Organic paste having gradient volatilization rate and method of preparing the same

The organic paste with a gradient volatilization rate addresses the challenges of uneven coatings and prolonged drying times by using a specific composition and processing method, ensuring efficient and uniform screen printing for neodymium iron boron magnets.

JP2024159557AActive Publication Date: 2024-11-08GRIREM ADVANCED MATERIALS CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024064230
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-11
Publication Date
2024-11-08
Estimated Expiration
2044-04-11

AI Technical Summary

Technical Problem

Existing screen printing pastes for neodymium iron boron magnets have difficulty achieving a gradient volatilization rate, leading to issues such as high room temperature volatilization causing paste viscosity increase and printing difficulties, and low high-temperature volatilization resulting in uneven coatings and prolonged drying times, which affect diffusion efficiency and magnet performance.

Method used

A screen printing organic paste composition comprising rare earth powders, organic solvents, resins, dispersants, anti-settling agents, and synergists, with specific weight percentages and processing methods to create a gradient volatilization rate, ensuring low volatilization at room temperature and high volatilization at high temperatures.

Benefits of technology

The paste achieves a gradient volatilization rate of 0.05%/h at room temperature and 1.2%/h at 120°C, preventing printing issues and significantly shortening drying times while maintaining magnet performance by reducing impurities and improving processing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159557000001_ABST
    Figure 2024159557000001_ABST
Patent Text Reader

Abstract

To provide an organic paste having a gradient volatilization rate and a method of preparing the same.SOLUTION: An organic paste comprises a rare earth powder, organic solvent and resin, and further a dispersant and / or an anti-settling agent and / or a synergist, having components by weight percentage of 50%-90% of a rare earth powder, 8%-50% of organic solvent, 0.4%-6% of resin, 0%-5% of a dispersant, 0%-3% of an anti-settling agent and 0%-3% of a synergist. The method of preparing includes: weighing a rare earth powder, organic solvent, resin, a dispersant and / or an anti-settling agent and / or a synergist by weight percentage respectively; obtaining an organic carrier by adding weighed components in order into a mixer so that they are stirred at constant temperature and then cooled down to room temperature; obtaining a coarse organic paste by adding the organic carrier and the rare earth powder weighed into a vacuum high-speed disperser; and obtaining a fine organic paste by transferring the coarse organic paste into a gap-adjustable triple roll mill to perform abrasion.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of screen printing technology, and in particular to an organic paste with gradient evaporation rate and a method for preparing the same. [Background technology]

[0002] Since the discovery of NdFeB (neodymium iron boron) permanent magnet material in the 1980s, it has been widely used in many fields such as the electronic information industry and the medical industry due to its excellent properties such as high remanence, coercive force, and maximum magnetic energy product. In recent years, in order to meet the required performance of sintered neodymium magnets used in drive motors for new energy vehicles and direct drive permanent magnet units for wind power generation, it is usually necessary to improve the coercive force by subjecting the magnet to grain boundary diffusion treatment. In traditional grain boundary diffusion, heavy rare earth monomers, fluorides, hydrides, oxides and alloys are often used as diffusion sources and applied to the magnet surface by methods such as sputtering, deposition, electrophoresis, surface coating and impregnation. The above diffusion sources have low diffusion efficiency, large usage, and there is no low-cost grain boundary diffusion process suitable for industrialized mass stable production, which limits the development and application promotion of high-end NdFeB magnets.

[0003] To make up for the shortcomings of the existing grain boundary diffusion method, screen printing technology has been applied to the neodymium industry. Screen printing refers to using a screen plate and paste, and printing the paste onto the substrate through the holes in the plate by scraping. The screen printing method integrates the advantages of the sputtering method and the surface coating method, and is expected to develop into the mainstream process of NdFeB grain boundary diffusion, with low cost, high production efficiency, and easy automation. As the raw material of screen printing, the paste has a direct impact on the printing and subsequent diffusion effects.

[0004] In the prior art, the paste is mainly produced by dispersing rare earth powder in an organic solution such as alcohol / acetone under stirring. It is difficult for the organic paste to simultaneously meet the requirements of low volatilization rate at room temperature and high volatilization rate at high temperature. Due to the high volatilization rate at room temperature, a large amount of organic solvent in the paste will volatilize during the printing process, which increases the viscosity of the organic paste and makes it difficult to pass through the screen, while the low volatilization rate at high temperature not only prolongs the drying time, but also causes the flow of the coated film layer, making the film layer uneven, and ultimately affecting the diffusion effect. Summary of the Invention

[0005] The object of the present invention is to provide an organic paste with gradient evaporation rate and a preparation method thereof, thereby solving at least one of the above technical problems and realizing gradient evaporation of the paste.

[0006] An embodiment of the present invention is implemented as follows.

[0007] An organic paste having a gradient volatility rate, comprising a rare earth powder, an organic solvent and a resin, further comprising a dispersant and / or an anti-settling agent and / or a synergist, the weight percentage of each component being: Rare earth powder 50%~90%, Organic solvent 8%~50%, Resin 0.4%~6%, Dispersant 0%~5% Anti-settling agent 0%~3%, Synergist 0%-3%.

[0008] In a preferred embodiment of the present invention, the rare earth powder in the above-mentioned NdFeB screen printing organic paste comprises one or two mixtures selected from the following: pure metal powder of heavy rare earth element, alloy powder containing heavy rare earth element or light rare earth element, and heavy rare earth powder containing hydride, fluoride and oxide of heavy rare earth element.

[0009] In a preferred embodiment of the present invention, the pure metal powder in the NdFeB screen printing organic paste contains one or a mixture of two or more of Tb, Dy, Ho, and Gd; The alloy powder is configured, in weight percent, as RExMy, where RE is one or a mixture of two or more of Tb, Dy, Ho, Gd, Pr, Nd, La, Ce, Y, and M is one or a mixture of two or more of Ga, Cu, Al, Ni, Fe, and 60≦x≦95, 5≦y≦40.

[0010] In a preferred embodiment of the present invention, the particle size of the rare earth powder in the above NdFeB screen printing organic paste is D50<3μm.

[0011] In a preferred embodiment of the present invention, the organic solvent in the above-mentioned NdFeB screen printing organic paste comprises one or a mixture of two or more of propylene glycol phenyl ether, DBE, methyl isobutyl ketone and propylene glycol methyl ether acetate.

[0012] In a preferred embodiment of the present invention, the resin in the above-mentioned NdFeB screen printing organic paste comprises one or a mixture of two or more of ethyl cellulose, polyvinyl butyral, acrylic resin, polyvinyl chloride resin, polyester resin and polyurethane.

[0013] Its technical effect is that the resin improves the adhesion of the organic paste to the substrate and ensures the subsequent grain boundary diffusion effect.

[0014] In a preferred embodiment of the present invention, the dispersant in the NdFeB screen printing organic paste comprises one or a mixture of two or more of polyvinyl butyral, polyvinylpyrrolidone, sodium polyacrylate and polyvinylamide.

[0015] The technical effect is that the dispersant prevents re-agglomeration of the diffusion source powder in the organic paste, reduces the powderiness of the organic paste itself, and enhances the uniformity of the weight gain during screen printing.

[0016] In a preferred embodiment of the present invention, the anti-settling agent in the above NdFeB screen printing organic paste comprises one or a mixture of two or more of polyamide wax, polyethylene wax, organic bentonite and fumed silica.

[0017] The technical effects of this are that the anti-settling agent improves the stability of the organic paste when left standing, inhibits the occurrence of delamination, and further reduces the room temperature volatilization rate.

[0018] In a preferred embodiment of the present invention, the synergist in the above NdFeB screen printing organic paste is one or a mixture of two or more of modified polyhydroxycarboxylic acid ester, BYK-SYNERGIST 2105, BYK-SYNERGIST 2100.

[0019] The technical effect is that the synergist can improve the mesh structure of the organic carrier.

