Ink composition for metal printing
The ink composition for metal printing uses rosin-modified resin and hydrophilic silica to improve compatibility with water-based overprint varnishes, addressing repellency and transfer issues without increasing oil length, ensuring effective printing performance.
Patent Information
- Application Number
- JP2023120353
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2023-07-25
- Publication Date
- 2024-11-08
AI Technical Summary
Existing ink compositions for metal printing face issues with repellency and reduced quality of the coating film when using water-based overprint varnishes, and there is a trade-off between transfer properties and compatibility with aqueous overprint varnishes due to the use of high oil lengths in alkyd resins.
Incorporating a rosin-modified resin with a hydroxyl value of 10 mgKOH/g or more and a polyoxyalkylene alkyl ether solvent, along with hydrophilic silica particles, to enhance the ink composition's compatibility with water-based overprint varnishes while maintaining transfer properties without increasing the oil length of the alkyd resin.
The ink composition achieves good transfer properties and suppresses repellency of water-based overprint varnishes, ensuring compatibility and maintaining fluidity during printing, even when applied wet-on-wet.
Smart Images

Figure 2024159390000001 
Figure 2024159390000002 
Figure 2024159390000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an ink composition for metal printing. [Background technology]
[0002] For printing on the outer metal surfaces of metal materials, such as galvanized or tinned iron sheets, aluminum sheets, or metal cans made from these metal materials, ink compositions for metal printing are used which contain, as the main vehicle components, binder resins such as alkyd resins, polyester resins, and epoxy resins, and organic solvents such as mineral oils or higher alcohols.
[0003] Moreover, these printing surfaces are generally coated with an overprint varnish to improve the adhesion of the ink coating, bending resistance, impact resistance, abrasion resistance, etc. The most widely used overprint varnishes are solvent-based varnishes that contain binder resins such as alkyd resins, polyester resins, acrylic resins, and epoxy resins, hardeners such as melamine resins and benzoguanamine resins, and organic solvents such as mineral oils and cellosolves.
[0004] When printing on the outer metal surface, ink is printed using an offset printing machine, dry offset printing machine, etc., and then an overprint varnish is applied wet-on-wet onto the ink coating using a coater, etc., and then baked at 150 to 280°C.
[0005] In recent years, in the field of metal printing, it has become common to use water-based overprint varnishes instead of the solvent-based overprint varnishes that have been used in the past, due to the problems of air pollution caused by solvents and the hygiene and safety aspects of the printing work environment. However, when a water-based overprint varnish is applied onto an ink coating film of a conventional ink composition for metal printing, there are problems such as the repelling of the water-based overprint varnish and the penetration of the water-based overprint varnish into the ink film, resulting in a significant decrease in the quality of the coating film, such as gloss or adhesion. Therefore, there has been a demand for ink compositions to have excellent suitability for water-based overprint varnishes.
[0006] As a method for improving suitability for such aqueous overprint varnish, for example, Patent Document 1 proposes the use of an alkylene glycol-based solvent having 4 to 8 carbon atoms, Patent Document 2 proposes the use of a polyoxyalkylene glycol-based solvent, Patent Document 3 proposes the use of a polyoxyalkylene alkyl ether-based organic solvent, and Patent Document 4 proposes the use of a polyoxyalkylene alkyl ester-based solvent. These organic solvents used in ink compositions are effective in improving the suitability of the ink composition for aqueous overprint varnish, but there is room for improvement in that the ink composition tends to have insufficient fluidity and tends to cause misting during printing.
[0007] When attempting to improve the fluidity of an ink composition for metal printing or misting during printing, there is a method of using a solvent with low polarity, such as a high-boiling aromatic hydrocarbon, as described in the examples of Patent Document 5. However, in recent years, with the aim of further reducing the environmental load, water-based overprint varnish products in which the solvent content has been reduced to the minimum have been distributed, and when such an overprint varnish is used, there is also a problem of repelling occurring with an ink composition that uses a solvent with low polarity.
