Molding material and molding
A molding material with a thermoplastic resin, antistatic agent, ultraviolet absorber, and antioxidant addresses the deterioration of antistatic properties and weather resistance in synthetic resin slides, ensuring effective static charge dissipation and durability outdoors.
Patent Information
- Application Number
- JP2024139915
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-07-29
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Synthetic resin slides installed outdoors face issues with deteriorating antistatic properties and weather resistance due to ultraviolet rays, leading to ineffective static charge dissipation and material degradation.
A molding material comprising a thermoplastic resin, an antistatic agent, an ultraviolet absorber, a light stabilizer with a molecular weight of 500 or more, and an antioxidant is used to create a molded article that retains these additives, enhancing antistatic properties and weather resistance.
The molded article exhibits excellent antistatic properties and weather resistance, maintaining performance even when exposed to outdoor conditions.
Smart Images

Figure 2024159896000001 
Figure 2024159896000002 
Figure 2024159896000003
Abstract
Description
[Technical field]
[0001] The present disclosure generally relates to molding materials and molded articles. More specifically, the present disclosure relates to molding materials containing thermoplastic resins and molded articles using the molding materials. [Background technology]
[0002] Patent Document 1 discloses a slide made of synthetic resin. This slide includes a slide body, a step body, side plates, a contact plate, and a nut. The slide body, the step body, the side plates, the contact plate, and the nut are made of synthetic resin. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Utility Model Application Publication No. 01-006990 Summary of the Invention [Problem to be solved by the invention]
[0004] A slide made of synthetic resin as described in Patent Document 1 has a problem in that static electricity generated by friction with the human body is unlikely to leak. Therefore, the addition of an antistatic agent to the synthetic resin from which the slide is made has been considered.
[0005] On the other hand, synthetic resin slides are sometimes installed not only indoors but also outdoors. In this case, the inventors have found that the following problem occurs. That is, when a synthetic resin slide containing an antistatic agent is installed outdoors, the physical performance (particularly antistatic properties and weather resistance) of the slide is likely to be deteriorated by ultraviolet rays contained in sunlight.
[0006] An object of the present disclosure is to provide a molding material that can give a molded article having excellent antistatic properties and weather resistance, and a molded article having excellent antistatic properties and weather resistance. [Means for solving the problem]
[0007] A molding material according to an embodiment of the present disclosure includes a thermoplastic resin, an antistatic agent, an ultraviolet absorber, a light resistance stabilizer, and an antioxidant. The light resistance stabilizer includes a light resistance stabilizer having a molecular weight of 500 or more.
[0008] A molded article according to one embodiment of the present disclosure includes a molded product of the molding material. Effect of the Invention
[0009] According to the present disclosure, a molded article having excellent antistatic properties and weather resistance can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] 1. Overview The molding material according to this embodiment (hereinafter also referred to as "molding material (X)") contains a thermoplastic resin (A), an antistatic agent (B), an ultraviolet absorber (C), a light stabilizer (D), and an antioxidant (E). The light stabilizer (D) contains a light stabilizer (D1) having a molecular weight of 500 or more. This makes it difficult for the light stabilizer (D1) to evaporate when the molding material (X) is heated and melted to be shaped into a desired shape. Therefore, the light stabilizer (D1) tends to remain in the molded product. In this way, the light stabilizer (D1) remaining in the molded product also suppresses photodegradation of the antistatic agent (B).
[0011] Therefore, according to this embodiment, a molded product having excellent antistatic properties and weather resistance can be obtained.
[0012] 2.Details The molding material (X) and the molded product according to this embodiment will be described in more detail below.
[0013] (1) Molding material (X) The molding material (X) according to this embodiment contains a thermoplastic resin (A), an antistatic agent (B), an ultraviolet absorber (C), a light resistance stabilizer (D), and an antioxidant (E). The molding material (X) may further contain other components (F). The components contained in the molding material (X) are described below.
[0014] <Thermoplastic resin (A)> Thermoplastic resin (A) is a raw material that accounts for the majority of molding material (X). Thermoplastic resin (A) is roughly classified into general-purpose plastics (heat-resistant temperature of about 100°C or less), general-purpose engineering plastics (heat-resistant temperature of about 100 to 150°C), and super engineering plastics (heat-resistant temperature of about 150°C or more). Thermoplastic resin (A) may be any of these.
