Separator for power storage device

A three-layer polyimide porous membrane with tailored pore diameters and surface properties addresses productivity and wettability issues, enhancing performance in power storage devices at higher temperatures.

JP2024159357AInactive Publication Date: 2024-11-083DOM ALLIANCE INC

Patent Information

Application Number
JP2023081124
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The production of polyimide porous membranes for separators in power storage devices is less productive compared to polyolefin porous membranes, and existing electrolytes with increased viscosity at higher temperatures affect the wettability and performance of separators.

Method used

A polyimide porous membrane with a three-layer structure, featuring specific pore diameters and surface properties, is developed to enhance wettability and permeability, allowing use at higher temperatures.

Benefits of technology

The polyimide porous membrane provides improved wettability and permeability, enabling effective use in power storage devices at elevated temperatures, such as 60°C, with optimized porosity and thickness for enhanced performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159357000001
    Figure 2024159357000001
  • Figure 2024159357000002
    Figure 2024159357000002
Patent Text Reader

Abstract

To provide a separator for a power storage device which is preferable for use at higher temperatures.SOLUTION: The separator for a power storage device according to the present invention has a three-layer structure including an intermediate layer and a surface layer on both sides of the intermediate layer and is formed of a polyimide porous membrane obtained by removing fine particles and forming small holes in the surface layers and the intermediate layer. The largest hole diameter of the surface layers is at least 600 nm. Also, the surface aperture ratio of the surface layers is preferably at least 20%. The average small hole diameter (average flow hole diameter) of the separator is at least 250 nm. The porosity of the separator is at least 67% in the surface layer and is 60% at largest in the intermediate layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a separator used in an electricity storage device such as a lithium ion battery or a lithium ion capacitor. [Background technology]

[0002] In recent years, electricity storage devices such as lithium-ion batteries and capacitors have become widespread. Among these, remarkable advances have been made in the technologies of lithium-ion batteries and lithium-ion capacitors, which use graphite as the anode, and lithium-metal batteries, which use metallic lithium as the anode. These electricity storage devices have a structure in which a positive electrode, a separator, and a negative electrode are stacked in this order, filled with an electrolyte, and the positive electrode and the negative electrode are insulated by a separator. For example, metallic lithium, an alloy of lithium and other metals, carbon, graphite, etc. are often used as the negative electrode.

[0003] In particular, the use of polyimide porous membranes, which have relatively high heat resistance, as separators in electricity storage devices has been considered. However, compared with polyolefin porous membranes, the production of polyimide porous membranes requires more time and effort, making it difficult to improve productivity. In response to this, Patent Document 1 discloses a method for producing a polyimide porous film that is simpler and more productive than conventional methods by using resin particles. [Prior art documents] [Patent documents] [Patent Document 1] Patent No. 6358663 Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, electrolytes in which ethylene carbonate (EC) or methyl ethyl carbonate (MEC) is added with LiPF6 as a lithium salt at a concentration of 1M are often used, but in order to enable use at higher temperatures, the composition of the electrolyte is sometimes modified by using propylene carbonate as a solvent or by adding vinylene carbonate. When the composition of the electrolyte is modified to enable use at higher temperatures, as described above, it is known that the viscosity of the electrolyte increases from the conventional viscosity of around 5 mPa·s. However, when an electrolyte with a viscosity of, for example, 30 mPa·s is used, there is a problem in that it is difficult to impregnate the polyolefin separator with the electrolyte. The present invention has been made in view of the above circumstances, and has been made with the object of providing a separator for an electricity storage device that is suitable for use at higher temperatures. [Means for solving the problem]

[0005] In order to achieve the above-mentioned object, the polyimide porous film of the present invention has the following constitutions [1] to [3].

[0006] [1] The separator for an electricity storage device of the present invention comprises: A separator for an electricity storage device, which has a three-layer structure in which surface layers are layered on both sides of an intermediate layer, and is made of a polyimide porous film in which fine particles are removed to form interconnected pores in the surface layers and the intermediate layer, The maximum pore size of the surface layer is 600 nm or more. In particular, when 1.0 μL of an electrolyte solution having a viscosity of 30 mPa·s is dropped onto the surface layer, the contact angle 65 milliseconds after the electrolyte solution lands is preferably 90 degrees or less. This contact angle is more preferably 85 degrees or less, even more preferably 80 degrees or less, and even more preferably 75 degrees or less. The smaller the contact angle, the easier it is for the electrolyte to wet, which is preferable. Although an electrolyte solution having a viscosity of 30 mPa·s at 20°C is given as an example, any electrolyte solution having a viscosity of 10 mPa·s or higher will suffice, and the wettability of the separator should be evaluated using an electrolyte solution having a viscosity of preferably 20 mPa·s or higher, more preferably 30 mPa·s or higher, and even more preferably 40 mPa·s or higher. Alternatively, a liquid absorption test of the solvent constituting the electrolyte may be used. For example, a known method may be used, such as measuring the time it takes for a solvent such as ethylene carbonate, ethyl methyl carbonate, or propylene carbonate constituting the electrolyte to completely penetrate under predetermined conditions, or measuring the liquid absorption height of the solvent. When it is difficult to measure the contact angle, the above-mentioned liquid absorption test can be used to evaluate wettability or impregnation.

[0007] [2] Furthermore, when measuring the contact angle, it is recommended to use an electrolyte solution with a composition in which 1.5 mol / L LiFSI is dissolved in a mixed solvent of ethylene carbonate and propylene carbonate (for example, a 1:1 volume ratio). The composition of the electrolyte solution is not limited to this; it is recommended to change it appropriately to a composition with a viscosity of 10 mPa·s or more at room temperature (20°C), as explained above. When evaluating the wettability of a separator, it is often easier to clearly distinguish between high-viscosity electrolyte solutions and low-viscosity ones. Note that the electrolyte composition used when actually fabricating an energy storage device does not need to be the one described above; it is recommended to use one that suits the user's needs.

