Thermosetting resin foam
By integrating composite particles with polymer graft chains into thermosetting resin foams, the challenge of maintaining moldability and achieving superior vibration damping is addressed, resulting in enhanced strain energy absorption and damping performance.
Patent Information
- Application Number
- JP2023144731
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2023-09-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing thermosetting resin foams face challenges in maintaining foam moldability while achieving excellent vibration damping properties, as composite particles are difficult to knead into the resin and uniformly disperse, and adding hydrophilic or hydrophobic silica does not improve damping properties.
Incorporating composite particles with polymer graft chains bonded to the particle surface into the thermosetting resin foam composition, which enhances vibration damping performance without compromising moldability.
The thermosetting resin foam maintains foam moldability and exhibits significantly improved vibration damping properties, with enhanced strain energy absorption and damping performance across a controlled temperature range.
Smart Images

Figure 2024159407000001 
Figure 2024159407000002 
Figure 2024159407000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting resin foam and a method for producing the same. [Background technology]
[0002] In recent years, there has been a demand for vibration countermeasures for various devices, especially in the fields of automobiles, home appliances, and precision instruments. Generally, materials with high vibration damping properties include composite materials such as metal plates bonded to vibration absorbing materials such as rubber or asphalt, or vibration-damping steel plates in which vibration absorbing materials are sandwiched between metal plates. These vibration-damping materials maintain their shape with high-rigidity metal plates and absorb vibrations with vibration absorbing materials. In addition, there are alloy-type materials that use only metals to convert kinetic energy into thermal energy and absorb vibrations by using twin crystals or ferromagnetism. However, composite-type materials have limitations in formability because different materials are bonded together, and because metal steel plates are used, there is a problem that the product itself is heavy. In addition, alloy-type materials are heavy because they use only metal, and their vibration damping performance is insufficient.
[0003] In contrast to such conventional technology, in Patent Document 1, the present inventors propose using a thermoplastic resin composition containing a thermoplastic resin and composite particles having polymer graft chains bonded to the particle surface as a vibration-damping material.
[0004] Thermosetting resin foams such as polyurethane foam are also used as vibration-damping materials. For example, Patent Document 2 discloses a high-density polyurethane foam that is mixed with slag and has excellent sound absorption, sound insulation, vibration-proofing, and flame resistance. On the other hand, Patent Document 3 discloses that blending hydrophobic silica and light calcium carbonate as foam retaining agents into polyurethane foam, and blending untreated silica (hydrophilic silica) that has not been subjected to hydrophobic treatment results in poor foaming properties and poor appearance after molding. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-196877 A [Patent Document 2] Japanese Patent Application Publication No. 52-54797 [Patent Document 3] JP 2020-84173 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention relates to providing a new thermosetting resin foam that has excellent vibration damping properties while maintaining foam moldability, and a production method thereof. [Means for solving the problem]
[0007] The present invention relates to the following [1] to [9]. [1] A thermosetting resin foam containing composite particles with polymer graft chains bonded to the particle surface. [2] The thermosetting resin foam according to [1], which is a polyurethane foam. [3] A method for producing a thermosetting resin foam, comprising the step of foaming a thermosetting resin foam composition containing composite particles having polymer graft chains bonded to the particle surface. [4] A method for producing a polyurethane foam, comprising the step of preparing a polyol mixture containing composite particles having polymer graft chains bonded to the particle surface and a polyol component. [5] A vibration-damping material comprising the thermosetting resin foam described in [1] or [2]. [6] A method for improving vibration damping properties by incorporating composite particles having polymer graft chains bonded to the particle surface into a thermosetting resin foam. [7] A composite particle for use in a thermosetting resin foam according to the above item [1] or [2], in which polymer graft chains are bonded to the particle surface. [8] A polyol mixture for polyurethane foam, comprising composite particles having polymer graft chains bonded to the particle surface and a polyol component, for use in the polyurethane foam described in [2]. [9] A dispersion for use in the thermosetting resin foam according to [1] or [2], comprising composite particles having polymer graft chains bonded to their particle surfaces and a dispersion medium. Effect of the Invention
[0008] According to the present invention, it is possible to provide a new thermosetting resin foam that has excellent vibration damping properties while maintaining foam moldability, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] In the above Patent Document 1, an excellent vibration-damping effect was found in a thermoplastic resin composition containing composite particles with polymer graft chains bonded to the particle surface, but sound absorption and sound insulation properties were not considered. In addition, in the foam formulation, it is not possible to knead the composite particles into the resin, and uniform dispersion of the composite particles in the foam was also an issue. In the above Patent Document 2, slag is mixed into polyurethane foam to increase its specific gravity, thereby aiming to improve sound insulation and vibration damping properties. However, sufficient sound insulation and vibration damping properties cannot be obtained by simply increasing the specific gravity. As disclosed in the above Patent Document 3, in thermosetting resin foam, the foam moldability is deteriorated when hydrophilic silica is blended, and hydrophobic silica is also used as a foam retention agent, and the relationship between these and vibration damping was not known. Therefore, the present inventors have studied the above problem and found that the vibration damping does not improve even if hydrophilic silica or hydrophobic silica is blended in thermosetting resin foam. On the other hand, unexpectedly, it has been newly found that the vibration damping can be significantly improved while maintaining the foam moldability of thermosetting resin foam by blending composite particles in which polymer graft chains are bonded to the particle surface. Although the mechanism is unclear, it is speculated that the vibration damping is improved by blending composite particles in which polymer graft chains are bonded to the particle surface, since the foam moldability is not hindered and high strain energy and damping energy can be generated in the polymer graft chains.
[0010] The thermosetting resin foam of the present invention is a foam containing a thermosetting resin and composite particles having polymer graft chains bonded to the particle surface (hereinafter, may be simply referred to as "composite particles").
[0011] Examples of thermosetting resin foams include polyurethane foam, urea resin foam, phenolic resin foam, unsaturated polyester resin foam, alkyd resin foam, melamine resin foam, epoxy resin foam, and silicon resin foam. From the viewpoint of sound absorption and sound insulation, polyurethane foam is preferred.
[0012] From the viewpoint of sound absorption and sound insulation, the expansion ratio of the thermosetting resin foam of the present invention is preferably 1.1 times or more, more preferably 5 times or more, and even more preferably 10 times or more, and from the same viewpoint, it is preferably 500 times or less, more preferably 200 times or less, and even more preferably 100 times or less. In this specification, the expansion ratio of the thermosetting resin foam is measured by the method described in the examples below.
[0013] The core density of the thermosetting resin foam of the present invention is preferably 5 kg / m from the viewpoint of noise reduction. 3 More preferably, 10 kg / m 3 More preferably, 30 kg / m 3 From the same viewpoint, it is preferably 1200 kg / m 3 Less than or equal to 500 kg / m 3 More preferably, 250 kg / m 3 In this specification, the core density in a thermosetting resin foam is measured by the method described in the Examples below.
[0014] The content of the thermosetting resin in the thermosetting resin foam is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more from the viewpoint of foam moldability. On the other hand, from the viewpoint of vibration damping property, it is preferably 99% by mass or less, more preferably 95% by mass or less, and even more preferably 90% by mass or less. For example, when the thermosetting resin foam is a polyurethane foam, the content of the thermosetting resin in the thermosetting resin foam refers to the total amount of the polyol component and the isocyanate component in the polyurethane foam.