[0015] Commodity plastics include, for example, polyethylene (PE), polypropylene (PP), polyvinyl chloride (PVC), polystyrene (PS), and acrylonitrile-butadiene-styrene (ABS). Polyethylene (PE) is further classified into low-density polyethylene (PE-LD), linear low-density polyethylene (PE-LLD), and high-density polyethylene (PE-HD).
[0016] General-purpose engineering plastics include, for example, polyacetal (POM), polyamide (PA), polycarbonate (PC), modified polyphenylene ether (m-PPE), and polybutylene terephthalate (PBT).
[0017] Super engineering plastics include, for example, polyarylates (PAR) and polyphenylene sulfides (PPS).
[0018] Thermoplastic resins (A) are classified into amorphous plastics and crystalline plastics based on their solidified state. Thermoplastic resin (A) may be any of these. Amorphous plastics include, for example, polyvinyl chloride (PVC), polycarbonate (PC), and polyarylate (PAR). Crystalline plastics include, for example, polyethylene (PE), polyacetal (POM), and polyphenylene sulfide (PPS).
[0019] Specifically, the thermoplastic resin (A) is not particularly limited, but examples thereof include polyethylene (PE), polypropylene (PP), polycarbonate (PC), polyamide (PA), polyvinyl chloride (PVC), polyvinyl alcohol (PVA), and polyvinyl acetate (PVAc). The thermoplastic resin (A) may contain one or more resins selected from the group consisting of the resins listed above.
[0020] Preferably, the thermoplastic resin (A) contains polyethylene (PE). One of the reasons for this is that polyethylene resin is lightweight, does not generate toxic gases when incinerated, is easy to recycle, has excellent oil resistance and chemical resistance, and has excellent impact strength. The polyethylene (PE) may contain one or more types of polyethylene (PE) selected from the group consisting of low-density polyethylene (PE-LD), linear low-density polyethylene (PE-LLD), and high-density polyethylene (PE-HD).
[0021] <Antistatic agent (B)> The antistatic agent (B) is an additive that promotes leakage of the surface charge of the molded article. The antistatic agent (B) is classified into a coating type and a kneading type according to the method of use. The antistatic agent (B) may be any of these, but preferably, the antistatic agent (B) includes a kneading type antistatic agent. The kneading type antistatic agent is kneaded into the interior of the molded article, while the coating type antistatic agent is only physically adsorbed on the surface of the molded article. Therefore, the kneading type antistatic agent can obtain higher durability than the coating type antistatic agent. For example, even if the molded article is installed outdoors and exposed to rainfall, the antistatic agent (B) can be prevented from flowing out of the molded article due to rainwater.
[0022] Antistatic agents (B) are roughly classified into low molecular weight type and high molecular weight type according to their structure. The antistatic agent (B) may be any of these, but preferably contains a high molecular weight type antistatic agent. This is because the high molecular weight type antistatic agent is less likely to bleed onto the surface of a molded article than the low molecular weight type antistatic agent. Therefore, by containing a high molecular weight type antistatic agent in the antistatic agent (B), the appearance of the molded article is less likely to deteriorate. Furthermore, as in the case of the kneading type antistatic agent described above, even if the molded article is placed outdoors and exposed to rainfall, the antistatic agent (B) can be prevented from flowing out of the molded article by rainwater.
[0023] The antistatic agent (B) is classified into nonionic, cationic, anionic, and amphoteric types based on its structural characteristics. The antistatic agent (B) may be any of these, but preferably, the antistatic agent (B) contains a nonionic antistatic agent. This is because the nonionic antistatic agent has better compatibility with the thermoplastic resin (A) than the ionic (cationic, anionic, and amphoteric) antistatic agents.
[0024] The nonionic antistatic agent is not particularly limited, but examples thereof include polyether ester amide-based, ethylene oxide-epichlorohydrin-based, polyether ester-based, glycerin monofatty acid ester-based, and fatty acid diethanol amide-based antistatic agents.
