Carbon coated particles

Carbon-coated particles address the issue of degraded recycled pyrolytic carbon by optimizing surface properties, improving rubber reinforcement and reducing environmental impact through cost-effective manufacturing processes.

JP2024159759APending Publication Date: 2024-11-08CABOT CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024121317
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2016-03-07
Filing Date
2024-07-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing reinforcing particles, such as recycled pyrolytic carbon, exhibit degraded interaction with rubber molecules, leading to inferior reinforcement properties in rubber compounds, and there is a need for cost-effective alternatives that reduce environmental impact and improve manufacturing efficiency.

Method used

Carbon-coated particles are produced by coating core materials, including recycled pyrolytic carbon, with a carbon layer using plasma or furnace processes, optimizing surface properties to enhance rubber reinforcement and interaction.

Benefits of technology

The carbon-coated particles achieve improved rubber reinforcement properties, reduce manufacturing costs, and promote recycling, offering enhanced performance in tire applications while minimizing environmental waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159759000001_ABST
    Figure 2024159759000001_ABST
Patent Text Reader

Abstract

To provide generally a novel carbon-containing material, typically a particulate material, a process for making such a material, and methods for using it.SOLUTION: Core particles produced in situ or introduced as preformed core particles are coated with a layer of carbon. Non-carbon and some carbon-based core materials can be utilized. The resulting carbon coated particles can find applications in rubber products, for instance as a reinforcement for tire components.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Related Applications This application claims priority to U.S. Provisional Application No. 62 / 155,142, filed April 30, 2015, entitled "Carbon Coated Particles and Methods of Making and Using Same," and U.S. Provisional Application No. 62 / 304,694, filed March 7, 2016, entitled "Carbon Coated Plasma Carbon Black," which are incorporated herein by reference in their entireties. [Background technology]

[0002] Small, typically submicron-sized particles are compounded into synthetic and natural rubber compounds used in various rubber products such as tires, hoses, belts, gaskets, bushings, etc. A variety of particles have been used or proposed for rubber compounds, the most common being carbon black (CB). These particles allow the material properties of the compound to be substantially engineered and improved in terms of application performance. For example, it allows control of the stiffness, hardness, modulus, and fracture properties of the rubber. Rubbers compounded with reinforced CB can have a large improvement in abrasion resistance, making them useful for tire treads and other demanding service applications.

[0003] A side effect of compounding rubber with reinforcing particles is that the rubber changes from highly elastic to viscoelastic, and the filled rubber dissipates energy as it cycles mechanically. An important practical effect of this viscoelastic behavior is that the tire dissipates mechanical energy as it flexes as it rolls, resulting in reduced vehicle fuel economy. Precipitated silica (PS) is commonly used in combination with synthetic rubber for automobile tire treads; PS provides the rubber compound with somewhat reduced wear compared to similar CB-based rubber compounds, but offers attractive improvements in energy loss, and therefore improved tire rolling resistance and vehicle fuel economy.

[0004] Generally, CB exists in the form of aggregates formed of CB primary particles in turn. In most cases, the primary particles do not exist independently of the CB aggregates. The primary particles can have an average primary particle diameter in the range of about 10 nanometers (nm) to about 50 nm, e.g., about 10 nm to about 15 nm; about 10 nm to about 20 nm; about 10 nm to about 25 nm; about 10 nm to about 30 nm; or about 10 nm to about 40 nm, and the aggregates can be significantly larger. CB aggregates have a fractal shape and are often referred to in the art as CB "particles" (not to be confused with "primary particles" above).

[0005] A wide variety of CBs are produced in furnace-type reactors by pyrolysis of a hydrocarbon feedstock (FS) with hot combustion gases producing a calcined product containing particulate CBs. The properties of a given CB typically depend on the production conditions and can be varied by, for example, changing temperature, pressure, FS, residence time, quench temperature, throughput, and other parameters.

[0006] Apparatus and methods for producing CB are known in the art. Examples are given in U.S. Reissue Patent No. 28974, U.S. Reissue Patent No. 3619140 by Morgan et al., which are incorporated herein by reference in their entirety. The process involves burning a fuel gas, such as natural gas, with oxygen under conditions of very high heat release in a small combustion zone to produce a very fast moving, hot combustion gas stream, essentially a plug flow. A separate stream of liquid hydrocarbons (preheated carbon black product oil or FS) is injected transversely into the high velocity combustion stream under conditions where the liquid hydrocarbons enter the high velocity combustion stream at a linear velocity of greater than about 100 feet per second.

[0007] The fuel in the combustion zone is completely burned with excess oxygen. CB nuclei are produced when the CB FS is injected, and these nuclei then coalesce and grow into product CB aggregates.

[0008] Methods for preparing silicon-treated CBs in situ from CB FS and silicon precursor materials in a CB reactor are disclosed in U.S. Pat. No. 5,904,762 to Mahmud et al.; and U.S. Pat. No. 5,830,930 to Mahmud et al. Furthermore, U.S. Pat. No. 5,830,930 discloses an elastomeric compound incorporating silicon-treated CBs. U.S. Pat. No. 6,057,387 to Mahmud et al. discloses aggregate particles comprising a carbon phase and a silicon-containing species phase having certain particle surface area and size distribution characteristics. In such silicon-treated CBs, silicon-containing species such as oxides or carbides of silicon are distributed throughout at least a portion of the CB aggregates as an inherent part of the CB. Such CB aggregates can be modified by depositing silicon-containing species such as silica on at least a portion of the surface of the CB aggregates during the formation of the CB aggregates in the CB reactor. The result can be described as a silicon-coated CB. In silicon-treated CB, the aggregate contains two phases. One phase is carbon present as graphitic crystallites and / or amorphous carbon, while the second, discontinuous phase is silica (and possibly other silicon-containing species). The silicon-containing phase can be present in an amount of 0.1-25% by weight of the CB aggregate. Thus, the silicon-containing species phase of silicon-treated CB is an inherent part of the aggregate; it is distributed over at least a portion of the aggregate, or over the surface of the aggregate. Wang et al., US Patent No. 6,017,980, discloses an elastomer composite comprising an aggregate of a carbon phase and 0.1-25% by weight of a metal-containing species phase (e.g., Al or Zn), as well as the formation of such aggregates in situ in a CB reactor. Alternatively, the silicon-containing phase can be incorporated with the metal-containing species phase in the CB phase.

[0009] Krejci, US Patent 2,632,713, discloses in-situ treated CB materials containing 0.01-10 wt.% silicon, boron or germanium species. Additive materials are introduced into the CB reactor together with the FS or separately and can be added further downstream in the reactor to provide a surface coating to the CB particles. CB materials containing silica surface domains are disclosed in Linster et al., US Patent 7,351,763, and Labauze, US Patent 6,071,995.

[0010] US Patent No. 6,099,818 to Freund et al. describes a method in which CB nuclei are formed by partial combustion of fuel oil in an oxygen-containing gas in a combustion chamber. The CB nuclei are carried by a stream of hot combustion gas to a reaction zone and immediately brought into contact with a CB feedstock, which coalesces and forms CB particles that grow into aggregates. According to US Patent No. 6,056,933 to Vogler et al., inversion CB is produced in a conventional CB reactor by controlled combustion in a combustion chamber to form CB nuclei and immediately brought into contact with a CB feedstock. US Patent No. 6,391,274 to Vogler et al. describes a method in which CB seeds (or nuclei) formed in a combustion zone are carried with a flow of combustion gas to a reaction zone where they initiate seed-induced CB formation with added CB feedstock. A silicon-containing compound, such as silane or silicone oil, is mixed with a CB feedstock to produce CBs containing 0.01-20% silicon by weight.

[0011] Plasma-based methods for preparing CB have also been developed. The Kvaerner process or Kvaerner CB and Hydrogen process (CB&H) is a process for producing CB and hydrogen gas from hydrocarbons such as methane, natural gas, and biogas. According to U.S. Patent No. 5,527,518 to Lynum et al., issued June 18, 1996, and incorporated herein by reference in its entirety, a method for producing carbon black material includes transporting feedstock through a feed tube to a plasma torch, a reaction zone, a first stage in which the temperature of the feedstock is increased to about 1600°C, and then passing the dehydrogenated carbon material to a second stage to complete the decomposition to carbon black and hydrogen. Additional feedstock quenches and reacts with the formed carbon black to increase the particle size density and quantity produced.

[0012] U.S. Patent Application Publication No. 2008 / 0289494 to Boutot et al., published Nov. 27, 2008, and incorporated herein by reference in its entirety, describes a method and apparatus for decomposing natural gas or methane into gaseous components (hydrogen and acetylene) and carbon particles using cold arc discharge (CAD).

[0013] According to U.S. Pat. No. 7,452,514 issued Nov. 18, 2008 to Fabry et al., and U.S. Patent Application Publication No. 2009 / 0142250 published Jun. 4, 2009 to Fabry et al., which are incorporated herein by reference in their entireties, CBs or carbon-containing compounds are formed by coating a carbon-containing FS using a method that includes the steps of: generating a plasma gas by electrical energy, directing the plasma gas through a venturi whose diameter narrows in the direction of the plasma gas flow, directing the plasma gas to a reaction zone (under the prevailing flow conditions generated by aerodynamic and electromagnetic forces, there is not sufficient recirculation of the FS back into the plasma gas in the reaction zone), recovering reaction products from the reaction zone, and separating the CBs or carbon-containing compounds from other reaction products.

[0014] In the method described in U.S. Pat. No. 4,101,639, issued Jul. 18, 1978 to Surovikin et al., which is incorporated herein by reference in its entirety, a hydrocarbon FS is introduced into a reaction chamber into a plasma stream saturated with water vapor.

[0015] U.S. Patent Application Publication No. 2015 / 0210856 to Johnson et al., published on July 30, 2015 and incorporated herein by reference in its entirety, describes a method and apparatus for flowing plasma gas to a plasma formation region having at least one magnetically isolated plasma torch including at least one electrode. The plasma is collected in a cooled header and flowed to a CB formation region that receives a CB-forming FS. A gas throat assembly connecting the plasma and CB formation regions is described by Hoermann et al. in U.S. Patent Application Publication No. 2015 / 0210858, published on July 30, 2015 and incorporated herein by reference in its entirety.

[0016] U.S. Patent Application Publication No. 2015 / 0210857 to Johnson et al., published July 30, 2015 and incorporated by reference in its entirety, describes the combustion of FS (typically methane) with plasma in an apparatus having a series of unit operations with individual volumes. The individual volumes of the unit operations are substantially balanced by replacing at least a portion of the FS with a FS having a molecular weight greater than methane.

[0017] Because sufficient amounts of CB material are used to reinforce the rubber components of tires, used tires and other CB reinforced rubber products represent a significant waste stream. To treat such waste, used tires can be pyrolyzed and attempts are being made to recover and reuse the carbon-based components.

[0018] Generally, pyrolysis is carried out in a reactor in an oxygen-free atmosphere. During the process, the rubber softens and then the rubber polymer decomposes into vapors (which can later be condensed into the liquid oil phase) and smaller molecules that are discharged from the reactor as gases. Also formed is a carbon-containing solid residue that can further include silica, alumina, zinc oxide, and / or other compounds. See, for example, U.S. Patent No. 4,251,500 to Morita et al., U.S. Patent No. 5,264,640 to Platz, and U.S. Patent No. 6,221,329 to Faukner et al.

[0019] With the development of equipment and technology, the main products of current tire pyrolysis units are oil, steel (recovered as steel wire), and a carbon char component ("pyrolytic carbon"). The properties of pyrolytic carbon are discussed, for example, in C. J. Norris et al., Maney Online, Vol. 43(8), 2014, pp. 245-256, which is incorporated herein by reference in its entirety. Possible applications of carbon obtained by pyrolyzing waste tires are described, for example, in the article "The vacuum pyrolysis of used tires-End-uses for oil and carbon black products" by C. Roy et al., Journal of Analytical and Applied Pyrolysis, Vol. 51, pp. 201-221 (1999). Summary of the Invention [Problem to be solved by the invention]

[0020] There is continuing interest in developing reinforcing particles or agents that can provide beneficial tire performance attributes. Lowering the cost, reducing the environmental burden of manufacturing, and widening the range of available reinforcing agents are also desirable goals.

