Prepolymer, and high-molecular-weight water-soluble polymer prepared using prepolymer
The use of a prepolymer produced via radical polymerization with a RAFT agent addresses the challenges of conventional flocculants by enabling controlled production of high molecular weight water-soluble polymers for efficient sludge dewatering with improved properties and reduced costs.
Patent Information
- Application Number
- JP2023075328
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
Conventional cationic polymer flocculants and cross-linked polymers face challenges such as high viscosity, narrow addition range, and high cost, while copolymerization methods are complex and difficult due to insoluble components, making it hard to effectively dewater difficult sludge.
A prepolymer is produced through radical polymerization with an exchange chain transfer mechanism type control agent, allowing for the production of high molecular weight water-soluble polymers with controlled chain length and structure, using a reversible addition-fragmentation chain transfer agent (RAFT agent) to facilitate easier adjustment of properties.
The prepolymer enables the production of high molecular weight water-soluble polymers with improved properties, facilitating easier control over chain length and structure, leading to enhanced dewatering efficiency and reduced costs.
Smart Images

Figure 2024159353000001 
Figure 2024159353000002 
Figure 2024159353000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a prepolymer which serves as an intermediate material for producing a high-molecular-weight, water-soluble polymer, and to a high-molecular-weight, water-soluble polymer produced by using the prepolymer. [Background technology]
[0002] There is a strong global movement towards carbon neutrality, and sewage treatment and wastewater treatment in various industries are no exception. In the B-DASH project related to sewage treatment, attention is being paid to the development of high-concentration sewage digesters and low-power dehydrators. Digested sludge has low organic and fibrous content and is classified as difficult-to-dehydrate sludge. If high concentration is achieved in the digestion reaction, the digested sludge that comes out as residue will also become highly concentrated, and there is a high possibility that it will become even more difficult to dehydrate. Furthermore, in the case of developing a low-power dehydrator, it is considered that the power of the drive unit itself will be reduced, and for this reason it will be necessary to reduce the moisture content of the dehydrated sludge using chemicals such as polymer flocculants.
[0003] Cationic polymer flocculants are effective for organic sludge and wastewater, and are always used in coagulation and sedimentation and dewatering operations. Cationic polymer flocculants are also used to dewater digested sludge, which is difficult to dewater. Conventional cationic polymer flocculants have high viscosity due to strong intermolecular interactions and strong molecular entanglement. Since the entanglement of polymer molecules can be stronger than the interaction between polymer molecules and sludge, linear polymers tend to have a narrow range of dosage when added to sludge, and the moisture content of the dewatered sludge cake may not decrease unless the appropriate amount is added. Crosslinked polymers are sometimes used as polymer flocculants, and emulsion-type crosslinked polymers maintain the three-dimensional molecular structure, have weak intermolecular interactions, and have low viscosity. As a result, they react quickly with sludge to form strong flocs, which is expected to reduce the moisture content of the dehydrated cake (Patent Document 1). However, because their molecular weight is lower than that of conventional cationic polymer flocculants, they tend to be added in larger amounts, resulting in higher chemical costs than conventional cationic polymer flocculants. In some cases, conventional cationic polymer flocculants are used in combination with crosslinked polymers, but because different dissolution equipment is used, the operation can become complicated depending on the treatment plant. There is also a method for copolymerizing a relatively hydrophobic monomer with the aim of hydrophobically modifying a powdered polymer, but this method produces a large amount of insoluble matter due to insufficient polymerization, making hydrophobic modification difficult. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2016-094584 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a high molecular weight water-soluble polymer that can impart superior properties compared to conventional high molecular weight water-soluble polymers, and to provide a prepolymer that can be used as an intermediate raw material for producing the high molecular weight water-soluble polymer. [Means for solving the problem]
[0006] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by producing a high molecular weight water-soluble polymer by living radical polymerization using, as an intermediate raw material (macro chain transfer agent), a prepolymer obtained by radical polymerization of a monomer component in the presence of a chain transfer mechanism type inhibitor, the prepolymer having a structure derived from the chain transfer mechanism type inhibitor at its terminal. This prepolymer has led to the completion of the present invention.
[0007] The present invention which solves the above problems is described below.
[0008] [1] A prepolymer for producing a high molecular weight water-soluble polymer, comprising: It is a prepolymer obtained by radical polymerization of a monomer component in the presence of a chain exchange transfer mechanism type control agent, A prepolymer having a structure derived from the exchange chain transfer mechanism regulator at its terminal.
[0009] [2] The prepolymer according to [1], wherein the exchange chain transfer mechanism type control agent is a reversible addition-fragmentation chain transfer agent (RAFT agent).
[0010] [3] The reversible addition-fragmentation chain transfer agent (RAFT agent) is represented by the following formula (1): [ka] (In the formula, R 3 and R 4 represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a heteroaryl group which may have a substituent, or an aralkyl group which may have a substituent. The prepolymer according to [2], comprising a trithiocarbonate compound represented by the following formula:
[0011] [4] The prepolymer according to any one of [1] to [3], which has a weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) of 1,000 to 300,000.
[0012] The inventions described in [1] to [4] above are prepolymers that serve as intermediate raw materials for producing high molecular weight water-soluble polymers. The prepolymers are produced by radically polymerizing monomer components in the presence of an exchange chain transfer mechanism regulator, and are characterized in that a structure derived from the exchange chain transfer mechanism regulator is bonded to the end of the polymer chain obtained by polymerizing the monomer components. The prepolymers can be used as macro-chain transfer agents in the production of high molecular weight water-soluble polymers.
[0013] [5] A high molecular weight water-soluble polymer obtained by radical polymerization of a monomer component in the presence of the prepolymer according to any one of [1] to [4].
[0014] [6] The high molecular weight water-soluble polymer according to [5], which is a polymer obtained by polymerization by irradiation with active energy rays.
[0015] [7] The high molecular weight water-soluble polymer according to [5] or [6], wherein the high molecular weight water-soluble polymer is a polymeric flocculant.
[0016] The inventions described in [5] to [7] above are high molecular weight water-soluble polymers produced using the prepolymer described in any one of [1] to [4] as a macro chain transfer agent. The high molecular weight water-soluble polymer is produced by radically polymerizing a monomer component different from the monomer component of [1] in the presence of the prepolymer, and is a block copolymer of a polymer chain derived from the prepolymer and a polymer chain obtained by polymerizing the monomer component. Effect of the Invention
[0017] When producing a high molecular weight water-soluble polymer, the prepolymer of the present invention is used as an intermediate raw material (macro chain transfer agent), which makes it easier to control the chain length, structure, and properties of the high molecular weight water-soluble polymer, and therefore makes it possible to impart various properties to the high molecular weight water-soluble polymer compared to conventional high molecular weight water-soluble polymers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The prepolymer, the high molecular weight water-soluble polymer, and the polymer flocculant of the present invention will be described below. In addition, there are circumstances in which it is impossible or almost impractical to directly identify the prepolymers, high molecular weight water-soluble polymers, and polymer flocculants of the present invention based on their structure or properties, and it may be possible to clearly identify them only based on the process (manufacturing method) for obtaining the composition. In the following description, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid, and "(meth)acrylate" means acrylate and / or methacrylate. All physical properties are measured at 25°C and normal pressure unless otherwise specified.
[0019] (1) Prepolymer The prepolymer of the present invention is a prepolymer obtained by radical polymerization of a monomer component in the presence of a chain transfer mechanism type regulator, and has a structure derived from the chain transfer mechanism type regulator bonded to its terminal. That is, it is a prepolymer in which a structure derived from the chain transfer mechanism type regulator is bonded to the terminal of a polymer block (hereinafter also referred to as polymer block (A)) obtained by polymerizing a monomer component.
[0020] Examples of exchange chain transfer mechanism type control agents include reversible addition-fragmentation chain transfer agents in the RAFT method (hereinafter also referred to as "RAFT agents"), control agents in the iodine transfer polymerization method, control agents in the TERP method, control agents in the SBRP method, control agents in the BIRP method, etc. Among these, RAFT agents are particularly preferably used from the viewpoint of ease of implementation.
