Metallized film, electromagnetic wave shield film, shield printed wiring board and method for producing the same
The metallized film with controlled crystal form and vacuum evaporation method addresses the challenge of maintaining low electrical resistance and gas transmission, ensuring stable electromagnetic shielding by preventing interlayer adhesion issues during high-temperature processes.
Patent Information
- Application Number
- JP2024138891
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-03-29
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 2024159836000005 
Figure 2024159836000006 
Figure 2024159836000007
Abstract
Description
[Technical field]
[0001] The present invention relates to an electromagnetic wave shielding film, a metallized film that can be used for the electromagnetic wave shielding film, and a method for producing the same. [Background technology]
[0002] In recent years, smartphones and tablet-type information terminals are required to have the ability to transmit large volumes of data at high speeds, and high-speed transmission of large volumes of data requires the use of high-frequency signals.
[0003] However, when high-frequency signals are used, electromagnetic noise is generated from the signal circuits on the printed wiring board, which can easily cause peripheral devices to malfunction. To prevent such malfunctions, it is therefore important to shield the printed wiring board from electromagnetic waves.
[0004] As a method for shielding a printed wiring board, an electromagnetic wave shielding film having a shielding layer and a conductive adhesive layer is used.
[0005] In these electromagnetic shielding films, the conductive adhesive layer is placed over an opening provided in an insulating layer covering the ground circuit of a printed wiring board, and the opening is filled with the conductive adhesive under heating and pressure. This connects the shielding layer and the ground circuit of the printed wiring board via the conductive adhesive, shielding the printed wiring board. The shielded printed wiring board is then exposed to a high temperature of about 270°C in a reflow process to connect the printed wiring board to electronic components.
[0006] Furthermore, after attaching an electronic component to a printed wiring board, in order to finely adjust the position of the electronic component, a process called repair may be performed in which the printed wiring board is heated to remove the electronic component from the printed wiring board and then the electronic component is attached again. Since it is necessary to attach the electronic component to the printed wiring board after the repair process, the electromagnetic wave shielding film is exposed to high temperatures again in the reflow process (Patent Document 1).
[0007] On the other hand, as the transmission signal becomes higher in frequency, the shield needs to have ground stability to reduce noise in the signal line, and is required to have low electrical resistance. When using a metal film for the shield, it is necessary to use a low-resistance metal (gold, silver, copper, etc.) and to make the film thicker. In this case, gas may be generated from the adhesive layer of the electromagnetic shielding film or the insulating film of the printed wiring board, and the gas may be blocked by the metal film, causing problems. In particular, when the base film of the printed wiring board is made of a highly hygroscopic resin such as polyimide, water vapor is generated from the base film when heated. These volatile components generated from the adhesive layer, insulating film, and base film cannot pass through the metal film, so they accumulate between the metal film and the adhesive layer. Therefore, if rapid heating is performed in the solder reflow process, the volatile components accumulated between the metal film and the adhesive layer may destroy the interlayer adhesion between the metal film and the adhesive layer. As a method for preventing this problem, a method has been proposed in which multiple openings are formed in the metal film to allow the volatile components to pass through (Patent Document 2). [Prior art documents] [Patent documents]
[0008] [Patent Document 1] International Publication No. 2017 / 111158 [Patent Document 2] Patent No. 6219383 Summary of the Invention [Problem to be solved by the invention]
[0009] In the metal film forming the openings as in Patent Document 2, soluble components that are highly soluble in the etching solution (solvent) are dispersed in the metal film, so if the soluble components are not uniform in shape and size and dispersed uniformly, the metal film after the openings are formed will have uneven film resistance, which may cause signal noise. In addition, since the etching rate of the etching solution changes depending on the frequency of use, it is necessary to manage the etching solution in order to form stable openings, which is as difficult and costly as the etching process used to form wiring. In particular, the examples described in the same document include a pretreatment process in which rolled copper foil and electrolytic copper foil are etched uniformly and thinly, but in order to etch uniformly and thinly, the management of dedicated equipment and dedicated etching solution is very strict, which increases costs.
[0010] The present invention has been made in consideration of the above problems, and has an object to stably provide a metallized film that has low electrical resistance yet is permeable to volatile components, and an electromagnetic wave shielding film using the same. [Means for solving the problem]
[0011] Means for Solving the Problems The present inventors have conducted extensive research in light of the above problems and have succeeded in obtaining a metallized film that has low electrical resistance yet is permeable to volatile components by controlling the crystal morphology using a vacuum deposition method.
[0012] That is, the present invention provides a metallized film having a metal film consisting of at least one metal layer on at least one side of the film, the metal film having a surface resistance of 0.04 Ω / □ or less, and a water vapor transmission rate of the metallized film according to JIS K7129:2008 of 3.5 g / (m) at a temperature of 40° C. and a humidity of 90% RH. 2 1.0 day) or more for metallized films.
[0013] The present invention also relates to a method for producing a metallized film, in which the metal film is formed by a vacuum deposition method.
[0014] The present invention further relates to an electromagnetic wave shielding film having an adhesive layer on one surface of the metal film of the metallized film. Effect of the Invention
[0015] In the present invention, a metal film with controlled crystal morphology is formed by vacuum deposition by roughening the surface of the film, making it possible to provide a metallized film that has low electrical resistance yet is permeable to volatile components, and an electromagnetic wave shielding film using the same. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic cross-sectional view of a typical method for producing a metal film on a metallized film by a vacuum deposition method. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a method for producing a metal film on a metallized film when an oblique deposition method of a vacuum deposition method is used. [Diagram 3] 1 is a cross-sectional schematic diagram of a method for producing a metal film of the metallized film of the present invention by a vacuum deposition method. [Figure 4] This is an image quality map of a cross section of a 2.0 μm thick metal film (two 1 μm thick metal layers) formed by copper vapor deposition on a flat PET film. [Diagram 5] This is an image quality map of a cross section of a 2.0 μm thick metal film (two 1 μm thick metal layers) formed by copper vapor deposition on a surface-roughened PET film. [Figure 6] 1 is a cross-sectional view of a metallized film according to an embodiment of the present invention. [Figure 7] 1 is a cross-sectional view of a metallized film according to an embodiment of the present invention. [Figure 8] 1 is a cross-sectional view of an electromagnetic wave shielding film according to an embodiment of the present invention. [Figure 9] 1 is a cross-sectional view of an electromagnetic wave shielding film according to an embodiment of the present invention. [Figure 10] 1 is a cross-sectional view of a shielded printed wiring board according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present invention will be described in detail below.
[0018] <Metallized film> Metallized film 1 of the present invention has metal film 301 on one or both surfaces of film 101 (FIGS. 6 and 7).
[0019] <Electromagnetic wave shielding film> Electromagnetic wave shielding film 2 has adhesive layer 601 on one surface of metal film 301 of metallized film 1 (FIGS. 8 and 9).
[0020] <Metal film> The metal film according to the present invention is an assembly of metal layers, which is a laminate of one or more layers containing metal as the main component (hereinafter referred to as metal layer). The main component means that the metal accounts for more than 50 atomic % when the entire layer is taken as 100 atomic %.
[0021] The surface resistance of the metal film 301 in the present invention is preferably 0.04 Ω / □ or less, and more preferably 0.02 Ω / □ or less. When transmitting high-frequency signals, the shield is required to shield noise generated by the signal line as well as to provide ground stability. If the electrical resistance of the shield is high, in addition to reducing the noise shielding rate, a voltage drop occurs due to the resistance, generating an electric potential on the shield, which is one of the causes of transmission attenuation of the signal line. The lower the surface resistance of the metal film, the more preferable it is, and for high-frequency signals of 1 GHz or more, the surface resistance value is preferably 0.04 Ω / □ or less, and more preferably 0.02 Ω / □ or less. The lower the resistance value, the more preferable it is, but the lower limit is 10 -5 It is about Ω / □.
[0022] The main component of the metal layer in the present invention is preferably any metal selected from the group consisting of copper, silver, and aluminum. The main component here refers to a metal that is more than 35 atomic % when the entire layer is taken as 100 atomic %. This is because the lower the electrical resistance is, the more desirable it is in terms of the shielding properties and signal attenuation properties of the metal layer. Gold can also be used in terms of performance, but it is expensive in terms of cost and is not suitable for use as an electromagnetic wave shielding film. Considering cost and electrical resistance, the main component of the metal layer is preferably copper. From the viewpoint of keeping the surface resistance value at 0.04 Ω / □ or less, the film thickness of the metal film is preferably 0.5 μm or more. Note that as long as the surface resistance is within the specified range, it does not matter if it contains oxides, nitrides, etc. in part. In addition, for the purpose of rust prevention, a metal layer of nickel or titanium of 1 nm or more may be formed on the surface layer by a deposition method such as sputtering. In the present invention, it is preferable that the metal layer includes a layer whose main component is any metal selected from the group consisting of copper, silver, and aluminum, and when the metal film is composed of multiple metal layers, it is not necessarily required that the main component of each of all of the metal layers is any metal selected from the group consisting of copper, silver, and aluminum.