[0020] In a preferred embodiment of the present invention, the weight percentage of each component in the NdFeB screen printing organic paste is: Pure metal powder 65%~75%, 10% to 30% of one or more of propylene glycol phenyl ether, DBE, and propylene glycol methyl ether acetate, 0.4% to 4% of one or more of ethyl cellulose, polyvinyl butyral, and polyester resin, Polyethylene glycol, polyvinylpyrrolidone, and polyvinylamide, 0% to 3% of one or more of these, Modified polyhydroxycarboxylic acid ester, BYK-SYNERGIST 2105 and / or BYK-SYNERGIST 2100, 0%-2%.

[0021] In a preferred embodiment of the present invention, the weight percentage of each component in the NdFeB screen printing organic paste is: Alloy powder 70%~80%, 20% to 30% of one or more of propylene glycol phenyl ether, DBE, and propylene glycol methyl ether acetate, 0.4% to 5% of one or more of acrylic resin, polyurethane and polyester resin, Polyethylene glycol, polyvinylpyrrolidone, and polyvinylamide, 0% to 3% of one or more of these, Polyamide wax and / or polyethylene wax, 0% to 2% Modified polyhydroxycarboxylic acid ester, BYK-SYNERGIST 2105 and / or BYK-SYNERGIST 2100, 0%-2%.

[0022] In a preferred embodiment of the present invention, the weight percentage of each component in the NdFeB screen printing organic paste is: Heavy rare earth powder 60%~80%, DBE and / or propylene glycol methyl ether acetate, 10% to 30%, 0.4% to 4% of one or more of vinyl chloride resin, polyester resin, and polyurethane, Polyethylene glycol, polyvinylpyrrolidone, and polyvinylamide, 0% to 3% of one or more of these, Polyamide wax and / or polyethylene wax, 0% to 2% Modified polyhydroxycarboxylic acid ester, BYK-SYNERGIST 2105 and / or BYK-SYNERGIST 2100, 0%-2%.

[0023] A method for preparing an organic paste having a gradient evaporation rate as described above, comprising the steps of: Weighing out the rare earth powder, the organic solvent, the resin, the dispersant and / or the anti-settling agent and / or the synergist, each in weight percent; the weighed rare earth powder, the organic solvent, the resin, the dispersant and / or the anti-settling agent and / or the synergist are sequentially added to a mixer, and the mixture is stirred at a constant temperature of 20 to 70°C and a rotation speed of 600 r / min to 1200 r / min for 0.25 to 6 hours, and then cooled to room temperature to obtain an organic carrier; The technical effect is that the organic carrier produced is homogeneous and free of agglomerated material; Add the organic carrier and the weighed rare earth powder to a vacuum high-speed disperser, and disperse the mixture at a high speed for 0.25 to 1 hour at a rotation speed of 1000 r / min to 4000 r / min to obtain a crude organic paste. The technical effect is that the crude organic paste produced is bubble-free and homogeneously dispersed; The coarse organic paste is transferred to a gap-adjustable three-roller mill and ground 1 to 3 times to obtain a fine organic paste; The technical effect is that the fine organic paste produced has a particle size of less than 5 μm.

[0024] The beneficial effects of the embodiments of the present invention are as follows:

[0025] In the organic paste with gradient volatilization rate and the preparation method thereof of the present invention, a gradient of organic components is formed, and the organic carrier is formed into a mesh structure by the strong interaction of polishing, so that the volatilization rate at room temperature is less than 0.05% / h, and the volatilization rate at a high temperature of 120°C is more than 1.2% / h, thereby achieving gradient volatilization of the paste. The prepared organic paste for screen printing of rare earth permanent magnet material has a low volatilization rate at room temperature, which can effectively prevent clogging and printing unevenness caused by the volatilization of organic solvent during printing, and at high temperatures, its volatilization rate is high and the curing time is short, which can greatly shorten the drying time, improve the processing efficiency, and reduce the amount of oxygen, carbon and other impurities entering the magnet during the curing and subsequent heat treatment stages. [Brief description of the drawings]

[0026] In order to more clearly explain the technical solutions of the embodiments of the present invention, the drawings used in the embodiments are briefly introduced below. However, the following drawings only illustrate certain embodiments of the present invention, and should not be regarded as limiting the scope. It should be understood that those skilled in the art can obtain other related drawings based on these drawings without creative efforts. [Figure 1] FIG. 2 is a schematic diagram showing the flow of a method for preparing an organic paste having a gradient evaporation rate according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram of the volatilization profile of an example of an organic paste having a gradient volatilization rate according to the present invention, which was held at 40° C., 80° C., and 120° C. for 2 hours. [Diagram 3] FIG. 2 is a schematic diagram of the volatilization profile of a comparative example of an organic paste having a gradient volatilization rate according to the present invention, which was held at 40° C., 80° C., and 120° C. for 2 hours. [Figure 4] FIG. 2 is a schematic diagram showing a metal structure photograph of a coating surface of an example of an organic paste having a gradient volatilization rate according to the present invention after drying at 120° C. for 10 minutes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] In order to more clearly describe the objectives, technical solutions and advantages of the embodiments of the present invention, the following clearly and completely describes the technical solutions in the embodiments of the present invention in conjunction with the drawings in the embodiments of the present invention, and it is obvious that the described embodiments are only a part, but not all, of the embodiments of the present invention. In general, the components of the embodiments of the present invention described and illustrated in the drawings can be arranged and designed in various configurations.

[0028] A first embodiment of the present invention provides an organic paste having a gradient volatility rate, comprising a rare earth powder, an organic solvent and a resin, further comprising a dispersant and / or an anti-settling agent and / or a synergist, the weight percentage of each component being: Rare earth powder 50%~90%, Organic solvent 8%~50%, Resin 0.4%~6%, Dispersant 0%~5% Anti-settling agent 0%~3%, Synergist 0%-3%.

[0029] Preferably, the weight percentage of each component is: Rare earth powder 60%~80%, Organic solvent 10% to 30%, Resin 0.4%~5%, Dispersant 0%~3%, Anti-settling agent 0%~2%, Synergist: 0%-2%.

[0030] In a preferred embodiment of the present invention, the rare earth powder in the above-mentioned NdFeB screen printing organic paste comprises one or two mixtures selected from the following: pure metal powder of heavy rare earth element, alloy powder containing heavy rare earth element or light rare earth element, and heavy rare earth powder containing hydride, fluoride and oxide of heavy rare earth element.

[0031] In a preferred embodiment of the present invention, the pure metal powder in the NdFeB screen printing organic paste includes one or a mixture of two or more of Tb, Dy, Ho, and Gd.

[0032] The alloy powder is RE in weight percentage x M y and is composed of, where RE is one or a mixture of two or more of Tb, Dy, Ho, Gd, Pr, Nd, La, Ce, Y, and M is one or a mixture of two or more of Ga, Cu, Al, Ni, Fe, and 60 ≦ x ≦ 95, 5 ≦ y ≦ 40.

[0033] In a preferred embodiment of the present invention, the pure metal powder in the organic paste for NdFeB screen printing contains one or two of Tb and Dy.

[0034] The alloy powder is RE in weight percentage x M y and is composed of, where RE is one or a mixture of two or more of Tb, Dy, Pr, Nd. When RE is Tb, M is one or a mixture of two or more of Ga, Cu, Al, Ni, and 70 ≦ x ≦ 90, 10 ≦ y ≦ 30. When RE is Dy, M is one or a mixture of two or more of Ni, Fe, Ga, and 60 ≦ x ≦ 80, 20 ≦ y ≦ 40. When RE is two or three of Tb, Pr, Nd, M is one or a mixture of two of Cu and Al, and 80 ≦ x ≦ 95, 5 ≦ y ≦ 20. By adding the above alloying elements, the melting point of the diffusion source decreases, the diffusion changes from solid-liquid diffusion to liquid-liquid diffusion, and the diffusion efficiency is greatly improved. Also, after the above alloying elements diffuse into the magnet, most of them are distributed at the grain boundaries, and the intergranular magnetic exchange coupling can be reduced.