[0008] [3] Moreover, it is desirable that the surface opening ratio of the surface layer is 20% or more. The average pore size (also called the mean flow pore size) of the separator is preferably 250 nm or more. The larger the average pore diameter, the better the electrolyte wettability, so if you want to improve wettability, it's a good idea to increase the average pore diameter as well. Increasing the surface opening rate and average pore diameter makes it possible to further improve the electrolyte's permeability. The degree of tortuosity can also be designed according to the purpose. For example, if you want to improve the mobility of Li ions from one surface to the other, it's a good idea to minimize the number of tortuosities, or to reduce the degree of curvature. The porosity of the separator is preferably 67% or more for the surface layer and 60% or less for the intermediate layer. [Effects of the Invention]

[0009] For example, a separator for an electricity storage device suitable for use at higher temperatures such as 60°C can be provided. DETAILED DESCRIPTION OF THE INVENTION

[0010] The polyimide porous membrane of the present invention, which is made of a copolymer of a carboxylic acid and a diamine, may be used as a separator for an electricity storage device such as a lithium ion battery, a lithium metal battery, or a capacitor, or may be used for other purposes, and there is no limitation on the use thereof.

[0011] When the polyimide porous membrane of the present invention is used as a separator for an electricity storage device, the porosity by weight is preferably 45 to 75%, and the Gurley value (air permeability) is preferably 300 seconds or less. If the porosity is 45% or more, for example, the Gurley value can be 300 seconds / 100 cc or less at a membrane thickness of 20 μm, and a separator that is preferable not only from the viewpoint of the Li reaction amount described later but also from the viewpoint of the Gurley value can be provided. Increasing the porosity can reduce the Gurley value, but the higher the porosity, for example, above 70%, the weaker the polyimide porous membrane becomes, which can lead to damage during actual battery manufacturing, making it difficult to assemble batteries using polyimide porous membranes with a porosity of 80% or more.

[0012] The thickness of the polyimide porous film is preferably, for example, about 4 μm to 50 μm. If the thickness of the polyimide porous film is too thick, the ion conductivity tends to decrease. This is also related to the short-circuit resistance, and the thinner the film, the less insulating properties can be maintained. If the polyimide porous film is too thin, the film strength decreases. Furthermore, the maximum stress of the polyimide porous film is 25 N / mm 2 It is preferable that this is equal to or greater than this.

[0013] The polyimide porous membrane of the present invention can be produced by a known method, such as chemical imidization or imidization of polyamic acid by heating, and can be produced by the following steps: a step of preparing a slurry by mixing fine particles for forming holes into a polyimide precursor solution containing polyamic acid (so-called polyimide varnish) made from a carboxylic acid anhydride and an organic amine compound; a step of forming a thin film of the prepared slurry on a support to form a non-porous raw sheet; peeling the raw sheet from the support; A step of firing the raw sheet to make it porous. The removal of the fine particles for forming holes and the imidization of the raw sheet can be carried out simultaneously, but the fine particles can also be removed from the raw sheet, holes can be formed, and then the imidization can be carried out.

[0014] [Slurry preparation] The polyimide precursor solution contains polyamic acid prepared from a carboxylic acid anhydride and an organic amine compound. A polyimide precursor solution can be prepared by mixing polyamic acid or a mixture of polyamic acid and a solvent with fine particles for forming openings to prepare a slurry. The polyimide precursor solution may be a solution obtained by polymerizing a tetracarboxylic acid dianhydride and a diamine in the presence of an organic solvent, or a solution obtained by dissolving a polyamic acid in an organic solvent.

[0015] A slurry for film formation is prepared by mixing a polyimide precursor solution, microparticles for pore formation, a dispersant, a solvent, etc. This slurry can be formed into a thin film to produce a non-porous base fabric. A dispersant is not essential, but can be used as needed. The material of the pore-forming particles may be any material as long as it is insoluble in the organic solvent used in the polyimide precursor solution and can be selectively removed after film formation. For example, fine particles made of inorganic materials include silica (silicon dioxide), titanium oxide, and metal oxides such as alumina (Al2O3). Examples of microparticles made of organic materials include microparticles (hereinafter referred to as resin microparticles) made of organic polymers such as polyolefins such as polypropylene and polyethylene, polystyrene (PS), acrylic resins (e.g., methyl methacrylate, isobutyl methacrylate, polymethyl methacrylate (PMMA), etc.), polyurethane resin (PUR), melamine resin (MF), urea resin (UF), phenolic resin (PF), epoxy resin, cellulose, polyvinyl alcohol, polyvinyl butyral, polyvinyl acetate (PVAc), ABS resin, AS resin, polyacrylonitrile (PAN), polycarbonate (PC), polyamide (PA), polyethylene terephthalate (PET), polyester, and polyether.

[0016] There are no limitations on the shape of the fine particles, but spherical or nearly spherical shapes are desirable. Basically, a shape close to a perfect sphere is desirable, but a nearly spherical shape such as an elliptical shape with some distortion or fine irregularities may also be acceptable. Furthermore, fine particles that are nearly spherical and have a small particle size distribution index (small particle size variation) are preferred. By using fine particles that satisfy these conditions, it is possible to reduce the variation in the pore size of the pores formed in the polyimide porous film. This allows lithium to move more uniformly on the separator when the polyimide porous membrane is used as a separator for an electricity storage device. The particle size of the fine particles is preferably 800 nm or less. This allows the pore size of the porous membrane obtained by removing the fine particles to be 800 nm or less. The particle size of the fine particles is more preferably 600 nm or less, and even more preferably 500 nm or less.

[0017] A dispersant may be added to the polyimide precursor solution in order to uniformly disperse the fine particles in the polyimide precursor solution. By adding a dispersant, the polyamic acid and the fine particles can be mixed more uniformly, and the fine particles can be distributed more uniformly in the raw sheet described below. By distributing the fine particles uniformly, the pore distribution can be made more uniform in the polyimide porous film finally obtained by removing the fine particles.

[0018] <Carboxylic acid anhydrides and polyamic acids> The polyamic acid may be one obtained by polymerizing a carboxylic dianhydride and a diamine. The amounts of the carboxylic dianhydride and diamine used are not particularly limited, but the amount of diamine used is preferably 0.50 to 1.50 mol, more preferably 0.60 to 1.30 mol, and particularly preferably 0.70 to 1.20 mol per mol of the carboxylic dianhydride. The carboxylic acid dianhydride may be appropriately selected from those conventionally used as raw materials for synthesizing polyamic acid. The carboxylic acid dianhydride may be an aromatic tetracarboxylic acid dianhydride or an aliphatic tetracarboxylic acid dianhydride, but from the viewpoint of the heat resistance of the resulting polyimide resin, it is preferable to use an aromatic tetracarboxylic acid dianhydride. Two or more types of carboxylic acid dianhydrides may be used in combination.

