Adhesive film, foldable device and rollable device

The adhesive film addresses the flexibility and transparency issues of conventional films by using a specialized layer structure with specific viscoelastic properties and a top coat, ensuring reliable adhesion and durability in foldable and rollable devices.

JP2024159866APending Publication Date: 2024-11-08NITTO DENKO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024139398
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-06-13
Filing Date
2024-08-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Conventional adhesive films used for reinforcing semiconductor elements and flexible or rollable devices suffer from poor bending characteristics, leading to issues such as wrinkling, lifting, and crease formation due to inadequate flexibility and transparency, especially when repeatedly bent.

Method used

An adhesive film with a base material layer and adhesive layer, characterized by a tan δ (0.7%) of 0.1 or less and a difference in tan δ between 0.7% and 0.1% strain of 0.05 or less, featuring a top coat layer with a binder containing polyester or urethane resins, and optionally an antistatic component, ensuring excellent flexibility and transparency.

Benefits of technology

The adhesive film provides enhanced flexibility and transparency, allowing it to be effectively used in foldable and rollable devices without significant wrinkling or lifting, maintaining adhesion even after repeated bending.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159866000001_ABST
    Figure 2024159866000001_ABST
Patent Text Reader

Abstract

To provide an adhesive film having excellent bendability and transparency and to provide a foldable device and a rollable device having excellent bendability.SOLUTION: There is provided an adhesive film having a substrate layer and an adhesive layer, wherein tanδ(0.7%) at a strain of 0.7% measured in the tension mode of a viscoelasticity measurement device is 0.1 or less. There is provided an adhesive film having a substrate layer and an adhesive layer, wherein the difference (tanδ(0.7%)-tanδ(0.1%)) between tanδ(0.7%) at a strain of 0.7% and tanδ(0.1%) at a strain of 0.1% measured in the tension mode of a viscoelasticity measurement device is 0.05 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive film. The present invention also relates to a foldable device including such an adhesive film, and a rollable device including such an adhesive film. [Background technology]

[0002] Adhesive films are used for reinforcing members of various shapes and for protecting the surfaces.

[0003] For example, when joining an integrated circuit (IC) or a flexible printed circuit (FPC) to a substrate of a semiconductor element (e.g., a TFT substrate, etc.), thermocompression bonding is usually performed using an anisotropic conductive film (ACF). When performing such thermocompression bonding, an adhesive film may be attached to the back side of the substrate of the semiconductor element in advance to reinforce the substrate (e.g., Patent Document 1).

[0004] In addition, in a manufacturing method for flexible devices and rollable devices, which have been developed in recent years, a release layer and a flexible or rollable film substrate are generally formed on a support substrate such as glass, a TFT substrate is formed on the film substrate, and an organic EL layer is further formed on the TFT substrate. The support substrate is then peeled off to manufacture the flexible device or rollable device, but since the flexible display layer or rollable display layer is very thin, problems occur in the device due to handling, etc. For this reason, an adhesive film may be attached to the back side for reinforcement (for example, Patent Document 2).

[0005] Substrates of semiconductor elements, flexible devices, and rollable devices may be repeatedly bent, and if the bending properties of the adhesive film attached to the back side of the substrate are poor, the recovery after bending may be poor, or in the worst case, the film may break due to repeated bending. Specifically, when an adhesive film is attached to a bending portion (e.g., a movable bending portion of a folding member), the following problems may occur.

[0006] When an adhesive film is bent at an angle, a compressive force acts on the bent inner diameter side, and the adhesive film itself deforms in an attempt to relieve this force. Specifically, for example, the film becomes more prone to wrinkles.

[0007] When an adhesive film is bent at an angle, a tensile stress acts on the outer diameter side of the bent part, and when the stress is relieved, the film floats off the adherend.

[0008] When an adhesive film is bent at an angle, the thickness of the bent or pulled part of the adhesive film changes significantly, and even in this state, the adhesive film is prone to wrinkles and lifting. For example, when an adhesive film is pulled, the thickness of the adhesive film becomes significantly thinner, making it more likely to lift off from the adherend.

[0009] Thus, conventional adhesive films are unable to adequately conform to uneven corners and bent portions.

[0010] In particular, when an adhesive film is attached to a movable bending portion, repeated bending causes the adhesive film to develop fold marks (so-called "creases") on the movable bending portion.

[0011] In addition, when an integrated circuit (IC) or flexible printed circuit board (FPC) is bonded to a semiconductor element substrate (such as a TFT substrate) by thermocompression bonding, the bonding position is confirmed from the back side of the substrate before compression bonding. For this reason, the adhesive film that is bonded to the back side of the substrate must be transparent. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] Patent No. 5600039 [Patent Document 2] Patent No. 6376271 Summary of the Invention [Problem to be solved by the invention]

[0013] An object of the present invention is to provide a pressure-sensitive adhesive film having excellent flexibility and transparency. Another object of the present invention is to provide a foldable device and a rollable device having excellent flexibility. [Means for solving the problem]

[0014] The adhesive film of the present invention is An adhesive film having a base layer and an adhesive layer, The tan δ(0.7%) at a strain of 0.7% measured using a tensile mode with a viscoelasticity measuring device is 0.1 or less.

[0015] The adhesive film of the present invention is A pressure-sensitive adhesive film having a base layer and a pressure-sensitive adhesive layer, The difference between tan δ(0.7%) at a strain of 0.7% and tan δ(0.1%) at a strain of 0.1%, measured in the tensile mode of a viscoelasticity measuring device, (tan δ(0.7%)-tan δ(0.1%)) is 0.05 or less.

[0016] In one embodiment, the adhesive film of the present invention is bent at 6Φ and held at 90°C for 48 hours, then released and left at 23°C and 50% RH for 24 hours, after which the bend angle is 60 degrees to 180 degrees.

[0017] In one embodiment, the pressure-sensitive adhesive film of the present invention has a top coat layer on the surface of the base layer opposite to the surface having the pressure-sensitive adhesive layer.

[0018] In one embodiment, the top coat layer contains a binder including at least one selected from a polyester resin and a urethane resin.

[0019] In one embodiment, the binder includes a urethane-based resin.

[0020] In one embodiment, the topcoat layer contains an antistatic component.

[0021] In one embodiment, the Young's modulus of the base layer at 23° C. is 6.0×10 7 Pa or more.

[0022] In one embodiment, the material of the base layer is at least one selected from polyimide and polyether ether ketone.

[0023] In one embodiment, the pressure-sensitive adhesive film of the present invention has a topcoat layer on the side of the base layer opposite to the side having the pressure-sensitive adhesive layer, the topcoat layer contains a binder containing a urethane resin and an antistatic component, and the material of the base layer is at least one selected from polyimide and polyether ether ketone.

[0024] In one embodiment, the pressure-sensitive adhesive film of the present invention has a total light transmittance of 20% or more.

[0025] In one embodiment, the pressure-sensitive adhesive film of the present invention has a haze of 15% or less.

[0026] In one embodiment, the adhesive strength of the pressure-sensitive adhesive layer to a SUS plate at 23° C., at a tensile speed of 300 mm / min and at 180° peel is 1 N / 25 mm or more.

[0027] In one embodiment, the pressure-sensitive adhesive layer contains an acrylic pressure-sensitive adhesive.

[0028] In one embodiment, the adhesive film of the present invention is attached to a foldable member.

[0029] In one embodiment, the foldable member is an OLED.

[0030] In one embodiment, the adhesive film of the present invention is attached to a rollable member.

[0031] In one embodiment, the rollable member is an OLED.

[0032] The foldable device of the present invention includes the above-mentioned adhesive film.

[0033] The rollable device of the present invention comprises the above-mentioned adhesive film. Effect of the Invention

[0034] According to the present invention, it is possible to provide a pressure-sensitive adhesive film having excellent flexibility and transparency. According to the present invention, it is also possible to provide a foldable device and a rollable device having excellent flexibility. [Brief description of the drawings]

[0035] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of a foldable device of the present invention, and shows one mode of use of the adhesive film of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view illustrating a method for evaluating flex recovery. [Diagram 3] FIG. 3 is a schematic cross-sectional view illustrating the evaluation method for peeling evaluation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] <<Adhesive film>> The pressure-sensitive adhesive film of the present invention has a base layer and a pressure-sensitive adhesive layer. That is, the pressure-sensitive adhesive film of the present invention may have any appropriate other layer as long as it has the base layer and the pressure-sensitive adhesive layer, as long as the effects of the present invention are not impaired.

[0037] The substrate layer may be one layer or two or more layers, and is preferably one layer in that the effects of the present invention can be more effectively exhibited.

[0038] The pressure-sensitive adhesive layer may be one layer or two or more layers, and is preferably one layer in that the effect of the present invention can be more effectively exhibited.

[0039] The pressure-sensitive adhesive film of the present invention may be provided with any appropriate release liner on the surface of the pressure-sensitive adhesive layer opposite the substrate layer for protection until use.

[0040] Examples of the release liner include a release liner in which the surface of a substrate (liner substrate) such as paper or plastic film is silicone-treated, a release liner in which the surface of a substrate (liner substrate) such as paper or plastic film is laminated with a polyolefin resin, etc. Examples of the plastic film as the liner substrate include a polyethylene film, a polypropylene film, a polybutene film, a polybutadiene film, a polymethylpentene film, a polyvinyl chloride film, a vinyl chloride copolymer film, a polyethylene terephthalate film, a polybutylene terephthalate film, a polyurethane film, an ethylene-vinyl acetate copolymer film, etc.

[0041] The thickness of the release liner is preferably from 1 μm to 500 μm, more preferably from 3 μm to 450 μm, even more preferably from 5 μm to 400 μm, and particularly preferably from 10 μm to 300 μm.

[0042] The pressure-sensitive adhesive film of the present invention has a total thickness d of preferably 1 μm to 500 μm, more preferably 5 μm to 200 μm, even more preferably 10 μm to 150 μm, particularly preferably 20 μm to 100 μm, and most preferably 30 μm to 80 μm. When the total thickness d of the pressure-sensitive adhesive film of the present invention is within the above range, the effects of the present invention can be more effectively exhibited.

[0043] The pressure-sensitive adhesive film of the present invention has a tan δ(0.7%) at a strain of 0.7% measured in a tensile mode with a viscoelasticity measuring device of 0.1 or less, preferably 0.09 or less, more preferably 0.08 or less, even more preferably 0.07 or less, and particularly preferably 0.06 or less. If the tan δ(0.7%) at a strain of 0.7% measured in a tensile mode with a viscoelasticity measuring device of the present invention is within the above range, the effects of the present invention can be more effectively exhibited.

[0044] Tan δ (0.7%) at a strain of 0.7% measured in the tension mode of a viscoelasticity measuring device of an adhesive film is an index showing the loss tangent when the adhesive film is greatly bent. In completing the present invention, it was found based on various experimental data that if this value is within the above range, the effect of the present invention can be more effectively expressed. The method for measuring tan δ (0.7%) at a strain of 0.7% measured in the tension mode of a viscoelasticity measuring device will be described in detail later.

[0045] The pressure-sensitive adhesive film of the present invention has a tan δ(0.1%) at a strain of 0.1% measured in a tensile mode with a viscoelasticity measuring device of preferably 0.1 or less, more preferably 0.08 or less, even more preferably 0.06 or less, and particularly preferably 0.05 or less. If the tan δ(0.1%) at a strain of 0.1% measured in a tensile mode with a viscoelasticity measuring device of the present invention is within the above range, the effects of the present invention can be more effectively exhibited.

[0046] Tan δ(0.1%) at a strain of 0.1% measured in the tension mode of a viscoelasticity measuring device for an adhesive film is an index showing the loss tangent when the adhesive film is bent slightly. In completing the present invention, it was found based on various experimental data that if this value is within the above range, the effect of the present invention can be more effectively expressed. The method for measuring tan δ(0.1%) at a strain of 0.1% measured in the tension mode of a viscoelasticity measuring device will be described in detail later.

[0047] The adhesive film of the present invention preferably has a difference (tan δ(0.7%)-tan δ(0.1%)) between tan δ(0.7%) at a strain of 0.7% and tan δ(0.1%) at a strain of 0.1% measured in the tensile mode of a viscoelasticity measuring device of 0.05 or less, more preferably 0.04 or less, and even more preferably 0.03 or less. If the difference (tan δ(0.7%)-tan δ(0.1%)) between tan δ(0.7%) at a strain of 0.7% and tan δ(0.1%) at a strain of 0.1% measured in the tensile mode of a viscoelasticity measuring device of the adhesive film of the present invention is within the above range, the effects of the present invention can be more effectively achieved.

[0048] The difference between tan δ(0.7%) at a strain of 0.7% and tan δ(0.1%) at a strain of 0.1% measured in the tensile mode of a viscoelasticity measuring device for an adhesive film (tan δ(0.7%)-tan δ(0.1%)) is an index showing the difference between the loss tangent when the adhesive film is bent significantly and the loss tangent when the adhesive film is bent slightly. In completing the present invention, it was found based on various experimental data that the effects of the present invention can be more effectively expressed if this value is within the above range.

[0049] The pressure-sensitive adhesive film of the present invention is bent at 6Φ and held at 90 ° C for 48 hours, then released and left at 23 ° C and 50% RH for 24 hours, and the bending angle is preferably 60 degrees to 180 degrees, more preferably 80 degrees to 180 degrees, even more preferably 100 degrees to 180 degrees, particularly preferably 120 degrees to 180 degrees, and most preferably 150 degrees to 180 degrees. If the bending angle of the pressure-sensitive adhesive film of the present invention, bent at 6Φ and held at 90 ° C for 48 hours, then released and left at 23 ° C and 50% RH for 24 hours, is within the above range, the effects of the present invention can be more effectively exhibited.

