Molded product

By optimizing the thickness and temperature conductivity of the base material in molded articles with handles, the issue of discoloration in high-temperature environments is addressed, ensuring the handle's appearance is preserved.

JP2024159192APending Publication Date: 2024-11-08TOTO LTD

Patent Information

Application Number
JP2023075031
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Molded articles with handles decorated using sublimable ink are prone to discoloration when exposed to high-temperature environments, such as those encountered in kitchen or bathroom settings, due to inadequate consideration of temperature conductivity and thickness, leading to degradation of the handle's appearance.

Method used

The molded article is designed with a base material that satisfies a specific relationship between thickness (L), temperature conductivity (α), and the temperature (T) at which discoloration occurs, using materials like epoxy, polystyrene, polycarbonate, and glass, ensuring the handle maintains its appearance by suppressing discoloration through controlled heat diffusion.

Benefits of technology

The design effectively prevents handle discoloration in high-temperature conditions, maintaining the original appearance quality and design integrity of the molded article.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159192000001_ABST
    Figure 2024159192000001_ABST
Patent Text Reader

Abstract

To provide a molded product that can prevent the discoloration of a patterned portion even when its surface is exposed to high-temperature environment during use, ensuring that the appearance quality of the patterned portion remains at the same level as its original quality during or after use.SOLUTION: A molded product 1 has a substrate 2. The substrate has a patterned portion 23 including a dye on its back side. The thickness L(m) of the substrate, the temperature conductivity α(m2 / sec) of the substrate, and the temperature T(°C) at which the patterned portion experiences discoloration have the relation represented by formula (1).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a molded article. More specifically, the present invention relates to a molded article having a handle portion on the back side, which is capable of suppressing discoloration of the handle portion even when the front surface is exposed to a high-temperature environment during use. [Background technology]

[0002] Resin molded bodies and glass molded bodies have been used as water-related components such as kitchen and washroom counters and bathtubs in bathrooms. In order to impart design to these water-related components, for example, the back side of the resin molded body or glass molded body is decorated. As a method for such decoration, a dye sublimation transfer method is known.

[0003] For example, JP 2000-1096 A (Patent Document 1) discloses a decoration method characterized by placing a sublimation transfer sheet, on which a predetermined pattern of heat-sublimable decorative material is printed, on the surface of a water-related resin molding to be decorated, and then using a heat press to sublimate the decorative material and cause it to soak into the surface to be decorated, thereby transferring the pattern of the sublimation transfer sheet to the surface to be decorated.

[0004] Furthermore, JP 2000-233598 A (Patent Document 2) discloses a decorated molded body having a colored portion that is colored all the way to the inside of the back side of a transparent base made of synthetic resin, and discloses that the colored portion is obtained by placing a transfer sheet printed with sublimation ink on the back side of the base, and then performing transfer heating in this state to cause the sublimation dye to penetrate into the inside of the base.

[0005] On the other hand, JP 2006-321057 A (Patent Document 3) discloses that when an insulation panel (such as a refrigerator door exterior panel) is produced by sublimation-transferring an ink containing a sublimable dye to a resin layer, permeating the resin layer, forming a pattern on the laminated steel sheet, and subjecting the laminated steel sheet to urethane foaming, the sublimable dye is re-sublimated by the heat of urethane foaming, and discoloration of the pattern caused by the re-sublimation is prevented by raising the glass transition temperature of the resin layer on which the pattern is formed to a temperature equal to or higher than the heat of urethane foaming (see, for example, paragraph 0072). Also, Patent Document 3 discloses that the sublimable dye forming the pattern of the refrigerator door exterior panel produced as described above does not re-sublimate due to heat within the range of the living environment when the panel is used. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2000-1096 A [Patent Document 2] JP 2000-233598 A [Patent Document 3] JP 2006-321057 A Summary of the Invention [Problem to be solved by the invention]

