ORGANIC SLURRY FOR NdFeB SILK SCREEN PRINTING AND PREPARATION METHOD

The organic slurry for NdFeB silk screen printing, with a specific composition and preparation method, addresses particle agglomeration and stability issues, enhancing printing uniformity and product quality.

JP2024159556AInactive Publication Date: 2024-11-08GRIREM ADVANCED MATERIALS CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024064144
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-11
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional methods for preparing NdFeB slurry for silk screen printing face issues such as particle agglomeration, low dispersion efficiency, and poor storage stability, which affect printing uniformity and product quality.

Method used

An organic slurry composition for NdFeB silk screen printing comprising rare earth powder, organic solvent, resin, dispersant, and leveling agent, with specific weight percentages and preparation steps involving stirring, high-speed dispersion, and polishing to achieve uniformity and stability.

Benefits of technology

The prepared slurry exhibits excellent dispersibility, stability, and adhesion, ensuring consistent weight gain and uniform film thickness during silk screen printing, thereby improving the quality and efficiency of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159556000001_ABST
    Figure 2024159556000001_ABST
Patent Text Reader

Abstract

To provide an organic slurry for NdFeB silk screen printing which is excellent in dispersibility and stability, and stabilizes increase in weight of printing, and a preparation method of the same.SOLUTION: An organic slurry contains rare earth powder, an organic solvent and a resin, and further contains a dispersion agent and / or a leveling agent, wherein as a weight percentage of each component, the rare earth powder is 50 to 90%, the organic solvent is 8 to 50%, the resin is 0.4 to 6%, the dispersion agent is 0 to 5%, and the leveling agent is 0 to 3%. A preparation method includes the steps of: successively adding the weighed organic solvent, resin, dispersion agent and / or leveling agent to a stirrer, stirring the mixture under a constant temperature condition, then cooling the mixture to a room temperature, and obtaining an organic carrier; adding the organic carrier and the weighed rare earth powder to a vacuum high speed dispersing machine, dispersing the mixture at a high speed, and obtaining a coarse organic slurry; and moving the coarse organic slurry to three roll mills capable of adjusting its interval, polishing the coarse organic slurry, and obtaining a fine organic slurry.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of silk screen printing, especially to an organic slurry and preparation method for NdFeB silk screen printing. [Background technology]

[0002] Since its discovery in the 1980s, neodymium iron boron (NdFeB) permanent magnet material has been widely applied in many fields such as electronic information and medical industries due to its excellent performance such as high residual magnetic flux density, high coercive force and maximum electric energy product. In recent years, in order to meet the performance requirements of neodymium sintered magnets for new energy vehicle drive motors and direct drive permanent magnet wind generators, it is generally necessary to carry out grain boundary diffusion treatment on magnets to improve their coercive force. In conventional grain boundary diffusion, heavy rare earth elements, fluorides, hydrides, oxides and alloys are used as diffusion sources, and the diffusion sources are often coated on the surface of magnets by sputtering, deposition, electrophoresis, surface coating and immersion. The above diffusion sources have low diffusion efficiency, large consumption, and lack a low-cost grain boundary diffusion process suitable for large-scale and stable industrialized production, which restricts the development and popularization of high-end neodymium magnets.

[0003] In order to make up for the shortcomings of existing grain boundary diffusion methods, silk screen printing technology has been applied to the NdFeB industry. Silk screen printing is a method of using a screen stencil and a slurry to print on the substrate by passing the slurry through the holes in the stencil with a squeegee. Silk screen printing combines the advantages of both sputtering and surface coating methods, and has the characteristics of low cost, high production efficiency, and ease of realizing automated production. It is expected to develop into the mainstream process of NdFeB grain boundary diffusion. The slurry is the raw material of silk screen printing, which directly affects the printing and subsequent diffusion effects.

[0004] In the prior art, the method of preparing a slurry is mainly to disperse rare earth powder in an organic solution such as alcohol / acetone by stirring. The powder particles have a particle size of less than 10 μm, and are very susceptible to particle aggregation due to electrostatic attraction between particles, surface tension, etc., which results in the presence of large particles in the organic slurry, which is unfavorable to the storage stability and printing uniformity of the organic slurry. In addition, the conventional dispersion method only uses a stirrer to carry out the dispersion process, which generally faces problems such as low dispersion effect, long dispersion time, and large amount of bubbles, which seriously affects the performance of the organic slurry and the quality of silk screen printing. Summary of the Invention

[0005] The present invention aims to provide an organic slurry and preparation method for NdFeB silk screen printing, which can be used to solve at least one of the above technical problems, and the prepared slurry has excellent dispersibility, stability, and stable weight gain of printing.

[0006] An embodiment of the present invention is implemented as follows. An organic slurry for NdFeB silk screen printing, comprising rare earth powder, an organic solvent and a resin, further comprising a dispersing agent and / or a leveling agent, the weight percentage of each component being: The rare earth powder is 50% to 90%. The organic solvent is 8% to 50%. Resin is 0.4% to 6%. Dispersant is 0% to 5%. The leveling agent content is 0% to 3%.

[0007] In a preferred embodiment of the present invention, in the organic slurry for NdFeB silk screen printing, the rare earth powder comprises one or more mixtures of heavy rare earth element pure metal powder, alloy powder containing heavy rare earth element or light rare earth element, heavy rare earth powder containing heavy rare earth hydride, fluoride and oxide.

[0008] In a preferred embodiment of the present invention, in the organic slurry for NdFeB silk screen printing, the heavy rare earth elements include one or a mixture of two or more of Tb, Dy, Ho, and Gd.

[0009] The composition of the alloy powder in mass percentage is RE x M y where RE is a mixture of one or more of Tb, Dy, Ho, Gd, Pr, Nd, La, Ce, and Y, M is a mixture of one or more of Ga, Cu, Al, Ni, and Fe, and 60%≦x≦95% and 5%≦y≦40%. In a preferred embodiment of the present invention, in the organic slurry for NdFeB silk screen printing, the particle size of the rare earth powder is D50<2μm.

[0010] In a preferred embodiment of the present invention, in the organic slurry for NdFeB silk screen printing, the organic solvent comprises one or a mixture of two or more of butyl carbitol, 2-(2-butoxyethoxy)ethyl acetate, N-methylpyrrolidone, Texanol, propylene glycol phenyl ether, 2-acetoxy-1-methoxypropane and DBE.

[0011] In a preferred embodiment of the present invention, in the organic slurry for NdFeB silk screen printing, the resin comprises one or a mixture of two or more of polyvinylidene fluoride, nitrocellulose, ethyl cellulose, polyvinyl butyral, acrylic resin, polyester resin and polyurethane.

[0012] The technical effects are as follows: by adding the resin, not only can the viscosity of the organic slurry itself be improved, which contributes to improving the dispersion and stability of the organic slurry, but also the adhesion of the organic slurry to the substrate can be improved, thereby ensuring the subsequent grain boundary diffusion effect.

[0013] In a preferred embodiment of the present invention, in the organic slurry for NdFeB silk screen printing, the dispersant includes one or a mixture of two or more of butyl acetate, modified polyurethane polymer, polyethylene glycol, polyvinylpyrrolidone and polyethylene amide.

[0014] Its technical effects are as follows: the dispersant can prevent the rare earth powder from re-agglomerating in the organic slurry, reduce the fineness of the organic slurry itself, and improve the consistency of weight gain during silk screen printing.

[0015] In a preferred embodiment of the present invention, in the organic slurry for NdFeB silk screen printing, the leveling agent includes one or a mixture of two or more of silicone, acrylate, modified acrylic acid and polyacrylic acid.

[0016] Its technical effects are as follows: the leveling agent is especially applied to high viscosity organic slurry such as high content of rare earth powder / high content of resin, etc., thereby improving its leveling property and ensuring the uniformity of the thickness of the film layer after silk screen printing.

[0017] In a preferred embodiment of the present invention, the organic slurry for NdFeB silk screen printing contains the following components in weight percentage: The pure metal powder is 60% to 80%. One or more of butyl carbitol, 2-(2-butoxyethoxy)ethyl acetate, and DBE is 10% to 30%; One or more of ethyl cellulose, acrylic resin, and polyvinyl butyral is 0.4% to 5%; One or two of polyethylene glycol and butyl acetate are 0% to 3%; One or more of acrylate, polyacrylic acid, and silicone is 0% to 1.5%.

