Resin composition
A resin composition with a long-chain aliphatic hydrocarbon group, epoxy resin, and active ester compound addresses the challenge of enhancing crack and desmear resistance in insulating layers, ensuring stable wiring and reduced transmission loss in high-density circuit boards and semiconductor packages.
Patent Information
- Application Number
- JP2024138457
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The increasing wiring density in circuit boards and semiconductor chip packages has led to a need for improved crack resistance and desmear resistance in insulating layers, as conventional stress-relieving components enhance crack resistance but compromise desmear resistance, leading to surface roughness and transmission loss.
A resin composition comprising a specific combination of a long-chain aliphatic hydrocarbon group-containing phenolic curing agent, epoxy resin, and active ester compound, which forms a crosslinked structure that absorbs stress and resists oxidation, maintaining both crack and desmear resistance.
The resin composition achieves a cured product with excellent crack resistance and desmear resistance, supporting stable thin wiring and reducing transmission loss, while maintaining low dielectric properties and adhesion with conductor layers.
Smart Images

Figure 2024159834000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition. The present invention also relates to a cured product, a sheet-like laminate material, a resin sheet, a circuit board, a semiconductor chip package, and a semiconductor device using the resin composition. [Background technology]
[0002] In general, an insulating layer is provided on a circuit board and a semiconductor chip package. For example, an interlayer insulating layer may be provided as an insulating layer on a printed wiring board, which is a type of circuit board. In addition, for example, a rewiring formation layer may be provided as an insulating layer on a semiconductor chip package. These insulating layers are usually formed of a cured product obtained by curing a resin composition. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-23714 A [Patent Document 2] JP 2020-136542 A [Patent Document 3] JP 2019-48952 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, with the progress of high density wiring in circuit boards and semiconductor chip packages, there is a demand for improving the crack resistance of insulating layers. The present inventors have attempted to use a component capable of relaxing stress in a cured product (hereinafter sometimes referred to as a "stress relaxation component") in order to improve crack resistance. However, it has been found that when a conventional stress relaxation component is used, crack resistance can be improved, but desmear resistance tends to be low. When desmear resistance is low, the surface roughness of the insulating layer after desmear treatment increases, and transmission loss may increase due to the skin effect. In addition, it becomes difficult to stably form thin wiring on the insulating layer, which may hinder high density wiring.
[0005] The present invention has been made in view of the above problems, and has an object to provide: a resin composition capable of giving a cured product having excellent crack resistance and desmear resistance; a cured product of the resin composition; a sheet-like laminate material and a resin sheet containing the resin composition; and a circuit board, a semiconductor chip package, and a semiconductor device each containing a cured product of the resin composition. [Means for solving the problem]
[0006] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that a resin composition containing a specific phenolic curing agent containing a long-chain aliphatic hydrocarbon group, an epoxy resin, and an active ester compound in combination can solve the above problems, thereby completing the present invention. That is, the present invention includes the following.
[0007] [1] A resin composition comprising: (A) a resin represented by the following formula (A-1), (B) an epoxy resin, and (C) an active ester compound: [ka] (In formula (A-1), R 1 represents an optionally substituted chain aliphatic hydrocarbon group having 7 or more carbon atoms, R 2represents a hydrocarbon group which may have a substituent, n represents a number equal to or greater than 1; m represents a number equal to or greater than 0. However, R 1 includes a chain unsaturated aliphatic hydrocarbon group having 7 or more carbon atoms which may have a substituent.) [2] The resin composition according to [1], wherein component (A) has a weight average molecular weight of 1,000 or less. [3] The resin composition according to [1] or [2], wherein the component (A) is a resin represented by any one of formulas (a-1) to (a-4) or a combination thereof. [ka] (In formulas (a-1) to (a-4), R 1 represents a chain aliphatic hydrocarbon group having 7 or more carbon atoms which may have a substituent, provided that R 1 includes a chain unsaturated aliphatic hydrocarbon group having 7 or more carbon atoms which may have a substituent.) [4] The resin composition according to any one of [1] to [3], wherein the amount of component (A) is 0.01% by mass or more and 10% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. [5] The resin composition according to any one of [1] to [4], further comprising (D) an inorganic filler. [6] The resin composition according to any one of [1] to [5], further comprising a curing agent (E) other than the component (A) and the component (C). [7] The resin composition according to any one of [1] to [6], further comprising a curing accelerator (F). [8] The resin composition according to any one of [1] to [7], further comprising a thermoplastic resin (G). [9] The resin composition according to any one of [1] to [8], which is for forming an insulating layer of a printed wiring board.
[10] A cured product of the resin composition according to any one of [1] to [9].
[11] A sheet-like laminate material comprising the resin composition according to any one of [1] to [9].
[12] A support and a resin composition layer formed on the support, A resin sheet, wherein a resin composition layer comprises the resin composition according to any one of [1] to [9].
[13] A circuit board comprising an insulating layer containing a cured product of the resin composition according to any one of [1] to [9].
[14] A semiconductor chip package comprising a cured product of the resin composition described in any one of [1] to [9].
[15] A semiconductor device comprising the circuit board described in
[13] .
[16] A semiconductor device comprising the semiconductor chip package described in
[14] . Effect of the Invention
[0008] According to the present invention, there are provided a resin composition capable of giving a cured product having excellent crack resistance and desmear resistance; a cured product of the resin composition; a sheet-like laminate material and a resin sheet containing the resin composition; and a circuit board, a semiconductor chip package, and a semiconductor device each containing a cured product of the resin composition. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic diagram of a fan-out type WLP as an example of a semiconductor chip package according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified and implemented as desired without departing from the scope of the claims and their equivalents.
[0011] In the following description, the term "optionally substituted" in reference to a compound or group means both the case where none of the hydrogen atoms of the compound or group are substituted with a substituent, and the case where some or all of the hydrogen atoms of the compound or group are substituted with a substituent.
[0012] In the following description, the term "(meth)acrylic acid" includes acrylic acid, methacrylic acid, and combinations thereof, and the term "(meth)acrylate" includes acrylate, methacrylate, and combinations thereof.
[0013] In the following description, the term "dielectric constant" refers to the relative dielectric constant unless otherwise specified.
[0014] [Resin composition overview] A resin composition according to one embodiment of the present invention contains (A) a resin represented by the following formula (A-1), (B) an epoxy resin, and (C) an active ester compound. Hereinafter, the "resin represented by formula (A-1) (A)" may be referred to as "long-chain aliphatic phenol resin (A)".
[0015] [ka] (In formula (A-1), R 1 represents an optionally substituted chain aliphatic hydrocarbon group having 7 or more carbon atoms, R 2 represents a hydrocarbon group which may have a substituent, n represents a number equal to or greater than 1; m represents a number equal to or greater than 0. However, R 1 includes a chain unsaturated aliphatic hydrocarbon group having 7 or more carbon atoms which may have a substituent.)
[0016] The long-chain aliphatic phenolic resin (A) may include not only a compound having a single structure, but also a composition containing one or more compounds selected from the group of compounds represented by formula (A-1). Therefore, in formula (A-1) representing the long-chain aliphatic phenolic resin (A), the linear aliphatic hydrocarbon group R 1 may include multiple groups having different structures within the scope of the definition stipulated in formula (A-1). However, the chain aliphatic hydrocarbon group R 1R includes a chain unsaturated aliphatic hydrocarbon group having 7 or more carbon atoms which may have a substituent. That is, R of at least some of the compounds contained in the (A) long-chain aliphatic phenol resin 1 is a chain unsaturated aliphatic hydrocarbon group having 7 or more carbon atoms which may have a substituent. Therefore, for example, when the (A) long-chain aliphatic phenol resin contains only a compound having a single structure, the group R of the compound 1 represents a linear unsaturated aliphatic hydrocarbon group having 7 or more carbon atoms which may have a substituent. In addition, for example, when the (A) long-chain aliphatic phenolic resin is a composition containing a plurality of compounds having different structures, the group R 1 represents a chain unsaturated aliphatic hydrocarbon group having 7 or more carbon atoms which may have a substituent.
[0017] According to the resin composition according to one embodiment of the present invention, a cured product having excellent crack resistance and desmear resistance can be obtained. The present inventors speculate that the mechanism by which such excellent effects are obtained is as follows. However, the scope of the present invention is not limited to the mechanism described below.
[0018] The resin composition according to one embodiment of the present invention can be cured because the phenolic hydroxyl group of the long-chain aliphatic phenol resin (A), the epoxy group of the epoxy resin (B), and the active ester group of the active ester compound (C) react with each other to form a crosslinked structure. 1 As shown in the figure, the long-chain aliphatic phenol resin (A) contains a long-chain aliphatic hydrocarbon group. Since this long-chain aliphatic hydrocarbon group has a flexible carbon skeleton, it acts as a stress relaxation component that can absorb stress in the cured product. Therefore, even if stress occurs in the cured product, the destruction of the cured product due to the stress can be suppressed, and the crack resistance can be improved.
[0019] In the desmear treatment, an oxidizing agent is generally brought into contact with the cured product. When the oxidizing agent comes into contact with the cured product, if the bonds generated by the reaction of the phenolic hydroxyl group, the epoxy group, and the active ester group are largely broken by oxidation, the crosslinked structure may be excessively destroyed, and the surface roughness may become large. However, when the cured product of the resin composition according to one embodiment of the present invention is brought into contact with an oxidizing agent, the unsaturated bonds of the long-chain aliphatic hydrocarbon group of the long-chain aliphatic phenolic resin (A) are preferentially oxidized, and the oxidation of the bonds generated by the reaction of the phenolic hydroxyl group, the epoxy group, and the active ester group is suppressed. Therefore, the destruction of the crosslinked structure can be suppressed, and excellent desmear resistance can be achieved.
[0020] The resin composition according to one embodiment of the present invention can usually have a low minimum melt viscosity. In addition, the cured product of the resin composition according to one embodiment of the present invention can usually have low dielectric properties such as dielectric constant and dielectric loss tangent. In addition, the cured product of the resin composition according to one embodiment of the present invention can usually increase adhesion to a conductor layer when a conductor layer is formed on the cured product.
[0021] [(A) Long-chain aliphatic phenolic resin] The resin composition according to one embodiment of the present invention contains a long-chain aliphatic phenol resin (A) as component (A). The long-chain aliphatic phenol resin (A) is any one or a combination of compounds represented by the following formula (A-1).
[0022] [ka] (In formula (A-1), R 1 represents an optionally substituted chain aliphatic hydrocarbon group having 7 or more carbon atoms, R 2 represents a hydrocarbon group which may have a substituent, n represents a number equal to or greater than 1; m represents a number equal to or greater than 0. However, R 1 includes a chain unsaturated aliphatic hydrocarbon group having 7 or more carbon atoms which may have a substituent.)
[0023] In formula (A-1), R 1 represents a chain aliphatic hydrocarbon group having 7 or more carbon atoms which may have a substituent. The chain aliphatic hydrocarbon group represents a group obtained by removing one hydrogen atom from a chain aliphatic hydrocarbon compound. Examples of the aliphatic hydrocarbon group include chain saturated aliphatic hydrocarbon groups such as alkyl groups; chain unsaturated aliphatic hydrocarbon groups such as alkenyl groups and alkapolyenyl groups; and the like. The chain aliphatic hydrocarbon group may be linear or branched, but is preferably linear.
[0024] R 1 The chain aliphatic hydrocarbon group in R has a specific range of carbon atom number. 1 The number of carbon atoms in the chain aliphatic hydrocarbon group in is usually 7 or more, preferably 9 or more, more preferably 12 or more, particularly preferably 14 or more, and is preferably 50 or less, more preferably 40 or less, still more preferably 30 or less, particularly preferably 20 or less. Here, the number of carbon atoms does not include the number of carbon atoms of the substituent.
[0025] Examples of the alkyl group include a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, an octadecyl group, a nonadecyl group, and an icosyl group.
[0026] Examples of the alkenyl group include a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, an undecenyl group, a dodecenyl group, a tridecenyl group, a tetradecenyl group, a pentadecenyl group, a hexadecenyl group, a heptadecenyl group, an octadecenyl group, a nonadecenyl group, and an icosenyl group.
[0027] The number of double bonds in the alkapolyenyl group is usually 2 or more, and may be 3 or more, and is preferably 10 or less, more preferably 6 or less, and particularly preferably 4 or less. Examples of the alkapolyenyl group include alkadienyl groups such as a heptadienyl group, an octadienyl group, a nonadienyl group, a decadienyl group, an undecadienyl group, a dodecadienyl group, a tridecadienyl group, a tetradecadienyl group, a pentadecadienyl group, a hexadecadienyl group, a heptadecadienyl group, an octadecadienyl group, a nonadecadienyl group, and an icosadienyl group; and alkatrienyi groups such as a heptatrienyl group, an octatrienyl group, a nonatrienyl group, a decatrienyl group, an undecatrienyl group, a dodecatrienyl group, a tridecatrienyl group, a tetradecatrienyl group, a pentadecatrienyl group, a hexadecatrienyl group, a heptadecatrienyl group, an octadecatrienyl group, a nonadecatrienyl group, and an icosatrienyl group.
[0028] R 1 The chain aliphatic hydrocarbon group represented by may have a substituent. Examples of the substituent include a halogen atom, a cycloalkyl group, a cycloalkenyl group, an alkoxy group, a cycloalkyloxy group, an aryl group, an aryloxy group, an arylalkoxy group, a monovalent heterocyclic group, an alkylidene group, an amino group, a silyl group, an acyl group, an acyloxy group, a carboxy group, a sulfo group, a cyano group, a nitro group, a hydroxy group, a mercapto group, and an oxo group. Among them, R 1 The chain aliphatic hydrocarbon group represented by the formula (I) preferably has no substituent.
[0029] As described above, the long-chain aliphatic phenol resin (A) includes not only compounds having a single structure but also compositions containing one or more compounds selected from the group of compounds represented by formula (A-1). Thus, the long-chain aliphatic phenol resin (A) may contain one or more types of compounds represented by formula (A-1).