[0023] The water vapor permeability of metallized film 1 according to JIS K7129:2008 is 3.5g / (m2) at a temperature of 40°C and a humidity of 90% RH. 2 ·day) or more, and 5.0 g / (m 2 ·day) or more. The water vapor permeability is preferably 3.5g / (m 2 ·day), if rapid heating is performed during the solder reflow process, the metal film will block out the volatile components, including water vapor, and the volatile components will vaporize rapidly, increasing the possibility of destroying the interlayer adhesion. The water vapor permeability of metallized film 1 is 3.5g / (m 2 ·day), the possibility of interlayer adhesion being destroyed during solder reflow is low, and 2 ·day), the possibility of destruction is even lower. The upper limit of water vapor permeability is 1,000g / (m 2 ·day).
[0024] Water vapor permeability of 3.5g / (m 2 A preferred example of a method for producing a metallized film 1 having a deposition time of 100 s (days) or more is the vacuum deposition method. It is known that the crystal structure of a metal layer formed by a sputtering method and a metal layer formed by a vacuum deposition method depends on the deposition temperature. In general, when Td<0.7Tm, where Tm is the melting point of the metal and Td is the deposition temperature, the deposited metal layer has columnar crystals. Since the melting point of copper is 1083°C, if the deposition temperature is sufficiently lower than 758°C, which is 0.7Tm, the copper layer has a columnar crystal structure. Since the deposition temperature of the copper layer is considered to be almost the same as the temperature on the film, it can be confirmed that the temperature on the film can be kept sufficiently low and heat damage can be reduced by the copper layer having columnar crystals. Regarding the crystal structure, the cross-sectional area of the metal layer can be observed using the EBSD (Electron Backscattered Diffraction) method. If the film does not shrink or deform significantly due to heat when the metal layer is deposited, it is sufficiently cooled and the crystal structure is columnar. In typical vacuum deposition, as shown in Figure 1, the deposited metal is incident on the substrate film 101 in a vertical direction 201, forming a metal film 301 on the film 101. At this time, it is known that the crystal growth of the metal layer occurs in a columnar shape in a vertical direction 401 to the film 101, and the metal film 301 becomes a columnar crystal. As the deposition progresses and the film thickness increases, the columnar crystals grow wider in the lateral direction, and adjacent columnar crystals grow in close contact with each other, eliminating gaps through which gases such as water vapor can pass, resulting in high gas barrier properties.
[0025] In contrast, there is a technique called oblique deposition, as shown in Figure 2, in which deposition is performed from an oblique direction on the film substrate. When the deposition metal is incident on the film 101 in the deposition direction oblique direction 201, the metal grows into columnar crystals in a direction 401 different from the deposition direction, and the columnar crystals do not grow horizontally, so gaps are generated between the columnar crystals. If gaps exist between the columnar crystals of the metal layer, a low-density film with good gas permeability can be produced. In addition, according to this technique, the columnar crystals do not spread horizontally even if the metal film thickness is increased, so gaps exist in the metal film, and gas permeability is maintained even if the metal film thickness is increased. However, in general oblique deposition, deposition is performed at an angle of 60 to 80 degrees, which reduces the material utilization efficiency and significantly reduces the film formation speed of vacuum deposition. In addition, since the crystal orientation is aligned and gaps exist, it is also characterized by being mechanically fragile.
[0026] In the present invention, as a method for maintaining the gas permeability of the metal film formed by this oblique deposition without decreasing the deposition rate, the inventors have focused on the fact that by forming unevenness on the surface of the film as a substrate, partial oblique deposition occurs on the film surface in all directions, and gaps can be secured between the crystals. As shown in Figure 3, the evaporated metal is incident in a vertical direction 201 on the film 102, which is a substrate having an uneven surface, to form a metal film 301 on the film 102. At this time, the unevenness of the film 201 makes the deposition direction oblique to the film surface, resulting in oblique deposition, and the metal begins to grow columnarly in a direction different from the deposition incidence direction. However, since the deposition incidence direction is random at the film position, the columnar growth direction is random, and the columnar growth is hindered by contact with the growth direction of adjacent crystals, and intermittent short columnar growth is repeated. Since the lateral growth, which is a characteristic of oblique deposition, is small, gaps are generated between the columnar crystals, and a metal film with excellent gas permeability can be produced. In addition, since the crystal growth direction is not uniform compared to the general oblique deposition as shown in Figure 2, the film strength is not fragile.
[0027] The arithmetic mean roughness Ra of the surface of the film on the side having the metal film is preferably 0.4 μm or more, and the ten-point mean roughness Rz is preferably 2.5 μm or more. Ra and Rz are parameters according to JIS B0601:1994. When the surface roughness Ra is 0.4 μm or more and Rz is 2.5 μm or more, the same effect as oblique deposition is exhibited, and a metal film with good gas permeability can be produced. The detailed conditions for measuring the mean roughness are described later in the examples, but the area of 500 μm x 500 μm is measured using a stylus with a tip R of 2 μm using a high-precision micro-shape measuring instrument Surfcorder ET4000A manufactured by Kosaka Laboratory Co., Ltd.
[0028] The root mean square slope RΔq of the roughness curve on the surface of the film having the metal film is preferably 0.18 or more. The arithmetic mean slope angle RΔa of the roughness curve on the surface having the metal film is preferably 7.0° or more, more preferably 8.0° or more. The root mean square slope RΔq is a parameter based on JIS B0601:2001, and represents the root mean square of the local slope dZ / dX in the reference length. The local slope here is the differentiation of the roughness curve Z(x) indicating the cross-sectional roughness, and the differentiation is basically performed using the seven-point formula. On the other hand, the arithmetic mean slope angle RΔa is the absolute value of the slope of the line segment formed by the surface irregularities with respect to the reference length X of the roughness curve, and is averaged. In order to obtain the same effect as oblique deposition by the surface irregularities of the film, it is preferable that the slope of the irregularities is large, since the crystal growth direction is easily oblique. If the root mean square slope RΔq is smaller than 0.18 or the arithmetic mean slope angle RΔa is smaller than 7.0°, the change in the crystal growth direction due to unevenness is small, so the crystals tend to grow in the same direction, and the crystals grow large and become dense, which may reduce gas permeability. Details of the measurement conditions will be described later in the examples, but measurements were taken with a Keyence Corporation shape measurement laser microscope VK-9710 (laser light source wavelength 408 nm) using a 50x objective lens, and the average value of the line roughness measured in two perpendicular directions over a length of 200 μm was used.
[0029] Regarding the inclination of the film surface, it is preferable that the root-mean-square inclination angle obtained by measurement with the above-mentioned laser microscope is also large. The root-mean-square inclination angle of the roughness curve on the surface having the metal film is preferably 10.0° or more, and more preferably 12.0° or more. The root-mean-square inclination angle is the square root of the mean square of the inclination of the line segment formed by the surface irregularities with respect to the reference length X of the roughness curve.
[0030] Figure 4 shows the image quality (IQ) map of a cross section of a PET film with a surface roughness of 0.066μm, Rz of 0.958μm, average slope RΔq of 0.02, and RΔa of 0.69°, in which a 2.0μm thick metal film (two 1μm thick metal layers) was formed by copper deposition. The image quality map is a grayscale image that shows the Image Quality (IQ) value, which is an index of the clarity of an EBSD (Electron Backscattered Diffraction) pattern. Dark areas indicate that the pattern is unclear due to the presence of grain boundaries or surface distortion, or surface contamination. This image quality map allows the size of the crystals to be determined. In Figure 4, the surface is flat with no irregularities, so it can be determined that the crystals of the copper film have grown large and columnar. Figure 5 is an Image Quality (IQ) Map of a cross section when a 2.0 μm metal film (two 1 μm-thick metal layers) was formed by copper deposition on a PET film with a film surface roughness of 0.447 μm, Rz of 5.376 μm, average slope RΔq of 0.29, and RΔa of 8.07°. Figure 5 shows that there are many areas where columnar growth has been inhibited due to the large unevenness of the PET film surface. In the areas where columnar crystals are inhibited, there are gaps between the crystals, which is presumably why the gas permeability is good.
[0031] The size of the crystal grain size is important because localized oblique deposition caused by surface roughening suppresses the lateral and vertical growth of columnar crystals, generating gaps between the crystals and producing a metal film with good gas permeability. The average crystal grain size of metal film 301 is preferably 50 nm or more and 200 nm or less, and more preferably 50 nm or more and 180 nm or less. If the average crystal grain size is less than 50 nm, the gaps between the crystals will become too large, and the surface resistance of the metal film may increase above the appropriate range. On the other hand, if the average crystal grain size exceeds 200 nm, the gaps between the crystals will become small, reducing gas permeability and causing the water vapor transmission rate of metallized film 1 to be 3.5 g / (m 2 ·day) or more. The average crystal grain size can be determined by examining the cross section of the metal film of the laminate using the transmission EBSD (Electron Backscattered Diffraction) method.
[0032] Since metal film 301 of metallized film 1 of the present invention preferably has low electrical resistance, the thicker the film, the greater the film thickness is. However, when forming a metal film by vacuum deposition, increasing the film thickness increases the amount of heat applied to the film substrate during deposition, which may cause thermal deformation of the substrate. Therefore, the film thickness is preferably 3.0 μm or less.
[0033] Pinholes and other openings in the metal film 301 are undesirable because they reduce the mechanical strength of the film and increase the electrical resistance (surface resistance) of the film. 2 Less than or even 1 piece / cm 2 However, when a metal film with a surface resistance of 0.04 Ω / □ or less is produced by vacuum deposition, the metal film is usually thick enough, at 0.5 μm or more in copper film equivalent, so that many openings such as pinholes do not occur. Unless the film surface is extremely dirty or openings are intentionally formed in the metal film, it is preferable that the number of openings is 10 / cm. 2 It rarely goes beyond that.
