Sheet for structure

The structural sheet with a functional, intermediate, and adhesive layer addresses shear deformation and peeling issues in roof repairs, ensuring durability and watertightness by maintaining adhesion across varying temperatures.

JP2024159637AInactive Publication Date: 2024-11-08KEIWA INCORPORATED
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024070944
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-24
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing roof repair methods using polymer cement and resin layers are prone to shear deformation and peeling, leading to water infiltration, especially in deteriorated slate roofs and other structures.

Method used

A structural sheet with a functional layer, intermediate layer, and adhesive layer, featuring a storage modulus of 1.0×10^2 Pa at 80°C and 1.0×10^7 Pa at -10°C, which minimizes shear deformation and peeling, ensuring effective adhesion and water resistance.

Benefits of technology

The sheet effectively prevents shear deformation and peeling, even under extreme temperature conditions, providing a durable and watertight repair solution for roofs and other structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159637000001_ABST
    Figure 2024159637000001_ABST
Patent Text Reader

Abstract

To provide a sheet for a structure that is less prone to shear deformation and detachment from the substrate.SOLUTION: A sheet 2 for a structure comprises a functional layer 4, an intermediate layer 6, and an adhesive layer 8. The functional layer 4 has excellent weather resistance. The intermediate layer 6 contributes to the rigidity or the like of the sheet 2. The adhesive layer 8 contacts a foundation. The sheet 2 is affixed to the structure by the adhesive force of the adhesive layer 8. The material of the adhesive layer 8 is an adhesive composition comprising a polymer as a base material. The storage elastic modulus of the adhesive layer 8 at 80°C is 1.0×102 Pa or greater. The storage elastic modulus of the adhesive layer 8 at -10°C is 1.0×107 Pa or less.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This specification discloses a sheet that is attached to a structure for use. [Background technology]

[0002] When a slate roof of a house is exposed to wind and rain for a long period of time, it deteriorates. There is concern that a deteriorated slate roof may leak. To prevent leaks, paint is applied to the slate roof. However, in the case of a severely deteriorated slate roof, the leaks may not be prevented even by applying paint.

[0003] JP 2022-101896 A discloses a method for repairing a roof using a sheet having a polymer cement layer and a resin layer. By attaching this sheet to the roof, roof leakage can be suppressed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2022-101896 Summary of the Invention [Problem to be solved by the invention]

[0005] When a roof is repaired with the sheet disclosed in JP 2022-101896 A, a worker may step on the sheet. When the worker's weight is applied to the sheet, a shear force may be applied to the sheet. This shear force induces shear deformation (shift) of the sheet.

[0006] A multi-sheet repair can cover a large area of ​​a roof. In this repair, a second sheet is placed partially on top of a first sheet and adjacent to the first sheet. At the overlap, the second sheet can peel away from the underlying first sheet. This peeling can lead to water infiltration into the roof.

[0007] Similar problems arise when repairing roofs other than slate roofs, and when repairing or reinforcing structures other than roofs.

[0008] The applicant's intention is to provide a sheet for structures which is less susceptible to deformation due to shear force and which is less susceptible to peeling from the base. [Means for solving the problem]

[0009] The structural sheet disclosed in the present specification has a functional layer and an adhesive layer. The storage modulus of the adhesive layer at 80° C. is 1.0×10 2 The storage modulus of this adhesive layer at -10°C is 1.0 x 10 7 Pa or less. Effect of the Invention

[0010] This structural sheet is resistant to shear deformation even when applied in summer, and is resistant to peeling off from the base even in winter. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a perspective view showing a portion of a sheet for structures according to one embodiment. [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 3 is an enlarged view showing a portion marked with reference numeral III in FIG. [Figure 4] FIG. 4 is a front view of the structural sheet of FIG. 1 shown together with a roof. [Diagram 5] FIG. 5 is an enlarged view showing a portion marked with the symbol V in FIG. [Figure 6] FIG. 6 is an enlarged cross-sectional view taken along the line VI-VI in FIG. [Figure 7] FIG. 7 is an enlarged cross-sectional view taken along line VII-VII in FIG. [Figure 8]FIG. 8 is a flowchart showing a method of repairing a roof using the structural sheet of FIG. [Figure 9] FIG. 9 is a cross-sectional view showing a portion of the structure sheet according to the second embodiment. [Figure 10] FIG. 10 is a cross-sectional view showing a portion of the structural sheet according to the third embodiment. [Figure 11] FIG. 11 is a perspective view showing a method for measuring the shear force of the structural sheet according to the embodiment. [Figure 12] FIG. 12 is a cross-sectional view illustrating a structure of a structural sheet according to a fourth embodiment. [Figure 13] FIG. 13 is a cross-sectional view illustrating a structure of a structural sheet according to the fifth embodiment. [Figure 14] FIG. 14 is a cross-sectional view illustrating a structure of a structural sheet according to the sixth embodiment. [Figure 15] FIG. 15 is a schematic diagram showing the structure of a supply item containing a structural sheet according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, preferred embodiments will be described in detail with reference to the drawings as appropriate. First Embodiment [Layer structure] FIG. 1-3 shows a sheet 2 for a structure (hereinafter, also referred to as the sheet 2). The planar shape of the sheet 2 is generally rectangular. As is clear from FIG. 3, the sheet 2 includes a functional layer 4, an intermediate layer 6, and an adhesive layer 8, each of which includes at least one layer. As is clear from FIG. 3, the sheet 2 includes, for example, a single functional layer 4, an intermediate layer 6, and an adhesive layer 8. The sheet 2 is attached to a structure. The sheet 2 may have a release paper or a release film (see the release film 9 in FIG. 12). The release paper and the release film are laminated with the adhesive layer 8. The release paper or the release film may remain until a predetermined timing, such as when the sheet 2 is used. As will be described later, at least one of the adhesive layer 8 and the functional layer 4 may contain a filler.

[0013] [Functional Layer] In this embodiment, the functional layer 4 is located at the top. In other words, when the sheet 2 is attached to a base (such as a structure), the functional layer 4 is located at the furthest position from the base. The functional layer 4 in this embodiment is disposed above the adhesive layer 8. The functional layer 4 contributes to a function desired for the sheet 2. Examples of such functions include light resistance, weather resistance, heat resistance, abrasion resistance, chemical resistance, water impermeability, moisture impermeability, and moisture permeability. The functional layer 4 can contribute to one or more functions.

[0014] The material of the functional layer 4 is a polymer composition. This functional layer 4 is generally flexible. The sheet 2 having this functional layer 4 can conform to the unevenness of the substrate. The polymer composition includes a base polymer. Synthetic resins, synthetic rubbers, and natural rubbers can be included in the composition as base polymers.

[0015] When weather resistance is desired for the functional layer 4, the weather resistance of the functional layer 4 can be controlled, for example, by adjusting the material of the functional layer 4 or the selection and content of the material in the functional layer 4. When weather resistance is desired for the functional layer 4, the material of the functional layer 4 is preferably, for example, a base polymer that is not easily deteriorated by ultraviolet rays. Specifically, examples of the method include arranging a material (polymer, etc.) that can form a large number of bond structures having a bond energy stronger than ultraviolet rays (410 KJ / mol) in the functional layer 4, or increasing the content of the material in the functional layer 4. Examples of polymers that can contribute to the weather resistance of the functional layer 4 and the flexibility of the sheet 2 include acrylic resin, acrylic urethane resin, acrylic silicone resin, fluororesin, soft epoxy resin, and polybutadiene.

[0016] In addition, from the viewpoint of reducing the number of reaction sites in the functional layer 4 and chemically stabilizing the functional layer 4, the functional layer 4 may contain a material having a structure with few double bonds. If the material is present in a large amount in the functional layer 4, the chemical stability of the functional layer 4 increases. An example of such a material is a non-diene rubber. Specifically, the non-diene rubber may be at least one of CIIR (chlorinated butyl rubber), BIIR (brominated butyl rubber), and EPDM (ethylene propylene rubber). As a method for forming a large number of the bond structures in the functional layer 4, for example, a method of unevenly distributing at least one of a radical trapping material that traps radicals generated by irradiation of energy rays such as ultraviolet (UV), an additive such as HALS that absorbs UV and suppresses the generation of radicals, and an antioxidant such as a phenolic or thioether type can be exemplified.

[0017] From the viewpoint of weather resistance, an example of a resin that is particularly suitable for the base polymer of the functional layer 4 of this embodiment is an acrylic silicone resin. The acrylic silicone resin contains a siloxane bond. The acrylic silicone resin is also excellent in heat resistance and cold resistance. Specific examples of compositions containing an acrylic silicone resin include "Cool Life SP Black (CB1) P5-0" manufactured by Dainichi Seikagaku Kogyo Co., Ltd., "Bell Earth Elastic Black" manufactured by Fujikura Kasei Co., Ltd., "Aronbull Coat T-1000" manufactured by Toagosei Co., Ltd., and "Acryset EMN325E" and "U-Double EF008" manufactured by Nippon Shokubai Co., Ltd. The polymer composition of the functional layer 4 may contain additives such as pigments, fillers, reinforcing materials, and antifouling agents as necessary. The functional layer 4 containing a pigment has excellent cosmetic properties. The polymer composition may contain organic pigments and inorganic pigments. Examples of fillers include metal oxide particles such as silica, alumina, and titania. Examples of reinforcing materials include cellulose nanofibers. The content of each additive is adjusted according to its function.

[0018] In Fig. 3, the arrow T1 indicates the thickness of the functional layer 4. From the viewpoint of functionality, the thickness T1 is preferably 10 µm or more, more preferably 30 µm or more, and particularly preferably 40 µm or more. From the viewpoints of flexibility, productivity, and light weight of the sheet 2, the thickness T1 is preferably 500 µm or less, more preferably 300 µm or less, and particularly preferably 200 µm or less. The structure sheet 2 may have two or more functional layers 4. When the functional layer 4 contains a filler, it may contain the same filler as the filler contained in the intermediate layer 6 described later.