[0030] Therefore, R in formula (A-1) 1 may include multiple chain aliphatic hydrocarbon groups which may have a substituent.1 The optionally substituted aliphatic hydrocarbon group represented by R includes an optionally substituted chain unsaturated aliphatic hydrocarbon group. 1 may represent a combination of a chain saturated aliphatic hydrocarbon group which may have a substituent and a chain unsaturated aliphatic hydrocarbon group which may have a substituent, or a chain unsaturated aliphatic hydrocarbon group which may have a substituent.
[0031] (A) R 1 The amount of the compound representing a linear unsaturated aliphatic hydrocarbon group which may have a substituent is preferably 70 mass % or more, more preferably 80 mass % or more, particularly preferably 90 mass % or more, and is usually 100 mass % or less.
[0032] R in formula (A-1) 1 R preferably contains a chain-like unsaturated aliphatic hydrocarbon group which may have a substituent and contains one carbon-carbon double bond. 1 The amount of the compound representing a linear unsaturated aliphatic hydrocarbon group which may have a substituent and contains one carbon-carbon double bond is preferably 10 mass % or more, more preferably 20 mass % or more, particularly preferably 30 mass % or more, and is preferably 60 mass % or less, more preferably 50 mass % or less, particularly preferably 40 mass % or less.
[0033] R in formula (A-1) 1 R preferably contains a chain-like unsaturated aliphatic hydrocarbon group which may have a substituent and contains two carbon-carbon double bonds. 1The amount of the compound representing a linear unsaturated aliphatic hydrocarbon group which may have a substituent and contains two carbon-carbon double bonds is preferably 5 mass % or more, more preferably 10 mass % or more, particularly preferably 15 mass % or more, and is preferably 50 mass % or less, more preferably 40 mass % or less, particularly preferably 30 mass % or less.
[0034] R in formula (A-1) 1 R preferably contains a chain unsaturated aliphatic hydrocarbon group which may have a substituent and contains three carbon-carbon double bonds. 1 The amount of the compound representing a linear unsaturated aliphatic hydrocarbon group which may have a substituent and contains three carbon-carbon double bonds is preferably 10 mass % or more, more preferably 20 mass % or more, particularly preferably 30 mass % or more, and is preferably 70 mass % or less, more preferably 60 mass % or less, particularly preferably 50 mass % or less.
[0035] (A) R 1 The amount of the compound represented by R may be 0% by mass or more than 0% by mass. 1 The amount of the compound representing a linear saturated aliphatic hydrocarbon group which may have a substituent is usually 0 mass % or more, preferably 30 mass % or less, more preferably 20 mass % or less, and particularly preferably 10 mass % or less.
[0036] In formula (A-1), R 2 represents a hydrocarbon group which may have a substituent. The hydrocarbon group may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. The aliphatic hydrocarbon group may be a saturated aliphatic hydrocarbon group or an unsaturated aliphatic hydrocarbon group. The aliphatic hydrocarbon group may be linear or branched, or may have a ring structure. R 2The hydrocarbon group represented by is preferably 1 to 20, more preferably 1 to 14, still more preferably 1 to 12, still more preferably 1 to 6, and particularly preferably 1 to 3 carbon atoms.
[0037] R 2 Examples of the hydrocarbon group represented by include saturated aliphatic hydrocarbon groups such as alkyl groups and cycloalkyl groups; unsaturated aliphatic hydrocarbon groups such as alkenyl groups, alkynyl groups, alkapolyenyl groups, and cycloalkenyl groups; and aromatic hydrocarbon groups such as aryl groups. Among these, saturated aliphatic hydrocarbon groups are preferred, and alkyl groups are preferred. Examples of the alkyl group include methyl groups, ethyl groups, propyl groups, isopropyl groups, butyl groups, sec-butyl groups, isobutyl groups, tert-butyl groups, pentyl groups, hexyl groups, heptyl groups, octyl groups, nonyl groups, and decyl groups, and methyl groups are particularly preferred.
[0038] R 2 The hydrocarbon group represented by R may have a substituent. 2 Examples of the substituent in 1 The same examples as those of the substituents in R 2 The hydrocarbon group represented by the formula (I) preferably has no substituent.
[0039] In formula (A-1), n represents a number of 1 or more. This n can represent the average number of hydroxyl groups bonded to the benzene ring shown in formula (A-1). n is usually 1 or more and usually 2 or less. Therefore, n may be 1, 2, or a number greater than 1 and less than 2. When n is 1, an example of the compound represented by formula (A-1) includes cardanol. When n is 2, an example of the compound represented by formula (A-1) includes cardol, methyl cardol, urushiol, etc. Thus, for example, when the long-chain aliphatic phenolic resin (A) contains cardanol in combination with one or more selected from the group consisting of cardol, methyl cardol, and urushiol, n can be a number greater than 1 and less than 2.
[0040] In formula (A-1), m represents a number equal to or greater than 0. This m represents the number of groups R bonded to the benzene ring shown in formula (A-1). 2 m may be 0 or a number greater than 0, and is preferably 1 or less, more preferably less than 1. When m is 0, examples of the compound represented by formula (A-1) include cardanol, cardul, and urushiol. When m is 1, examples of the compound represented by formula (A-1) include methyl cardul. Thus, for example, when the long-chain aliphatic phenolic resin (A) contains a combination of methyl cardul with one or more selected from the group consisting of cardanol, cardul, and urushiol, m may be a number greater than 0 and less than 1.
[0041] Examples of the (A) long-chain aliphatic phenol resin include resins represented by any one of the following formulas (a-1) to (a-4) and combinations thereof.
[0042] [ka]
[0043] (In formulas (a-1) to (a-4), R 1 has the same meaning as in formula (A-1).
[0044] Examples of the long-chain aliphatic phenol resin (A) include cardanol (resin of formula (a-1)), cardol (resin of formula (a-2)), 2-methyl cardol (resin of formula (a-3)), and urushiol (resin of formula (a-4)). These are commercially available as resins derived from natural organic substances.
[0045] The phenolic hydroxyl group equivalent of the (A) long-chain aliphatic phenolic resin is preferably 50 g / eq. to 3000 g / eq., more preferably 100 g / eq. to 1000 g / eq., even more preferably 100 g / eq. to 500 g / eq., and particularly preferably 100 g / eq. to 300 g / eq. The phenolic hydroxyl group equivalent represents the mass of the resin per equivalent of the phenolic hydroxyl group. The phenolic hydroxyl group represents a hydroxyl group bonded to a benzene ring.
[0046] When the number of epoxy groups in the (B) epoxy resin is taken as 1, the number of phenolic hydroxyl groups in the (A) long-chain aliphatic phenolic resin is preferably 0.01 or more, more preferably 0.02 or more, particularly preferably 0.05 or more, and preferably 1 or less, more preferably 0.5 or less, particularly preferably 0.3 or less. The "number of phenolic hydroxyl groups in the (A) long-chain aliphatic phenolic resin" refers to the total value obtained by dividing the mass of the non-volatile components of the (A) long-chain aliphatic phenolic resin present in the resin composition by the phenolic hydroxyl group equivalent. The "number of epoxy groups in the (B) epoxy resin" refers to the total value obtained by dividing the mass of the non-volatile components of the (B) epoxy resin present in the resin composition by the epoxy equivalent. When the number of phenolic hydroxyl groups in the (A) long-chain aliphatic phenolic resin is within the above range, the crack resistance and desmear resistance of the cured product of the resin composition can be particularly good, and moreover, the minimum melt viscosity of the resin composition, the dielectric properties of the cured product, and the adhesion to the conductor layer can be effectively improved.
[0047] When the number of active ester groups of the (C) active ester compound is taken as 1, the number of phenolic hydroxyl groups of the (A) long-chain aliphatic phenolic resin is preferably 0.01 or more, more preferably 0.02 or more, even more preferably 0.03 or more, and preferably 1 or less, more preferably 0.5 or less, and more preferably 0.2 or less. The "number of active ester groups of the (C) active ester compound" refers to the total value obtained by dividing the mass of the non-volatile components of the (C) active ester compound present in the resin composition by the active ester group equivalent. When the number of phenolic hydroxyl groups of the (A) long-chain aliphatic phenolic resin is within the above range, the crack resistance and desmear resistance of the cured product of the resin composition can be particularly improved, and moreover, the minimum melt viscosity of the resin composition, the dielectric properties of the cured product, and the adhesion to the conductor layer can be effectively improved.
[0048] The weight average molecular weight of the (A) long-chain aliphatic phenol resin is preferably 1,000 or less, more preferably 800 or less, and particularly preferably 500 or less. There is no particular lower limit, and the lower limit may be, for example, 50 or more, 100 or more, 150 or more, 186 or more, or 200 or more. The weight average molecular weight can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).
[0049] The amount of the (A) long-chain aliphatic phenol resin is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, particularly preferably 0.2% by mass or more, and is preferably 10% by mass or less, more preferably 5% by mass or less, particularly preferably 3% by mass or less, based on 100% by mass of the nonvolatile components of the resin composition. When the amount of the (A) long-chain aliphatic phenol resin is within the above range, the crack resistance and desmear resistance of the cured product of the resin composition can be particularly good, and moreover, the minimum melt viscosity of the resin composition, the dielectric properties of the cured product, and the adhesion to the conductor layer can be effectively improved.
[0050] The amount of the (A) long-chain aliphatic phenol resin is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, particularly preferably 1% by mass or more, and preferably 20% by mass or less, more preferably 15% by mass or less, particularly preferably 10% by mass or less, based on 100% by mass of the resin components of the resin composition. The resin components of the resin composition refer to the non-volatile components of the resin composition excluding the (D) inorganic filler described below. When the amount of the (A) long-chain aliphatic phenol resin is within the above range, the crack resistance and desmear resistance of the cured product of the resin composition can be particularly improved, and moreover, the minimum melt viscosity of the resin composition, the dielectric properties of the cured product, and the adhesion to the conductor layer can be effectively improved.
[0051] The mass ratio of the (A) long-chain aliphatic phenol resin to the (B) epoxy resin ((A) long-chain aliphatic phenol resin / (B) epoxy resin) is preferably 0.01 or more, more preferably 0.02 or more, particularly preferably 0.05 or more, and is preferably 1 or less, more preferably 0.5 or less, particularly preferably 0.3 or less. When the mass ratio ((A) long-chain aliphatic phenol resin / (B) epoxy resin) is within the above range, the crack resistance and desmear resistance of the cured product of the resin composition can be particularly excellent, and furthermore, usually, the minimum melt viscosity of the resin composition, the dielectric properties of the cured product, and the adhesion to a conductor layer can be effectively improved.
[0052] [(B) Epoxy resin] The resin composition according to one embodiment of the present invention contains an epoxy resin (B) as the component (B). The epoxy resin (B) may be a curable resin having an epoxy group. The epoxy resin (B) does not include those that fall under the above-mentioned component (A).
[0053] Examples of the epoxy resin (B) include bixylenol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol novolac type epoxy resin, phenol novolac type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidyl ester type epoxy resin, cresol novolac type epoxy resin, phenol aralkyl type epoxy resin, biphenyl type epoxy resin, linear aliphatic epoxy resin, epoxy resin having a butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro ring-containing epoxy resin, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, naphthylene ether type epoxy resin, trimethylol type epoxy resin, tetraphenylethane type epoxy resin, isocyanurate type epoxy resin, and phenolphthalimidine type epoxy resin. The (B) epoxy resin may be used alone or in combination of two or more kinds.
[0054] From the viewpoint of obtaining a cured product having excellent heat resistance, the (B) epoxy resin preferably contains an epoxy resin containing an aromatic structure. The aromatic structure is a chemical structure generally defined as aromatic, and includes polycyclic aromatic rings and aromatic heterocycles. Examples of epoxy resins containing an aromatic structure include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, bisxylenol type epoxy resins, glycidylamine type epoxy resins having an aromatic structure, glycidyl ester type epoxy resins having an aromatic structure, cresol novolac type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins having an aromatic structure, epoxy resins having a butadiene structure having an aromatic structure, alicyclic epoxy resins having an aromatic structure, heterocyclic epoxy resins, spiro ring-containing epoxy resins having an aromatic structure, cyclohexane dimethanol type epoxy resins having an aromatic structure, naphthylene ether type epoxy resins, trimethylol type epoxy resins having an aromatic structure, and tetraphenylethane type epoxy resins having an aromatic structure.
[0055] The resin composition preferably contains, as the (B) epoxy resin, an epoxy resin having two or more epoxy groups in one molecule. The proportion of the epoxy resin having two or more epoxy groups in one molecule relative to 100% by mass of the non-volatile components of the (B) epoxy resin is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more.
[0056] Epoxy resins include epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as "solid epoxy resins"). The resin composition may contain only liquid epoxy resins as the epoxy resin, or may contain only solid epoxy resins, or may contain a combination of liquid epoxy resins and solid epoxy resins.
[0057] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.
[0058] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, and epoxy resin having a butadiene structure are preferred.
[0059] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "828EL", "jER828EL", "825", and "Epicoat 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630", "630LSD", and "604" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (glycirol type epoxy resin) manufactured by ADEKA Corporation; and "EP-3950L" and "EP-3980S" manufactured by ADEKA Corporation. (glycidylamine type epoxy resin); "EP-4088S" (dicyclopentadiene type epoxy resin) manufactured by ADEKA; "ZX1059" (mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nippon Steel Chemical & Material; "EX-721" (glycidyl ester type epoxy resin) manufactured by Nagase Chemtex; "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton) manufactured by Daicel; "PB-3600" manufactured by Daicel, "JP-100" and "JP-200" (epoxy resin having a butadiene structure) manufactured by Nippon Steel Chemical & Material; "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel Chemical & Material. These may be used alone or in combination of two or more types.
[0060] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.
[0061] Preferred solid epoxy resins include bixylenol type epoxy resins, naphthalene type epoxy resins, naphthalene type tetrafunctional epoxy resins, naphthol novolac type epoxy resins, cresol novolac type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol type epoxy resins, biphenyl type epoxy resins, naphthylene ether type epoxy resins, anthracene type epoxy resins, bisphenol A type epoxy resins, bisphenol AF type epoxy resins, phenol aralkyl type epoxy resins, tetraphenylethane type epoxy resins, and phenolphthalimidine type epoxy resins.