[0008] In recent years, the printing speed of metal printing has been increased in order to improve productivity. From the viewpoint of responding to such high-speed printing, the transferability of the ink composition is important. From the viewpoint of ensuring the transferability of the ink composition, it is effective to increase the oil length of the alkyd resin contained in the ink composition. However, an ink composition containing an alkyd resin with a long oil length is incompatible with the above-mentioned aqueous overprint varnish, and is likely to cause the problem of repelling of the aqueous overprint varnish on the surface of the printed ink composition. In other words, there is a trade-off between the increase in oil length based on the viewpoint of transferability and the suitability for application to the aqueous overprint varnish, which has been one of the technical challenges. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Special Publication No. 5-75031 [Patent Document 2] Special Publication No. 5-40791 [Patent Document 3] Special Publication No. 5-40792 [Patent Document 4] Japanese Patent Publication No. 64-60670 [Patent Document 5] JP 2009-249435 A Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been made in consideration of these circumstances, and has as its object to provide an ink composition for metal printing which can obtain good transferability during printing without excessively increasing the oil length of the alkyd resin. [Means for solving the problem]
[0011] As a result of intensive research into solving the above problems, the present inventors have found that the above problems can be solved by using an ink composition containing both a rosin-modified resin having a hydroxyl value of 10 mgKOH / g or more as at least a part of the resin contained in the ink composition and a polyoxyalkylene alkyl ether solvent represented by the following general formula (1), and have completed the present invention. Specifically, the present invention provides the following:
[0012] (1) The present invention is an ink composition for metal printing comprising a color pigment, a resin and a solvent, characterized in that at least a part of the resin contains a rosin-modified resin having a hydroxyl value of 10 mgKOH / g or more, and the solvent contains at least one compound selected from the group consisting of compounds represented by the following general formula (1): [ka] (In the above general formula (1), each A is independently an alkylene group having 2 to 4 carbon atoms which may be branched, R is an alkyl group having 1 to 13 carbon atoms which may have a branched and / or cyclic structure, and n is an integer of 2 to 8.)
[0013] (2) The present invention also relates to the ink composition for metal printing according to item (1), further comprising 1 to 8 mass % of hydrophilic silica particles.
[0014] (3) The present invention also relates to an ink composition for metal printing according to item (1) or (2), in which the acid value of the rosin-modified resin is 100 mgKOH / g or less.
[0015] (4) The present invention also relates to an ink composition for metal printing according to any one of items (1) to (3), characterized in that when 70 g of the rosin-modified resin is dissolved in 30 g of tripropylene glycol monobutyl ether heated to 130°C by stirring for 60 minutes, a dissolved varnish is obtained having an n-hexane tolerance of more than 50 g / 5 g as measured by the following procedure. Procedure: After allowing the dissolved varnish to cool to room temperature, place 5 g in a beaker, and while maintaining the liquid temperature in the beaker at 25°C, add n-hexane to the dissolved varnish in the beaker in small amounts while stirring, and determine the mass (g) of n-hexane required until the liquid in the beaker begins to become cloudy. The mass (g) of n-hexane thus determined is the n-hexane tolerance (g / 5g).
[0016] (5) The present invention also relates to the ink composition for metal printing according to any one of (1) to (4), wherein the rosin-modified resin is a rosin ester resin. Effect of the Invention
[0017] According to the present invention, there is provided an ink composition for metal printing which is capable of achieving good transferability during printing without excessively increasing the oil length of the alkyd resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, one embodiment of the ink composition for metal printing of the present invention will be described. Note that the present invention is not limited to the following embodiment, and can be practiced by making appropriate modifications within the scope of the present invention.
[0019] The ink composition of the present invention is for metal printing, and is preferably applied to printing by the so-called dry offset printing method using a relief plate as a printing plate, or the offset printing method using a lithographic plate as a printing plate, but can be applied to all printing methods commonly used in metal printing. In addition, the ink composition of the present invention can suppress repelling of the applied OP varnish even if an aqueous overprint varnish (OP varnish) is applied wet-on-wet immediately after printing with the ink composition, so it can be preferably applied to two-piece can printing in which such printing and coating methods are adopted, and can also be preferably used in three-piece can printing. According to the ink composition of the present invention, good transferability can be maintained even in cases where the pigment content must be set high, such as in a white ink composition. Furthermore, according to the ink composition of the present invention, good transferability during printing can be obtained without extremely increasing the oil length of the alkyd resin, so that printing can be performed that achieves both suppression of repelling and good transferability during printing, even if an aqueous OP varnish with a reduced solvent component is applied wet-on-wet.
