Hollow resin particles

Hollow resin particles with an acid-modified polyphenylene ether and vinyl resin shell overcome heat resistance and redispersibility issues, enhancing dielectric performance and manufacturing efficiency.

JP2024159545APending Publication Date: 2024-11-08UNITIKA LTD

Patent Information

Application Number
JP2024062450
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-09
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Conventional hollow resin particles face issues with heat resistance, dielectric properties, and redispersibility due to the use of inorganic components or acrylic resins, leading to poor flexibility and high manufacturing costs.

Method used

Hollow resin particles with a shell made of acid-modified polyphenylene ether resin and vinyl resin, incorporating functional groups like sulfo, carboxy, or carboxylic acid anhydride groups, and a crosslinking monomer, produced through dispersion or emulsion polymerization.

Benefits of technology

The resulting particles exhibit excellent heat resistance, dielectric properties, and improved redispersibility, addressing the limitations of previous materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159545000001
    Figure 2024159545000001
Patent Text Reader

Abstract

To provide hollow resin particles excellent in heat resistance, dielectric characteristics, and redispersibility after drying.SOLUTION: The hollow resin particles each have a shell part and a hollow portion surrounded by the shell part. The shell part comprises an acid-modified polyphenylene ether resin and a vinyl resin. The acid-modified polyphenylene ether resin is acid-modified with at least one functional group selected from the group consisting of a sulfo group, a carboxy group, a carboxylic acid anhydride group, and a phosphate group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to hollow resin particles. [Background technology]

[0002] In recent years, in order to keep up with the increasing demand for high-speed lines in the communications industry, there has been an effort to develop resin materials with low transmission loss, i.e., resin materials with low dielectric constant (Dk) and dielectric dissipation factor (Df). There are various known methods for reducing the dielectric constant of resin materials (reducing their dielectric constant and dielectric dissipation factor), such as making the resin material porous by using air, which has a Dk of 1, or adding hollow particles to the resin material.

[0003] The hollow particles used in the above-mentioned method may be, for example, hollow particles surrounded by a shell made of an inorganic component. However, due to the hardness of the inorganic component, there is a problem that the obtained resin material has poor flexibility.

[0004] In light of this background, hollow particles made of organic polymers have been studied in recent years. For example, Patent Document 1 discloses hollow resin particles made of a divinylbenzene polymer (crosslinked polystyrene), and Patent Document 2 discloses hollow resin particles made of a copolymer of a multifunctional acrylate and a monofunctional methacrylate.

[0005] The hollow resin particles described in Patent Document 1 are made of a material (crosslinked polystyrene) with low relative dielectric constant and dielectric tangent, and therefore can be said to be effective particles to be added for the purpose of reducing the dielectric constant of resin materials. However, the high-boiling point saturated hydrocarbons (specifically, hexadecane) used in the production are difficult to remove from the hollow parts by distillation or the like, and the production costs are high in order to completely replace the hollow parts with air. Furthermore, the hollow resin particles described in Patent Document 1 are made of a styrene-based material, and therefore have insufficient heat resistance.

[0006] The hollow resin particles described in Patent Document 2 are made of crosslinked acrylic resin. In general, acrylic resins are known to have high dielectric constants and dielectric loss tangents, insufficient heat resistance, and high water absorption. For these reasons, the hollow resin particles described in Patent Document 2 are not suitable for addition to resin materials for the purpose of lowering their dielectric constant and dielectric loss tangent.

[0007] In view of the above problems, hollow resin particles made of a copolymer of a polyphenylene ether oligomer having a radical polymerizable functional group and divinylbenzene are disclosed in Patent Document 3. However, the hollow particles described in Patent Document 3 tend to have poor redispersibility even when added to a resin material, because some of the particles form aggregates during the drying process of the hollow particles. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2002-080503 A [Patent Document 2] JP 2020-33503 A [Patent Document 3] International Publication No. 2022 / 131127 Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide hollow resin particles which are superior in heat resistance, dielectric properties, and redispersibility after drying, as compared with conventional hollow resin particles.

[0010] As a result of intensive research, the present inventors have found that hollow resin particles, the shell of which is made of a polyphenylene ether resin modified with a specific functional group and a vinyl resin, can solve the above-mentioned problems. This finding led to the present invention. That is, the gist of the present invention is as follows.

[0011] (1) A hollow resin particle having a shell portion and a hollow portion surrounded by the shell portion, the shell portion being made of an acid-modified polyphenylene ether resin and a vinyl resin, the acid-modified polyphenylene ether resin being acid-modified with at least one functional group selected from the group consisting of a sulfo group, a carboxy group, a carboxylic anhydride group, and a phosphate group. (2) The hollow resin particles according to (1), wherein the acid-modified polyphenylene ether resin has an acid value of 0.5 to 80 mgKOH / g. (3) The hollow resin particles according to (1) or (2), characterized in that the volume average particle diameter is 0.1 to 50 μm. (4) The hollow resin particles according to (1) or (2), wherein the vinyl resin contains a crosslinkable monomer as a copolymerization component. (5) The hollow resin particles according to (4), wherein the crosslinkable monomer as a copolymerization component is at least one selected from the group consisting of divinylnaphthalene, diallyl phthalate, and divinylbenzene. (6) A hollow resin particle dispersion comprising the hollow resin particles according to (1) or (2) above and a medium. (7) A method for producing the hollow resin particles described in (1) above, comprising the following steps (I) and (II): (I) A step of dispersion polymerizing or emulsion polymerizing a vinyl monomer in the presence of a dispersion liquid in which particles made of an acid-modified polyphenylene ether resin are dispersed in a medium. (II) A step of drying the dispersion obtained in (I) above. Effect of the Invention

[0012] According to the present invention, hollow resin particles excellent in heat resistance, dielectric properties, and redispersibility after drying can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below. The hollow resin particles of the present invention have a shell portion made of an acid-modified polyphenylene ether resin and a vinyl resin, and a hollow portion surrounded by the shell portion.