[0062] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", "HP-7200H", and "HP-7200L" (dicyclopentadiene type epoxy resins) manufactured by DIC Corporation; "EXA-7311" and "EXA-7321" manufactured by DIC Corporation. A-7311-G3, EXA-7311-G4, EXA-7311-G4S, HP6000 (naphthylene ether type epoxy resin); EPPN-502H (trisphenol type epoxy resin) manufactured by Nippon Kayaku; NC7000L (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku; NC3000H, NC3000, NC3000L, NC3000FH, NC3100 (biphenyl type epoxy resin) manufactured by Nippon Steel Chemical & Material; ESN475V (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material. ), "ESN4100V" (naphthalene type epoxy resin); "ESN485" (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN375" (dihydroxynaphthalene type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YX4000HK", "YL7890" (bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd. Examples of epoxy resins that can be used include "YX7700" (phenol aralkyl type epoxy resin) manufactured by Osaka Gas Chemicals; "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals; "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "jER1010" (bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Corporation; and "WHR991S" (phenolphthalimidine type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.These may be used alone or in combination of two or more.
[0063] When a liquid epoxy resin and a solid epoxy resin are used in combination as the (B) epoxy resin, the mass ratio thereof (liquid epoxy resin:solid epoxy resin) is preferably 20:1 to 1:20, more preferably 10:1 to 1:10, and particularly preferably 7:1 to 1:7.
[0064] The epoxy equivalent of the (B) epoxy resin is preferably 50 g / eq. to 5,000 g / eq., more preferably 60 g / eq. to 3,000 g / eq., further preferably 80 g / eq. to 2,000 g / eq., and particularly preferably 110 g / eq. to 1,000 g / eq. The epoxy equivalent represents the mass of the resin per equivalent of epoxy group. This epoxy equivalent can be measured according to JIS K7236.
[0065] The weight average molecular weight (Mw) of the epoxy resin (B) is preferably from 100 to 5,000, more preferably from 250 to 3,000, and further preferably from 400 to 1500. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.
[0066] The amount of the (B) epoxy resin in the resin composition is preferably 1% by mass or more, more preferably 2% by mass or more, particularly preferably 4% by mass or more, and is preferably 30% by mass or less, more preferably 20% by mass or less, particularly preferably 10% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. When the amount of the (B) epoxy resin is within the above range, the crack resistance and desmear resistance of the cured product of the resin composition can be particularly good, and furthermore, the minimum melt viscosity of the resin composition, the dielectric properties of the cured product, and the adhesion to the conductor layer can usually be effectively improved.
[0067] The amount of the (B) epoxy resin in the resin composition is preferably 5% by mass or more, more preferably 10% by mass or more, particularly preferably 20% by mass or more, and is preferably 60% by mass or less, more preferably 50% by mass or less, particularly preferably 40% by mass or less, based on 100% by mass of the resin components in the resin composition. When the amount of the (B) epoxy resin is within the above range, the crack resistance and desmear resistance of the cured product of the resin composition can be particularly good, and moreover, the minimum melt viscosity of the resin composition, the dielectric properties of the cured product, and the adhesion to the conductor layer can be effectively improved.
[0068] [(C) Active ester compound] The resin composition according to one embodiment of the present invention contains an active ester compound (C) as the component (C). The active ester compound (C) does not include those corresponding to the above-mentioned components (A) to (B). The active ester compound (C) can function as an epoxy resin curing agent that reacts with the epoxy resin (B) to cure the resin composition. The active ester compound (C) may be used alone or in combination of two or more.
[0069] As the (C) active ester compound, generally, compounds having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are preferably used. The active ester compound is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester compound obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester compound obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.
[0070] Specifically, the (C) active ester compound is preferably a dicyclopentadiene type active ester compound, a naphthalene type active ester compound containing a naphthalene structure, an active ester compound containing an acetylated product of phenol novolac, or an active ester compound containing a benzoylated product of phenol novolac, and among these, at least one selected from a dicyclopentadiene type active ester compound and a naphthalene type active ester compound is more preferable. As the dicyclopentadiene type active ester compound, an active ester compound containing a dicyclopentadiene type diphenol structure is preferable.
[0071] (C) Commercially available active ester compounds include, for example, active ester compounds containing a dicyclopentadiene-type diphenol structure such as "EXB9451", "EXB9460", "EXB9460S", "EXB-8000L", "EXB-8000L-65M", "EXB-8000L-65TM", "HPC-8000L-65TM", "HPC-8000", "HPC-8000-65T", "HPC-8000H", and "HPC-8000H-65TM" (manufactured by DIC Corporation); and active ester compounds containing a naphthalene structure such as "HP-B-8151-62T", "EXB-8100L-65T", "EXB-8150-60T", and "EXB-81 Examples of such active ester compounds include "EXB-9416-70BK", "HPC-8150-60T", "HPC-8150-62T", and "EXB-8" (manufactured by DIC Corporation); an active ester compound containing phosphorus, such as "EXB9401" (manufactured by DIC Corporation); an active ester compound which is an acetylated product of phenol novolac, such as "DC808" (manufactured by Mitsubishi Chemical Corporation); active ester compounds which are benzoylated products of phenol novolac, such as "YLH1026", "YLH1030", and "YLH1048" (manufactured by Mitsubishi Chemical Corporation); and an active ester compound containing a styryl group and a naphthalene structure, such as "PC1300-02-65MA" (manufactured by Air Water Corporation).
[0072] The active ester group equivalent of the (C) active ester compound is preferably 50 g / eq. to 500 g / eq., more preferably 50 g / eq. to 400 g / eq., and further preferably 100 g / eq. to 300 g / eq. The active ester group equivalent represents the mass of the active ester compound per equivalent of the active ester group.
[0073] When the number of epoxy groups in the (B) epoxy resin is taken as 1, the number of active ester groups in the (C) active ester compound is preferably 0.1 or more, more preferably 0.5 or more, even more preferably 1 or more, and is preferably 6 or less, more preferably 5 or less, and particularly preferably 4 or less. When the number of active ester groups in the (C) active ester compound is within the above range, the crack resistance and desmear resistance of the cured product of the resin composition can be particularly excellent, and moreover, usually the minimum melt viscosity of the resin composition, the dielectric properties of the cured product, and the adhesion to a conductor layer can be effectively improved.
[0074] The amount of the (C) active ester compound in the resin composition is preferably 1% by mass or more, more preferably 5% by mass or more, particularly preferably 10% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, particularly preferably 20% by mass or less, based on 100% by mass of the non-volatile components of the resin composition. When the amount of the (C) active ester compound is within the above range, the crack resistance and desmear resistance of the cured product of the resin composition can be particularly good, and furthermore, the minimum melt viscosity of the resin composition, the dielectric properties of the cured product, and the adhesion to the conductor layer can usually be effectively improved.
[0075] The amount of the (C) active ester compound in the resin composition is preferably 20% by mass or more, more preferably 30% by mass or more, particularly preferably 40% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, particularly preferably 60% by mass or less, based on 100% by mass of the resin components of the resin composition. When the amount of the (C) active ester compound is within the above range, the crack resistance and desmear resistance of the cured product of the resin composition can be particularly good, and furthermore, usually, the minimum melt viscosity of the resin composition, the dielectric properties of the cured product, and the adhesion to the conductor layer can be effectively improved.
[0076] The mass ratio of the (C) active ester compound to the (A) long-chain aliphatic phenol resin ((C) active ester compound / (A) long-chain aliphatic phenol resin) is preferably 1 or more, more preferably 2 or more, and particularly preferably 5 or more, and is preferably 50 or less, more preferably 40 or less, and particularly preferably 30 or less. When the mass ratio ((C) active ester compound / (A) long-chain aliphatic phenol resin) is within the above range, the crack resistance and desmear resistance of the cured product of the resin composition can be particularly excellent, and further usually, the minimum melt viscosity of the resin composition, the dielectric properties of the cured product, and the adhesion to a conductor layer can be effectively improved.
[0077] [(D) Inorganic filler] The resin composition according to one embodiment of the present invention may further contain an inorganic filler (D) as an optional component. The inorganic filler (D) as the component (D) does not include those corresponding to the above-mentioned components (A) to (C). The inorganic filler (D) is usually contained in the resin composition in the form of particles.
[0078] (D) An inorganic compound is used as the material of the inorganic filler. (D) Examples of the material of the inorganic filler include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica and alumina are preferred, and silica is particularly preferred. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. In addition, spherical silica is preferred as the silica. The (D) inorganic filler may be used alone or in combination of two or more kinds.
[0079] (D) Inorganic fillers can be classified into hollow inorganic fillers having voids inside and solid inorganic fillers having no voids inside. (D) Inorganic fillers may be used only with hollow inorganic fillers, only with solid inorganic fillers, or in combination with hollow inorganic fillers and solid inorganic fillers. When using hollow inorganic fillers, the dielectric constant of the cured product of the resin composition can be particularly reduced in general.
[0080] Since the hollow inorganic filler has pores, it usually has a porosity of more than 0 volume%. From the viewpoint of lowering the relative dielectric constant of the insulating layer containing the cured product of the resin composition, the porosity of the hollow inorganic filler is preferably 5 volume% or more, more preferably 10 volume% or more, and particularly preferably 15 volume% or more. In addition, from the viewpoint of the mechanical strength of the cured product of the resin composition, the porosity of the hollow inorganic filler is preferably 95 volume% or less, more preferably 90 volume% or less, and particularly preferably 85 volume% or less.
[0081] The porosity P (volume %) of a particle is defined as the volume ratio of the total volume of one or more pores present inside the particle to the total volume of the particle based on the outer surface of the particle (total volume of pores / volume of particle). This porosity P is calculated by multiplying the measured value of the actual density D of the particle by the volume ratio of the particle. M (g / cm 3 ), and the theoretical density of the material that forms the particle D T (g / cm 3 ) can be calculated using the following formula (M1).
[0082]
number
[0083] The hollow inorganic filler may be produced, for example, by the methods described in Japanese Patent Nos. 5,940,188 and 5,864,299 or methods equivalent thereto.
[0084] (D) Commercially available inorganic fillers include, for example, "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; "UFP-30", "DAW-03", and "FB-105FD" manufactured by Denka Co., Ltd.; "Silfil NSS-3N", "Silfil NSS-4N", and "Silfil NSS-5N" manufactured by Tokuyama Corporation; "Sferique" manufactured by JGC Catalysts and Chemicals Co., Ltd.; and "MG-005" and "Cellpheares" manufactured by Taiheiyo Cement Corporation.
[0085] From the viewpoint of significantly obtaining the desired effects of the present invention, the average particle size of the (D) inorganic filler is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and particularly preferably 0.2 μm or more, and is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less.
[0086] (D) The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is prepared on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is used as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing the mixture by ultrasonic waves for 10 minutes. The measurement sample can be measured using a laser diffraction particle size distribution measuring device with blue and red light wavelengths as the light source, and the volume-based particle size distribution of the inorganic filler can be measured using a flow cell method, and the average particle size can be calculated from the obtained particle size distribution as the median diameter. An example of a laser diffraction particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.
[0087] The specific surface area of the (D) inorganic filler is preferably 0.1 m from the viewpoint of significantly obtaining the desired effects of the present invention. 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, particularly preferably 3m 2 / g or more, preferably 100m 2 / g or less, more preferably 70m 2 / g or less, more preferably 50m 2 / g or less, particularly preferably 40m 2 The specific surface area of the inorganic filler can be measured by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.
[0088] (D) The inorganic filler is preferably treated with a surface treatment agent from the viewpoint of improving moisture resistance and dispersibility. Examples of the surface treatment agent include fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, titanate coupling agents, etc. The surface treatment agent may be used alone or in any combination of two or more.
[0089] Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).
[0090] From the viewpoint of improving the dispersibility of the inorganic filler, the degree of surface treatment with the surface treatment agent is preferably within a specific range. Specifically, 100% by mass of the inorganic filler is preferably surface-treated with 0.2% to 5% by mass of the surface treatment agent, more preferably with 0.2% to 3% by mass of the surface treatment agent, and even more preferably with 0.3% to 2% by mass of the surface treatment agent.
[0091] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin composition, it is more preferable that the content is 1.0 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:
[0092] (D) The amount of carbon per unit surface area of the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, the "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.
[0093] The amount of the (D) inorganic filler in the resin composition may be 0% by mass or more, and is preferably 20% by mass or more, more preferably 40% by mass or more, particularly preferably 60% by mass or more, and is preferably 90% by mass or less, more preferably 85% by mass or less, particularly preferably 80% by mass or less, based on 100% by mass of the non-volatile components of the resin composition. When the amount of the (D) inorganic filler is within the above range, the crack resistance and desmear resistance of the cured product of the resin composition can be particularly good, and furthermore, the minimum melt viscosity of the resin composition, the dielectric properties of the cured product, and the adhesion to the conductor layer can be effectively improved.
[0094] [(E) Optional Hardener] The resin composition according to one embodiment of the present invention may further contain an optional curing agent (E) as an optional component. The optional curing agent (E) as the component (E) does not include those corresponding to the above-mentioned components (A) to (D). Therefore, the optional curing agent (E) refers to a component other than the long-chain aliphatic phenol resin (A) and the active ester compound (C) among the epoxy resin curing agents that react with the epoxy resin (B) to cure the resin composition. The optional curing agent (E) may be used alone or in combination of two or more kinds.
[0095] As described above, the (E) optional curing agent has the function of reacting with the (B) epoxy resin to cure the resin composition, similar to the (A) long-chain aliphatic phenolic resin and the (C) active ester compound. Examples of the (E) optional curing agent include phenolic curing agents, carbodiimide curing agents, acid anhydride curing agents, amine curing agents, benzoxazine curing agents, cyanate ester curing agents, and thiol curing agents. However, the phenolic curing agents classified as the (E) optional curing agent do not include those corresponding to the (A) long-chain aliphatic phenolic resin. Among them, it is preferable to use one or more curing agents selected from the group consisting of phenolic curing agents and carbodiimide curing agents.