[0025] Commercially available products can be used as the nonionic antistatic agent. Examples of commercially available nonionic antistatic agents include "Pelestat 300" (polyolefin / polyether copolymer) and "Pelectron PVL" manufactured by Sanyo Chemical Industries, Ltd., "Pebax MV" and "Pebax MH" manufactured by ARKEMA Corporation, "Adeka STAB AS301E" manufactured by ADEKA Corporation, and "ELESTMASTER HE110" and "HE510" manufactured by Kao Corporation.
[0026] The antistatic agent (B) has both hydrophilic and hydrophobic groups in the molecule. The hydrophilic group is a structure that contributes to leakage of electric charge. The hydrophobic group is a structure that has affinity with the thermoplastic resin (A). In this way, by having both a hydrophilic group and a hydrophobic group, it is possible to impart compatibility with the thermoplastic resin (A), molecular orientation on the surface of the molded article, and adsorption properties, and it is possible to improve the antistatic effect and its durability. It is believed that the antistatic effect is exerted in the molded article by the hydrophilic group of the antistatic agent (B) forming a leakage path for electric charge.
[0027] The content (lower limit) of the antistatic agent (B) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, based on 100 parts by mass of the thermoplastic resin (A), thereby making it possible to further improve the antistatic effect of the molded article.
[0028] The content (upper limit) of the antistatic agent (B) is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, relative to 100 parts by mass of the thermoplastic resin (A). One of the causes of deterioration in the appearance of the molded article is poor dispersion of the antistatic agent (B). As described above, by making the content of the antistatic agent (B) 20 parts by mass or less, poor dispersion of the antistatic agent (B) is suppressed, and deterioration in the appearance of the molded article is less likely to occur. Furthermore, it is also effective in reducing costs.
[0029] <Ultraviolet absorber (C)> UV absorbers (C) are additives that suppress the deterioration of physical performance (photodegradation) of molded products caused by photoinduced reactions. In particular, UV absorbers (C) suppress the photoinduced reactions that lead to photodegradation of thermoplastic resin (A) by absorbing ultraviolet rays with high energy levels.
[0030] Preferably, the ultraviolet absorber (C) includes at least one selected from the group consisting of benzotriazole-based ultraviolet absorbers, triazine-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, and benzoate-based ultraviolet absorbers.
[0031] Commercially available products can be used as the ultraviolet absorber (C). Examples of commercially available ultraviolet absorbers (C) include the trade name "Tinuvin P" (molecular weight 225), trade name "Tinuvin 234" (following formula (1), molecular weight 448), trade name "Tinuvin 326" (molecular weight 316), trade name "Tinuvin 329" (molecular weight 323), trade name "Tinuvin 360", trade name "Tinuvin 1577", trade name "Tinuvin 1600", trade name "Chimasobu 81", trade name "Tinuvin 120", and the trade name "Adeka STAB LA24", trade name "Adeka STAB LA29", trade name "Adeka STAB LA31", trade name "Adeka STAB LA32", trade name "Adeka STAB LA36", trade name "Adeka STAB LA46", trade name "Adeka STAB LAF70", and trade name "Adeka STAB 1413" manufactured by ADEKA CORPORATION.
[0032] [ka]
[0033] The ultraviolet absorber (C) preferably contains an ultraviolet absorber (C2) having a molecular weight of 320 or more and 1200 or less. The ultraviolet absorber (C2) having a molecular weight of 320 or more is suitable for molding at high temperatures because of its low volatility. It is particularly effective for rotational molding. An example of the ultraviolet absorber (C2) having a molecular weight of 320 or more is the above-mentioned product name "Tinuvin 234" (above formula (1), molecular weight 448).
[0034] The content (lower limit) of the ultraviolet absorber (C) is preferably 0.05 parts by mass or more, more preferably 0.15 parts by mass or more, and even more preferably 0.2 parts by mass or more, based on 100 parts by mass of the thermoplastic resin (A), thereby making it possible to further suppress the photoinduced reaction.
[0035] The content (upper limit) of the ultraviolet absorber (C) is preferably 0.7 parts by mass or less, and more preferably 0.5 parts by mass or less, based on 100 parts by mass of the thermoplastic resin (A).