[0019] [Middle layer] The intermediate layer 6 contributes to the rigidity of the sheet 2. The intermediate layer 6 is, for example, a layer that determines the shape of the sheet 2. The intermediate layer 6 has, for example, a function of maintaining the overall shape of the sheet 2. A preferred material for the intermediate layer 6 is a composite material of a polymer and a filler. This makes it easier to impart a predetermined rigidity to the structural sheet 2. Examples of the polymer include acrylic resin, acrylic silicone resin, fluororesin, and silicone resin. Examples of the filler include cement, mortar, silica, alumina, titanium oxide, calcium carbonate, and carbon black. A preferred composite material includes acrylic resin and mortar. In particular, polymer cement is preferred. The materials exemplified above may be used alone or in combination.

[0020] By controlling the ratio of the resin component and mortar, which are the materials of the intermediate layer 6, the rigidity of the sheet for structure 2 can be easily controlled and the freedom of material design can be improved. In addition, the thickness of the intermediate layer 6 can be obtained to an extent that makes it easy to handle. Furthermore, for example, by adjusting the particle shape of the filler, the rigidity of the sheet for structure 2 can be controlled. Specific examples of the particle shape of the filler include spherical, acicular, amorphous, and tetrapod shapes. Furthermore, by adjusting the thickness of the intermediate layer 6, the rigidity of the sheet for structure 2 can be controlled.

[0021] Specific examples of compositions containing a polymer suitable for the intermediate layer 6 include "Spring Coat Brush Mixture" manufactured by Kikusui Chemical Industry Co., Ltd. and "Aronbull Coat A450 Base" manufactured by Toagosei Co., Ltd. Specific examples of compositions containing cement suitable for the intermediate layer 6 include "Spring Coat Brush Powder" manufactured by Kikusui Chemical Industry Co., Ltd. and "Aronbull Coat A450 Setter" manufactured by Toagosei Co., Ltd.

[0022] When the intermediate layer 6 contains resin and mortar, the ratio of the resin to the total of the resin and mortar is preferably 10% by mass or more and 90% by mass or less. When this ratio is 10% by mass or more, the intermediate layer 6 has excellent adhesion to other layers (functional layer 4). From this viewpoint, this ratio is more preferably 30% by mass or more, and particularly preferably 40% by mass or more. When this ratio is 90% by mass or less, the intermediate layer 6 has excellent rigidity. From this viewpoint, this ratio is more preferably 70% by mass or less, and particularly preferably 60% by mass or less.

[0023] In Fig. 3, the arrow T2 indicates the thickness of the intermediate layer 6. From the viewpoint of the rigidity of the sheet 2, the thickness T2 is preferably 100 µm or more, more preferably 200 µm or more, and particularly preferably 300 µm or more. From the viewpoint of the productivity and light weight of the sheet 2, the thickness T2 is preferably 1500 µm or less, more preferably 1000 µm or less, and particularly preferably 700 µm or less. The sheet 2 for a structure may have two or more intermediate layers 6. The sheet 2 for a structure may have a layer structure that does not include an intermediate layer 6.

[0024] The sheet for structure 2 may include one or more intermediate layers 6. The number of intermediate layers 6 included in the sheet for structure 2 is set in consideration of, for example, the overall thickness of the sheet for structure 2, the function to be imparted to the intermediate layer 6, the length of the production line of the factory, or the production cost of the sheet for structure 2. For example, when a single intermediate layer 6 having a predetermined thickness cannot be obtained due to the short length of the production line of the factory, a laminated structure of multiple intermediate layers 6 having a predetermined overall thickness may be formed by applying the material of the intermediate layer 6 in layers.

[0025] [Adhesive layer] The adhesive layer 8 abuts against the base. The sheet 2 is attached to the structure by the adhesive force of the adhesive layer 8. The adhesiveness of the adhesive layer 8 can be controlled, for example, by adjusting the thickness and surface properties of the adhesive layer 8, and the material of the adhesive layer 8. When controlling the surface properties of the adhesive layer 8, for example, a microstructure described later can be adopted. Furthermore, setting the thickness of the adhesive layer 8 to an appropriate value that is neither too thick nor too thin is also effective in controlling the adhesiveness of the adhesive layer 8. Moreover, from the viewpoint of easily controlling the adhesive force of the adhesive layer 8 within a predetermined range, it is also preferable to adjust the adhesive material and the thickness of the adhesive layer 8 in combination.

[0026] More specifically, examples of the material of the adhesive layer 8 include adhesives that have a low glass transition temperature (Tg) and can utilize van der Waals forces or electrostatic forces, such as acrylic, silicone having a siloxane bond, rubber, urethane-based, and polyester-based adhesives. The adhesive strength of the adhesive layer 8 can be controlled by adjusting the thickness of the adhesive layer 8 or the degree of crosslinking of the adhesive layer 8. The attachment surface of the adhesive layer 8 may be configured to have a microstructure (a structure that has a large surface area and can utilize intermolecular forces) like the limbs of a gecko. Furthermore, the adhesive and the microstructure may be used in combination.

[0027] The material of the adhesive layer 8 in this embodiment is, for example, a pressure-sensitive adhesive composition based on a polymer. Examples of polymers suitable for the pressure-sensitive adhesive composition include acrylic resin, silicone, polyurethane, polyester, natural rubber, and synthetic rubber. Acrylic resin is a particularly preferred polymer for the base material because of its excellent weather resistance and heat resistance and a wide variety of raw materials. Acrylic resin has the advantage that the molecular weight can be adjusted by polymerization, and by making it into a copolymer, a cohesive component and / or a functional group component can be incorporated into the skeleton of the base polymer.

[0028] Specific examples of acrylic adhesive compositions include trade names "Olivine BPS6574", "Olivine BPS6554" and "Olivine BPS5565K" manufactured by Toyochem Co., Ltd. Specific examples of urethane adhesive compositions include trade names "Polysic UPK-2" and "Polysic UPS-2A" manufactured by Sanyo Chemical Industries, Ltd. Specific examples of polyester adhesive compositions include trade names "LP-050S50TO", "SNT", "NP-120S45EO", "NP-110S50EO", "S-0091S55EO", "S-0097S55EO" manufactured by Mitsubishi Chemical Corporation. Specific examples of rubber adhesive compositions include trade names "GR-1139", "GR-1045M-1", "GR-1025M-1", "GRN-13B" manufactured by Big Technos Co., Ltd. Specific examples of silicone-based pressure-sensitive adhesive compositions include those available under the trade names "X-40-3237", "X-40-3240", and "X-40-3291-1" manufactured by Shin-Etsu Chemical Co., Ltd. For the reasons described above, an acrylic pressure-sensitive adhesive composition is preferably used for the structural sheet of the present disclosure.

[0029] The adhesive composition may contain a curing agent. The type of the curing agent is not particularly limited, and an appropriate curing agent can be selected and used depending on the type of polymer. Examples of the curing agent include isocyanate curing agents, epoxy curing agents, and metal chelate curing agents. If necessary, irradiation crosslinking with ultraviolet light (UV) or electron beam (EB) may be used in combination. The amount of the curing agent is not particularly limited, and can be adjusted depending on the type of polymer and curing agent. For example, the amount of the curing agent relative to 100 parts by mass of the base polymer of the adhesive composition may be 0.5 parts by mass or more, 1.0 parts by mass or more, 2.0 parts by mass or more, 3.0 parts by mass or more, 20 parts by mass or less, 15 parts by mass or less, or 10 parts by mass or less.

[0030] When the substrate is an acrylic resin, a preferred curing agent is an isocyanate curing agent. This is because isocyanates are highly reactive and easily undergo a curing reaction with compounds having active hydrogen, such as amines, alcohols, carboxylic acids, mercaptans, urethanes, and carboxylic acid amides. The ratio of the isocyanate curing agent to 100 parts by mass of the acrylic resin is preferably 1.0 parts by mass or more, more preferably 2.0 parts by mass or more, and particularly preferably 2.5 parts by mass or more. This ratio is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and particularly preferably 7 parts by mass or less. By containing an appropriate amount of the curing agent, an appropriate storage modulus (described in detail later) of the adhesive layer 8 can be achieved.

[0031] The adhesive composition may contain a tackifier. Generally, the resin or elastomer used as the base material of the adhesive composition has adhesive strength because of its high molecular weight, but it may have poor wettability to the object to be adhered and may have low cohesive strength because of its softness. The tackifier has a function of improving the wettability to the object to be adhered. Therefore, the adhesive composition containing the tackifier quickly wets and spreads on the object, and its adhesive strength is fully exerted.

[0032] Examples of the tackifier include rosin resin-based tackifiers, rosin derivative resin-based tackifiers, terpene resin-based tackifiers, petroleum resin-based tackifiers such as C5 resin, C5 / C9 resin, and C9 resin, phenol resin-based tackifiers, terpene phenol resin-based tackifiers, and chroman-styrene resin-based tackifiers. The ratio of the tackifier to 100 parts by mass of the base polymer is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and particularly preferably 1.5 parts by mass or more. This ratio is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and particularly preferably 7 parts by mass or less. The type and amount of the tackifier are selected so that the storage modulus value described below is achieved. By containing an appropriate amount of a tackifier having an appropriate softening point, an excellent storage modulus of the adhesive layer 8 can be achieved.