[0096] As the phenol-based curing agent, a curing agent having one or more, preferably two or more, hydroxyl groups (phenolic hydroxyl groups) bonded to an aromatic ring such as a benzene ring or a naphthalene ring in one molecule can be used. From the viewpoint of heat resistance and water resistance, a phenol-based curing agent having a novolac structure is preferred. From the viewpoint of adhesion, a nitrogen-containing phenol-based curing agent is preferred, and a triazine skeleton-containing phenol-based curing agent is more preferred. Among them, from the viewpoint of highly satisfying heat resistance, water resistance, and adhesion, a triazine skeleton-containing phenol novolac resin is preferred. Specific examples of phenol-based curing agents include "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Kasei Co., Ltd., "NHN" and "CBN" manufactured by Nippon Kayaku Co., Ltd., "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-375", and "SN-395" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "LA-7052", "LA-7054", "LA-3018", "LA-3018-50P", "LA-1356", "TD2090", and "TD-2090-60M" manufactured by DIC Corporation.
[0097] As the carbodiimide-based curing agent, a curing agent having one or more, preferably two or more, carbodiimide structures in one molecule can be used. Specific examples of the carbodiimide-based curing agent include aliphatic biscarbodiimides such as tetramethylene-bis(t-butylcarbodiimide) and cyclohexane bis(methylene-t-butylcarbodiimide); aromatic biscarbodiimides such as phenylene-bis(xylylcarbodiimide); aliphatic polycarbodiimides such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), and poly(isophoronecarbodiimide); poly(phenylenecarbodiimide), poly( Examples of polycarbodiimides include aromatic polycarbodiimides such as poly(naphthylenecarbodiimide), poly(tolylenecarbodiimide), poly(methyldiisopropylphenylenecarbodiimide), poly(triethylphenylenecarbodiimide), poly(diethylphenylenecarbodiimide), poly(triisopropylphenylenecarbodiimide), poly(diisopropylphenylenecarbodiimide), poly(xylylenecarbodiimide), poly(tetramethylxylylenecarbodiimide), poly(methylenediphenylenecarbodiimide), and poly[methylenebis(methylphenylene)carbodiimide]. Commercially available carbodiimide curing agents include, for example, "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-07", and "Carbodilite V-09" manufactured by Nisshinbo Chemical Inc.; and "Stavaxol P", "Stavaxol P400", and "Hi-Kasil 510" manufactured by Rhein Chemie.
[0098] As the acid anhydride curing agent, a curing agent having one or more acid anhydride groups in one molecule can be used, and a curing agent having two or more acid anhydride groups in one molecule is preferable. Specific examples of the acid anhydride curing agent include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic dianhydride, and benzophenonetetracarboxylic dianhydride. Examples of acid anhydrides include anhydrides, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and polymeric acid anhydrides such as styrene-maleic acid resin, which is a copolymer of styrene and maleic acid. Commercially available acid anhydride curing agents include, for example, "HNA-100", "MH-700", "MTA-15", "DDSA", and "OSA" manufactured by New Japan Chemical Co., Ltd.; "YH-306" and "YH-307" manufactured by Mitsubishi Chemical Corporation; "HN-2200" and "HN-5500" manufactured by Hitachi Chemical Co., Ltd.; and "EF-30", "EF-40", "EF-60", and "EF-80" manufactured by Clay Valley.
[0099] As the amine-based curing agent, a curing agent having one or more, preferably two or more, amino groups in one molecule can be used. As the amine-based curing agent, for example, aliphatic amines, polyether amines, alicyclic amines, aromatic amines, etc. can be mentioned, among which aromatic amines are preferred. As the amine-based curing agent, primary amines or secondary amines are preferred, and primary amines are more preferred. Specific examples of amine-based curing agents include 4,4'-methylenebis(2,6-dimethylaniline), 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, and 2,2-bis(3-amino-4-hydroxyphenyl)propane. propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, and the like. Commercially available amine-based curing agents include, for example, "SEIKACURE-S" manufactured by Seika Corporation; "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", and "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd.; "Epicure W" manufactured by Mitsubishi Chemical Corporation; and "DTDA" manufactured by Sumitomo Seika Chemicals Co., Ltd.
[0100] Specific examples of benzoxazine-based curing agents include "JBZ-OP100D" and "ODA-BOZ" manufactured by JFE Chemical Corporation; "HFB2006M" manufactured by Showa Polymer Co., Ltd.; and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.
[0101] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (both of which are phenol novolac-type multifunctional cyanate ester resins), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.
[0102] Examples of thiol-based curing agents include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), and tris(3-mercaptopropyl)isocyanurate.
[0103] The active group equivalent of the (E) optional curing agent is preferably 50 g / eq. to 3000 g / eq., more preferably 100 g / eq. to 1000 g / eq., further preferably 100 g / eq. to 500 g / eq., and particularly preferably 100 g / eq. to 300 g / eq. The active group equivalent represents the mass of the curing agent per equivalent of the active group.
[0104] When the number of epoxy groups in the (B) epoxy resin is taken as 1, the number of active groups in the (E) optional curing agent is preferably 0.01 or more, more preferably 0.1 or more, even more preferably 0.2 or more, and is preferably 3 or less, more preferably 2 or less, and particularly preferably 1 or less. The "number of active groups in the (E) optional curing agent" refers to the total value obtained by dividing the mass of the non-volatile components of the (E) optional curing agent present in the resin composition by the active group equivalent.
[0105] The amount of the optional curing agent (E) in the resin composition may be 0% by mass or may be more than 0% by mass, and is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and particularly preferably 1% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably 5% by mass or less, relative to 100% by mass of the non-volatile components of the resin composition.
[0106] The amount of the optional curing agent (E) in the resin composition may be 0% by mass or may be greater than 0% by mass, and is preferably 0.1% by mass or more, more preferably 1% by mass or more, and particularly preferably 5% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, and particularly preferably 30% by mass or less, relative to 100% by mass of the resin component of the resin composition.
[0107] [(F) Curing accelerator] The resin composition according to one embodiment of the present invention may further contain a curing accelerator (F) as an optional component. The curing accelerator (F) as the component (F) does not include those corresponding to the above-mentioned components (A) to (E). The curing accelerator (F) functions as a curing catalyst that accelerates the curing of the epoxy resin (B).
[0108] Examples of the (F) curing accelerator include phosphorus-based curing accelerators, urea-based curing accelerators, guanidine-based curing accelerators, imidazole-based curing accelerators, metal-based curing accelerators, and amine-based curing accelerators. Among these, imidazole-based curing accelerators are preferred. The (F) curing accelerators may be used alone or in combination of two or more.
[0109] Examples of the phosphorus-based curing accelerator include aliphatic phosphonium salts such as tetrabutyl phosphonium bromide, tetrabutyl phosphonium chloride, tetrabutyl phosphonium acetate, tetrabutyl phosphonium decanoate, tetrabutyl phosphonium laurate, bis(tetrabutyl phosphonium)pyromellitate, tetrabutyl phosphonium hydrogenhexahydrophthalate, tetrabutyl phosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, and di-tert-butyldimethylphosphonium tetraphenylborate; methyl triphenyl phosphonium bromide, ethyl triphenyl phosphonium bromide, propyl triphenyl phosphonium bromide, butyl triphenyl phosphonium bromide, benzyl triphenyl phosphonium chloride, tetraphenyl phosphonium bromide, p-tolyl triphenyl phosphonium tetra-p-tolylborate, tetraphenyl phosphonium bromide, and the like. aromatic phosphonium salts such as tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone adducts such as triphenylphosphine-p-benzoquinone adduct; aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine;Dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tris(4-ethylphenyl)phosphine, tris(4-propylphenyl)phosphine, tris(4-isopropylphenyl)phosphine, tris(4-butylphenyl)phosphine, tris(4-tert-butylphenyl)phosphine, tris(2,4-dimethylphenyl)phosphine, tris(2,5-dimethylphenyl)phosphine, tris(2,6-dimethylphenyl)phosphine Examples of aromatic phosphines include tris(3,5-dimethylphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, tris(2,6-dimethyl-4-ethoxyphenyl)phosphine, tris(2-methoxyphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(4-ethoxyphenyl)phosphine, tris(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, and 2,2'-bis(diphenylphosphino)diphenyl ether.
[0110] Examples of the urea-based curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, and 3-(3,4-dimethylphenyl)-1,1-dimethylurea. aromatic dimethylureas such as butylurea, 3-(4-isopropylphenyl)-1,1-dimethylurea, 3-(4-methoxyphenyl)-1,1-dimethylurea, 3-(4-nitrophenyl)-1,1-dimethylurea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethylurea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethylurea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethylurea, N,N-(1,4-phenylene)bis(N',N'-dimethylurea), and N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethylurea) [toluene bisdimethylurea].
[0111] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide.
[0112] Examples of the imidazole-based curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-methylimidazole. Phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl -(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct , 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, 2-phenylimidazoline, and other imidazole compounds and adducts of imidazole compounds and epoxy resins. Commercially available imidazole curing accelerators include, for example, "1B2PZ", "2E4MZ", "2MZA-PW", "2MZ-OK", "2MA-OK", "2MA-OK-PW", "2PHZ", "2PHZ-PW", "Cl1Z", "Cl1Z-CN", "Cl1Z-CNS", and "C11Z-A" manufactured by Shikoku Chemical Industry Co., Ltd.; and "P200-H50" manufactured by Mitsubishi Chemical Corporation.
[0113] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.
[0114] Examples of the amine-based curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo(5,4,0)-undecene, etc. Commercially available amine-based curing accelerators may be used, such as "MY-25" manufactured by Ajinomoto Fine-Techno Co., Ltd.
[0115] The amount of the (F) curing accelerator in the resin composition may be 0% by mass or may be more than 0% by mass, and is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, particularly preferably 0.03% by mass or more, and is preferably 2% by mass or less, more preferably 1% by mass or less, and particularly preferably 0.5% by mass or less, relative to 100% by mass of the non-volatile components of the resin composition.
[0116] The amount of the (F) curing accelerator in the resin composition may be 0 mass% or more than 0 mass%, and is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, and particularly preferably 0.1 mass% or more, and is preferably 5 mass% or less, more preferably 2 mass% or less, and particularly preferably 1 mass% or less, relative to 100 mass% of the resin component of the resin composition.
[0117] [(G)Thermoplastic resin] The resin composition according to one embodiment of the present invention may further contain a thermoplastic resin (G) as an optional component. The thermoplastic resin (G) as the component (G) does not include those corresponding to the above-mentioned components (A) to (F).
[0118] Examples of the (G) thermoplastic resin include phenoxy resin, polyimide resin, polyvinyl acetal resin, polyolefin resin, polybutadiene resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, polyester resin, etc. The (G) thermoplastic resin may be used alone or in combination of two or more kinds.
[0119] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. Specific examples of phenoxy resins include "1256" and "4250" manufactured by Mitsubishi Chemical Corporation (both of which are phenoxy resins containing a bisphenol A skeleton); "YX8100" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol S skeleton); "YX6954" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol acetophenone skeleton); "FX280" and "FX293" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", "YL7482", and "YL7891BH30" manufactured by Mitsubishi Chemical Corporation.
[0120] Specific examples of polyimide resins include "SLK-6100" manufactured by Shin-Etsu Chemical Co., Ltd., and "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd.
[0121] Examples of polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred.Specific examples of polyvinyl acetal resin include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd.; S-LEC BH series, BX series (e.g. BX-5Z), KS series (e.g. KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.
[0122] Examples of polyolefin resins include ethylene-based copolymer resins such as low-density polyethylene, very low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-methyl acrylate copolymer; and polyolefin polymers such as polypropylene and ethylene-propylene block copolymer.
[0123] Examples of polybutadiene resins include hydrogenated polybutadiene skeleton-containing resins, hydroxy group-containing polybutadiene resins, phenolic hydroxy group-containing polybutadiene resins, carboxy group-containing polybutadiene resins, acid anhydride group-containing polybutadiene resins, epoxy group-containing polybutadiene resins, isocyanate group-containing polybutadiene resins, urethane group-containing polybutadiene resins, polyphenylene ether-polybutadiene resins, and the like.
[0124] Specific examples of polyamide-imide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as "KS9100" and "KS9300" (polysiloxane skeleton-containing polyamide-imide) manufactured by Hitachi Chemical Co., Ltd.
[0125] A specific example of the polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd.
[0126] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.
[0127] A specific example of the polyphenylene ether resin is NORYL SA90 manufactured by SABIC, etc. A specific example of the polyetherimide resin is ULTEM manufactured by GE, etc.
[0128] Examples of polycarbonate resins include hydroxyl group-containing carbonate resins, phenolic hydroxyl group-containing carbonate resins, carboxyl group-containing carbonate resins, acid anhydride group-containing carbonate resins, isocyanate group-containing carbonate resins, and urethane group-containing carbonate resins. Specific examples of polycarbonate resins include "FPC0220" manufactured by Mitsubishi Gas Chemical Co., Ltd., "T6002" and "T6001" (polycarbonate diol) manufactured by Asahi Kasei Chemicals Corporation, and "C-1090", "C-2090", and "C-3090" (polycarbonate diol) manufactured by Kuraray Co., Ltd. Specific examples of polyether ether ketone resins include "Sumiploy K" manufactured by Sumitomo Chemical Co., Ltd.
[0129] Examples of polyester resins include polyethylene terephthalate resins, polyethylene naphthalate resins, polybutylene terephthalate resins, polybutylene naphthalate resins, polytrimethylene terephthalate resins, polytrimethylene naphthalate resins, and polycyclohexane dimethyl terephthalate resins.
[0130] The weight average molecular weight (Mw) of the thermoplastic resin (G) is preferably greater than 5,000, more preferably at least 8,000, even more preferably at least 10,000, particularly preferably at least 20,000, and is preferably at most 100,000, more preferably at most 70,000, even more preferably at most 60,000, particularly preferably at most 50,000. The weight average molecular weight can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).
