Ceramic electronic component
The ceramic electronic component addresses crack issues by controlling continuity rate differences and standard deviations in internal electrode layers, ensuring high adhesion and voltage resistance in compact designs.
Patent Information
- Application Number
- JP2023075094
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
As ceramic electronic components, such as multilayer ceramic capacitors, become smaller and denser, increasing the continuity rate of internal electrode layers leads to decreased adhesion at the dielectric and electrode interfaces, causing cracks and electrostrictive phenomena that reduce breakdown and withstand voltages.
A ceramic electronic component with a laminated structure where internal electrode layers are alternately drawn out to end faces, maintaining specific continuity rate differences and standard deviations to alleviate stress and suppress crack formation.
The proposed structure effectively suppresses cracks and enhances adhesion, maintaining high breakdown and withstand voltages while supporting small size and large capacity.
Smart Images

Figure 2024159239000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a ceramic electronic component. [Background technology]
[0002] In recent years, with the miniaturization and increased density of electronic devices, ceramic electronic components such as multilayer ceramic capacitors (see, for example, Patent Documents 1 to 6) are also required to be smaller and have higher capacitance. In order to increase the capacitance of a multilayer ceramic capacitor, it is necessary to increase the intersection area of the internal electrode layers, and it is effective to increase the continuity rate of the internal electrode layers. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-164446 A [Patent Document 2] Patent Publication No. 2021-086972 [Patent Document 3] JP 2015-111651 A [Patent Document 4] JP 2017-103262 A [Patent Document 5] JP 2013-89944 A [Patent Document 6] JP 2015-053526 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, as the continuity rate of the internal electrode layers increases, the adhesive strength at the interface between the dielectric layers and the internal electrode layers decreases, and cracks such as delamination may occur due to internal stress caused by shrinkage differences during firing. In addition, electrostriction (reverse piezoelectric phenomenon) occurs when a voltage is applied to the dielectric layer. Electrostriction is a phenomenon in which mechanical displacement occurs due to expansion in the direction in which an electric field is applied. When electrostriction occurs, cracks may occur in areas with low strength. The occurrence of these cracks causes problems such as a decrease in breakdown voltage and withstand voltage.
[0005] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a ceramic electronic component that can suppress the occurrence of cracks. [Means for solving the problem]
[0006] The ceramic electronic component according to the present invention comprises a laminated structure having a plurality of dielectric layers and a plurality of internal electrode layers provided via the plurality of dielectric layers and alternately drawn out to two end faces opposing each other, and a pair of side margins sandwiching the laminated structure in a third direction perpendicular to a first direction in which the plurality of internal electrode layers oppose each other and a second direction in which the two end faces oppose each other, wherein for at least two adjacent layers of the plurality of internal electrode layers, when the width of the two layers in the third direction is taken as 100%, a continuity difference within a 5% range inward from the side margin side end in the third direction is 20% or more, and in a capacitive section in which the internal electrode layers alternately drawn out to the two end faces oppose each other, a continuity difference between the internal electrode layers within a range of ±20% from the center in the third direction and a range of ±20% from the center in the first direction is within a range of ±10%.
[0007] Another ceramic electronic component according to the present invention comprises a laminated structure having a plurality of dielectric layers and a plurality of internal electrode layers provided via the plurality of dielectric layers and alternately drawn out to two end faces opposing each other, and a pair of side margins sandwiching the laminated structure in a third direction perpendicular to a first direction in which the plurality of internal electrode layers oppose each other and a second direction in which the two end faces oppose each other, wherein, when a width of the plurality of internal electrode layers in the third direction is taken as 100%, a standard deviation of a continuity ratio of each internal electrode layer within a range of 5% inward from the side margin side end in the third direction is greater than a standard deviation of a continuity ratio of each internal electrode layer within a range of ±20% from the center in the third direction and a range of ±20% from the center in the first direction, in a capacitive section in which the internal electrode layers alternately drawn out to the two end faces oppose each other.
[0008] In the above ceramic electronic component, when the width of the multiple internal electrode layers in the third direction is 100%, an average value of the continuity ratio of each internal electrode layer within 5% inward from the side margin end in the third direction may be smaller than an average value of the continuity ratio of each internal electrode layer within a range of ±20% from the center in the third direction and a range of ±20% from the center in the first direction in the capacitive section.
[0009] In the above ceramic electronic component, when the width of the multiple internal electrode layers in the third direction is 100%, a continuity ratio of the multiple internal electrode layers may differ for each layer within a range of 5% inward from the side margin end in the third direction.
[0010] The ceramic electronic component according to the present invention comprises a laminated chip having a substantially rectangular parallelepiped shape, the laminated chip having a plurality of dielectric layers and a plurality of internal electrode layers provided via the plurality of dielectric layers and alternately drawn out to two end faces opposing each other in a second direction, the laminated chip having end margins where internal electrode layers exposed on the same end face face each other without an internal electrode layer exposed on a different end face therebetween, and for at least two adjacent layers of the plurality of internal electrode layers, when the length of the two layers in the second direction is taken as 100%, a continuity difference within a range of 5% inward from the end margin side in the second direction is 15% or more, and in a capacitive section in which the internal electrode layers alternately drawn out to the two end faces face each other, a continuity difference between the internal electrode layers within a range of ±20% from the center in the second direction and within a range of ±20% from the center in the first direction in which the plurality of internal electrode layers face each other is within a range of ±10%.
[0011] Another ceramic electronic component according to the present invention comprises a laminated chip having a substantially rectangular parallelepiped shape, the laminated chip having a plurality of dielectric layers and a plurality of internal electrode layers provided via the plurality of dielectric layers and alternately drawn out to two end faces opposing each other in a second direction, the laminated chip having end margins where internal electrode layers exposed on the same end face face each other without an internal electrode layer exposed on a different end face therebetween, and when the length of the plurality of internal electrode layers in the second direction is taken as 100%, the standard deviation of the continuity ratio of each internal electrode layer in a range of 5% inward from the end margin side end in the second direction is greater than the standard deviation of the continuity ratio of each internal electrode layer in a range of ±20% from the center in the second direction and in a range of ±20% from the center in the first direction in which the plurality of internal electrode layers face each other, in a capacitive section in which the internal electrode layers alternately drawn out to the two end faces face each other.
