Fluorine-containing compound
A fluorine-containing compound with controlled polymerization addresses the limitations of fluororesins by providing superior electrical properties and thermal stability, enabling high-frequency substrate production with reduced thermal expansion and enhanced crosslinking, thus supporting next-generation communication needs.
Patent Information
- Application Number
- JP2023221746
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2023-12-27
- Publication Date
- 2024-11-08
AI Technical Summary
Existing fluororesins face challenges in supporting next-generation high frequencies exceeding 5 GHz due to insufficient electrical properties, dimensional instability, and manufacturing limitations, particularly in terms of crosslinking properties and thermal expansion.
A fluorine-containing compound with a specific structure and low degree of polymerization (n=1 to 4) is developed, offering excellent electrical properties, low thermal expansion, and high crosslinking density, enabling reliable prepreg molding for high-frequency substrates.
The fluorine-containing compound achieves low dielectric constant and loss tangent, high solvent solubility, and stable thermal expansion, facilitating the production of substrates that can handle frequencies up to 28 GHz with improved durability and manufacturing efficiency.
Smart Images

Figure 2024159458000001 
Figure 2024159458000002 
Figure 2024159458000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a fluorine-containing compound, and more particularly to a fluorine-containing compound that can be suitably used for next-generation high-frequency substrates. [Background technology]
[0002] In recent years, development has been progressing towards next-generation radio frequency technologies that will enable high-speed, large-capacity transmission in the field of information and communications devices such as smartphones and tablet terminals. To accommodate this, the circuit board materials used are also being required to have low dielectric constants and low dielectric tangents that can reduce transmission losses. Conventionally, materials such as epoxy resins and polyphenylene ether resins have been used as resin materials for high-speed communication and transmission (Patent Document 1). However, it is difficult for epoxy resins and polyphenylene ether resins to meet the recent high-speed and large-capacity transmission requirements.
[0003] On the other hand, fluororesins are known as materials with excellent electrical properties. In particular, perfluororesins, in which all hydrogen in the molecular chain is replaced by fluorine, are known to exhibit particularly excellent electrical properties (low dielectric constant and low dielectric loss). However, fluororesins (perfluororesins) have problems such as being prone to deformation due to stress and having a large thermal expansion coefficient, making them difficult to use as substrate materials.
[0004] It has been proposed to use fluorinated poly(arylene ether) and crosslinkable fluorinated poly(arylene ether) as dielectric materials in electronic components (Patent Documents 2 and 3). However, the electrical properties of these materials do not satisfy the current requirements for high-speed communication and transmission. In addition, from the viewpoint of mass production and reducing manufacturing costs, it is required to lower the crosslinking temperature so that they can be manufactured using existing substrate manufacturing equipment.
[0005] To solve these problems, the present inventors have proposed a fluororesin as shown in Patent Document 4. The fluororesin described in Patent Document 4 is a resin material that has excellent electrical properties (low dielectric constant and low dielectric loss) as a substrate material for high-speed communication and transmission, high solvent solubility for facilitating thin film formation, and excellent crosslinkability that enables film formation by heating at about 200°C. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2017-128718 A [Patent Document 2] U.S. Pat. No. 5,115,082 [Patent Document 3] U.S. Pat. No. 5,179,188 [Patent Document 4] Patent Publication No. 2022-89150 Summary of the Invention [Problem to be solved by the invention]
[0007] However, although the fluororesin specifically disclosed in Patent Document 4 above is satisfactory in terms of electrical properties at 1 GHz, it is unclear whether it has the electrical properties and dimensional stability (coefficient of thermal expansion) required for producing a substrate compatible with next-generation high-frequency waves exceeding 5 GHz, or whether it is possible to reliably mold the prepreg used for producing the substrate. The present inventors have discovered that a fluorine-containing compound with a low degree of polymerization, which was not focused on in Patent Document 4, has better dimensional stability (coefficient of thermal expansion) and crosslinkability than the fluororesins specifically disclosed in Patent Document 4, and can be reliably molded into prepregs for producing substrates compatible with next-generation high frequency waves exceeding 5 GHz.
[0008] Therefore, an object of the present invention is to provide a fluorine-containing compound that has excellent electrical properties required for next-generation high-frequency waves, and in addition, has a significantly reduced thermal expansion coefficient (thermal expansion coefficient) and can be used to fabricate a substrate having excellent thermosetting properties. [Means for solving the problem]
[0009] According to the present invention, there is provided a fluorine-containing compound having a structure represented by the following formula (I):
[0010] [ka] In the formula, L is a structure represented by the following formula (II) or (III):
[0011] [ka]
[0012] R 1 and R 2 are each independently a hydrogen atom, C1 to C 10 Alkyl groups, C1-C 10 Haloalkyl groups, C6-C 10 or R 1 and R 2 are groups which together form a ring structure which may have a substituent, R 3 and R 4 each independently represents a hydrogen atom, a fluorine atom, or a C1-C6 in which some or all of the hydrogen atoms may be substituted with halogen 10 and C6-C in which some or all of the hydrogen may be substituted with halogen. 10 is a group selected from the group consisting of aryl groups n is in the range of 1 to 4; X is a group containing an olefinic carbon-carbon double or triple bond.
