Polyamide block copolymer, polyamide block copolymer composition, and molded article
A polyamide block copolymer with defined endothermic peak shape characteristics addresses the lack of flexibility and tensile property improvement in existing copolymers, achieving balanced heat resistance and mechanical properties through specific polymer block compositions.
Patent Information
- Application Number
- JP2024071225
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-25
- Publication Date
- 2024-11-08
AI Technical Summary
Existing polyamide block copolymers do not fully exhibit the flexibility of soft segments and the physical properties of hard segments, and there is a need for improved tensile properties and endothermic peak shape analysis in DSC curves.
A polyamide block copolymer with specific endothermic peak shape characteristics, comprising a polymer block (A) with 50 mol% semi-aromatic polyamide and a polymer block (B) with a glass transition temperature of 20°C or less, where the maximum endothermic peak temperature (Tm0) ranges from 70 to 320°C, and the distance between peak temperatures (Tm1 and Tm2) satisfies certain relationships, ensuring excellent tensile properties.
The polyamide block copolymer achieves enhanced tensile properties and physical properties by optimizing the endothermic peak shape, balancing heat resistance and mechanical properties.
Smart Images

Figure 2024159647000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyamide block copolymer having a specific endothermic peak shape, a polyamide block copolymer composition, and a molded article. [Background technology]
[0002] Thermoplastic elastomers can be melt-molded and are used in a wide range of fields, such as automotive interior and exterior parts, electronic equipment parts, and sporting goods. Thermoplastic elastomers contain soft segments that exhibit flexibility and hard segments that exhibit crosslinking points, and are classified into, for example, olefin-based, amide-based, urethane-based, ester-based, acrylic-based, and styrene-based. Thermoplastic elastomers can exhibit good physical properties such as mechanical strength, abrasion resistance, heat resistance, and oil resistance according to the above classification, and further improvements are being considered.
[0003] For example, Patent Document 1 aims to provide a method for producing a high molecular weight polyether ester amide block copolymer that exhibits useful properties as a molded product, and discloses a method for producing a polyether ester amide block copolymer, characterized in that at least two components, a polyamide component (a) having carboxyl groups or carboxylate groups at both ends and a polyoxyalkylene glycol component (b) having hydroxyl groups at both ends, are reacted in a molten state in the presence of a specific catalyst. Patent Document 2 aims to provide a method for producing a polyether nylon in which the compatibility between polyether and polyamide is not very good and the melt viscosity of the final product is extremely high, and discloses a method for producing a polyether nylon in which a nylon salt aqueous solution is concentrated in a batch reaction vessel to prepare a molten polyamide prepolymer, and then a polyether, which is a polyalkylene oxide having active hydrogen groups at both ends, and the polyamide prepolymer are continuously fed into a polymerization apparatus to achieve a high degree of polymerization. Patent Document 3 aims to provide a polymer that exhibits excellent heat resistance and low temperature properties, and discloses a polyamide block copolymer obtained by polymerizing a dicarboxylic acid, a diamine, and a polyether diamine and / or a polyether dicarboxylic acid. Furthermore, Patent Document 4 aims to provide a polyamide having high heat resistance and flexibility, and discloses a flexible polyamide in which units consisting of an aliphatic dicarboxylic acid (A1) having 18 or more carbon atoms and / or units consisting of an aliphatic diamine (B1) having 18 or more carbon atoms form soft segments. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 62-246930 [Patent Document 2] Japanese Patent Application Publication No. 8-208833 [Patent Document 3] JP 2000-154248 A [Patent Document 4] International Publication No. 2020 / 085360 Summary of the Invention [Problem to be solved by the invention]
[0005] Although the techniques disclosed in the above patent documents provide polyamide block copolymers with excellent physical properties, further improvements in physical properties may be required depending on the application, and there is room for improvement. In addition, the above patent documents do not disclose the influence of the endothermic peak shape of the DSC curve on various physical properties. There is a demand for polyamide block copolymers that can fully exhibit the flexibility exhibited by the soft segment, and also exhibit the physical properties exhibited by the hard segment, while having excellent physical properties such as tensile properties.
[0006] Therefore, an object of the present invention is to provide a polyamide block copolymer, a polyamide block copolymer composition, and a molded article, which are excellent in physical properties such as tensile properties. Furthermore, other objects of the present invention will be apparent to those skilled in the art upon reading this specification. [Means for solving the problem]
[0007] As a result of intensive research aimed at solving the above problems, the present inventors have conceived the following invention and found that the problems can be solved. That is, the present invention is as follows.
[0008] [1] A polyamide block copolymer comprising a polymer block (A) containing 50 mol % or more of structural units derived from a semi-aromatic polyamide and a polymer block (B) having a glass transition temperature of 20° C. or lower, wherein in a DSC curve measured using a differential scanning calorimeter in accordance with ISO 11357-3 (2011, 2nd edition) by heating from 50° C. to 340° C. at a heating rate of 10° C. / min, the maximum endothermic peak temperature (Tm0) is within the range of 70 to 320° C., and the straight line connecting the two points of 50° C. and 340° C. on the DSC curve is taken as the baseline, and L is the distance of the line segment connecting the endothermic peak top at the maximum endothermic peak temperature (Tm0) to the baseline, the relationship of the following formulas (1) to (3) is satisfied. Formula (1): Tm1 <Tm0 Formula (2): Tm2>Tm0 Formula (3): (Tm2-Tm1)≦35 Where: The Tm1 (° C.) is a temperature that satisfies formula (1), and the distance of the line segment that connects the DSC curve at Tm1 (° C.) to the baseline is (1 / 2)L. The Tm2 (° C.) is a temperature that satisfies formula (2), and the distance of the line segment that connects the DSC curve at Tm2 (° C.) to the baseline is (1 / 2)L. [2] The polyamide block copolymer according to [1], wherein the polymer block (B) contains 50 mol % or more of structural units derived from a polymer having an amino group or a carboxyl group as a terminal group. [3] The polyamide block copolymer according to [1] or [2], wherein the polymer block (B) contains 50 mol % or more of structural units derived from a polyether polyol, an amine derivative thereof, or a carboxyl derivative thereof. [4] The polyamide block copolymer according to any one of [1] to [3], having a tensile elongation at break of 30% or more as measured in accordance with JIS K 7161-1:2014. [5] The polyamide block copolymer according to any one of [1] to [4], wherein the semi-aromatic polyamide contains diamine units mainly composed of structural units derived from at least one aliphatic diamine selected from the group consisting of linear aliphatic diamines and branched aliphatic diamines, and dicarboxylic acid units mainly composed of structural units derived from an aromatic dicarboxylic acid. [6] The polyamide block copolymer according to [5], wherein the semi-aromatic polyamide contains 30 mol % or more of structural units derived from an aliphatic diamine having 4 to 18 carbon atoms relative to the total diamine units. [7] The polyamide block copolymer according to any one of [1] to [6], wherein the semi-aromatic polyamide contains a structural unit derived from at least one aliphatic diamine selected from the group consisting of 1,9-nonanediamine and 2-methyl-1,8-octanediamine. [8] The polyamide block copolymer according to any one of [1] to [7], wherein the semi-aromatic polyamide contains a structural unit derived from at least one aromatic dicarboxylic acid selected from the group consisting of terephthalic acid, 1,4-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and 2,7-naphthalenedicarboxylic acid. [9] The polyamide block copolymer according to any one of [1] to [8], wherein the polymer block (A) has a number average molecular weight of 300 to 12,000.
[10] The polyamide block copolymer according to any one of [1] to [9], wherein the polymer block (A) has a weight average molecular weight of 1,000 to 50,000.
[11] The polyamide block copolymer according to any one of [1] to
[10] , wherein the molecular weight distribution (weight average molecular weight / number average molecular weight) of the polymer block (A) is 1.5 to 10.0.
[12] The polyamide block copolymer according to any one of [1] to
[11] , wherein the polyamide block copolymer has a molecular weight distribution (weight average molecular weight / number average molecular weight) of 2.0 to 20.0.
[13] A polyamide block copolymer composition comprising the polyamide block copolymer according to any one of [1] to
[12] .
[14] A molded article formed from the polyamide block copolymer according to any one of [1] to
[12] .
[15] A molded article formed from the polyamide block copolymer composition according to
[13] . Effect of the Invention
[0009] According to the present invention, it is possible to provide a polyamide block copolymer, a polyamide block copolymer composition, and a molded article, which are excellent in physical properties such as tensile properties. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a diagram illustrating a DSC curve for explaining an endothermic peak shape. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, the present invention will be described based on an example of an embodiment. However, the embodiment shown below is an example for embodying the technical idea of the present invention, and the present invention is not limited to the following description. In addition, in this specification, preferred embodiments are shown, but a combination of two or more of the individual preferred embodiments is also a preferred embodiment. When there are several numerical ranges for matters shown as numerical ranges, the lower limit and upper limit can be selectively combined to form a preferred embodiment. In this specification, when a numerical range is stated as "XX to YY", it means "not less than XX and not more than YY". Furthermore, in this specification, a "unit" (where "" indicates a monomer) means a "structural unit derived from", for example, a "dicarboxylic acid unit" means a "structural unit derived from a dicarboxylic acid", and a "diamine unit" means a "structural unit derived from a diamine".
[0012] <Polyamide block copolymer> The polyamide block copolymer of this embodiment comprises a polymer block (A) containing 50 mol % or more of structural units derived from a semi-aromatic polyamide and a polymer block (B) having a glass transition temperature of 20°C or less, and is characterized in that in a DSC curve measured using a differential scanning calorimeter in accordance with ISO11357-3 (2011, 2nd edition) by heating from 50°C to 340°C at a heating rate of 10°C / min, the maximum endothermic peak temperature (Tm0) is within the range of 70 to 320°C and the polyamide block copolymer has a specific endothermic peak shape described later.
[0013] The polyamide block copolymer of this embodiment has excellent physical properties such as tensile properties because the maximum endothermic peak temperature shows a specific temperature and the DSC curve has a specific endothermic peak shape. In addition, in the polyamide block copolymer of this embodiment, the polymer block (A) is a hard segment and the polymer block (B) is a soft segment, and the properties of each polymer block can be fully exhibited. Specifically, the polyamide block copolymer of this embodiment is likely to have the polymer blocks constituting each segment formed to be sufficiently large, and therefore the polymer block (A) has excellent heat resistance and mechanical properties, and the polymer block (B) has excellent flexibility.
[0014] <Maximum endothermic peak temperature (Tm0)> The maximum endothermic peak temperature (hereinafter also referred to as "Tm0") of the polyamide block copolymer of this embodiment is the peak top temperature (melting point) of the maximum endothermic peak in the DSC curve. The DSC curve is obtained by measuring the polyamide block copolymer using a differential scanning calorimeter, heating from 50°C to 340°C at a heating rate of 10°C / min in accordance with ISO11357-3 (2011, 2nd edition). The differential scanning calorimeter measurement can be performed in more detail by the method described in the Examples. The polyamide block copolymer of this embodiment has a Tm0 in the range of 70 to 320° C. If the Tm0 is less than 70° C., the copolymer is susceptible to the environmental temperature in use and has insufficient heat resistance and mechanical properties. If the Tm0 is more than 320° C., the copolymer has insufficient moldability.
[0015] The polyamide block copolymer has a Tm0 of preferably 120 to 320° C., more preferably 180 to 320° C., even more preferably 200 to 320° C., still more preferably 230 to 320° C., still more preferably 235 to 320° C., and still more preferably 240 to 320° C. If the polyamide block copolymer has a Tm0 of 230° C. or higher, excellent heat resistance can be imparted to a molded article obtained using the polyamide block copolymer, which is preferable.