[0012] In the above ceramic electronic component, when the length of the multiple internal electrode layers in the second direction is 100%, an average value of the continuity ratio of each internal electrode layer within a range of 5% inward from the end margin side end in the second direction may be smaller than an average value of the continuity ratio of each internal electrode layer in the capacitive section within a range of ±20% from the center in the second direction and within a range of ±20% from the center in the first direction.
[0013] In the above ceramic electronic component, when a length of the plurality of internal electrode layers in the second direction is taken as 100%, a continuity ratio of the plurality of internal electrode layers may differ for each layer within a range of 5% inward from the end margin side end in the second direction. Effect of the Invention
[0014] According to the present invention, it is possible to provide a ceramic electronic component capable of suppressing the occurrence of cracks, and a method for manufacturing the same. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a partial cross-sectional perspective view of a multilayer ceramic capacitor. [Diagram 2] 2 is a cross-sectional view taken along line AA in FIG. 1. [Diagram 3] FIG. 2 is a cross-sectional view taken along line BB in FIG. [Figure 4] FIG. 4 is an enlarged cross-sectional view of the vicinity of an external electrode. [Diagram 5] FIG. 13 is a diagram illustrating a continuity rate. [Figure 6] (a) and (b) are TW cross sections of a multilayer ceramic capacitor. [Figure 7] This is an LT cross section of a multilayer ceramic capacitor. [Figure 8] 1A to 1C are diagrams illustrating a flow of a method for manufacturing a multilayer ceramic capacitor. [Figure 9] 11A to 11C are diagrams illustrating an internal electrode forming step. [Figure 10] FIG. 1 is a diagram illustrating an example of an SEM photograph. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment will be described with reference to the drawings.
[0017] (Embodiment) FIG. 1 is a partial cross-sectional perspective view of a multilayer ceramic capacitor 100 according to an embodiment. FIG. 2 is a cross-sectional view taken along line AA in FIG. 1. FIG. 3 is a cross-sectional view taken along line BB in FIG. 1. As illustrated in FIGS. 1 to 3, the multilayer ceramic capacitor 100 includes a laminated chip 10 having a substantially rectangular parallelepiped shape, and external electrodes 20a, 20b provided on any two opposing end faces of the laminated chip 10. Of the four faces of the laminated chip 10 other than the two end faces, the two faces other than the top and bottom faces in the stacking direction are referred to as side faces. The external electrodes 20a, 20b extend on the top, bottom and two side faces in the stacking direction of the laminated chip 10. However, the external electrodes 20a, 20b are spaced apart from each other.
[0018] 1 to 3, the T-axis direction (first direction) is the stacking direction, and is the direction in which the internal electrode layers face each other. The L-axis direction (second direction) is the length direction of the laminated chip 10, and is the direction in which the two end faces of the laminated chip 10 face each other, and in which the external electrodes 20a and 20b face each other. The W-axis direction (third direction) is the width direction of the internal electrode layers, and is the direction in which the two side faces other than the two end faces of the four side faces of the laminated chip 10 face each other. The T-axis direction, the L-axis direction, and the W-axis direction are mutually perpendicular.
[0019] The laminated chip 10 has a configuration in which dielectric layers 11 containing a ceramic material that functions as a dielectric and internal electrode layers are alternately laminated. The internal electrode layers include a plurality of first internal electrode layers 12a and a plurality of second internal electrode layers 12b. The first internal electrode layers 12a and the second internal electrode layers 12b are alternately laminated. The edge of the first internal electrode layer 12a is drawn to a first end surface on which the external electrode 20a of the laminated chip 10 is provided. The edge of the second internal electrode layer 12b is drawn to a second end surface on which the external electrode 20b of the laminated chip 10 is provided. Thereby, the first internal electrode layer 12a and the second internal electrode layer 12b are alternately conductive to the external electrode 20a and the external electrode 20b. As a result, the laminated ceramic capacitor 100 has a configuration in which capacitor units are laminated. In the laminate of the dielectric layers 11 and the internal electrode layers, the internal electrode layers are disposed on the outermost layers in the lamination direction, and the upper and lower surfaces of the laminate are covered with cover layers 13. The cover layers 13 are mainly composed of a ceramic material. For example, the cover layers 13 may have the same composition as the dielectric layers 11 or may have a different composition.
[0020] The size of the multilayer ceramic capacitor 100 is, for example, 0.25 mm long, 0.125 mm wide, and 0.125 mm high, or 0.4 mm long, 0.2 mm wide, and 0.2 mm high, or 0.6 mm long, 0.3 mm wide, and 0.3 mm high, or 1.0 mm long, 0.5 mm wide, and 0.5 mm high, or 3.2 mm long, 1.6 mm wide, and 1.6 mm high, or 4.5 mm long, 3.2 mm wide, and 2.5 mm high, but is not limited to these sizes. However, since it is believed that larger products are more effective in suppressing cracks, it is better if the size is 3.2 mm long and 1.6 mm wide or more.
[0021] The first internal electrode layer 12a and the second internal electrode layer 12b are mainly composed of base metals such as nickel (Ni), copper (Cu), and tin (Sn), or alloys thereof. Precious metals such as platinum (Pt), palladium (Pd), silver (Ag), and gold (Au), or alloys containing these metals, may be used as the main components of the first internal electrode layer 12a and the second internal electrode layer 12b. The average thickness per layer of the first internal electrode layer 12a and the second internal electrode layer 12b in the T-axis direction is 2 μm or less. The average thickness per layer of the first internal electrode layer 12a can be measured by observing the cross section of the multilayer ceramic capacitor 100 with a SEM (scanning electron microscope), measuring the thickness at 10 points for each of 10 different first internal electrode layers 12a, and deriving the average value of all the measurement points. The average thickness per layer of the second internal electrode layer 12b can be measured by observing a cross section of the multilayer ceramic capacitor 100 with a SEM (scanning electron microscope), measuring the thickness at 10 points on each of 10 different second internal electrode layers 12b, and deriving the average value of all the measurement points.
