Ink repellent member and inkjet head

The use of a fluorine compound bonded to a silicon oxide or tantalum oxide base in ink-repellent members addresses the issue of poor alkali resistance in ink repellent films, ensuring high ink repellency and uniformity, thus maintaining print quality.

JP2024159523APending Publication Date: 2024-11-08CANON KK

Patent Information

Application Number
JP2024045268
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-03-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Ink repellent films formed by bonding a fluorine-containing silane coupling agent to a base film can suffer from poor alkali resistance when exposed to alkaline inks, leading to reduced ink repellency due to insufficient wettability and aggregation of the agent, resulting in voids and exposure of the base film.

Method used

An ink-repellent member with a base containing silicon oxide or tantalum oxide, where a fluorine compound is bonded to the surface, achieving a static contact angle of 100° or more and a receding contact angle difference of less than 20° through a manufacturing process involving hydroxyl group formation, application of a fluoropolymer, and dehydration condensation of a reactive silyl group.

Benefits of technology

The solution provides an ink-repellent member with enhanced alkali resistance, ensuring high ink repellency and uniformity even when exposed to alkaline inks, maintaining print quality by preventing ink droplet direction variations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159523000001_ABST
    Figure 2024159523000001_ABST
Patent Text Reader

Abstract

To provide an ink repellent member excellent in ink resistance.SOLUTION: Provided is an ink repellent member comprising a base containing at least one of a silicon oxide and a tantalum oxide, where a fluorine compound is bonded to a surface of the base, the ink repellent member is characterized in that when a static contact angle and a receding contact angle of the surface after the ink repellent member is subjected to the following immersion treatment are represented by θ and θr, respectively, θ is 100° or more and θ-θr is less than 20°. (Immersion treatment): (1) a test piece including the surface is cut out from the ink repellent member, put in a sealable vessel containing an aqueous solution of pH11, and immersed so that the entire test piece is immersed, and (2) after the immersion in (1), the entire test piece is maintained at 70°C for 170 hours in a sealed state.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ink-repellent member and an ink-jet head. [Background technology]

[0002] Known examples of heads in inkjet recording devices that eject ink from nozzles include bubble jet (trademark) heads, which use a heater to instantly vaporize the ink to cause droplets to fly, and piezo jet heads, which use a piezoelectric element to cause ink to fly.

[0003] In such inkjet heads, if ink adheres to the ink ejection surface (nozzle plate surface) and becomes residue, it can affect the ink droplets ejected from the nozzles, causing the ejection direction of the ink droplets to vary. If the ejection direction varies, it becomes difficult to land the ink droplets at the specified positions on the recording medium, causing a decrease in print quality.

[0004] Therefore, it has been proposed to give the ink ejection surface a water-repellent function. For example, it is known to provide a base film made of an inorganic oxide on the ink ejection surface, and chemically bond a fluorine-containing silane coupling agent to form an ink-repellent film (Patent Document 1). By forming an ink-repellent film, the wetting and spreading of ink onto the ink ejection surface is suppressed, and even if ink adheres to the surface, it is easy to wipe it off with a wiper or the like. This suppresses variation in the ejection direction of droplets, increases linearity, improves the accuracy of the landing position on the recording medium, and improves print quality.

[0005] Since typical water-based inks are alkaline, such ink-repellent films are required to maintain ink-repellency (ink resistance) when they come into contact with alkaline inks with high pH values. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2015-3483 A Summary of the Invention [Problem to be solved by the invention]

[0007] As described in Patent Document 1, when forming an ink-repellent film by bonding a fluorine-containing silane coupling agent, it is common to apply the ink-repellent agent evenly to the base film in order to increase the uniformity of the ink-repellent film. This makes it possible to prevent the exposure of the undercoat film, which has poor alkali resistance, and therefore makes it possible to maintain ink repellency even when the ink ejection surface comes into contact with alkaline ink. However, if the ink repellent does not have sufficient wettability with respect to the undercoat film, the undercoat film may repel the ink repellent or the ink repellent agents may aggregate together, resulting in the formation of voids in the ink repellent film on the surface of the undercoat film. As a result, the undercoat film, which has poor alkali resistance, is exposed and is easily dissolved by contact with alkaline ink, resulting in a problem of reduced ink repellency. [Means for solving the problem]

[0008] According to one aspect of the present invention, there is provided an ink-repellent member having a base containing at least one of silicon oxide and tantalum oxide, and a fluorine compound bonded to the surface of the base, characterized in that after the ink-repellent member is subjected to the following immersion treatment, when the static contact angle of the surface is θ and the receding contact angle is θr, θ is 100° or more and θ-θr is less than 20°. (Immersion treatment) (1) A test piece including the surface is cut out from the ink-repellent member, and placed in a sealable container containing an aqueous solution of pH 11 so that the entire test piece is immersed. (2) After immersion in (1), keep the container sealed at 70°C for 170 hours.

[0009] According to another aspect of the present invention, there is provided a method for producing an ink-repellent member having a base containing at least one of silicon oxide and tantalum oxide, and a fluorine compound bonded to a surface of the base, the method comprising the following steps (1) to (3): (1) The process of forming hydroxyl groups on the surface of the substrate (2) A step of forming a thin film containing a fluoropolymer having a main chain with a perfluoropolyether structure and having perfluoromethyl structures at both ends on the surface of the base on which hydroxyl groups have been formed in the step (1). (3) A step of applying a fluorine compound having a reactive silyl group represented by the following formula (1) onto the thin film formed in the step (2) and carrying out dehydration condensation: *-Si(Y 1 ) n (OR) m (1) (In formula (1), n ​​and m are integers from 0 to 3, and n+m=3. Y 1 Each independently represents an alkyl group, a chloro group, or a bromo group. Each R independently represents a hydrogen atom or an alkyl group. * indicates the bonding position in the fluorine compound.

[0010] According to another aspect of the present invention, there is provided an inkjet head having an ink ejection surface having a base containing at least one of silicon oxide and tantalum oxide, and a fluorine compound bonded to the surface of the base, wherein, after the inkjet head is subjected to the following immersion treatment, when a static contact angle of the surface is θ and a receding contact angle is θr, θ is 100° or more and θ-θr is less than 20°. (Immersion treatment) (1) A test piece including the surface is cut out from the inkjet head and placed in a sealable container containing an aqueous solution of pH 11 so that the entire test piece is immersed. (2) After immersion in (1), keep the container sealed at 70°C for 170 hours.