[0016] <Endothermic peak shape> In this embodiment, the term "endothermic peak shape" refers to the shape of an endothermic peak shown in a DSC curve. The endothermic peak shape exhibited by the polyamide block copolymer of this embodiment will be described with reference to Fig. 1. Fig. 1 is a diagram illustrating a DSC curve for explaining the endothermic peak shape. The DSC curve illustrated in Fig. 1 is obtained by the same measurement method as that for Tm0 described above. As shown in FIG. 1, the straight line connecting two points, 50° C. (not shown) and 340° C. (not shown) on the DSC curve is taken as the baseline. Next, the maximum endothermic peak Q0 (the point at which the heat flow value is minimal with respect to the baseline) is identified on the DSC curve. In the example shown in FIG. 1, since the DSC curve is unimodal, there is only one endothermic peak, and this endothermic peak is taken as the maximum endothermic peak. When the DSC curve is multimodal, the point at which the heat flow value is minimal with respect to the baseline is taken as the maximum endothermic peak among the multiple endothermic peaks. In addition, at the maximum endothermic peak temperature Tm0 (° C.), the distance of the line segment connecting the endothermic peak top Q0 to the baseline Q0b is taken as L. Tm1 (° C.) is calculated using the following formula (1): Formula (1): Tm1 <Tm0 and the distance of the line segment connecting the DSC curve at Tm1 (°C) to the baseline is (1 / 2)L (i.e., half of L). In other words, the distance of the line segment parallel to the vertical axis of the DSC curve graph connecting Q1 to Q1b in FIG. 1 is (1 / 2)L, and Tm1 (°C) is the temperature of the DSC curve that shows the heat quantity at Q1. Tm2 (℃) is calculated using the following formula (2): Formula (2): Tm2>Tm0 and the distance of the line segment connecting the DSC curve at Tm2 (°C) to the baseline is (1 / 2)L (i.e., half of L). In other words, the distance of the line segment parallel to the vertical axis of the DSC curve graph connecting Q2 to Q2b in FIG. 1 is (1 / 2)L, and Tm2 (°C) is the temperature of the DSC curve that shows the heat quantity at Q2. In the polyamide block copolymer of this embodiment, in the DSC curve as shown in FIG. 1 , the following formula (3): Formula (3): (Tm2-Tm1)≦35 Meet the following. Here, in a DSC curve, when a plurality of Tm1s are present, when a plurality of Tm2s are present, or when a plurality of Tm1s and a plurality of Tm2s are present, in the polyamide block copolymer of this embodiment, the minimum value among the possible differences (Tm2-Tm1) (i.e., the difference between Tm2 showing the minimum temperature among the plurality of Tm2s and Tm1 showing the maximum temperature among the plurality of Tm1s) satisfies the above formula (3). That is, the polyamide block copolymer of this embodiment satisfies the relationships of the above formulas (1) to (3) in the DSC curve. In other words, when the polyamide block copolymer of this embodiment is measured using a differential scanning calorimeter, a DSC curve having an endothermic peak shape that satisfies the above formula (3) is obtained.
[0017] Here, "(Tm2-Tm1)" in the above formula (3) may be considered as the full width at half maximum of the maximum endothermic peak temperature. The heat resistance and mechanical properties are insufficient when (Tm2-Tm1) exceeds 35. From the viewpoint of heat resistance and mechanical properties, (Tm2-Tm1) preferably satisfies the following formula (3-1), more preferably satisfies the following formula (3-2), and further preferably satisfies the following formula (3-3). Formula (3-1): (Tm2-Tm1)≦30 Formula (3-2): (Tm2-Tm1)≦25 Formula (3-3): (Tm2-Tm1)≦20
[0018] Preferably, the polyamide block copolymer of this embodiment satisfies the following relations of formulas (4) to (6) in addition to the relations of formulas (1) to (3) in the DSC curve. Alternatively, the polyamide block copolymer of this embodiment may satisfy the following relations of formulas (4) to (6) in the DSC curve, regardless of whether the relations of formulas (1) to (3) are satisfied. Formula (4): Tm3 <Tm0 Formula (5): Tm4>Tm0 Formula (6): (Tm4-Tm3)≦33 Where: The Tm3 (° C.) is a temperature that satisfies formula (4), and the distance of the line segment that connects the DSC curve at the Tm3 (° C.) to the baseline is (3 / 4)L. The Tm4 (° C.) is a temperature that satisfies formula (5), and the distance of the line segment that connects the DSC curve at Tm4 (° C.) to the baseline is (3 / 4)L. Here, in the DSC curve, when a plurality of Tm3s are present, when a plurality of Tm4s are present, or when a plurality of Tm3s and a plurality of Tm4s are present, in the polyamide block copolymer of this embodiment, the minimum value among the possible differences (Tm4-Tm3) (i.e., the difference between Tm4 showing the minimum temperature among the plurality of Tm4s and Tm3 showing the maximum temperature among the plurality of Tm3s) satisfies the above formula (6). Heat resistance and mechanical properties may be insufficient if (Tm4-Tm3) exceeds 33. From the viewpoint of heat resistance and mechanical properties, (Tm4-Tm3) preferably satisfies the following formula (6-1), more preferably satisfies the following formula (6-2), and further preferably satisfies the following formula (6-3). Formula (6-1): (Tm4-Tm3)≦29 Formula (6-2): (Tm4-Tm3)≦24 Formula (6-3): (Tm4-Tm3)≦19
[0019] The polyamide block copolymer of this embodiment can be obtained, for example, by mixing and polymerizing the respective polymers constituting the hard segment and the soft segment. In this way, by mixing and polymerizing a pre-prepared polymer block (A) and a pre-prepared polymer block (B), the polyamide block copolymer of this embodiment contains blocks intended as polymer blocks constituting each segment. When the polyamide block copolymer of this embodiment contains the intended blocks as described above, the shape of the endothermic peak is sharp, and the value indicated by the above (Tm2-Tm1) tends to be small. In addition, when the polymer blocks constituting each segment are derived from a pre-prepared polymer, the characteristics of each polymer block are easily exhibited. As a result, the polyamide block copolymer of this embodiment is considered to have excellent physical properties such as tensile properties.
[0020] <Polymer block (A)> The polymer block (A) contains 50 mol % or more of structural units derived from a semi-aromatic polyamide. From the viewpoint of easily obtaining even more excellent heat resistance, the polymer block (A) contains preferably 70 mol % or more, more preferably 90 mol % or more, and may contain 100 mol % of structural units derived from a semi-aromatic polyamide. In the polymer block (A), structural units other than the structural units derived from a semi-aromatic polyamide are not limited as long as the effects of the present invention can be obtained.
[0021] The semi-aromatic polyamide refers to a polyamide containing diamine units mainly composed of structural units derived from an aliphatic diamine and dicarboxylic acid units mainly composed of structural units derived from an aromatic dicarboxylic acid, or a polyamide resin containing dicarboxylic acid units mainly composed of structural units derived from an aliphatic dicarboxylic acid and diamine units mainly composed of structural units derived from an aromatic diamine. Here, "mainly composed" means that the diamine units or dicarboxylic acid units constitute 50 to 100 mol %, preferably 60 to 100 mol %, of all units in the diamine units or dicarboxylic acid units. In this embodiment, from the viewpoint of being more likely to have excellent heat resistance, it is preferable that the semi-aromatic polyamide contains diamine units mainly composed of structural units derived from an aliphatic diamine and dicarboxylic acid units mainly composed of structural units derived from an aromatic dicarboxylic acid.
[0022] [Aliphatic diamine unit] The aliphatic diamine used in the aliphatic diamine unit is preferably an aliphatic diamine having 4 to 18 carbon atoms, more preferably an aliphatic diamine having 4 to 16 carbon atoms, even more preferably an aliphatic diamine having 4 to 12 carbon atoms, even more preferably an aliphatic diamine having 6 to 12 carbon atoms, even more preferably an aliphatic diamine having 6 to 10 carbon atoms, and even more preferably an aliphatic diamine having 7 to 10 carbon atoms. In addition, from the viewpoint of ensuring that the polymerization reaction with dicarboxylic acid proceeds smoothly and being advantageous in improving physical properties such as heat resistance and flexibility, the content of structural units derived from aliphatic diamines having 4 to 18 carbon atoms relative to all diamine units constituting the semi-aromatic polyamide is preferably 30 mol% or more, more preferably 30 to 100 mol%, even more preferably 50 to 100 mol%, even more preferably 70 to 100 mol%, even more preferably 90 to 100 mol%, or may be 100 mol%.
[0023] Examples of aliphatic diamines having 4 to 18 carbon atoms include linear aliphatic diamines such as 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine (hexamethylenediamine), 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,13-tridecanediamine, 1,14-tetradecanediamine, 1,15-pentadecanediamine, 1,16-hexadecanediamine, 1,17-heptadecanediamine, and 1,18-octadecanediamine; 1-Butyl-1,2-ethanediamine, 1,1-Dimethyl-1,4-butanediamine, 1-Ethyl-1,4-butanediamine, 2-Ethyl-1,4-butanediamine, 1,2-Dimethyl-1,4-butanediamine, 1,3-Dimethyl-1,4-butanediamine, 1,4-Dimethyl-1,4-butanediamine, 2-Methyl-1,3-propanediamine, 2-Methyl-1,4-butanediamine, 2,3-Dimethyl-1,4-butanediamine, 2-Methyl-1, 5-Pentanediamine, 3-Methyl-1,5-pentanediamine, 2-Ethyl-1,5-pentanediamine, 2-Propyl-1,5-pentanediamine, 2-Butyl-2-Ethyl-1,5-pentanediamine, 2,5-Dimethyl-1,6-Hexanediamine, 2,4-Dimethyl-1,6-Hexanediamine, 3,3-Dimethyl-1,6-Hexanediamine, 2,2-Dimethyl-1,6-Hexanediamine, 2,2,4-Trimethyl-1,6-Hexanediamine amine, 2,4,4-trimethyl-1,6-hexanediamine, 2-ethyl-1,6-hexanediamine, 2-propyl-1,6-hexanediamine, 2,4-diethyl-1,6-hexanediamine, 2-ethyl-1,7-heptanediamine, 2-propyl-1,7-heptanediamine, 2-methyl-1,8-octanediamine, 3-methyl-1,8-octanediamine, 1,3-dimethyl-1,8-octanediamine, 1,4-dimethyl-1,8-octanediamine branched aliphatic diamines such as nonanediamine, 2,4-dimethyl-1,8-octanediamine, 3,4-dimethyl-1,8-octanediamine, 4,5-dimethyl-1,8-octanediamine, 2,2-dimethyl-1,8-octanediamine, 3,3-dimethyl-1,8-octanediamine, 4,4-dimethyl-1,8-octanediamine, 2-ethyl-1,8-octanediamine, 2-methyl-1,9-nonanediamine, and 5-methyl-1,9-nonanediamine; Alicyclic diamines such as 1,2-cyclohexanediamine, 1,4-cyclohexanediamine, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, bis(4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, and bis(aminopropyl)piperazine may be used alone or in combination of two or more.
[0024] From the viewpoint of heat resistance, the aliphatic diamine is preferably at least one selected from the group consisting of linear aliphatic diamines and branched aliphatic diamines, and more preferably a combination of a linear aliphatic diamine and a branched aliphatic diamine. That is, the semi-aromatic polyamide preferably contains diamine units mainly composed of structural units derived from at least one aliphatic diamine selected from the group consisting of linear aliphatic diamines and branched aliphatic diamines, and dicarboxylic acid units mainly composed of structural units derived from aromatic dicarboxylic acids, and more preferably contains diamine units mainly composed of structural units derived from linear aliphatic diamines and branched aliphatic diamines, and dicarboxylic acid units mainly composed of structural units derived from aromatic dicarboxylic acids.
[0025] When a linear aliphatic diamine and a branched aliphatic diamine are used in combination, the molar ratio of the linear aliphatic diamine to the branched aliphatic diamine is preferably 99:1 to 1:99, more preferably 95:5 to 5:95, even more preferably 90:10 to 10:90, and even more preferably 85:15 to 15:85, and the above molar ratio may be 80:20 to 20:80, 70:30 to 30:70, or 65:35 to 35:65. When the molar ratio of the linear aliphatic diamine to the branched aliphatic diamine is within the above range, the polymerization reaction with the polymer block (B) proceeds well, and the obtained polyamide block copolymer can be expected to have excellent heat resistance and flexibility.
[0026] Furthermore, from the viewpoint of more prominently exhibiting the effects of the present invention and excellent raw material availability, the semi-aromatic polyamide preferably contains a structural unit derived from at least one aliphatic diamine selected from the group consisting of 1,4-butanediamine, 1,6-hexanediamine, 1,9-nonanediamine, 2-propyl-1,6-hexanediamine, 2-ethyl-1,7-heptanediamine, 2-methyl-1,8-octanediamine, 1,10-decanediamine, 1,11-undecanediamine, and 1,12-dodecanediamine, more preferably contains a structural unit derived from at least one aliphatic diamine selected from the group consisting of 1,6-hexanediamine, 1,9-nonanediamine, 2-methyl-1,8-octanediamine, and 1,10-decanediamine, and even more preferably contains a structural unit derived from at least one aliphatic diamine selected from the group consisting of 1,9-nonanediamine and 2-methyl-1,8-octanediamine. Among these, it is even more preferable that the semi-aromatic polyamide contains structural units derived from both 1,9-nonanediamine and 2-methyl-1,8-octanediamine, and contains structural units derived from both 1,6-hexanediamine and 1,10-decanediamine, and from the viewpoint of easily obtaining moldability and even more excellent heat resistance, it is even more preferable that the semi-aromatic polyamide contains structural units derived from both 1,9-nonanediamine and 2-methyl-1,8-octanediamine.
