally leveled in the initial stage (before the decomposition step is started). The height h refers to the height at the central axis CI of the microwave absorber-containing layer 2 (in the embodiment of Figs. 1 to 4, the central axis CI of the microwave absorber-containing layer 2 coincides with the central axis of the reaction vessels 1, 1a, 1b, and 1c).

[0045] Specific examples of the height h of the microwave absorber-containing layer 2 include, for example, 0.1 to 200 mm, and from the viewpoint of further increasing the temperature difference Δ2 (TR-TE) and further improving the selectivity of the constituent monomer of the fluororesin, the height h is preferably 1 to 100 mm, more preferably 3 to 50 mm, and further preferably 5 to 30 mm. When the microwave absorber-containing layer 2 is in the form of a fixed bed, the height h is preferably 3 to 50 mm, more preferably 5 to 30 mm, and when the microwave absorber-containing layer 2 is in the form of a fluidized bed, the height h is preferably 5 to 30 mm.

[0046] In addition, when the center of the opening of the outlet 1E of the reaction vessel 1, 1a, 1b, 1c is defined as point Pe, and the intersection point between the central axis CI of the microwave absorber-containing layer 2 and the surface of the microwave absorber-containing layer 2 on the opposite side to the outlet 1E is defined as point Pl, the ratio (h / H) of the height h of the microwave absorber-containing layer 2 when the height H from point Pl to point Pe is defined as 1 is, for example, 0.01 to 0.8, and from the viewpoint of further increasing the temperature difference Δ2 (TR-TE) and further improving the selectivity of the constituent monomer of the fluororesin, the ratio is preferably 0.01 to 0.5, more preferably 0.05 to 0.4, even more preferably 0.1 to 0.3, and even more preferably 0.15 to 0.25.

[0047] [5. Carrier gas] [5-1. Examples of carrier gases] The carrier gas introduced from the carrier gas inlet of the reaction vessel is not particularly limited as long as it has chemically inactive properties under the decomposition reaction conditions of the fluororesin, and examples thereof include water vapor, nitrogen, rare gases (Xe, Ar, Ne, He, etc.). These carrier gases may be used alone or in combination of two or more. Among these carrier gases, water vapor and nitrogen are preferable.

[0048] [5-2. Carrier gas temperature TI at the inlet and its setting] In the present invention, the temperature TI of the carrier gas at the inlet is defined as the temperature at the center of the opening of the inlet 1I (hereinafter also referred to as "point Pi").

[0049] In the present invention, in order to improve the selectivity of the constituent monomers of the fluororesin among the low molecular weight fluorine compounds produced, the temperature TI of the carrier gas at the inlet can be set so as to obtain the temperature difference Δ1 (TR-TI) shown in (i) above.

[0050] The temperature difference Δ1(TR-TI) is not particularly limited as long as it is more than 500° C., but from the viewpoint of further improving the selectivity of the constituent monomer of the fluororesin, it is preferably 530° C. or more, 540° C. or more, 550° C. or more, 570° C. or more, 590° C. or more, or 600° C. or more, more preferably 620° C. or more, 640° C. or more, 660° C. or more, 680° C. or more, 700° C. or more, 720° C. or more, and even more preferably 740° C. or more, 760° C. or more, or 780° C. or more. The upper limit of the temperature difference Δ1(TR-TI) is not particularly limited either, but examples thereof include 1000° C. or less, 900° C. or less, or 800° C. or less.

[0051] In the present invention, when setting (ii), the temperature difference Δ1 (TR-TI) is allowed to be more than 250°C (preferably 300°C or more, more preferably 350°C or more, even more preferably 400°C or more, and even more preferably 450°C or more).

[0052] In the present invention, the value obtained by dividing the temperature difference Δ1(TR-TI) by the temperature TR (°C) is, for example, 0.5 or more, preferably 0.85 or more, more preferably 0.9 or more, even more preferably 0.93 or more, even more preferably 0.94 or more, and even more preferably more than 0.97, and from the viewpoint of further improving the selectivity of the constituent monomer of the fluororesin, is preferably 0.965 or more, more preferably 0.972 or more, and even more preferably 0.976 or more. The upper limit of the value obtained by dividing the temperature difference Δ1(TR-TI) by the temperature TR is not particularly limited, and may be, for example, 0.990 or less, 0.985 or less, or 0.980 or less.

[0053] In order to perform the control (i) above, the value obtained by dividing the temperature difference Δ1(TR-TI) by the temperature TR (°C) can be set to preferably more than 0.97, more preferably 0.965 or more, even more preferably 0.972 or more, and even more preferably 0.976 or more. In order to control Δ1(TR-TI) to a larger value, this value can be set higher.

