Poly-arm-type resin having polyamide structure or heterocyclic structure, lithography film-forming composition containing the same, and production method

A multibranched resin with a polyamide or heterocyclic structure is created by condensing specific compounds, addressing PBO's solubility and film-forming issues, resulting in improved lithography performance and optical applications.

JP2024159726APending Publication Date: 2024-11-08KANSAI UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024072452
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-26
Publication Date
2024-11-08

Smart Images

  • Figure 2024159726000039
    Figure 2024159726000039
  • Figure 2024159726000040
    Figure 2024159726000040
  • Figure 2024159726000041
    Figure 2024159726000041
Patent Text Reader

Abstract

To provide a resin with excellent film-forming properties.SOLUTION: A poly-arm-type resin having a polyamide structure is produced by a method comprising: (I) a step for preparing a diamino compound represented by formula (A) and a tricarboxylic acid-based compound represented by formula (B) (in the formulae, Y represents an alkylene group optionally having a fluorine atom, Z's independently represent -OH, -SH, or -NH2, E represents -COOH, -COHal (Hal is a halogen atom) or the like; and (II) a step for causing a condensation reaction in these compounds to form a polyamide structure.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hyperbranched resin having a polyamide structure or a heterocyclic structure, a lithography film-forming composition containing the same, and a production method. [Background technology]

[0002] Polybenzoxazole (PBO) resins have excellent heat resistance, chemical resistance, and mechanical properties, and are therefore expected to be used in a variety of applications. However, because the resins have a rigid structure, they are poor in solubility and film-forming properties. Therefore, PBOs with branched chains have been proposed (e.g., Non-Patent Document 1). [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] Hiroto Kudo et. al., Journal of Polymer Science Part A Polymer Chemistry 44(11):3640 - 3649 (2006). Summary of the Invention [Problem to be solved by the invention]

[0004] The resin described in Non-Patent Document 1 is amorphous and soluble in a solvent. However, there is room for improvement in terms of film-forming properties. In view of the above circumstances, an object of the present invention is to provide a resin with excellent film-forming properties. [Means for solving the problem]

[0005] The inventors have found that a resin having a group with a specific structure introduced therein can solve the above problems. Aspect 1 (I) preparing a diamino compound represented by formula (A) described below and a tricarboxylic acid compound represented by formula (B) described below; (II) condensation reaction of these compounds to form a polyamide structure; Manufactured by a method comprising: A hyperbranched resin with a polyamide structure. Aspect 2 2. The resin according to embodiment 1, wherein Y in the formula is a branched alkylene group. Aspect 3 3. The resin of any one of the preceding claims, wherein Y is a fluorinated alkylene group. Aspect 4 (i) preparing a hyperbranched resin having a polyamide structure according to any one of aspects 1 to 3; and (ii) intramolecularly condensing the resin to form a heterocyclic structure; Manufactured by a method comprising: A hyperbranched resin with a heterocyclic structure. Aspect 5 There are units in which Y is an alkylene group and units in which Y is a fluorinated alkylene group, The resin according to embodiment 4, wherein the molar ratio of the alkylene groups to the fluorinated alkylene groups is 1:(1.5 to 10). Aspect 6 A lithographic film-forming composition comprising the resin according to any one of the first to fifth aspects. Aspect 7 A lithographic underlayer film-forming composition comprising the resin according to embodiment 3. Aspect 8 8. The composition of embodiment 6 or 7, comprising a solvent. Aspect 9 The composition of any one of embodiments 6 to 8, comprising a component selected from the group consisting of a solvent, an acid generator, an acid crosslinker, and combinations thereof. Aspect 10 A lithographic underlayer film formed using the composition of embodiment 7. Aspect 11 A lithographic underlayer film comprising a resin according to embodiment 4 or 5. Aspect 12 forming an underlayer film on a substrate using the composition according to embodiment 7, and heating the precursor to 300° C. or higher to form an underlayer film containing a hyperbranched resin having a heterocyclic structure; forming at least one photoresist layer on the underlayer film; and exposing predetermined areas of the photoresist layer to radiation and developing; A method for forming a resist pattern comprising the steps of: Aspect 13 A hyperbranched resin having a polyamide structure represented by the formula (1) described below. Aspect 14 A hyperbranched resin having a heterocyclic structure, represented by the formula (2) described below. Aspect 15 The resin according to embodiment 13 or 14, wherein X in the formula is represented by any of formulas (X1) to (X4) described below. Effect of the Invention

[0006] It is possible to provide a resin with excellent film-forming properties. [Brief description of the drawings]

[0007] [Figure 1A] 1H-NMR and 13C-NMR spectra of tricarboxylic acids (esters) [Figure 1B] FT-IR spectrum of tricarboxylic acid (ester) [Diagram 2] 1H-NMR spectra of tricarboxylic acid compounds [Figure 3A] 1H-NMR spectrum of hyperbranched PA resin [Figure 3B] GPC chart of hyperbranched PA resin [Figure 4] 1H-NMR and 13C-NMR spectra of tricarboxylic acid compounds [Figure 5A] 1H-NMR spectrum of hyperbranched PA resin [Figure 5B] GPC chart of hyperbranched PA resin [Figure 5C] TGA (thermogravimetric analysis) chart of hyperbranched PA resin [Figure 6] GPC chart of hyperbranched PA resin [Figure 7A] GPC chart of hyperbranched PA resin [Figure 7B] FT-IR spectrum of hyperbranched PA resin [Figure 8A] FT-IR spectrum of hyperbranched PBO resin [Figure 8B] TGA (thermogravimetric analysis) chart of hyperbranched PBO resin [Figure 9] 1H-NMR spectrum of hyperbranched PA resin (protected and unprotected) [Figure 10] FT-IR spectrum of hyperbranched PA resin (protected and unprotected) DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1. Hyperbranched resin with polyamide structure In one embodiment, the hyperbranched resin having a polyamide structure is obtained by reacting a diamino compound represented by formula (A) with a tricarboxylic acid compound represented by formula (B). The hyperbranched resin is a resin having a branched chain bonded to the main chain, and the branched chain is not so long as to form a gel. In the present disclosure, "X to Y" include the end values.

[0009] (1)(A) Diamino compound The diamino compound represented by formula (A) (hereinafter also referred to as "compound A") is a compound essentially containing two amino groups. The amino groups are preferably primary amino groups. In addition to the two amino groups, compound A has a group Z. The group Z is selected from the group consisting of -OH, -SH, -NH2, and combinations thereof.

[0010] [ka]

[0011] Y is an alkylene group which may contain fluorine. Examples of Y include an alkylene group having 1 to 6 carbon atoms and a fluorinated alkylene group having 1 to 6 carbon atoms. The number of carbon atoms in these groups is more preferably 1 to 3. Y is preferably a branched alkylene group or a branched fluorinated alkylene group. From the viewpoint of availability, etc., Y is preferably -CH2-, -CH(CH3)-, -C(CH3)2-, -CH(CF3)-, -C(CF3)2-, etc.

[0012] Z is independently -OH, -SH, or -NH2. Among them, from the viewpoint of solubility in a solvent or easy availability of a polyamide structure-containing multi-branched resin, Z is preferably -OH.

[0013] R is each independently a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 40 carbon atoms which may have a substituent, an aralkyl group having 7 to 40 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an arylalkenyl group having 7 to 40 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, a halogen atom, a nitro group, an amino group, a cyano group, a carboxylic acid group, a thiol group, or a hydroxyl group. The aryl group, aralkyl group, alkenyl group, alkynyl group, and arylalkenyl group may contain an ether bond, a ketone bond, an ester bond, or a urethane bond. However, in consideration of heat resistance, etc., R is preferably a hydrogen atom.

[0014] m, when R is a group other than hydrogen, is the number of such groups and is an integer of 1 to 3. When R is a group other than hydrogen, in consideration of heat resistance, etc., m is preferably 1. Examples of preferred embodiments of compound A are shown below.

[0015] [ka]

[0016] (2)(B) Tricarboxylic acid compounds The tricarboxylic acid compound represented by formula (B) (hereinafter also referred to as "compound B") is a compound having three carboxyl groups or derivative groups thereof. The derivative groups are preferably acid halide groups.

[0017] [ka]

[0018] Ar is a group having an aromatic group, including, but not limited to, an aryltriyl group obtained by removing three hydrogen atoms from an aromatic compound, or a group obtained by removing three hydrogen atoms from the aromatic ring of a triarylalkane.

[0019] E is -COOH, -COHal, -OR b -COOH or -OR b -COHal. Hal is a halogen atom, preferably a chlorine atom. b is an alkylene group having 1 to 6 carbon atoms, and preferably an alkylene group having 1 to 3 carbon atoms. More preferably, R b is a methylene group or an ethylene group. Preferred embodiments of compound B are exemplified below.

[0020] [ka]

[0021] (3) Structure The resin (hereinafter, for convenience, also referred to as "hyperbranched PA resin") is obtained by a condensation reaction between compound A and compound B. The reaction produces an amide bond, resulting in a polymer having a polyamide structure. The structure of the hyperbranched PA resin is represented as follows:

[0022] [ka]

[0023] In the formula, Y, Z, R, and m are defined as above. n is the number of repetitions in the main chain, and r is the number of repetitions in the branched chain, where n>r. n is not limited, but is preferably 1 to 100, more preferably 2 to 30. If r is too large, gelation occurs, and if r is too small, solubility in the solvent decreases. r is selected so that the hyperbranched PA resin does not gel and exhibits solubility. In one embodiment, r can be about 10 to 60% of n.

[0024] The group Z of the hyperbranched PA resin represented by formula (1) may be a group protected by a protecting group. That is, the hyperbranched PA resin represented by formula (1) can be represented by formula (1-1) in a preferred embodiment.

[0025] [ka]

[0026] In formula (1-1), Z1 is -OH, -SH, -NH2, or a group in which these are protected by a protecting group, and Y, Z, R, m, n, and r are defined as above. In this specification, a protecting group refers to a group that dissociates under specific conditions, and is also called a dissociable group. From the viewpoint of solubility, Z1 is preferably a group in which -OH, -SH, and -NH2 are protected by a protecting group. A resin having such a group is excellent as a lithography material because it has improved solubility in, for example, PGMEA and PGME, which are solvents frequently used in lithography applications. The protecting group is preferably an acid-dissociable group that dissociates in the presence of an acid.

[0027] A preferred example of the group protected by the protecting group is a group in which a hydroxy group is protected by an acid-dissociable group. The acid-dissociable group is not particularly limited, but can be appropriately selected from those proposed in, for example, hydroxystyrene-based resins and (meth)acrylic acid-based resins used in chemically amplified resist compositions for KrF and ArF. Not particularly limited, examples include substituted methyl groups, 1-substituted ethyl groups, 1-substituted n-propyl groups, 1-branched alkyl groups, silyl groups, acyl groups, 1-substituted alkoxymethyl groups, cyclic ether groups, alkoxycarbonyl groups, and alkoxycarbonylalkyl groups.

[0028] Specific examples of the acid-dissociable group include those described in WO 2016 / 158168. Among these acid-dissociable groups, from the viewpoint of high resolution, an acid-dissociable group selected from the group consisting of groups represented by the following formulas is particularly preferred.

[0029] [ka]

[0030] In the above formula, R 5 is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, R 6 is a hydrogen atom, a linear or branched alkyl group having 1 to 4 carbon atoms, a cyano group, a nitro group, a heterocyclic group, a halogen atom, or a carboxyl group, and n 11 is an integer between 0 and 4, n 12 is an integer between 1 and 5, n 10 is an integer between 0 and 4. 7 is a C1-6 alkyl group, a C6-11 aryl group, or a C7-12 alkaryl group.