[0022] The dielectric layer 11 has a main phase made of a ceramic material having a perovskite structure represented by the general formula ABO3. 3-α For example, the ceramic material includes barium titanate (BaTiO3), calcium zirconate (CaZrO3), calcium titanate (CaTiO3), strontium titanate (SrTiO3), magnesium titanate (MgTiO3), BaTiO3, which forms a perovskite structure, 1-x-y Ca x Sr y Ti 1-z Zr z O3 (0≦x≦1, 0≦y≦1, 0≦z≦1), etc. 1-x-y Ca x Sr y Ti 1-z Zr zO3 is barium strontium titanate, barium calcium titanate, barium zirconate, barium titanate zirconate, calcium titanate zirconate, barium calcium titanate zirconate, etc. For example, the dielectric layer 11 contains 90 at% or more of the main component ceramic. The average thickness of each dielectric layer 11 in the T-axis direction is 10 μm or less. The average thickness of each dielectric layer 11 in the T-axis direction can be measured by observing the cross section of the multilayer ceramic capacitor 100 with a SEM (scanning electron microscope), measuring the thickness at 10 points for each of 10 different dielectric layers 11, and deriving the average value of all the measurement points.
[0023] An additive may be added to the dielectric layer 11. Examples of the additive to the dielectric layer 11 include oxides of zirconium (Zr), hafnium (Hf), magnesium (Mg), manganese (Mn), molybdenum (Mo), vanadium (V), chromium (Cr), and rare earth elements (yttrium (Y), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), and ytterbium (Yb)), or oxides containing cobalt (Co), nickel (Ni), lithium (Li), boron (B), sodium (Na), potassium (K), or silicon (Si), or glasses containing cobalt, nickel, lithium, boron, sodium, potassium, or silicon.
[0024] 2, the region where the first internal electrode layer 12a connected to the external electrode 20a and the second internal electrode layer 12b connected to the external electrode 20b face each other is a region that generates capacitance in the multilayer ceramic capacitor 100. Therefore, the region that generates capacitance is referred to as a capacitance portion 14. In other words, the capacitance portion 14 is a region where adjacent internal electrode layers connected to different external electrodes face each other.
[0025] The region where the first internal electrode layers 12a connected to the external electrodes 20a face each other in the stacking direction without the second internal electrode layer 12b connected to the external electrode 20b being interposed therebetween is called the first end margin 15a. The region where the second internal electrode layers 12b connected to the external electrodes 20b face each other in the stacking direction without the first internal electrode layer 12a connected to the external electrode 20a being interposed therebetween is called the second end margin 15b. Each end margin is a region where the internal electrode layers connected to the same external electrode face each other in the stacking direction without the internal electrode layer connected to a different external electrode being interposed therebetween. The first end margin 15a and the second end margin 15b are regions that do not generate capacitance.
[0026] As illustrated in Fig. 3, in the laminated chip 10, the side margin 16 is a region provided so as to cover the ends (ends in the W-axis direction) of two side surfaces of the laminated structure of the dielectric layer 11, the first internal electrode layer 12a, and the second internal electrode layer 12b. That is, in Fig. 3, the side margin 16 is a region provided outside the capacitive section 14 in the W-axis direction. That is, the side margin 16 is an outer region adjacent to the capacitive section 14 as seen from the lamination direction, and is an outer region adjacent to the capacitive section 14 on the side where the internal electrode layers are not drawn out. The side margin 16 is also a region that does not generate electrical capacitance.
[0027] Fig. 4(a) is an enlarged cross-sectional view of the vicinity of the external electrode 20a. Hatching is omitted in Fig. 4(a). As illustrated in Fig. 4(a), the external electrode 20a has a structure in which a plating layer 22a is provided on an underlayer 21a. The underlayer 21a functions as a contact layer that contacts the first end surface of the laminated chip 10. The underlayer 21a is mainly composed of Ni, Cu, etc. The underlayer 21a may also contain a glass component.
[0028] The plating layer 22a is mainly composed of a metal such as Ni, Cu, Al, Zn, or Sn, or an alloy of two or more of these metals. The plating layer 22a may be a plating layer of a single metal component, or may be a plurality of plating layers of different metal components. For example, in FIG. 4, the plating layer 22a has a structure in which a first plating layer 23a, a second plating layer 24a, and a third plating layer 25a are formed in this order from the underlayer 21a side. The first plating layer 23a is, for example, a Sn plating layer. The second plating layer 24a is, for example, a Ni plating layer. The third plating layer 25a is, for example, a Sn plating layer.
[0029] Fig. 4(b) is an enlarged cross-sectional view of the vicinity of the external electrode 20b. Hatching is omitted in Fig. 4(b). As illustrated in Fig. 4(b), the external electrode 20b has a structure in which a plating layer 22b is provided on an underlayer 21b. The underlayer 21b functions as a contact layer that contacts the second end surface of the laminated chip 10. The underlayer 21b is mainly composed of Ni, Cu, etc. The underlayer 21b may also contain a glass component.
[0030] The plating layer 22b is mainly composed of a metal such as Ni, Cu, Al, Zn, or Sn, or an alloy of two or more of these metals. The plating layer 22b may be a plating layer of a single metal component, or may be a plurality of plating layers of different metal components. For example, the plating layer 22b has a structure in which a first plating layer 23b, a second plating layer 24b, and a third plating layer 25b are formed in this order from the underlayer 21b side. The first plating layer 23b is, for example, a Sn plating layer. The second plating layer 24b is, for example, a Ni plating layer. The third plating layer 25b is, for example, a Sn plating layer.
[0031] The underlayer 21a and the underlayer 21b may have the same composition, or may have different compositions. The plating layer 22a and the plating layer 22b may have the same layered structure, or may have different layered structures. For example, the number of layers of the plating layers may be different. The first plating layer 23a and the first plating layer 23b may have the same composition, or may have different compositions. The second plating layer 24a and the second plating layer 24b may have the same composition, or may have different compositions. The third plating layer 25a and the third plating layer 25b may have the same composition, or may have different compositions.
[0032] In such a structure, in order to realize a small size and large capacity, it is preferable to increase the continuity rate of the first internal electrode layer 12a and the second internal electrode layer 12b to increase the intersection area between the internal electrode layers.
[0033] Here, the continuity ratio will be explained. Fig. 5 is a diagram showing the continuity ratio. As illustrated in Fig. 5, in an observation area of length L0 in the first internal electrode layer 12a or the second internal electrode layer 12b, the lengths L1, L2,..., Ln of the metal parts are measured and summed up, and the ratio of the metal parts, ΣLn / L0, can be defined as the continuity ratio of the layer. The closer this continuity ratio is to 100%, the better the continuity of the internal electrode layer is.