[0011] According to another aspect of the present invention, there is provided a method for manufacturing an inkjet head having an ink ejection surface having a base containing at least one of silicon oxide and tantalum oxide and a fluorine compound bonded to a surface of the base, the method comprising the following steps (1) to (3): (1) The process of forming hydroxyl groups on the surface of the substrate (2) A step of forming a thin film containing a fluoropolymer having a main chain with a perfluoropolyether structure and having perfluoromethyl structures at both ends on the surface of the base on which hydroxyl groups have been formed in the step (1). (3) A step of applying a fluorine compound having a reactive silyl group represented by the following formula (1) onto the thin film formed in the step (2) and carrying out dehydration condensation: *-Si(Y 1 ) n (OR) m (1) (In formula (1), n ​​and m are integers from 0 to 3, and n+m=3. Y 1 Each independently represents an alkyl group, a chloro group, or a bromo group. Each R independently represents a hydrogen atom or an alkyl group. * indicates the bonding position in the fluorine compound.

[0012] According to another aspect of the present invention, there is provided an ink ejection device having the above-mentioned inkjet head. According to another aspect of the present invention, there is provided a method for manufacturing an article, comprising the step of ejecting a liquid using the above-mentioned inkjet head, wherein the liquid is an ink containing a functional material for forming a functional thin film or a functional element.

[0013] According to another aspect of the present invention, it is possible to provide an ink-repellent member having a surface and a base containing an inorganic oxide, characterized in that after the ink-repellent member is subjected to the following immersion treatment, when the static contact angle of the surface is θ and the receding contact angle is θr, θ is 100° or more and θ-θr is less than 20°. (Immersion treatment) (1) A test piece including the surface is cut out from the ink-repellent member, and placed in a sealable container containing an aqueous solution of pH 11 so that the entire test piece is immersed. (2) After immersion in (1), keep the container sealed at 70°C for 170 hours. Effect of the Invention

[0014] According to one aspect of the present invention, an ink-repellent member having excellent ink resistance can be obtained. [Brief description of the drawings]

[0015] [Figure 1] 1A is a schematic perspective view showing a part of an example of the configuration of an ink-jet head according to the present invention, and FIG. [Diagram 2] FIG. 2 is a schematic diagram for explaining the coating state of a fluorine compound on an undercoat film in an ink-repellent member according to the prior art (A) and the surface of the ink-repellent member after formation of Si—O—Si bonds (B). [Diagram 3] 1A is a schematic diagram illustrating a coating state of a fluorine compound on an undercoat film to which the fluorine compound is not bonded in an ink-repellent member according to the present invention, and FIG. 1B is a schematic diagram illustrating the surface of the ink-repellent member after formation of Si-O-Si bonds. [Figure 4] FIG. 2 is a diagram illustrating the contact angle and contact radius in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The expressions "XX or more and YY or less" or "XX to YY" representing a numerical range mean a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified. When numerical ranges are stated in stages, the upper and lower limits of each numerical range can be combined in any way.

[0017] Hereinafter, embodiments of the present invention will be described, however, the present invention is not limited to these embodiments.

[0018] <Ink-repellent material> The ink-repellent member of the present invention has a base containing at least one of silicon oxide and tantalum oxide, and a fluorine compound is bonded to the surface of the base, and is characterized in that after the ink-repellent member is subjected to the immersion treatment described below, when the static contact angle of the surface is θ and the receding contact angle is θr, θ is 100° or more and θ-θr is less than 20°. (Immersion treatment) (1) A test piece including the surface is cut out from the ink-repellent member, and placed in a sealable container containing an aqueous solution of pH 11 so that the entire test piece is immersed. (2) After immersion in (1), keep the container sealed at 70°C for 170 hours. In addition, the ink-repellent member of the present invention is an ink-repellent member having a surface and a base containing an inorganic oxide, and is characterized in that after the ink-repellent member is subjected to the following immersion treatment, when the static contact angle of the surface is θ and the receding contact angle is θr, θ is 100° or more and θ-θr is less than 20°. (Immersion treatment) (1) A test piece including the surface is cut out from the ink-repellent member, and placed in a sealable container containing an aqueous solution of pH 11 so that the entire test piece is immersed. (2) After immersion in (1), keep the container sealed at 70°C for 170 hours.

[0019] The ink-repellent member is a member including an ink-repellent film, and can be used as various devices where ink repellency is preferable, such as devices to which ink may adhere, such as inkjet heads, and machines that use ink, or as components of such devices, etc. In this specification, the ink-repellent film refers to a film made of a fluorine compound.

[0020] The ink-repellent member may or may not include a substrate. When the ink-repellent member includes a substrate, the undercoat can be provided on the substrate of the ink-repellent member. When the ink-repellent member is an inkjet head, the flow path substrate of the inkjet head can be used as the base material of the ink-repellent member. Silicon is a suitable material for the base material, but other materials that can be used include silicon carbide, silicon nitride, various types of glass such as quartz glass and borosilicate glass, various types of ceramics such as alumina and gallium arsenide, and resins such as polyimide.

[0021] (Base) The base in the present invention contains an inorganic oxide and is preferably a film (base film). The base not bonded with a fluorine compound has a hydroxyl group (-OH, hydroxy group) on its surface, and therefore can form a chemical bond with a fluorine compound (fluorine-containing silane coupling agent) having a reactive silyl group. By forming a chemical bond, the adhesion between the base and the fluorine compound, which is an ink repellent, can be improved.

[0022] Here, it is also known to use a base film mainly made of resin, but since it is soft, frictional force may be applied by the action of wiping off the ink attached to the head with a wipe, and the water repellency may be reduced. In the present invention, a hard film containing an inorganic oxide is used as the base, which is advantageous against frictional force. As the inorganic oxide, oxides such as silicon oxide, zirconia, alumina, titania, hafnia, tantalum oxide, cerium oxide, tungsten oxide, niobium oxide, yttrium oxide, indium oxide, and strontium oxide can be used. In the present invention, from the viewpoint of easily forming Si-O-Si bonds with a fluorine compound (fluorine-containing silane coupling agent), it is preferable that the base film contains silicon oxide. In addition, from the viewpoint of excellent alkali resistance, it is preferable that the base film contains tantalum oxide.

[0023] As the silicon oxide, it is preferable to use SiO2 because it contains many hydroxyl groups on the surface, which serve as reactive sites. However, silicon oxides with different oxidation numbers (SiO α , α represents an integer of 1 or more), or a mixture thereof.

[0024] Methods for forming silicon oxide include, but are not limited to, a method in which silicon, which is a flow path substrate, or silicon carbide (SiC) formed on silicon is oxidized using heat, plasma, UV, or the like, a method in which a silicon oxide target is used for sputter deposition, an ALD (atomic layer deposition) method, a CVD (chemical vapor deposition) method, a spin coating method, or the like. The tantalum oxide preferably contains Ta2O5. The method for forming the tantalum oxide is not particularly limited, and the tantalum oxide can be formed by sputtering deposition using an oxide target, electron beam deposition, or the like. When the ink-repellent member has a base material, the undercoat can be provided on the base material. The base material is, for example, a silicon substrate having an oxide film such as a thermal oxide film provided on its surface. When the base material itself is configured to include an inorganic oxide on its surface, the base material itself may be used as the undercoat.