[0033] Specific examples of rosin resin-based tackifiers include trade names "Ester Gum H," "Ester Gum AA-V," and "Ester Gum 105" manufactured by Arakawa Chemical Industries, Ltd. The hot softening points of these are as follows: Ester gum H: 68℃ to 75℃ Ester gum AA-V: 82℃ to 95℃ Ester gum 105: 100℃ to 110℃

[0034] In FIG. 3, the arrow T3 indicates the thickness of the adhesive layer 8. From the viewpoint of adhesiveness, the thickness T3 is preferably 30 μm or more, and more preferably 50 μm or more. From the viewpoint of suppressing shear deformation of the sheet 2 and from the viewpoint of productivity and light weight of the sheet 2, the thickness T3 is preferably 300 μm or less, more preferably 200 μm or less, and particularly preferably 150 μm or less. From the viewpoint of easily obtaining an adhesive layer that is not easily susceptible to shear deformation and has excellent adhesive strength, the preferred thickness of the adhesive layer is 50 μm or more and 200 μm or less, and more preferably 100 μm or more and 150 μm or less. The structure sheet 2 may have two or more adhesive layers 8.

[0035] [Release film] The release film 9 is disposed (attached) on the surface of the adhesive layer 8 opposite to the intermediate layer 6. The release film 9 is preferably attached to the sheet for structure 2 for the purpose of protecting the surface of the adhesive layer 8 before use. The release film 9 is peeled off when the sheet for structure 2 is attached. The sheet for structure 2, with the adhesive layer 8 exposed by peeling off the release film 9, is attached to the structure by bringing the adhesive layer 8 into contact with the surface of the structure.

[0036] The structure of the release film 9 is not particularly limited, and may be, for example, a sheet having a support layer and a peeling layer. Examples of materials constituting the support layer include polyesters such as polyethylene terephthalate and polyethylene naphthalate, polyolefins such as polyethylene, polypropylene, and polymethylpentene, polyamides such as nylon 6, vinyl resins such as polyvinyl chloride, acrylic resins such as polymethyl methacrylate, cellulose resins such as cellulose acetate, and synthetic resins such as polycarbonate. The support layer may be formed mainly from paper. Furthermore, the support layer may be a laminate having two or more constituent layers.

[0037] Examples of materials constituting the release layer include silicone resins, melamine resins, fluorinated polymers, etc. The release layer can be formed, for example, by applying a coating liquid containing the material constituting the release layer and an organic solvent onto the support layer by a known coating method such as gravure coating, roll coating, comma coating, or lip coating, and drying and curing the coating film formed by the application. In addition, when forming the release layer, the surface of the support layer on which the release layer is to be formed may be previously subjected to corona treatment or easy-adhesion treatment.

[0038] [Other layers] The sheet for structure 2 may have another layer located on the functional layer 4. A typical other layer is, for example, a clear paint layer. The sheet for structure 2 may have a layer located between the functional layer 4 and the intermediate layer 6. The sheet for structure 2 may have a layer located between the intermediate layer 6 and the adhesive layer 8.

[0039] [Total thickness] The total thickness of the structure sheet 2 is preferably 150 μm or more, more preferably 300 μm or more, and particularly preferably 400 μm or more. The total thickness is preferably 5.0 mm or less, more preferably 3.0 mm or less, and particularly preferably 1.0 mm or less.

[0040] [Flexibility of structural sheets] The structure sheet 2 has the above-mentioned rigidity and also has a suitable flexibility. For example, the structure sheet 2 has flexibility to the extent that it can be wound into a roll. The roll-like winding referred to here refers to winding the structure sheet 2 around a roll core material having a diameter of, for example, several centimeters or more and several tens of centimeters or less (specifically, for example, a diameter of 10 mm or more and 300 mm or less). Even with a thinner roll core material, the structure sheet 2 can be wound up to several meters by hand winding or the like. Therefore, for example, the structure sheet 2 can be managed in a roll. Furthermore, it is also possible to unfold the structure sheet 2 wound in a roll at the construction site, and quickly prepare and construct the structure sheet 2 cut into a predetermined size. Therefore, the structure sheet 2 can be easily and simply applied to a construction target having a relatively large area.

[0041] Sheet 2 has a shear strength of 14.0 N / cm at 80°C. 2 That's all. This makes it possible to appropriately prevent so-called lateral slippage, a phenomenon in which the sheet for structure 2 becomes too flexible in summer, causing the attachment position to shift when an external force acts on the surface. The sheet 2 also has an adhesive strength of 4.0 N / 25 mm or more at -10°C. This makes it possible to maintain the sheet securely attached to the surface of the structure even in winter.

[0042] The shear strength of Sheet 2 at 80°C is 42.0N / cm 2 If the adhesive strength of the sheet 2 at -10°C is 18.0 N / 25 mm or less, particularly 15.0 N / 25 mm or less, the strength of the sheet 2 can be easily maintained within a range that allows easy processing of the sheet 2. If the adhesive strength of the sheet 2 at -10°C is 18.0 N / 25 mm or less, particularly 15.0 N / 25 mm or less, for example, even if it becomes necessary to reattach the sheet 2 for use in a structure, the sheet 2 for use in a structure can be easily peeled off from the surface of the structure and reattached while preventing damage. The shear strength of the sheet 2 at 80°C is, for example, 14.0 N / cm 2 It is preferable that the resistance is 20N / cm or more. 2 More preferably, it is 25N / cm or more. 2The adhesive strength of the sheet 2 at -10°C is, for example, preferably 4.0 N / 25 mm or more, more preferably 6.0 N / 25 mm or more, and even more preferably 9.0 N / 25 mm or more.

[0043] [Manufacturing method] An example of a manufacturing method for this structure sheet 2 will be described below. In this manufacturing method, the polymer composition of the functional layer 4 is mixed with a solvent to obtain a first coating material. This first coating material is applied onto a base film (see base film 39 in FIG. 14) to obtain a first coating film. This first coating film is heated, and the solvent volatilizes from the first coating material. This heating hardens the base polymer in the first coating film, and the functional layer 4 is obtained. The base film is a shape-imparting film (sheet) that imparts a shape to the first coating film.

[0044] Next, the composite material of the intermediate layer 6 is mixed with a solvent to obtain a second coating. This second coating is applied onto the functional layer 4 to obtain a second coating. This second coating is heated to evaporate the solvent from the second coating. This heating hardens the polymer, and the intermediate layer 6 is obtained.

[0045] Next, the adhesive composition of the adhesive layer 8 is mixed with a solvent to obtain a third coating material. This third coating material is applied onto a release paper or film to obtain a third coating film. This third coating film is heated to volatilize the solvent from the third coating material, and the adhesive layer 8 is obtained.

[0046] This adhesive layer 8 is overlaid on the intermediate layer 6. Furthermore, the base film is peeled off from the functional layer 4, and the release film is peeled off from the adhesive layer 8 to obtain the sheet for structure 2. At least one of the release paper or release film and the base film may be peeled off and removed before use.

[0047] Here, specific examples of the base film will be described. The base film is used as a substrate when manufacturing the sheet for structure 2. The base film may include a resin laminated paper, which is a process paper used in the manufacturing process of the sheet for structure 2, or a resin film. The resin laminated paper referred to here may have an olefin resin layer such as polypropylene or polyethylene. Specifically, for example, a PP laminated sheet (manufactured by, for example, Lintec Corporation) can be used as the base film. The thickness of this PP laminated sheet is, for example, 50 μm or more and 200 μm or less.

[0048] [Roof repair] A typical application of this structural sheet 2 is roof repair. A repaired roof 10 is shown in Figures 4 and 5. In these figures, two sheets 2 (a first sheet 2a and a second sheet 2b) are shown together with the roof 10. The specifications of the second sheet 2b are the same as those of the first sheet 2a. Examples of the roof 10 include a slate roof, a tile roof, a steel roof (including a folded plate roof), a copper roof, a galvanized iron roof, and a concrete roof.

[0049] In FIG. 4, the position of the lower edge 12a of the first sheet 2a generally coincides with the position of the lower end 14 of the roof 10. The first sheet 2a is affixed as a whole to the roof 10. The second sheet 2b overlaps the vicinity of the upper edge 16a of the first sheet 2a near its lower edge 12b (see FIG. 5). This overlap forms a seam 18. The portion of the second sheet 2b other than the seam 18 is affixed to the roof 10.

[0050] FIG. 6 is an enlarged cross-sectional view taken along line VI-VI in FIG. 4. FIG. 6 shows the roof 10 and the first sheet 2a, as well as the primer layer 20. FIG. 6 shows the functional layer 4a, intermediate layer 6a, and adhesive layer 8a of the first sheet 2a. The primer layer 20 covers the surface of the roof 10. The first sheet 2a is attached to the roof 10 via the primer layer 20. The first sheet 2a is attached to the base (roof 10 or primer layer 20) by the adhesive force of the adhesive layer 8a. In this specification, the phrase "the sheet is attached to the roof" is used to refer to the case where the sheet 2 is attached to the roof 10 via the primer layer 20 or the like.

[0051] FIG. 7 is an enlarged cross-sectional view taken along line VII-VII in FIG. 5. FIG. 7 shows a cross section of the seam 18. FIG. 7 shows the roof 10, the primer layer 20, the first sheet 2a, and the second sheet 2b. FIG. 7 shows the functional layer 4b, the intermediate layer 6b, and the adhesive layer 8b of the second sheet 2b. As mentioned in FIG. 6, the first sheet 2a is attached to the substrate. The second sheet 2b is attached to the first sheet 2a at the seam 18. The second sheet 2b is attached to the functional layer 4a of the first sheet 2a by the adhesive force of the adhesive layer 8b of the second sheet 2b. The part of the second sheet 2b other than the seam 18 is attached to the roof 10 or the primer layer 20, similar to the first sheet 2a shown in FIG. 6.

[0052] [Repair method] FIG. 8 shows a method for repairing a roof 10 using this sheet 2. In this repair method, first, a primer is applied to the surface of the roof 10 (STEP 1). This primer is dried to form a primer layer 20. Next, a plurality of sheets 2 are prepared (STEP 2). These sheets 2 have the same specifications. These sheets 2 include a first sheet 2a (see FIGS. 4 and 5) and a second sheet 2b.