[0131] The amount of the (G) thermoplastic resin in the resin composition may be 0% by mass or may be greater than 0% by mass, and is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and particularly preferably 0.1% by mass or more, and is preferably 5% by mass or less, more preferably 2% by mass or less, and particularly preferably 1% by mass or less, relative to 100% by mass of the non-volatile components of the resin composition.
[0132] The amount of the (G) thermoplastic resin in the resin composition may be 0% by mass or may be greater than 0% by mass, and is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and particularly preferably 0.1% by mass or more, and is preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably 3% by mass or less, relative to 100% by mass of the resin components of the resin composition.
[0133] [(H) Radical polymerizable compound] The resin composition according to one embodiment of the present invention may further contain an arbitrary radical polymerizable compound (H) as an optional component. The radical polymerizable compound (H) as the component (H) does not include those corresponding to the above-mentioned components (A) to (G). The radical polymerizable compound (H) may be used alone or in combination of two or more kinds.
[0134] The radical polymerizable compound (H) may contain an ethylenically unsaturated bond. Thus, the radical polymerizable compound (H) may have a radical polymerizable group containing an ethylenically unsaturated bond. Examples of the radical polymerizable group include unsaturated hydrocarbon groups such as vinyl group, allyl group, 1-propenyl group, 3-cyclohexenyl group, 3-cyclopentenyl group, 2-vinylphenyl group, 3-vinylphenyl group, and 4-vinylphenyl group; and α,β-unsaturated carbonyl groups such as acryloyl group, methacryloyl group, and maleimide group (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl group). The radical polymerizable compound (H) preferably has two or more radical polymerizable groups.
[0135] Examples of the (H) radically polymerizable compound include (meth)acrylic radically polymerizable compounds, styrene radically polymerizable compounds, allyl radically polymerizable compounds, and maleimide radically polymerizable compounds.
[0136] The (meth)acrylic radical polymerizable compound is, for example, a compound having one or more, preferably two or more, acryloyl groups and / or methacryloyl groups. Examples of the (meth)acrylic radical polymerizable compound include cyclohexane-1,4-dimethanol di(meth)acrylate, cyclohexane-1,3-dimethanol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,8-octanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,2-diphenylmethane di(meth)acrylate, 1,3-diphenylmethane di(meth)acrylate, 1,4-diphenylmethane di(meth)acrylate, 1,5-diphenylmethane di(meth)acrylate, 1,6-diphenylmethane di(meth)acrylate, 1,8-diphenylmethane di(meth)acrylate, 1,9-diphenylmethane ...5-diphenylmethane di(meth)acrylate, 1,5-diphenylmethane di(meth)acrylate, 1,6-diphenylmethane di(meth)acrylate, 1,8-diphenylmethane di(meth)acrylate, 1,9-diphenylmethane di(meth)acrylate, 1,5-diphenylmethane di(meth)acrylate, 1,5-diphenylmethane di(meth)acrylate, 1,5-diphenylmethane di(meth)acrylate, 1,5-diphenylmethane aliphatic (meth)acrylic acid ester compounds with low molecular weight (molecular weight less than 1000), such as dioxane glycol di(meth)acrylate, 3,6-dioxa-1,8-octanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, glycerin tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate; Examples of the ether-containing (meth)acrylic acid ester compound include low molecular weight (molecular weight less than 1000) ether-containing (meth)acrylic acid ester compounds such as 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene, ethoxylated bisphenol A di(meth)acrylate, and propoxylated bisphenol A di(meth)acrylate; low molecular weight (molecular weight less than 1000) isocyanurate-containing (meth)acrylic acid ester compounds such as tris(3-hydroxypropyl)isocyanurate tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, and ethoxylated isocyanuric acid tri(meth)acrylate; and high molecular weight (molecular weight 1000 or more) acrylic acid ester compounds such as (meth)acrylic modified polyphenylene ether resin.Examples of commercially available (meth)acrylic radically polymerizable compounds include "A-DOG" (dioxane glycol diacrylate) manufactured by Shin-Nakamura Chemical Co., Ltd., "DCP-A" (tricyclodecane dimethanol diacrylate) and "DCP" (tricyclodecane dimethanol dimethacrylate) manufactured by Kyoeisha Chemical Co., Ltd., "KAYARAD R-684" (tricyclodecane dimethanol diacrylate) and "KAYARAD R-604" (dioxane glycol diacrylate) manufactured by Nippon Kayaku Co., Ltd., and "SA9000" and "SA9000-111" (methacrylic-modified polyphenylene ether) manufactured by SABIC Innovative Plastics.
[0137] The styrene radical polymerizable compound is, for example, a compound having one or more, preferably two or more, vinyl groups directly bonded to an aromatic carbon atom. Examples of the styrene radical polymerizable compound include low molecular weight (molecular weight less than 1000) styrene compounds such as divinylbenzene, 2,4-divinyltoluene, 2,6-divinylnaphthalene, 1,4-divinylnaphthalene, 4,4'-divinylbiphenyl, 1,2-bis(4-vinylphenyl)ethane, 2,2-bis(4-vinylphenyl)propane, and bis(4-vinylphenyl)ether; high molecular weight (molecular weight 1000 or more) styrene compounds such as vinylbenzyl-modified polyphenylene ether resin and styrene-divinylbenzene copolymer. Examples of commercially available styrene-based radically polymerizable compounds include "ODV-XET(X03)", "ODV-XET(X04)", and "ODV-XET(X05)" (styrene-divinylbenzene copolymers) manufactured by Nippon Steel Chemical & Material Co., Ltd., and "OPE-2St 1200" and "OPE-2St 2200" (vinylbenzyl-modified polyphenylene ether resins) manufactured by Mitsubishi Gas Chemical Co., Inc.
[0138] The allyl radical polymerizable compound is, for example, a compound having one or more, preferably two or more, allyl groups. Examples of allyl radical polymerizable compounds include aromatic carboxylic acid allyl ester compounds such as diallyl diphenate, triallyl trimellitate, diallyl phthalate, diallyl isophthalate, diallyl terephthalate, diallyl 2,6-naphthalenedicarboxylate, and diallyl 2,3-naphthalenecarboxylate; isocyanuric acid allyl ester compounds such as 1,3,5-triallyl isocyanurate and 1,3-diallyl-5-glycidyl isocyanurate; epoxy-containing aromatic allyl compounds such as 2,2-bis[3-allyl-4-(glycidyloxy)phenyl]propane; benzoxazine-containing aromatic allyl compounds such as bis[3-allyl-4-(3,4-dihydro-2H-1,3-benzoxazin-3-yl)phenyl]methane; ether-containing aromatic allyl compounds such as 1,3,5-triallyl ether benzene; and allyl silane compounds such as diallyl diphenyl silane. Commercially available allyl radical polymerizable compounds include, for example, "TAIC" (1,3,5-triallyl isocyanurate) manufactured by Nippon Kasei Chemical Industry Co., Ltd., "DAD" (diallyl diphenate) manufactured by Nisshoku Techno Fine Chemical Co., Ltd., "TRIAM-705" (triallyl trimellitate) manufactured by Wako Pure Chemical Industries, Ltd., trade name "DAND" (2,3-naphthalene carboxylate diallyl) manufactured by Nippon Distillation Industry Co., Ltd., "ALP-d" (bis[3-allyl-4-(3,4-dihydro-2H-1,3-benzoxazin-3-yl)phenyl]methane) manufactured by Shikoku Kasei Corporation, "RE-810NM" (2,2-bis[3-allyl-4-(glycidyloxy)phenyl]propane) manufactured by Nippon Kayaku Co., Ltd., and "DA-MGIC" (1,3-diallyl-5-glycidyl isocyanurate) manufactured by Shikoku Kasei Corporation.
[0139] The maleimide radical polymerizable compound is, for example, a compound having one or more, preferably two or more, maleimide groups. The maleimide radical polymerizable compound may be an aliphatic maleimide compound containing an aliphatic amine skeleton, or an aromatic maleimide compound containing an aromatic amine skeleton. Commercially available maleimide radical polymerizable compounds include, for example, "SLK-2600" manufactured by Shin-Etsu Chemical Co., Ltd., "BMI-1500", "BMI-1700", "BMI-3000J", "BMI-689", and "BMI-2500" (dimer diamine structure-containing maleimide compounds) manufactured by DigiCner Molecules, Inc., "BMI-6100" (aromatic maleimide compound) manufactured by DigiCner Molecules, "MIR-5000-60T" and "MIR-3000-70MT" (biphenylaralkyl-type maleimide compounds) manufactured by Nippon Kayaku Co., Ltd., "BMI-70" and "BMI-80" manufactured by K.I. Chemical Industry Co., Ltd., and "BMI-2300" and "BMI-TMH" manufactured by Daiwa Kasei Kogyo Co., Ltd. In addition, as the maleimide-based radically polymerizable compound, a maleimide resin (maleimide compound containing an indane ring skeleton) disclosed in the Japan Institute of Invention and Innovation's Technical Journal Publication No. 2020-500211 may be used.
[0140] The ethylenically unsaturated bond equivalent of the radical polymerizable compound (H) is preferably 20 g / eq. to 3,000 g / eq., more preferably 50 g / eq. to 2,500 g / eq., further preferably 70 g / eq. to 2,000 g / eq., and particularly preferably 90 g / eq. to 1,500 g / eq. The ethylenically unsaturated bond equivalent represents the mass of the radical polymerizable compound per equivalent of the ethylenically unsaturated bond.
[0141] The weight average molecular weight (Mw) of the radical polymerizable compound (H) is preferably 40,000 or less, more preferably 10,000 or less, further preferably 5,000 or less, and particularly preferably 3,000 or less. The lower limit is not particularly limited, but may be, for example, 150 or more. The weight average molecular weight can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).
[0142] The amount of the (H) radically polymerizable compound in the resin composition may be 0% by mass or more than 0% by mass, and is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and particularly preferably 0.5% by mass or more, and is preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably 2% by mass or less, relative to 100% by mass of the non-volatile components in the resin composition.
[0143] The amount of the (H) radical polymerizable compound in the resin composition may be 0 mass% or more than 0 mass%, and is preferably 0.01 mass% or more, more preferably 0.1 mass% or more, particularly preferably 1 mass% or more, and is preferably 15 mass% or less, more preferably 10 mass% or less, particularly preferably 5 mass% or less, relative to 100 mass% of the resin components in the resin composition.
[0144] (I) Optional Additives The resin composition according to one embodiment of the present invention may further contain (I) an optional additive as an optional component. (I) The optional additive may be, for example, an organic filler such as rubber particles; an organic metal compound such as an organic copper compound, an organic zinc compound, or an organic cobalt compound; a colorant such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, or carbon black; a polymerization inhibitor such as hydroquinone, catechol, pyrogallol, or phenothiazine; a leveling agent such as a silicone-based leveling agent or an acrylic polymer-based leveling agent; a thickener such as bentone or montmorillonite; an antifoaming agent such as a silicone-based antifoaming agent, an acrylic-based antifoaming agent, a fluorine-based antifoaming agent, or a vinyl resin-based antifoaming agent; an ultraviolet absorbing agent such as a benzotriazole-based ultraviolet absorbing agent; an adhesion improver such as urea silane; a triazole-based adhesion imparting agent, a tetrazole-based adhesion imparting agent, ... triazole-based adhesion imparting agent, a triazole-based adhesion imparting agent, a triazole-based adhesion imparting agent, a triazole-based adhesion imparting agent, a triazole-based adhesion imparting agent, a triazole-based adhesion imparting agent, a triazole-based adhesion imparting agent, a triazole-based adhesion imparting agent, a triazole-based adhesion Examples of the additives include adhesion imparting agents such as stilbene derivatives, hindered phenol antioxidants, and other antioxidants; fluorescent whitening agents such as stilbene derivatives; surfactants such as fluorine surfactants and silicone surfactants; flame retardants such as phosphorus flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen flame retardants (e.g., melamine sulfate), halogen flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate ester dispersants, polyoxyalkylene dispersants, acetylene dispersants, silicone dispersants, anionic dispersants, and cationic dispersants; stabilizers such as borate stabilizers, titanate stabilizers, aluminate stabilizers, zirconate stabilizers, isocyanate stabilizers, carboxylic acid stabilizers, and carboxylic anhydride stabilizers. (I) The optional additives may be used alone or in combination of two or more.
[0145] [(J) Solvent] The resin composition according to one embodiment of the present invention may further contain a (J) solvent as an optional volatile component in combination with the non-volatile components such as the above-mentioned components (A) to (I). As the (J) solvent, an organic solvent is usually used. Examples of the organic solvent include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, and anisole; alcohol-based solvents such as methanol, ethanol, propanol, butanol, and ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, and methyl methoxypropionate. Examples of suitable solvents include ether ester solvents such as ethyl acetate, ester alcohol solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate, ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butylcarbitol), amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone, sulfoxide solvents such as dimethyl sulfoxide, nitrile solvents such as acetonitrile and propionitrile, aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane, and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. (J) Solvents may be used alone or in combination of two or more.
[0146] The amount of (J) solvent is not particularly limited, but may be, for example, 60 mass% or less, 40 mass% or less, 30 mass% or less, 20 mass% or less, 15 mass% or less, 10 mass% or less, etc., relative to 100 mass% of all components of the resin composition, or may be 0 mass%.
[0147] [Method of producing resin composition] The resin composition according to one embodiment of the present invention can be produced, for example, by mixing the above-mentioned components. The above-mentioned components may be mixed in part or in whole simultaneously, or may be mixed in order. In the process of mixing each component, the temperature may be appropriately set, and thus heating and / or cooling may be performed temporarily or throughout. In addition, stirring or shaking may be performed in the process of mixing each component.
[0148] [Characteristics of resin composition] A cured product is obtained by curing the resin composition according to one embodiment of the present invention. During the curing, heat is usually applied to the resin composition. Thus, among the components contained in the resin composition, volatile components such as (J) solvent can usually be volatilized by heat during curing, but non-volatile components such as components (A) to (I) do not volatilize by heat during curing. Thus, the cured product of the resin composition can contain the non-volatile components of the resin composition or their reaction products.