[0014] In the hollow resin particles of the present invention, "hollow" means that the inside is filled with a substance other than resin, such as a gas or liquid, and preferably means that the inside is filled with gas, in that the effects of the present invention can be more effectively expressed.

[0015] The shell portion and the hollow portion surrounded by the shell portion may be composed of one hollow region, or may be composed of a plurality of hollow regions. The hollow portion may have a porous structure. When the hollow portion has a porous structure, the hollow portion may have one hollow region (continuous pores), multiple hollow regions (closed pores), or a mixture of these.

[0016] <Acid-modified polyphenylene ether resin> The acid-modified polyphenylene ether resin constituting the shell of the hollow resin particle of the present invention must be acid-modified with at least one functional group selected from the group consisting of a sulfo group, a carboxy group, a carboxylic anhydride group, and a phosphoric acid group. The acid-modified polyphenylene ether resin constituting the shell has these functional groups, so that the hollow resin particles have excellent redispersibility after drying. From the viewpoint of the redispersibility of the hollow resin particles, it is preferable that the acid-modified polyphenylene ether resin has at least one functional group selected from the group consisting of a carboxy group and a carboxylic anhydride group.

[0017] The method for producing the acid-modified polyphenylene ether resin is not particularly limited, and examples thereof include a method in which a polyphenylene ether resin and a vinyl compound having the above-mentioned functional group are reacted by heating and melting the polyphenylene ether resin to a temperature equal to or higher than the melting point of the polyphenylene ether resin in the presence of a radical generator, or a method in which a polyphenylene ether resin and a vinyl compound having the above-mentioned functional group are dissolved in an organic solvent, and then heated and stirred in the presence of a radical generator to react the polyphenylene ether resin. By these methods, the vinyl compound having the above-mentioned functional group can be graft-copolymerized onto the polyphenylene ether resin. In addition, in the method for producing a polyphenylene ether resin modified with an acid having a sulfo group, a method of treating the polyphenylene ether resin with a sulfonating agent can be adopted. Examples of the sulfonating agent include concentrated sulfuric acid, fuming sulfuric acid, and chlorosulfonic acid.

[0018] Examples of vinyl compounds having a sulfo group that can be used include vinyl sulfonic acid, styrene sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, 3-allyloxy-2-hydroxypropanesulfonic acid, and salts of these compounds.

[0019] Examples of vinyl compounds having a carboxy group that can be used include acrylic acid, methacrylic acid, maleic acid, fumaric acid, oleic acid, itaconic acid, citraconic acid, mesaconic acid, glutaconic acid, aconitic acid, cinnamic acid, maleic acid monoalkyl esters, fumaric acid monoalkyl esters, and salts of these compounds.

[0020] Examples of vinyl compounds having a carboxylic acid anhydride group that can be used include maleic anhydride, itaconic anhydride, aconitic anhydride, acrylic anhydride, and methacrylic anhydride.

[0021] Examples of vinyl compounds having a phosphoric acid group that can be used include vinylphosphonic acid, allylphosphonic acid, 2-hydroxyethyl methacrylic acid phosphate, and salts of these compounds.

[0022] Examples of the radical generator include organic peroxides such as di-tert-butyl peroxide, dicumyl peroxide, tert-butyl hydroperoxide, tert-butyl cumyl peroxide, benzoyl peroxide, dilauryl peroxide, cumene hydroperoxide, tert-butyl peroxybenzoate, methyl ethyl ketone peroxide, and di-tert-butyl diperphthalate, and azo compounds such as azobisisobutyronitrile. Compounds such as 2,3-dimethyl-2,3-diphenylbutane, 2,3-diethyl-2,3-diphenylbutane, 2,3-diethyl-2,3-diphenylhexane, and 2,3-diethyl-2,3-di(p-methylphenyl)butane can also be used as radical generators. These can be appropriately selected and used depending on the reaction temperature.

[0023] In the present invention, the acid value of the acid-modified polyphenylene ether resin is preferably 0.5 to 80 mgKOH / g, more preferably 1.5 to 50 mgKOH / g, even more preferably 3 to 45 mgKOH / g, and particularly preferably 5 to 25 mgKOH / g. If the acid value of the acid-modified polyphenylene ether resin is less than 0.5 mgKOH / g, it becomes difficult to obtain a dispersion of the acid-modified polyphenylene ether resin in the method described below, and the obtained hollow resin particles have poor redispersibility after drying. If the acid value of the acid-modified polyphenylene ether resin exceeds 80 mgKOH / g, the obtained hollow resin particles tend to have poor dielectric properties.

[0024] The number average molecular weight of the polyphenylene ether resin is preferably 2,000 to 100,000, more preferably 5,000 to 90,000, further preferably 8,000 to 80,000, and particularly preferably 8,000 to 55,000. If the number average molecular weight of the polyphenylene ether resin is less than 2,000, the shell strength of the obtained hollow resin particles may be poor. If the number average molecular weight of the polyphenylene ether resin is more than 100,000, the melt viscosity or solution viscosity increases during acid modification in the above method, and the operability tends to decrease.

[0025] <Vinyl resin> In the present invention, the vinyl resin is a resin obtained by polymerizing a vinyl monomer.

[0026] (Vinyl Monomer) As the vinyl monomer, known ones can be used, and examples thereof include styrene-based monomers, (meth)acrylic acid-based monomers, diene-based monomers, and (meth)acrylamide-based monomers.

[0027] The styrene-based monomer is not particularly limited, and specific examples include styrene, α-methylstyrene, ethylvinylbenzene, vinyltoluene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, vinylbiphenyl, vinylnaphthalene, and sodium p-styrenesulfonate.

[0028] The (meth)acrylic acid monomer is not particularly limited, and examples thereof include acrylic acid, methacrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, and Octyl acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate Examples of the acrylates include acrylates having the formula: acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-(diethylamino)ethyl (meth)acrylate, benzyl (meth)acrylate, allyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, 3-(trimethoxysilyl)propyl (meth)acrylate, 3-(triethoxysilyl)propyl (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, 2-(perfluorobutyl)ethyl (meth)acrylate, and glycidyl (meth)acrylate.