[0050] The bending angle of the adhesive film after bending it at 6Φ and holding it at 90° C. for 48 hours, releasing the bending, and leaving it at 23° C. and 50% RH for 24 hours is an index showing the recovery after bending. The method for measuring the bending angle after bending it at 6Φ and holding it at 90° C. for 48 hours, releasing the bending, and leaving it at 23° C. and 50% RH for 24 hours will be described in detail later.

[0051] The pressure-sensitive adhesive film of the present invention has a total light transmittance of preferably 20% or more, more preferably 30% or more, even more preferably 40% or more, particularly preferably 50% or more, and most preferably 60% or more. If the total light transmittance of the pressure-sensitive adhesive film of the present invention is within the above range, excellent transparency can be more easily exhibited.

[0052] The adhesive film of the present invention has a haze of preferably 15% or less, more preferably 13% or less, even more preferably 10% or less, particularly preferably 8% or less, and most preferably 6% or less. When the adhesive film of the present invention has a haze within the above range, excellent transparency can be more easily exhibited.

[0053] The adhesive film of the present invention is excellent in flexibility and transparency, so it is preferably attached to a foldable member. Any suitable member can be adopted as the foldable member as long as it can be repeatedly bent. Examples of such foldable members include foldable optical members, foldable electronic members, and the like, and a representative example is a foldable OLED.

[0054] The adhesive film of the present invention is excellent in flexibility and transparency, so it is preferably attached to a rollable member. Any suitable member can be adopted as the rollable member as long as it can be repeatedly wound and unwound. Such rollable members include, for example, rollable optical members, rollable electronic members, etc., and a representative example is rollable OLED.

[0055] ≪Base material layer≫ The thickness of the substrate layer is preferably 1 μm to 500 μm, more preferably 5 μm to 300 μm, further preferably 10 μm to 100 μm, particularly preferably 15 μm to 80 μm, and most preferably 20 μm to 60 μm. When the thickness of the substrate layer is within the above range, the effects of the present invention can be more effectively exhibited.

[0056] The base layer preferably has a Young's modulus at 23° C. of 6.0×10 7 Pa or more, more preferably 1.0×10 8 Pa or more, and more preferably 5.0×10 8 Pa or more, and particularly preferably 8.0×10 8 Pa or more, and most preferably 1.0×10 9 The upper limit of the Young's modulus of the base layer at 23° C. is typically preferably 1.0×10 11 Pa or less. If the Young's modulus of the base layer at 23°C is within the above range, the effect of the present invention can be more effectively achieved. If the Young's modulus of the base layer at 23°C is too low, when the adhesive film is bent at an angle, the tension on the outer diameter side may not be sufficiently maintained against the compression on the inner diameter side, and the thickness may easily change, and the adhesive film may easily float from the adherend. If the Young's modulus of the base layer at 23°C is too high, the adhesive film may not be easily deformed. The method for measuring the Young's modulus will be described in detail later.

[0057] As the material for the base layer, any appropriate material may be used as long as it does not impair the effects of the present invention. A representative example of the material for the base layer is a resin material.

[0058] Examples of resin materials for the base layer include acrylic resins such as polyimide (PI), polyether ether ketone (PEEK), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polymethyl methacrylate (PMMA), polycarbonate, triacetyl cellulose (TAC), polysulfone, polyarylate, polyethylene (PE), polypropylene (PP), ethylene-propylene copolymer, ethylene-vinyl acetate copolymer (EVA), polyamide (nylon), wholly aromatic polyamide (aramid), polyvinyl chloride (PVC), polyvinyl acetate, polyphenylene sulfide (PPS), fluorine-based resins, and cyclic olefin polymers.

[0059] As the resin material for the base layer, in terms of being able to more effectively exhibit the effects of the present invention, preferably, at least one selected from polyimide (PI), polyether ether ketone (PEEK), and cyclic olefin polymer is used, and more preferably, at least one selected from polyimide (PI) and polyether ether ketone (PEEK) is used.

[0060] <Adhesive layer> The thickness of the pressure-sensitive adhesive layer is preferably 1 μm to 500 μm, more preferably 5 μm to 300 μm, even more preferably 10 μm to 100 μm, particularly preferably 15 μm to 80 μm, and most preferably 20 μm to 60 μm. When the thickness of the pressure-sensitive adhesive layer is within the above range, the effects of the present invention can be more effectively exhibited.

[0061] The adhesive strength of the adhesive layer to a glass plate at 23 ° C., tensile speed 300 mm / min, 180 ° peel is preferably 1 N / 25 mm or more, more preferably 5 N / 25 mm or more, even more preferably 10 N / 25 mm or more, particularly preferably 12 N / 25 mm or more, and most preferably 15 N / 25 mm or more. The upper limit of the adhesive strength of the adhesive layer to a glass plate at 23 ° C., tensile speed 300 mm / min, 180 ° peel is typically preferably 1000 N / 25 mm or less, more preferably 5000 N / 25 mm or less, even more preferably 300 N / 25 mm or less, particularly preferably 200 N / 25 mm or less, and most preferably 100 N / 25 mm or less. If the adhesive strength of the adhesive layer to a glass plate at 23 ° C., tensile speed 300 mm / min, 180 ° peel is within the above range, the effect of the present invention can be more effectively exhibited.

[0062] The pressure-sensitive adhesive layer contains a base polymer. The base polymer may be of only one type, or may be of two or more types. The content of the base polymer in the pressure-sensitive adhesive layer is preferably 20% by weight to 100% by weight, more preferably 30% by weight to 95% by weight, even more preferably 40% by weight to 90% by weight, particularly preferably 45% by weight to 85% by weight, and most preferably 50% by weight to 80% by weight, in order to further exert the effects of the present invention.

[0063] As the base polymer, any suitable polymer may be adopted as long as it does not impair the effects of the present invention. In terms of being able to further exhibit the effects of the present invention, the base polymer is preferably at least one selected from an acrylic polymer, a rubber polymer, a silicone polymer, and a urethane polymer. That is, the adhesive layer preferably contains at least one selected from an acrylic adhesive containing an acrylic polymer, a rubber adhesive containing a rubber polymer, a silicone adhesive containing a silicone polymer, and a urethane adhesive containing a urethane polymer. In terms of being able to further exhibit the effects of the present invention, the adhesive layer preferably contains an acrylic adhesive. Hereinafter, an acrylic adhesive will be described in detail as a representative example of an adhesive that can be contained in the adhesive layer.

[0064] <Acrylic adhesive> The acrylic adhesive contains an acrylic polymer as a base polymer. The acrylic adhesive may contain a tackifier resin. The acrylic adhesive may contain a crosslinking agent.

[0065] When the acrylic pressure-sensitive adhesive comprises an acrylic polymer, a tackifier resin, and a crosslinking agent, the combined content of the acrylic polymer, tackifier resin, and crosslinking agent relative to the total amount of the acrylic pressure-sensitive adhesive is preferably 95% by weight or more, more preferably 97% by weight or more, and even more preferably 99% by weight or more, in order to further exert the effects of the present invention.

[0066] (Acrylic polymer) The acrylic polymer is preferably a polymer of monomer components that contains, for example, an alkyl (meth)acrylate as a main monomer and may further contain a sub-monomer copolymerizable with the main monomer, where the main monomer is a component that accounts for more than 50% by weight of the total monomer components.

[0067] As the alkyl(meth)acrylate, for example, a compound represented by the following formula (1) can be suitably used. CH2=C(R 1 )COOR2 (1)

[0068] Here, R in the above formula (1) 1 is a hydrogen atom or a methyl group, and R 2 is a chain alkyl group having 1 to 20 carbon atoms (hereinafter, such a range of the number of carbon atoms may be expressed as "C1-20"). From the viewpoint of the storage modulus of the adhesive layer, R 2 is preferably a C1-14 chain alkyl group, more preferably a C2-10 chain alkyl group, and further preferably a C4-8 chain alkyl group. Here, chain alkyl group includes linear and branched chains.

[0069] R 2 Examples of alkyl(meth)acrylates in which is a C1-20 chain alkyl group include methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, isopropyl(meth)acrylate, n-butyl(meth)acrylate, isobutyl(meth)acrylate, s-butyl(meth)acrylate, pentyl(meth)acrylate, isopentyl(meth)acrylate, hexyl(meth)acrylate, heptyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, octyl(meth)acrylate, isooctyl(meth)acrylate, Examples of the alkyl (meth)acrylate include acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate. These alkyl (meth)acrylates may be used alone or in combination of two or more kinds.

[0070] As the alkyl (meth)acrylate, from the viewpoint of further exerting the effects of the present invention, preferred examples include n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA).

[0071] The content of alkyl (meth)acrylate in all monomer components used in the synthesis of the acrylic polymer is preferably 70% by weight or more, more preferably 85% by weight or more, and even more preferably 90% by weight or more, in order to more effectively exhibit the effects of the present invention. The upper limit of the content of alkyl (meth)acrylate is preferably 99.5% by weight or less, more preferably 99% by weight or less. However, the acrylic polymer may be obtained by substantially polymerizing only alkyl (meth)acrylate.

[0072] R 2 When using an alkyl (meth)acrylate in which R is a C4-8 chain alkyl group, the alkyl (meth)acrylate in the monomer component 2 The proportion of the alkyl (meth)acrylate in which the alkyl group is a C4-8 chain alkyl group is preferably 50% by weight or more, more preferably 70% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 99% by weight to 100% by weight, in order to further exert the effects of the present invention.

[0073] One embodiment of the acrylic polymer is an acrylic polymer in which 50% by weight or more of the total monomer components is n-butyl acrylate (BA). In this case, the content of n-butyl acrylate (BA) in the total monomer components is preferably more than 50% by weight and not more than 100% by weight, more preferably 55% to 95% by weight, even more preferably 60% to 90% by weight, particularly preferably 63% to 85% by weight, and most preferably 65% ​​to 80% by weight, in order to further exhibit the effects of the present invention. The total monomer components may further contain 2-ethylhexyl acrylate (2EHA) in a proportion less than n-butyl acrylate (BA).

[0074] One embodiment of the acrylic polymer is an acrylic polymer in which less than 50% by weight of the total monomer components is 2-ethylhexyl acrylate (2EHA). In this case, the content of 2-ethylhexyl acrylate (2EHA) in the total monomer components is preferably more than 0% by weight and not more than 48% by weight, more preferably 5% to 45% by weight, even more preferably 10% to 43% by weight, particularly preferably 15% to 40% by weight, and most preferably 20% to 35% by weight, in order to further exhibit the effects of the present invention. The total monomer components may further contain n-butyl acrylate (BA) in a proportion greater than 2-ethylhexyl acrylate (2EHA).

[0075] The acrylic polymer may be copolymerized with other monomers within a range that does not impair the effects of the present invention. The other monomers can be used for the purpose of, for example, adjusting the glass transition temperature (Tg) of the acrylic polymer, adjusting the adhesive performance, etc. For example, as monomers that can improve the cohesive strength and heat resistance of the adhesive, there can be mentioned sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, cyano group-containing monomers, vinyl esters, aromatic vinyl compounds, etc., with vinyl esters being preferred. Specific examples of vinyl esters include, for example, vinyl acetate (VAc), vinyl propionate, vinyl laurate, etc., with vinyl acetate (VAc) being preferred.

[0076] The "other monomer" may be one type or two or more types. The content of the other monomer in the total monomer components is preferably 0.001% by weight to 40% by weight, more preferably 0.01% by weight to 40% by weight, even more preferably 0.1% by weight to 10% by weight, particularly preferably 0.5% by weight to 5% by weight, and most preferably 1% by weight to 3% by weight.

[0077] Examples of other monomers that can introduce a functional group that can serve as a crosslinking base point into the acrylic polymer or that can contribute to improving adhesive strength include hydroxyl group (OH group)-containing monomers, carboxy group-containing monomers, acid anhydride group-containing monomers, amide group-containing monomers, amino group-containing monomers, imide group-containing monomers, epoxy group-containing monomers, (meth)acryloylmorpholine, and vinyl ethers.

[0078] As an embodiment of the acrylic polymer, there is an acrylic polymer in which a carboxyl group-containing monomer is copolymerized as another monomer. Examples of the carboxyl group-containing monomer include acrylic acid (AA), methacrylic acid (MAA), carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid. Among these, in terms of being able to more effectively exhibit the effects of the present invention, the carboxyl group-containing monomer is preferably acrylic acid (AA) or methacrylic acid (MAA), and more preferably acrylic acid (AA).

[0079] When a carboxy group-containing monomer is used as the other monomer, the content of the other monomer in the total monomer components is preferably 0.1 wt % to 10 wt %, more preferably 0.2 wt % to 8 wt %, even more preferably 0.5 wt % to 5 wt %, particularly preferably 0.7 wt % to 4 wt %, and most preferably 1 wt % to 3 wt %, in order to further exert the effects of the present invention.

[0080] One embodiment of the acrylic polymer is an acrylic polymer copolymerized with a hydroxyl group-containing monomer as another monomer. Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; polypropylene glycol mono(meth)acrylate; and N-hydroxyethyl (meth)acrylamide. Among these, the hydroxyl group-containing monomer is preferably a hydroxyalkyl (meth)acrylate in which the alkyl group has 2 to 4 carbon atoms and is linear, in terms of being able to more effectively exhibit the effects of the present invention. Specifically, examples of the hydroxyl group-containing monomer include 2-hydroxyethyl acrylate (HEA) and 4-hydroxybutyl acrylate (4HBA), and more preferably 4-hydroxybutyl acrylate (4HBA).

[0081] When a hydroxyl group-containing monomer is used as the other monomer, the content of the other monomer in the total monomer components is preferably 0.001 wt % to 10 wt %, more preferably 0.01 wt % to 5 wt %, even more preferably 0.02 wt % to 2 wt %, particularly preferably 0.03 wt % to 1 wt %, and most preferably 0.05 wt % to 0.5 wt %, in order to further exert the effects of the present invention.