[0053] This first sheet 2a is attached to the roof 10 (STEP 3). As described above, the position of the lower edge 12a of the first sheet 2a roughly coincides with the position of the lower end 14 of the roof 10. A second sheet 2b is patched onto this first sheet 2a (STEP 4). By patching, a seam 18 is formed between the first sheet 2a and the second sheet 2b. A third sheet 2 is patched onto this second sheet 2b, and a fourth sheet 2 is patched onto this third sheet 2. This patching process is repeated in the same manner. When the desired zones on the surface of the roof 10 are covered with sheets 2, the repair is completed.

[0054] [Storage modulus] The storage modulus G'(1) of the adhesive layer 8 at 80°C is 1.0 x 10 2 After the sheet 2 is attached to the roof 10, a worker may step on the sheet 2. At this time, a shear force is applied to the sheet 2. When an object is placed on the sheet 2, a shear force may also be applied to the sheet 2. The storage elastic modulus G'(1) of the adhesive layer 8 is preferably 1.0×10 Pa or more. 2 In the sheet 2 having a modulus of elasticity of 3.1×10 Pa or more, shear deformation when a shear force is applied can be suppressed. This sheet 2 is not easily displaced. With this sheet 2, shear deformation can be suppressed even in a high temperature environment such as in the summer. From the viewpoint of suppressing shear deformation, the storage modulus G'(1) is 3.1×10 3 Pa or more is preferable, and 2.3×10 4 Pa or more is particularly preferred.

[0055] The storage modulus G'(2) of the adhesive layer 8 at -10°C is 1.0 x 10 7 As described above, the adhesive layer 8 is in contact with the base and the functional layer 4 of the other sheet 2. The storage modulus G'(2) of the adhesive layer 8 is preferably 1.0×10 Pa or less. 7The sheet 2, which has a compressive strength of 0.1 x 10 Pa or less, is unlikely to peel off from the base and the functional layer 4 of another sheet 2. This adhesive layer 8 can sufficiently suppress peeling even at the point where the adhesive layer 8 abuts another sheet 2 without the primer layer 20 in between (i.e., the seam 18). In a structure repaired with this sheet 2, the intrusion of water or the like due to peeling is unlikely to occur. With this sheet 2, peeling can be suppressed even in a low-temperature environment such as winter. From the viewpoint of suppressing peeling, the storage modulus G'(2) is 2.3 x 10 6 Pa or less is more preferable, 8.7×10 5 Pa or less is particularly preferred.

[0056] The storage modulus G'(1) and G'(2) can be measured by a viscoelasticity measuring device. An example of a device suitable for the measurement is a DMAQ850 Rheometer DHR-2 manufactured by TA Instruments Japan Co., Ltd. In this measurement, a slab having a thickness of 2.0 mm is prepared from the same composition as the adhesive layer 8. This slab is punched out to obtain a disk-shaped sample having a diameter of 5.0 mm. The measurement conditions are as follows: Frequency: 1.0Hz Temperature range: -80℃ to 80℃ Heating rate: 5℃ / min Mode: Shear

[0057] As mentioned above, (1) Selection of hardener type (2) Adjustment of hardener content (3) Selection of tackifier type or (4) Adjustment of the amount of tackifier This allows the preferred values ​​of storage modulus G'(1) and G'(2) to be achieved. moreover, (5) Selection of molecular weight of base polymer (6) Selection of filler type (7) Adjusting the amount of filler (8) Selection of the type of reinforcement (9) Adjustment of the amount of reinforcement The preferred values ​​of the storage moduli G'(1) and G'(2) can also be achieved by such means.

[0058] [effect] As described above, this sheet 2 is less susceptible to water seeping in through the seams 18. By patching this sheet 2, a wide area of ​​the surface of the roof 10 can be covered with the sheet 2. Because the sheet 2 is flexible, it can conform to steps. Therefore, even if the roof 10 has steps on its surface, the surface of the roof 10 can be covered with the sheet 2 over a wide area. Because the adhesive layer 8 has excellent adhesiveness, even if the surface of the roof 10 is made of a mixture of materials, the surface of the roof 10 can be covered with the sheet 2 over a wide area. For example, even if the surface of the roof 10 includes both metal and slate, the surface of the roof 10 can be covered with the sheet 2 over a wide area.

[0059] The entire surface of the roof 10 may be covered with the sheet 2. In this specification, the surface of the roof 10 means the surface that can be seen when the roof 10 is viewed from above in the vertical direction. A repair method in which the entire surface of the roof 10 is covered with a single type of sheet 2 is not found in conventional construction methods.

[0060] This sheet 2 is lighter than steel plates, copper plates, galvanized iron sheets, etc. Therefore, even if a wide area of ​​the surface of the roof 10 is covered with the sheet 2, the adverse effect on the earthquake resistance of the building is small. When deterioration occurs in the sheet 2 over time, another sheet 2 may be laminated on this sheet 2. Even in this case, the adverse effect on the earthquake resistance of the building is small. From the viewpoint of earthquake resistance, the density of the sheet 2 is 4.0 g / cm 3 Less than 3.0 g / cm is preferred. 3 Less than 2.5 g / cm is more preferable. 3 The following is particularly preferable. This density is much smaller than the density of aluminum-zinc alloy plated steel sheet (trade name "Galvalume Steel Sheet (registered trademark)") which is commonly used for repairing the roof 10.

[0061] [Other uses] This sheet 2 can contribute to the repair or reinforcement of structures other than the roof 10. Examples of structures other than the roof 10 include residential walls, pillars, eaves, fences, gates, doors, parapets, rows of trees, etc. This sheet 2 may also be used in commercial buildings, factories, warehouses, bridges, sewage facilities, railway facilities, tunnels, etc.

[0062] <Second embodiment> [Layer structure] FIG. 9 shows a sheet for a structure 22 according to the second embodiment. This sheet 22 has a functional layer 24, an intermediate layer 26, and an adhesive layer 28. The material, thickness, and other configurations of the functional layer 24 are the same as those of the functional layer 4 of the sheet 2 shown in FIG. 1-7. The material, thickness, and other configurations of the adhesive layer 28 are the same as those of the adhesive layer 8 of the sheet 2 shown in FIG. 1-7. This sheet 22 is attached to a structure. The sheet 22 may have a release paper or a release film. The release paper and the release film are laminated with the adhesive layer 28.

[0063] [Middle layer] The intermediate layer 26 is disposed between the functional layer 24 and the adhesive layer 28. The intermediate layer 26 includes a reinforcing material 30. The material of the intermediate layer 26 except for the reinforcing material 30 is the same as the material of the intermediate layer 6 of the sheet 2 shown in Fig. 1-7. As an example, the reinforcing material 30 in this embodiment is a mesh.

[0064] Examples of the material of the reinforcing material 30 include synthetic resins and metals. Examples of preferred synthetic resins include vinylon, polyethylene terephthalate, polypropylene, polystyrene, and polyvinylidene fluoride. Examples of preferred metals include aluminum alloys, carbon steel, and alloy steels. The reinforcing material 30 can contribute to the rigidity of the sheet 22. The sheet 22 including the reinforcing material 30 has excellent handling properties. The reinforcing material 30 may include a resin film or a metal foil instead of a mesh. The resin film may be, for example, a biaxially stretched film. The reinforcing material 30 is pressed against the coating film for the intermediate layer 26 before the coating film dries, thereby obtaining the intermediate layer 26 including the reinforcing material 30.

[0065] When the reinforcing material 30 is a mesh, the reinforcing material 30 has, for example, a biaxial woven structure in which warp and weft fibers are arranged in a lattice pattern. The shape of the reinforcing material 30 is not particularly limited. When the reinforcing material 30 is a mesh, the shape of the reinforcing material 30 can be any shape, such as a biaxial woven structure or a triaxial woven structure. As the reinforcing material 30, for example, a mesh material such as a high-strength vinylon mesh (for example, for civil engineering applications) or vinylon (for example, for agricultural applications), cheesecloth formed from polyester, polyvinyl alcohol, or the like, is preferable. With these reinforcing materials 30, the elastic range of the structure sheet 22 can be easily expanded. In addition, it is easy to impart appropriate rigidity to the structure sheet 22. Furthermore, the handleability of the structure sheet 22 can be improved.

[0066] For example, the line pitch of the reinforcing material 30 is preferably 50 mm or more and 1.2 mm or less. In other words, for example, the line density of the reinforcing material 30 is preferably 0.2 lines / cm or more and 8.0 lines / cm or less. Such a reinforcing material 30 can easily impart rigidity to the structure sheet 22 while ensuring the tensile strength of the structure sheet 22.

[0067] For example, when the intermediate layer 26 is viewed in a plan view, the reinforcing material 30 may have a size sufficient to cover the entire surface of the intermediate layer 26, or may have a size smaller than that of the intermediate layer 26. In other words, the area of ​​the reinforcing material 30 when viewed in a plan view may be equal to or smaller than the area of ​​the intermediate layer 26 when viewed in a plan view.

[0068] The area of ​​the reinforcing material 30 in plan view (area in plan view) is preferably, for example, 60% or more and 95% or less of the area in plan view of the intermediate layer 26. If the area in plan view of the reinforcing material 30 is 60% or more, for example, it is easy to ensure the rigidity of the sheet for structure 22 and easy to control the elongation rate of the sheet for structure 22. In addition, it is easy to suppress the variation in rigidity in different regions of the sheet for structure 22. If the area in plan view of the reinforcing material 30 is 95% or less, for example, when the intermediate layer 26 is formed so as to sandwich the reinforcing material 30 in the thickness direction of the sheet for structure 22, it is easy to ensure the adhesive strength of the reinforcing material 30 to the intermediate layer 26 in the entire intermediate layer 26. The area in plan view of the reinforcing material 30 can be measured by a known method.