[0029] The diene monomer is not particularly limited, but examples thereof include butadiene, isoprene, farnesene, and myrcene.

[0030] The (meth)acrylamide monomer is not particularly limited, but examples thereof include (meth)acrylamide, N-isopropyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, and 2-(meth)acrylamide-2-methylpropanesulfonic acid.

[0031] In addition to the above vinyl monomers, any vinyl compound exhibiting polymerizability can be used without particular limitation. For example, vinylpyrrolidone, (meth)acryloylmorpholine, vinyl acetate, (meth)acrylonitrile, 1-vinylimidazole, maleic acid, fumaric acid, itaconic acid, citraconic acid, mesaconic acid, glutaconic acid, aconitic acid, cinnamic acid, maleic acid alkyl esters, fumaric acid alkyl esters, maleic anhydride, itaconic anhydride, aconitic anhydride, etc. can be used.

[0032] (Crosslinking Monomer) In the present invention, the vinyl resin preferably contains a crosslinkable monomer as a copolymerization component. The crosslinkable monomer refers to a monomer having two or more polymerizable vinyl groups in one molecule. The amount of the crosslinkable monomer in the total monomer mass constituting the vinyl resin is preferably 10% by mass or more, more preferably 25% by mass or more, even more preferably 40% by mass or more, and particularly preferably 50% by mass or more. When the vinyl resin contains 10% by mass or more of the crosslinkable monomer, the obtained hollow resin particles tend to have improved heat resistance.

[0033] The crosslinkable monomer is not particularly limited, and examples thereof include polyfunctional (meth)acrylic acid monomers such as ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, glycerin tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate; polyfunctional (meth)acrylamide monomers such as N,N'-methylene bis(meth)acrylamide and N,N'-ethylene bis(meth)acrylamide; polyfunctional allyl monomers such as diallylamine and tetraallyloxyethane; and styrene-based crosslinkable monomers such as divinylbenzene, divinylnaphthalene, and diallylphthalate. In terms of being able to more effectively exhibit the effects of the present invention, the crosslinkable monomer is preferably a styrene-based crosslinkable monomer, and more preferably divinylbenzene. The crosslinkable monomer may be one type only, or may be two or more types.

[0034] In the present invention, the vinyl resin may form a covalent bond with the acid-modified polyphenylene ether resin.

[0035] In the shell portion of the hollow resin particles of the present invention, the mass ratio (acid-modified polyphenylene ether resin / vinyl resin) is preferably 97 / 3 to 3 / 97, more preferably 85 / 15 to 15 / 85, further preferably 75 / 25 to 30 / 70, and particularly preferably 70 / 30 to 35 / 65. When the mass ratio in the shell portion of the hollow resin particles is within this range, both the dielectric properties and redispersibility are excellent.

[0036] The volume average particle diameter of the hollow resin particles of the present invention is preferably 0.1 to 50 μm, more preferably 0.1 to 20 μm, even more preferably 0.1 to 5 μm, and particularly preferably 0.1 to 2 μm. If the volume average particle diameter of the hollow resin particles is less than 0.1 μm, the thickness of the shell part becomes relatively thin, and not only may the hollow resin particles not have sufficient strength, but also may have poor redispersibility when dispersed in a resin or a resin solution. In addition, if the hollow resin particles have a volume average particle diameter of more than 50 μm, it may be difficult to make the resin material into a thin film when added to the resin material.

[0037] <Method for producing hollow resin particles> The method for producing the hollow resin particles of the present invention is not particularly limited, and examples thereof include a method comprising: (I) a step of dispersion polymerizing or emulsion polymerizing a vinyl monomer in the presence of a dispersion liquid in which particles made of an acid-modified polyphenylene ether resin are dispersed in a medium (hereinafter, referred to as an acid-modified polyphenylene ether resin dispersion liquid); and (II) a step of drying the dispersion liquid of the hollow resin particles obtained in the above (I).

[0038] The method for producing the acid-modified polyphenylene ether resin dispersion is not particularly limited, and for example, the method described in JP-A-2022-019608 can be used.

[0039] The volume average particle diameter of the particles made of the acid-modified polyphenylene ether resin is preferably 0.005 to 20 μm, more preferably 0.01 to 5 μm, further preferably 0.02 to 3 μm, and particularly preferably 0.05 to 1 μm. When the volume average particle diameter of the particles made of the acid-modified polyphenylene ether resin is within this range, hollow resin particles having a volume average particle diameter within the preferred range are easily obtained.

[0040] (Dispersion polymerization) In the present invention, the dispersion polymerization is a method in which a vinyl monomer is dissolved in a medium, and a polymerization initiator is added to the solution to polymerize the monomer. The medium used in the dispersion polymerization must dissolve the vinyl monomers used as the raw material but not dissolve the acid-modified polyphenylene ether resin or the vinyl resin produced by polymerization. The medium used in the dispersion polymerization is not particularly limited, and examples thereof include water; alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-amyl alcohol, isoamyl alcohol, sec-amyl alcohol, tert-amyl alcohol, 1-ethyl-1-propanol, 2-methyl-1-butanol, n-hexanol, and cyclohexanol; ketones such as methyl ethyl ketone, methyl isobutyl ketone, ethyl butyl ketone, cyclohexanone, and isophorone; ethers such as tetrahydrofuran and dioxane; esters such as ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, sec-butyl acetate, 3-methoxybutyl acetate, methyl propionate, ethyl propionate, diethyl carbonate, and dimethyl carbonate; ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether, glycol derivatives such as ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol ethyl ether acetate, diethylene glycol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol ethyl ether acetate, propylene glycol, propylene glycol monomethyl ether, propylene glycol monobutyl ether, and propylene glycol methyl ether acetate; amines such as N,N-dimethylethanolamine, triethylamine, N,N-diethylethanolamine, monoethanolamine, diethanolamine, triethanolamine, morpholine, and pyridine; saturated hydrocarbons such as n-pentane, n-hexane, n-heptane, and n-octane; alicyclic hydrocarbons such as cyclopentane and cyclohexane; aromatic hydrocarbons such as benzene, toluene, ethylbenzene, o-xylene, m-xylene, and p-xylene;Other examples include 3-methoxy-3-methylbutanol, 3-methoxybutanol, acetonitrile, N-methyl-2-pyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide, diacetone alcohol, ethyl acetoacetate, etc., which may be used alone or in combination of two or more kinds.