[0082] The Tg of the base polymer may be, for example, -80°C or higher, from the viewpoint of further exerting the effects of the present invention. The base polymer (preferably an acrylic polymer) is designed to have a Tg of preferably -15°C or lower, from the viewpoint of enhancing the deformability of the pressure-sensitive adhesive layer in the shear direction. In some embodiments, the Tg of the base polymer is, for example, preferably -25°C or lower, more preferably -40°C or lower, and even more preferably -50°C or lower. The Tg of the base polymer is designed to have a Tg of preferably -70°C or higher (more preferably -65°C or higher, and even more preferably -60°C or higher), from the viewpoint of enhancing cohesiveness and shape recovery.

[0083] The Tg of the base polymer is a value calculated from the Fox formula based on the Tg of the homopolymer of each monomer constituting the base polymer and the weight fraction of the monomer (copolymerization ratio by weight). The Fox formula is a relational expression between the Tg of the copolymer and the glass transition temperature Tgi of the homopolymer obtained by homopolymerizing each of the monomers constituting the copolymer, as shown below. 1 / Tg=Σ(Wi / Tgi)

[0084] In the above Fox formula, Tg is the glass transition temperature (unit: K) of the copolymer, Wi is the weight fraction (copolymerization ratio by weight) of monomer i in the copolymer, and Tgi is the glass transition temperature (unit: K) of a homopolymer of monomer i. As the Tg of the homopolymer, a value described in a publicly known document is adopted.

[0085] As the Tg of the homopolymer, for example, the following values ​​can be specifically used: 2-Ethylhexyl acrylate -70℃ n-Butyl acrylate -55℃ Acrylic acid 106℃ 2-Hydroxyethyl acrylate -15℃ 4-Hydroxybutyl acrylate -40℃

[0086] For the Tg of homopolymers other than those exemplified above, the values ​​listed in "Polymer Handbook" (3rd edition, John Wiley & Sons, Inc., 1989) can be used. When multiple values ​​are listed in the "Polymer Handbook," the conventional values ​​are used. For monomers not listed in the "Polymer Handbook," the catalog values ​​of the monomer manufacturers are used. For the Tg of homopolymers of monomers not listed in the "Polymer Handbook" and for which no catalog values ​​are provided by the monomer manufacturers, the values ​​obtained by the measurement method described in JP 2007-51271 A are used.

[0087] As a method for obtaining an acrylic polymer, various polymerization methods known as a synthesis method for an acrylic polymer, such as a solution polymerization method, an emulsion polymerization method, a bulk polymerization method, a suspension polymerization method, etc., can be appropriately adopted. Among these polymerization methods, a solution polymerization method can be preferably used. As a monomer supply method when performing solution polymerization, a lump-sum charging method in which the entire amount of the monomer component is supplied at once, a continuous supply (dropping) method, a divided supply (dropping) method, etc. can be appropriately adopted. The polymerization temperature can be appropriately selected depending on the type of monomer and solvent used, the type of polymerization initiator, etc., and is preferably 20°C or higher, more preferably 30°C or higher, even more preferably 40°C or higher, preferably 170°C or lower, more preferably 160°C or lower, and even more preferably 140°C or lower. As a method for obtaining an acrylic polymer, photopolymerization (typically performed in the presence of a photopolymerization initiator) performed by irradiating light such as UV rays, or radiation polymerization performed by irradiating radiation such as β rays or γ rays, etc., may be adopted.

[0088] The solvent (polymerization solvent) used in the solution polymerization can be appropriately selected from any suitable organic solvent, for example, aromatic compounds (typically aromatic hydrocarbons) such as toluene, acetate esters such as ethyl acetate, aliphatic or alicyclic hydrocarbons such as hexane and cyclohexane, etc.

[0089] The initiator (polymerization initiator) used for polymerization can be appropriately selected from any suitable polymerization initiator depending on the type of polymerization method. The polymerization initiator may be one type or two or more types. Examples of such polymerization initiators include azo-based polymerization initiators such as 2,2'-azobisisobutyronitrile (AIBN); persulfates such as potassium persulfate; peroxide-based initiators such as benzoyl peroxide and hydrogen peroxide; substituted ethane-based initiators such as phenyl-substituted ethane; and aromatic carbonyl compounds. Other examples of polymerization initiators include redox-based initiators formed by combining a peroxide with a reducing agent.

[0090] The amount of the polymerization initiator used is preferably 0.005 to 1 part by weight, and more preferably 0.01 to 1 part by weight, based on 100 parts by weight of the total monomer components.

[0091] The Mw of the acrylic polymer is preferably 10×10 4 ~500×10 4 and more preferably 10×10 4 ~150×10 4 and more preferably 20×10 4 ~75×10 4 and particularly preferably 35×10 4 ~65×10 4 Here, Mw refers to a value calculated in terms of standard polystyrene obtained by GPC (gel permeation chromatography). As the GPC device, for example, a model named "HLC-8320GPC" (column: TSKgel GMH-H(S), manufactured by Tosoh Corporation) can be used.

[0092] (tackifier resin) The acrylic adhesive may contain a tackifier resin so as to more effectively exert the effects of the present invention. Examples of the tackifier resin include rosin-based tackifier resins, terpene-based tackifier resins, hydrocarbon-based tackifier resins, epoxy-based tackifier resins, polyamide-based tackifier resins, elastomer-based tackifier resins, phenol-based tackifier resins, and ketone-based tackifier resins. The tackifier resin may be one type or two or more types.

[0093] The amount of the tackifier resin used, in order to further exert the effects of the present invention, is preferably 5 parts by weight to 70 parts by weight, more preferably 10 parts by weight to 60 parts by weight, even more preferably 15 parts by weight to 50 parts by weight, still more preferably 20 parts by weight to 45 parts by weight, particularly preferably 25 parts by weight to 40 parts by weight, and most preferably 25 parts by weight to 35 parts by weight, relative to 100 parts by weight of the base polymer.

[0094] The tackifier resin preferably contains a tackifier resin TL having a softening point of less than 105°C, in order to more effectively exert the effects of the present invention. The tackifier resin TL can effectively contribute to improving the deformability in the planar direction (shear direction) of the pressure-sensitive adhesive layer. From the viewpoint of obtaining a higher effect of improving deformability, the softening point of the tackifier resin used as the tackifier resin TL is preferably 50°C to 103°C, more preferably 60°C to 100°C, even more preferably 65°C to 95°C, particularly preferably 70°C to 90°C, and most preferably 75°C to 85°C.

[0095] The softening point of a tackifier resin is defined as a value measured based on the softening point test method (ring and ball method) specified in JIS K5902 and JIS K2207. Specifically, the sample is melted as quickly as possible at the lowest possible temperature, and is carefully filled into a ring placed on a flat metal plate, taking care not to create bubbles. After cooling, the part that protrudes from the flat surface, including the top end of the ring, is cut off with a slightly heated knife. Next, a holder (ring stand) is placed in a glass container (heating bath) with a diameter of 85 mm or more and a height of 127 mm or more, and glycerin is poured in until it is 90 mm or more deep. Next, a steel ball (diameter 9.5 mm, weight 3.5 g) and the ring filled with the sample are immersed in glycerin without touching each other, and the temperature of the glycerin is kept at 20°C ± 5°C for 15 minutes. Next, the steel ball is placed in the center of the surface of the sample in the ring, and this is placed in a fixed position on the holder. Next, keeping the distance from the top of the ring to the glycerin surface at 50 mm, place a thermometer and align the center of the thermometer's mercury bulb to the same height as the center of the ring, then heat the container. The flame of the Bunsen burner used for heating should be midway between the center of the bottom of the container and its edge, and heating should be uniform. After heating begins and the temperature of the bath reaches 40°C, the rate of increase must be 5.0 ± 0.5°C per minute. The sample gradually softens and flows down the ring, and the temperature is read when it finally touches the bottom plate, and this is the softening point. The softening point is measured for two or more samples at the same time, and the average value is used.

[0096] The amount of tackifier resin TL used is preferably 5 to 50 parts by weight, more preferably 10 to 45 parts by weight, even more preferably 15 to 40 parts by weight, particularly preferably 20 to 35 parts by weight, and most preferably 25 to 32 parts by weight, relative to 100 parts by weight of base polymer, in order to further exert the effects of the present invention.

[0097] As the tackifier resin TL, one or more types may be used that are appropriately selected from the tackifier resins exemplified above that have a softening point of less than 105° C. The tackifier resin TL preferably contains a rosin-based resin.

[0098] Examples of rosin-based resins that can be preferably used as the tackifier resin TL include rosin esters such as unmodified rosin ester and modified rosin ester. Examples of modified rosin esters include hydrogenated rosin ester.

[0099] The tackifier resin TL preferably contains a hydrogenated rosin ester, which can further exert the effects of the present invention. The softening point of the hydrogenated rosin ester is preferably less than 105°C, more preferably 50°C to 100°C, even more preferably 60°C to 90°C, particularly preferably 70°C to 85°C, and most preferably 75°C to 85°C, which can further exert the effects of the present invention.

[0100] The tackifier resin TL may contain a non-hydrogenated rosin ester. The term "non-hydrogenated rosin ester" as used herein is a general term referring to the above-mentioned rosin esters other than the hydrogenated rosin ester. Examples of the non-hydrogenated rosin ester include unmodified rosin ester, disproportionated rosin ester, and polymerized rosin ester.

[0101] The softening point of the non-hydrogenated rosin ester is preferably less than 105°C, more preferably from 50°C to 100°C, even more preferably from 60°C to 90°C, particularly preferably from 70°C to 85°C, and most preferably from 75°C to 85°C, in order to better exhibit the effects of the present invention.

[0102] The tackifier resin TL may contain other tackifier resins in addition to the rosin resin. As the other tackifier resins, one or more types appropriately selected from the tackifier resins exemplified above having a softening point of less than 105° C. may be used. The tackifier resin TL may contain, for example, a rosin resin and a terpene resin.

[0103] The content of the rosin-based resin in the entire tackifier resin TL is preferably more than 50% by weight, more preferably 55% by weight to 100% by weight, even more preferably 60% by weight to 99% by weight, particularly preferably 65% ​​by weight to 97% by weight, and most preferably 75% by weight to 97% by weight, in order to further exert the effects of the present invention.

[0104] The tackifier resin may contain a combination of a tackifier resin TL and a tackifier resin TH having a softening point of 105° C. or higher (preferably 105° C. to 170° C.), in order to further exert the effects of the present invention.

[0105] As the tackifier resin TH, one or more types appropriately selected from the above-listed tackifier resins having a softening point of 105° C. or higher can be used. The tackifier resin TH can include at least one type selected from rosin-based tackifier resins (e.g., rosin esters) and terpene-based tackifier resins (e.g., terpene phenol resins).

[0106] (Crosslinking agent) The acrylic adhesive may contain a crosslinking agent. The crosslinking agent may be one type or two or more types. The use of the crosslinking agent can impart an appropriate cohesive force to the acrylic adhesive. The crosslinking agent can also be useful for adjusting the slippage distance and return distance in the holding power test. The acrylic adhesive containing the crosslinking agent can be obtained, for example, by forming an adhesive layer using an adhesive composition containing the crosslinking agent. The crosslinking agent may be contained in the acrylic adhesive in a form after crosslinking reaction, a form before crosslinking reaction, a form partially crosslinked, an intermediate or composite form thereof, or the like. The crosslinking agent is typically contained in the acrylic adhesive exclusively in a form after crosslinking reaction.

[0107] The amount of the crosslinking agent used is preferably 0.005 to 10 parts by weight, more preferably 0.01 to 7 parts by weight, even more preferably 0.05 to 5 parts by weight, particularly preferably 0.1 to 4 parts by weight, and most preferably 1 to 3 parts by weight, relative to 100 parts by weight of the base polymer, in order to further exert the effects of the present invention.

[0108] Examples of the crosslinking agent include an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, a silicone-based crosslinking agent, an oxazoline-based crosslinking agent, an aziridine-based crosslinking agent, a silane-based crosslinking agent, an alkyl etherified melamine-based crosslinking agent, a metal chelate-based crosslinking agent, a peroxide-based crosslinking agent, and the like. From the viewpoint of being able to further exert the effects of the present invention, an isocyanate-based crosslinking agent or an epoxy-based crosslinking agent is preferable, and an isocyanate-based crosslinking agent is more preferable.

[0109] The isocyanate crosslinking agent may be a compound having two or more isocyanate groups (including isocyanate regenerating functional groups in which the isocyanate groups are temporarily protected by a blocking agent or oligomerization) in one molecule. Examples of the isocyanate crosslinking agent include aromatic isocyanates such as tolylene diisocyanate and xylylene diisocyanate; alicyclic isocyanates such as isophorone diisocyanate; and aliphatic isocyanates such as hexamethylene diisocyanate.

[0110] More specifically, the isocyanate-based crosslinking agent may be, for example, lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate; aromatic diisocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate and polymethylene polyphenyl isocyanate; trimethylolpropane / tolylene diisocyanate trimer adduct (e.g., manufactured by Tosoh Corporation, trade name: Coronate L), trimethylolpropane / hexamethylene diisocyanate trimer adduct (e.g., manufactured by Tosoh Corporation, trade name: Coronate HL), and isocyanurate of hexamethylene diisocyanate (e.g., manufactured by Tosoh Corporation, trade name: Coronate HL). isocyanate adducts such as CORONATE HX (manufactured by Mitsui Chemicals, Inc.); trimethylolpropane adduct of xylylene diisocyanate (e.g., Takenate D110N, manufactured by Mitsui Chemicals, Inc.), trimethylolpropane adduct of xylylene diisocyanate (e.g., Takenate D120N, manufactured by Mitsui Chemicals, Inc.), trimethylolpropane adduct of isophorone diisocyanate (e.g., Takenate D140N, manufactured by Mitsui Chemicals, Inc.), trimethylolpropane adduct of hexamethylene diisocyanate (e.g., Takenate D160N, manufactured by Mitsui Chemicals, Inc.); polyether polyisocyanate, polyester polyisocyanate, and adducts of these with various polyols; polyisocyanates multifunctionalized with isocyanurate bonds, biuret bonds, allophanate bonds, etc.; Among these, aromatic isocyanates and alicyclic isocyanates are preferred because they can achieve a good balance between deformability and cohesive strength.