[0034] The number of apertures referred to here is the number of pinholes with a diameter of 5 μm or more, measured visually in a dark room using a consumer photo backlight as the light source. The measurement was performed over a 10 cm 2 The area must be 1cm or more. 2 This shall be converted into the number of sides.
[0035] The arithmetic mean roughness Ra of the metal film surface is preferably 0.5 μm or more, and the ten-point mean roughness Rz is preferably 3.5 μm or more. The definitions and measurement methods of the parameters are the same as those of the above-mentioned film. When Ra is 0.5 μm or more and Rz is 3.5 μm or more, the surface unevenness exerts the same effect as oblique deposition, resulting in a metal film with good gas permeability. When Ra is less than 0.5 μm or Rz is less than 3.5 μm, the effect of the film unevenness is insufficient in the process of forming the metal film, and the crystals may grow large, resulting in low gas permeability.
[0036] The root mean square slope RΔq of the roughness curve on the surface of the metal film is preferably 0.10 or more, and the arithmetic mean slope angle RΔa is preferably 3.0° or more, more preferably 7.0° or more. The definition and measurement method of the parameters are the same as those of the above-mentioned film. When RΔq is 0.10 or more or RΔa is 3.0° or more, it is considered that the crystal size of the metal film is small due to the unevenness slope of the film, and the water vapor permeability is high. On the other hand, when RΔq is less than 0.10 or RΔa is less than 3.0°, the effect of the unevenness slope of the film is small, and crystal growth does not occur as in oblique deposition, and the crystal size becomes large, which may decrease the gas permeability.
[0037] As with the above-mentioned film, the metal film surface preferably has a large root mean square inclination angle. The root mean square inclination angle of the roughness curve on the surface of the metal film is preferably 6.0° or more, and more preferably 10.0° or more.
[0038] <Film> The film 101 used in the present invention is a thin film made of a polymer such as a synthetic resin. For example, a polyester film such as a polyethylene terephthalate film or a polyethylene naphthalate film, a polyimide film, a polyphenylene sulfide film, a polypropylene film, or a polyether ether ketone film can be used as the film 101. Of these, a polyethylene terephthalate film is more preferably used. These films may be used alone or in combination. Furthermore, a film surface coated with a resin, an adhesive, or the like may be used.
[0039] Considering gas permeability, the thinner the film 101, the more preferable it is, and therefore the thickness is preferably 10 μm or less, and more preferably 6 μm or less. However, if the film 101 is too thin, the strength of the film itself is weakened, and wrinkles or the like occur during the process of deposition or lamination to a printed circuit board, making handling difficult. For this reason, as shown in FIG. 7, the film 101 may be formed on a carrier film 501 having a release layer, and a metal film 301 may be formed thereon to produce a metallized film 1. There are no particular limitations on the carrier film 501, but a polyethylene terephthalate film is more preferably used. The thickness of the carrier film is also preferably 25 μm or more and 100 μm or less, as this makes it easy to handle.
[0040] Also, as the film 101, a film formed by coating a resin on a carrier film having a release layer can be used. As the resin, a thermoplastic resin composition, a thermosetting resin composition, an active energy ray curable composition, or the like can be used. The thermoplastic resin composition is not particularly limited, but examples thereof include a styrene-based resin composition, a vinyl acetate-based resin composition, a polyester-based resin composition, a polyethylene-based resin composition, a polypropylene-based resin composition, an imide-based resin composition, or an acrylic-based resin composition. The thermosetting resin composition is not particularly limited, but examples thereof include a phenol-based resin composition, an epoxy-based resin composition, a urethane-based resin composition having an isocyanate group at the end, a urea-based resin having an isocyanate group at the end, a urethane urea-based resin having an isocyanate group at the end, a melamine-based resin composition, or an alkyd-based resin composition. In addition, as the active energy ray curable composition, it is not particularly limited, but for example, a polymerizable compound having at least two (meth)acryloyloxy groups in the molecule can be used. These resins may be used alone, or two or more of them may be used in combination.
[0041] Among these, from the viewpoint of improving reflow resistance and preventing deterioration of the electrical connection between the electromagnetic wave shielding film 2 and the printed wiring board 3, a urethane urea resin having an isocyanate group at the end or a resin using a urethane urea resin having an isocyanate group at the end in combination with an epoxy resin is preferable. The urethane resin having an isocyanate group at the end or the urethane urea resin having an isocyanate group at the end preferably has an acid value of 1 to 30 mgKOH / g, more preferably an acid value of 3 to 20 mgKOH / g. In addition, two or more urethane resins or urethane urea resins having different acid values within the range of 1 to 30 mgKOH / g may be used in combination. When the acid value is 1 mgKOH / g or more, the reflow resistance of the electromagnetic wave shielding film is good, and when it is 30 mgKOH / g or less, the bending resistance of the electromagnetic wave shielding film is good. The acid value is measured in accordance with JIS K0070:1992. Moreover, film 101 formed by coating a carrier film with a resin may be made of a single material or may be made of two or more materials.
[0042] The film 101 formed by coating a resin on a carrier film may contain at least one of a curing accelerator, a tackifier, an antioxidant, a pigment, a dye, a plasticizer, an ultraviolet absorber, an antifoaming agent, a leveling agent, a filler, a flame retardant, a viscosity adjuster, and an antiblocking agent, as necessary.
[0043] Film 101 formed by coating a carrier film with a resin may be a laminate of two or more layers having different materials or physical properties such as hardness or elastic modulus. For example, if a laminate is formed of an outer layer having a low hardness and an inner layer having a high hardness, the outer layer has a cushioning effect, so that the pressure applied to metal film 301 in the process of heating and pressing electromagnetic wave shielding film 2 to printed wiring board 3 can be reduced. This makes it possible to prevent metal film 301 from being destroyed by steps provided on the printed wiring board.
[0044] The thickness of the film 101 formed by coating a carrier film with a resin is not particularly limited and can be appropriately set as necessary, but is preferably 1 μm or more and 20 μm or less, more preferably 1 μm or more and 10 μm or less, and even more preferably 4 μm or more and 6 μm or less. If the thickness of the film 101 formed by coating a carrier film with a resin is 1 μm or more, the adhesive layer 601 and the metal film 301 can be sufficiently protected. Furthermore, if the thickness of the film 101 formed by coating a carrier film with a resin is 20 μm or less, the flexibility of the electromagnetic wave shielding film 2 can be ensured, and it becomes easy to apply one sheet of the electromagnetic wave shielding film 2 to a member that requires flexibility.
[0045] For this reason, it is preferable that the surface of the film that contacts the metal film contains at least one resin selected from the group consisting of polyester, polyimide, polyphenylene sulfide, polypropylene, polyether ether ketone, and epoxy resin. Considering solder reflow passability, film 101 needs to have excellent heat resistance, so it is more preferable to use polyimide, polyphenylene sulfide, polyether ether ketone, and epoxy resin among these.
[0046] There is no particular limitation on the method for creating unevenness on the film surface. Examples of the method that can be used include forming unevenness on the film by blasting, thinly applying a resin containing large particles such as filler and forming unevenness with the particles, and kneading particles into the film when it is molded.
[0047] Blasting is a method of spraying fine particles such as an abrasive onto a film to create fine irregularities. Known abrasives can be used, such as ceramic beads and glass beads made of silica sand, alumina, zirconia, silica, etc., and dry ice particles. The method of spraying the abrasive is not particularly limited, and may include shot blasting (centrifugal blasting) in which the abrasive is sprayed by centrifugal force, air blasting using compressed air, and wet blasting in which a slurry is made and sprayed at high pressure.
[0048] When forming unevenness by applying a resin containing particles, the type of resin is not particularly limited, but in order to ensure adhesion between the film and the resin layer, it is preferable to use a resin mainly composed of an organic component. Examples of the type of resin include polyester resin, polyurethane resin, acrylic resin, methacrylic resin, polyamide resin, polyethylene resin, polypropylene resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, and polyvinyl acetate resin. These resins may be used alone, or may be used as a copolymer or mixture of two or more kinds. Among them, polyester resin, polyurethane resin, acrylic resin, or methacrylic resin is preferable in terms of adhesion and particle dispersibility.
[0049] The shape of the particles used to form the irregularities can be, for example, a non-spherical shape such as a star shape, flat shape, rhomboid shape, rectangular shape, needle shape, confetti shape, or irregular shape, or a spherical shape (meaning that the cross-sectional shape of the particle is surrounded by a curved surface), etc. Furthermore, the particles may be porous, non-porous, or hollow, and particles having different particle shapes may be mixed.
[0050] The material of the particles may be any of organic compounds and inorganic compounds, and is not particularly limited, and particles of different materials may be mixed and used. As the material of the particles, in the case of organic compounds, resins mainly composed of crosslinked polymer components having a high melting point are preferable, and examples thereof include polyester resins, polyamide resin particles such as benzoguanamine, polyurethane resins, acrylic resins, methacrylic resins, polyamide resins, polyethylene resins, polypropylene resins, polyvinyl chloride resins, polyvinylidene chloride resins, polystyrene resins, polyvinyl acetate resins, fluorine-based resins, silicone resins, etc. These resins may be used alone, or may be used as copolymers or mixtures of two or more kinds. In the case of inorganic compounds, examples thereof include calcium carbonate, magnesium carbonate, zinc carbonate, titanium oxide, zinc oxide, cerium oxide, magnesium oxide, barium sulfate, zinc sulfide, calcium phosphate, silica, alumina, mica, titanium mica, talc, clay, kaolin, lithium fluoride, calcium fluoride, etc.