[0021] As the RAFT agent, various known RAFT agents such as dithioester compounds, xanthate compounds, trithiocarbonate compounds, and dithiocarbamate compounds can be used. Among these, the following formula (1) is preferred in terms of excellent polymerization control of (meth)acrylic monomers (especially (meth)acrylic acid ester compounds):
[0022] [ka]
[0023] In the formula (1), a trithiocarbonate compound represented by the formula: 3 and R 4 represents an optionally substituted alkyl group, an optionally substituted aryl group, an optionally substituted heteroaryl group, or an optionally substituted aralkyl group.
[0024] Specific examples of the trithiocarbonate compound include S,S-dibenzyl trithiocarbonate, bis[4-(2,3-dihydroxypropoxycarbonyl)benzyl]trithiocarbonate, bis[4-(2-hydroxyethoxycarbonyl)benzyl]trithiocarbonate, 1,4-bis(n-dodecylsulfanylthiocarbonylsulfanylmethyl)benzene, 2-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}propanoic acid, and 4-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}-4-cyanopentanoic acid.
[0025] The amount of the exchange chain transfer mechanism type regulator used can be appropriately adjusted depending on the type of monomer and exchange chain transfer mechanism type regulator used, etc. In general, the amount is 0.01 to 20 mol %, preferably 0.02 to 10 mol %, and more preferably 0.05 to 5 mol %, based on the total amount of the monomer components.
[0026] The prepolymer of the present invention is formed by bonding a structure derived from an exchange chain transfer mechanism type control agent to an end. In the present invention, the structure derived from an exchange chain transfer mechanism type control agent is derived from an exchange chain transfer mechanism type control agent and contains at least a part of the exchange chain transfer mechanism type control agent. In the case of a RAFT agent, it means a dithioester structure, a xanthate structure, a trithiocarbonate structure (hereinafter referred to as a "trithio structure"), a dithiocarbamate compound (collectively referred to as an S-containing structure), and / or an organic group bonded to the S-containing structure. For example, when the exchange chain transfer mechanism type control agent is represented by the above chemical formula (1), the end of the prepolymer is an organic group bonded to the trithio structure in formula (1) (i.e., R 3 or R 4 The term "a" means that a trithio structure or a composite group of a trithio structure and an organic group bonded to the trithio structure is bonded to the trithio structure. The prepolymer has an S-containing structure and / or a composite group of an organic group bonded to the S-containing structure and an S-containing structure at at least one end. The prepolymer may have at least one selected from an organic group bonded to the S-containing structure, an S-containing structure, and a composite group of an organic group bonded to the S-containing structure and a trithio structure at the other end, and may be a mixture of these. It is preferable that the prepolymer has a composite group of an organic group bonded to the S-containing structure and an S-containing structure at one end, and an organic group bonded to the S-containing structure at the other end.
[0027] The monomer components to be radically polymerized in the presence of a chain transfer mechanism type control agent may be selected depending on the compatibility with the chain transfer mechanism type control agent and the properties to be imparted to the final high molecular weight water-soluble polymer. The compatibility with the chain transfer mechanism type control agent can be selected in consideration of the monomer conversion rate, etc. Specific examples include (meth)acrylic acid alkyl ester compounds, (meth)acrylic acid aliphatic cyclic ester compounds, (meth)acrylic acid aromatic ester compounds, and the following formula (2): CH2=CR 1 -C(=O)O-(R 2 O) n -R 3 ···(2) (In formula (2), R 1 represents a hydrogen atom or a methyl group, R 2 represents a linear or branched alkylene group having 2 to 6 carbon atoms; R 3 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms; and n represents an integer of 1 to 100. Examples of the vinyl monomer include compounds represented by the following formula: styrene-based compounds, maleimide compounds, amide group-containing vinyl compounds, and vinyl-based monomers having a crosslinkable functional group.
[0028] Specific examples of the (meth)acrylic acid alkyl ester compound include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and icosyl (meth)acrylate.
[0029] Specific examples of the aliphatic cyclic ester compounds of (meth)acrylic acid include cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, cyclododecyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentanyl (meth)acrylate.
[0030] Specific examples of the aromatic ester compounds of (meth)acrylic acid include phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxymethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, and 3-phenoxypropyl (meth)acrylate.
[0031] Examples of the compound in which n is 1 in the above formula (2) include an alkoxyalkyl (meth)acrylate compound and a hydroxyalkyl (meth)acrylate compound.
[0032] The (meth)acrylic acid alkoxyalkyl ester compound has an oxyalkylene structure (e.g., an oxyethylene chain, an oxypropylene chain, an oxybutylene chain, etc.). Specific examples of the (meth)acrylic acid alkoxyalkyl ester compound include methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, n-propoxyethyl (meth)acrylate, n-butoxyethyl (meth)acrylate, methoxypropyl (meth)acrylate, ethoxypropyl (meth)acrylate, n-propoxypropyl (meth)acrylate, n-butoxypropyl (meth)acrylate, methoxybutyl (meth)acrylate, ethoxybutyl (meth)acrylate, n-propoxybutyl (meth)acrylate, and n-butoxybutyl (meth)acrylate.
[0033] Specific examples of the (meth)acrylic acid hydroxyalkyl ester compound include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.
[0034] When n in the above formula (2) is 2 or more, the compound represented by the above formula (2) has a polyoxyalkylene structure (e.g., a polyoxyethylene chain, a polyoxypropylene chain, a polyoxybutylene chain, etc.). When n is 2 or more, two or more R2 in the above formula (2) may be the same or different from each other. Therefore, the compound in which n in the above formula (2) is 2 or more may have different types of polyoxyalkylene structures in one molecule, such as a block structure consisting of polyoxyethylene / polyoxypropylene.
[0035] Specific examples of the compound in which n in the above formula (2) is 2 or more include polyoxyethylene (meth)acrylate, polyoxypropylene (meth)acrylate, polyoxybutylene (meth)acrylate, polyoxyethylene-polyoxypropylene (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, lauroxypolyethylene glycol (meth)acrylate, stearoxypolyethylene glycol (meth)acrylate, octoxypolyethylene glycol polypropylene glycol (meth)acrylate, nonylphenoxypolypropylene glycol (meth)acrylate, and phenoxypolyethylene glycol polypropylene glycol (meth)acrylate.
[0036] Specific examples of styrene-based compounds include styrene, α-methylstyrene, β-methylstyrene, vinylxylene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene, pn-butylstyrene, p-isobutylstyrene, pt-butylstyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, p-hydroxystyrene, m-hydroxystyrene, o-hydroxystyrene, p-isopropenylphenol, m-isopropenylphenol, o-isopropenylphenol, o-vinylbenzoic acid, m-vinylbenzoic acid, p-vinylbenzoic acid, divinylbenzene, and vinylnaphthalene.
[0037] Specific examples of the maleimide compound include maleimide and N-substituted maleimide compounds. Examples of the N-substituted maleimide compound include N-alkyl-substituted maleimide compounds such as N-methylmaleimide, N-ethylmaleimide, Nn-propylmaleimide, N-isopropylmaleimide, Nn-butylmaleimide, N-isobutylmaleimide, N-tert-butylmaleimide, N-pentylmaleimide, N-hexylmaleimide, N-heptylmaleimide, N-octylmaleimide, N-laurylmaleimide, and N-stearylmaleimide; N-cyclopentylmaleimide; imide, and N-cycloalkyl-substituted maleimide compounds such as N-cyclohexylmaleimide; and N-aryl-substituted maleimide compounds such as N-phenylmaleimide, N-(4-hydroxyphenyl)maleimide, N-(4-acetylphenyl)maleimide, N-(4-methoxyphenyl)maleimide, N-(4-ethoxyphenyl)maleimide, N-(4-chlorophenyl)maleimide, N-(4-bromophenyl)maleimide, and N-benzylmaleimide.
[0038] Specific examples of the amide group-containing vinyl compound include (meth)acrylamide, (meth)acrylamide derivatives, and N-vinylamide monomers. Specific examples of the (meth)acrylamide derivatives include tert-butyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, and (meth)acryloylmorpholine. Specific examples of the N-vinylamide monomers include N-vinylacetamide, N-vinylformamide, and N-vinylisobutylamide.
[0039] Regarding the vinyl monomer having a crosslinkable functional group, examples of the crosslinkable functional group include a crosslinkable silyl group, a silanol group, a carboxyl group, a hydroxyl group, an epoxy group, an oxazoline group, an isocyanate group, and a polymerizable unsaturated group. Examples of the crosslinkable silyl group include an alkoxysilyl group and a halogenosilyl group. Among these, an alkoxysilyl group is preferred in terms of easy control of reactivity, and examples of the alkoxysilyl group include a trimethoxysilyl group, a methyldimethoxysilyl group, a dimethylmethoxysilyl group, a triethoxysilyl group, a methyldiethoxysilyl group, and a dimethylethoxysilyl group.