[0069] The thickness of the reinforcing material 30 is, for example, 10% or more of the thickness of the intermediate layer 26. The thickness of the reinforcing material 30 is, for example, preferably 20% or more of the thickness of the intermediate layer 26, more preferably 30% or more, particularly preferably 40% or more, and most preferably 50% or more. On the other hand, the thickness of the reinforcing material 30 is, for example, 80% or less of the thickness of the intermediate layer 26. The thickness of the reinforcing material 30 is, for example, preferably 70% or less of the thickness of the intermediate layer 26, more preferably 60% or less, and particularly preferably 55% or less. By setting the thickness of the intermediate layer 26 in this way, it is possible to easily impart appropriate rigidity to the structure sheet 22.

[0070] Furthermore, by setting the thickness of the reinforcing material 30 and the thickness of the intermediate layer 26 to have the above-mentioned relationship, the structure sheet 22 of the present disclosure can be configured to have excellent adhesion between the adhesive layer 28 and the intermediate layer 26 and appropriate rigidity. Therefore, excellent handleability is obtained when attaching the structure sheet 22 to the roof of the structure, and the structure can be protected by the structure sheet 22 for a long period of time without causing wrinkles or gaps with the roof of the structure. For example, the lower limit of the thickness of the reinforcing material 30 relative to the thickness of the intermediate layer 26 is preferably 45%, and the upper limit of the thickness is preferably 55%.

[0071] In Fig. 9, an arrow T2 indicates the thickness of the intermediate layer 26. From the viewpoint of the rigidity of the sheet 22, the thickness T2 is preferably 100 µm or more, more preferably 200 µm or more, and particularly preferably 300 µm or more. From the viewpoint of the productivity and light weight of the sheet 22, the thickness T2 is preferably 1500 µm or less, more preferably 1000 µm or less, and particularly preferably 700 µm or less. The sheet 22 for a structure may have two or more intermediate layers 26. The sheet 22 for a structure may have a layer structure that does not include an intermediate layer 26.

[0072] [Application] This sheet 22 is suitable for roof repair, similar to the sheet 2 shown in Fig. 1-7. This sheet 22 can also be used for residential walls, pillars, eaves, fences, gates, doors, parapets, row of trees, etc. This sheet 22 may also be used for commercial buildings, factories, warehouses, bridges, sewage facilities, railway facilities, tunnels, etc.

[0073] [Storage modulus] As described above, the material of the adhesive layer 28 is the same as the material of the adhesive layer 8 of the sheet 2 shown in FIG. 1-7. Therefore, the storage moduli G'(1) and G'(2) of the adhesive layer 28 are the same as those of the adhesive layer 8. Shear deformation can be suppressed in the sheet 22. Furthermore, the sheet 22 is not easily peeled off from the base and the functional layer 24 of the other sheet 22.

[0074] [density] The density of the sheet 22 is 4.0 g / cm 3 Less than 3.0 g / cm is preferred. 3 Less than 2.5 g / cm is more preferable. 3 The following are particularly preferred:

[0075] <Third embodiment> [Layer structure] FIG. 10 shows a sheet for a structure 32 according to a third embodiment. This sheet 32 ​​has a functional layer 34 and an adhesive layer 36. The material of the functional layer 34 is the same as the material of the functional layer 4 of the sheet 2 shown in FIG. 1-7. The material, thickness, and other configurations of the adhesive layer 36 are the same as those of the adhesive layer 8 of the sheet 2 shown in FIG. 1-7. This sheet 32 ​​is attached to a structure. The sheet 32 ​​may have a release paper or a release film. The release paper and the release film are laminated with the adhesive layer 36.

[0076] [Application] This sheet 32 ​​is suitable for roof repair, similar to the sheet 2 shown in Fig. 1-7. This sheet 32 ​​can also be used for residential walls, pillars, eaves, fences, gates, doors, parapets, row of trees, etc., similar to the sheet 2 shown in Fig. 1-7. This sheet 32 ​​may also be used for commercial buildings, factories, warehouses, bridges, sewage facilities, railway facilities, tunnels, etc.

[0077] [Storage modulus] As described above, the material of the adhesive layer 36 is the same as the material of the adhesive layer 8 of the sheet 2 shown in FIG. 1-7. Therefore, the storage moduli G'(1) and G'(2) of the adhesive layer 36 are the same as those of the adhesive layer 8. Shear deformation can be suppressed in the sheet 32. Furthermore, the sheet 32 ​​is not easily peeled off from the base and the functional layer 34 of the other sheet 32.

[0078] [density] The density of the sheet 32 ​​is 4.0 g / cm 3 Less than 3.0 g / cm is preferred. 3 Less than 2.5 g / cm is more preferable. 3 The following are particularly preferred:

[0079] <Other supplementary information> [About the rigidity of structural sheets] From the viewpoint of ensuring ease of handling when applied to a structure, the sheet for structure 2 preferably has a rigidity that can withstand folding. For this reason, for example, the sheet for structure 2 may be configured so that at least one of the first layer arranged on the application surface side and the second layer arranged on the opposite side to the application surface has a predetermined rigidity. Alternatively, the sheet for structure 2 may be configured so that it includes the first layer arranged on the application surface side, the second layer arranged on the opposite side to the application surface, and a third layer arranged between the first layer and the second layer, and the third layer has a predetermined rigidity. This will be specifically described below.

[0080] The first layer arranged on the attachment surface side of the sheet for structure 2 can be exemplified by the adhesive layer 8. As a method for imparting rigidity to the adhesive layer 8, a method in which the adhesive layer 8 is configured to include an adhesive and a filler can be exemplified. In this case, the adhesive layer 8 includes an adhesive having a relatively low glass transition temperature (Tg) such as acrylic, silicone having a siloxane bond, rubber, or urethane, and capable of utilizing van der Waals force or electrostatic force, and a filler such as silica, alumina, titanium oxide, calcium carbonate, or carbon black. For example, the rigidity of the adhesive layer 8 can be controlled by adjusting at least one of the amount of filler added to the adhesive layer 8 and the particle shape of the filler. Specifically, examples of the particle shape of the filler include spherical, acicular, amorphous, and tetrapod shapes. In addition, the rigidity of the sheet for structure 2 can be controlled by adjusting the thickness of the functional layer 4. In addition, the rigidity of the sheet for structure 2 can be controlled by adjusting the Tg of the adhesive in the functional layer 4.

[0081] The layer disposed on the surface side of the sheet for structure 2, i.e., the second layer disposed on the opposite side of the sheet for structure 2 to be attached, can be exemplified by the functional layer 4. As a method for imparting rigidity to the functional layer 4, a method of forming the functional layer 4 so as to include a main material and a filler can be exemplified. In this case, the functional layer 4 includes a main material such as acrylic silicone, fluororesin, silicone resin, non-diene rubber, and a filler such as silica, alumina, titanium oxide, calcium carbonate, and carbon black. For example, the rigidity of the functional layer 4 can be controlled by adjusting at least one of the amount of filler added to the functional layer 4 and the particle shape of the filler. Specifically, examples of the particle shape of the filler include spherical, needle-like, amorphous, and tetrapod-like shapes. In addition, the rigidity of the sheet for structure 2 can be controlled by adjusting at least one of the thickness of the functional layer 4 and the Tg of the main material of the functional layer 4. In this manner, in the sheet for structure 2, at least one of the adhesive layer 8 and the functional layer 4 may include a filler.

[0082] In a structural sheet 2 comprising a first layer (e.g., adhesive layer 8) arranged on the attachment surface side, a second layer (e.g., functional layer 4) arranged on the opposite side to the attachment surface, and a third layer arranged between the first and second layers, the third layer being configured to have a predetermined rigidity, one method of imparting rigidity to the third layer is, for example, to configure the third layer as an intermediate layer 6 described below and impart rigidity to the intermediate layer 6.

[0083] Furthermore, the rigidity of the sheet 2 for a structure can be controlled by adjusting the Tg of the resin component contained in the intermediate layer 6. The rigidity of the sheet 2 for a structure can also be controlled by adjusting the amount and diameter of voids in the intermediate layer 6. When the sheet 2 for a structure has a plurality of intermediate layers 6, for example, it may have a first intermediate layer 6 containing a resin component whose Tg is a predetermined value, and a second intermediate layer 6 containing a resin component whose Tg is lower than that of the resin component contained in the first intermediate layer 6.

[0084] From the viewpoint of ensuring the rigidity of the sheet for structure 2, the thickness of the intermediate layer 6 is, for example, 100 μm or more. The thickness of the intermediate layer 6 is, for example, preferably 200 μm or more, more preferably 300 μm or more, and most preferably 350 μm or more. On the other hand, taking into consideration the productivity and the like, the thickness of the intermediate layer 6 is, for example, 1500 μm or less. The thickness of the intermediate layer 6 is preferably 1200 μm or less, more preferably 1000 μm or less, and most preferably 750 μm or less. In this way, by appropriately adjusting the thickness of the intermediate layer 6, appropriate rigidity of the sheet for structure 2 can be obtained.

[0085] When a resin component, a mortar component, and a reinforcing material 30 are used as materials for the intermediate layer 6, as a specific example, a Spring Coat (Brush) admixture liquid manufactured by Kikusui Chemical Industry Co., Ltd. can be used as the resin component. Also, a Spring Coat (Brush) powder manufactured by Kikusui Chemical Industry Co., Ltd. can be used as the mortar component. Also, a vinylon-based mesh material (cheesecloth (BINEO (registered trademark) "V520")) manufactured by Unitika Co., Ltd. can be used as the reinforcing material 30 (mesh component).

[0086] [Reinforcement material details] In order to control the internal structure of the sheet for structure 2, as described above, it is preferable to place the reinforcing material 30 inside the intermediate layer 6. In this case, the internal structure of the sheet for structure 2 can be controlled by changing the content of the reinforcing material 30 in the intermediate layer 6. Furthermore, when the sheet for structure 2 has a plurality of layers, the sheet for structure 2 may have a reinforcing material 30 with a layer structure placed inside. In this case, the reinforcing material 30 with a layer structure imparts a predetermined rigidity to the sheet for structure 2, thereby making it possible to control the internal structure of the sheet for structure 2.