[0019] Specific preferred examples of the aromatic tetracarboxylic dianhydride include pyromellitic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, oxydiphthalic dianhydride, 2,2-bis(2,3-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, carboxylic dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride, benzophenonetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,3,4-benzenetetracarboxylic dianhydride, diphthalic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 1,2,7,8-phenanthrenetetracarboxylic dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, and the like. Examples of the aliphatic tetracarboxylic dianhydride include ethylene tetracarboxylic dianhydride, butane tetracarboxylic dianhydride, cyclopentane tetracarboxylic dianhydride, cyclohexane tetracarboxylic dianhydride, 1,2,4,5-cyclohexane tetracarboxylic dianhydride, 1,2,3,4-cyclohexane tetracarboxylic dianhydride, etc. It is particularly preferable to include at least one of biphenyl tetracarboxylic dianhydride and oxydiphthalic dianhydride as the carboxylic dianhydride.

[0020] <Organic amine compounds> The diamine, which is an organic amine compound, may be appropriately selected from diamines conventionally used as raw materials for synthesizing polyamic acids. The diamine may be an aromatic diamine or an aliphatic diamine, and may be appropriately selected in consideration of the properties of the target polyimide resin, but aromatic diamines are preferred. Two or more diamines may also be used in combination.

[0021] Examples of aromatic diamines include phenylenediamine and derivatives thereof, diaminobiphenyl compounds and derivatives thereof, diaminodiphenyl compounds and derivatives thereof, diaminotriphenyl compounds and derivatives thereof, diaminonaphthalene and derivatives thereof, aminophenylaminoindan and derivatives thereof, diaminotetraphenyl compounds and derivatives thereof, diaminohexaphenyl compounds and derivatives thereof, and cardo-type fluorenediamine derivatives.

[0022] Specific examples of diamines based on the number of benzene rings are as follows: 1) to 4): 1) Benzenediamine with one benzene nucleus 2,4-diaminotoluene, phenylenediamine, 2,6-diaminotoluene, etc.

[0023] 2) Diamine with two benzene rings 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dicarboxy-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, bis(4-aminophenyl) sulfide, 4,4'-Diaminobenzanilide, dimethylbenzidine, 3,3'-dimethoxybenzidine, 2,2'-dimethoxybenzidine, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, oxydianiline, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl diphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminobenzophenone, 3,3'-diamino-4,4'-dichlorobenzophenone, 3,3'-diamino-4,4'-dimethoxybenzophenone, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 2,2-bis(3-aminophenyl)propane, 2, 2-bis(4-aminophenyl)propane, 2,2-bis(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diamino-3,3'-dimethyldiphenylmethane, 4,4'-diaminodiphenyl sulfoxide, and the like.

[0024] 3) Diamine with three benzene rings 1,3-bis(3-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(3-aminophenyl)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenoxy)benzene, etc.

[0025] 4) Diamine with four benzene rings 3,3'-bis(3-aminophenoxy)biphenyl, bis[3-(3-aminophenoxy)phenyl]methane, bis[3-(4-aminophenoxy)phenyl]methane, 9,9-bis(4-aminophenyl)fluorene, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(4-aminophenoxy)phenyl]methane, 2,2-bis[3-(3-aminophenoxy)phenyl]propane, 2,2-bis[3-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and the like.

[0026] <Organic solvents> The reaction between tetracarboxylic dianhydride and diamine is generally carried out in an organic solvent. The organic solvent used in the reaction between tetracarboxylic dianhydride and diamine is not particularly limited as long as it can dissolve the tetracarboxylic dianhydride and diamine and does not react with the tetracarboxylic dianhydride and diamine. The organic solvent may be used alone or in combination of two or more, and may be selected appropriately. Examples of organic solvents used in the reaction of tetracarboxylic dianhydride with diamine include N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-diethylacetamide, N,N-dimethylformamide, N,N-diethylformamide, N-methylcaprolactam, β-propiolactone, γ-butyrolactone, dimethyl sulfoxide, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, dioxane, phenolic solvents, cyclic ketones such as cyclopentanone and cyclohexanone, aromatics such as toluene and xylene, and alicyclic compounds such as cyclopentane and cyclohexane. These organic solvents can be used alone or in combination. There are no particular limitations on the amount of organic solvent used, but it is desirable that the content of the resulting polyamic acid be 5 to 50% by mass.

[0027] The organic solvent used in the polyimide precursor solution may be any solvent that dissolves the polyamic acid or polyimide resin used but does not dissolve the fine particles. Of all the components in the polyimide precursor solution, the content of the organic solvent is preferably 50 to 95 mass %, more preferably 60 to 85 mass %, and the solid content in the polyimide precursor solution is preferably 5 to 50 mass %, more preferably 15 to 40 mass %. In addition to the above components, the polyimide precursor solution may contain an appropriate amount of additives such as an antistatic agent, a flame retardant, a chemical imidizing agent, a condensing agent, a release agent, a surface conditioner, and a dimensional stabilizer, for the purposes of preventing static buildup, imparting flame retardancy, low-temperature baking, releasability, coatability, low moisture absorption, a low coefficient of linear expansion, reduced thermal shrinkage, and the like.

[0028] The specific manufacturing procedures for the polyimide porous membrane are as follows (1) to (6). However, when the raw sheet is made porous using inorganic particles such as silica, the raw sheet must be immersed in a solvent to remove the inorganic particles, making it difficult to simultaneously perform the porosity-making step and the firing step. In this case, it is desirable to perform the porosity-making step before the firing step. On the other hand, when resin particles are used to make the raw sheet porous, the porous forming step and the firing step can be carried out simultaneously, which makes it possible to further simplify and compact the manufacturing process. The procedure for producing a polyimide porous membrane is as follows: (1) preparing a polyimide precursor solution having a polyamic acid synthesized from a carboxylic acid anhydride and an organic amine compound; (2) preparing a slurry by mixing a polyimide precursor solution with fine particles; (3) a raw sheet forming step of coating the slurry on a support to form a non-porous raw sheet; (4) a peeling step of peeling the raw fabric formed in the raw fabric forming step from the support; (5) a porous forming step of forming porous material on the raw sheet peeled from the support in the peeling step; and (6) Firing process for firing the raw fabric.