[0025] (Fluorine compounds) The fluorine compound used in the present invention is a fluorine-containing silane coupling agent, and can act as an ink repellent. The fluorine compound will be described below. Fluorine compounds have a linear main chain structure, and only one of the two ends of the main chain chemically bonds to the hydroxyl group on the surface of the substrate. Specifically, when the substrate contains silicon oxide, the fluorine compound is chemically bonded to the surface of the substrate via a Si-O-Si bond. When the substrate contains tantalum oxide, the fluorine compound is chemically bonded to the surface of the substrate via a Ta-O-Si bond. In order to form a Si-O-Si bond or a Ta-O-Si bond, the fluorine compound used in the manufacture of the ink-repellent member or the inkjet head has at least one reactive silyl group represented by the following formula (1). By having a reactive silyl group at only one end, it is possible to suppress the reaction between fluorine compounds. *-Si(Y 1 ) n (OR) m (1) (In formula (1), n ​​and m are integers from 0 to 3, and n+m=3. Y 1Each independently represents an alkyl group, a chloro group, or a bromo group. Each R independently represents a hydrogen atom or an alkyl group. * indicates the bonding position in the fluorine compound. When n=3 and m=0, Y 1 At least one of the groups may be a chloro group or a bromo group. The other end preferably has a perfluoromethyl group (structure). The perfluoromethyl structure has a small surface free energy and can exhibit high ink repellency.

[0026] From the viewpoint of ink repellency and abrasion resistance, the main chain structure preferably has a perfluoropolyether (hereinafter, also referred to as PFPE) structure. That is, a preferred structure of the fluorine compound used in the manufacture of the ink-repellent member or ink-jet head can be represented by the following formula (9). [ka] (In formula (9), R 1 represents a reactive silyl group represented by formula (1), and R 2 represents a structure having a perfluoropolyether structure.

[0027] The fluorine compound preferably has at least one of the following structures as a PFPE structure: a structure represented by the following formula (2), a structure represented by the following formula (3), a structure represented by the following formula (4), and a structure represented by the following formula (5). A fluorine compound having at least one of the following structures as a PFPE structure: a structure represented by the following formula (2), a structure represented by the following formula (3), a structure represented by the following formula (4), and a structure represented by the following formula (5) is easily commercially available. [ka] [ka] [ka] [ka] (In formula (2), formula (3), formula (4), and formula (5), n1, n2, n3, and n4 each independently represent an integer of 1 or more.)

[0028] Preferable specific examples of the fluorine compound include a compound represented by the following formula (6), a compound represented by the following formula (7), and a compound represented by the following formula (8). [ka] (In formula (6), n5, m5, and l5 each independently represent an integer of 1 or more.) [ka] (In formula (7), s and m6 each independently represent an integer of 1 or more.) [ka] (In formula (8), h represents an integer of 1 or more.)

[0029] The fluorine compound contained in the ink repellent member or ink jet head is preferably a fluorine compound having a main chain with a perfluoropolyether structure and having a perfluoromethyl group at the end.

[0030] That is, a preferred structure of a fluorine compound in a state where the fluorine compound is chemically bonded to the surface of the base via a Si—O—Si bond or a Ta—O—Si bond can be represented by the following formula (10). [ka] (In formula (10), R 2 represents a structure having a perfluoropolyether structure, and R 3 indicates a Si-O bond, and the fluorine compound represented by formula (10) is chemically bonded to the surface of the substrate via a Si-O-Si bond or a Ta-O-Si bond including the Si-O bond. * indicates the bond position with a silicon atom or a tantalum atom.

[0031] (Fluoropolymer) The present inventors have conducted extensive research to obtain an ink-repellent member that has excellent ink repellency even when the wettability of a fluorine compound to a base to which the fluorine compound is not bonded is insufficient. As a result, they have found that the above object can be achieved by providing a step of forming a thin film of a fluoropolymer on the surface of a base in the ink-repellent film forming step.

[0032] FIG. 2 is a schematic diagram for explaining the state of application of a fluorine compound on a base film in an ink-repellent member in the prior art (A) and the surface of the ink-repellent member after the formation of Si-O-Si bonds (B). If the wettability of the fluorine compound to the base film is insufficient, when the fluorine compound is applied to the base film, the fluorine compound is repelled or the fluorine compounds aggregate with each other, resulting in a non-uniform state as shown in FIG. 2 (A). Therefore, after the formation of the Si-O-Si bonds, voids that are not covered by the fluorine compound are likely to be formed, resulting in a state as shown in FIG. 2 (B). In that case, the part of the base film that has poor alkali resistance is likely to come into contact with the ink, the base film dissolves, and the ink resistance decreases. Therefore, when a fluorine compound is applied after a thin film of a fluorine polymer is provided on the surface of the base film to which the fluorine compound is not bonded, the fluorine compound is uniformly dispersed in the thin film of the fluorine polymer, and repelling and aggregation are suppressed, so that the formation of voids is thought to be suppressed. FIG. 3 is a schematic diagram for explaining (A) the applied state of a fluorine compound on a base film to which the fluorine compound is not bonded of an ink-repellent member according to the present invention, and (B) the surface (base surface) of the ink-repellent member in which the fluorine compound is bonded to the surface of the base film via Si-O-Si bonds after reaching the state of (A).

[0033] The fluoropolymer can be selected from fluorine materials that have a high affinity with both the undercoat (inorganic oxide) and the fluorine compound. By applying a fluorine compound with a thin film of this fluoropolymer on the undercoat without fluorine compound bonding, it is possible to suppress the aggregation of the fluorine compound. As a result, the fluorine compound can form Si-O-Si bonds or Ta-O-Si bonds with uniform arrangement in the undercoat, making it possible to form an ink-repellent film with few voids on the surface.

[0034] The fluoropolymer used in the manufacture of the ink-repellent member or ink-jet head has a main chain having a perfluoropolyether structure and has perfluoromethyl groups (structures) at both ends. The fluoropolymer used in the manufacture of the ink-repellent member or ink-jet head can be represented by, for example, the following formula (11). [ka] (In formula (11), R 4 represents a structure having a perfluoropolyether structure.

[0035] The fluoropolymer having a perfluoromethyl structure at its terminal has high affinity with fluorine compounds, improving the dispersibility of the fluorine compounds.

[0036] From the viewpoint of affinity with fluorine compounds, the fluorine polymer is preferably a fluorine oil having a PFPE structure as the main chain structure. Fluorine oil has good wettability with inorganic oxides contained in the undercoat film, and is viscous, so that a thin film can be formed uniformly without repelling the undercoat film.

[0037] The fluoropolymer used in the manufacture of the ink-repellent member or inkjet head preferably has at least one of the structures represented by formula (2), (3), (4), and (5) as a PFPE structure. Furthermore, the fluoropolymer used in the manufacture of the ink-repellent member or inkjet head preferably has a structure represented by formula (4) and a structure represented by formula (5). The fluoropolymer having at least one of the structures represented by formula (2), (3), (4), and (5) is easily commercially available.