[0035] In a preferred embodiment of the present invention, the particle size of the rare earth powder in the organic paste for NdFeB screen printing is D50 < 3 μm.

[0036] Preferably, the particle size of the rare earth powder is 1.6 < D50 < 2.4. When the particle size of the powder is within this range, due to the small particle size of the powder, the preparation efficiency of the powder will not be significantly reduced, and excellent stability can be obtained.

[0037] In a preferred embodiment of the present invention, the organic solvent in the above-mentioned NdFeB screen printing organic paste comprises one or a mixture of two or more of propylene glycol phenyl ether, DBE, methyl isobutyl ketone and propylene glycol methyl ether acetate.

[0038] Preferably, the organic solvent is one or a mixture of two or more of propylene glycol phenyl ether, DBE, and propylene glycol methyl ether acetate, and since the above organic solvents are easily volatilized at high temperatures, they can improve the drying efficiency after screen printing, reduce impurities such as C and O that enter the interior of the magnet during grain boundary diffusion, and ensure the performance of the magnet after diffusion.

[0039] In a preferred embodiment of the present invention, the resin in the above-mentioned NdFeB screen printing organic paste comprises one or a mixture of two or more of ethyl cellulose, polyvinyl butyral, acrylic resin, polyvinyl chloride resin, polyester resin and polyurethane.

[0040] Preferably, the resin is one or a mixture of two or more of polyvinyl butyral, polyvinyl chloride resin, polyester resin and polyurethane, and the resin has a high molecular weight, and a small amount of the resin can significantly improve the viscosity of the organic paste. The resin has a low thermal decomposition rate, and can reduce the intrusion of C and O elements into the magnet by grain boundary diffusion treatment.

[0041] Its technical effect is that the resin improves the adhesion of the organic paste to the substrate and ensures the subsequent grain boundary diffusion effect.

[0042] In a preferred embodiment of the present invention, the dispersant in the NdFeB screen printing organic paste comprises one or a mixture of two or more of polyvinyl butyral, polyvinylpyrrolidone, sodium polyacrylate and polyvinylamide.

[0043] Preferably, the dispersant is one or a mixture of two or more of polyethylene glycol, polyvinylpyrrolidone, and polyvinylamide. The dispersant is easily soluble in an organic solvent and has good wettability with respect to the diffusion source powder, and is therefore advantageous for dispersing the diffusion source powder.

[0044] The technical effect is that the dispersant prevents re-agglomeration of the diffusion source powder in the organic paste, reduces the powderiness of the organic paste itself, and enhances the uniformity of the weight gain during screen printing.

[0045] In a preferred embodiment of the present invention, the anti-settling agent in the above NdFeB screen printing organic paste comprises one or a mixture of two or more of polyamide wax, polyethylene wax, organic bentonite and fumed silica.

[0046] Preferably, the anti-settling agent includes a mixture of one or two of polyamide wax and polyethylene wax, and the anti-settling agent is completely decomposed at high temperatures, so that the C remaining on the magnet surface during high-temperature grain boundary diffusion can be reduced. The technical effects of the anti-settling agent are that the anti-settling agent improves the stability of the organic paste when left standing, suppresses the occurrence of delamination, and further reduces the room temperature volatilization rate.

[0047] In a preferred embodiment of the present invention, the synergist in the above NdFeB screen printing organic paste is one or a mixture of two or more of modified polyhydroxycarboxylic acid ester, BYK-SYNERGIST 2105, BYK-SYNERGIST 2100.

[0048] Preferably, the synergist is a modified polyhydroxycarboxylic acid ester, and the addition of the synergist can greatly improve the high-temperature drying speed of the organic paste without affecting the room temperature evaporation rate, and can reliably achieve a gradient evaporation rate.

[0049] The technical effect is that the synergist can improve the mesh structure of the organic carrier.

[0050] In a preferred embodiment of the present invention, the weight percentage of each component in the NdFeB screen printing organic paste is: Pure metal powder 65%~75%, 10% to 30% of one or more of propylene glycol phenyl ether, DBE, and propylene glycol methyl ether acetate, 0.4% to 4% of one or more of ethyl cellulose, polyvinyl butyral, and polyester resin, Polyethylene glycol, polyvinylpyrrolidone, and polyvinylamide, 0% to 3% of one or more of these, Modified polyhydroxycarboxylic acid ester, BYK-SYNERGIST 2105 and / or BYK-SYNERGIST 2100, 0%-2%.

[0051] In a preferred embodiment of the present invention, the weight percentage of each component in the NdFeB screen printing organic paste is: Alloy powder 70%~80%, 20% to 30% of one or more of propylene glycol phenyl ether, DBE, and propylene glycol methyl ether acetate, 0.4% to 5% of one or more of acrylic resin, polyurethane and polyester resin, Polyethylene glycol, polyvinylpyrrolidone, and polyvinylamide, 0% to 3% of one or more of these, Polyamide wax and / or polyethylene wax, 0% to 2% Modified polyhydroxycarboxylic acid ester, BYK-SYNERGIST 2105 and / or BYK-SYNERGIST 2100, 0%-2%.

[0052] In a preferred embodiment of the present invention, the weight percentage of each component in the NdFeB screen printing organic paste is: Heavy rare earth powder 60%~80%, DBE and / or propylene glycol methyl ether acetate, 10% to 30%, 0.4% to 4% of one or more of vinyl chloride resin, polyester resin, and polyurethane, Polyethylene glycol, polyvinylpyrrolidone, and polyvinylamide, 0% to 3% of one or more of these, Polyamide wax and / or polyethylene wax, 0% to 2% Modified polyhydroxycarboxylic acid ester, BYK-SYNERGIST 2105 and / or BYK-SYNERGIST 2100, 0%-2%.

[0053] Referring to FIG. 1, the second embodiment of the present invention provides a method for preparing an organic paste having the above-mentioned gradient evaporation rate, Weighing out the rare earth powder, the organic solvent, the resin, the dispersant and / or the anti-settling agent and / or the synergist, each in weight percent; the weighed rare earth powder, the organic solvent, the resin, the dispersant and / or the anti-settling agent and / or the synergist are sequentially added to a mixer, and the mixture is stirred at a constant temperature of 20 to 70°C and a rotation speed of 600 r / min to 1200 r / min for 0.25 to 6 hours, and then cooled to room temperature to obtain an organic carrier; The technical effect is that the organic carrier produced is homogeneous and free of agglomerated material; Add the organic carrier and the weighed rare earth powder to a vacuum high-speed disperser, and disperse the mixture at a high speed for 0.25 to 1 hour at a rotation speed of 1000 r / min to 4000 r / min to obtain a crude organic paste. The technical effect is that the crude organic paste produced is bubble-free and homogeneously dispersed; The coarse organic paste is transferred to a gap-adjustable three-roller mill and ground 1 to 3 times to obtain a fine organic paste; The technical effect is that the fine organic paste produced has a particle size of less than 5 μm.

[0054] Specifically, the effects of the present invention will be described in more detail with reference to the following examples and comparative examples. The distribution of various components in each example is shown in Table 1.

[0055] [Table 1] JPEG2024159557000003.jpg211170JPEG2024159557000004.jpg218170JPEG2024159557000005.jpg207170 EXAMPLES

[0056] 70%Dy 80 Ni 20 Weigh out the diffusion source powder, 15% propylene glycol methyl ether acetate, 10% DBE, 1% polyvinyl chloride resin, 2% polyester resin, and 2% sodium polyacrylate in weight percent, where Dy 80 Ni 20 The particle size of the diffusion source powder is D50=2.83 μm.

[0057] Propylene glycol methyl ether acetate, DBE, polyvinyl chloride resin, polyester resin, and sodium polyacrylate were added sequentially to the mixer and stirred at a constant temperature of 60 °C and a rotation speed of 1200 r / min for 5 h to obtain a homogeneous and non-aggregated organic carrier.