[0040] Specific examples of vinyl monomers having a crosslinkable functional group include crosslinkable silyl group-containing vinyl compounds, unsaturated carboxylic acids, unsaturated acid anhydrides, hydroxy group-containing vinyl compounds, epoxy group-containing vinyl compounds, primary or secondary amino group-containing vinyl compounds, oxazoline group-containing vinyl compounds, and isocyanate group-containing vinyl compounds.
[0041] Examples of the crosslinkable silyl group-containing vinyl compound include vinyl silanes such as vinyl trimethoxysilane, vinyl triethoxysilane, vinyl methyl dimethoxysilane, and vinyl dimethyl methoxysilane; alkoxysilyl group-containing (meth)acrylic acid esters such as trimethoxysilylpropyl (meth)acrylate, triethoxysilylpropyl (meth)acrylate, methyl dimethoxysilylpropyl (meth)acrylate, and dimethyl methoxysilylpropyl (meth)acrylate; alkoxysilyl group-containing vinyl ethers such as trimethoxysilylpropyl vinyl ether; and alkoxysilyl group-containing vinyl esters such as vinyl trimethoxysilyl undecanoate. The crosslinkable silyl group-containing vinyl compound forms a crosslinked structure by dehydration condensation between crosslinkable silyl groups, and is therefore suitable in that it can efficiently carry out the polymerization reaction and the subsequent crosslinking reaction when producing a polymer.
[0042] Examples of the unsaturated carboxylic acid include (meth)acrylic acid, maleic acid, fumaric acid, itaconic acid, crotonic acid, citraconic acid, cinnamic acid, and further, monoalkyl esters of unsaturated dicarboxylic acids (monoalkyl esters of maleic acid, fumaric acid, itaconic acid, citraconic acid, etc.), etc. Examples of the unsaturated acid anhydrides include maleic anhydride, itaconic anhydride, citraconic anhydride, etc.
[0043] Examples of the hydroxy group-containing vinyl compound include the above-mentioned (meth)acrylic acid hydroxyalkyl ester compounds, (meth)acrylic acid esters of polyalkylene glycols (e.g., polyethylene glycol, polypropylene glycol, etc.); styrene-based compounds such as o-hydroxystyrene, m-hydroxystyrene, and p-hydroxystyrene; and maleimide compounds such as N-(4-hydroxyphenyl)maleimide.
[0044] Examples of the epoxy group-containing vinyl compound include glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, 3,4-epoxycyclohexylmethyl (meth)acrylate, etc. The vinyl monomer constituting the polymer (PA) may be one or more of the above.
[0045] By producing a high molecular weight water-soluble polymer using the prepolymer of the present invention as an intermediate raw material, the high molecular weight water-soluble polymer can be modified. For example, when the prepolymer of the present invention is used as an intermediate raw material for producing a polymer flocculant, the polymer flocculant can be modified by the monomer component propagated in the prepolymer, and the affinity of the polymer flocculant to water or sludge can be adjusted.
[0046] The prepolymer of the present invention is preferably water-soluble because it is easy to make the high molecular weight water-soluble polymer produced in the subsequent process water-soluble and easy to use in the production process. Therefore, the prepolymer of the present invention is preferably composed of a water-soluble monomer unit. As such a water-soluble monomer, a compound represented by the above chemical formula (2) or an amide group-containing vinyl compound is preferable. In addition, from the viewpoint of ease of adjusting affinity to water and sludge, it is preferable to be composed of a nonionic water-soluble monomer unit. Furthermore, from the viewpoint of low degradation such as hydrolysis during long-term storage, a monomer that does not contain an ester skeleton is preferable. As such a monomer, a water-soluble amide group-containing vinyl compound that is difficult to hydrolyze is preferable, and among them, acrylamide, N-substituted acrylamide, and N,N-disubstituted acrylamide are preferable from the viewpoint of ease of polymerization control. Specific examples of such compounds include acrylamide, acryloylmorpholine, N,N-dimethylacrylamide, and 2-hydroxyethylacrylamide. The prepolymer of the present invention is preferably a copolymer of a hydrophobic monomer and a hydrophilic monomer, and is preferably a block copolymer consisting of a hydrophobic block consisting of a hydrophobic monomer and a hydrophilic block consisting of a hydrophilic monomer. The high molecular weight water-soluble polymer finally produced using such a prepolymer tends to be able to achieve a high degree of compatibility between affinity with sludge and water solubility. Furthermore, the prepolymer of the present invention is preferably formed by bonding a growing end structure of radical polymerization derived from an exchange chain transfer mechanism type control agent to the end of the hydrophilic block. The high molecular weight water-soluble polymer produced using such a prepolymer has a hydrophobic block at one end thereof, which increases affinity with sludge and tends to have particularly high flocculation and gelation performance due to polymer-polymer interaction.
[0047] The prepolymer of the present invention preferably has a weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) of 1,000 to 300,000, more preferably 1,000 to 100,000, and particularly preferably 1,200 to 100,000. If it is less than 1,000, the properties of the polymer chain formed by growing the monomer component used in the production of the prepolymer are unlikely to be reflected in the high molecular weight water-soluble polymer finally obtained. That is, the effect of modification is small. If it exceeds 300,000, it is difficult to prepare a prepolymer with high purity. In addition, separation is likely to occur when used in the production of a high molecular weight water-soluble polymer.
[0048] The prepolymer of the present invention preferably has a polystyrene-equivalent number average molecular weight (Mn) measured by gel permeation chromatography (GPC) of 1,000 to 300,000, more preferably 1,000 to 100,000, and particularly preferably 1,200 to 100,000.
[0049] The molecular weight distribution (Mw / Mn), which is the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn), is not particularly limited, but is, for example, 1.00 to 3.00, preferably 1.05 to 2.50, and particularly preferably 1.10 to 1.50. If it is within this range, the quality of the high molecular weight water-soluble polymer produced using this prepolymer can be easily stabilized.
[0050] (2) Method for producing prepolymer The prepolymer of the present invention can be produced by using a known polymerization solvent and polymerizing the above-mentioned monomer components in the solvent in the presence of the above-mentioned exchange chain transfer mechanism type regulator and polymerization initiator.
[0051] The polymerization solvent used may be, for example, a solvent capable of dissolving a monomer. Examples of the polymerization solvent include organic solvents and water. Examples of the organic solvent include aromatic compounds such as benzene, toluene, xylene, and anisole; ester compounds such as methyl acetate, propyl acetate, and butyl acetate; ketone compounds such as acetone, methyl ethyl ketone, and cyclohexanone; and alcohols such as methanol and ethanol. In the production of a high molecular weight water-soluble polymer in the subsequent step, in consideration of use in aqueous solution polymerization, it is most preferable that the polymerization solvent is water. When an organic solvent is used, it is preferable to use methanol, ethyl acetate, and acetonitrile, which are unlikely to cause a chain transfer reaction in radical polymerization and have a boiling point of less than 100° C., making water replacement in the subsequent step easy. The polymerization solvent may be used alone or in combination of two or more kinds.
[0052] The amount of the polymerization solvent used is preferably 5 to 200 parts by mass, more preferably 10 to 100 parts by mass, based on 100 parts by mass of the total amount of the monomers used in the reaction. When the amount of the polymerization solvent used is 200 parts by mass or less, it is preferable in that a high polymerization rate can be achieved in a short time.
[0053] The radical polymerization initiator used in the polymerization reaction is not particularly limited. For example, persulfates such as potassium persulfate and ammonium persulfate, organic peroxides such as t-butyl hydroperoxide, azo initiators, redox initiators, and photopolymerization initiators can be appropriately used. Among these, azo initiators are preferred because they are easy to handle and do not easily cause side reactions during radical polymerization. These radical polymerization initiators may be used alone or in combination of two or more kinds.
[0054] Specific examples of the azo initiator include 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylpropionitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(3,4,5,6-tetrahydropyrimidinyl)propane] dihydrochloride, and 2,2'-azobis[2-(3,4,5,6-tetrahydropyrimidinyl)propane] dihydrochloride. Examples include dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanopentanoic acid), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]-propionamide, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], and 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide].