[0149] The cured product of the resin composition according to one embodiment of the present invention has excellent crack resistance. Therefore, when an insulating layer is formed from this cured product, an insulating layer having excellent crack resistance can be obtained. For example, when crack resistance is evaluated by the method described in <Test Example 5: Evaluation of Crack Resistance> in the Examples described later, the yield can be preferably 40% or more, more preferably 60% or more, and particularly preferably 80% or more. Usually, the higher the yield value, the more excellent the crack resistance.
[0150] The cured product of the resin composition according to one embodiment of the present invention has excellent desmear resistance. Therefore, when an insulating layer is formed from this cured product, the surface roughness of the insulating layer after desmear treatment can be reduced. For example, when the arithmetic mean roughness Ra of the surface of the insulating layer after desmear treatment is measured by the method described in <Test Example 3: Measurement of arithmetic mean roughness (Ra)> in the Examples below, the arithmetic mean roughness Ra can be preferably 95 nm or less, more preferably 90 nm or less. Usually, the smaller the arithmetic mean roughness Ra, the more excellent the desmear characteristics.
[0151] The cured product of the resin composition according to one embodiment of the present invention can usually have excellent dielectric properties. For example, the relative dielectric constant of the cured product is preferably 4.0 or less, more preferably 3.6 or less, and particularly preferably 3.4 or less. The lower limit of the relative dielectric constant is not particularly limited, and can be, for example, 1.5 or more, 2.0 or more, etc. Also, for example, the dielectric loss tangent of the cured product is preferably 0.0040 or less, more preferably 0.0035 or less, even more preferably 0.0030 or less, and particularly preferably 0.0027 or less. The lower limit of the dielectric loss tangent is not particularly limited, and can be, for example, 0.0010 or more. The relative dielectric constant and dielectric loss tangent of the cured product can be measured by the method described in <Test Example 1: Measurement of relative dielectric constant (Dk) and dielectric loss tangent (Df)> in the examples described later.
[0152] The cured product of the resin composition according to one embodiment of the present invention can usually have high adhesion to the conductor layer when a conductor layer is formed on the cured product. For example, when a conductor layer is formed on an insulating layer made of a cured product by the method described in <Test Example 4: Measurement of peel strength of plated conductor layer> in the Examples below, the peel strength between the insulating layer and the conductor layer is preferably 0.30 kgf / cm or more, more preferably 0.38 kgf / cm or more, and particularly preferably 0.40 kgf / cm or more. The higher the upper limit, the better, but it is usually 0.8 kgf / cm or less. The peel strength represents the magnitude of the force required to peel the conductor layer from the insulating layer. Therefore, usually, the higher the peel strength, the better the adhesion.
[0153] The resin composition according to one embodiment of the present invention can usually have a low minimum melt viscosity. For example, when the minimum melt viscosity is measured by the method described in <Test Example 2: Measurement of Minimum Melt Viscosity> in the Examples below, the minimum melt viscosity is preferably 2,500 poise or less, more preferably 2,000 poise or less, and particularly preferably 1,500 poise or less. From the viewpoint of smoothly forming a thick insulating layer, the lower limit can be, for example, 500 poise or more, 700 poise or more, etc.
[0154] [Uses of resin composition] The resin composition according to one embodiment of the present invention can be used as a resin composition for insulating purposes, and can be particularly preferably used as a resin composition for forming an insulating layer (resin composition for forming an insulating layer). For example, the resin composition according to this embodiment can be preferably used as a resin composition for forming an insulating layer of a semiconductor chip package (resin composition for insulating layer of a semiconductor chip package) and a resin composition for forming an insulating layer of a circuit board (including a printed wiring board) (resin composition for insulating layer of a circuit board). In particular, the resin composition is suitable for forming an interlayer insulating layer provided between conductor layers. In addition, the resin composition is particularly suitable as a resin composition for forming an insulating layer of a printed wiring board (resin composition for forming an insulating layer of a printed wiring board).
[0155] Examples of semiconductor chip packages include FC-CSP, MIS-BGA package, ETS-BGA package, Fan-out type WLP (Wafer Level Package), Fan-in type WLP, Fan-out type PLP (Panel Level Package), and Fan-in type PLP.
[0156] The resin composition may also be used as an underfill material, for example, as a material for MUF (Molding Under Filling) that is used after a semiconductor chip is connected to a substrate.
[0157] Furthermore, the resin composition can be used in a wide range of applications in which resin compositions are used, such as sheet-like laminate materials such as resin sheets and prepregs, solder resists, die bonding materials, semiconductor encapsulating materials, hole filling resins, and component embedding resins.
[0158] [Sheet-type laminated material] The resin composition may be used by coating in the form of a varnish, but from an industrial perspective, it is preferable to use the resin composition in the form of a sheet-like laminate material containing the resin composition.
[0159] As the sheet-like laminate material, the following resin sheets and prepregs are preferred.
[0160] In one embodiment, the resin sheet includes a support and a resin composition layer formed on the support. The resin composition layer is formed of the above-mentioned resin composition. Thus, the resin composition layer usually contains a resin composition, and preferably contains only the resin composition.
[0161] The thickness of the resin composition layer is preferably 50 μm or less, more preferably 40 μm or less, from the viewpoint of thinning and of being able to provide a cured product having excellent insulation even if it is thin, by using the resin composition. The lower limit of the thickness of the resin composition layer is not particularly limited, but may be 5 μm or more, 10 μm or more, etc.
[0162] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.
[0163] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0164] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.
[0165] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.
[0166] As the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.
[0167] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.
[0168] In one embodiment, the resin sheet may further include an optional layer as necessary. For example, such an optional layer may be a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, it is possible to suppress adhesion of dirt and scratches on the surface of the resin composition layer.
[0169] The resin sheet can be produced, for example, by preparing a liquid (varnish-like) resin composition as is or by dissolving the resin composition in a solvent, applying this onto a support using a coating device such as a die coater, and then drying to form a resin composition layer.
[0170] The solvent may be the same as the (J) solvent described as a component of the resin composition. One type of solvent may be used alone, or two or more types may be used in combination.
[0171] Drying may be performed by a drying method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of the solvent in the resin composition layer is usually 10 mass % or less, preferably 5 mass % or less. Although it varies depending on the boiling point of the solvent in the resin composition, for example, when a resin composition containing 30 mass % to 60 mass % of the solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.
[0172] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it is usually possible to use the resin sheet by peeling off the protective film.
[0173] In one embodiment, the prepreg is formed by impregnating a sheet-like fiber substrate with the above-mentioned resin composition.
[0174] The sheet-like fiber substrate used for the prepreg may be, for example, a commonly used substrate for prepreg, such as glass cloth, aramid nonwoven fabric, or liquid crystal polymer nonwoven fabric. From the viewpoint of thinning, the thickness of the sheet-like fiber substrate is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less. The lower limit of the thickness of the sheet-like fiber substrate is not particularly limited, and is usually 10 μm or more.
[0175] The prepreg can be produced by a method such as a hot melt method or a solvent method.
[0176] The thickness of the prepreg can be in the same range as that of the resin composition layer in the resin sheet described above.
[0177] The sheet-like laminate material can be suitably used, for example, to form an insulating layer in the manufacture of a semiconductor chip package (resin sheet for insulating a semiconductor chip package). Examples of applicable semiconductor chip packages include fan-out type WLP, fan-in type WLP, fan-out type PLP, and fan-in type PLP. The sheet-like laminate material can also be used, for example, to form an insulating layer of a circuit board (resin sheet for insulating layer of a circuit board). Furthermore, the sheet-like laminate material may be used as a material for a MUF used after connecting a semiconductor chip to a board. In particular, the sheet-like laminate material is suitable for forming an interlayer insulating layer.
[0178] [Circuit board] A circuit board according to one embodiment of the present invention includes a cured product of a resin composition. Typically, the circuit board includes an insulating layer formed of the cured product of the resin composition. The insulating layer includes the cured product of the above-mentioned resin composition, and preferably includes only the cured product of the above-mentioned resin composition. This circuit board can be manufactured, for example, by a manufacturing method including the following steps (I) and (II). (I) A step of forming a resin composition layer on an inner layer substrate. (II) A step of curing the resin composition layer to form an insulating layer.
[0179] The "inner layer substrate" used in step (I) is a member that serves as the base material of a circuit board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The substrate may have a conductor layer on one or both sides, and the conductor layer may be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of the substrate may be called an "inner layer circuit substrate". In addition, an intermediate product on which an insulating layer and / or a conductor layer is to be further formed during the manufacture of a circuit substrate is also included in the above-mentioned "inner layer substrate". When the circuit substrate is a circuit board with built-in components, an inner layer substrate with built-in components may be used.
[0180] When the conductor layer of the inner layer substrate is patterned, the minimum line / space ratio of the conductor layer is preferably small in order to utilize the advantage of excellent crack resistance. "Line" refers to the circuit width of the conductor layer, and "space" refers to the distance between the circuits. The range of the minimum line / space ratio is preferably 50 / 50 μm or less (i.e., pitch is 100 μm or less), more preferably 30 / 30 μm or less, even more preferably 20 / 20 μm or less, even more preferably 15 / 15 μm or less, and even more preferably 10 / 10 μm or less. The lower limit may be, for example, 0.5 / 0.5 μm or more. The pitch may be uniform or non-uniform throughout the conductor layer. The minimum pitch of the conductor layer may be, for example, 100 μm or less, 60 μm or less, 40 μm or less, 36 μm or less, or 30 μm or less.
[0181] The resin composition layer can be formed on the inner layer substrate by, for example, laminating the inner layer substrate and the resin sheet. The inner layer substrate and the resin sheet can be laminated by, for example, thermocompression bonding the resin sheet to the inner layer substrate from the support side. Examples of the member for thermocompression bonding the resin sheet to the inner layer substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (such as a SUS roll). It is preferable to press the thermocompression bonding member through an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the inner layer substrate, rather than directly pressing the resin sheet with the thermocompression bonding member.
[0182] The lamination of the inner layer substrate and the resin sheet may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably performed under reduced pressure conditions of 26.7hPa or less.
[0183] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.
[0184] After lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.
[0185] The support may be removed between step (I) and step (II) or after step (II).
[0186] In step (II), the resin composition layer is cured to form an insulating layer made of a cured product of the resin composition. The resin composition layer is usually cured by thermal curing. Specific curing conditions for the resin composition layer may vary depending on the type of resin composition. In one example, the curing temperature is preferably 120°C to 240°C, more preferably 150°C to 220°C, and even more preferably 170°C to 210°C. The curing time may be preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.
[0187] The method for producing a circuit board preferably includes preheating the resin composition layer at a temperature lower than the curing temperature before the thermal curing of the resin composition layer. For example, prior to thermal curing of the resin composition layer, the resin composition layer may be preheated at a temperature of usually 50° C. to 150° C., preferably 60° C. to 140° C., more preferably 70° C. to 130° C. for usually 5 minutes or more, preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes.
[0188] In producing a circuit board, the steps of (III) drilling holes in the insulating layer, (IV) desmearing the insulating layer, and (V) forming a conductor layer may be further carried out. These steps (III) to (V) may be carried out according to various methods known to those skilled in the art for use in producing circuit boards. When the support is removed after step (II), the support may be removed between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V). If necessary, the steps (I) to (V) of forming the insulating layer and the conductor layer may be repeated to produce a circuit board having a multilayer structure such as a multilayer printed wiring board.
[0189] In another embodiment, the circuit board can be manufactured using the above-mentioned prepreg. The manufacturing method can be basically the same as when a resin sheet is used.
[0190] Step (III) is a step of drilling holes in the insulating layer, which allows holes such as via holes and through holes to be formed in the insulating layer. Step (III) may be performed using, for example, a drill, a laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The size and shape of the hole may be appropriately determined depending on the design of the circuit board.
[0191] Step (IV) is a step of removing smears (resin residues) that may be present on the insulating layer. Usually, in this step (IV), the surface of the insulating layer is roughened, so the desmear treatment is sometimes called a "roughening treatment". The procedure and conditions of the desmear treatment are not particularly limited, and known procedures and conditions that are usually used when forming an insulating layer of a circuit board can be adopted. For example, the desmear treatment can be applied to the insulating layer by carrying out a swelling treatment using a swelling liquid, a roughening treatment using an oxidizing agent, and a neutralization treatment using a neutralizing liquid in this order.
[0192] Examples of the swelling liquid used in the desmear treatment include an alkaline solution and a surfactant solution, and an alkaline solution is preferred. As the alkaline solution, a sodium hydroxide solution and a potassium hydroxide solution are more preferred. Examples of commercially available swelling liquids include "Swelling Dip Securigans P" and "Swelling Dip Securigans SBU" manufactured by Atotech Japan. The swelling treatment using a swelling liquid can be performed by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferred to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes.
[0193] An example of an oxidizing agent used in the desmear treatment is an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 minutes to 30 minutes. The concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securigans P" manufactured by Atotech Japan.
[0194] The neutralizing solution used in the desmear treatment is preferably an acidic aqueous solution, and a commercially available product is, for example, "Reduction Solution Securigant P" manufactured by Atotech Japan. The treatment with the neutralizing solution can be performed by immersing the surface that has been roughened with an oxidizing agent in a neutralizing solution at 30°C to 80°C for 5 to 30 minutes. From the viewpoint of workability, etc., a method in which the object that has been roughened with an oxidizing agent is immersed in a neutralizing solution at 40°C to 70°C for 5 to 20 minutes is preferred.
[0195] Step (V) is a step of forming a conductor layer, and the conductor layer is formed on the insulating layer. The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among these, from the viewpoints of versatility in forming the conductor layer, cost, ease of patterning, and the like, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.
[0196] The conductor layer may be a single-layer structure, or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.
[0197] The thickness of the conductor layer depends on the desired design of the circuit board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.
[0198] In one embodiment, the conductor layer may be formed by plating. For example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method. From the viewpoint of ease of production, the semi-additive method is preferred. Below, an example of forming the conductor layer by the semi-additive method is shown.
[0199] First, a plating seed layer is formed on the surface of an insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.