[0027] In the total amount of diamine units constituting the semi-aromatic polyamide, the content of 1,9-nonanediamine units and / or 2-methyl-1,8-octanediamine units is preferably 50 to 100 mol%, more preferably 60 to 100 mol%, even more preferably 75 to 100 mol%, and even more preferably 90 to 100 mol%. When the content of 1,9-nonanediamine units and / or 2-methyl-1,8-octanediamine units in the total amount of diamine units constituting the semi-aromatic polyamide is within the above range, the heat resistance is further improved and excellent chemical resistance can also be expected.
[0028] When 1,9-nonanediamine and 2-methyl-1,8-octanediamine are used in combination, the molar ratio of 1,9-nonanediamine:2-methyl-1,8-octanediamine is preferably 99:1 to 1:99, more preferably 95:5 to 5:95, even more preferably 90:10 to 10:90, and even more preferably 85:15 to 15:85, and the above molar ratio may be 80:20 to 20:80, 70:30 to 30:70, or 65:35 to 35:65. When the molar ratio of 1,9-nonanediamine and 2-methyl-1,8-octanediamine is within the above range, the polymerization reaction with the polymer block (B) proceeds well, and the obtained polyamide block copolymer can be expected to have excellent heat resistance and flexibility.
[0029] In the total amount of diamine units constituting the semi-aromatic polyamide, the content of 1,6-hexanediamine units and / or 1,10-decanediamine units is preferably 50 to 100 mol%, more preferably 60 to 100 mol%, even more preferably 75 to 100 mol%, and even more preferably 90 to 100 mol%.
[0030] When 1,6-hexanediamine and 1,10-decanediamine are used in combination, the molar ratio of 1,6-hexanediamine:1,10-decanediamine is preferably 99:1 to 1:99, more preferably 95:5 to 5:95, even more preferably 90:10 to 10:90, and even more preferably 85:15 to 15:85.
[0031] In addition, the semi-aromatic polyamide may contain, as a diamine unit, a structural unit derived from a diamine other than an aliphatic diamine, such as an aromatic diamine, as long as the effect of the present invention is not impaired. Only one type of structural unit derived from a diamine other than an aliphatic diamine may be contained, or two or more types of structural units derived from a diamine other than an aliphatic diamine may be contained. The content of constituent units derived from other than the above aliphatic diamines in the diamine units is preferably 30 mol % or less, more preferably 20 mol % or less, even more preferably 10 mol % or less, and even more preferably 5 mol % or less.
[0032] [Aromatic dicarboxylic acid unit] Examples of aromatic dicarboxylic acids used in the aromatic dicarboxylic acid unit include isophthalic acid, terephthalic acid, 1,4-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, diphenic acid, 4,4'-biphenyldicarboxylic acid, diphenylmethane-4,4'-dicarboxylic acid, and diphenylsulfone-4,4'-dicarboxylic acid. These aromatic dicarboxylic acids may be used alone or in combination of two or more. From the viewpoint of ensuring that the polymerization reaction with the diamine proceeds smoothly and being advantageous in improving physical properties such as heat resistance, the semi-aromatic polyamide preferably contains a structural unit derived from at least one aromatic dicarboxylic acid selected from the group consisting of terephthalic acid, 1,4-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and 2,7-naphthalenedicarboxylic acid, and from the viewpoint of further improving heat resistance, it is more preferable that the semi-aromatic polyamide contains a structural unit derived from at least one aromatic dicarboxylic acid selected from the group consisting of terephthalic acid and 2,6-naphthalenedicarboxylic acid.
[0033] From the viewpoint of heat resistance and mechanical strength, the content of constituent units derived from at least one aromatic dicarboxylic acid selected from the group consisting of terephthalic acid and 2,6-naphthalenedicarboxylic acid relative to all dicarboxylic acid units is preferably 30 mol% or more, more preferably 30 to 100 mol%, even more preferably 50 to 100 mol%, even more preferably 70 to 100 mol%, even more preferably 90 to 100 mol%, and may be 100 mol%.
[0034] In addition, the semi-aromatic polyamide may contain, as a dicarboxylic acid unit, a constitutional unit derived from a dicarboxylic acid other than an aromatic dicarboxylic acid, such as an aliphatic dicarboxylic acid, as long as the effect of the present invention is not impaired. Only one type of constitutional unit derived from a dicarboxylic acid other than an aromatic dicarboxylic acid may be contained, or two or more types of constitutional units derived from a dicarboxylic acid other than an aromatic dicarboxylic acid may be contained. Examples of the aliphatic dicarboxylic acid include linear aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedicarboxylic acid, and dodecanedicarboxylic acid; Branched aliphatic dicarboxylic acids such as 2,2-diethylsuccinic acid, 2,2-dimethylglutaric acid, 2-methyladipic acid, and trimethyladipic acid; alicyclic dicarboxylic acids such as 1,3-cyclopentanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid; and the like. The content of constituent units derived from other than the aromatic dicarboxylic acid in the dicarboxylic acid unit is preferably 30 mol % or less, more preferably 20 mol % or less, even more preferably 10 mol % or less, and even more preferably 5 mol % or less.
[0035] (Content of Aliphatic Diamine Units and Aromatic Dicarboxylic Acids) The content of the structural units derived from aliphatic diamines relative to all structural units constituting the semi-aromatic polyamide is preferably from 15 to 55 mol %, and more preferably from 25 to 55 mol %. The content of constituent units derived from aromatic dicarboxylic acid relative to all constituent units constituting the semi-aromatic polyamide is preferably from 15 to 55 mol %, and more preferably from 25 to 55 mol %. The total content of the structural units derived from aliphatic diamines and aromatic dicarboxylic acids relative to all structural units constituting the semi-aromatic polyamide is preferably 30 to 100 mol%, more preferably 50 to 100 mol%, and even more preferably 70 to 100 mol%, and may be 90 to 100 mol%, or may be 100 mol%.
[0036] [Other building blocks] The semi-aromatic polyamide may contain other structural units than the diamine unit and the dicarboxylic acid unit, as long as the effect of the present invention is not impaired. Examples of the other structural units include a polycarboxylic acid unit, an aminocarboxylic acid unit, and a lactam unit. Examples of the polyvalent carboxylic acid unit include structural units derived from trivalent or higher polyvalent carboxylic acids such as trimellitic acid, trimesic acid, pyromellitic acid, etc. These polyvalent carboxylic acid units can be contained to the extent that melt molding is possible. Examples of the aminocarboxylic acid unit include structural units derived from lactams such as caprolactam and lauryllactam; and aminocarboxylic acids such as 11-aminoundecanoic acid and 12-aminododecanoic acid. Examples of the lactam unit include structural units derived from ε-caprolactam, enantholactam, undecane lactam, lauryllactam, α-pyrrolidone, α-piperidone, and the like. The content of other structural units relative to all structural units constituting the semi-aromatic polyamide is preferably 30 mol % or less, and more preferably 10 mol % or less.
[0037] [Specific examples of semi-aromatic polyamides] Representative semi-aromatic polyamides containing diamine units mainly composed of aliphatic diamine units and dicarboxylic acid units mainly composed of aromatic dicarboxylic acid units include polytetramethylene terephthalamide (polyamide 4T), polypentamethylene terephthalamide (polyamide 5T), polyhexamethylene terephthalamide (polyamide 6T), polyhexamethylene terephthalamide / polypentamethylene terephthalamide copolymer (polyamide 6T / 5T), polyhexamethylene terephthalamide / poly(2-methylpentamethylene) terephthalamide, and polytetramethylene terephthalamide (polyamide 4T). Polynonamethylene terephthalamide copolymer (Polyamide 6T / M5T), Polynonamethylene terephthalamide (Polyamide 9T), Poly(2-methyloctamethylene) terephthalamide (Polyamide M8T), Polynonamethylene terephthalamide / Poly(2-methyloctamethylene) terephthalamide copolymer (Polyamide 9T / M8T), Polynonamethylene naphthalene dicarboxamide (Polyamide 9N), Poly(2-methyloctamethylene) naphthalene dicarboxamide (Polyamide M8N), Polynonamethylene naphthalene dicarboxamide / Poly(2-methyloctamethylene) Poly(2-methylpentamethylene) terephthalamide copolymer (Polyamide 10T / M5T), Poly(2-methyloctamethylene) terephthalamide copolymer (Polyamide 10T / M8T), Poly(hexamethylene) terephthalamide copolymer (Polyamide 10T / M8T), Poly(2-methyloctam ... polyisophthalamide (polyamide 6I), copolymer of polyamide 6I and polyamide 6T (polyamide 6I / 6T), copolymer of polyhexamethylene adipamide (polyamide 66) and polyamide 6T (polyamide 66 / polyamide 6T), copolymer of polyamide 66, polyamide 6I and polyamide 6T (polyamide 66 / polyamide 6I / 6T), copolymer of polyamide 6T and polycaprolactam (polyamide 6) (polyamide 6T / 6), copolymer of polyamide 6T and polyundecaneamide (polyamide 11) (polyamide 6T / 11),Examples of the copolymer include a copolymer of polyamide 6T and polydodecanamide (polyamide 12) (polyamide 6T / 12), polydecamethylene isophthalamide (polyamide 10I), a copolymer of polyamide 10I and polyamide 10T (polyamide 10I / 10T), a copolymer of polyamide 6T and polyamide 10T (polyamide 6T / 10T), a copolymer of polyamide 10T and polyamide 6 (polyamide 10T / 6), a copolymer of polyamide 10T and polyamide 11 (polyamide 10T / 11), and a copolymer of polyamide 10T and polyamide 12 (polyamide 10T / 12).
[0038] [End-capping agent] In this embodiment, the semi-aromatic polyamide contained in the polymer block (A) may or may not contain a structural unit derived from an end-capping agent. The content of the structural units derived from the terminal blocking agent relative to the diamine units is preferably 0 mol % or more and 10 mol % or less, more preferably more than 0 mol % and 10 mol % or less, even more preferably 1.0 to 10 mol %, even more preferably 2.0 to 7.5 mol %, and still more preferably 2.5 to 6.5 mol %. The content of the structural unit derived from the terminal blocking agent can be adjusted by the amount of the terminal blocking agent charged relative to the diamine when the polymerization raw materials are charged. In consideration of the volatilization of the monomer components during polymerization, it is desirable to finely adjust the amount of the terminal blocking agent charged when the polymerization raw materials are charged so that a desired amount of the structural unit derived from the terminal blocking agent is introduced into the obtained semi-aromatic polyamide. In addition, when polymerizing the polymer constituting the polymer block (A) and the polymer constituting the polymer block (B), the terminal blocking agent can be charged so as to be within the above-mentioned desired range. In addition, the terminal blocking agent can be charged to the polymer constituting the polymer block (A) together with the terminal functionalizing agent described later so as to be within the above-mentioned desired range.
[0039] As a method for determining the content of structural units derived from an end-capping agent in a polyamide, for example, as disclosed in JP-A-07-228690, a method can be mentioned in which the solution viscosity is measured, the total amount of end groups is calculated from the relational equation between the viscosity and the number average molecular weight, and the amount of amino groups and the amount of carboxyl groups determined by titration are subtracted from the total amount of end groups. As the terminal blocking agent, a monofunctional compound having reactivity with a terminal amino group or a terminal carboxyl group can be used.Specific examples include monocarboxylic acid, acid anhydride, monoisocyanate, monoacid halide, monoester, monoalcohol, monoamine, etc. From the viewpoint of reactivity and the stability of the blocked end, a monocarboxylic acid is preferable as a terminal blocking agent for a terminal amino group, and a monoamine is preferable as a terminal blocking agent for a terminal carboxyl group.From the viewpoint of ease of handling, etc., a monocarboxylic acid is more preferable as a terminal blocking agent.
[0040] The monocarboxylic acid used as the terminal blocking agent is not particularly limited as long as it has reactivity with an amino group. Examples of the monocarboxylic acid include aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, decanoic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, behenic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclopentane carboxylic acid and cyclohexane carboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, α-naphthalene carboxylic acid, β-naphthalene carboxylic acid, and methylnaphthalene carboxylic acid; monocarboxylic acids having aromatic alkyl groups such as phenyl acetic acid; and any mixtures thereof. Among these, at least one selected from acetic acid, propionic acid, butyric acid, decanoic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, and benzoic acid is preferred from the standpoint of reactivity, stability of blocked terminals, and price.
[0041] The monoamine used as the terminal blocking agent is not particularly limited as long as it has reactivity with carboxyl group. Examples of the monoamine include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, dodecylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; aromatic monoamines such as aniline, toluidine, diphenylamine, and naphthylamine; and any mixtures thereof. Among these, at least one selected from methylamine, ethylamine, propylamine, dodecylamine, stearylamine, cyclohexylamine, and aniline is preferred from the viewpoints of reactivity, high boiling point, stability of blocked terminals, and price.
