Method for manufacturing etching mask pattern and resin composition for etching mask pattern formation
Patent Information
- Application Number
- JP2024067050
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-22
- Filing Date
- 2024-04-17
- Publication Date
- 2024-11-08
Smart Images

Figure 2024159590000042 
Figure 2024159590000043 
Figure 2024159590000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an etching mask pattern and a resin composition for forming an etching mask pattern. [Background technology]
[0002] In recent years, with the further miniaturization of large-scale integrated circuits (LSIs), there is a demand for technology to process more delicate structures. In response to such demands, technology is being developed to form finer patterns by utilizing a phase-separated structure formed by the self-organization of a block copolymer in which mutually incompatible blocks are bonded together (see, for example, Patent Document 1). In order to utilize the phase separation structure of a block copolymer, it is essential to form the self-organized nanostructure formed by microphase separation only in a specific region and to align it in a desired direction. To achieve this position control and orientation control, processes such as graphoepitaxy, which controls the phase separation pattern by a guide pattern, and chemical epitaxy, which controls the phase separation pattern by differences in the chemical state of the substrate, have been proposed (see, for example, Non-Patent Document 1).
[0003] Block copolymers form structures with regular periodic structures through phase separation. The "period of the structure" refers to the period of the phase structure observed when a phase-separated structure is formed, and refers to the sum of the lengths of each phase that is incompatible with each other. When the phase-separated structure forms a cylindrical structure perpendicular to the substrate surface, the period (L0) of the structure is the center-to-center distance (pitch) between two adjacent cylindrical structures.
[0004] L0 ∝ a N 2 / 3 χ 1 / 6 (1) [In the formula, L0 represents the period of the structure, a represents a parameter indicating the size of the monomer, N represents the degree of polymerization, and χ represents an interaction parameter, and the larger this value is, the higher the phase separation performance is.]
[0005] Therefore, the period (L0) of the structure can be adjusted by adjusting the composition and total molecular weight of the block copolymer. The periodic structure formed by block copolymers changes from cylinders to lamellae to spheres depending on the volume ratio of the polymer components, and the period is known to depend on the molecular weight.
[0006] In order to form a fine pattern by utilizing a phase-separated structure formed by the self-organization of a block copolymer, it is preferable that the phase-separated structure formed by the block copolymer has a vertical alignment property. For example, in the examples of Patent Document 2, a block copolymer capable of forming a phase-separated structure having a vertical alignment property is described when the film thickness of the block copolymer formed on a substrate is 24 nm. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2008-36491 A [Patent Document 2] JP 2022-20519 A [Non-patent literature]
[0008] [Non-Patent Document 1] Proceedings of SPIE, Vol. 7637, No. 76370G-1 (2010). Summary of the Invention [Problem to be solved by the invention]
[0009] In order to apply the phase-separated structure formed by the block copolymer to an etching mask, it is necessary to vertically align the film at a relatively large thickness (for example, 25 nm or more). However, the block copolymer described in Patent Document 2 is difficult to form a vertically oriented phase-separated structure when the film thickness is large.
[0010] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a resin composition for forming an etching mask pattern, which is capable of forming a vertically oriented phase-separated structure even in a film thickness of 25 nm or more, and a method for producing an etching mask pattern using the same. [Means for solving the problem]
[0011] The present invention includes the following aspects. A first aspect of the present invention is a method for producing an etching mask pattern, comprising the steps of: applying a resin composition for forming an etching mask pattern onto a support to form a layer containing a block copolymer having a thickness of 25 nm or more; and phase-separating the layer containing the block copolymer, wherein the resin composition for forming an etching mask pattern contains a block copolymer having a first block and a second block, the first block is composed of a polymer having a repeating structure of a constitutional unit represented by the following general formula (b1), the second block is composed of a random copolymer having a structure in which a constitutional unit represented by the following general formula (b2m) and a constitutional unit represented by the following general formula (b2g) are randomly arranged, and the ratio of the volume of the first block to the total volume of the first block and the second block is 20 to 80 volume %.
[0012] [ka] [In formula (b1), R 1 is an alkyl group which may have an oxygen atom or a silicon atom. n is an integer of 0 to 5. When n is an integer of 2 or more, a plurality of R 1 may be the same or different. b1is a hydrogen atom or a methyl group. In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear or branched alkylene group having 1 to 10 carbon atoms which may have a hydroxy group. In formula (b2g) and formula (b2m), R b2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 may be the same or different. x represents a molar ratio and is greater than 0 and equal to or less than 0.10.
[0013] A second aspect of the present invention is a resin composition for forming an etching mask pattern, which contains a block copolymer having a first block and a second block, wherein the first block is composed of a polymer having a repeating structure of a structural unit represented by the following general formula (b1), and the second block is composed of a random copolymer having a structure in which a structural unit represented by the following general formula (b2m) and a structural unit represented by the following general formula (b2g) are randomly arranged, and the proportion of the volume of the first block to the total volume of the first block and the second block is 20 to 80 volume%.
[0014] [ka] [In formula (b1), R 1 is an alkyl group which may have an oxygen atom or a silicon atom. n is an integer of 0 to 5. When n is an integer of 2 or more, a plurality of R 1 may be the same or different. b1 is a hydrogen atom or a methyl group. In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear or branched alkylene group having 1 to 10 carbon atoms which may have a hydroxy group. In formula (b2g) and formula (b2m), R b2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 may be the same or different. x represents a molar ratio and is greater than 0 and equal to or less than 0.10. Effect of the Invention
[0015] According to the present invention, it is possible to provide a resin composition that can be used for an etching mask pattern, and a method for producing an etching mask pattern using the same. [Brief description of the drawings]
[0016] [Figure 1] 1A to 1C are schematic process diagrams illustrating an embodiment of a method for producing a structure including a phase-separated structure. [Diagram 2] FIG. 13 is a diagram illustrating an embodiment of an optional step. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] In this specification and claims, the term "aliphatic" is a relative concept to aromaticity and is defined as meaning a group, compound, etc. that does not have aromaticity. Unless otherwise specified, the term "alkyl group" includes linear, branched and cyclic monovalent saturated hydrocarbon groups. The same applies to the alkyl group in an alkoxy group. Unless otherwise specified, the term "alkylene group" includes linear, branched and cyclic divalent saturated hydrocarbon groups. The term "halogenated alkyl group" refers to an alkyl group in which some or all of the hydrogen atoms have been substituted with halogen atoms, and examples of the halogen atoms include fluorine, chlorine, bromine and iodine atoms. The term "fluorinated alkyl group" or "fluorinated alkylene group" refers to an alkyl group or alkylene group in which some or all of the hydrogen atoms have been substituted with fluorine atoms. The term "structural unit" refers to a monomer unit that constitutes a polymeric compound (resin, polymer, copolymer). The term "optionally substituted" refers to the case where a hydrogen atom (-H) is replaced with a monovalent group, or the case where a methylene group (-CH 2 -) is replaced with a divalent group. The term "exposure" is intended to include any concept including irradiation with radiation. Unless otherwise specified, the "α-position (carbon atom at the α-position)" refers to the carbon atom to which the side chain of the block copolymer is bonded. The "α-position carbon atom" of a methyl methacrylate unit refers to the carbon atom to which the carbonyl group of methacrylic acid is bonded. The "α-position carbon atom" of a styrene unit refers to the carbon atom to which a benzene ring is bonded. "Number average molecular weight" (Mn) is the number average molecular weight measured by size exclusion chromatography in terms of standard polystyrene unless otherwise specified. "Weight average molecular weight" (Mw) is the weight average molecular weight measured by size exclusion chromatography in terms of standard polystyrene unless otherwise specified. The Mn or Mw value is expressed in units (g mol - ) indicates the molar mass. In the present specification and claims, some structures represented by chemical formulas may have asymmetric carbons and may have enantiomers or diastereomers, in which case a single formula represents all the isomers. These isomers may be used alone or as a mixture.
[0018] (Method of manufacturing an etching mask pattern) The method for producing an etching mask pattern of the present embodiment includes a step of applying a resin composition for forming an etching mask pattern onto a support to form a layer containing a block copolymer (hereinafter referred to as "step (i)"), and a step of phase-separating the layer containing the block copolymer (hereinafter referred to as "step (ii)"). Hereinafter, such a method for producing an etching mask pattern will be specifically described with reference to Fig. 1. However, the present invention is not limited to this.
[0019] FIG. 1 shows an embodiment of a method for producing an etching mask pattern. In the embodiment shown in FIG. 1, first, a primer is applied onto a support 1 to form a primer layer 2 (FIG. 1(I)). Next, the resin composition for forming an etching mask pattern of the above-mentioned embodiment is applied onto the undercoat agent layer 2 to form a layer (BCP layer) 3 containing the above-mentioned (BCP) component (Figure 1 (II); this is step (i)). Next, an annealing treatment is performed by heating, so that the BCP layer 3 is separated into a phase 3a and a phase 3b (FIG. 1(III); step (ii)). According to the manufacturing method of this embodiment, i.e., the manufacturing method including steps (i) and (ii), a structure 3' including a phase-separated structure is obtained on the support 1 on which the undercoat agent layer 2 is formed. An etching mask pattern can be manufactured using this structure 3' including a phase-separated structure. In addition, the "first block" and the "second block" in the resin composition for forming an etching mask pattern described below may be referred to as "block (b1)" and "block (b2)", respectively.
[0020] [Step (i)] In step (i), a resin composition for forming an etching mask pattern is applied onto a support 1 to form a BCP layer 3 having a thickness of 25 nm or more. The thickness of the BCP layer 3 may be 28 nm or more, 30 nm or more, 32 nm or more, 34 nm or more, or 36 nm or more. In the embodiment shown in FIG. 1, first, a base agent is applied onto a support 1 to form a base agent layer 2 . By providing the undercoat agent layer 2 on the support 1, a balance of hydrophilicity and hydrophobicity between the surface of the support 1 and the layer (BCP layer) 3 containing a block copolymer can be achieved. That is, when the primer layer 2 contains a resin component having the structural units constituting the block (b1), the adhesion between the phase of the BCP layer 3 consisting of the block (b1) and the support 1 is enhanced. When the primer layer 2 contains a resin component having the structural units constituting the block (b2), the adhesion between the phase of the BCP layer 3 consisting of the block (b2) and the support 1 is enhanced. As a result, due to phase separation of the BCP layer 3, cylindrical structures and lamellar structures oriented in the direction perpendicular to the surface of the support 1 are easily formed.