[0051] The thickness of the resin layer applied to form the unevenness is not particularly limited, but is preferably 0.05 μm to 5 μm. If the thickness is less than 0.05 μm, the resin layer may become uneven or particles may fall off, and if the thickness is more than 5 μm, the resin layer may crack or the properties of the film itself, such as heat resistance, may be impaired.
[0052] <Anchor layer> An anchor layer may be provided between film 101 and metal film 301 of metallized film 1 of the present invention. By providing an anchor layer, it is expected that the adhesion between the film and the metal film will be improved. As the anchor layer, it is preferable to form a metal anchor layer on film 101 by a sputtering method. The sputtering method makes it possible to reduce the thickness of the anchor layer, and is optimal for electromagnetic wave shielding film applications that require even thinner layers.
[0053] The anchor layer is preferably a metal layer containing at least one selected from the group consisting of nickel, titanium, copper, and chromium. When the metal film 301 is copper, it is preferable to use the same metal, copper, for the anchor layer as well, as this has less effect on the metal film 301. However, if the film 101 is made of a material that diffuses copper, such as polyimide, adhesion cannot be ensured. In such a case, the anchor layer can be made to function as a buffer layer by selecting from nickel, titanium, chromium, and the like, which are less likely to react with both the film 101 and the metal film 301.
[0054] The thickness of the anchor layer is preferably 5 nm or more and 30 nm or less, and more preferably 10 nm or more and 20 nm or less. If the thickness is less than 5 nm, sufficient adhesion may not be obtained. On the other hand, if the thickness exceeds 30 nm, the average crystal grain size of the anchor layer formed by the sputtering method becomes large, and depending on the type of metal, the metal film 301 formed thereon by vacuum deposition may be affected by the size of the crystal grain size of the anchor layer, and the average crystal grain size of the metal film 301 may also become large, making it difficult to control. When the anchor layer is made to function as a buffer layer that prevents the film 101 and the metal film 301 from directly contacting each other, the thickness is preferably 10 nm or more, and in order to reduce the influence of crystal control of the metal film 301, the anchor layer is preferably 20 nm or less.
[0055] <Adhesive layer> The electromagnetic wave shielding film of the present invention has an adhesive layer on one surface of the metal film of the metallized film of the present invention, and the adhesive layer will be described below. The adhesive layer 601 is not particularly limited as long as it can fix the electromagnetic wave shielding film 2 to the printed wiring board 3, but it is preferably a conductive adhesive layer having an adhesive resin composition and a conductive filler.
[0056] The adhesive resin composition is not particularly limited, but may be a thermoplastic resin composition such as a styrene-based resin composition, a vinyl acetate-based resin composition, a polyester-based resin composition, a polyethylene-based resin composition, a polypropylene-based resin composition, an imide-based resin composition, an amide-based resin composition, or an acrylic-based resin composition, or a thermosetting resin composition such as a phenol-based resin composition, an epoxy-based resin composition, a urethane-based resin composition, a melamine-based resin composition, or an alkyd-based resin composition. These may be used alone or in combination of two or more.
[0057] The adhesive layer 601 may contain, as necessary, a curing accelerator, a tackifier, an antioxidant, a pigment, a dye, a plasticizer, an ultraviolet absorber, an antifoaming agent, a leveling agent, a filler, a flame retardant, a viscosity adjuster, and the like.
[0058] The thickness of the adhesive layer 601 is not particularly limited and can be appropriately set as necessary, but is preferably 3 μm or more and 10 μm or less, and more preferably 4 μm or more and 7 μm or less.
[0059] The conductive filler is not particularly limited, and examples thereof include metal fillers, metal-coated resin fillers, carbon fillers, and mixtures thereof. The metal fillers include copper powder, silver powder, nickel powder, silver-coated copper powder, gold-coated copper powder, silver-coated nickel powder, and gold-coated nickel powder, and these metal powders can be produced by electrolysis, atomization, or reduction.
[0060] In particular, in order to facilitate contact between the fillers, it is preferable that the average particle size of the conductive filler is 3 μm or more and 50 μm or less. The shape of the conductive filler may be spherical, flaky, dendritic, fibrous, etc. Among these, from the viewpoints of connection resistance and cost, it is preferable that the conductive filler be at least one selected from the group consisting of silver powder, silver-coated copper powder, and copper powder.
[0061] By containing a conductive filler in the adhesive layer 601, an anisotropic conductive adhesive layer or an isotropic conductive It may be an adhesive layer.
[0062] In the case of an isotropic conductive adhesive layer, the amount of conductive filler to be mixed is the total amount of the adhesive layer 601. In the case of an anisotropic conductive adhesive layer, the additive may be added in the range of 3 to 39 weight % based on the total weight of the adhesive layer 601. (Metallized film manufacturing method) Next, a description will be given of an example of a method for producing metallized film 1 of the present invention. The method for producing metallized film 1 of the present invention is not particularly limited, but an example can be a production method having a step of preparing film 101, a step of forming an anchor layer on film 101 as necessary, and a step of forming metal film 301.
[0063] <Film preparation process> When using film 101 formed by molding a polymer such as synthetic resin into a thin film, the surface on the side on which metal film 301 is to be formed is roughened. There are no particular limitations on the roughening method, but examples include a method of making the film surface uneven by sandblasting or the like, and a method of covering the surface with a coating material containing particles such as filler to make the surface uneven.
[0064] Blasting is a method of spraying fine particles such as an abrasive onto a film to create fine irregularities. Known abrasives can be used, such as ceramic beads and glass beads made of silica sand, alumina, zirconia, silica, etc., and dry ice particles. The method of spraying the abrasive is not particularly limited, and may include shot blasting (centrifugal blasting) in which the abrasive is sprayed by centrifugal force, air blasting using compressed air, and wet blasting in which a slurry is made and sprayed at high pressure.
[0065] When forming the unevenness by coating a resin containing particles, the coating method is not particularly limited, and various coating methods such as gravure coating, roll coating, die coating, spin coating, reverse coating, bar coating, screen coating, blade coating, air knife coating and dip coating can be used.
[0066] When using a film 101 formed by coating a carrier film with a resin, a resin composition is prepared. This resin composition can be prepared by adding an appropriate amount of a solvent and other compounding agents to the resin composition. The solvent can be, for example, toluene, acetone, methyl ethyl ketone, methanol, ethanol, propanol, dimethylformamide, etc. As other compounding agents, a crosslinking agent, a polymerization catalyst, a curing accelerator, a colorant, etc. can be added. In addition, particles such as silica can be added for the purpose of forming surface irregularities. Other compounding agents may be added as necessary.
[0067] Next, the prepared resin composition is applied to one side of the carrier film 501. The method for applying the resin composition to one side of the carrier film 501 is not particularly limited, and known techniques such as lip coating, comma coating, gravure coating, and slot die coating can be applied.
[0068] The carrier film 501 is not particularly limited, and can be made of, for example, a polyolefin-based material, a polyester-based material, a polyimide-based material, a polyphenylene sulfide-based material, etc. A release agent layer may be provided between the carrier film 501 and the film 101 formed by coating with a resin.
[0069] Then, after the carrier film 501 is coated with resin, the resin is dried by heating to remove the solvent, thereby forming the resin-coated film 101. The carrier film 501 can be peeled off from the resin-coated film 101, but it is preferable to peel off the carrier film 501 after the electromagnetic wave shielding film 2 is attached to the printed wiring board 3. In this way, the electromagnetic wave shielding film 2 can be protected by the supporting substrate.
[0070] The surface of film 101 formed by coating with a resin is also roughened. The method of roughening is not particularly limited, but examples include a method of making the film surface uneven by sandblasting or the like (same as above) and a method of covering the surface with a coating material containing particles such as filler to make the surface uneven (same as above).
[0071] <Anchor layer forming process> Next, when forming an anchor layer on the surface of the film 101, specifically, the film is placed in a batch-type vacuum deposition apparatus (EBH-800 manufactured by ULVAC), and a metal target of 50 mm×550 mm is used, and the film is evaporated in an argon gas atmosphere to a vacuum level of 5×10 -1 The anchor layer can be formed by adjusting the pressure to below 1 Pa and continuously applying a DC power supply for a time period that results in a predetermined metal film thickness. Note that the vacuum deposition for forming the metal film 301 that is performed after sputtering can be performed continuously, and the process can be performed without coming into contact with the air between sputtering and deposition.
[0072] <Metal film forming process> Next, a metal film 301 is formed on the surface of the film 101 or the surface of the anchor layer. More specifically, the film is placed in a batch-type vacuum deposition apparatus (EBH-800 manufactured by ULVAC), and an amount of metal to achieve a desired thickness is placed on a deposition boat. Then, the deposition boat is heated to a vacuum level of 9.0×10 -3After drawing a vacuum until the pressure reaches or below Pa, the evaporation boat can be heated to perform vacuum deposition. When forming an anchor layer, the anchor layer formation and metal film formation can be performed consecutively, so that the substrate is not exposed to the air between sputtering and deposition.