[0021] The specific properties of the rubber compound can be optimized not only by the size, morphology and other physical properties of the reinforcing particles used, as is known in the art, but also by the bulk chemical composition and surface of the particles. For example, the high reinforcing properties of CB can be at least partially attributed to the details of the interaction between the rubber molecules and the CB surface.

[0022] While it may be beneficial to utilize recycled pyrolytic carbon by compounding it into new rubber compounds, recycled pyrolytic carbon generally provides significantly deteriorated reinforcement and other rubber properties compared to virgin CB. Among other deficiencies, it is believed that a significant problem with recycled pyrolytic carbon is that the particle surface is significantly altered and deteriorated with respect to interactions with rubber molecules compared to virgin CB.

[0023] In some cases, virgin CB particles may also exhibit poor rubber reinforcement properties. For example, the CB manufacturing process or post-manufacturing treatment of the CB particles can remove chemical groups from the CB particle surface, or thermally anneal or graphitize the CB particle surface to create crystalline regions, or degrade the activity of the CB particle surface, creating poor rubber reinforcement properties. [Means for solving the problem]

[0024] To address these and other challenges, the present invention relates generally to carbon-containing materials, typically particulate materials, methods of making such materials, and methods of using same.

[0025] The particles disclosed in this disclosure generally include a core and a carbon-based outer region, also referred to in this disclosure as a "coating," "layer," "deposit," or "shell," and one aspect of the invention features a carbon-coated particle that includes a core (material) coated with a carbon layer. In some implementations, the core is an aggregate or agglomerate that is covered in whole or in part by the carbon coating. The carbon coating or carbon-coated particle can be a tufted material that has the morphology and properties of a typical carbon black material. Illustrative examples of carbon-coated particles include a non-carbon core, a regenerated pyrolytic carbon, or a plasma carbon core coated with a carbon layer.

[0026] Another aspect of the invention relates to a method for producing carbon-coated particles. In the method, core particles are coated with a carbon layer in a reactor, which is often a CB reactor or a section thereof. Other suitable reactors, such as, for example, plasma reactors or other types of reactors, those using methane, natural gas, etc., can also be used to carry out the coating operation. Generally, the carbon layer is prepared from a liquid or gaseous carbon-producing FS.

[0027] In some embodiments, the core particles are already manufactured or "preformed" core particles that are introduced into the reactor and coated with a carbon layer to form carbon-coated particles. In other embodiments, the core particles are manufactured in situ, and in one implementation, the core particles are produced and coated in a stepwise assembly process carried out in a common reactor.

[0028] The core particles can consist of, consist essentially of, or include carbon. Examples of suitable preformed carbon core particles include regenerated pyrolytic carbon particles, plasma CB particles, preformed CB particles, especially CB particles having poor reinforcement or other poor surface properties, etc.

[0029] Carbon-based core particles can also be produced in situ. For example, core CB particles can be prepared via a plasma process or by another method in which a FS, such as natural gas or methane, is converted (decomposed) to produce carbon and hydrogen, and then coated with a carbon layer to form carbon-coated particles. Exemplary equipment that can be used includes a plasma zone; a reaction zone downstream of the plasma zone; a finishing zone downstream of the reaction zone; a line for introducing plasma gas into the plasma zone; one or more inlets for introducing a first FS into the reactor; one or more inlets for introducing a second FS into the reactor; a convergence zone between the plasma zone and the reaction zone; and optionally a convergence zone between the reaction zone and the finishing zone.

[0030] Non-carbon core particles can also be used. Examples include, but are not limited to, silica, rice husk silica, precipitated silica, clay, calcium carbonate, other preformed non-carbon particles, and mixtures thereof. In one example, preformed non-carbon core particles are introduced into a reactor, such as a CB reactor, and coated to produce carbon-coated particles. In another example, non-carbon (e.g., silica) core particles are generated in situ (e.g., in a CB reactor, using a suitable core precursor) and coated with a carbon layer in the reactor to form carbon-coated particles.

[0031] Some example implementations are given below.

[0032] In one embodiment, a method for producing carbon coated particles includes generating core particles in situ, which are plasma CB core particles or non-carbon core particles; and coating the core particles with a carbon layer in a CB process to form carbon coated particles.

[0033] In another embodiment, a method for producing carbon-coated particles includes introducing preformed core particles into a CB reactor; and coating the core particles with a carbon layer obtained by pyrolysis of a liquid or gaseous feedstock in the CB reactor, thereby forming carbon-coated particles.

[0034] In yet another embodiment, a method for preparing carbon-coated particles includes preparing CB core particles in situ in a CB reactor; and coating the CB core particles with a carbon layer obtained by pyrolysis of a gaseous feedstock in the CB reactor, thereby forming carbon-coated particles.

[0035] In further embodiments, a method for producing carbon-coated particles includes preparing CB core particles in a plasma process; and coating the CB core particles with a carbon layer to form carbon-coated particles. In some cases, the CB core particles are prepared by a process that includes generating a plasma in a plasma zone of a reactor; and converting a core-generating FS introduced downstream of the plasma zone of the reactor into CB core particles and hydrogen gas.

[0036] In yet another embodiment, a method for preparing carbon coated particles comprises introducing preformed core particles into a CB reactor or a plasma CB reactor; and coating the core particles with a carbon layer generated from a gaseous FS.

[0037] In a further embodiment, a method for producing carbon coated particles includes coating core particles, such as non-carbon core particles, plasma CB core particles, preformed particles, such as regenerated pyrolytic carbon (also referred to simply in this disclosure as "pyrolytic carbon") particles, degraded CB particles (i.e., particles of CB having inferior rubber reinforcement properties compared to the reinforcement properties expected from their morphology), or other types of CB particles, with a carbon layer in a CB reactor or finishing section thereof.

[0038] The present invention exhibits many advantages. In many implementations, the carbon-based outer region, alone or in conjunction with the core material, provides properties, such as bulk or surface properties, and / or chemical, electrical properties, aggregate and / or primary size distributions, performance-related features, etc. that can be the same, similar, or improved compared to a desired grade of CB.

[0039] The properties of the particles can be tailored for a particular end use, and in some instances, the carbon coated particles are used as reinforcement in tires or other rubber components. In certain implementations, the particles described in this disclosure produce rubber properties and application performance that can be the same, similar, or improved relative to a comparative rubber composition formulated with a given grade of CB, such as an uncoated plasma CB of similar morphology, or a standard ASTM furnace black.

[0040] Having a carbon-based outer layer that can provide the desired CB properties adds a lot of flexibility to the choice of core material. For example, in comparison with conventional CB particles that show good particle-polymer interactions but also strong particle-particle interactions, it is believed that using a silica core, the latter that is easier to disperse and prevents increased rubber hysteresis or energy loss, can reduce particle-particle interactions, while the carbon-based coating promotes particle-polymer interactions and high reinforcement. In combination, these two trends can provide some of the materials described in this disclosure with attractive properties for rubber, e.g., tire applications.

[0041] The methods described herein can also be applied to alter the surface properties of recycled pyrolytic carbon, or CB particles that exhibit poor reinforcement or other properties that have been found to be useful in rubber applications.

[0042] While it may be beneficial to use recycled pyrolytic carbon, for example by compounding it into new rubber compounds, recycled pyrolytic carbon generally provides substantially inferior reinforcement and other rubber properties compared to virgin CB. Among other deficiencies, it is believed that the main problem with recycled pyrolytic carbon compared to virgin CB is that the particle surface is substantially altered and degraded due to interactions with rubber molecules. Aspects of the present invention address these deficiencies and render recycled pyrolytic carbon, or other compounds derived from waste products, more attractive for certain applications, such as rubber reinforcement. This can have significant environmental impacts while facilitating recycling and reducing waste management and treatment burdens.

[0043] Practicing the present invention can also enable the use of lower cost core particles, such as clay, rice husk silica, calcium carbonate, recycled pyrolytic carbon, etc. Since the cores of the particles described in this disclosure can be formed not only from pure or valuable compounds, but also from scraps recovered from other processes, aspects of the present invention can contribute to lower costs for the final product and / or the production of certain CB grades. The incorporation of such core materials into the particles described in this disclosure also reduces the consumption of petroleum-based feeds typically required for the production of CB. Importantly, non-carbon core particles (i.e., composites or agglomerated particles in which the continuous phase is formed from a non-carbon material) can even be formed in situ during the overall production of the materials as described in this disclosure.

[0044] In the production of CB, plasma-based processes can offer substantial economic benefits, such as the use of materials that can often be relatively cheap and widely available, such as natural gas (NG). Other advantages include the typically high yields of useful products, namely carbon (C) and hydrogen (H). 2 ) gas, as well as carbon dioxide (CO 2) or reduced nitrogen oxide (NOx) emissions. However, the resulting CB products may lack some properties associated with the superior performance currently required in tires and other rubber components. When compared to conventional furnace CB, plasma CB may have a lower level of interaction with rubber molecules resulting in inferior reinforcement performance. Thus, in some cases, the present invention utilizes the benefits associated with plasma-based methods of preparing CB while also producing CB surface properties that improve the performance of tire components or other rubber products.

[0045] Certain embodiments of the present invention relate to deagglomerating the core material introduced into the CB reactor; this is believed to promote more efficient and effective coating.

[0046] When used in coating operations, liquid hydrocarbons must first be vaporized and then mixed with the core particles. Due to the very short time available, the resulting deposit may not be as thin and / or uniform as desired. If a gaseous hydrocarbon is used to produce the coating, it may produce a thinner and / or more uniform deposit, since the vaporization step is avoided. Implementations in which the layer formed on the core particles is produced using NG or other gaseous hydrocarbons are not covered by the SO x And / or NO x Emissions can also be reduced or minimized.

[0047] The above and other features of the invention, including various detailed configurations and combinations of parts and other advantages, will be more particularly described with reference to the accompanying drawings and pointed out in the claims. It will be understood that the particular methods and devices embodying the invention are shown by way of example and not as limitations of the invention. The principles and features of the invention can be employed in many different embodiments without departing from the scope of the invention. [Brief description of the drawings]

[0048] In the accompanying drawings, reference characters refer to the same parts throughout the different views. The drawings are not necessarily to scale, emphasis instead being placed upon illustrating the principles of the invention. [Figure 1] FIG. 1 is a cross-sectional view of a reactor suitable for preparing carbon coated particles according to a further embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of an apparatus suitable for preparing carbon coated particles according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a more detailed view of the upper portion of the apparatus of FIG. [Figure 4] FIG. 4 is a cross-sectional view of an apparatus for preparing coated particles using a finishing zone in a CB reactor. [Diagram 5] FIG. 5 is a transmission electron micrograph of a dual-phase particle having a silica core coated with a carbon layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0049] The present invention generally relates to coated particles, and methods of making and using the same. A typical particle contains a core coated with a carbon layer. The core can consist of, consist essentially of, or include a material different from the carbon coating. Generally, the core and coating material have different origins, chemical compositions, and / or other properties. Coated particles can often be considered composite particles with one or more properties different from those of the core. By itself, for example, the core may not have the properties required or desired for a particular end use, such as for superior reinforcement of tire components. Due to the external carbon deposition, the coated particles described in the present disclosure can exhibit different properties and therefore find important applications in reinforced rubber compositions.

[0050] To produce coated particles as described in this disclosure, a core is coated with a carbon layer, which in some embodiments has the morphology and properties of typical carbon black materials.

[0051] In some embodiments, the core material is provided as preformed or pre-manufactured particles. They can be commercially available or prepared in a process and / or equipment other than the process or equipment used to perform the coating operation. Thus, the process by which the preformed core particles are prepared can be independent and often separate from the coating operation. Preformed cores can be composed of virgin materials, materials reclaimed or salvaged from waste products or other products, or both.

[0052] The amount of preformed core material provided can be determined by routine experimentation and can be based on theoretical modeling, prior experience, or other techniques. Factors to consider in determining the amount can include the equipment used, process parameters, type of core material, FS used, and / or other streams used, downstream processing, desired properties, etc.

[0053] In other embodiments, the cores are produced in situ and coated in a common process and / or reactor. In situ techniques may require one or more suitable precursors, i.e., one or more substances that can undergo a reaction under certain conditions to produce the core material. The core precursors can be provided in any suitable amount as determined by routine experimentation, modeling, desired properties of the coated particles, experience, process and / or equipment parameters, or other factors.