[0034] However, increasing the continuity rate of the first internal electrode layer 12a and the second internal electrode layer 12b may reduce the adhesive strength at the interface between the dielectric layer 11 and the first internal electrode layer 12a or the second internal electrode layer 12b. If the adhesive strength at the interface between the dielectric layer 11 and the internal electrode layer is reduced, cracks such as delamination may occur due to internal stress caused by shrinkage differences during firing.
[0035] In addition, when a voltage is applied to the dielectric layer of a multilayer ceramic capacitor, an electrostrictive phenomenon (reverse piezoelectric phenomenon) occurs. The electrostrictive phenomenon is a phenomenon in which mechanical displacement occurs due to expansion in the direction of application of an electric field. Due to the electrostrictive phenomenon, cracks may occur near the side margin 16, the first end margin 15a, or the second end margin 15b, which have low strength. The occurrence of these cracks may lead to a decrease in breakdown voltage and withstand voltage. It is considered that the larger the product, the more effective it is in suppressing cracks. In general, the larger the product, the greater the amount of deformation due to stress such as electrostriction, and therefore the more likely it is that cracks will occur. The large product referred to here is, for example, a product with a length of 3.2 mm and a width of 1.6 mm or more.
[0036] Therefore, the multilayer ceramic capacitor 100 according to this embodiment has a configuration capable of suppressing various cracks caused by internal stress.
[0037] First, the names of the regions of the capacitance section 14 described in FIG. 2 will be described. FIG. 6(a) and FIG. 6(b) are TW cross sections of the multilayer ceramic capacitor 100. For example, they are TW cross sections at the center in the L-axis direction. As illustrated in FIG. 6(a) and FIG. 6(b), in the capacitance section 14, when the width of the first internal electrode layer 12a and the second internal electrode layer 12b in the W-axis direction is 100%, a region in a range of 5% inward from the side margin 16 side end in the W-axis direction is called the outer region E_W. It is better if the outer region E_W is in a range of 4%. In the capacitance section 14, when the width of the capacitance section 14 in the W-axis direction is 100%, a region in a range of ±20% from the center in the W-axis direction and a region in a range of ±20% from the center in the T-axis direction are called the central region C_W.
[0038] In the outer region E_W, when focusing on at least two adjacent internal electrode layers (the first internal electrode layer 12a and the second internal electrode layer 12b), the continuity difference is 20% or more. For example, the continuity ratio of the first internal electrode layer 12a is 50%, and the continuity ratio of the adjacent second internal electrode layer 12b is 70%. Therefore, in the outer region E_W, internal electrode layers with high continuity ratios and internal electrode layers with low continuity ratios are mixed. Next, in the central region C_W, the continuity difference between the internal electrode layers is within a range of ±10%. Therefore, in the central region C_W, the continuity difference between the internal electrode layers is small. With this configuration, the continuity difference becomes smaller stepwise toward the inside, so that the shrinkage difference during firing is mitigated, the internal stress (shrinkage stress) itself is suppressed, and the occurrence of cracks is suppressed.
[0039] From the viewpoint of increasing the continuity difference in the outer region E_W, when focusing on at least two adjacent internal electrode layers (the first internal electrode layer 12a and the second internal electrode layer 12b), it is preferable that the continuity difference be 25% or more, and more preferably 30% or more.
[0040] On the other hand, if the continuity difference is large, there is a concern that the capacity will decrease due to the decrease in the continuity of the first internal electrode layer 12a. Therefore, it is preferable to set an upper limit on the continuity difference when focusing on at least two adjacent internal electrode layers (the first internal electrode layer 12a and the second internal electrode layer 12b). The continuity difference is preferably 50% or less, more preferably 45% or less, and even more preferably 40% or less.
[0041] For example, in the outer region E_W, when focusing on each two adjacent internal electrode layers (the first internal electrode layer 12a and the second internal electrode layer 12b) except for the two outermost internal electrode layers in the T-axis direction, the continuity difference is preferably 20% or more, more preferably 25% or more, and even more preferably 30% or more. Also, the continuity difference is preferably 50% or less, more preferably 45% or less, and even more preferably 40% or less.
[0042] For example, in the outer region E_W, the difference between the average value of the continuity rate of each first internal electrode layer 12a and the average value of the continuity rate of each second internal electrode layer 12b is preferably 20% or more, more preferably 25% or more, and even more preferably 30% or more.
[0043] From the viewpoint of reducing the variation of each internal electrode layer in the central region C_W, the continuity difference of each internal electrode layer in the central region C_W is preferably within a range of ±8%, and more preferably within a range of ±5%.
[0044] It is preferable that the average value of the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the outer region E_W is smaller than the average value of the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the central region C_W. According to this configuration, the continuity ratios of the internal electrode layers in the outer region E_W close to the side margin 16 are lowered, so that the ceramic ratio is higher in the vicinity of the side margin 16, the strength of the outer region E_W is increased, and the occurrence of cracks is suppressed, and the adhesion between the dielectric layer 11 and each internal electrode layer is increased in the outer region E_W, and delamination is suppressed. In addition, since the average value of the continuity ratios of the internal electrode layers is high in the central region C_W, the ceramic ratio is gradually reduced from the outer region E_W to the central region C_W, and the shrinkage difference during firing is mitigated, the internal stress (shrinkage stress) itself is suppressed, and the occurrence of cracks is suppressed.
[0045] The difference between the average value of the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the central region C_W and the average value of the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the outer region E_W is preferably 10% or more, more preferably 15% or more, and even more preferably 20% or more.
[0046] It is preferable that the variation in the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the outer region E_W is greater than the variation in the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the central region C_W. In this case, while layers with low continuity ratios are provided in the outer region E_W, layers with high continuity ratios are also provided. This makes it possible to suppress a decrease in capacity. For example, it is preferable that the continuity ratios of the internal electrode layers in the outer region E_W are alternately low and high.
[0047] For example, it is preferable that the standard deviation of the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the outer region E_W is greater than the standard deviation of the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the central region C_W.