[0038] From the viewpoint of affinity, it is preferable that the fluorine compound and the fluorine polymer have the same PFPE structure.

[0039] The thin film of the fluoropolymer used in the manufacture of the ink-repellent member or inkjet head is preferably thicker than the molecular chain length of the fluoropolymer, and preferably has a thickness of 100 nm or more, from the viewpoint of enhancing the effect of suppressing the aggregation of the fluoropolymer on the surface of the base film. The film thickness can be appropriately selected depending on the coating process and conditions. When the fluoropolymer is directly coated, it can be coated by vacuum deposition or heat deposition. In this case, the film thickness can be controlled by selecting the degree of vacuum, deposition temperature, and deposition amount. In addition, the fluoropolymer solution can be coated by spray coating, spin coating, dip coating, etc., and the solvent can be dried to form a coating film. In this case, the film thickness can be controlled by selecting the solution concentration, coating time, rotation speed, etc.

[0040] <Method of manufacturing ink-repellent member> The method for manufacturing an ink-repellent member according to the present invention is a method for manufacturing an ink-repellent member having a base containing at least one of silicon oxide and tantalum oxide, and a fluorine compound bonded to the surface of the base, characterized in that it includes the following steps (1) to (3). (1) A process for forming hydroxyl groups on the surface of a substrate that is not bound to a fluorine compound (2) A step of forming a thin film containing a fluoropolymer having a main chain with a perfluoropolyether structure and having perfluoromethyl structures at both ends on the surface of the base on which hydroxyl groups have been formed in the step (1) and on which no fluorine compound is bonded. (3) A step of applying a fluorine compound having a reactive silyl group represented by the following formula (1) onto the thin film formed in the step (2) and carrying out dehydration condensation: *-Si(Y 1 ) n (OR) m (1) (In formula (1), n ​​and m are integers from 0 to 3, and n+m=3. Y 1 Each independently represents an alkyl group, a chloro group, or a bromo group. Each R independently represents a hydrogen atom or an alkyl group. * indicates the bonding position in the fluorine compound.

[0041] (Method of forming ink-repellent film) An example of a method for forming an ink-repellent film by bonding a fluorine compound to a substrate is described below. A method for forming an ink-repellent member and an inkjet head having a substrate containing silicon oxide and a fluorine compound chemically bonded to the surface of the substrate via a Si-O-Si bond can be performed by a silane coupling treatment.

[0042] First, a base film containing silicon oxide is formed on a silicon substrate, and silanol groups containing hydroxyl groups are formed on the surface. Methods for forming a base film containing silicon oxide include, for example, a method of forming the base film by oxidizing silicon, which is a flow path substrate, or silicon carbide (SiC) formed on silicon, using heat, plasma, UV, or the like, a method of forming the base film by sputter deposition using a silicon oxide target, an ALD (atomic layer deposition) method, a CVD (chemical vapor deposition) method, a spin coating method, or the like, but are not limited to these. One method for forming silanol groups containing hydroxyl groups (-OH) on the surface of an undercoat film containing silicon oxide is to form surface hydroxyl groups (-OH) by reacting the surface of the undercoat film with moisture.

[0043] Next, a fluoropolymer is applied to the surface of the undercoat film on which the silanol groups have been formed. The coating method is not particularly limited, and for example, the material may be directly coated by a deposition method such as vacuum deposition or thermal deposition, or a solution diluted with a fluorine solvent may be coated by a spray coating method, spin coating method, dip coating method, or the like, and the solvent may be dried to form a coating film.

[0044] Next, a fluorine compound is applied to the surface of the base on which the thin film containing a fluoropolymer has been formed. The coating method is not particularly limited, and may be, for example, a method in which the material is directly coated by a deposition method such as vacuum deposition or thermal deposition, or a solution diluted in a fluorine solvent is coated by a spray coating method, spin coating method, dip coating method, or the like, and the solvent is then dried.

[0045] Subsequently, the alkoxysilyl group or halogenated silyl group at the end of the fluorine compound can be hydrolyzed to convert it to a silanol group.

[0046] Then, a dehydration condensation reaction occurs with the hydroxyl groups formed on the undercoat film to form Si-O-Si bonds. Hydrolysis occurs when exposed to moisture, and can also occur due to adsorbed water present on the surface of the base film, but can be accelerated by placing the film in a high humidity environment (for example, 60% RH to 100% RH). In addition, the dehydration condensation reaction occurs even at room temperature (for example, 23° C.), but can be accelerated by raising the temperature (for example, 60° C. to 150° C.). The reaction time for the hydrolysis and dehydration condensation reactions can be appropriately selected depending on the humidity and temperature. For example, under conditions of 60° C. and 80% RH, the reaction time is about 2 hours in total.

[0047] Subsequently, washing is carried out to remove unbonded fluorine compounds and fluorine polymers. The cleaning method is not particularly limited, and may be, for example, immersed in a cleaning solvent that is compatible with the fluorine compound. In this case, the fluorine solvent may be heated or ultrasonic waves may be applied, if necessary.

[0048] When using an undercoat film containing tantalum oxide, a silane coupling treatment can be carried out to form a Ta-O-Si bond between the hydroxyl group on the undercoat film surface and the reactive silyl group of the fluorine compound, in the same manner as when using an undercoat film containing silicon oxide. The method of forming the tantalum oxide is not particularly limited, and it can be formed by sputtering deposition using an oxide target, electron beam deposition, or the like.

[0049] <Inkjet head> An example of the ink repellent member is an inkjet head. The inkjet head according to the present invention can be mounted in an ink discharge device, and the ink discharge device according to the present invention is an ink discharge device characterized by having the inkjet head according to the present invention. The inkjet head according to the present invention is an inkjet head having an ink ejection surface having a base containing at least one of silicon oxide and tantalum oxide and a fluorine compound bonded to the surface of the base, characterized in that after the inkjet head is subjected to the following immersion treatment, when the static contact angle of the surface is θ and the receding contact angle is θr, θ is 100° or more and θ-θr is less than 20°. (Immersion treatment) (1) A test piece including the surface is cut out from the inkjet head and placed in a sealable container containing an aqueous solution of pH 11 so that the entire test piece is immersed. (2) After immersion in (1), keep the container sealed at 70°C for 170 hours.

[0050] FIG. 1(A) is a schematic perspective view showing a portion of an example of the configuration of an inkjet head according to an embodiment of the present invention, in which a first flow path substrate 1 and a second flow path substrate 2 are joined with an adhesive 3, and a third flow path substrate 6 having an ejection port 4 is joined.