[0015] The composite particles in the thermosetting resin foam of the present invention can be those proposed in the above Patent Document 1. The composite particles are particles in which polymer graft chains are bonded to the particle surface. As the particles, known fillers can be used, and examples thereof include metal oxides, metal oxide salts, metal hydroxides, metal carbonates, cellulose, etc., and preferably one or more types selected from the group consisting of metal oxides, metal oxide salts, metal hydroxides, and metal carbonates, more preferably one or more types selected from the group consisting of silicon oxides such as silica, and silicates such as mica and talc, and even more preferably silica. The shape of the particles is not particularly limited, and examples thereof include plate-like, granular, needle-like, and fibrous shapes. When simply described as "particles" in this specification, it refers to particles used in the production of composite particles. Examples of the polymer graft chain include homopolymers or copolymers of styrene-based monomers, nitrile-based monomers, (meth)acrylic-based monomers, unsaturated olefins, conjugated diene-based monomers, etc., and from the viewpoint of obtaining a molded article or a vibration-damping material exhibiting the desired vibration-damping properties, it is preferably one or more homopolymers or copolymers selected from the group consisting of acrylic acid, methacrylic acid, and derivatives thereof, more preferably one or more homopolymers or copolymers selected from methacrylic acid and its derivatives, and even more preferably polybutyl methacrylate. From the viewpoint of obtaining a molded article or a vibration-damping material exhibiting the desired vibration-damping properties, the bond is preferably a chemical bond, and even more preferably a covalent bond.
[0016] The glass transition temperature (Tg) of the polymer graft chain in the composite particle is preferably -30°C or higher, more preferably -20°C or higher, and even more preferably -10°C or higher from the viewpoint of improving the temperature range for vibration damping property expression, and from the same viewpoint, is preferably 80°C or lower, more preferably 70°C or lower, and even more preferably 60°C or lower. The polymer graft chain in the composite particle may have two or more glass transition temperatures (Tg), and may have a Tg other than Tg of -30°C or higher and 80°C or lower. The glass transition temperature (Tg) of the polymer graft chain in the composite particle can be controlled by the monomer, molecular weight, and molecular weight distribution used in the production of the composite particle. For example, in the case of the composite particle, it is known that Tg increases when the graft density increases and the polymer chain becomes an extended chain. In that case, Tg can be controlled by adjusting the graft density. In the temperature range near Tg, the tan δ of the viscoelasticity of the resin becomes maximum, which is effective for vibration damping property expression, and vibration damping property in a desired temperature range can be increased by controlling Tg. The glass transition temperature (Tg) is measured by the method described in the Examples below.
[0017] The graft density of the polymer graft chains in the composite particles is preferably 0.001 chains / nm from the viewpoint of increasing the strain energy in the polymer graft chains. 2 More preferably, 0.01 chains / nm 2 More preferably, 0.1 chains / nm 2 On the other hand, from the viewpoint of ease of grafting of polymer chains, it is preferable to set the number of chains to 5 / nm. 2 Less than or equal to 3 chains / nm, more preferably 2 More preferably, 1 chain / nm or less 2 Less than 0.3 chains / nm, more preferably 0.3 chains / nm 2 The graft density is measured by the method described in the Examples below.
[0018] The thickness of the polymer graft chain in the composite particle is preferably 1 nm or more, more preferably 3 nm or more, and even more preferably 5 nm or more, from the viewpoint of efficiently increasing the strain energy in the polymer graft chain. From the same viewpoint, the thickness is preferably 1 μm or less, more preferably 100 nm or less, more preferably 40 nm or less, and even more preferably 25 nm or less. The thickness of the polymer graft chain is calculated by the method described in the examples below.
[0019] The number average molecular weight of the polymer graft chain in the composite particle is preferably 10,000 or more, more preferably 20,000 or more, even more preferably 30,000 or more, and even more preferably 50,000 or more, from the viewpoint of controlling the film thickness of the polymer graft chain. From the same viewpoint, it is preferably 1,000,000 or less, more preferably 500,000 or less, even more preferably 200,000 or less, and even more preferably 100,000 or less. The number average molecular weight of the polymer graft chain is measured by the method described in the examples below.
[0020] The content of the composite particles in the thermosetting resin foam of the present invention is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more from the viewpoint of vibration damping property, and is preferably 70% by mass or less, more preferably 50% by mass or less, and even more preferably 30% by mass or less from the viewpoint of foam moldability. When two or more types of composite particles are contained, the blending amount is the total amount of the composite particles.
[0021] The composite particles can improve vibration damping while maintaining the foaming moldability of the thermosetting resin foam. Therefore, the present invention also provides a method for improving vibration damping by incorporating composite particles having polymer graft chains bonded to the particle surface into a thermosetting resin foam. The present invention also provides composite particles for thermosetting resin foam having polymer graft chains bonded to the particle surface. Here, the composite particles can also be dispersed in a dispersion medium such as toluene, xylene, ethanol, methanol, water, hydrofluoroolefin, liquid flame retardant (e.g., tris(chloropropyl)phosphate, etc.), amine catalyst (e.g., Kao Raiser No. 25, Kao Raiser No. 26, Kao Raiser No. 31, etc.; all manufactured by Kao), silicone foam stabilizer (e.g., VORASURF PRX-607, VORASURF SZ-1919, etc.; all manufactured by DOW). Therefore, the present invention also provides a dispersion for thermosetting resin foam containing composite particles having polymer graft chains bonded to the particle surface and a dispersion medium.
[0022] The dispersed particle size of the composite particles in the thermosetting resin foam of the present invention is preferably 1 nm or more, more preferably 10 nm or more, and even more preferably 100 nm or more from the viewpoint of vibration damping property expression and foam moldability, and is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 10 μm or less from the same viewpoint. The composite particles may exist alone or as aggregates. The dispersed particle size of the composite particles is measured by the method described in the Examples below.
[0023] The composite particles are obtained by bonding a polymer graft chain to the particle surface. The method of bonding a polymer graft chain to the particle surface is not particularly limited as long as it is a method that can graft a polymer chain, but the grafting from method in which the polymer graft chain is polymerized from the polymerization initiation point on the particle surface is preferred. The polymerization method is not particularly limited, but examples thereof include radical polymerization, anionic polymerization, and cationic polymerization. Among these, from the viewpoint of easy control of the molecular weight and molecular weight distribution of the polymer chain and the viewpoint of easy grafting of various copolymers, living radical polymerization, living anionic polymerization, and living cationic polymerization are preferred, and living radical polymerization is more preferred from the viewpoint of application to a wide range of monomers. As the living radical polymerization method, atom transfer radical polymerization method (ATRP method), reversible addition fragmentation chain transfer polymerization method (RAFT method), and living radical polymerization method mediated by nitroxide (NMP method) can be used, and from the same viewpoint, atom transfer radical polymerization method (ATRP method) is preferred.
[0024] More specifically, the method for producing the composite particles includes, for example, a production embodiment including the following step 2, and if necessary, the following step 1 may be carried out. The following steps 1 and 2 can be carried out under known conditions for living radical polymerization. Step 1: Attaching a polymerization initiating group to the particle surface Step 2: contacting particles having polymerization initiation groups on their surfaces with a monomer under living radical polymerization conditions
[0025] The particles having a polymerization initiating group on the surface in step 2 are not particularly limited as long as they have a binding group that bonds the particle surface and the polymer chain. The polymerization initiating group is a living radical polymerization initiating group from the viewpoint of binding a polymer graft chain to the particle surface, and is preferably an atom transfer radical polymerization initiating group, more preferably a haloacyl group, even more preferably an α-haloacyl group, even more preferably an α-bromoacyl group, and even more preferably a 2-bromoisobutyryl group. The compound that is the raw material of the binding group includes a compound having a group and a polymerization initiating group that are bound to the particle surface, and a compound having a group or a polymerization initiating group that are bound to the particle surface. Step 1 includes a step of introducing an amino group or a hydroxy group to the particle surface and a step of introducing a polymerization initiating group, and from the viewpoint of binding a polymer graft chain to the particle surface, preferably includes a step of introducing a polymerization initiating group to the particle surface after a step of introducing an amino group or a hydroxy group to the particle surface. The compound used in the step of introducing an amino group or a hydroxyl group to the particle surface is a compound having a group that bonds to the particle surface and an amino group or a hydroxyl group, and from the viewpoint of easy availability, it is preferably a silane compound, more preferably an aminoalkylsilane compound, and even more preferably 3-aminopropyltrimethoxysilane. The compound used in the step of introducing a polymerization initiator group to the particle surface is a compound having a functional group that reacts with a polymerization initiator group and an amino group or a hydroxyl group, and from the viewpoint of bonding a polymer graft chain to the particle surface, it is preferably a haloalkanoic acid derivative, more preferably a bromoalkanoic acid derivative, even more preferably a 2-bromo-2-methylpropionic acid derivative, and even more preferably 2-bromoisobutyl bromide. For example, when the particle originally has a polymerization initiation site or is formed as a result of surface treatment by plasma treatment or the like, it has a polymerization initiator group, so step 1 is not necessary, but when silica, mica, talc, glass filler, etc. that does not have a polymerization initiator group are used, step 1 may be performed. Note that, from the viewpoint of graft density adjustment, in step 1, a silane coupling agent that does not contain a polymerization initiator group may be added to the polymerization initiator group-containing silane coupling agent and used. In the step 1, in which the polymerization initiating groups are bonded to the particle surface, a method in which the particles are dispersed in a dispersion medium is preferred from the viewpoint of preventing the particles from agglomerating.