[0054] In some cases, the preformed core particle preparation and coating operations are performed in separate steps or units that are part of an overall manufacturing process or system, typically performed in a single facility.

[0055] A variety of core materials can be used. The non-carbon core can be made in whole or in part from, for example, non-carbon materials such as silica, alumina, other metal oxides such as titania, zirconia, ceria, tin oxide, magnesium oxide, magnesium aluminum silicate, clays such as bentonite, natural or synthetic zeolites, regenerated adsorbents, electronic components, catalytic materials, ash, non-carbon nanoparticles, and the like. A core is defined as a "non-carbon core" if the continuous phase in the core is a non-carbon material. Similarly, a core particle, core aggregate, or core agglomerate is a "non-carbon core particle," a "non-carbon core aggregate," or a "non-carbon core agglomerate," respectively, if the continuous phase in the particle, aggregate, or agglomerate is a non-carbon material.

[0056] In one particular example, the core is made of silica, e.g., colloidal silica, PS, recycled PS (e.g., from used tires), carbon black aggregates containing regions of silica (e.g., Ecoblack TM particles), recovered fumed silica, unmodified fumed silica, typically produced by a pyrolytic process, hydrophobically modified fumed, colloidal, or other silica nanoparticles, mixtures containing one or more of silica, etc. The silica core material can be supplied in the form of already manufactured silica core particles. Virgin materials or recovered waste products can be used.

[0057] It is also possible to prepare the silica core in situ. Suitable precursors can consist of, consist essentially of, or include one or more silicon-containing materials, such as organosilicon compounds. Specific examples of compounds that can be used include silicones, such as volatile silicone polymers, such as octamethylcyclotetrasiloxane (OMTS), silicates, such as tetraethoxyorthosilicate (TEDS) and tetramethoxyorthosilicate, silanes, siloxanes, silazanes, etc.

[0058] Other exemplary embodiments include cores consisting of, consisting essentially of, or including clay, rice hull silica, calcium carbonate, nanoparticles of these materials, other nanoparticles, or mixtures thereof. Typically, these core materials are provided as preformed particles.

[0059] Carbon cores may also be used. As used in this disclosure, a core, core particle, core aggregate, or core agglomerate is a "carbon core," "carbon core particle," "carbon aggregate," or "carbon agglomerate," respectively, when the core consists of, consists essentially of, or includes a material whose continuous phase is carbon or CB.

[0060] Some aspects of the invention use CB cores that are produced in whole or in part in a process that uses electrical energy, typically a plasma-based process. The plasma process converts hydrocarbon FS (e.g., methane) into its components, namely carbon (referred to in this disclosure as "plasma carbon black" or "plasma CB" core particles) and hydrogen. For example: CH 4 (g) → C(s) + H 2 (g).

[0061] In addition to carbon and hydrogen, the conversion of hydrocarbons may produce small amounts of acetylene and / or traces of other hydrocarbons. The reaction is often carried out in the absence of oxygen. In cases where oxygen-containing compounds are used, the tail gas contains some CO and CO. 2 the latter typically being present in small or trace amounts.

[0062] According to some methods (see, for example, U.S. Pat. No. 3,409,403), the reaction proceeds as follows: the hydrocarbon FS is first converted to acetylene, and then CB and H 2 The decomposition proceeds through intermediate stages such that

[0063] The plasma CB core particles are, for example, about 50 to about 250 m 2 / g (ASTM D6556) 2 SA surface area; 50~220m 2 / g STSA surface area (ASTM D5816); 50-300 cm 3 / 100g OAN structure (ASTM D2414-16); 40~150cm 3 / 100g COAN structure (ASTM D3493-16); toluene 70-87% (ASTM D1618-99, 2011); pH 7-9; ash content 0.05-0.5% (ASTM D1506); CB yield 60-100%.

[0064] Various approaches to preparing plasma CB are known, as seen, for example, in U.S. Patent No. 5,527,518 to Lynum et al., issued June 18, 1996; U.S. Patent No. 4,101,639 to Surovikin et al., issued July 18, 1978; U.S. Patent Application Publication No. 2008 / 0289494 to Boutot et al., published November 27, 2008; U.S. Patent Application Publication No. 2009 / 0142250 to Fabry et al., published June 4, 2009; U.S. Patent Application Publication Nos. 2015 / 0210856 and 2015 / 0210857 to Johnson et al., both published July 30, 2015; and U.S. Patent Application Publication No. 2015 / 0210858 to Hoermann et al., all of which are incorporated by reference in their entirety into this disclosure.

[0065] Both cold arc and hot arc discharges can be used to prepare plasma CB core particles to be coated. Hot arc discharges create a continuous plasma arc that typically generates reactor temperatures in the range of about 1700°C to about 4000°C and higher, while cold arc discharges can be considered to be intermittent arc discharges that allow the reactor to operate at relatively low temperatures, typically below 200°C. An arrangement based on cold arc discharges to produce solid carbon particles and gaseous components such as hydrogen and acetylene mixed with unreacted methane or natural gas is described, for example, in U.S. Patent Application Publication No. 2008 / 0289494, published Nov. 27, 2008, by Boutot et al.

[0066] Other methods of preparing plasma CB core particles can be used as known in the art or adapted or developed. For example, the core particles can be prepared in a microwave plasma reactor. An example of such a reactor can be found in U.S. Patent Application Publication No. 2007 / 0274893 to Wright et al., published Nov. 29, 2007, and incorporated herein by reference in its entirety. U.S. Patent No. 5,782,085 to Steinwandel et al., published Jul. 21, 1998, and incorporated herein by reference in its entirety, shows a method of generating a plasma jet using microwaves (e.g., in the range of 0.95-24 GHz). The high frequencies used can be generated by a magnetron system or a traveling wave tube. The waves can be guided through a waveguide whose shape is designed to allow only certain types of waves. For example, methods using electromagnetic energy in the microwave, radio, radio, ultra-high, or acoustic frequency ranges can be used, as described in U.S. Patent Application Publication No. 2015 / 0174550 by Tranquilla, published June 25, 2015, and incorporated by reference in its entirety.

[0067] The plasma CB cores can be generated in situ or provided as already manufactured (preformed) plasma CB particles. Suitable solid plasma CB materials in particulate form can be obtained commercially or prepared in processes or equipment other than those used to perform the coating operation.

[0068] Another aspect of the invention utilizes a core consisting of, consisting essentially of, or including recycled pyrolytic carbon. This type of material is obtained from the pyrolysis of waste rubber products, such as used tires. In contrast to the carbon coatings described in this disclosure, recycled pyrolytic carbon typically contains not only carbon, but also other compounds used in the manufacture of tire components, such as alumina, silica, zinc oxide, etc.

[0069] Regenerated pyrolytic carbon can be, for example, 2 / g), structure or DBP No. (cm 3 The carbon can be characterized by properties such as specific surface area, DBP No., ash and / or sulfur content. For exemplary purposes, the specific surface area, DBP No., ash and sulfur content for carbon reclaimed from pyrolyzed truck tires reported by C. Roy (Journal of Analytical and Applied Pyrolysis, Vol. 51, pp. 201-221 (1999)) are 95 m 2 / g;102cm 3 / 100g; 0.7% and 0.5%. Typically, regenerated pyrolytic carbon is provided in the form of already manufactured (preformed) core particles.

[0070] Other types of carbon-based core materials can be used. One illustrative example uses CB prepared or obtained from an independent or separate process and / or equipment and provided as preformed particles. In a specific implementation, the CB particles have inferior reinforcement or other undesirable surface quality or material properties (degraded carbon black) relative to typical carbon blacks with the same or comparable morphology. Such degraded carbon blacks can be purposely manufactured to achieve a desired property at the expense of a different desired property (e.g., producing particles with very high surface area but with a high I2 / STSA ratio and an etched porous surface). Other examples include annealed CB particles, CB particles with low content of polycyclic aromatic hydrocarbons (PAH), or CB products of post-manufacturing treatment of CB that can remove chemical groups from the CB particle surface to create crystalline regions, or thermally anneal, or graphitize the CB particle surface, or otherwise degrade the activity of the CB particle surface to create inferior rubber reinforcement properties. Examples of poor surface quality core CB resulting from full or partial CB graphitization are disclosed, for example, in U.S. Patent No. 4,138,471, issued Feb. 6, 1979 to Lamont et al., and U.S. Patent Application Publication No. 2005 / 063892 to Tandon et al., both of which are incorporated by reference in their entirety into this disclosure.

[0071] The core particles can be provided or generated in situ to have certain characteristics such as average particle size, particle size distribution, microstructure, etc. In many cases, the core particles are aggregates of primary particles or small agglomerates (e.g., containing several aggregates). In many cases, the core aggregates can have an average aggregate size in the range of about 25 nanometers (nm) to about 500 nm, such as about 25 nm to about 200 nm, for example about 25 nm to about 100 nm. In the case of CB materials, such as plasma CB, suitable core particles, i.e., aggregates of primary carbon particles, can have an average aggregate size in the range of about 20 nanometers (nm) to about 500 nm, such as about 25 nm to about 200 nm, for example about 25 nm to 100 nm. The core aggregates can have a characteristic microstructure, such as a tufted morphology, caused in the CB or silica aggregation. The core agglomerates can contain the same or different aggregates.

[0072] Some embodiments of the present invention relate to the use of mixtures of core particles. Any combination of preformed, in-situ formed, virgin, regenerated, and other types of core materials can be used, and mixtures of core particles with different chemical compositions and / or properties can be used. One type of core particle, whether in-situ formed or preformed, can be combined with other carbon or non-carbon core materials and then coated. Thus, other core materials can be prepared in-situ or provided as already manufactured particles. By way of example, examples of other materials that can be added to the plasma CB core particles include, but are not limited to, other types of carbon or CB, such as other CB grades, two-phase particles (e.g., CB and silica), acetylene black, lamp black, graphene, carbon nanotubes, non-carbon materials such as silica, alumina, other metal oxides such as titania, zirconia, ceria, tin oxide, magnesium oxide, magnesium aluminum silicate, clays such as bentonite, natural or synthetic zeolites, regenerated adsorbents, electronic components, catalytic materials, ash, non-carbon nanoparticles, etc.

[0073] To prepare carbon-coated particles, the core is coated with a carbon layer. The carbon layer is produced from a suitable carbon source, often liquid hydrocarbons, such as by-products of coking and olefin production operations, such as decant oils from catalytic cracking operations, coal tar, other petroleum refining sources, etc. Specific examples of carbon-producing FS compositions that can be used to coat the core particles are given in U.S. Patent No. 5,190,739 to MacKay et al., which is incorporated herein by reference in its entirety.

[0074] However, liquid hydrocarbons may contain sulfur (S) and / or nitrogen (N), and therefore the resulting exhaust gas stream may contain SO x And / or NO xSuch a process may require scrubbing or other types of exhaust cleaning to remove waste products such as sintering, sintering, and the like. Thus, in some of the embodiments disclosed herein, the layer deposited on the core particles is generated from a source that is free or substantially free of S and / or N. Examples include, but are not limited to, methane, NG, or another gaseous source (one or more C1-C4 hydrocarbons). Without requiring a vaporization step, the gaseous hydrocarbons can facilitate the formation of a thinner and / or more uniform coating.

[0075] In an illustrative example, a silica core material is coated with carbon produced by pyrolysis of NG, propane, or butane. In some cases, the silica is premixed with a gaseous FS (e.g., NG, propane, or butane), and optionally air. In another illustrative example, the core material coated with a carbon layer produced by pyrolysis of a gaseous hydrocarbon FS (e.g., one or more C1-C4 hydrocarbons), such as methane, NG, and butane, consists of, consists essentially of, or comprises CB particles. For example, CB core particles can be coated with a carbon layer produced by pyrolysis of NG in a CB reactor. These CB core particles can be preformed or produced in situ.

[0076] The core particles are coated in a process carried out in a suitable apparatus. Optionally, the cores themselves are also manufactured in the same process and / or apparatus. Alternatively, or in addition, the core material is coated as a preformed particle. Some exemplary implementations are described below.