[0054] To control (ii) above, the temperature difference Δ1(TR-TI) divided by the temperature TR (°C) can be set to, for example, 0.5 or more, preferably 0.85 or more, more preferably 0.9 or more, even more preferably 0.93 or more, and even more preferably 0.94 or more, and can also be controlled to be greater than 0.97, more preferably 0.965 or more, even more preferably 0.972 or more, and even more preferably 0.976 or more. To control Δ2(TR-TE) to a larger value, the value can be set higher.

[0055] In the present invention, the carrier gas at the inlet may or may not be preheated. That is, in the present invention, a step of preheating the carrier gas may or may not be included. Specific examples of the temperature TI include, for example, 10 to 400°C, preferably 15 to 300°C, and more preferably 20 to 200°C. More specifically, preferred examples of the temperature TI when not preheated include, for example, 10 to 30°C, preferably 13 to 25°C, and more preferably 15 to 23°C, and preferred examples of the temperature TI when not preheated include, for example, 80 to 400°C, preferably 90 to 200°C, and more preferably 100 to 150°C.

[0056] [5-3. Carrier gas introduction rate R] The introduction speed of the carrier gas from the carrier gas inlet (hereinafter also referred to as "introduction speed R") is not particularly limited and may be, for example, 0.005 to 20 m / s. From the viewpoint of further increasing the temperature difference Δ2 (TR-TE) and further improving the selectivity of the constituent monomer of the fluororesin, the introduction speed is preferably 0.007 to 2 m / s, more preferably 0.009 to 0.2 m / s, even more preferably 0.011 to 0.08 m / s, and even more preferably 0.013 to 0.02 m / s.

[0057] [6. Decomposition Reaction] The decomposition reaction is carried out by heating a microwave absorber by microwave irradiation in a reaction vessel and bringing the heated microwave absorber into contact with particles of a material containing a fluororesin, thereby decomposing the fluororesin into low molecular weight fluorine compounds.

[0058] [6-1. Reaction temperature TR] The temperature TR of the heated microwave absorber may be any temperature at which the fluororesin is decomposed. Specific examples of the temperature TR include 280 to 1500° C., preferably 490 to 1400° C. or 530 to 1300° C., more preferably 640 to 1100° C., further preferably 680 to 1000° C., and even more preferably 760 to 900° C. The microwave irradiation conditions (wavelength and frequency) for heating the microwave absorber may be appropriately set according to the temperature TR.

[0059] In order to carry out the control of (i) above, the temperature TR of the heated microwave absorber can be set to preferably 490 to 1400°C, or 530 to 1300°C, more preferably 640 to 1100°C, further preferably 680 to 1000°C, and even more preferably 760 to 900°C. Also, in order to control Δ1(TR-TI) to be larger, the temperature TR can be set higher.

[0060] The temperature TR is a temperature measured at the center position in the height h direction of the microwave absorber-containing layer from the side of the reaction vessel in an insulated state. The reaction vessel is insulated when the temperature TR is measured by surrounding the reaction vessel with ceramic wool to a thickness of 20% of the maximum outer periphery width of the reaction vessel. An optical fiber thermometer or a non-contact thermometer can be used for the temperature measurement. The insulation method constitutes the measurement condition of the temperature TR defined in the present invention, and the manufacturing method of the present invention is not limited to the form in which the insulation method is performed.

[0061] [6-2. Temperature TE of generated gas at outlet and its setting] The low molecular weight fluorine compound generated by the decomposition reaction of the fluororesin is discharged as a gas (generated gas) from the outlet 1E to the outside of the reaction vessel. In the present invention, the temperature TE of the generated gas at the outlet is the temperature at the center of the opening of the outlet 1E (hereinafter also referred to as "point Pe"). The temperature TE in the present invention is the temperature at the time when the decomposition gas (generated gas) that has passed through the microwave absorber-containing layer reaches the point Pe of the decomposition gas outlet of the reaction vessel without being cooled by a quenching method. Here, the quenching method refers to a method of cooling the decomposition gas to a temperature lower than that in the case of natural cooling (i.e., the temperature at the time when the decomposition gas that has passed through the microwave absorber-containing layer is naturally cooled before reaching the decomposition gas outlet of the reaction vessel and reaches the decomposition gas outlet), and specific methods are known in the technical field, and examples thereof include a method of expanding the decomposition gas (generated gas), a method of cooling using a separately prepared cooling gas, and a method of cooling using a cooling liquid.

[0062] In the present invention, in order to improve the selectivity of the constituent monomers of the fluororesin among the generated low molecular weight fluorine compounds, the temperature TE of the generated gas at the outlet can be set so as to obtain the temperature difference Δ2 (TR-TE) shown in (ii) above.