[0026] The monomer in step 2 can be a monomer constituting a thermoplastic elastomer known as a vibration-damping elastomer. Examples of the monomer constituting such a thermoplastic elastomer include styrene-based monomers, nitrile-based monomers, (meth)acrylic monomers, unsaturated olefins, conjugated diene monomers, and other monomers having specific groups in their side chains can also be used. In the step of contacting the particles having polymerization initiation groups on the surface with the monomer under living radical polymerization conditions in step 2, a method in which the particles, monomers, and composite particles are dispersed in a dispersion medium and polymerized is preferred from the viewpoint of preventing aggregation of the particles, monomers, and composite particles.
[0027] After polymerization, the composite particles may be optionally purified. In the purification step of the composite particles, it is preferable to disperse the composite particles in a dispersion medium in the polymer from the viewpoint of preventing the composite particles from agglomerating, and although the solvent may be optionally removed, it is preferable to leave a part of the dispersion medium and keep the polymer in a wet state. Furthermore, a method of removing the metal catalyst used in the polymerization step is preferable.
[0028] The thermosetting resin foam of the present invention may contain, in addition to the composite particles having polymer graft chains bonded to the particle surfaces and the thermosetting resin, additives such as surfactants, plasticizers, crosslinking agents, flame retardants, stabilizers, pigments, fillers, viscosity reducers, compatibilizers, and antistatic agents as optional components.
[0029] Examples of the surfactant include known nonionic surfactants and anionic surfactants, which are used for purposes such as viscosity reduction and compatibilization. Examples of the nonionic surfactant include ether-type surfactants such as polyoxyethylene alkyl ether, polyoxyethylene lauryl ether, polyoxyalkylene alkyl ether, polyoxyethylene polyoxypropylene alkyl ether, polyoxyethylene polyoxypropylene monobutyl ether, polyoxyethylene alkylphenyl ether, polyoxyethylene nonylphenyl ether, and polyoxyethylene polyoxypropylene monobutyl ether; polyoxyethylene oleate, glycerin fatty acid ester, polyoxyethylene stearate, polyoxyethylene fatty acid (lauryl) methyl ester, polyethylene glycol oleate monoester, and poly Examples of the ester ether type include oxyethylene sorbitan fatty acid esters; ester types such as polyoxyethylene alkyl esters, sucrose fatty acid esters, and sorbitan fatty acid esters; alkyl glycosides such as octyl glucoside; alkanolamide types such as polyoxyethylene oleic acid amide and polyoxyethylene alkyl amide; amine oxides such as dodecyl dimethylamine oxide and tetradecyl dimethylamine oxide; alkylamine types such as polyoxyethylene alkylamine and polyoxypropylene polyoxyethylene alkylamine; higher alcohols such as cetanol, stearyl alcohol, and oleyl alcohol; and polyoxyethylene distyrenated phenyl ether. From the viewpoint of high affinity and viscosity reducing effect, polyoxyethylene alkyl ethers are preferred, and commercially available products such as Emulgen LS106 (manufactured by Kao Corporation) can be used. Examples of the anionic surfactant include alkali metal salts of sulfonic acids such as olefin sulfonic acids, alkanesulfonic acids, alkylbenzenesulfonic acids, alkylnaphthalenesulfonic acids, alkyldiphenyletherdisulfonic acids, and polyoxyethylenealkylphenylethersulfonic acids; alkali metal salts of saturated or unsaturated fatty acids; and sulfate salts such as alkyl sulfate salts and polyoxyethylenealkylsulfate salts.The hydrophilic portion of the anionic surfactant may be a salt formed from an anionic polar group and an alkali metal, such as a sodium salt or a potassium salt.
[0030] Examples of the plasticizer include known ether-type and ester-type plasticizers. Examples of the ether-type plasticizer include ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, diethylene glycol monoisobutyl ether, ethylene glycol monohexyl ether, diethylene glycol monohexyl ether, ethylene glycol mono 2-ethylhexyl ether, diethylene glycol mono 2-ethylhexyl ether, ethylene glycol monoallyl ether, ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, and diethylene glycol monobenzyl ether. propylene oxide-based glycol ethers such as propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monomethyl ether, propylene glycol monopropyl ether, dipropylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monobutyl ether and propylene glycol monophenyl ether; and dialkyl glycol ethers such as ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether and dipropylene glycol dimethyl ether, of which diethylene glycol dibutyl ether is preferred from the viewpoint of high affinity and viscosity reducing effect.Examples of ester-type plasticizers include phthalate-based plasticizers such as dimethyl phthalate, diethyl phthalate, di-n-butyl phthalate, diheptyl phthalate, dioctyl phthalate, diisononyl phthalate, diisodecyl phthalate, ditridecyl phthalate, butyl benzyl phthalate, dicyclohexyl phthalate, and tetrahydrophthalic acid esters; phosphate-based plasticizers such as triethyl phosphate, tributyl phosphate, tri(2-ethylhexyl) phosphate, tributoxyethyl phosphate, triphenyl phosphate, diphenyldecyl phosphate, diphenyloctyl phosphate, and trixylenyl phosphate; benzoate-based plasticizers such as diethylene glycol dibenzoate, dipropylene glycol dibenzoate, triethylene glycol dibenzoate, and tripropylene glycol dibenzoate; ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monoisopropyl ether acetate, and ethylene glycol monoisopropyl ether acetate. Examples of the acetate-based plasticizers include ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monoisopropyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monoisopropyl ether acetate, propylene glycol monobutyl ether acetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol monoethyl ether acetate, dipropylene glycol monoisopropyl ether acetate, dipropylene glycol monobutyl ether acetate, triethylene glycol monomethyl ether acetate, and triethylene glycol monoethyl ether acetate.
[0031] The thermosetting resin foam of the present invention can be produced by foaming a thermosetting resin foam composition containing composite particles with polymer graft chains bonded to the particle surface by a known method. For example, when producing a polyurethane foam as a thermosetting resin foam, a polyurethane foam composition containing composite particles with polymer graft chains bonded to the particle surface, a polyol component, an isocyanate component, etc. can be foamed by a known method such as hand mixing foaming, simple foaming, injection method, froth injection method, spray method, etc.
[0032] In terms of improving foam moldability, a preferred method for producing a polyurethane foam is to prepare a polyol mixture containing composite particles having polymer graft chains bonded to the particle surface and a polyol component, and then foaming the polyurethane foam using the obtained polyol mixture and an isocyanate component.