[0018] In a preferred embodiment of the present invention, the organic slurry for NdFeB silk screen printing contains the following components in weight percentage: The alloy powder is 60% to 80%. One or more of butyl carbitol, propylene glycol phenyl ether, and DBE is 10% to 30%; One or more of polyester resin, ethyl cellulose, and acrylic resin is 0.4% to 3%; One or two of polyethyleneamide and polyvinylpyrrolidone are 0% to 3%; One or both of the modified acrylic acid and acrylate are 0% to 1.5%.

[0019] In a preferred embodiment of the present invention, the organic slurry for NdFeB silk screen printing contains the following components in weight percentage: Heavy rare earth powder is 60% to 80%; One or more of butyl carbitol, 2-(2-butoxyethoxy)ethyl acetate, and propylene glycol phenyl ether are 10% to 30%; One or more of polyvinyl butyral, ethyl cellulose, and polyurethane are 0.4% to 5%; One or two of butyl acetate and polyethylene glycol are 0% to 3%; One or both of polyacrylic acid and acrylate is 0% to 1.5%.

[0020] A method for preparing organic slurry for NdFeB silk screen printing as above, the method for preparing includes the following steps:

[0021] The rare earth powder, organic solvent, resin, dispersant and / or leveling agent are each weighed out in weight percentage.

[0022] The weighed organic solvent, resin, dispersant and / or leveling agent are added in this order to a stirrer, and stirred at a constant temperature of 20 to 70°C and a rotation speed of 600 r / min to 1200 r / min for 0.1 to 6 hours, and then cooled to room temperature to obtain an organic carrier.

[0023] Its technical effect is as follows: the organic carrier produced is homogeneous and free of flocculent material.

[0024] The organic carrier and the weighed rare earth powder are added to a vacuum high-speed disperser and dispersed at high speed at a rotation speed of 1000 r / min to 4000 r / min for 0.25 to 1 hour to obtain a crude organic slurry.

[0025] Its technical effect is as follows: the crude organic slurry prepared is bubble-free and uniformly dispersed.

[0026] The coarse organic slurry is transferred to a three-roll mill with adjustable gap and polished 1 to 3 times to obtain a fine organic slurry.

[0027] Its technical effect is that the fineness of the prepared fine organic slurry is less than 2.5 μm.

[0028] The beneficial effects of the embodiments of the present invention are as follows: The organic slurry for NdFeB silk screen printing prepared according to the present invention is prepared by suitably selecting the organic carrier, and by relying on the strong mechanical action of the vacuum high-speed disperser and the three-roll mill, the powder particles aggregated by the high-speed shearing action and grinding are dispersed, so that the organic slurry has high dispersibility and suspension stability. The fineness of the prepared slurry is less than 2.5 μm, the monthly settling rate of the slurry is less than 5%, and the consistency of the weight gain during printing is less than ±5%. The prepared slurry has excellent dispersibility and stability. [Brief description of the drawings]

[0029] In order to more clearly describe the technical solutions of the embodiments of the present invention, the following briefly describes the drawings required for use in the embodiments. The following drawings only show some embodiments of the present invention, so they should not be considered as limiting the scope, and it should be understood that those skilled in the art can further conceive other related drawings based on these drawings without creative efforts. [Figure 1] FIG. 1 is a flow diagram of the method for preparing organic slurry for NdFeB silk screen printing according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] In order to make the objectives, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be described clearly and completely below with reference to the drawings in the embodiments of the present invention, and it should be understood that the described embodiments are only a part of the embodiments of the present invention, and are not all of the embodiments. Generally, the assemblies of the embodiments of the present invention described and shown in the drawings herein can be arranged and configured in various arrangement manners.

[0031] An embodiment of the present invention provides an organic slurry for NdFeB silk screen printing, which includes rare earth powder, an organic solvent and a resin, and further includes a dispersing agent and / or a leveling agent, the weight percentage of each component being: The rare earth powder is 50% to 90%. The organic solvent is 8% to 50%. Resin is 0.4% to 6%. Dispersant is 0% to 5%. The leveling agent content is 0% to 3%.

[0032] In a preferred embodiment of the present invention, in the organic slurry for NdFeB silk screen printing, the rare earth powder comprises one or more mixtures of heavy rare earth element pure metal powder, alloy powder containing heavy rare earth element or light rare earth element, heavy rare earth powder containing heavy rare earth hydride, fluoride and oxide.

[0033] In a preferred embodiment of the present invention, in the organic slurry for NdFeB silk screen printing, the heavy rare earth elements include one or a mixture of two or more of Tb, Dy, Ho, and Gd.

[0034] The composition of the alloy powder in mass percentage is RE x M y where RE is a mixture of one or more of Tb, Dy, Ho, Gd, Pr, Nd, La, Ce, and Y, M is a mixture of one or more of Ga, Cu, Al, Ni, and Fe, and 60%≦x≦95% and 5%≦y≦40%.

[0035] In a preferred embodiment of the present invention, in the organic slurry for NdFeB silk screen printing, the heavy rare earth elements include one or a mixture of two of Tb and Dy.

[0036] The composition of the alloy powder in mass percentage is RE x M y where RE is one or more of Tb, Dy, Pr, and Nd. When RE is Tb, M is one or more of Ga, Cu, Al, and Ni, and 70≦x≦90 and 10≦y≦30. When RE is Dy, M is one or more of Ni, Fe, and Ga, and 60≦x≦80 and 20≦y≦40. When RE is two or three of Tb, Pr, and Nd, M is one or two of Cu and Al, and 80≦x≦95 and 5≦y≦20. The addition of the above alloying elements can lower the melting point of the diffusion source and change the diffusion from solid-liquid diffusion to liquid-liquid diffusion, thereby significantly improving the diffusion efficiency. In addition, after diffusing into the magnet, the alloying elements are often distributed at the grain boundaries, which can reduce the magnetic exchange coupling between the crystal grains.

[0037] In a preferred embodiment of the present invention, in the organic slurry for NdFeB silk screen printing, the particle size of the rare earth powder is D50<2μm.

[0038] Preferably, the particle size of the diffusion source powder satisfies 1.6 < D50 < 1.8. When the particle size of the powder is within this range, excellent stability can be obtained, and the powder preparation efficiency will not be significantly reduced due to an overly small particle size of the powder.

[0039] In a preferred embodiment of the present invention, in the organic slurry for the NdFeB silk screen printing, the organic solvent includes one or a mixture of two or more of butyl carbitol, 2-(2-butoxyethoxy)ethyl acetate, N-methylpyrrolidone, texanol, propylene glycol phenyl ether, 2-acetoxy-1-methoxypropane, and DBE.

[0040] Preferably, the organic solvent is one or a mixture of two or more of butyl carbitol, 2-(2-butoxyethoxy)ethyl acetate, propylene glycol phenyl ether, 2-acetoxy-1-methoxypropane, and DBE. The above organic solvent is easy to volatilize at high temperatures, thereby improving the drying efficiency after silk screen printing, reducing impurities such as C and O that enter the interior of the magnet during grain boundary diffusion, and ensuring the performance of the magnet after diffusion.

[0041] In a preferred embodiment of the present invention, in the organic slurry for the NdFeB silk screen printing, the resin includes one or a mixture of two or more of polyvinylidene fluoride, nitrocellulose, ethyl cellulose, polyvinyl butyral, acrylic resin, polyester resin, and polyurethane.

[0042] Preferably, the resin is one or a mixture of two or more of ethyl cellulose, polyvinyl butyral, and acrylic resin. The above resin has a large molecular weight, and when added in a small amount, it can significantly improve the viscosity of the organic slurry, and has a low degree of thermal decomposition, reducing the C and O elements that enter the magnet during the grain boundary diffusion treatment.

[0043] The technical effects are as follows: by adding the resin, not only can the viscosity of the organic slurry itself be improved, which contributes to improving the dispersion and stability of the organic slurry, but also the adhesion of the organic slurry to the substrate can be improved, thereby ensuring the subsequent grain boundary diffusion effect.

[0044] In a preferred embodiment of the present invention, in the organic slurry for NdFeB silk screen printing, the dispersant includes one or a mixture of two or more of butyl acetate, modified polyurethane polymer, polyethylene glycol, polyvinylpyrrolidone and polyethylene amide.