[0087] When the sheet for structure 2 contains a filler for adjusting strength, specific methods for imparting rigidity to the sheet for structure 2 include, for example, a method of controlling at least one of the material of the filler, the amount of the filler added to the sheet for structure 2, and the size and shape of the filler particles. In this case, the material of the filler may be either an inorganic material or an organic material, or an inorganic material and an organic material may be mixed.

[0088] In addition, nonwoven fabric can also be used as the reinforcing material 30. In this case, the nonwoven fabric is not particularly limited as long as it is a nonwoven fabric formed into a sheet shape without weaving fibers. In addition, examples of fibers constituting the nonwoven fabric include at least one of natural fibers and chemical fibers. Examples of chemical fibers include fibers made of polyolefin resins such as polypropylene and polyethylene, polyester resins, polyacrylic resins, and polyamide resins such as nylon, as well as copolymers and modified products of these resins, and synthetic fibers made of combinations of these. Among these, polyester fibers are preferable as fibers excellent in water resistance, heat resistance, dimensional stability, weather resistance, etc.

[0089] As a specific method for imparting rigidity to the sheet for structure 2, the thickness of the sheet for structure 2 may be controlled. In the case of the sheet for structure 2 having an intermediate layer 6, the rigidity of the sheet for structure 2 can also be controlled by adjusting the viscoelasticity of the intermediate layer 6. In this case, the viscoelasticity of the intermediate layer 6 may be adjusted by adjusting the glass transition temperature (Tg, hereinafter also simply referred to as Tg) of the resin contained in the intermediate layer 6 or by changing the degree of crosslinking of the resin. In this way, various methods can be used as a method for controlling the rigidity of the sheet for structure 2.

[0090] <Other embodiments> Further configurations of the sheet for structure 2 are illustrated below. Fig. 12 is a cross-sectional configuration diagram that shows a schematic diagram of the sheet for structure according to the fourth embodiment. When the release film 9 described above is the first release film 9, the sheet for structure 2 of this embodiment includes a second release film 17 arranged on the opposite side of the adhesive layer 48 of the functional layer 44. As an example, the sheet for structure 2 has the first release film 9, the adhesive layer 48, the intermediate layer 46, the functional layer 44, and the second release film 17 arranged in this order in the thickness direction.

[0091] The second release film 17 is configured so that the surfaces 17a, 9a are unlikely to adhere to each other when the surface 17a exposed to the outside comes into contact with the surface 9a exposed to the outside of the first release film 9. For this reason, when the structure sheet 2 is unwound from a roll body 51 (see FIG. 15) around which the sheet 2 described below is wound, the first release film 9 can be easily separated from the second release film 17, and the structure sheet 2 can be easily unwound.

[0092] In addition, the second release film 17 has a predetermined rigidity. Therefore, the rigidity of the remaining structure sheet 2 after the first release film 9 is peeled off can be improved. Therefore, even if the rigidity of the remaining structure sheet 2 after the first release film 9 and the second release film 17 are peeled off is low, the handling when attaching the sheet 2 can be improved and the structure sheet 2 can be easily attached to the surface of the structure. In addition, the remaining structure sheet 2 after the first release film 9 and the second release film 17 are peeled off can be designed to have a relatively small rigidity. Therefore, for example, even if the shape of the surface of the structure to which the structure sheet 2 is attached is not flat due to height differences caused by unevenness or defects, the structure sheet 2 can be attached by being well conformed to the surface. In addition, for example, the anchor effect on the surface can be improved, so that the adhesive force of the structure sheet 2 can be sufficiently improved within an allowable range.

[0093] The structure of the second release film 17 can be appropriately set. For example, as shown in Fig. 12, the second release film 17 has a contact layer 11 that contacts the first release film 9 when the structure sheet 2 is wound into a roll, and a weak adhesive layer 13 that is disposed on the first release film 9 side of the contact layer 11 when the structure sheet 2 is disposed flat.

[0094] The contact layer 11 may be composed of a single layer or multiple layers. The contact layer 11 may contain a resin. In other words, the contact layer 11 may be a resin layer. Examples of the resin contained in the contact layer 11 include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefins such as polyethylene, polypropylene, and polymethylpentene, polyamides such as nylon 6 and aramid, vinyl resins such as polyvinyl chloride, acrylic resins such as polymethyl methacrylate, cellulose resins such as cellulose acetate, synthetic resins such as polycarbonate, and urethane.

[0095] Alternatively, the contact layer 11 may be a fiber layer containing a fiber component and a binder component that binds the fiber component. Alternatively, the contact layer 11 may contain paper. In this case, the contact layer 11 may contain paper as a main component, or may contain paper together with a predetermined main component. When the contact layer 11 contains paper, the contact layer 11 preferably contains paper having a strength such that the contact layer 11 is not accidentally torn when the structural sheet 2 is attached to the target. When the contact layer 11 contains paper, the contact layer 11 preferably contains silicone having a siloxane bond together with the paper. The contact layer 11 has a higher rigidity than the remaining portion of the structural sheet 2 from which the release film 9 and the second release film 17 are omitted and the contact layer 11 and the weak adhesive layer 13 are omitted.

[0096] The thickness of the contact layer 11 can be appropriately set, for example, to a value of 20 μm or more and 500 μm or less. When the contact layer 11 contains polyethylene terephthalate (PET), the thickness of the contact layer 11 is preferably, for example, a value of 20 μm or more and 50 μm or less.

[0097] The weakly adhesive layer 13 has a relatively low adhesive strength. For example, the adhesive strength of the weakly adhesive layer 13 to the functional layer 44 is lower than the adhesive strength of the adhesive layer 48 to the intermediate layer 46. Also, for example, the adhesive strength of the weakly adhesive layer 13 to the contact layer 11 is higher than the adhesive strength of the weakly adhesive layer 13 to the functional layer 44. The weakly adhesive layer 13 may be attached to the functional layer 44 by, for example, static electricity. The weakly adhesive layer 13 may contain a main component whose Tg is substantially 0. The weakly adhesive layer 13 may contain, for example, ethylene vinyl acetate (EVA), urethane, silicone having a siloxane bond, acrylic, or the like. The second release film 17 is not limited to the above-mentioned configuration, and may be, for example, a base film 39 described later.

[0098] 13 is a cross-sectional view showing a schematic configuration of a structure sheet 2 according to a fifth embodiment. The structure sheet 2 of this embodiment includes a release sheet 29 arranged on the side of the functional layer 44 opposite to the adhesive layer 48 side. As an example, the structure sheet 2 has the adhesive layer 48, intermediate layer 46, functional layer 44, and release sheet 29 arranged in this order in the thickness direction. In the structure sheet 2 of this embodiment, the release film 9 is omitted.

[0099] The release sheet 29 contains a surface 29a exposed to the outside and a release agent disposed in the vicinity thereof. An example of the release agent is silicone having a siloxane bond. This makes it difficult for the surface 29a and the attachment surface 48a to adhere to each other when the surface 29a exposed to the outside of the release sheet 29 comes into contact with the attachment surface 48a of the adhesive layer 48 in the roll body 51. Therefore, when the structure sheet 2 is unwound from the roll body 51, the adhesive layer 48 can be easily peeled off from the release sheet 29, and the structure sheet 2 can be easily unwound.

[0100] In this manner, in the present disclosure, when the structure sheet 2 is unwound from the roll body 51, for example, the structure sheet 2 may be made easy to unwound from the roll body 51 in advance so that the portion of the structure sheet 2 provided with the adhesive component does not adhere to other portions of the structure sheet 2 and become difficult to remove. The release sheet 29 has a predetermined rigidity. Therefore, in this embodiment, even if the release film 9 is omitted, the rigidity of the structure sheet 2 can be improved. Therefore, the handleability of the structure sheet 2 is improved, and the structure sheet 2 can be easily attached to the attachment target of the structure. In this case, the release sheet 29 has a higher rigidity than the remaining structure sheet 2 from which the release sheet 29 is peeled off and removed.

[0101] The structure of the release sheet 29 can be set appropriately. For example, as shown in FIG. 13, the release sheet 29 has a release intermediate layer 15 having a surface 29a that contacts the attachment surface 48a of the adhesive layer 48 when the structure sheet 2 is wound into a roll, and a weak adhesive layer 13 that is arranged on the adhesive layer 48 side of the release intermediate layer 15 when the structure sheet 2 is arranged flat. The release intermediate layer 15 may have the same structure as the contact layer 11, except that it contains a release agent. The release sheet 29 may also have a release agent layer arranged on the surface 29a.

[0102] 14 is a cross-sectional view showing a schematic configuration of a structure sheet 2 according to a sixth embodiment. When laid flat, the structure sheet 2 of this embodiment includes a base film 39 arranged on the opposite side of the functional layer 44 from the adhesive layer 48 side. The base film 39 is a base film used when forming the above-mentioned functional layer 4. The structure sheet 2 of this embodiment includes the base film 39, which is not peeled off even after the functional layer 44 is formed.

[0103] As an example, the structure sheet 2 has the release film 9, the adhesive layer 48, the intermediate layer 46, the functional layer 44, and the base film 39 arranged in this order in the thickness direction. The surface 39a exposed to the outside of the base film 39 and the surface 9a exposed to the outside of the release film 9 are configured so as not to adhere to each other when they come into contact with each other. Therefore, when the structure sheet 2 is unwound from the roll body 51, the structure sheet 2 can be easily unwound. The base film 39 has a predetermined rigidity. In this case, the base film 39 has a higher rigidity than the remaining structure sheet 2 from which the release film 9 and the base film 39 have been peeled off. Therefore, in the remaining structure sheet 2 from which the release film 9 has been peeled off, the rigidity of the structure sheet 2 can be improved by the base film 39. Therefore, even if the rigidity of the remaining structural sheet 2 after the first release film 9 and the base film 39 have been peeled off is low, the handleability of the structural sheet 2 can be improved and the structural sheet 2 can be easily attached to the target object of the structure.