[0029] [Preparation of polyimide precursor solution] As described above, polyamic acid can be obtained by polymerizing a carboxylic acid dianhydride and an organic amine compound. The polyamic acid can be imidized by applying heat (thermal imidization) or chemically imidized (chemical imidization) to form a polyimide by ring closure of the carboxylic acid moiety. The imidization rate is preferably about 80% or more, more preferably 85% or more, more preferably 90% or more, and even more preferably 95% or more, but this can also be adjusted according to the desired physical properties.

[0030] As described above, the present invention provides a polyimide porous membrane composed of a copolymer of carboxylic acid and diamine, having numerous interconnected pores formed by removing fine particles, characterized in that the carboxylic acid is contained in a molar ratio of more than 70% BPDA to less than 30% ODPA. The ratio of BPDA to ODPA is not limited to more than 70% BPDA to less than 30% ODPA, but is preferably, for example, 80% or more BPDA to 20% or less ODPA, more preferably 87% or more BPDA to less than 13% ODPA, and even more preferably 85% or more BPDA to 15% or less ODPA. As described above, the carboxylic acid preferably contains both biphenyltetracarboxylic acid and oxydiphthalic anhydride, but may further contain at least one selected from benzophenonetetracarboxylic dianhydride and 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride. When it is desired to increase the initial Coulomb efficiency in a lithium ion battery or a lithium metal battery by using the porous membrane of the present invention as a separator, a polyimide that can further reduce the property of adsorbing or reacting with Li is preferred.

[0031] Regarding the diamine, among o-phenylenediamine, m-phenylenediamine and p-phenylenediamine, m-phenylenediamine and p-phenylenediamine are preferred, and p-phenylenediamine is more preferred. Diaminodiphenylmethane includes 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, and 4,4'-diaminodiphenylmethane, with 4,4'-diaminodiphenylmethane being particularly preferred. Generally, the diamine is preferably at least one selected from p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diamino-3,3'-dimethyldiphenylmethane, o-dianisidine, 9,9-bis(4-aminophenyl)fluorene, etc. One type of diamine may be used, or two or more types may be mixed.

[0032] As described above, for example, an organic polar solvent can be used as a solvent for polymerizing polyamic acid, and preferred organic polar solvents include, for example, tetramethylurea, phenol, N-methyl-2-pyrrolidone (NMP), pyridine, N,N-dimethylacetamide (DMAc), N,N-dimethylformamide, p-chlorophenol, o-chlorophenol, dimethyl sulfoxide, and cresol.

[0033] Other conditions for producing polyamic acid include, for example, reacting tetracarboxylic dianhydride and diamine in approximately equimolar amounts (approximately equimolar amounts) at a temperature of preferably about 80°C or less, more preferably 70°C or less, even more preferably 0 to 65°C, and particularly preferably 10 to 60°C. The reaction time is preferably about 0.1 hour or more, more preferably 0.2 to 72 hours, and even more preferably 0.5 to 60 hours, to produce polyamic acid. When producing the polyimide precursor solution, a component for adjusting the molecular weight can also be added to the reaction solution. The prepared polyimide precursor solution contains, for example, 5 to 50% by mass of polyamic acid and 50 to 95% by mass of an organic polar solvent. If the content of polyamic acid is less than 5% by mass, the strength of the porous polyimide film produced will decrease, while if it exceeds 50% by mass, the viscosity of the porous polyimide film will be too high, making it difficult to handle.

[0034] [Slurry preparation] A slurry is prepared by mixing the polyimide precursor solution, fine particles, etc., to which an organic solvent for adjusting the concentration, as well as the additives already mentioned, such as antistatic, low-temperature baking, mold releasability, coatability, low moisture absorption, low linear expansion coefficient, and chemical imidization agents, may be added as appropriate. The slurry is made up of 5 to 90% by mass of polyimide precursor solution, 2 to 40% by mass of fine particles for opening pores, 0 to 95% by mass of organic solvent for adjusting the concentration, and additives, although not particularly limited, preferably 0 to 20% by mass, and is mixed in a stirring device, preferably a planetary centrifugal mixer such as the "Thinky Mixer" (Thinky Corporation).

[0035] The solution viscosity of the slurry can be determined appropriately depending on the characteristics of the die and coater machine used for coating. For example, from the viewpoint of ease of coating and film strength, a viscosity of about 0.1 to 1000 Pa·s, preferably 0.5 to 300 Pa·s, and more preferably 1 to 250 Pa·s can be used with various dies and coater machines.

[0036] [Original fabric formation process] The prepared slurry can be coated onto a support to form a base roll. There are no particular limitations on the coating method, and for example, a slurry blade or a T-die can be used to coat onto a support such as a glass plate, a stainless steel plate, a PET (polyethylene terephthalate) film, or a PEN (polyethylene naphthalate) film. This allows the formation of a raw sheet in which the slurry is spread in a layer on the support. Furthermore, as the support, an endless mechanism such as a metal belt or a resin film may be used. The support may be any material that is not affected or is less affected by the prepared slurry. For an endless mechanism, a metal such as stainless steel may be used, and for a resin film, a resin such as PET or polytetrafluoroethylene may be used. When producing a polyimide porous film with a multilayer structure, a feedblock or multi-manifold die may be used as the T-die. The present invention may also be applied to a polyimide porous film having a multilayer structure. By applying the present invention to, for example, the surface layer or the intermediate layer of the multilayer structure, it is possible to provide a multilayer polyimide porous film that achieves all physical properties such as maximum stress, elongation, and elastic modulus at higher levels than conventionally possible.

[0037] [Peeling process] After forming the raw roll on the support, the raw roll is peeled off from the support at an appropriate timing before the firing step. There is no particular limitation on the length of the raw roll, but from the viewpoint of productivity, it is preferably long (for example, 5 m or more), more preferably 10 m or more, and even more preferably 20 m or more. There is no particular limitation on the upper limit of the length of the raw roll, but for example, it is 4000 m or less, and typically 1000 m or less makes the raw roll easier to handle. It is advisable to properly dry the raw roll to make it easier to peel off the raw roll from the support.