[0031] (4)Characteristics The hyperbranched PA resin has flexibility due to the presence of Y, and has a moderately low density due to the branched chain. Therefore, it has good solubility in a solvent and good film-forming properties. Furthermore, when part or all of Y is a fluorinated alkylene group, the density of the resin is appropriately reduced and the solubility is further increased, which is preferable. Furthermore, when part or all of Y is a fluorinated alkylene group, deterioration of the resin can be avoided when the hyperbranched PA resin is subjected to intramolecular condensation. When there are units in which Y is an alkylene group and units in which Y is a fluorinated alkylene group, the molar ratio of the alkylene group to the fluorinated alkylene group is preferably 1:(1.5-10), more preferably 1:(2-6).

[0032] The resin is useful as a lithography material. In addition, since the resin has a high refractive index, it is also useful as an optical component. Furthermore, since the amino group reacts with Z to form a ring, the hyperbranched PA resin can be converted into a resin having a heterocyclic structure. The resin having a heterocyclic structure has extremely high heat resistance and is useful as a lithography film, especially a lithography underlayer film.

[0033] 2. Manufacturing method of hyperbranched PA resin The hyperbranched PA resin is obtained by condensing compound A and compound B. The charge ratio is selected so as to produce a desired molecular weight and branched chain. The charge ratio of the two can be determined as the ratio of functional group equivalents forming an amide bond. The functional group equivalent ratio (functional group equivalent of compound A: functional group equivalent of compound B) is preferably (1-2):1, more preferably (1.1-1.6):1. The reaction temperature is selected so as not to produce a gel, and is 20-40°C in one embodiment. The reaction time is not limited, and can be, for example, about 20-72 hours.

[0034] If the amount of the solvent is small, gel is easily formed, and if it is large, the production efficiency decreases. In one embodiment, the amount of the solvent is 8 to 10 parts by weight per 1 part by weight of the total amount of the compounds A and B. The solvent is preferably an aprotic solvent such as NMP (N-methylpyrrolidone) or DMF (dimethylformamide). The reaction is preferably carried out under an inert atmosphere. In addition, a known condensing agent can also be used for the condensation reaction.

[0035] 3. Hyperbranched resin with heterocyclic structure The resin (hereinafter, for convenience, also referred to as "multi-branched heterocyclic resin") is obtained by intramolecular condensation reaction of multi-branched PA resin. Through this reaction, the amino group and Z or Z1 form a heterocyclic structure. When Z1 is a group protected by a protecting group, the heterocyclic structure is formed through a deprotection reaction. As described above, it is preferable that a part or all of Y is a fluorinated alkylene group. When there are units in which Y is an alkylene group and units in which Y is a fluorinated alkylene group, the molar ratio of the alkylene group:fluorinated alkylene group is preferably 1:(1.5-10), more preferably 1:(2-6). The structure of the resin is preferably represented as follows:

[0036] [ka]

[0037] Y 1 and Y 2 Y comes from the hyperbranched PA resin Y. 1 is a fluorinated alkylene group, Y 2 is an alkylene group. The alkylene group is as explained in the description of the hyperbranched PA resin.

[0038] Z' is derived from Z or Z1 of the hyperbranched PA resin. Z' is independently -O-, -S-, or -NH-. From the viewpoint of ease of synthesis, Z' is preferably -O-. In this case, the heterocycle is a benzoxazole ring, and the resin in this case is also called a "hyperbranched PBO resin."

[0039] X is a group having an aromatic group derived from Ar of the hyperbranched PA resin. X is preferably a group represented by the following formula:

[0040] [ka]

[0041] Ar is an aromatic group, as explained for the hyperbranched PA resin. b is an alkylene group having 1 to 6 carbon atoms, and the preferred embodiments are as explained for the hyperbranched PA resin.

[0042] R and m are as explained for the hyperbranched PA resin.

[0043] n 1 and n 2 is the repeat number in the main chain. r 1 and r 2 is the number of repeats in the branched chain. 1 >r 1 And 2 >r 2 n 1 and n 2 The sum of these corresponds to n of the hyperbranched PA resin, and r 1 and r 2 The sum of these corresponds to the r of the hyperbranched PA resin. 1 :n 2 and r 1 :r 2 The ratio of Y 1 :Y 2 For example, when the hyperbranched PA resin does not contain a fluorinated alkylene as Y, the ratio of n 1 and r 1 is 0. In one embodiment, r 1 andr 2 The sum of n 1 and 2 This may be approximately 10 to 60% of the total.

[0044] 4. Manufacturing method of hyperbranched heterocyclic resin The resin is produced by a method including the steps of (i) preparing a hyperbranched PA resin, and (ii) intramolecularly condensing the resin to form a heterocyclic structure. Step (i) is as described above. Step (ii) can be carried out by heating the hyperbranched PA resin to 250°C or higher. The temperature is preferably 300 to 320°C. The step is preferably carried out in an inert atmosphere.

[0045] The hyperbranched heterocyclic resin has extremely high chemical resistance, so it is preferable to cast the precursor hyperbranched PA resin into a desired shape (such as a membrane) and carry out this step in that state.

[0046] 5. Composition [Composition] The hyperbranched resin is suitable for lithography or optical article applications, and is therefore useful in compositions for such applications.

[0047] [Lithography film-forming composition] The lithography film-forming composition is a composition containing the hyperbranched resin as an essential component, and preferably contains a solvent. The composition is capable of reducing film defects (forming a thin film), has good storage stability, has high sensitivity, a high refractive index in a specific wavelength region, and has heat resistance and chemical resistance, and can provide a good resist pattern shape. From the viewpoint of solubility in a solvent, the hyperbranched resin is preferably a hyperbranched PA resin.

[0048] (Physical properties of lithography film-forming composition, etc.) The composition can be used to form an amorphous film by a known method such as spin coating. Depending on the type of developer used, either a positive resist pattern or a negative resist pattern can be produced. The following describes the use of the composition as a resist composition.

[0049] When the lithography film-forming composition is a positive resist pattern, the dissolution rate of the amorphous film formed by spin coating in a developer at 23°C is preferably 5 Å / sec or less, more preferably 0.0005 to 5 Å / sec, and even more preferably 0.05 to 5 Å / sec. If the dissolution rate is 5 Å / sec or less, the resist can be insoluble in the developer. If the dissolution rate is 0.0005 Å / sec or more, the resolution may be improved. This is presumably because the contrast at the interface between the exposed part that dissolves in the developer and the unexposed part that does not dissolve in the developer increases due to the change in solubility of the resin before and after exposure. In addition, there is an effect of reducing line edge roughness and reducing defects.

[0050] When the lithography film-forming composition is a negative resist pattern, the dissolution rate of the amorphous film formed by spin coating in a developer at 23°C is preferably 10 Å / sec or more. When the dissolution rate is 10 Å / sec or more, the film is easily soluble in the developer, and is more suitable for resist. When the dissolution rate is 10 Å / sec or more, the resolution may be improved. This is presumably because the micro surface portion of the resin dissolves, reducing line edge roughness. There is also an effect of reducing defects. The dissolution rate can be determined by immersing the amorphous film in a developer for a predetermined time at 23°C, and measuring the film thickness before and after the immersion by a known method such as visual observation, an ellipsometer, or a QCM method.

[0051] In the case of a positive resist pattern, the dissolution rate in a developer at 23°C of the portion of the amorphous film formed by spin coating that has been exposed to radiation such as KrF excimer laser, extreme ultraviolet light, electron beam or X-ray is preferably 10 Å / sec or more. If the dissolution rate is 10 Å / sec or more, the film is easily soluble in a developer and is more suitable for use as a resist. In addition, if the film has a dissolution rate of 10 Å / sec or more, the resolution may be improved. This is presumably because the micro surface portion of the resin dissolves, reducing line edge roughness. In addition, there is an effect of reducing defects.

[0052] In the case of a negative resist pattern, the dissolution rate in a developer at 23°C of the part of the amorphous film formed by spin coating that is exposed to radiation such as KrF excimer laser, extreme ultraviolet ray, electron beam or X-ray is preferably 5 Å / sec or less, more preferably 0.0005 to 5 Å / sec, and even more preferably 0.05 to 5 Å / sec. If the dissolution rate is 5 Å / sec or less, the resist can be insoluble in the developer. If the dissolution rate is 0.0005 Å / sec or more, the resolution may be improved. This is presumably because the contrast at the interface between the unexposed part that dissolves in the developer and the exposed part that does not dissolve in the developer increases due to the change in solubility of the resin before and after exposure. In addition, there is an effect of reducing line edge roughness and reducing defects.

[0053] (Other ingredients) The solvent used in the lithography film-forming composition is not particularly limited, and those disclosed in International Publication No. 2020 / 226150 can be used. The solvent is preferably a safe solvent, more preferably at least one selected from PGMEA (propylene glycol monomethyl ether acetate), PGME (propylene glycol monomethyl ether), CHN (cyclohexanone), CPN (cyclopentanone), 2-heptanone, anisole, butyl acetate, ethyl propionate, and ethyl lactate, and more preferably at least one selected from PGMEA, PGME, and CHN. In addition, it may be a mixed solvent by combining these solvents.

[0054] In the composition, the relationship between the amount of solid components and the amount of solvent is not particularly limited, but may be the following, with the total weight of the solid components and the solvent being 100% by weight. Solid content 1-80% by weight: Solvent 20-99% by weight Solid content 1-50% by weight: Solvent 50-99% by weight Solid content 2-40% by weight: Solvent 60-98% by weight Solid content 2-10% by weight: Solvent 90-98% by weight

[0055] The composition may contain, as other solid components, at least one selected from the group consisting of an acid generator (C), an acid crosslinking agent (G), an acid diffusion controller (E) and other components (F).

[0056] In the composition, the content of the hyperbranched resin is not particularly limited, but is preferably 50 to 99.4% by weight, more preferably 55 to 90% by weight, even more preferably 60 to 80% by weight, and particularly preferably 60 to 70% by weight, of the total weight of solid components (the sum of optionally used solid components such as the resin, acid generator (C), crosslinking agent (G), acid diffusion controller (E), and other components (F), the same applies below). With this content, the resolution is further improved and the line edge roughness (LER) is further reduced.

[0057] (Acid Generator (C)) The composition preferably contains one or more acid generators (C) that generate an acid directly or indirectly when irradiated with any radiation selected from visible light, ultraviolet light, excimer laser, electron beam, extreme ultraviolet light (EUV), X-rays, and ion beams.

[0058] In this case, the content of the acid generator (C) in the composition is preferably 0.001 to 49% by weight, more preferably 1 to 40% by weight, further preferably 3 to 30% by weight, and particularly preferably 10 to 25% by weight, based on the total weight of the solid components. By using the acid generator (C) within the above content range, a pattern profile with higher sensitivity and lower edge roughness can be obtained.

[0059] In the present composition, the method of generating the acid is not limited as long as the acid is generated in the system. If an excimer laser is used instead of ultraviolet rays such as g-rays or i-rays, finer processing is possible, and if high-energy rays such as electron beams, extreme ultraviolet rays, X-rays, or ion beams are used, further finer processing is possible.