[0063] The temperature difference Δ2(TR-TE) is not particularly limited as long as it is 300° C. or more, but from the viewpoint of further improving the selectivity of the constituent monomer of the fluororesin, it is preferably 400° C. or more, more preferably 460° C. or more, 480° C. or more, 500° C. or more, 520° C. or more, 540° C. or more, 560° C. or more, 580° C. or more, or 600° C. or more, even more preferably 610° C. or more, 630° C. or more, 650° C. or more, 670° C. or more, 690° C. or more, or 710° C. or more, and even more preferably 730° C. or more, 750° C. or more, or 770° C. or more. The upper limit of the temperature difference Δ2(TR-TE) is not particularly limited either, but examples thereof include 1000° C. or less, 900° C. or less, or 850° C. or less.

[0064] In order to control the above (i), Δ2(TR-TE) can be set to preferably 460° C. or more, 480° C. or more, 500° C. or more, 520° C. or more, 540° C. or more, 560° C. or more, 580° C. or more, or 600° C. or more, more preferably 610° C. or more, 630° C. or more, 650° C. or more, 670° C. or more, 690° C. or more, or 710° C. or more, and even more preferably 730° C. or more, 750° C. or more, or 770° C. or more. In order to control Δ1(TR-TI) to be larger, Δ2(TR-TE) can be set to be larger.

[0065] Specific examples of the temperature TE include, for example, 20° C. or more and less than 250° C. The upper limit of the temperature range (20° C. or more and less than 250° C.) is preferably 200° C. or less, more preferably 150° C. or less, even more preferably 100° C. or less, and even more preferably 90° C. or less, 85° C. or less, or 80° C. or less, and the lower limit includes 30° C. or more, 40° C. or more, 50° C. or more, 55° C. or more, 60° C., 65° C. or more, 70° C., or 75° C. or more.

[0066] In order to perform the control (i) above, the temperature TE can be set preferably to 50° C. or more, 55° C. or more, 60° C., 65° C. or more, 70° C., or 75° C. or more, and in order to control Δ1(TR-TI) to a larger value, the temperature TE can be set higher.

[0067] [6-3. Decomposition products] The low molecular weight fluorine compounds, which are the products of the decomposition reaction, are compounds that are generated from the raw material fluorine resin and have a lower molecular weight than the fluorine resin, and usually contain a plurality of compounds. According to the present invention, the selectivity of the constituent monomers of the fluorine resin among the low molecular weight fluorine compounds generated is high (i.e., the proportion of the constituent monomers of the fluorine resin in the low molecular weight fluorine compounds generated is high).

[0068] Among the low molecular weight fluorine compounds produced, the constituent monomers of the target fluorine resin are determined according to the polymer structure of the raw material fluorine resin. Specifically, the constituent monomers of the fluorine resin are represented by the general formula CF2=CF-Rd f [In the formula, R d f represents F or a perfluoroalkyl group having 1 to 10, preferably 1 to 5, carbon atoms.], preferably tetrafluoroethylene (TFE) and hexafluoropropylene (HFP). Other specific examples of fluoroolefins include vinylidene fluoride (VDF), chlorotrifluoroethylene (CTFE), perfluorovinyl ether, and perfluoroallyl ether.

[0069] Of the low molecular weight fluorine compounds produced, compounds other than the constituent monomers of the fluororesin include polymers with a low degree of polymerization that have not decomposed to the constituent monomers of the above-mentioned fluororesin (dimers, trimers, or oligomers with a higher degree of polymerization that are gaseous at the temperature TE), and by-products (e.g., octafluorocyclobutane) and other by-products produced by further side reactions of the constituent monomers of the above-mentioned fluororesin.

[0070] The product, low molecular weight fluorine compound (product gas), is discharged from the outlet of the reaction vessel by the air flow and recovered by appropriately cooling and / or concentrating the product gas.

[0071] During the decomposition step, the material containing the fluororesin may not be additionally supplied (i.e., a batch process may be used), or the fluororesin may be additionally supplied continuously or intermittently. EXAMPLES

[0072] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0073] A continuous-tank type reaction vessel 1b shown in Fig. 3 was prepared. A microwave absorber-containing layer 2 containing a microwave absorber with a predetermined particle size d and particles of a material containing a fluororesin (PTFE, i.e., a homopolymer of tetrafluoroethylene) was provided in the cylindrical reaction vessel 1b at a predetermined height h (cm). The size of the particles of the material containing a fluororesin was 20 μm, and the amount of the microwave absorber used per part by weight of the particles of the material containing a fluororesin was 20 to 40 parts by weight.