[0045] Preferably, the dispersant is one or a mixture of two or more of polyethylene glycol, polyvinylpyrrolidone, and polyethylene amide, and the dispersant is easily soluble in an organic solvent and has high wettability to the diffusion source powder, contributing to the dispersion of the diffusion source powder.

[0046] Its technical effects are as follows: the dispersant can prevent the rare earth powder from re-agglomerating in the organic slurry, reduce the fineness of the organic slurry itself, and improve the consistency of weight gain during silk screen printing.

[0047] In a preferred embodiment of the present invention, in the organic slurry for NdFeB silk screen printing, the leveling agent includes one or a mixture of two or more of silicone, acrylate, modified acrylic acid and polyacrylic acid.

[0048] Preferably, the leveling agent is one or a mixture of two or more of acrylate, modified acrylic acid and polyacrylic acid, which ensures that the organic slurry has high leveling properties, and also has a defoaming effect due to its high molecular weight, and further improves the uniformity during silk screen printing.

[0049] Its technical effects are as follows: the leveling agent is especially applied to high viscosity organic slurry such as high content of rare earth powder / high content of resin, etc., thereby improving its leveling property and ensuring the uniformity of the thickness of the film layer after silk screen printing.

[0050] In a preferred embodiment of the present invention, the organic slurry for NdFeB silk screen printing contains the following components in weight percentage: The pure metal powder is 60% to 80%. One or more of butyl carbitol, 2-(2-butoxyethoxy)ethyl acetate, and DBE is 10% to 30%; One or more of ethyl cellulose, acrylic resin, and polyvinyl butyral is 0.4% to 5%; One or two of polyethylene glycol and butyl acetate are 0% to 3%; One or more of acrylate, polyacrylic acid, and silicone is 0% to 1.5%. In a preferred embodiment of the present invention, the organic slurry for NdFeB silk screen printing contains the following components in weight percentage: The alloy powder is 60% to 80%. One or more of butyl carbitol, propylene glycol phenyl ether, and DBE is 10% to 30%; One or more of polyester resin, ethyl cellulose, and acrylic resin is 0.4% to 3%; One or two of polyethyleneamide and polyvinylpyrrolidone are 0% to 3%; One or both of the modified acrylic acid and acrylate are 0% to 1.5%.

[0051] In a preferred embodiment of the present invention, the organic slurry for NdFeB silk screen printing contains the following components in weight percentage: Heavy rare earth powder is 60% to 80%; One or more of butyl carbitol, 2-(2-butoxyethoxy)ethyl acetate, and propylene glycol phenyl ether are 10% to 30%; One or more of polyvinyl butyral, ethyl cellulose, and polyurethane are 0.4% to 5%; One or two of butyl acetate and polyethylene glycol are 0% to 3%; One or both of polyacrylic acid and acrylate is 0% to 1.5%.

[0052] Referring to Figure 1, the second embodiment of the present invention provides a method for preparing organic slurry for NdFeB silk screen printing as above. The method includes the following steps:

[0053] The rare earth powder, organic solvent, resin, dispersant and / or leveling agent are each weighed out in weight percentage.

[0054] The weighed organic solvent, resin, dispersant and / or leveling agent are added in this order to a stirrer, and stirred at a constant temperature of 20 to 70°C and a rotation speed of 600 r / min to 1200 r / min for 0.1 to 6 hours, and then cooled to room temperature to obtain an organic carrier.

[0055] Its technical effect is as follows: the organic carrier produced is homogeneous and free of flocculent material.

[0056] The organic carrier and the weighed rare earth powder are added to a vacuum high-speed disperser and dispersed at high speed at a rotation speed of 1000 r / min to 4000 r / min for 0.25 to 1 hour to obtain a crude organic slurry.

[0057] Its technical effect is as follows: the crude organic slurry prepared is bubble-free and uniformly dispersed.

[0058] The coarse organic slurry is transferred to a three-roll mill with adjustable gap and polished 1 to 3 times to obtain a fine organic slurry.

[0059] Its technical effect is that the fineness of the prepared fine organic slurry is less than 2.5 μm.

[0060] Specifically, the practical effects of the present invention will be further illustrated by the following examples and comparative examples. The blending ratios of various components in each example are as shown in Table 1. [Table 1] JPEG2024159556000003.jpg238170JPEG2024159556000004.jpg238170JPEG2024159556000005.jpg133170 EXAMPLES

[0061] 70% Pr by weight 70 Cu 15 Al 15 Metal powder, 10% butyl carbitol, 13% DBE, 3% ethyl cellulose, 2% polyvinylpyrrolidone, 2% modified acrylic acid were weighed out, where the particle size of the metal powder is D50=1.67 μm.

[0062] Butyl carbitol, DBE, ethyl cellulose, polyvinylpyrrolidone, and modified acrylic acid are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0063] Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 0300 r / min for 60 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.3 μm. EXAMPLES

[0064] 70% Pr by weight 70 Cu15 Al 15 Metal powder, 23% propylene glycol phenyl ether, 2% ethyl cellulose, 1% polyester resin, 2% modified polyurethane polymer, 2% acrylate were weighed out, where the particle size of the metal powder is D50=1.86 μm.

[0065] Propylene glycol phenyl ether, ethyl cellulose, polyester resin, modified polyurethane polymer, and acrylate are added to the mixer in order, and the mixture is stirred at a constant temperature of 60°C and a rotation speed of 1200 r / min for 6 hours to obtain a homogeneous, non-flocculant organic carrier.

[0066] Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3000 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.2 μm. EXAMPLES

[0067] 70% by weight of Tb 70 Ni 30 Metal powder, 23% N-methylpyrrolidone, 3% ethylcellulose, 1% polyethyleneamide, 1% butyl acetate, 2% silicone were weighed out, where the particle size of the metal powder is D50=1.8 μm.

[0068] N-methylpyrrolidone, ethyl cellulose, polyethyleneamide, butyl acetate, and silicone are added to the stirrer in this order, and stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0069] Tb 70 Ni 30The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3000 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and ground three times to obtain an organic slurry with a fineness of less than 1.9 μm. EXAMPLES

[0070] 70% by weight of Tb 80 Cu 15 Weigh out Al5 metal powder, 23% N-methylpyrrolidone, 3% ethylcellulose, 2% polyethyleneamide, and 2% silicone, where the particle size of the metal powder is D50=1.94 μm.

[0071] N-methylpyrrolidone, ethyl cellulose, polyethyleneamide, and silicone are added in sequence to the stirrer, and stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0072] Tb 80 Cu 15 The Al5 metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 3000 r / min for 60 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.3 μm. EXAMPLES

[0073] 70% Nd by weight 60 Fe 30 Ga 10 Metal powder, 15% butyl carbitol, 8% N-methylpyrrolidone, 3% polyurethane, 2% polyethyleneamide, 2% polyacrylic acid were weighed out, where the particle size of the metal powder is D50=1.99 μm.

[0074] Butyl carbitol, N-methylpyrrolidone, polyurethane, polyethyleneamide, and polyacrylic acid are added to the mixer in order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0075] Nd 60 Fe 30 Ga 10 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2500 r / min for 60 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and ground three times to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0076] The weight percentages are 30% DyH+40% TbH metal powder, 23.5% propylene glycol phenyl ether, 3% polyester resin, 2% polyethylene glycol, and 1.5% silicone, where the particle size of the metal powder is D50=1.71 μm.

[0077] Propylene glycol phenyl ether, polyester resin, polyethylene glycol, and silicone are added to the mixer in order, and the mixture is stirred at a constant temperature of 60°C and a rotation speed of 1200 r / min for 6 hours to obtain a homogeneous, flocculent-free organic carrier.

[0078] The 30% DyH+40% TbH metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 30 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished three times to obtain an organic slurry with a fineness of less than 1.8 μm. EXAMPLES

[0079] 70% by weight of Tb 80 Cu 15Weigh out Al5 metal powder, 23% butyl carbitol, 3% ethyl cellulose, 2% polyethylene glycol, and 2% silicone, where the particle size of the metal powder is D50=1.87 μm.

[0080] Butyl carbitol, ethyl cellulose, polyethylene glycol, and silicone are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25° C. and a rotation speed of 1200 r / min for 15 minutes to obtain a homogeneous, non-flocculant organic carrier.

[0081] Tb 80 Cu 15 The Al5 metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 3500 r / min for 60 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0082] The weight percentages were 80% TbH metal powder, 17% butyl carbitol, and 3% ethyl cellulose, where the particle size of the TbH metal powder was D50=1.96 μm.