[0111] The amount of the isocyanate-based crosslinking agent used is preferably 0.005 to 10 parts by weight, more preferably 0.01 to 7 parts by weight, even more preferably 0.05 to 5 parts by weight, particularly preferably 0.1 to 4 parts by weight, and most preferably 1 to 3 parts by weight, relative to 100 parts by weight of the base polymer, in order to further exert the effects of the present invention.

[0112] When the monomer component constituting the acrylic polymer contains a hydroxyl group-containing monomer, the weight ratio of the isocyanate-based crosslinking agent / hydroxyl group-containing monomer is preferably more than 20 and less than 50, more preferably 22 to 45, even more preferably 25 to 40, particularly preferably 27 to 40, and most preferably 30 to 35, in order to further exert the effects of the present invention.

[0113] When the acrylic adhesive contains a tackifier resin TL having a softening point of 105°C or less, in order to further exert the effects of the present invention, the weight ratio of the tackifier resin TL / isocyanate-based crosslinking agent is preferably more than 2 and less than 15, more preferably 5 to 13, even more preferably 7 to 12, and particularly preferably 7 to 11.

[0114] As the epoxy crosslinking agent, a polyfunctional epoxy compound having two or more epoxy groups in one molecule can be used. Examples of the epoxy crosslinking agent include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, sorbitol polyglycidyl ether, and the like. Examples of epoxy crosslinking agents include glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl-tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. Examples of commercially available epoxy crosslinking agents include "Tetrad C" and "Tetrad X" manufactured by Mitsubishi Gas Chemical Company, Inc.

[0115] The amount of the epoxy-based crosslinking agent used is preferably 0.005 parts by weight to 10 parts by weight, more preferably 0.01 parts by weight to 5 parts by weight, even more preferably 0.015 parts by weight to 1 part by weight, particularly preferably 0.15 parts by weight to 0.5 parts by weight, and most preferably 0.015 parts by weight to 0.3 parts by weight, relative to 100 parts by weight of the base polymer, in terms of being able to further exhibit the effects of the present invention.

[0116] (Other ingredients) The acrylic pressure-sensitive adhesive may contain, as necessary, various additives commonly used in the field of pressure-sensitive adhesives, such as a leveling agent, a crosslinking assistant, a plasticizer, a softener, a filler, an antistatic agent, an antiaging agent, an ultraviolet absorber, an antioxidant, a light stabilizer, etc. As for such various additives, conventionally known ones can be used in the usual manner.

[0117] <Antistatic layer> The pressure-sensitive adhesive film of the present invention may have an antistatic layer on the surface of the base layer opposite to the surface having the pressure-sensitive adhesive layer. By having an antistatic layer on the surface of the base layer opposite to the surface having the pressure-sensitive adhesive layer, the pressure-sensitive adhesive film itself can be suppressed from being charged, making it difficult for dust to be adsorbed, which is a preferred embodiment.

[0118] For the antistatic layer, for example, a method of applying an antistatic resin consisting of an antistatic agent and a resin component, a conductive polymer, or a conductive resin containing a conductive substance, or a method of depositing or plating a conductive substance can be mentioned.

[0119] Examples of antistatic agents contained in the antistatic resin include cationic antistatic agents having cationic functional groups such as quaternary ammonium salts, pyridinium salts, and primary, secondary, and tertiary amino groups; anionic antistatic agents having anionic functional groups such as sulfonates, sulfates, phosphonates, and phosphates; amphoteric antistatic agents such as alkylbetaines and their derivatives, imidazolines and their derivatives, and alanine and their derivatives; nonionic antistatic agents such as aminoalcohols and their derivatives, glycerin and its derivatives, and polyethylene glycol and its derivatives; ionic conductive polymers obtained by polymerizing or copolymerizing monomers having the above-mentioned cationic, anionic, and amphoteric ion-conductive groups; etc. These antistatic agents may be used alone or in combination.

[0120] Examples of cationic antistatic agents include alkyl trimethyl ammonium salts, acyloyl amidopropyl trimethyl ammonium methosulfate, alkyl benzyl methyl ammonium salts, acyl choline chloride, (meth)acrylate copolymers having a quaternary ammonium group such as polydimethylaminoethyl methacrylate, styrene copolymers having a quaternary ammonium group such as polyvinyl benzyl trimethyl ammonium chloride, diallyl amine copolymers having a quaternary ammonium group such as polydiallyl dimethyl ammonium chloride, etc. These antistatic agents may be used alone or in combination of two or more kinds.

[0121] Examples of anionic antistatic agents include alkyl sulfonates, alkyl benzene sulfonates, alkyl sulfates, alkyl ethoxy sulfates, alkyl phosphates, sulfonic acid group-containing styrene copolymers, etc. These antistatic agents may be used alone or in combination of two or more kinds.

[0122] Examples of amphoteric ion type antistatic agents include alkyl betaine, alkyl imidazolium betaine, carbobetaine graft copolymer, etc. These antistatic agents may be used alone or in combination of two or more kinds.

[0123] Examples of nonionic antistatic agents include fatty acid alkylolamides, di(2-hydroxyethyl)alkylamines, polyoxyethylene alkylamines, fatty acid glycerin esters, polyoxyethylene glycol fatty acid esters, sorbitan fatty acid esters, polyoxysorbitan fatty acid esters, polyoxyethylene alkylphenyl ethers, polyoxyethylene alkyl ethers, polyethylene glycols, polyoxyethylene diamines, copolymers of polyethers, polyesters and polyamides, methoxypolyethylene glycol (meth)acrylates, etc. These antistatic agents may be used alone or in combination of two or more kinds.

[0124] Examples of the conductive polymer include polyaniline, polypyrrole, polythiophene, etc. These conductive polymers may be used alone or in combination of two or more kinds.

[0125] Examples of the conductive substance include tin oxide, antimony oxide, indium oxide, cadmium oxide, titanium oxide, zinc oxide, indium, tin, antimony, gold, silver, copper, aluminum, nickel, chromium, titanium, iron, cobalt, copper iodide, and alloys or mixtures thereof. Only one type of these conductive substances may be used, or two or more types may be used.

[0126] Resin components used in the antistatic resin and conductive resin include, for example, general-purpose resins such as polyester resin, acrylic resin, polyvinyl resin, urethane resin, melamine resin, and epoxy resin. In the case of a polymer-type antistatic agent, it is not necessary to include a resin component. In addition, it is also possible to include, as a crosslinking agent, a methylolated or alkylolated melamine compound, a urea compound, a glyoxal compound, an acrylamide compound, an epoxy compound, an isocyanate compound, or the like, as a component of the antistatic resin.

[0127] The antistatic layer can be formed, for example, by diluting the above-mentioned antistatic resin, conductive polymer, conductive resin, or the like with a solvent such as an organic solvent or water, applying the resulting coating liquid to a substrate, and drying the coating liquid.

[0128] Examples of the dilution solution used for forming the antistatic layer include methyl ethyl ketone, acetone, ethyl acetate, tetrahydrofuran, dioxane, cyclohexanone, n-hexane, toluene, xylene, methanol, ethanol, n-propanol, isopropanol, water, etc. These solvents may be used alone or in combination of two or more kinds.

[0129] Regarding the coating method in forming the antistatic layer, any appropriate coating method can be appropriately used, such as roll coating, gravure coating, reverse coating, roll brushing, spray coating, air knife coating, impregnation, curtain coating, etc.

[0130] The method for depositing or plating the conductive material may be any suitable method, such as vacuum deposition, sputtering, ion plating, chemical vapor deposition, spray pyrolysis, chemical plating, or electroplating.

[0131] The thickness of the antistatic layer may be any appropriate thickness as long as the effects of the present invention are not impaired. In terms of further exerting the effects of the present invention, the thickness of the antistatic layer is preferably 0.001 μm to 5 μm, and more preferably 0.005 μm to 1 μm.

[0132] <Topcoat layer> The pressure-sensitive adhesive film of the present invention may have a topcoat layer on the surface of the base layer opposite to the surface having the pressure-sensitive adhesive layer. The topcoat layer preferably contains a binder, more preferably contains a binder and a slipping agent. By having the topcoat layer in the pressure-sensitive adhesive film of the present invention, the scratch resistance of the pressure-sensitive adhesive film is improved, which is a preferred embodiment.

[0133] <Binder> The binder may be any appropriate resin as long as it does not impair the effects of the present invention. In terms of being able to more effectively exert the effects of the present invention, such a resin is preferably at least one selected from the group consisting of polyester resins and urethane resins.

[0134] (polyester resin) When the binder contains a polyester resin, the polyester resin may be of only one kind, or of two or more kinds.

[0135] The polyester resin is preferably a resin containing polyester as a main component. The content of polyester in the polyester resin is preferably more than 50% by weight, more preferably 75% by weight or more, and further preferably 90% by weight or more.

[0136] The polyester preferably has a structure obtained by condensing at least one compound (polycarboxylic acid component) selected from polycarboxylic acids (preferably dicarboxylic acids) having two or more carboxyl groups in one molecule and derivatives thereof (anhydrides, esters, halides, etc. of polycarboxylic acids) with at least one compound (polyhydric alcohol component) selected from polyhydric alcohols (preferably diols) having two or more hydroxyl groups in one molecule.

[0137] Examples of compounds that can be used as the polyvalent carboxylic acid component include oxalic acid, malonic acid, difluoromalonic acid, alkylmalonic acid, succinic acid, tetrafluorosuccinic acid, alkylsuccinic acid, (±)-malic acid, meso-tartaric acid, itaconic acid, maleic acid, methylmaleic acid, fumaric acid, methylfumaric acid, acetylenedicarboxylic acid, glutaric acid, hexafluoroglutaric acid, methylglutaric acid, glutaconic acid, adipic acid, dithioadipic acid, methyladipic acid, dimethyladipic acid, tetramethyladipic acid, methyleneadipic acid, muconic acid, galactosamine ... Aliphatic dicarboxylic acids such as lactaric acid, pimelic acid, suberic acid, perfluorosuberic acid, 3,3,6,6-tetramethylsuberic acid, azelaic acid, sebacic acid, perfluorosebacic acid, brassylic acid, dodecyldicarboxylic acid, tridecyldicarboxylic acid, and tetradecyldicarboxylic acid; cycloalkyl dicarboxylic acids (e.g., 1,4-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid), 1,4-(2-norbornene)dicarboxylic acid, 5-norbornene-2,3-dicarboxylic acid (himic acid), and adamantane dicarboxylic acid. alicyclic dicarboxylic acids such as phthalic acid, isophthalic acid, dithioisophthalic acid, methylisophthalic acid, dimethylisophthalic acid, chloroisophthalic acid, dichloroisophthalic acid, terephthalic acid, methylterephthalic acid, dimethylterephthalic acid, chloroterephthalic acid, bromoterephthalic acid, naphthalenedicarboxylic acid, oxofluorenedicarboxylic acid, anthracenedicarboxylic acid, biphenyldicarboxylic acid, biphenylenedicarboxylic acid, dimethylbiphenylenedicarboxylic acid, 4,4”-p-terephenylenedicarboxylic acid, 4 aromatic dicarboxylic acids such as 4,4'-p-quartylphenyldicarboxylic acid, bibenzyldicarboxylic acid, azobenzenedicarboxylic acid, homophthalic acid, phenylenediacetic acid, phenylenedipropionic acid, naphthalenedicarboxylic acid, naphthalenedipropionic acid, biphenyldiacetic acid, biphenyldipropionic acid, 3,3'-[4,4'-(methylenedi-p-biphenylene)dipropionic acid, 4,4'-bibenzyldiacetic acid, 3,3'(4,4'-bibenzyl)dipropionic acid, and oxydi-p-phenylenediacetic acid; anhydrides of any of the above-mentioned polycarboxylic acids;Examples of the polycarboxylic acid include esters of any of the above polycarboxylic acids (e.g., alkyl esters, monoesters, diesters, etc.); acid halides corresponding to any of the above polycarboxylic acids (e.g., dicarboxylic acid chlorides, etc.); and the like.

[0138] Suitable examples of compounds that can be used as the polyvalent carboxylic acid component include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, and their acid anhydrides; aliphatic dicarboxylic acids such as adipic acid, sebacic acid, azelaic acid, succinic acid, fumaric acid, maleic acid, himic acid, and 1,4-cyclohexanedicarboxylic acid, and their acid anhydrides; and lower alkyl esters of the above dicarboxylic acids (for example, esters with monoalcohols having 1 to 3 carbon atoms).

[0139] Examples of compounds that can be used as the polyhydric alcohol component include diols such as ethylene glycol, propylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 3-methylpentanediol, diethylene glycol, 1,4-cyclohexanedimethanol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, xylylene glycol, hydrogenated bisphenol A, and bisphenol A. Other examples include alkylene oxide adducts of these compounds (e.g., ethylene oxide adducts, propylene oxide adducts, etc.).