[0060] The acid generator (C) is not particularly limited, and examples thereof include compounds disclosed in International Publication No. 2017 / 033943. As the acid generator (C), an acid generator having an aromatic ring is preferable, an acid generator having a sulfonate ion having an aryl group is more preferable, and diphenyltrimethylphenylsulfonium p-toluenesulfonate, triphenylsulfonium p-toluenesulfonate, triphenylsulfonium trifluoromethanesulfonate, and triphenylsulfonium nonafluorobutanesulfonate are particularly preferable. By using the acid generator, line edge roughness can be reduced.

[0061] The composition preferably further contains a diazonaphthoquinone photoactive compound described in WO 2020 / 226150 as an acid generator. Among these, from the viewpoint of low roughness and solubility, a non-polymeric diazonaphthoquinone photoactive compound is preferable, more preferably a low molecular weight compound having a molecular weight of 1500 or less, even more preferably a molecular weight of 1200 or less, and particularly preferably a molecular weight of 1000 or less. A preferred specific example of such a non-polymeric diazonaphthoquinone photoactive compound includes a non-polymeric diazonaphthoquinone photoactive compound disclosed in WO 2016 / 158881. The acid generator (C) can be used alone or in two or more kinds.

[0062] (Crosslinking agent (G)) When the resist is used as a negative resist material or as an additive for increasing the strength of the pattern in a positive resist material, it is preferable to include one or more crosslinking agents (G). The crosslinking agent is preferably an acid crosslinking agent. The acid crosslinking agent (G) is a compound capable of intramolecular or intermolecular crosslinking of the resin in the presence of an acid generated from the acid generator (C). Such an acid crosslinking agent (G) is not particularly limited, but may be, for example, a compound having one or more groups capable of crosslinking the resin (hereinafter referred to as "crosslinkable groups").

[0063] Specific examples of such crosslinkable groups include, but are not limited to, those described in International Publication No. 2020 / 226150. As the crosslinkable group of the acid crosslinker (G), hydroxyalkyl groups and alkoxyalkyl groups are preferred, and alkoxymethyl groups are particularly preferred.

[0064] The acid crosslinking agent (G) having a crosslinkable group is not particularly limited, but examples thereof include those described in WO 2020 / 226150.

[0065] Further examples of the acid crosslinking agent (G) include compounds having a phenolic hydroxyl group as described in WO 2020 / 226150, and compounds and resins to which the crosslinkable group has been introduced into the acidic functional group in an alkali-soluble resin to impart crosslinking properties.

[0066] In the composition, the acid crosslinker (G) is preferably an alkoxyalkylated urea compound or its resin, or an alkoxyalkylated glycoluril compound or its resin (acid crosslinker (G1)), a phenol derivative having 1 to 6 benzene rings in the molecule, having two or more hydroxyalkyl groups or alkoxyalkyl groups in the entire molecule, and the hydroxyalkyl groups or alkoxyalkyl groups are bonded to any of the benzene rings (acid crosslinker (G2)), or a compound having at least one α-hydroxyisopropyl group (acid crosslinker (G3)). For example, the compounds disclosed in International Publication No. 2017 / 033943 can be mentioned.

[0067] In the composition, the content of the acid crosslinker (G) is preferably 0.5 to 49% by weight, more preferably 0.5 to 40% by weight, even more preferably 1 to 30% by weight, and particularly preferably 2 to 20% by weight, based on the total weight of the solid components. The content of the acid crosslinker (G) of 0.5% by weight or more is preferable because it improves the effect of suppressing the solubility of the resist film in an alkaline developer, and can suppress a decrease in the residual film rate and the occurrence of swelling and meandering of the pattern, while the content of 49% by weight or less is preferable because it can suppress a decrease in the heat resistance of the resist.

[0068] The content of at least one compound selected from the acid crosslinkers (G1), (G2), and (G3) in the acid crosslinker (G) is not particularly limited, and can be in various ranges depending on factors such as the type of substrate used when forming a resist pattern.

[0069] (Acid diffusion controller (E)) The composition may contain an acid diffusion controller (E) that has the effect of controlling the diffusion of the acid generated from the acid generator by irradiation in the resist film, thereby preventing undesirable chemical reactions in unexposed regions. By using such an acid diffusion controller (E), the storage stability of the composition is improved. In addition, the resolution is further improved, and the change in line width of the resist pattern caused by the variation in the exposure time before and after irradiation can be suppressed, resulting in extremely excellent process stability.

[0070] Such an acid diffusion controller (E) is not particularly limited, and examples thereof include radiolytic basic compounds such as nitrogen atom-containing basic compounds, basic sulfonium compounds, and basic iodonium compounds. Examples of the acid diffusion controller (E) include compounds disclosed in International Publication No. 2017 / 033943. The acid diffusion controller (E) can be used alone or in combination of two or more.

[0071] The content of the acid diffusion controller (E) is preferably 0.001 to 49% by weight, more preferably 0.01 to 10% by weight, further preferably 0.01 to 5% by weight, and particularly preferably 0.01 to 3% by weight, based on the total weight of the solid components. When the content of the acid diffusion controller (E) is within the above range, the deterioration of resolution, pattern shape, dimensional fidelity, etc. can be further suppressed. Furthermore, even if the waiting time from electron beam irradiation to heating after radiation irradiation is long, the shape of the upper layer part of the pattern does not deteriorate. Furthermore, when the content of the acid diffusion controller (E) is 10% by weight or less, the deterioration of sensitivity, developability of unexposed parts, etc. can be prevented. Furthermore, by using such an acid diffusion controller, the storage stability of the composition is improved, the resolution is improved, and the line width change of the resist pattern due to the variation of the waiting time before radiation irradiation and the waiting time after radiation irradiation can be suppressed, resulting in extremely excellent process stability.

[0072] (Other ingredients (F)) To the composition, one or more of various additives such as a dissolution promoter, a dissolution control agent, a sensitizer, a surfactant, and an organic carboxylic acid or a phosphorus oxo acid or a derivative thereof can be added as other components (F) as necessary, within the scope of not impairing the object of this embodiment. Examples of other components (F) include the compounds disclosed in WO 2017 / 033943.

[0073] The total content of the other components (F) is preferably 0 to 49 wt % of the total weight of the solid components, more preferably 0 to 5 wt %, even more preferably 0 to 1 wt %, and particularly preferably 0 wt %.

[0074] In the composition, the content of the resin, the acid generator (C), the acid diffusion controller (E) and the other components (F) (the resin / the acid generator (C) / the acid diffusion controller (E) / the other components (F)) is, in weight % on a solid basis, preferably 50-99.4 / 0.001-49 / 0.001-49 / 0-49, more preferably 55-90 / 1-40 / 0.01-10 / 0-5, still more preferably 60-80 / 3-30 / 0.01-5 / 0-1, and particularly preferably 60-70 / 10-25 / 0.01-3 / 0. The content of each component is selected from the respective ranges so that the sum of the components is 100% by weight. When the content is within the above range, the sensitivity, resolution, developability, and other performances are further improved.

[0075] The method for preparing the composition is not particularly limited, and examples of the method include dissolving each component in a solvent at the time of use to prepare a homogeneous solution, and then filtering the solution, if necessary, through a filter having a pore size of about 0.2 μm.

[0076] The composition may contain other resins to the extent that the effect is not impaired. The other resins are not particularly limited, and examples thereof include novolac resins, polyvinylphenols, polyacrylic acid, polyvinyl alcohol, styrene-maleic anhydride resins, and polymers containing acrylic acid, vinyl alcohol, or vinylphenol as monomer units, or derivatives thereof. The content of the other resins is not particularly limited, and is appropriately adjusted depending on the type. The content of the other resins is preferably 30 parts by weight or less, more preferably 10 parts by weight or less, even more preferably 5 parts by weight or less, and particularly preferably 0 parts by weight, per 100 parts by weight of the multi-branched resin.

[0077] [Pattern formation method] The pattern forming method includes a film forming step of applying the lithography film forming composition on a substrate to form a film (resist film), an exposure step of exposing the formed film (resist film), and a development step of developing the film (resist film) exposed in the exposure step to form a pattern (resist pattern). The resist pattern can also be used as an upper layer resist in a multilayer process.

[0078] (film formation process) For example, this step can be carried out as follows. First, the resist composition is applied onto a conventionally known substrate by a coating means such as spin coating, casting coating, or roll coating to form a resist film. The conventionally known substrate is not particularly limited, and examples thereof include substrates for electronic components and those on which a predetermined wiring pattern is formed. More specifically, examples thereof include, but are not particularly limited to, silicon wafers, metal substrates such as copper, chromium, iron, and aluminum, and glass substrates. Examples of materials for the wiring pattern include, but are not particularly limited to, copper, aluminum, nickel, and gold. If necessary, an inorganic film or an organic film may be provided on the substrate. Examples of inorganic films include, but are not particularly limited to, inorganic anti-reflective films (inorganic BARC). Examples of organic films include, but are not particularly limited to, organic anti-reflective films (organic BARC). Surface treatment with hexamethylenedisilazane or the like may be performed. Next, if necessary, the coated substrate is heated. The heating conditions vary depending on the composition of the composition, etc., but are preferably 20 to 250° C., more preferably 20 to 150° C. Heating is preferable because it may improve the adhesion of the resist to the substrate.

[0079] (Exposure process) For example, this step can be carried out as follows. The resist film is exposed to any radiation selected from the group consisting of visible light, ultraviolet light, excimer laser, electron beam, extreme ultraviolet light (EUV), X-rays, and ion beams in a desired pattern. The exposure conditions and the like are appropriately selected depending on the composition and the like of the composition. In the method for forming a resist pattern, it is preferable to heat the film after irradiation with radiation in order to stably form a highly accurate fine pattern in the exposure. The heating conditions vary depending on the composition and the like of the composition, but are preferably 20 to 250°C, more preferably 20 to 150°C.

[0080] (Developing process) For example, this process can be carried out as follows. The exposed resist film is developed with a developer to form a predetermined resist pattern. As the developer, it is preferable to select a solvent having a solubility parameter (SP value) close to that of the resin. Suitable solvents include those disclosed in International Publication No. 2020 / 226150.

[0081] An appropriate amount of a surfactant can be added to the developer as necessary. The surfactant is not particularly limited, but for example, an ionic or nonionic fluorine-based or silicon-based surfactant can be used. Examples of these surfactants include those disclosed in International Publication No. 2020 / 226150. It is more preferable to use a fluorine-based surfactant or a silicon-based surfactant as the nonionic surfactant.

[0082] The amount of the surfactant used is usually from 0.001 to 5% by weight, preferably from 0.005 to 2% by weight, and more preferably from 0.01 to 0.5% by weight, based on the total amount of the developer.

[0083] Examples of the developing method include a method of immersing a substrate in a tank filled with a developer for a certain period of time (dip method), a method of piling up the developer on the substrate surface by surface tension and leaving it for a certain period of time (paddle method), a method of spraying the developer on the substrate surface (spray method), and a method of continuously dispensing the developer while scanning a developer dispensing nozzle at a constant speed on a substrate rotating at a constant speed (dynamic dispense method). There is no particular limit to the time for developing the pattern, but it is preferably 10 seconds to 90 seconds. In addition, after the developing step, a step of stopping the development while replacing it with another solvent may be performed.

[0084] (Other processes) After development, it is preferable to include a step of washing with a rinse solution containing an organic solvent. Examples of the rinse solution and rinse method used in the rinse step after development include those disclosed in International Publication No. 2020 / 226150.

[0085] After forming the resist pattern, the patterned wiring board is obtained by etching. The etching method can be a known method such as dry etching using plasma gas or wet etching using an alkaline solution, a cupric chloride solution, a ferric chloride solution, or the like.