[0041] When dispersion polymerization of a vinyl monomer is carried out in the presence of an acid-modified polyphenylene ether resin dispersion, a surfactant and / or a dispersion stabilizer described below can also be used.

[0042] (Emulsion Polymerization) In the present invention, emulsion polymerization is a method in which a vinyl monomer is mixed in a medium, and a polymerization initiator is added to carry out polymerization. In the step of obtaining a dispersion of hollow resin particles by emulsion polymerization of a vinyl monomer in the presence of an acid-modified polyphenylene ether resin dispersion, it is necessary to use a medium that does not easily dissolve the vinyl monomer.

[0043] The medium used in the emulsion polymerization is not particularly limited, and examples thereof include water; alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-amyl alcohol, isoamyl alcohol, sec-amyl alcohol, tert-amyl alcohol, 1-ethyl-1-propanol, 2-methyl-1-butanol, n-hexanol, and cyclohexanol; ketones such as methyl ethyl ketone, methyl isobutyl ketone, ethyl butyl ketone, cyclohexanone, and isophorone; ethers such as tetrahydrofuran and dioxane; esters such as ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, sec-butyl acetate, 3-methoxybutyl acetate, methyl propionate, ethyl propionate, diethyl carbonate, and dimethyl carbonate; ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether, glycol derivatives such as ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol ethyl ether acetate, diethylene glycol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol ethyl ether acetate, propylene glycol, propylene glycol monomethyl ether, propylene glycol monobutyl ether, and propylene glycol methyl ether acetate; amines such as N,N-dimethylethanolamine, triethylamine, N,N-diethylethanolamine, monoethanolamine, diethanolamine, triethanolamine, morpholine, and pyridine; saturated hydrocarbons such as n-pentane, n-hexane, n-heptane, and n-octane; alicyclic hydrocarbons such as cyclopentane and cyclohexane; aromatic hydrocarbons such as benzene, toluene, ethylbenzene, o-xylene, m-xylene, and p-xylene;Other examples include 3-methoxy-3-methylbutanol, 3-methoxybutanol, acetonitrile, N-methyl-2-pyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide, diacetone alcohol, ethyl acetoacetate, etc., which may be used alone or in combination of two or more kinds.

[0044] When emulsion polymerization of a vinyl monomer is carried out in the presence of an acid-modified polyphenylene ether resin dispersion, a surfactant and / or a dispersion stabilizer described below can also be used.

[0045] (Polymerization initiator) In the present invention, the polymerization initiator used for the purpose of polymerizing the vinyl monomer is not particularly limited, and known azo compounds and peroxides can be used. For example, azo compounds include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,3-dimethylbutyronitrile), 2,2'-azobis-(2-methylbutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,3,3-trimethylbutyronitrile), ), 2,2'-azobis(2-isopropylbutyronitrile), 2,2'-azobis[N-(2-hydroxyethyl)-2-methylpropanamide], 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, and the like. Examples of peroxides include di-tert-butyl peroxide, dicumyl peroxide, tert-butyl hydroperoxide, tert-butylcumyl peroxide, benzoyl peroxide, dilauryl peroxide, cumene hydroperoxide, tert-butyl peroxybenzoate, methyl ethyl ketone peroxide, di-tert-butyl diperphthalate, cyclohexanone peroxide, diisopropylbenzene hydroperoxide, peracetic acid, sodium persulfate, potassium persulfate, and ammonium persulfate. Also, the peroxide can be used as a redox polymerization initiator in combination with a reducing agent. The reducing agent is not particularly limited, but examples thereof include alkali metal salts and ammonium salts such as sulfite, hydrogen sulfite, and pyrosulfite; carboxylic acids such as L-ascorbic acid and tartaric acid; amines such as dimethylaniline; and thiourea dioxide. These reducing agents can be used alone or in combination of two or more. The amount of the reducing agent used is preferably 1 to 1000 parts by mass per 100 parts by mass of the peroxide.

[0046] In the polymerization of the vinyl monomer, the method of adding the vinyl monomer and the polymerization initiator is not particularly limited, and they may be added all at once, may be added in several divided portions, or may be added dropwise. The polymerization atmosphere for the vinyl monomer is not particularly limited, but from the viewpoint of suppressing polymerization inhibition due to oxygen, an inert gas atmosphere such as nitrogen is preferable. The polymerization temperature of the vinyl monomer is preferably 0 to 160° C., more preferably 25 to 130° C. If the polymerization temperature is lower than 0° C., the polymerization rate may decrease, which is undesirable from the viewpoint of productivity. If the polymerization temperature exceeds 160° C., the molecular weight of the obtained vinyl resin tends to be small, which tends to decrease the strength of the shell of the obtained hollow resin particles.

[0047] (Surfactants, dispersion stabilizers) In producing the acid-modified polyphenylene ether resin dispersion and the hollow resin particle dispersion, a surfactant and / or a dispersion stabilizer can also be used. The method of using a surfactant and / or a dispersion stabilizer includes a method of including them in the medium, and a method of chemically bonding them to the acid-modified polyphenylene ether resin and / or the vinyl resin. The mode of bonding between the surfactant and the acid-modified polyphenylene ether resin and / or the vinyl-based resin is not particularly limited, and examples thereof include a mode in which a so-called reactive surfactant having a radically polymerizable vinyl group in the molecule is copolymerized with the acid-modified polyphenylene ether resin and / or the vinyl-based resin by radical polymerization. In addition, the manner in which the dispersion stabilizer is bonded to the acid-modified polyphenylene ether resin and / or the vinyl resin is not particularly limited, and examples thereof include a manner in which the dispersion stabilizer is graft-copolymerized with the acid-modified polyphenylene ether resin and / or the vinyl resin.