[0051] The surface of the first flow path substrate 1 has energy generating elements 5, particularly electrothermal conversion elements and piezoelectric elements for ejecting ink, and may also include wiring (not shown) for driving the energy generating elements 5. The energy generating elements 5 are formed on the first flow path substrate 1 so as to correspond to the positions of the ejection ports 4. The first flow path substrate 1 is formed with a third flow path substrate 6 and electrodes 7. The ink passes through a second through-flow path 9 and a first through-flow path 8 formed on the second flow path substrate 2 and the first flow path substrate 1, respectively, is given ejection energy by the energy generating elements 5, and is ejected from the ejection port 4. FIG. 1(B) is a top view of the first flow path substrate 1 and the third flow path substrate 6.

[0052] The ink-repellent film in the present invention is formed on the surface of the third flow path substrate 6 opposite to the surface bonded to the first flow path substrate 1. That is, this surface has an undercoat containing at least one of silicon oxide and tantalum oxide, and an ink ejection surface is formed in which a fluorine compound is bonded to the surface of the undercoat.

[0053] Silicon is suitable as the material for the flow path substrate, but other materials such as silicon carbide, silicon nitride, various glasses such as quartz glass and borosilicate glass, various ceramics such as alumina and gallium arsenide, and resins such as polyimide may also be used.

[0054] Methods for forming the first through-flow paths 8 and the second through-flow paths 9 in the first flow path substrate 1 and the second flow path substrate 2 include dry etching, wet etching, laser processing, etc. In order to adjust the height of the flow paths in the cross-sectional direction, the members can also be thinned by polishing using back grinding or CMP (chemical mechanical polishing).

[0055] <Inkjet head manufacturing method> The method for manufacturing an inkjet head according to the present invention is a method for manufacturing an inkjet head having an ink ejection surface having a base containing at least one of silicon oxide and tantalum oxide and a fluorine compound bonded to a surface of the base, and is characterized by comprising the following steps (1) to (3): (1) A process for forming hydroxyl groups on the surface of a substrate that is not bound to a fluorine compound (2) A step of forming a thin film containing a fluoropolymer having a main chain with a perfluoropolyether structure and having perfluoromethyl structures at both ends on the surface of the base on which hydroxyl groups have been formed in the step (1) and on which no fluorine compound is bonded. (3) A step of applying a fluorine compound having a reactive silyl group represented by the following formula (1) onto the thin film formed in the step (2) and carrying out dehydration condensation: *-Si(Y 1 ) n (OR) m (1) (In formula (1), n ​​and m are integers from 0 to 3, and n+m=3. Y 1 Each independently represents an alkyl group, a chloro group, or a bromo group. Each R independently represents a hydrogen atom or an alkyl group. * indicates the bonding position in the fluorine compound.

[0056] <Contact angle> The ink-repellent member or inkjet head of the present invention is characterized in that, after the immersion treatment described below, the static contact angle of the surface or the ink ejection surface (base surface) of the ink-repellent member or ink-jet head is θ and the receding contact angle is θr, where θ is 100° or more and θ-θr is less than 20°.

[0057] The contact angle is the angle formed by a droplet dropped on a solid surface and the solid surface. Among them, the static contact angle is the angle between the liquid surface and the solid surface when the droplet is stationary on the solid. Also, the receding contact angle is the contact angle formed by the liquid on the rear side of the moving direction of the droplet when the liquid moves in a certain direction. The static contact angle and the receding contact angle can be obtained by calculating the contact angle from an image of the droplet by image analysis. The static contact angle can be obtained by, for example, the θ / 2 method or the tangent method. The receding contact angle can be obtained by, for example, the expansion / contraction method or the sliding method. Also, the receding contact angle can be obtained by continuously measuring the contact radius at a certain time interval after the droplet lands by the droplet method. In the present invention, a test piece including the surface or ink discharge surface (underlying surface) for which the static contact angle or the receding contact angle is to be obtained is taken from the ink-repellent member or the inkjet head, and the test piece is measured to obtain the static contact angle or the receding contact angle. FIG. 4 is a diagram for explaining the contact angle θ1 and the contact radius r.

[0058] The ink repellency of an ink-repellent member or inkjet head can be evaluated by the static contact angle of the surface or ink ejection surface (underlying surface) and the difference between the static contact angle and the receding contact angle. When the static contact angle of the surface or ink ejection surface (underlying surface) is 100° or more, the water repellency is high, ink can be easily removed, and the ink repellency can be considered to be high. When the difference between the static contact angle and the receding contact angle is small, the ink repellency of the surface or ink ejection surface can be considered to be uniform. When the hydrophilic portion is exposed in a large amount on the surface or ink ejection surface and the hydrophilic portion and the water-repellent (ink-repellent) portion are mixed (when the surface is not homogeneous), the receding contact angle becomes small due to the pinning effect, and the difference between the static contact angle and the receding contact angle may become large.

[0059] In this specification, the static contact angle of the ink-repellent member or the surface of the inkjet head or the ink ejection surface (the surface of the base) after the immersion treatment described below is defined as θ, and the receding contact angle is defined as θr. If θ is 100° or more and θ-θr is less than 20° after the immersion treatment described below, it can be said that the ink repellency is high and uniform even against alkaline inks with high pH. θ-θr is preferably less than 15°. More preferably, it is less than 12°.

[0060] (Immersion treatment) (1) A test piece including the surface or ink ejection surface (base surface) is cut out from an ink-repellent material or an inkjet head, and placed in a sealable container containing an aqueous solution of pH 11 so that the entire test piece is immersed. (2) After immersion in (1), keep the container sealed at 70°C for 170 hours.

[0061] (Method of manufacturing an article using an ink-repellent member) The method for manufacturing an article according to one embodiment of the present invention can be characterized in that it includes a step of ejecting a liquid using the ink-repellent member (e.g., an inkjet head) described above, and the liquid is an ink containing a functional material for forming a functional thin film or a functional element. EXAMPLES

[0062] The present invention will be specifically described below using examples, but the present invention is not limited to the following examples.