[0086] After the resist pattern is formed, plating may be performed. The plating method is not particularly limited, but examples thereof include copper plating, solder plating, nickel plating, and gold plating.

[0087] The remaining resist pattern after etching can be peeled off with an organic solvent. Examples of the organic solvent and peeling method include those disclosed in International Publication No. 2020 / 226150.

[0088] The wiring board can also be formed by a method in which a resist pattern is formed, a metal is evaporated in a vacuum, and then the resist pattern is dissolved in a solution, that is, by a lift-off method.

[0089] [Lithography underlayer film forming composition, lithography underlayer film, and pattern formation method] First Embodiment <Lithography underlayer film forming composition> The lithography underlayer film-forming composition according to this embodiment (hereinafter also referred to as "underlayer film-forming composition") contains the above-mentioned multi-branched resin and a silicon-containing compound (e.g., hydrolyzable organosilane, its hydrolysate, or its hydrolyzed condensate). The underlayer film-forming composition has a relatively high carbon concentration, a relatively low oxygen concentration, high heat resistance, and high solvent solubility. Therefore, the pattern has excellent rectangularity. In addition, it is possible to reduce film defects (thin film formation), has good storage stability, has high sensitivity, a high refractive index and transparency in a specific wavelength region, and can impart a good resist pattern shape.

[0090] The underlayer film forming composition can be suitably used in a multi-layer resist method in which a resist underlayer film is further provided between an upper layer resist (photoresist, etc.) and a hard mask or an organic underlayer film. In such a multi-layer resist method, for example, a resist underlayer film is formed on an organic underlayer film or a hard mask on a substrate by a coating method or the like, and an upper layer resist (for example, a photoresist, an electron beam resist, an EUV resist) is formed on the resist underlayer film. Then, a resist pattern is formed by exposure and development, and the resist underlayer film is dry-etched using the resist pattern to transfer the pattern, and the organic underlayer film is etched to transfer the pattern, and the substrate is processed using the organic underlayer film.

[0091] That is, the lithography underlayer film (resist underlayer film) formed using the underlayer film-forming composition is less likely to cause intermixing with the upper layer resist and has heat resistance. For example, the etching rate of the underlayer film against a halogen-based (fluorine-based) etching gas is higher than that of the patterned upper layer resist used as a mask, so that a good rectangular pattern can be obtained. Furthermore, since the resist underlayer film has high resistance to oxygen-based etching gas, it can function as a good mask when patterning a layer provided on a substrate, such as a hard mask. The underlayer film-forming composition can also be used in an embodiment in which a plurality of resist underlayer films are laminated. In this case, the position of the resist underlayer film (which layer it is laminated in) is not particularly limited, and it may be directly under the upper layer resist, may be the layer located closest to the substrate, or may be sandwiched between the resist underlayer films. In the present disclosure, the terms lithography underlayer film and resist underlayer film are used interchangeably.

[0092] In forming a fine pattern, the resist film tends to be thin in order to prevent the pattern from collapsing. Dry etching for transferring a pattern to a film existing in an underlying layer by thinning the resist film must have a higher etching rate than the film in the upper layer in order to transfer the pattern. In this embodiment, an organic underlayer film is placed on a substrate, and the resist underlayer film (containing a silicon-based compound) of this embodiment is coated on the organic underlayer film, which is then coated with a resist film (organic resist film). The dry etching rate of an organic component film and an inorganic component film differs greatly depending on the etching gas selected, and the dry etching rate of an organic component film is increased by an oxygen-based gas, and the dry etching rate of an inorganic component film is increased by a halogen-containing gas. For example, a resist underlayer film with a pattern transferred thereto is dry-etched with an oxygen-based gas to transfer the pattern to the organic underlayer film, and the organic underlayer film with the pattern transferred thereto can be used to process the substrate using a halogen-containing gas.

[0093] In addition, when the resist underlayer film contains the hyperbranched resin and a silicon-containing compound (for example, hydrolyzable organosilane, its hydrolyzate, or its hydrolyzed condensate), the sensitivity of the upper resist layer is improved, no intermixing occurs with the upper resist layer, and the pattern of the resist underlayer film formed after exposure and development becomes rectangular. This makes it possible to process substrates with fine patterns.

[0094] In particular, it is preferable that the resist underlayer film is composed of a multi-branched heterocyclic resin (for example, a multi-branched PBO resin), since this has extremely high heat resistance and is extremely unlikely to cause intermixing with the upper resist layer.

[0095] In addition, the resist underlayer film has high heat resistance, so it can be used under high temperature baking conditions.Furthermore, since it has a relatively low molecular weight and low viscosity, it is easy to fill even the corners of a substrate having a step (especially a fine space or hole pattern, etc.), so that the planarization property and filling property tend to be relatively advantageously improved.

[0096] The underlayer film-forming composition may further contain, in addition to the multi-branched resin and the silicon-containing compound, a solvent, an acid, an acid crosslinking agent, etc. Furthermore, as optional components, it may contain an organic polymer compound, an acid generator, a surfactant, and other components such as water, alcohol, and a curing catalyst. From the viewpoint of coatability and quality stability, the content of the multi-branched resin in the lithography underlayer film is preferably 0.1 to 70% by weight, more preferably 0.5 to 50% by weight, and particularly preferably 3.0 to 40% by weight.

[0097] As the solvent, any known solvent can be used as long as the multi-branched resin can be dissolved in it. The type and amount of the solvent can be as disclosed in International Publication No. 2020 / 226150.

[0098] The underlayer film-forming composition may contain an acid from the viewpoint of promoting curing. The type and amount of the acid may be as disclosed in WO 2020 / 226150.

[0099] The underlayer film forming composition may contain one or more acid crosslinkers when used as a negative resist material or as an additive for increasing the strength of a pattern in a positive resist material. An acid crosslinker is a compound that can intramolecularly or intermolecularly crosslink the resin in the presence of the above-mentioned acid. The type and amount of the acid crosslinker may be as disclosed in WO 2020 / 226150.

[0100] The underlayer film-forming composition contains a silicon-containing compound. The silicon-containing compound may be either an organic silicon-containing compound or an inorganic silicon-containing compound, but is preferably an organic silicon-containing compound. The type and amount of the silicon-containing compound may be as disclosed in International Publication No. 2020 / 226150.

[0101] In addition to the above components, the underlayer film-forming composition may optionally contain an organic polymer compound, a crosslinking agent, a photoacid generator, a surfactant, etc. The types and amounts of these components may be as disclosed in WO 2020 / 226150.

[0102] <Lithography Underlayer Film and Pattern Formation Method> The lithography underlayer film of this embodiment can be suitably used as an underlayer (resist underlayer film) of a photoresist (upper layer) used in a multi-layer resist method.

[0103] In the present embodiment, for example, a resist underlayer film is formed using the underlayer film forming composition, at least one photoresist layer is formed on the resist underlayer film, and then a predetermined region of the photoresist layer is irradiated with radiation and developed to form a pattern. The resist underlayer film is preferably formed by forming an underlayer film precursor from a hyperbranched PA resin, heating the precursor at 300° C. or higher, and converting the hyperbranched PA resin into a hyperbranched PBO resin.

[0104] Also, as one aspect of the pattern forming method according to the first embodiment, there can be mentioned a method comprising the following steps: forming an organic underlayer film on a substrate using a coating type organic underlayer film material; forming a resist underlayer film on the organic underlayer film using the underlayer film forming composition of the first embodiment; forming an upper-layer resist film on the resist underlayer film using an upper-layer resist film composition; forming an upper-layer resist pattern on the upper-layer resist film, and transferring the pattern to the resist underlayer film by etching using the upper-layer resist pattern as a mask; transferring the pattern to the organic underlayer film by etching using the resist underlayer film to which the pattern has been transferred as a mask; transferring the pattern to the substrate (workpiece) by etching using the organic underlayer film to which the pattern has been transferred as a mask.

[0105] As another embodiment, a method including the following steps can be mentioned: a step of forming an organic hard mask mainly composed of carbon on a substrate by a CVD method; a step of forming a resist underlayer film on the organic hard mask using the underlayer film forming composition of the first embodiment; a step of forming an upper layer resist film on the resist underlayer film using an upper layer resist film composition; a step of forming an upper layer resist pattern on the upper layer resist film and transferring the pattern to the resist underlayer film by etching using the upper layer resist pattern as a mask; a step of transferring the pattern to the organic hard mask by etching using the resist underlayer film to which the pattern has been transferred as a mask; a step of transferring the pattern to the substrate (workpiece) by etching using the organic hard mask to which the pattern has been transferred as a mask.

[0106] As the substrate, for example, a semiconductor substrate can be used. As the semiconductor substrate, a silicon substrate can generally be used, but is not particularly limited, and a material different from the workpiece layer, such as Si, amorphous silicon (α-Si), p-Si, SiO2, SiN, SiON, W, TiN, or Al, can be used. In addition, as the metal constituting the substrate (workpiece; including the semiconductor substrate), those disclosed in International Publication No. 2020 / 226150 can be used.

[0107] In the pattern forming method of the present embodiment, an organic underlayer film or an organic hard mask can be formed on a substrate. Among them, the organic underlayer film can be formed from a coating-type organic underlayer film material by using a spin-coating method or the like, and the organic hard mask can be formed from a carbon-based organic hard mask material by using a CVD method. The types of such organic underlayer film and organic hard mask are not particularly limited, but when the upper resist film is patterned by exposure, it is preferable that the organic underlayer film and organic hard mask exhibit sufficient anti-reflective film function. By forming such an organic underlayer film or organic hard mask, the pattern formed by the upper resist film can be transferred onto the substrate (workpiece) without causing a size conversion difference. A "carbon-based" hard mask means a hard mask in which 50% or more by weight of the solid content is composed of a carbon-based material such as amorphous hydrogenated carbon, also called amorphous carbon and denoted as aC:H. The aC:H film can be deposited by various techniques, but plasma enhanced chemical vapor deposition (PECVD) is widely used due to its cost-effectiveness and film quality adjustability. As an example of the hard mask, for example, the one described in JP-T-2013-526783 can be referred to.

[0108] The resist underlayer film used in the pattern forming method of this embodiment can be formed by spin coating or the like on a workpiece provided with an organic underlayer film or the like. When forming the resist underlayer film by spin coating, it is desirable to evaporate the solvent after spin coating and bake to promote a crosslinking reaction in order to prevent mixing with the upper resist film. The bake temperature is preferably within a range of 50 to 500°C. At this time, depending on the structure of the device to be manufactured, the bake temperature is particularly preferably 400°C or less in order to reduce thermal damage to the device. The bake time is preferably within a range of 10 to 300 seconds.

[0109] In the pattern forming method of the present embodiment, the method of forming a pattern on the upper resist film can be suitably selected from the following methods: lithography using light having a wavelength of 300 nm or less or EUV light, electron beam direct writing, and directed self-organization. By using such methods, a fine pattern can be formed on the upper resist film.

[0110] The upper layer resist film composition can be appropriately selected according to the method of forming a pattern on the above-mentioned upper layer resist film.For example, when performing lithography using light of 300 nm or less or EUV light, the upper layer resist film composition can be a chemically amplified photoresist film material.As such a photoresist film material, after forming a photoresist film and exposing it, it is possible to exemplify a material that forms a positive pattern by dissolving the exposed part using an alkaline developer, or a material that forms a negative pattern by dissolving the unexposed part using an organic solvent developer.