[0042] [Method of producing semi-aromatic polyamide] Semi-aromatic polyamides can be produced, for example, from dicarboxylic acids and diamines as raw materials by melt polymerization, solid-state polymerization, melt extrusion polymerization, etc. Specifically, semi-aromatic polyamides can be produced as follows. First, a nylon salt is produced by mixing a diamine, a dicarboxylic acid, and, if necessary, an aminocarboxylic acid, a lactam, a catalyst, an end-capping agent, etc. Next, the produced nylon salt is heated to a temperature of 200 to 250°C and thermally polymerized to obtain a semi-aromatic polyamide as a prepolymer. Furthermore, the molecular weight of the semi-aromatic polyamide can be adjusted to a desired level by subjecting the prepolymer to solid-state polymerization or by increasing the degree of polymerization using a melt extruder. When the high polymerization stage is carried out by solid-phase polymerization, it is preferably carried out under reduced pressure or in an inert gas flow, and the polymerization rate is high, productivity is excellent, and coloration and gelation can be effectively suppressed if the polymerization temperature is within the range of 200 to 280° C. Furthermore, when the high polymerization stage is carried out by a melt extruder, the polymerization temperature is preferably 370° C. or less, and when polymerization is carried out under such conditions, a semi-aromatic polyamide with almost no decomposition and little deterioration can be obtained.
[0043] Examples of catalysts that can be used in producing semi-aromatic polyamides include phosphoric acid, phosphorous acid, hypophosphorous acid, and salts or esters thereof. Examples of the salts or esters include salts of phosphoric acid, phosphorous acid, or hypophosphorous acid with metals such as potassium, sodium, magnesium, vanadium, calcium, zinc, cobalt, manganese, tin, tungsten, germanium, titanium, and antimony; ammonium salts of phosphoric acid, phosphorous acid, or hypophosphorous acid; ethyl esters, isopropyl esters, butyl esters, hexyl esters, isodecyl esters, octadecyl esters, decyl esters, stearyl esters, and phenyl esters of phosphoric acid, phosphorous acid, or hypophosphorous acid. The amount of the catalyst used is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, based on the total mass (100% by mass) of the raw materials for the semi-aromatic polyamide. The amount of the catalyst used is preferably 1.0% by mass or less, more preferably 0.5% by mass or less. If the amount of the catalyst used is equal to or more than the lower limit, the polymerization proceeds more smoothly.
[0044] [Terminal amino group content (before terminal conversion)] In this embodiment, the terminals of the semi-aromatic polyamide can be adjusted to a desired functional group or amount of functional groups by a terminal functionalizing agent described below. On the other hand, the terminal amino group content referred to here is the terminal amino group content in the polyamide before the terminals are converted with a terminal functionalizing agent. The semi-aromatic polyamide before the above-mentioned terminal conversion has a terminal amino group content ([NH2]) of preferably 1 to 4,000 μmol / g, more preferably 1 to 3,000 μmol / g, even more preferably 1 to 2,500 μmol / g, still more preferably 1 to 2,000 μmol / g, even more preferably 1 to 1,500 μmol / g, and even more preferably 1 to 1,000 μmol / g. The terminal amino group content ([NH2]) in this specification refers to the amount of terminal amino groups (unit: μmol) contained in 1 g of semi-aromatic polyamide, and can be determined by neutralization titration method using an indicator.
[0045] [Terminal carboxyl group content (before terminal conversion)] The semi-aromatic polyamide before the above-mentioned terminal conversion has a terminal carboxyl group content ([COOH]), which is the content of terminal carboxyl groups, of preferably 1 to 5,000 μmol / g, more preferably 25 to 4,000 μmol / g, even more preferably 50 to 3,000 μmol / g, still more preferably 75 to 2,500 μmol / g, even more preferably 75 to 2,000 μmol / g, and even more preferably 75 to 1,500 μmol / g. The terminal carboxyl group content ([COOH]) in this specification refers to the amount (unit: μmol) of terminal carboxyl groups contained in 1 g of a semi-aromatic polyamide, and can be determined by potentiometric titration.
[0046] [Melting point] The melting point of the semi-aromatic polyamide is preferably 120°C or higher, more preferably 180°C or higher, even more preferably 200°C or higher, even more preferably 205°C or higher, even more preferably 210°C or higher, even more preferably 230°C or higher, even more preferably 240°C or higher, and even more preferably 250°C or higher. If the melting point of the semi-aromatic polyamide is 120°C or higher, the heat resistance and mechanical properties of the polyamide block copolymer tend to be good. Furthermore, if the melting point of the semi-aromatic polyamide is 230°C or higher, the heat resistance of the polyamide block copolymer is more easily improved. There is no particular limit to the upper limit of the melting point of the semi-aromatic polyamide, but from the viewpoint of moldability, it is preferably 320°C or lower. That is, the melting point of the semi-aromatic polyamide is preferably 120 to 320°C. In the present invention, the melting point can be determined as the peak temperature of a melting peak that appears when the temperature is raised at a rate of 10° C. / min using a differential scanning calorimetry (DSC) analyzer. More specifically, it can be determined by the method described in the examples below.
[0047] [Semi-aromatic ratio] The semi-aromatic ratio (%) of a polyamide can be determined by a method well known to those skilled in the art. The semi-aromatic ratio of a polyamide means the ratio (percentage) of repeating units of a semi-aromatic polyamide among the repeating units constituting the polyamide. The semi-aromatic ratio of a polyamide can be determined, for example, by using NMR, and in this case, is a molar ratio. From the viewpoint of obtaining a polyamide block copolymer that enhances the usability under high temperatures, the semi-aromatic ratio of a polyamide is preferably 30% or more, more preferably 60% or more, even more preferably 75% or more, even more preferably 80% or more, and even more preferably 85% or more. The upper limit of the semi-aromatic ratio of a polyamide may be 100%. In a preferred aspect of this embodiment, the semi-aromatic ratio of a polyamide is 90% or more, preferably 94% or more. In a specific aspect, the semi-aromatic ratio of a polyamide is 100%.
[0048] From the viewpoint of increasing the usability of the polyamide block copolymer at high temperatures, the polymer block (A) preferably contains less than 50 mol % of structural units derived from a non-semi-aromatic polyamide, more preferably contains 10 mol % or less of structural units derived from a non-semi-aromatic polyamide, and even more preferably contains no structural units derived from a non-semi-aromatic polyamide (i.e., 0 mol %).
[0049] [Molecular weight] The number average molecular weight of the polymer block (A) is preferably 300 to 12,000, more preferably 300 to 11,000, even more preferably 350 to 10,000, still more preferably 400 to 9,500, and even more preferably 500 to 9,000, and may be 600 to 8,500 or may be 700 to 8,000. Within the above numerical range, the compatibility between the polymer block (A) and the polymer block (B) is excellent, and the endothermic peak shape is likely to be sharp, so that physical properties such as tensile properties tend to be even more excellent. The weight average molecular weight of the polymer block (A) is preferably 1,000 to 50,000, more preferably 1,100 to 45,000, even more preferably 1,200 to 40,000, still more preferably 1,300 to 40,000, even more preferably 1,400 to 30,000, 1,600 to 25,000, or 2,000 to 20,000. Within the above numerical ranges, the compatibility between the polymer block (A) and the polymer block (B) is likely to be excellent, and the endothermic peak shape is likely to be sharp, so that physical properties such as tensile properties tend to be even more excellent. The molecular weight distribution (weight average molecular weight / number average molecular weight) of the polymer block (A) is preferably 1.5 to 10.0, more preferably 1.7 to 8.0, even more preferably 1.8 to 6.0, still more preferably 2.0 to 5.0, and even more preferably 2.0 to 4.0. Within the above numerical range, the compatibility between the polymer block (A) and the polymer block (B) is likely to be excellent, and the endothermic peak shape is likely to be sharp, so that physical properties such as tensile properties tend to be even more excellent. In the present invention, the number average molecular weight and the weight average molecular weight can be measured by gel permeation chromatography, and more specifically, are values measured by the method described in the examples.
[0050] [End functionalizing agent] In this embodiment, a terminal functionalizing agent can be used to adjust the terminal of the polymer block (A), preferably the terminal of the semi-aromatic polyamide, to a desired functional group or amount of functional groups. For example, the terminals of the polyamide can be converted by reacting a terminal functionalizing agent with the above-mentioned polyamide prepolymer. It is also possible to convert the terminals of the polyamide by making either the dicarboxylic acid unit or the diamine unit in excess at the stage of charging the raw materials. By adjusting the terminals of the polymer block (A) to a desired functional group or amount of functional groups, the polymer block (A) and the polymer block (B) can be bonded more satisfactorily. The units derived from the terminal functionalizing agent are included in the polymer block (A).
[0051] In addition, when the semi-aromatic polyamide obtained by the above-mentioned method for producing a semi-aromatic polyamide has a desired functional group or amount of functional groups, a terminal functionalizing agent does not need to be used. That is, in this case, the polymer constituting the polymer block (A) and the polymer constituting the polymer block (B) are reacted without using a terminal functionalizing agent, whereby the polymer block (A) and the polymer block (B) can be bonded well to each other. The amount of active terminal functional groups in the semi-aromatic polyamide described below can be adjusted, for example, by adjusting the amount of carboxyl groups and the amount of amino groups contained in the reaction raw materials in the production of the semi-aromatic polyamide.
[0052] There are no limitations on the terminal functionalizing agent as long as it does not impair the effects of the present invention, and examples of such agents include those that can introduce functional groups such as hydroxyl groups, carboxyl groups, amino groups, epoxy groups, mercapto groups, sulfonyl groups, halogen atoms, vinyl groups, and vinylidene groups to the terminals of the polyamide.
[0053] In this embodiment, the terminal functionalizing agent is preferably a compound selected from the group consisting of dicarboxylic acids and diamines. In this case, the polymer block (A) contains a structural unit derived from the polyamide and a structural unit derived from a compound selected from the group consisting of dicarboxylic acids and diamines. Dicarboxylic acids which can be used as end-functionalizing agents include aliphatic dicarboxylic acids and aromatic dicarboxylic acids. Examples of the aliphatic dicarboxylic acid include linear aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedicarboxylic acid, and dodecanedicarboxylic acid; Branched aliphatic dicarboxylic acids such as 2,2-diethylsuccinic acid, 2,2-dimethylglutaric acid, 2-methyladipic acid, and trimethyladipic acid; alicyclic dicarboxylic acids such as 1,3-cyclopentanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid; and the like. Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, diphenic acid, 4,4'-biphenyldicarboxylic acid, diphenylmethane-4,4'-dicarboxylic acid, diphenylsulfone-4,4'-dicarboxylic acid, 1,2-naphthalenedicarboxylic acid, 1,3-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 1,7-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 2,3-furandicarboxylic acid, 2,4-furandicarboxylic acid, 2,5-furandicarboxylic acid, and 3,4-furandicarboxylic acid.
[0054] Diamines that can be used as end-functionalizing agents include aliphatic and aromatic diamines. Examples of the aliphatic diamines include linear aliphatic diamines such as ethylenediamine, 1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,13-tridecanediamine, 1,14-tetradecanediamine, 1,15-pentadecanediamine, 1,16-hexadecanediamine, 1,17-heptadecanediamine, and 1,18-octadecanediamine; 1,2-propanediamine, 1-butyl-1,2-ethanediamine, 1,1-dimethyl-1,4-butanediamine, 1-ethyl-1,4-butanediamine, 2-ethyl-1,4-butanediamine, 1,2-dimethyl-1,4-butanediamine, 1,3-dimethyl-1,4-butanediamine, 1,4-dimethyl-1,4-butanediamine, 2-methyl-1,3-propanediamine, 2-methyl-1,4-butanediamine, 2,3-dimethyl-1,4-butanediamine , 2-methyl-1,5-pentanediamine, 3-methyl-1,5-pentanediamine, 2-ethyl-1,5-pentanediamine, 2-propyl-1,5-pentanediamine, 2-butyl-2-ethyl-1,5-pentanediamine, 2,5-dimethyl-1,6-hexanediamine, 2,4-dimethyl-1,6-hexanediamine, 3,3-dimethyl-1,6-hexanediamine, 2,2-dimethyl-1,6-hexanediamine, 2,2,4-trimethyl-1,6- Hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, 2-ethyl-1,6-hexanediamine, 2-propyl-1,6-hexanediamine, 2,4-diethyl-1,6-hexanediamine, 2-ethyl-1,7-heptanediamine, 2-propyl-1,7-heptanediamine, 2-methyl-1,8-octanediamine, 3-methyl-1,8-octanediamine, 1,3-dimethyl-1,8-octanediamine, 1,4-dimethyl-1,8- branched aliphatic diamines such as octanediamine, 2,4-dimethyl-1,8-octanediamine, 3,4-dimethyl-1,8-octanediamine, 4,5-dimethyl-1,8-octanediamine, 2,2-dimethyl-1,8-octanediamine, 3,3-dimethyl-1,8-octanediamine, 4,4-dimethyl-1,8-octanediamine, 2-ethyl-1,8-octanediamine, 2-methyl-1,9-nonanediamine, and 5-methyl-1,9-nonanediamine; Alicyclic diamines such as 1,2-cyclohexanediamine, 1,4-cyclohexanediamine, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, bis(4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, and bis(aminopropyl)piperazine; and the like. Examples of aromatic diamines include p-phenylenediamine, m-phenylenediamine, p-xylylenediamine, m-xylylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 4,4'-diaminodiphenylether, and 4,4'-methylenedi-2,6-diethylaniline. The above terminal functionalizing agent may be used alone or in combination of two or more kinds.