[0063] Example 1 A Φ3 inch silicon substrate was heated at 900℃ in an oxygen atmosphere to form a thermal oxide film containing SiO2 as an undercoat on the surface. Next, using FP-1 shown below as a fluoropolymer, a FP-1 solution was spin-coated onto the silicon substrate on which the above-mentioned undercoat film had been formed to a film thickness of 80 nm, and a thin film of FP-1 was formed by volatilizing the solvent. The FP-1 solution was prepared by dissolving FP-1 at a concentration of 5 wt% in a fluorosolvent (Novec7300, manufactured by 3M). Next, the silicon substrate on which the thin film of FP-1 was formed was placed in a vacuum deposition machine, and the surface on which FP-1 was formed was coated by deposition with FC-1, shown below, as a fluorine compound. Deposition was performed by placing 60 mg of FC-1 impregnated in steel wool in a Cu container, and resistively heating the Cu container. Next, the silicon substrate on which FC-1 was deposited was placed in a thermo-hygrostat and left to stand for 3 hours in an environment of 60° C. and 80% RH. The silicon substrate was removed and kept immersed in a fluorine solvent (Novec7300, 3M) for 20 seconds to clean the surface. The cleaning was repeated three times using a separately prepared fluorine solvent. After that, the substrate was immersed in the fluorine solvent again and ultrasonic cleaning was performed. After washing, the fluorine solvent was removed by air drying. In this manner, an ink-repellent member 1 having an ink-repellent film (a fluorine compound is bonded to the surface of the base film) was produced. FC-1: A compound represented by formula (6) having a number average molecular weight of 5000 (X-71-195, manufactured by Shin-Etsu Chemical Co., Ltd.) FP-1: Fomblin M03 (Fomblin M series, manufactured by Solvay) having a main chain structure including a structure represented by formula (4) and a structure represented by formula (5)

[0064] (Examples 2 to 4) Ink-repellent members 2 to 4 according to each example were produced in the same manner as in Example 1, except that the material type of the fluorine compound and the material type and film thickness of the fluorine polymer shown in Table 1 were used. The FP-2 used as the fluoropolymer in Example 4 is shown below. FP-2: Krytox GPL Oil 103 (manufactured by Chemours) having a main chain structure containing the structure represented by formula (3)

[0065] Example 5 Ta2O5 was formed by electron beam deposition on a Φ3 inch silicon substrate, and this was used as a base film. When forming the base film, the thickness of the base film was observed using a quartz crystal oscillator, and deposition was stopped when the film thickness reached 100 nm (calculated with a refractive index of 2.165). An ink-repellent member 5 was produced in the same manner as in Example 1, except that the base film was changed and that the material type of the fluorine compound and the material type and film thickness of the fluorine polymer were changed as shown in Table 1.

[0066] Comparative Example 1 An ink-repellent member 6 according to Comparative Example 1 was produced in the same manner as in Example 1, except that no fluoropolymer was used.

[0067] Comparative Example 2 An ink-repellent member 7 according to Comparative Example 2 was produced in the same manner as in Example 5, except that the fluoropolymer was not used.

[0068] (Evaluation preparation: ink immersion treatment) The ink-repellent members 1 to 7 thus prepared were subjected to an immersion treatment according to the following procedure. First, test pieces measuring 3 cm x 3 cm and 1 mm thick were cut out from each of the ink-repellent members 1 to 7, including the surface of each ink-repellent member (the surface of the base to which the fluorine compound is bonded). Then, an aqueous solution (potassium hydroxide) adjusted to pH 11 was placed in a sealed container made of PFA (tetrafluoroethylene-perfluoroalkoxyethylene copolymer resin), and each test piece was immersed so that the entire test piece was in contact with the aqueous solution, and the container was sealed with a lid. In this state, the container was placed in an oven and heated at 70°C for one week (170 hours). After thoroughly washing each of the removed test pieces with water to remove the aqueous solution, the static contact angle and receding contact angle of the surfaces of the ink-repellent members 1 to 7 (the surface of the base to which the fluorine compound is bonded) were measured by the method described below in (Evaluation: Contact angle measurement).

[0069] (Evaluation: Contact angle measurement) Using a contact angle meter (product name: DM-701, manufactured by Kyowa Interface Science Co., Ltd., analysis software: FAMAS (ver.3.5.5)), the static contact angle θ and receding contact angle θr of the surface of the ink-repellent member (the surface of the base to which the fluorine compound is bonded) with respect to pure water after the above immersion treatment were measured. The measurement conditions were as follows. ·Droplet: 2μL Static contact angle θ: The contact angle 1 second after the droplet landed was taken as the static contact angle θ. Receding contact angle θr: Calculated by the sessile drop method. Specifically, the receding contact angle θr was measured as follows. The contact angle was measured at 80 points at 15-second intervals after the droplet landed. Using the contact angle and contact radius (unit: μm) at a certain time calculated by the above software, the following calculations were performed starting from time 0 seconds, and the following processes (A) and (B) were performed. (A) Value of contact radius R at time t t , the value of the contact radius R after t+90 seconds t+90 Then, (R t -R t+90 ) 2 The value x was calculated. (B) When the value of x was 200 or less, the process of (A) was repeated, and the contact angle at the time t when the value of x first exceeded 200 was defined as the receding contact angle θr. (θ-θr evaluation criteria) Rank A: θ-θr is less than 12° Rank B: θ-θr is 12° or more and less than 15° Rank C: θ-θr is 15° or more and less than 20° Rank D: θ-θr is 20° or more In this embodiment, when θ is 100° or more and the evaluation of θ-θr is rank C or higher, it can be said that the ink-repellent member has excellent ink resistance.

[0070] [Table 1]

[0071] Table 2 shows the evaluation results of θ-θr for the ink-repellent members 1 to 7 produced in Examples 1 to 5 and Comparative Examples 1 and 2. [Table 2]

[0072] It is apparent from Tables 1 and 2 that ink-repellent members having excellent ink resistance can be obtained according to the examples of the present invention.