[0021] Primer: As the undercoat agent, a resin composition containing a resin component can be used. The resin component for the undercoat agent can be appropriately selected from among conventionally known resin components used for thin film formation, depending on the type of block constituting the (BCP) component. The resin component for the undercoat agent may be, for example, a thermally polymerizable resin, or may be a photosensitive resin contained in a positive resist composition or a negative resist composition. In addition, a compound may be used as a surface treatment agent, and a non-polymerizable film formed by applying the compound may be used as the undercoat agent layer. For example, a siloxane-based organic monomolecular film formed using phenethyltrichlorosilane, octadecyltrichlorosilane, hexamethyldisilazane, or the like as a surface treatment agent may also be suitably used as the undercoat agent layer.
[0022] Examples of such a resin component include a resin containing a resin having both of the structural units constituting each of the blocks (b1) and (b2), and a resin having both of the structural units having high affinity with each of the blocks constituting the (BCP) component.
[0023] As the resin component for the primer, it is preferable to use, for example, a compound or resin that contains both a portion that has a high affinity for styrene, such as an aromatic ring, and a portion that has a high affinity for methyl methacrylate (such as a highly polar functional group). An example of a resin component that includes both a site with high affinity for styrene and a site with high affinity for methyl methacrylate is a resin obtained by polymerizing at least a monomer having an aromatic ring and a monomer having a highly polar functional group. Examples of monomers having an aromatic ring include monomers having aryl groups in which one hydrogen atom has been removed from an aromatic hydrocarbon ring, such as a phenyl group, a biphenyl group, a fluorenyl group, a naphthyl group, an anthryl group, or a phenanthryl group, or monomers having heteroaryl groups in which a part of the carbon atoms constituting the ring of these groups is substituted with a heteroatom such as an oxygen atom, a sulfur atom, or a nitrogen atom. Examples of monomers having a highly polar functional group include monomers having a trimethoxysilyl group, a trichlorosilyl group, an epoxy group, a glycidyl group, a carboxy group, a hydroxyl group, a cyano group, or a hydroxyalkyl group in which a part of the hydrogen atoms of an alkyl group is substituted with a hydroxyl group. Other examples of compounds that contain both a moiety with high affinity for styrene and a moiety with high affinity for methyl methacrylate include compounds that contain both an aryl group and a highly polar functional group, such as phenethyltrichlorosilane, and compounds that contain both an alkyl group and a highly polar functional group, such as alkylsilane compounds.
[0024] Examples of the resin component for the base agent include a resin having both styrene and methyl methacrylate as structural units, and a resin having all of styrene, methyl methacrylate, and (hydroxyethyl) methacrylate as structural units.
[0025] When the resin composition for the base agent has two or more different types of constituent units, examples of the resin include a random copolymer, an alternating polymer of styrene and methyl methacrylate (in which each monomer is copolymerized alternately), and the like.
[0026] The primer can be prepared by dissolving the above-mentioned resin components in a solvent. Such a solvent may be any solvent capable of dissolving each component used to form a homogeneous solution, and examples thereof include the same organic solvent components as those exemplified in the description of the resin composition for forming an etching mask pattern of the above embodiment.
[0027] The type of the support 1 is not particularly limited as long as the resin composition can be applied to the surface thereof. For example, a substrate made of an inorganic material such as metal (silicon, copper, chromium, iron, aluminum, etc.), glass, titanium oxide, silica, or mica; SiO 2 Examples of suitable substrates include substrates made of oxides such as silicon nitride, substrates made of nitrides such as silicon oxide, and substrates made of organic materials such as acrylic, polystyrene, cellulose, cellulose acetate, and phenol resin. Among these, metal substrates are preferred, and for example, silicon substrates (Si substrates) and copper substrates (Cu substrates) are likely to form structures with vertically oriented cylinder structures and lamellar structures. Among these, Si substrates are particularly preferred. The size and shape of the support 1 are not particularly limited. The support 1 does not necessarily have to have a smooth surface, and substrates of various shapes can be appropriately selected. For example, substrates having a curved surface, flat plates with an uneven surface, and substrates having a flaky shape can be mentioned.
[0028] The surface of the support 1 may be provided with an inorganic and / or organic film. Examples of inorganic films include inorganic anti-reflective coatings (inorganic BARCs). Examples of organic films include organic anti-reflective coatings (organic BARCs). The inorganic film can be formed, for example, by applying an inorganic anti-reflective coating composition, such as a silicon-based material, onto a support and baking the composition. The organic film can be formed, for example, by applying an organic film-forming material, which is a resin component that constitutes the film, dissolved in an organic solvent, onto a substrate using a spinner or the like, and baking the material at a temperature of preferably 200 to 300° C., preferably for 30 to 300 seconds, more preferably for 60 to 180 seconds. This organic film-forming material does not necessarily need to be sensitive to light or electron beams, as in the case of a resist film, and may or may not be sensitive. Specifically, resists and resins that are commonly used in the manufacture of semiconductor elements and liquid crystal display elements can be used. In addition, the organic film forming material is preferably a material capable of forming an organic film that can be etched, particularly dry etched, so that the organic film pattern can be formed by etching the organic film using a pattern made of block copolymer formed by processing the BCP layer 3. Among them, it is preferable that the material be a material capable of forming an organic film that can be etched by oxygen plasma etching or the like. Such an organic film forming material may be a material that has been used to form an organic film such as organic BARC. For example, the ARC series manufactured by Nissan Chemical Industries, Ltd., the AR series manufactured by Rohm and Haas, and the SWK series manufactured by Tokyo Ohka Kogyo Co., Ltd. can be mentioned.
[0029] The method for applying the primer onto the support 1 to form the primer layer 2 is not particularly limited, and may be any conventionally known method. For example, the undercoat layer 2 can be formed by applying the undercoat agent onto the support 1 by a conventionally known method such as spin coating or using a spinner to form a coating film, and then drying the coating film. The method for drying the coating film may be any method capable of volatilizing the solvent contained in the undercoat agent, such as baking. In this case, the baking temperature is preferably 80 to 300° C., more preferably 180 to 270° C., and further preferably 220 to 270° C. The baking time is preferably 30 to 500 seconds, and more preferably 60 to 400 seconds. The thickness of the undercoat agent layer 2 after the coating film has dried is preferably about 10 to 100 nm, and more preferably about 20 to 50 nm.
[0030] The surface of the support 1 may be washed before forming the primer layer 2 on the support 1. Washing the surface of the support 1 improves the coatability of the primer. The cleaning treatment may be carried out by any of the conventional methods known in the art, including, for example, oxygen plasma treatment, ozone oxidation treatment, acid-alkali treatment, and chemical modification treatment.
[0031] After forming the primer layer 2, the primer layer 2 may be rinsed with a rinsing liquid such as a solvent, if necessary. The rinsing removes uncrosslinked portions and the like in the primer layer 2, improving the affinity with at least one block constituting the block copolymer, and facilitating the formation of a phase-separated structure consisting of a cylindrical structure and a lamellar structure oriented in a direction perpendicular to the surface of the support 1. The rinse liquid may be any liquid capable of dissolving the uncrosslinked portions, and solvents such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), ethyl lactate (EL), or commercially available thinners may be used. After the cleaning, post-baking may be performed to volatilize the rinsing liquid. The temperature condition for this post-baking is preferably 80 to 250°C, more preferably 80 to 200°C, and further preferably 80 to 150°C. The baking time is preferably 30 to 500 seconds, and more preferably 60 to 240 seconds. The thickness of the undercoat agent layer 2 after such post-baking is preferably about 1 to 10 nm, and more preferably about 2 to 7 nm.
[0032] Next, on the undercoat agent layer 2, a layer (BCP layer) 3 containing a (BCP) component is formed. The method for forming the BCP layer 3 on the undercoat layer 2 is not particularly limited, and examples thereof include a method in which the resin composition for forming an etching mask pattern of the above-mentioned embodiment is applied onto the undercoat layer 2 by a conventionally known method such as using spin coating or a spinner to form a coating film, and then drying.
[0033] The thickness of the BCP layer 3 need only be sufficient so that it can be used as an etching mask and so that phase separation occurs. The film thickness of the BCP layer 3 is 25 nm or more, and may be 28 nm or more, 30 nm or more, 32 nm or more, 34 nm or more, or 36 nm or more. When the film thickness is equal to or more than the lower limit, the phase-separated structure formed from the BCP layer 3 is more likely to remain during etching and is more likely to function as a mask. The thickness of the BCP layer 3 may be 100 nm or less, 75 nm or less, 50 nm or less, or 45 nm or less. When the thickness is equal to or less than the upper limit, a phase-separated structure having a desired periodic size can be easily obtained, and the uniformity of the nanostructure can be easily improved. The thickness of the BCP layer 3 is preferably 25 to 100 nm. For example, when the support 1 is a Si substrate, the thickness of the BCP layer 3 is preferably adjusted to 25 to 100 nm, more preferably 30 to 75 nm.
[0034] [Step (ii)] In step (ii), the BCP layer 3 formed on the support 1 is subjected to phase separation. By heating the support 1 after step (i) to perform an annealing treatment, the block copolymer is selectively removed to form a phase-separated structure exposing at least a part of the surface of the support 1. That is, a structure 3' including a phase-separated structure separated into a phase 3a and a phase 3b is produced on the support 1. The temperature condition of the annealing treatment is preferably equal to or higher than the glass transition temperature of the (BCP) component used and lower than the thermal decomposition temperature, and for example, when the block copolymer is a polystyrene-polymethyl methacrylate (PS-PMMA) block copolymer (mass average molecular weight 5000 to 100000), the temperature is preferably 180 to 270° C. The heating time is preferably 30 to 3600 seconds. Moreover, the annealing process is preferably carried out in a gas with low reactivity, such as nitrogen.
[0035] [Step (iii)] In step (iii), a phase consisting of at least one of the first and second blocks constituting the (BCP) component in the structure 3' is selectively removed, forming a fine pattern (polymer nanostructure) and obtaining an etching mask pattern.