[0055] The amount of the polymerization initiator added is not particularly limited, and may be appropriately adjusted depending on the type of polymerization initiator and the monomer composition. From the viewpoint of obtaining a prepolymer with a narrower molecular weight distribution, the amount is preferably 0.5 mol or less, more preferably 0.4 mol or less, relative to 1 mol of the exchange chain transfer mechanism type regulator. Also, from the viewpoint of stably carrying out the polymerization reaction, the amount is preferably 0.01 mol or more, more preferably 0.03 mol or more, relative to 1 mol of the exchange chain transfer mechanism type regulator. The amount of the polymerization initiator used relative to 1 mol of the exchange chain transfer mechanism type regulator is preferably 0.01 to 0.5 mol, more preferably 0.03 to 0.4 mol.
[0056] The polymerization reaction may be carried out in the presence of a chain transfer agent (for example, an alkylthiol compound having 2 to 20 carbon atoms) as necessary.
[0057] The reaction temperature during polymerization is not particularly limited, but from the viewpoint of suppressing side reactions during polymerization to obtain a prepolymer with a narrow molecular weight distribution, from the viewpoint of obtaining a prepolymer with less variation in physical properties between lots, and from the viewpoint of easing restrictions on usable polymerization initiators and solvents, it is preferably 100° C. or less, more preferably 90° C. or less, and even more preferably 80° C. or less. In addition, from the viewpoint of smoothly progressing the polymerization reaction, the reaction temperature is preferably 40° C. or more, more preferably 45° C. or more, and even more preferably 50° C. or more. The reaction time in the polymerization reaction can be appropriately set depending on the monomers used, etc., but is preferably 1 hour or more and 48 hours or less, more preferably 2 hours or more and 24 hours or less, and even more preferably 2 hours or more and 12 hours or less.
[0058] (3) High molecular weight water-soluble polymer The high molecular weight water-soluble polymer of the present invention is characterized in that it is a high molecular weight water-soluble polymer obtained by radical polymerization of any monomer component in the presence of the above-mentioned prepolymer of the present invention. That is, the high molecular weight water-soluble polymer of the present invention is a block copolymer of a polymer block (A) formed by polymerizing the monomer component used in the production of the above-mentioned prepolymer of the present invention, and a polymer block (hereinafter also referred to as polymer block (B)) formed by polymerizing any monomer component. The end of the polymer block may have the end structure of the prepolymer of the present invention, i.e., a structure derived from the exchange chain transfer mechanism type regulator.
[0059] The "high molecular weight" of the high molecular weight water-soluble polymer of the present invention can be defined as a 0.5% by mass (polymer equivalent) salt viscosity at 25°C of 3.0 mPa·s or more. The 0.5% by mass (polymer equivalent) salt viscosity at 25°C is preferably 3.0 to 200 mPa·s, more preferably 5.0 to 90 mPa·s, and particularly preferably 10 to 85 mPa·s. If it exceeds 200 mPa·s, the water solubility of the water-soluble polymer may decrease. The 0.5% by mass (polymer equivalent) salt viscosity refers to the salt viscosity at 25°C of a salt solution in which a polymer flocculant is dissolved at a concentration of 0.5% by mass in a 4% by mass aqueous sodium chloride solution. A high molecular weight water-soluble polymer having a 0.5 mass% (polymer equivalent) salt viscosity of 3.0 mPa s or more at 25°C can be determined to have a weight average molecular weight (Mw) of approximately 1 million or more as measured by gel permeation chromatography (GPC).
[0060] The "water-soluble" of the high molecular weight water-soluble polymer of the present invention means that it has a solubility to such an extent that a sample aqueous solution for measuring the salt viscosity of at least 0.5% by mass (polymer equivalent) can be prepared. More preferred "water-soluble" means that the insoluble content in a 0.1% by mass aqueous solution of the high molecular weight water-soluble polymer of the present invention is 5.0% by mass or less, and even more preferably 4.0% by mass or less.
[0061] The monomer component for forming the polymer block (B) can be appropriately selected depending on the properties to be imparted to the high molecular weight water-soluble polymer and its application. In addition to the monomers described for the polymer block (A) above, various monomer components can be used. The monomer component constituting the polymer block (A) and the monomer component constituting the polymer block (B) are usually different (not completely identical) monomer components.
[0062] (3-1) Polymer flocculants When the high molecular weight water-soluble polymer of the present invention is used as a polymer flocculant, the cationic monomers, nonionic monomers, anionic monomers, and the like described below can be preferably used.
[0063] The cationic monomer may be a monomer represented by the following formula (3): CH2=CR 1 -CO-XQ-N+R 2a R 2b R 2c Z - ···(3) (However, in chemical formula (3), R 1 is a hydrogen atom or a methyl group, R 2a and R 2beach independently represents an alkyl group having 1 to 3 carbon atoms or a benzyl group; R 2c represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a benzyl group, and may be the same or different; X represents an oxygen atom or NH; Q represents an alkylene group having 1 to 4 carbon atoms or a hydroxyalkylene group having 2 to 4 carbon atoms; Z - represents a counter anion.) It is preferable that the (meth)acrylate monomer is represented by the following formula:
[0064] Specific examples of the (meth)acrylate monomer represented by the above chemical formula (3) include hydrochlorides and sulfates of dialkylaminoalkyl (meth)acrylates such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and dimethylamino-2-hydroxypropyl (meth)acrylate, and dialkylaminoalkyl (meth)acrylamides such as dimethylaminopropyl (meth)acrylamide. In addition, quaternary salts of dialkylaminoalkyl (meth)acrylates and dialkylaminoalkyl (meth)acrylamides, such as alkyl halide adducts such as methyl chloride, benzyl halide adducts such as benzyl chloride, and dialkyl sulfate adducts such as dimethyl sulfate, are exemplified. These (meth)acrylate monomers may be used alone or in combination of two or more. Among these preferred (meth)acrylate monomers, it is most preferred to use the quaternary methyl chloride salt of dimethylaminoethyl acrylate (DAC), since it has particularly excellent performance as a polymer flocculant and is also excellent in quality and storage stability of the acrylate monomer.
[0065] The polymer block (B) preferably contains 50 to 100 mol %, more preferably 55 to 95 mol %, and particularly preferably 60 to 90 mol % of the cationic monomer unit. If the molar fraction of the cationic monomer is outside the above range, the coagulation property may decrease.
[0066] The high molecular weight water-soluble polymer (polymer flocculant) produced in the present invention may be a copolymer of the above cationic monomer and a nonionic monomer. The nonionic monomer is not particularly limited, but examples thereof include (meth)acrylamide-based compounds represented by the following chemical formula (4), as well as alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and hydroxyethyl (meth)acrylate, styrene, acrylonitrile, and vinyl acetate. Among these nonionic monomers, the following chemical formula (4): is preferred because it has excellent copolymerizability with cationic monomers, is easy to increase the molecular weight required for a polymer flocculant, and has excellent performance as a polymer flocculant. CH2=CR 1 -CO-NR 2 R 3 ···(4) (However, in the above chemical formula (4), R 1 is a hydrogen atom or a methyl group, R 2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. Preferred is a (meth)acrylamide-based compound represented by the following formula:
[0067] Among these (meth)acrylamide compounds, acrylamide (AM) is most preferred because it is water-soluble and has particularly excellent performance as a polymer flocculant. These nonionic monomers may be used alone or in combination of two or more kinds.
[0068] The polymer block (B) preferably contains 0 to 50 mol %, more preferably 5 to 45 mol %, and particularly preferably 10 to 40 mol % of the nonionic monomer unit. If the molar fraction of the nonionic monomer is outside the above range, it is difficult to exert an effect on sludge with a wide range of properties.
[0069] Examples of the anionic monomer include (meth)acrylic acid and salts thereof represented by the following chemical formula (5), as well as vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, maleic acid, and salts thereof. Among these anionic monomers, the following chemical formula (5): is particularly preferred because it has excellent copolymerizability with cationic monomers, is easy to increase the molecular weight required for a polymer flocculant, and has excellent performance as a polymer flocculant. CH2=CR 1 -CO-OM···(5) (However, in chemical formula (5), R 1 represents a hydrogen atom or a methyl group, and M represents a hydrogen atom, an ammonium group, or an alkali metal atom. and salts thereof. As the salts, ammonium salts and alkali metal salts such as sodium salts and potassium salts are preferred.