[0055] (Active terminal functional group content) In the present invention, the "active terminal functional group content" refers to the content of the active terminal functional group of the polymer block (A) contained in the polyamide block copolymer, and the total content of the active terminal functional groups of the semi-aromatic polyamide is the active terminal functional group content of the polymer block (A). The "active terminal functional group" refers to a functional group that exhibits reactive activity toward the terminal functional group of the polymer block (B), and examples of such groups include an amino group and a carboxyl group. When the terminals of a semi-aromatic polyamide are converted using a terminal functionalizing agent, the "active terminal functional group content" refers to the content of the active terminal functional groups after the terminal functional groups are converted. For example, when a semi-aromatic polyamide having an amino group at its terminal is converted to a carboxyl group using a terminal functionalizing agent, the total content of the terminal carboxyl groups after conversion and the terminal amino groups that have not been converted is the active terminal functional group content of the polymer block (A).
[0056] The content of the active terminal functional group of the polymer block (A) may be a content of functional group capable of sufficiently reacting with the terminal functional group of the polymer block (B), and is preferably 5 μmol / g or more or 50 to 5,000 μmol / g, more preferably 75 to 4,500 μmol / g, even more preferably 100 to 4,000 μmol / g, still more preferably 120 to 4,000 μmol / g, still more preferably 150 to 3,000 μmol / g, still more preferably 200 to 2,000 μmol / g, still more preferably 250 to 1,500 μmol / g, and still more preferably 300 to 1,250 μmol / g. If the content of the active terminal functional group is 5 μmol / g or more, the compatibility between the polymer block (A) and the polymer block (B) is excellent, and the flexibility of the polyamide block copolymer can be further improved. Furthermore, if the content of the active terminal functional group is 5,000 μmol / g or less, the heat resistance of the polyamide block copolymer can be further improved. The active terminal functional group content as used herein refers to the amount (unit: μmol) of active terminal functional groups contained in 1 g of polyamide (or polyamide after conversion when a terminal functionalizing agent is used), and can be determined by neutralization titration method and potentiometric titration method using an indicator.
[0057] <Polymer block (B)> The polymer block (B) has a glass transition temperature of 20° C. or lower. If the glass transition temperature exceeds 20° C., it becomes difficult for the polyamide block copolymer to have excellent flexibility. The glass transition temperature of the polymer block (B) is preferably 0° C. or lower, more preferably −20° C. or lower, from the viewpoint of easily exhibiting excellent flexibility at room temperature in the polyamide block copolymer. The lower the glass transition temperature of the polymer block (B), the more preferable it is, but from the viewpoint of heat resistance, it may be −120° C. or higher. That is, the glass transition temperature of the polymer block (B) is preferably from -120 to 20°C. In the present invention, the glass transition temperature can be determined as the temperature of the inflection point that appears when the temperature is raised at a rate of 2°C / min using a differential scanning calorimetry (DSC) analyzer. More specifically, it can be determined by the method described in the Examples below. Alternatively, when it is difficult to measure the glass transition temperature by the above method, the glass transition temperature can be a literature value or a measurement result by a manufacturer. However, the glass transition temperature is preferentially determined by the method described in the Examples below.
[0058] [Polymer unit] Examples of the polymer constituting the polymer block (B) include oxygen atom-containing polymers (hereinafter referred to as "oxygen atom-containing polymers") such as polyethers, polyesters, polycarbonates, and polysiloxanes. Details of polyethers, polyesters, polycarbonates, and polysiloxanes will be described later. The oxygen atom-containing polymer preferably contains oxygen atoms in the main chain. The polymer block (B) more effectively contributes to the development of flexibility by containing oxygen atoms, preferably ether bonds, in the main chain. From the viewpoint of easily obtaining excellent flexibility of the polyamide block copolymer, the content ratio of the constitutional unit derived from the oxygen atom-containing polymer in the polymer block (B) is preferably 50 mol% or more, more preferably 70 mol% or more, further preferably 90 mol% or more, and may be 100 mol%. Also, the content ratio of the constitutional unit derived from the oxygen atom-containing polymer in the polymer block (B) may be 100 mol% or less. That is, the content of structural units derived from the oxygen atom-containing polymer in the polymer block (B) is preferably 50 to 100 mol %.
[0059] Among the above oxygen atom-containing polymers, polyethers are preferred from the viewpoint of easily imparting excellent flexibility. In the polymer block (B), there are no limitations on the constituent units other than the constituent units derived from the oxygen atom-containing polymer, so long as the effects of the present invention can be obtained.
[0060] Furthermore, the polymer block (B) preferably contains 50 mol % or more of structural units derived from a polymer having an amino group or a carboxyl group as a terminal group. The polymer block (B) preferably contains 50 mol % or more of structural units derived from a polymer having an amino group or a carboxyl group as a terminal group, from the viewpoint of reactivity with the polymer block (A). From the viewpoint of reactivity, the content of the structural units derived from a polymer having an amino group or a carboxyl group as a terminal group in the polymer block (B) is more preferably 70 mol% or more, further preferably 90 mol% or more, and may be 100 mol%. Also, the content of the structural units derived from a polymer having an amino group or a carboxyl group as a terminal group in the polymer block (B) may be 100 mol% or less. That is, the content of structural units derived from a polymer having an amino group or a carboxyl group as a terminal group in the polymer block (B) is preferably 50 to 100 mol %. In the polymer block (B), there are no limitations on the constituent units other than the above-mentioned constituent units derived from a polymer having an amino group or a carboxyl group as a terminal group, so long as the effects of the present invention can be obtained.
[0061] <Polyether> In this embodiment, "polyether" means polyether polyol, and includes derivatives such as amine derivatives and carboxyl derivatives of polyether polyol. One or more kinds of polyethers can be used. When the oxygen atom-containing polymer is polyether polyol, its amine derivative, or its carboxyl derivative, the polymer block (B) contains a structural unit derived from polyether polyol, its carboxyl derivative, or its amine derivative. Preferably, the polymer block (B) contains 50 mol % or more of structural units derived from polyether polyol, its amine derivative, or its carboxyl derivative. Examples of polyethers include polyethylene glycol (PEG), polypropylene glycol (PPG), polytrimethylene ether glycol (PO3G), poly(oxybutylene) glycol, polytetramethylene ether glycol (PTMG), poly(3-alkyltetrahydrofuran), particularly poly(3-methyltetrahydrofuran) (poly(3MeTHF)), polypentamethylene ether glycol, polyhexamethylene ether glycol, polyoctamethylene ether glycol, and copolymers thereof. These may be used alone or in combination.
[0062] Examples of the amine derivatives and carboxyl derivatives of polyether include polyetherdiamines and polyetherdicarboxylic acids, etc. Among them, polyetherdiamines are preferred from the viewpoint of imparting better flexibility to the polyamide block copolymer having the polymer block (A) as a hard segment and being expected to exhibit good chemical resistance to the polyamide block copolymer. Examples of polyether diamines include polyethylene glycol (PEG), polypropylene glycol (PPG), polytrimethylene ether glycol (PO3G), poly(oxybutylene) glycol, polytetramethylene ether glycol (PTMG), poly(3-alkyltetrahydrofuran), particularly poly(3-methyltetrahydrofuran) (poly(3MeTHF)), polypentamethylene ether glycol, polyhexamethylene ether glycol, polyoctamethylene ether glycol, and the like, and polyether diamines having amino groups at two ends of their copolymers. These can be used alone or in combination. Such polyether diamines can be obtained, for example, by cyanoacetylation of polyether diol.
[0063] Examples of polyether dicarboxylic acids include polyethylene glycol (PEG), polypropylene glycol (PPG), polytrimethylene ether glycol (PO3G), poly(oxybutylene) glycol, polytetramethylene ether glycol (PTMG), poly(3-alkyltetrahydrofuran), particularly poly(3-methyltetrahydrofuran) (poly(3MeTHF)), polypentamethylene ether glycol, polyhexamethylene ether glycol, polyoctamethylene ether glycol, and polyether dicarboxylic acids having carboxyl groups at two ends of their copolymers. These can be used alone or in combination.
[0064] <polyester> In this embodiment, "polyester" means polyester polyol, and includes derivatives such as amine derivatives and carboxyl derivatives of polyester polyol. One or more types of polyester can be used. When the oxygen atom-containing polymer is polyester polyol, its amine derivative, or its carboxyl derivative, the polymer block (B) contains a constitutional unit derived from polyester polyol, its amine derivative, or its carboxyl derivative. Examples of polyesters include poly(caprolactone), poly(methyl valerolactone), poly(butylene adipate), poly(ethylene adipate), poly(methyl pentanediol adipate), poly(butylene-1,4-hexanediol-1,6-adipate), etc. These may be used alone or in combination of two or more.
[0065] The polyester that can be used is, for example, one produced by polycondensation of a dicarboxylic acid and a polyhydric alcohol. Examples of dicarboxylic acids include aliphatic dicarboxylic acids such as 1,4-cyclohexyldicarboxylic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; and dimer fatty acids consisting of one or two kinds selected from unsaturated fatty acids such as oleic acid, linoleic acid, linolenic acid, palmitoleic acid, and elaidic acid. These may be used alone or in combination of two or more kinds. Examples of polyhydric alcohols include ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,4-cyclohexanedimethanol, etc. These may be used alone or in combination.
[0066] Examples of the amine derivative in polyester include those in which an amino group is introduced at the end of polyester polyol, etc. These can be used alone or in combination of two or more kinds. In addition, the above-mentioned carboxyl derivative in polyester may be, for example, a polyester polyol having a carboxyl group introduced at the end. The above-mentioned carboxyl derivative may have at least one carboxyl group at the end, and may have, for example, a carboxyl group at all ends, or may have both a carboxyl group and a hydroxyl group at the end. These may be used alone or in combination.
[0067] <Polycarbonate> In this embodiment, "polycarbonate" means polycarbonate polyol, and includes derivatives such as amine derivatives and carboxyl derivatives of polycarbonate polyol. One or more types of polycarbonate can be used. When the oxygen atom-containing polymer is polycarbonate polyol, its amine derivative, or its carboxyl derivative, the polymer block (B) contains a structural unit derived from polycarbonate polyol, its amine derivative, or its carboxyl derivative. Examples of polycarbonates include poly(hexanediol-1,6-carbonate), polytetrahydrofuran carbonate, etc. These may be used alone or in combination of two or more.
[0068] The polycarbonate polyol may be, for example, one produced by an esterification reaction between a carbonate ester and a polyhydric alcohol, or one produced by an interfacial polycondensation method in which a polyhydric alcohol is reacted with phosgene. One or more kinds of polycarbonate polyols may be used. Examples of carbonate esters include methyl carbonate, ethyl carbonate, phenyl carbonate, etc. These can be used alone or in combination of two or more. Examples of polyhydric alcohols include ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,4-cyclohexanedimethanol, etc. These may be used alone or in combination.
[0069] The amine derivatives in polycarbonate include, for example, polycarbonate polyols having amino groups at the terminals thereof, etc. These may be used alone or in combination of two or more. In addition, the above-mentioned carboxyl derivative in polycarbonate may be, for example, a polycarbonate polyol having a carboxyl group introduced at the end. The above-mentioned carboxyl derivative may have at least one carboxyl group at the end, and may have, for example, a carboxyl group at all ends, or may have both a carboxyl group and a hydroxyl group at the end. These may be used alone or in combination.