[0036] The ultraviolet absorber (C) preferably contains an ultraviolet absorber (C1) having a melting point of 100° C. or more, and more preferably contains a benzotriazole-based ultraviolet absorber having a melting point of 100° C. or more. This makes it difficult for the ultraviolet absorber (C1) having a melting point of 100° C. or more to vaporize in the molding process. Therefore, bubbles (pinholes) caused by the vaporization of the ultraviolet absorber (C) are unlikely to remain on the surface of the molded article. Therefore, the appearance of the molded article is unlikely to deteriorate.
[0037] The content of the ultraviolet absorber (C1) having a melting point of 100° C. or higher is preferably 50 mass % or more, more preferably 75 mass % or more, and even more preferably 100 mass % based on the total amount of the ultraviolet absorber (C).
[0038] <Light resistance stabilizer (D)> Similar to UV absorbers (C), light resistance stabilizers (D) are additives that suppress the decline in physical performance (light degradation) of molded products caused by light-induced reactions. The difference between them and UV absorbers (C) is that light resistance stabilizers (D) capture and detoxify radicals derived from thermoplastic resin (A) that are generated by light degradation. In this way, UV absorbers (C) and light resistance stabilizers (D) suppress light degradation through different mechanisms, so using them together can produce a synergistic effect.
[0039] In particular, radicals derived from the thermoplastic resin (A) are presumed to be one of the causes of deterioration of the antistatic agent (B). Therefore, if the radicals derived from the thermoplastic resin (A) are captured by the light resistance stabilizer (D), the deterioration of the antistatic agent (B) can also be suppressed.
[0040] In this embodiment, the light resistance stabilizer (D) includes a light resistance stabilizer (D1) having a molecular weight of 500 or more. The molecular weight of the light resistance stabilizer (D1) is preferably 1000 or more, more preferably 1500 or more. This makes it difficult for the light resistance stabilizer (D1) to evaporate when the molding material (X) is heated and melted to be shaped into a desired shape. Therefore, the light resistance stabilizer (D1) is likely to remain in the molded article. In this way, the light resistance stabilizer (D1) remaining in the molded article captures radicals derived from the thermoplastic resin (A), and the photodegradation of the antistatic agent (B) is also suppressed. Therefore, a molded article having excellent antistatic properties and weather resistance can be obtained. The upper limit of the molecular weight of the light resistance stabilizer (D1) is not particularly limited, but is, for example, 5000 or less. The light resistance stabilizer (D) may further include a light resistance stabilizer (D2) having a molecular weight of less than 500.
[0041] Preferably, the light stabilizer (D) includes a hindered amine light stabilizer. The hindered amine light stabilizer is commonly called HALS (Hindered Amine Light Stabilizer), and is a compound having a 2,2,6,6-tetramethylpiperidine structure as a basic skeleton.
[0042] Commercially available products can be used as the light stabilizer (D). Commercially available products of the light stabilizer (D) include, for example, the trade names "Chimasoab 2020", "Chimasoab 944FDL" (the following formula (2), molecular weight 2000 to 3100), "Tinuvin 622SF" (the following formula (3), molecular weight 3100 to 4000), "Tinuvin 144", "Tinuvin 765", "Tinuvin 770", "Tinuvin XT55", "Tinuvin 111", and "Tinuvin 783FDL" ("Chimasoab 944FDL": "Tinuvin 622SF" manufactured by BASF Japan Ltd. (a blend of 1:1 by mass ratio), trade name "Tinuvin 791", and ADEKA Corporation's trade names "ADK STAB LA52", "ADK STAB LA57", "ADK STAB LA63P", "ADK STAB LA68", "ADK STAB LA72", "ADK STAB LA77", "ADK STAB LA81", "ADK STAB LA82", "ADK STAB LA87", "ADK STAB LA402AF", and "ADK STAB LA502XP".
[0043] [ka]
[0044] [ka]
[0045] The content (lower limit) of the light resistance stabilizer (D) is preferably 0.15 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.35 parts by mass or more, based on 100 parts by mass of the thermoplastic resin (A), which makes it easier to capture radicals derived from the thermoplastic resin (A).
[0046] The content (upper limit) of the light resistance stabilizer (D) is preferably 2.0 parts by mass or less, and more preferably 1.5 parts by mass or less, based on 100 parts by mass of the thermoplastic resin (A).