[0033] A method for preparing a polyol mixture containing composite particles with polymer graft chains bonded to the particle surface and a polyol component is preferably a method of dispersing the composite particles in a dispersion medium such as toluene, ethyl acetate, propyl acetate, methanol, isopropyl alcohol, propylene glycol monomethyl ether, hexane, or dimethylformamide in advance, and then replacing the solvent with a polyol from there. As the dispersion medium, a dispersion medium having compatibility with the polyol is preferable, and toluene, ethyl acetate, propyl acetate, methanol, isopropyl alcohol, or propylene glycol monomethyl ether is more preferable, and toluene, methanol, isopropyl alcohol, or propylene glycol monomethyl ether is even more preferable. Examples of a method for replacing the solvent include a method of separating the composite particles by centrifugation and redispersing them in a new solvent, or a method of transferring the particles to a column and passing a new solvent 3 to 10 times the column volume through the column to replace the solvent. Alternatively, the composite particles with polymer graft chains bonded to the particle surface may be directly mixed with a polyol, and in the case of direct mixing, a method of mixing using an appropriate device such as a lab mixer is preferable. Additives such as surfactants, plasticizers, catalysts, foaming agents, foam stabilizers, interconnecting agents, crosslinking agents, flame retardants, stabilizers, pigments, fillers, viscosity reducers, compatibilizers, and antistatic agents may be added to the polyol mixture in appropriate amounts.In particular, from the viewpoint of the effect of reducing the viscosity of the polyol mixture, it is preferable to add the above-mentioned surfactants and plasticizers, and ether-type surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene lauryl ethers, polyoxyalkylene alkyl ethers, polyoxyethylene polyoxypropylene alkyl ethers, polyoxyethylene polyoxypropylene monobutyl ethers, polyoxyethylene alkyl phenyl ethers, polyoxyethylene nonyl phenyl ethers, and polyoxyethylene polyoxypropylene monobutyl ether, and dialkyl glycol ether-type plasticizers such as ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, and dipropylene glycol dimethyl ether are more preferable, and one or more selected from polyoxyethylene alkyl ethers and diethylene glycol dibutyl ether are even more preferable.
[0034] In the above polyurethane foam embodiment, the amount of the composite particles having polymer graft chains bonded to the particle surface in the polyol mixture is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, based on 100 parts by mass of the polyol, from the viewpoint of vibration damping property expression, while it is preferably 100 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 70 parts by mass or less, from the viewpoint of dispersibility and foam moldability expression.
[0035] Examples of the polyol component include those that have been conventionally used in producing polyurethane foams.
[0036] Representative examples of polyol components include polyester polyols, polyether polyols, polymer polyols, phenolic resin polyols, Mannich polyols, etc., which are described in "Polyurethane Resin Handbook" edited by Iwata Keiji (September 25, 1987, Nikkan Kogyo Shimbun), and these can be used alone or in combination of two or more.
[0037] The polyester polyols are obtained by polymerization of a polyfunctional alcohol, preferably having 2 to 12 carbon atoms, more preferably 2 to 6 carbon atoms, with a polyfunctional carboxylic acid, preferably having 2 to 12 carbon atoms, more preferably 2 to 6 carbon atoms. The polyfunctional alcohol for preparing the polyester polyols is preferably a diol or triol, more preferably a mixture of diols and triols, including ethylene glycol, propylene glycol, butylene glycol, pentylene glycol, or hexylene glycol. The polyfunctional carboxylic acid is selected from the group consisting of succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, decanedicarboxylic acid, maleic acid, fumaric acid, preferably phthalic acid, isophthalic acid, terephthalic acid, isomeric naphthalenedicarboxylic acids, and combinations thereof. The polyester polyols are preferably terminated with at least two hydroxyl groups.
[0038] The polyether polyols preferably have an average hydroxyl functionality of 2 to 8, more preferably 3 to 6, and are prepared by polymerization in the presence of a catalyst with one or more alkylene oxides selected from propylene oxide (PO), ethylene oxide (EO), butylene oxide, tetrahydrofuran and mixtures thereof, with a suitable starter molecule. The starter molecules preferably include compounds having at least two, more preferably 3 to 8, hydroxyl groups or two or more primary or secondary amino groups in the molecule.
[0039] Representative examples of polymer polyols include those in which polymer fine particles obtained by polymerizing a polymerizable unsaturated group-containing monomer are dispersed in a polyether polyol. For example, this can be produced by mixing and dispersing the polymer fine particles obtained by polymerizing a polymerizable unsaturated group-containing monomer with a polyether polyol, or by polymerizing the polymerizable unsaturated group-containing monomer in the polyether polymer to disperse the polymer fine particles obtained from the polymerizable unsaturated group-containing monomer in the polyether polyol. Among these methods, the latter method is preferred because it can easily obtain a polymer polyol in which the polymer fine particles are uniformly dispersed in the polyether polyol. As the polymer fine particles, polystyrene, polyacrylonitrile and styrene-acrylonitrile copolymers are preferred.
[0040] Among these, from the viewpoint of improving the foam moldability of a thermosetting resin foam containing composite particles having polymer graft chains bonded to the particle surface while maintaining vibration damping and sound insulation, it is preferable to use one or more selected from polyether polyols and polymer polyols as the polyol component, and it is more preferable to use polyether polyols and polymer polyols. More specifically, one or more selected from polyether polyols having an average functional group of 2 to 8 hydroxyl groups and obtained by polymerization of one or more alkylene oxides selected from propylene oxide (PO), ethylene oxide (EO), butylene oxide, tetrahydrofuran and mixtures thereof with a compound having at least two hydroxyl groups or two or more primary or secondary amino groups in the molecule, and polymer polyols in which at least one or more polymer fine particles selected from polystyrene, polyacrylonitrile and styrene-acrylonitrile copolymers are dispersed in the polyether polyol are used. It is preferable to use polyether polyols having an average functional group of 2 to 8 hydroxyl groups and obtained by polymerization of one or more alkylene oxides selected from propylene oxide (PO), ethylene oxide (EO), butylene oxide, tetrahydrofuran, and mixtures thereof, with a compound having at least two hydroxyl groups or two or more primary or secondary amino groups in the molecule, and it is more preferable to use polymer polyols in which at least one or more polymer fine particles selected from polystyrene, polyacrylonitrile, and styrene-acrylonitrile copolymers are dispersed in the polyether polyol.
[0041] The average hydroxyl value of the polyol component is preferably 14 to 100 mgKOH / g, more preferably 17 to 75 mgKOH / g, and even more preferably 17 to 70 mgKOH / g, from the viewpoints of imparting viscosity and elasticity to the foam.
[0042] A foam stabilizer can be used as required, and any foam stabilizer generally used in the production of polyurethane foams may be used.
[0043] Representative examples of the foam stabilizer include silicone surfactants such as dimethylpolysiloxane and polyoxyalkylene-modified dimethylpolysiloxane, and anionic surfactants such as fatty acid salts, sulfate salts, phosphate salts, and sulfonate salts. These may be used alone or in combination of two or more.
[0044] The amount of foam stabilizer used varies depending on the type of foam stabilizer and the type and density of the desired polyurethane foam, and therefore cannot be determined in general terms. It is therefore desirable to adjust the amount appropriately depending on the type of foam stabilizer, etc.
[0045] As the stabilizer, any stabilizer generally used in the production of polyurethane foams can be used as necessary. From the viewpoint of improving the foam strength, however, triphenyl phosphite and pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] are preferably used, and it is particularly preferable to use these in combination.
[0046] The amount of stabilizer used varies depending on the type of stabilizer, the type and density of the desired polyurethane foam, etc., and therefore cannot be determined in general terms. It is therefore desirable to adjust the amount appropriately depending on the type of stabilizer, etc.
[0047] Examples of the isocyanate component include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, polymethylene polyphenylene polyisocyanate, xylylene diisocyanate, and naphthylene diisocyanate; aliphatic polyisocyanates such as hexamethylene diisocyanate and lysine diisocyanate; alicyclic polyisocyanates such as hydrogenated diphenylmethane diisocyanate, hydrogenated tolylene diisocyanate, and isophorone diisocyanate; and modified polyisocyanates containing one or more of a urethane bond, a carbodiimide bond, a uretoimine bond, an allophanate bond, a urea bond, a biuret bond, an isocyanurate bond, and the like. These may be used alone or in combination of two or more.
[0048] Among the isocyanate components, from the viewpoint of imparting appropriate impact absorption and elasticity, tolylene diisocyanate, diphenylmethane diisocyanate, polymethylene polyphenylene polyisocyanate, and polyisocyanate modified products containing one or more of these urethane bonds, carbodiimide bonds, etc. are preferred. Diphenylmethane diisocyanate and polymethylene polyphenylene polyisocyanate are more preferred, and these can be used alone or in combination of two or more.
[0049] The amount of the isocyanate component varies depending on the required properties of the polyurethane foam and cannot be determined in general. However, it is usually preferable to adjust the ratio of the polyol mixture described below to the isocyanate component (isocyanate index) to 30 to 200, more preferably 80 to 110, and even more preferably 95 to 105.