[0007] According to Patent Document 3, during the manufacture of a refrigerator door exterior panel, it is possible to prevent discoloration of a pattern formed with a sublimation ink due to heat of urethane foaming and discoloration of the pattern in a heat environment to which the door exterior panel may be exposed when the refrigerator is used. However, since a refrigerator door exterior panel is not usually placed in a high-temperature environment during use, it is understood that Patent Document 3 does not take into consideration the possibility that the molded body will be placed in a high-temperature environment during use. On the other hand, the present inventors have considered the case where a molded body having a pattern part formed by sublimation ink on the back side is used in a high-heat environment, and have found a new problem that the pattern part once formed (hereinafter referred to as "initial pattern part") discolors due to high heat, and the design of the pattern part is damaged over time. For example, when the molded body is used as a material constituting a water-related part or a part thereof, a pot heated on a stove may be placed on the kitchen counter, and a hair dryer or a curling iron that generates high heat may be placed on the washbasin counter. Therefore, the molded body is exposed to a high-temperature environment during use, and the initial pattern part may discolor due to high heat. Then, the inventors have found that the thermal conductivity, which is a material property specific to the molded body and indicates the degree of ease of heat spread within an object, and the thickness of the molded body are important factors in preventing the pattern part from discoloring due to high heat during use. The present invention is based on such findings.

[0008] Therefore, an object of the present invention is to provide a molded body that is capable of suppressing discoloration of the handle even when the surface is exposed to a high-temperature environment during use, and that is capable of maintaining the appearance quality of the handle during or after use at the same level as the initial appearance quality of the handle. [Means for solving the problem]

[0009] The molded body according to the present invention is A substrate is provided, The substrate has a pattern portion containing a dye on a back side thereof, The thickness L (m) of the substrate and the thermal conductivity α (m 2 / sec) and the temperature T (°C) at which discoloration occurs in the handle portion, the following formula (1):

number

[0010] According to the present invention, a molded article is provided which is capable of suppressing discoloration of the handle even when the surface is exposed to a high-temperature environment during use, and which is capable of maintaining the appearance quality of the handle during or after use at the same level as the initial appearance quality of the handle. [Brief description of the drawings]

[0011] [Figure 1] 1A is a schematic cross-sectional view showing an example of a molded body according to the present invention, and FIG. 1B is a schematic cross-sectional view showing an example of a substrate provided in the molded body according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Molded body The molded body according to the present invention will be described with reference to Fig. 1. As shown in Fig. 1(a), the molded body 1 according to the present invention includes a substrate 2. In the present invention, the molded body 1 may be made of the substrate 2. The substrate 2 may be a single layer or a laminate made of multiple layers. The molded body 1 may include a back surface layer 3 on the back surface 22 of the substrate 2 as shown in Fig. 1(a).

[0013] Base material As shown in Fig. 1(b), the substrate 2 has a pattern portion 23 containing a dye on its back side. The pattern portion 23 is capable of expressing a desired pattern. The molded body 1 is capable of expressing various patterns by having the pattern portion 23. The pattern portion 23 contains one or more types of dye at predetermined positions, making it possible to express various patterns.

[0014] In the present invention, the thickness of the substrate 2 is L (m), and the thermal conductivity of the substrate 2 is α (m 2 / sec) and the temperature at which the color of the handle portion 23 of the base material 2 changes is T (°C), the following formula (1) is satisfied between L, α, and T:

number

[0015] In the present invention, the substrate 2 may be any substrate that allows the sublimation dye to penetrate from the back surface 22 to the inside to a desired depth 24 when the sublimation ink containing the dye printed on the transfer paper is sublimation-transferred to the back surface 22 of the substrate 2. Examples of such substrates include one or more selected from epoxy resin, polystyrene resin, polycarbonate resin, urea resin, melamine resin, (meth)acrylic resin, unsaturated polyester resin, polyester resin, and a glass molded body that has been processed to allow the sublimation ink to penetrate.

[0016] Thickness In the present invention, the thickness L (m) of the base material 2 is set to satisfy the above formula (1) by adjusting the thermal conductivity α (m 2 The thickness L (m) of the base material 2 is determined taking into consideration the temperature T (° C.) at which discoloration occurs in the handle portion and the time required for the resin to be removed (single-sided resin). The thickness L (m) of the base material 2 is, for example, preferably 1 mm or more and 20 mm or less, and more preferably 5 mm or more and 15 mm or less. The thickness L of the substrate 2 can be measured using a known measuring device. For example, a vernier caliper can be used as the measuring device. For example, Mitutoyo Corporation's ABS Digimatic Caliper CD-AX can be used as the vernier caliper.