[0048] The surfactant includes anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants. Examples of the anionic surfactant include alkyl sulfate salts, polyoxyethylene alkyl ether sulfate salts, alkylbenzene sulfonates, alkylnaphthalene sulfonates, alkyl sulfosuccinates, alkyldiphenyl ether disulfonates, naphthalenesulfonate-formaldehyde condensates, polyoxyethylene polycyclic phenyl ether sulfate salts, polyoxyethylene distyrenated phenyl ether sulfate salts, fatty acid salts, alkyl phosphates, and polyoxyethylene alkyl phenyl ether sulfate salts. Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyalkylene alkyl ethers, polyoxyethylene polycyclic phenyl ethers, polyoxyethylene distyrenated phenyl ethers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene fatty acid esters, polyoxyethylene alkylamines, alkyl alkanolamides, and polyoxyethylene alkyl phenyl ethers. Examples of the cationic surfactant include quaternary ammonium salts such as alkyltrimethylammonium bromide, alkylpyridinium bromide, and imidazolinium laurate, pyridinium salts, and imidazolinium salts. Examples of the amphoteric surfactant include lauryl betaine and lauryl dimethylamine oxide.

[0049] Examples of reactive surfactants include polyoxyethylene alkyl ether sulfates (e.g., Aqualon KH-05, KH-10, and KH-20 manufactured by Daiichi Kogyo Seiyaku Co., Ltd., Adeka Reasoap SR-10N and SR-20N manufactured by ADEKA Corporation, and Latemul PD-104 manufactured by Kao Corporation), polyoxyalkylene styrenated phenyl ether sulfates (e.g., Aqualon AR-10 and AR-20 manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), sulfosuccinates (e.g., Latemul S-120, S-120A, S-180P, and S-180P manufactured by Kao Corporation), and the like. 80A, Eleminol JS-2 manufactured by Sanyo Chemical Industries, etc.), polyoxyethylene alkylphenyl ether sulfates or polyoxyethylene alkylphenyl ester sulfates (e.g., Aqualon HS-10, HS-20, HS-30, BC-10, BC-20 manufactured by Daiichi Kogyo Seiyaku Co., Ltd., Adeka Reasoap SDX-222, SDX-223, SDX-232, SDX-233, SDX-259, SE-10N, SE-20N manufactured by ADEKA Corporation, etc.), (meth)acrylate sulfates (e.g., Adeka Reasoap SDX-222, SDX-223, SDX-232, SDX-233, SDX-259, SE-10N, SE-20N manufactured by Nippon Nyukazai Co., Ltd., etc.), Examples of the anionic reactive surfactant include anionic reactive surfactants such as phosphate esters (e.g., H-3330PL manufactured by Daiichi Kogyo Seiyaku Co., Ltd., and Adeka Reasoap PP-70 manufactured by ADEKA Corporation), polyoxyethylene alkyl ethers (e.g., Adeka Reasoap ER-10, ER-20, ER-30, ER-40 manufactured by ADEKA Corporation, and Latemul PD-420, PD-430, PD-450 manufactured by Kao Corporation), polyoxyalkylene styrenated phenyl ethers (e.g., Adeka Reasoap ER-10, ER-20, ER-30, ER-40 manufactured by ADEKA Corporation, and Latemul PD-420, PD-430, PD-450 manufactured by Kao Corporation), and polyoxyalkylene styrenated phenyl ethers. and nonionic reactive surfactants such as ether-based surfactants (e.g., AQUALON AN-10, AN-20, etc., manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), polyoxyethylene alkylphenyl ether-based or alkylphenyl ester-based surfactants (e.g., AQUALON RN-10, RN-20, RN-30, RN-50, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., and ADEKA REASOAP NE-10, NE-20, NE-30, NE-40, etc., manufactured by ADEKA Corporation), and (meth)acrylate sulfate-based surfactants (e.g., RMA-564, RMA-568, RMA-1114, manufactured by Nippon Nyukazai Co., Ltd.).

[0050] Examples of the dispersion stabilizer include, but are not limited to, polyether, polyvinyl alcohol, polyvinylpyrrolidone, poly(vinylpyrrolidone-vinyl acetate) copolymer, polyacrylic acid, starch, gum arabic, gum tragacanth, casein, gelatin, dextrin, carboxylated starch, cationized starch, dextrin, ethyl cellulose, carboxylated methyl cellulose, hydroxyethyl cellulose, and cationized cellulose.

[0051] The above surfactants and dispersion stabilizers can be used alone or in combination of two or more kinds. EXAMPLES

[0052] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these. (1) Number average molecular weight of (acid-modified) polyphenylene ether resin The number average molecular weight was measured by gel permeation chromatography (GPC) in terms of standard polystyrene. GPC measurements were performed using Shodex LF-804×2 (manufactured by Resonac) as the column, chloroform at 50°C as the eluent, and an RI (refractometer) as the detector, and the number average molecular weight was calculated from the relationship between the molecular weight of the standard polystyrene sample measured under the same conditions and the elution time.

[0053] (2) Acid value of acid-modified polyphenylene ether resin 0.15 g of the acid-modified polyphenylene ether resin was refluxed in 20 mL of tetrahydrofuran (THF), and after confirming that the resin was completely dissolved, the temperature of the solution was maintained at 60°C while stirring. A few drops of cresol red indicator were added to the THF solution of the acid-modified polyphenylene ether resin, and the solution was titrated with a 0.1 mol / L solution of potassium hydroxide in methanol. The acid value of the polyphenylene ether resin was calculated from the titration amount.

[0054] (3) Volume average particle size of particles made of acid-modified polyphenylene ether resin and hollow resin particles The volume average particle size was determined using a Microtrac particle size distribution analyzer UPA150 (Model No. 9340) manufactured by Nikkiso Co., Ltd. The refractive index of the resin used to calculate the volume average particle size was set to 1.50.