[0070] Among these (meth)acrylic acids and their salts, acrylic acid (AA) and its ammonium salts are most preferred because of their particularly excellent performance as polymer flocculants. These anionic monomers may be used alone or in combination of two or more.
[0071] The polymer block (B) contains anionic monomer units in an amount of preferably 0 to 50 mol %, more preferably 0 to 40 mol %, and particularly preferably 0 to 30 mol %.
[0072] The 0.5% by mass (polymer equivalent) salt viscosity of the polymer flocculant of the present invention at 25°C is preferably 3.0 to 200 mPa·s, more preferably 5.0 to 90 mPa·s, and even more preferably 10 to 85 mPa·s. If it is less than 3.0 mPa·s, the molecular weight is too small, and the flocculation properties of the sludge may be poor. If it exceeds 200 mPa·s, the molecular weight is too large, and the solubility of the polymer flocculant may decrease, and the flocculation properties of the sludge may deteriorate.
[0073] (3-2) Skin patch base The high molecular weight water-soluble polymer produced as described above can be used as a polymer flocculant, but can also be used as a base material for skin patches. The following description will be given of the case where the high molecular weight water-soluble polymer is used as a base material for skin patches, but the following description of the constituent elements is an example of one embodiment of the present invention, and the present invention is not limited to these contents.
[0074] The high molecular weight water-soluble polymer of the present invention is an excellent base for skin patches such as poultices, and the base can be combined with water, a polyvalent metal compound as a crosslinking agent, and a polyhydric alcohol as a water-retaining agent and mixed to form a gel-like paste. In addition to the above-mentioned ingredients, additives such as inorganic powders and medicinal ingredients can be mixed into the above-mentioned plaster. The ingredients are added and mixed all at once or successively so as to obtain a prescribed mixing ratio, and then kneaded to obtain the above-mentioned plaster.
[0075] The blending ratios when preparing the paste are usually, relative to the total amount of the paste, 5 to 20 mass% of the high molecular weight water-soluble polymer of the present invention (base for skin patches), 1 to 50 mass% of a humectant such as glycerin, 0.001 to 2 mass% of a polyvalent metal compound such as aluminum hydroxide, 1 to 10 mass% of an inorganic additive such as kaolin, 0.01 to 10 mass% of a medicinal ingredient, and 30 to 80 mass% of water.
[0076] If the high molecular weight water-soluble polymer (skin patch base) of the present invention is less than 5% by mass relative to the total amount of the paste, the adhesiveness, thickening properties, and formability decrease, and if it exceeds 20% by mass, the viscosity increases too much, making kneading difficult and making it impossible to knead uniformly. Therefore, it is usually 5 to 20% by mass, preferably 7 to 12% by mass.
[0077] The polyvalent metal compound used in preparing the paste functions as a crosslinking agent, and specifically, there are no particular limitations on the polyvalent metal compound, so long as it is a compound containing a metal having a valence of two or more (polyvalent metal compound), such as aluminum compounds typified by dihydroxyaluminum aminoacetate, aluminum hydroxide, aluminum chloride, aluminum sulfate, aluminum silicate, aluminum phosphate, aluminum magnesium hydroxide, aluminum glycinate, etc., calcium chloride, ferric sulfate, etc., but of the above-mentioned polyvalent metals, aluminum compounds are preferred. These polyvalent metals may be used alone or in combination, and may be used whether they are water-soluble or hydrophobic.
[0078] The amount of the polyvalent metal compound to be blended varies depending on the degree of polymerization and blending amount of the copolymer, the type of polyvalent metal compound, and the influence of other blends, but is usually preferably 0.001 to 2 mass%, and more preferably 0.01 to 1 mass%, of the total amount of the paste.
[0079] When preparing a cataplasm using the base or paste for skin patches of the present invention, in addition to the above-mentioned components, additives generally used in topical preparations, i.e., water-soluble polymers such as gelatin, polyvinyl alcohol, sodium carboxymethylcellulose, polyvinylpyrrolidone, and sodium alginate, may be blended as thickeners or tackifiers for the purpose of further improving suitability during production and quality during use.
[0080] As the water-retaining agent, for example, polyhydric alcohols such as glycerin, propylene glycol, sorbitol, and butylene glycol can be used. In addition, kaolin, titanium oxide, silicic anhydride, etc. can be used as powdered inorganic fillers, dibutylhydroxytoluene, butylhydroxyanisole, etc. as antioxidants, and methyl parahydroxybenzoate, propyl parahydroxybenzoate, etc. as preservatives, and one or more of these can be blended into the plaster as necessary.
[0081] Specific examples of other medicinal ingredients that can be incorporated into the skin patch include antihistamines such as methyl salicylate, glycol salicylate, menthol, camphor, thymol, peppermint oil, borneol, and glycyrrhizic acid; anti-inflammatory analgesics such as indomethacin and flurbiprofen; and local anesthetics such as dibucaine hydrochloride and lidocaine. However, the present invention is not limited to these, and there is no particular restriction on the other medicinal ingredients as long as they are natural products or synthetic chemical substances having medicinal ingredients that can be used as transdermal drugs for clinical or research purposes. One or more of these may be used as necessary, and the amount of such medicinal ingredients blended is usually preferably 0.1 to 10% by mass based on the total amount of the paste.
[0082] The skin patch is prepared by applying and spreading the gel-like paste prepared as described above onto the surface of a support such as a nonwoven fabric, covering the applied surface with a peelable film for protection, cutting, and packaging.
[0083] (4) Method for producing high molecular weight water-soluble polymer The high molecular weight water-soluble polymer of the present invention is produced by radically polymerizing the monomers for forming the polymer block (B) in a solution in the presence of the above-mentioned prepolymer of the present invention, that is, by radically polymerizing the monomer components for forming the polymer block (B) using the above-mentioned prepolymer of the present invention as a macro chain transfer agent. The polymerization method is preferably a method in which polymerization is performed by irradiation with active energy rays, and particularly preferably photopolymerization. The polymerization conditions may be any of the conventionally known conditions. The method for producing the high molecular weight water-soluble polymer of the present invention will now be described in detail.
[0084] The high molecular weight water-soluble polymer of the present invention is produced by radical polymerization of a monomer mixture for forming a polymer block (B) containing a cationic monomer, an anionic monomer, a nonionic monomer and other monomers in the presence of the above-mentioned prepolymer of the present invention.
[0085] First, an aqueous solution of a monomer mixture containing a cationic monomer, an anionic monomer, a nonionic monomer and other monomers is prepared. The monomer concentration in the aqueous solution is 20 to 70% by mass, preferably 30 to 60% by mass. If the monomer concentration is less than 20% by mass, the polymerization proceeds slowly, resulting in an increase in the amount of residual monomer in the product. If the monomer concentration exceeds 70% by mass, the polymerization proceeds rapidly and foaming occurs due to evaporation of water, which may cause equipment trouble. Next, the prepolymer of the present invention is added to the aqueous monomer solution. The amount of the prepolymer added is preferably 10 to 100,000 ppm, and more preferably 100 to 10,000 ppm, based on the total mass of the monomers in the aqueous monomer solution.
[0086] Thereafter, the dissolved oxygen in the aqueous monomer solution is removed using nitrogen gas or the like, and then the polymerization reaction is started. The polymerization reaction is started by adding a polymerization initiator to the aqueous monomer solution prepared by the above method. The polymerization initiation temperature, i.e., the temperature of the aqueous monomer solution at the start of polymerization, is preferably -5 to 30°C. When the monomer concentration is high, the polymerization initiation temperature is set to a low level, and when the monomer concentration is low, the polymerization initiation temperature is set to a high level. As the polymerization initiator, a redox polymerization initiator or a photopolymerization initiator is preferable.
[0087] The redox initiator can be prepared by combining a known oxidizing agent and a reducing agent. Examples of the oxidizing agent include ammonium persulfate, potassium persulfate, hydrogen peroxide, and tertiary butyl hydroperoxide. Examples of the reducing agent include ferrous sulfate, ammonium ferrous sulfate, sodium hydrogen sulfite, and trimethylamine. The amount of the redox initiator to be added is preferably 1 to 200 ppm relative to the mass of the aqueous monomer solution for both the oxidizing agent and the reducing agent. Polymerization can be initiated by adding aqueous solutions of the oxidizing agent and the reducing agent to the aqueous monomer solution immediately before the initiation of polymerization.