[0013] According to the fluorine compound of the present invention, (1) The thermal expansion coefficient of the cured product at 240 to 290°C is 200 ppm / °C or less. To do so, (2) the n is 1; (3) said X contains at least one fluorine atom; (4) The above L is a cyclopentylidene group which may have a substituent, A cyclohexylidene group and a cyclododecylidene group which may have a substituent. being selected from the group consisting of (5) The gel fraction of the cured product is 50% or more. is preferred.
[0014] The present invention also provides a fluorine-containing composition comprising the above fluorine-containing compound and a crosslinking agent. The present invention further provides a prepreg comprising the fluorine-containing compound or the fluorine-containing composition and a fibrous base material. The present invention still further provides a copper-clad laminate comprising the cured product of the prepreg and at least one copper layer. According to the present invention, there is provided a printed circuit board comprising a cured product of the prepreg and a conductor pattern formed on the surface thereof. Effect of the Invention
[0015] The fluorine-containing compound of the present invention not only has excellent electrical properties (low dielectric constant and low dielectric loss), sufficient heat resistance, an appropriate glass transition temperature (Tg), and sufficient solvent solubility, but also exhibits a very low thermal expansion coefficient of 200 ppm / °C or less at 240°C or higher of the cured product cured under conditions of 200°C for 120 minutes, due to the value of n being in the range of 1 to 4, particularly when the value of n is 1, and is therefore capable of exhibiting extremely high dimensional stability. It also has excellent thermosetting properties (crosslinkability), and the gel fraction of the cured product is very high, at 50% or more. Such unexpected and unique effects of the present invention are also evident from the results of the Examples described below. That is, in the case of a fluororesin in which the value of n in the formula (I) is 30 (Comparative Example 1), the thermal expansion coefficient measured under the above conditions was 274 ppm / °C, whereas in the case of a fluorine-containing compound (Example 1) having the same structure as the above fluororesin except that the value of n is 1, the thermal expansion coefficient of the cured product measured under the above conditions was 128 ppm / °C, which is an unexpected and significantly low value for a fluororesin in which the value of n is 30. Similarly, in the case of the fluororesin of Comparative Example 1, in which the value of n is 30, the gel fraction of the cured product cured under the above conditions was 16%, whereas in the case of the fluorine-containing compound of Example 1, in which the value of n is 1, the gel fraction of the cured product cured under the above conditions was 100%. In this respect as well, it is clear that an unexpected, remarkably high, ideal value was obtained from the fluororesin in which the value of n is 30.
[0016] Furthermore, molding of prepregs using thermosetting resins requires impregnation into glass fibers and curing to a semi-cured state. The fluorine-containing compound of the present invention can be easily composited with glass fibers, and prepregs for producing circuit boards compatible with next-generation high-frequency waves exceeding 5 GHz can be efficiently molded. That is, as is clear from the results of the gel fraction (crosslink density) above, the fluorine-containing compound of the present invention has excellent curability, so that even when a pressing pressure is applied or a vacuum is applied while the fluorine-containing compound is impregnated into glass fibers, it does not protrude from the glass fibers and can be reliably composited with the glass fibers (Examples 1 to 5), but when the fluorine resin of Comparative Example 1 in which the value of n is 30 was used in the same method, it was difficult to uniformly composite with the glass fibers. In this respect, it is clear that the fluorine resin in which the value of n is 30 in the present invention provides an unexpected effect. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] (Fluorine-containing compounds) An important feature of the fluorine-containing compound of the present invention is that in the formula (I), n is in the range of 1 to 4, and preferably 1. As a result, as described above, the fluorine-containing compound represented by the formula (I) has sufficient heat resistance, an appropriate glass transition temperature (Tg), and sufficient solvent solubility, and also has the unexpected effects of having a reduced thermal expansion coefficient, a high gel fraction, and ease of composite formation with glass fibers, compared to when n is greater than 4, and can achieve excellent electrical properties (low dielectric constant and low dielectric loss) even at a high frequency of 28 GHz.
[0018] In the formula (I), n represents an average degree of polymerization. The average degree of polymerization can be predicted from the stoichiometric ratio of monomers, and can also be measured by a conventionally known method such as nuclear magnetic resonance spectroscopy. In the present invention, "n is 1" means that the average degree of polymerization of the compound is 0.5 to 1.4.
[0019] In the fluorine-containing compound of the present invention represented by the formula (I), R 1 and R 2 are each independently a hydrogen atom, C1 to C 10 Alkyl groups, C1-C 10 Haloalkyl groups, C6-C 10 The aryl group may be selected from the group consisting of C1 to C 10 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a 2-methylpropyl group (isobutyl group), a butyl group, and a pentyl group. 10 Examples of haloalkyl groups include trifluoromethyl, pentafluoroethyl, and perfluoropropyl groups. 10 Examples of the aryl group include a phenyl group and a naphthyl group (including 1-isomers and 2-isomers).