[0055] (4) Redispersibility Polyarylate resin (UNIFINER M-2000H manufactured by Unitika Ltd.) was dissolved in cyclohexanone to a concentration of 15% by mass. 0.6 g of each of the hollow resin particles obtained in the Examples and Comparative Examples was added to 15 g of the cyclohexanone solution of this polyarylate resin, and the mixture was degassed and stirred using a planetary centrifugal mixer (ARE-250 manufactured by THINKY Corporation) to prepare a coating material. The prepared coating material was applied to a 5 mm thick glass plate using an applicator to a wet thickness of 120 μm, and then heated at 160° C. for 40 minutes to remove cyclohexanone. After cooling to room temperature, the obtained dried coating film was visually observed, and the coating film was measured at a thickness of 100 cm 2 The number of convex bumps per square inch was counted. Based on the number of bumps, the redispersibility of the hollow resin particles added to the resin material was evaluated according to the following criteria. ◎: 3 or less (best redispersibility) ○: 4 to 6 or less (better than redispersibility) △: 7~9 pieces (good redispersibility) ×: 10 or more (poor redispersibility)

[0056] (5) Dielectric constant The coating material prepared in (4) above was applied to a 5 mm thick glass plate using an applicator to a wet thickness of 250 μm, and then heated at 160° C. for 40 minutes to remove cyclohexanone. After cooling to room temperature, the dielectric constant of the resulting film was measured by a cavity resonance method (measurement frequency: 5 GHz). The dielectric constant of the film that did not contain hollow resin particles was measured and found to be 2.6.

[0057] (6) Heat resistance The heat resistance was evaluated by measuring the 5% thermal weight loss temperature using a differential thermal and thermogravimetric simultaneous measurement device (TG / DTA6200, AST-2, manufactured by SII NanoTechnology Co., Ltd.). The sampling method and temperature conditions were as follows. The bottom of a platinum measuring container was packed with 10.5±0.5 mg of hollow resin particles without gaps to prepare a measurement sample. The 5% thermal weight loss temperature was measured using alumina as a reference material under a nitrogen gas flow rate of 230 mL / min. The TG / DTA curve was obtained by heating the sample from 30°C to 500°C at a heating rate of 10°C / min. The temperature at 5% weight loss was calculated from the obtained curve using the analysis software attached to the device, and the heat resistance was evaluated.

[0058] Synthesis Example 1: Acid-modified polyphenylene ether resin (P-1) 50 g of polyphenylene ether resin (A) (number average molecular weight 33,000), 10 g of maleic anhydride, and 318 g of xylene were charged into a separable flask equipped with a stirrer and a reflux condenser, and the system was replaced with nitrogen, and then heating and stirring were started in a 140°C oil bath. After confirming that the polyphenylene ether resin and maleic anhydride had dissolved, 40 g of a xylene solution of dicumyl peroxide (20 mass%, previously replaced with nitrogen) was dropped into the separable flask over 30 minutes. After completion of the dropwise addition, the reaction was continued for 5 hours in a nitrogen atmosphere while maintaining the reflux state, and stirring was continued. After completion of the reaction, the obtained solution was poured into a large amount of methanol to precipitate the resin. This resin was washed several times with acetone to remove unreacted maleic anhydride and decomposition products of dicumyl peroxide, and then dried under reduced pressure in a vacuum dryer to obtain a polyphenylene ether resin (P-1) modified with a carboxylic acid anhydride group. The acid value of the resulting acid-modified polyphenylene ether resin (P-1) was 18.5 mg / KOH, and the number average molecular weight was 29,000.

[0059] Synthesis Example 2: Acid-modified polyphenylene ether resin (P-2) 50 g of polyphenylene ether resin (A) (number average molecular weight 33,000), 10 g of fumaric acid, and 334 g of xylene were charged into a separable flask equipped with a stirrer and a reflux condenser, and the system was replaced with nitrogen, and then heating and stirring were started in a 140°C oil bath. After confirming that the polyphenylene ether resin and fumaric acid had dissolved, 40 g of a xylene solution of dicumyl peroxide (20 mass%, previously replaced with nitrogen) was dropped into the separable flask over 30 minutes. After completion of the dropwise addition, the reaction was carried out by continuing stirring for 5 hours in a nitrogen atmosphere while maintaining the reflux state. After the reaction was completed, the obtained solution was poured into a large amount of methanol to precipitate the resin. This resin was washed several times with acetone to remove unreacted fumaric acid and decomposition products of dicumyl peroxide, and then dried under reduced pressure in a vacuum dryer to obtain a polyphenylene ether resin (P-2) modified with a carboxy group. The acid value of the resulting acid-modified polyphenylene ether resin was 17.2 mg / KOH and the number average molecular weight was 28,000.

[0060] Synthesis Example 3: Acid-modified polyphenylene ether resin (P-3) A carboxy-modified polyphenylene ether resin (P-3) was obtained in the same manner as in Synthesis Example 2, except that the amount of fumaric acid was changed from 10 g to 0.8 g. The acid value of the obtained acid-modified polyphenylene ether resin was 0.4 mg / KOH, and the number average molecular weight was 27,000.

[0061] Synthesis Example 4: Acid-modified polyphenylene ether resin (P-4) 50 g of polyphenylene ether resin (B) (number average molecular weight 18,000) and 1000 g of orthodichlorobenzene were charged into a separable flask equipped with a stirrer, and heating and stirring were started in a 90°C oil bath. After confirming that the polyphenylene ether resin had dissolved, the temperature of the system was cooled to 40°C, and a mixed solution of 15 g of chlorosulfonic acid and 23 g of sulfolane was dropped into the separable flask over 30 minutes. After completion of the dropwise addition, the reaction was carried out by continuing stirring for 4.5 hours while maintaining the system at 40°C. After completion of the reaction, the obtained solution was poured into a large amount of methanol to precipitate the resin. This resin was washed several times with water, and then dried under reduced pressure in a vacuum dryer to obtain a polyphenylene ether resin (P-4) modified with a sulfo group. The acid value of the obtained acid-modified polyphenylene ether resin was 30.5 mg / KOH, and the number average molecular weight was 16,000.