[0077] In one embodiment, the coating of the core particles, whether produced in situ or introduced already produced (preformed), is carried out using a process and / or reactor (furnace) suitable for producing CB or in a section of such a reactor. CB processes, reactors or furnaces are known in the art. Examples include, but are not limited to, those described in U.S. Reissue Patent No. 28,974 to Morgan et al., U.S. Reissue Patent No. 3,619,140 to Morgan et al.; U.S. Patent No. 5,877,238 to Mahmud et al.; U.S. Patent No. 5,190,739 to MacKay et al.; International Publication No. 2014 / 140228 to Schcwaiger et al.; U.S. Patent No. 6,277,350 to Gerspacher; U.S. Patent No. 7,097,822 to Godal et al.; U.S. Patent No. 4,582,695 to Dilbert et al.; U.S. Patent No. 6,099,818 to Freund et al.; U.S. Patent No. 6,056,933 to Vogler et al.; and U.S. Patent No. 6,391,274 to Vogler et al. Multi-stage reactors and processes for producing CB are described in U.S. Patent No. 7,829,057, issued November 9, 2010 to Kutsovsky et al., and U.S. Patent Application Publication No. 2007 / 0104636, published May 10, 2007 to Kutsovsky et al. Multi-stage reactors and processes for producing CB and producing composite silicon- or metal-containing CB aggregate particles are disclosed in U.S. Patent No. 5,904,762, issued to Mahmud et al., which are incorporated by reference in their entireties into this disclosure. Other CB reactors and / or methods known in the art can be used.

[0078] In the example shown in Figure 1, hot combustion gases are generated in the combustion zone 1 by contacting a liquid or gaseous fuel stream 9 with an oxidant stream 5, such as air, oxygen, or a mixture of air and oxygen (also referred to in the art as "oxygen-enriched air"). The fuel may be a readily combusted gas, steam, or liquid stream, such as a hydrocarbon (e.g., methane, natural gas, acetylene), hydrogen, alcohol, kerosene, fuel mixture, etc. In many cases, the fuel selected has a high content of carbon-containing components.

[0079] Thus, a variety of gaseous or liquid fuels, such as hydrocarbons, can be used as the combustion fuel. Equivalence ratio is the ratio of fuel to the amount of oxidizer required for the combustion of the fuel. Typical values ​​for equivalence ratio in the combustion zone range from 1.2 to 0.2. The oxidizer stream can be preheated to facilitate the production of hot combustion gases.

[0080] Many embodiments of the present invention relate to a combustion process that completely consumes the combustion fuel. Excess, oxygen, fuel selection, burner design, injection speed, mixing conditions and patterns, fuel to air, oxygen-enriched air or pure oxygen ratio, temperature, and other factors can be adjusted or optimized, for example, to ensure that the combustion produces little or no carbon seeds or nuclei. Rather, in a typical CB process, these nuclei are formed only after the CB-generating FS is introduced into the reactor. When using non-carbon core particles in situ, the delay in the formation of carbon nuclei relative to those of the core particles reduces or minimizes the carbon content in the core.

[0081] The hot combustion gas stream flows downstream from zones 1 and 2 to zones 3 and 4. The coating-producing FS (also referred to in this disclosure as coating FS, carbon-producing FS, CB-producing FS, or CB-FS) is introduced at one or more suitable locations relative to the other reactor components and feeds. In the arrangement shown in Figure 1, coating FS 6 is introduced into reactor zone 3 at injection point 7.

[0082] The coating FS can be injected into the gas stream through a nozzle designed for optimal distribution of the oil in the gas stream. Such nozzles can be single or dual fluid. Dual fluid nozzles can use, for example, nitrogen, steam, or air to atomize the fuel. Single fluid nozzles can be pressure atomized or the FS can be injected directly into the gas stream. In the latter example, atomization occurs due to the force of the gas stream.

[0083] The coating FS can be a liquid or gaseous hydrocarbon that can produce CB, for example, by pyrolysis or partial combustion. Suitable examples include, but are not limited to, petroleum refining sources, such as decant oil from catalytic cracking operations, and by-products from coking and olefin manufacturing operations. Specific examples of carbon-producing FS compositions are given in U.S. Pat. No. 5,190,729 to MacKay et al., which is incorporated by reference in its entirety. NG, methane, hydrocarbons, such as C2-C8 hydrocarbons (propane, butane, ethylene, propylene, butadiene, other gaseous carbon sources, or mixtures of liquid, gaseous, or liquid and gaseous sources can also be used.

[0084] In specific implementations, gaseous hydrocarbons, such as methane, NG, or butane, are reacted in a CB process, reactor, or furnace, e.g., U.S. Reissue Patent No. 28974 to Morgan et al., U.S. Reissue Patent No. 3,619,140 to Morgan et al., U.S. Patent No. 5,877,238 to Mahmud et al., U.S. Patent No. 5,190,739 to MacKay et al., WO 2014 / 140228 to Schwaiger et al., U.S. Patent No. 6,277,350 to Gerspacher, U.S. Patent No. 7,097,822 to Godal et al., U.S. Patent No. 4,097,822 to Dibert et al., U.S. Patent No. 4 ... No. 582,695 to Freund et al.; U.S. Pat. No. 6,099,818 to Freund et al.; U.S. Pat. No. 6,056,933 to Vogler et al.; U.S. Pat. No. 6,391,274 to Vogler et al.; U.S. Pat. No. 7,829,057 to Kutsovsky et al. issued Nov. 9, 2010; U.S. Pat. No. 5,904,762 to Mahmud et al.; and U.S. Patent Application Publication No. 2007 / 0104636 to Kutsovsly et al. published May 10, 2007, to coat in situ the formed CB core particles.

[0085] CB core particles can be generated in situ from a core-generating FS, often one or more liquid hydrocarbons or oils, such as commercially available FS with properties listed in US Pat. No. 5,190,739. Typically, the core-generating FS is introduced into a reactor, such as reactor 50 in FIG. 1, upstream from the injection of the coating FS. Suitable injection points or locations that can be used are described, for example, in US Pat. No. 7,829,057. The core-generating FS can be introduced in any conventional manner, such as a single stream or multiple streams, and the introduction of the FS can occur at any rate. With multiple streams, the rate of each stream can be the same or different.

[0086] In many cases, injection of the core-generating FS is performed to promote penetration into the inner regions of the hot combustion gas stream and / or high rates of mixing and shear of the hot fuel gas and the core-generating FS to ensure that the FS rapidly and completely decomposes and converts to the core CB material.

[0087] With respect to the later introduction of the gaseous coating FS, this second FS can be converted downstream of the core-generating FS in an amount and under conditions suitable for in-situ coating of the CB core particles with a carbon layer. The gaseous coating FS can be used to cool the reactor, which is often to a greater extent than the cooling obtained with an equivalent amount of oil FS. Also, the restriction of the injector tip caused by the oil FS is avoided. In contrast to the use of liquids, e.g., oil, hydrocarbons, the gaseous coating FS can provide environmental benefits and improvements in the quality of the coating.

[0088] A further implementation relates to the introduction of one or more precursors that produce non-carbon core particles in situ. Such precursors can be premixed with the coating FS and introduced into the reaction zone with the FS. In one implementation, the precursors are co-injected with the coating FS6. In another implementation, the precursors are introduced away from the coating FS injection point.

[0089] According to a particular embodiment of the present invention, the carbon coating step follows the in situ formation of the core particles, and the injection point of the core precursor can be determined based on temperature, reactor parameters, reaction kinetics, mixing time and pattern, residence time, etc. Thus, in each case, the precursor can be introduced upstream, downstream, or at the same point as the coating FS injection point. Typically, the precursor is introduced upstream from the injection of the quench fluid. In one implementation, the reaction required for the production of the core particles occurs faster than the one that results in the formation of the carbon material (CB precursor) required for the implementation of the core coating. As a result, the core precursor can be co-injected with the coating FS, or can be injected separately upstream along the reactor, at the same point, and downstream of the injection point of the coating FS. With reference to FIG. 1, for example, a precursor, such as a silicon-containing precursor that produces a silica core, can be co-injected with the coating FS6. If desired, such a precursor can also be introduced upstream or slightly downstream of FS6.

[0090] The amount of precursor used can be determined by routine experimentation, calculation, modeling, experience, etc. Factors to consider include, but are not limited to, the type of material used, the equipment and / or process parameters such as production rate and / or capacity, various input and output streams, the desired properties of the core, etc.

[0091] Conditions that promote the formation of a non-carbon core (in preference to incorporating a carbon continuous phase into the core) include, but are not limited to, the ratio of CB-generating FS to non-carbon precursor, and especially the reactor temperature in the reactor zone. For example, increasing the amount of silicon precursor relative to the CB-generating feedstock favors the formation of a non-carbon core and then the carbon coating process. It is also possible to use a lower-producing CB feedstock, such as certain vegetable oils, such as soybean oil, thus reducing the amount of carbon material available in the reaction zone. Alternatively, or in addition, the reaction zone can be maintained at a sufficiently high temperature to favor the rapid conversion of the precursor to a non-carbon core (i.e., a core in which the continuous phase is a non-carbon material) over the slower conversion of the CB-generating FS to CB. In one example, the reaction zone temperature used to form a silica core from a silicon-containing compound is in the range of about 1680°C to about 1800°C, a temperature at which the silica precursor reacts much faster than the CB-generating FS.

[0092] Preformed core particles (e.g. silica, rice husk silica, clay, precipitated silica, calcium carbonate, nanoparticles, regenerated pyrolytic carbon, plasma CB, other types of pre-made CB, e.g. aged CB (i.e. CB with inferior rubber reinforcement properties compared to the reinforcement properties expected from its morphology), etc.) can be introduced into the reactor as shown in FIG. 1 at a suitable injection point, e.g. upstream or downstream of injection point 7. More than one means and injection points can be used. The preformed core particles can be fed in one of the existing gaseous or vapor reactor feed streams or co-injected with the coating FS (stream 6 in FIG. 4). Alternatively or in addition, the preformed core particles can be dispersed in a liquid stream, e.g. aqueous solution, water, light hydrocarbons, etc., or can be independently introduced into the carrier gas fed to the reactor at a suitable location, e.g. stream 10 in FIG. 1. Inert gas, recycled CB tail gas, and / or other carrier gases can be used. The preformed core particles can be mixed with, e.g. supercritical CO 2or can be introduced with an existing stream, such as the air or fuel stream (streams 5 and 9, respectively, in FIG. 1). At least a portion can be used as fuel in the combustion zone.

[0093] The amount of preformed core material provided can be determined by routine experimentation and can be based on theoretical modeling, prior experience, or other methods. Factors to consider in determining the amount can include the equipment used, process parameters, details of materials used, type of FS and / or other streams used, downstream processing, properties desired, etc.

[0094] In some circumstances, the formation of agglomerates of preformed particles can adversely affect the production of a final product having desired properties, such as properties that provide end-use coating particles suitable for incorporation in rubber compositions for tire applications. This problem can be addressed by homogenizing preformed core particles into the coating FS stream, or by various deagglomeration techniques by milling, such as fluid energy milling, jet milling, or other powder milling equipment immediately prior to injection via a gas carrier stream.

[0095] In one implementation, the preformed core material is dispersed into particles fine enough for effective subsequent coating. For example, the core material can be mixed or homogenized with the liquid carbon-producing FS and injected as a slurry of core particles in the coating FS. The preformed core particles can also be homogenized into water or other aqueous or solvent liquid and then injected separately from the coating FS or after mixing with the coating FS. The preformed core material can also be carried to the reactor by new (see, for example, stream 10 in FIG. 1) or existing (gas) streams, including combustion air streams or natural gas (combustion fuel) streams. Inert gases, recycled CB exhaust gases, and / or other carrier gases can also be used.

[0096] Homogenization of the preformed core particles can be performed as known in the art, for example, homogenizers such as the colloid mill described in U.S. Patent No. 3,048,559, issued August 7, 1962 to Heller et al. Wet-operated micromills can also be used, as can other means of mechanical influence similar to the described micromills, or grinding action similar to the colloid mill. Other examples of suitable homogenizers include, but are not limited to, Microfluidizer® systems commercially available from Microfluidics International Corporation (Newton, Mass., USA); Model MS18, MS45 and MC120 series homogenizers available from APV Homogenizer Division of APV Gaulin, Inc. (Wilmington, Mass., USA), and other commercially available or custom-made equipment.