[0070] <Polysiloxane> In this embodiment, "polysiloxane" means polysiloxane polyol, and includes derivatives such as amine derivatives and carboxyl derivatives of polysiloxane polyol. One or more types of polysiloxane can be used. When the oxygen atom-containing polymer is polysiloxane polyol, its amine derivative, or its carboxyl derivative, the polymer block (B) contains a structural unit derived from polysiloxane polyol, its amine derivative, or its carboxyl derivative. Examples of polysiloxanes include compounds having a hydroxyl group at the end of a polyorganosiloxane having a repeating unit represented by the following formula (X): Specific examples include polydimethylsiloxane diol, polydiphenylsiloxane diol, polytrifluoropropylmethylsiloxane diol, polyphenylmethylsiloxane diol, polydiethylsiloxane diol, polydivinylsiloxane diol, polyvinylmethylsiloxane diol, poly(5-hexenyl)methylsiloxane diol, and the like.
[0071] [ka]
[0072] R and R' in formula (X) are organic groups, and may be the same or different. The organic group is not limited as long as it does not impair the effects of the present invention, and examples thereof include alkyl groups having 1 to 8 carbon atoms, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, and octyl groups; alkenyl groups having 1 to 5 carbon atoms, such as vinyl, allyl, 1-butenyl, 2-butenyl, 3-butenyl, 1-methylvinyl, and 1-methylallyl groups; alicyclic alkyl groups, such as cyclohexyl groups; aryl groups, such as phenyl, tolyl, xylyl, benzyl, and 2-phenylethyl groups; and the like.
[0073] Examples of the amine derivative in polysiloxane include those in which an amino group is introduced at the end of polysiloxane polyol, etc. These can be used alone or in combination of two or more kinds. Furthermore, the above-mentioned carboxyl derivative in polysiloxane includes, for example, polysiloxane polyols having a carboxyl group introduced at the end thereof, etc. These can be used alone or in combination of two or more kinds.
[0074] [Molecular weight] The number average molecular weight of the polymer block (B) is preferably 100 or more, 150 or more, or 200 or more, more preferably 300 or more, or 400 or more, and may be 500 or more, 700 or more, or 800 or more from the viewpoint of obtaining a polyamide block copolymer having excellent flexibility, particularly tensile properties. The number average molecular weight of the polymer block (B) is not limited as long as the polymerization reaction with the polymer block (A) proceeds well, but may be, for example, 7,000 or less, 6,000 or less, or 5,000 or less. That is, the number average molecular weight of the polymer block (B) is preferably 100 to 7,000, more preferably 200 to 5,000. Within the above numerical range, the polymerization reaction with the polymer block (A) proceeds well, and the flexibility of the polyamide block copolymer is excellent, so that the tensile properties tend to be further excellent.
[0075] <Method of producing polyamide block copolymer> The method for producing the polyamide block copolymer of this embodiment preferably comprises mixing and polymerizing a polymer constituting the polymer block (A) containing 50 mol % or more of structural units derived from the above-mentioned semi-aromatic polyamide and a polymer constituting the above-mentioned polymer block (B) having a glass transition temperature of 20° C. or less. The method for producing the polyamide block copolymer of this embodiment may also use the above-mentioned terminal functionalizing agent and / or the above-mentioned terminal capping agent. For example, a polyamide block copolymer may be produced by mixing the monomer constituting the polymer block (A) and, if necessary, the terminal capping agent and / or the terminal functionalizing agent, melt-polymerizing the mixture to obtain a polymer constituting the polymer block (A) in which the terminal functional groups have been adjusted, and then adding the polymer constituting the polymer block (B) and melt-polymerizing the mixture. As a first specific example, a polyamide block copolymer may be produced by dry-blending a polymer constituting the polymer block (A), in which the terminal functional groups have been adjusted by melt polymerization in the presence of the terminal capping agent as necessary in the polymerization stage of the polymer block (A), with a polymer constituting the polymer block (B), in the presence of the terminal capping agent as necessary, and melt-kneading the mixture. As a second specific example, the polymer constituting the polymer block (A) may be reacted with the terminal functionalizing agent and / or the terminal capping agent as necessary, followed by pulverization to adjust the terminal functional groups of the polymer block (A), and then the polymer constituting the polymer block (B) may be added and dry-blended, and the mixture may be melt-polymerized. As a third specific example, the polymer constituting the polymer block (A) and, if necessary, the terminal functionalizing agent and / or the terminal capping agent may be charged from an upper hopper of a melt kneader and reacted, and then the polymer block (B) may be added from a side feed port downstream of the extruder, thereby performing melt extrusion polymerization in a stepwise manner.
[0076] As the polymerization method, methods such as melt polymerization, solid-phase polymerization, and melt extrusion polymerization can usually be adopted. The melt polymerization method or the melt extrusion polymerization method may be combined with the solid-phase polymerization method. As the melt extrusion polymerization method, a method of melt kneading using a single screw extruder, a twin screw extruder, a kneader, a Banbury mixer, or the like is preferably adopted. The melt kneading conditions are not particularly limited, but for example, a method of melt kneading for about 1 to 120 minutes at a temperature range of about 0 to 60° C. higher than the melting point of the polyamide is preferable from the viewpoint of making it easier to exhibit the effects of the present invention.
[0077] <Mass ratio (A) / (B)> In the polyamide block copolymer of this embodiment, the mass ratio (A) / (B) of the polymer block (A) to the polymer block (B) is preferably 1 / 99 to 99 / 1, more preferably 5 / 95 to 95 / 5, more preferably 10 / 90 to 95 / 5, even more preferably 20 / 80 to 95 / 5, even more preferably 40 / 60 to 90 / 10, even more preferably 50 / 50 to 85 / 15, and even more preferably 60 / 40 to 85 / 15. If the mass ratio (A) / (B) is within the above range, the polyamide block copolymer is preferred because it is easy to achieve both excellent heat resistance and flexibility.
[0078] <Polymer block content> The content of the polymer block (A) in 100% by mass of the total amount of the polyamide block copolymer is preferably 40% by mass or more, more preferably 45% by mass or more, even more preferably 46% by mass or more, and even more preferably 49% by mass or more or 50% by mass or more, from the viewpoint of obtaining a polyamide block copolymer having excellent physical properties such as tensile properties, etc. The content of the polymer block (A) in 100% by mass of the total amount of the polyamide block copolymer is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 88% by mass or less or 85% by mass or less, from the viewpoint of obtaining a polyamide block copolymer having excellent elongation. The content of the polymer block (B) in 100% by mass of the total amount of the polyamide block copolymer is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 12% by mass or more or 15% by mass or more, and in some cases may be 20% by mass or more or 25% by mass or more, from the viewpoint of obtaining a polyamide block copolymer having excellent physical properties such as tensile properties. The content of the polymer block (B) in 100% by mass of the total amount of the polyamide block copolymer is preferably 60% by mass or less, more preferably 55% by mass or less, even more preferably 54% by mass or less or 51% by mass or less, from the viewpoint of obtaining a polyamide block copolymer having excellent physical properties such as tensile properties. The total amount of polymer block (A) and polymer block (B) in the total amount of the polyamide block copolymer (100% by mass) is, for example, 50% by mass or more, 60% by mass or more, 70% by mass or more, or 80% by mass or more. From the viewpoint of obtaining a polyamide block copolymer having an excellent balance between strength and elongation, it is preferably 85% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more.
[0079] <Molecular weight of polyamide block copolymer> The number average molecular weight of the polyamide block copolymer is preferably 50,000 or less or 3,000 to 50,000, more preferably 3,000 to 40,000, even more preferably 4,000 to 30,000, even more preferably 4,500 to 25,000, and even more preferably 5,000 to 20,000. The higher the molecular weight, the better the heat resistance, but the molding processability tends to decrease. Within the above numerical range, the heat resistance of the polyamide block copolymer can be further improved and good molding processability can be expected. The weight average molecular weight of the polyamide block copolymer is preferably 500,000 or less or 30,000 to 500,000, more preferably 40,000 to 300,000, more preferably 50,000 to 280,000, even more preferably 75,000 to 250,000, and still more preferably 100,000 to 230,000, and may be 120,000 to 200,000. Within the above numerical ranges, the polyamide block copolymer can be expected to exhibit stronger material properties and have good moldability. The molecular weight distribution (weight average molecular weight / number average molecular weight) of the polyamide block copolymer is preferably 2.0 to 20.0, more preferably 3.0 to 17.0 or 3.0 to 15.0, and further preferably 3.5 to 14.0, 3.5 to 13.8, or 3.5 to 12.0. When the molecular weight distribution is within the above numerical range, the heat resistance of the polyamide block copolymer can be further improved and good moldability can be expected.
[0080] <Tensile strength and elongation at break of polyamide block copolymer> For the polyamide block copolymer of this embodiment, the tensile break strength measured in accordance with JIS K 7161-1:2014 is preferably 5 MPa or more, more preferably 10 MPa or more, even more preferably 20 MPa or more, still more preferably 30 MPa or more, and can also be 40 MPa or more. For the polyamide block copolymer of this embodiment, the tensile elongation at break measured in accordance with JIS K 7161-1:2014 is preferably 30% or more, more preferably 50% or more, even more preferably 100% or more, even more preferably 155% or more, even more preferably 200% or more, even more preferably 250% or more, and can even be 300% or more. It can be said that the larger the tensile elongation at break value, the more excellent the tensile properties of the polyamide block copolymer. More specifically, the tensile breaking strength and tensile breaking elongation can be determined by the method described in the examples below.
[0081] <Polyamide block copolymer composition> One embodiment of the present invention is a polyamide block copolymer composition containing the polyamide block copolymer. The polyamide block copolymer composition is produced by adding components other than the polyamide block copolymer to the polyamide block copolymer, such as additives such as antioxidants, antiozonants, weather stabilizers, UV absorbers, hydrolysis-resistant stabilizers, fillers, crystal nucleating agents, reinforcing agents, carbon black, pigments, inorganic dyes, organic dyes, colorants, color inhibitors, gelling inhibitors, matting agents, antistatic agents, plasticizers, lubricants, mold release agents, shrinkage resistance agents, compatibilizers, flame retardants, flame retardant assistants, and foaming agents. These may be contained alone or in combination of two or more kinds. The content of the additives is not particularly limited as long as it does not impair the effects of the present invention, but can be 0.02 to 200 parts by mass based on 100 parts by mass of the polyamide block copolymer. Examples of the method for adding the additives include a method of adding them during polymerization of the polyamide block copolymer, and a method of dry blending the additives with the polyamide block copolymer and melt kneading the mixture.
[0082] [Method of producing polyamide block copolymer composition] The method for producing the polyamide block copolymer composition is not particularly limited, and a method capable of uniformly mixing the polyamide block copolymer and the above-mentioned additives can be preferably adopted. The mixing is usually preferably performed by melt-kneading using a single-screw extruder, a twin-screw extruder, a kneader, a Banbury mixer, or the like. The melt-kneading conditions are not particularly limited, and examples thereof include a method of melt-kneading for about 1 to 120 minutes at a temperature range of about 0 to 60°C higher than the melting point of the polyamide block copolymer.
[0083] <Molded body> In one embodiment of the present invention, a molded article may be formed from the polyamide block copolymer or the polyamide block copolymer composition. The molded article of this embodiment can be used as various molded articles of any shape and purpose, including electric and electronic parts, automobile parts, industrial parts, fibers, films, sheets, household goods, and the like.
[0084] <Method of manufacturing molded body> The method for producing the molded product is not particularly limited, and examples thereof include various conventional molding methods, such as injection molding, blow molding, press molding, extrusion molding, calendar molding, vacuum molding, compressed air molding, bead molding, batch foam molding, etc. Examples of the form of the molded product include pellets, sheets, plates, pipes, tubes, rods, granules, and foams.
[0085] <Application> The polyamide block copolymer and polyamide block copolymer composition of this embodiment can be excellent in physical properties such as tensile properties, and can be used in a wide range of fields where such properties are required. For example, the polyamide block copolymer and polyamide block copolymer composition of this embodiment can be widely used as various parts materials such as electric and electronic parts, automobile parts, industrial material parts, industrial parts, daily necessities, household goods, sports parts, leisure parts, and medical parts. In particular, they can be applied as complex shaped parts by injection molding, hollow molded parts by blow molding, hose and tube shaped parts, films and sheets by extrusion molding, lightweight members and heat insulating materials by injection and / or extrusion foam molding, and additives for resin modification. They can also be applied as foams by injection molding, blow molding, press molding, extrusion molding, calendar molding, vacuum molding, compressed air molding, bead molding, or batch foam molding. More specifically, among electronic and electrical parts, it can be used as a material for the hinge parts of mobile phones and game machines, camera grips, printer tractor belts, electric wire coverings, tubes for home appliances, etc. More specifically, among automobile parts, the material can be used as a material for constant velocity joint boot parts, curl cords, airbag doors, hydraulic hoses, shift levers, cable liners, automobile belts, fuel tether caps, door locks, steering switches, seat locks, accelerator pedals, air ducts, airless tires, tire frames, tire inner liners, etc. More specifically, among industrial material parts and / or industrial parts, the material can be used as a material for submersible pumps, seal members, bushes, tubes, spiral tubes, diaphragms, mop joints, noiseless gears, mandrels, films, nonwoven fabrics, monofilaments, ball joint sheets, resistor rods, fire hoses, conveyor belts, pulleys, wire cables, etc. More specifically, among daily necessities and / or household goods, the material can be used as a material for hair dryer brushes, nail polish cases, hot curlers, zipper pulls, bobbin cases, console shutters, corrugated tubes, corrugated hoses, cushioning materials for pillows, cushioning materials for mattresses, cushioning materials for chairs, etc. More specifically, the material can be used for sports parts such as running shoes, spiked shoes, and ski boots. More specifically, among medical parts, the material can be used as a material for medical catheters, wearable devices, optical products, eye care parts, etc.