[0088] Examples of photopolymerization initiators include benzophenone, anthraquinone, acylphosphine oxide compounds, and azo compounds. The amount of photopolymerization initiator added is preferably 200 to 5000 ppm based on the mass of the aqueous monomer solution. The photopolymerization initiator is added to the aqueous monomer solution, and polymerization can be initiated by irradiating the aqueous monomer solution with light containing light of the maximum absorption wavelength of the photopolymerization initiator. Examples of light sources include high-pressure mercury lamps and low-pressure mercury lamps. The light irradiation conditions such as the wavelength, irradiation intensity, and irradiation time of light used in the photopolymerization are not particularly limited. They may be appropriately adjusted depending on the type and amount of the photopolymerization initiator used and the physical properties and performance of the polymer. When the water-soluble azo initiator is used as the photopolymerization initiator, light with a wavelength of about 365 nm is preferred, and the irradiation intensity is 0.1 to 10.0 mW / cm measured by a UV illuminometer for 365 nm. 2 The irradiation time is usually preferably 0.1 to 3 hours.
[0089] An azo-based polymerization initiator may be added to the aqueous monomer solution in order to promote polymerization at high temperatures in the latter half of the polymerization reaction.
[0090] Examples of azo polymerization initiators include 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylpropionitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, and 2,2'-azobis[2-(3,4,5,6-tetrahydropyrimidin-2-yl)propane] dihydrochloride. Examples of the azobis(2-methylpropionate) are hydrochloride, dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanopentanoic acid), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]-propionamide, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], and 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide]. These may be used alone or in combination of two or more.
[0091] The amount of the azo polymerization initiator added is preferably 100 ppm or more in total relative to the mass of the aqueous monomer solution, and particularly preferably 200 to 10,000 ppm. When the azo polymerization initiator is water-soluble, the azo polymerization initiator may be added directly to the aqueous monomer solution, or may be added after forming an aqueous solution. When the azo polymerization initiator is water-insoluble, polymerization may be difficult to start even if the azo polymerization initiator is added directly to the aqueous monomer solution. In this case, the azo polymerization initiator may be dissolved in a polar organic solvent such as methanol, which has a relatively small chain transfer property and is easily mixed with water, and then added to the aqueous monomer solution. In addition to the above-mentioned monomer and polymerization initiator, a chain transfer agent, a pH adjuster, etc. may be added to the aqueous monomer solution, if necessary.
[0092] The polymerization reaction reaches a maximum temperature of 50 to 100°C 30 minutes to 5 hours after the start of polymerization and is almost completed. The aqueous solution containing the polymer obtained by the polymerization reaction is in a gel state at room temperature (hereinafter, this is also referred to as "polymer gel").
[0093] The polymerization reaction can be carried out batchwise in a suitable reaction vessel, or can be carried out continuously by continuously pouring an aqueous monomer solution onto a belt such as a belt conveyor.
[0094] The polymer gel obtained by the above polymerization reaction may be subjected to a heat treatment in order to reduce the content of residual monomers such as acrylamide. The heat treatment is performed by heating the polymer gel in a reaction vessel or on a belt conveyer. Alternatively, the polymer gel is cut into pieces of appropriate size, sealed and packaged in a vinyl bag or the like, and then heated in a heating bath such as a hot water bath. The heat treatment conditions are preferably 70 to 100°C and 1 to 5 hours. The heat-treated polymer gel can be dried and pulverized by a known method to obtain the present high molecular weight water-soluble polymer in powder form. EXAMPLES
[0095] (Example of prepolymer production) Examples of prepolymer production will be described in detail below. The present invention is not limited to these examples. Various analyses and evaluations were carried out by the following methods.
[0096] [Measurement of molecular weight of polymer] The resulting polymer was subjected to gel permeation chromatography (GPC) under the conditions described below to obtain the number average molecular weight (Mn) and weight average molecular weight (Mw) in terms of polystyrene. The molecular weight distribution (Mw / Mn) was calculated from the obtained values. (GPC measurement conditions) Column: Tosoh Corporation TSKgel SuperMultiporeHZ-M x 4 Eluent:THF Column temperature: 40℃ Detector: RI Flow rate: 1.0mL / min Molecular weight calculation method: pSt converted molecular weight is calculated based on a calibration curve created using pSt standard substances.
[0097] [Monomer conversion rate] In each production example, the above GPC measurement was performed before the addition of the initiator and after the reaction was stopped, and the monomer conversion rate was calculated from the ratio of the peak intensities of the monomer components. When drying was performed during the production process, the GPC measurement was performed before that, and the monomer conversion rate (%) was calculated.
[0098] [Appearance in aqueous solution] Aqueous solutions of the prepolymer obtained in each production example at concentrations of 10%, 20%, and 50% were prepared, and the appearance was visually inspected and evaluated according to the following criteria. Uniform: No turbidity at any concentration. Turbidity: Turbidity will occur at any concentration.
[0099] (Production Example 1) In a 500mL flask equipped with a stirrer and a thermometer, 0.254g of 2-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}propanoic acid ("BM1429" manufactured by Boron Molecular) as an exchange chain transfer mechanism type control agent, 100g of methoxypolyethylene glycol (n≒9) monoacrylate ("Blenmer AME-400" manufactured by NOF Corp.) as a monomer component, and 65g of ion-exchanged water as a polymerization medium were charged, and the mixture was heated to 70°C after sufficient degassing with nitrogen bubbling. 0.014g of 4,4'-azobis(4-cyanovaleric acid) ("ACVA" manufactured by Otsuka Chemical Co., Ltd.) was added as an initiator to start polymerization. After 5 hours while maintaining the temperature at 70°C, the mixture was cooled to room temperature to stop the reaction and obtain prepolymer PP1. The obtained prepolymer PP1 had Mn=63,500, Mw=94,500, and Mw / Mn=1.49, and the monomer conversion was 95%.
[0100] (Manufacturing Examples 2-6, 8, 9) Prepolymers PP2 to 6, 8, and 9 were obtained in the same manner as in Production Example 1, except that the types and amounts of the exchange chain transfer mechanism type regulator and the monomer components were changed as shown in Table 1. The Mn, Mw, Mw / Mn and monomer conversion rate of the obtained prepolymer are shown in Table 1.
[0101] (Production Example 7) A prepolymer acetonitrile solution was obtained in the same manner as in Production Example 1, except that the types and amounts of the exchange chain transfer mechanism regulator, monomer components, and polymerization medium were changed as shown in Table 1. The acetonitrile was removed by vacuum drying at 80°C for 3 hours, and then 65 g of ion-exchanged water was added and dissolved to obtain prepolymer PP7.
[0102] (Production Example 10) In a 500mL flask equipped with a stirrer and a thermometer, 1.27g of 2-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}propanoic acid ("BM1429" manufactured by Boron Molecular) as an exchange chain transfer mechanism type control agent, 80g of methoxypolyethylene glycol (n≒9) monoacrylate ("Blenmer AME-400" manufactured by NOF Corp.) as the 1st monomer of the monomer component, and 65g of ion-exchanged water as a polymerization medium were charged, and the mixture was heated to 70°C after sufficient degassing with nitrogen bubbling. Here, 0.014g of 4,4'-azobis(4-cyanovaleric acid) ("ACVA" manufactured by Otsuka Chemical Co., Ltd.) was added as an initiator to start polymerization. After 3 hours while maintaining the temperature at 70°C, a small amount was sampled and GPC was measured, and it was confirmed that the monomer conversion rate was 95%. Then, 20 g of N-isopropylacrylamide was added as the second monomer of the monomer component, and the mixture was allowed to react for another 3 hours. The mixture was then cooled to room temperature to terminate the reaction, thereby obtaining a prepolymer PP10. The obtained prepolymer PP10 (block polymer) had Mn=18,000, Mw=21,000, and Mw / Mn=1.17. The conversion rate of the 1st monomer was 98%, and the conversion rate of the 2nd monomer was 95%.
[0103] (Examples 11 and 12) Acetonitrile solutions of each prepolymer were obtained in the same manner as in Production Example 10, except that the types and amounts of the chain transfer mechanism regulator, monomer components, and polymerization medium were changed as shown in Table 1. After removing the acetonitrile by vacuum drying at 80°C for 3 hours, 65 g of ion-exchanged water was added and dissolved to obtain prepolymers PP11 and PP12 (block polymers).