[0073] Generally, the metal film 301 is formed on one side of the film 101, but if necessary, the metal film may be formed on both sides of the film 101. However, when the metal film 301 is formed on both sides, both sides of the film 101 need to be roughened in advance.
[0074] (Manufacturing method of electromagnetic wave shielding film) Next, an example of a method for producing the electromagnetic shielding film 2 of the present invention will be described. The electromagnetic shielding film of the present invention has an adhesive layer on the surface of one of the metal films of the metallized film of the present invention, and the method for producing such an electromagnetic shielding film 2 of the present invention is not particularly limited. For example, there can be mentioned a production method in which an adhesive layer composition is applied to the surface of one of the metal films 301 of the metallized film 1 of the present invention, and then the adhesive layer 601 is formed by curing the adhesive layer composition.
[0075] <Adhesive layer formation process> When the adhesive layer 601 is formed by applying a composition for adhesive layer to the surface of the metal film 301 of the metallized film 1 of the present invention, the composition for adhesive layer contains a resin composition and a solvent. The resin composition is not particularly limited, but may be a thermoplastic resin composition such as a styrene-based resin composition, a vinyl acetate-based resin composition, a polyester-based resin composition, a polyethylene-based resin composition, a polypropylene-based resin composition, an imide-based resin composition, an amide-based resin composition, or an acrylic-based resin composition, or a thermosetting resin composition such as a phenol-based resin composition, an epoxy-based resin composition, a urethane-based resin composition, a melamine-based resin composition, or an alkyd-based resin composition. These may be used alone or in combination of two or more kinds.
[0076] Examples of the solvent that can be used include toluene, acetone, methyl ethyl ketone, methanol, ethanol, propanol, and dimethylformamide. If necessary, the adhesive layer composition may contain at least one of a curing accelerator, a tackifier, an antioxidant, a pigment, a dye, a plasticizer, an ultraviolet absorber, an antifoaming agent, a leveling agent, a filler, a flame retardant, and a viscosity regulator. The ratio of the resin composition in the adhesive layer composition may be appropriately set depending on the thickness of the adhesive layer 601, the coating method, the liquid viscosity, and the like.
[0077] The method for applying the adhesive layer composition to the surface of metal film 301 of metallized film 1 is not particularly limited, and lip coating, comma coating, gravure coating, slot die coating, or the like can be used.
[0078] Then, the adhesive layer composition is applied onto the surface of metal film 301 of metallized film 1 of the present invention, and then heated and dried to remove the solvent, thereby forming adhesive layer 601. If necessary, a release film may be attached to the surface of adhesive layer 601.
[0079] (Shielded printed circuit board) The electromagnetic wave shielding film 2 of this embodiment is, for example, a shielding printed wiring shown in FIG. The shielded printed wiring board 4 includes a printed wiring board 3 and an electromagnetic wave shielding film 2.
[0080] The printed wiring board 3 has a base layer 702, a printed circuit (ground circuit) 801 formed on the base layer 702, an insulating adhesive layer 901 provided adjacent to the printed circuit 801 on the base layer 702, and an insulating coverlay 701 provided to cover the insulating adhesive layer 901 and having an opening for exposing a part of the printed circuit 801. The insulating adhesive layer 901 and the coverlay 701 form an insulating layer of the printed wiring board 3.
[0081] The base layer 702, the insulating adhesive layer 901, and the coverlay 701 are not particularly limited and may be, for example, a resin film, and may be formed of a resin such as polypropylene, cross-linked polyethylene, polyester, polybenzimidazole, polyimide, polyimideamide, polyetherimide, polyphenylene sulfide, etc. The printed circuit 801 may be, for example, a copper wiring pattern formed on the base layer 702.
[0082] The electromagnetic wave shielding film 2 is printed with the adhesive layer 601 facing the coverlay 701. It is glued to wire plate 3.
[0083] Next, a method for manufacturing the shielded printed wiring board 4 will be described. The electromagnetic wave shielding film 2 is placed on the printed wiring board 3, and is heated and pressed by a press. A part of the adhesive layer 601 softened by heating flows into an opening formed in the coverlay 701 by pressure. As a result, the metal film 301 and the ground circuit 801 of the printed wiring board 3 are connected via the conductive adhesive, and the metal film 301 and the ground circuit 801 are connected. EXAMPLES
[0084] The present invention will be described below based on examples. Note that the present invention is not limited to these examples, and these examples can be modified or changed based on the spirit of the present invention, and they are not excluded from the scope of the present invention.
[0085] (Magnetron sputtering) The film was placed in a batch-type vacuum deposition apparatus (ULVAC EBH-800), and a nickel target of 50 mm × 550 mm was used, and the deposition was performed in an argon gas atmosphere at a vacuum level of 5 × 10 -1 The pressure was adjusted to less than 1 Pa, and a DC power supply was applied continuously for a period of time until a predetermined metal film thickness was achieved.
[0086] The vacuum deposition performed after the sputtering was carried out continuously, so that the film was not exposed to the air between the sputtering and the deposition.
[0087] (Vacuum deposition) The film was placed in a batch-type vacuum deposition device (ULVAC EBH-800), and the amount of copper to be the target thickness was placed on the deposition boat. After that, the vacuum level was adjusted to 9.0×10 -3 After evacuation to a pressure of 0.1 Pa or less, the evaporation boat was heated to carry out vacuum deposition.
[0088] (Surface roughness measurement) Surface roughness was measured using a micro-shape measuring instrument, Surfcorder ET4000A, manufactured by Kosaka Laboratory Co., Ltd. The sample was fixed to the attached semi-cylindrical glass plate, and a stylus with a tip R of 2μm was used. Data was also analyzed using a three-dimensional surface roughness analysis system, i-Face model TDA31. Data was collected by measuring three random locations, and the averages were used as the Ra and Rz values.
[0089] Measurement conditions: X measurement length 500 μm, pitch 1 μm Y measurement length 500μm, pitch 5μm Measurement speed 0.1mm / sec.
[0090] (surface slope measurement) The surface inclination was measured using a laser microscope VK-9700 manufactured by Keyence Corporation, and analyzed using the shape analysis application VK-H1A1. Measurements were performed at three random locations, and the average values of RΔq and RΔa were used.
[0091] Measurement conditions: 50x objective lens, 1x zoom Analysis conditions: Automatic noise removal: Noise detection area Normal Tilt correction: Face tilt correction (automatic) Line roughness analysis Analysis length 200μm Height smoothing: simple average ±2.
[0092] For the line roughness profile, cross-sectional data of 200 μm length was collected at the center of each of the horizontal and vertical directions in the captured image, and the average values of the two values were taken as RΔq and RΔa for that image.
[0093] (Measurement of surface resistance) Surface resistance was measured using the four-terminal method. The sample to be measured was cut into a 100 mm square, and the center of the cut film was measured three times, and the average of the three measurements was taken as the measured surface resistance. A simple low resistivity meter (Loresta EP MCP-T360 ASP probe, manufactured by Mitsubishi Chemical Analytech Co., Ltd.) was used for the measurement, and the unit is displayed as Ω / □.
[0094] (Method for measuring average grain size) The average crystal grain size of the metal film was calculated using EBSD. First, a thin cut was made from the cross section of the metal film of the laminate, and its diffraction pattern was captured. In the obtained diffraction pattern, crystal grains were identified as being the same grain when there were two or more consecutive measurement points with a specified azimuth angle difference of within 5°, and the circle equivalent diameter (diameter of a circle with the same area) of each crystal grain was calculated. The crystal grain sizes thus obtained were averaged according to the following formula to obtain the average crystal grain size. In the formula, N is the total number of grains, d i indicates the particle diameter (equivalent circle diameter) of each particle.
[0095]
number
[0096] The conditions for capturing the diffraction pattern are as follows. Equipment used: Thermal field emission scanning electron microscope (TFE-SEM) JSM-6500F (manufactured by JEOL Ltd.) OIM Orientation Analysis Device DigiViewIV Slow Scan CCD Camera OIM Data Collection ver.7.x OIM Analysis ver.7.x Analysis conditions: Accelerating voltage 15 kV Irradiation current 15nA Specimen tilt: -30deg (transmission EBSD method) Surface measurement magnification: 5,000x Measurement field of view 3×20μm Interval 20nm / step.
[0097] (Counting the number of openings) The number of apertures was measured by visually counting the number of pinholes with a diameter of 5 μm or more in a dark room using a consumer photo backlight as the light source. 2 Do the above area, 1cm 2 Converted into number of neighborhoods.
[0098] (Copper layer thickness measurement) The thickness of the metal layer was measured using a fluorescent X-ray thickness gauge (SSI NanoTechnology, SFT9400).
[0099] (Anchor layer thickness) The transmittance of the sputtered metal layer formed on the transparent PET film was measured with a transmittance meter, and the obtained value was used to calculate the Lambert-Beer law.
[0100]
number
[0101] The film thickness was calculated from I 0 is the amount of light before passing through the thin film, I is the amount of light after passing through the thin film, α is the absorption coefficient, Z is the film thickness, k is the extinction coefficient, and λ is the wavelength. I / I 0 The extinction coefficient at a wavelength of 555 nm was adopted as 2.56 for titanium and 3.2588 for nickel, and these values were used as the film thickness of the sputtered metal layer, which was the anchor layer.