[0097] A different approach concerns methods designed to coat relatively large (e.g., 200 nm to about 1, 5 or 20 microns) cores. Such agglomerates containing the same or different aggregates can be coated with a CB coating sufficient to provide an "effective" CB layer, i.e., improved reinforcement and / or balance of rubber performance properties compared to an appropriate reference. If the agglomerates can be dispersed to a size less than 20 microns, preferably significantly smaller than 20 microns, the coating of the agglomerates can be as effective as that obtained by coating aggregates of primary particles. A complete coating may not be necessary to realize the associated benefits, for example of carbon-coated silica cores. The CB precursor can penetrate and coat even when only partially core aggregated within the agglomerates. When these coating agglomerates are mixed into rubber, they can be broken down and dispersed sufficiently that those with incomplete coating of the core aggregates provide a beneficial combination of performance and cost.

[0098] Whether introduced as an already manufactured material (preformed) or generated in situ, the core particles move downstream through the reactor and are coated with carbon. Typically, with appropriate heating, the carbon-producing (coating) FS is pyrolyzed to generate a CB precursor that deposits on the core particles. In a reactor such as that of FIG. 1, the coating can begin to occur at any point or after the injection of the coating FS and can continue through one or more subsequent stages.

[0099] The reaction is stopped in a quench zone of the reactor. The quench 8 is located downstream of the reaction zone and sprays a quench fluid, such as water, into the stream of newly formed CB particles. The quench serves to cool the CB particles, reduce the temperature of the gaseous stream, and decrease the reaction rate. Q is the distance from the beginning of the reaction zone 4 to the quench point 8, and varies with the location of the quench. Optionally, the quench can be staged or occur at several points in the reactor. Pressure spraying, gas atomization spraying, or other quenching methods can also be used.

[0100] After quenching, the cooled gas and carbon coated particles pass downstream through any conventional cooling and separation means whereby the product is recovered. Separation of the carbon coated particles from the gas stream is readily accomplished by conventional means such as dust collectors, cyclone separators, bag filters or other means known to those skilled in the art. After the carbon coated particles are separated from the gas stream, they are optionally subjected to a pelletizing process.

[0101] Another embodiment uses plasma CB core particles that are produced in situ and then coated in a stepwise approach. The process and system for performing both the formation of the plasma CB core particles and their subsequent coating with a carbon layer is referred to as "assembly" in this disclosure and is further described below with reference to the embodiments shown in Figures 2, 3 and 4.

[0102] Shown in FIG. 2 by way of example is a reactor 101 comprising a chamber 102 having a cylindrical or other suitable shape. In many cases, the inner wall of the reactor chamber is made of graphite. The formation of the core particle and its coating with a carbon layer is carried out in a reactor zone or region, as further described below. The reactor 101 comprises, as indicated by the arrows, conduits and injection means for supplying plasma gas (PG), a first FS (HC in FIG. 1) and a second (coating) FS (FS). If desired, one or more of these streams can be preheated as known in the art or developed or adapted to the specific process conditions or equipment design. The reactor can include additional inlets, one or more outlets, for example, units for further processing of products, by-products or unreacted materials, valves, flow meters, temperature controllers, devices used to monitor or control the process steps, computer interfaces, automation means, etc., for collecting the products.

[0103] In the illustrative example described in this disclosure, the reactor 101 includes a head section 103 (shown in more detail in FIG. 3) that defines the upper end of the reactor. Attached at this end are three graphite electrodes 108 (only two are shown in FIG. 3). The electrodes are connected to a power source 104 (shown in FIG. 2) capable of transporting a three-phase AC current. The frequency of the current can be the network frequency (50-60 Hz) or any other, e.g. higher, frequency.

[0104] PG is supplied to the reaction chamber 102 at the center of the head section 103 (injection port 107 in FIG. 3) at a flow rate that can be adjusted depending on the nature of the PG and the power. For example, it may be about 0.001 cubic meters per hour (Nm) per kW of power. 3 / h) ~ approx. 0.3Nm 3 / h. Other flow rates can be selected taking into account power requirements, production capacity, specific process parameters, or equipment design, etc., as known in the art or arrived at by calculation, modeling, or routine experimentation. In some implementations, the power supplied to the electrode 8 is about 2.0 MW and the hydrogen PG is about 10 Nm 3 / h ~ approx. 1000Nm 3 / h, for example, about 100 to about 900, about 200 to about 800, about 300 to about 700, about 400 to about 600, for example, about 500 Nm 3 / h to the reactor as described above. Examples of gases other than hydrogen gas that can be used as PG include, but are not limited to, nitrogen, carbon monoxide (CO), inert or noble gases such as argon, helium, and other gases or mixtures of two or more gases, such as 50% by volume of CO and H 2 A mixture of the above may be mentioned.

[0105] The tips of electrodes 108 are positioned in the path of the PG flow and are positioned close enough together to ignite an electric compound arc (when sufficient power is provided by power source 4), generating a plasma in the arc or plasma zone 109. The temperature of this plasma can be controlled, for example, by the PG flow and the power provided to electrodes 108. In certain implementations, the arc zone 109 is optionally viewed through an opening 115, allowing for automatic control of the temperature and / or amount of plasma gas flow.

[0106] The PG stream or jet from the arc zone proceeds downstream. The velocity of the PG flow can be increased by providing a venturi element 111, typically made of graphite, and a converging zone, such as a throat or contraction 120. In some implementations, the lower end of the venturi is formed as a sharp end (rather than as a continuously expanding section) to facilitate the sudden expansion of the PG gas as it enters the reaction zone 110. Other embodiments use a gas throat assembly as described in U.S. Patent Application Publication No. 2015 / 0210858, which is incorporated by reference in its entirety.

[0107] Also introduced into reaction zone 110 is a carbon source (Stream HC in FIG. 2) for preparing plasma CB core particles, also referred to in this disclosure as the "first FS," "core-producing FS," or simply "core FS." In many aspects of the invention, the first FS consists of, consists essentially of, or comprises methane or natural gas. Examples of other suitable materials that can be used include, but are not limited to, hydrocarbons, such as C2-C8 hydrocarbons (e.g., propane, butane, ethylene, propylene, butadiene), light oils, heavy oils, waste oils, pyrolysis oils, biogas, other fuels containing carbon and hydrogen, combinations thereof, and the like.

[0108] The first FS can be injected through one or more (2, 3, 4, 5 or more) ports or injectors at locations 113 located in the wall 112 of the reactor chamber 102. Introducing the core-generating HS below, preferably directly below the venturi 111, is believed to improve mixing with the PG. The first FS can be injected directly or radially toward the center of the reaction zone 110. It can also be injected more tangentially, thus entering the reaction zone 110 away from the center or at an angle of co- or counter-flow. A suitable flow rate for introducing the first FS can be determined based on calculations, modeling, experience, routine experimentation, etc., taking into account the nature of the feedstock, reactor size, production capacity, power, yield, other flow rates and / or other considerations. In some implementations, the first FS, which is methane or natural gas, is injected at a flow rate of about 100 to about 1000 Nm 3 / h, for example, about 200 to about 800, about 300 to about 700, or about 400 to about 600 Nm 32 and 3 at a flow rate in the range of about 10 to about 500 kg / h, such as about 100 to about 400, about 100 to about 300, or about 100 to about 200 kg / h. Higher or lower amounts can also be used. In some cases, the first FS is introduced at a rate of at least 2, 5, 10, 12, 15, 18, 20, 22, 25, 28, 30, 32, 35, or more metric tons per hour.

[0109] The temperature in the reaction zone can be adjusted by controlling one or more parameters, such as the PG flow rate, its temperature, the nature and / or flow rate of the first FS, the power supplied to the electrode 108, and / or other process conditions. In certain examples, the temperature in the reaction zone is in the range of about 900° C. to about 3000° C., such as about 1300° C. to about 1900° C., such as about 1400° C. to about 1800° C. The pressure at which the FS is injected can affect the surface area of ​​the core particles.

[0110] In many cases, the pressure within the reactor is maintained slightly above atmospheric, thus preventing the ingestion of oxygen from the ambient air.

[0111] One or more of the process steps that result in the formation of plasma CB core particles can be designed such that the units operate in individual capacities, for example as described in U.S. Patent Application Publication No. 2015 / 0210857.

[0112] The plasma CB core particles produced in the reaction zone 110 are coated with a carbon layer in a finishing operation in which a second FS (also referred to in this disclosure as a "coating-producing FS" or "coating FS") is pyrolyzed to deposit an activated carbon surface on the plasma CB core particles. Suitable materials that can be used as the second FS include, but are not limited to, decant oil from catalytic cracking operations, by-products from coking operations and olefin production operations, petroleum refinery sources such as ECR fuels. Examples of coating FS compositions can be found in U.S. Patent No. 5,190,739 to MacKay et al., which is incorporated by reference in its entirety into this disclosure. In many embodiments, the second FS is different from the first FS. In other cases, the second FS is the same as the first FS.

[0113] Typically, the second FS is supplied downstream from the injection point of the first FS through one or more ports or injectors at location 114. In the example shown in Figure 3, the second FS may be introduced at or below the convergence zone 116 and injected radially inward from the periphery of the convergence section. The convergence zone 116 includes an optional contraction or throat 122, which allows the plasma CB core particles and H 2 It serves to accelerate the reaction products. The design of the convergence zone 116 can be the same or different from the first convergence zone (Venturi element 111 in FIG. 3). Similarly, the configurations of the first and second throats (120 and 122, respectively) can be the same or different. The taper angle and / or diameter can be selected based on flow rate, capacity, design parameters, and / or other considerations. For example, the throat 122 can be wider than the throat 120 to accommodate additional gases released during pyrolysis of the first FS. In other situations, the diameter of the throat 122 is smaller or equal to that of the throat 120. Cones or other arrangements resulting in smaller rings can also be used.

[0114] In a further embodiment, the finishing operation is carried out without a convergence zone by simply spraying the coating FS into the stream carrying the plasma CB core particles, the coating FS being introduced at one or more suitable locations. Also, approaches that reduce or minimize the distinction between the first stage (formation of the core particles) and the second stage (finishing stage) are possible, as long as the core particles are essentially completely formed (i.e., mass addition to the core particles is essentially complete) before starting the coating operation.

[0115] The injection of the second FS can be performed through a nozzle designed for optimal distribution of the FS in the gas stream. Such a nozzle can be single or dual fluid. Dual fluid nozzles can use, for example, nitrogen steam or air to atomize the fuel. Single fluid nozzles can be pressure atomizers. In some cases, the second FS can be injected through a nozzle designed for optimal distribution of the FS in the gas stream. 4 , H 2 and can be injected directly into the stream containing PG.

[0116] The second FS can be provided in an amount sufficient to produce the desired coating of the core material. The typical ratio of the first FS to the second FS depends on various factors and can be determined by routine experimentation, calculation, prior experience, or other means. The ratio of the first FS to the second FS can be about 10:1 to about 1:10, for example about 3:1 to about 1:1, or about 2:1 to about 1:1 (by weight).

[0117] The temperature facilitating the pyrolysis of the coating FS can be within the range of about 900°C to about 3000°C, for example, about 1300°C to about 1900°C, for example, about 1400°C to about 1800°C.

[0118] The coating or finishing zone (located around and downstream of the injection point 114) can be heated in whole or in part by passing a hot gaseous stream through the reactor. In some implementations, the plasma operation used to form the core particles is carried out at a temperature high enough to provide all the thermal energy required to carry out the coating process. For example, one or more additional plasma sources can be used. Additional or alternative heating can be provided by preheating a second FS, circulating hot exhaust gas in an indirect heat exchange arrangement, or by other means. Suitable temperatures that can be used to preheat the second FS (or other feed used in the methods or apparatuses disclosed herein) are described, for example, in U.S. Pat. No. 3,095,273 issued Jun. 25, 1963 to Austin; U.S. Pat. No. 3,288,696 issued Nov. 29, 1966 to Orbach; U.S. Pat. No. 3,984,528 issued Oct. 5, 1976 to Cheng et al.; U.S. Pat. No. 4,315,901 issued Feb. 16, 1982 ... Gravley et al.; and U.S. Pat. No. 4,315,901 issued Jul. 23, 1982 to Gravley et al. The preheating arrangements may be the same as or similar to those taught in U.S. Patent No. 4,765,964, issued Aug. 23, 1988; U.S. Patent No. 5,997,837, issued Dec. 7, 1999 to Lynum et al.; U.S. Patent No. 7,097,822, issued Aug. 29, 2006 to Godal et al.; U.S. Patent No. 8,871,173, issued Oct. 28, 2014 to Nester et al.; or CA 682982, all of which are incorporated by reference in their entirety into this disclosure. One particular approach uses exhaust gas from a reactor that has been heated, e.g., by plasma heating, and dehydrated, as described, for example, in U.S. Patent No. 7,655,209, issued Feb. 2, 2010 to Rumpf et al., which is incorporated by reference in its entirety into this disclosure.