[0020] Alternatively, R 1 and R 2may be a group that, together with each other, forms a ring structure that may have a substituent. Examples of the group that forms a ring structure include a tetramethylene group (forming a cyclopentane ring), a pentamethylene group (forming a cyclohexane ring), an undecamethylene group (forming a cyclododecane ring), a 2-methyl-pentamethylene group (forming a methylcyclohexane ring), a 2,2,4-trimethyl-pentamethylene group (forming a trimethylcyclohexane ring), and a biphenyl-2,2'-diyl group (forming a fluorene ring).
[0021] In the formula (I), R 3 and R 4 each independently represents a hydrogen atom, a fluorine atom, or a C1-C6 in which some or all of the hydrogen atoms may be substituted with halogen 10 or a C6-C saturated or unsaturated hydrocarbon group in which some or all of the hydrogen may be substituted with halogen. 10 An aryl group having a structure of C1 to C6 in which some or all of the hydrogen atoms may be substituted with halogen. 10 Examples of the saturated or unsaturated hydrocarbon group include a methyl group, an ethyl group, a propyl group, a 2-methylpropyl group (isobutyl group), a butyl group, a pentyl group, a trifluoromethyl group, a pentafluoroethyl group, a perfluoropropyl group, a vinyl group, an allyl group, a 1-methylvinyl group, a 2-butenyl group, a 3-butenyl group, and the like. 10 Examples of aryl groups include phenyl groups, naphthyl groups (including 1-isomers and 2-isomers), perfluorophenyl groups, and the like.
[0022] In the formula (I), X is a group containing an olefinic carbon-carbon double bond or a carbon-carbon triple bond, and is preferably a group containing at least one fluorine atom. Examples of X include the following structures (X-1) to (X-10).
[0023] [ka]
[0024] In the formula, p is an integer from 0 to 4, and in some embodiments, p is 4. In other embodiments, p is 0. R is a C1-C 10 Alkyl groups of C6 to C 10 R' represents a hydrogen atom or a C1-C 10 represents an alkyl group represented by the formula:
[0025] Preferably, X has any of the following structures (X-11) to (X-15).
[0026] [ka]
[0027] In the present invention, preferred fluorine-containing compounds include, for example, resins having the following structure (wherein "n" is a value of 1 to 4, and "(*)" indicates the bonding position).
[0028] [ka]
[0029] [ka]
[0030] [ka]
[0031] In the present invention, the fluorine-containing compound is preferably soluble in a solvent. The term "soluble in a solvent" means that 1 g or more, preferably 10 g or more of the fluorine-containing compound is dissolved in 100 g of a solution obtained from a given solvent. The fluorine-containing compound of the present embodiment is preferably soluble in a hydrocarbon to be described later. In addition, the fluorine-containing compound of the present embodiment is particularly preferably soluble in toluene from the viewpoint of cost.
[0032] As described above, the cured product obtained by crosslinking the fluorine-containing compound of the present invention preferably has a gel fraction (crosslink density) of 50% or more, more preferably 80% or more, even more preferably 90% or more, and most preferably 100%. A high gel fraction (crosslink density) is believed to have the effect of suppressing a decrease in durability due to the presence of unreacted crosslinked sites, and reducing the thermal expansion coefficient by increasing the crosslink density. In this specification, the gel fraction (crosslink density) of the cured product is a value measured for a cured product obtained by thermally curing a fluorine-containing compound under the curing conditions of 200° C. for 120 minutes. The method for measuring the gel fraction will be described later.
[0033] The cured product obtained by crosslinking the fluorine-containing compound of the present invention preferably has a glass transition temperature of 200°C or higher. Furthermore, the thermal expansion coefficient in a temperature environment exceeding the glass transition temperature is preferably less than 200 ppm / °C, more preferably less than 180 ppm / °C, and even more preferably less than 150 ppm / °C. By having a glass transition temperature of 200°C or higher, the thermal expansion coefficient (thermal expansion coefficient) in a normal use environment is reduced, and durability is improved when used as an electronic substrate. In addition, the small thermal expansion coefficient (thermal expansion coefficient) at high temperatures has the advantage of being easy to use in high-temperature environments and easy to solder. In this specification, the glass transition temperature and thermal expansion coefficient of the cured product are values measured for a cured product obtained by thermally curing a fluorine-containing compound under the curing conditions of 200°C for 120 minutes. The method for measuring the glass transition temperature and thermal expansion coefficient will be described later.
[0034] (Preparation of Fluorine-Containing Compounds) The fluorine-containing compound of the present invention can be produced by mixing a bisphenol derivative (A), a perfluorobiphenyl (B), and a precursor of a substituent X (C) simultaneously or at a timing that does not cause a condensation reaction of the bisphenol derivative (A) and the perfluorobiphenyl (B) in the presence of a base, as shown in the following reaction formula, and then heating and mixing.