[0058] Dy 80 Ni 20 The diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and ground twice to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0059] 70%Tb 83 Cu7Al 10 The diffusion source powder, 10% methyl isobutyl ketone, 12% polyester resin, 2% acrylic resin, 0.4% polyvinylpyrrolidone, 0.6% polyvinylamide, 3% organic bentonite, 2% BYK-SYNERGIST 2100 were weighed out in weight percent, where Tb 80 Cu 10 Al 10 The particle size of the diffusion source powder is D50=2.54 μm.

[0060] Methyl isobutyl ketone, polyester resin, acrylic resin, polyvinylpyrrolidone, polyvinylamide, organic bentonite, and BYK-SYNERGIST 2100 were added sequentially to the mixer and stirred at a constant temperature of 25 °C and a rotation speed of 1000 r / min for 25 min to obtain a homogeneous and non-aggregated organic carrier.

[0061] Tb 80 Cu 10 Al 10 The diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0062] 70% Dy diffusion source powder, 10% propylene glycol, 16% methyl ether acetate, 3% polyester resin, 1% modified polyhydroxycarboxylic acid ester were weighed out in weight percent, where the particle size of the Dy diffusion source powder was D50=2.31 μm.

[0063] Propylene glycol, methyl ether acetate, polyester resin, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 50 °C and a rotation speed of 900 r / min for 6 h to obtain a homogeneous and non-aggregating organic carrier.

[0064] The Dy diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0065] 70%Pr 90 Weigh out Al5Ga5 diffusion source powder, 11% methyl isobutyl ketone, 11% polyester resin, 0.5% polyurethane, 1.5% polyester resin, 0.5% polyvinylpyrrolidone, 0.5% polyvinylamide, 1% polyamide wax, 1% polyethylene wax, 3% BYK-SYNERGIST 2105 in weight percent, where Pr 90 The particle size of the Cu5Ga5 diffusion source powder is D50=1.89 μm.

[0066] Methyl isobutyl ketone, polyester resin, polyurethane, polyester resin, polyvinylpyrrolidone, polyvinylamide, polyamide wax, polyethylene wax, and BYK-SYNERGIST 2105 were added sequentially to the mixer and stirred at a constant temperature of 30°C and a rotation speed of 1000 r / min for 1 h to obtain a homogeneous and non-aggregated organic carrier.

[0067] Pr 90 The Cu5Ga5 diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0068] 70%Dy 80 Ni 20The diffusion source powder, 12% propylene glycol methyl ether acetate, 12.5% ​​DBE, 1% polyvinyl chloride resin, 2% polyester resin, 2% sodium polyacrylate, 0.5% modified polyhydroxycarboxylic acid ester were weighed out in weight percent, where Dy 80 Ni 20 The particle size of the diffusion source powder is D50=2.5 ​​μm.

[0069] Propylene glycol methyl ether acetate, DBE, vinyl chloride resin, polyester resin, sodium polyacrylate, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 60 °C and a rotation speed of 1000 r / min for 6 h to obtain a homogeneous and non-aggregating organic carrier.

[0070] Dy 80 Ni 20 The diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and ground three times to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0071] 60% Tb-H diffusion source powder, 35% propylene glycol phenyl ether, 5% ethyl cellulose were weighed out by weight percent, where the particle size of the Tb-H diffusion source powder is D50=1.99 μm.

[0072] Propylene glycol phenyl ether and ethyl cellulose were added to the mixer in sequence and stirred at a constant temperature of 25° C. and a rotation speed of 900 r / min for 15 min to obtain a homogeneous and non-aggregated organic carrier.

[0073] The Tb-H diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2000 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0074] 70% DyO diffusion source powder, 23% propylene glycol methyl ether acetate, 1% polyester resin, 1% polyvinylpyrrolidone, 0.5% organic bentonite, 1.5% fumed silica, 2% BYK-SYNERGIST 2100 were weighed out in weight percent, where the particle size of the TbO diffusion source powder is D50=2.27 μm.

[0075] Propylene glycol methyl ether acetate, polyester resin, polyvinylpyrrolidone, organic bentonite, fumed silica, and BYK-SYNERGIST 2100 were added sequentially to the mixer and stirred at a constant temperature of 55 °C and a rotation speed of 1000 r / min for 4 h to obtain a homogeneous and non-aggregated organic carrier.

[0076] The DyO diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 30 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished three times to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0077] Weigh out 90% TbH diffusion source powder, 8% propylene glycol phenyl ether, and 2% ethyl cellulose by weight percent, where the particle size of the Tb-H diffusion source powder is D50<2.5 μm.

[0078] Propylene glycol phenyl ether and ethyl cellulose were added to the mixer in sequence and stirred at a constant temperature of 25° C. and a rotation speed of 900 r / min for 15 min to obtain a homogeneous and non-aggregated organic carrier.

[0079] The Tb-H diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2500 r / min for 50 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished twice to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0080] 70% TbF diffusion source powder, 12% propylene glycol methyl ether acetate, 10.5% DBE, 1.5% polyvinyl chloride resin, 1.5% polyester resin, 2% sodium polyacrylate, 2.5% modified polyhydroxycarboxylic acid ester were weighed out by weight percent, where Tb 80 Ni 20 The particle size of the diffusion source powder is D50=2.33 μm.

[0081] Propylene glycol methyl ether acetate, DBE, vinyl chloride resin, polyester resin, sodium polyacrylate, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 55 °C and a rotation speed of 1000 r / min for 5 h to obtain a homogeneous and non-aggregating organic carrier.

[0082] The TbF diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished three times to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0083] Weigh out 70% TbO diffusion source powder, 20% propylene glycol methyl ether acetate, 4% polyester resin, 1% polyvinylpyrrolidone, 0.5% organic bentonite, 1.5% fumed silica, 2% BYK-SYNERGIST 2100 by weight percent, where the particle size of the TbO diffusion source powder is D50=2.17 μm.

[0084] Propylene glycol methyl ether acetate, polyester resin, polyvinylpyrrolidone, organic bentonite, fumed silica, and BYK-SYNERGIST 2100 were added sequentially to the mixer and stirred at a constant temperature of 60 °C and a rotation speed of 1000 r / min for 5.5 h to obtain a homogeneous and non-aggregated organic carrier.

[0085] The TbO metal powder and the prepared organic carrier were added to a vacuum high-speed disperser and dispersed at a rotation speed of 2200 r / min for 40 minutes to prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and ground three times to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0086] 70% Tb diffusion source powder, 24% DBE, 4% polyvinyl butyral, 1% polyethylene glycol, 1% modified polyhydroxycarboxylic acid ester were weighed out by weight percent, where the particle size of the Tb diffusion source powder was D50=1.63 μm.

[0087] DBE, polyvinyl butyral, polyethylene glycol, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 25 °C and a rotation speed of 900 r / min for 15 min to obtain a homogeneous and non-aggregated organic carrier.

[0088] The Tb diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2000 r / min for 15 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0089] 50% Tb-H diffusion source powder, 44% propylene glycol phenyl ether, 6% ethyl cellulose were weighed out by weight percent, where the particle size of the Tb-H diffusion source powder is D50=2.43 μm.

[0090] Propylene glycol phenyl ether and ethyl cellulose were added to the mixer in sequence and stirred at a constant temperature of 25° C. and a rotation speed of 900 r / min for 15 min to obtain a homogeneous and non-aggregated organic carrier.

[0091] The Tb-H diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2000 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0092] 70% Dy diffusion source powder, 12% propylene glycol, 12% methyl ether acetate, 3% polyester resin, 2% polyvinylpyrrolidone, 1% modified polyhydroxycarboxylic acid ester were weighed out in weight percent, where the particle size of the Dy diffusion source powder was D50=1.67 μm.

[0093] Propylene glycol, methyl ether acetate, polyester resin, polyvinylpyrrolidone, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 45 °C and a rotation speed of 1000 r / min for 6 h to obtain a homogeneous and non-aggregating organic carrier.