[0048] Next, the names of the regions of the capacitance section 14 in the LT cross section will be described. FIG. 7 is an LT cross section of the multilayer ceramic capacitor 100. For example, it is an LT cross section at the center in the W-axis direction. As illustrated in FIG. 7, in the capacitance section 14, when the length of the internal electrode layer 12 in the L-axis direction is 100%, a region in a range of 5% inward from the first end margin 15a side end in the L-axis direction and a region in a range of 5% inward from the second end margin 15b side end in the L-axis direction are called outer regions E_L. It is better if the outer region E_L is in a range of 3%. In the capacitance section 14, when the width of the capacitance section 14 in the L-axis direction is 100%, a region in a range of ±20% from the center in the L-axis direction and a region in a range of ±20% from the center in the T-axis direction are called central regions C_L.
[0049] In the outer region E_L, when focusing on at least two adjacent internal electrode layers (the first internal electrode layer 12a and the second internal electrode layer 12b), the continuity difference is 15% or more. For example, the continuity ratio of the first internal electrode layer 12a is 55%, and the continuity ratio of the adjacent second internal electrode layer 12b is 70%. Therefore, in the outer region E_L, internal electrode layers with high continuity ratios and internal electrode layers with low continuity ratios are mixed. Next, in the central region C_L, the continuity difference of each internal electrode layer is within a range of ±10%. Therefore, in the central region C_L, the continuity difference of each internal electrode layer becomes smaller. With this configuration, the continuity difference becomes smaller stepwise toward the inside, so that the shrinkage difference during firing is mitigated, the internal stress (shrinkage stress) itself is suppressed, and the occurrence of cracks is suppressed.
[0050] From the viewpoint of increasing the continuity difference in the outer region E_L, when focusing on at least two adjacent internal electrode layers (the first internal electrode layer 12a and the second internal electrode layer 12b), it is preferable that the continuity difference be 20% or more, and more preferably 25% or more.
[0051] On the other hand, there is a concern that the capacity may decrease due to the decrease in the continuity ratio of the outer region E_L. Therefore, it is preferable to set an upper limit on the continuity ratio difference when focusing on at least two adjacent internal electrode layers (the first internal electrode layer 12a and the second internal electrode layer 12b). The continuity ratio difference is preferably 50% or less, more preferably 45% or less, and further preferably 40% or less.
[0052] For example, in the outer region E_L, when focusing on each two adjacent internal electrode layers (the first internal electrode layer 12a and the second internal electrode layer 12b) except for the two outermost internal electrode layers in the T-axis direction, the continuity difference is preferably 15% or more, more preferably 20% or more, and even more preferably 25% or more. Also, the continuity difference is preferably 50% or less, more preferably 45% or less, and even more preferably 40% or less.
[0053] For example, in the outer region E_L, the difference between the average value of the continuity rate of each first internal electrode layer 12a and the average value of the continuity rate of each second internal electrode layer 12b is preferably 15% or more, more preferably 20% or more, and even more preferably 25% or more.
[0054] From the viewpoint of reducing the variation of each internal electrode layer in the central region C_L, the continuity difference of each internal electrode layer in the central region C_L is preferably within a range of ±8%, and more preferably within a range of ±5%.
[0055] It is preferable that the average value of the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the outer region E_L is smaller than the average value of the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the central region C_L. According to this configuration, the continuity ratios of the internal electrode layers in the outer region E_L close to the first end margin 15a and the second end margin 15b are lowered, so that the ceramic ratio is higher in the vicinity of the first end margin 15a and the second end margin 15b, the strength of the outer region E_L is increased, and the occurrence of cracks is suppressed, and the adhesion between the dielectric layer 11 and each internal electrode layer is increased in the outer region E_L, and delamination is suppressed. In addition, since the average value of the continuity ratios of the internal electrode layers is high in the central region C_L, the ceramic ratio is gradually reduced from the outer region E_L to the central region C_L, and the shrinkage difference during firing is mitigated, the internal stress (shrinkage stress) itself is suppressed, and the occurrence of cracks is suppressed.
[0056] The difference between the average value of the continuity ratio of all the first internal electrode layers 12a and the second internal electrode layers 12b in the central region C_L and the average value of the continuity ratio of all the first internal electrode layers 12a and the second internal electrode layers 12b in the outer region E_L is preferably 10% or more, more preferably 15% or more, and even more preferably 20% or more.
[0057] It is preferable that the variation in the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the outer region E_L is greater than the variation in the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the central region C_L. In this case, while layers with low continuity ratios are provided in the outer region E_L, layers with high continuity ratios are also provided. This makes it possible to suppress a decrease in capacity. For example, it is preferable that the continuity ratios of the internal electrode layers in the outer region E_L are alternately low and high.
[0058] For example, it is preferable that the standard deviation of the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the outer region E_L is greater than the standard deviation of the continuity ratios of all the first internal electrode layers 12a and the second internal electrode layers 12b in the central region C_L.
[0059] Next, a description will be given of a method for manufacturing the multilayer ceramic capacitor 100. FIG 8 is a diagram illustrating a flow of the method for manufacturing the multilayer ceramic capacitor 100.
[0060] (Raw powder production process) First, a dielectric material for forming the dielectric layer 11 is prepared. The A-site elements and B-site elements contained in the dielectric layer 11 are usually contained in the dielectric layer 11 in the form of a sintered body of ABO3 particles. For example, barium titanate is a tetragonal compound having a perovskite structure and exhibits a high dielectric constant. This barium titanate can generally be obtained by synthesizing barium titanate by reacting a titanium raw material such as titanium dioxide with a barium raw material such as barium carbonate. In this embodiment, hydrothermal synthesis is performed in an aqueous solution of barium hydroxide using titanium dioxide having an elliptical or needle shape. This allows the synthesis of a flat-shaped barium titanate powder. In addition, the particle size of the obtained barium titanate powder is made uniform.
[0061] A predetermined additive compound is added to the obtained ceramic powder according to the purpose. Examples of the additive compound include oxides of zirconium, hafnium, magnesium, manganese, molybdenum, vanadium, chromium, rare earth elements (yttrium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, and ytterbium), oxides containing cobalt, nickel, lithium, boron, sodium, potassium, or silicon, or glasses containing cobalt, nickel, lithium, boron, sodium, potassium, or silicon.
[0062] For example, a compound containing an additive compound is wet-mixed with a ceramic raw material powder, and then dried and pulverized to prepare a ceramic material. For example, the ceramic material obtained as described above may be pulverized as necessary to adjust the particle size, or may be combined with a classification process to adjust the particle size. Through the above steps, a dielectric material is obtained.