[0035] [ka]
[0036] Z in the precursor (C) in the above reaction scheme is a leaving group, preferably selected from the group consisting of F, Cl, Br, and I, and more preferably F.
[0037] The base used preferably includes an alkali metal carbonate, hydrogen carbonate, and hydroxide. Preferred examples of the base include sodium carbonate, potassium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, sodium hydroxide, and potassium hydroxide. It is preferable to use a base having a normality of 2 or more, preferably 4 to 6, per mole of the bisphenol derivative (A).
[0038] The above-mentioned heating and mixing is preferably carried out in an aprotic polar solvent or a mixed solvent containing an aprotic polar solvent. Preferred aprotic polar solvents include N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), sulfolane, and the like. The mixed solvent may contain a low-polarity solvent as long as it does not reduce the solubility of the fluorine-containing compound and does not affect the reaction. Examples of low-polarity solvents that can be used include toluene, xylene, benzene, tetrahydrofuran, benzotrifluoride ((trifluoromethyl)benzene), xylenehexafluoride (1,3-bis(trifluoromethyl)benzene), and the like. The polarity (dielectric constant) of the solvent mixture can be changed by adding a low-polarity solvent, thereby controlling the reaction rate.
[0039] The above-mentioned heated mixing is preferably carried out under conditions of a reaction temperature of 10 to 200°C and a reaction time of 1 to 80 hours, preferably a reaction temperature of 20 to 180°C and a reaction time of 2 to 60 hours, and more preferably a reaction temperature of 50 to 160°C and a reaction time of 3 to 40 hours.
[0040] (Fluorine-containing composition) The second embodiment of the present invention relates to a fluorine-containing composition containing the fluorine-containing compound of the first embodiment and a crosslinking agent. The fluorine-containing compound of the present invention has excellent crosslinking properties by itself, and therefore can exhibit excellent curing properties even without the crosslinking agent. However, by containing a crosslinking agent, it is possible to obtain even more excellent curing properties and impart sufficient hardness to a cured product made of the fluorine-containing composition.
[0041] The crosslinking agent used in this embodiment includes a compound having two or more olefinic carbon-carbon double bonds in the molecule. Examples of the crosslinking agent used in this embodiment include a multifunctional methacrylate compound having two or more methacrylic groups in the molecule, a multifunctional acrylate compound having two or more acrylic groups in the molecule, a trialkenyl isocyanurate compound such as triallyl isocyanurate (TAIC), divinylbenzene, etc. Examples of the multifunctional acrylate / methacrylate compound include a dicyclopentadiene type acrylate compound such as tricyclodecane dimethanol diacrylate, and a dicyclopentadiene type methacrylate compound such as tricyclodecane dimethanol dimethacrylate.
[0042] The fluorine-containing composition of the present embodiment may contain a crosslinking agent. In addition, in the fluorine-containing composition of the present embodiment, the mass ratio of the fluorine-containing compound to the crosslinking agent is preferably within the range of 9.5:0.5 to 5:5, more preferably 7.5:2.5 to 5.5:4.5. By using a mass ratio within this range, the cured product of the fluorine-containing composition can be given sufficient hardness.
[0043] The fluorine-containing composition of the present embodiment may further include a solvent, a reaction initiator, and / or a filler. The fluorine-containing composition of the present embodiment may further include any additive known in the art, such as a defoamer, a heat stabilizer, an antistatic agent, an ultraviolet absorber, a colorant (dye or pigment), a flame retardant, a lubricant, a dispersant, etc.
[0044] The fluorine-containing composition of the present embodiment may be a varnish-like composition containing a solvent. In the present embodiment, various solvents can be used. From the viewpoint of solvent solubility, it is preferable to use an aprotic solvent in the present invention. The solvents used in this embodiment include: hydrocarbons such as benzene, toluene, xylene, heptane, cyclohexane, methylcyclohexane, and mineral spirits; ketones such as acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), and diisobutyl ketone (DIBK); cyclic ketones such as cyclohexanone, cycloheptanone, and cyclooctanone; esters such as ethyl acetate, butyl acetate, and γ-butyrolactone; cyclic ethers such as tetrahydrofuran (THF), and 1,3-dioxolane; amides such as N,N-dimethylformamide (DMF), diethylformamide (DEF), N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), and N-cyclohexylpyrrolidone; sulfones such as sulfolane and dimethylsulfone; and sulfoxides such as dimethylsulfoxide (DMSO). In the present invention, preferred solvents are hydrocarbons, and aromatic hydrocarbons are particularly preferred.