[0102] (Water vapor permeability) The water vapor transmission rate was measured according to a method conforming to JIS K7129:2008 (infrared). It was measured at a temperature of 40°C and a humidity of 90% RH using a water vapor transmission rate measuring device (model name: PERMATRAN (registered trademark) W3 / 31) manufactured by MOCON, USA. The measurement was performed twice for two test pieces, and the average value of the four measured values was taken as the water vapor transmission rate. (Reflow passability) When a heat-resistant film was used, the reflow resistance of the prepared shielded printed wiring board was evaluated as follows: Assuming lead-free solder, the reflow conditions were set with a temperature profile in which the shielding film on the shielded printed wiring board was exposed to 265°C for 1 second.
[0103] The shielded printed wiring board was exposed to the temperature conditions of the above profile three times, and then visually inspected to see if any blistering had occurred due to destruction of interlayer adhesion. Those that did not have any blistering were marked with an ◯, and those that had blistering were marked with an ×.
[0104] (Evaluation of electric field shielding and magnetic field shielding) The near electric field and near magnetic field shielding performance of the metallized film alone was measured using the KEC method. The measuring equipment used was a microwave / millimeter wave band evaluation system (Agilent E5071C ENA, network analyzer (9kHz~4.5GHz)), and the electric field shielding performance (near electric field shielding performance) and magnetic field shielding performance (near magnetic field shielding performance) at 1GHz were measured.
[0105] Example 1 <Production of Metallized Film> One side of a 50μm-thick biaxially oriented polyethylene terephthalate film (Toray Industries, Inc., "Lumirror (registered trademark)" type: S10) was treated with a shot blasting method in which silica sand with an average particle size of 200μm was shot at the film from a distance of 1m, and then the film was washed with water to obtain a surface-roughened film. After surface roughening, the film's surface roughness was Ra 0.87μm, Rz 7.96μm, and the slope of the unevenness was RΔq 0.56, RΔa 15.5°.
[0106] Next, nickel was deposited to a thickness of 5 nm on the surface with the surface irregularities formed by magnetron sputtering. The conditions were a sputtering output of 3.0 kW using a DC power supply. After that, copper was vacuum deposited to a thickness of 2.0 μm by vacuum deposition. The average crystal grain size of the copper metal film of the metallized film thus produced was 74 nm, the surface resistance was 0.0198 Ω / □, and the number of pinholes (number of openings) was 0.4 / cm. 2 The surface roughness of the metal film was Ra 1.05 μm, Rz 8.15 μm, and the slope of the unevenness was RΔq 0.70 and RΔa 16.3°. The water vapor permeability of the metallized film was 6.68 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 80 dB, and the magnetic field shielding effect at 1 GHz was 60 dB.
[0107] Example 2 <Production of Metallized Film> A 50 μm-thick biaxially oriented polyethylene terephthalate film (Toray Industries, Inc., "Lumirror (registered trademark)" type: S10) was coated with a resin containing particles to prepare a surface-roughened film. The particle-containing resin was prepared by dispersing 15% by weight of silica spherical particles "Seahorster" KE-P30 (average particle diameter 0.3 μm) manufactured by Nippon Shokubai Co., Ltd. in an acrylic resin "Acrydic (registered trademark)" WFL-908 manufactured by DIC Corporation. The acrylic resin was coated with a Mayer bar and dried at 120°C for 1 minute to form a layer with a thickness of 0.5 μm, to obtain a surface-roughened film. The surface roughness of the obtained surface-roughened film was Ra 0.51 μm, Rz 3.36 μm, and the slope of the unevenness was RΔq 0.21 and RΔa 7.3°.
[0108] Next, nickel was deposited on the film surface to a thickness of 5 nm by magnetron sputtering. The conditions were a sputtering output of 3.0 kW using a DC power supply. After that, copper was vacuum-deposited to a thickness of 1.0 μm by vacuum deposition. The average crystal grain size of the copper metal film of the metallized film thus produced was 102 nm, the surface resistance of the metal film was 0.0280 Ω / □, and the number of pinholes (number of openings) was 0.5 / cm.2 The surface roughness of the metal film was Ra 0.57 μm, Rz 4.92 μm, and the slope of the unevenness was RΔq 0.13 and RΔa 4.6°. The water vapor permeability of the metallized film was 3.54 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 65 dB, and the magnetic field shielding effect at 1 GHz was 51 dB.
[0109] Example 3 <Production of Metallized Film> A metallized film was obtained under the same conditions as in Example 2, except that copper was vacuum-deposited to a thickness of 0.7 μm by a vacuum deposition method. The average crystal grain size of the copper metal film of the metallized film thus produced was 106 nm, the surface resistance was 0.0384 Ω / □, and the number of pinholes (number of openings) was 0.6 / cm. 2 The surface roughness of the metal film was Ra 0.54 μm, Rz 4.28 μm, and the slope of the unevenness was RΔq 0.18 and RΔa 6.1°. The water vapor permeability of the metallized film was 3.76 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 60 dB, and the magnetic field shielding effect at 1 GHz was 49 dB.
[0110] Example 4 <Production of Metallized Film> A PET film with a thickness of 60 μm and a surface treated with a release agent was used as a supporting substrate, and a composition (solid content 30 mass%) consisting of a bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, jER1256) and methyl ethyl ketone was applied thereon, followed by heating and drying to produce an epoxy resin film with a thickness of 5 μm. The surface of the epoxy resin film was roughened by shot blasting and washing with water in the same manner as in Example 1. The film surface roughness after surface roughening was Ra 0.46 μm, Rz 2.57 μm, and the slope of the unevenness was RΔq 0.49 and RΔa 13.4°.
[0111] Next, the above-mentioned film was placed in a batch-type vacuum deposition apparatus (ULVAC EBH-800) and evaporated in an argon gas atmosphere at a vacuum level of 5×10 -1The pressure was adjusted to 0.1 Pa or less, and nickel was formed as an anchor layer to a thickness of 5 nm by magnetron sputtering (DC power output: 3.0 kW).
[0112] Next, copper was placed on the deposition boat, and the vacuum level was 9.0×10 -3 The vacuum was drawn until the pressure was below 1 Pa, and then the evaporation boat was heated to form a 2.0 μm copper metal film by vacuum deposition. The formation of the anchor layer and the metal film were performed consecutively, and the copper metal film was not exposed to the air between sputtering and deposition. The average crystal grain size of the copper metal film of the metallized film produced in this way was 115 nm, the surface resistance was 0.0144 Ω / □, and the number of pinholes (openings) was 0.4 / cm. 2 The surface roughness of the metal film was Ra 0.64 μm, Rz 3.61 μm, and the slope of the unevenness was RΔq 0.53 and RΔa 14.7°. The water vapor permeability of the metallized film was 10.96 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 80 dB, and the magnetic field shielding effect at 1 GHz was 61 dB.
[0113] Since this is an epoxy resin film with reflow resistance, the following evaluations were added: <Production of electromagnetic wave shielding film> The surface of the metal film of the metallized film is coated with epoxy resin and spherical silver particles with an average particle size of 3 μm. An adhesive made of coated copper powder (50% by weight) was applied to form an adhesive layer having a thickness of 5 μm.
[0114] <Preparation of shielded printed circuit board> The electromagnetic wave shielding film and printed wiring board thus prepared were overlapped so that the adhesive layer of the electromagnetic wave shielding film faced the printed wiring board, and the films were heated and pressed for 1 minute at 170°C and 3.0 MPa using a press, and then heated and pressed for 3 minutes at the same temperature and pressure to produce a shielded printed wiring board.
[0115] The printed wiring board had two copper foil patterns extending parallel to each other with a gap between them, and an insulating layer (thickness: 25 μm) made of polyimide that covered the copper foil patterns. The insulating layer had openings (diameter: 1 mm) that exposed each copper foil pattern. The adhesive layer of the electromagnetic shielding film and the printed wiring board were overlapped so that the openings were completely covered by the electromagnetic shielding film. After obtaining the shielded printed wiring board, the PET film that had been subjected to a release treatment was peeled off. The reflow passability of this shielded printed wiring board was rated as good.
[0116] Example 5 <Production of Metallized Film> A PET film with a thickness of 60 μm and a surface treated with a release agent was used as a supporting substrate, and a PEEK film with a thickness of 5 μm was laminated on the supporting substrate. The surface of the resulting PEEK film with supporting substrate was roughened by shot blasting and washing with water in the same manner as in Example 1. The film surface roughness after surface roughening was Ra 0.43 μm, Rz 2.51 μm, and the slope of the unevenness was RΔq 0.47 and RΔa 12.6°.
[0117] Next, an anchor layer was formed on the roughened surface of the PEEK film. The film was placed in a batch-type vacuum deposition apparatus (ULVAC EBH-800) and heated to a vacuum of 5×10 in an argon gas atmosphere. -1 The pressure was adjusted to 0.1 Pa or less, and a titanium anchor layer having a thickness of 5 nm was formed by magnetron sputtering (DC power output: 3.0 kW).
[0118] Next, copper was placed on the deposition boat, and the vacuum level was 9.0×10 -3 The vacuum was drawn until the pressure was below 1 Pa, and then the evaporation boat was heated to form a 1.0 μm metal film by vacuum deposition. The formation of the anchor layer and the metal film were performed consecutively, and the metal film was not exposed to the air between sputtering and deposition. The average crystal grain size of the copper metal film of the metallized film produced in this way was 128 nm, the surface resistance was 0.0279 Ω / □, and the number of pinholes (openings) was 0.5 / cm. 2The surface roughness of the metal film was Ra 0.57 μm, Rz 3.59 μm, and the slope of the unevenness was RΔq 0.50 and RΔa 13.5°. The water vapor permeability of the metallized film was 9.77 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 65 dB, and the magnetic field shielding effect at 1 GHz was 50 dB.