[0094] The Dy diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished twice to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0095] 70% Tb diffusion source powder, 15% DBE, 12.6% polyurethane, 0.4% polyvinyl butyral, 1% polyethylene glycol, 1% modified polyhydroxycarboxylic acid ester were weighed out by weight percent, where the particle size of the Tb diffusion source powder was D50=1.84 μm.

[0096] DBE, polyvinyl butyral, polyethylene glycol, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 25 °C and a rotation speed of 900 r / min for 20 min to obtain a homogeneous and non-aggregated organic carrier.

[0097] The Tb diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 30 minutes to prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0098] 70% TbF diffusion source powder, 11% propylene glycol methyl ether acetate, 12% DBE, 1.5% polyvinyl chloride resin, 1.5% polyester resin, 2% sodium polyacrylate, and 2% modified polyhydroxycarboxylic acid ester were weighed out by weight percent, where Tb 80 Ni 20 The particle size of the diffusion source powder is D50=2.45 μm.

[0099] Propylene glycol methyl ether acetate, DBE, vinyl chloride resin, polyester resin, sodium polyacrylate, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 70 °C and a rotation speed of 1200 r / min for 5 h to obtain a homogeneous and non-aggregating organic carrier.

[0100] The TbF diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 40 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0101] 70%Tb 60 Ni 40 The diffusion source powder, 10% propylene glycol methyl ether acetate, 13.5% DBE, 2% polyvinyl chloride resin, 1% polyester resin, 2% sodium polyacrylate, 1.5% modified polyhydroxycarboxylic acid ester were weighed out in weight percent, where Tb 60 Ni 40 The particle size of the diffusion source powder is D50=2.25 μm.

[0102] Propylene glycol methyl ether acetate, DBE, vinyl chloride resin, polyester resin, sodium polyacrylate, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 65 °C and a rotation speed of 1200 r / min for 5 h to obtain a homogeneous and non-aggregating organic carrier.

[0103] Tb 60 Ni 40 The diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and ground twice to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0104] Weigh out 70% TbO diffusion source powder, 23% propylene glycol methyl ether acetate, 1% polyester resin, 1% polyvinylpyrrolidone, 0.5% organic bentonite, 1.5% fumed silica, 2% BYK-SYNERGIST 2100 by weight percent, where the particle size of the TbO diffusion source powder is D50<3 μm.

[0105] Propylene glycol methyl ether acetate, polyester resin, polyvinylpyrrolidone, organic bentonite, fumed silica, and BYK-SYNERGIST 2100 were added sequentially to the mixer and stirred at a constant temperature of 45 °C and a rotation speed of 1000 r / min for 4 h to obtain a homogeneous and non-aggregated organic carrier.

[0106] The TbO diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 35 minutes to prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished twice to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0107] 70% Dy diffusion source powder, 9% propylene glycol, 12% methyl ether acetate, 3% polyester resin, 5% polyvinylpyrrolidone, 1% modified polyhydroxycarboxylic acid ester were weighed out in weight percent, where the particle size of the Dy diffusion source powder was D50=2.46 μm.

[0108] Propylene glycol, methyl ether acetate, polyester resin, polyvinylpyrrolidone, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 55 °C and a rotation speed of 1200 r / min for 5 h to obtain a homogeneous and non-aggregating organic carrier.

[0109] The Dy diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0110] 5%Tb 82 Fe 18 , 25% La 80 Al20 , 30% Ce 80 Fe 20 The diffusion source powder, 10% propylene glycol, 12% methyl ether acetate, 2% polyester resin, 1% polyvinylpyrrolidone, 0.5% organic bentonite, 1.5% fumed silica, 1.5% modified polyhydroxy carboxylic acid ester, 1.5% BYK-SYNERGIST 2100 were weighed out in weight percent, where Tb 82 Fe 18 , La 80 Al 20 , Ce 80 Fe 20 The particle size D50 of the diffusion source powders is 2.33, 2.17 and 2.48 μm, respectively.

[0111] Propylene glycol, methyl ether acetate, polyester resin, polyvinylpyrrolidone, organic bentonite, fumed silica, modified polyhydroxycarboxylic acid ester, and BYK-SYNERGIST 2100 were added sequentially to the mixer and stirred at a constant temperature of 55 °C and a rotation speed of 1000 r / min for 5 h to obtain a homogeneous and non-aggregated organic carrier.

[0112] Tb 82 Fe 180 , La 80 Al 20 , Ce 80 Fe 20 The metal powder and the prepared organic carrier were added to a vacuum high-speed disperser and dispersed at a rotation speed of 2200 r / min for 30 minutes to prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0113] 5%Nd 90 Cu5Al5, 60%Dy 90Cu5Al5, 5% TbF diffusion source powder, 10% propylene glycol methyl ether acetate, 12% methyl isobutyl ketone, 2% polyester resin, 1% polyvinylpyrrolidone, 1% polyamide wax, 1% polyethylene wax, 2% modified polyhydroxy carboxylic acid ester, 1% BYK-SYNERGIST 2100 were weighed out in weight percent, where Nd 90 Cu5Al5, Dy 90 The particle size D50 of the Cu5Al5 and TbF diffusion source powders are 1.73, 2.07 and 1.88 μm, respectively.

[0114] Propylene glycol methyl ether acetate, methyl isobutyl ketone, polyester resin, polyvinylpyrrolidone, polyamide wax, polyethylene wax, modified polyhydroxycarboxylic acid ester, and BYK-SYNERGIST 2100 were added sequentially to the mixer and stirred at a constant temperature of 55°C and a rotation speed of 1000 r / min for 5 hours to obtain a homogeneous and non-aggregating organic carrier.

[0115] Nd 90 Cu5Al5, Dy 90 The Cu5Al5, TbF diffusion source powders and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 30 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0116] 5%Nd 90 Cu5Al5, 50%Dy 90 Cu5Al5, 15%Dy 80 Fe 20 Weigh out the diffusion source powder, 22% methyl isobutyl ketone, 2% acrylic resin, 0.5% polyvinylpyrrolidone, 0.5% polyvinylamide, 2% polyamide wax, 3% BYK-SYNERGIST 2105 in weight percent, where Nd 90 Cu5Al5, Dy 90 Cu5Al5, Dy 80 Fe20 The particle sizes D50 of the diffusion source powders are 2.02, 2.13 and 2.27 μm, respectively.

[0117] Methyl isobutyl ketone, acrylic resin, polyvinylpyrrolidone, polyvinylamide, polyamide wax, and BYK-SYNERGIST 2105 were added sequentially to the mixer and stirred at a constant temperature of 25 °C and a rotation speed of 1000 r / min for 20 min to obtain a homogeneous and non-aggregated organic carrier.

[0118] Nd 90 Cu5Al5, Dy 90 Cu5Al5, Dy 80 Fe 20 The diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 40 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and ground twice to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0119] 80% Tb-H diffusion source powder, 17% propylene glycol phenyl ether, 3% ethyl cellulose were weighed out by weight percent, where the particle size of the Tb-H diffusion source powder is D50=1.67 μm.

[0120] Propylene glycol phenyl ether and ethyl cellulose were added to the mixer in sequence and stirred at a constant temperature of 25° C. and a rotation speed of 900 r / min for 15 min to obtain a homogeneous and non-aggregated organic carrier.

[0121] The Tb-H diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2000 r / min for 45 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished three times to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0122] 10%Tb, 20%Nd 90 Cu5Al5, 40%Tb 90 Cu5Ho5 diffusion source powder, 10% methyl isobutyl ketone, 12% polyester resin, 0.5% polyurethane, 1.5% polyester resin, 0.6% polyvinylpyrrolidone, 0.4% polyvinylamide, 0.5% polyamide wax, 1.5% polyethylene wax, 3% BYK-SYNERGIST 2105 were weighed out in weight percent, where Tb, Nd 90 Cu5Al5, Tb 90 The particle size D50 of the Cu5Ho5 diffusion source powders are 1.45, 1.56 and 1.73 μm, respectively.