[0083] Butyl carbitol and ethyl cellulose are added to the stirrer in this order, and the mixture is stirred at a constant temperature of 25° C. and a rotation speed of 1000 r / min for 15 minutes to obtain a homogeneous organic carrier without flocculants.

[0084] The TbH metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 3000 r / min for 40 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished three times to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0085] 40% Tb by weight 80 Cu 15 Al5+30%Pr 70 Cu 15Al 15 Metal powder, 23% 2-(2-butoxyethoxy)ethyl acetate, 3% polyvinylidene fluoride, 2% butyl acetate, 2% silicone were weighed out, where the particle size D50 of the metal powder is 1.82 and 1.79 μm, respectively.

[0086] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, butyl acetate, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 40 minutes to obtain a uniform, flocculent-free organic carrier.

[0087] Tb 80 Cu 15 Al5, Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3500 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and ground twice to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0088] 70% by weight of Tb 80 Cu 15 Weigh out Al5 metal powder, 20% butyl carbitol, 3% DBE, 3% ethyl cellulose, 2% butyl acetate, 1% silicone, and 1% modified acrylic acid, where the particle size of the metal powder is D50=1.98 μm.

[0089] Butyl carbitol, DBE, ethyl cellulose, butyl acetate, silicone, and modified acrylic acid are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0090] Tb 80 Cu 15The Al5 metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 3000 r / min for 60 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and ground three times to obtain an organic slurry with a fineness of less than 2.3 μm. EXAMPLES

[0091] 70% Nd by weight 60 Fe 30 Ga 10 Metal powder, 23% propylene glycol phenyl ether, 3% polyester resin, 2% polyethylene glycol, 2% silicone were weighed out, where the particle size of the metal powder is D50=1.83 μm.

[0092] Propylene glycol phenyl ether, polyester resin, polyethylene glycol, and silicone are added to the mixer in order, and the mixture is stirred at a constant temperature of 60°C and a rotation speed of 1200 r / min for 6 hours to obtain a homogeneous, flocculent-free organic carrier.

[0093] Nd 60 Fe 30 Ga 10 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 2500 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.4 μm. EXAMPLES

[0094] 70% Nd by weight 60 Fe 30 Ga 10 Metal powder, 23% N-methylpyrrolidone, 3% ethylcellulose, 2% polyethyleneamide, 2% acrylate were weighed out, where the particle size of the metal powder is D50=1.56 μm.

[0095] N-methylpyrrolidone, ethyl cellulose, polyethylene amide, and acrylate are added in sequence to a stirrer, and stirred at a constant temperature of 25° C. and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0096] Nd 60 Fe 30 Ga 10 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2500 r / min for 60 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and ground three times to obtain an organic slurry with a fineness of less than 1.7 μm. EXAMPLES

[0097] 70% by weight of Tb 70 Ni 30 Metal powder, 23% N-methylpyrrolidone, 3% ethylcellulose, 2% polyethyleneamide, 2% silicone were weighed out, where the particle size of the metal powder is D50=1.75 μm.

[0098] N-methylpyrrolidone, ethyl cellulose, polyethyleneamide, and silicone are added in sequence to the stirrer, and stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0099] Tb 70 Ni 30 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3000 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 1.5 μm. EXAMPLES

[0100] The weight percentages were 70% TbH metal powder, 26% butyl carbitol, and 4% ethyl cellulose, where the particle size of the TbH metal powder was D50=1.8 μm.

[0101] Butyl carbitol and ethyl cellulose are added to the stirrer in this order, and the mixture is stirred at a constant temperature of 25° C. and a rotation speed of 1000 r / min for 15 minutes to obtain a homogeneous organic carrier without flocculants.

[0102] The TbH metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2200 r / min for 30 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.3 μm. EXAMPLES

[0103] 70% by weight of Tb 70 Ni 30 Weigh out metal powder, 15% butyl carbitol, 8% DBE, 3% ethyl cellulose, 2% butyl acetate, 1% silicone, 1% acrylate, where the particle size of the metal powder is D50=1.82 μm.

[0104] Butyl carbitol, DBE, ethyl cellulose, butyl acetate, silicone, and acrylate are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25° C. and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0105] Tb 70 Ni 30 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3000 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0106] The weight percentages were 70% DyO metal powder, 23% 2-(2-butoxyethoxy)ethyl acetate, 1.5% polyvinylidene fluoride, 0.5% polyester resin, 1% modified polyurethane polymer, 1% butyl acetate, 1% polyethyleneamide, 1% silicone, and 1% modified acrylic acid, where the particle size of the metal powder was D50=1.97 μm.

[0107] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, polyester resin, modified polyurethane polymer, butyl acetate, polyethylene amide, silicone, and modified acrylic acid are added to the mixer in that order, and the mixture is stirred at a constant temperature of 60°C and a rotation speed of 1200 r / min for 6 hours to obtain a uniform, cotton-free organic carrier.

[0108] The DyO metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.4 μm. EXAMPLES

[0109] The weight percentages are 30% DyH+40% TbH metal powder, 22.5% propylene glycol phenyl ether, 3% polyester resin, 2% polyethylene glycol, and 2.5% silicone, where the particle diameters D50 of the metal powders are 1.67 and 1.88 μm, respectively.

[0110] Propylene glycol phenyl ether, polyester resin, polyethylene glycol, and silicone are added to the mixer in order, and the mixture is stirred at a constant temperature of 70°C and a rotation speed of 1200 r / min for 5 hours to obtain a uniform, flocculent-free organic carrier.

[0111] The 30% DyH+40% TbH metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 30 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0112] The weight percentages were 70% Dy metal powder, 23% N-methylpyrrolidone, 3% polyvinyl butyral, 3% polyethylene glycol, and 1% acrylate, where the particle size of the Dy metal powder was D50=1.56 μm.

[0113] N-methylpyrrolidone, polyvinyl butyral, polyethylene glycol, and polyacrylic acid are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0114] The Dy metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished three times to obtain an organic slurry with a fineness of less than 1.5 μm. EXAMPLES

[0115] 70% Pr by weight 70 Cu 15 Al 15 Metal powder, 10% butyl carbitol, 13% N-methylpyrrolidone, 3% polyurethane, 2% polyethyleneamide, 1% polyacrylic acid, 1% acrylate were weighed out, where the particle size of the metal powder is D50=1.79 μm.

[0116] Butyl carbitol, N-methylpyrrolidone, polyurethane, polyethyleneamide, polyacrylic acid, and acrylate are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a homogeneous, flocculent-free organic carrier.

[0117] Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3000 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.2 μm. EXAMPLES

[0118] The weight percentages are 30% DyH+40% TbH metal powder, 23% propylene glycol phenyl ether, 3% polyester resin, 2% polyethylene glycol, and 1% silicone, where the particle size of the metal powder is D50=1.96 μm.

[0119] Propylene glycol phenyl ether, polyester resin, polyethylene glycol, and silicone are added in sequence to a stirrer, and stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0120] The 30% DyH+40% TbH metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 30 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished three times to obtain an organic slurry with a fineness of less than 2.3 μm. EXAMPLES

[0121] 70% by weight of Tb 70 Ni 30Metal powder, 15% butyl carbitol, 8% N-methylpyrrolidone, 3% polyurethane, 2% polyethyleneamide, 2% polyacrylic acid were weighed out, where the particle size of the metal powder is D50=1.91 μm.

[0122] Butyl carbitol, N-methylpyrrolidone, polyurethane, polyethyleneamide, and polyacrylic acid are added to the mixer in order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0123] Tb 70 Ni 30 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3000 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and ground twice to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0124] The weight percentages were 70% Dy metal powder, 21% N-methylpyrrolidone, 3% polyvinyl butyral, 5% polyethylene glycol, 0.5% silicone, and 0.5% polyacrylic acid, where the particle size of the Dy metal powder was D50=1.85 μm.

[0125] N-methylpyrrolidone, polyvinyl butyral, polyethylene glycol, silicone, and polyacrylic acid are added to the mixer in order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0126] The Dy metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.4 μm. EXAMPLES

[0127] 40% Tb by weight 80 Cu 15 Al5+30%Pr 70 Cu 15 Al 15 Metal powder, 23% 2-(2-butoxyethoxy)ethyl acetate, 3% polyvinylidene fluoride, 1.5% butyl acetate, 0.5% polyethylene glycol, 2% silicone were weighed out, where the particle size of the metal powder is D50=1.97 μm.