[0047] <Antioxidants (E)> Antioxidants (E) are additives that inhibit autoxidation, especially that triggered by heat, and are also called thermal antioxidants.
[0048] The antioxidant (E) may include one or more selected from the group consisting of phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, and hydroxylamine-based antioxidants. Phenol-based antioxidants function primarily as radical scavengers (primary antioxidants). Phosphorus-based antioxidants and sulfur-based antioxidants function primarily as peroxide decomposers (secondary antioxidants). Hydroxylamine-based antioxidants have the functions of both primary and secondary antioxidants.
[0049] Phenol-based antioxidants capture peroxy radicals generated during the thermal oxidation process, and include, for example, hindered phenols and semi-hindered phenols.
[0050] Phosphorus-based antioxidants decompose hydroperoxides generated during the thermal oxidation process. Phosphorus-based antioxidants have higher reactivity with hydroperoxides than sulfur-based antioxidants, and are effective in stabilizing materials during processing. Phosphorus-based antioxidants include, for example, phosphite-based and phosphonite-based antioxidants.
[0051] Preferably, the antioxidant (E) contains a phosphorus-based antioxidant. The thermoplastic resin (A) is exposed to high temperatures in the compounding and molding processes and is susceptible to thermo-oxidative degradation. It is believed that hydroperoxides of the thermoplastic resin (A) are most likely to be generated in these processes. Since the phosphorus-based antioxidant reacts quickly with the hydroperoxide, the hydroperoxide can be rapidly converted into a stable alcohol compound. In particular, in the rotational molding method, the heating temperature is likely to be high, so it is effective to include a phosphorus-based antioxidant in the antioxidant (E).
[0052] Commercially available products can be used as phosphorus-based antioxidants. Commercially available products of phosphorus-based antioxidants include, for example, the trade name "Irgastab FS042" (the following formula (4), molecular weight 537), the trade name "Irgafos 168" (the following formula (5), molecular weight 647), and the trade name "Irgastab FS301FF" (a blend of "Irgastab FS042": "Irgafos 168" (mass ratio) = 1:1) manufactured by BASF Japan Co., Ltd., the trade name "Adeka STAB 2112", the trade name "Adeka STAB 1178", the trade name "Adeka STAB 3010", the trade name "Adeka STAB TPP", the trade name "Adeka STAB PEP-36", and the trade name "Adeka STAB HP-10" manufactured by ADEKA Corporation.
[0053] [ka]
[0054] [ka]
[0055] Preferably, the antioxidant (E) contains a phosphorus-based antioxidant and a hydroxylamine-based antioxidant. By using a phosphorus-based antioxidant and a hydroxylamine-based antioxidant in combination, excellent processing stability and color stability can be obtained. An example of the antioxidant (E) containing a phosphorus-based antioxidant and a hydroxylamine-based antioxidant is the above-mentioned product name "Irgastab FS301FF".
[0056] The content of the phosphorus-based antioxidant based on the total amount of the antioxidant (E) is preferably 20 mass % or more, more preferably 50 mass % or more, and further preferably 66 mass % or more.
[0057] Sulfur-based antioxidants decompose hydroperoxides generated during the thermal oxidation process. Compared with phosphorus-based antioxidants, sulfur-based antioxidants can decompose a larger number of hydroperoxides, and are therefore effective in extending the life of materials in the environment in which they are used. Examples of sulfur-based antioxidants include thioether-based antioxidants.
[0058] The antioxidant (E) may be a commercially available product such as the following. Examples of commercially available products other than the above-mentioned commercially available products include, for example, the product names "Irganox 1010", "Irganox 1035", "Irganox 1076", "Irganox 1098", "Irganox 1135", "Irganox 1330", "Irganox 1520", "Irganox 245", "Irganox 259", and "Irganox 31", all manufactured by BASF Japan Ltd. Examples of such products include ADK STAB 14, trade name "Irganox 565", and products manufactured by ADEKA Corporation such as ADK STAB AO-20, ADK STAB AO-40, ADK STAB AO-50, ADK STAB AO-60, ADK STAB AO-330, ADK STAB PEP8, ADK STAB 2112, ADK STAB 1500, ADK STAB C, and ADK STAB 135A.