[0119] Since this is a PEEK film with reflow resistance, the following evaluations were added as in Example 4.
[0120] <Production of electromagnetic wave shielding film> <Production of shielded printed wiring board> The electromagnetic wave shielding film was produced and the shielded printed wiring board was fabricated in the same manner as in Example 4. The reflow passability of this shielded printed wiring board was rated good.
[0121] Example 6 <Production of Metallized Film> One side of a 50 μm-thick biaxially oriented polyethylene terephthalate film (Toray Industries, Inc., "Lumirror (registered trademark)" type: S10) was roughened by shot blasting and washing with water in the same manner as in Example 1. After surface roughening, the film had a surface roughness of Ra 0.87 μm and Rz 7.96 μm, and the slope of the unevenness was RΔq 0.56 and RΔa 15.5°.
[0122] Next, a metal film was formed on the surface of the film. The film was placed in a batch-type vacuum deposition apparatus (ULVAC EBH-800), aluminum was placed on the deposition boat, and the vacuum level was 9.0×10 -3 The vacuum was drawn until the pressure reached 0.02 Pa or less, and then the evaporation boat was heated to form a 2.0 μm metal film by vacuum deposition. The average crystal grain size of the aluminum metal film of the metallized film thus produced was 91 nm, the surface resistance was 0.0379 Ω / □, and the number of pinholes (number of openings) was 0.5 / cm. 2The surface roughness of the metal film was Ra 1.1 μm, Rz 8.3 μm, and the slope of the unevenness was RΔq 0.72 and RΔa 16.5°. The water vapor permeability of the metallized film was 7.23 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 60 dB, and the magnetic field shielding effect at 1 GHz was 50 dB.
[0123] Example 7 One side of a 37.5 μm-thick polyimide film (manufactured by DuPont-Toray Co., Ltd., "Kapton (registered trademark)" type: 150EN-A) was roughened by shot blasting and washing with water in the same manner as in Example 1. The film surface roughness after surface roughening was Ra 0.71 μm, Rz 7.39 μm, and the slope of the unevenness was RΔq 0.48 and RΔa 13.7°.
[0124] Next, an anchor layer was formed on the roughened surface of the polyimide film. The film was placed in a batch-type vacuum deposition apparatus (ULVAC EBH-800) and evaporated in an argon gas atmosphere to a vacuum of 5×10 -1 The pressure was adjusted to 0.1 Pa or less, and nickel was formed as an anchor layer to a thickness of 5 nm by magnetron sputtering (DC power output: 3.0 kW).
[0125] Next, copper was placed on the deposition boat, and the vacuum level was 9.0×10 -3 The vacuum was drawn until the pressure was below 1 Pa, and then the evaporation boat was heated to form a 2.0 μm metal film by vacuum deposition. The formation of the anchor layer and the metal film were performed consecutively, and the metal film was not exposed to the air between sputtering and deposition. The average crystal grain size of the copper metal film of the metallized film produced in this way was 101 nm, the surface resistance was 0.0159 Ω / □, and the number of pinholes (openings) was 0.4 / cm. 2 The surface roughness of the metal film was Ra 0.77 μm, Rz 7.69 μm, and the slope of the unevenness was RΔq 0.54 and RΔa 14.8°. The water vapor permeability of the metallized film was 8.92 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 80 dB, and the magnetic field shielding effect at 1 GHz was 60 dB.
[0126] Since this is a polyimide film having reflow resistance, the following evaluations were added as in Example 4.
[0127] <Production of electromagnetic wave shielding film> <Production of shielded printed wiring board> The electromagnetic wave shielding film was produced and the shielded printed wiring board was fabricated in the same manner as in Example 4. The reflow passability of this shielded printed wiring board was rated good.
[0128] Example 8 One side of a 37.5 μm-thick polyimide film (manufactured by DuPont-Toray Co., Ltd., "Kapton (registered trademark)" type: 150EN-A) was roughened by shot blasting and washing with water in the same manner as in Example 1. The film surface roughness after surface roughening was Ra 0.71 μm, Rz 7.39 μm, and the slope of the unevenness was RΔq 0.48 and RΔa 13.7°.
[0129] Next, an anchor layer was formed on the roughened surface of the polyimide film. The film was placed in a batch-type vacuum deposition apparatus (ULVAC EBH-800) and evaporated in an argon gas atmosphere to a vacuum of 5×10 -1 The pressure was adjusted to 0.1 Pa or less, and nickel was formed as an anchor layer to a thickness of 5 nm by magnetron sputtering (DC power output: 3.0 kW).
[0130] Next, copper was placed on the deposition boat, and the vacuum level was 9.0×10 -3 The vacuum was drawn until the pressure was below 1 Pa, and then the evaporation boat was heated to form a 1.0 μm metal film by vacuum deposition. The formation of the anchor layer and the metal film were performed consecutively, and the metal film was not exposed to the air between sputtering and deposition. The average crystal grain size of the copper metal film of the metallized film produced in this way was 96 nm, the surface resistance was 0.0301 Ω / □, and the number of pinholes (openings) was 0.5 / cm. 2The surface roughness of the metal film was Ra 0.73 μm, Rz 7.52 μm, and the slope of the unevenness was RΔq 0.51 and RΔa 14.2°. The water vapor permeability of the metallized film was 10.33 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 65 dB, and the magnetic field shielding effect at 1 GHz was 51 dB.
[0131] Since this is a polyimide film having reflow resistance, the following evaluations were added as in Example 4.
[0132] <Production of electromagnetic wave shielding film> <Production of shielded printed wiring board> The electromagnetic wave shielding film was produced and the shielded printed wiring board was fabricated in the same manner as in Example 4. The reflow passability of this shielded printed wiring board was rated good.
[0133] Example 9 One side of a 37.5 μm-thick polyimide film (manufactured by DuPont-Toray Co., Ltd., "Kapton (registered trademark)" type: 150EN-A) was roughened by shot blasting and washing with water in the same manner as in Example 1. The film surface roughness after surface roughening was Ra 0.71 μm, Rz 7.39 μm, and the slope of the unevenness was RΔq 0.48 and RΔa 13.7°.
[0134] Next, a metal film was formed on the surface of the film. The film was placed in a batch-type vacuum deposition apparatus (ULVAC EBH-800), aluminum was placed on the deposition boat, and the vacuum level was 9.0×10 -3 The vacuum was drawn until the pressure reached 0.02 Pa or less, and then the evaporation boat was heated to form a 2.0 μm metal film by vacuum deposition. The average crystal grain size of the aluminum metal film of the metallized film thus produced was 94 nm, the surface resistance was 0.0363 Ω / □, and the number of pinholes (number of openings) was 0.5 / cm. 2 The surface roughness of the metal film was Ra 0.91 μm, Rz 8.16 μm, and the slope of the unevenness was RΔq 0.67 and RΔa 14.9°. The water vapor permeability of the metallized film was 9.61 g / (m 2·day), the electric field shielding effect at 1 GHz was 60 dB, and the magnetic field shielding effect at 1 GHz was 50 dB.
[0135] Since this is a polyimide film having reflow resistance, the following evaluations were added as in Example 4.
[0136] <Production of electromagnetic wave shielding film> <Production of shielded printed wiring board> The electromagnetic wave shielding film was produced and the shielded printed wiring board was fabricated in the same manner as in Example 4. The reflow passability of this shielded printed wiring board was rated good.
[0137] Comparative Example 1 <Production of Metallized Film> A metallized film was obtained under the same conditions as in Example 1, except that the film surface was not roughened by shot blasting. The surface roughness of the film before metal lamination was Ra 0.03 μm, Rz 0.83 μm, and the slope of the unevenness was RΔq 0.02 and RΔa 0.69°. A metal film was formed on the film surface to obtain a metallized film, and the copper metal film had an average crystal grain size of 263 nm, a surface resistance of 0.0102 Ω / □, and pinholes (number of openings) of 0.1 / cm. 2 The surface roughness of the metal film was Ra 0.06 μm, Rz 0.52 μm, and the slope of the unevenness was RΔq 0.01 and RΔa 0.41°. The water vapor permeability of the metallized film was 0.06 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 86 dB, and the magnetic field shielding effect at 1 GHz was 64 dB.
[0138] Comparative Example 2 <Production of Metallized Film> A metallized film was obtained under the same conditions as in Comparative Example 1, except that a 1.5 μm metal film was formed by copper vapor deposition. The surface roughness of the film before metal lamination was Ra 0.03 μm, Rz 0.83 μm, and the slope of the unevenness was RΔq 0.02 and RΔa 0.69°. The average crystal grain size of the copper metal film of the metallized film obtained by forming a metal film on the film surface was 231 nm, the surface resistance was 0.0133 Ω / □, and the number of pinholes (number of openings) was 0.1 / cm. 2 The surface roughness of the metal film was Ra 0.04 μm, Rz 0.62 μm, and the slope of the unevenness was RΔq 0.02 and RΔa 0.52°. The water vapor permeability of the metallized film was 2.06 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 81 dB, and the magnetic field shielding effect at 1 GHz was 60 dB.