[0140] The polyester resin preferably contains a water-dispersible polyester, and more preferably contains a water-dispersible polyester as a main component. Such a water-dispersible polyester may be, for example, a polyester having improved water dispersibility by introducing a hydrophilic functional group (for example, at least one selected from hydrophilic functional groups such as a metal sulfonate group, a carboxyl group, an ether group, and a phosphate group) into the polymer. As described above, any suitable method can be appropriately adopted as a method for introducing a hydrophilic functional group into the polymer, such as a method for copolymerizing a compound having a hydrophilic functional group, or a method for modifying a polyester or its precursor (for example, a polyvalent carboxylic acid component, a polyhydric alcohol component, an oligomer thereof, etc.) to generate a hydrophilic functional group. A preferred water-dispersible polyester is a polyester (copolymerized polyester) in which a compound having a hydrophilic functional group is copolymerized.

[0141] The polyester resin used as the binder may be one that is mainly composed of saturated polyester or one that is mainly composed of unsaturated polyester. The polyester resin is preferably one that is mainly composed of saturated polyester, more preferably one that is water-dispersible (e.g., saturated copolymer polyester). Such a polyester resin (polyester resin that may be prepared in the form of a water dispersion) can be synthesized by any suitable method, or can be easily obtained as a commercially available product.

[0142] The molecular weight of the polyester resin is preferably 0.5×10 as a weight average molecular weight (Mw) converted into standard polystyrene as measured by gel permeation chromatography (GPC). 4 ~15×10 4 and more preferably 1×10 4 ~6×10 4 It is.

[0143] The glass transition temperature (Tg) of the polyester resin is preferably from 0°C to 100°C, and more preferably from 10°C to 80°C.

[0144] (Urethane resin) When a urethane-based resin is contained in the binder, the urethane-based resin may be of only one type, or of two or more types.

[0145] The urethane-based resin is preferably a urethane-based resin obtained by curing a composition containing a polyol (A) and a polyfunctional isocyanate compound (B).

[0146] The polyol (A) may be of only one type, or of two or more types.

[0147] Any suitable polyol having two or more OH groups may be used as the polyol (A). Examples of such polyol (A) include a polyol (diol) having two OH groups, a polyol (triol) having three OH groups, a polyol (tetraol) having four OH groups, a polyol (pentaol) having five OH groups, and a polyol (hexaol) having six OH groups.

[0148] As the polyol (A), a glycol having two or more OH groups, such as ethylene glycol or propylene glycol, is preferably used as an essential component. By using a glycol as an essential component in this way, for example, a urethane-based cured resin having excellent strength of the coating film after curing, excellent adhesion to the substrate, and excellent retention of added substances can be provided. The content of the glycol in the polyol (A) is preferably 30% by weight to 100% by weight, more preferably 50% by weight to 100% by weight, even more preferably 70% by weight to 100% by weight, even more preferably 90% by weight to 100% by weight, particularly preferably 95% by weight to 100% by weight, and most preferably substantially 100% by weight.

[0149] Examples of the polyol (A) include ethylene glycol, diethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2,4-diethyl-1,5-pentanediol, 1,2-hexanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, 1,8-decanediol, octadecanediol, glycerin, trimethylolpropane, pentaerythritol, hexanetriol, polyethylene glycol, polypropylene glycol, polyester polyol, polyether polyol, polycaprolactone polyol, polycarbonate polyol, and castor oil polyol.

[0150] The polyester polyol can be obtained, for example, by an esterification reaction between a polyol component and an acid component. etc.

[0151] Examples of the acid component include succinic acid, methylsuccinic acid, adipic acid, pimelic acid, azelaic acid, sebacic acid, 1,12-dodecanedioic acid, 1,14-tetradecanedioic acid, dimer acid, 2-methyl-1,4-cyclohexanedicarboxylic acid, 2-ethyl-1,4-cyclohexanedicarboxylic acid, terephthalic acid, isophthalic acid, phthalic acid, isophthalic acid, terephthalic acid, 1,4-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, and acid anhydrides thereof.

[0152] Examples of polyether polyols include polyether polyols obtained by addition polymerization of alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide using water, low molecular weight polyols (propylene glycol, ethylene glycol, glycerin, trimethylolpropane, pentaerythritol, etc.), bisphenols (bisphenol A, etc.), dihydroxybenzenes (catechol, resorcin, hydroquinone, etc.) as initiators. Specific examples include polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.

[0153] Examples of polycaprolactone polyols include caprolactone-based polyester diols obtained by ring-opening polymerization of cyclic ester monomers such as ε-caprolactone and σ-valerolactone.

[0154] Examples of the polycarbonate polyol include polycarbonate polyols obtained by subjecting the above polyol components to a polycondensation reaction with phosgene; polycarbonate polyols obtained by subjecting the above polyol components to an ester exchange condensation reaction with carbonate diesters such as dimethyl carbonate, diethyl carbonate, dipropyl carbonate, diisopropyl carbonate, dibutyl carbonate, ethyl butyl carbonate, ethylene carbonate, propylene carbonate, diphenyl carbonate, and dibenzyl carbonate; copolymer polycarbonate polyols obtained by using two or more of the above polyol components in combination; polycarbonate polyols obtained by subjecting the above various polycarbonate polyols to an esterification reaction with a carboxyl group-containing compound; Examples of the polycarbonate polyol include polycarbonate polyols obtained by subjecting a recarbonate polyol to an etherification reaction with a hydroxyl group-containing compound; polycarbonate polyols obtained by subjecting the above-mentioned various polycarbonate polyols to an ester exchange reaction with an ester compound; polycarbonate polyols obtained by subjecting the above-mentioned various polycarbonate polyols to an ester exchange reaction with a hydroxyl group-containing compound; polyester-based polycarbonate polyols obtained by subjecting the above-mentioned various polycarbonate polyols to a polycondensation reaction with a dicarboxylic acid compound; and copolymerized polyether-based polycarbonate polyols obtained by copolymerizing the above-mentioned various polycarbonate polyols with an alkylene oxide.

[0155] Examples of castor oil-based polyols include castor oil-based polyols obtained by reacting castor oil fatty acid with the above-mentioned polyol component.Specific examples of castor oil-based polyols include castor oil-based polyols obtained by reacting castor oil fatty acid with polypropylene glycol.

[0156] The polyfunctional isocyanate compound (B) may be of only one type, or of two or more types.

[0157] As the polyfunctional isocyanate compound (B), any suitable polyfunctional isocyanate compound that can be used in the urethane reaction can be adopted. Examples of such polyfunctional isocyanate compounds (B) include polyfunctional aliphatic isocyanate compounds, polyfunctional alicyclic isocyanates, and polyfunctional aromatic isocyanate compounds.

[0158] Examples of polyfunctional aliphatic isocyanate compounds include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate.

[0159] Examples of polyfunctional alicyclic isocyanate compounds include 1,3-cyclopentene diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, hydrogenated tolylene diisocyanate, and hydrogenated tetramethylxylylene diisocyanate.

[0160] Examples of polyfunctional aromatic diisocyanate compounds include phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-toluidine diisocyanate, 4,4'-diphenylether diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, and xylylene diisocyanate.

[0161] Examples of the polyfunctional isocyanate compound (B) include trimethylolpropane adducts of the various polyfunctional isocyanate compounds as described above, biuret products reacted with water, and trimers having an isocyanurate ring. These may also be used in combination.

[0162] The content of the polyfunctional isocyanate compound (B) is preferably 5% by weight to 60% by weight, more preferably 8% by weight to 60% by weight, and further preferably 10% by weight to 60% by weight, relative to the polyol (A). By adjusting the content of the polyfunctional isocyanate compound (B) within the above range, the effects of the present invention can be further exhibited.

[0163] The urethane resin is typically obtained by curing a composition containing a polyol (A) and a polyfunctional isocyanate compound (B). Such a composition may contain any other appropriate components other than the polyol (A) and the polyfunctional isocyanate compound (B) within a range that does not impair the effects of the present invention. Examples of such other components include catalysts, other resin components other than polyurethane resins, tackifiers, inorganic fillers, organic fillers, metal powders, pigments, foils, softeners, plasticizers, antioxidants, conductive agents, antioxidants, ultraviolet absorbers, light stabilizers, surface lubricants, leveling agents, corrosion inhibitors, heat stabilizers, polymerization inhibitors, lubricants, and solvents.

[0164] As a method for obtaining a urethane-based resin by curing a composition containing a polyol (A) and a polyfunctional isocyanate compound (B), any appropriate method can be adopted as long as it does not impair the effects of the present invention, such as a urethanization reaction method using bulk polymerization or solution polymerization.

[0165] (Other resins) The topcoat layer may further contain other resins other than polyester resins and urethane resins (for example, at least one resin selected from acrylic resins, acrylic-styrene resins, acrylic-silicone resins, silicone resins, polysilazane resins, fluororesins, and polyolefin resins) as binders to the extent that the performance of the adhesive film is not significantly impaired. In a preferred embodiment of the topcoat layer, the binder of the topcoat layer is substantially composed of at least one resin selected from the group consisting of polyester resins and urethane resins, and the ratio of at least one resin selected from the group consisting of polyester resins and urethane resins in the binder is preferably 98% by weight to 100% by weight, more preferably 99% by weight to 100% by weight, and even more preferably 99.5% by weight to 100% by weight. The ratio of the binder to the entire topcoat layer is preferably 15% by weight to 95% by weight, and more preferably 25% by weight to 80% by weight.

[0166] <Slip agent> The slip agent preferably contains an ester of a higher fatty acid and a higher alcohol (hereinafter sometimes referred to as "wax ester").

[0167] The "higher fatty acid" is preferably a carboxylic acid having 8 or more carbon atoms, more preferably 10 or more carbon atoms, and further preferably 10 to 40. The carboxylic acid is preferably a monocarboxylic acid.

[0168] The "higher alcohol" is preferably an alcohol having 6 or more carbon atoms, more preferably 10 or more carbon atoms, and further preferably 10 to 40. The alcohol is preferably a monohydric or dihydric alcohol, and more preferably a monohydric alcohol.

[0169] The topcoat layer having a composition containing such a wax ester in combination with the binder described above is less likely to whiten even when kept under high temperature and high humidity conditions. Therefore, a pressure-sensitive adhesive film having a substrate having such a topcoat layer can have a higher appearance quality.

[0170] The top coat layer having the above composition provides excellent whitening resistance (e.g., the property of being less likely to whiten even when kept under high temperature and humidity conditions) for the following reasons. That is, it is presumed that the silicone-based lubricants used in the past exert a function of imparting slipperiness to the surface of the top coat layer by bleeding onto the surface. However, the degree of bleeding of these silicone-based lubricants is likely to vary depending on the storage conditions (temperature, humidity, time, etc.). For this reason, for example, if the amount of silicone-based lubricant used is set so that a suitable slipperiness is obtained for a relatively long period (e.g., about 3 months) from immediately after the production of the adhesive film when kept under normal storage conditions (e.g., 25°C, 50% RH), when this adhesive film is stored under high temperature and humidity conditions (e.g., 60°C, 95% RH) for 2 weeks, the bleeding of the lubricant will proceed excessively. Such excessive bleeding of the silicone-based lubricant may cause whitening of the top coat layer (and thus the adhesive film).

[0171] A preferred embodiment of the topcoat layer employs a specific combination of a wax ester as a slipping agent and a polyester resin as a binder. With such a combination of a slipping agent and a binder, the degree of bleeding of the wax ester from the topcoat layer is less affected by storage conditions. This can improve the whitening resistance of the PSA film.

[0172] As the wax ester, one or more compounds represented by the general formula (W) can be preferably used. X-COO-Y (W)

[0173] X and Y in formula (W) are each independently preferably a hydrocarbon group having 10 to 40 carbon atoms, more preferably 10 to 35 carbon atoms, further preferably 14 to 35 carbon atoms, and particularly preferably 20 to 32 carbon atoms. If the number of carbon atoms is too small, the effect of imparting slipperiness to the top coat layer may be insufficient. The hydrocarbon group may be a saturated hydrocarbon group or an unsaturated hydrocarbon group. The hydrocarbon group is preferably a saturated hydrocarbon group. In addition, the hydrocarbon group may be a structure containing an aromatic ring, a structure not containing an aromatic ring (aliphatic hydrocarbon group), a hydrocarbon group having a structure containing an aliphatic ring (alicyclic hydrocarbon group), or a chain (including linear and branched) hydrocarbon group.

[0174] The wax ester is preferably a compound in which X and Y in formula (W) are each independently a chain alkyl group having 10 to 40 carbon atoms, more preferably a linear alkyl group having 10 to 40 carbon atoms. Specific examples of such compounds include myricyl cerotenate (CH3(CH2) 24 COO(CH2) 29 CH3), myricyl palmitate (CH3(CH2) 14 COO(CH2) 29 CH3), Cetyl Palmitate (CH3(CH2) 14 COO(CH2) 15 CH3), Stearyl stearate (CH3(CH2) 16 COO(CH2) 17 CH3) etc.

[0175] The wax ester has a melting point of preferably 50°C or higher, more preferably 60°C or higher, even more preferably 70°C or higher, and particularly preferably 75°C or higher. Such wax esters can realize higher whitening resistance. The wax ester has a melting point of preferably 100°C or lower. Such wax esters have a high effect of imparting slipperiness, so that a top coat layer with higher scratch resistance can be formed. The wax ester has a melting point of 100°C or lower, which is also preferable in terms of the ease of preparing an aqueous dispersion of the wax ester. As such a wax ester, for example, myricyl cerotic acid can be preferably adopted.

[0176] As a raw material for the top coat layer, a natural wax containing such a wax ester can be used. As such a natural wax, the content ratio of the above-mentioned wax ester (when two or more kinds of wax esters are contained, the total content ratio of them) is preferably more than 50% by weight, more preferably 65% ​​by weight or more, and even more preferably 75% by weight or more, based on the non-volatile content (NV). As such a natural wax, for example, carnauba wax (generally containing myricyl cerotenate at a ratio of preferably 60% by weight or more, more preferably 70% by weight or more, and even more preferably 80% by weight or more), vegetable wax such as palm wax, beeswax, whale wax, and the like can be mentioned. The melting point of such a natural wax is preferably 50°C or more, more preferably 60°C or more, even more preferably 70°C or more, and particularly preferably 75°C or more. As a raw material for the top coat layer, a chemically synthesized wax ester may be used, or a wax obtained by refining a natural wax to increase the purity of the wax ester may be used. These raw materials may be one kind or two or more kinds.