[0104] The base film 39 may contain a resin laminated paper having pseudo-adhesion, which is a property that two components attached to each other cannot be adhered again once they are peeled off. In this case, for example, the base film 39 may contain a resin laminated paper in which a resin layer and paper are laminated, and the resin layer and the paper are adhered to each other by pseudo-adhesion in the resin laminated paper. According to this configuration, when the paper in the resin laminated paper is peeled off from the resin layer with the resin layer attached to the functional layer 44, only the paper is peeled off and removed, and the resin layer remains attached to the functional layer 44 of the structure sheet 2.

[0105] Next, in the fourth to sixth embodiments, a construction method for reinforcing or repairing a structure by attaching the structure sheet 2 to the structure will be illustrated. In this construction method, the worker unrolls the required length of the structure sheet 2 from the roll body 51. Next, in the fourth and sixth embodiments, the worker peels off the release film 9 of the structure sheet 2 and attaches the exposed attachment surface 48a of the adhesive layer 48 to the surface of the structure to be attached. At this time, the worker may peel off the release film 9 little by little from the structure sheet 2 and attach the exposed attachment surface 48a of the adhesive layer 48 to the surface of the structure to be attached. On the other hand, in the fifth embodiment, the worker attaches the attachment surface 48a of the adhesive layer 48 of the structure sheet 2 to the surface of the structure to be attached.

[0106] Then, in the cases of the fourth to sixth embodiments, after the worker has attached the structural sheet 2 to the object to which it is to be attached, he or she peels and removes the corresponding second release film 17, release sheet 29, or base film 39 from the structural sheet 2.

[0107] That is, the present construction methods according to the fourth to sixth embodiments include a preparation step of preparing a roll 51 in which the structure sheet 2 is wound in a roll shape, a payout step of paying out the structure sheet 2 from the roll 51, and an attachment step of peeling the first release film 9 from the paid-out structure sheet 2 and attaching the attachment surface exposed to the outside to the surface of the structure. Here, in the preparation step of the fourth and sixth embodiments, the roll 51 is prepared using the structure sheet 2 whose attachment surface 48a is covered with the first release film 9.

[0108] In this construction method, the structure sheet 2 in the roll body 51 prepared in the preparation step has a laminated structure including a functional layer 44 and an adhesive layer 48, and a cover sheet is disposed on the side of the functional layer 44 opposite to the adhesive layer 48 side, and the structure sheet 2 including this cover sheet is wound in a roll shape in the roll body 51, and the cover sheet may be peeled off and removed during or after the attachment step. This cover sheet may be any one of the second release film 17, the release sheet 29, and the base film 39.

[0109] Furthermore, in the construction method of the fourth embodiment, the structure sheet 2 of the roll body 51 prepared in the preparation step has a laminated structure including a functional layer 44 and an adhesive layer 48, and has a release sheet 29 that is arranged on the opposite side of the adhesive layer 48 of the functional layer 44 and is separate from the release film 9, and in the preparation step, a roll body 51 is prepared in which the structure sheet 2 is wound into a roll shape so that the release sheet 29 is in contact with the adhesive layer 48.

[0110] When using the structure sheet 2 of the present disclosure, for example, the following supply item 45 can be used. FIG. 15 is a schematic diagram showing the structure of the supply item 45 containing the structure sheet 2 of the present disclosure. FIG. 15 shows, as an example, the structure sheet 2 having a release film 9. The supply item 45 shown in FIG. 15 includes a roll body 51 around which the belt-shaped structure sheet 2 is wound, and a container 50 having a storage space 50a for storing the roll body 51. The container 50 has a supply port 50b that can unwind and supply the structure sheet 2 from the roll body 51 stored in the storage space 50a to the outside. The supply port 50b has a width dimension equal to or greater than the width dimension of the structure sheet 2 in the axial direction of the roll body 51.

[0111] For example, a worker can carry the supply item 45 to a construction site, unwind the required length of the structure sheet 2 from the supply item 45, and use the structure sheet 2 for construction. Therefore, the supply item 45 allows the structure sheet 2 to be stored in the form of a roll body 51 suitable for storage. Furthermore, when the structure sheet 2 is to be used, only the required amount can be unwound from the supply item 45. This improves work efficiency.

[0112] In addition, when the worker unrolls the structure sheet 2 from the supply port 50b, for example, the worker can unroll the structure sheet 2 while applying uniform tension to the entire widthwise area of ​​the structure sheet 2 by pressing the entire widthwise area of ​​the structure sheet 2 against the opening periphery of the supply port 50b. This allows the structure sheet 2 to be attached to the surface of the structure with uniform tension. Therefore, it is possible to prevent the structure sheet 2 from being subjected to uneven tension after application, which causes unexpected contraction or expansion of the structure sheet 2 after application. Note that in order to apply uniform tension to the entire widthwise area of ​​the structure sheet 2, a separate member such as a long member that extends in the widthwise direction of the structure sheet 2 and comes into contact with the structure sheet 2 may be disposed, for example, around the opening periphery of the supply port 50b.

[0113] Furthermore, the structure sheet provided in the supply item 45 may be any structure sheet according to the present disclosure, and may be, for example, the structure sheet 2 according to any of the fourth to sixth embodiments, or the structure sheet 2 according to other embodiments.

[0114] <Example> The effects of the structural sheet according to the embodiment will be described below. The scope of the present disclosure should not be construed as being limited based on the description of the embodiment. [Example 1] 2.0 parts by mass of a tackifier (the above-mentioned product name "Estergum AAV") was added to 100 parts by mass of an acrylic resin (the above-mentioned product name "Olivine BPS5565K"), and 6.0 parts by mass of an isocyanate curing agent (the product name "BHS8515" manufactured by Toyochem Co., Ltd.) was further added to obtain a pressure-sensitive adhesive composition A. A 2.0 mm thick adhesive layer was formed using this pressure-sensitive adhesive composition A, and the storage modulus was measured. The storage modulus G'(1) at 80°C of the adhesive layer of Example 1 was 8.4 x 10 4 Pa, and the storage modulus G'(2) at -10°C is 5.8×10 5 It was Pa.

[0115] A 130 μm thick base film, a PP laminate sheet manufactured by Lintec Corporation, was prepared. A functional layer-forming composition containing an acrylic resin (a mixture of "Cool Life SP Black (CB1) P5-0" manufactured by Dainichi Seikagaku Kogyo Co., Ltd. and FC Coat Water-Based Silicone Elastic Black manufactured by Fujikura Kasei Co., Ltd. in a weight ratio of 50:50) was applied onto the base film. The formed coating was dried to form a single-layer functional layer having a thickness of 110 μm.

[0116] Next, a mixture of cement and a mixture of a composition for forming an intermediate layer (manufactured by Kikusui Chemical Industry Co., Ltd. under the trade name "Spring Coat (Trowel)") in a ratio of 60:40 was prepared. This mixture was applied onto the functional layer. A vinylon-based mesh material (manufactured by Kuraray Co., Ltd. under the trade name "Cremona", cheesecloth, #600 (No. 600, thickness 230 μm) was placed so as to be pressed onto the surface of the coating of this mixture. This caused the coating to harden, forming an intermediate layer on the functional layer with a thickness of 450 μm after hardening. Thereafter, an adhesive layer was combined with the functional layer and intermediate layer to produce the structural sheet shown in FIG. 1-3 as the structural sheet of Example 1.

[0117] [Examples 2-5 and Comparative Examples 1-3] Except for changing the type and amount of tackifier as shown in Table 1 below, structural sheets of Examples 2-5 and Comparative Examples 1-3 were produced in the same manner as in Example 1. The storage modulus G'(1) at 80°C and the storage modulus G'(2) at -10°C of the adhesive layers of the structural sheets of Examples 2-5 and Comparative Examples 1-3 are shown in Table 1 below.

[0118] [Example 6] 2-Ethylhexyl acrylate (2-EHA) and acrylic acid (AA) were mixed in ethyl acetate so that the molar ratio (2-EHA / AA) was 97 / 3, and then azobisisobutyronitrile (AIBN) was added as a crosslinking agent to carry out solution polymerization to synthesize an acrylic polymer. The result of measuring the obtained acrylic polymer by gel permeation chromatography (GPC) was that the weight average molecular weight Mw was 412,000, the number average molecular weight Mn was 42,000, and the molecular weight distribution Mw / Mn was 9.8. The GPC measurement was performed with tetrahydrofuran as the eluent and at 40°C.

[0119] To 100 parts by mass of the obtained acrylic polymer, 1.0 part by mass of a tackifier (polymerized rosin manufactured by Arakawa Chemical Industries, Ltd., product name "Aradigm R-95") was added, and 1.0 part by mass of a curing agent (product name "Tetrad C" manufactured by Mitsubishi Gas Chemical Trading Co., Ltd.) was further added to obtain an adhesive composition M. An adhesive layer and a sheet for structures for measuring the storage modulus were produced as Example 6 in the same manner as in Example 1, except that this adhesive composition M was used. The storage modulus G'(1) at 80°C of the adhesive layer of the sheet for structures in Example 6 was 1.4×10 2 Pa, and the storage modulus G'(2) at -10°C is 2.6×10 4 It was Pa.