[0059] The mass ratio of the antistatic agent (B) to the antioxidant (E) is preferably within a range of 20:1 to 170:1, and more preferably within a range of 30:1 to 180:1, whereby the thermal deterioration of the antistatic agent (B) can be easily suppressed by the antioxidant (E), and the antistatic effect can be more easily sustained.
[0060] <Other ingredients (F)> The other components (F) are not particularly limited, but include, for example, a pigment, a dispersant, and a release agent.
[0061] Pigments The pigment is not particularly limited. When the molding material (X) contains a pigment, the molded product can be colored in a predetermined color.
[0062] <Dispersant> The dispersant is not particularly limited, but may be, for example, a metal soap. The metal soap may, for example, be 12-hydroxystearic acid soap. By including a dispersant in the molding material (X), the dispersibility of each component can be improved.
[0063] <Release agent> The mold release agent is not particularly limited, but may be, for example, zinc stearate. When the molding material (X) contains a mold release agent, the molded product can be easily peeled off from the mold.
[0064] <Production of molding materials> The molding material (X) may be in the form of pellets (X1) or powder (X2). In particular, the powder (X2) is suitable for use in rotational molding.
[0065] The pellets (X1) can be produced by using the above-mentioned components through a compounding process.
[0066] That is, in the compounding process, first, the thermoplastic resin (A), the antistatic agent (B), the ultraviolet absorber (C), the light resistance stabilizer (D), the antioxidant (E), and optionally other components (F) are premixed in a predetermined ratio to obtain a mixed material.
[0067] Next, the mixed material is put into the hopper of an extruder. The extruder may be a twin-screw extruder or a single-screw extruder. Either of these may be used, but a twin-screw extruder is preferably used. This is because a twin-screw extruder can disperse each component in the molding material (X) more uniformly than a single-screw extruder.
[0068] The mixed material is then melt-kneaded in an extruder, and strands are extruded from a die, cooled, and cut by a pelletizer to obtain pellets (X1).
[0069] On the other hand, the powder (X2) can be produced by pulverizing the pellets (X1) with a fine grinding mill.
[0070] (2) Molded products The molded article according to this embodiment includes a molded product of the above-mentioned molding material (X).
[0071] The molded article is produced through a molding process. That is, the molded article is produced by heating and melting the molding material (X), forming it into a desired shape, and cooling and solidifying it. The molding method for producing the molded article is not particularly limited, but examples thereof include rotational molding, press molding, and injection molding.
[0072] In the rotational molding method, powder (X2) is first put into a mold, which is then rotated on multiple axes while being heated from the outside. The powder (X2) is then melted and fused to the inner surface of the mold, after which the mold is cooled and the molded product is removed from the mold.
[0073] The heating temperature in the rotational molding method is preferably in the range of 150° C. to 250° C., more preferably in the range of 180° C. to 220° C. The heating time in the rotational molding method is preferably in the range of 5 minutes to 60 minutes, more preferably in the range of 15 minutes to 35 minutes.
[0074] Rotational molding is suitable for forming large-sized molded articles. Examples of molded articles by rotational molding include, but are not limited to, tanks (drinking water tanks, automobile gasoline tanks, fish farm tanks, etc.), playground equipment (slides, climbing walls, etc.), and structures (benches, tables, etc.).
[0075] The press molding method is a method in which a pellet (X1) is sandwiched between two heated dies, one above and one below, to form a sheet (resin plate).
[0076] Injection molding is a method in which molding material (X) is plasticized, then injected into a mold and cooled to solidify. Injection molding can be used to manufacture a wide range of molded products, from everyday items to industrial parts.
[0077] The molded article according to this embodiment contains a molded product of the molding material (X), and therefore has excellent antistatic properties and weather resistance, and can be installed not only indoors but also outdoors. EXAMPLES
[0078] (Examples 1 to 8 and Comparative Example 1) The details of the components of the molding material (X) are as follows:
[0079] <Thermoplastic resin (A)> Thermoplastic resin: polyethylene, product name "SP4030S" (Prime Polymer Co., Ltd.).