[0074] Carrier gas (nitrogen) 3 was introduced from the inlet 1I at a predetermined carrier gas temperature TI and a predetermined introduction speed R, and while stirring with a stirrer (not shown), the microwave absorber in the microwave absorber-containing layer 2 was heated to a predetermined temperature TR by a microwave generator (not shown), and the temperature TE at the outlet 1E of the generated gas (specifically, point Pe which is the center of the opening of the outlet 1E) was measured. The temperature TR was measured using a non-contact thermometer at the center position in the height h direction of the microwave absorber-containing layer 2 from the side of the reaction vessel, with the reaction vessel being insulated by surrounding the outer periphery of the reaction vessel with ceramic wool to a thickness of 20% of the outer diameter of the vessel. The generated gas was collected from the outlet 1E, and the mass fractions of the three main components were derived from the composition analysis results. The set conditions and the composition analysis results of the generated gas are shown in Table 1.

[0075] [Table 1]

[0076] As shown in Table 1, according to Examples 1 to 3, it was confirmed that the ratio of by-products (HFP, C318) among the low molecular weight fluorine compounds produced was extremely low, and the selectivity of the constituent monomer (TFE) of the fluororesin (TFE homopolymer) was extremely high. The components of the produced gas consisted of TFE, HFP, C138, and other products, and in all of Examples 1 to 3, about 95% or more of the area value of the gas chromatograph (detector FID: Flame Ionization Detector) among the components was occupied by TFE, HFP, and C138, and it was also confirmed that the proportion of the remaining products in the produced gas was the same between Examples 1 to 3. [Explanation of symbols]

[0077] 1, 1a, 1b, 1c Reaction vessel 1I Carrier gas inlet TI Carrier gas temperature at inlet 1I Pi Center of inlet 1I 1E Carrier gas outlet TE: Temperature of produced gas at outlet 1E Pe Center of outlet 1E 2. Microwave absorber-containing layer CI Central axis of microwave absorber-containing layer 2 Pl: Intersection of the central axis CI and the surface of the microwave absorber-containing layer 2 on the opposite side to the outlet 1E TR is the temperature of the heated microwave absorber 3. Carrier gas H Height from point Pl to point Pe h Height of microwave absorber-containing layer 2

Claims

1. The method includes a decomposition step of heating a microwave absorber by microwave irradiation in a reaction vessel provided with a carrier gas inlet and a decomposition gas outlet, and decomposing the fluororesin into a low molecular weight fluorine compound by contacting the heated microwave absorber with a material containing a fluororesin, (i) A method for producing a low-molecular-weight fluorine compound, wherein a temperature difference Δ1 (TR−TI) obtained by subtracting a carrier gas temperature TI (°C) at the inlet from a temperature TR (°C) of the heated microwave absorber is set to be more than 500°C.

2. The method includes a step of heating a microwave absorber by microwave irradiation in a reaction vessel provided with a carrier gas inlet and a decomposition gas outlet, and decomposing the fluororesin into low molecular weight fluorine compounds by contacting the heated microwave absorber with a material containing a fluororesin, (ii) A method for producing a low-molecular-weight fluorine compound, wherein a temperature difference Δ2 (TR-TE) obtained by subtracting a temperature TE (°C) of the generated gas at the outlet of the reaction vessel from a temperature TR (°C) of the heated microwave absorber is set to be 300°C or more.

3. 3. The method according to claim 1, wherein an introduction speed R of the carrier gas from the inlet is 0.005 to 20 m / s.

4. 3. The method according to claim 1, wherein a temperature TE (°C) of the generated gas discharged from the reaction vessel at the outlet is 20°C or higher and lower than 250°C.

5. the microwave absorber is prepared in the form of a microwave absorber-containing layer that contains particles of a material containing the microwave absorber and the fluororesin and is provided so as to pass an airflow from the carrier gas inlet to the decomposition gas outlet, 3. The manufacturing method according to claim 1, wherein, when a center of an opening of the outlet is defined as point Pe and an intersection point between a central axis of the microwave absorber-containing layer and a surface of the microwave absorber-containing layer opposite to the outlet is defined as point Pl, a ratio h / H of a height h of the microwave absorber-containing layer to a height H from point Pl to point Pe is 0.01 to 0.

8.

6. The method according to claim 1 or 2, wherein the microwave absorber has a particle size d of 0.1 to 25 mm.

7. The method according to claim 5, wherein the microwave absorber-containing layer has a height h of 0.1 to 200 mm.

8. The manufacturing method according to claim 2, wherein a temperature difference Δ1 (TR-TI) obtained by subtracting a carrier gas temperature TI (°C) at the inlet from a temperature TR (°C) of the heated microwave absorber is set to be more than 250°C.

Citation Information

Patent Citations

  • Production process of fluoroolefins by thermal decomposition of fluorinated materials

    JP2012504633A

  • Upcycling perfluoropolymers into fluorinated olefins

    WO2021165923A1

  • Method for producing low-molecular-weight fluorine compound

    WO2023210826A1

  • Chemically recycling method

    JP2004346000A

Cited By

  • Method for decomposing fluorine-containing material, and composition

    WO2026182237A1