[0119] In some aspects of the invention, the carbon-producing FS used to coat the plasma CB in situ is introduced into the finishing zone of the CB reactor, for example as described above. Shown in Figure 4 is an apparatus 200 including essentially the arc or plasma zone 109, the reaction zone 110, both, and the finishing zone 202 of a CB reactor, for example reactor 50 of Figure 1, as described above. A second FS is introduced via feed line 214 and injection point 207 at the throat 122. The coating reaction is placed in zone 4, for example by placing a quench 8 downstream of the coating operation.

[0120] By introducing a second FS after the preparation of the core particles is completed, the carbon precursor (generated by pyrolyzing the coating FS to form dehydrogenated molecular fragments) is deposited (coated) onto the surface of the core particles to form a carbon coating.

[0121] Various additional steps can be performed. Turning to FIG. 2, for example, the lower end of the chamber 102 is connected to an extraction means 105 through which the reaction products are removed from the reactor. These can be directed to standard separation means 106, such as a cyclone and / or filter, where the coating particles are separated from the hydrogen and other reaction products or by-products. The hydrogen can be separated from the other exhaust gas components and recycled, for example, as PG or its components. It can be used in other operations at the facility or transported for use off-site. Unreacted HC, acetylene and / or other exhaust gas components can be directed to further use, used up, or added to the unused HC in the production of plasma CB core particles.

[0122] In some embodiments, a plasma reactor, such as a conventional plasma reactor, can be used to coat a coating FS, typically a preformed core particle, such as NG, methane, a hydrocarbon, such as C2-C8 hydrocarbons (e.g., propane, butane, ethylene, propylene, butadiene), light oil, heavy oil, waste oil, pyrolysis oil, biogas, or other coating FS compositions that contain carbon and hydrogen. Because gaseous FS does not require vaporization, more uniform and / or thinner coatings can be produced. In certain instances, the coating FS contains little or no S and / or N, and therefore does not contain SO x And / or NO x Limit emissions and reduce exhaust gas purification requirements.

[0123] The amount of preformed core material can be determined by routine experimentation and can be based on theoretical modeling, prior experience, or other methods. Factors to consider in determining the amount can include the equipment used, process parameters, details of the plasma CB material used, FS used, and / or other streams used, downstream processes, properties desired, etc.

[0124] In an exemplary implementation, dry or wet cake silica is passed through a fluid energy mill with NG as the fluid gas. With reference to Figures 2 and 3, the milled mixture is mixed with a high temperature plasma stream, the NG is dehydrogenated, and carbon is deposited on the silica. The gas and particles can then be separated, for example, by conventional means. The process results in carbon coatings on the silica cores (compared to coatings obtained from fluid FS, which requires vaporization and then mixing), high performance particles from the silica core / C coating, little or no SO x And / or NO x This approach can avoid carbon grit formation because the total carbon amount is less than that required to prepare regular plasma CB.

[0125] Coating FS, H 2, N 2 , or with other suitable plasma gases, such as those mentioned above. In many instances, the injection points of the plasma gas and gaseous FS (preferably downstream, to avoid recirculation behind the electrodes) are selected to reduce or minimize coking of the plasma electrodes. Coking can also be reduced or avoided using microwave plasma processes.

[0126] In some cases, CB plasma core particles are prepared in one step, and then these particles are directed to a finishing step where they are coated with carbon deposition. This type of arrangement is referred to in this disclosure as a "manufacturing line" system, arrangement, or process, and is composed of various steps or unit operations that can be performed independently of each other. In this approach, one step can be stopped, for example for repair or maintenance, while the other can continue to operate. The need to synchronize various operations is reduced or minimized. In other examples, two or more of the steps in a manufacturing line system operate in an interphase manner or simultaneously to increase throughput, minimize energy requirements, realize reuse advantages, and / or other benefits. The manufacturing line system or process can be configured for batch, semi-continuous, or continuous operation. Similar manufacturing line arrangements can be used with cores other than plasma CB cores.

[0127] The coated particles described in this disclosure can be produced simultaneously with the formation of carbon particles, such as conventional CB. A mixture of composite particles and single-phase carbon particles can be used as is.

[0128] The carbon coated particles disclosed in the present disclosure can have a core that is coated entirely or partially (e.g., 99%, 98%, 95%, 90%, 85%, 80%, 75%, 70%, 65%, 60%, 55%, 50%, 45%, 40%, 35%, 30%, 25%, 20%, 15%, 10% or less) with carbon. In certain instances, the coating is amorphous carbon.

[0129] In certain implementations, the carbon layer or shell coats aggregates made of primary particles, such as silica aggregates, having a particle size in the range of about 20 nm to about 500 nm, such as about 25 nm, 50 nm, or 100 nm to about 200 nm, about 200 nm to about 300 nm, or about 200 to about 400 nm. The coating can be as thin as a few nm or less (e.g., about 0.5 to about 5 nm). In many cases, the coating can be about 20 nm thick. For example, the coating can be 0.5 to about 1 nm; 0.5 nm to about 5 nm, 1 nm to about 10 nm; about 1 nm to about 15 nm; or about 1 nm to about 20 nm thick. The resulting coated particles can have a particle size in the range of about 20 nm to about 500 nm.

[0130] The carbon layer can also be deposited on small agglomerates, e.g., agglomerates made of aggregates, having a typical agglomerate or agglomerate size in the range of about 200 nm to about 5 microns, e.g., about 200 nm to about 1 micron, e.g., about 200 nm to about 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, or 900 nm.

[0131] Larger agglomerates (eg, comprising the same or different aggregates and / or agglomerates) can also be coated, eg, having characteristic dimensions of 1 micron or more, often greater than 2, 3, 4, or 5 microns.

[0132] In some cases, the coated particles described herein maintain at least some of the properties characteristic of the core material, for example, when the carbon coating is thin enough and / or does not completely cover the core. In other cases, the carbon coating dominates the overall properties. For rubber applications, a thin coating can preserve the morphology and / or other properties of the core particle in the subsequent rubber compound. A thicker coating can serve to impart primarily CB type properties and rubber performance. In some implementations, the carbon coated particles are designed to balance the properties contributed by the core material and the properties provided by the carbon coating.

[0133] The coated particles can be characterized by the same properties used to analyze CB. These include, but are not limited to, specific surface area, structure, aggregate size, shape, and distribution; and surface chemical and physical properties. CB properties are determined analytically by tests known in the art, such as nitrogen adsorption surface area and static thickness surface area (STSA), another measure of surface area, determined by nitrogen adsorption according to ASTM test procedure D6556-10. Iodine number can be measured using ASTM procedure D-1510-13. CB "structure" describes the size and complexity of CB aggregates formed by the fusion of primary CB particles with each other. As used in this disclosure, CB structure can be measured as the oil absorption number (OAN) of unground CB, expressed as milliliters of oil per 100 grams of CB, according to the procedure described in ASTM D-2414-13. Compressed sample oil absorption number (COAN) measures the portion of the CB structure that is not easily altered by the application of mechanical stress. COAN is measured according to ASTM D3493-13. Aggregate size distribution (ASD) is measured according to ISO 15825 method using disc centrifuge photosedimentation velocity measurement with a model BI-DCP manufactured by Brookhaven Instruments.

[0134] CB materials having properties suitable for a particular application can be selected and defined by Cabot Corporation specifications (see the website www.cabot-corp.com) or specifications for other commercially available grades, by ASTM standards (see, for example, the ASTM D1765-03 Standard Classification System for Carbon Blacks Used in Rubber Products).

[0135] The coated particles disclosed in this disclosure have a 5 mm viscoelasticity measured by the Brunauer / Emmett / Teller (BET) method according to the procedure of ASTM D6556. 2 / g~300m 2 / g, e.g. 50m 2 / g~300m 2 / g, e.g. 100m 2 / g~300m 2 / g. In some cases, the BET surface area is about 100 m 2 / g~about 200m 2 In other cases, the BET surface area is in the range of about 200 m 2 / g~about 300m 2 The oil absorption number (OAN) can be 40mL / 100g to 200mL / 100g, for example 60mL / 100g to 200mL / 100g, for example 80mL / 100g to 200mL / 100g, for example 100mL / 100g to 200mL / 100g, or 120mL / 100g to 200mL / 100g, mL / 100g 140mL / 100g to 200mL / 100g mL / 100g, 160 to 200mL / 100g, or for example 40mL / 100g to 150mL / 100g, or 40mL / 100g to 150mL / 100g. The STSA is about 5m 2 / g ~ approx. 275m 2 / g, for example, about 30m 2 / g ~ approx. 250m 2 / g, for example 30m 2 / g~200m 2The COAN can be in the range of about 40 mL / 100 g to about 150 mL / 100 g, such as about 55 mL / 100 g to about 150 mL / 100 g, for example, 80 mL / 100 g to 120 mL / 100 g. In certain implementations, the carbon coated particles have a viscosity of about 30 to about 250 μm. 2 In another embodiment, the STSA is in the range of about 30 to about 250 m / g; and the COAN is in the range of about 55 to about 110 cc / 100 g. 2 / g; COAN is in the range of about 55 to about 150 cc / 100g. In some cases, the coated particles disclosed herein have a viscosity of about 30 to about 250 m. 2 / g and an OAN in the range of about 55 to about 400 cc / 100g.

[0136] In some instances, the carbon core and the carbon outer region exhibit different properties and different levels of interaction with elastomer molecules and performance in rubber composites. In an assembly process, such as the plasma process described above, the properties of the core particles can be determined by carrying out the entire process without adding a second FS, and thus obtaining uncoated core particles that can be examined by one or more suitable methods. The introduction of a second FS produces coated particles that can also be examined. The results obtained for the core particles and the results obtained for the coated particles can then be compared. If desired, correlations in performance can be estimated.

[0137] Other approaches can be used, for example a core using regenerated pyrolytic carbon can be distinguished from an outer carbon layer based on elements typically present in the core and not found in carbon coatings (e.g. alumina, silica, zinc oxide, etc.).

[0138] The coated particles described in this disclosure can be further processed, if desired, for example, they can be surface treated or surface modified by methods known and practiced for CB materials.

[0139] Thus, coated particles can be prepared that contain ionic or non-ionic small molecules and / or polymers adsorbed to their surfaces.

[0140] In certain examples, the carbon-coated particles have functional groups (e.g., from ionic or non-ionic small molecules or polymers) directly attached to the carbon surface. Examples of functional groups that can be directly (e.g., covalently) attached to the surface of CB particles and methods for carrying out surface modification are described, for example, in U.S. Patent No. 5,554,739 to Belmont, issued September 10, 1996, and U.S. Patent No. 5,922,118 to Johnson et al., issued July 13, 1999, both of which are incorporated by reference in their entirety into this disclosure. As an example, a surface-modified CB that can be used in this disclosure is a CB prepared by reacting sulfanilic acid or para-amino-benzoic acid (PABA) with HCl and NaNO. 2 Surface modification with diazonium salts, for example, by the sulfanyl or para-aminobenzoic acid process, results in CBs with an effective amount of hydrophilic moieties on the carbon coating.

[0141] Other methods that can be used to provide surface-bound functional groups to carbon-coated particles are described in US Pat. No. 7,300,964, issued Nov. 27, 2007 to Niedermeier et al.