[0036] Methods for selectively removing the phase made of blocks include a method of subjecting the BCP layer to oxygen plasma treatment, a method of subjecting the BCP layer to hydrogen plasma treatment, and the like. For example, by subjecting a BCP layer containing the (BCP) component to phase separation and then subjecting the BCP layer to oxygen plasma treatment, hydrogen plasma treatment, or the like, the phase consisting of block (b1) is not selectively removed, but the phase consisting of block (b2) is selectively removed.
[0037] FIG. 2 shows an example embodiment of step (iii). In the embodiment shown in Figure 2, the structure 3' produced on the support 1 in step (ii) is subjected to an oxygen plasma treatment to selectively remove the phase 3a and form a pattern (polymer nanostructure) consisting of spaced phases 3b, where phase 3b is a phase consisting of blocks (b1) and phase 3a is a phase consisting of blocks (b2).
[0038] The support 1 on which a pattern has been formed by phase separation of the BCP layer 3 made of the (BCP) component as described above can be used as is, but the shape of the pattern (polymer nanostructure) on the support 1 can also be changed by further heating. The heating temperature is preferably equal to or higher than the glass transition temperature of the block copolymer used and lower than its thermal decomposition temperature, and is preferably carried out in a gas with low reactivity such as nitrogen.
[0039] In the method for producing an etching mask pattern of this embodiment, a vertically oriented phase separation structure can be formed even in a film thickness of 25 nm or more by using the following resin composition for forming an etching mask pattern. Hereinafter, this resin composition for forming an etching mask pattern will be described in detail.
[0040] [Resin composition for forming etching mask pattern] The resin composition for forming an etching mask pattern used in the method for producing an etching mask pattern of this embodiment contains a block copolymer having a first block and a second block. The first block is composed of a polymer having a repeating structure of a constitutional unit represented by the following general formula (b1). The second block is composed of a random copolymer having a structure in which a constitutional unit represented by the following general formula (b2m) and a constitutional unit represented by the following general formula (b2g) are randomly arranged. The ratio of the volume of the first block to the total volume of the first block and the second block is 20 to 80 volume %.
[0041] [ka] [In formula (b1), R 1 is an alkyl group which may have an oxygen atom or a silicon atom. n is an integer of 0 to 5. When n is an integer of 2 or more, a plurality of R 1 may be the same or different. b1 is a hydrogen atom or a methyl group. In formula (b2g), R2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear or branched alkylene group having 1 to 10 carbon atoms which may have a hydroxy group. In formula (b2g) and formula (b2m), R b2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 may be the same or different. x represents a molar ratio and is greater than 0 and equal to or less than 0.10.
[0042] <Block copolymer (BCP) component> A block copolymer is a polymer in which multiple types of blocks (partial constituent components in which the same type of structural unit is repeatedly bonded) are bonded together. The blocks constituting a block copolymer may be of two types, or three or more types. The block copolymer in this embodiment (hereinafter also referred to as "(BCP) component") has a first block and a second block.
[0043] <First Block> The first block is composed of a polymer having a repeating structure of a structural unit represented by the following general formula (b1) (hereinafter, also referred to as structural unit (b1)).
[0044] [ka] [In the formula, R 1 is an alkyl group which may have an oxygen atom or a silicon atom. n is an integer of 0 to 5. When n is an integer of 2 or more, a plurality of R 1 may be the same or different. b1 is a hydrogen atom or a methyl group.
[0045] In the formula (b1), R 1 R is an alkyl group which may have an oxygen atom or a silicon atom.1 When the alkyl group has a silicon atom, the silicon atom is preferably bonded to a methylene group (-CH 2 R 1 When the alkyl group has an oxygen atom, the oxygen atom is not substituted by a methylene group (-CH 2 The alkyl group preferably has 1 to 5 carbon atoms, more preferably has 1 to 4 carbon atoms, and further preferably has 1 to 3 carbon atoms, and is particularly preferably an ethyl group or a methyl group, and most preferably a methyl group.
[0046] In the formula (b1), R b1 is a hydrogen atom or a methyl group.
[0047] In the formula (b1), n is preferably an integer of 0 to 3, more preferably an integer of 0 to 2, and further preferably 0 or 1.
[0048] <Second Block> The second block is composed of a random copolymer having a structure in which a structural unit represented by the following general formula (b2m) (hereinafter also referred to as structural unit (b2m)) and a structural unit represented by the following general formula (b2g) (hereinafter also referred to as structural unit (b2g)) are arranged in a disordered manner.
[0049] [ka] [In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. R 3 is a linear or branched alkylene group having 1 to 10 carbon atoms which may have a hydroxy group. In formula (b2g) and formula (b2m), R b2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 may be the same or different. x represents a molar ratio and is greater than 0 and equal to or less than 0.10.
[0050] (B2M) The structural unit (b2m) is a structural unit represented by the above general formula (b2m). In the above formula (b2m), R b2 R is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 The alkyl group having 1 to 5 carbon atoms is preferably a linear or branched alkyl group having 1 to 5 carbon atoms, and specific examples thereof include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, a pentyl group, an isopentyl group, and a neopentyl group. The halogenated alkyl group having 1 to 5 carbon atoms is a group in which some or all of the hydrogen atoms of the alkyl group having 1 to 5 carbon atoms are substituted with halogen atoms. As the halogen atom, a fluorine atom is particularly preferable. R b2 is preferably a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a fluorinated alkyl group having 1 to 5 carbon atoms, and from the viewpoint of industrial availability, a hydrogen atom or a methyl group is more preferable, and a methyl group is even more preferable.
[0051] (B2G) The structural unit (b2g) is a structural unit represented by the above general formula (b2g).
[0052] In the above formula (b2g), R b2 R is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 is R in the above formula (b2m). b2 is the same as:
[0053] In the above formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group or a phosphate group. The alkyl group may be linear, branched or may contain a ring structure. The alkyl group is preferably a linear, branched or cyclic alkyl group, more preferably a linear or cyclic alkyl group. When the alkyl group is linear, the carbon number may be 1 or more, and preferably 2 or more. There is no particular upper limit on the carbon number of the linear alkyl group, but from the viewpoint of phase separation performance, the carbon number is preferably 15 or less, more preferably 10 or less, even more preferably 8 or less, and particularly preferably 6 or less. When the alkyl group is branched, it is sufficient that the alkyl group has 3 or more carbon atoms. There is no particular upper limit on the number of carbon atoms of the branched alkyl group, but from the viewpoint of phase separation performance, the alkyl group preferably has 15 or less carbon atoms, more preferably has 10 or less carbon atoms, even more preferably has 8 or less carbon atoms, and particularly preferably has 6 or less carbon atoms. The alkyl group preferably has 2 to 15 carbon atoms, more preferably has 2 to 10 carbon atoms, even more preferably has 2 to 8 carbon atoms, even more preferably has 2 to 6 carbon atoms, and particularly preferably has 2 to 5 carbon atoms. When the alkyl group contains a ring structure, R 2 may be a cycloalkyl group, a straight-chain or branched alkyl group having a cycloalkylene group interposed therein, or a straight-chain or branched alkyl group having a cycloalkyl group bonded to an end thereof. The cycloalkyl group and cycloalkylene group may be a monocyclic group or a polycyclic group, but a monocyclic group is preferred. When the cycloalkyl group or cycloalkylene group is a monocyclic group, a 3- to 8-membered ring is preferred, a 3- to 6-membered ring is more preferred, and a 5- to 6-membered ring is even more preferred. When the alkyl group contains a ring structure, R 2 may have 3 or more carbon atoms. The upper limit of the number of carbon atoms of the alkyl group containing a ring structure is not particularly limited, but from the viewpoint of phase separation performance, the number of carbon atoms is preferably 15 or less, more preferably 10 or less, even more preferably 8 or less, and still more preferably 6 or less. R 2 The alkyl group in the formula (I) preferably has 2 to 15 carbon atoms, more preferably has 2 to 10 carbon atoms, further preferably has 2 to 8 carbon atoms, and further more preferably has 2 to 6 carbon atoms. R 2 The alkyl group is preferably a linear alkyl group or a cycloalkyl group having 2 to 6 carbon atoms.
[0054] R 2 The alkyl group of R may have a silicon atom, a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group, or a phosphoric acid group. 2 When the alkyl group has a fluorine atom, a carboxy group, an amino group, a cyano group, a hydroxy group, or a phosphoric acid group, the fluorine atom, the carboxy group, the amino group, the cyano group, the hydroxy group, or the phosphoric acid group may be a substituent that replaces a hydrogen atom of the alkyl group. The number of hydrogen atoms replaced by the group is not particularly limited, but is preferably 1 to 3. R 2 When the alkyl group has a silicon atom, the silicon atom is preferably bonded to a methylene group (-CH 2 The number of methylene groups substituted with silicon atoms is not particularly limited, but one is preferred. R 2 is preferably an alkyl group which may be substituted with an alkylsilyl group, a fluoromethyl group, a carboxy group, an amino group, a hydroxy group, or a phosphate group. The alkyl group in the alkylsilyl group preferably has 1 to 3 carbon atoms, more preferably has 1 or 2 carbon atoms. The alkylsilyl group is preferably a trialkylsilyl group, more preferably a triethylsilyl group or a trimethylsilyl group, and even more preferably a trimethylsilyl group. The fluoromethyl group is preferably a trifluoromethyl group.
[0055] R 2 When R is a linear alkyl group having a substituent, 2 Preferred examples are shown below, but are not limited to these: In the following formula, * represents a bond bonded to the sulfur atom (S) in the above formula (b2g).
[0056] [ka] [In the formula, Y 2 is a single bond or a linear or branched alkylene group having 1 to 15 carbon atoms. p is an integer of 1 to 10.
[0057] In the above formulas (r2-1) to (r2-9), Y 2 is a single bond or a linear or branched alkylene group having 1 to 15 carbon atoms. When the alkylene group is linear, it more preferably has 1 to 10 carbon atoms, further preferably has 1 to 8 carbon atoms, and particularly preferably has 1 to 5 carbon atoms. When the alkylene group is branched, it more preferably has 2 to 10 carbon atoms, further preferably has 2 to 8 carbon atoms, and particularly preferably has 2 to 6 carbon atoms. Y 2 The alkylene group is preferably a linear alkylene group having 1 to 5 carbon atoms or a branched alkylene group having 2 to 6 carbon atoms. R 2 is a group represented by any one of the formulas (r2-1) to (r2-8), Y 2 R is preferably a linear or branched alkylene group having 1 to 15 carbon atoms, more preferably a linear alkylene group having 1 to 5 carbon atoms or a branched alkylene group having 2 to 6 carbon atoms. 2 is a group represented by the formula (r2-9), Y 2 is preferably a single bond or a linear alkylene group having 1 to 5 carbon atoms, and more preferably a single bond. In the above formula (r2-9), p is preferably an integer of 1 to 6, more preferably an integer of 1 to 4, and even more preferably 3 or 4.