[0104] (Comparative Manufacturing Example 1) A 500mL flask equipped with a stirrer and a thermometer was charged with 65g of acetonitrile as a polymerization medium, and the temperature was raised to 70℃ after sufficient degassing with nitrogen bubbling. 100g of methoxypolyethylene glycol (n≒9) monoacrylate (NOF Corp., "Blenmer AME-400") as a monomer component and 1.8g of 3-mercaptopropionic acid as a polymerization inhibitor were each added dropwise over 2 hours. Immediately after the start of the dropwise addition, 0.2g of 2,2'-azobis(2-methylvaleronitrile) (FUJIFILM Wako Pure Chemical Corp., "V-65") was added as an initiator, and the reaction was continued for 6 hours while maintaining the temperature at 70℃. A small amount was sampled and GPC and acid value were measured. The results were Mn=5,600, Mw=10,200, Mw / Mn=1.82, monomer conversion rate 96%, and acid value 5.9mgKOH / g (as is). After that, the temperature was raised to 75°C, 0.01g of 4-methoxyphenol as an inhibitor, 1.0g of tetrabutylammonium bromide as a catalyst, and 2.41g of glycidyl methacrylate (NOF Corp.'s "Blenmer GH") as a reactant were added, and the reaction was continued for 8 hours while maintaining the temperature at 75°C. At this point, a small amount was sampled and the acid value was measured, which was 0.1mgKOH / g (as is), and the reaction rate was determined to be 98% or more, so the mixture was cooled to room temperature and the reaction was stopped. The acetonitrile solution of the obtained prepolymer was vacuum dried at 80°C for 3 hours to remove the acetonitrile, and then 65 g of ion-exchanged water was added to dissolve the prepolymer, obtaining prepolymer PP13 (macromonomer). The obtained prepolymer PP13 had Mn=5,800, Mw=10,500, and Mw / Mn=1.81.
[0105] [Table 1]
[0106] (Example A of High Molecular Weight Water-Soluble Polymer) (1) Production of high molecular weight water-soluble polymers (cationic flocculants) Hereinafter, examples of high molecular weight water-soluble polymers (cationic flocculants) produced using the prepolymers produced in the above production examples will be specifically described. The present invention is not limited to these examples. Various analyses and evaluations were carried out by the following methods.
[0107] [Foaming] In the step of bubbling nitrogen into the monomer preparation liquid described below, the degree of foaming was visually observed and judged based on the following criteria. ○: Almost no foaming occurs (bubbling bubbles disappear quickly). △: The bubbles are a little hard to eliminate, making it difficult to continue bubbling for long periods of time. ×: Vigorous foaming and difficult bubbling (switch to nitrogen seal and continue process).
[0108] [Gel appearance] The state of the hydrogel after polymerization was visually observed and rated based on the following criteria. ○: A transparent, uniform gel was formed. △: A slightly cloudy gel was formed. ×: The gel was separated into two layers (evaluation could not be continued after that).
[0109] [0.5% salt viscosity] 500g of pure water was placed in a 500mL conical beaker, 20.8g of accurately weighed first-grade sodium chloride powder was added and dissolved, and while stirring with a magnetic stirrer, a powder sample of cationic copolymer was added, the amount of which was accurately weighed so that the concentration after dissolution was 0.5% by mass in terms of solid content, and after stirring at 200 rpm for 4 hours, the solution was left to dissolve sufficiently to prepare a 0.5% by mass solution, and the viscosity was measured at 25°C, 60 rpm, and 5 minutes later using a BM type viscometer manufactured by Tokyo Keiki Co., Ltd. In addition, when insoluble matter was visually confirmed, accurate measurement was not possible, so it was evaluated as x.
[0110] [0.1% insoluble matter] 400 g of pure water was placed in a 500 mL conical beaker, and while stirring with a magnetic stirrer, 0.4 g of each powder sample was accurately weighed and added, and after stirring for 1 hour, the solution was left to stand sufficiently to dissolve, preparing a polymer solution with a concentration of 0.1%, which was then suction filtered through an 83 mesh filter cloth, and the mass of the residue on the filter cloth was measured, and the ratio (mass%) of the residue to the total amount of the aqueous solution was calculated as the content of the insoluble matter. Note that when the insoluble matter was visually confirmed at the time of dissolution, it was evaluated as x.
[0111] [0.5% viscosity stability] A 0.5% aqueous solution was prepared in the same manner as the above 0.5% salt viscosity sample, except that the 4% sodium chloride aqueous solution was replaced with pure water. This was placed in a 500 mL glass bottle, sealed, and placed in a thermostatic bath at 80°C and heated and left undisturbed for 30 days. The viscosity was measured at 20°C and 30 rpm before and after heating and leaving undisturbed using a BM type viscometer manufactured by Tokyo Keiki Co., Ltd., and the viscosity stability was judged based on the following criteria. ○: The viscosity after heating and standing is more than 90% of the 0.5% viscosity before heating and standing. △: The viscosity after heating and standing is in the range of 80 to 90% of the 0.5% viscosity before heating and standing. ×: The viscosity after heating and standing is less than 80% of the 0.5% viscosity before heating and standing.
[0112] [Sludge dewatering test] A sludge dehydration test was carried out using each powder sample of the examples. The sludge used was organic sludge from the S sewage treatment plant. The physical properties of the sludge were pH = 5.40, TS = 34,100 (mg / L), and crude suspended solids (relative to SS) = 38.2%.
[0113] 200 mL of sludge was collected in a 300 mL beaker, and each powder sample dissolved at 0.2 mass % was added so that the powder concentration was 140 ppm, and the mixture was stirred in a jar tester for 30 seconds to carry out an agglomeration reaction. The flocculated sludge was poured all at once into a stainless steel sieve with an inner diameter of 75 mm, a depth of 100 mm, and an opening of 80 mesh, and gravity filtered. The volume of the filtrate was measured after 5, 10, 20, and 30 seconds using a measuring cylinder, and the liquid volume (mL) after 10 seconds was compared and evaluated. The moisture content of the dehydrated cake was measured by dehydrating the cake for 10 minutes at 1000 rpm in a laboratory centrifuge, drying it overnight in a dryer at 110°C, and then measuring the moisture content. Note that if any insoluble matter was visually confirmed at the time of dissolution of the powder sample, the test was discontinued.
[0114] (Example A1) A stainless steel tray with the inner surface coated with Teflon (registered trademark) was used as a reaction vessel, and a 78% by mass dimethylaminoethyl acrylate methyl chloride aqueous solution and a 50% by mass acrylamide aqueous solution were added as monomer components, and ion-exchanged water was further added to make the monomer concentration 58% by mass and the total amount 1.0 kg, and mixed uniformly. Prepolymer PP1 was added to the total amount of the monomer components to make it 5000 ppm, and the solution was adjusted to pH = 4 using hydrochloric acid, and this was used as a monomer preparation liquid. While maintaining the temperature at 5°C, dissolved oxygen was removed by nitrogen bubbling. Thereafter, under a nitrogen gas flow, 2,2'-azobis(2-methylpropionamidine) dihydrochloride ("V-50" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added in an amount of 200 ppm relative to the total amount of the monomer components to form a polymerization solution. Next, the light was passed through a 5 mm thick borosilicate glass (manufactured by Corning Incorporated, product name: Pyrex (registered trademark)) as a light-transmitting material, and a black light fluorescent lamp manufactured by Toshiba Corporation emitting light of 300 to 450 nm with a peak wavelength of 352 nm was used to measure 0.40 mW / cm using a UV meter UIT-150 (UVD-S365) manufactured by Ushio Inc. 2 The polymerization solution was then exposed to light to initiate polymerization. After the start of exposure, the light was irradiated for 15 minutes, and then the intensity was increased to 0.65 mW / cm 2 The lamp conditions were then switched to 2.0 mW / cm, and light irradiation was continued for 15 minutes. 2 The lamp conditions were changed so that the light irradiation was continued for 30 minutes to obtain a hydrous gel-like material. The hydrous gel-like material was chopped, dried and pulverized to obtain a powder sample A1 of a high molecular weight water-soluble polymer. The physical properties of powder sample A1 were evaluated according to the above-mentioned analysis and evaluation methods. The results are shown in Table 2.