[0017] Thermal Diffusivity In the present invention, the thermal conductivity α(m 2 / sec) is determined taking into consideration the thickness L (m) of the substrate described above and the temperature T (°C) at which discoloration occurs in the handle portion described below, so as to satisfy the above formula (1). The thermal conductivity of the substrate is the value obtained by dividing the thermal conductivity of the substrate by the density and specific heat of the substrate, and is also called the thermal diffusivity or thermal diffusivity. When the substrate is a single layer, the thermal conductivity of the substrate is the value obtained by dividing the thermal conductivity of the substrate by the density and specific heat of the substrate. When the substrate is a laminate consisting of multiple (i) layers, the thermal conductivity of the substrate is the value obtained by dividing the thermal conductivity λ of the following laminate by the density and specific heat of the following laminate. Here, in the case of a laminate in which each layer is laminated in the plane direction, the thermal conductivity λ of the laminate is expressed as λ = f1 × λ1 + f2 × λ2 + f i ×λ i (In the formula, f i represents the volume ratio of each layer, and λ i represents the thermal conductivity of each layer.) On the other hand, in the case of a laminate in which each layer is stacked in the stacking direction (perpendicular to the surface direction), the thermal conductivity λ of the laminate is 1 / λ=f1×1 / λ1+f2×1 / λ2+···+f i ×1 / λ i The specific heat Cp of the laminate can be calculated as follows: Cp = Cp1 × f1 + Cp2 × f2 + ··· Cp i ×f i (In the formula, Cp i represents the specific heat of each layer. The density d of the laminate can be calculated as follows: d = d1 × f1 + d2 × f2 + d i ×f i (In the formula, d i represents the density of each layer. In the present invention, the thermal conductivity α(m 2 / sec) is, for example, 0.7×10 -7 m 2 / sec or more 15m 2 / sec or less. More preferably, it is 1.1×10 -7 m 2 / sec or more 6.6×10 -7 m 2 / sec or less.

[0018] <Thermal conductivity> In the present invention, the thermal conductivity (W / m·K) of the substrate can be measured using a thermal conductivity measuring device based on ASTM D2326.

[0019] <density> In the present invention, the density of the substrate (kg / m 3 ) can be measured using a precision balance based on JIS Z 8807:2012.

[0020] <Specific heat> In the present invention, the specific heat (J / kg·K) of the base material can be determined by a heat flux differential scanning calorimetry (power compensation DSC) test method using a differential scanning calorimeter.

[0021] Temperature at which discoloration occurs on the handle In the present invention, the temperature T (°C) at which the handle portion 23 changes color is determined by the thickness L (m) of the base material 2 and the thermal conductivity α (m 2 In the present invention, the temperature at which discoloration occurs in the pattern portion is determined by the color difference ΔE * ab is defined as the temperature at which the temperature exceeds 0.6.

[0022] <Temperature evaluation test for discoloration of handle> The test is carried out according to the following procedure, and the temperature at which the handle changes color is evaluated. (1) Store the substrate test pieces in a constant temperature incubator (Yamato Scientific Co., Ltd.) for 72 hours at temperatures of 60°C, 70°C, 80°C, 90°C, and 100°C. (2) Using a spectrophotometer (CM-5, manufactured by Konica Minolta, D65 light source, 2° field of view, transmission method), measure the color of the test piece stored under the conditions in (1). Specifically, the color measurement value (L1 * , a1 * , b1 * After the test, the color measurement value (L2 * , a2 * , b2 *From these color measurement values, the color difference ΔE of the test piece before and after the test is calculated. * ΔE * ab =[(L1 * -L2 * ) 2 +(a1 * -a2 * )2+(b1 * -b2 * ) 2 ] 1 / 2 The calculated ΔE * ab The temperature at which discoloration occurs in the handle is determined as the temperature at which the color exceeds 0.6. In the present invention, the temperature T (° C.) at which discoloration occurs in the handle portion 23 is, for example, preferably 60° C. or higher, and more preferably 80° C. or higher.

[0023] Insulation (heat resistance) As already explained, in the molded product 1 according to the present invention, since the base material 2 satisfies the condition represented by the above formula (1), discoloration of the handle due to heat can be effectively suppressed even when the surface is exposed to a high-temperature environment during use. This effect can be more easily achieved if the base material 2 has good thermal insulation properties (heat resistance). In the present invention, the thermal insulation properties of the base material 2 can be expressed as an index using the back surface temperature reached as measured by the following oil pan test.