[0038] [Porous process] By selecting an appropriate method to remove the fine particles from the raw film peeled from the support, a polyimide porous film having spherical or nearly spherical pores can be produced. Methods for removing the fine particles include dissolving the fine particles in a solvent, acid, or alkali, or removing the fine particles by baking, but this method depends on the fine particles used. Considering productivity and cost, resin particles are preferred as the fine particles for forming the pores. When inorganic particles such as silica are used as the porous particles, they can be removed by dissolving them in contact with an acid or alkali. When the fine particles are resin particles, the resin particles can be dissolved and removed by an organic solvent that does not dissolve the polyimide film but dissolves the resin particles. Examples of such organic solvents include ethers such as tetrahydrofuran; aromatics such as toluene; ketones such as acetone; and esters such as ethyl acetate. Among these, ethers such as tetrahydrofuran are preferred, and tetrahydrofuran is more preferred. In addition, in the case of resin fine particles, openings can be formed by heating the resin fine particles to a temperature above the thermal decomposition temperature of the resin fine particles and below the thermal decomposition temperature of the polyimide resin, thereby decomposing and removing the resin fine particles.

[0039] [Firing process] The obtained raw sheet or perforated raw sheet is heated to imidize it (hereinafter referred to as thermal imidization), thereby forming a polyimide porous film. The shrinkage rate of the polyimide porous film after thermal imidization should be controlled to 5% or less in the machine direction (MD) and also 5% or less in the transverse direction (TD). There are no particular limitations on the means or method for controlling the shrinkage rate, but it is recommended to reduce the tension applied to the raw sheet or the film after perforation. The temperature conditions are, for example, in the range of 250 to 500° C. and the firing time is 1 to 300 minutes, preferably 5 to 240 minutes, and more preferably 10 to 120 minutes. To increase productivity, it is desirable to keep the heating and firing time as short as possible. In this thermal imidization treatment, the temperature rise rate is desirably 20°C / min or more, preferably 30°C / min or more, in a temperature range of 200°C or higher. By heating at the above temperature rise rate in the temperature range of 100 to 250°C, where the imidization reaction occurs significantly, it is possible to obtain a porous polyimide film of the present invention with significantly improved surface opening ratio and pore size.

[0040] The baking temperature varies depending on the type of polyamic acid and the desired degree of imidization, but is preferably 120 to 500°C, more preferably 150 to 500°C. When firing, the drying process and the firing process may be separated, or may not be strictly separated. For example, when firing at 360°C, there are methods of continuously raising the temperature from room temperature to 360°C and then firing at 360°C for several tens of minutes, and methods of raising the temperature stepwise from room temperature to 360°C and then firing at 360°C for several tens of minutes. A suitable procedure can be selected. The raw sheet can be peeled off from the support at an appropriate timing during the temperature rise from room temperature.

[0041] The baked polyimide porous film may be wound around a core having a diameter of, for example, 2.5 cm (1 inch) to 25 cm (10 inches). The diameter of the core is preferably 5 cm (2 inches) to 10 cm (4 inches). There are no particular restrictions on the material of the core, but examples include paper, metals such as stainless steel, and hard plastics such as ABS, PP, PE, PVC, PET, FRP, and Bakelite.

[0042] When the baking process also serves to remove the resin particles, if the organic material constituting the resin particles decomposes at a lower temperature than the polyimide, the resin particles alone can be removed without thermally damaging the polyimide. For this reason, the decomposition temperature of the resin particles is preferably, for example, 120°C or higher and 500°C or lower.

[0043] The polyimide porous membrane produced by the above procedure has a plurality of spherical or nearly spherical pores formed therein, at least some of which are interconnected. The pore sizes on the surface and inside of the polyimide porous membrane can be controlled by appropriately selecting or adjusting the type and size of the microparticles used in producing the film. In the polyimide porous membrane of the present invention, it is preferable that the pores have little variation in pore size and a more uniform distribution. As an index showing the small variation in pore size and distribution within the film, a method can be used in which the Gurley value of the film is measured at several points in different locations and the variation in the values ​​is evaluated. At 10 arbitrary points on the polyimide porous membrane, the air permeability (the number of seconds it takes 100 mL of air to permeate the film) can be measured by the Gurley method in accordance with JIS P 8117, and the average air permeability and standard deviation can be determined.

[0044] A film having pores with small variations in pore size and distribution can be produced by using fine particles with a high sphericity and a small particle size distribution index during film production, or by adjusting the viscosity of a polyimide precursor solution containing fine particles and a polyamic acid or polyimide resin to an appropriate viscosity that enables uniform application. The air permeability measured by the Gurley method as described above is preferably 400 seconds or less, more preferably 300 seconds or less, and even more preferably 250 seconds or less. It is believed that such an air permeability allows lithium and lithium ions to migrate with lower resistance.

[0045] When the polyimide porous film of the present invention is used as a battery separator, the film thickness is preferably 2 μm to 100 μm, more preferably 3 μm to 80 μm, and even more preferably 4 μm to 50 μm. The film thickness can be determined by measuring the thickness at multiple points with a micrometer or the like and averaging the measured values.

[0046] The above has described the manner of producing a polyimide porous film having a single layer structure. Below, a procedure for producing a polyimide porous film having a multilayer structure by co-extrusion will be described. The basic manufacturing procedure is the same as for the single-layer structure described above, but the die used is different. The manufacturing procedure for the multilayer porous polyimide film is as follows: a first slurry preparation step of mixing fine particles for forming pores into a polyimide precursor solution to prepare a first slurry; a second slurry preparation step of preparing a second slurry different from the first slurry; feeding the first slurry and the second slurry into a coextrusion die; a step of continuously extruding a layer made of the first slurry and a layer made of the second slurry as an integrated thin film onto a smooth support from the discharge port of the co-extrusion die (multilayer raw sheet forming step); a step of drying the multilayer thin film on the support and peeling the multilayer thin film from the support (peeling step); and This is a process in which the multilayer thin film is heat-treated to remove fine particles and make it porous (porosity process). The multilayer thin film before perforation is also called a multilayer raw sheet.

[0047] In the multilayer polyimide porous film of the present invention, the temperature of the polyamic acid solution when extruded from the multilayer extrusion die onto the support is 0 to 150° C., preferably 5 to 100° C., and more preferably 10 to 60° C. The polyamic acid solution extruded in the form of a film is dried to some extent in order to peel it off from the support, and the drying temperature may be appropriately set within the range of 50 to 200° C., and particularly 60 to 180° C. The polyamic acid film peeled off from the support is preferably heated at a temperature of 300 to 500°C for a time of about 1 to 80 minutes, particularly about 2 to 60 minutes, to imidize the polyamic acid and remove the resin particles.