[0177] The ratio of the slip agent to the entire topcoat layer is preferably 5% by weight to 50% by weight, more preferably 10% by weight to 40% by weight. If the content of the slip agent is too low, the scratch resistance may be easily deteriorated. If the content of the slip agent is too high, the effect of improving the whitening resistance may be insufficient.

[0178] The topcoat layer may contain other slipping agents in addition to the wax ester. Examples of other slipping agents include various waxes other than wax esters, such as petroleum wax (paraffin wax, etc.), mineral wax (montan wax, etc.), higher fatty acids (cerotic acid, etc.), and neutral fats (palmitic acid triglyceride, etc.). In addition to the wax ester, silicone-based lubricants, fluorine-based lubricants, etc. may be contained. A preferred embodiment of the topcoat layer is one that does not substantially contain silicone-based lubricants or fluorine-based lubricants, and for example, the total content of the silicone-based lubricant and the fluorine-based lubricant is preferably 0.01% by weight or less of the entire topcoat layer, and more preferably below the detection limit.

[0179] The top coat layer may contain additives such as antistatic components, crosslinking agents, antioxidants, colorants (pigments, dyes, etc.), flow control agents (thixotropic agents, thickeners, etc.), film-forming aids, surfactants (defoamers, dispersants, etc.), and preservatives, as necessary.

[0180] <Antistatic component in top coat layer> A preferred embodiment of the topcoat layer contains an antistatic component. The antistatic component is a component that can prevent or suppress the static charge of the adhesive film. When the topcoat layer contains an antistatic component, the antistatic component can be, for example, an organic or inorganic conductive material, various antistatic agents, etc. Also, it is possible to use the antistatic agent that can be used in the above-mentioned antistatic layer.

[0181] Examples of organic conductive substances include cationic antistatic agents having cationic functional groups such as quaternary ammonium salts, pyridinium salts, primary amino groups, secondary amino groups, and tertiary amino groups; anionic antistatic agents having anionic functional groups such as sulfonates, sulfates, phosphonates, and phosphates; amphoteric antistatic agents such as alkylbetaines and their derivatives, imidazolines and their derivatives, and alanines and their derivatives; nonionic antistatic agents such as aminoalcohols and their derivatives, glycerin and its derivatives, and polyethylene glycols and its derivatives; ionic conductive polymers obtained by polymerizing or copolymerizing monomers having the above-mentioned cationic, anionic, and amphoteric ion conductive groups (e.g., quaternary ammonium bases); conductive polymers such as polythiophene, polyaniline, polypyrrole, polyethyleneimine, and allylamine-based polymers; and the like. Such antistatic agents may be used alone or in combination of two or more kinds.

[0182] Examples of inorganic conductive substances include tin oxide, antimony oxide, indium oxide, cadmium oxide, titanium oxide, zinc oxide, indium, tin, antimony, gold, silver, copper, aluminum, nickel, chromium, titanium, iron, cobalt, copper iodide, ITO (indium oxide / tin oxide), ATO (antimony oxide / tin oxide), etc. Only one type of such inorganic conductive substance may be used, or two or more types may be used.

[0183] Examples of the antistatic agent include cationic antistatic agents, anionic antistatic agents, amphoteric ion antistatic agents, nonionic antistatic agents, and ionic conductive polymers obtained by polymerizing or copolymerizing monomers having the above-mentioned cationic, anionic or amphoteric ion conductive groups.

[0184] When the top coat layer contains an antistatic component, the antistatic component preferably contains an organic conductive substance. As the organic conductive substance, various conductive polymers can be preferably used. With this configuration, it is possible to achieve both good antistatic properties and high scratch resistance.

[0185] Examples of conductive polymers include polythiophene, polyaniline, polypyrrole, polyethyleneimine, and allylamine polymers. Such conductive polymers may be used alone or in combination with other antistatic components (inorganic conductive substances, antistatic agents, etc.).

[0186] The amount of the conductive polymer used is preferably 1 to 100 parts by weight, more preferably 2 to 70 parts by weight, and even more preferably 3 to 50 parts by weight, relative to 100 parts by weight of the binder contained in the top coat layer. If the amount of the conductive polymer used is too small, the antistatic effect may be reduced. If the amount of the conductive polymer used is too large, the compatibility of the conductive polymer in the top coat layer may be insufficient, and the appearance quality of the top coat layer may be reduced or the solvent resistance may be reduced.

[0187] The conductive polymer is preferably polythiophene or polyaniline. The polythiophene has a weight average molecular weight Mw of preferably 40×10 4 More preferably, it is 30×10 or less. 4 The polyaniline preferably has a weight average molecular weight Mw of 50×10 or less in terms of polystyrene. 4 More preferably, it is 30×10 or less. 4 The weight average molecular weight Mw of the conductive polymer in terms of polystyrene is preferably 0.1×10 4 More preferably, it is 0.5×10 4 That is all. In this specification, polythiophene refers to a polymer of unsubstituted or substituted thiophene. An example of the substituted thiophene polymer is poly(3,4-ethylenedioxythiophene).

[0188] When a method for forming a topcoat layer is adopted in which a coating material for forming a topcoat layer is applied to a substrate and dried or cured, the conductive polymer used for preparing the coating material is preferably a conductive polymer dissolved or dispersed in water (a conductive polymer aqueous solution). Such a conductive polymer aqueous solution can be prepared, for example, by dissolving or dispersing a conductive polymer having a hydrophilic functional group (a conductive polymer that can be synthesized by a method such as copolymerizing a monomer having a hydrophilic functional group in the molecule) in water. Examples of the hydrophilic functional group include a sulfo group, an amino group, an amide group, an imino group, a hydroxyl group, a mercapto group, a hydrazino group, a carboxyl group, a quaternary ammonium group, a sulfate ester group (-O-SO3H), and a phosphate ester group (for example, -O-PO(OH)2). Such a hydrophilic functional group may form a salt. Examples of commercially available polythiophene aqueous solutions include the "Denatron" series manufactured by Nagase Chemtec Corporation. An example of a commercially available aqueous solution of polyaniline sulfonic acid is "aqua-PASS" manufactured by Mitsubishi Rayon Co., Ltd.

[0189] In preparing the coating material, a polythiophene aqueous solution is preferably used. The polythiophene aqueous solution is preferably a polythiophene aqueous solution containing polystyrene sulfonate (PSS) (for example, a form in which PSS is added to polythiophene as a dopant). Such a polythiophene aqueous solution may contain polythiophene:PSS in a mass ratio of preferably 1:1 to 1:10. The total content of polythiophene and PSS in such a polythiophene aqueous solution is preferably 1 mass% to 5 wt%. Examples of commercially available products of such polythiophene aqueous solutions include the product name "Baytron" of HC Stark. In addition, when using a polythiophene aqueous solution containing PSS as described above, the total amount of polythiophene and PSS is preferably 5 to 200 parts by weight, more preferably 10 to 100 parts by weight, and even more preferably 25 to 70 parts by weight, relative to 100 parts by weight of the binder.

[0190] The topcoat layer may contain both the conductive polymer and one or more other antistatic components (such as an organic conductive substance other than the conductive polymer, an inorganic conductive substance, or an antistatic agent) as necessary. Preferably, the topcoat layer does not substantially contain any antistatic component other than the conductive polymer. In other words, it is preferable that the antistatic component contained in the topcoat layer is substantially composed of only the conductive polymer.

[0191] <Crosslinking agent> The topcoat layer preferably contains a crosslinking agent. The crosslinking agent may be appropriately selected from melamine-based crosslinking agents, isocyanate-based crosslinking agents, epoxy-based crosslinking agents, and other crosslinking agents used in general resin crosslinking. By using such a crosslinking agent, at least one of the following effects may be achieved: improved scratch resistance, improved solvent resistance, improved print adhesion, and reduced friction coefficient (i.e., improved slipperiness). Preferably, the crosslinking agent contains a melamine-based crosslinking agent. The topcoat layer may be substantially composed of a melamine-based crosslinking agent (melamine-based resin) (i.e., substantially does not contain any crosslinking agent other than the melamine-based crosslinking agent).

[0192] A preferred embodiment of the topcoat layer is that when the material of the base layer is at least one selected from polyimide and polyether ether ketone, the topcoat layer contains a binder containing a urethane resin and an antistatic component. In this way, by adopting a binder containing a urethane resin as the binder of the antistatic component of the topcoat layer, the coating formability of the topcoat layer on the surface of the base layer made of at least one material selected from polyimide and polyether ether ketone becomes excellent, and the appearance can be good and excellent antistatic properties can be exhibited.

[0193] As the binder of the antistatic component of the topcoat layer, a binder containing polyester resin is often preferred, but for a specific base layer in which the material of the base layer is at least one selected from polyimide and polyether ether ketone, the affinity of the binder containing polyester resin may be low, and there is a risk that the appearance after the topcoat layer is coated and formed may be poor or excellent antistatic properties may not be exhibited. As described above, when the material of the base layer is at least one selected from polyimide and polyether ether ketone, if the topcoat layer contains a binder containing a urethane resin and an antistatic component, the coating formability of the topcoat layer on the surface of the base layer becomes excellent, the appearance can be good, and excellent antistatic properties can be exhibited.

[0194] <Formation of topcoat layer> The topcoat layer can be suitably formed by a method including applying a liquid composition (a coating material for forming a topcoat layer) in which the resin component and additives used as necessary are dispersed or dissolved in an appropriate solvent to a substrate. For example, a method of applying the coating material to the first surface of the substrate, drying, and performing a curing treatment (heat treatment, ultraviolet treatment, etc.) as necessary can be preferably adopted. The NV (non-volatile content) of the coating material is preferably 5 wt % or less, more preferably 0.05 wt % to 5 wt %, further preferably 0.05 wt % to 1 wt %, and particularly preferably 0.10 wt % to 1 wt %. When a topcoat layer with a small thickness is formed, the NV of the coating material is preferably 0.05 wt % to 0.50 wt %, more preferably 0.10 wt % to 0.30 wt %. By using a coating material with a low NV in this way, a more uniform topcoat layer can be formed.

[0195] The solvent constituting the coating material for forming the topcoat layer is preferably one that can stably dissolve or disperse the topcoat layer forming components. Such a solvent can be an organic solvent, water, or a mixed solvent thereof. Examples of the organic solvent include at least one selected from esters such as ethyl acetate; ketones such as methyl ethyl ketone, acetone, and cyclohexanone; cyclic ethers such as tetrahydrofuran (THF) and dioxane; aliphatic or alicyclic hydrocarbons such as n-hexane and cyclohexane; aromatic hydrocarbons such as toluene and xylene; aliphatic or alicyclic alcohols such as methanol, ethanol, n-propanol, isopropanol, and cyclohexanol; glycol ethers such as alkylene glycol monoalkyl ethers (e.g., ethylene glycol monomethyl ether, ethylene glycol monoethyl ether), and dialkylene glycol monoalkyl ethers. Preferably, the solvent constituting the coating material for forming the topcoat layer is water or a mixed solvent mainly composed of water (e.g., a mixed solvent of water and ethanol).

[0196] <Properties of the topcoat layer> The thickness of the topcoat layer is preferably 3 nm to 500 nm, more preferably 3 nm to 100 nm, and further preferably 3 nm to 60 nm. If the thickness of the topcoat layer is too large, the transparency (light transmittance) of the adhesive film may be easily reduced. If the thickness of the topcoat layer is too small, it may be difficult to form the topcoat layer uniformly, for example, the thickness of the topcoat layer may vary greatly from place to place, and therefore, the appearance of the adhesive film may be easily uneven.

[0197] The thickness of the topcoat layer can be grasped by observing the cross section of the topcoat layer with a transmission electron microscope (TEM). For example, a target sample (such as a substrate on which a topcoat layer is formed or an adhesive film having a substrate) is subjected to a heavy metal staining process in order to clarify the topcoat layer, and then embedded in a resin. The result obtained by performing TEM observation of the cross section of the sample by ultra-thin sectioning can be preferably used as the thickness of the topcoat layer. For example, a TEM (model number "H-7650") manufactured by Hitachi can be used as the TEM. In the examples described later, a cross-sectional image obtained under conditions of an acceleration voltage of 100 kV and a magnification of 60,000 times is subjected to a binarization process, and then the thickness of the topcoat layer (average thickness within the field of view) is actually measured by dividing the cross-sectional area of ​​the topcoat by the sample length within the field of view. Note that if the topcoat layer can be observed sufficiently clearly without heavy metal staining, the heavy metal staining process may be omitted. Alternatively, the thickness of the topcoat layer may be determined by creating a calibration curve and performing calculations to correlate the thickness determined by TEM with the results of detection using various thickness detection devices (e.g., surface roughness meter, interference thickness meter, infrared spectrometer, various X-ray diffraction devices, etc.).

[0198] The surface resistivity measured on the surface of the topcoat layer is preferably 10 12 Ω or less, and more preferably 10 4 Ω~10 12 Ω, and more preferably 10 4 Ω~10 11 Ω, and particularly preferably 5×10 4 Ω~10 10 Ω, and most preferably 10 4 Ω~10 9 Ω. An adhesive film exhibiting such a surface resistivity can be suitably used as an adhesive film used in the processing or transport process of products that are sensitive to static electricity, such as liquid crystal cells and semiconductor devices. The surface resistivity value can be calculated from the surface resistance value measured under an atmosphere of 23°C and 50% RH using a commercially available insulation resistance measuring device.