[0058] R 2 Specific examples of are shown below, but are not limited to these. In the following formula, * represents a bond bonded to the sulfur atom (S) in the above formula (b2g).
[0059] [ka] [In the formula, q is an integer of 1 to 15. q' is an integer of 0 to 15. p is an integer of 1 to 10. Each p' is independently an integer of 0 to 10.]
[0060] In the above formula, q is preferably an integer of 1 to 10, more preferably an integer of 1 to 8, further preferably an integer of 1 to 6, and particularly preferably an integer of 1 to 5. In the formulae (r2-18) and (r2-19), q′ is preferably an integer of 0 to 10, more preferably an integer of 0 to 8, even more preferably an integer of 0 to 6, and particularly preferably an integer of 0 to 5. In the above formula (r2-18), p is preferably an integer of 1 to 6, more preferably an integer of 1 to 4, and even more preferably 3 or 4. In the above formula (r2-19), p' is preferably an integer of 1 to 8, more preferably an integer of 1 to 6, even more preferably an integer of 1 to 3, and particularly preferably 1 or 2.
[0061] In the above formula (b2g), R 3 is a linear or branched alkylene group having 1 to 10 carbon atoms, which may have a hydroxyl group. When the alkylene group is linear, the number of carbon atoms may be 1 or more, but preferably 3 or more. The upper limit of the carbon number of the linear alkylene group is preferably 8 or less, more preferably 5 or less, and even more preferably 4 or less, from the viewpoint of phase separation performance. The carbon number of the linear alkylene group is particularly preferably 3. When the alkylene group is branched, the number of carbon atoms may be 3 or more, but preferably 4 or more. The upper limit of the carbon number of the branched alkylene group is preferably 8 or less, more preferably 5 or less, from the viewpoint of phase separation performance. The carbon number of the alkylene group is preferably 3 to 10, more preferably 3 to 8, even more preferably 3 to 5, even more preferably 3 to 4, and especially preferably 3. R 3 The alkylene group is preferably a linear alkylene group having 3 carbon atoms.
[0062] R 3 The alkylene group may have a hydroxy group. The hydroxy group may be a substituent that replaces a hydrogen atom of the alkylene group. The number of hydrogen atoms replaced by the hydroxy group is not particularly limited, but is preferably 1 to 3, more preferably 1 or 2, and even more preferably 1.
[0063] The structural unit (b2g) is preferably a structural unit represented by general formula (b2g-1) shown below.
[0064] [ka] [In the formula, R 4 is a hydrogen atom or a hydroxyl group. k1 and k2 each independently represent an integer of 1 to 5. R b2 and R 2 is R in the above formula (b2g). b2 and R 2 is the same as:
[0065] In the above formula (b2g-1), R b2 and R 2 is R in the above formula (b2g). b2 and R 2 Same as R 2 is preferably one represented by the above formulas (r2-1) to (r2-9), and more preferably one represented by (r2-10) to (r2-19).
[0066] In the above formula (b2g-1), R 4 is a hydrogen atom or a hydroxy group.
[0067] In the formula (b2g-1), k1 and k2 each independently represent an integer of 1 to 5. k1 and k2 each preferably represent an integer of 1 to 3, more preferably 1 or 2, and further preferably 1.
[0068] Specific examples of the structural unit (b2g) are shown below, but are not limited to these. In the following formula, R represents a methyl group or a hydrogen atom, and a methyl group is preferable.
[0069] [ka]
[0070] [ka]
[0071] [ka]
[0072] [ka]
[0073] The second block is composed of a random copolymer having a structure in which the structural unit (b2g) and the structural unit (b2m) are randomly arranged. In the formulas (b2g) and (b2m), x and 1-x represent the molar ratio of the structural unit (b2g) and the structural unit (b2m). x is more than 0 and 0.10 or less. x is preferably less than 0.10, more preferably 0.09 or less, even more preferably 0.08 or less, and particularly preferably 0.07 or less. x is preferably 0.0050 or more, more preferably 0.0070 or more, even more preferably 0.0090 or more, particularly preferably 0.0095 or more, and most preferably 0.0099 or more. When x is equal to or greater than the lower limit, a vertically oriented phase-separated structure is easily formed even in a film thickness of 25 nm or more.When x is equal to or less than the upper limit, a vertically oriented phase-separated structure is easily formed even in a film thickness of 25 nm or more.
[0074] In the (BCP) component, the ratio of the volume of the first block to the total volume of the first block and the second block is 20 to 80 volume %. The volume ratio of the first block is preferably 30 volume % or more, and more preferably 35 volume % or more. The upper limit of the volume ratio of the first block is preferably 70 volume % or less, more preferably 65 volume % or less, and even more preferably 60 volume % or less.
[0075] The ratio of the volume of the first block to the total volume of the first block and the second block in the (BCP) component can be calculated as follows. 1From the results of H NMR analysis, the mole percentages of the first block and the second block in the (BCP) component are calculated, and furthermore, the mass percentage of each block is calculated from the molecular weight of each block. The mass percentage of each block is divided by the density of each block to calculate the volume ratio of each block, and the volume percentage of the first block in the (BCP) component is calculated from the volume ratio. The density of each block can be estimated by the atomic group contribution method (Fedors, RF Polym. Eng. Sci. 1974, 14, 147-154.). When the first block is a polystyrene block (PS), the density of PS is 1.05 gm -3 When the second block is a polystyrene block (PS), the density of PS is 1.05 gm -3 When the second block has a structural unit derived from methyl methacrylate, the density of the structure composed of the structural units is 1.18 gcm -3 When the second block has a structural unit derived from 2-hydroxy-3-(2,2,2-trifluoroethylsulfanyl)propyl methacrylate, the density of the structure composed of the structural units is 1.43 gcm -3 When the second block has a structural unit derived from 2-hydroxy-3-(ethylsulfanyl)propyl methacrylate, 2-hydroxy-3-(1-propyl)propyl methacrylate, 2-hydroxy-3-(1-hexyl)propyl methacrylate, or 2-hydroxy-3-(cyclohexyl)propyl methacrylate, the density of the structure composed of the structural units can be 1.18 gcm -3 can be used. The density of each block may be determined based on the literature (Polymer Handbook, 4th ed.; Wiley: New York, 2004).
[0076] The (BCP) component may have other blocks in addition to the first block and the second block. In a preferred embodiment, the (BCP) component is a block copolymer composed of a first block and a second block.
[0077] The number average molecular weight (Mn) of the (BCP) component (based on polystyrene conversion by size exclusion chromatography) is not particularly limited, but is preferably 3,000 to 100,000, more preferably 5,000 to 50,000, further preferably 6,000 to 40,000, and particularly preferably 8,000 to 30,000. The molecular weight dispersity (Mw / Mn) of each block constituting the (BCP) component is preferably from 1.0 to 1.5, more preferably from 1.0 to 1.4, and even more preferably from 1.0 to 1.3.
[0078] <Organic solvent components> The above-mentioned resin composition for forming an etching mask pattern can be prepared by dissolving the above-mentioned (BCP) component in an organic solvent component. The organic solvent component may be any solvent capable of dissolving each component used to form a homogeneous solution, and any solvent known in the art as a solvent for film compositions mainly composed of resins may be used.
[0079] Examples of the organic solvent component include lactones such as γ-butyrolactone; ketones such as acetone, methyl ethyl ketone, cyclohexanone, methyl-n-pentyl ketone, methyl isopentyl ketone, and 2-heptanone; polyhydric alcohols such as ethylene glycol, diethylene glycol, propylene glycol, and dipropylene glycol; compounds having an ester bond such as ethylene glycol monoacetate, diethylene glycol monoacetate, propylene glycol monoacetate, and dipropylene glycol monoacetate; and ether bonds such as monoalkyl ethers, monomethyl ether, monoethyl ether, monopropyl ether, and monobutyl ether of the polyhydric alcohols or the compounds having an ester bond, or monophenyl ether. derivatives of polyhydric alcohols such as compounds having a bond [among which, propylene glycol monomethyl ether acetate (PGMEA) and propylene glycol monomethyl ether (PGME) are preferred]; cyclic ethers such as dioxane, esters such as methyl lactate, ethyl lactate (EL), methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, and ethyl ethoxypropionate; and aromatic organic solvents such as anisole, ethyl benzyl ether, cresyl methyl ether, diphenyl ether, dibenzyl ether, phenetole, butyl phenyl ether, ethylbenzene, diethylbenzene, pentylbenzene, isopropylbenzene, toluene, xylene, cymene, and mesitylene. The organic solvent component may be used alone or in a mixture of two or more kinds. Among them, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), cyclohexanone, and EL are preferred.
[0080] A mixed solvent obtained by mixing PGMEA and a polar solvent is also preferred. The mixing ratio (mass ratio) may be appropriately determined in consideration of the compatibility between PGMEA and the polar solvent, and is preferably within a range of 1:9 to 9:1, and more preferably 2:8 to 8:2. For example, when EL is blended as the polar solvent, the mass ratio of PGMEA:EL is preferably 1:9 to 9:1, more preferably 2:8 to 8:2. When PGME is blended as the polar solvent, the mass ratio of PGMEA:PGME is preferably 1:9 to 9:1, more preferably 2:8 to 8:2, and even more preferably 3:7 to 7:3. When PGME and cyclohexanone are blended as the polar solvent, the mass ratio of PGMEA:(PGME+cyclohexanone) is preferably 1:9 to 9:1, more preferably 2:8 to 8:2, and even more preferably 3:7 to 7:3.
[0081] As the organic solvent component in the resin composition for forming an etching mask pattern, a mixed solvent of PGMEA or EL, or a mixed solvent of the PGMEA and a polar solvent, and γ-butyrolactone is also preferred. In this case, the mass ratio of the former to the latter is preferably 70:30 to 95:5. The organic solvent component contained in the resin composition for forming an etching mask pattern is not particularly limited, and is appropriately set at a coatable concentration according to the coating film thickness, and is generally used so that the solid content concentration is within the range of 0.2 to 70 mass %, preferably 0.2 to 50 mass %.