[0050] The blowing agent may suitably be water, azo compounds such as azodicarbonamide, azobisisobutyrodinitrile, and barium azodicarboxylate, hydrazide compounds such as 4,4'-oxybisbenzenesulfonylhydrazide and p-toluenesulfonylhydrazide, nitroso compounds such as dinitrosopentamethylenetetramine, hydrazo compounds such as hydrazodicarbonamide, tetrazole compounds such as 5-phenyltetrazole, 5-aminotetrazole, azobistetrazole, and bistetrazole, ester compounds such as hydrazodicarboxylate, azodicarboxylate, and citrate, isocyanate compounds, sodium bicarbonate, and sodium carbonate. In addition to the chemical blowing agents, low-boiling point hydrocarbons such as isopentane, normal pentane, and cyclopentane, nitrogen, air, carbon dioxide, hydrofluoroolefins, and hydrochlorofluoroolefins may be used as physical blowing agents within the scope of the present invention. The blowing agent preferably contains water from the viewpoint of less environmental load, and preferably uses water alone or in combination with other blowing agents, more preferably water alone. Examples of hydrofluoroolefins (HFOs) include pentafluorobutene isomers (HFO1354), hexafluorobutene isomers (HFO1336) such as 1,1,1,4,4,4-hexafluoro-2-butene (HFO1336mzz), heptafluoropentene isomers (HFO1447), and octafluoropentene isomers (HFO1438). Examples of hydrochlorofluoroolefins (HCFOs) include 1-chloro-3,3,3-trifluoropropene (HCFO-1233zd), 2-chloro-3,3,3-trifluoropropene (HCFO-1233xf), and 1-chloro-2,3,3-tetrafluoropropene (HCFO-1224yd). From the viewpoint of low global warming potential and viscosity reducing effect, hydrochlorofluoroolefin is preferred, and 1-chloro-3,3,3-trifluoropropene is more preferred.
[0051] The amount of foaming agent to be mixed varies depending on the core density of the target polyurethane foam, and therefore cannot be determined in general, and is preferably adjusted appropriately according to the target core density. For example, when water is used as a chemical foaming agent, the amount is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, based on 100 parts by mass of polyol, from the viewpoint of foam moldability. On the other hand, from the viewpoint of vibration damping property and foam moldability, the amount is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less.
[0052] The composite particles having the polymer graft chains bonded to the particle surface for use in thermosetting resin foams can be stored in various forms and can be used appropriately for the production of thermosetting resin foams. The composite particles themselves can be stored and suitably stored in the form of a polyol mixture in which the composite particles are dispersed in a polyol, or a composite particle dispersion in which the composite particles are dispersed in a dispersion medium other than the polyol before the solvent replacement with the polyol. As the dispersion medium other than the polyol, a dispersion medium compatible with the polyol is preferable, and toluene, ethyl acetate, propyl acetate, methanol, isopropyl alcohol, and propylene glycol monomethyl ether are more preferable, and toluene, methanol, isopropyl alcohol, and propylene glycol monomethyl ether are even more preferable.
[0053] The content of the composite particles in the polyol mixture is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, based on 100 parts by mass of polyol, from the viewpoint of vibration damping property expression. On the other hand, from the viewpoint of dispersibility and foam moldability expression, it is preferably 100 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 70 parts by mass or less. In addition, the content of the composite particles in the composite particle dispersion medium is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, based on 100 parts by mass of the dispersion medium other than polyol, from the viewpoint of vibration damping property expression. On the other hand, from the viewpoint of dispersibility and foam moldability expression, it is preferably 100 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 70 parts by mass or less.
[0054] The thermosetting resin foam of the present invention can be suitably used as a sound insulation material and a vibration damping material for products such as acoustic equipment, electrical products, buildings, industrial equipment, automobile parts, motorcycle parts, containers, etc., or their parts or housings. The application to these can be appropriately set according to the manufacturing method, application location, and desired purpose of the parts, housings, devices, and equipment, and can be used according to the usual methods in the technical field.
[0055] In addition, it is known that thermosetting resin foams, such as polyurethane foam, exhibit high sound insulation. The sound absorbing property is due to the fact that sound (air waves and vibrations) enter the bubbles of polyurethane foam and bounce in various directions, dispersing the sound energy. Although this sound insulation performance is highly effective in the high frequency range, it is relatively ineffective in the low frequency range. Furthermore, it is said that sound insulation performance decreases in the frequency range where the foam resonates and the frequency range where the coincidence effect occurs. On the other hand, the present invention significantly improves the vibration damping properties of polyurethane foam, and is therefore expected to improve sound insulation performance in a wide frequency range.
[0056] <1> A thermosetting resin foam comprising composite particles having polymer graft chains attached to the particle surface. <2> The foam is a polyurethane foam, a urea resin foam, a phenolic resin foam, an unsaturated polyester resin foam, an alkyd resin foam, a melamine resin foam, an epoxy resin foam, or a silicone resin foam. <1> 2. The thermosetting resin foam according to claim 1 . <3> The expansion ratio is preferably 1.1 times or more, more preferably 5 times or more, even more preferably 10 times or more, and preferably 500 times or less, more preferably 200 times or less, even more preferably 100 times or less. <1> or <2> 2. The thermosetting resin foam according to claim 1 . <4> The core density is preferably 5 kg / m 3 More preferably, 10 kg / m 3More preferably, 30 kg / m 3 More than 1200kg / m 3 Less than or equal to 500 kg / m 3 More preferably, 250 kg / m or less 3 Below is the <1> ~ <3> 2. The thermosetting resin foam according to claim 1 .
[0057] <5> A method for producing a thermosetting resin foam, comprising a step of foaming a thermosetting resin foam composition containing composite particles having polymer graft chains bonded to the particle surface. <6> The method includes the step of preparing a polyol mixture containing composite particles having polymer graft chains bonded to the particle surface and a polyol component. <5> A method for producing a thermosetting resin foam according to claim 1. <7> the step of preparing a polyol mixture comprises a step of dispersing composite particles having polymer graft chains bonded to the particle surface in one or more solvents selected from toluene, ethyl acetate, propyl acetate, methanol, isopropyl alcohol, propylene glycol monomethyl ether, hexane, and dimethylformamide, preferably a dispersion medium compatible with polyol, more preferably toluene, ethyl acetate, propyl acetate, methanol, isopropyl alcohol, and propylene glycol monomethyl ether, and further preferably toluene, methanol, isopropyl alcohol, and propylene glycol monomethyl ether, and then replacing the solvent with a polyol; <6> A method for producing a thermosetting resin foam according to claim 1. <8> The amount of the composite particles having polymer graft chains bonded to the particle surface in the polyol mixture is preferably 1 part by mass or more, more preferably 5 parts by mass or more, even more preferably 10 parts by mass or more, and preferably 100 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 70 parts by mass or less, relative to 100 parts by mass of the polyol. <6> or <7> A method for producing a thermosetting resin foam according to claim 1. <9> The polyol component is preferably one or more selected from polyether polyols and polymer polyols, more preferably polyether polyols and polymer polyols, and even more preferably polyether polyols having an average functional group of 2 to 8 hydroxyl groups and obtained by polymerization of one or more alkylene oxides selected from propylene oxide (PO), ethylene oxide (EO), butylene oxide, tetrahydrofuran and mixtures thereof with a compound having at least two hydroxyl groups or two or more primary or secondary amino groups in the molecule, and at least one or more polymer fine particles selected from polystyrene, polyacrylonitrile and styrene-acrylonitrile copolymers. one or more selected from polymer polyols dispersed in polyether polyols, more preferably polyether polyols obtained by polymerization of one or more alkylene oxides selected from propylene oxide (PO), ethylene oxide (EO), butylene oxide, tetrahydrofuran and mixtures thereof with a compound having at least two hydroxyl groups or two or more primary or secondary amino groups in the molecule, and polymer polyols in which at least one or more polymer fine particles selected from polystyrene, polyacrylonitrile and styrene-acrylonitrile copolymers are dispersed in polyether polyols; <6> ~ <8> A method for producing the thermosetting resin foam according to any one of claims 1 to 4. <10> The isocyanate component preferably includes tolylene diisocyanate, diphenylmethane diisocyanate, polymethylene polyphenylene polyisocyanate, and polyisocyanate-modified products thereof containing one or more of a urethane bond, a carbodiimide bond, etc., more preferably diphenylmethane diisocyanate and polymethylene polyphenylene polyisocyanate. <6> ~ <9> A method for producing the thermosetting resin foam according to any one of claims 1 to 4. <11> The ratio of the polyol mixture to the isocyanate component (isocyanate index) is preferably 30 to 200, more preferably 80 to 110, and even more preferably 95 to 105. <6> ~ <10> A method for producing the thermosetting resin foam according to any one of claims 1 to 4. <12> water, azo compounds such as azodicarbonamide, azobisisobutyrodinitrile, and barium azodicarboxylate, hydrazide compounds such as 4,4'-oxybisbenzenesulfonylhydrazide and p-toluenesulfonylhydrazide, nitroso compounds such as dinitrosopentamethylenetetramine, hydrazo compounds such as hydrazodicarbonamide, tetrazole compounds such as 5-phenyltetrazole, 5-aminotetrazole, azobistetrazole, and bistetrazole, ester compounds such as hydrazodicarboxylate esters, azodicarboxylate esters, and citric acid esters, isocyanate compounds, low-boiling point hydrocarbons such as sodium bicarbonate, sodium carbonate, isopentane, normal pentane, and cyclopentane, nitrogen, air, carbon dioxide, and one or more blowing agents selected from the group consisting of hydrofluoroolefins; <6> ~ <11> A method for producing the thermosetting resin foam according to any one of claims 1 to 4. <13> the blowing agent contains water, and the content of the blowing agent is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the polyol; <6> ~ <12> A method for producing the thermosetting resin foam according to any one of claims 1 to 4. <14> the content of the composite particles having polymer graft chains bonded to the particle surface in the polyol mixture is preferably 1 part by mass or more, more preferably 5 parts by mass or more, even more preferably 10 parts by mass or more, and preferably 100 parts by mass or less, more preferably 80 parts by mass or less, even more preferably 70 parts by mass or less, relative to 100 parts by mass of the polyol; <6> ~ <13> A method for producing the thermosetting resin foam according to any one of claims 1 to 4.