[0142] Oxidized (modified) carbon coated particles can be prepared similarly to those used on CBs described, for example, in U.S. Patent No. 7,922,805 to Kowalski et al., issued April 12, 2011, and U.S. Patent No. 6,471,763 to Karl, issued October 20, 2002, which are incorporated herein by reference in their entirety. Oxidized carbon coated particles are those that have been oxidized using an oxidizing agent to introduce ionic and / or ionizable groups onto the surface. Such particles can have a higher degree of oxygen-containing groups on the surface. Oxidizing agents include, but are not limited to, oxygen gas, ozone, peroxides, such as hydrogen peroxide, persulfates such as sodium and potassium persulfate, hypohalites such as sodium hypochlorite, oxidizing acids such as nitric acid, and transition metal containing oxidizing agents, such as permanganates, osmium tetroxide, chromium oxide, or cerium ammonium nitrate. Mixtures of oxidizing agents can also be used, particularly mixtures of gaseous oxidizing agents, such as oxygen and ozone. Other surface modification methods such as chlorination and sulfonylation can also be used to introduce ionic or ionizable groups.

[0143] In certain embodiments, the coated particles are surface modified by the methods of US Pat. No. 8,975,316 to Belmont et al., which is incorporated by reference in its entirety.

[0144] The coated particles can be used in a variety of applications, for example as reinforcement for rubber products, such as tire components. Without wishing to be bound by a particular mechanism, it is believed that the activity of CB rubber interaction is directly or indirectly related to the type of molecules on which the CB surface is formed.

[0145] A further aspect of the present invention relates to the end use of the coated particles described in the present disclosure, including, for example, unmodified or surface-modified carbon coated particles.For example, the particles can be incorporated into rubber articles used in, for example, tire threads, especially treads of passenger car, light vehicle, truck and bus tires, off-the-road ("OTR") tires, aircraft tires, etc.; subtreads; wire skim, sidewalls, cushion rubber of reprocessed tires; and other tire applications.In other applications, the particles can be used in industrial rubber articles, such as engine mounts, hydro mounts, bridge bearings and seismic isolators, tank trucks or treads, mining belts, hoses, gaskets, seals, blades, gap filling articles, bumpers, vibration-resistant parts, etc.

[0146] The particles can be added in place of or in addition to conventional reinforcement agents for tire components and / or other industrial rubber end uses. In many cases, it is provided in the same or similar manner as known methods for introducing virgin CB into rubber products. For example, the materials described in this disclosure can be combined with natural and / or synthetic rubber in a suitable dry mixing process based on an internal batch mixer, a continuous mixer, or a roll mill.

[0147] Alternatively, the coating particles described herein can be mixed into rubber via a liquid masterbatch process. For example, a slurry containing the particles described herein can be mixed with an elastomer latex in a vat and then coagulated by the addition of a coagulant such as an acid using the method described in U.S. Pat. No. 6,841,606.

[0148] In certain embodiments, the particles are introduced according to the teachings of U.S. Patent No. 6,048,923, issued April 11, 2000 to Mabry et al., which is incorporated herein by reference in its entirety. For example, a method for preparing an elastomer masterbatch can include simultaneously feeding a particulate filler fluid and an elastomer latex fluid into a mixing zone of a coagulation reactor. The coagulation zone extends from the mixing zone, preferably from the inlet end to the discharge end, with a gradually increasing cross-sectional area in the downstream direction. The elastomer latex can be natural or synthetic, and the particulate filler comprises, consists essentially of, or consists of such materials. The particulate filler is fed into the mixing zone, preferably as a continuous high velocity jet of injection fluid, while the latex fluid is fed at a lower velocity. The velocity, flow rate and particulate concentration of the particulate filler fluid are sufficient to cause the mixture to undergo high shear of the latex fluid and flow turbulence of the mixture in at least the upstream portion of the coagulation zone to substantially completely coagulate the elastomeric latex with the particulate filler prior to the discharge end. Substantially complete coagulation can occur without the need for acid or salt coagulants. Additional elastomer can be added to the material exiting the discharge end of the coagulation reactor as disclosed in U.S. Pat. No. 6,075,084, which is incorporated herein by reference in its entirety. The coagulate can then be fed to a dewatering extruder as disclosed in U.S. Pat. No. 6,929,783, which is incorporated herein by reference in its entirety. Other examples of suitable masterbatch processes are disclosed in U.S. Pat. No. 6,929,783 to Chung et al.; U.S. Patent Application Publication No. 2012 / 0264875 to Berriot et al.; U.S. Patent Application Publication No. 2003 / 0088006 to Yanagisawa et al.; and European Patent No. 1,834,985 to Yamada et al.

[0149] The particles can be evaluated in a suitable rubber formulation using natural or synthetic rubber. The suitable amount of coating particles to be used can be determined by routine experimentation, calculation, taking into account factors such as the typical amount of standard ASTM furnace black in a comparable manufacturing process, process specific parameters and / or equipment used, the presence or absence of other additives, and the properties desired in the final product.

[0150] The performance of the coated particles described herein as toughening agents for rubber compounds can be evaluated, for example, by determining the performance of the rubber composition using the particles against the performance of a comparable rubber composition that is similar in all respects except for using a CB grade appropriate for a given application. In another approach, the values ​​obtained for the compositions prepared according to the present invention can be compared with values ​​known in the art related to the parameters desired in a given application.

[0151] Suitable tests include the Green Rubber Test, the Cure Test, and the Cured Rubber Test. Among the suitable Green Rubber Tests, ASTM D4483 describes the test method for the ML1+4 Mooney Viscosity Test at 100° C. Scorch time is measured according to ASTM D4818.

[0152] Cure curves are obtained with a Rubber Process Analyzer (RPA2000) at 0.5°, 100 cpm, and 150c (NR) to 160C (SBR) according to ASTM D5289.

[0153] The performance properties of the cured samples can be determined by a series of suitable tests. Tensile strength, elongation at break, and stress at various strains (e.g., 100% and 300%) are all obtained via ASTM D412 Method A. Dynamic mechanical properties including storage modulus, loss modulus, and tan δ are obtained by strain sweep testing at 10 Hz, 60C, and various strain amplitudes from 0.1% to 63%. Shore A hardness is measured according to ASTM D2240. Tear strength of die B cured rubber samples is measured according to ASTM D624.

[0154] The undispersed area is calculated by analyzing images obtained by a reflected mode optical microscope on a cut cross-sectional area of ​​the cured rubber compound according to various reported methods. Dispersion can also be expressed by the Z value (measured after reticulation according to the method described by S. Otto and Al in Kautschuk Gummi Kunststoffe, 58 Jahrgang, NR7-8 / 2005, entitled New Reference value for the description of Filler Dispersion with the Dispergrader 1000NT). Standard ISO 11345 describes a visual method for the rapid relative assessment of the degree of CB and CB / silica macrodispersion in rubber.

[0155] Abrasion resistance is quantified as an index based on friction loss of cured rubber by Cabot Abrader (Lamboun type). Attractive abrasion results may indicate favorable friction properties. Good hysteresis results may correlate with lower rolling resistance (and correspondingly higher fuel economy) for motor tire applications, reduced heat generation, tire durability, tread and casing life, motor fuel economy properties, etc.

[0156] The invention is further described by the following non-limiting examples.

[0157] Example 1 The experiments were carried out in a pilot plant using a CB reactor as shown in Figure 1. The conditions for runs A, B and C are shown in Table 1.

[0158] In each case, a combustion zone equivalence ratio of 1.43 to 1.67 was used. This constitutes a 30-40% fuel-rich combustion reaction. The primary fuel for the combustion reaction was natural gas, introduced into the reactor through stream 9. The natural gas fed to the CB formation process was at approximately ambient temperature of about 77°F. The liquid carbon FS used was a commercially available FS with typical properties listed in U.S. Patent No. 5,190,739 to MacKay et al. The precursor forming the silica core was octamethylcyclotetrasiloxane [D4] (Xiameter® brand) supplied by Dow Corning coportation, Midland, MI. Both the CB-generating FS and the precursor were co-injected in the presence of a stream of hot gases formed in the combustion zone in zone 3 through stream 6. The liquid silicon-containing precursor and the liquid CB-generating FS were introduced into the process in varying amounts as shown in Table 1. The reaction was stopped using a water quench in zone 8.

[0159] [Table 1]

[0160] The resulting particles having a silica core and a carbon coating, prepared as described above and having the properties shown in Table 1, were observed by transmission electron microscopy (TEM).

[0161] Samples were prepared by sonication in alcohol and chloroform and dropping onto holey carbon grids. Dispersion was found to be sufficient to obtain the appearance of aggregates above the holes. As shown in Figure 5, the dominant microstructure was tufted silica coated by a 1-5 nm thick layer of carbon. This was determined by the amorphous contrast of the silica core and the turbostratic fringes of the carbon coating. The carbon-coated silica aggregates as a whole rather than as individual primary particles. Some single-phase CB particles were also observed.

[0162] Example 2 Ground rice husk particles containing about 20% naturally occurring nano-silica domains are added to preheated air fed to the combustion zone by a mass loss feeder (Schenck AccuRate Mechatron MC Feeder manufactured by Schenck Process, Chagrin Falls, OH) in stream 5 in FIG. 1. The air is enriched to 25% oxygen. The process is carried out in a reactor as shown in FIG. 1. The particles are conveyed through the combustion zone and due to the presence of high temperature and excess oxygen in both the air duct and especially in the combustion zone, a significant portion of the external carbonaceous material in the rice husk is vaporized leaving small domains of silica behind. These particles are conveyed with the combustion gases to the reaction zone (zone 3 in FIG. 1). The CB FS is sprayed into the combustion gas stream via stream 6 perpendicular to the flow and vaporized, after which nucleation and pyrolysis begins to occur. Due to the presence of a large amount of silica particles in the combustion zone, deposition is favored over nucleation and most of the CB formed is deposited as a coating on the existing silica particles. The reaction mixture is quenched downstream (zone 8) with water to cool the coated particles and stop the pyrolysis reaction. The result is particles with an interior composed mainly of silica and an outer coating of CB. Table 2 shows the various input flow rates to the reactor.

[0163] [Table 2]

[0164] Example 3 160m 2 PS with a surface area of ​​10000 / g is mixed with CB FS in a shear mixing tank along with a suitable surfactant to produce a slurry of 30 wt% PS. The process is carried out in a reactor as shown in Figure 1. Combustion fuel is burned with excess air in combustion zone 1 and the hot product gas is conveyed downstream to reaction zone 3. The CB FS / PS slurry is injected into the reactor through stream 6 under pressure perpendicular to the combustion gas flow. The FS is first vaporized leaving a porous liquid-like domain behind the silica. As the vaporized CB FS begins to pyrolyze and condense, deposition onto the silica particles dominates the nucleation and most of the CB formed is a coating on the existing silica particles. The reaction mixture is quenched downstream (zone 8) with water to cool the coated particles and stop the pyrolysis reaction. Table 3 shows the various input flow rates to the reactor.

[0165] [Table 3]

[0166] Example 4 Regenerated pyrolytic carbon particles are added upstream of the reactor to preheated air (stream 5 in FIG. 1) fed to the combustion zone by a mass loss feeder (Schenck AccuRate Mechatron MC Feeder manufactured by Schenck Process, Chagrin Falls, OH). The air is enriched to 25% oxygen. The particles are conveyed through the combustion zone and due to the high temperature and the presence of excess oxygen in both the air duct and especially in the combustion zone, a significant portion of the particles are vaporized leaving some portion of the particles remaining in the combustion gas stream. The carbon consumed in the combustion zone is replaced by natural gas as the combustion fuel. The particles are conveyed with the combustion gas to the reaction zone (zone 3 in FIG. 1). The CBFS is sprayed into the combustion gas stream via stream 6 perpendicular to the flow and vaporized, after which nucleation and pyrolysis begin to occur. A carbon coating is deposited on the regenerated pyrolytic carbon cores. The reaction mixture is quenched downstream (zone 8) with water to cool the coated particles and stop the pyrolysis reaction. The result is particles with an interior composed primarily of regenerated pyrolytic carbon and an outer coating of CB. Table 4 gives the various input flow rates to the reactor.