[0082] <Optional ingredients> In addition to the (BCP) component and organic solvent component, the above-mentioned resin composition for forming an etching mask pattern may further contain, as desired, miscible additives such as an additional resin for improving the performance of the layer, a surfactant for improving coatability, a dissolution inhibitor, a plasticizer, a stabilizer, a colorant, an antihalation agent, a dye, a sensitizer, a base amplifier, a basic compound, and the like.
[0083] According to the method for producing an etching mask pattern of the embodiment described above, since the resin composition for forming an etching mask pattern of the embodiment described above is used, even if the layer containing the block copolymer has a thickness of 25 nm or more, it is possible to form a phase separation structure having vertical alignment. By selectively removing a specific phase of the vertically aligned BCP layer, an etching mask can be obtained. Since the etching mask obtained in this manner has a thickness of 25 nm or more, it is likely to remain during etching, and etching resistance is easily increased.
[0084] In addition, according to the method for producing an etching mask pattern of the embodiment, it is possible to produce a support having nanostructures on the support surface, the positions and orientations of which can be more freely designed. For example, the structure formed has high adhesion to the support and is likely to have a phase-separated structure consisting of cylindrical structures and lamellar structures oriented perpendicular to the support surface.
[0085] [Optional process] Guide pattern formation process In the method for producing an etching mask pattern according to this embodiment, the above-mentioned step (i) may include a step of providing a guide pattern on the undercoat layer (guide pattern forming step). This allows the arrangement structure of the phase separation structure to be controlled. That is, a resin composition for forming an etching mask pattern may be applied onto the undercoat layer on which the guide pattern is formed. For example, even in the case of a block copolymer that forms a random fingerprint-like phase separation structure when no guide pattern is provided, by providing a groove structure of the resist film on the surface of the undercoat layer, a phase separation structure oriented along the groove can be obtained. Based on this principle, a guide pattern may be provided on the undercoat layer 2. In addition, by having the surface of the guide pattern have affinity with any of the blocks constituting the (BCP) component, a phase separation structure consisting of a cylindrical structure or a lamellar structure oriented perpendicular to the support surface can be easily formed.
[0086] The guide pattern can be formed using, for example, a resist composition. The resist composition for forming the guide pattern can be appropriately selected from resist compositions generally used for forming resist patterns and their modifications, and can be used by selecting one having affinity with any of the blocks constituting the (BCP) component. The resist composition may be either a positive resist composition for forming a positive pattern in which the exposed portion of the resist film is dissolved and removed, or a negative resist composition for forming a negative pattern in which the unexposed portion of the resist film is dissolved and removed, but is preferably a negative resist composition. As the negative resist composition, for example, a resist composition containing an acid generator and a base component whose solubility in a developer containing an organic solvent is reduced by the action of an acid, and the base component contains a resin component having a structural unit that is decomposed by the action of an acid to increase polarity, is preferable. After the BCP composition is poured onto the undercoat layer on which the guide pattern is formed, an annealing treatment is performed to cause phase separation. Therefore, the resist composition for forming the guide pattern is preferably one capable of forming a resist film having excellent solvent resistance and heat resistance.
[0087] (Resin composition for forming etching mask pattern) The resin composition for forming an etching mask pattern of this embodiment may be any of those described above in the previous embodiment. The block copolymer ((BCP) component) in the resin composition for forming an etching mask pattern may be produced, for example, by a production method having the steps shown below.
[0088] <Production method of block copolymer (BCP) component> Step (p1): A step of obtaining a block copolymer having a first block and a precursor of a second block (hereinafter, also referred to as a "BCP precursor"). Step (p2): Adding R to the precursor of the second block in the BCP precursor 2 Compounds represented by -SH (R 2 is R in the above formula (b2g). 2) to obtain a block copolymer (component (BCP)) containing a first block and a second block.
[0089] Process (p1): The precursor of the second block is a random copolymer having a structure in which the structural unit (b2gp), which is a precursor of the structural unit (b2g), and the structural unit (b2m) are randomly arranged. The structural unit (b2gp) is a structural unit containing an epoxy group or a vinyl group, and examples of the structural unit represented by the following general formula (b2gp) are:
[0090] [ka] [In the formula, R b2 and x represents R in the formula (b2g) and the formula (b2m). b2 and x. Yp 2 Rp represents a linear or branched alkyl group having 1 to 8 carbon atoms. 2 represents an epoxy group or a vinyl group.
[0091] In the formulas (b2gp) and (b2m), x and 1-x represent the molar ratio of the structural unit (b2gp) and the structural unit (b2m). x is more than 0 and 0.10 or less. x is preferably less than 0.10, more preferably 0.09 or less, even more preferably 0.08 or less, and particularly preferably 0.07 or less. x is preferably 0.0050 or more, more preferably 0.0070 or more, even more preferably 0.0090 or more, particularly preferably 0.0095 or more, and most preferably 0.0099 or more. When x is equal to or greater than the lower limit, a vertically oriented phase-separated structure is easily formed even in a film thickness of 25 nm or more.When x is equal to or less than the upper limit, a vertically oriented phase-separated structure is easily formed even in a film thickness of 25 nm or more.
[0092] The BCP precursor can be obtained, for example, by carrying out a polymerization reaction of a monomer (e.g., styrene or a derivative thereof, hereinafter also referred to as monomer (b1)) that derives the structural unit (b1), and then adding a monomer (e.g., glycidyl methacrylate, allyl methacrylate, etc., hereinafter also referred to as monomer (b2gp)) that derives the structural unit (b2m) to the polymerization reaction liquid and further carrying out a polymerization reaction. Alternatively, the BCP precursor can be obtained by carrying out a polymerization reaction using a mixture of monomer (b2gp) and monomer (b2m), and then adding monomer (b1) to the polymerization reaction liquid and further carrying out a polymerization reaction. The polymerization reaction is preferably living polymerization because it is narrowly dispersed and easy to synthesize. Preferred living polymerization methods include living anionic polymerization and living radical polymerization, and living anionic polymerization is particularly preferred because it can achieve a more narrow dispersion.
[0093] In the process for producing a random copolymer consisting of the structural unit (b2gp) and the structural unit (b2m), the ratio of the number of moles of the monomer (b2gp) in the mixture of the monomer (b2gp) and the monomer (b2m) to the total number of moles of the monomer (b2gp) and the monomer (b2m) is more than 0 and 0.10 or less. The ratio of the number of moles of the monomer (b2gp) is preferably less than 0.10, more preferably 0.09 or less, even more preferably 0.08 or less, and particularly preferably 0.07 or less. The ratio of the number of moles of the monomer (b2gp) is preferably 0.0050 or more, more preferably 0.0070 or more, even more preferably 0.0090 or more, particularly preferably 0.0095 or more, and most preferably 0.0099 or more. When the ratio of the number of moles of the monomer (b2gp) is equal to or greater than the lower limit, a vertically oriented phase-separated structure is easily formed even in a film thickness of 25 nm or more.When the ratio of the number of moles of the monomer (b2gp) is equal to or less than the upper limit, a vertically oriented phase-separated structure is easily formed even in a film thickness of 25 nm or more.
[0094] In the process for producing a random copolymer consisting of the structural unit (b2gp) and the structural unit (b2m), the ratio of the number of moles of the monomer (b2m) in the mixture of the monomer (b2gp) and the monomer (b2m) is 0.90 or more and less than 1.0 relative to the total number of moles of the monomer (b2gp) and the monomer (b2m). The ratio of the number of moles of the monomer (b2m) is preferably more than 0.90, more preferably 0.91 or more, even more preferably 0.92 or more, and particularly preferably 0.93 or more. The ratio of the number of moles of the monomer (b2m) is preferably 0.9950 or less, more preferably 0.9930 or less, even more preferably 0.9910 or less, particularly preferably 0.9905 or less, and even more preferably 0.9901 or less. When the ratio of the number of moles of the monomer (b2m) is equal to or greater than the lower limit, a vertically oriented phase-separated structure is easily formed even in a film thickness of 25 nm or more. When the ratio of the number of moles of the monomer (b2m) is equal to or less than the upper limit, a vertically oriented phase-separated structure is easily formed even in a film thickness of 25 nm or more.
[0095] In the process for producing a BCP precursor, the ratio of the number of moles of the monomer (b1) to the total number of moles of the monomer (b2gp) and the monomer (b2m) is preferably from 0.25 to 4.0, more preferably from 0.33 to 3.0, and even more preferably from 0.5 to 2.0. When the molar ratio of the monomer (b1) is within the above numerical range, a vertically oriented phase-separated structure is easily formed even in a film thickness of 25 nm or more.
[0096] Process (p2): R 2 A compound represented by the formula (hereinafter referred to as "compound (R 2 The compound (b2gp) reacts with the epoxy group or vinyl group of the structural unit (b2gp) to convert the structural unit (b2gp) into the structural unit (b2g). When the building block (b2gp) contains an epoxy group, the BCP precursor and the compound (R 2The reaction of R2gp with the compound (R-SH) can be carried out in an organic solvent such as tetrahydrofuran in the presence of a catalyst such as lithium hydroxide. The reaction temperature can be set, for example, at 20 to 60°C, preferably 30 to 50°C, and more preferably 35 to 45°C. The reaction time can be appropriately set depending on the amount of BCP precursor used, and may be a time sufficient for all of the structural units (b2gp) in the precursor of the second block to be converted to structural units (b2g). The reaction time can be set, for example, for 1 to 10 hours. When the structural unit (b2gp) contains a vinyl group, the reaction of the BCP precursor with the compound (R2gp with 2 The reaction of -SH) can be carried out by a thiol-ene reaction. The thiol-ene reaction can be carried out in an organic solvent such as tetrahydrofuran in the presence of a catalyst such as azobisisobutyronitrile (AIBN). The reaction temperature can be, for example, 60 to 90°C, preferably 70 to 90°C, and more preferably 75 to 85°C. The reaction time can be appropriately set depending on the amount of the BCP precursor used, and may be a time sufficient for all of the structural units (b2gp) in the precursor of the second block to be converted to structural units (b2g). The reaction time can be, for example, 1 to 10 hours.