[0045] The fluorine-containing composition of the present embodiment preferably contains a reaction initiator for the crosslinking reaction. Although crosslinking and curing by heating are possible even in the absence of a reaction initiator, the presence of a reaction initiator allows for more efficient crosslinking and curing under milder conditions. Examples of reaction initiators that can be used include benzoyl peroxide, di-t-butyl peroxide, t-butyl hydroperoxide, dicumyl peroxide, cumyl hydroperoxide, α,α'-di(t-butylperoxy)-diisopropylbenzene (Perbutyl® P, manufactured by NOF Corp.), bis(1-methyl-1-phenylethyl)peroxide (Percumyl® D, manufactured by NOF Corp.), t-butyl α,α-dimethylbenzyl peroxide (Perbutyl® C, manufactured by NOF Corp.), 2,5-dimethyl-2,5-di(t-butylperoxy)-3-hexyne, 3,3',5,5'-tetramethyl-1,4-diphenoquinone, chloranil, 2,4,6-tri-t-butylphenoxyl, t-butylperoxyisopropyl monocarbonate, azobisisobutyronitrile, and the like.
[0046] The fluorine-containing composition of the present embodiment may further include one or more fillers. The filler may be an organic filler or an inorganic filler. Usable organic fillers include engineering plastics such as polyphenylene sulfide, polyether ether ketone (PEEK), polyamide, polyimide, and polyamideimide; and solvent-insoluble fluororesins such as polytetrafluoroethylene (PTFE), perfluoroalkoxyalkane (PFA), and copolymers of tetrafluoroethylene and hexafluoropropylene (FEP). Usable inorganic fillers include metals; metal oxides such as aluminum oxide, zinc oxide, tin oxide, and titanium oxide; metal hydroxides; metal titanates; zinc borate; zinc stannate; boehmite; silica; glass; silicon oxide; silicon carbide; boron nitride; calcium fluoride; carbon black; mica; talc; barium sulfate; and molybdenum disulfide. Solvent-insoluble fluororesins are preferred in terms of improving the electrical properties (dielectric constant, dielectric loss, etc.) of the cured product of the fluorine-containing composition. Silica is also preferred in that it can reduce the coefficient of thermal expansion without impairing the electrical properties (dielectric constant, dielectric loss, etc.) of the cured product of the fluorine-containing composition.
[0047] The fluorine-containing composition of this embodiment can be formed by mixing the fluorine-containing compound of the first embodiment, a crosslinking agent, and optional components. Heating may be performed during mixing. Mixing can be performed using any mixing device known in the art, such as various stirrers, ball mills, bead mills, planetary mixers, and roll mills.
[0048] (Prepreg) The third embodiment of the present invention relates to a prepreg comprising the semi-cured product of the fluorine-containing compound described in the first embodiment and a fibrous substrate. The prepreg of this embodiment may further comprise a reaction initiator for a crosslinking reaction. The reaction initiator that can be used in this embodiment is the same as that in the second embodiment.
[0049] The fibrous substrate that can be used in the present embodiment includes glass woven fabric, aramid woven fabric, polyester woven fabric, carbon fiber woven fabric, glass nonwoven fabric, aramid nonwoven fabric, polyester nonwoven fabric, carbon fiber nonwoven fabric, pulp paper, linter paper, etc. A preferred fibrous substrate is glass woven fabric, which can realize excellent mechanical strength. The fibrous substrate preferably has a thickness of 0.01 mm to 0.3 mm.
[0050] The prepreg of this embodiment can be formed by impregnating a fibrous substrate with the fluorine-containing compound and optional reaction initiator described in the first embodiment and drying. Here, the fluorine-containing compound to be impregnated is desirably in a varnish state containing a solvent. The solvent that can be used is the same as that in the second embodiment. As a result of the drying treatment, the solvent in the varnish is at least partially removed, and the fluorine-containing compound is in a semi-cured state (so-called "B stage"). The impregnation step can be carried out by any method known in the art, such as immersion or coating. The content of the fluorine-containing compound in the prepreg can be adjusted by carrying out the impregnation of the fluorine-containing compound and the optional reaction initiator multiple times. The conditions (temperature and time) of the drying step depend on the type of fluorine-containing compound and the type of the optional reaction initiator and / or solvent. For example, the drying step can be carried out by heating to a temperature of 80°C to 170°C for 1 to 60 minutes.
[0051] The fourth embodiment of the present invention relates to a prepreg including a semi-cured product of the fluorine-containing composition described in the second embodiment and a fibrous base material. The fibrous base material that can be used in this embodiment is the same as that in the third embodiment.
[0052] The prepreg of this embodiment can be formed by impregnating a fibrous substrate with the fluorine-containing composition of the second embodiment and drying it. Here, the fluorine-containing composition to be impregnated is desirably in a varnish state containing a solvent. As a result of the drying treatment, the solvent in the varnish is at least partially removed, and the fluorine-containing composition is in a semi-cured state (so-called "B stage"). The impregnation step can be carried out by any method known in the art, such as immersion or coating. By carrying out the impregnation of the fluorine-containing composition multiple times, the content of the fluorine-containing compound in the prepreg can be adjusted. The conditions (temperature and time) of the drying step depend on the type of the fluorine-containing compound, crosslinking agent, and optional solvent contained in the fluorine-containing composition. For example, the drying step can be carried out by heating to a temperature of 80°C to 170°C for 1 to 60 minutes.