[0167] [Table 4]

[0168] Example 5 Approximately 160m in the form of wet cake 2PS with a surface area (SA) of 1000 / g is ground using a fluid energy mill. The ground material is conveyed to the combustion zone through stream 10, which can be a gas such as air or nitrogen. Water is driven off by heat from the combustion reaction and the silica particles are entrained in the combustion gas stream. CB FS is sprayed into the combustion gas stream via stream 6, perpendicular to the combustion stream, and vaporized, after which nucleation and pyrolysis begins to occur. A carbon coating is deposited on the PS cores. The reaction mixture is quenched downstream (zone 8) with water to cool the coated particles and stop the pyrolysis reaction. The result is a particle with an interior composed mainly of silica and an outer coating of CB. Various input flow rates to the reactor are shown in FIG. 5.

[0169] [Table 5]

[0170] Example 6 In a plasma reactor as shown in FIG. 3 A hydrogen flow of 1000 kg / h is added through port 107. The electrode (108) is powered with 2.0 MW to create a hot plasma gas. The hot plasma gas passes through a 2.5 inch diameter throat 120 with increasing velocity. At injection location 13, 150 kg / h of liquid hydrocarbon FS is added to the hot plasma gas flowing through three radially arranged pressurized nozzles (each with a 0.5 mm orifice, 700 psig). The liquid carbon FS used is decant oil (commercially available CB FS). When mixed with the hot plasma gas, the liquid hydrocarbon FS undergoes pyrolysis to form CB and hydrogen gas. The hot H 2 The mixture of CB and other exhaust gases is then accelerated through a convergence zone 116 and a contraction (throat) 122 having a diameter of 3 inches, and a second injection at location 114 of 75 kg / h of liquid carbon FS (also decant oil) is added to the mixture through three radially arranged pressurized tips (each with a 0.4 mm orifice, 400 psig).2 The second FS pyrolysis into preferentially coats the plasma CB core particles formed in zone 110, increasing their mass, decreasing their surface area, and increasing their structure.

[0171] Example 7 In a plasma reactor as shown in FIG. 3 A hydrogen flow of 440 Nm / h is added through port 107. The electrode (108) is powered at 2.0 MW to create a hot plasma gas. The hot plasma gas passes at increasing velocity through a 2.5 inch diameter throat 120. At point 113, a pressure of 440 Nm 3 / h of methane is injected into the plasma gas through three radially arranged injection ports, each with a diameter of 6.5 mm. Upon collision and mixing with the plasma gas, methane undergoes pyrolysis to form CB and hydrogen gas. High temperature H 2 The mixture of CB and other exhaust gases is then accelerated through a convergence zone 116 and a contraction (throat) 122 having a diameter of 3 inches, and a second injection at location 114 of 75 kg / h of liquid carbon FS (also decant oil) is added to the mixture through three radially arranged pressurized tips (each with a 0.4 mm orifice, 400 psig). 2 The second FS pyrolysis into preferentially coats the plasma CB core particles formed in zone 110, increasing their mass, decreasing their surface area, and increasing their structure.

[0172] While the present invention has been particularly shown and described with reference to preferred embodiments, it will be understood by those skilled in the art that various changes in form and details can be made therein without departing from the scope of the invention as encompassed by the appended claims.

Claims

1. 1. A method for producing carbon coated particles, comprising coating a core particle with a carbon layer in a CB reactor or finishing section thereof to form a carbon coated particle, wherein the core particle is a non-carbon core particle, a plasma CB core particle or a preformed core particle.

2. The method of claim 1 , wherein the carbon bed is prepared from a carbon-producing liquid or gaseous feedstock.

3. The method of claim 1 , wherein the non-carbon core particles or plasma CB core particles are generated in situ.

4. The method of claim 1 further comprising introducing preformed core particles into the CB reactor.

5. The method of claim 4 , wherein the preformed core particles are CB core particles, recycled pyrolytic carbon particles, non-carbon core particles, or any combination thereof.

6. The carbon coated particles are about 30 to about 250 mm 2 10. The method of claim 1, wherein the polymer has a STSA in the range of about 55 to about 110 cc / 100 g; and a COAN in the range of about 55 to about 110 cc / 100 g.

7. The carbon coated particles are about 30 to about 250 mm 2 10. The method of claim 1, wherein the polymer has a STSA in the range of about 55 to about 150 cc / 100 g; and a COAN in the range of about 55 to about 150 cc / 100 g.

8. The carbon coated particles are about 30 to about 250 mm 2 10. The method of claim 1, wherein the polymer has a STSA in the range of about 100 to about 200 cc / 100 g; and an OAN in the range of about 55 to about 400 cc / 100 g.

9. A rubber composition or rubber article comprising carbon coated particles prepared by the method of claim 1.

10. The method of claim 1 further comprising modifying the surface of the carbon coated particles.

11. generating core particles in situ, the core particles being plasma CB core particles or non-carbon core particles; and Coating the core particles with a carbon layer in a CB process to form carbon-coated particles.

1. A method for preparing carbon coated particles, comprising:

12. The method of claim 11 , wherein the carbon bed is formed from a liquid or gaseous carbon-producing feedstock.

13. The method of claim 11 , wherein the plasma CB core particles are formed in a plasma process.

14. The method of claim 11 , wherein the non-carbon core particles are produced in a reaction zone of a CB reactor.

15. The method of claim 11 , wherein the non-carbon core particle is a silica core particle.

16. The method of claim 11 , wherein the non-carbon core particles are produced from a core precursor.

17. 17. The method of claim 16, wherein the core precursor is introduced upstream, at the injection point, or downstream relative to the carbon-producing feedstock injection point.

18. The method of claim 16 , wherein the core precursor is co-injected with the carbon-producing feedstock.

19. 17. The method of claim 16, wherein the core precursor is introduced prior to the injection of the quench fluid.

20. The method of claim 11 further comprising collecting the carbon coated particles from the reactor.

21. The method of claim 11, wherein the carbon layer is in the range of about 0.5 nm to about 20 nm thick.

22. The method of claim 11 , wherein the core particle is an aggregate of primary particles.

23. The method of claim 11, wherein the coating particles have a particle size in the range of about 20 nm to about 500 nm.

24. The method of claim 11 , wherein the carbon layer partially or completely covers the core particles.

25. The carbon coated particles are about 30 to about 250 mm 2 12. The method of claim 11, wherein the polymer has a STSA in the range of from about 55 to about 110 cc / 100 g; and a COAN in the range of from about 55 to about 110 cc / 100 g.

26. The carbon coated particles are about 30 to about 250 mm 2 12. The method of claim 11, wherein the polymer has a STSA in the range of from about 55 to about 150 cc / 100 g; and a COAN in the range of from about 55 to about 150 cc / 100 g.

27. The carbon coated particles are about 30 to about 250 mm 2 12. The method of claim 11, wherein the polymer has a STSA in the range of about 55 to about 400 cc / 100 g; and an OAN in the range of about 55 to about 400 cc / 100 g.

28. A rubber composition or rubber article comprising carbon coated particles prepared by the method of claim 11.

29. The method of claim 11 further comprising modifying the surface of the carbon coated particles.

30. Introducing preformed core particles into a CB reactor; and Coating the core particles with a carbon layer obtained by pyrolysis of a liquid or gaseous feedstock in a CB reactor, thereby forming carbon-coated particles. A method for producing carbon-coated particles, comprising:

31. 31. The method of claim 30, further comprising deagglomerating the preformed core particles prior to introducing the preformed core particles into the CB reactor.

32. 31. The method of claim 30, wherein the preformed core particles are introduced with a gaseous or vapor reactor stream and dispersed in the liquid feedstock, the separated gaseous stream, or the separated aqueous stream.

33. 31. The method of claim 30, further comprising collecting the carbon coated particles from the reactor.

34. 31. The method of claim 30, wherein the preformed core particle is a preformed non-carbon core particle, a preformed CB particle, or a regenerated pyrolytic carbon particle.

35. 31. The method of claim 30, wherein the preformed core particles are nanoparticles of clay, rice hull silica, precipitated silica, or calcium carbonate.

36. 31. The method of claim 30, wherein the carbon coated particles contain a core that is an aggregate or an agglomerate of the same or different aggregates.

37. The method of claim 36, wherein the core has a size in the range of about 50 nm to about 10 microns.

38. The method of claim 30, wherein the carbon layer has a thickness in the range of about 0.5 nm to about 20 nm.

39. 31. The method of claim 30, wherein the carbon layer partially or completely covers the core.

40. The carbon coated particles are about 30 to about 250 mm 2 31. The method of claim 30, wherein the polymer has a STSA in the range of from about 55 to about 110 cc / 100 g; and a COAN in the range of from about 55 to about 110 cc / 100 g.

41. The carbon coated particles are about 30 to about 250 mm 2 31. The method of claim 30, wherein the polymer has a STSA in the range of from about 55 to about 150 cc / 100 g; and a COAN in the range of from about 55 to about 150 cc / 100 g.

42. The carbon coated particles are about 30 to about 250 mm 2 31. The method of claim 30, wherein the polymer has a STSA in the range of about 55 to about 400 cc / 100 g; and an OAN in the range of about 55 to about 400 cc / 100 g.

43. 31. The method of claim 30, further comprising modifying the surface of the carbon coated particles.

44. 31. A rubber composition or rubber article comprising carbon coated particles prepared by the method of claim 30.

45. Introducing preformed core particles into a plasma CB reactor; and Coating the core particles with a carbon layer generated from gaseous FS 1. A method for preparing carbon coated particles, comprising:

46. Preparing CB core particles in situ in a CB reactor; and Coating the CB core particles with a carbon layer obtained by pyrolysis of a gaseous feedstock in a CB reactor, thereby forming carbon-coated particles.

1. A method for preparing carbon coated particles, comprising:

47. Preparing CB core particles in a plasma process; and Coating the CB core particles with a carbon layer to form carbon-coated particles. A method for producing carbon-coated particles, comprising:

48. The CB core particle is generating a plasma within a plasma zone of the reactor; and Converting the core-producing FS into CB core particles and hydrogen gas 48. The method of claim 47, prepared by a process comprising:

49. Carbon coated particles, including a non-carbon core, a regenerated pyrolytic carbon core, or a plasma CB core coated with a carbon layer.

50. 50. The carbon coated particle of claim 49, wherein the non-carbon core is formed from a material selected from the group consisting of precipitated silica, fumed silica, surface modified silica, and any combination thereof.

51. 50. The carbon coated particle of claim 49, wherein the core is formed from nanoparticles of clay, rice hull silica, calcium carbonate, and any combination thereof.

52. 50. The carbon coated particle of claim 49, wherein the carbon layer is about 0.5 nm to about 20 nm thick.

53. 50. The carbon coated particle of claim 49, wherein the carbon layer is amorphous carbon.

54. 50. The carbon coated particle of claim 49, wherein the core has a tufted microstructure.

55. Approximately 30 to approximately 250m 2 50. The carbon coated particles of claim 49, having a STSA in the range of from about 55 to about 110 cc / 100 g; and a COAN in the range of from about 55 to about 110 cc / 100 g.

56. Approximately 30 to approximately 250m 2 50. The carbon coated particles of claim 49, having a STSA in the range of from about 55 to about 150 cc / 100 g; and a COAN in the range of from about 55 to about 150 cc / 100 g.

57. The carbon coated particles are about 30 to about 250 mm 2 50. The method of claim 49, having a STSA in the range of about 55 to about 400 cc / 100 g; and an OAN in the range of about 55 to about 400 cc / 100 g.

58. 50. A rubber composition or rubber article comprising the particles of claim 49.

59. 50. The carbon coated particle of claim 49, wherein the surface of the coated particle is modified.

60. Plasma zone; a reaction zone downstream of the plasma zone; a finishing zone downstream of the reaction zone; a conduit for introducing a plasma gas into the plasma zone; one or more inlets for introducing a first feedstock into the reactor; one or more inlets for introducing a second feedstock into the reactor; A convergence zone between the plasma zone and the reaction zone; and Optionally, a convergence zone between the reaction zone and the finishing zone. An apparatus for preparing carbon coated particles, comprising:

Citation Information

Patent Citations

  • Method and system for preparing regenerative carbon black by deashing and modifying pyrolytic carbon of waste rubber and plastic products

    CN103540172A

  • Heat treatment method for carbon material

    JP1999513051A

  • Method and apparatus for producing fullerenes

    JP2002504057A

  • Carbon particles coated with a polymer film, method for producing the same, and use

    JP2012505277A

  • Method for recycling carbonaceous materials from waste tires and products derived from waste tires

    JP2012521443A