[0097] [ka] [In the formula, R 1 and R b1 is R in the formula (b1). 1 and R b1 n is the same as n in the above formula (b1). R 2 and R 3 is R in the formula (b2g). 2 and R 3 is the same as R b2 and x represents R in the formula (b2g) and the formula (b2m). b2 and x. Yp 2 Rp represents a linear or branched alkyl group having 1 to 8 carbon atoms. 2 represents an epoxy group or a vinyl group.
[0098] According to the resin composition for forming an etching mask pattern of the present embodiment described above, even when the film thickness of the layer containing the block copolymer is 25 nm or more, it is possible to form a vertically aligned phase separation structure. Therefore, the phase separation structure can be used as an etching mask.
Examples
[0099] Hereinafter, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples.
[0100] (Synthesis of BCP precursor) (Synthesis of BCP precursor (1)) All anionic polymerizations were carried out under an argon atmosphere. 30 mL of tetrahydrofuran (THF) and lithium chloride (LiCl) (21.2 mg, 0.500 mmol) were transferred to a 50 mL Schlenk tube and cooled to -78 °C in a Cool-Nexus bath. Sec-butyllithium (Sec-BuLi) (1.05 M hexane / cyclohexane solution) was added to the Schlenk tube until the color of the solution turned yellow. The Schlenk tube was removed from the Cool-Nexus bath and warmed to room temperature until the solution became colorless. The Schlenk tube was cooled again to -78 °C in the Cool-Nexus bath, and sec-BuLi (0.095 mL, 0.100 mmol) was added as an initiator. Styrene (0.977 mL, 8.50 mmol) was added and stirred for 30 minutes. As a result, a bright orange solution was obtained. 1,1-Diphenylethylene (DPE) (0.088 mL, 0.50 mmol) was added, and the color of the solution changed to dark red. After stirring for 30 minutes, a monomer mixture of methyl methacrylate (MMA) (0.730 mL, 6.85 mmol) and glycidyl methacrylate (GMA) (0.244 mL, 2.05 mmol) was added and stirred for 30 minutes. The color of the solution changed from red to transparent. As a terminator, 3 mL of degassed methanol (MeOH) was added to the Schlenk tube to terminate the polymerization. The Schlenk tube was lifted out of the Cool-Nexus bath, and the solution was poured into MeOH for reprecipitation. After filtering the solid of the precipitate, it was dried under reduced pressure at 40 °C to obtain a white powder of BCP precursor (1) (1.86 g, 88% yield).
[0101] <Synthesis of BCP Precursor (2)> The BCP precursor (2) was synthesized in the same manner as the synthesis of the above BCP precursor (1), except that the amount of styrene used was 1.07 mL (9.29 mmol), the amount of MMA used was 0.936 mL (8.79 mmol), and the amount of GMA used was 0.117 mL (0.976 mmol).
[0102] <Synthesis of BCP Precursor (3)> The BCP precursor (3) was synthesized in the same manner as the synthesis of the above BCP precursor (1), except that the amount of styrene used was 1.15 mL (10.00 mmol), the amount of MMA used was 1.03 mL (9.69 mmol), and the amount of GMA used was 0.087 mL (0.729 mmol).
[0103] <Synthesis of BCP Precursor (4)> The BCP precursor (4) was synthesized in the same manner as the synthesis of the above BCP precursor (1), except that the amount of styrene used was 1.08 mL (9.42 mmol), the amount of MMA used was 1.14 mL (10.72 mmol), and the amount of GMA used was 0.067 mL (0.564 mmol).
[0104] <Synthesis of BCP Precursor (5)> The BCP precursor (5) was synthesized in the same manner as the synthesis of the above BCP precursor (1), except that the amount of styrene used was 1.30 mL (11.28 mmol), the amount of MMA used was 1.37 mL (12.90 mmol), and the amount of GMA used was 0.016 mL (0.130 mmol).
[0105] (Synthesis of Block Copolymer) <Synthesis of BCP (1)> 0.2 g of the BCP precursor (1) and THF (20 wt% solution) were placed in a 10 mL glass tube and immersed in an ice water bath. An aqueous solution of 1 wt% lithium hydroxide (LiOH) (0.05 molar equivalent of LiOH / GMA unit) and 2,2,2-trifluoroethanethiol (2 molar equivalents / GMA unit) were added to the glass tube. After stirring at room temperature for 20 minutes, the reactor was set to 40 °C and stirred for 3 hours to synthesize BCP (1). Depending on the Mn and PHFMA fraction of the synthesized BCP (1), precipitation was repeated several times with methanol or methanol / hexane to remove residual reagents. The product was dried under reduced pressure at room temperature overnight to obtain a white powder of BCP (1). The Mn and dispersity (PDI = Mw / Mn) of the BCP precursor (1) measured by size exclusion chromatography (SEC) were 21000 gmol -1 and 1.03, respectively.
[0106] <Synthesis of BCP (2) - (5)> BCP (2) - (5) were synthesized in the same manner as the synthesis of BCP (1) above, except that BCP precursors (2) - (5) were used instead of the BCP precursor (1). The Mn and dispersity (PDI = Mw / Mn) of BCP (2) measured by size exclusion chromatography (SEC) were 21000 gmol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP (3) measured by size exclusion chromatography (SEC) were 22000 gmol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP (4) measured by size exclusion chromatography (SEC) were 22000 gmol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP (5) measured by size exclusion chromatography (SEC) were 25000 gmol -1 and 1.03, respectively.
[0107]
Chemical formula
[0108] The value of x in the obtained BCPs (1) to (5) was the same as the ratio of the number of moles of GMA to the total number of moles of MMA and GMA used in the synthesis of the BCP precursor.
[0109] <Measurement of the volume of each block> The mole percentage of each block in the block copolymer is 1 The mass percentage of each block was calculated from the results of H NMR analysis, and the mass percentage of each block was further calculated. The mass percentage of each block was then divided by the density of each block to calculate the volume ratio of each block. From the volume ratio, the proportion of the volume of the polystyrene block in the total volume of the block copolymer was calculated. The density of each block was estimated by the atomic group contribution method (Fedors, RF Polym. Eng. Sci. 1974, 14, 147-154.). The density of the polystyrene block was 1.05 gm -3 The density of the structure composed of structural units derived from methyl methacrylate was 1.18 gcm -3 The density of the structure composed of building blocks derived from 2-hydroxy-3-(2,2,2-trifluoroethylsulfanyl)propyl methacrylate was 1.43 gcm -3 The density of the structure composed of building blocks derived from 2-hydroxy-3-(ethylsulfanyl)propyl methacrylate, 2-hydroxy-3-(1-propyl)propyl methacrylate, 2-hydroxy-3-(1-hexyl)propyl methacrylate, or 2-hydroxy-3-(cyclohexyl)propyl methacrylate was 1.18 gcm -3 was used.
[0110] Table 1 shows the number average molecular weight (Mn) of each block copolymer synthesized above, the volume ratio (vol %) of the polystyrene block (PS) to the total volume of the block copolymer, and the value of x in the above reaction formula.
[0111] [Table 1]
[0112] <Preparation of Resin Composition for Forming Etching Mask Pattern> Each of the components shown in Table 2 was mixed and dissolved in an organic solvent component to prepare a resin composition for forming an etching mask pattern (solid content concentration: 1.6% by mass). PGMEA (polyethylene glycol monomethyl ether acetate) was used as the organic solvent component.
[0113] [Table 2]
[0114] In Table 1, the abbreviations have the following meanings. The numbers in brackets [ ] indicate the blend amount (parts by mass). BCP-1: BCP(1). BCP-2: BCP(2). BCP-3: BCP(3). BCP-4: BCP(4). BCP-5: BCP(5). (S)-1: PGMEA (polyethylene glycol monomethyl ether acetate)
[0115] Using the resin composition for forming an etching mask pattern of each of the above examples, a structure including a phase-separated structure was obtained by a production method including the steps (i) to (iii) shown below.
[0116] (Rating 1) <Production of Structure Including Phase Separation Structure> (Preparation of primer) To prepare the primer, primer resins NL-(1) to NL-(4) were prepared. All of NL-(1) to NL-(4) are random copolymers made of styrene, methyl methacrylate, and (hydroxyethyl) methacrylate.
[0117] The composition ratio (proportion (molar ratio) of each structural unit in the structural formula) St / MMA / HEMA of NL-(1) to NL-(4) was as follows. "St" means styrene, "MMA" means methyl methacrylate, and HEMA means (hydroxyethyl) methacrylate. The number average molecular weight (Mn) and water contact angle (WCA) of NL-(1) to NL-(4) were as follows.
[0118] NL-(1) had St / MMA / HEMA=39 / 56 / 5, Mn was 24,000, and WCA was 72°. NL-(2) had St / MMA / HEMA=49 / 46 / 5, Mn was 28,000, and WCA was 75°. NL-(3) had St / MMA / HEMA=61 / 34 / 5, Mn was 30,000, and WCA was 77°. NL-(4) had St / MMA / HEMA=70 / 25 / 5, Mn was 29,000, and WCA was 79°.
[0119] 100 parts by mass of each of the primer resins NL-(1) to NL-(4) were mixed and dissolved in 9900 parts by mass of PGMEA to prepare primers NL-1 to NL-4.
[0120] Process (i): A 12-inch silicon wafer was prepared as a support.
[0121] A silicon substrate was spin-coated with any one of the primers NL-1 to NL-4, and then heated in air at 250° C. for 5 minutes. As a result, a 30 nm-thick primer layer made of any one of the primer resins NL-(1) to NL-(4) was formed on the substrate surface. The undercoat layer was then rinsed with a rinse solution (PGME / PGMEA=7 / 3) consisting of propylene glycol monomethyl ether (PGME) and propylene glycol monomethyl ether acetate (PGMEA), and then heated at 100° C. for 1 minute to volatilize the rinse solution.
[0122] Next, the resin composition of each example was spin-coated onto the substrate so as to have a film thickness of 36 nm, thereby forming a resin composition layer (a layer containing a block copolymer).
[0123] Step (ii): The resin composition layer formed on the substrate was prebaked at 90° C. for 60 seconds in a nitrogen atmosphere, and then annealed at 240° C. for 5 minutes in a nitrogen atmosphere to form a phase-separated structure.