[0111] The resist underlayer film formed in this embodiment may absorb light depending on the wavelength of light used in the lithography process, and in such a case, it can function as an anti-reflection film having the effect of preventing light from being reflected from the substrate.

[0112] In addition, the resist underlayer film formed in this embodiment can be used as an underlayer film of an EUV resist, not only as a hard mask but also as an underlayer anti-reflective film of an EUV resist. In addition, the film formed from the underlayer film-forming composition has excellent EUV absorption ability, so it can exert a sensitizing effect on the upper layer resist composition, contributing to improving sensitivity. When the resist underlayer film formed in this embodiment is used as an EUV resist underlayer film, the process can be carried out in the same manner as the underlayer film for photoresist.

[0113] Second Embodiment <Resist underlayer film forming composition> The composition for forming a resist underlayer film according to the second embodiment (hereinafter also referred to as "underlayer film forming composition") contains the multi-branched resin, but may not contain a silicon-containing compound.

[0114] The underlayer film-forming composition of this embodiment is applicable to a wet process and is useful for forming a photoresist underlayer film having excellent heat resistance, step filling properties, and flatness. The underlayer film-forming composition uses a compound having a specific structure with a relatively high carbon concentration, a relatively low oxygen concentration, and high solvent solubility, and therefore can form an underlayer film that is suppressed from deteriorating during baking and has excellent etching resistance against fluorine gas-based plasma etching and the like. Furthermore, it is also excellent in adhesion to the resist layer, so that an excellent resist pattern can be formed. The underlayer film-forming composition of this embodiment is particularly excellent in heat resistance, step filling properties, and flatness, so that it can be used, for example, to form a resist underlayer film that is provided at the bottom layer of a plurality of resist layers. However, the resist underlayer film formed in this embodiment may further include another resist underlayer between the substrate.

[0115] The underlayer film-forming composition according to the present embodiment may further contain a solvent, an acid generator, an acid crosslinking agent, etc. In addition, as optional components, a basic compound, water, an alcohol, a curing catalyst, etc. In terms of coatability and quality stability, the content of the resin in the underlayer film-forming composition is preferably 0.1 to 70% by weight, more preferably 0.5 to 50% by weight, and particularly preferably 3.0 to 40% by weight.

[0116] As the solvent used in this embodiment, any known solvent can be used as long as it can dissolve at least the resin. The type and amount of the solvent can be as disclosed in International Publication No. 2020 / 226150.

[0117] The underlayer film-forming composition of this embodiment may contain an acid crosslinker as necessary from the viewpoint of suppressing intermixing, etc. The type and amount of the acid crosslinker may be as disclosed in WO 2020 / 226150.

[0118] The underlayer film-forming composition of the present embodiment may contain an acid generator as necessary from the viewpoint of further promoting the crosslinking reaction by heat. The type and amount of the acid generator may be as disclosed in WO 2020 / 226150.

[0119] Furthermore, the underlayer film-forming composition of the present embodiment may contain a basic compound from the viewpoint of improving storage stability, etc. The type and amount of the basic compound may be as disclosed in WO 2020 / 226150.

[0120] In addition, the underlayer film forming composition of this embodiment may contain other resins or compounds for the purpose of imparting thermosetting properties or controlling absorbance. As such other resins or compounds, those disclosed in International Publication No. 2020 / 226150 can be used.

[0121] <Lithography Resist Underlayer Film and Pattern Forming Method> The pattern formed in this embodiment can be used as, for example, a resist pattern or a circuit pattern. The method for producing the resist underlayer film in this embodiment is the same as that described in the first embodiment.

[0122] The pattern forming method according to the second embodiment includes a step (A-1 step) of forming a resist underlayer film on a substrate using the underlayer film forming composition according to the second embodiment, a step (A-2 step) of forming at least one photoresist layer on the resist underlayer film, and a step (A-3 step) of irradiating a predetermined region of the photoresist layer with radiation and developing the photoresist layer after forming at least one photoresist layer in the A-2 step. The photoresist layer means the outermost layer of the resist layer, i.e., the layer provided on the outermost side (opposite side from the substrate) of the resist layer.

[0123] Further, another pattern forming method of the second embodiment includes a step (B-1 step) of forming a resist underlayer film on a substrate using the underlayer film forming composition of the second embodiment, a step (B-2 step) of forming a resist intermediate layer film on the underlayer film using a resist intermediate layer film material (e.g., a silicon-containing resist layer), a step (B-3 step) of forming at least one photoresist layer on the resist intermediate layer film, a step (B-4 step) of irradiating a predetermined region of the photoresist layer with radiation and developing the photoresist layer to form a resist pattern after the at least one photoresist layer is formed in the B-3 step, and a step (B-5 step) of etching the resist intermediate layer film using the resist pattern as a mask after the resist pattern is formed in the B-4 step, etching the underlayer film using the obtained intermediate layer film pattern as an etching mask, and etching the substrate using the obtained underlayer film pattern as an etching mask to form a pattern on the substrate.

[0124] When forming the resist underlayer film, it is preferable to perform a bake treatment in order to suppress the occurrence of a mixing phenomenon with the upper resist (for example, a photoresist layer or a resist intermediate layer film) and to promote a crosslinking reaction. The conditions can be as disclosed in WO 2020 / 226150.

[0125] After preparing a resist underlayer film on a substrate, a resist intermediate layer film can be provided between the photoresist layer and the resist underlayer film. For example, in the case of a two-layer process, a silicon-containing resist layer or a monolayer resist made of a normal hydrocarbon can be provided as a resist intermediate layer film on the resist underlayer film. Also, for example, in the case of a three-layer process, it is preferable to prepare a silicon-containing intermediate layer between the resist intermediate layer film and the photoresist layer, and a silicon-free monolayer resist layer on top of that. These photoresist layers, resist intermediate layer films, and photoresist materials for forming the resist layers provided between these layers can be known. As the silicon-containing resist material, those disclosed in International Publication No. 2020 / 226150 can be used. In addition, a resist intermediate layer formed by a Chemical Vapour Deposition (CVD) method can also be used.

[0126] Furthermore, the resist underlayer film of the present embodiment can be used as an anti-reflection film for a normal single-layer resist or as an underlayer material for suppressing pattern collapse. Since the resist underlayer film of the present embodiment has excellent etching resistance for underlayer processing, it can also be expected to function as a hard mask for underlayer processing.

[0127] When forming a resist layer using the above-mentioned known photoresist material, wet processes such as spin coating and screen printing are preferably used, as in the case of forming the resist underlayer film. After applying the resist material by spin coating or the like, pre-baking is usually performed, and this pre-baking is preferably performed at a baking temperature of 80 to 180° C. and for a baking time of 10 to 300 seconds. Thereafter, exposure is performed according to a conventional method, followed by post-exposure baking (PEB) and development to obtain a resist pattern. The thickness of each resist film is not particularly limited, but is generally preferably 30 nm to 500 nm, more preferably 50 nm to 400 nm.

[0128] The exposure light may be appropriately selected depending on the photoresist material used. In general, high energy rays having a wavelength of 300 nm or less, specifically, excimer lasers having wavelengths of 248 nm, 193 nm, and 157 nm, soft X-rays having wavelengths of 3 to 20 nm, electron beams, X-rays, and the like can be used.

[0129] The resist pattern formed by the above-mentioned method is one in which pattern collapse is suppressed by the resist underlayer film of the present embodiment. Therefore, by using the resist underlayer film of the present embodiment, a finer pattern can be obtained, and the exposure dose required to obtain the resist pattern can be reduced.

[0130] Next, etching is performed using the obtained resist pattern as a mask. Gas etching is preferably used for etching the resist underlayer film in the two-layer process. Etching using oxygen gas is suitable for gas etching. In addition to oxygen gas, it is also possible to add inert gases such as He and Ar, or CO, CO2, NH3, SO2, N2, NO2, and H2 gases. Gas etching can also be performed using only CO, CO2, NH3, SO2, N2, NO2, and H2 gases without using oxygen gas. In particular, the latter gas is preferably used for sidewall protection to prevent undercutting of the pattern sidewall.

[0131] On the other hand, gas etching is also preferably used for etching the middle layer (the layer located between the photoresist layer and the resist underlayer film) in the three-layer process. The gas etching can be the same as that described in the two-layer process. In particular, the processing of the middle layer in the three-layer process is preferably performed using a fluorocarbon-based gas with the resist pattern as a mask. Thereafter, the resist underlayer film can be processed by, for example, performing oxygen gas etching with the middle layer pattern as a mask as described above.

[0132] Here, when forming an inorganic hard mask intermediate layer film as the intermediate layer, a silicon oxide film, a silicon nitride film, or a silicon oxynitride film (SiON film) is formed by a CVD method, an ALD method, or the like. The method for forming the nitride film is not limited to the following, but for example, the methods described in JP-A-2002-334869 and WO 2004 / 066377 can be used. A photoresist film can be formed directly on such an intermediate layer film, but an organic anti-reflective coating (BARC) may be formed on the intermediate layer film by spin coating, and a photoresist film may be formed on the organic anti-reflective coating (BARC).

[0133] As the intermediate layer, a polysilsesquioxane-based intermediate layer is also preferably used. By making the resist intermediate layer have an effect as an anti-reflection film, reflection tends to be effectively suppressed. The specific material of the polysilsesquioxane-based intermediate layer is not limited to the following, but for example, those described in JP-A-2007-226170 and JP-A-2007-226204 can be used.

[0134] Etching of the substrate can also be performed by conventional methods; for example, if the substrate is SiO2 or SiN, etching can be performed mainly with fluorocarbon-based gases, and if it is p-Si, Al, or W, etching can be performed mainly with chlorine- or bromine-based gases. When etching the substrate with fluorocarbon-based gases, the silicon-containing resist of the two-layer resist process and the silicon-containing intermediate layer of the three-layer process are stripped at the same time as the substrate is processed. On the other hand, when the substrate is etched with chlorine- or bromine-based gases, the silicon-containing resist layer or the silicon-containing intermediate layer is stripped separately, and generally, dry etching stripping with fluorocarbon-based gases is performed after the substrate is processed.

[0135] The resist underlayer film of this embodiment has excellent etching resistance to these substrates. As the substrate, a known one can be appropriately selected and used, and is not particularly limited, but includes Si, α-Si, p-Si, SiO2, SiN, SiON, W, TiN, Al, etc. The substrate may also be a laminate having a processed film (processed substrate) on a base material (support). Such processed films include various low-k films such as Si, SiO2, SiON, SiN, p-Si, α-Si, W, W-Si, Al, Cu, Al-Si, and the like, and stopper films thereof, and usually, a film made of a material different from the base material (support) is used. The thickness of the substrate or processed film to be processed is not particularly limited, but is usually preferably about 50 nm to 10,000 nm, more preferably 75 nm to 5,000 nm.

[0136] The resist underlayer film of this embodiment has excellent flatness and embedding ability in a substrate having steps.As an evaluation method of embedding flatness, a known method can be appropriately selected and used, and is not particularly limited.For example, the solution of each compound adjusted to a predetermined concentration is applied by spin coating on a silicon substrate having steps, and the solvent is removed and dried at 110°C for 90 seconds, and the underlayer film is formed to a predetermined thickness, and then the difference (ΔT) in the underlayer film thickness between the line & space region and the open region without pattern is measured by an ellipsometer after baking for a predetermined time at a temperature of about 240 to 300°C, and the embedding flatness in a substrate having steps can be evaluated.