[0024] <Oil pan test> The oil pan test is carried out according to the procedure described below in accordance with JIS K 6902:2007, 8.2 Method B, 8.2.4 Procedure, and the temperature reached on the back side of the formed body 1 is measured. (1) The wooden insulation board, the thermocouple (for measuring temperature), and the test piece of the base material (depth 120 mm × width 50 mm) (with the handle 23 facing down) are stacked and adhered in that order. The thermocouple is placed between the test piece and the wooden insulation board at a position on the test piece that is 60 mm deep × 25 mm wide. (2) Place approximately 500 mL of vegetable oil in a flat-bottom aluminum container (outer diameter 130 to 160 mm) and heat the oil using a heating device until the temperature reaches 200°C. (3) A heated aluminum container is placed on the test piece, and the back surface temperature of the test piece is measured with a thermocouple for 20 minutes. (4) The maximum temperature on the back side of the test piece within 20 minutes shall be the temperature reached on the back side of the substrate. In the present invention, the temperature reached by the rear surface of the substrate 2 is preferably 60°C or higher and lower than 108°C, and more preferably 60°C or higher and lower than 100°C.

[0025] transparency In the present invention, the substrate 2 is preferably transparent. In the present invention, "having transparency" refers to a state or property in which the color, shape, pattern, etc. of the pattern of the pattern part 23 on the back side of the substrate 2 can be seen through when the molded body 1 is viewed from the front side (from above). When the substrate 2 has transparency, visible light can pass through the substrate 2, so that the color, shape, pattern, etc. of the pattern of the pattern part 23 on the back side 22 can be visually recognized as if they are floating up. That is, when the molded body 1 is observed from the front side, the presence of a transparent part on the front side and the presence of the pattern part 23 on the back side allows the molded body 1 to exhibit a design property in which the pattern of the pattern part 23 is floating up, and the appearance can be maintained well. Within the range in which such an action and effect can be achieved, the substrate 2 may be semi-transparent.

[0026] The substrate 2 may be colored as long as it is transparent or translucent. When a colored substrate 2 is used, the coloring material and the dye contained in the pattern portion 23 can be distinguished by observation with an optical microscope or the like.

[0027] The transparency of the substrate 2 can also be quantitatively expressed, for example, the total light transmittance can be used as an index. For example, the transparency of the substrate is preferably such that the total light transmittance is 90% or more when the substrate has a thickness of about 10 mm and the arithmetic mean surface roughness Ra of the front and back surfaces of the substrate is about 0.3 μm or less. The total light transmittance of the substrate can be measured, for example, based on JIS K 7375-2008. For example, a haze meter can be used as the measuring device. For example, haze-gard i (manufactured by BYK) can be used as the haze meter.

[0028] In the present invention, the substrate 2 is preferably a sheet or plate having a predetermined thickness, and more preferably a plate.

[0029] When the substrate 2 contains a (meth)acrylic resin, a (meth)acrylic resin prepared by polymerizing a monomer such as methyl methacrylate, or a commercially available (meth)acrylic resin sheet can be used as the substrate 2. For example, Paraglass, Comoglass, and Kurarex manufactured by Kuraray Co., Ltd., Acrylite (L, S, EX, etc.) manufactured by Mitsubishi Chemical Corporation, Kanaselite manufactured by Kanase Co., Ltd., Acryace manufactured by JSP Corporation, and acrylic sheet manufactured by Acrysundae Co., Ltd. can be suitably used.

[0030] When the substrate 2 contains an unsaturated polyester resin, for example, a commercially available unsaturated polyester resin plate or an unsaturated polyester resin plate obtained by curing a commercially available unsaturated polyester resin precursor, such as Sandoma manufactured by DIC Corporation, with an appropriate curing agent can be suitably used as the substrate 2.

[0031] When the substrate 2 contains a polyester resin, for example, commercially available polyester resin plates such as Petec manufactured by Takiron C.I. Co., Ltd. and Sunday PET manufactured by Acri Sunday Co., Ltd., and polyester resin plates obtained by polymerizing polyester precursors such as polycarboxylic acid and polyol can be suitably used as the substrate 2.

[0032] When the substrate 2 contains a polystyrene resin, for example, a commercially available resin plate such as a polystyrene plate manufactured by Acrisanday Co., Ltd., or a polystyrene resin plate obtained by polymerizing a styrene monomer or the like can be suitably used as the substrate 2.