[0124] Step (iii): The substrate on which the phase-separated structure was formed was subjected to oxygen plasma treatment (200 mL / min, 40 Pa, 40°C, 200 W, 10 seconds) using TCA-3822 (Tokyo Ohka Kogyo Co., Ltd.) to selectively remove the PMMA phase.
[0125] [Resolution evaluation] The phase separation structure on the surface of the obtained substrate was analyzed by SEM image at 100,000x magnification using Hitachi High-Technologies' "CG6300". Next, the pattern period was analyzed from the SEM image using Hitachi High-Technologies' "Terminal PC Software". The results of the resolution evaluation are shown in Table 3.
[0126] Judgment criteria: A: The period was less than 24 nm. B: The period was 24 nm or more. When the resin composition of Comparative Example 1 was used, a phase-separated structure was not formed, and therefore the resolution could not be calculated. These are indicated by "-".
[0127] [Evaluation of vertical alignment margin] The margin of vertical alignment was evaluated using the undercoating agents NL-1 to NL-4. Judgment criteria: A: In all cases where NL-1 to NL-4 were used, the phase-separated structure had a perpendicular orientation. B: When any of NL-1 to NL-4 is used, the phase-separated structure does not have a perpendicular alignment property. C: In all the cases where NL-1 to NL-4 were used, the phase-separated structure did not have a perpendicular orientation. The evaluation results of the margin of vertical alignment are shown in Table 3.
[0128] [Table 3]
[0129] Examples 1 to 4 were rated A in the [Evaluation of resolution]. Compared with Comparative Example 1, Examples 1 to 4 exhibited superior results in the [Evaluation of margin of vertical alignment].
[0130] Using the resin composition for forming an etching mask pattern of each of the above examples, a structure including a phase-separated structure was obtained by a production method including the steps (i) and (ii) described below. [Evaluation of vertical alignment] was carried out according to the evaluation method described in <Evaluation 2> below. The results are shown in Table 4.
[0131] (Rating 2) <Production of Structure Including Phase Separation Structure> As in <Production of structure containing phase-separated structure> in (Evaluation 1), a base layer was formed on a 12-inch silicon wafer using the above NL-2. Next, a guide pattern was formed, and then a structure containing a phase-separated structure was produced as in <Production of structure containing phase-separated structure> in (Evaluation 1).
[0132] The guide pattern was formed as follows. The organic anti-reflective coating composition "ARC-29A" (trade name, Brewer Science) was applied onto a 12-inch silicon wafer using a spinner, and baked on a hot plate at 205°C for 60 seconds to dry, forming an organic anti-reflective coating with a thickness of 89 nm. The organic anti-reflective coating was spin-coated with the undercoat agent NL-2, and then heated at 250°C for 600 seconds. As a result, a thin film with a thickness of 10 nm made of the undercoat agent resin NL-(2) was formed on the substrate surface. A resist film for forming a guide pattern was applied onto the film, applied using a spinner, pre-baked (PAB) on a hot plate, and dried to form a resist film for forming a guide pattern with a thickness of 90 nm. An ArF excimer laser (193 nm) was selectively irradiated through a mask pattern using an ArF exposure device XT-1900Gi (ASML). Then, post-exposure baking (PEB) was performed, and the wafer was developed with butyl acetate and dried by shaking off. Next, post-baking was performed under conditions of 100° C. for 1 minute and then 200° C. for 5 minutes to form a guide pattern that matched the space dimension five times the d value of the block copolymer used.
[0133] [Evaluation of vertical alignment] The surface (phase-separated state) of the obtained substrate was observed with a length measuring SEM (scanning electron microscope, product name: CG6300, manufactured by Hitachi High-Technologies Corporation) to evaluate the vertical alignment of the phase-separated structure. The results are shown in Table 4.
[0134] Judgment criteria: A: A phase-separated structure having a vertical alignment is formed over the entire surface of the substrate on which the guide pattern is formed. B: In a part of the substrate on which the guide pattern is formed, a phase-separated structure having a perpendicular alignment property is not formed.
[0135] [Table 4]
[0136] In Examples 1 to 4, a phase separation structure having vertical alignment could be formed better than in Comparative Example 1.
[0137] Furthermore, BCPs (6) to (25) were synthesized. Using these, a structure including a phase separation structure was manufactured by the same method as the evaluation methods of (Evaluation 1) and (Evaluation 2) described above, and the obtained phase separation structure was evaluated.
[0138] (Synthesis of block copolymer) <Synthesis of BCPs (6) to (10)> BCPs (6) to (10) were synthesized by the same method as the synthesis method of BCPs (1) to (5), except that ethanethiol was used instead of 2,2,2-trifluoroethanethiol for the above-described BCP precursors (1) to (5).
[0139] The Mn and dispersity (PDI = Mw / Mn) of BCP (6) measured by size exclusion chromatography (SEC) were 21000 g / mol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP (7) measured by size exclusion chromatography (SEC) were 21000 g / mol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP (8) measured by size exclusion chromatography (SEC) were 22000 g / mol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP (9) measured by size exclusion chromatography (SEC) were 22000 g / mol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP (10) measured by size exclusion chromatography (SEC) were 25000 g / mol -1 and 1.03, respectively.
[0140] The analysis results of the NMR measurement for BCP (7) were as follows. 11H NMR (400 MHz, CDCl 3 , δ, ppm): 0.85 - 1.02 (α-CH 3 , PMMA, PGEMA), 1.23 - 1.69 (-S-CH 2 -CH 3 , PGEMA, -CH 2 -CH-, PS backbone), 1.74 - 2.02 (-CH 2 -CH-, PS backbone, -CH 2 -C(CH 3 )-, PGEMA and PMMA), 2.63 (-CH(OH)-CH 2 -S-CH 2 -CH 3 , PGEMA), 3.60 (-O-CH 3 , PMMA), 3.99 (-(C=O)O-CH 2 -CH(OH), PGEMA), 6.39 - 6.85 (o-aromatic, PS), 6.91 - 7.42 (p-, m-aromatic, PS).
[0141]
Chem.
[0142] <Synthesis of BCP(11)~(15)> For the above BCP precursors (1)~(5), BCP(11)~(15) were synthesized by the same method as the synthesis method of BCP(1)~(5), except that 1-propanethiol was used instead of 2,2,2-trifluoroethanethiol.
[0143] The Mn and dispersity (PDI = Mw / Mn) of BCP(11) measured by size exclusion chromatography (SEC) were 21000 g / mol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP(12) measured by size exclusion chromatography (SEC) were 21000 g / mol -1 and 1.03, respectively. The Mn and polydispersity (PDI = Mw / Mn) of BCP(13) measured by size exclusion chromatography (SEC) were 22,000 gmol -1 and 1.03. The Mn and polydispersity index (PDI = Mw / Mn) of BCP(14) measured by size exclusion chromatography (SEC) were 22,000 gmol -1 and 1.03. The Mn and polydispersity (PDI = Mw / Mn) of BCP(15) measured by size exclusion chromatography (SEC) were 25,000 gmol -1 and 1.03.
[0144] The analytical results of NMR measurement for BCP(12) were as follows: 1 H NMR (400 MHz, CDCl 3 , δ, ppm): 0.85-1.02 (α-CH 3 ,PMMA, PGPMA,-S-CH 2 -CH 2 -CH 3 ,PGPMA,), 1.23-1.69(-S-CH 2 -CH 2 -CH 3 ,PGPMA, -CH 2 -CH-,PS backbone), 1.74-2.02(-CH 2 -CH-,PS backbone, -CH 2 -C(CH 3 )-,PGPMA and PMMA), 2.63(-CH(OH)-CH 2 -S-CH 2 -CH 2 -,PGPMA), 3.60(-O-CH 3 , PMMA), 3.99(-(C=O)O-CH 2 -CH(OH),PGPMA), 6.39-6.85(o-aromatic,PS),6.91-7.42(p-, m-aromatic,PS).
[0145] [ka]
[0146] <Synthesis of BCP(16) - (20)> For the above - mentioned BCP precursors (1) - (5), BCP(16) - (20) were synthesized by the same method as the synthesis method of BCP(1) - (5), except that 1 - hexanethiol was used instead of 2,2,2 - trifluoroethanethiol.
[0147] The Mn and dispersity (PDI = Mw / Mn) of BCP(16) measured by size - exclusion chromatography (SEC) were 21000 g / mol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP(17) measured by size - exclusion chromatography (SEC) were 21000 g / mol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP(18) measured by size - exclusion chromatography (SEC) were 22000 g / mol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP(19) measured by size - exclusion chromatography (SEC) were 22000 g / mol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP(20) measured by size - exclusion chromatography (SEC) were 25000 g / mol -1 and 1.03, respectively.
[0148] The analysis results of the NMR measurement for BCP(17) were as follows. 1 H NMR(400 MHz, CDCl 3 , δ, ppm): 0.85 - 1.02 (α - CH 3 , PMMA, PGHMA, - CH 2 - CH 2 - CH 3 , PGHMA,), 1.23 - 1.69 (- S - CH2 -CH 2 -CH 2 -CH 2 -CH 2 -, PGHMA, -CH 2 -CH-, PS backbone), 1.74 - 2.02(-CH 2 -CH-, PS backbone, -CH 2 -C(CH 3 )-, PGHMA and PMMA), 2.63(-CH(OH)-CH 2 -S-CH 2 -CH 2 -, PGHMA), 3.60(-O-CH 3 , PMMA), 3.99(-(C=O)O-CH 2 -CH(OH), PGHMA), 6.39 - 6.85(o-aromatic, PS), 6.91 - 7.42(p-, m-aromatic, PS).
[0149]
Chem.
[0150] <Synthesis of BCP(21) - (25)> For the above BCP precursors (1) - (5), BCP(21) - (25) were synthesized by the same method as the synthesis method of BCP(1) - (5), except that cyclohexanethiol was used instead of 2,2,2-trifluoroethanethiol.
[0151] The Mn and dispersity (PDI = Mw / Mn) of BCP(21) measured by size exclusion chromatography (SEC) were 21000 g / mol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP(22) measured by size exclusion chromatography (SEC) were 21000 g / mol -1 and 1.03, respectively. The Mn and polydispersity (PDI = Mw / Mn) of BCP (23) measured by size exclusion chromatography (SEC) were 22,000 gmol -1 and 1.03. The Mn and polydispersity (PDI = Mw / Mn) of BCP(24) measured by size exclusion chromatography (SEC) were 22,000 gmol -1 and 1.03. The Mn and polydispersity (PDI = Mw / Mn) of BCP(25) measured by size exclusion chromatography (SEC) were 25,000 gmol -1 and 1.03.