[0137] [Optical article-forming composition and cured product thereof] The multi-branched resin is useful for optical materials. An optical component forming composition containing the resin can provide optical components with a high refractive index, and is expected to have excellent storage stability, structure forming ability (film forming ability), and heat resistance. The refractive index of the optical article is preferably 1.60 or more, more preferably 1.65 or more, even more preferably 1.70 or more, and even more preferably 1.75 or more, from the viewpoint of miniaturization of optical components and improvement of light collection rate. The transparency of the optical article is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more, from the viewpoint of improvement of light collection rate. There is no particular limit to the method of measuring the refractive index, and a known method is used. For example, the spectroscopic ellipsometry method, the minimum deviation method, the critical angle method (Abbe method, Pulfrich method), the V-block method, the prism coupler method, and the liquid immersion method (Becke line method) can be mentioned. There is no particular limit to the method of measuring the transparency, and a known method is used. For example, a spectrophotometer and a spectroscopic ellipsometry method can be mentioned.

[0138] Furthermore, the cured product obtained by curing the optical part-forming composition can be a three-dimensional crosslinked product, and coloring is suppressed by heat treatment over a wide range from low temperature to high temperature, and it is expected to have a high refractive index and high transparency.

[0139] The optical part-forming composition of the present embodiment may further contain a solvent in addition to the resin. The solvent may be the same as the solvent used in the above-mentioned lithography film-forming composition.

[0140] In the optical component-forming composition of this embodiment, the relationship between the amount of solid components and the amount of solvent is not particularly limited, but is preferably 1-80% by weight of solid components and 20-99% by weight of solvent, more preferably 1-50% by weight of solid components and 50-99% by weight of solvent, even more preferably 2-40% by weight of solid components and 60-98% by weight of solvent, and particularly preferably 2-10% by weight of solid components and 90-98% by weight of solvent, relative to 100% by weight of the total of solid components and solvent. The optical component-forming composition of this embodiment may not contain a solvent.

[0141] The optical component forming composition of the present embodiment may contain, as other solid components, at least one selected from the group consisting of an acid generator (C), an acid crosslinking agent (G), an acid diffusion controller (E) and other components (F).

[0142] In the optical component forming composition of the present embodiment, the content of the hyperbranched resin is not particularly limited, but is preferably 50 to 99.4 wt % of the total weight of the solid components, more preferably 55 to 90 wt %, even more preferably 60 to 80 wt %, and particularly preferably 60 to 70 wt %.

[0143] The acid generator (C), acid crosslinker (G), acid diffusion controller (E) and other components (F) contained in the optical component forming composition of this embodiment may be similar to those that may be contained in the above-mentioned lithographic film-forming composition.

[0144] In the optical part forming composition of the present embodiment, the content of the resin, the acid generator (C), the acid diffusion controller (E), and the other components (F) (the resin / the acid generator (C) / the acid diffusion controller (E) / the other components (F)) is preferably 50 to 99.4 / 0.001 to 49 / 0.001 to 49 / 0 to 49, more preferably 55 to 90 / 1 to 40 / 0.01 to 10 / 0 to 5, still more preferably 60 to 80 / 3 to 30 / 0.01 to 5 / 0 to 1, and particularly preferably 60 to 70 / 10 to 25 / 0.01 to 3 / 0, in terms of weight % based on solid matter. The content ratio of each component is selected from each range so that the sum of the components is 100% by weight. When the content ratio is set as above, the performance such as sensitivity, resolution, and developability is further improved.

[0145] The method for preparing the optical part-forming composition of the present embodiment is not particularly limited, and examples thereof include a method in which each component is dissolved in a solvent at the time of use to prepare a homogeneous solution, and then, if necessary, filtered through a filter with a pore size of about 0.2 μm, for example.

[0146] The optical component forming composition of the present embodiment may contain other resins to the extent that the intended purpose is not hindered. The types and amounts of the other resins may be as disclosed in WO 2020 / 226150.

[0147] The cured product of the present embodiment is obtained by curing the optical component-forming composition and can be used as various resins. These cured products can be used for various purposes as highly versatile materials that impart various properties such as a high melting point, a high refractive index, and high transparency. The cured products can be obtained by subjecting the composition to light irradiation, heating, or other known methods corresponding to each composition.

[0148] These cured products can be used as various synthetic resins such as epoxy resins, polycarbonate resins, and acrylic resins, and further, taking advantage of their functionality, can be used as optical parts such as lenses and optical sheets.

[0149] 6. Purification method The multi-branched resin is preferably purified. The purification method is not particularly limited, but the method described in International Publication No. 2015 / 080240 or the method described in International Publication No. 2018 / 159707 can be used. Specifically, the purification method includes a step of dissolving the resin in an organic solvent that is not miscible with water to obtain an organic phase, contacting the organic phase with an acidic aqueous solution to perform an extraction process, thereby transferring metals contained in the organic phase containing the resin and the organic solvent to the aqueous phase, and then separating the organic phase from the aqueous phase. The organic solvent that is not miscible with water is usually an organic solvent classified as a non-water-soluble solvent. The organic solvent is not particularly limited, but an organic solvent that can be safely applied to a semiconductor manufacturing process is preferable. The amount of the organic solvent used is usually about 1 to 100 times by weight relative to the compound used.

[0150] Specific examples of the organic solvent to be used include those described in International Publication No. 2015 / 080240. Among these, toluene, 2-heptanone, cyclohexanone, cyclopentanone, methyl isobutyl ketone, propylene glycol monomethyl ether acetate, ethyl acetate, and the like are preferred, and cyclohexanone and propylene glycol monomethyl ether acetate are particularly preferred.

[0151] The acidic aqueous solution is appropriately selected from among aqueous solutions in which a generally known organic or inorganic compound is dissolved in water. For example, those described in International Publication No. 2015 / 080240 can be mentioned. These acidic aqueous solutions can be used alone or in combination of two or more. Examples of the acidic aqueous solution include mineral acid aqueous solutions and organic acid aqueous solutions. Examples of the mineral acid aqueous solution include an aqueous solution containing one or more selected from the group consisting of hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid. Examples of the organic acid aqueous solution include an aqueous solution containing one or more selected from the group consisting of acetic acid, propionic acid, oxalic acid, malonic acid, succinic acid, fumaric acid, maleic acid, tartaric acid, citric acid, methanesulfonic acid, phenolsulfonic acid, p-toluenesulfonic acid, and trifluoroacetic acid. The pH range of the acidic aqueous solution is about 0 to 5, and more preferably about pH 0 to 3. EXAMPLES

[0152] [Example 1] Hyperbranched resin 1 having a polyamide structure (1) Synthesis of tricarboxylic acid compounds (esters) The reaction shown in the following scheme was carried out.

[0153] [ka]

[0154] The following was placed in a 100 mL recovery flask: 4,4',4”-Trihydroxytriphenylmethane (MTP) 10.0mmol, 2.92g K2CO3 35.0mmol, 4.83g Dimethylformamide (DMF) 20 mL The contents were stirred for 60 minutes at 80° C. Then, 35 mmol and 3.87 mL of ethyl bromoacetate (EBA) were added to the flask, and the mixture was further stirred at 80° C. for 24 hours to carry out the reaction.

[0155] The reaction mixture was poured into a 0.01N aqueous hydrochloric acid solution to cause reprecipitation. The precipitate was collected and subjected to an extraction operation using chloroform. This extraction operation was carried out twice in total. Next, a saturated sodium bicarbonate solution was added to the organic phase for liquid separation and washing. Furthermore, a saturated saline solution was added to the organic phase for liquid separation and washing.

[0156] The organic phase obtained after the washing step was dried by adding anhydrous magnesium sulfate. The dried organic phase was concentrated using an evaporator to obtain a dark yellow liquid. The dark yellow liquid was subjected to column separation using ethyl acetate / hexane = 1:1 as the mobile phase to separate the residue. The liquid obtained by the column separation was further concentrated using an evaporator to obtain a light yellow viscous liquid. The light yellow viscous liquid was analyzed, and it was confirmed that the desired ester was produced (Figures 1A and 1B). The yield was 99%.

[0157] (2) Synthesis of tricarboxylic acid compounds The following reactions were carried out:

[0158] [ka]

[0159] The following was placed in a 300 mL flask: The ester obtained in the above step: 10 mmol, 5.5 g KOH 90mmol 5.05g Tetrahydrofuran (THF):water = 1:1 mixed solvent 150mL The contents were stirred at 50° C. for 72 hours and the aqueous phase was collected.

[0160] The aqueous phase was made weakly acidic and subjected to extraction with ethyl acetate. The ethyl acetate phase was washed with saturated saline and anhydrous magnesium sulfate. The ethyl acetate phase after washing was concentrated with an evaporator and washed with hexane. The ethyl acetate phase was filtered using a Kiriyama funnel and dried under reduced pressure at room temperature. In this way, the target tricarboxylic acid compound (orange solid, molecular weight: 466.43) was obtained. The analysis results are shown in Figure 2.

[0161] (3) Synthesis of hyperbranched resins with polyamide structures The following reactions were carried out:

[0162] [ka]

[0163] The following was placed in a test tube: 0.23 g of the tricarboxylic acid compound synthesized in (2) above N-methylpyrrolidone (NMP) 3.0 mL 2,2-bis(3-amino-4-hydroxyphenyl)propane (BAHP) 0.085g Diisopropylcarbodiimide (DIC) 0.25mL The contents were stirred and reacted for 24 hours at 25° C. The reaction mixture was reprecipitated using dichloromethane, and the precipitate was filtered using a Kiriyama funnel to obtain the target resin. 1 The results of H-NMR and GPC analysis are shown in Figures 3A and 3B. Yield: 97% Mn=7400, Mn / Mn=2.40

[0164] The synthesis reaction of this resin was carried out in the same manner as above, except that the amount of solvent was changed as shown in the table below. However, when the amount of solvent was too small, gelation occurred, and the desired resin could not be obtained.

[0165] [Table 1]

[0166] [Example 2] Hyperbranched resin having a polyamide structure (1) Synthesis of tricarboxylic acid compounds (halides: tricarboxylic acid chlorides) The reaction shown in the following scheme was carried out.

[0167] [ka]

[0168] The following was placed in a 200 mL recovery flask: Tricarboxylic acid obtained in Example 1(2): 2.33 g, 7.76 mmol Chloroform: 30mL Thionyl chloride: 60 mmol, 7.14 g, 4.36 mL Dimethylformamide (DMF): 1 drop

[0169] The contents were stirred at 70°C for 18 hours. The reaction mixture was concentrated using an evaporator and washed with hexane. The target product was an orange viscous solid. The yield was 98%. The analytical results are shown in Figure 4.

[0170] (2) Synthesis of hyperbranched resins with polyamide structures The following reactions were carried out:

[0171] [ka]

[0172] The following was placed in a test tube: 0.26 g 0.5 mmol of the tricarboxylic acid compound (tricarboxylic acid chloride (MBOAC)) obtained in (1) above 2,2-Bis(3-amino-4-hydroxyphenyl)propane (BAHP) 0.19g 0.75mmol Dimethylformamide (DMF) 0.3 mL 4-Dimethylaminopyridine (DMAP) 0.19g

[0173] The contents were stirred at 25°C for 20 hours to carry out the reaction. The reaction mixture was reprecipitated using diethyl ether. The precipitate was collected and washed with 1N aqueous hydrochloric acid solution. The product was dried under reduced pressure to obtain the desired hyperbranched resin having a polyamide structure. 1 The results of H-NMR and GPC analysis are shown in Figures 5A and 5B.