[0062] Preparation Example 1: Dispersion (E-1) of Acid-Modified Polyphenylene Ether Resin (P-1) Using a stirrer equipped with a sealable pressure-resistant 1 L glass container equipped with a heater and a pressure gauge, 30 g of acid-modified polyphenylene ether resin (P-1), 108 g of tetrahydrofuran, 3 g of triethylamine and 159 g of pure water were charged into the glass container, and the system was sealed. Then, the stirring blade was rotated at a speed of 350 rpm, and the heater was turned on to heat. After confirming that the temperature in the system reached 120°C, the mixture was stirred for 60 minutes while maintaining the temperature at 120°C. At this time, the pressure gauge indicated 0.41 MPa. After that, the temperature was lowered to 50°C while stirring at a rotation speed of 350 rpm by air cooling, and 200 g of pure water was added. This dispersion was cooled to room temperature, and the liquid components in the glass container were filtered with a stainless steel filter (78 mesh plain weave) to obtain a milky white dispersion (E-1) of acid-modified polyphenylene ether resin (P-1). The volume average particle size of the acid-modified polyphenylene ether resin (P-1) in this dispersion was 0.14 μm.

[0063] Preparation Example 2A: Dispersion (E-2A) of Acid-Modified Polyphenylene Ether Resin (P-2) A dispersion (E-2A) of the acid-modified polyphenylene ether resin (P-2) was obtained in the same manner as in Preparation Example 1, except that the acid-modified polyphenylene ether resin (P-2) was used. The volume average particle size of the acid-modified polyphenylene ether resin (P-2) in this dispersion was 0.15 μm.

[0064] Preparation Example 2B: Dispersion of Acid-Modified Polyphenylene Ether Resin (P-2) (E-2B) A dispersion (E-2B) of an acid-modified polyphenylene ether resin (P-2) was obtained in the same manner as in Preparation Example 2A, except that the amount of triethylamine was changed from 3 g to 1.2 g and the amount of pure water was changed from 159 g to 160.8 g. The volume average particle size of the acid-modified polyphenylene ether resin (P-2) in this dispersion was 0.25 μm.

[0065] Preparation Example 3: Dispersion (E-3) of acid-modified polyphenylene ether resin (P-3) A dispersion (E-3) of the acid-modified polyphenylene ether resin (P-3) was obtained in the same manner as in Preparation Example 1, except that the acid-modified polyphenylene ether resin (P-3) was used. The volume average particle size of the acid-modified polyphenylene ether resin (P-3) in this dispersion was 0.58 μm.

[0066] Preparation Example 4A: Dispersion of Acid-Modified Polyphenylene Ether Resin (P-4) (E-4A) A dispersion (E-4A) of the acid-modified polyphenylene ether resin (P-4) was obtained in the same manner as in Preparation Example 1, except that the acid-modified polyphenylene ether resin (P-4) was used. The volume average particle size of the acid-modified polyphenylene ether resin (P-4) in this dispersion was 0.11 μm.

[0067] Preparation Example 4B: Dispersion of Acid-Modified Polyphenylene Ether Resin (P-4) (E-4B) A dispersion (E-4B) of an acid-modified polyphenylene ether resin (P-4) was obtained in the same manner as in Preparation Example 4A, except that the amount of triethylamine was changed from 3 g to 6 g and the amount of pure water was changed from 159 g to 156 g. The volume average particle size of the acid-modified polyphenylene ether resin (P-4) in this dispersion was 0.07 μm.

[0068] Preparation Example 5: Dispersion of polyphenylene ether resin (E-5) 3 g of polyphenylene ether resin (B) (number average molecular weight 18,000) was heated and dissolved in 27 g of toluene to prepare an oil phase. Next, 0.15 g of sodium dodecyl sulfate and 200 g of pure water were mixed to prepare an aqueous phase. The oil phase was added to the aqueous phase, and the mixture was treated with an ultrasonic homogenizer (manufactured by Hielscher) for 5 minutes to prepare a dispersion. 150 g of pure water was added to this dispersion, and the entire amount was transferred to an eggplant flask, and the pressure was reduced using an evaporator while the flask was placed in a hot water bath, and the toluene was distilled off and the dispersion was concentrated at the same time. The obtained dispersion was cooled to room temperature, and the liquid components in the eggplant flask were filtered with a stainless steel filter (78 mesh plain weave) to obtain a milky white dispersion (E-5) of polyphenylene ether resin (B). The volume average particle size of the polyphenylene ether resin (B) in this dispersion was 0.23 μm.

[0069] Example 1 In a Schlenk flask containing a stirrer bar, 20.83 g of the dispersion (E-1) of the acid-modified polyphenylene ether resin (P-1), 0.75 g of divinylbenzene (DVB-810 manufactured by Nippon Steel Chemical & Material Co., Ltd., purity 81%), 0.1 g of sodium dodecyl sulfate, and 3.67 g of pure water were charged, and the system was replaced with nitrogen. After sealing the Schlenk flask with a septum rubber, the mixture was heated in a 70°C oil bath and stirred with a magnetic stirrer for 60 minutes. Next, 0.52 g of an aqueous solution of ammonium persulfate (4% by mass, previously replaced with nitrogen) was added to the Schlenk flask in one go, and emulsion polymerization was carried out for 24 hours by stirring while maintaining the system at 70°C. Thereafter, the liquid components in the Schlenk flask were cooled to room temperature and diluted with pure water, and the solid matter was collected by centrifugation, and the obtained solid matter was redispersed in pure water. This series of steps consisting of centrifugation and redispersion of the obtained solid matter in pure water was repeated three times to obtain a dispersion of hollow resin particles (H-1). The volume average particle diameter of the hollow resin particles (H-1) in this dispersion was 0.19 μm. The obtained dispersion liquid was dried at 80° C. to obtain hollow resin particles (H-1).

[0070] Example 2 Except for using the dispersion (E-2A) of the acid-modified polyphenylene ether resin (P-2), a dispersion of hollow resin particles (H-2A) was obtained in the same manner as in Example 1. The volume average particle diameter of the hollow resin particles (H-2A) in this dispersion was 0.21 μm. The obtained dispersion liquid was dried at 80° C. to obtain hollow resin particles (H-2A).