[0200] In another embodiment, the conductor layer may be formed using a metal foil. When the conductor layer is formed using a metal foil, it is preferable to carry out step (V) between steps (I) and (II). For example, after step (I), the support is removed, and a metal foil is laminated on the exposed surface of the resin composition layer. The lamination of the resin composition layer and the metal foil may be carried out by a vacuum lamination method. The lamination conditions may be the same as those described for step (I). Next, step (II) is carried out to form an insulating layer. Thereafter, a conductor layer having a desired wiring pattern can be formed by a conventionally known technique such as a subtractive method or a modified semi-additive method, using the metal foil on the insulating layer.
[0201] The metal foil can be produced by a known method such as an electrolytic method, a rolling method, etc. Commercially available metal foils include, for example, HLP foil and JXUT-III foil manufactured by JX Nippon Mining & Metals Corporation, and 3EC-III foil and TP-III foil manufactured by Mitsui Mining & Smelting Co., Ltd.
[0202] [Semiconductor chip package] A semiconductor chip package according to an embodiment of the present invention includes a cured resin composition. Typically, the semiconductor chip package includes an insulating layer formed of the cured resin composition. The insulating layer includes the cured resin composition described above, and preferably includes only the cured resin composition described above. Examples of this semiconductor chip package include the following.
[0203] The semiconductor chip package according to the first example includes the above-mentioned circuit board and a semiconductor chip mounted on the circuit board. This semiconductor chip package can be manufactured by bonding the semiconductor chip to the circuit board.
[0204] The bonding conditions between the circuit board and the semiconductor chip may be any conditions that allow conductive connection between the terminal electrodes of the semiconductor chip and the circuit wiring of the circuit board. For example, the conditions used in flip-chip mounting of the semiconductor chip may be used. Also, for example, the semiconductor chip and the circuit board may be bonded via an insulating adhesive.
[0205] An example of a bonding method is a method of bonding a semiconductor chip to a circuit board. The bonding conditions are that the bonding temperature is usually in the range of 120°C to 240°C (preferably in the range of 130°C to 200°C, more preferably in the range of 140°C to 180°C), and the bonding time is usually in the range of 1 second to 60 seconds (preferably in the range of 5 seconds to 30 seconds).
[0206] Another example of the bonding method is a method of bonding a semiconductor chip to a circuit board by reflow. The reflow conditions may be in the range of 120°C to 300°C.
[0207] After the semiconductor chip is bonded to the circuit board, the semiconductor chip may be filled with a molded underfill material, which may be the resin composition described above.
[0208] The semiconductor chip package according to the second example includes a semiconductor chip and an insulating layer formed of a cured product of a resin composition. Examples of the semiconductor chip package according to the second example include a fan-out type WLP and a fan-out type PLP.
[0209] Fig. 1 is a cross-sectional view showing a fan-out type WLP as an example of a semiconductor chip package according to an embodiment of the present invention. A semiconductor chip package 100 as a fan-out type WLP includes, for example, a semiconductor chip 110, a sealing layer 120 formed to cover the periphery of the semiconductor chip 110, a rewiring formation layer 130 as an insulating layer provided on the surface of the semiconductor chip 110 opposite to the sealing layer 120, a rewiring layer 140 as a conductor layer, a solder resist layer 150, and bumps 160, as shown in Fig. 1.
[0210] The method for manufacturing such a semiconductor chip package includes: (i) laminating a temporary fixing film onto a substrate; (ii) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (iii) forming an encapsulation layer on the semiconductor chip; (iv) peeling the substrate and the temporary fixing film from the semiconductor chip; (v) forming a rewiring formation layer on the surface from which the substrate and the temporary fixing film of the semiconductor chip have been peeled off; (vi) forming a redistribution layer as a conductor layer on the redistribution layer; and (vii) forming a solder resist layer on the rewiring layer; The method for manufacturing the semiconductor chip package further comprises: (viii) dicing the plurality of semiconductor chip packages into individual semiconductor chip packages; may also include
[0211] (Step (i)) Step (i) is a step of laminating a temporary fixing film on a substrate. The lamination conditions for the substrate and the temporary fixing film can be the same as the lamination conditions for the inner layer substrate and the resin sheet in the method for producing a circuit board.
[0212] Examples of the substrate include silicon wafers; glass wafers; glass substrates; metal substrates such as copper, titanium, stainless steel, and cold-rolled steel (SPCC); substrates such as FR-4 substrates in which glass fibers are impregnated with epoxy resin or the like and then heat-cured; and substrates made of bismaleimide triazine resins such as BT resin.
[0213] The temporary fixing film may be made of any material that can be peeled off from the semiconductor chip and can temporarily fix the semiconductor chip. Commercially available products include "Riva Alpha" manufactured by Nitto Denko Corporation.
[0214] (Step (ii)) Step (ii) is a step of temporarily fixing the semiconductor chip on the temporary fixing film. The temporary fixing of the semiconductor chip can be performed using, for example, a device such as a flip chip bonder or a die bonder. The layout and number of the semiconductor chips can be appropriately set depending on the shape and size of the temporary fixing film, the number of semiconductor chip packages to be produced, etc. For example, the semiconductor chips may be temporarily fixed by arranging them in a matrix shape of multiple rows and multiple columns.
[0215] (Step (iii)) Step (iii) is a step of forming an encapsulating layer on the semiconductor chip. The encapsulating layer can be formed, for example, from a photosensitive resin composition or a thermosetting resin composition. This encapsulating layer may be formed from a cured product of the resin composition according to the above-mentioned embodiment. The encapsulating layer can usually be formed by a method including a step of forming a resin composition layer on the semiconductor chip and a step of curing this resin composition layer to form the encapsulating layer.
[0216] (Step (iv)) Step (iv) is a step of peeling off the substrate and the temporary fixing film from the semiconductor chip. It is desirable to adopt an appropriate peeling method according to the material of the temporary fixing film. For example, the peeling method may be a method of heating, foaming or expanding the temporary fixing film to peel it off. In addition, for example, the peeling method may be a method of irradiating the temporary fixing film with ultraviolet light through the substrate to reduce the adhesive strength of the temporary fixing film to peel it off.
[0217] When the base material and the temporary fixing film are peeled off from the semiconductor chip as described above, the surface of the encapsulating layer is exposed. The manufacturing method of the semiconductor chip package may include polishing the exposed surface of the encapsulating layer. By polishing, the smoothness of the surface of the encapsulating layer can be improved.
[0218] (Process (v)) Step (v) is a step of forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film are peeled off. Usually, this rewiring formation layer is formed on the semiconductor chip and the sealing layer. The rewiring formation layer can be formed by a cured product of the resin composition according to the above-mentioned embodiment. Usually, the rewiring formation layer can be formed by a method including a step of forming a resin composition layer on the semiconductor chip and a step of curing the resin composition layer to form the rewiring formation layer. The formation of the resin composition layer on the semiconductor chip can be performed by the same method as the method of forming the resin composition layer on the inner layer substrate described in the above-mentioned method for producing a circuit board, except that a semiconductor chip is used instead of the inner layer substrate.
[0219] After forming a resin composition layer on a semiconductor chip, the resin composition layer is cured to obtain a rewiring formation layer as an insulating layer containing a cured product of the resin composition. The curing conditions of the resin composition layer may be the same as the curing conditions of the resin composition layer in the manufacturing method of a circuit board. When the resin composition layer is thermally cured, the resin composition layer may be subjected to a preheating treatment in which the resin composition layer is heated at a temperature lower than the curing temperature before the thermal curing. The treatment conditions of this preheating treatment may be the same as the preheating treatment in the manufacturing method of a circuit board. Usually, after forming the rewiring formation layer, holes are formed in the rewiring formation layer to connect the semiconductor chip and the rewiring layer.
[0220] (Step (vi)) Step (vi) is a step of forming a redistribution layer as a conductor layer on the redistribution formation layer. The method of forming the redistribution layer on the redistribution formation layer may be the same as the method of forming a conductor layer on an insulating layer in the method of manufacturing a circuit board. Steps (v) and (vi) may be repeated to alternately stack the redistribution layer and the redistribution formation layer (build up).
[0221] (Step (vii)) Step (vii) is a step of forming a solder resist layer on the rewiring layer. The material of the solder resist layer can be any material having insulating properties. Among them, from the viewpoint of ease of manufacturing the semiconductor chip package, a photosensitive resin composition and a thermosetting resin composition are preferred. The solder resist layer may be formed by a cured product of the resin composition according to the above-mentioned embodiment.
[0222] In step (vii), bumping may be performed to form bumps, if necessary. The bumping may be performed by a method such as solder balls or solder plating. In the bumping, via holes may be formed in the same manner as in step (v).
[0223] (Step (viii)) The method for producing a semiconductor chip package may include a step (viii) in addition to the steps (i) to (vii). The step (viii) is a step of dicing a plurality of semiconductor chip packages into individual semiconductor chip packages to separate them. The method for dicing the semiconductor chip packages into individual semiconductor chip packages is not particularly limited.
[0224] [Semiconductor Devices] The semiconductor device includes the above-mentioned circuit board or semiconductor chip package. Examples of the semiconductor device include various semiconductor devices used in electrical products (e.g., computers, mobile phones, smartphones, tablet devices, wearable devices, digital cameras, medical devices, televisions, etc.) and vehicles (e.g., motorcycles, automobiles, trains, ships, aircraft, etc.). EXAMPLES
[0225] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the following examples. In the following description, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Furthermore, unless otherwise specified, the temperature and pressure conditions were room temperature (25°C) and atmospheric pressure (1 atm). In the following description, "L / S" represents the line / space ratio of the wiring pattern, unless otherwise specified.
[0226] <Reagent Description> The long-chain aliphatic phenol resin ("LB-7000" manufactured by Tohoku Kako Co., Ltd., active group equivalent weight approximately 262 g / eq.) was a resin containing 90% cardanol represented by the following formula (a-1-1) and 10% cardol represented by the following formula (a-2-1). The long-chain aliphatic phenol resin ("LB-7250" manufactured by Tohoku Kako Co., Ltd., active group equivalent weight approximately 273 g / eq.) was a resin containing 95% cardanol represented by the following formula (a-1-1) and 5% cardol represented by the following formula (a-2-1).
[0227] [ka]
[0228] (In the above formula, "*" represents a bond.)
[0229] <Synthesis Example 1: Synthesis of phenolic hydroxyl group-containing polybutadiene resin (elastomer X)> In a reaction vessel, 69 g of bifunctional hydroxyl-terminated polybutadiene ("G-3000" manufactured by Nippon Soda Co., Ltd., number average molecular weight = 3000, hydroxyl equivalent = 1800 g / eq.), 40 g of aromatic hydrocarbon mixed solvent ("IPZOL 150" manufactured by Idemitsu Kosan Co., Ltd.), and 0.005 g of dibutyltin laurate were placed and mixed to dissolve uniformly. When the mixture became uniform, the temperature was raised to 60°C, and 8 g of isophorone diisocyanate ("IPDI" manufactured by Evonik Japan Co., Ltd., isocyanate equivalent = 113 g / eq.) was added while stirring, and the reaction was carried out for about 3 hours.
[0230] Next, 23 g of cresol novolak resin (DIC "KA-1160", hydroxyl equivalent = 117 g / eq.) and 60 g of ethyl diglycol acetate (Daicel) were added to the reaction mixture, and the mixture was heated to 150°C with stirring and reacted for about 10 hours. -1 The disappearance of the NCO peak was confirmed. The disappearance of the NCO peak was regarded as the end point of the reaction, and the reaction product was cooled to room temperature. The reaction product was then filtered through a 100-mesh filter cloth to obtain an elastomer X having a butadiene structure and a phenolic hydroxyl group (phenolic hydroxyl group-containing butadiene resin: non-volatile components 50% by mass). The number average molecular weight of the elastomer X was 5900, and the glass transition temperature was -7°C.
[0231] <Example 1> 15 parts of biphenyl type epoxy resin ("NC3000L" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 269 g / eq.) and 5 parts of bisphenol type epoxy resin ("ZX1059" manufactured by Nippon Steel Chemical & Material Co., Ltd., 1:1 mixture of bisphenol A type and bisphenol F type, epoxy equivalent of about 169 g / eq.) were dissolved in 25 parts of solvent naphtha with stirring under heating to obtain a solution. This solution was cooled to room temperature to prepare a dissolved composition of epoxy resin.
[0232] The epoxy resin solution composition was mixed with 2 parts of a long-chain aliphatic phenolic resin (Tohoku Kako Co., Ltd. "LB-7000", active group equivalent of about 262 g / eq.), 68 parts of an active ester compound (DIC Corporation "HPC-8150-62T", active ester group equivalent of about 220 g / eq., toluene solution with non-volatile content of 62 mass%), and 10 parts of a triazine skeleton-containing phenolic hardener (DIC Corporation "LA-3018-50P", active group equivalent of about 100 g / eq.). 151g / eq., 2-methoxypropanol solution with non-volatile content of 50%), 5 parts of a carbodiimide curing agent (Nisshinbo Chemical's "V-03", active group equivalent of approximately 216g / eq., toluene solution with non-volatile content of 50%), 12 parts of spherical silica (Admatechs' "SO-C2", average particle size 0.5μm, specific surface area 5.8m) surface-treated with a silane coupling agent (Shin-Etsu Chemical's "KBM-573"). 2 A resin composition was prepared by mixing 200 parts of a 200% polyaniline stearate copolymer (1.2 g / g), 0.3 parts of an imidazole curing accelerator ("1B2PZ" manufactured by Shikoku Chemical Industry Co., Ltd., 1-benzyl-2-phenylimidazole), and 4 parts of a phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK and cyclohexanone with a non-volatile content of 30% by mass) and dispersing the mixture uniformly in a high-speed rotating mixer.