[0174] Resins were produced in the same manner by changing the ratio of 2,2-bis(3-amino-4-hydroxyphenyl)propane (BAHP) (Table 2 (B)) and tricarboxylic acid chloride (Table 2 (A)). The ratio was set to a value that would achieve the functional group equivalent ratio shown in the table below. The results are shown in the table.

[0175] [Table 2]

[0176] (3) Physical properties 1) Heat resistance The thermal decomposition temperature of the obtained hyperbranched resin was measured by TGA (thermogravimetry). The results are shown in Figure 5C. The resin had excellent heat resistance.

[0177] 2) Solubility The solubility of the hyperbranched resin in various solvents was evaluated. When 2 mg of the resin dissolved in 2 g of solvent at 20°C, it was evaluated as "completely soluble (+)", and when it did not dissolve, it was evaluated as "insoluble (-)". The results are shown in the table below. It is clear that the resin has good solubility in major solvents.

[0178] [Table 3]

[0179] THF: tetrahydrofuran DMF: Dimethylformamide DMSO: Dimethyl sulfoxide PGMEA: Propylene glycol monomethyl ether acetate) NMP: N-methylpyrrolidone DMAc: N,N-dimethylacetamide MEK: Methyl ethyl ketone PGME: Propylene glycol monomethyl ether

[0180] 3) Film formability The hyperbranched resin was dissolved in dimethylformamide (DMF) to obtain a composition with a concentration of 3% by weight. The solution was spin-coated on a silicon wafer under the following conditions, and post-baked to obtain a film. The film-forming properties were good. Rotational speed: 2500 rpm Drying: 10 minutes at 200℃ Film thickness: 32.4 nm However, when dimethyl sulfoxide (DMSO), N,N-dimethylacetamide (DMAc), or N-methylpyrrolidone (NMP) was used as the solvent, the film could not be formed.

[0181] [Example 3] The following reaction was carried out to synthesize a hyperbranched resin having a polyamide structure.

[0182] [ka]

[0183] The following was placed in a test tube: 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoromethylpropane (BAHFP) 0.75mmol, 0.275g Tricarboxylic acid compound (1,3,5-benzenetricarbonyl trichloride (BCC)) 0.5mmol, 0.132g Dimethylformamide (DMF) 1.5mL 4-Dimethylaminopyridine (DMAP) 1.5mmol 0.183g

[0184] The contents were stirred at 25°C for 20 hours to carry out the reaction. The reaction mixture was reprecipitated using water. The precipitate was collected and washed with diethyl ether. The precipitate was then filtered using a Kiriyama funnel and dried under reduced pressure at room temperature to obtain the target resin. The analysis results by GPC are shown in Figure 6.

[0185] Resins were produced in the same manner, but the charging ratio of tricarboxylic acid chloride (BCC) and 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoromethylpropane (BAHFP) and the amount of the solvent used were changed as shown in Table 4. The charging ratio was as shown in the table below. The results are shown in the table. The results of the GPC analysis are shown in Figure 6.

[0186] [Table 4]

[0187] [Example 4] Except for changing the reaction temperature, the resin was produced in the same manner as in Example 3. The results are shown in Table 5. The analysis results by GPC and FT-IR are shown in Figures 7A and 7B.

[0188] [Table 5]

[0189] The solubility and film-forming ability of the resin in Run 3 in Table 4 were evaluated by the above-mentioned method. The results are shown in Tables 6 and 7, respectively.

[0190] [Table 6]

[0191] [Table 7]

[0192] The refractive index was measured by the following procedure. The resin was dissolved in DMF, and the solution was spin-coated onto a silicon wafer to prepare a thin film. The refractive index of the thin film at 620 nm was measured using a film thickness / refractive index distribution measuring device SE-101 manufactured by Photonic Lattice Co., Ltd.

[0193] [Example 5] Synthesis of hyperbranched polybenzoxazole A 70 nm thick film (corresponding to the 70 nm thick film in Table 7) made from the hyperbranched PA resin obtained in Run 3 in Table 4 was heated at 300°C for 60 minutes in an inert atmosphere. As a result, intramolecular cyclization occurred and a hyperbranched polybenzoxazole (PBO) film was produced. The analysis results are shown in Figures 8A and 8B.

[0194] Furthermore, a film of BCA[4]-DBH was formed on the film of the hyperbranched polybenzoxazole according to a standard method. BCA[4]-DBH is a main chain decomposition type cyclic molecular resist material synthesized from calixarene (see International Publication No. 2021 / 230185 or Journal of Photopolymer Science and Technology Volume 33, Number 1 (2020) 45-51). The material has the following structure, and is a highly sensitive extreme ultraviolet resist material with excellent solubility and film-forming properties.

[0195] [ka]

[0196] [Table 8]

[0197] [Example 6] Examination of fluorine introduction rate A hyperbranched PA resin was synthesized in the same manner as in Example 3. However, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoromethylpropane (BAHFP) and 2,2-bis(3-amino-4-hydroxyphenyl)propane (BAHP) were used as diamino compounds, 1,3,5-benzenetricarboxylic acid chloride (BCC) was used as tricarboxylic acid compound, and the amounts charged were changed as shown in Table 9. Furthermore, the reaction conditions were set to 25°C and 24 hours. Next, the hyperbranched PA resin was heated in the same manner as in Example 5 to attempt the production of a hyperbranched polybenzoxazole (PBO) resin film. The results are shown in Table 9.

[0198] [Table 9]

[0199] In Run 1, BAHP was used as a diamino compound that does not contain fluorine. Meanwhile, from Run 2 onwards, BAHP was replaced with BAHFP, which contains fluorine, to increase the fluorine introduction rate. It became clear that as the fluorine introduction rate increases, intramolecular cyclization becomes more likely, making it possible to form a hyperbranched PBO resin film. When fluorine atoms are introduced, the fluorine atoms repel each other, decreasing the polymer density, which is thought to improve solubility and film formability.

[0200] [Example 7] A BOC-protected product of Poly(BCC-co-BAHFP) was obtained using the hyperbranched resin Poly(BCC-co-BAHFP) having a polyamide structure obtained in RUN3 of Example 3. Specifically, the protected product was obtained by the following method.

[0201] The following was placed in a test tube: Poly(BCC-co-BAHFP)0.5mmol, 0.285g N-methylpyrrolidone (NMP) 20mL Di-tert-butyl dicarbonate 1.0mmol, 0.228g Triethylamine 0.2g

[0202] The contents were stirred at 25°C for 24 hours to carry out the reaction. The reaction mixture was reprecipitated using water. The precipitate was collected and dried under reduced pressure to obtain the target white resin. The production of the target product was confirmed by the disappearance of the hydroxyl group peak of Poly(BCC-co-BAHFP) and the appearance of the BOC group peak in NMR measurement, and the appearance of a peak derived from the BOC group in IR measurement (Figures 9 and 10).

[0203] [ka]

[0204] The solubility of the above-mentioned protected product was evaluated according to the above-mentioned method, and the results are shown in the table below.

[0205] [Table 9A]

[0206] The above-mentioned protector was found to be excellent as a lithography material because it was soluble in PGME and PGMEA, which are often used in lithography applications.

[0207] (Comparative Synthesis Example 1) Synthesis of CR-1 A four-neck flask with a capacity of 10 L, equipped with a Dimroth condenser, a thermometer and an agitator, and capable of being opened from the bottom, was prepared. In this four-neck flask, 1.09 kg (7 mol, manufactured by Mitsubishi Gas Chemical Co., Ltd.), 2.1 kg of 40 wt% formalin aqueous solution (28 mol as formaldehyde, manufactured by Mitsubishi Gas Chemical Co., Ltd.) and 0.97 mL of 98 wt% sulfuric acid (manufactured by Kanto Chemical Co., Ltd.) were charged in a nitrogen stream, and the mixture was reacted for 7 hours while refluxing at 100°C under normal pressure. Then, 1.8 kg of ethylbenzene (special grade reagent manufactured by Wako Pure Chemical Industries, Ltd.) was added as a dilution solvent to the reaction solution, and after standing, the aqueous phase of the lower phase was removed. Furthermore, the mixture was neutralized and washed with water, and ethylbenzene and unreacted 1,5-dimethylnaphthalene were distilled off under reduced pressure to obtain 1.25 kg of dimethylnaphthalene formaldehyde resin as a light brown solid. The molecular weight Mn of the resulting dimethylnaphthalene formaldehyde was 562.

[0208] Next, a four-neck flask with an internal volume of 0.5 L equipped with a Dimroth condenser, a thermometer, and a stirring blade was prepared. Into this four-neck flask, 100 g (0.51 mol) of the dimethylnaphthalene formaldehyde resin and 0.05 g of paratoluenesulfonic acid were charged under a nitrogen stream, and the temperature was raised to 190° C. and heated for 2 hours, and then stirred. Then, 52.0 g (0.36 mol) of 1-naphthol was added, and the temperature was raised to 220° C. and reacted for 2 hours. After dilution with a solvent, neutralization and washing with water were performed, and the solvent was removed under reduced pressure to obtain 126.1 g of a modified resin (CR-1) as a black-brown solid. The obtained resin (CR-1) had Mn: 885, Mw: 2220, and Mw / Mn: 4.17. The Mn, Mw and Mw / Mn of the resin (CR-1) were determined in terms of polystyrene by gel permeation chromatography (GPC) analysis under the following measurement conditions. Equipment: Shodex GPC-101 type (Showa Denko K.K. product) Column: KF-80M x 3 Eluent: THF 1mL / min Temperature: 40℃

[0209] (Synthesis Example 1) Synthesis of AC-1 A reaction solution was prepared by dissolving 4.15 g of 2-methyl-2-methacryloyloxyadamantane, 3.00 g of methacryloyloxy-γ-butyrolactone, 2.08 g of 3-hydroxy-1-adamantyl methacrylate, and 0.38 g of azobisisobutyronitrile in 80 mL of tetrahydrofuran. The reaction solution was stirred under a nitrogen atmosphere and kept at 63° C. for 22 hours to polymerize. The reaction solution was then dripped into 400 mL of n-hexane. The resulting resin was coagulated and purified, and the resulting white powder was filtered and then dried overnight at 40° C. under reduced pressure to obtain AC-1 represented by the following formula.

[0210] [ka]

[0211] In formula AC-1, "40", "40", and "20" indicate the ratio of each constituent unit and do not indicate that it is a block copolymer.

[0212] [Example A, Comparative Example A] Using the resins shown in Table 10 and CR-1, compositions for forming a film for lithography (compositions for forming a film for lithography) having the compositions shown in Table 10 were prepared.

[0213] The acid generator, acid diffusion controller, crosslinker, and organic solvent used were as follows: In Table 10, the numbers in parentheses indicate the amounts (parts by weight) used. <Acid generator> Triphenylsulfonium trifluoromethanesulfonate (TPS-109 (trade name)) manufactured by Midori Chemical Co., Ltd. Di-tertiary butyl diphenyl iodonium nonafluorobutanesulfonate (DTDPI) manufactured by Midori Chemical Co., Ltd. Pyridinium paratoluenesulfonate (listed as "PPTS" in the table) manufactured by Kanto Chemical <Acid diffusion control agent> Tri-n-octylamine (TOA, Kanto Chemical Co., Ltd.) <Crosslinking agent> Nikalac MW-100LM (MW-100LM, product name, manufactured by Sanwa Chemical Co., Ltd.) Sanwa Chemical's Nikalac MX270 Honshu Chemical Industry Co., Ltd. TMOM-BP <Organic solvent> N,N-Dimethylformamide (DMF, Kanto Chemical Co., Ltd.) Propylene glycol monomethyl ether (PGME, Kanto Chemical Co., Ltd.) Propylene glycol monomethyl ether acetate (PGMEA, Kanto Chemical Co., Ltd.)