[0048] <Multilayer fabric formation process> In the multilayer raw sheet forming step, the slurry is laminated in layers on a support using a multilayer die. In this co-extrusion method, multiple types of slurries are simultaneously extruded onto a support to form a multilayered, non-porous raw sheet. The slurries come into direct contact with each other without drying, resulting in strong adhesion between the layers of the multilayered raw sheet. This not only reduces the number of steps, but also shortens the time required to form the multilayer raw material compared to the sequential coating method, and when using additives such as dehydrating agents, the risk of them remaining between the layers can be reduced compared to the sequential coating method.

[0049] As mentioned above, there are no limitations on the material of the support onto which the slurry is discharged, as long as it is smooth and does not dissolve in the slurry. Preferably, it has excellent peelability for the multilayer raw fabric. Examples include belts (endless mechanisms) made of metal such as stainless steel, resin films such as PET, and rotating drums, but the present invention is not limited to these and any suitable material may be used.

[0050] From the viewpoint of manufacturing efficiency, a rotating drum or an endless mechanism is preferable as the support, but this can also be selected appropriately. If an endless mechanism is used, it can be rotated to continuously form a multilayer raw fabric, eliminating the need to dispose of plastic films, etc., which leads to reduced manufacturing costs. When firing the multilayer raw fabric, the width of the end portions of the multilayer raw fabric may be fixed by fixing means such as tenter pins or chucks.

[0051] The present invention is configured so that multiple types of polyimide-based varnishes can be simultaneously ejected onto a support, and one means for achieving this is to use a multi-layer co-extrusion die. Compared to the method of laminating the second layer after the first layer (sequential coating method), the co-extrusion method, which forms multiple liquid films simultaneously, can improve adhesion between layers and also reduces the formation of interfaces between layers, eliminating problems such as delamination.

[0052] <Peeling process> In the peeling step, the multilayer raw sheet is peeled off from the support as a self-standing non-porous film. The conditions for peeling the multilayer raw fabric from the support are not limited, and any conditions are sufficient as long as the organic solvent can be partially evaporated from the multilayer raw fabric or a portion of the polyamic acid can be imidized to allow the multilayer raw fabric to be satisfactorily peeled from the support. The temperature for peeling the multilayer raw fabric from the support is preferably 50°C or higher and 200°C or lower, and may be appropriately set to 60°C or higher and 180°C or lower. By setting the temperature at which the multilayer raw sheet is peeled off from the support to within the range of 60 to 200°C, the multilayer raw sheet can be made more gel-like and can be more easily peeled off from the support. There is no particular limitation on the heating time, and it may be determined appropriately in consideration of the film thickness and productivity.

[0053] <Porous process> In the porosity forming process, the multilayer raw sheet peeled from the support is baked to promote imidization while burning off the resin particles and remaining solvent, thereby forming a multilayer porous polyimide film. The baking in this porosity forming process simultaneously evaporates the solvent components contained in the multilayer raw sheet, promotes the imidization reaction of the polyamic acid, and removes the resin particles. This allows the production of a multilayer porous polyimide film in which multiple polyimide porous layers are stacked.

[0054] The heating method used in the firing in this porous forming step is not particularly limited as long as it can effectively heat the multilayer raw sheet peeled off from the support. For example, a method of blowing hot air at 100°C or higher onto the entire multilayer raw sheet from the top (one side) or bottom (the other side) or both sides of the multilayer raw sheet to heat it, or a method of irradiating the raw sheet with far infrared rays may be used. The heating temperature is preferably between 200°C and 600°C, but can be determined appropriately taking into account the composition of the polyamic acid. The temperature should be increased in stages. Rapidly increasing the heating temperature can lead to uneven firing of the multilayer raw sheet, potentially affecting the smoothness of the film surface. Furthermore, if the heating temperature is too low or the heating time is too short, the resin particles may not be sufficiently burned off, potentially resulting in insufficient porosity.

[0055] [Uses of polyimide porous membrane] The polyimide porous membrane of the present invention can be used as a separator in power storage devices such as nickel-cadmium batteries, nickel-metal hydride batteries, lithium ion primary / secondary batteries using graphite as the negative electrode, and lithium metal primary / secondary batteries using metallic lithium as the negative electrode. Among these, it is preferable to use it as a separator for lithium ion secondary batteries or lithium metal secondary batteries. The polyimide porous membrane of the present invention may also be used as an electrolyte membrane for fuel cells or a substrate for electronic circuits.

[0056] An electricity storage device using the polyimide porous membrane of the present invention as a separator includes a negative electrode, a positive electrode, and an electrolyte solution in addition to the separator. There are various types of electricity storage devices, such as a wound type (cylindrical or rectangular in appearance), a laminate type, and a coin type. An electrode structure in which a positive electrode, a separator, and a negative electrode are laminated in this order is contained in an exterior body, and an electrolyte solution is injected into this exterior body to produce an electricity storage device.

[0057] The negative electrode of a lithium-ion battery has a structure in which a negative electrode mixture consisting of a negative electrode active material, a conductive additive, and a binder is formed on a current collector. Materials capable of being electrochemically doped with lithium can be used as the negative electrode active material, including carbon materials, silicon, aluminum, tin, and Wood's alloy. Lithium metal batteries, as is well known, use metallic lithium as the negative electrode.

[0058] Examples of conductive additives for the negative electrode include carbon materials such as acetylene black and ketjen black. The binder is made of an organic polymer, such as polyvinylidene fluoride or carboxymethyl cellulose. The current collector can be made of copper foil, stainless steel foil, nickel foil, or the like.

[0059] The positive electrode may have a structure in which a positive electrode mixture consisting of a positive electrode active material, a conductive additive, and a binder is formed on a current collector. For example, nickel hydroxide can be used as the positive electrode active material in nickel-cadmium batteries, and nickel hydroxide or nickel oxyhydroxide can be used in nickel-metal hydride batteries. For lithium-ion secondary batteries, examples of the positive electrode active material include lithium-containing transition metal oxides, such as LiCoO2, LiNiO2, LiMn0.5Ni0.5O2, LiCo1 / 3Ni1 / 3Mn1 / 3O2, LiMn2O4, LiFePO4, LiCo0.5Ni0.5O2, and LiAl0.25Ni0.75O2. Examples of conductive additives include carbon materials such as acetylene black and ketjen black.