[0058] <15> the composite particles having polymer graft chains bonded to their particle surfaces are silica particles having polymer graft chains bonded to their particle surfaces, The polymer graft chain comprises one or more homopolymers or copolymers selected from the group consisting of acrylic acid, methacrylic acid, and derivatives thereof; At least one of the polymer graft chains has a glass transition temperature of -30°C or higher and 80°C or lower; The graft density of the polymer graft chains is 0.01 chains / nm 2 More than 1 chain / nm 2 is as follows: The film thickness of the polymer graft chain is 3 nm or more and 40 nm or less, The number average molecular weight of the polymer graft chain is 30,000 or more and 200,000 or less. <1> ~ <4> The thermosetting resin foam according to any one of claims 1 to 4, <5> ~ <14> A method for producing the thermosetting resin foam according to any one of claims 1 to 4. <16> The dispersed particle size of the composite particles in the thermosetting resin foam is preferably 1 nm or more, more preferably 10 nm or more, even more preferably 100 nm or more, and preferably 200 μm or less, more preferably 100 μm or less, even more preferably 10 μm or less. <1> ~ <4> , <15> 2. The thermosetting resin foam according to claim 1 . <17> The content of the composite particles in the thermosetting resin foam is preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and preferably 70% by mass or less, more preferably 50% by mass or less, even more preferably 30% by mass or less. <1> ~ <4> , <15> ~ <16> 2. The thermosetting resin foam according to claim 1 . <18> <1> ~ <4> , <15> ~ <17> The thermosetting resin foam according to any one of claims 1 to 4, <5> ~ <14> A method for producing composite particles for use in any one of the methods for producing a thermosetting resin foam, the method comprising the following step 2, or the method for producing composite particles comprising the following steps 1 and 2. Step 1: Attaching a polymerization initiating group to the particle surface Step 2: contacting particles having polymerization initiation groups on their surfaces with a monomer under living radical polymerization conditions <19> <1> ~ <4> , <15> ~ <16> A dispersion for use in the thermosetting resin foam described in any one of the above, comprising composite particles having polymer graft chains bonded to the particle surface and a dispersion medium. <20> The content of the composite particles in the dispersion medium is preferably 1 part by mass or more, more preferably 5 parts by mass or more, even more preferably 10 parts by mass or more, and preferably 100 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 70 parts by mass or less, relative to 100 parts by mass of the dispersion medium other than the polyol. <19> 2. The dispersion for a thermosetting resin foam according to claim 1 . EXAMPLES
[0059] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples in any way.
[0060] <Glass transition temperature of polymer graft chains in composite particles> Measurement was performed according to the method of JIS K 7121. Using a differential scanning calorimeter (DSC7020 manufactured by Hitachi High-Tech Science), the composite particles were heated from 40°C to 200°C at a rate of 10°C / min, and the heat capacity was measured. The midpoint glass transition temperature Tmg (°C) was determined as the temperature at the point where a straight line equidistant in the vertical direction from the extended straight line of each baseline intersected with the curve of the stepwise change portion of the glass transition in the DSC thermogram.
[0061] <Number average molecular weight of polymer graft chains in composite particles> The number average molecular weight of the polymer graft chains in the composite particles was measured by taking the number average molecular weight of the polymer chains not bonded to the composite particles, which were simultaneously produced in the process of producing the composite particles, as the number average molecular weight of the polymer graft chains. The number average molecular weight was measured by gel permeation chromatogram (GPC) using GMHHR-H+GMHHR-H (cation) as a column, chloroform as a solvent, a flow rate of 1.0 mL / min, and a column temperature of 40°C, using polystyrene as a molecular weight standard.
[0062] <Graft density of polymer chains in composite particles> Graft density (chains / nm 2 ) was calculated by measuring the graft amount (W) and the number average molecular weight (Mn) of the graft chains and using the following formula. The graft amount was calculated by thermal weight loss measurement (TG). More specifically, the temperature was raised from 40°C to 500°C at a rate of 10°C / min in air, and the weight loss rate at that time was measured. The number average molecular weight of the graft chains was calculated by the gel permeation chromatography (GPC) method shown below. Graft density (chains / nm 2 ) = Graft amount (g / nm 2 ) / number average molecular weight of grafted chains × (Avogadro's number)
[0063] <Film thickness of polymer graft chains in composite particles> The film thickness was calculated from the following formula. The polymer density of the polymer chains not bonded to the composite particles, which are generated simultaneously in the process of producing the composite particles, was taken as the polymer density of the polymer graft chains. It was measured by the pycnometer method according to JIS K 7112.
[0064]
number
[0065] <Dispersion particle size of composite particles> The fracture surface of a test piece of thermosetting resin foam composite particles was observed with a scanning electron microscope (SEM). From the image observed with the SEM, the cross sections of 30 composite particles were selected, and the major axis of each was visually read, and the average value was taken as the dispersed particle diameter. conditions Equipment: Field emission scanning electron microscope (S-4000, Hitachi, Ltd.) Acceleration magnification: 10kV Spot diameter: 8mm Magnification: 400x~5000x
[0066] [Preparation of composite particle 1] a) A step of bonding a polymerization initiating group to the particle surface a-1) Introduction of amino groups onto the surface of silica particles 40 g of silica particles (Admafine SO-C1, manufactured by Admatechs, average particle size 200 nm) and 2 g of 3-aminopropyltrimethoxysilane (KBM-903, manufactured by Shin-Etsu Chemical Co., Ltd.) were added to 200 mL of ethanol. The mixture was stirred at room temperature for 12 hours. After that, it was washed with ethanol, and the silica particles were collected by a centrifuge, and then heated at 110°C for 1 hour to obtain amino group-introduced silica particles.