[0020] The ink composition of the present invention is an ink composition for printing on metal, comprising a color pigment, a resin and a solvent, characterized in that at least a part of the resin contains a rosin-modified resin having a hydroxyl value of 10 mgKOH / g or more, and the solvent contains at least one compound selected from the group consisting of compounds represented by general formula (1). Each component will be described below.
[0021] [resin] The ink composition of the present invention contains, as at least a part thereof, a rosin-modified resin having a hydroxyl value of 10 mgKOH / g or more. The ink composition of the present invention was completed based on the finding that the inclusion of such a rosin-modified resin having a high hydroxyl value improves the transferability of the ink composition during printing. At the same time, the inclusion of such a rosin-modified resin in the ink composition of the present invention is thought to increase the polarity of the composition itself, and thus increases the affinity for water-based OP varnish, which also has a high polarity, and this also has the effect of suppressing repelling even when the ink composition is applied wet-on-wet.
[0022] Rosin-modified resins are resins prepared using rosin as one of the raw materials. Rosin contains a mixture of resin acids such as abietic acid, palustric acid, isopimaric acid, and levopimaric acid, and these resin acids contain hydrophilic and chemically active carboxyl groups, some of which have conjugated double bonds. For this reason, various rosin-modified resins are prepared by combining polyhydric alcohols and polybasic acids and polycondensing them, adding resol, which is a condensate of phenol, to the benzene ring contained in the rosin skeleton, or by carrying out a Diels-Alder reaction with dienophiles such as maleic anhydride and maleic acid to add maleic acid or maleic anhydride skeletons. Various types of such rosin-modified resins are commercially available, and it is also possible to obtain and use them.
[0023] Examples of the rosin modified resin include rosin ester resin, maleic rosin, fumarated rosin resin, rosin modified maleic acid resin, rosin modified fumaric acid resin, rosin modified phenolic resin, rosin modified alkyd resin, rosin modified polyester resin, etc. In the present invention, any of the rosin modified resins may be used, but among these, rosin ester resins are preferably used.
[0024] The hydroxyl value of the rosin-modified resin is 10 mgKOH / g or more, preferably 15 mgKOH / g or more, and more preferably 20 mgKOH / g or more. The upper limit of the hydroxyl value of the rosin-modified resin is not particularly limited, but is, for example, about 200 mgKOH / g, preferably about 150 mgKOH / g, and more preferably about 100 mgKOH / g.
[0025] Although not particularly limited, the acid value of the rosin-modified resin is preferably 100 mgKOH / g or less. The acid value of the rosin-modified resin is preferably 100 mgKOH / g or less, since it is possible to suppress repelling when the aqueous OP varnish is applied wet-on-wet, and to achieve printability such as suppressing misting and bubbly. The acid value of the rosin-modified resin is more preferably 80 mgKOH / g or less, and even more preferably 50 mgKOH / g or less.
[0026] The rosin-modified resin is used in a state in which it is dissolved or dispersed by heating together with a solvent described later to form a varnish. The rosin-modified resin may be used as a dissolved varnish in a state in which it is dissolved or dispersed in a solvent, or may be used in a state in which a divalent or higher metal alkoxy compound is added as a gelling agent to the dissolved varnish obtained by dissolving the resin when preparing the varnish, and the resin is used in a gelled varnish. Among these, it is preferable to prepare a dissolved varnish from the rosin-modified resin and use this to prepare the ink composition, since this can improve the transferability of the ink composition during printing. In addition, by preparing a gelled varnish from the rosin-modified resin and using this to prepare the ink composition, the ink composition is given an appropriate viscoelasticity, which can improve the flowability and reduce misting, and can form a tougher cured coating.
[0027] The content of the rosin-modified resin in the ink composition is preferably 5 to 50 mass% relative to the entire composition, more preferably 5 to 25 mass% relative to the entire composition, and even more preferably 7 to 20 mass% relative to the entire composition.
[0028] The ink composition of the present invention preferably contains an alkyd resin in addition to the rosin-modified resin. The alkyd resin is a condensation polymer of a polyhydric alcohol and a polybasic acid, and is a type of polyester. It can also be prepared by condensation polymerization with animal and vegetable oils and / or their fatty acids. At this time, the animal and vegetable oils are transesterified with the polyhydric alcohol to become fatty acids, which are incorporated into the structure of the alkyd resin. The proportion of fatty acids derived from animal and vegetable oils in the alkyd resin is called the oil length, and the oil length of the alkyd resin used in the present invention is preferably 20 to 50 mass%. An oil-free alkyd resin that does not contain fatty acid components of animal and vegetable oils may be used.