[0060] Lithium-ion batteries and lithium metal batteries typically use nonaqueous electrolytes in which lithium salts are dissolved in nonaqueous solvents, but aqueous electrolytes may also be used depending on the desired properties. Examples of lithium salts include LiPF6, LiBF4, LiClO4, and LiFSI. Examples of nonaqueous solvents include propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, and vinylene carbonate. These may be used alone or in combination with additives.

[0061] Examples of the exterior packaging include a metal can or an aluminum laminate pack. The shape of the battery may be rectangular, cylindrical, coin-shaped, etc., and the separator of the present invention can be suitably applied to any shape. As an example, the procedures for producing a laminated battery, a cylindrical battery, and a coin battery will be described below. [Laminated lithium-ion secondary batteries and lithium metal secondary batteries] [Positive and negative electrodes] Commercially available products can be used for the positive and negative electrodes. For example, the positive electrode active material is a mixture of Li1.1Mn1.9O4, which has a spinel structure, and lithium-nickel-cobalt-manganese oxide (Ni / Li molar ratio 0.7). Polyvinylidene fluoride can be used as the binder, and carbon black powder can be used as the conductive additive.

[0062] For the negative electrode, graphite or other materials can be used as the negative electrode active material, and the porosity and pore size of the positive and negative electrode active material layers can be adjusted appropriately. The active material layer on one side of the positive and negative electrode current collectors is peeled off and cut into pieces measuring, for example, 29 mm x 40 mm. Alternatively, a metallic lithium layer can be formed to a specified thickness instead of graphite and used as the negative electrode. In this case, improved energy density can be expected.

[0063] An aluminum positive electrode tab is welded to the positive electrode current collector of the positive electrode, and a copper negative electrode tab (negative electrode current collector) is welded to the negative electrode current collector of the negative electrode. The positive electrode active material layer with these tabs welded and the negative electrode active material layer are placed opposite each other, and a separator is sandwiched between them to create a plate-shaped electrode structure.

[0064] The above-mentioned electrode structure is sandwiched between an exterior material made of a laminate film with an aluminum layer (size and shape: for example, a square of 60 mm x 60 mm), and three of the four sides of the square are heat-pressed and sealed to form an exterior body. An electrolyte solution is injected into this exterior body using a vacuum impregnation device (e.g., TOSPACK V-307GII; manufactured by Tosei Electric Co., Ltd.), and the remaining side is vacuum-sealed by thermocompression to produce a cell. Thereafter, the cell may be left to stand for a predetermined time, for example, at room temperature, until the injected electrolyte solution has sufficiently impregnated the pores of the electrode structure.

[0065] [Wound-type lithium-ion secondary battery / lithium metal battery] A wound-type lithium ion secondary battery / lithium metal secondary battery (hereinafter referred to as a lithium secondary battery) has a configuration in which, for example, an electrode structure is housed in a cylindrical exterior body together with a nonaqueous electrolyte. The electrode structure in a wound-type lithium secondary battery is produced by preparing a strip-shaped positive electrode, a strip-shaped negative electrode, and two separators, and then stacking and winding them into a layered structure. This electrode structure is housed in a cylindrical exterior body, and an electrolyte solution is poured into the exterior body and sealed, to produce a wound-type battery.

[0066] A wound-type lithium secondary battery may use, for example, a positive electrode composed of a long sheet-shaped positive electrode current collector and a positive electrode composite layer containing a positive electrode active material and provided on the positive electrode current collector, or a negative electrode composed of a long sheet-shaped negative electrode current collector and a negative electrode composite layer containing a negative electrode active material and provided on the negative electrode current collector. The separator is formed in the shape of a long sheet, similar to the positive electrode and negative electrode, and this separator is wound up in a state in which it is interposed between the positive electrode and negative electrode.

[0067] The exterior body includes a cylindrical case body with a bottom and a lid that closes the opening of the case body. The lid and case body are made of, for example, metal and are insulated from each other. The lid is electrically connected to the positive electrode current collector, and the case body is electrically connected to the negative electrode current collector. The lid may also serve as the positive electrode terminal, and the case body may also serve as the negative electrode terminal.

[0068] Lithium secondary batteries can be charged and discharged at temperatures between -10 and 80°C, for example. Measures to prevent an increase in internal pressure within the battery include providing a safety valve in the battery lid or making cuts in the battery case body or the gasket combined with this case body. Furthermore, to prevent overcharging, a current interruption mechanism that detects the internal pressure of the battery and interrupts the current can be provided in the lid. [Example]

[0069] The present invention will be explained in more detail below by showing examples, but the scope of the present invention is not limited to these examples. [Film thickness] The thickness was measured using a contact type thickness gauge (Peacock).

[0070] [Gurley value (air permeability)] A test piece 80 mm wide in the MD direction was taken from the produced microporous membrane, and measurements were performed at three points, the center and the left and right edges (50 mm inward from the edge faces), using a B-type Gurley densometer (Kumagaya Riki Kogyo Co., Ltd., Catalog No. 2060) in accordance with JIS P8117. The average value of the three points was calculated as the Gurley value.

[0071] [Porosity (gravimetric method)] Twenty porous membranes measuring 3.5 x 4.5 cm were punched out to prepare porous membranes with a total area of ​​315 cm2, and the membrane thickness and weight were measured. The true density of the porous membrane was measured using a true density measuring device (BELPycno: manufactured by Microtrack-Bell). The size of the measurement cell used was 3.5 cc, and the porosity was calculated using the following formula, where D is the true density result, S is the area of ​​the porous membrane, d is the membrane thickness, and w is the weight: Porosity=(1-(w / (S×d×D)×100 (1)

[0072] Tensile Strength Test pieces in the sample shape specified in JIS K-6251-6 were subjected to measurements at a tensile speed of 1 mm / min and a chuck distance of 50 mm at 25°C (room temperature). The maximum stress was the highest tensile stress (MPa) measured until the film broke. The tensile tester used was an Autograph AGS-50NX manufactured by Shimadzu Corporation.