[0067] a-2) Introduction of polymerization initiator groups onto the surface of amino group-introduced silica particles 40 g of the above amino group-introduced silica microparticles, 200 mL of anhydrous THF, 1 mL of anhydrous triethylamine (Tokyo Chemical Industry Co., Ltd.), and 1 mL of 2-bromoisobutyl bromide (BIBB, Tokyo Chemical Industry Co., Ltd.) were placed in a 500 mL eggplant flask and stirred at room temperature for 2 hours. After that, the silica microparticles were washed with THF and anisole, and the polymerization initiator group-introduced silica microparticles into which 2-bromoisobutyryl groups were introduced as polymerization initiator groups were collected by a centrifuge and then stored as an anisole-wet form of the polymerization initiator group-introduced silica microparticles.
[0068] b) contacting particles having polymerization initiation groups on their surfaces with a monomer under living radical polymerization conditions; In a 500 mL separable flask, the anisole wet body containing 12 g of the prepared silica microparticles having polymerization initiator groups, 60 g of anisole, and 180 g of butyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) were placed, thoroughly stirred, and then reduced pressure and nitrogen replacement were performed. The temperature was then raised to 80°C, and an acetonitrile solution in which 860 mg of Cu(I)Br (manufactured by Tokyo Chemical Industry Co., Ltd.) and 2080 mg of pentamethyldiethylenetriamine (manufactured by Tokyo Chemical Industry Co., Ltd.) had been stirred in advance in 5 mL of acetonitrile under nitrogen was poured in, and polymerization was initiated. The mixture was then stirred for 10 minutes. Then, ice water cooling and air bubbling were performed, and an excess of methanol was added to quench the reaction. Then, washing with methanol and removal of the solution by a centrifuge were repeated three times, and the solvent was dried to obtain silica microparticles grafted with polybutyl methacrylate. The content of polymer graft chains was 28.3% by mass. The glass transition temperature was 30°C, the number average molecular weight was 70,000, and the graft density was 0.20 chains / nm 2 The film thickness was 20 nm.
[0069] [Preparation of composite particle 2] In the above-mentioned step of contacting the particles having polymerization initiation groups on the surface with the monomer under living radical polymerization conditions, 180 g of butyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) was replaced with 72 g of butyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) and 108 g of butyl acrylate (manufactured by Tokyo Chemical Industry Co., Ltd.), and the same process was used to obtain silica microparticles grafted with a copolymer of polybutyl methacrylate and polybutyl acrylate. The content of polymer graft chains was 20.1% by mass. The glass transition temperature was -20°C, the number average molecular weight was 65,000, and the graft density was 0.14 chains / nm 2 The film thickness was 13 nm.
[0070] [Preparation of hydrophobic silica] 40 g of silica particles (Admafine SO-C1, manufactured by Admatechs, average particle size 200 nm) and 2 g of 1,1,1,3,3,3-hexamethyldisilazane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to 200 mL of ethanol. The mixture was stirred at room temperature for 12 hours. After that, it was washed with ethanol, and the silica particles were collected by a centrifuge, and then heated at 110°C for 1 hour to obtain hydrophobic silica particles.
[0071] Example 1 a) Dispersing the composite particles in a polyol 9 g of the obtained silica microparticles grafted with polybutyl methacrylate (composite particles 1) were thoroughly stirred in toluene and further irradiated with ultrasonic waves to obtain a toluene dispersion. After that, the toluene was simply removed using a centrifuge, and 13 g of diol-type polypropylene glycol (PPG3000, Fujifilm Wako Pure Chemical Industries, Ltd.) was added thereto and stirred for 2 hours at room temperature. After that, stirring and dispersion were performed for 6 minutes at a revolution speed of 1600 rpm and a rotation speed of 1600 rpm using a planetary rotation / revolution mixer (ARE-400TWIN, Thinky Corporation). After that, the toluene was removed using an evaporator, and the mixture was dried at 100°C for 12 hours to obtain a polyol dispersion.
[0072] b) obtaining a desired polyol mixture A polyol mixture was obtained by mixing 21 g of the obtained polyol dispersion, 11 g of polyol B [PPG type polymer polyol (average hydroxyl value: 28 mgKOH / g, manufactured by Sanyo Chemical Industries, Ltd., product name: Sannix FA-728R)], 0.4 g of triethanolamine, 1 g of water as a foaming agent, 0.06 g of a silicone foam stabilizer [manufactured by DOW, product name: VORASURF PRX607], 0.1 g of a metal catalyst (dibutyltin dilaurate, manufactured by Sigma-Aldrich), and 0.06 g of an amine catalyst (a 33 mass % solution of triethylenediamine in dipropylene glycol, product name: Kaolizer No. 31) in a laboratory mixer.
[0073] [Preparation of thermosetting urethane resin composition and molding of polyurethane foam] The obtained polyol mixture and the isocyanate component [Cosmonate TM-20 (polyisocyanate (mixture of 80% by mass of 2,4-tolylene diisocyanate and 2,6-tolylene diisocyanate in a mass ratio of 80:20 (TDI) 80% by mass and polymethylene polyphenylene polyisocyanate 20% by mass), isocyanate group content: 45% by mass, manufactured by Mitsui Chemicals Polyurethanes)] were adjusted to a liquid temperature of 20°C. A total of 30 g of these were collected in a 300 mL disposable cup so that the isocyanate index was 100, and they were mixed and stirred at room temperature of 20°C in a laboratory mixer to form a polyurethane free form. The obtained molded body was left at room temperature of 20°C for 1 day to obtain a polyurethane foam.
[0074] Examples 2 to 5, Comparative Examples 1 to 3 A polyurethane foam was prepared in the same manner as in Example 1, except that the composition was changed to that shown in Table 1. The amount of composite particles 2 in Example 5 was adjusted so that the amount of grafted polymer therein was the same as that in Example 1.
[0075] <Foam moldability> [exterior] The size of the depression (after the health bubble) of the free foam during foam molding and the average bubble diameter (excluding air entrapment) were visually evaluated. The results are shown in Table 1. ⊚: Compared with the appearance of the sample of Comparative Example 1, the free form depression is the same or smaller, and the bubble diameter is the same or smaller. ◯: Compared to the appearance of the sample in Comparative Example 1, the free form depression is the same or smaller, and the bubble diameter is larger. △: Compared to the appearance of the sample of Comparative Example 1, the free form has a large depression, and the bubble diameter is the same or smaller. ×: Compared with the appearance of the sample of Comparative Example 1, the free form has a large depression and the bubble diameter is large.
[0076] [Core Density] After the free form was produced, it was left for one day, and then a test piece measuring 50 mm x 50 mm x 20 mm was cut out from the core, and the weight of the test piece was measured and divided by its volume. The results are shown in Table 1.
[0077] [Expansion ratio] The expansion ratio of the obtained polyurethane foam was calculated by dividing the density of the raw material resin before foaming by the core density. The expansion ratios of the obtained polyurethane foam are shown in Table 1. The density of the raw material before foaming is calculated by dividing the density of the main component, polypropylene glycol (1.0×10 3 kg / m 3 ), Polyol B (1.0×10 3 kg / m 3 ) Polyisocyanate (1.2 x 10 3 kg / m 3 ), composite particles (1.7×10 3 kg / m 3 ) arithmetic mean value (total of 96 mass%; approximately 1.1 × 10 3 kg / m 3 ) was estimated.
[0078] <Vibration damping> [Tan δ value of peak top, Tan δ temperature of peak top] The free form was heated and compressed at 150 ° C. using an auto press molding machine (manufactured by Toyo Seiki Seisakusho), cooled and molded at 15 ° C., and then a viscoelasticity measurement test piece (20 mm × 5 mm × 1 mm) was cut out. This test piece was heated from -20 ° C. to 120 ° C. at a heating rate of 2 ° C. / min using a DMA device (manufactured by SII, EXSTAR6000) with a measurement frequency of 1 Hz and a strain amplitude of 0.05%, and the peak top tan δ value and the peak top tan δ temperature were measured. The higher the tan δ value, the higher the vibration damping performance. An improvement of 0.01 or more can be judged to be a significant difference, and an improvement of preferably 0.03 or more, more preferably 0.05 or more can be judged to be a significant improvement in vibration damping performance.