[0123] Methyl isobutyl ketone, polyester resin, polyurethane, polyester resin, polyvinylpyrrolidone, polyvinylamide, polyamide wax, polyethylene wax, and BYK-SYNERGIST 2105 were added sequentially to the mixer and stirred at a constant temperature of 70 °C and a rotation speed of 1200 r / min for 6 h to obtain a homogeneous and non-aggregated organic carrier.

[0124] Tb, Nd 90 Cu5Al5, Tb 90 The Cu5Ho5 diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and ground three times to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0125] 70%Tb 80 Cu 10 Al 10 Weigh out the diffusion source powder, 22% methyl isobutyl ketone, 3% acrylic resin, 0.5% polyvinylpyrrolidone, 0.5% polyvinylamide, 2% polyamide wax, 2% BYK-SYNERGIST 2100 in weight percent, where Tb 80 Cu 10 Al 10 The particle size of the diffusion source powder is D50<=2.17 μm.

[0126] Methyl isobutyl ketone, acrylic resin, polyvinylpyrrolidone, polyvinylamide, polyamide wax, and BYK-SYNERGIST 2100 were added sequentially to the mixer and stirred at a constant temperature of 25 °C and a rotation speed of 1000 r / min for 25 min to obtain a homogeneous and non-aggregated organic carrier.

[0127] Tb 80 Cu 10 Al 10 The diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0128] 70% TbF diffusion source powder, 10% propylene glycol methyl ether acetate, 12% DBE, 2% polyvinyl chloride resin, 1% polyester resin, 2% sodium polyacrylate, 3% modified polyhydroxycarboxylic acid ester were weighed out by weight percent, where Tb 80 Ni 20 The particle size of the diffusion source powder is D50=2.36 μm.

[0129] Propylene glycol methyl ether acetate, DBE, vinyl chloride resin, polyester resin, sodium polyacrylate, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 55 °C and a rotation speed of 1200 r / min for 4 h to obtain a homogeneous and non-aggregating organic carrier.

[0130] The TbF diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0131] 70% Tb diffusion source powder, 22% DBE, 6% polyvinyl butyral, 1% polyethylene glycol, 1% modified polyhydroxycarboxylic acid ester were weighed out by weight percent, where the particle size of the Tb diffusion source powder was D50=2.53 μm.

[0132] DBE, polyvinyl butyral, polyethylene glycol, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 25 °C and a rotation speed of 1000 r / min for 30 min to obtain a homogeneous and non-aggregated organic carrier.

[0133] The Tb diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2000 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0134] 70% Tb diffusion source powder, 23% DBE, 5% polyvinyl butyral, 1% polyethylene glycol, 1% modified polyhydroxycarboxylic acid ester were weighed out by weight percent, where the particle size of the Tb diffusion source powder was D50=1.93 μm.

[0135] DBE, polyvinyl butyral, polyethylene glycol, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 25 °C and a rotation speed of 900 r / min for 25 min to obtain a homogeneous and non-aggregated organic carrier.

[0136] The Tb diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and dispersed at a rotation speed of 2000 r / min for 25 minutes to prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished twice to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0137] 70% Tb diffusion source powder, 10% DBE, 16% polyurethane, 2% polyvinyl butyral, 1% polyethylene glycol, 1% modified polyhydroxycarboxylic acid ester were weighed out by weight percent, where the particle size of the Tb diffusion source powder was D50=2.07 μm.

[0138] DBE, polyvinyl butyral, polyethylene glycol, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 25 °C and a rotation speed of 600 r / min for 40 min to obtain a homogeneous and non-aggregated organic carrier.

[0139] The Tb diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 35 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0140] 70%Dy 80 Ni 20 The diffusion source powder, 11% propylene glycol methyl ether acetate, 12% DBE, 3% polyester resin, 2% polyvinylpyrrolidone, 1% modified polyhydroxycarboxylic acid ester were weighed out in weight percent, where Dy 80 Ni 20 The particle size of the diffusion source powder is D50 = 2.5 μm; Propylene glycol methyl ether acetate, DBE, polyester resin, polyvinylpyrrolidone, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 55 °C and a rotation speed of 1000 r / min for 4 h to obtain a homogeneous and non-aggregating organic carrier.

[0141] Dy 80 Ni 20The diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0142] 70% Tb diffusion source powder, 10% DBE, 17% polyurethane, 1% polyvinyl butyral, 1% polyethylene glycol, 1% modified polyhydroxycarboxylic acid ester were weighed out by weight percent, where the particle size of the Tb diffusion source powder was D50=2.36 μm.

[0143] DBE, polyvinyl butyral, polyethylene glycol, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 25 °C and a rotation speed of 900 r / min for 20 min to obtain a homogeneous and non-aggregated organic carrier.

[0144] The Tb diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and dispersed at a rotation speed of 2200 r / min for 30 minutes to prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished twice to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0145] 70%Tb 80 Cu 10 Al 10 Weigh out the diffusion source powder, 22% methyl isobutyl ketone, 3% acrylic resin, 0.5% polyvinylpyrrolidone, 0.5% polyvinylamide, 1% polyamide wax, 3% BYK-SYNERGIST 2100 in weight percent, where Tb 80 Cu 10 Al 10 The particle size of the diffusion source powder is D50=1.91 μm.

[0146] Methyl isobutyl ketone, acrylic resin, polyvinylpyrrolidone, polyvinylamide, polyamide wax, and BYK-SYNERGIST 2100 were added sequentially to the mixer and stirred at a constant temperature of 25 °C and a rotation speed of 1000 r / min for 25 min to obtain a homogeneous and non-aggregated organic carrier.

[0147] Tb 80 Cu 10 Al 10 The diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 45 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and ground three times to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0148] 70% TbO diffusion source powder, 22% propylene glycol methyl ether acetate, 2% polyester resin, 2% polyvinylpyrrolidone, 0.5% organic bentonite, 1.5% fumed silica, 2% BYK-SYNERGIST 2100 were weighed out in weight percent, where the particle size of the TbO diffusion source powder is D50=2.38 μm.

[0149] Propylene glycol methyl ether acetate, polyester resin, polyvinylpyrrolidone, organic bentonite, fumed silica, and BYK-SYNERGIST 2100 were added sequentially to the mixer and stirred at a constant temperature of 45 °C and a rotation speed of 1000 r / min for 4 h to obtain a homogeneous and non-aggregated organic carrier.

[0150] The TbO diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 30 minutes to prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished three times to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0151] 30%Nd 90Cu5Al5, 20%Y 80 Fe 20 , 20% Tb diffusion source powder, 10% propylene glycol methyl ether acetate, 12% DBE, 0.5% polyester resin, 1.5% polyester resin, 1% acrylic resin, 2% polyamide wax, 1% modified polyhydroxy carboxylic acid ester, 2% BYK-SYNERGIST 2105 were weighed out in weight percent, where Nd 90 Cu5Al5, Y 80 Fe 20 The particle sizes D50 of the Tb diffusion source powders are 1.67, 1.85 and 2.02 μm, respectively.

[0152] Propylene glycol methyl ether acetate, DBE, polyester resin, polyester resin, acrylic resin, polyamide wax, modified polyhydroxycarboxylic acid ester, and BYK-SYNERGIST 2105 were added sequentially to the mixer and stirred at a constant temperature of 55 °C and a rotation speed of 1200 r / min for 3 h to obtain a homogeneous and non-aggregated organic carrier.

[0153] Nd 90 Cu5Al5, Y 80 Fe 20 The Tb diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0154] 70% DyO diffusion source powder, 22% propylene glycol methyl ether acetate, 4% polyester resin, 2% polyvinylpyrrolidone, 0.5% organic bentonite, 1.5% fumed silica, 2% BYK-SYNERGIST 2100 were weighed out in weight percent, where the particle size of the TbO diffusion source powder is D50=2.32 μm.