[0073] The disclosure of this embodiment includes the following configurations and methods. (Configuration 1) An ink-repellent member having a base containing at least one of silicon oxide and tantalum oxide, and a fluorine compound bonded to a surface of the base, An ink-repellent member, characterized in that after the ink-repellent member is subjected to the following immersion treatment, when the static contact angle of the surface is θ and the receding contact angle is θr, θ is 100° or more and θ-θr is less than 20°. (Immersion treatment) (1) A test piece including the surface is cut out from the ink-repellent member, and placed in a sealable container containing an aqueous solution of pH 11 so that the entire test piece is immersed. (2) After immersion in (1), keep the container sealed at 70°C for 170 hours. (Configuration 2) The ink-repellent member according to configuration 1, wherein the θ-θr is less than 15°. (Configuration 3) When the underlayer contains silicon oxide, the fluorine compound is bonded to the surface via a Si-O-Si bond; 3. The ink-repellent member according to claim 1 or 2, wherein when the undercoat contains tantalum oxide, the fluorine compound is bonded to the surface via a Ta-O-Si bond. (Configuration 4) 4. The ink-repellent member according to any one of configurations 1 to 3, comprising a substrate, the undercoat being provided on the substrate. (Configuration 5) 5. The ink-repellent member according to any one of configurations 1 to 4, wherein the fluorine compound has a main chain having a perfluoropolyether structure and has a perfluoromethyl group at an end thereof. (Configuration 6) The ink-repellent member according to any one of configurations 1 to 5, wherein the fluorine compound has at least one of a structure represented by the following formula (2), a structure represented by the following formula (3), a structure represented by the following formula (4), and a structure represented by the following formula (5). [ka] [ka] [ka] [ka] (In formula (2), formula (3), formula (4), and formula (5), n1, n2, n3, and n4 each independently represent an integer of 1 or more.) (Method 7) A method for manufacturing an ink-repellent member having an underlayer containing at least one of silicon oxide and tantalum oxide, and a fluorine compound bonded to a surface of the underlayer, the method comprising the following steps (1) to (3): (1) The process of forming hydroxyl groups on the surface of the substrate (2) A step of forming a thin film containing a fluoropolymer having a main chain with a perfluoropolyether structure and having perfluoromethyl structures at both ends on the surface of the base on which hydroxyl groups have been formed in the step (1). (3) A step of applying a fluorine compound having a reactive silyl group represented by the following formula (1) onto the thin film formed in the step (2) and carrying out dehydration condensation: *-Si(Y 1 ) n (OR) m (1) (In formula (1), n ​​and m are integers from 0 to 3, and n+m=3. Y 1 Each independently represents an alkyl group, a chloro group, or a bromo group. Each R independently represents a hydrogen atom or an alkyl group. * indicates the bonding position in the fluorine compound. (Method 8) Method 8. The method for producing an ink-repellent member according to Method 7, wherein the thin film has a thickness of 100 nm or more. (Method 9) The method for producing an ink-repellent member described in Method 7 or 8, wherein the fluoropolymer has at least one of a structure represented by the following formula (2), a structure represented by the following formula (3), a structure represented by the following formula (4), and a structure represented by the following formula (5). [ka] [ka] [ka] [ka] (In formula (2), formula (3), formula (4), and formula (5), n1, n2, n3, and n4 each independently represent an integer of 1 or more.) (Method 10) The method for producing an ink-repellent member according to Method 9, wherein the fluoropolymer has a structure represented by Formula (4) and a structure represented by Formula (5). (Configuration 11) An inkjet head having an ink ejection surface having a base containing at least one of silicon oxide and tantalum oxide, and a fluorine compound bonded to a surface of the base, The inkjet head is characterized in that, after the inkjet head is subjected to the following immersion treatment, when the static contact angle on the surface is θ and the receding contact angle is θr, θ is 100° or more and θ-θr is less than 20°. (Immersion treatment) (1) A test piece including the surface is cut out from the inkjet head and placed in a sealable container containing an aqueous solution of pH 11 so that the entire test piece is immersed. (2) After immersion in (1), keep the container sealed at 70°C for 170 hours. (Configuration 12) 12. The inkjet head according to configuration 11, wherein the θ-θr is less than 15°. (Configuration 13) When the underlayer contains silicon oxide, the fluorine compound is bonded to the surface via a Si-O-Si bond; 13. The inkjet head according to claim 11 or 12, wherein when the undercoat contains tantalum oxide, the fluorine compound is bonded to the surface via a Ta—O—Si bond. (Configuration 14) 14. The inkjet head according to any one of Configurations 11 to 13, wherein the fluorine compound has a main chain having a perfluoropolyether structure and has a perfluoromethyl group at an end. (Configuration 15) The inkjet head according to any one of configurations 11 to 14, wherein the fluorine compound has at least one of a structure represented by the following formula (2), a structure represented by the following formula (3), a structure represented by the following formula (4), and a structure represented by the following formula (5). [ka] [ka] [ka] [ka] (In formula (2), formula (3), formula (4), and formula (5), n1, n2, n3, and n4 each independently represent an integer of 1 or more.) (Method 16) A method for manufacturing an inkjet head having an ink ejection surface having a base containing at least one of silicon oxide and tantalum oxide, and a fluorine compound bonded to a surface of the base, comprising the steps of: (1) The process of forming hydroxyl groups on the surface of the substrate (2) A step of forming a thin film containing a fluoropolymer having a main chain with a perfluoropolyether structure and having perfluoromethyl structures at both ends on the surface of the base on which hydroxyl groups have been formed in the step (1). (3) A step of applying a fluorine compound having a reactive silyl group represented by the following formula (1) onto the thin film formed in the step (2) and carrying out dehydration condensation: *-Si(Y 1 ) n (OR) m (1) (In formula (1), n ​​and m are integers from 0 to 3, and n+m=3. Y 1 Each independently represents an alkyl group, a chloro group, or a bromo group. Each R independently represents a hydrogen atom or an alkyl group. * indicates the bonding position in the fluorine compound. (Method 17) 17. The method for producing an inkjet head according to claim 16, wherein the thin film has a thickness of 100 nm or more. (Method 18) The method for producing an inkjet head according to Method 16 or 17, wherein the fluoropolymer has at least one of a structure represented by the following formula (2), a structure represented by the following formula (3), a structure represented by the following formula (4), and a structure represented by the following formula (5). [ka] [ka] [ka] [ka] (In formula (2), formula (3), formula (4), and formula (5), n1, n2, n3, and n4 each independently represent an integer of 1 or more.) (Method 19) 19. The method for producing an inkjet head according to Method 18, wherein the fluoropolymer has a structure represented by the formula (4) and a structure represented by the formula (5). (Configuration 20) An ink-ejecting device having the ink-jet head according to any one of configurations 11 to 15. (Configuration 21) An ink-repellent member having a surface and a base containing an inorganic oxide, An ink-repellent member, characterized in that after the ink-repellent member is subjected to the following immersion treatment, when the static contact angle of the surface is θ and the receding contact angle is θr, θ is 100° or more and θ-θr is less than 20°. (Immersion treatment) (1) A test piece including the surface is cut out from the ink-repellent member, and placed in a sealable container containing an aqueous solution of pH 11 so that the entire test piece is immersed. (2) After immersion in (1), keep the container sealed at 70°C for 170 hours. (Method 22) A method for producing an article, comprising a step of ejecting a liquid using the inkjet head according to any one of configurations 11 to 15, The method for manufacturing an article, wherein the liquid is an ink containing a functional material for forming a functional thin film or a functional element. [Explanation of symbols]

[0074] 1. First flow path substrate 2. Second flow path substrate 3. Glue 4 outlet 5 Energy generating elements 6. Third flow path substrate 7 electrodes 8 First through passage 9 Second through passage

Claims

1. An ink-repellent member having a base containing at least one of silicon oxide and tantalum oxide, and a fluorine compound bonded to a surface of the base, The ink-repellent member is characterized in that, after the ink-repellent member is subjected to the following immersion treatment, when the static contact angle of the surface is θ and the receding contact angle is θr, θ is 100° or more and θ-θr is less than 20°. (Immersion treatment) (1) A test piece including the surface is cut out from the ink-repellent member, and placed in a sealable container containing an aqueous solution of pH 11, so that the entire test piece is immersed. (2) After immersion in (1), keep the container sealed at 70° C. for 170 hours.

2. 2. The ink repellent member according to claim 1, wherein the θ-θr is less than 15°.

3. When the underlayer contains silicon oxide, the fluorine compound is bonded to the surface via a Si—O—Si bond; 2. The ink repellent member according to claim 1, wherein when the undercoat contains tantalum oxide, the fluorine compound is bonded to the surface via a Ta-O-Si bond.