[0128] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, butyl acetate, polyethylene glycol, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 40 minutes to obtain a uniform, flocculent-free organic carrier.

[0129] Tb 80 Cu 15 Al5, Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3500 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.4 μm. EXAMPLES

[0130] 70% by weight of Tb 80 Cu 15 Weigh out Al5 metal powder, 23% N-methylpyrrolidone, 3% polyvinyl butyral, 2% polyethylene glycol, and 2% silicone, where the particle size of the metal powder is D50=1.69 μm.

[0131] N-methylpyrrolidone, polyvinyl butyral, polyethylene glycol, and silicone are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0132] Tb80 Cu 15 The Al5 metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 3000 r / min for 60 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.3 μm. EXAMPLES

[0133] The weight percentages were 70% DyO metal powder, 23% 2-(2-butoxyethoxy)ethyl acetate, 1.5% polyvinylidene fluoride, 1.5% polyester resin, 2% butyl acetate, and 2% silicone, where the particle size of the metal powder was D50=1.93 μm.

[0134] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, polyester resin, butyl acetate, and silicone are added in sequence to a stirrer, and stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 40 minutes to obtain a uniform, flocculent-free organic carrier.

[0135] The DyO metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.2 μm. EXAMPLES

[0136] The weight percentages were 70% Dy metal powder, 22% N-methylpyrrolidone, 3% polyvinyl butyral, 4% polyethylene glycol, 0.5% silicone, and 0.5% polyacrylic acid, where the particle size of the Dy metal powder was D50=1.88 μm.

[0137] N-methylpyrrolidone, polyvinyl butyral, polyethylene glycol, silicone, and polyacrylic acid are added to the mixer in order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0138] The Dy metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.2 μm. EXAMPLES

[0139] 70% by weight of Tb 70 Ni 30 Metal powder, 15% butyl carbitol, 8% N-methylpyrrolidone, 1.5% polyurethane, 1.5% ethyl cellulose, 2% polyethyleneamide, 2% polyacrylic acid were weighed out, where the particle size of the metal powder is D50=1.77 μm.

[0140] Butyl carbitol, N-methylpyrrolidone, polyurethane, ethyl cellulose, polyethyleneamide, and polyacrylic acid are added to the mixer in order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0141] Tb 70 Ni 30 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 3000 r / min for 60 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.3 μm. EXAMPLES

[0142] 70% by weight of Tb 70 Ni 30 Metal powder, 23% N-methylpyrrolidone, 3% ethylcellulose, 1% polyethyleneamide, 0.5% butyl acetate, 0.5% modified polyurethane polymer, 2% silicone were weighed out, where the particle size of the metal powder is D50=1.47 μm.

[0143] N-methylpyrrolidone, ethyl cellulose, polyethyleneamide, butyl acetate, and silicone are added to the stirrer in this order, and stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0144] Tb 70 Ni 30 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 50 minutes at a rotation speed of 3000 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.2 μm. EXAMPLES

[0145] The weight percentages were 70% TbF metal powder, 24% 2-(2-butoxyethoxy)ethyl acetate, 4% polyvinylidene fluoride, 1% butyl acetate, and 1% silicone, where the particle size of the TbF metal powder was D50=1.68 μm.

[0146] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, butyl acetate, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 40 minutes to obtain a uniform, flocculent-free organic carrier.

[0147] The TbF metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished three times to obtain an organic slurry with a fineness of less than 1.5 μm. EXAMPLES

[0148] 70% by weight of Tb 80 Cu 15 Weigh out Al5 metal powder, 20% butyl carbitol, 3% DBE, 3% ethyl cellulose, 2% polyethyleneamide, and 2% silicone, where the particle size of the metal powder is D50=1.62 μm.

[0149] Butyl carbitol, DBE, ethyl cellulose, polyethylene amide, and silicone are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25° C. and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0150] Tb 80 Cu 15 The Al5 metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 3000 r / min for 60 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 1.7 μm. EXAMPLES

[0151] The weight percentages were 70% TbF metal powder, 25% 2-(2-butoxyethoxy)ethyl acetate, 3% polyvinylidene fluoride, 1% polyethyleneamide, and 1% silicone, where the particle size of the TbF metal powder was D50=1.58 μm.

[0152] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, polyethyleneamide, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 40 minutes to obtain a uniform, flocculent-free organic carrier.

[0153] The TbF metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished three times to obtain an organic slurry with a fineness of less than 1.5 μm. EXAMPLES

[0154] 70% Pr by weight 70 Cu 15 Al 15Metal powder, 23% N-methylpyrrolidone, 1% polyvinyl butyral, 2% ethyl cellulose, 2% polyethyleneamide, 2% silicone were weighed out, where the particle size of the metal powder is D50=1.79 μm.

[0155] N-methylpyrrolidone, polyvinyl butyral, ethyl cellulose, polyethylene amide, and silicone are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 20 minutes to obtain a uniform, flocculent-free organic carrier.

[0156] Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 3000 r / min for 50 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.3 μm. EXAMPLES

[0157] The weight percentages were 70% TbF metal powder, 22% 2-(2-butoxyethoxy)ethyl acetate, 6% polyvinylidene fluoride, 1% polyethyleneamide, and 1% silicone, where the particle size of the TbF metal powder was D50=1.89 μm.

[0158] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, polyethyleneamide, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 40 minutes to obtain a uniform, flocculent-free organic carrier.

[0159] The TbF metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 30 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0160] 70% by weight of Tb 80 Cu 15 Weigh out Al5 metal powder, 23% 2-(2-butoxyethoxy)ethyl acetate, 3% polyvinylidene fluoride, 2% polyethylene glycol, and 2% silicone, where the particle size of the metal powder is D50=1.94 μm.

[0161] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, polyethylene glycol, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 40 minutes to obtain a uniform, flocculent-free organic carrier.

[0162] Tb 80 Cu 15 The Al5 metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 3000 r / min for 60 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0163] 70% Nd by weight 60 Fe 30 Ga 10 Metal powder, 23% N-methylpyrrolidone, 2% ethylcellulose, 1% polyester resin, 1.5% polyethyleneamide, 0.5% modified polyurethane polymer, 2% acrylate were weighed out, where the particle size of the metal powder is D50=1.85 μm.

[0164] N-methylpyrrolidone, ethyl cellulose, polyester resin, polyethylene amide, modified polyurethane polymer, and acrylate are added in sequence to a stirrer, and stirred at a constant temperature of 60°C and a rotation speed of 1200 r / min for 5 hours to obtain a uniform, flocculent-free organic carrier.

[0165] Nd 60 Fe 30The Ga1 metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2500 r / min for 60 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.1 μm. EXAMPLES

[0166] 70% by weight of Tb 70 Ni 30 Weigh out metal powder, 23% 2-(2-butoxyethoxy)ethyl acetate, 3% polyvinylidene fluoride, 2% butyl acetate, and 2% silicone, where the particle size of the metal powder is D50=1.87 μm.

[0167] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, butyl acetate, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 40 minutes to obtain a uniform, flocculent-free organic carrier.

[0168] Tb 70 Ni 30 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3000 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.1 μm. EXAMPLES

[0169] The weight percentages were 70% TbF metal powder, 27.6% 2-(2-butoxyethoxy)ethyl acetate, 0.4% polyvinylidene fluoride, 0.5% polyethyleneamide, 0.5% polyethylene glycol, and 1% silicone, where the particle size of the TbF metal powder was D50=1.82 μm.

[0170] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, polyethylene amide, polyethylene glycol, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 40 minutes to obtain a uniform, flocculent-free organic carrier.

[0171] The TbF metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished three times to obtain an organic slurry with a fineness of less than 1.7 μm. EXAMPLES

[0172] The weight percentages were 70% DyO metal powder, 10% butyl carbitol, 13% DBE, 3% ethyl cellulose, 2% polyvinylpyrrolidone, and 2% polyacrylic acid, where the particle size of the metal powder was D50=1.98 μm.

[0173] Butyl carbitol, DBE, ethyl cellulose, polyvinylpyrrolidone, and polyacrylic acid are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a homogeneous, flocculent-free organic carrier.

[0174] The DyO metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished three times to obtain an organic slurry with a fineness of less than 2.2 μm. EXAMPLES

[0175] The weight percentages were 70% Dy metal powder, 25% N-methylpyrrolidone, 3% polyvinyl butyral, 1% polyethylene glycol, and 1% modified acrylic acid, where the particle size of the Dy metal powder was D50=1.75 μm.