[0139] Comparative Example 3 <Production of Metallized Film> A metallized film was obtained under the same conditions as in Comparative Example 1, except that a 0.5 μm metal film was formed by copper vapor deposition. The surface roughness before metal lamination was Ra 0.03 μm, Rz 0.83 μm, and the slope of the unevenness was RΔq 0.02 and RΔa 0.69°. The average crystal grain size of the copper metal film in the metallized film obtained by forming a metal film on the film surface was 227 nm, the surface resistance was 0.0389 Ω / □, and the number of pinholes (number of openings) was 0.5 / cm. 2 The surface roughness of the metal film was Ra 0.04 μm, Rz 0.76 μm, and the slope of the unevenness was RΔq 0.02 and RΔa 0.59°. The water vapor permeability of the metallized film was 2.93 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 60 dB, and the magnetic field shielding effect at 1 GHz was 50 dB.
[0140] Comparative Example 4 <Production of Metallized Film> A metallized film was obtained under the same conditions as in Example 4, except that the film surface was not roughened by shot blasting. The surface roughness of the epoxy resin film surface before metal lamination was Ra 0.282 μm, Rz 2.02 μm, and the slope of the unevenness was RΔq 0.02 and RΔa 0.63°. The metallized film obtained by forming a metal film on the surface of this epoxy resin film had an average crystal grain size of 214 nm, a surface resistance of 0.0122 Ω / □, and pinholes (number of openings) of 0.1 / cm. 2 The surface roughness of the metal film was Ra 0.31 μm, Rz 1.78 μm, and the slope of the unevenness was RΔq 0.01 and RΔa 0.39°. The water vapor permeability of the metallized film was 1.22 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 86 dB, and the magnetic field shielding effect at 1 GHz was 63 dB.
[0141] Since this is an epoxy resin film with reflow resistance, the following evaluations were added as in Example 4.
[0142] <Production of electromagnetic wave shielding film> <Production of shielded printed wiring board> The electromagnetic wave shielding film was produced and the shielded printed wiring board was prepared in the same manner as in Example 4. The reflow passability of this shielded printed wiring board was rated x.
[0143] Comparative Example 5 <Production of Metallized Film> A metallized film was obtained under the same conditions as in Example 6, except that the film surface was not roughened by shot blasting. The surface roughness of the film before metal lamination was Ra 0.03 μm, Rz 0.83 μm, and the slope of the unevenness was RΔq 0.02 and RΔa 0.69°. The metallized film obtained by forming a metal film on the film surface had an average crystal grain size of 272 nm, a surface resistance of 0.0371 Ω / □, and pinholes (number of openings) of 0.1 / cm. 2The surface roughness of the metal film was Ra 0.05 μm, Rz 0.61 μm, and the slope of the unevenness was RΔq 0.01 and RΔa 0.56°. The water vapor permeability of the metallized film was 0.03 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 60 dB, and the magnetic field shielding effect at 1 GHz was 50 dB.
[0144] Comparative Example 6 <Production of Metallized Film> A metallized film was obtained under the same conditions as in Example 7, except that the film surface was not roughened by shot blasting. The surface roughness of the polyimide film surface before metal lamination was Ra 0.028 μm, Rz 0.303 μm, and the slope of the unevenness was RΔq 0.02 and RΔa 0.63°. The metallized film obtained by forming a metal film on the surface of this polyimide film had an average crystal grain size of 268 nm, a surface resistance of 0.0101 Ω / □, and pinholes (number of openings) of 0.1 / cm. 2 The surface roughness of the metal film was Ra 0.03 μm, Rz 0.29 μm, and the slope of the unevenness was RΔq 0.02 and RΔa 0.54°. The water vapor permeability of the metallized film was 0.31 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 86 dB, and the magnetic field shielding effect at 1 GHz was 64 dB.
[0145] Since this is a polyimide film having reflow resistance, the following evaluation was added as in Example 4.
[0146] <Production of electromagnetic wave shielding film> <Production of shielded printed wiring board> The electromagnetic wave shielding film was produced and the shielded printed wiring board was prepared in the same manner as in Example 4. The reflow passability of this shielded printed wiring board was rated x. Comparative Example 7 <Production of Metallized Film> A metallized film was obtained under the same conditions as in Example 9, except that the film surface was not roughened by shot blasting. The surface roughness of the polyimide film surface before metal lamination was Ra 0.028 μm, Rz 0.303 μm, and the slope of the unevenness was RΔq 0.02 and RΔa 0.63°. The metallized film obtained by forming a metal film on the surface of this polyimide film had an average crystal grain size of 264 nm, a surface resistance of 0.0369 Ω / □, and pinholes (number of openings) of 0.1 / cm. 2 The surface roughness of the metal film was Ra 0.04 μm, Rz 0.40 μm, and the slope of the unevenness was RΔq 0.01 and RΔa 0.68°. The water vapor permeability of the metallized film was 0.35 g / (m 2 ·day), the electric field shielding effect at 1 GHz was 60 dB, and the magnetic field shielding effect at 1 GHz was 50 dB.
[0147] Since this is a polyimide film having reflow resistance, the following evaluation was added as in Example 4.
[0148] <Production of electromagnetic wave shielding film> <Production of shielded printed wiring board> The electromagnetic wave shielding film was produced and the shielded printed wiring board was prepared in the same manner as in Example 4. The reflow passability of this shielded printed wiring board was rated x.
[0149] [Table 1-1]
[0150] [Table 1-2] [Explanation of symbols]
[0151] 1 Metallized Film 2. Electromagnetic wave shielding film 3 Flexible printed wiring boards (printed wiring boards) 4 Shielded printed wiring board 101, 102 Film 201 Deposition direction 301 Metal Film 401 Deposited film growth direction 501 Carrier Film 601 Adhesive layer 701 Cover Film 702 Base Layer 801 Printed Circuit (Ground Circuit) 901 Insulating adhesive layer
Claims
1. A metallized film having a metal film composed of at least one metal layer on at least one side of the film, The surface resistance of the metal film is 0.04 Ω / □ or less, The water vapor permeability of the metallized film according to JIS K7129:2008 is 3.5 g / (m) at a temperature of 40° C. and a humidity of 90% RH. 2 - day) or more.
2. 2. The metallized film of claim 1, wherein the surface resistivity of the metal film is 0.02 Ω / □ or less.
3. 3. The metallized film of claim 1, wherein the root mean square slope RΔq of the film surface on the side having the metal film is 0.18 or greater.
4. 3. The metallized film according to claim 1, wherein the arithmetic mean tilt angle RΔa of the film surface on the side having the metal film is 7.0° or more.
5. The metallized film according to claim 1 , wherein the film surface having the metal film has an arithmetic mean roughness Ra of 0.4 μm or more.
6. 3. The metallized film according to claim 1, wherein the ten-point average roughness Rz of the film surface having the metal film is 2.5 μm or more.
7. 3. The metallized film of claim 1, wherein the metal film has an average crystal grain size of 50 nm or more and 200 nm or less.
8. 3. The metallized film of claim 1, wherein the main component of the metal layer is at least one metal selected from the group consisting of copper, silver, and aluminum.
9. 3. The metallized film of claim 1, wherein the metal film has a thickness of 0.5 μm or more and 3.0 μm or less.
10. 3. The metallized film of claim 1, wherein the metal film surface has an arithmetic root mean square slope RΔq of 0.10 or greater.
11. 3. The metallized film of claim 1, wherein the metal film surface has an arithmetic mean tilt angle RΔa of 3.0° or more.
12. 3. The metallized film of claim 1, wherein the metal film surface has an arithmetic mean roughness Ra of 0.5 μm or more.
13. 3. The metallized film of claim 1, wherein the metal film surface has a ten-point average roughness Rz of 3.5 μm or more.
14. 3. The metallized film according to claim 1, further comprising at least one resin selected from the group consisting of polyester, polyimide, polyphenylene sulfide, polypropylene, polyether ether ketone, and epoxy resin on the surface of the film that contacts the metal film.
15. The metallized film of claim 1 or 2, further comprising an anchor layer between the film and the metal membrane.
16. 16. The metallized film of claim 15, wherein the anchor layer is a metal layer containing at least one selected from the group consisting of nickel, titanium, copper, and chromium.
17. 16. The metallized film of claim 15, wherein the anchor layer has a thickness of 5 nm or greater and 30 nm or less.
18. A method for producing the metallized film according to claim 1 or 2, comprising the steps of: The method for producing a metallized film includes forming the metal film by a vacuum deposition method.
19. 16. A method for producing a metallized film according to claim 15, comprising the steps of: The anchor layer is formed by sputtering. The method for producing a metallized film includes forming the metal film by a vacuum deposition method.
20. The method for producing a metallized film according to claim 18, wherein the metal film is formed by oblique deposition.
21. The method for producing a metallized film according to claim 20 , further comprising forming projections and recesses on a surface of the film.
22. 3. An electromagnetic wave shielding film comprising the metallized film according to claim 1 or 2, and an adhesive layer on one surface of the metal film.
Citation Information
Patent Citations
Electromagnetic wave shielding film, printed wire board using same, and rolled copper foil
WO2014192494A1
Bolt delivery device
JP1987019383A
Electromagnetic wave shielding film and method for manufacturing same
WO2017111158A1