[0033] When the substrate 2 contains a polycarbonate resin, for example, commercially available polycarbonate resins such as Toughlon manufactured by Idemitsu Kosan Co., Ltd. and Panlite manufactured by Teijin Limited, and polycarbonate resin plates obtained by polycondensation reaction of bisphenol A and phosgene can be suitably used as the substrate 2.

[0034] When the substrate 2 contains an epoxy resin, a commercially available epoxy resin plate, a general-purpose bisphenol A diglycidyl ether, or an epoxy resin plate obtained by curing, with an appropriate curing agent, hydrogenated bisphenol A diglycidyl ether, a bisphenol-type epoxy resin obtained from a dihydric phenol such as bisphenol F and epichlorohydrin, a cyclic aliphatic epoxy resin, a glycidyl ester-type epoxy resin, a glycidyl ether-type epoxy resin of a long-chain polyol, a novolac-type epoxy resin, a polyolefin-type epoxy resin, or the like, can be suitably used as the substrate 2.

[0035] When the substrate 2 includes a glass molded body, the substrate 2 may preferably be glass coated with a transparent resin or a multi-layer structure including a glass layer and a resin layer.

[0036] In the present invention, the midpoint glass transition temperature (Tmg) of the substrate 2 is preferably 60° C. or more and 240° C. or less. A substrate with a Tmg within the above range has high heat resistance, and therefore can maintain a good appearance of the molded body 1. The Tg of the substrate 2 is more preferably 100° C. or more and 180° C. or less. The midpoint glass transition temperature (Tmg) of the substrate can be determined by a heat flux differential scanning calorimetry (heat flux DSC) method using a differential scanning calorimeter.

[0037] In the present invention, the arithmetic mean surface roughness (Ra) of the surface 21 of the substrate is preferably 0.2 μm or less. This can prevent a decrease in total light transmittance due to diffuse transmission caused by scratches on the surface. The Ra of the surface 21 of the substrate means the definition described in JIS B0601-2013, and can be measured based on JIS B0633-2001. For example, a surface roughness meter (Tokyo Seimitsu Co., Ltd.) can be used as a measuring instrument. Ra can be measured by adjusting the conditions of the measurement length and cutoff wavelength based on JIS B0633-2001.

[0038] dye In the present invention, the pattern portion 23 contains a dye. The dye contained in the pattern portion 23 is preferably a sublimable dye. As the sublimable dye, a known dye can be used, for example, a sublimable disperse dye. For example, CI Disperse Yellow 1, 3, 4, 5, 7, 8, 31, 33, 39, 42, 54, 60, 61, 64, 83, 124; CI Disperse Red 1, 4, 5, 7, 11, 12, 13, 15, 17, 31, 32, 33, 34, 35, 36, 52, 54, 55, 56, 58, 60, 72, 73, 76, 80, 84, 88, 91, 92, 93, 99, 111, 113, 135, 204, 205, 206, 207, 224, 225, 227, 239, 240; CI Disperse Blue 20, 26, 54, 55, 56, 58, 60, 61, 62, 64, 72, 79, 81, 85, 87, 90, 91, 92, 94, 97, 98, 99, 10.3, 104, 105, 106, 108, 128, 148, 149, 176, 186, 187, 193, 194, 195, 197, 201, 205, 207, 211, 212, 213, 214, 215, 216, 217, 218, 219, 220, 221, 222, 223, 224, 225, 226, 227; C.1. Disperse dyes such as Disperse Black 1, 3, 10, 24 can be used.

[0039] Back layer In the present invention, the molded body 1 may further include other layers in addition to the substrate 2. For example, the molded body 1 may further include a back surface layer 3 on the back surface 22 of the substrate 2, as shown in FIG. 1(a). That is, the molded body 1 may include the substrate 2 and the back surface layer 3 formed on the back surface 22 of the substrate 2.

[0040] The back surface layer 3 preferably contains a resin and a pigment. The resin and pigment may be publicly known or commercially available. As the pigment, one or more selected from inorganic pigments, organic pigments, metal pigments, and pearlescent (pearl) pigments may be used. The pigment contained in the back surface layer 3 is preferably a white pigment. Since the white pigment has a light color, it is possible to improve the visibility of the pattern of the pattern portion 23. That is, since visible light incident from the surface 21 of the substrate 2 is reflected by the back surface layer 3, it is possible to improve the visibility of the color, shape, pattern, etc. of the pattern of the pattern portion 23. In addition, the white pigment can exhibit concealment. Concealment means that, for example, when the molded body 1 is used as a kitchen countertop board, the influence of the counter base can be blocked. This prevents disadvantages such as the appearance of the pattern portion 23 of the molded body 1 being impaired by the color of the base. In addition, in the present invention, the concealment of the back surface layer 3 containing the white pigment, in particular, can prevent the phenomenon of the back surface 22 of the substrate being visible through the back surface 22.