[0029] As the alkyd resin in the present invention, various types can be used, among which coconut oil modified alkyd resin is preferably used. By using coconut oil modified alkyd resin as the alkyd resin, the dispersion stability of the ink composition becomes good, and it is preferable in that a good hue with high transparency can be obtained.
[0030] As such an alkyd resin, one prepared using phthalic acid (orthophthalic acid) as a polybasic acid and having a phthalic acid skeleton can be preferably used. By using such an alkyd resin, the transferability of the ink can be improved and the whiteness of the white ink can be further increased.
[0031] The content of the alkyd resin in the ink composition is preferably from 10 to 40 mass % relative to the entire composition, more preferably from 10 to 30 mass %, and even more preferably from 15 to 25 mass % relative to the entire composition.
[0032] In addition to the above-mentioned rosin-modified resin or alkyd resin, the ink composition of the present invention can also contain resins that have been used in the preparation of conventional ink compositions for metal printing. That is, known resins that are compatible with the above-mentioned rosin-modified resin or alkyd resin can be used alone or in combination depending on the required performance such as printability and coating film properties. Examples of such resins include polyester resins, petroleum resins, epoxy resins, ketone resins, amino resins, and benzoguanamine resins.
[0033] [solvent] The ink composition of the present invention contains at least one solvent selected from the group consisting of compounds represented by the following general formula (1). Hereinafter, the at least one solvent selected from the group consisting of compounds represented by the following general formula (1) is also referred to as a specific solvent.
[0034] [ka]
[0035] In the above general formula (1), each A is independently determined and is an alkylene group having 2 to 4 carbon atoms which may have a branch. Examples of such an alkylene group include an ethylene group [-(CH2)2-], a propylene group [-CH2(CH3)-CH2- or -CH2CH2(CH3)-], a trimethylene group [-(CH2)3-], and an isopropylidene group [-C(CH3)2-].
[0036] In the above general formula (1), R is an alkyl group having 1 to 13 carbon atoms, which may have a branched and / or cyclic structure. This alkyl group may be not only an aliphatic group but also an alicyclic group. Examples of such an alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a hexyl group, a 2-ethylhexyl group, an octyl group, a decyl group, and a cyclohexyl group.
[0037] In the above general formula (1), n is an integer of 2 to 8. When n is 2 or more, a sufficient boiling point of the specific solvent can be secured to provide stability to the ink composition on a printing machine, which is preferable, and when n is 8 or less, a viscosity suitable for the solvent of the ink composition can be achieved.
[0038] Examples of the compound represented by the above general formula (1) include dipropylene glycol monomethyl ether, dipropylene glycol monobutyl ether, dipropylene glycol monooctyl ether, dipropylene glycol tridecyl ether, tripropylene glycol monobutyl ether, tripropylene glycol monodecyl ether, tetrapropylene glycol monohexyl ether, pentapropylene glycol monobutyl ether, and hexapropylene glycol monomethyl ether.
[0039] The content of the specific solvent in the ink composition of the present invention is preferably 5 to 40% by mass, more preferably 10 to 30% by mass, based on the entire composition. The content of the specific solvent is 5% by mass or more based on the entire composition, which is preferable because it can increase the compatibility of the rosin-modified resin in the ink composition and can effectively suppress repelling when a water-based OP varnish is applied wet-on-wet after printing.
[0040] Here, the above-mentioned rosin-modified resin is preferably one that gives a dissolved varnish with an n-hexane tolerance of more than 50 g / 5 g when 70 g of the resin is dissolved in 30 g of tripropylene glycol monobutyl ether heated to 130° C. by stirring for 60 minutes. Since the measurement of n-tolerance is not particularly time-consuming as described later, this selection process does not require excessive trial and error. By using a rosin-modified resin that satisfies these conditions, the compatibility of the rosin-modified resin in the ink composition can be improved, and the transferability of the ink composition during printing can be further improved. Moreover, the above-mentioned tripropylene glycol monobutyl ether is an ether of tripropylene glycol and butanol formed by polymerization of three molecules of propylene oxide, and is one of the specific solvents in the present invention.