[0063] (Coating process) Next, a binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer are added to the obtained raw material powder and wet mixed. The obtained slurry is used to coat the dielectric green sheets 51a and 51b on a substrate by, for example, a die coater method or a doctor blade method, and then dried. The substrate is, for example, a polyethylene terephthalate (PET) film. Figures illustrating the coating process are omitted.
[0064] (Internal electrode formation process) Next, as illustrated in FIG. 9, the internal electrode pattern 53 is arranged by printing a metal conductive paste for forming an internal electrode containing an organic binder on the surface of the dielectric green sheet 51a. The internal electrode pattern 53 is composed of an internal electrode pattern 53a and an internal electrode pattern 53b, and the internal electrode pattern 53b indicates a portion where the film thickness is thin. On the surface of the dielectric green sheet 51a, the internal electrode pattern 53 extends to one end in the L-axis direction, but does not extend to the other end. Also, on the surface of the dielectric green sheet 51a, the internal electrode pattern 53 does not extend to both ends in the W-axis direction. Since the internal electrode pattern 53 uses a low-viscosity metal conductive paste, it is easy to wet and spread, and the film thickness around the internal electrode pattern is thin. The internal electrode pattern 53 corresponds to the shape of the first internal electrode layer 12a. The dielectric green sheet 51a on which the internal electrode pattern 53 is arranged is called a first lamination unit.
[0065] Next, the internal electrode pattern 52 is arranged by printing a metal conductive paste for forming an internal electrode containing an organic binder on the surface of the dielectric green sheet 51b. The internal electrode pattern 52 is composed of an internal electrode pattern 52a and an internal electrode pattern 52b, and the internal electrode pattern 52b indicates a portion where the film thickness is thin. On the surface of the dielectric green sheet 51b, the internal electrode pattern 52 extends to the other end in the L-axis direction, but does not extend to one end. Also, on the surface of the dielectric green sheet 51b, the internal electrode pattern 52 does not extend to both ends in the W-axis direction and one end in the L-axis direction. Since the internal electrode pattern 52 uses a metal conductive paste with high viscosity, it has poor wettability, and the film thickness of one end of the internal electrode pattern in the L-axis direction is thin. The internal electrode pattern 52 corresponds to the shape of the second internal electrode layer 12b. The dielectric green sheet 51b on which the internal electrode pattern 52 is arranged is called a second lamination unit.
[0066] The viscosity of the metal conductive paste contained in the internal electrode pattern 52 is set to be higher than the viscosity of the metal conductive paste contained in the internal electrode pattern 53. For example, the viscosity of the metal conductive paste contained in the internal electrode pattern 52 is set to be 10 times or more the viscosity of the metal conductive paste contained in the internal electrode pattern 53.
[0067] Incidentally, on the surface of the dielectric green sheet 51a, a dielectric pattern may be disposed in an area where the internal electrode pattern 52 is not disposed to fill in any steps. On the surface of the dielectric green sheet 51b, a dielectric pattern may be disposed in an area where the internal electrode pattern 53 is not disposed to fill in any steps.
[0068] Thereafter, as illustrated in Fig. 9, the first stacking units and the second stacking units are alternately stacked. For example, the total number of stacked layers is 100 to 500. A predetermined number of cover sheets 54 (for example, 2 to 10 layers) are stacked on the top and bottom of the stack in which the first stacking units and the second stacking units are stacked, and then thermocompression bonded. The cover sheets 54 are also green sheets containing ceramic powder.
[0069] In such a laminate, in the region corresponding to the capacitance section 14, the viscosity of the internal electrode pattern alternates between high and low at both ends in the L-axis direction and both ends in the W-axis direction.
[0070] (Firing process) The ceramic laminate thus obtained was subjected to a binder removal treatment in an N2 atmosphere, after which a metal paste that would become the undercoat layers of the external electrodes 20a and 20b was applied thereto by a dipping method. -12 MPa~10 -9 The mixture is fired in a reducing atmosphere at 1160° C. to 1280° C. (for example, 1180° C. or higher and 1230° C. or lower) under reduced pressure of MPa for 5 minutes to 10 hours.
[0071] (Reoxidation treatment process) In order to return oxygen to barium titanate, which is the partially reduced main phase of the dielectric layer 11 fired in a reducing atmosphere, a heat treatment may be performed in a mixed gas of N2 and water vapor at about 1000°C or in the air at 500°C to 700°C to the extent that the first internal electrode layer 12a and the second internal electrode layer 12b are not oxidized. This process is called a reoxidation treatment process.
[0072] (Plating process) Thereafter, the underlayers of the external electrodes 20a, 20b are plated with a metal coating of copper, nickel, tin, etc. Through the above steps, the multilayer ceramic capacitor 100 is completed.
[0073] According to the manufacturing method of this embodiment, in the laminate of the first and second stacking units, in the region corresponding to the capacitance section 14, the viscosity of the metal conductive paste included in the internal electrode pattern alternates between low and high at both ends in the L-axis direction and both ends in the W-axis direction. As a result, in the capacitance section 14 after firing, the continuity ratio of the internal electrode layer alternates between low and high in the outer region E_L and the outer region E_W. Specifically, in the internal electrode pattern including the metal conductive paste with low viscosity, both ends become thinner, so that the continuity ratio after firing decreases. As a result, in the outer region E_L and the outer region E_W, the continuity difference between the two adjacent internal electrode layers becomes large, and in the central region C_L and the central region C_W, the continuity difference becomes small. The structure of the multilayer ceramic capacitor 100 is obtained by adjusting the viscosity of the metal conductive paste included in the internal electrode pattern. The printing film thickness may be adjusted by changing the design of the printing plate to make both ends of the internal electrode pattern thinner, thereby decreasing the continuity ratio at both ends after firing.
[0074] In Fig. 9, the internal electrode patterns are arranged after cutting each dielectric green sheet, but this is not limited to this. For example, areas corresponding to multiple dielectric green sheets may be formed on a large substrate, internal electrode patterns may be arranged thereon, and the substrate may be cut into individual pieces.