[0071] Example 3 Except for using the dispersion (E-2B) of the acid-modified polyphenylene ether resin (P-2), a dispersion of hollow resin particles (H-2B) was obtained in the same manner as in Example 1. The volume average particle diameter of the hollow resin particles (H-2B) in this dispersion was 0.37 μm. The obtained dispersion liquid was dried at 80° C. to obtain hollow resin particles (H-2B).

[0072] Example 4 Except for using the dispersion (E-3) of the acid-modified polyphenylene ether resin (P-3), a dispersion of hollow resin particles (H-3) was obtained in the same manner as in Example 1. The volume average particle diameter of the hollow resin particles (H-3) in this dispersion was 0.78 μm. The obtained dispersion liquid was dried at 80° C. to obtain hollow resin particles (H-3).

[0073] Example 5 Except for using the dispersion (E-4A) of the acid-modified polyphenylene ether resin (P-4), a dispersion of hollow resin particles (H-4A) was obtained in the same manner as in Example 1. The volume average particle diameter of the hollow resin particles (H-4A) in this dispersion was 0.15 μm. The obtained dispersion liquid was dried at 80° C. to obtain hollow resin particles (H-4A).

[0074] Example 6 Except for using the dispersion (E-4B) of the acid-modified polyphenylene ether resin (P-4), a dispersion of hollow resin particles (H-4B) was obtained in the same manner as in Example 1. The volume average particle diameter of the hollow resin particles (H-4B) in this dispersion was 0.09 μm. The obtained dispersion liquid was dried at 80° C. to obtain hollow resin particles (H-4B).

[0075] Comparative Example 1 A dispersion of resin particles (H-5) was obtained in the same manner as in Example 1, except that 20.83 g of the dispersion (E-5) of polyphenylene ether resin (B), 0.75 g of divinylbenzene (DVB-810, purity 81%, manufactured by Nippon Steel Chemical & Material Co., Ltd.) and 3.67 g of pure water were charged into a Schlenk flask containing a stirrer bar. The volume average particle diameter of the resin particles (H-5) in this dispersion was 0.28 μm. The resulting dispersion was dried at 80° C. to obtain resin particles (H-5).

[0076] Comparative Example 2 An oil phase was prepared by mixing 1.5 g of a bifunctional polyphenylene ether oligomer (product name "OPE-2St 1200", manufactured by Mitsubishi Gas Chemical Co., Ltd.), 1.5 g of 81% purity divinylbenzene (DVB-810, manufactured by Nippon Steel Chemical & Material Co., Ltd.), 3.0 g of n-heptane, and 0.09 g of Perloyl L (manufactured by NOF Corporation) as a polymerization initiator. Next, 34 g of ion-exchanged water and 0.0128 g of Rapisol A-80 (NOF Corp.) were mixed to prepare an aqueous phase. The oil phase was added to the aqueous phase, and a suspension was prepared using an ultrasonic homogenizer (BRANSON Corp., "SONIFIER450", conditions: Duty Cycle = 50%, Output Control = 5, processing time 3 minutes). The resulting suspension was heated at 70°C for 4 hours to carry out a reaction. After the reaction, the suspension was cooled to room temperature to obtain a dispersion of hollow resin particles. The volume average particle diameter of this dispersion was measured, and was found to be 0.27 μm. The obtained dispersion liquid was dried at 80° C. to obtain hollow resin particles (H-6).

[0077] Table 1 shows the configurations and characteristics of the shell portions of the hollow resin particles of the examples and the configurations and characteristics of the resin particles of the comparative examples. The particles obtained in the examples and comparative examples were cross-sectionally prepared by ion milling, platinum was deposited, and the particles were observed using a field emission scanning electron microscope (SEM-8020, Hitachi Technologies). It was found that the particles obtained in the examples and comparative example 2 all had hollow regions. On the other hand, the particles obtained in comparative example 1 did not have hollow regions.

[0078] [Table 1]

[0079] The hollow resin particles of the Examples had excellent redispersibility because the polyphenylene ether resin constituting the shell was acid-modified, whereas the resin particles of the Comparative Examples had poor redispersibility because the polyphenylene ether resin constituting the particles was not acid-modified with a specific functional group, and the resin particles of Comparative Example 1 did not have a hollow portion.

Claims

1. A hollow resin particle having a shell portion and a hollow portion surrounded by the shell portion, the shell portion is made of an acid-modified polyphenylene ether resin and a vinyl resin, 1. A hollow resin particle comprising an acid-modified polyphenylene ether resin, the polyphenylene ether resin being acid-modified with at least one functional group selected from the group consisting of a sulfo group, a carboxy group, a carboxylic anhydride group, and a phosphoric acid group.

2. 2. The hollow resin particle according to claim 1, wherein the acid-modified polyphenylene ether resin has an acid value of 0.5 to 80 mgKOH / g.

3. 3. The hollow resin particles according to claim 1, wherein the volume average particle diameter is 0.1 to 50 μm.

4. 3. The hollow resin particle according to claim 1, wherein the vinyl resin contains a crosslinkable monomer as a copolymerization component.

5. 5. The hollow resin particle according to claim 4, wherein the crosslinkable monomer as a copolymerization component is at least one selected from the group consisting of divinylnaphthalene, diallyl phthalate, and divinylbenzene.

6. A hollow resin particle dispersion comprising the hollow resin particles according to claim 1 or 2 and a medium.

7. A method for producing the hollow resin particles according to claim 1, comprising the following steps (I) and (II): (I) A step of dispersion polymerizing or emulsion polymerizing a vinyl monomer in the presence of a dispersion liquid in which particles made of an acid-modified polyphenylene ether resin are dispersed in a medium. (II) A step of drying the dispersion obtained in (I) above.

Citation Information

Patent Citations

  • Hollow polymer fine particle and method for producing the same

    JP2002080503A

  • Resin particle

    JP2020033503A

  • Hollow resin particles, method for producing hollow resin particles, and use of hollow resin particles

    WO2022131127A1

Cited By

  • Hollow particles and use thereof

    WO2026186325A1