[0041] Next, the method for measuring the n-hexane tolerance of a resin in the present invention will be described. First, 70 g of the rosin-modified resin to be measured is prepared, and this is dissolved in 30 g of tripropylene glycol monobutyl ether heated to 130° C. by stirring for 60 minutes to prepare a dissolved varnish. The obtained dissolved varnish is allowed to cool to room temperature, and then 5 g is collected in a beaker. While maintaining the liquid temperature in the beaker at 25° C., n-hexane is added to the dissolved varnish in the beaker little by little while stirring, and the mass (g) of n-hexane required until the liquid in the beaker starts to become cloudy is obtained. The mass (g) of n-hexane obtained is the n-hexane tolerance (g / 5g). This measurement is so sensitive that the solution immediately begins to become cloudy when only one drop of n-hexane is added to the solution just before it becomes cloudy, so measurement errors due to the difference in judgment of cloudiness caused by differences in the measurer are not particularly problematic.
[0042] [Coloring pigments] The color pigment is a component for imparting coloring power to the ink composition. Examples of the color pigment include, without particular limitation, organic and / or inorganic pigments that have been conventionally used in printing ink compositions.
[0043] Examples of such color pigments include yellow pigments such as disazo yellow (pigment yellow 12, pigment yellow 13, pigment yellow 17, pigment yellow 1) and Hansa Yellow, magenta pigments such as brilliant carmine 6B, lake red C, and watching red, cyan pigments such as phthalocyanine blue, phthalocyanine green, and alkali blue, black pigments such as carbon black, white pigments such as titanium oxide, and fluorescent pigments. Metal powder pigments for imparting metallic colors such as gold and silver to the ink composition are also treated as color pigments in the present invention. Examples of such metal powder pigments include gold powder, bronze powder, aluminum paste obtained by processing aluminum powder into a paste, and mica powder.
[0044] The amount of the color pigment added is, for example, about 5 to 50% by mass relative to the entire ink composition, but is not particularly limited. When preparing a yellow ink composition using a yellow pigment, a magenta ink composition using a magenta pigment, a cyan ink composition using a cyan pigment, or a black ink composition using a black pigment, it is also possible to use a pigment of another color in combination or add an ink composition of another color as a complementary color.
[0045] [Other ingredients] To the ink composition of the present invention, known curing agents, pigment dispersants, solvents other than the above-mentioned specific solvents, wax, silica particles, stabilizers, and the like can be added as other components as necessary.
[0046] As the curing agent, for example, an amino resin such as a melamine resin or a benzoguanamine resin can be used.
[0047] Examples of solvents other than the above specific solvents include aliphatic or alicyclic hydrocarbons having a boiling point range of about 230 to 400° C., aromatic hydrocarbons such as alkylbenzenes, and higher alcohols.
[0048] Silica particles are commercially available as SiO2 powder, and are easily available in the form of hydrophilic particles that have not been surface-treated or that have been hydrophilized, or hydrophobic particles that have been hydrophobized. Among these silica particles, hydrophilic silica particles are preferably used in the ink composition of the present invention. By using hydrophilic silica particles, the transferability of the ink composition during printing can be improved, and the fluidity of the ink composition can be increased, which is preferable. The content of silica particles in the ink composition is preferably 1 to 8 mass%, and more preferably 2 to 5 mass%.
[0049] The ink composition of the present invention can be prepared by mixing the various components, such as the color pigment, resin, and solvent containing the specific solvent, in a conventional manner using a roll mill, ball mill, bead mill, etc. The viscosity of the ink composition can be, for example, 10 to 70 Pa s at 25°C measured with a Raleigh viscometer, but is not particularly limited.
[0050] The metal for use in metal printing in the ink composition of the present invention is not particularly limited, but examples thereof include galvanized or tinned iron plate, aluminum plate, and metal cans made of these metal materials.
[0051] As the aqueous OP varnish to be applied onto the printed ink composition, any commonly used one can be used, and specific examples thereof include those using an aqueous acrylic resin, an aqueous polyester resin, an aqueous alkyd resin, an aqueous epoxy resin, or a modified resin of two or more of these as a binder in combination with an amino resin as a curing agent.