[0176] N-methylpyrrolidone, polyvinyl butyral, polyethylene glycol, and modified acrylic acid are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0177] The Dy metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished three times to obtain an organic slurry with a fineness of less than 1.7 μm. EXAMPLES

[0178] 70% by weight of Tb 70 Ni 30 Metal powder, 23% propylene glycol phenyl ether, 3% polyester resin, 2% polyethylene glycol, 2% silicone were weighed out, where the particle size of the metal powder is D50=1.88 μm.

[0179] Propylene glycol phenyl ether, polyester resin, polyethylene glycol, and silicone are added to the mixer in order, and the mixture is stirred at a constant temperature of 60°C and a rotation speed of 1200 r / min for 6 hours to obtain a homogeneous, flocculent-free organic carrier.

[0180] Tb 70 Ni 30 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3000 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.0 μm. EXAMPLES

[0181] The weight percentages were 30% DyH+40% TbH metal powder, 24.5% propylene glycol phenyl ether, 3% polyester resin, 2% polyethylene glycol, 0.5% silicone, and 0.5% polyacrylic acid, where the particle diameters D50 of the metal powders were 1.73 and 1.69 μm, respectively.

[0182] Propylene glycol phenyl ether, polyester resin, polyethylene glycol, silicone, and polyacrylic acid are added to the mixer in order, and the mixture is stirred at a constant temperature of 70°C and a rotation speed of 1200 r / min for 5 hours to obtain a uniform, flocculent-free organic carrier.

[0183] The 30% DyH+40% TbH metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 30 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 1.6 μm. EXAMPLES

[0184] The weight percentages are 30% DyH+40% TbH metal powder, 25% propylene glycol phenyl ether, 3% polyester resin, and 2% polyethylene glycol, where the particle size of the metal powder is D50=1.96 μm.

[0185] Propylene glycol phenyl ether, polyester resin, and polyethylene glycol are added to the mixer in order, and the mixture is stirred at a constant temperature of 60°C and a rotation speed of 1200 r / min for 6 hours to obtain a homogeneous, flocculent-free organic carrier.

[0186] The 30% DyH+40% TbH metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 30 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0187] 70% by weight of Tb 70 Ni 30 Weigh out metal powder, 15% butyl carbitol, 8% DBE, 3% ethyl cellulose, 1.5% butyl acetate, 0.5% polyethylene glycol, 1% silicone, 1% acrylate, where the particle size of the metal powder is D50=1.92 μm.

[0188] Butyl carbitol, DBE, ethyl cellulose, butyl acetate, polyethylene glycol, silicone, and acrylate are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 25 minutes to obtain a homogeneous, flocculent-free organic carrier.

[0189] Tb 70 Ni 30 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3000 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.4 μm. EXAMPLES

[0190] 70% Nd by weight 60 Fe 30 Ga 10 Metal powder, 15% butyl carbitol, 8% DBE, 3% ethyl cellulose, 2% butyl acetate, 1% silicone, 1% modified acrylic acid were weighed out, where the particle size of the metal powder is D50=1.66 μm.

[0191] Propylene glycol phenyl ether, polyester resin, polyethylene glycol, and silicone are added to the mixer in order, and the mixture is stirred at a constant temperature of 60°C and a rotation speed of 1200 r / min for 6 hours to obtain a homogeneous, flocculent-free organic carrier.

[0192] Nd 60 Fe 30 Ga 10The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2500 r / min for 60 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0193] 70% Pr by weight 70 Cu 15 Al 15 Weigh out metal powder, 10% butyl carbitol, 6% N-methylpyrrolidone, 7% DBE, 3% polyurethane, 2% polyethyleneamide, 1% polyacrylic acid, and 1% acrylate, where the particle size of the metal powder is D50=2.0 μm.

[0194] Butyl carbitol, N-methylpyrrolidone, DBE, polyurethane, polyethyleneamide, polyacrylic acid, and acrylate are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0195] Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3000 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.1 μm. EXAMPLES

[0196] 40% Tb by weight 80 Cu 15 Al5+30%Pr 70 Cu 15 Al 15 Metal powder, 15% butyl carbitol, 8% DBE, 3% ethyl cellulose, 2% butyl acetate, 2% acrylate were weighed out, where the particle size of the metal powder is D50=1.62 and 1.65 μm.

[0197] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, butyl acetate, polyethylene glycol, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 40 minutes to obtain a uniform, flocculent-free organic carrier.

[0198] Tb 80 Cu 15 Al5, Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 3500 r / min for 60 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and ground three times to obtain an organic slurry with a fineness of less than 1.8 μm. EXAMPLES

[0199] 70% Pr by weight 70 Cu 15 Al 15 Metal powder, 23% N-methylpyrrolidone, 3% polyvinyl butyral, 2% butyl acetate, 2% silicone were weighed out, where the particle size of the metal powder is D50=1.96 μm.

[0200] N-methylpyrrolidone, polyvinyl butyral, polyethyleneamide, and silicone are added in sequence to the mixer, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0201] Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3000 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0202] 40% Tb by weight 80 Cu 15 Al5+30%Pr 70 Cu 15 Al 15 Metal powder, 15% butyl carbitol, 8% N-methylpyrrolidone, 3% polyurethane, 2% polyethyleneamide, 2% polyacrylic acid were weighed out, where the particle size D50 of the metal powder is 1.86 and 1.83 μm, respectively.

[0203] Butyl carbitol, N-methylpyrrolidone, polyurethane, polyethyleneamide, and polyacrylic acid are added to the mixer in order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0204] Tb 80 Cu 15 Al5, Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 3000 r / min for 60 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.3 μm. EXAMPLES

[0205] 70% Pr by weight 70 Cu 15 Al 15 Metal powder, 23% N-methylpyrrolidone, 1% polyvinyl butyral, 1% ethyl cellulose, 1% polyurethane, 2% polyethyleneamide, 2% silicone were weighed out, where the particle size of the metal powder is D50=1.87 μm.

[0206] N-methylpyrrolidone, polyvinyl butyral, ethyl cellulose, polyurethane, polyethylene amide, and silicone are added to the mixer in order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 1200 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0207] Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 60 minutes at a rotation speed of 3000 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.3 μm. EXAMPLES

[0208] The weight percentages were 70% TbF metal powder, 27% 2-(2-butoxyethoxy)ethyl acetate, 1% polyvinylidene fluoride, 1% polyvinylpyrrolidone, and 1% silicone, where the particle size of the TbF metal powder was D50=1.73 μm.

[0209] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, polyvinylpyrrolidone, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 40 minutes to obtain a uniform, flocculent-free organic carrier.

[0210] The TbF metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished three times to obtain an organic slurry with a fineness of less than 1.7 μm. EXAMPLES

[0211] The weight percentages were 70% Dy metal powder, 26% N-methylpyrrolidone, 3% polyvinyl butyral, and 1% polyacrylic acid, where the particle size of the Dy metal powder was D50=1.94 μm.

[0212] N-methylpyrrolidone, polyvinyl butyral, and polyacrylic acid are added in sequence to the mixer, and the mixture is stirred for 15 minutes at a constant temperature of 25°C and a rotation speed of 1200 r / min to obtain a uniform, flocculent-free organic carrier.

[0213] The Dy metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.3 μm. EXAMPLES

[0214] The weight percentages were 70% TbF metal powder, 26% 2-(2-butoxyethoxy)ethyl acetate, 2% polyvinylidene fluoride, 1% modified polyurethane polymer, and 1% silicone, where the particle size of the TbF metal powder was D50=1.6 μm.

[0215] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, modified polyurethane polymer, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 40 minutes to obtain a uniform, flocculent-free organic carrier.

[0216] The TbF metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished three times to obtain an organic slurry with a fineness of less than 1.6 μm. EXAMPLES

[0217] The weight percentages were 50% TbH metal powder, 44% butyl carbitol, and 6% ethyl cellulose, where the particle size of the TbH metal powder was D50=1.8 μm.

[0218] Butyl carbitol and ethyl cellulose are added to the stirrer in this order, and the mixture is stirred at a constant temperature of 25° C. and a rotation speed of 1000 r / min for 15 minutes to obtain a homogeneous organic carrier without flocculants.