[0041] Uses of the molded body The molded article according to the present invention is preferably used as a material constituting a water-related component or a part thereof, preferably a surface. In the present invention, the water-related component means a component used in a bathroom, a toilet space, a dressing room, a washroom, or a kitchen. Specifically, the molded article can be suitably used as a kitchen counter, a washbasin counter, a bathtub, a kitchen sink, a washbasin, a wall material, a door or panel surface material, etc. In the present invention, it is more preferable that the water-related component is a kitchen counter or a washbasin counter, and the surface of the base material is used as the surface of the kitchen counter or the washbasin counter. In other words, the molded product according to the present invention is preferably used in a state where the surface of the base material is exposed.

[0042] Manufacturing method of molded body The molded article according to the present invention can be produced, for example, by the following method. A preparation step of placing a printed surface of a transfer paper printed with a dye-containing sublimation ink on the back surface of a substrate; a step of hot pressing the transfer paper from the side opposite to the printed side, and allowing the sublimation ink to permeate into the inside of the base material from the back side (sublimation transfer), thereby forming a pattern portion; The composition can be produced by a method comprising the steps of:

[0043] <Preparation> · Base material The substrate is prepared as described above. Sublimation ink A sublimation ink containing a dye is prepared. The dye is as described above. The sublimation ink may contain known ink components in addition to the dye. For example, the sublimation ink may contain a solvent, a dispersant, a surfactant, water, etc. Transfer paper A transfer paper may be prepared using any known sublimation transfer medium.

[0044] <Printing sublimation ink onto transfer paper> The prepared sublimation ink is printed on a transfer paper, preferably by an inkjet printing method.

[0045] <Sublimation transfer onto substrate> The printed side of the transfer paper, on which the dye-containing sublimation ink is printed, is placed on the back side of the prepared substrate. Next, the transfer paper is heat-pressed from the side opposite the printed side. The sublimation ink printed on the transfer paper is sublimation-transferred by the heat press. That is, the dye contained in the sublimation ink permeates into the substrate from the back side 22. In the present invention, the heat press can be performed, for example, at a temperature of 100 to 180°C, for 5 to 20 minutes, and at a pressure of 0.7 MPa. The dye is then fixed in the substrate, and the pattern portion 23 is obtained. In this manner, the molded body 1 can be obtained.

[0046] <Formation of back layer> In the present invention, a back surface layer 3 may be formed on the back surface 22 of the substrate 2. The back surface layer 3 can be formed, for example, as follows. Preferably, the entire back surface of the substrate is degreased using an appropriate solvent. Then, a resin composition containing a pigment is applied to the back surface of the substrate. As the resin composition, for example, a resin composition containing a known heat- or light-curing type resin component can be used. The coating can be performed using a known coating method and coating device. After coating, the resin composition can be cured at an appropriate temperature to form a back surface layer. EXAMPLES

[0047] The present invention will be described in detail based on the following examples, but the present invention is not limited to these examples.

[0048] preparation 1. Base material A total of seven types of substrates were prepared, each of the three types below, and had a thickness (mm) as shown in Table 1. Epoxy resin base material Midpoint glass transition temperature is 122°C, thermal conductivity is 0.172 W / m K, and density is 1176 kg / m 3 It has a specific heat of 1098 J / (kg·K) and is a colorless, transparent solid at room temperature. When its thickness was 12 mm, the total light transmittance was 91% when the arithmetic mean surface roughness Ra of the front side was 0.022 μm and that of the back side was 0.18 μm. Acrylic resin Midpoint glass transition temperature is 118°C, thermal conductivity is 0.197 W / m K, and density is 1185 kg / m 3 It has a specific heat of 1193 J / (kg K) and is a colorless, transparent solid at room temperature. When its thickness was 11 mm, the total light transmittance was 93% when the arithmetic mean surface roughness Ra of the front side was 0.0059 μm and that of the back side was 0.0041 μm. PVC resin Midpoint glass transition temperature is 68°C, thermal conductivity is 0.181 W / m K, and density is 1386 kg / m 3 It has a specific heat of 948 J / (kg·K) and is a colorless, transparent solid at room temperature. When its thickness was 10 mm, the total light transmittance was 80% when the arithmetic mean surface roughness Ra of the front side was 0.0071 μm and the Ra of the back side was 0.0073 μm.