[0155] Propylene glycol methyl ether acetate, polyester resin, polyvinylpyrrolidone, organic bentonite, fumed silica, and BYK-SYNERGIST 2100 were added sequentially to the mixer and stirred at a constant temperature of 55 °C and a rotation speed of 1000 r / min for 5 h to obtain a homogeneous and non-aggregated organic carrier.

[0156] The DyO diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 30 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0157] 70%Dy 80 Ni 20 The diffusion source powder, 11% propylene glycol methyl ether acetate, 13% DBE, 2% polyvinyl chloride resin, 1% polyester resin, 2% sodium polyacrylate, 1% modified polyhydroxycarboxylic acid ester were weighed out in weight percent, where Tb 80 Ni 20 The particle size of the diffusion source powder is D50=1.99 μm.

[0158] Propylene glycol methyl ether acetate, DBE, vinyl chloride resin, polyester resin, sodium polyacrylate, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 65 °C and a rotation speed of 1200 r / min for 6 h to obtain a homogeneous and non-aggregating organic carrier.

[0159] Dy 80 Ni 20 The diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 45 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and ground twice to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0160] 70% DyO diffusion source powder, 20% propylene glycol methyl ether acetate, 4% polyester resin, 1% polyvinylpyrrolidone, 0.5% organic bentonite, 1.5% fumed silica, 2% BYK-SYNERGIST 2100 were weighed out in weight percent, where the particle size of the TbO diffusion source powder is D50=2.35 μm.

[0161] Propylene glycol methyl ether acetate, polyester resin, polyvinylpyrrolidone, organic bentonite, fumed silica, and BYK-SYNERGIST 2100 were added sequentially to the mixer and stirred at a constant temperature of 79 °C and a rotation speed of 1200 r / min for 6 h to obtain a homogeneous and non-aggregated organic carrier.

[0162] The TbO metal powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 30 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0163] 70% Dy diffusion source powder, 11% propylene glycol, 12% methyl ether acetate, 3% polyester resin, 3% polyvinylpyrrolidone, 1% modified polyhydroxycarboxylic acid ester were weighed out in weight percent, where the particle size of the Dy diffusion source powder was D50=1.96 μm.

[0164] Propylene glycol, methyl ether acetate, polyester resin, polyvinylpyrrolidone, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 70 °C and a rotation speed of 900 r / min for 5 h to obtain a homogeneous and non-aggregating organic carrier.

[0165] The Dy diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished twice to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0166] 10%Nd 90 Cu5Al5, 40%Dy 90 Cu5Al5, 20%Dy 80 Fe 20 Weigh out the diffusion source powder, 11% propylene glycol methyl ether acetate, 11% DBE, 1% polyester resin, 1% polyester resin, 1% acrylic resin, 2% polyamide wax, 1% modified polyhydroxy carboxylic acid ester, and 2% BYK-SYNERGIST 2105 in weight percent, where Nd 90 Cu5Al5, Dy 90 Cu5Al5, Dy 80 Fe 20 The particle sizes D50 of the diffusion source powders are 2.34, 2.47 and 2.35 μm, respectively.

[0167] Propylene glycol methyl ether acetate, DBE, polyester resin, polyester resin, acrylic resin, polyamide wax, modified polyhydroxycarboxylic acid ester, and BYK-SYNERGIST 2105 were added sequentially to the mixer and stirred at a constant temperature of 55 °C and a rotation speed of 1000 r / min for 5 h to obtain a homogeneous and non-aggregated organic carrier.

[0168] Nd 90 Cu5Al5, Dy 90 Cu5Al5, Dy 80 Fe 20 The diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 35 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0169] 70% Dy diffusion source powder, 10% propylene glycol, 12% methyl ether acetate, 3% polyester resin, 4% polyvinylpyrrolidone, 1% modified polyhydroxycarboxylic acid ester were weighed out in weight percent, where the particle size of the Dy diffusion source powder was D50=1.97 μm.

[0170] Propylene glycol, methyl ether acetate, polyester resin, polyvinylpyrrolidone, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 55 °C and a rotation speed of 1000 r / min for 4.5 h to obtain a homogeneous and non-aggregating organic carrier.

[0171] The Dy diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished three times to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0172] 70% Tb-H diffusion source powder, 26% propylene glycol phenyl ether, 4% ethyl cellulose were weighed out by weight percent, where the particle size of the Tb-H diffusion source powder is D50=1.64 μm.

[0173] Propylene glycol phenyl ether and ethyl cellulose were added to the mixer in sequence and stirred at a constant temperature of 25° C. and a rotation speed of 600 r / min for 15 min to obtain a homogeneous and non-aggregated organic carrier.

[0174] The Tb-H diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2000 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0175] 70% Dy diffusion source powder, 15% propylene glycol, 10% methyl ether acetate, 3% polyester resin, 1% polyvinylpyrrolidone, 1% modified polyhydroxycarboxylic acid ester were weighed out by weight percent, where the particle size of the Dy diffusion source powder was D50=2.06 μm.

[0176] Propylene glycol, methyl ether acetate, polyester resin, polyvinylpyrrolidone, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 45 °C and a rotation speed of 1200 r / min for 6 h to obtain a homogeneous and non-aggregating organic carrier.

[0177] The Dy diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2300 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished twice to obtain an organic paste with a fineness of less than 5 μm. EXAMPLES

[0178] 70% Tb diffusion source powder, 25% DBE, 3% polyvinyl butyral, 1% polyethylene glycol, 1% modified polyhydroxycarboxylic acid ester were weighed out by weight percent, where the particle size of the Tb diffusion source powder was D50=2.08 μm.

[0179] DBE, polyvinyl butyral, polyethylene glycol, and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 25 °C and a rotation speed of 900 r / min for 20 min to obtain a homogeneous and non-aggregated organic carrier.

[0180] The Tb diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2000 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm.

[0181] <Comparative Example 1> 60% Tb diffusion source powder, 35.7% absolute ethanol, 2% polyvinyl butyral, 1% polyvinylpyrrolidone, 1% polyamide wax and 0.3% modified polyhydroxycarboxylic acid ester are weighed out by weight percent, where the particle size of the Tb diffusion source powder is D50<3 μm.

[0182] Anhydrous ethanol, polyvinyl butyral, polyvinylpyrrolidone, polyamide wax and modified polyhydroxycarboxylic acid ester were added sequentially to the mixer and stirred at a constant temperature of 25°C and a rotation speed of 900 r / min for 15 min to obtain a homogeneous and non-aggregated organic carrier.

[0183] The Tb diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2000 r / min for 25 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm.

[0184] <Comparative Example 2> 80% TbNi diffusion source powder, 17.5% acetone, 1.5% polyvinyl butyral, 1% polyethylene glycol were weighed out by weight percent, where the particle size of the TbNi diffusion source powder was D50<3 μm.

[0185] Acetone, polyvinyl butyral, and polyethylene glycol were added sequentially to the mixer and stirred at a constant temperature of 25°C and a rotation speed of 1000 r / min for 20 min to obtain a homogeneous and non-aggregated organic carrier.

[0186] The weighed TbNi diffusion source powder and the prepared organic carrier were added to a vacuum high-speed disperser and high-speed dispersed at a rotation speed of 2200 r / min for 15 minutes to pre-prepare an organic paste. The organic paste obtained by high-speed dispersion was then transferred to a three-roller mill and polished once to obtain an organic paste with a fineness of less than 5 μm.