[0219] The TbH metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 1000 r / min for 15 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0220] The weight percentages were 70% DyO metal powder, 23% 2-(2-butoxyethoxy)ethyl acetate, 3% polyvinylidene fluoride, 2% butyl acetate, 1% silicone, and 1% acrylate, where the particle size of the metal powder was D50=1.63 μm.

[0221] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, butyl acetate, silicone, and acrylate are added to the mixer in that order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 40 minutes to obtain a uniform, flocculent-free organic carrier.

[0222] The DyO metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a speed of 2000 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 1.9 μm. EXAMPLES

[0223] The weight percentages are 30% DyH+40% TbH metal powder, 23% propylene glycol phenyl ether, 3% polyester resin, 2% polyethylene glycol, and 2% silicone, where the particle size of the metal powder is D50=1.81 μm.

[0224] Propylene glycol phenyl ether, polyester resin, polyethylene glycol, and silicone are added to the mixer in order, and the mixture is stirred at a constant temperature of 60°C and a rotation speed of 1200 r / min for 5 hours to obtain a uniform, flocculent-free organic carrier.

[0225] The 30% DyH+40% TbH metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 40 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.3 μm. EXAMPLES

[0226] The weight percentages were 70% Dy metal powder, 24% N-methylpyrrolidone, 3% polyvinyl butyral, 2% polyethylene glycol, and 1% silicone, where the particle size of the Dy metal powder was D50=1.63 μm.

[0227] N-methylpyrrolidone, polyvinyl butyral, polyethylene glycol, and silicone are added to the mixer in this order, and the mixture is stirred at a constant temperature of 25°C and a rotation speed of 800 r / min for 20 minutes to obtain a uniform, flocculent-free organic carrier.

[0228] The Dy metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished three times to obtain an organic slurry with a fineness of less than 1.7 μm. EXAMPLES

[0229] 70% Pr by weight 70 Cu 15 Al 15 Weigh out metal powder, 23% 2-(2-butoxyethoxy)ethyl acetate, 3% polyvinylidene fluoride, 2% butyl acetate, and 2% silicone, where the particle size of the metal powder is D50=1.99 μm.

[0230] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, butyl acetate, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1200 r / min for 30 minutes to obtain a uniform, flocculent-free organic carrier.

[0231] Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2200 r / min for 30 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.6 μm. EXAMPLES

[0232] The weight percentages were 70% DyO metal powder, 23% 2-(2-butoxyethoxy)ethyl acetate, 1.5% polyvinylidene fluoride, 1.5% polyester resin, 1.5% butyl acetate, 0.5% polyethyleneamide, and 2% silicone, where the particle size of the metal powder was D50=1.93 μm.

[0233] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, polyester resin, butyl acetate, polyethyleneamide, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 70°C and a rotation speed of 1200 r / min for 6 hours to obtain a uniform, flocculent-free organic carrier.

[0234] The DyO metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 40 minutes at a rotation speed of 3500 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0235] The weight percentages are 30% DyH+40% TbH metal powder, 24.5% propylene glycol phenyl ether, 3% polyester resin, 2% polyethylene glycol, and 0.5% silicone, where the particle diameters D50 of the metal powders are 1.78 and 1.77 μm, respectively.

[0236] Propylene glycol phenyl ether, polyester resin, polyethylene glycol, and silicone are added in sequence to a stirrer, and stirred at a constant temperature of 60°C and a rotation speed of 1200 r / min for 60 minutes to obtain a uniform, flocculent-free organic carrier.

[0237] The 30% DyH+40% TbH metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 3000 r / min for 30 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished twice to obtain an organic slurry with a fineness of less than 2.0 μm. EXAMPLES

[0238] The weight percentages were 70% DyO metal powder, 10% butyl carbitol, 13% N-methylpyrrolidone, 3% polyurethane, 2% polyethyleneamide, 1% acrylate, and 1% polyacrylic acid, where the particle size of the metal powder was D50=1.97 μm.

[0239] Butyl carbitol, N-methylpyrrolidone, polyurethane, polyethylene amide, acrylate, and polyacrylic acid are added to the mixer in order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1000 r / min for 30 minutes to obtain a uniform, flocculent-free organic carrier.

[0240] The DyO metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a speed of 2500 r / min for 30 minutes to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.4 μm. EXAMPLES

[0241] 40% Tb by weight 80 Cu 15 Al5+30%Pr 70 Cu 15 Al 15Metal powder, 23% 2-(2-butoxyethoxy)ethyl acetate, 1.5% polyvinylidene fluoride, 1.5% ethyl cellulose, 2% butyl acetate, 2% silicone were weighed out, where the particle sizes of the metal powder were 1.75 and 1.92 μm, respectively.

[0242] 2-(2-butoxyethoxy)ethyl acetate, polyvinylidene fluoride, ethyl cellulose, butyl acetate, and silicone are added to the mixer in that order, and the mixture is stirred at a constant temperature of 50°C and a rotation speed of 600 r / min for 40 minutes to obtain a homogeneous, flocculent-free organic carrier.

[0243] Tb 80 Cu 15 Al5, Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2000 r / min for 40 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.2 μm. EXAMPLES

[0244] The weight percentages were 90% TbH metal powder, 8% butyl carbitol, and 2% ethyl cellulose, where the particle size of the TbH metal powder was D50=1.83 μm.

[0245] Butyl carbitol and ethyl cellulose are added to the stirrer in this order, and the mixture is stirred at a constant temperature of 25° C. and a rotation speed of 600 r / min for 30 minutes to obtain a homogeneous, flocculent-free organic carrier.

[0246] The TbH metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 4000 r / min for 30 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.5 μm. EXAMPLES

[0247] 70% Pr by weight 70 Cu 15 Al 15 Metal powder, 23% propylene glycol phenyl ether, 3% polyester resin, 2% modified polyurethane polymer, 2% acrylate were weighed out, where the particle size of the metal powder is D50=1.62 μm.

[0248] Propylene glycol phenyl ether, polyester resin, modified polyurethane polymer, and acrylate are added in sequence to a stirrer, and stirred at a constant temperature of 70°C and a rotation speed of 1200 r / min for 6 hours to obtain a uniform, flocculent-free organic carrier.

[0249] Pr 70 Cu 15 Al 15 The metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at a rotation speed of 2300 r / min for 60 minutes to prepare an initial organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and ground three times to obtain an organic slurry with a fineness of less than 1.8 μm. EXAMPLES

[0250] The weight percentages were 70% DyO metal powder, 10% butyl carbitol, 8% DBE, 5% N-methylpyrrolidone, 3% polyurethane, 2% polyethyleneamide, and 2% polyacrylic acid, where the particle size of the metal powder was D50=1.95 μm.

[0251] Butyl carbitol, DBE, N-methylpyrrolidone, polyurethane, polyethyleneamide, and polyacrylic acid are added to the mixer in this order, and the mixture is stirred at a constant temperature of 40°C and a rotation speed of 1000 r / min for 15 minutes to obtain a uniform, flocculent-free organic carrier.

[0252] The DyO metal powder and the prepared organic carrier are added to a vacuum high-speed disperser and dispersed at high speed for 40 minutes at a rotation speed of 2200 r / min to initially prepare an organic slurry. The high-speed dispersed organic slurry is then transferred to a three-roll mill and polished once to obtain an organic slurry with a fineness of less than 2.1 μm.

[0253] <Comparative Example 1> Weigh out 60% Tb rare earth powder, 30.8% anhydrous ethanol, 7.7% phenolic resin, 1% polyvinylpyrrolidone, and 0.5% silicone leveling agent by weight percentage, where the particle size of the Tb rare earth powder is D50=1.89 μm;

[0254] Anhydrous ethanol, phenolic resin, polyvinylpyrrolidone and silicone leveling agent are added in sequence to the mixer, and the mixture is stirred for 15 minutes at a constant temperature of 25°C and a rotation speed of 800 r / min to obtain a uniform, flocculent-free organic carrier. The Tb rare earth powder and the prepared organic carrier were added to a stirrer and stirred at high speed at a rotation speed of 1500 r / min for 30 minutes to prepare an organic slurry.