[0049] <Thickness measurement> The thickness of each substrate was measured using a caliper (Mitutoyo Corporation ABS Digimatic Caliper CD-AX). The results are shown in Table 1.

[0050] <Measurement of midpoint glass transition temperature> The midpoint glass transition temperature (Tmg) of each substrate was determined by a heat flux differential scanning calorimetry (heat flux DSC) test method using a differential scanning calorimeter (Rigaku Co., Ltd.) For the measurement sample of the midpoint glass transition temperature, about 10 mg of each substrate was placed in an aluminum non-sealed container and heated to 220°C at a heating rate of 10°C per minute in a nitrogen gas (40 ml per minute) flow.

[0051] <Thermal conductivity> The thermal conductivity (W / m K) of each substrate was measured using a thermal conductivity measuring device (Kyoto Electronics Manufacturing Co., Ltd.) in accordance with ASTM D2326. The results are shown in Table 1.

[0052] <density> Density of each base material (kg / m 3 ) was measured using a precision balance (Sartorius) in accordance with JIS Z 8807: 2012. The results are shown in Table 1.

[0053] <Specific heat> The specific heat (J / kg K) of each substrate was determined by heat flux differential scanning calorimetry (power compensation DSC) using a differential scanning calorimeter (PerkinElmer). For the specific heat measurement sample, approximately 5 to 15 mg of each substrate was placed in an aluminum non-sealed container and heated from 20°C to 100°C at a heating rate of 10°C per minute in a nitrogen gas (20 ml per minute) flow. The value at 25°C was used as the specific heat of the substrate. The results are shown in Table 1.

[0054] <Measurement of total light transmittance> The total light transmittance of each substrate was measured using a haze meter (Hazeguard i, manufactured by BYK, D65 light source) based on JIS K 7375-2008.

[0055] <Measurement of arithmetic mean surface roughness (Ra)> The arithmetic mean surface roughness (Ra) of the front and back surfaces of each substrate was measured using a surface roughness meter (Tokyo Seimitsu Co., Ltd.) based on JIS B0601-2013 and JIS B0633-2001. The measurement conditions based on JIS B0633-2001 were measurement length: 4 mm, measurement speed: 0.3 mm, and cutoff wavelength: 0.8 mm.

[0056] 2. Sublimation ink Four types of sublimation ink were prepared: cyan, magenta, yellow, and black.

[0057] Preparation of test pieces for compacts <Printing sublimation ink onto transfer paper> Six colors of sublimation ink (cyan ink, light cyan ink, magenta ink, light magenta ink, yellow ink, black ink) were printed on inkjet sublimation transfer paper using an inkjet printer to obtain a pattern. 2The print volume per ink was 0.05cc of light cyan ink, 0.30cc of cyan ink, 0.27cc of light magenta ink, 0.12cc of magenta ink, 0.05cc of yellow ink, and 0.01cc of black ink. In other words, the proportion of the print volume of each ink was 6% for light cyan ink, 38% for cyan ink, 33% for light magenta ink, 15% for magenta ink, 6% for yellow ink, and 2% for black ink.

[0058] <Sublimation transfer onto substrate> The surface of the transfer paper on which the pattern was printed was placed against the back surface of each substrate, and the transfer paper was heat-pressed from its back surface (the surface opposite to the surface on which the pattern was printed). The heat-pressing was performed at a temperature of 100 to 180°C for a time of 5 to 20 minutes under a pressure of 0.7 MPa. In this manner, molded articles of Examples 1 to 5 and Comparative Examples 1 and 2 in which the pattern was sublimation-transferred were produced.

[0059] evaluation The following properties were evaluated for each molded article.

[0060] <Thermal diffusivity> The thermal conductivity of each molded body (i.e., each substrate) was calculated by dividing the thermal conductivity of the substrate by the density and specific heat of the substrate. The results are shown in Table 1.