[0187] The organic pastes for neodymium magnet screen printing with gradient volatilization rates prepared in Examples 1 to 4 and the organic pastes prepared in Comparative Examples 1 and 2 were sequentially tested for volatilization profiles when held at 40°C, 80°C, and 120°C for 2 hours, and the results are shown in Figures 2 and 3. As can be seen from Figure 2, Examples 1 to 4 have extremely low volatilization rates at 40°C, all of which are less than 0.15%, ensuring storage and printing stability, and when the temperature is raised to 120°C, the volatilization rate increases significantly, ensuring drying efficiency. As can be seen from Figure 3, Comparative Examples 1 and 2 have very high volatilization rates at high temperatures, but the volatilization rates at 40°C exceed 10% and 40%, respectively, which seriously affect the stability of the organic paste during printing and are not suitable for continuous production.

[0188] The organic paste prepared in Example 1 was applied to the surface of a neodymium magnet by screen printing and dried at 120°C for 10 minutes, after which the magnet coating was observed using a metallurgical microscope as shown in Figure 4. The coating after drying had good uniformity, no obvious cracks or bubbles, and was well bonded to the substrate, which indicates that the volatilization rate of the organic substances during the drying process was appropriate.

[0189] The organic pastes prepared in Examples 1 to 8 were applied to the surface of the neodymium magnet by screen printing, and after drying, the neodymium magnet was heat-treated at 900°C for 5 hours, and then tempered at 500°C for 3 hours. The measured magnet performance is shown in Table 2. The reduction in remanence magnetization after diffusion is < 0.3 kGs. It can be seen that the organic paste did not affect the subsequent diffusion process.

[0190] [Table 2] The embodiments of the present invention aim to provide an organic paste with gradient volatilization rate and its preparation method, and have the following effects:

[0191] The organic component gradient is formed, and the organic carrier is formed into a mesh structure by the strong interaction of polishing, so that the volatilization rate at room temperature is less than 0.05% / h, and the volatilization rate at a high temperature of 120°C is more than 1.2% / h, thereby achieving gradient volatilization of the paste. The prepared organic paste for screen printing of rare earth permanent magnet material has a low volatilization rate at room temperature, which can effectively prevent clogging and printing unevenness caused by the volatilization of organic solvent during printing, and at high temperatures, its volatilization rate is high and the curing time is short, which can greatly shorten the drying time, improve the processing efficiency, and reduce the amount of oxygen, carbon and other impurities that enter the magnet during the curing and subsequent heat treatment stages.

[0192] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and are not intended to limit the present invention. Therefore, any modifications, equivalent replacements, improvements, etc. made without departing from the spirit and scope of the present invention shall be included in the protection scope of the present invention. Furthermore, the claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.

Claims

1. The composition includes a rare earth powder, an organic solvent, and a resin, and further includes a dispersant and / or an anti-settling agent and / or a synergist, the weight percentage of each component being: Rare earth powder 50% to 90% Organic solvent 8% to 50%, Resin 0.4% to 6%, Dispersant 0% to 5% Anti-settling agent 0% to 3%, An organic paste with a gradient stripping rate, characterized by 0% to 3% synergist.

2. 2. The organic paste having a gradient volatilization rate according to claim 1, characterized in that the rare earth powder comprises a mixture of one or two kinds selected from a pure metal powder of a heavy rare earth element, an alloy powder containing a heavy rare earth element or a light rare earth element, and a heavy rare earth powder of a hydride, a fluoride, or an oxide containing a heavy rare earth element.

3. The pure metal powder contains one or a mixture of two or more of Tb, Dy, Ho, and Gd, The alloy powder comprises, in weight percent, RE x M y wherein RE is one or a mixture of two or more of Tb, Dy, Ho, Gd, Pr, Nd, La, Ce, and Y; M is one or a mixture of two or more of Ga, Cu, Al, Ni, and Fe; and 60≦x≦95, 5≦y≦40. The NdFeB screen printing organic paste according to claim 2,

4. The organic paste with gradient volatilization rate according to claim 1 , wherein the rare earth powder has a particle size of D50<3 μm.

5. The organic paste having a gradient volatility according to claim 2, characterized in that the organic solvent comprises one or a mixture of two or more of propylene glycol phenyl ether, DBE, methyl isobutyl ketone and propylene glycol methyl ether acetate.

6. The organic paste having a gradient volatility rate according to claim 5, characterized in that the resin comprises one or a mixture of two or more of ethyl cellulose, polyvinyl butyral, acrylic resin, polyvinyl chloride resin, polyester resin and polyurethane.

7. 7. The organic paste having a gradient volatility rate according to claim 6, characterized in that the dispersant comprises one or a mixture of two or more of polyvinyl butyral, polyvinyl pyrrolidone, sodium polyacrylate and polyvinyl amide.

8. 8. The organic paste with gradient volatility according to claim 7, characterized in that the anti-settling agent comprises one or a mixture of two or more of polyamide wax, polyethylene wax, organic bentonite and fumed silica.

9. The organic paste with gradient evaporation rate according to claim 8, characterized in that the synergist comprises one or a mixture of two or more of modified polyhydroxycarboxylic acid esters, BYK-SYNERGIST 2105 and BYK-SYNERGIST 2100.

10. The weight percentage of each component is: Pure metal powder 65% to 75%, 10% to 30% of one or more of propylene glycol phenyl ether, DBE, and propylene glycol methyl ether acetate; 0.4% to 4% of one or more of ethyl cellulose, polyvinyl butyral, and polyester resin; 0% to 3% of one or more of polyethylene glycol, polyvinylpyrrolidone, and polyvinylamide; The organic paste with gradient evaporation rate according to claim 8, characterized in that one or more of the modified polyhydroxycarboxylic acid ester, BYK-SYNERGIST 2105 and BYK-SYNERGIST 2100 are present in an amount of 0% to 2%.

11. The weight percentage of each component is: Alloy powder 70% to 80%, 20% to 30% of one or more of propylene glycol phenyl ether, DBE, and propylene glycol methyl ether acetate; 0.4% to 5% of one or more of acrylic resin, polyurethane and polyester resin, 0% to 3% of one or more of polyethylene glycol, polyvinylpyrrolidone, and polyvinylamide; 0% to 2% of one or both of polyamide wax and polyethylene wax; The organic paste with gradient evaporation rate according to claim 8, characterized in that one or more of the modified polyhydroxycarboxylic acid ester, BYK-SYNERGIST 2105 and BYK-SYNERGIST 2100 are present in an amount of 0% to 2%.

12. The weight percentage of each component is: Heavy rare earth powder 60% to 80%, 10% to 30% of one or both of DBE and propylene glycol methyl ether acetate, 0.4% to 4% of one or more of vinyl chloride resin, polyester resin, and polyurethane, 0% to 3% of one or more of polyethylene glycol, polyvinylpyrrolidone, and polyvinylamide; 0% to 2% of one or both of polyamide wax and polyethylene wax; The organic paste with gradient evaporation rate according to claim 8, characterized in that one or more of the modified polyhydroxycarboxylic acid ester, BYK-SYNERGIST 2105 and BYK-SYNERGIST 2100 are present in an amount of 0% to 2%.

13. Weighing out the rare earth powder, the organic solvent, the resin, the dispersant and / or the anti-settling agent and / or the synergist, each in weight percent; the weighed rare earth powder, the organic solvent, the resin, the dispersant and / or the anti-settling agent and / or the synergist are sequentially added to a mixer, and the mixture is stirred at a constant temperature of 20 to 70° C. and a rotation speed of 600 r / min to 1200 r / min for 0.25 to 6 hours, and then cooled to room temperature to obtain an organic carrier; Add the organic carrier and the weighed rare earth powder to a vacuum high-speed disperser and disperse the mixture at a high speed at a rotation speed of 1000 r / min to 4000 r / min for 0.25 to 1 hour to obtain a crude organic paste. The method for preparing an organic paste having a gradient volatilization rate according to any one of claims 1 to 12, characterized in that the coarse organic paste is transferred to a gap-adjustable three-roller mill and ground 1 to 3 times to obtain a fine organic paste.

Citation Information

Patent Citations

  • Method for manufacturing r-t-b based sintered magnet

    JP2017162900A

  • Method for manufacturing r-t-b based sintered magnet

    JP2018026390A