[0052] When printing on the surface of a metal material using the ink composition and aqueous OP varnish, first, printing is performed using the ink composition of the present invention with a dry offset printing machine, offset printing machine, or the like, and then, while the ink composition is still in a wet state (wet-on-wet), the aqueous OP varnish is overcoated with a coater or the like, and then baking is performed at 150 to 280°C for a few seconds to a few minutes. EXAMPLES
[0053] The ink composition of the present invention will be explained in more detail below by showing examples, but the present invention is not limited to the following examples in any way.
[0054] [Synthesis of alkyd resin] 5.98 parts by mass of neopentyl glycol, 8.53 parts by mass of pentaerythritol, 10.10 parts by mass of coconut oil fatty acid, 11.95 parts by mass of isophthalic acid, and 2.48 parts by mass of terephthalic acid were reacted at 220°C under a nitrogen atmosphere until the acid value of the mixture reached 7 mgKOH / g to perform the first stage of esterification, and then 0.70 parts by mass of trimellitic anhydride was added and heated at 165°C for 30 minutes under a nitrogen atmosphere to perform the second stage of esterification. These esterification reactions were carried out according to a conventional method to obtain an alkyd resin with a weight average molecular weight of 15303 and a number average molecular weight of 1484. 21.8 parts by mass of tripropylene glycol monobutyl ether (which corresponds to the above-mentioned specific solvent) and 2.0 parts by mass of triethanolamine were added to this alkyd resin to obtain an alkyd resin varnish.
[0055] [Preparation of Varnish 1] 61.6 parts by mass of rosin ester resin (hydroxyl value 40-50 mgKOH / g, acid value 10-20 mgKOH / g, weight average molecular weight 744, number average molecular weight 701) and 35.9 parts by mass of tripropylene glycol monobutyl ether were heated at 130°C for 1 hour to dissolve them, and 2.5 parts by mass of aluminum ethyl acetoacetate diisopropylate was added and heated at 130°C for 30 minutes to obtain varnish 1. This varnish 1 is a gelled varnish containing rosin ester resin (hydroxyl value 40-50 mgKOH / g). The n-hexane tolerance of the rosin ester resin used in preparing varnish 1 was determined according to the procedure specified in the present invention, and was found to be 50. <g / 5gだった。
[0056] [Preparation of varnish 2] 63.2 parts by mass of rosin ester resin (hydroxyl value 20-30 mgKOH / g, acid value <10 mgKOH / g, weight average molecular weight 632, number average molecular weight 565) and 36.8 parts by mass of tripropylene glycol monobutyl ether were heated at 130°C for 1 hour to dissolve them, to obtain varnish 2. This varnish 2 is a dissolved varnish containing rosin ester resin (hydroxyl value 20-30 mgKOH / g). The n-hexane tolerance of the rosin ester resin used in preparing varnish 2 was determined according to the procedure specified in the present invention, and was found to be 50 <g / 5gだった。
[0057] [Preparation of Varnish 3] 61.4 parts by mass of the same rosin ester resin (hydroxyl value 20-30 mgKOH / g, acid value <10 mgKOH / g, weight average molecular weight 632, number average molecular weight 565) used in the preparation of Varnish 2 above and 35.7 parts by mass of tripropylene glycol monobutyl ether were heated at 130°C for 1 hour to dissolve them, and then 2.9 parts by mass of aluminum ethyl acetoacetate diisopropylate was added and heated at 130°C for 30 minutes to obtain Varnish 3. Varnish 3 is a gelled varnish prepared using the same rosin ester used in the preparation of Varnish 2 above.
[0058] [Preparation of Varnish 4] 61.4 parts by mass of maleated rosin resin (hydroxyl value ≒ 0 mg KOH / g, acid value 220 ≦ mg KOH / g, weight average molecular weight 877, number average molecular weight 766) and 35.5 parts by mass of tripropylene glycol monobutyl ether were heated at 130 ° C for 1 hour to dissolve them, and 3.1 parts by mass of aluminum ethyl acetoacetate diisopropylate was added and heated at 130 ° C for 30 minutes to obtain varnish 4. This varnish 4 is a gelled varnish containing maleated rosin resin (hydroxyl value ≒ 0 mg KOH / g). The n-hexane tolerance of the maleated rosin resin used in the preparation of varnish 4 was determined by the procedure specified in the present invention, and was 4.9 g / 5 g.