[0075] In the above embodiments, a multilayer ceramic capacitor has been described as an example of a multilayer ceramic electronic component, but the present invention is not limited to this. For example, other multilayer ceramic electronic components such as a varistor or a thermistor may be used. EXAMPLES
[0076] (Example) In the example, a multilayer ceramic capacitor was fabricated according to the manufacturing method of the above embodiment. Specifically, in a laminate of the first and second laminate units, in a region corresponding to the capacitance section 14, the viscosity of the internal electrode pattern was alternately low and high at both ends in the L-axis direction and both ends in the W-axis direction. A total of 654 layers of the first and second laminate units were laminated.
[0077] In the WT cross section, assuming that the width of the internal electrode layer in the W-axis direction is 100%, an outer region E_W in a range of 5% inward from the side margin end in the W-axis direction was photographed with an SEM, and the continuity rate of the internal electrode layer was measured for each layer. FIG. 10 is an SEM photograph of the region. The shaded areas correspond to the internal electrode layers. In the outer region E_W, the continuity rate of the internal electrode layer differed for each layer. Internal electrode layers having a continuity rate of 40% to 50% and internal electrode layers having a continuity rate of 60% to 70% were alternately laminated.
[0078] In the WT cross section, an SEM photograph was taken of the central region C_W at the center in the W-axis direction with the same field of view as the outer region E_W, and the continuity ratio of the internal electrode layers was measured for each layer, similar to Fig. 10. In the central region C_W, the continuity ratio of each internal electrode layer was 60% to 70%, and it was confirmed that the difference in continuity ratio between layers was small.
[0079] In the LT cross section, assuming that the length of the internal electrode layer in the L-axis direction is 100%, an outer region E_L in a range of 5% inward from the end margin side end in the L-axis direction was photographed by SEM, and the continuity rate of the internal electrode layer was measured for each layer, as in Fig. 10. In the outer region E_L, the continuity rate of the internal electrode layer was different for each layer. Internal electrode layers having a continuity rate of 50% to 60% and internal electrode layers having a continuity rate of 60% to 70% were alternately laminated.
[0080] In the LT cross section, assuming that the length of the internal electrode layer in the L-axis direction is 100%, an outer region E_L in a range of 5% inward from the end margin side end on the opposite side of the L-axis direction was photographed with an SEM, and the continuity rate of the internal electrode layer was measured for each layer, as in Figure 10. In the outer region E_L, the continuity rate of the internal electrode layer was different for each layer. Internal electrode layers having a continuity rate of 50% to 60% and internal electrode layers having a continuity rate of 60% to 70% were laminated alternately.
[0081] In the LT cross section, an SEM photograph was taken of the central region C_L in the center of the L axis direction in the same field of view as the outer region E_L, and the continuity ratio of the internal electrode layers was measured for each layer, as in FIG. 10. In the central region C_L, the continuity ratio of the internal electrode layers was different for each layer. Internal electrode layers having a continuity ratio of 50% to 70% and internal electrode layers having a continuity ratio of 60% to 70% were alternately laminated.
[0082] (Comparative Example) In the comparative example, in the laminate of the first and second stacking units, the viscosity of the internal electrode pattern was set to be the same for each layer at both ends in the L-axis direction and both ends in the W-axis direction in the region corresponding to the capacitance section 14. The other conditions were the same as those in the example.
[0083] In the WT cross section, assuming that the width of the internal electrode layer in the W-axis direction is 100%, an outer region E_W in a range of 5% inward from the side margin end in the W-axis direction was photographed with an SEM, and the continuity rate of the internal electrode layer was measured for each layer, similar to Figure 10. In the outer region E_W, the continuity rate of each internal electrode layer was about 60% to 75%.
[0084] In the WT cross section, an SEM photograph was taken of the central region C_W in the center of the W axis direction with the same field of view as the outer region E_W, and the continuity ratio of the internal electrode layers was measured for each layer, similar to Fig. 10. In the central region C_W, the continuity ratio of each internal electrode layer was about 60% to 75%.
[0085] In the LT cross section, assuming that the length of the internal electrode layer in the L-axis direction is 100%, an outer region E_L in a range of 5% inward from the end margin side end in the L-axis direction was photographed with an SEM, and the continuity rate of the internal electrode layer was measured for each layer in the same manner as in Figure 10. In the outer region E_W, the continuity rate of each internal electrode layer was about 60% to 75%.
[0086] In the LT cross section, an SEM photograph was taken of the central region C_L in the center of the L axis direction in the same field of view as the outer region E_L, and the continuity ratio of the internal electrode layers was measured for each layer in the same manner as in Figure 10. In the central region C_L, the continuity ratio of each internal electrode layer was about 60% to 75%.
[0087] The measurement results for each continuity ratio are shown in Tables 1 and 2. In the examples, the maximum difference in the continuity ratio between two adjacent internal electrode layers in the outer region E_W was 20% or more, and the maximum difference in the continuity ratio between two adjacent internal electrode layers in the central region C_W was within 10%. Thus, in the examples, the difference in the continuity ratio was larger in the outer region E_W compared to the central region C_W.
[0088] In the comparative example, the maximum difference in the continuity ratio between two adjacent internal electrode layers in the outer region E_W was within 10%, and the maximum difference in the continuity ratio between two adjacent internal electrode layers in the central region C_W was within 10%. Thus, in the comparative example, the difference in the continuity ratio was small in the outer region E_W and the central region C_W.
[0089] Next, in the embodiment, the average value of the continuity ratio of all the internal electrode layers in the outer region E_W was 60%, and the average value of the continuity ratio of all the internal electrode layers in the central region C_W was 70%. Thus, in the embodiment, the average value of the continuity ratio in the outer region E_W was smaller than that in the central region C_W.
[0090] In the comparative example, the average value of the continuity ratio of all the internal electrode layers in the outer region E_W was 70%, and the average value of the continuity ratio of all the internal electrode layers in the central region C_W was 70%. Thus, in the comparative example, the average value of the continuity ratio was small in the central region C_W and the outer region E_W. [Table 1]
[0091] In the embodiment, the maximum difference in continuity ratio between two adjacent internal electrode layers in the outer region E_L was 20% or more, and the maximum difference in continuity ratio between two adjacent internal electrode layers in the central region C_L was within 10%. Thus, in the embodiment, the difference in continuity ratio was larger in the outer region E_L than in the central region C_L.
[0092] In the comparative example, the maximum difference in continuity ratio between two adjacent internal electrode layers in the outer region E_L was within 10%, and the maximum difference in continuity ratio between two adjacent internal electrode layers in the central region C_L was within 10%. Thus, in the comparative example, the difference in continuity ratio was small in the outer region E_L and the central region C_L.