[0053] (Copper-clad laminate) A fifth embodiment of the present invention relates to a copper-clad laminate comprising a cured product of the prepreg according to the third or fourth embodiment and at least one copper layer.
[0054] The copper-clad laminate of this embodiment can be formed by laminating one or more prepregs, laminating copper foil on one or both surfaces of the prepregs, and integrating the resulting laminate by heating and pressing. The fluorine-containing compound or composition in the copper-clad laminate is preferably in a state where curing is completed (so-called "C stage"). The conditions of the heating and pressing can be appropriately set based on the thickness of the copper-clad laminate to be produced, the composition of the fluorine-containing compound or composition in the prepreg, and the like. For example, a copper-clad laminate can be produced by heating to a temperature of 170°C to 220°C for 60 to 150 minutes and applying a pressure of 1.0 MPa to 10 MPa.
[0055] (printed circuit board) A sixth embodiment of the present invention relates to a printed circuit board including a cured product of the prepreg according to the third or fourth embodiment and a conductor pattern formed on the surface of the cured product.
[0056] The printed circuit board of this embodiment can be manufactured by etching the copper layer of the copper-clad laminate of the fifth embodiment to form a conductor pattern. Alternatively, the printed circuit board can be manufactured by a method in which one or more prepregs are laminated and heated and pressed to form a laminate, and a conductive material is laminated in a pattern on the surface of the laminate to form a conductor pattern. EXAMPLES
[0057] Example 1 (Synthesis of fluorine-containing compound, n=1) A glass reaction vessel was charged with 0.805 g (3.0 mmol) of 1,1-bis(4-hydroxyphenyl)cyclohexane (bisphenol Z), 0.501 g (1.5 mmol) of decafluorobiphenyl, and 0.912 g (6.6 mmol) of potassium carbonate. The inside of the glass reaction vessel was evacuated to vacuum, and then substituted with nitrogen. Then, 10 mL of DMAc and 0.582 g (3.0 mmol) of 2,3,4,5,6-pentafluorostyrene were added to the glass reaction vessel. The reaction mixture was shielded from light, heated to 80° C. with stirring, and stirred for 15 hours. After the heating, the reaction mixture was cooled to room temperature. Then, the reaction mixture was poured into 0.5 L of pure water. The reaction mixture was suction filtered, and the obtained solid was washed with pure water and methanol. The washed solid was dried under reduced pressure to obtain 1.54 g of a fluorine-containing compound. The average degree of polymerization calculated from the nuclear magnetic resonance spectrum (X-Plus, Oxford Instruments) was 1.0.
[0058] Example 2 (Synthesis of fluorine-containing compound, n=2) The procedure of Example 1 was repeated, except that 0.805 g (3.0 mmol) of bisphenol Z was used, 0.668 g (2.0 mmol) of decafluorobiphenyl, and 0.388 g (2.0 mmol) of 2,3,4,5,6-pentafluorostyrene were used, to give 1.50 g of fluorine-containing compound. The average degree of polymerization calculated from nuclear magnetic resonance spectroscopy was 1.9.
[0059] (Example 3) (Synthesis of fluorine-containing compounds, n=3) The procedure of Example 1 was repeated, except that 0.805 g (3.0 mmol) of bisphenol Z was used, 0.752 g (2.3 mmol) of decafluorobiphenyl, and 0.291 g (1.5 mmol) of 2,3,4,5,6-pentafluorostyrene were used, to give 1.61 g of fluorine-containing compound. The average degree of polymerization calculated from nuclear magnetic resonance spectroscopy was 2.8.
[0060] (Example 4) (Synthesis of fluorine-containing compounds, n=4) The procedure of Example 1 was repeated, except that 0.805 g (3.0 mmol) of bisphenol Z was used, 0.802 g (2.4 mmol) of decafluorobiphenyl, and 0.233 g (1.2 mmol) of 2,3,4,5,6-pentafluorostyrene were used, to give 1.58 g of fluorine-containing compound. The average degree of polymerization calculated from nuclear magnetic resonance spectroscopy was 3.5.
[0061] (Example 5) (Synthesis of fluorine-containing compound, n=1) The procedure of Example 1 was repeated, except that 0.889 g (3.0 mmol) of 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane was used instead of 0.805 g (3.0 mmol) of 1,1-bis(4-hydroxyphenyl)cyclohexane (bisphenol Z), to give 1.68 g of a fluorine-containing compound. The average degree of polymerization calculated from nuclear magnetic resonance spectroscopy was 1.0.