[0152] The analytical results of NMR measurement for BCP(22) are as follows: 1 H NMR (400 MHz, CDCl 3 , δ, ppm): 0.85-1.02 (α-CH 3 ,PMMA, PGCMA), 1.23-1.69(-S-CH(CH 2 -CH 2 )-CH 2 -CH 2 -CH 2 -,PGCMA, -CH 2 -CH-,PS backbone), 1.74-2.02(-S-CH(CH 2 -CH 2 )-CH 2 -CH 2 -CH 2 -,PGCMA,-CH 2 -CH-,PS backbone, -CH 2 -C(CH 3 )-,PGCMA and PMMA), 2.63(-CH(OH)-CH 2 -S-CH(CH 2 -CH 2 )-CH 2 -CH 2 -CH 2 -,PGCMA), 3.60(-O-CH 3 , PMMA), 3.99(-(C=O)O-CH 2-CH(OH),PGCMA), 6.39-6.85(o-aromatic,PS),6.91-7.42(p-, m-aromatic,PS).
[0153] [ka]
[0154] The value of x in the obtained BCPs (6) to (25) was the same as the ratio of the number of moles of GMA to the total number of moles of MMA and GMA used in the synthesis of the BCP precursor.
[0155] The volume ratio of the polystyrene block was calculated in the same manner as in <Measurement of the volume of each block> above.
[0156] The number average molecular weight (Mn) of each block copolymer synthesized above, the volume ratio (volume %) of the polystyrene block (PS) to the total volume of the block copolymer, and the value of x in the above reaction formula are summarized in Tables 5 to 8. In all of BCP(6) to BCP(25), the density of the structure composed of constitutional units derived from methyl methacrylate was 1.18 gcm -3 was used.
[0157] [Table 5]
[0158] [Table 6]
[0159] [Table 7]
[0160] [Table 8]
[0161] (Comparative Examples 2 to 5, Examples 5 to 20) <Preparation of Resin Composition for Forming Etching Mask Pattern> Each of the components shown in Tables 9 to 12 was mixed and dissolved in an organic solvent component to prepare a resin composition for forming an etching mask pattern (solid content concentration: 1.6% by mass). PGMEA (polyethylene glycol monomethyl ether acetate) was used as the organic solvent component.
[0162] [Table 9]
[0163] [Table 10]
[0164] [Table 11]
[0165] [Table 12]
[0166] In Tables 9 to 12, the numbers in brackets [ ] indicate the blend amount (parts by mass). BCP-6 to BCP-25 mean the above-mentioned BCP(6) to BCP(25), respectively.
[0167] Using the resin compositions for forming etching mask patterns of Examples 5 to 20 and Comparative Examples 2 to 5, [Evaluation of resolution] and [Evaluation of margin of vertical alignment] were carried out in the same manner as in (Evaluation 1) above. The results are shown in Table 13. When the resin compositions of Comparative Examples 2 to 5 were used, a phase separation structure was not formed, so it was not possible to calculate the resolution. These are indicated with "-". The evaluation of the vertical alignment was carried out in the same manner as in the above-mentioned (Evaluation 2). The results are shown in Table 14.
[0168]
Table 13
[0169] In Examples 5 - 8, 9 - 12, 13 - 16, and 17 - 20, [Evaluation of Resolution] was A. In Examples 5 - 8, 9 - 12, 13 - 16, and 17 - 20, the results of [Evaluation of Margin of Vertical Alignment] were superior to those of Comparative Examples 2 - 5.
[0170]
Table 14
[0171] In Examples 5 - 8, 9 - 12, 13 - 16, and 17 - 20, a phase - separation structure having vertical alignment could be formed better than in Comparative Examples 2 - 5.
[0172] <Synthesis of BCP(26) - (30)> BCP(26) - (30) were synthesized in the same manner as the synthesis method of BCP(1) - (5), except that 3 - mercapto - 1 - hexanol was used instead of 2,2,2 - trifluoroethanethiol for the above - mentioned BCP precursors (1) - (5).
[0173] The Mn and dispersity (PDI = Mw / Mn) of BCP(26) measured by size - exclusion chromatography (SEC) were 21000 g / mol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP(27) measured by size - exclusion chromatography (SEC) were 21000 g / mol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP(28) measured by size - exclusion chromatography (SEC) were 22000 g / mol -1 and 1.03, respectively. The Mn and dispersity (PDI = Mw / Mn) of BCP(29) measured by size - exclusion chromatography (SEC) were 22000 g / mol-1 and 1.03. The Mn and polydispersity (PDI = Mw / Mn) of BCP(30) measured by size exclusion chromatography (SEC) were 25,000 gmol -1 and 1.03.
[0174] The analytical results of NMR measurement for BCP(27) were as follows: 1 H NMR (400MHz, CDCl3, δ, ppm): 0.71-1.05(α-CH3,PMMA and PGOMA, -S-CH-CH2-CH2-CH3, PGOMA),1.43-2.02( -S-CH-CH2-CH2-CH3 ,PGOMA,-S-CH-CH2-CH2-OH ,PGOMA, -CH2-CH-,PS backbone, -CH2-C(CH3)-,PGOMA and PMMA),2.68-2.88(-CH(OH)-CH2-S-CH(-,PGOMA),3.60(-O-CH3,PMMA),3.73(-S-CH-CH2-CH2-OH ,PGOMA),4.08(-(C=O)O-CH2-CH(OH),PGOMA),6.39-6.85(o-aromatic,PS),6.91-7.42(p-, m-aromatic,PS).
[0175] [ka]
[0176] The value of x in the obtained BCPs (26) to (30) was the same as the ratio of the number of moles of GMA to the total number of moles of MMA and GMA used in the synthesis of the BCP precursor.
[0177] The volume ratio of the polystyrene block was calculated in the same manner as in <Measurement of the volume of each block> above.
[0178] The number average molecular weight (Mn) of each block copolymer synthesized above, the volume ratio (volume %) of the polystyrene block (PS) to the total volume of the block copolymer, and the value of x in the above reaction formula are summarized in Table 15. In all of BCP(26) to BCP(30), the density of the structure composed of constitutional units derived from methyl methacrylate was 1.18 gcm -3 was used.
[0179] [Table 15]
[0180] (Comparative Example 6, Examples 21 to 24) <Preparation of Resin Composition for Forming Etching Mask Pattern> Each of the components shown in Table 16 was mixed and dissolved in an organic solvent component to prepare a resin composition for forming an etching mask pattern (solid content concentration: 1.6% by mass). PGMEA (polyethylene glycol monomethyl ether acetate) was used as the organic solvent component.
[0181] [Table 16]
[0182] In Table 16, the numbers in brackets [ ] indicate the blend amount (parts by mass). BCP-26 to BCP-30 mean the above-mentioned BCP(26) to BCP(30), respectively.
[0183] Using the resin compositions for forming etching mask patterns of Examples 21 to 24 and Comparative Example 6, [Evaluation of resolution] and [Evaluation of margin of vertical alignment] were performed in the same manner as in (Evaluation 1) above. The results are shown in Table 17. When the resin composition of Comparative Example 6 was used, a phase separation structure was not formed, so the resolution could not be calculated. These are indicated with "-". The evaluation of the vertical alignment was carried out in the same manner as in the above-mentioned (Evaluation 2). The results are shown in Table 18.
[0184] [Table 17]
[0185] [Table 18]
[0186] In comparison with Comparative Example 6, in Examples 21 to 24, a phase-separated structure having vertical alignment was successfully formed.
Claims
1. A step of applying a resin composition for forming an etching mask pattern onto a support to form a layer containing a block copolymer and having a thickness of 25 nm or more; allowing the layer containing the block copolymer to phase separate; having The resin composition for forming an etching mask pattern contains a block copolymer having a first block and a second block, The first block is composed of a polymer having a repeating structure of a structural unit represented by the following general formula (b1): The second block is composed of a random copolymer having a structure in which a constitutional unit represented by the following general formula (b2m) and a constitutional unit represented by the following general formula (b2g) are randomly arranged, A ratio of the volume of the first block to a total volume of the first block and the second block is 20 to 80 volume %. A method for producing an etching mask pattern. 【Chemistry 1】 [In formula (b1), R 1 is an alkyl group which may have an oxygen atom or a silicon atom. n is an integer of 0 to 5. When n is an integer of 2 or more, a plurality of R 1 may be the same or different. b1 is a hydrogen atom or a methyl group. In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, a cyano group, an amino group, a hydroxy group or a phosphate group. R 3 is a linear or branched alkylene group having 1 to 10 carbon atoms which may have a hydroxyl group. In formula (b2g) and formula (b2m), R b2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 may be the same or different. x represents a molar ratio and is greater than 0 and not greater than 0.
10.
2. A resin composition for forming an etching mask pattern, comprising a block copolymer having a first block and a second block, The first block is composed of a polymer having a repeating structure of a structural unit represented by the following general formula (b1): The second block is composed of a random copolymer having a structure in which a constitutional unit represented by the following general formula (b2m) and a constitutional unit represented by the following general formula (b2g) are randomly arranged, A ratio of the volume of the first block to a total volume of the first block and the second block is 20 to 80 volume %. A resin composition for forming an etching mask pattern. 【Chemistry 2】 [In formula (b1), R 1 is an alkyl group which may have an oxygen atom or a silicon atom. n is an integer of 0 to 5. When n is an integer of 2 or more, a plurality of R 1 may be the same or different. b1 is a hydrogen atom or a methyl group. In formula (b2g), R 2 is an alkyl group which may have a silicon atom, a fluorine atom, a carboxy group, a cyano group, an amino group, a hydroxy group or a phosphate group. R 3 is a linear or branched alkylene group having 1 to 10 carbon atoms which may have a hydroxyl group. In formula (b2g) and formula (b2m), R b2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. b2 may be the same or different. x represents a molar ratio and is greater than 0 and equal to or less than 0.10.
Citation Information
Patent Citations
Pattern formation method and mold
JP2008036491A
Resin composition for forming phase separation structure, method for producing structure body including phase separation structure, and block copolymer
JP2022020519A