[0233] <Example 2> In Example 1, 20 parts of naphthalene type epoxy resin (DIC Corporation's "HP-4032-SS", 1,6-bis(glycidyloxy)naphthalene, epoxy equivalent of about 145 g / eq.) were used instead of 15 parts of biphenyl type epoxy resin (Nippon Kayaku Co., Ltd.'s "NC3000L", epoxy equivalent of about 269 g / eq.) and 5 parts of bisphenol type epoxy resin (Nippon Steel Chemical & Material Co., Ltd.'s "ZX1059", 1:1 mixture of bisphenol A type and bisphenol F type, epoxy equivalent of about 169 g / eq.). In addition, the amount of long chain aliphatic phenol resin (Tohoku Kako Co., Ltd.'s "LB-7000", active group equivalent of about 262 g / eq.) was increased from 2 parts to 4 parts. Further, instead of 68 parts of an active ester compound (DIC Corporation's "HPC-8150-62T", active ester group equivalent of about 220 g / eq., toluene solution with non-volatile content of 62 mass%), 62 parts of an active ester compound (DIC Corporation's "HPC-8000-65T", active ester group equivalent of about 223 g / eq., toluene solution with non-volatile content of 65%) was used. Except for the above, a resin composition was prepared in the same manner as in Example 1.
[0234] <Example 3> In Example 1, instead of 15 parts of the biphenyl type epoxy resin ("NC3000L" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 269 g / eq.), 15 parts of naphthol type epoxy resin ("ESN475V" manufactured by Nippon Steel Chemical & Material Co., Ltd., epoxy equivalent of about 330 g / eq.) were used. In addition, instead of 2 parts of the long chain aliphatic phenol resin ("LB-7000" manufactured by Tohoku Kako Co., Ltd., active group equivalent of about 262 g / eq.), 2 parts of another long chain aliphatic phenol resin ("LB-7250" manufactured by Tohoku Kako Co., Ltd., active group equivalent of about 273 g / eq.) were used. A resin composition was prepared in the same manner as in Example 1 except for the above.
[0235] <Example 4> In Example 3, 2 parts of another long-chain aliphatic phenolic resin ("Urushiol" manufactured by Tokyo Chemical Industry Co., Ltd., active group equivalent of about 174 g / eq.) was used instead of 2 parts of the long-chain aliphatic phenolic resin ("LB-7250" manufactured by Tohoku Kako Co., Ltd., active group equivalent of about 273 g / eq.). A resin composition was prepared in the same manner as in Example 3, except for the above.
[0236] <Example 5> In Example 1, 4 parts of biphenylaralkylnovolac maleimide ("MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd., MEK / toluene mixed solution with non-volatile content of 70%) was added to the resin composition. A resin composition was prepared in the same manner as in Example 1 except for the above.
[0237] <Example 6> In Example 1, 3 parts of a bimaleimide-terminated polyimide compound ("BMI-1500" manufactured by DMI Corporation) was added to the resin composition. A resin composition was prepared in the same manner as in Example 1 except for the above.
[0238] <Example 7> In Example 1, 3 parts of methacrylic modified polyphenylene ether (SA9000-111 manufactured by SABIC Innovative Plastics) was added to the resin composition. A resin composition was prepared in the same manner as in Example 1 except for the above.
[0239] <Example 8> In Example 1, 4 parts of vinylbenzyl-modified polyphenylene ether ("OPE-2St 2200" manufactured by Mitsubishi Gas Chemical Co., Ltd., a toluene solution with a non-volatile content of 65%) was added to the resin composition. A resin composition was prepared in the same manner as in Example 1 except for the above.
[0240] <Comparative Example 1> In Example 1, 2 parts of the long-chain aliphatic phenol resin (Tohoku Kako Co., Ltd. "LB-7000", active group equivalent weight: about 262 g / eq.) was not used. A resin composition was prepared in the same manner as in Example 1 except for the above.
[0241] <Comparative Example 2> In Example 2, 4 parts of a novolac-type phenolic curing agent (DIC Corporation's "TD-2090", active group equivalent: about 105 g / eq.) was used instead of 4 parts of a long-chain aliphatic phenolic resin (Tohoku Kako Corporation's "LB-7000", active group equivalent: about 262 g / eq.). A resin composition was prepared in the same manner as in Example 2, except for the above.
[0242] <Comparative Example 3> In Example 1, 2.5 parts of an epoxidized polybutadiene resin (Daicel Corporation's "PB3600M", epoxy equivalent: about 193 g / eq.) was used as a stress relaxation component instead of 2 parts of the long-chain aliphatic phenol resin (Tohoku Kako Corporation's "LB-7000", active group equivalent: about 262 g / eq.). A resin composition was prepared in the same manner as in Example 1, except for the above.
[0243] <Comparative Example 4> In Example 1, 10 parts of the elastomer X prepared in Synthesis Example 1 were used as a stress relaxation component instead of 2 parts of the long-chain aliphatic phenolic resin (Tohoku Kako Co., Ltd. "LB-7000", active group equivalent weight approximately 262 g / eq.). Except for the above, a resin composition was prepared in the same manner as in Example 1.
[0244] <Production of resin sheets> A polyethylene terephthalate film with a release layer ("AL5" manufactured by Lintec Corporation, thickness 38 μm) was prepared as a support. The resin compositions obtained in the above-mentioned Examples and Comparative Examples were uniformly applied onto the release layer of this support so that the thickness of the resin composition layer after drying was 40 μm. Thereafter, the resin composition was dried at 80°C to 100°C (average 90°C) for 4 minutes to obtain a resin sheet including a support and a resin composition layer.
[0245] <Test Example 1: Measurement of relative dielectric constant (Dk) and dielectric loss tangent (Df)> The resin sheet was heated at 200°C for 90 minutes to heat-cure the resin composition layer, and then the support was peeled off to obtain a cured film formed of the cured product of the resin composition. The cured film was cut into a piece having a width of 2 mm and a length of 80 mm to obtain a cured product A for evaluation.
[0246] The dielectric constant (Dk value) and dielectric loss tangent (Df value) of the obtained cured product A for evaluation were measured by the cavity resonance perturbation method at a measurement frequency of 5.8 GHz and a measurement temperature of 23° C. using an “HP8362B” manufactured by Agilent Technologies. Measurements were performed on three test pieces, and the average values were calculated.
[0247] <Test Example 2: Measurement of minimum melt viscosity> 25 resin composition layers of the resin sheet were stacked to obtain a resin composition layer having a thickness of 1 mm. This resin composition layer was punched out to a diameter of 20 mm to prepare a measurement sample. The minimum melt viscosity (poise) was obtained by measuring the dynamic viscoelastic modulus of the prepared measurement sample using a dynamic viscoelasticity measuring device (UBM's "Rheogel-G3000") under the measurement conditions of starting temperature from 60°C to 200°C, heating rate of 5°C / min, measurement temperature interval of 2.5°C, and vibration frequency of 1Hz.
[0248] <Test Example 3: Measurement of arithmetic mean roughness (Ra)> (1) Surface preparation for interior boards: A glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, substrate thickness 0.8 mm, Panasonic "R1515A") with copper foil on the surface was prepared as an inner layer substrate. The copper foil on the surface of this inner layer substrate was etched with a microetching agent (Mec "CZ8101") with a copper etching amount of 1 μm to perform a roughening treatment. Then, it was dried at 190°C for 30 minutes.
[0249] (2) Lamination and curing of resin sheets: The resin sheet was laminated on both sides of the inner layer substrate using a batch type vacuum pressure laminator (two-stage build-up laminator "CVP700" manufactured by Nikko Materials Co., Ltd.) so that the resin composition layer was bonded to the inner layer substrate. This lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at a temperature of 100°C and a pressure of 0.74 MPa for 30 seconds.
[0250] The laminated resin sheet was then heat-pressed at atmospheric pressure at 100°C and a pressure of 0.5 MPa for 60 seconds to smooth it out. It was then placed in an oven at 130°C and heated for 30 minutes, and then transferred to an oven at 170°C and heated for 30 minutes. The resin composition layer was cured by the above heating, and an insulating layer was formed.
[0251] (3) Formation of via holes: Using a CO2 laser processing machine (LK-2K212 / 2C) manufactured by Via Mechanics, the insulating layer was processed under the conditions of a frequency of 2000Hz, a pulse width of 3μsec, an output of 0.95W, and a shot number of 3 to form a via hole. The opening diameter (top diameter, diameter) of the via hole on the insulating layer surface was 50μm, and the diameter of the via hole on the insulating layer bottom surface was 40μm. Then, the polyethylene terephthalate film as the support was peeled off to obtain a sample substrate having a layer structure of insulating layer / inner layer substrate / insulating layer.
[0252] (4) Desmear treatment: The sample substrate was immersed in a swelling solution, Swelling Dip Securigant P (manufactured by Atotech Japan), at 60°C for 10 minutes. Next, the sample substrate was immersed in a roughening solution, Concentrate Compact P (aqueous solution of KMnO4: 60g / L, NaOH: 40g / L) (manufactured by Atotech Japan), at 80°C for 20 minutes. Finally, the sample substrate was immersed in a neutralizing solution, Reduction Solution Securigant P (manufactured by Atotech Japan), at 40°C for 5 minutes to obtain evaluation substrate A as a sample substrate after desmearing.
[0253] (5) Measurement of arithmetic mean roughness (Ra): The arithmetic mean roughness Ra of the surface of the insulating layer of the obtained evaluation substrate A was measured using a non-contact surface roughness meter (WYKO NT3300 manufactured by B-CO Instruments) under the measurement conditions of VSI mode, 50x lens, and measurement range of 121μm×92μm. For each evaluation substrate A, the arithmetic mean roughness Ra was measured at 10 randomly selected points, and the average value was calculated.
[0254] <Test Example 4: Measurement of peel strength of plated conductor layer> The evaluation substrate A obtained in the step "(4) desmear treatment" in the same manner as in the above-mentioned Test Example 3 was immersed in an electroless plating solution containing PdCl2 at 40°C for 5 minutes, and then immersed in an electroless copper plating solution at 25°C for 20 minutes. After heating at 150°C for 30 minutes to perform an annealing treatment, an etching resist was formed, and after pattern formation by etching, copper sulfate electrolytic plating was performed to form a conductor layer with a thickness of 30 μm on the insulating layer. Next, an annealing treatment was performed at 200°C for 60 minutes to obtain an evaluation substrate B.
[0255] A cut was made in the conductor layer of evaluation board B, surrounding an area 10 mm wide and 150 mm long. One end of this area was peeled off and held with the grip of a tensile tester (Autocom type tester "AC-50C-SL" manufactured by TSE Corporation). It was pulled perpendicular to the insulating layer at a speed of 50 mm / min at room temperature (25°C), and the load [kgf / cm] when 100 mm was peeled off was measured as the peel strength.
[0256] <Test Example 5: Evaluation of crack resistance> (1) Lamination of resin sheet: An inner layer substrate (Hitachi Chemical's "MCL-E700G", conductor layer thickness 35 μm, total thickness 0.4 mm, residual copper ratio 40%) having circuit conductors (copper) formed on both sides in a wiring pattern of L / S = 8 μm / 8 μm was prepared. Resin sheets were laminated on both sides of this inner layer substrate so that the resin composition layer was in contact with the inner layer substrate. This lamination was performed using a vacuum pressure laminator (Meiki Seisakusho's "MVLP-500"), with vacuum suction at a temperature of 120°C for 30 seconds, followed by lamination at a temperature of 120°C and a pressure of 7.0 kg / cm. 2 Then, the substrate was pressed for 30 seconds using a heat-resistant rubber under atmospheric pressure at a temperature of 120°C and a pressure of 5.5 kg / cm using a stainless steel end plate. 2 The press was performed for 60 seconds under the above conditions.
[0257] (2) Thermal curing of the resin composition layer: The resin composition layer was thermally cured by heating at 130° C. for 30 minutes and then at 170° C. for 30 minutes to obtain an insulating layer as a cured layer made of the cured resin composition. The support was then peeled off to obtain a sample substrate having a layer structure of insulating layer / inner layer substrate / insulating layer.
[0258] (3) Roughening treatment: The insulating layer of the sample substrate was subjected to a roughening treatment. Specifically, the sample substrate was immersed in a swelling solution, Swelling Dip Securigant P (manufactured by Atotech Japan), at 60°C for 10 minutes. Next, it was immersed in a roughening solution, Concentrate Compact P (aqueous solution of KMnO4: 60g / L, NaOH: 40g / L) (manufactured by Atotech Japan), at 80°C for 20 minutes. Finally, it was immersed in a neutralizing solution, Reduction Solution Securigant P (manufactured by Atotech Japan), at 40°C for 5 minutes.
[0259] (4) Crack evaluation: The surface of the insulating layer after the roughening treatment was observed on the wiring pattern of the inner layer board. The surface of the insulating layer was checked for cracks along the pattern shapes of 100 inner layer boards, and the percentage of the number of parts on the pattern where cracks did not occur was counted. This percentage was calculated as the "yield." The calculated yield was also scored according to the following criteria. 1 point: 0% or more but less than 20%. 2 points: 20% or more but less than 40%. 3 points: 40% or more but less than 60%. 4 points: 60% or more but less than 80%. 5 points: 80% or above. A score of 3 or more was evaluated as "○", and a score of 2 or less was evaluated as "×".
[0260] <Result> The results of the above examples and comparative examples are shown in the table below.
[0261] [Table 1]
[0262] [Table 2] [Explanation of symbols]
[0263] 100 Semiconductor chip package 110 Semiconductor Chip 120 Sealing layer 130 Rewiring formation layer 140 Redistribution layer 150 Solder resist layer 160 Bump
Claims
[Claim 1] A resin composition comprising (A) a resin represented by the following formula (A-1), (B) an epoxy resin, and (C) an active ester compound: 【Chemistry 1】 (In formula (A-1), R 1 represents an optionally substituted chain aliphatic hydrocarbon group having 7 or more carbon atoms, R 2 represents a hydrocarbon group which may have a substituent, n represents a number of 1 or more; m represents a number of 0 or more. However, R 1 includes a chain unsaturated aliphatic hydrocarbon group having 7 or more carbon atoms which may have a substituent.
Citation Information
Patent Citations
Resin composition
JP2019048952A
Resin material and multilayer printed board
JP2020023714A
Manufacturing method of print circuit board
JP2020136542A