[0255] <Comparative Example 2> Weigh out 60% Tb rare earth powder, 30.8% acetone, 7.7% phenolic resin, 1% polyvinylpyrrolidone, and 0.5% silicone leveling agent by weight percentage, where the particle size of the Tb rare earth powder is D50=1.73 μm;

[0256] Anhydrous ethanol, phenolic resin, polyvinylpyrrolidone and silicone leveling agent are added in sequence to the mixer, and the mixture is stirred for 15 minutes at a constant temperature of 25°C and a rotation speed of 800 r / min to obtain a uniform, flocculent-free organic carrier. The Tb rare earth powder and the prepared organic carrier were added to a stirrer and stirred at high speed at a rotation speed of 1500 r / min for 30 minutes to prepare an organic slurry.

[0257] The fineness of the organic slurries prepared in Examples 1-8 and Comparative Examples 1-2 was measured using a grain gauge, and the results are shown in Table 2. The fineness of the organic slurries prepared in Examples 1-8 was only 1.5-2.5 μm, which shows that the dispersion degree of the powder particles in the organic slurries is good and the particles are not obviously aggregated. Compared with the particle size of the original powder, the fineness of the organic slurries prepared in Comparative Examples 1 and 2 is significantly larger, which shows that the powder particles cannot be effectively dispersed during preparation and there are many aggregated particles in the organic slurries. [Table 2]

[0258] The organic slurries prepared in Examples 1-64 and Comparative Examples 1 and 2 were aged for 48 hours at 60° C. After the aging experiment, the organic slurries prepared in Examples 1-64 did not show any obvious settling or stratification, but the organic slurries prepared in Comparative Examples 1-2 showed obvious stratification.

[0259] The organic slurries prepared in Examples 1-8 and Comparative Examples 1 and 2 were coated on the surface of neodymium magnets by silk screen printing and dried at 120°C for 15 minutes, after which the weight gain of the magnets was measured and the results are shown in Table 3. The organic slurries prepared in Examples 1-8 stabilized the weight gain of the magnets when silk screen printed, helping to ensure the consistency of subsequent diffusion. The organic slurries prepared in Comparative Examples 1-2 caused large fluctuations in the weight gain of the magnets when silk screen printed, making it difficult to ensure lot-to-lot stability. [Table 3] The embodiments of the present invention aim to protect the organic slurry and preparation method for NdFeB silk screen printing, and have the following effects:

[0260] The organic slurry for NdFeB silk screen printing prepared by the present invention is made by suitably selecting the organic carrier, and by relying on the strong mechanical action of the vacuum high-speed disperser and the three-roll mill to disperse the agglomerated powder particles by high-speed shearing action and grinding, so as to realize high dispersibility and suspension stability of the organic slurry. The fineness of the prepared slurry is less than 2.5μm, the monthly settling rate of the slurry is less than 5%, and the consistency of the weight gain during printing is less than ±5%. The prepared slurry has excellent dispersibility and stability.

[0261] It should be understood that the above specific embodiments of the present invention are merely for illustrative purposes of explaining or interpreting the principles of the present invention, and are not intended to limit the present invention. Therefore, any modifications, equivalent replacements, improvements, etc. made without departing from the spirit and scope of the present invention are intended to be included within the protection scope of the present invention. In addition, the claims attached to the present invention are intended to cover all changes and modifications included within the scope and boundaries of the attached claims, or equivalent forms of such scope and boundaries.

Claims

1. The composition includes a rare earth powder, an organic solvent, and a resin, and further includes a dispersant and / or a leveling agent, and the weight percentage of each component is as follows: The rare earth powder is 50% to 90%; The organic solvent is 8% to 50%; Resin is 0.4% to 6%; The dispersant is 0% to 5%; An organic slurry for NdFeB silk screen printing, characterized in that the leveling agent is 0%-3%.

2. 2. The organic slurry for NdFeB silk screen printing according to claim 1, characterized in that the rare earth powder comprises one or a mixture of two or more of the following: pure metal powder of heavy rare earth element, alloy powder containing heavy rare earth element or light rare earth element, heavy rare earth powder containing hydride, fluoride and oxide of heavy rare earth.

3. The heavy rare earth element includes one or a mixture of two or more of Tb, Dy, Ho, and Gd; The composition of the alloy powder in mass percentage is RE x M y The organic slurry for NdFeB silk screen printing according to claim 2, characterized in that, RE is a mixture of one or more of Tb, Dy, Ho, Gd, Pr, Nd, La, Ce, Y, M is a mixture of one or more of Ga, Cu, Al, Ni, Fe, 60%≦x≦95%, 5%≦y≦40%.

4. The organic slurry for NdFeB silk screen printing as claimed in claim 1, characterized in that the particle size of the rare earth powder is D50<2 μm.

5. The organic slurry for NdFeB silk screen printing according to claim 2, characterized in that the organic solvent comprises one or a mixture of two or more of butyl carbitol, 2-(2-butoxyethoxy)ethyl acetate, N-methylpyrrolidone, texanol, propylene glycol phenyl ether, 2-acetoxy-1-methoxypropane and DBE.

6. 6. The organic slurry for NdFeB silk screen printing as claimed in claim 5, characterized in that the resin comprises one or a mixture of two or more of polyvinylidene fluoride, nitrocellulose, ethyl cellulose, polyvinyl butyral, acrylic resin, polyester resin and polyurethane.

7. 7. The organic slurry for NdFeB silk screen printing as claimed in claim 6, characterized in that the dispersing agent comprises one or a mixture of two or more of butyl acetate, modified polyurethane polymer, polyethylene glycol, polyvinylpyrrolidone and polyethylene amide.

8. The organic slurry for NdFeB silk screen printing as claimed in claim 7, characterized in that the leveling agent comprises one or a mixture of two or more of silicone, acrylate, modified acrylic acid and polyacrylic acid.

9. The weight percentage of each component is: 60% to 80% pure metal powder; 10% to 30% of one or more of butyl carbitol, 2-(2-butoxyethoxy)ethyl acetate, and DBE; 0.4% to 5% of one or more of ethyl cellulose, acrylic resin, and polyvinyl butyral; One or two of the following are present: polyethylene glycol, butyl acetate, 0% to 3%; The organic slurry for NdFeB silk screen printing according to claim 8, characterized in that one or more of acrylate, polyacrylic acid, silicone is 0% to 1.5%.

10. The weight percentage of each component is: The alloy powder is 60% to 80%. butyl carbitol, propylene glycol phenyl ether, and DBE, from 10% to 30%; One or more of polyester resin, ethyl cellulose, and acrylic resin is 0.4% to 3%; One or two of polyethyleneamide, polyvinylpyrrolidone is 0% to 3%; The organic slurry for NdFeB silk screen printing according to claim 8, characterized in that one or two of modified acrylic acid, acrylate is 0%-1.5%.

11. The weight percentage of each component is: The heavy rare earth powder is 60% to 80%. butyl carbitol, 2-(2-butoxyethoxy)ethyl acetate, propylene glycol phenyl ether, from 10% to 30%; one or more of polyvinyl butyral, ethyl cellulose, and polyurethane, at 0.4% to 5%; butyl acetate, polyethylene glycol, 0% to 3%; The organic slurry for NdFeB silk screen printing according to claim 8, characterized in that one or two of polyacrylic acid, acrylate is 0%-1.5%.

12. Weighing out the rare earth powder, the organic solvent, the resin, the dispersant and / or the leveling agent in weight percentages, respectively; Adding the weighed organic solvent, the resin, the dispersant and / or the leveling agent to a stirrer in this order, stirring at a constant temperature of 20 to 70° C. and a rotation speed of 600 r / min to 1200 r / min for 0.1 to 6 hours, and then cooling to room temperature to obtain an organic carrier; Adding the organic carrier and the weighed rare earth powder to a vacuum high-speed disperser and dispersing at a rotation speed of 1000 r / min to 4000 r / min for 0.25 to 1 hour to obtain a crude organic slurry; The method for preparing organic slurry for NdFeB silk screen printing according to any one of claims 1-11, characterized in that the method includes the steps of: transferring the coarse organic slurry to an adjustable gap three-roll mill, and grinding it 1-3 times to obtain a fine organic slurry.

Citation Information

Patent Citations

  • Method of manufacturing bond magnet, bond magnet, and manufacturing apparatus

    JP2009158860A

  • Paste composition and magnetic body composition using it

    JP2012124355A

  • Paste for conductor, ceramic electronic component and manufacturing method for electronic component

    JP2017011164A

  • Method for manufacturing r-t-b based sintered magnet

    JP2017162900A

  • Method for manufacturing r-t-b based sintered magnet

    JP2018026390A