[0073] Elasticity Modulus Test pieces in the sample shape specified in JIS K-6251-6 were subjected to measurements at a tensile speed of 1 mm / min and a chuck distance of 50 mm at 25°C (room temperature), and the stress-strain curve was calculated from the gradient of the initial rising portion. The tensile tester used was an Autograph AGS-50NX manufactured by Shimadzu Corporation.

[0074] [stretch] A test piece in the sample shape specified in JIS K-6251-6 was subjected to measurement at 25°C (room temperature) with a tensile speed of 1 mm / min and a chuck distance of 50 mm. The breaking strain at which the film broke was taken as the elongation. The tensile tester used was an Autograph AGS-50NX manufactured by Shimadzu Corporation.

[0075] [Breaking energy] Using Shimadzu Corporation's Autograph AGS-50NX, measurements were performed on a test piece having the sample shape specified in JIS K-6251-6 at a tensile speed of 1 mm / min and a chuck distance of 50 mm in a measurement environment of 25°C (room temperature). The tensile test was performed under the above test conditions using Shimadzu Corporation's Autograph software TRAPEZIUM LITE X to obtain data on the "test force-displacement curve" calculated when the test was performed. The integral of this data until the film broke was defined as the breaking energy [J], and the breaking energy per unit film thickness [J / mm] was calculated using the following formula: Energy per unit film thickness [J / mm] = Energy [J] / Film thickness [mm]

[0076] [Membrane resistance] The sample was cut to a diameter of 18 mm, washed, and air-dried. Aluminum foil was cut to a diameter of 16 mm and lead tabs were attached. Two pieces of this aluminum foil were prepared, and the cut sample was sandwiched between them, taking care not to short-circuit the aluminum foil. The sample was impregnated with the electrolyte, 1 M LiPF6, EC:DEC (1:1 volume ratio). This was then sealed so that the tabs were exposed to the outside of the aluminum laminate. The cell was placed in a thermostatic bath at 25°C, and the resistance of the cell was measured using the AC impedance method at an amplitude of 14.1 mV and a frequency range of 1 MHz to 10 kHz. The membrane resistance (Ω·cm2) was calculated based on the measured cell resistance value.

[0077] [curvature rate] The tortuosity was calculated based on the following formula using the above-mentioned membrane resistance.

[0078]

number

[0079] [Ionic conductivity] The ionic conductivity was calculated based on the following formula using the above-mentioned membrane resistance.

[0080]

number

[0081] [Contact angle] The contact angle of the polyimide porous film was measured using a contact angle meter under the following measurement conditions: (Measurement equipment and measurement conditions) Measurement equipment: Kyowa Interface Science Co., Ltd. Contact angle meter DMo-701 Measurement environment: Temperature 20°C, relative humidity 40% Dropping solution: Electrolyte solution made by mixing 1.5 mol / l LiFSI and 0.1 mol / l LiPF6 in a mixed solvent of ethylene carbonate and propylene carbonate (mixing ratio 1:1 [volume ratio]) Electrolyte viscosity: 30 mPa·s ·Dropped amount: 1.0μL Measurement timing: Measured 65 milliseconds after the electrolyte hits the skin [Example]

[0082] Adjustment example 1 [Preparation of electrolyte for wettability evaluation] *The following is an example. We suspect there may be a more appropriate solution. The electrolyte was prepared by adding 0.06 mol / L of LiPF6 and 1.5 mol / L of LiFSI as lithium salts, based on the total amount of the electrolyte, and 3 wt% of VC and 0.5 wt% of PS as additives to an organic solvent having a composition of ethylene carbonate (EC):ethyl methyl carbonate (PC) = 1:1 (volume ratio). [Example]

[0083] [Preparation of polyamic acid] 2.3215 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride, 0.6119 g of 4,4'-oxydiphthalic anhydride, and 1.0666 g of p-phenylenediamine were added to 16 g of N,N-dimethylacetamide, and the mixture was stirred at 25°C for 12 hours in a separable flask to react, thereby obtaining a polyamic acid. A first slurry was prepared by adding polymethyl methacrylate particles having a particle size of 300 nm to the prepared polyamic acid, and a second slurry was prepared by adding polymethyl methacrylate particles having a particle size of 800 nm, which was different from the first slurry, to the above polyamic acid. The first and second slurries were extruded onto a support through a three-layer die to form a three-layer structure with the first slurry as the middle layer and the second slurry as the surface layer. The particles were then removed by heat treatment to produce a three-layer polyimide porous membrane. The theoretical porosity of the surface layer was 72%, that of the middle layer was 50%, and the layer ratio was 1:3:1 (surface layer:middle layer:surface layer). The resulting three-layer polyimide porous membrane had a thickness of 24 μm, a porosity of 65%, and an air permeability of 20 sec / 100 cc.

[0084] [Comparative Example 1] A polyolefin-based separator was produced by a known dry method, and the resulting polyolefin-based separator had a membrane thickness of 36 μm, a porosity of 43%, and an air permeability (Gurley value) of 692 seconds / 100 cc.

Claims

1. A separator for an electric storage device, which has a three-layer structure in which a surface layer is provided on both sides of an intermediate layer, and is made of a polyimide porous film in which fine particles are removed to form pores in the surface layer and the intermediate layer, The separator for an electricity storage device, wherein the maximum pore size of the surface layer is 600 nm or more.

2. 2. The separator for an electricity storage device according to claim 1, wherein when 1.0 μL of an electrolyte solution having a viscosity of 30 mPa·s is dropped onto the surface layer, the contact angle 65 milliseconds after the electrolyte solution lands on the surface layer is 90 degrees or less.

3. 3. The separator for an electricity storage device according to claim 2, wherein the electrolyte has a composition in which 1.5 mol / l of LiFSI is dissolved in a mixed solvent of ethylene carbonate and propylene carbonate (mixture ratio by volume: 1:1).

4. The separator for an electricity storage device according to claim 1 , wherein the surface layer has a surface opening ratio of 20% or more.

5. The separator for use in an electricity storage device according to claim 4 , having an average pore diameter of 250 nm or more.

6. 6. The separator for an electricity storage device according to claim 1, wherein the surface layer has a porosity of 67% or more, and the intermediate layer has a porosity of 60% or less.

Citation Information

Patent Citations

  • Jitter absorbing device for digital data

    JP1988058663A

Cited By

  • Disassemblable joined body, method for manufacturing disassemblable joined body, and method for disassembling disassemblable joined body