[0062] (Comparative Example 1) (Synthesis of fluororesin, n=30) A fluororesin was obtained according to the method described in Patent Document 4 (JP 2022-89150 A). That is, 0.805 g (3.0 mmol) of 1,1-bis(4-hydroxyphenyl)cyclohexane (bisphenol Z) and 0.912 g (6.6 mmol) of potassium carbonate were charged into a glass reaction vessel. The inside of the glass reaction vessel was evacuated to vacuum and then replaced with nitrogen. Then, 10 mL of DMAc was added into the glass reaction vessel. The reaction mixture was heated to 150° C. with stirring and stirred for 3 hours. After heating, the reaction mixture was cooled to room temperature. Then, 0.802 g (2.4 mmol) of decafluorobiphenyl was added to the reaction mixture. The reaction mixture was heated to 70° C. with stirring and stirred for 4 hours. Then, the reaction mixture was shielded from light and 0.17 mL (0.233 g, 1.2 mmol) of 2,3,4,5,6-pentafluorostyrene was added. Stirring was continued for 15 hours at a temperature of 70° C. After stirring was completed, the reaction mixture was cooled to room temperature. The reaction mixture was then poured into 0.5 L of pure water. The reaction mixture was filtered under suction, and the solid matter obtained was washed with pure water and methanol. The washed solid matter was dried under reduced pressure to obtain 1.14 g of a fluororesin. The average degree of polymerization was determined to be 30 by nuclear magnetic resonance spectroscopy.
[0063] (Reference example) Polyphenylene ether (PPE) resin As a control for demonstrating the performance of the fluorine-containing compound of the present invention, various measurements were also carried out on a polyphenylene ether (PPE) resin (NORYL SA9000 manufactured by SABIC), which is currently commonly used as a substrate material for high-frequency transmission.
[0064] (Evaluation 1: Evaluation of solvent solubility and thermosetting property (gel fraction)) 0.5 g of each of the fluorine-containing compounds obtained in Examples 1 to 5, the fluororesin obtained in Comparative Example 1, and the PPE resin of the Reference Example was weighed out, added with toluene, heated to 80°C, and mixed. If a 50% by mass solution was obtained, it was determined to be toluene-soluble. All of the resulting solution was placed in an aluminum cup and dried at 200°C for 2 hours using a thermostatic oven (SPHH-102, manufactured by Espec Corporation) to obtain a thermoset product. This thermoset product was removed from the aluminum cup and its weight was measured. 5 g of methyl ethyl ketone (MEK) and the cured product were placed in a 9 mL sample tube, and the cured product was immersed in MEK for 24 hours. The solvent was then volatilized, and the thermoset product was washed with MEK and dried. The mass after drying was measured, and the mass of the dried cured product after immersion in MEK was calculated. The gel fraction was calculated as follows: (mass of the dried and cured product after immersion in MEK) / (mass of the cured product before immersion in MEK)×100 (%). The results are shown in Table 1.
[0065] [Table 1]
[0066] As is clear from Table 1, the fluorine-containing compound of the present invention has a significantly larger gel fraction than the fluororesin of Comparative Example 1, and can be said to have curing properties equal to or superior to those of PPE resin.
[0067] (Rating 2: Coefficient of thermal expansion (CTE)) The fluorine-containing compound obtained in Example 1, the fluororesin obtained in Comparative Example 1, and the PPE resin of Reference Example were dissolved in toluene in the same manner as above to obtain 50% by mass solutions. The entire solution obtained was placed in an aluminum cup and heated in a thermostatic oven (SPHH-102, manufactured by Espec Corporation) at 150°C for 1 hour to remove the solvent, and then heated at 200°C for 2 hours to obtain a cured product. The cured product was then cooled to room temperature, and the peeled off product was used as a test specimen. The thermal expansion coefficient of this test piece was measured using a dynamic viscoelasticity measuring device (DMA ARES-G2, manufactured by TA Instruments). The thermal expansion coefficients from 240° C. to 290° C. are shown in Table 2.
[0068] [Table 2]
[0069] As can be seen from Table 2, the fluorine-containing compound of the present invention has a significantly smaller thermal expansion coefficient value than the comparative examples and reference examples, and has the unique feature of being less likely to expand even in the high temperature range of 240°C to 290°C, which is above the glass transition temperature.
[0070] (Evaluation 3: Electrical characteristics) [Preparation of varnish-like composition] The fluorine-containing compounds obtained in Examples 1 to 5, the fluorine resin obtained in Comparative Example 1, and the PPE resin of the Reference Example were dissolved in toluene in the same manner as above to obtain a 50% by mass solution. Furthermore, Perbutyl (registered trademark) P (manufactured by NOF Corporation) was added as a reaction initiator to give a concentration of 2% by mass relative to the fluorine-containing compounds to obtain a varnish-like composition. [Preparation of prepreg] Each varnish-like composition obtained by the above method was dropped onto a 7 cm x 7 cm glass cloth piece (L2-1078, manufactured by Asahi Kasei Corporation) to allow it to be uniformly impregnated. The impregnated material was then dried at 110°C for 10 minutes to obtain a prepreg. [Preparation of copper-clad laminate] The prepreg obtained by the above method was cut to a size of 5 cm x 5 cm, and together with electrolytic copper foil (thickness 18 μm) (Furukawa Electric Co., Ltd., HVLP), it was heated to 200°C while reducing the pressure in a vacuum hot press machine (Imoto Machinery Works, Ltd., Manual Hydraulic Vacuum Heating Press IMC-4900), and further pressed at 200°C for 120 minutes at 4 MPa to bond the prepreg and copper foil. Uniformly composited copper-clad laminates were obtained from the prepregs using the fluorine-containing compounds obtained in Examples 1 to 5. However, when the fluororesin obtained in Comparative Example 1 was used, it was not possible to uniformly composite it with the glass cloth, and a beautiful copper-clad laminate was not obtained.