[0199] The coefficient of friction of the topcoat layer is preferably 0.4 or less. If the topcoat layer has such a low coefficient of friction, when a load (a load that causes scratches) is applied to the topcoat layer, the load is deflected along the surface of the topcoat layer, and the frictional force due to the load can be reduced. This makes it difficult for the topcoat layer to undergo cohesive failure (a damage mode in which the topcoat layer is broken inside) or interfacial failure (a damage mode in which the topcoat layer is peeled off from the back surface of the substrate). Therefore, it is possible to more effectively prevent the occurrence of scratches on the adhesive film. The lower limit of the coefficient of friction is preferably 0.1 or more, more preferably 0.15 or more, taking into consideration the balance with other characteristics (for example, appearance quality, printability, etc.). For example, the value obtained by rubbing the surface of the topcoat layer with a vertical load of 40 mN under a measurement environment of 23°C and 50% RH can be adopted as the coefficient of friction. The amount of the slipping agent used may be set so as to realize a preferred coefficient of friction. In order to adjust the coefficient of friction, it is also effective to increase the crosslink density of the topcoat layer by, for example, adding a crosslinking agent or adjusting the film formation conditions.

[0200] The adhesive film preferably has a property that the back surface (surface of the topcoat layer) can be easily printed with oil-based ink (for example, using an oil-based marking pen). Such an adhesive film is suitable for marking and displaying the identification number of the adherend to be protected on the adhesive film during the processing and transportation of the adherend (for example, optical parts) performed with the adhesive film attached. Therefore, a surface protection film that is excellent in printability in addition to appearance quality is preferable. For example, it is preferable that the solvent is alcohol-based and has high printability against oil-based ink containing pigment. In addition, it is preferable that the printed ink is not easily removed by rubbing or transfer (i.e., excellent print adhesion). It is preferable that the adhesive film has solvent resistance to such an extent that the appearance does not change noticeably even if the print is wiped off with alcohol (for example, ethyl alcohol) when the print is corrected or erased.

[0201] The topcoat layer preferably contains a wax ester as a slipping agent, so that sufficient slip properties (e.g., the above-mentioned preferred friction coefficient) can be achieved even in an embodiment in which no further release treatment is applied to the surface of the topcoat layer (e.g., a treatment in which any suitable release agent such as a silicone-based release agent or a long-chain alkyl-based release agent is applied and dried). Such an embodiment in which no further release treatment is applied to the surface of the topcoat layer is preferable in that whitening caused by the release agent (e.g., whitening caused by storage under heated and humidified conditions) can be prevented in advance. It is also advantageous in terms of solvent resistance.

[0202] The adhesive film may be implemented in an embodiment that further includes other layers in addition to the substrate, the adhesive layer, and the topcoat layer. Examples of the arrangement of such "other layers" include between the first surface (back surface) of the substrate and the topcoat layer, and between the second surface (front surface) of the substrate and the adhesive layer. The layer arranged between the back surface of the substrate and the topcoat layer may be, for example, a layer containing an antistatic component (antistatic layer). The layer arranged between the front surface of the substrate and the adhesive layer may be, for example, an undercoat layer (anchor layer) that enhances the anchoring property of the adhesive layer to the second surface, an antistatic layer, etc. The adhesive film may be configured such that an antistatic layer is arranged on the front surface of the substrate, an anchor layer is arranged on the antistatic layer, and an adhesive layer is arranged on the anchor layer.

[0203] <<Foldable and rollable devices>> The adhesive film of the present invention is excellent in flexibility and transparency, and therefore can be suitably provided, for example, in bendable devices (devices that can be bent) having movable bending parts, foldable devices (devices that can be folded), and rollable devices (devices that can be rolled up). The adhesive film of the present invention is particularly excellent in flexibility and transparency, and therefore can be suitably provided in foldable devices (devices that can be folded) and rollable devices (devices that can be rolled up), which have been more difficult to apply up until now.

[0204] The foldable device of the present invention includes the pressure-sensitive adhesive film of the present invention. The foldable device of the present invention may include any other appropriate member as long as it includes the pressure-sensitive adhesive film of the present invention.

[0205] The rollable device of the present invention comprises the pressure-sensitive adhesive film of the present invention. The rollable device of the present invention may comprise any other appropriate member, so long as it comprises the pressure-sensitive adhesive film of the present invention.

[0206] FIG. 1 is a schematic cross-sectional view showing one embodiment of the foldable device of the present invention as a representative example of one use form of the adhesive film of the present invention. In FIG. 1, the foldable device 1000 of the present invention comprises a cover film 10, an adhesive layer 20, a polarizing plate 30, an adhesive layer 40, a touch sensor 50, an adhesive layer 60, an OLED 70, and an adhesive film 100 of the present invention. In FIG. 1, the adhesive film 100 of the present invention is composed of an adhesive layer 80 and a base layer 90. The adhesive layer 20, the adhesive layer 40, and the adhesive layer 60 may be an adhesive layer containing an adhesive of the same composition as the adhesive layer 80 constituting the adhesive film 100 of the present invention, or may be an adhesive layer containing an adhesive of a different composition.

[0207] The adhesive film of the present invention is excellent in flexibility and transparency, and therefore can be suitably provided on the back surface (opposite the display surface) of a bendable device (device that can be bent), a foldable device (device that can be folded), or a rollable device (device that can be rolled up) having a movable bending part. Figure 1 shows the adhesive film provided on the back surface (opposite the display surface) of a foldable device (device that can be folded). EXAMPLES

[0208] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited thereto. In the following description, "parts" and "%" are by weight unless otherwise specified.

[0209] <tanδ> Measurements were performed in tension mode using a viscoelasticity measuring device "RSA-G2" (manufactured by TA Instruments Japan Co., Ltd.) with a sample size of 5 mm wide x 15 mm distance and an axial force of 100 g. In the strain sweep (oscillation amplitude) mode, the frequency was set to 1 Hz, the measurement temperature was set to 90°C, the immersion time was set to 60 seconds, and the measurement range of strain was set to 0.01% to 1.0%, and measurements were performed at the strains in between. The tan δ values ​​at each strain were graphed, and the tan δ values ​​at 0.1% strain and 0.7% strain were obtained from the graph. Regarding the thickness, the stiffness of the substrate was large in both the storage modulus and loss modulus compared to the adhesive film, and the influence of the adhesive was negligible, so the measurement was performed by inputting only the thickness of the substrate excluding the thickness of the adhesive. Tan δ was calculated using the following formula. tan δ = loss modulus / storage modulus

[0210] <Bending test> The adhesive film in a flat state was bent at 6Φ with the adhesive layer surface facing outward as shown in Fig. 2, and fixed in a manner that sandwiched it between the silicone-treated surface of a silicone-treated separator, and held at 90°C for 48 hours. The bending was then released, and the film was left at 23°C and 50% RH for 24 hours, after which the angle of the bent film was measured. The angle was 180° when the film had completely returned to its original state, and 0° when the film maintained the bent state at the initial fixation.

[0211] <Peeling evaluation> An adhesive film was attached to a 50 μm thick PET film (Toray, S10), folded so that the adhesive film was on the inside as shown in Figure 3, and held at 90°C for 48 hours, after which the fixed state was released and peeling of the adhesive film from the PET film was visually observed. Evaluation was performed according to the following criteria. ○: No peeling from the PET film was observed. ×: Peeling from the PET film was observed.

[0212] <Haze and total light transmittance measurements> Using a haze meter HM-150 (manufactured by Murakami Color Research Laboratory Co., Ltd.), the haze was calculated according to JIS-K-7136 as follows: haze (%) = (Td / Tt) x 100 (Td: diffuse transmittance, Tt: total light transmittance). The total light transmittance was measured according to JIS-K-7316.

[0213] <Young's modulus> The sample pieces were cut into strips with a width of 10 mm, and the strip-shaped sample pieces were pulled in the longitudinal direction with a chuck distance of 100 mm in a universal tension and compression testing machine (Tensilon) in a temperature environment of 25°C, and Young's modulus was obtained from the obtained SS (Strain-Strength) curve. The measurement conditions were a tensile speed of 200 mm / min and a chuck distance of 50 mm. The Young's modulus was obtained from the SS curve by creating a graph of the SS curve, drawing a tangent (linear equation) to the graph in the displacement range of 1 mm to 2 mm, and obtaining the Young's modulus from the slope of the tangent.

[0214] <Adhesive strength> The adhesive film was cut to a width of 25 mm and a length of 150 mm to prepare a sample for evaluation. In an atmosphere of 23°C temperature and 50% RH humidity, the adhesive layer surface of the evaluation sample was attached to a glass plate (manufactured by Matsunami Glass Industry Co., Ltd., product name: Microslide Glass S) with a 2.0 kg roller going back and forth once. After curing for 30 minutes in an atmosphere of 23°C temperature and 50% RH humidity, the sample was peeled off at a peel angle of 180° and a pulling speed of 300 mm / min using a universal tensile tester (manufactured by Minebea Co., Ltd., product name: TCM-1kNB) to measure the adhesive strength.

[0215] <Applicability> The number of circular irregularities that occurred on the applied topcoat layer (containing an antistatic layer) was counted. Two A4 size sheets were prepared and the average number was calculated. A score of 2 or less was judged as good, and 3 or more was judged as bad. The circular uneven areas were areas where the thickness of the topcoat layer was thin, which was a defect in terms of appearance, and those where the antistatic agent was repelled and could not be applied at all were judged as "repellency."

[0216] <Surface resistance value (for Example 8)> In Example 8, the layer on which the antistatic treatment layer was formed was measured at a voltage of 10 V using a volume resistivity meter Model 152-1 152P-2P probe (manufactured by Trek Japan Co., Ltd.).

[0217] <Surface resistivity (for Examples 9 to 17 and Comparative Examples 6 to 9)> In Examples 9 to 17 and Comparative Examples 6 to 9, a resistivity meter (Mitsubishi Chemical Analytical's "Hiresta UP MCP-HT450 type") was used to contact a URS probe with the non-adhesive layer side of the adhesive film, and the surface resistivity was measured under the conditions of an applied voltage of 100 V and a voltage application time of 10 seconds.

[0218] [Production Example 1]: Preparation of adhesive composition A 2-Ethylhexyl acrylate (2EHA): 63 parts by weight, N-vinyl-2-pyrrolidone (NVP): 15 parts by weight, methyl methacrylate (MMA): 9 parts by weight, 2-hydroxyethyl acrylate (HEA): 13 parts by weight, 2,2'-azobisisobutyronitrile: 0.2 parts by weight as a polymerization initiator, and ethyl acetate: 133 parts by weight as a polymerization solvent were charged into a separable flask and stirred for 1 hour while introducing nitrogen gas. After removing oxygen from the polymerization system in this way, the temperature was raised to 65°C and reacted for 10 hours, and then ethyl acetate was added to obtain a solution of acrylic polymer (a) with a solid content concentration of 30% by weight. Next, an isocyanate-based crosslinking agent (product name "Takenate D110N", manufactured by Mitsui Chemicals, Inc.) was added to the solution of the acrylic polymer (a1) in an amount of 1 part by weight in terms of solid content per 100 parts by weight of the acrylic polymer (a) (solid content) to prepare a pressure-sensitive adhesive composition A.

[0219] [Production Example 2]: Preparation of Adhesive Composition B In a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser, 96.2 parts by weight of 2-ethylhexyl acrylate (2EHA), 3.8 parts by weight of hydroxyethyl acrylate (HEA), 0.2 parts by weight of 2,2'-azobisisobutyronitrile as a polymerization initiator, and 150 parts by weight of ethyl acetate were charged, and nitrogen gas was introduced while gently stirring. The liquid temperature in the flask was kept at around 60°C, and a polymerization reaction was carried out for 6 hours to prepare a solution (40% by weight) of acrylic polymer (b). The weight average molecular weight of the acrylic polymer (b) was 540,000. Next, a solution (40% by weight) of the acrylic polymer (b) was diluted to 25% by weight with ethyl acetate, and 4 parts by weight (4 parts by weight of solids) of an isocyanurate of hexamethylene diisocyanate (Tosoh Corporation, Coronate HX), which is a trifunctional isocyanate compound, as a crosslinking agent, 2 parts by weight (0.02 parts by weight of solids) of dioctyltin dilaurate (Tokyo Fine Chemical Co., Ltd., Envirizer OL-1, 1% by weight ethyl acetate solution) as a crosslinking catalyst, and 3 parts by weight of acetylacetone were added to 400 parts by weight (100 parts by weight of solids) of this solution, and the mixture was stirred to prepare adhesive composition B.

[0220] [Example 1] A commercially available release liner (Diafoil MRF-38, Mitsubishi Plastics, Inc.) was prepared. Adhesive composition A was applied to one surface (release surface) of the release liner so that the thickness after drying would be 25 μm, and dried at 130° C. for 3 minutes. In this way, an adhesive layer having a thickness of 25 μm and composed of acrylic adhesive A corresponding to adhesive composition A was formed on the release surface of the release liner. A polyimide-based substrate (trade name "Kapton", manufactured by Toray DuPont Co., Ltd.) having a thickness of 50 μm was prepared as the substrate layer. The adhesive layer formed on the release liner was attached to one side of this substrate layer. The release liner was left on the adhesive layer as it was and used to protect the surface of the adhesive layer (adhesive layer surface). The obtained structure was passed once through a laminator (0.3 MPa, speed 0.5 m / min) at 80° C., and then aged in an oven at 50° C. for one day. In this way, an adhesive film (1) was obtained. The results are shown in Table 1.

[0221] [Example 2] An adhesive film (2) was obtained in the same manner as in Example 1, except that a polyimide-based substrate (product name "Upilex-50S", manufactured by Ube Industries, Ltd.) having a thickness of 50 μm was used as the substrate layer. The results are shown in Table 1.