[0214] [Table 10]

[0215] [Evaluation method] (1) Thin film formation of a resist film-forming composition Each resist film-forming composition was prepared according to the composition shown in Table 10, and then the uniform resist film-forming composition was spin-coated on a clean silicon wafer. Then, the wafer was pre-exposure baked (PB) in an oven at 110°C to form a resist film with a thickness of 40 nm.

[0216] (2) Resist pattern Each resist film obtained in (1) above was irradiated with an electron beam using an electron beam lithography device (ELS-7500, Elionix Co., Ltd., 50 keV) with a 1:1 line and space setting with 50 nm intervals. After irradiation, the resist film was heated at 110°C and 90 seconds, respectively, and in Examples A1 to A16, it was developed by immersing it in a developer of N,N-dimethylformamide (DMF) for 60 seconds. Comparative Example A1 was carried out in the same manner as in Example A1, except that it was developed by immersing it in a developer of propylene glycol monomethyl ether (PGME) for 60 seconds. Then, each resist film was washed with ultrapure water for 30 seconds and dried to form a resist pattern.

[0217] The shape of the resulting L / S (1:1) resist pattern with 50 nm spacing was observed using an electron microscope (S-4800, product name) manufactured by Hitachi, Ltd. The shape of the resist pattern after development was evaluated according to the following criteria. A: There is no pattern collapse, and the rectangularity is better than that of Comparative Example A1. B: The rectangularity is better than Comparative Example A1, but 1 to 3 pattern collapses are observed within an area of ​​1 μm × 1.5 μm. C: Equivalent to or inferior to Comparative Example A1 In Comparative Example A1, the resist pattern shape after development showed pattern collapse and poor rectangularity.

[0218] (3) Etching resistance An etching test was performed on each resist film obtained by the evaluation method (1) above, and the etching rate was measured. In addition, a comparative composition was prepared using a novolac resin (PSM4357 (model number) manufactured by Gun-ei Chemical Industry Co., Ltd.) instead of the multi-branched resin having a polyamide structure (resin obtained in Run 4 of Example 1) used in Example A1 in the composition shown in Table 10. A resist film was prepared for the comparative composition by the same method as in (1) above, and an etching test was also performed on this resist film. The etching conditions were as follows.

[0219] (Etching conditions) Etching equipment: Samco Corporation RIE-10NR (product name) Output: 50W Pressure: 20Pa Time: 2 minutes Etching gas: Ar gas flow rate: CF4 gas flow rate: O2 gas flow rate = 50:5:5 (sccm)

[0220] The etching resistance of each resist film was evaluated according to the following criteria, based on the etching rate of the resist film obtained from the comparative composition using a novolak resin.

[0221] (Evaluation Criteria) S: The etching rate is less than -15% compared to the novolac resin resist film. A: The etching rate is -15% or more and less than -10% compared to a novolac resin resist film. B: The etching rate is −10% or more and less than 0% compared to the novolac resin resist film. C: The etching rate is 0% or more compared to the novolac resin resist film.

[0222] The results of these evaluations are shown in Table 11.

[0223] [Table 11]

[0224] [Example B] The etching resistance of the PBO films obtained in Examples 5 and 6 was measured in the same manner as in Example A. The results are shown in Table 12.

[0225] [Table 12]

[0226] [Example C] (1) Formation of resist underlayer film Using the same resin as in Example A, compositions for forming resist underlayer films were prepared with the compositions shown in Table 13. Next, these compositions for forming resist underlayer films were spin-coated onto silicon substrates, and then baked at 240° C. for 60 seconds and then at 400° C. for 120 seconds to prepare resist underlayer films with a thickness of 70 nm. The acid generators, crosslinking agents, and organic solvents used were as follows. <Acid generator> Di-tert-butyldiphenyliodonium nonafluoromethanesulfonate (referred to as "DTDPI" in the table) (manufactured by Midori Chemical Co., Ltd.) Triphenylsulfonium trifluoromethanesulfonate (TPS-109 (trade name)) (manufactured by Midori Chemical Co., Ltd.) Pyridinium paratoluenesulfonate (listed as "PPTS" in the table) manufactured by Kanto Chemical <Crosslinking agent> "Nicalac MX270" (shown as "MX270" in the table) (product name, manufactured by Sanwa Chemical Co., Ltd.) "Nicalac MW-100LM" (shown as "MW-100LM" in the table) (product name, manufactured by Sanwa Chemical) Honshu Chemical Industry Co., Ltd. TMOM-BP <Organic solvent> N,N-Dimethylformamide (DMF, Kanto Chemical Co., Ltd.) Propylene glycol monomethyl ether (PGME, Kanto Chemical Co., Ltd.) Propylene glycol monomethyl ether acetate (PGMEA, Kanto Chemical Co., Ltd.)

[0227] [Table 13]

[0228] As the underlayer film in Examples C19 to C22, a PBO film formed in the same manner as in Example B was used.

[0229] (2) Formation and evaluation of resist film An ArF resist solution was applied onto the resist underlayer film formed in (1) above, and baked for 60 seconds at 130° C. to form a photoresist film with a thickness of 140 nm. The ArF resist solution was prepared by mixing 5 parts by weight of the resin (AC-1) obtained in Synthesis Example 1 above, 1 part by weight of triphenylsulfonium nonafluoromethanesulfonate, 2 parts by weight of tributylamine, and 92 parts by weight of PGMEA.

[0230] The photoresist film was then exposed to light using an electron beam lithography system "ELS-7500" (product name, Elionix Co., Ltd., 50 keV). It was then baked (PEB) at 115°C for 90 seconds, and developed with a 2.38 wt% tetramethylammonium hydroxide (TMAH) aqueous solution for 60 seconds to obtain a positive resist pattern.

[0231] The results of observing defects in the resulting resist patterns of 55 nmL / S (1:1) and 80 nmL / S (1:1) are shown in Table 14. In the table, "Good" as shown in the results of "resist pattern after development" indicates that no pattern collapse was observed in the formed resist pattern, and "Poor" indicates that pattern collapse was observed in the formed resist pattern. In addition, as a result of the above observation, the minimum line width at which there was no pattern collapse and good rectangularity was used as an index for evaluation of "resolution". The results are shown in Table 14.

[0232] [Comparative Example C1] A photoresist film was formed directly on a SiO2 substrate in the same manner as in Example C1, except that no undercoat film was formed, to obtain a positive resist pattern. The results are shown in Table 14.

[0233] [Table 14]

[0234] It is clear that the resist underlayer films obtained in the examples have excellent resolution and can form good resist patterns.

Claims

1. (I) preparing a diamino compound represented by formula (A) and a tricarboxylic acid compound represented by formula (B); [Formula 1] (In the formula, Y is an alkylene group which may contain fluorine, Z is independently -OH, -SH, or -NH 2 and R's each independently represent a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 40 carbon atoms which may have a substituent, an aralkyl group having 7 to 40 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an arylalkenyl group having 7 to 40 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, a halogen atom, a nitro group, an amino group, a cyano group, a carboxylic acid group, a thiol group or a hydroxyl group, and the aryl group, aralkyl group, alkenyl group, alkynyl group and arylalkenyl group may contain an ether bond, a ketone bond, an ester bond or a urethane bond, m is an integer from 1 to 3 and represents the number of groups other than hydrogen when R is a group other than hydrogen; Ar is a group having an aromatic group; E is -COOH, -COHal, -O-R b -COOH or -O-R b -COHal, Hal is a halogen atom, R b is an alkylene group having 1 to 6 carbon atoms. (II) a step of condensing these compounds to form a polyamide structure; Manufactured by a method comprising: A hyperbranched resin with a polyamide structure.

2. 2. The resin of claim 1, wherein Y is a branched alkylene group.

3. 3. The resin of claim 1 or 2, wherein Y is a fluorinated alkylene group.

4. (i) preparing a hyperbranched resin having a polyamide structure according to any one of claims 1 to 3; and (ii) intramolecularly condensing the resin to form a heterocyclic structure; Manufactured by a method comprising: A hyperbranched resin with a heterocyclic structure.

5. There are units in which Y is an alkylene group and units in which Y is a fluorinated alkylene group, 5. The resin of claim 4, wherein the molar ratio of said alkylene groups to fluorinated alkylene groups is 1:(1.5 to 10).

6. A lithographic film-forming composition comprising the resin according to any one of claims 1 to 5.

7. A lithography underlayer film-forming composition comprising the resin according to claim 3 .

8. The composition according to claim 6 or 7, which contains a solvent.

9. The composition of any of claims 6 to 8, comprising a component selected from the group consisting of a solvent, an acid generator, an acid crosslinker, and combinations thereof.

10. A lithographic underlayer film formed using the composition of claim 7.

11. A lithographic underlayer film comprising the resin of claim 4 or 5.

12. A step of forming an underlayer film on a substrate using the composition according to claim 7, and heating the precursor to 300°C or higher to form an underlayer film containing a hyperbranched resin having a heterocyclic structure; forming at least one photoresist layer on the underlayer film; and exposing predetermined areas of the photoresist layer to radiation and developing; A method for forming a resist pattern comprising the steps of:

13. Represented by the following formula (1-1): [chemical 2] (In the formula, Y is an alkylene group which may contain fluorine, X is a group having an aromatic group; Z 1 -OH, -SH, -NH 2 or a group protected by a protecting group; R's each independently represent a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 40 carbon atoms which may have a substituent, an aralkyl group having 7 to 40 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an arylalkenyl group having 7 to 40 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, a halogen atom, a nitro group, an amino group, a cyano group, a carboxylic acid group, a thiol group or a hydroxyl group, and the aryl group, aralkyl group, alkenyl group, alkynyl group and arylalkenyl group may contain an ether bond, a ketone bond, an ester bond or a urethane bond, m is an integer from 1 to 3 and represents the number of groups other than hydrogen when R is a group other than hydrogen; n is the number of repeats in the main chain, r is the number of repeats in the branched chain, and n>r. A hyperbranched resin with a polyamide structure.

14. Represented by the following formula (2): [C3] (In the formula, Y 1 is a fluorinated alkylene group, Y 2 is an alkylene group, Z' is independently -O-, -S-, or -NH-; X is a group having an aromatic group; R's each independently represent a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 40 carbon atoms which may have a substituent, an aralkyl group having 7 to 40 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an arylalkenyl group having 7 to 40 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, a halogen atom, a nitro group, an amino group, a cyano group, a carboxylic acid group, a thiol group or a hydroxyl group, and the aryl group, aralkyl group, alkenyl group, alkynyl group and arylalkenyl group may contain an ether bond, a ketone bond, an ester bond or a urethane bond, m is an integer from 1 to 3 and represents the number of groups other than hydrogen when R is a group other than hydrogen; n 1 and n 2 is the number of repeats in the main chain, r 1 and r 2 is the number of repeats in the branched chain, and n 1 >r 1 And n 2 >r 2 It is.) A hyperbranched resin with a heterocyclic structure.

15. The X is represented by any one of the following formulas: [C4] (Ar is an aromatic group, R b is an alkylene group having 1 to 6 carbon atoms.

15. The resin according to claim 13 or 14.