[0086] <Foam> One of the advantageous aspects of the above-mentioned molded article is a foam, and foam will now be described. The method for producing a foam includes, for example, the steps of (1) extrusion, (2) crosslinking, (3) foaming, (4) expansion process, and (5) molding. In the (1) extrusion step, mixing and kneading are performed as necessary. (2) Crosslinking is performed by at least one of chemical crosslinking and physical crosslinking. In the (3) foaming step, a foaming agent, for example, an organic foaming agent, or a supersaturated gas, preferably an inert gas, may be used, or both a foaming agent and a supersaturated gas may be used. (4) As the expansion process, free expansion may be performed, for example, in an oven, or limited expansion may be performed, for example, in a mold. (5) Molding may be performed in a batch system or a continuous system. Examples of molding methods include press molding, vacuum molding, embossing, and overinjection. The method for producing a foam is not limited to the above examples. To produce foams, any of the following processes may be used instead of or in addition to the above processes: injection molding, blow molding, extrusion molding, calendar molding, pressure molding, bead molding, batch foam molding, cutting, punching, scraping, and coating (e.g., adhesive coating, extrusion coating). Applications for the foam include soccer balls, sports glove pads (goalkeeper, boxing, etc. pads), immersion suits, golf club grips, rebound layers for table tennis rackets, ski poles, sports bat grips, snowboard or windsurfing pads, saddles (e.g. bicycle saddles), cushions (e.g. ski lift seat cushions, pillow cushions, mattress cushions, chair cushions, etc.), ski boot components; anti-slip coated tapes; underwear products (e.g. bra cups); mouse pads, soft keyboards, buttons; product trays (e.g. automotive product trays); gaskets; flexographic printing rolls; single-sided adhesive coated tapes, double-sided adhesive coated tapes; orthopedic insoles or inlays, footwear insoles or inner soles, footwear midsoles, footwear linings, waterproof, breathable insoles or inner soles, footwear shaft or heel inserts, forefoot inserts; transdermal pads, transdermal absorption pads, wound healing plasters; sportswear, and apparel linings. EXAMPLES
[0087] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these.
[0088] <Measurement and evaluation methods> Various physical properties were measured or evaluated by the following methods.
[0089] [Molecular weight] The semi-aromatic polyamides produced in the Synthesis Examples, the polyethers used as the polymer block (B), and the polyamide block copolymers obtained in the Examples and Comparative Examples were used as samples, and the number average molecular weight (Mn), weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn) were determined by gel permeation chromatography (GPC) in terms of standard polymethyl methacrylate. A 1,1,1,3,3,3-hexafluoroisopropanol (HFIP) solution in which sodium trifluoroacetate was dissolved at a ratio of 0.85 g per 1 kg of HFIP was used as the eluent. 1.5 mg of the sample was weighed out in terms of resin, dissolved in 3 mL of the eluent, and the eluent was passed through a 0.4 μm membrane filter to prepare a measurement sample. The measurement conditions were as follows: (Measurement conditions) Equipment: HLC-8320GPC (Tosoh Corporation) Column: Two TSK gel Super HM-H columns (Tosoh Corporation) were connected in series. Eluent: 0.085% by mass sodium trifluoroacetate / HFIP solution Flow rate: 0.5 mL / min (reference column: 0.25 mL / min) Sample injection volume: 30 μL Column temperature: 40℃ Standard polymethyl methacrylate: Shodex Standard M-75 (Showa Denko K.K.), Polymethlmethacrylate molecular weight 1010 and molecular weight 535 (Agilent Technologies Inc.) Detector: UV (254 nm) detector, UV (210 nm) detector
[0090] [Measurement of terminal amino group content ([NH2])] The semi-aromatic polyamide produced in the synthesis example was used as a sample, and 1 g of the sample was dissolved in 35 mL of phenol and mixed with 3 mL of methanol to prepare a sample solution. Using thymol blue as an indicator, titration was carried out using a 0.01 or 0.1 N HCl aqueous solution to measure the terminal amino group content ([NH2], unit: μmol / g).
[0091] [Measurement of terminal carboxyl group content ([COOH])] The semi-aromatic polyamide produced in the synthesis example was used as a sample, and 0.5 g of the sample was dissolved in 40 mL of ortho-cresol to prepare a sample solution. Using a potentiometric titrator, titration was carried out using a 0.01 or 0.1 N KOH / EtOH solution under the following measurement conditions to measure the terminal carboxyl group content ([COOH], unit: μmol / g). (Measurement conditions) Measuring device: MCU-710M / S (Kyoto Electronics Manufacturing Co., Ltd.) Measurement unit: AT-710 Main control unit: MCU-710 The terminal carboxyl group content ([COOH], unit: μmol / g) of adipic acid and terephthalic acid used as terminal functionalizing agents was calculated from the molecular weight based on the fact that one molecule has two carboxyl groups.
[0092] [Melting point] The semi-aromatic polyamides produced in the synthesis examples were used as samples, and their melting points were measured using a differential scanning calorimeter "DSC25" manufactured by TA Instruments. The melting point was measured in accordance with ISO11357-3 (2011, 2nd edition). Specifically, in a nitrogen atmosphere, the sample was heated from 30°C to 340°C at a rate of 10°C / min, held at 340°C for 5 minutes to completely melt the sample, and then cooled to 50°C at a rate of 10°C / min and held at 50°C for 5 minutes. The peak temperature of the melting peak that appeared when the temperature was raised again to 340°C at a rate of 10°C / min was taken as the melting point (°C). If there were multiple melting peaks, the peak temperature of the melting peak on the highest temperature side was taken as the melting point (°C).
[0093] [Tm0 (melting point), Tm1, Tm2, Tm2-Tm1] (1) Preparation of DSC curve The polyamide block copolymers obtained in the Examples and Comparative Examples were used as samples, and a DSC curve was created during the second heating run measured under the following condition A using a differential scanning calorimeter "DSC25" manufactured by TA Instruments. The DSC curve was created by plotting data obtained every 0.1 seconds. Condition A: In accordance with ISO11357-3 (2011, 2nd edition), the sample was heated from 30°C to 340°C at a rate of 10°C / min in a nitrogen atmosphere, held at 340°C for 5 minutes to completely melt the sample, then cooled to 50°C at a rate of 10°C / min and held at 50°C for 5 minutes. The temperature was then raised again to 340°C at a rate of 10°C / min. (2) Tm2-Tm1 In the DSC curve, the peak top temperature of the maximum endothermic peak was designated as Tm0 (melting point). Next, a straight line connecting two points, 50°C and 340°C, was designated as the baseline, and the distance of the line segment parallel to the vertical axis of the DSC curve graph, which connects the endothermic peak top to the baseline at the peak top temperature Tm0, was designated as L. A line segment parallel to the vertical axis of the DSC curve graph, which connects the DSC curve to the baseline and has a distance of (1 / 2)L, was identified, and the intersections of the line segment and the DSC curve (Q1 and Q2 shown in FIG. 1) were identified. The temperature of the DSC curve showing the heat quantity at the intersection point Q1 on the low temperature side was designated as Tm1, and the temperature of the DSC curve showing the heat quantity at the intersection point Q1 on the high temperature side was designated as Tm2, and (Tm2-Tm1) was calculated.
[0094] [Tensile strength and elongation at break] The polyamide block copolymers obtained in the examples and comparative examples were melt-kneaded for 3 minutes at a cylinder temperature 20°C higher than the melting point of the polyamide block copolymer using a benchtop small kneader / injection molding machine ("Xplore MC15") manufactured by Xplore Instruments, and then small test pieces type 1BA (2 mm thick, total length 75 mm, parallel part width 5 mm) for tensile evaluation were prepared under the conditions of a mold temperature of 140°C for the T-runner mold of the injection molding machine and an injection pressure of 1.0 bar. The small test pieces type 1BA of the obtained polyamide block copolymer were left to stand in a dryer at 140°C for 6 hours, and then the tensile breaking strength and tensile breaking elongation were measured at 23°C in accordance with JIS K 7161-1:2014 using an Instron universal testing machine "5566 type" manufactured by Instron. Specifically, the chuck distance was 50 mm, and the test speed was 0.25 mm / min in the region of 0 to 0.3% strain, and then the test speed was 50 mm / min in the region of 0.3% strain or more. The tensile breaking elongation was the nominal strain value according to Method A of JIS K 7161-1:2014.
[0095] <Each material> The materials used in the examples and comparative examples are as follows.
[0096] <Polymer block (A)> As the constituent elements of the polymer block (A), PA-1 to PA-4 produced in the following synthesis examples were used.
[0097] [Synthesis Example 1] Manufacturing of semi-aromatic polyamide (PA-1) 1017.6g (6.13 mol) of terephthalic acid, 988.2g (6.24 mol) of a mixture of 1,9-nonanediamine (C9DA in Table 3) / 2-methyl-1,8-octanediamine (MC8DA in Table 3) (molar ratio 50 / 50), 18.2g (0.15 mol) of benzoic acid, 2.0g of sodium hypophosphite monohydrate (0.1% by mass relative to the total mass of the raw materials) and 788mL of distilled water were placed in an autoclave with an internal volume of 5L and substituted with nitrogen. The mixture was stirred at 100°C for 30 minutes, and the temperature inside the autoclave was raised to 220°C over 3 hours. At this time, the pressure inside the autoclave was raised to 2.0MPa. Heating was continued for 2 hours while maintaining the pressure at 2.0MPa, and the water vapor was gradually removed to cause the reaction. The reaction was continued for another hour to obtain a prepolymer that is a semi-aromatic polyamide. The obtained prepolymer was dried at 120°C under reduced pressure for 24 hours and pulverized to a particle size of 1 mm or less. This prepolymer is abbreviated as "PA-1". The semi-aromatic ratio (unit: %) is shown in Table 1.
[0098] [Synthesis Example 2] Manufacturing of semi-aromatic polyamide (PA-2) 1015.6g (6.11 mol) of terephthalic acid, 988.2g (6.24 mol) of a mixture of 1,9-nonanediamine / 2-methyl-1,8-octanediamine (molar ratio 80 / 20), 21.2g (0.17 mol) of benzoic acid, 2.0g of sodium hypophosphite monohydrate (0.1% by mass relative to the total mass of the raw materials) and 788mL of distilled water were placed in an autoclave with an internal volume of 5L and substituted with nitrogen. The mixture was stirred at 100°C for 30 minutes, and the temperature inside the autoclave was raised to 220°C over 3 hours. At this time, the pressure inside the autoclave was raised to 2.0MPa. Heating was continued for 2 hours while maintaining the pressure at 2.0MPa, and the water vapor was gradually removed to cause the reaction. The reaction was continued for another 1 hour to obtain a prepolymer which is a semi-aromatic polyamide. The obtained prepolymer was dried at 120°C under reduced pressure for 24 hours and pulverized to a particle size of 1mm or less. This prepolymer is abbreviated as "PA-2." The semi-aromatic ratio is shown in Table 1.
[0099] [Synthesis Example 3] Manufacturing of semi-aromatic polyamide (PA-3) 836.7g (3.87 mol) of 2,6-naphthalenedicarboxylic acid, 637.6g (4.03 mol) of a mixture of 1,9-nonanediamine / 2-methyl-1,8-octanediamine (molar ratio 85 / 15), 31.8g (0.26 mol) of benzoic acid, 1.5g of sodium hypophosphite monohydrate (0.1% by mass relative to the total mass of the raw materials) and 677mL of distilled water were placed in an autoclave with an internal volume of 5L and substituted with nitrogen. The mixture was stirred at 100°C for 30 minutes, and the temperature inside the autoclave was raised to 220°C over 3 hours. At this time, the pressure inside the autoclave was raised to 2.0MPa. Heating was continued for 2 hours while maintaining the pressure at 2.0MPa, and the water vapor was gradually removed to cause the reaction. The reaction was continued for another hour to obtain a prepolymer that is a semi-aromatic polyamide. The obtained prepolymer was dried at 120°C under reduced pressure for 24 hours and pulverized to a particle size of 1 mm or less. This prepolymer is abbreviated as "PA-3". The semi-aromatic ratio is shown in Table 1.