[0059] [Examples 1 to 6, Comparative Example 1] Each ink composition of Examples 1 to 6 and Comparative Example 1 was prepared by mixing each component according to the formulation in Table 1 and kneading the resulting mixture with a three-roll mill. In Table 1, "white pigment" is titanium oxide, "hydrophobic silica" is surface-treated silica particles (manufactured by Nippon Aerosil Co., Ltd., product name Aerosil R972), "hydrophilic silica" is surface-untreated silica particles (manufactured by Tokuyama Corporation, product name Reolosil CP102), "clay" is organophilic bentonite (manufactured by BYK, product name CRAYTONE-APA), and "specific solvent" is tripropylene glycol monobutyl ether. In Table 1, the numerical values of each blend amount mean parts by mass.
[0060] [Liquidity assessment] For each of the ink compositions of Examples 1 to 6 and Comparative Example 1, the slope measured at 25°C using a spreadmeter in accordance with JIS K5101-6-1:2004 is shown in the "Slope" column of Table 1. Note that a larger slope value indicates higher fluidity of the ink composition.
[0061] [Metastatic] The transferability of each of the ink compositions of Examples 1 to 6 and Comparative Example 1 was evaluated by the following procedure. First, 0.15 cc of the ink composition was spread on a blanket (Airtack FS, Kinyosha Co., Ltd.) using a 4-split roll of an RI tester (Akira Manufacturing Co., Ltd.), and after leaving it for 10 or 20 minutes, an aluminum plate to be printed was attached to the spread blanket, and when pressure was applied, whether the spread ink composition was transferred to the aluminum plate and the degree of transfer was visually judged to evaluate the transferability of the ink composition. The evaluation criteria were as follows, and the results are shown in the "Transferability Evaluation" column of Table 1. ○: Good transfer even after leaving for 20 minutes △~◯: When left for 20 minutes, the transfer was slightly insufficient, but when left for 10 minutes, the transfer was good. △: No transfer when left for 20 minutes, but good transfer when left for 10 minutes ×: No transfer even after leaving for 10 minutes
[0062] [Table 1]
[0063] Comparing the ink compositions of Examples 1 to 6 with the ink composition of Comparative Example 1, it is found that the use of a combination of a rosin-modified resin having a hydroxyl value specified in the present invention and a specific solvent can improve the transferability of the ink composition without changing the oil length of the alkyd resin. Also, comparing Example 1 with Example 2, it is found that the ink composition using hydrophilic silica particles can maintain higher fluidity than the ink composition using hydrophobic silica particles.
Claims
1. A metal printing ink composition comprising a color pigment, a resin and a solvent, An ink composition for metal printing, comprising as at least a part of the resin a rosin-modified resin having a hydroxyl value of 10 mg KOH / g or more, and as the solvent, at least one compound selected from the group consisting of compounds represented by the following general formula (1): 【Chemistry 1】 (In the above general formula (1), each A is independently an alkylene group having 2 to 4 carbon atoms which may have a branch, R is an alkyl group having 1 to 13 carbon atoms which may have a branched and / or cyclic structure, and n is an integer of 2 to 8.)
2. 2. The ink composition for metal printing according to claim 1, further comprising 1 to 8 mass % of hydrophilic silica particles.
3. 3. The ink composition for metal printing according to claim 1, wherein the rosin-modified resin has an acid value of 100 mg KOH / g or less.
4. 3. The ink composition for metal printing according to claim 1, wherein when 70 g of the rosin-modified resin is dissolved in 30 g of tripropylene glycol monobutyl ether heated to 130° C. by stirring for 60 minutes, a dissolved varnish is obtained which has an n-hexane tolerance of more than 50 g / 5 g as measured by the following procedure. Procedure: After allowing the dissolved varnish to cool to room temperature, place 5 g in a beaker, and while maintaining the liquid temperature in the beaker at 25°C, add n-hexane to the dissolved varnish in the beaker in small amounts while stirring, and determine the mass (g) of n-hexane required until the liquid in the beaker begins to become cloudy. The mass (g) of n-hexane thus determined is the n-hexane tolerance (g / 5g).
5. 3. The ink composition for metal printing according to claim 1, wherein the rosin-modified resin is a rosin ester resin.
Citation Information
Patent Citations
Printing ink for metal
JP1989060670A
Automatic register method for parts data base
JP1993040791A
Electronic card arranging book
JP1993040792A
Semiconductor device
JP1993075031A
Printing ink composition for seamless can
JP2009249435A