[0079] [Table 1]
[0080] Details of each component shown in Table 1 are as follows. PPG3000: Polypropylene glycol, diol type, 3000 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) Exenol 3030: Polypropylene glycol, triol type, average hydroxyl value: 56 KOHmg / g (AGC Corporation) Sumiphen 3900: Branched polyether polyol, a PPG with ethylene oxide added to the end, average hydroxyl value: 35 mg KOH / g (manufactured by Sumika Bayer Urethane Co., Ltd.) Sannix FA-728R: Polypropylene glycol type acrylonitrile polymer polyol, polymer concentration 20% by weight, average hydroxyl value: 28 mgKOH / g, (manufactured by Sanyo Chemical Industries, Ltd.) Silica: Silica fine particles, average particle size 200 nm (Admafine SO-C1, manufactured by Admatechs Co., Ltd.) Triethanolamine: (Sigma-Aldrich) Dibutyltin laurate: (Sigma-Aldrich) Kaolizer No. 31: 33% by weight solution of triethylenediamine in dipropylene glycol (Kao Corporation) Kaolizer No. 25: 6-Dimethylamino-1-hexanol (Kao Corporation) Kaolizer No.26: 2-[2-(dimethylamino)ethoxy]ethanol (Kao Corporation) PRX-607: Silicone foam stabilizer (VORASURF PRX607, manufactured by Dow Toray) Cosmonate TM-20: polyisocyanate (a mixture of 80% by mass of 2,4-tolylene diisocyanate and 2,6-tolylene diisocyanate (TDI) in an 80:20 mass ratio and 20% by mass of polymethylene polyphenylene polyisocyanate), isocyanate group content: 45% by mass (manufactured by Mitsui Chemicals Polyurethanes, Inc.)
[0081] As shown in Table 1, it can be seen that in all of Examples 1 to 5, which contained the specified composite particles, the vibration damping properties were significantly improved while maintaining the foam moldability. On the other hand, in Comparative Example 2, which contained silica, the foam moldability was deteriorated and no improvement in the vibration damping properties was observed. In Comparative Example 3, which contained hydrophobic silica, although there was no problem with the foam moldability, no improvement in the vibration damping properties was observed. Note that, since the tan δ of the peak top was broad for Comparative Examples 1 to 3, the temperature of the tan δ of the peak top could not be specified.
[0082] [Preparation of composite particle 3] Silica microparticles grafted with a copolymer of polybutyl methacrylate and polybutyl acrylate were obtained in the same manner as in Composite Particle 2, except that 90 g of butyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) and 90 g of butyl acrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) were used. The content of polymer graft chains was 19.2% by mass. The glass transition temperature was -10°C, the number average molecular weight was 62,000, and the graft density was 0.14 chains / nm 2 The film thickness was 12 nm.
[0083] Examples 6 to 10, Comparative Example 4 Polyurethane foams were prepared in the same manner as in Example 1, except that the formulation was changed to that shown in Table 2, and the foam moldability and vibration damping properties were evaluated. Examples 6 and 7 and Comparative Example 4 were also evaluated for sound insulation and sound absorption. The results are shown in Table 2. Details of each component shown in Table 2 are the same as those in Table 1, except as follows. Millionate MR200: Polymethylene polyphenylene polyisocyanate, isocyanate group content: 31% by mass (manufactured by Tosoh Corporation) Emulgen LS106: Polyoxyalkylene alkyl ether (Kao Corporation) HFO-1233zd(E): 1-chloro-3,3,3-trifluoropropene (Honeywell) DEG-DBE: Diethylene glycol dibutyl ether (Tokyo Chemical Industry Co., Ltd.)
[0084] <Sound insulation> A cylindrical test piece with a diameter of 41.8 mm and a thickness of 10 mm was cut out from the core of the freeform. For this test piece, normal incidence sound transmission loss was measured based on the transfer matrix method in accordance with ASTM E2611 using an acoustic material property measurement system (WinZac) manufactured by Nihon Acoustic Engineering Co., Ltd. Measurements were performed at room temperature (25°C) and measurement frequencies of 200 Hz to 5000 Hz, and data was obtained from 1 / 3 octave band analysis. Sound insulation can be determined to have improved when the transmission loss value improves by 1 dB or more. The results are shown in Table 2.
[0085] <Sound absorption> Cylindrical test specimens with a diameter of 41.8 mm and a thickness of 10 mm were cut from the core of the freeform. The normal incidence sound absorption coefficient of this test piece was measured in accordance with ASTM E1050 and JIS A1405 using an acoustic material property measurement system (WinZac) manufactured by Nihon Acoustic Engineering Co., Ltd. Measurements were performed at room temperature (25°C) and at measurement frequencies of 200Hz to 5000Hz, and data was obtained from 1 / 3 octave band analysis. An improvement in the sound absorption coefficient value of 0.01 or more can be considered to indicate improved sound absorption. The results are shown in Table 2.
[0086] [Table 2]
[0087] As shown in Table 2, Examples 6 to 10, which contained the specified composite particles, exhibited significantly improved vibration damping while maintaining foam moldability. Furthermore, as shown in Examples 6 and 7, it can be seen that the sound insulation and sound absorption properties were also superior to those of Comparative Example 4, which contained hydrophobic silica. Note that, for Comparative Example 4, the tan δ of the peak top was broad, so the temperature of the tan δ of the peak top could not be specified. [Industrial Applicability]
[0088] The thermosetting resin foam of the present invention can be suitably used in products such as audio equipment, electrical products, buildings, industrial equipment, automobile parts, motorcycle parts, and containers.
Claims
1. A thermosetting resin foam comprising composite particles having polymer graft chains attached to the particle surface.
2. 2. The thermosetting resin foam according to claim 1, wherein at least one of the polymer graft chains has a glass transition temperature of −30° C. or higher and 80° C. or lower.
3. The graft density of the polymer graft chains is 0.001 chains / nm 2 More than 5 chains / nm 2 3. The thermosetting resin foam according to claim 1, wherein:
4. The thermosetting resin foam according to any one of claims 1 to 3, wherein the content of the composite particles is 1% by mass or more and 70% by mass or less.
5. The thermosetting resin foam according to any one of claims 1 to 4, having an expansion ratio of 1.1 times or more.
6. The thermosetting resin foam according to any one of claims 1 to 5, which is a polyurethane foam.
7. A method for producing a thermosetting resin foam, comprising a step of foaming a thermosetting resin foam composition comprising composite particles having polymer graft chains bonded to the particle surface.
8. The method for producing a thermosetting resin foam according to claim 7, further comprising the step of preparing a polyol mixture containing composite particles having polymer graft chains bonded to the particle surface and a polyol component.
9. 9. The method for producing a thermosetting resin foam according to claim 8, wherein the step of preparing the polyol mixture comprises dispersing composite particles having polymer graft chains bonded to the particle surface in one or more solvents selected from toluene, ethyl acetate, propyl acetate, methanol, isopropyl alcohol, and propylene glycol monomethyl ether, and then replacing the solvent with a polyol.
10. A vibration-damping material comprising the thermosetting resin foam according to any one of claims 1 to 6.
11. A method for improving vibration damping properties by incorporating composite particles having polymer graft chains bonded to the particle surface into a thermosetting resin foam.
12. 7. A composite particle for use in a thermosetting resin foam according to claim 1, which has polymer graft chains bonded to the particle surface.
13. 7. A polyol mixture for polyurethane foams, comprising composite particles having polymer graft chains bonded to the particle surfaces and a polyol component, for use in the polyurethane foam according to claim 6.
14. A dispersion for use in the thermosetting resin foam according to any one of claims 1 to 6, comprising composite particles having polymer graft chains bonded to their particle surfaces and a dispersion medium.
Citation Information
Patent Citations
Highhdensity polyurethane foams having flmae resistant* soundproof and damping properties
JP1977054797A
Polyurethane foam and method for producing polyurethane foam
JP2020084173A
Thermoplastic resin composition
JP2020196877A