[0100] [Synthesis Example 4] Manufacturing of semi-aromatic polyamide (PA-4) 193.5g (1.17 mol) of terephthalic acid, 8.96g (0.06 mol) of adipic acid, 197.5g (1.25 mol) of a mixture of 1,9-nonanediamine / 2-methyl-1,8-octanediamine (molar ratio 50 / 50), 3.7g (0.03 mol) of benzoic acid as an end-capping agent, 0.4g of sodium hypophosphite monohydrate (0.1% by mass relative to the total mass of the raw materials), and 158mL of distilled water were placed in an autoclave with an internal volume of 1L and substituted with nitrogen. The mixture was stirred at 100°C for 30 minutes, and the temperature inside the autoclave was raised to 220°C over 3 hours. At this time, the pressure inside the autoclave was raised to 2.0MPa. Heating was continued for 2 hours while maintaining the pressure at 2.0MPa, and the water vapor was gradually removed to cause the reaction. The reaction was further allowed to proceed for 1 hour to obtain a prepolymer. The obtained prepolymer was dried at 120°C under reduced pressure for 24 hours and pulverized to a particle size of 1 mm or less. This prepolymer is abbreviated as "PA-4". The semi-aromatic ratio is shown in Table 1. The semi-aromatic ratio is shown in Table 1.
[0101] [End functionalizing agent] In addition, the following dicarboxylic acid monomer was used as a terminal functionalizing agent as a component of the polymer block (A). It was confirmed that the terminal amino groups of the semi-aromatic polyamide were quantitatively converted to carboxyl groups by the terminal functionalizing agent (dicarboxylic acid monomer). Terephthalic acid (abbreviated as "TA" in Table 3): manufactured by Tokyo Chemical Industry Co., Ltd. Adipic acid (abbreviated as "AA" in Table 3): manufactured by Tokyo Chemical Industry Co., Ltd.
[0102] The above-mentioned various physical property evaluations were carried out for PA-1 to PA-4. The results are shown in Tables 1 and 3 together with the physical properties of the terminal functionalizing agent. The notations in Table 1 are as follows: "n / i" indicates the molar ratio of 1,9-nonanediamine / 2-methyl-1,8-octanediamine. "[NH2]" indicates the terminal amino group content. "[COOH]" indicates the terminal carboxyl group content.
[0103] [Table 1]
[0104] <Polymer block (B)> As the polymer block (B), the following oxygen atom-containing polymer was used. [Polyether] PE-1: Polyether diamine (diamine of polyethylene glycol and polypropylene glycol copolymer), manufactured by Sigma-Aldrich, Jeffamine® ED-900 PE-2: Polyether diamine (polyoxytetramethylene diamine), manufactured by Koei Chemical Co., Ltd., PTMGPA-1000 PE-3: Polyetherdiamine (polyoxyethylenediamine), manufactured by Koei Chemical Co., Ltd., PEGPA-1000
[0105] The physical properties of the polymer block (B) are shown in Table 2. The notations in Table 2 are as follows: "[NH2]" indicates the terminal amino group content. "Tg" indicates the glass transition temperature measured by the following [Method of measuring glass transition temperature]. Note that "<-70" indicates that the glass transition temperature was below -70°C because no inflection point could be confirmed in the range of -70°C or higher, which is the measurement limit of the device. In addition, glass transition temperatures (based on literature values) for corresponding polyether diols are also shown in Table 2 as reference values. "~-70" indicates a range of -80 to -60°C, and "~-85" indicates a range of -95 to -75°C. [Method of measuring glass transition temperature] The polymer block (B) was used as a sample, and the glass transition temperature of each sample was measured using a differential scanning calorimeter "DSC25" manufactured by TA Instruments. The glass transition temperature (°C) was determined by cooling the sample from 25°C to -90°C at a rate of 2°C / min under a nitrogen atmosphere, holding the sample at -90°C for 10 minutes to allow the sample to cool completely, and then heating the sample to 25°C at a rate of 2°C / min.
[0106] [Table 2]
[0107] <Example 1> The raw materials used in the reaction were used in the mass ratios shown in Table 3, and the reaction was carried out. Specifically, "PA-1" of Synthesis Example 1 and adipic acid as a terminal functionalizing agent were added to a flask with an internal volume of 200 mL equipped with an apparatus capable of distilling off the generated volatile components and a vacuum pump, and the temperature was raised to 280°C while stirring under a nitrogen gas flow of 200 mL / min, and the temperature was maintained for 30 minutes. Then, "PE-1" was added, and the mixture was stirred for another hour at a resin temperature of 280°C, and the distillate was removed. Then, the reaction system was depressurized to 10 Pa, and the mixture was stirred for another hour at a resin temperature of 280°C, and the polyamide block copolymer was taken out. To explain the mass ratio (A) / (B) shown in Table 3 as an example, in Example 1, it means that 68 parts by mass (e.g., 68.5 g) of polyamide PA-1 functionalized with a terminal functionalizing agent was used with 32 parts by mass (e.g., 31.5 g) of polyether PE-1.
[0108] <Examples 2 to 5> The same procedure as in Example 1 was carried out except that the materials and mass ratios were changed as shown in Table 3, to obtain a polyamide block copolymer.
[0109] <Comparative Example 1> The raw materials used in the reaction were used in the mass ratios shown in Table 3, and the reaction was carried out. Specifically, 448.6 g (2.70 mol) of terephthalic acid, 900.0 g (0.9 mol) of "PE-2", 238 mL of distilled water, and 1.6 g of sodium hypophosphite monohydrate (0.1% by mass relative to the total mass of the raw materials) were stirred at room temperature in a glass beaker with an internal volume of 5 L until the mixture was homogenized. Subsequently, 284.9 g (1.80 mol) of a mixture of 1,9-nonanediamine / 2-methyl-1,8-octanediamine (molar ratio 70 / 30) and 171 mL of distilled water were added to the mixture, and stirring was continued. Then, a homogenous salt was obtained from the reaction liquid. The obtained salt was placed in an autoclave with an internal volume of 5 L and substituted with nitrogen. The mixture was stirred at 100°C for 30 minutes, and the temperature inside the autoclave was raised to 245°C over 3 hours. At this time, the pressure inside the autoclave was raised to 3.0 MPa. Heating was continued for 2 hours, then cooled, the reaction product was removed from the autoclave, dried at 120°C under reduced pressure for 24 hours, and pulverized to a particle size of 1 mm or less. 40 g of the pulverized product was transferred to a 200 mL flask and heated to a resin temperature of 300°C while stirring under a nitrogen gas flow of 200 mL / min. The reaction system was depressurized to 10 Pa, and stirred for 3 hours at a resin temperature of 300°C, after which the polyamide block copolymer was removed.
[0110] The polyamide block copolymers obtained in the above Examples and Comparative Examples were used to evaluate various physical properties. The results of the physical property evaluation are shown in Table 3.
[0111] [Table 3]
[0112] The results in Table 3 show that the polyamide block copolymers obtained in Examples 1 to 6 have excellent tensile properties. On the other hand, the polyamide block copolymer obtained in Comparative Example 1 had a large Tm2-Tm1 value, and thus had inferior tensile properties to the Examples. From these results, it is considered important that the endothermic peak shape is sharp and Tm2-Tm1 shows a specific range in order to exhibit excellent tensile properties. [Industrial Applicability]
[0113] The polyamide block copolymer of this embodiment has excellent physical properties such as tensile properties. Therefore, the polyamide block copolymer and polyamide block copolymer composition of this embodiment can be widely used as various parts materials such as electric and electronic parts, automobile parts, industrial material parts, industrial parts, daily necessities, clothing, household parts, sports parts, leisure parts and medical parts. In particular, it can be applied to complex shaped parts by injection molding, hollow molded parts by blow molding, hose and tube shaped parts and films and sheets by extrusion molding, lightweight members and heat insulating materials by injection and / or extrusion foam molding, and additives for resin modification. It can also be applied to foams by injection molding, blow molding, press molding, extrusion molding, calendar molding, vacuum molding, compressed air molding, bead molding or batch foam molding.
Claims
1. The polymer block (A) contains 50 mol % or more of a structural unit derived from a semi-aromatic polyamide, and the polymer block (B) has a glass transition temperature of 20° C. or lower, In a DSC curve measured using a differential scanning calorimeter in accordance with ISO 11357-3 (2011, 2nd edition), the temperature was increased from 50 ° C. to 340 ° C. at a rate of 10 ° C. / min. The maximum endothermic peak temperature (Tm0) is within the range of 70 to 320°C, A polyamide block copolymer, which satisfies the relationships of the following formulas (1) to (3), when a straight line connecting two points, 50° C. and 340° C., in the DSC curve is defined as a baseline, and a distance of a line segment connecting a top of an endothermic peak at the maximum endothermic peak temperature (Tm0) to the baseline is defined as L: Formula (1): Tm1 < Tm0 Formula (2): Tm2>Tm0 Formula (3): (Tm2-Tm1)≦35 Where: The Tm1 (° C.) is a temperature that satisfies formula (1), and the distance of a line segment that connects the DSC curve at Tm1 (° C.) to the baseline is (½)L. The Tm2 (° C.) is a temperature that satisfies formula (2), and the distance of a line segment that connects the DSC curve at Tm2 (° C.) to the baseline is (½)L.
2. The polyamide block copolymer according to claim 1 , wherein the polymer block (B) contains 50 mol % or more of a structural unit derived from a polymer having an amino group or a carboxyl group as a terminal group.
3. 2. The polyamide block copolymer according to claim 1, wherein the polymer block (B) contains 50 mol % or more of structural units derived from a polyether polyol, an amine derivative thereof, or a carboxyl derivative thereof.
4. The polyamide block copolymer according to claim 1, having a tensile elongation at break measured in accordance with JIS K 7161-1:2014 of 30% or more.
5. The polyamide block copolymer according to claim 1, wherein the semi-aromatic polyamide comprises a diamine unit mainly composed of a structural unit derived from at least one aliphatic diamine selected from the group consisting of a linear aliphatic diamine and a branched aliphatic diamine, and a dicarboxylic acid unit mainly composed of a structural unit derived from an aromatic dicarboxylic acid.
6. The polyamide block copolymer according to claim 5, wherein the semi-aromatic polyamide contains 30 mol% or more of structural units derived from an aliphatic diamine having 4 to 18 carbon atoms relative to all diamine units.
7. The polyamide block copolymer according to claim 1, wherein the semi-aromatic polyamide contains structural units derived from at least one aliphatic diamine selected from the group consisting of 1,9-nonanediamine and 2-methyl-1,8-octanediamine.
8. The polyamide block copolymer according to claim 1, wherein the semi-aromatic polyamide comprises a structural unit derived from at least one aromatic dicarboxylic acid selected from the group consisting of terephthalic acid, 1,4-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and 2,7-naphthalenedicarboxylic acid.
9. The polyamide block copolymer according to claim 1, wherein the polymer block (A) has a number average molecular weight of 300 to 12,000.
10. The polyamide block copolymer according to claim 1, wherein the weight average molecular weight of the polymer block (A) is 1,000 to 50,000.
11. The polyamide block copolymer according to claim 1, wherein the molecular weight distribution (weight average molecular weight / number average molecular weight) of the polymer block (A) is 1.5 to 10.
0.
12. The polyamide block copolymer according to claim 1, wherein the molecular weight distribution (weight average molecular weight / number average molecular weight) of the polyamide block copolymer is 2.0 to 20.
0.
13. A polyamide block copolymer composition comprising the polyamide block copolymer according to any one of claims 1 to 12.
14. A molded article formed from the polyamide block copolymer according to any one of claims 1 to 12.
15. A molded article formed from the polyamide block copolymer composition according to claim 13.
Citation Information
Patent Citations
Production of polyether ester amide block copolymer
JP1987246930A
Production of polyether nylon
JP1996208833A
Polyamide block copolymer and preparation thereof
JP2000154248A
Flexible polyamide
WO2020085360A1
Cited By
Adjustable knotless loops
US12303122B2
Method and apparatus for soft tissue fixation
US12329373B2
Method and apparatus for soft tissue fixation
US12336701B2
Method and apparatus for coupling anatomical features
US12419632B2
Polyamide block copolymer, polyamide block copolymer composition, molded body and various products containing same, and method for producing polyamide block copolymer
WO2026155181A1