4. The ink repellent member according to claim 1 , further comprising a substrate, the undercoat being provided on the substrate.

5. 2. The ink repellent member according to claim 1, wherein the fluorine compound has a main chain having a perfluoropolyether structure and has a perfluoromethyl group at an end thereof.

6. The ink-repellent member according to claim 1, characterized in that the fluorine compound has at least one of a structure represented by the following formula (2), a structure represented by the following formula (3), a structure represented by the following formula (4), and a structure represented by the following formula (5): 【Chemistry 1】 【Chemistry 2】 【Chemistry 3】 【Chemistry 4】 (In formula (2), formula (3), formula (4), and formula (5), n1, n2, n3, and n4 each independently represent an integer of 1 or more.)

7. A method for manufacturing an ink-repellent member having a base containing at least one of silicon oxide and tantalum oxide, and a fluorine compound bonded to a surface of the base, the method comprising the following steps (1) to (3): (1) A process for forming hydroxyl groups on the surface of a substrate (2) A step of forming a thin film containing a fluoropolymer having a main chain with a perfluoropolyether structure and having perfluoromethyl structures at both ends on the surface of the base on which hydroxyl groups have been formed in the step (1). (3) A step of applying a fluorine compound having a reactive silyl group represented by the following formula (1) onto the thin film formed in the step (2) and subjecting it to dehydration condensation: *-Si(Y 1 ) n (OR) m (1) (In formula (1), n ​​and m are integers from 0 to 3, and n+m=3. Y 1 Each independently represents an alkyl group, a chloro group, or a bromo group. Each R independently represents a hydrogen atom or an alkyl group. * indicates the bonding position in the fluorine compound.

8. The method for producing an ink-repellent member according to claim 7, wherein the thin film has a thickness of 100 nm or more.

9. The method for producing an ink-repellent member according to claim 7, characterized in that the fluoropolymer has at least one of a structure represented by the following formula (2), a structure represented by the following formula (3), a structure represented by the following formula (4), and a structure represented by the following formula (5). 【Chemistry 5】 【Chemistry 6】 【Chemistry 7】 【Chemistry 8】 (In formula (2), formula (3), formula (4), and formula (5), n1, n2, n3, and n4 each independently represent an integer of 1 or more.)

10. The method for producing an ink-repellent member according to claim 9 , wherein the fluoropolymer has a structure represented by the formula (4) and a structure represented by the formula (5).

11. An inkjet head having an ink ejection surface having a base containing at least one of silicon oxide and tantalum oxide, and a fluorine compound bonded to a surface of the base, The inkjet head is characterized in that, after the inkjet head is subjected to an immersion treatment described below, when a static contact angle on the surface is θ and a receding contact angle is θr, θ is 100° or more and θ-θr is less than 20°. (Immersion treatment) (1) A test piece including the surface is cut out from the inkjet head and placed in a sealable container containing an aqueous solution of pH 11, so that the entire test piece is immersed. (2) After immersion in (1), keep the container sealed at 70° C. for 170 hours.

12. 12. The ink jet head according to claim 11, wherein the value of θ-θr is less than 15°.

13. When the underlayer contains silicon oxide, the fluorine compound is bonded to the surface via a Si—O—Si bond; 12. The ink jet head according to claim 11, wherein when the underlayer contains tantalum oxide, the fluorine compound is bonded to the surface via a Ta-O-Si bond.

14. The inkjet head according to claim 11, wherein the fluorine compound has a main chain having a perfluoropolyether structure and has a perfluoromethyl group at an end thereof.

15. The inkjet head according to claim 11, characterized in that the fluorine compound has at least one of a structure represented by the following formula (2), a structure represented by the following formula (3), a structure represented by the following formula (4), and a structure represented by the following formula (5): 【Chemistry 9】 【Chemistry 10】 【Chemistry 11】 【Chemistry 12】 (In formula (2), formula (3), formula (4), and formula (5), n1, n2, n3, and n4 each independently represent an integer of 1 or more.)

16. A method for manufacturing an inkjet head having an ink ejection surface having a base containing at least one of silicon oxide and tantalum oxide, and a fluorine compound bonded to a surface of the base, the method comprising the steps of: (1) A process for forming hydroxyl groups on the surface of a substrate (2) A step of forming a thin film containing a fluoropolymer having a main chain with a perfluoropolyether structure and having perfluoromethyl structures at both ends on the surface of the base on which hydroxyl groups have been formed in the step (1). (3) A step of applying a fluorine compound having a reactive silyl group represented by the following formula (1) onto the thin film formed in the step (2) and subjecting it to dehydration condensation: *-Si(Y 1 ) n (OR) m (1) (In formula (1), n ​​and m are integers from 0 to 3, and n+m=3. Y 1 Each independently represents an alkyl group, a chloro group, or a bromo group. Each R independently represents a hydrogen atom or an alkyl group. * indicates the bonding position in the fluorine compound.

17. The method for manufacturing an ink jet head according to claim 16, wherein the thin film has a thickness of 100 nm or more.

18. 17. The method for manufacturing an inkjet head according to claim 16, wherein the fluoropolymer has at least one of a structure represented by the following formula (2), a structure represented by the following formula (3), a structure represented by the following formula (4), and a structure represented by the following formula (5): 【Chemistry 13】 【Chemistry 14】 【Chemistry 15】 【Chemistry 16】 (In formula (2), formula (3), formula (4), and formula (5), n1, n2, n3, and n4 each independently represent an integer of 1 or more.)

19. 19. The method for manufacturing an ink jet head according to claim 18, wherein the fluoropolymer has a structure represented by the formula (4) and a structure represented by the formula (5).

20. An ink ejection device comprising the ink-jet head according to any one of claims 11 to 15.

21. An ink-repellent member having a surface and a base containing an inorganic oxide, The static contact angle of the surface of the ink-repellent member after the ink-repellent member is subjected to the following immersion treatment is defined as θ, An ink-repellent member, characterized in that, when a receding contact angle is θr, θ is 100° or more, and θ-θr is less than 20°. (Immersion treatment) (1) A test piece including the surface is cut out from the ink-repellent member, and placed in a sealable container containing an aqueous solution of pH 11, so that the entire test piece is immersed. (2) After immersion in (1), keep the container sealed at 70° C. for 170 hours.

22. A method for manufacturing an article, comprising a step of ejecting a liquid using the inkjet head according to any one of claims 11 to 15, The method for manufacturing an article, wherein the liquid is an ink containing a functional material for forming a functional thin film or a functional element.

Citation Information

Patent Citations

  • Liquid discharge head and image formation device

    JP2015003483A

Cited By

  • Ink-repellent member, method of producing ink-repellent member, ink jet head, and method of producing article

    JP2025103956A

  • Ink-repellent material, method for manufacturing an ink-repellent material, inkjet head, method for manufacturing an article

    JP7939932B2