[0061] <Temperature reached on back side> The temperature reached on the back surface of each molded body (i.e., each substrate) was measured by carrying out the following oil pan test. The oil pan test was carried out according to the procedure described below, based on the description of JIS K 6902:2007, 8.2 Method B, 8.2.4 Procedure. Oil pan test (1) A wooden insulation board, a thermocouple (for measuring temperature), and a test piece of each substrate (depth 120 mm × width 50 mm, thickness as shown in Table 1) (with handle 23 facing down) were stacked and adhered in this order. The thermocouple was placed between the test piece and the wooden insulation board at a position of "depth 60 mm × width 25 mm" on the test piece. (2) Approximately 500 mL of vegetable oil was placed in a flat-bottom aluminum container (outer diameter 130 to 160 mm) and heated using a heating device until the oil temperature reached 200°C. (3) A heated aluminum container was placed on the test piece, and the back surface temperature of the test piece was measured with a thermocouple for 20 minutes. (4) The maximum temperature on the back side of the test piece during the 20 minutes was taken as the temperature reached on the back side of the substrate. The results are shown in Table 1.

[0062] <Temperature at which the handle discolors> The temperature at which discoloration occurred in the pattern of each molded product (i.e., each substrate) was determined by carrying out the following evaluation test for temperature at which discoloration of the pattern occurred. Temperature evaluation test for discoloration of the handle (1) Test pieces of each substrate (50 to 100 mm square, thickness as shown in Table 1) were stored in a constant temperature incubator (Yamato Scientific Co., Ltd.) at temperatures of 60°C, 70°C, 80°C, 90°C, and 100°C for 72 hours. (2) The test pieces stored under the conditions in (1) were measured using a spectrophotometer (CM-5, manufactured by Konica Minolta, D65 light source, 2° field of view, transmission method). Specifically, the color measurement value (L1 * , a1 * , b1 * After the test, the colorimetric value of the test piece (L2 * , a2 * , b2 * From these colorimetric values, the color difference ΔE * ΔE * ab =[(L1 * -L2 * ) 2 +(a1 * -a2 * )2+(b1 * -b2 * ) 2 ] 1 / 2 The calculated ΔE * ab The temperature at which discoloration occurs in the handle was determined to be the temperature at which the color exceeds 0.6. The results are shown in Table 1.

[0063] <Overall rating> In each molded body, the thickness L of the substrate, the thermal conductivity α of the substrate, and the temperature T at which discoloration occurs in the handle portion are related to the following formula (1):

number

[0064] [Table 1] [Explanation of symbols]

[0065] 1: Molded body 2: Base material 21: Surface of the substrate 22: Back side of the substrate 23: Handle 24: Thickness of handle 25: Top surface of handle L: thickness of substrate 3: Back layer

Claims

1. A molded article including a substrate, The substrate has a pattern portion containing a dye on a back side thereof, The thickness L (m) of the substrate and the thermal conductivity α (m 2 / sec) and a temperature T (° C.) at which discoloration occurs in the handle portion, the following formula (1): [0010] A molded body in which the relationship expressed by the following formula holds true.

2. The molded article according to claim 1 , wherein the substrate is transparent or translucent.

3. The molded article according to claim 1 or 2, which is used as a material constituting a water-related component or a part thereof.

4. The molded article according to claim 3 , wherein the water-related component is a kitchen counter or a washbasin counter, and the surface of the base material is used as the surface of the kitchen counter or the washbasin counter.

5. The molded article according to claim 4, wherein the substrate has a midpoint glass transition temperature (Tmg) of 60°C or more and 240°C or less.

6. The molded article according to claim 5 , wherein the substrate has a midpoint glass transition temperature (Tmg) of 100° C. or more and 180° C. or less.

7. The molded article according to claim 4, wherein the substrate has a total light transmittance of 90% or more when the substrate has a thickness of 10 mm.

8. The molded article according to claim 1 or 2, further comprising a back surface layer on a back surface of the substrate.

Citation Information

Patent Citations

  • Decorative acrylic sheet and method of manufacturing the same

    JP2003220672A

  • Decorating method of water supply system resin molded form made by sublimation transferring method

    JP2000001096A

  • Decorative molded article, and its manufacture

    JP2000233598A

  • Laminated steel sheet with temporary display layer for sublimation transfer and its manufacturing method

    JP2006321057A

Cited By

  • Handrail device and work machine comprising same

    US12434947B2