[0120] [Shear test] A plate 38 shown in FIG. 11 was prepared. The material of this plate 38 was steel. This plate 38 had a width of 30 mm and a length of 50 mm. Meanwhile, a test piece 40 having a width of 15 mm and a length of 50 mm was cut out from a structural sheet. This plate 38 and test piece 40 were placed in a thermostatic chamber at a temperature of 80° C. and left to stand for 30 minutes. As shown in FIG. 11, the test piece 40 was overlapped on the plate 38 so that the overlap length was 15 mm. An adhesive layer was in contact with the plate 38. The contact area between the plate 38 and the adhesive layer was 2.25 cm. 2The test specimen 40 was firmly attached to the plate 38 by rolling a roller having a mass of 2 kg back and forth on the test specimen 40 once. The plate 38 and the test specimen 40 were placed in a thermostatic chamber at a temperature of 80° C. and left to stand for 30 minutes. The plate 38 and the test specimen 40 were set in a tensile tester equipped with a temperature controller, and a tensile test was performed. In this test, the test specimen 40 was pulled relatively to the plate 38 in the direction indicated by the arrow A1. The test conditions were as follows: Temperature controller: Shimadzu Corporation product name "THC1 WF-200T-X" Tensile testing machine: Shimadzu Corporation product name "AGX-V" Test temperature: 80℃ Chuck distance: 50mm Tensile speed: 50mm / min When the rate of decrease in the test force reached 1% / s, the measurement was stopped and the maximum test force (N) was calculated. 2 ) to obtain the shear force (N / cm 2 ) was calculated. The results are shown in Table 1 below.

[0121] [Peel test] Using test pieces prepared in accordance with the provisions of "JIS Z0237:2022 10.1", a 180° peel test was performed in accordance with the provisions of "JIS Z0237:2022 11.5" to measure the adhesive strength (N / 25mm). The test conditions are as follows: Testing machine: Shimadzu Corporation product name "Autograph AGX-V" Test temperature: -10℃ Test speed: 300mm / min The results are shown in Table 1 below.

[0122] [Table 1]

[0123] [Examples 7-12]

[0124] Structural sheets of Examples 7-12 were produced in the same manner as in Example 1, except that the thickness of the adhesive layer was changed to the value shown in Table 2 below. The storage modulus G'(1) at 80°C and the storage modulus G'(2) at -10°C of the adhesive layer provided in the structural sheets of Examples 1-12 are shown in Table 2 below. In addition, the above-mentioned [shear test] and [peel test] were performed on each of the structural sheets of Examples 7-12, and the shear force (N / cm 2 ) and adhesive strength (N / 25 mm) were measured. The results are shown in Table 2 below. For comparison, the results of Example 1, in which the adhesive layer had a thickness of 100 μm, are also shown in Table 2.

[0125] [Table 2]

[0126] As is clear from Table 1, the structure sheets of each Example exert a sufficiently large shear force in an environment of 80°C. These sheets also exert a sufficiently large adhesive force in an environment of -10°C. Furthermore, as is clear from Table 2, in the structure sheets of each Example, the shear force and adhesive force can be controlled by changing the thickness of the adhesive layer. From these evaluation results, the superiority of the structure sheets according to the present disclosure is clear.

[0127] [Disclosure items]

[0128] Each of the following sections discloses a preferred embodiment.

[0129] [Item 1] The adhesive layer includes a functional layer and an adhesive layer. The storage modulus of the adhesive layer at 80°C is 1.0 x 10 2 Pa or more, and the storage modulus at -10°C is 1.0 x 10 7 Structural sheet with a tensile strength of less than 100 Pa.

[0130] [Item 2] 2. The structure sheet according to item 1, wherein the material of the adhesive layer is an adhesive composition, and the base material of the composition is an acrylic resin.

[0131] [Item 3] 3. The structure sheet according to item 2, wherein the pressure-sensitive adhesive composition contains an isocyanate curing agent.

[0132] [Item 4] 4. The sheet for structures according to item 2 or 3, wherein the pressure-sensitive adhesive composition contains a tackifier.

[0133] [Item 5] 5. The structure sheet according to any one of items 1 to 4, wherein the adhesive layer has a thickness of 30 μm or more and 300 μm or less.

[0134] [Item 6]

[0135] Shear force at 80℃ is 14.0N / cm 2 6. The sheet for structures according to any one of items 1 to 5, wherein the adhesive strength at -10°C is 4.0 N / 25 mm or more.

[0136] [Item 7]

[0137] 7. The structure sheet according to any one of items 1 to 6, further comprising an intermediate layer disposed between the functional layer and the adhesive layer.

[0138] [Item 8]

[0139] 8. The structural sheet according to item 7, wherein the intermediate layer comprises a reinforcing material.

[0140] [Item 9] Item 9. The structure sheet according to item 7 or 8, wherein at least one of the functional layer and the adhesive layer contains a filler.

[0141] [Item 10]

[0142] 10. The structure sheet according to any one of items 1 to 9, further comprising a release film disposed on the surface of the adhesive layer opposite the functional layer.

[0143] [Item 11] A method for repairing or reinforcing a structure, comprising: (1) Functional layer and storage modulus at 80°C of 1.0 × 10 2 Pa or more, and the storage modulus at -10°C is 1.0×10 7 preparing a first sheet having an adhesive layer having a compressive strength of 0.01 Pa or less; (2) Functional layer and storage modulus at 80°C of 1.0 × 10 2 Pa or more, and the storage modulus at -10°C is 1.0×10 7 preparing a second sheet having an adhesive layer having a compressive strength of 0.01 Pa or less; (3) attaching the first sheet to a surface of the structure by the adhesive force of the adhesive layer of the first sheet; and (4) A step of attaching the second sheet to a surface of the first sheet and a surface of the structure by the adhesive force of the adhesive layer of the second sheet while overlapping a part of the second sheet near the edge of the first sheet. A method for repairing or reinforcing a structure, comprising:

[0144] [Item 12] 1. A method of repairing a roof, comprising: (1) Each has a functional layer and a storage modulus of 1.0 × 10 at 80 °C. 2 Pa or more, and the storage modulus at -10°C is 1.0×10 7 preparing a plurality of sheets having an adhesive layer having a compressive strength of 0.01 Pa or less; and (2) A process of attaching the sheet to the surface of the roof by the adhesive strength of the adhesive layer of each sheet, thereby covering the entire surface of the roof with the multiple sheets. A method of repairing or reinforcing a roof comprising:

[0145] The configuration of the present disclosure is not limited to the above-mentioned embodiment and example, and the configuration and method can be changed, added, or deleted without departing from the spirit of the present disclosure. Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. For example, a part of the configuration described in one embodiment or example can be applied to the configuration described in any other embodiment or example. [Industrial Applicability]

[0146] The structural sheet described above can be used by being attached to various objects. [Explanation of symbols]

[0147] 2. Structural sheets 2a 1st sheet 2b: Second sheet 4. Functional layer 4a...Functional layer of the first sheet 4b...Functional layer of the second sheet 6. Middle tier 6a Middle layer of the first sheet 6b Middle layer of the second sheet 8...adhesive layer 8a: Adhesive layer of the first sheet 8b: Adhesive layer of second sheet 10. Roof 18. Seam 20 Primer layer 22....Structural sheet 24...Functional layer 26. Middle class 28...adhesive layer 30. Reinforcement materials 32...Structural sheet 34...Functional layer 36...adhesive layer 38 Plate 40 Test piece 44...Functional layer 46. ​​Middle class 48...adhesive layer

Claims

1. The adhesive layer includes a functional layer and an adhesive layer. The storage modulus of the adhesive layer at 80° C. is 1.0×10 2 Pa or more, and the storage modulus at −10° C. is 1.0×10 7 A structural sheet having a compressive strength of 100 Pa or less.

2. 2. The structural sheet according to claim 1, wherein the adhesive layer is made of an adhesive composition, and the base material of the composition is an acrylic resin.

3. The structural sheet according to claim 2 , wherein the pressure-sensitive adhesive composition contains an isocyanate curing agent.

4. The structural sheet according to claim 2 or 3, wherein the pressure-sensitive adhesive composition contains a tackifier.

5. 3. The structure sheet according to claim 1, wherein the adhesive layer has a thickness of 30 μm or more and 300 μm or less.

6. Shear force at 80°C is 14.0 N / cm 2 3. The structure sheet according to claim 1 or 2, wherein the adhesive strength at -10°C is 4.0 N / 25 mm or more.

7. The structure sheet according to claim 1 or 2, further comprising an intermediate layer disposed between the functional layer and the adhesive layer.

8. The structural sheet according to claim 7 , wherein the intermediate layer includes a reinforcing material.

9. The structure sheet according to claim 7 , wherein at least one of the functional layer and the adhesive layer contains a filler.

10. The structure sheet according to claim 1 or 2, further comprising a release film disposed on the surface of the adhesive layer opposite to the functional layer.

11. A method for repairing or reinforcing a structure, comprising: (1) Functional layer and a storage modulus at 80° C. of 1.0×10 2 Pa or more, and the storage modulus at -10°C is 1.0 x 10 7 preparing a first sheet having an adhesive layer having a viscosity of 0.05 Pa or less; (2) Functional layer and a storage modulus at 80° C. of 1.0×10 2 Pa or more, and the storage modulus at -10°C is 1.0 x 10 7 preparing a second sheet having an adhesive layer having a viscosity of 0.05 Pa or less; (3) attaching the first sheet to a surface of the structure by the adhesive force of the adhesive layer of the first sheet; and (4) A step of attaching the second sheet to a surface of the first sheet and a surface of the structure by the adhesive force of the adhesive layer of the second sheet while overlapping a part of the second sheet near the edge of the first sheet. A method for repairing or reinforcing a structure, comprising:

12. 1. A method of repairing a roof, comprising: (1) Each of the functional layers has a storage modulus of 1.0×10 at 80° C. 2 Pa or more, and the storage modulus at -10°C is 1.0 x 10 7 preparing a plurality of sheets each having an adhesive layer having a viscosity of 0.05 Pa or less; and (2) A step of attaching the sheet to the surface of the roof by the adhesive strength of the adhesive layer of each sheet, thereby covering the entire surface of the roof with the multiple sheets. A method of repairing or reinforcing a roof comprising:

Citation Information

Patent Citations

  • Method for repairing roof

    JP2022101896A