[0093] Next, in the embodiment, the average value of the continuity ratio of all the internal electrode layers in the outer region E_L was 60%, and the average value of the continuity ratio of all the internal electrode layers in the central region C_L was 70%. Thus, in the embodiment, the average value of the continuity ratio in the outer region E_L was smaller than that in the central region C_L.
[0094] In the comparative example, the average value of the continuity ratio of all the internal electrode layers in the outer region E_L was 70%, and the average value of the continuity ratio of all the internal electrode layers in the central region C_L was 70%. Thus, in the comparative example, the average value of the continuity ratio was small in the central region C_L and the outer region E_L. [Table 2]
[0095] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]
[0096] 10 Stacked Chip 11 Dielectric layer 12a 1st internal electrode layer 12b Second internal electrode layer 13 Cover Layer 14 Capacity part 15 End Margin 16 Side Margin 20a,20b external electrode 51 Dielectric green sheet 52a, 52b, 53a, 53b Internal electrode patterns 54 Cover Sheet 100 Multilayer ceramic capacitors
Claims
1. a laminated structure including a plurality of dielectric layers and a plurality of internal electrode layers provided via the plurality of dielectric layers and alternately extending to two end faces facing each other; a pair of side margins sandwiching the laminated structure in a third direction perpendicular to a first direction in which the internal electrode layers face each other and a second direction in which the two end faces face each other; for at least two adjacent layers of the plurality of internal electrode layers, when a width of the two layers in the third direction is taken as 100%, a continuity difference within a range of 5% inward from the side margin end in the third direction is 20% or more, a ceramic electronic component, in which in a capacitive section in which internal electrode layers alternately extended to the two end faces face each other, a continuity difference between the internal electrode layers within a range of ±20% from the center in the third direction and within a range of ±20% from the center in the first direction is within a range of ±10%.
2. a laminated structure including a plurality of dielectric layers and a plurality of internal electrode layers provided via the plurality of dielectric layers and alternately extending to two end faces facing each other; a pair of side margins sandwiching the laminated structure in a third direction perpendicular to a first direction in which the internal electrode layers face each other and a second direction in which the two end faces face each other; a ceramic electronic component, wherein, for the plurality of internal electrode layers, when the width of the plurality of internal electrode layers in the third direction is taken as 100%, the standard deviation of the continuity rate of each internal electrode layer within a range of 5% inward from the side margin end in the third direction is greater than the standard deviation of the continuity rate of each internal electrode layer within a range of ±20% from the center in the third direction and within a range of ±20% from the center in the first direction in a capacitive section in which the internal electrode layers alternately drawn out to the two end faces face each other.
3. 3. The ceramic electronic component according to claim 1, wherein, for the plurality of internal electrode layers, when a width of the plurality of internal electrode layers in the third direction is taken as 100%, an average value of a continuity ratio of each internal electrode layer that is 5% inward from the side margin end in the third direction is smaller than an average value of a continuity ratio of each internal electrode layer in a range of ±20% from a center in the third direction and a range of ±20% from a center in the first direction in the capacitive section.
4. 3. The ceramic electronic component according to claim 1, wherein, when a width of the plurality of internal electrode layers in the third direction is taken as 100%, a continuity ratio of the plurality of internal electrode layers differs for each layer within a range of 5% inward from the side margin end in the third direction.
5. a laminated chip having a plurality of dielectric layers and a plurality of internal electrode layers provided via the plurality of dielectric layers and alternately drawn out to two end faces opposing each other, the laminated chip having a substantially rectangular parallelepiped shape and formed such that the plurality of internal electrode layers are alternately drawn out to the two end faces opposing each other in a second direction; the laminated chip has end margins in which internal electrode layers exposed on the same end surface face each other without being sandwiched between internal electrode layers exposed on different end surfaces; With respect to at least two adjacent layers of the plurality of internal electrode layers, when a length of the two layers in the second direction is taken as 100%, a continuity difference within a range of 5% inward from the end margin side end in the second direction is 15% or more, a capacitance section in which internal electrode layers alternately drawn out to the two end faces face each other, the difference in continuity of each internal electrode layer within a range of ±20% from the center in the second direction and within a range of ±20% from the center in a first direction in which the multiple internal electrode layers face each other is within a range of ±10%.
6. a laminated chip having a plurality of dielectric layers and a plurality of internal electrode layers provided via the plurality of dielectric layers and alternately drawn out to two end faces opposing each other, the laminated chip having a substantially rectangular parallelepiped shape and formed such that the plurality of internal electrode layers are alternately drawn out to the two end faces opposing each other in a second direction; the laminated chip has end margins in which internal electrode layers exposed on the same end surface face each other without being sandwiched between internal electrode layers exposed on different end surfaces; a ceramic electronic component, in which, for the multiple internal electrode layers, when the length of the multiple internal electrode layers in the second direction is taken as 100%, the standard deviation of the continuity rate of each internal electrode layer within a range of 5% inward from the end margin side end in the second direction is greater than the standard deviation of the continuity rate of each internal electrode layer within a range of ±20% from the center in the second direction and within a range of ±20% from the center in the first direction in which the multiple internal electrode layers oppose each other, in a capacitive section in which the internal electrode layers alternately drawn out to the two end faces oppose each other.
7. 7. The ceramic electronic component according to claim 5, wherein, for the plurality of internal electrode layers, when a length of the plurality of internal electrode layers in the second direction is taken as 100%, an average value of a continuity ratio of each internal electrode layer within a range of 5% inward from the end margin side end in the second direction is smaller than an average value of a continuity ratio of each internal electrode layer within a range of ±20% from a center in the second direction and within a range of ±20% from a center in the first direction in the capacitive section.
8. 7. The ceramic electronic component according to claim 5, wherein, when a length of the plurality of internal electrode layers in the second direction is taken as 100%, a continuity ratio of the plurality of internal electrode layers is different for each layer within a range of 5% inward from the end margin side end in the second direction.
Citation Information
Patent Citations
Multilayer ceramic capacitor and method of manufacturing the same
JP2009164446A
Multilayer ceramic electronic component
JP2013089944A
Multilayer ceramic capacitor
JP2015053526A
Multilayer ceramic capacitor
JP2015111651A
Multilayer ceramic capacitor
JP2017103262A