[0115] (Examples A2 to A14, Comparative Examples AC1 to AC6) Powder samples A2 to A14 and AC1 to AC6 of high molecular weight water-soluble polymers were produced and evaluated in the same manner as in Example A1, except that the type and amount of prepolymer and the types and amounts of other components were changed as shown in Table 2. The results are shown in Table 2.
[0116] [Table 2]
[0117] [Table 3]
[0118] In Comparative Examples AC1 to AC5, since no prepolymer was used, the solubility in water was significantly poor or the 0.5% salt viscosity was high. In Comparative Example AC6, although a prepolymer was used, the prepolymer did not have a structure derived from an exchange chain transfer mechanism type regulator at the end, so the solubility in water was significantly poor. In contrast, in Examples A1 to A14, a prepolymer having a structure derived from an exchange chain transfer mechanism type regulator at the end was used as a macro chain transfer agent to produce a high molecular weight water-soluble polymer, so that the polymer flocculant showed excellent properties.
[0119] (High Molecular Weight Water-Soluble Polymer Example B) (2) Production of high molecular weight water-soluble polymers (anionic gelling agents) Hereinafter, examples of high molecular weight water-soluble polymers (anionic gelling agents) produced using the prepolymers produced in the above production examples will be specifically described. The present invention is not limited to these examples. Various analyses and evaluations were carried out by the following methods.
[0120] [Foaming] In the step of bubbling nitrogen into the monomer preparation liquid described below, the degree of foaming was visually observed and judged based on the following criteria. ○: Almost no foaming occurs (bubbling bubbles disappear quickly). △: The bubbles are a little hard to eliminate, making it difficult to continue bubbling for long periods of time. ×: Vigorous foaming and difficult bubbling (switch to nitrogen seal and continue process).
[0121] [Gel appearance] The state of the hydrogel after polymerization was visually observed and rated based on the following criteria. ○: A transparent, uniform gel was formed. △: A slightly cloudy gel was formed. ×: The gel was separated into two layers (evaluation could not be continued after that).
[0122] [0.2% viscosity] 400 g of pure water was placed in a 500 mL conical beaker, and while stirring with a magnetic stirrer, 0.8 g of each accurately weighed powder sample was added. After stirring for 1 hour, the mixture was left to stand sufficiently to dissolve, preparing a 0.2% polymer aqueous solution. The viscosity was measured at 20°C and 30 rpm using a BM type viscometer manufactured by Tokyo Keiki Co., Ltd.
[0123] [0.2% insoluble matter] A 0.2% aqueous polymer solution prepared in the same manner as in the measurement of the 0.2% viscosity was subjected to suction filtration through a 140 mesh filter cloth, and the mass of the residue on the filter cloth was measured. The ratio (mass%) of the residue to the total amount of the aqueous solution was calculated as the content of insoluble matter.
[0124] [0.2% viscosity stability] A 0.2% aqueous solution was prepared in the same manner as in the measurement of the 0.2% viscosity described above. This was placed in a 500 mL glass bottle, sealed, and placed in a thermostatic bath at 80°C and heated and left undisturbed for 30 days. The viscosity was measured at 20°C and 30 rpm using a BM type viscometer manufactured by Tokyo Keiki Co., Ltd. before and after heating and leaving undisturbed, and the viscosity stability was evaluated based on the following criteria. ○: The viscosity after heating and standing is more than 90% of the 0.2% viscosity before heating and standing. △: The viscosity after heating and standing is in the range of 80 to 90% of the 0.2% viscosity before heating and standing. ×: The viscosity after heating and standing is less than 80% of the 0.2% viscosity before heating and standing.
[0125] (Example B1) A stainless steel tray with the inner surface coated with Teflon (registered trademark) was used as a reaction vessel, and an aqueous solution of acrylic acid, an aqueous solution of sodium acrylate, and ion-exchanged water were charged so that the monomer concentration was 36 mass%, the total amount was 1160 g, and the compositions of acrylic acid and sodium acrylate were 51 mol% and 49 mol%, respectively. Prepolymer PP2 was added to this in an amount of 5000 ppm relative to the total amount of the monomer components to prepare a monomer preparation liquid. While maintaining the temperature at 8°C, dissolved oxygen was removed by nitrogen bubbling. Thereafter, under a nitrogen gas flow, 2,2'-azobis(2-methylpropionamidine) dihydrochloride ("V-50" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added in an amount of 1000 ppm relative to the total amount of the monomer components to form a polymerization solution. Next, the light was passed through a 5 mm thick borosilicate glass (manufactured by Corning Incorporated, product name: Pyrex (registered trademark)) as a light-transmitting material, and a black light fluorescent lamp manufactured by Toshiba Corporation emitting light of 300 to 450 nm with a peak wavelength of 352 nm was used to measure 0.40 mW / cm using a UV meter UIT-150 (UVD-S365) manufactured by Ushio Inc. 2 The polymerization solution was then exposed to light to initiate polymerization. After the start of exposure, the light was irradiated for 15 minutes, and then the intensity was increased to 0.65 mW / cm 2 The lamp conditions were then switched to 2.0 mW / cm, and light irradiation was continued for 15 minutes. 2 The lamp conditions were changed so that the light irradiation was continued for 30 minutes to obtain a hydrous gel-like material. The hydrous gel-like material was chopped, dried and pulverized to obtain the desired powder sample B1 of the high molecular weight water-soluble polymer. The physical properties of powder sample B1 at each step of the production were evaluated according to the above-mentioned analysis and evaluation methods. The results are shown in Table 3.
[0126] (Examples B2 to B9, Comparative Examples BC1 to BC4) Powder samples B2 to B9 and BC1 to BC4 of high molecular weight water-soluble polymers were produced and evaluated in the same manner as in Example B1, except that the type of prepolymer and the types and amounts of other components were changed as shown in Table 3 of Example B. The results are shown in Table 3.
[0127] [Table 4]
[0128] Comparative Examples BC1 to BC3 did not use a prepolymer, and therefore the solubility in water was extremely poor, or the 0.2% viscosity was high, and the viscosity stability was also low. Comparative Example BC4 used a prepolymer, but the prepolymer did not have a structure derived from an exchange chain transfer mechanism type regulator at the end, and therefore the solubility in water was extremely poor. In contrast, Examples B1 to B9 produced high molecular weight water-soluble polymers using a prepolymer having a structure derived from an exchange chain transfer mechanism type regulator at the end as a macro chain transfer agent, and therefore showed excellent properties as a polymer flocculant. [Industrial Applicability]
[0129] By using the prepolymer of the present invention as an intermediate raw material, it becomes possible to impart any desired properties to high molecular weight water-soluble polymers that have been produced in the past. Therefore, the prepolymer can be used not only as a polymer flocculant, but also in a wide range of applications such as adhesives, paints, industrial rubbers, coating agents, etc.
Claims
1. 1. A prepolymer for the preparation of a high molecular weight water-soluble polymer, comprising: It is a prepolymer obtained by radical polymerization of a monomer component in the presence of a chain exchange transfer mechanism type control agent, A prepolymer having a structure derived from the exchange chain transfer mechanism regulator at its terminal.
2. 2. The prepolymer of claim 1, wherein the exchange chain transfer mechanism type control agent is a reversible addition-fragmentation chain transfer agent (RAFT agent).
3. The reversible addition-fragmentation chain transfer agent (RAFT agent) is represented by the following formula (1): 【Chemistry 1】 (In the formula (1), R 3 and R 4 represents an alkyl group which may have a substituent, an aryl group which may have a substituent, a heteroaryl group which may have a substituent, or an aralkyl group which may have a substituent. The prepolymer according to claim 2 , comprising a trithiocarbonate compound represented by the formula:
4. 2. The prepolymer according to claim 1, which has a weight average molecular weight (Mw) of 1,000 to 300,000 as measured by gel permeation chromatography (GPC).
5. 5. A high molecular weight water-soluble polymer obtained by radical polymerization of a monomer component in the presence of the prepolymer according to claim 1.
6. The high molecular weight water-soluble polymer according to claim 5 , which is a polymer obtained by polymerization by irradiation with active energy rays.
7. The high molecular weight water-soluble polymer of claim 5 , wherein the high molecular weight water-soluble polymer is a polymeric flocculant.