[0071] The copper foil of the copper-clad laminate made from the prepreg was peeled off with tweezers and cut into 4 cm x 4 cm test pieces. The electrical properties (dielectric constant and dielectric tangent) of the test pieces were measured using a vector network analyzer (KEYSIGHT 5247B) under the conditions of 28 GHz and 25°C using the split cylinder method.
[0072] [Table 3]
[0073] From Table 3, it can be seen that the fluorine-containing compound of the present invention can be easily processed into a copper-clad laminate, and furthermore, the dielectric tangent is significantly reduced in the very high frequency range of 28 GHz, even compared to the PPE resin currently in general use as a substrate material for high-frequency transmission.
[0074] (Rating 4: Glass transition temperature) The copper-clad laminates of Examples 1 and 5, Comparative Example 1, and Reference Example prepared in the above electrical property evaluation were cut at an angle of 45 degrees to the mesh of the glass cloth to prepare test pieces measuring 25 mm in length and 25 mm in width. The test piece was subjected to the following temperature profile using a dynamic viscoelasticity measuring device (DMA ARES-G2, manufactured by TA Instruments) with a frequency of 1.0 Hz and a strain of 0.1%. (1) Hold at 25°C for 60 seconds and heat from 25°C to 360°C at a rate of 5°C / min. (2) The temperature is maintained at 360° C. for 60 seconds, and then the measurement is terminated. The temperature at the peak of the calculated loss factor (tan δ) versus temperature on the graph was taken as the glass transition temperature (Tg). The results are shown in Table 4.
[0075] [Table 4]
[0076] From the results in Table 4, the fluorine-containing compound of the present invention has a higher glass transition temperature (Tg) than the comparative examples. Because the Tg is high, the compound is less susceptible to the effects of deformation due to heat even when exposed to higher temperatures.
Claims
1. A fluorine-containing compound having a structure represented by the following formula (I): 【Chemistry 1】 In the formula, L is a structure represented by the following formula (II) or (III): 【Chemistry 2】 R 1 and R 2 each independently represents a hydrogen atom, C 1 ~C 10 Alkyl groups of C 1 ~C 10 haloalkyl group of C 6 ~C 10 or R 1 and R 2 are groups which together form a ring structure which may have a substituent, R 3 and R 4 each independently represents a hydrogen atom, a fluorine atom, or C in which some or all of the hydrogen atoms may be substituted by halogen 1 ~C 10 and C in which some or all of the hydrogen atoms may be substituted with halogen. 6 ~C 10 is a group selected from the group consisting of aryl groups n is in the range of 1 to 4; X is a group containing an olefinic carbon-carbon double bond or carbon-carbon triple bond.
2. 2. The fluorine-containing compound according to claim 1, wherein the cured product has a thermal expansion coefficient of 200 ppm / ° C. or less at 240° C. to 290° C.
3. 3. The fluorine-containing compound according to claim 1, wherein n is 1.
4. 3. The fluorine-containing compound according to claim 1, wherein said X comprises at least one fluorine atom.
5. 3. The fluorine-containing compound according to claim 1, wherein L is selected from the group consisting of a cyclopentylidene group which may have a substituent, a cyclohexylidene group which may have a substituent, and a cyclododecylidene group which may have a substituent.
6. 3. The fluorine-containing compound according to claim 1, wherein the gel fraction of the cured product is 50% or more.
7. A fluorine-containing composition comprising the fluorine-containing compound according to claim 1 and a crosslinking agent.
8. A prepreg comprising the fluorine-containing compound according to claim 1 and a fibrous base material.
9. A prepreg comprising the fluorine-containing composition according to claim 7 and a fibrous base material.
10. A copper-clad laminate comprising the cured prepreg according to claim 8 or 9 and at least one copper layer.
11. 10. A printed circuit board comprising the cured prepreg according to claim 8 or 9 and a conductor pattern formed on the surface thereof.
Citation Information
Patent Citations
Polyphenylene ether resin composition, prepreg, metal-clad laminate, and printed wiring board
JP2017128718A
Fluororesin
JP2022089150A
Fluorinated poly(arylene ether)
US5115082A
Crosslinkable fluorinated aromatic ether composition
US5179188A