[0222] [Example 3] An adhesive film (3) was obtained in the same manner as in Example 1, except that a polyimide-based substrate (product name "Pixio BP", manufactured by Kaneka Corporation) having a thickness of 50 μm was used as the substrate layer. The results are shown in Table 1.

[0223] [Example 4] An adhesive film (4) was obtained in the same manner as in Example 1, except that a polyimide-based substrate (product name "UPILEX-50RN", manufactured by Ube Industries, Ltd.) having a thickness of 50 μm was used as the substrate layer. The results are shown in Table 1.

[0224] [Example 5] The same procedure as in Example 1 was carried out except that a 50 μm-thick polyether ether ketone (PEEK)-based substrate (product name "Shin-Etsu Sepla Film", non-stretch film-forming, highly crystalline, manufactured by Shin-Etsu Polymer Co., Ltd.) was used as the substrate layer, to obtain an adhesive film (5). The results are shown in Table 1.

[0225] [Example 6] An adhesive film (6) was obtained in the same manner as in Example 1, except that a polyimide-based substrate (product name "Neoprim S100", manufactured by Mitsubishi Gas Chemical Company, Inc.) having a thickness of 50 μm was used as the substrate layer. The results are shown in Table 1.

[0226] [Example 7] An adhesive film (7) was obtained in the same manner as in Example 1, except that a polyether ether ketone (PEEK)-based substrate (product name "Expeak", manufactured by Kurabo Industries, Ltd.) having a thickness of 25 μm was used as the substrate layer. The results are shown in Table 1.

[0227] [Comparative Example 1] An adhesive film (C1) was obtained in the same manner as in Example 1, except that a polyester-based substrate (product name "Lumirror S10", manufactured by Toray Industries, Inc.) having a thickness of 25 μm was used as the substrate layer. The results are shown in Table 1.

[0228] [Comparative Example 2] An adhesive film (C2) was obtained in the same manner as in Example 1, except that a polyester-based substrate (product name "Lumirror S10", manufactured by Toray Industries, Inc.) having a thickness of 50 μm was used as the substrate layer. The results are shown in Table 1.

[0229] [Comparative Example 3] The same procedure as in Example 1 was carried out except that adhesive composition B was used instead of adhesive composition A, and a 50 μm-thick polyester-based substrate (product name "Lumirror S10", manufactured by Toray) was used as the substrate layer, to obtain an adhesive film (C3). The results are shown in Table 1.

[0230] [Comparative Example 4] The same procedure was carried out as in Example 6, except that adhesive composition B was used instead of adhesive composition A, to obtain an adhesive film (C4). The results are shown in Table 1.

[0231] [Comparative Example 5] The same procedure was carried out as in Example 7, except that adhesive composition B was used instead of adhesive composition A, to obtain an adhesive film (C5). The results are shown in Table 1.

[0232] [Table 1]

[0233] [Production Example 3]: Preparation of antistatic polyimide film A An antistatic agent solution was prepared by diluting 10 parts by weight of an antistatic agent (Solvex, Microsolver RMd-142, mainly composed of tin oxide and polyester resin) with a mixed solvent consisting of 30 parts by weight of water and 70 parts by weight of methanol. The obtained antistatic agent solution was applied to a 50 μm-thick polyimide substrate (trade name "Kapton", Toray DuPont Co., Ltd.) using a Mayer bar, and the solvent was removed by drying at 130°C for 1 minute to form an antistatic layer (thickness: 0.2 μm), and antistatic treated polyimide film A was produced.

[0234] [Example 8] An adhesive film (8) was obtained in the same manner as in Example 1, except that antistatic treated polyimide film A was used as the substrate. The surface resistance was 5×10 6 It was Omega.

[0235] [Production Example 4]: Preparation of topcoat layer-forming polyimide film B <Preparation of Coating Material B> A dispersion containing 25% by weight of a polyester resin (binder) was prepared (product of Toyobo Co., Ltd., trade name "Binalol MD-1480" (aqueous dispersion of saturated copolymerized polyester resin); hereinafter also referred to as "binder dispersion"). As a slipping agent, an aqueous dispersion of carnauba wax (manufactured by Nippon Wax Co., Ltd., product name "Refined Carnauba Wax No. 2 Powder") (hereinafter also referred to as "slipping agent dispersion") was prepared. Furthermore, an aqueous solution containing 0.5% by weight of poly(3,4-dioxythiophene) (PEDOT) and 0.8% by weight of polystyrene sulfonate (number average molecular weight 150,000) (PSS) (HC Stark product, product name "Baytron P"; hereinafter also referred to as "aqueous conductive polymer solution") was prepared as a conductive polymer. 100 parts by weight of the binder dispersion in terms of solid content, 30 parts by weight of the slip agent dispersion in terms of solid content, 50 parts by weight of the conductive polymer aqueous solution in terms of solid content, and 7 parts by weight of the melamine-based crosslinking agent were added to a mixed solvent of water and ethanol (weight ratio 50:50), and the mixture was stirred for about 20 minutes to thoroughly mix. In this way, a coating material B with a NV of about 0.15% by weight was prepared. <Preparation of topcoat layer-forming polyimide film B> The coating material B was applied to a 50 μm-thick polyimide substrate (trade name "Kapton", manufactured by DuPont-Toray Co., Ltd.) using a bar coater, and then dried by heating at 130° C. for 2 minutes. In this manner, a substrate (topcoat layer-formed polyimide film B) having a transparent topcoat layer of 10 nm thickness on one side of the polyimide substrate was produced.

[0236] [Production Example 5]: Preparation of topcoat layer-forming polyimide film C <Preparation of coating material C> As a binder, an aqueous solution containing 25% by weight of a polyester urethane resin composed of 25 mol % ethylene glycol, 25 mol % neopentylin glycol, 30 mol % terephthalic acid, 10 mol % adipic acid, and 10 mol % tolylene diisocyanate (hereinafter also referred to as "binder dispersion") was prepared. As a slipping agent, an aqueous dispersion of carnauba wax (manufactured by Nippon Wax Co., Ltd., product name "Refined Carnauba Wax No. 2 Powder") (hereinafter also referred to as "slipping agent dispersion") was prepared. Furthermore, an aqueous solution containing 0.5% by weight of poly(3,4-dioxythiophene) (PEDOT) and 0.8% by weight of polystyrene sulfonate (number average molecular weight 150,000) (PSS) (HC Stark product, product name "Baytron P"; hereinafter also referred to as "aqueous conductive polymer solution") was prepared as a conductive polymer. Furthermore, an aqueous solution containing 10% by weight of polyethylene glycol (PEG) alkyl ether and 10% by weight of polyvinyl alcohol was prepared as a dispersant. 40 parts by weight of the binder dispersion in terms of solid content, 5 parts by weight of the slip agent dispersion in terms of solid content, 8 parts by weight of the conductive polymer aqueous solution in terms of solid content, 40 parts by weight of the dispersant, and 7 parts by weight of the melamine-based crosslinking agent were added to a mixed solvent of water and ethanol (weight ratio 50:50), and the mixture was stirred for about 20 minutes to thoroughly mix. In this way, a coating material C with a NV of about 0.30% by weight was prepared. <Preparation of topcoat layer-forming polyimide film C> The coating material C was applied to a 50 μm-thick polyimide substrate (trade name "Kapton", manufactured by DuPont-Toray Co., Ltd.) using a bar coater, and then dried by heating at 130° C. for 2 minutes. In this manner, a substrate (topcoat layer-formed polyimide film C) having a transparent topcoat layer of 50 nm on one side of the polyimide substrate was produced.

[0237] [Example 9] An adhesive film (9) was obtained in the same manner as in Example 1, except that the topcoat layer-forming polyimide film B was used as the substrate. The results are shown in Table 2.

[0238] [Example 10] An adhesive film (10) was obtained in the same manner as in Example 2, except that the topcoat layer-forming polyimide film B was used as the substrate. The results are shown in Table 2.

[0239] [Example 11] An adhesive film (11) was obtained in the same manner as in Example 4, except that the topcoat layer-forming polyimide film B was used as the substrate. The results are shown in Table 2.

[0240] [Example 12] An adhesive film (12) was obtained in the same manner as in Example 7, except that the topcoat layer-forming polyimide film B was used as the substrate. The results are shown in Table 2.

[0241] [Example 13] An adhesive film (13) was obtained in the same manner as in Example 1, except that the topcoat layer-forming polyimide film C was used as the substrate. The results are shown in Table 2.

[0242] [Example 14] An adhesive film (14) was obtained in the same manner as in Example 2, except that the topcoat layer-forming polyimide film C was used as the substrate. The results are shown in Table 2.

[0243] [Example 15] An adhesive film (15) was obtained in the same manner as in Example 3, except that the topcoat layer-forming polyimide film C was used as the substrate. The results are shown in Table 2.

[0244] [Example 16] An adhesive film (16) was obtained in the same manner as in Example 4, except that the topcoat layer-forming polyimide film C was used as the substrate. The results are shown in Table 2.

[0245] [Example 17] An adhesive film (17) was obtained in the same manner as in Example 7, except that the topcoat layer-forming polyimide film C was used as the substrate. The results are shown in Table 2.

[0246] [Comparative Example 6] An adhesive film (C6) was obtained in the same manner as in Comparative Example 1, except that the topcoat layer-forming polyimide film B was used as the substrate. The results are shown in Table 2.

[0247] [Comparative Example 7] An adhesive film (C7) was obtained in the same manner as in Comparative Example 2, except that the topcoat layer-forming polyimide film B was used as the substrate. The results are shown in Table 2.

[0248] [Comparative Example 8] An adhesive film (C8) was obtained in the same manner as in Comparative Example 1, except that the topcoat layer-forming polyimide film C was used as the substrate. The results are shown in Table 2.

[0249] [Comparative Example 9] An adhesive film (C9) was obtained in the same manner as in Comparative Example 2, except that the topcoat layer-forming polyimide film C was used as the substrate. The results are shown in Table 2.

[0250] [Table 2] [Industrial Applicability]

[0251] The adhesive film of the present invention has excellent flexibility and transparency, and can therefore be suitably provided in, for example, bendable devices having movable bending parts, foldable devices, and rollable devices. [Explanation of symbols]

[0252] 1000 Foldable Devices 100 Adhesive Film 10 Cover film 20 Adhesive layer 30 Polarizing plate 40 Adhesive layer 50 Touch Sensor 60 Adhesive layer 70 OLED 80 Adhesive layer 90 Base material layer 1 6Φ glass rod 2 Silicone-treated separator 3 Adhesive layer 4 Fixed Glass 5. PET film

Claims

1. A pressure-sensitive adhesive film having a base layer and a pressure-sensitive adhesive layer, tan δ (0.7%) at a strain of 0.7% measured in a tensile mode of a viscoelasticity measuring device is 0.1 or less; Adhesive film.

2. A pressure-sensitive adhesive film having a base layer and a pressure-sensitive adhesive layer, The difference between tan δ (0.7%) at a strain of 0.7% and tan δ (0.1%) at a strain of 0.1% measured in a tensile mode of a viscoelasticity measuring device (tan δ (0.7%) - tan δ (0.1%)) is 0.05 or less. Adhesive film.

3. The pressure-sensitive adhesive film according to claim 1 or 2, which is bent at 6Φ and held at 90 ° C for 48 hours, then released and left at 23 ° C and 50% RH for 24 hours, has a bending angle of 60 degrees to 180 degrees.

4. The pressure-sensitive adhesive film according to claim 1 , further comprising a topcoat layer on a surface of the base layer opposite to the surface having the pressure-sensitive adhesive layer.

5. The pressure-sensitive adhesive film according to claim 4 , wherein the top coat layer contains a binder containing at least one selected from a polyester resin and a urethane resin.

6. The pressure-sensitive adhesive film according to claim 5 , wherein the binder comprises a urethane resin.

7. The pressure-sensitive adhesive film according to claim 4 , wherein the top coat layer contains an antistatic component.

8. The Young's modulus of the base layer at 23° C. is 6.0×10 7 The pressure-sensitive adhesive film according to claim 1 , having a modulus of elasticity of 1 Pa or more.

9. The pressure-sensitive adhesive film according to claim 8 , wherein the material of the base layer is at least one selected from polyimide and polyether ether ketone.

10. 4. The pressure-sensitive adhesive film according to claim 1, further comprising a topcoat layer on a surface of the base layer opposite to the surface having the pressure-sensitive adhesive layer, the topcoat layer containing a binder containing a urethane resin and an antistatic component, and the material of the base layer is at least one selected from polyimide and polyether ether ketone.

11. The pressure-sensitive adhesive film according to any one of claims 1 to 10, having a total light transmittance of 20% or more.

12. The pressure-sensitive adhesive film according to claim 1 , having a haze of 15% or less.

13. 13. The pressure-sensitive adhesive film according to claim 1, wherein the pressure-sensitive adhesive layer has an adhesive strength to a stainless steel plate of 1 N / 25 mm or more at 23°C, a tensile speed of 300 mm / min, and a 180° peel.

14. The pressure-sensitive adhesive film according to claim 1 , wherein the pressure-sensitive adhesive layer comprises an acrylic pressure-sensitive adhesive.

15. The adhesive film according to claim 1 , which is attached to a foldable member.

16. The adhesive film according to claim 15 , wherein the foldable member is an OLED.

17. The adhesive film according to claim 1 , which is attached to a rollable member.

18. The adhesive film of claim 17 , wherein the rollable member is an OLED.

19. A foldable device comprising the adhesive film according to any one of claims 1 to 14.

20. A rollable device comprising the adhesive film according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Optical recording and reproducing unit

    JP1981000039A

  • Alkailine zinc storage battery

    JP1988076271A