[0080] <Antistatic agent (B)> Antistatic agent: non-ionic antistatic agent, trade name "Pelestat 300" (polyolefin / polyether copolymer) (manufactured by Sanyo Chemical Industries, Ltd.).
[0081] <Ultraviolet absorber (C)> UV absorber 1: Benzotriazole-based UV absorber (melting point 137 to 141°C), product name "Tinuvin 234" (manufactured by BASF Japan Ltd.) Ultraviolet absorber 2: Benzotriazole-based ultraviolet absorber (melting point 137 to 141°C), trade name "Tinuvin 326" (manufactured by BASF Japan Ltd.).
[0082] <Light resistance stabilizer (D)> Light stabilizer 1: Trade name "Tinuvin 783FDL" (manufactured by BASF Japan Ltd.), trade name "Chimasoab 944FDL" (molecular weight 2000-3100): trade name "Tinuvin 622SF" (molecular weight 3100-4000) (mass ratio) = 1:1 blend Light stabilizer 2: trade name "Tinuvin 770DF" (manufactured by BASF Japan Ltd.), molecular weight 481.
[0083] <Antioxidants (E)> Antioxidant 1: Hydroxylamine-based antioxidant, trade name "Irgastab FS301FF" (manufactured by BASF Japan Ltd.), trade name "Irgastab FS042" (molecular weight approximately 538): trade name "Irgafos 168" (molecular weight 647, melting point 183 to 186°C) (mass ratio) = 1:1 blend Antioxidant 2: hindered phenol-based antioxidant, trade name "Irganox 1010" (manufactured by BASF Japan Ltd.).
[0084] <Other ingredients (F)> Pigment: Yellow pigment Dispersant: 12-hydroxystearic acid soap, trade name "MS-6" (manufactured by Nitto Kasei Kogyo Co., Ltd.) Release agent: zinc stearate.
[0085] Pellets (X1) were produced through a compounding process using each component so that the content (parts by mass) was as shown in Table 1. A twin-screw extruder and a single-screw extruder were used as extruders. The pellets (X1) were further pulverized in a fine grinder to produce powder (X2).
[0086] Next, the pellets (X1) were molded by press molding to produce a molded product. The powder (X2) was molded by rotational molding to produce a molded product. The heating temperature in the press molding method was 200°C, the pressure was 0.1 MPa, and the pressure time was 3 minutes, while the heating temperature in the rotational molding method was 300°C, and the heating time was 12.5 minutes.
[0087] (evaluation) (1) Weather resistance The molded product was punched out into a dumbbell shape conforming to JIS K 7127, and five test pieces were prepared from the molded product. Accelerated weather resistance tests were performed for the initial value, 1000 hours, and 2000 hours for each test piece using a sunshine weather meter.
[0088] After the accelerated weathering test, each test piece was subjected to measurement using a tensile testing machine under conditions of a temperature of 23°C ± 2°C and a humidity of 50 ± 5% RH, with a tensile speed of 50 mm / min, a chuck distance of 50 mm, and a dumbbell thickness of 2.0 mm. The tensile breaking strain of each test piece was calculated from the tensile breaking strain on the obtained tensile stress-strain curve using the following formula.
[0089] Tensile elongation at break = Δρ / Δε Δρ: Tensile breaking strain during tensile testing Δε: Length of parallel part before tensile test The weather resistance of each molded article was evaluated according to the following criteria.
[0090] A: The average tensile breaking elongation of the five test pieces is 50% or more of the tensile breaking elongation of the reference piece. B: The average tensile breaking elongation of the five test pieces is 50% or more of the tensile breaking elongation of the reference piece, but one or more of the five test pieces does not maintain 50% or more. C: The average tensile breaking elongation of the five test pieces is less than 50% of the tensile breaking elongation of the reference piece. The above reference piece was prepared in the same manner as the test piece, using only the thermoplastic resin (A).
[0091] (2) Antistatic properties The surface resistivity of the molded product was measured in an environment of 20°C and 50%±5% RH, and evaluated according to the following criteria.
[0092] A: The surface resistivity of the molded product is 1×10 13 less than B: The surface resistivity of the molded product is 1×10 13 More than 1×10 15 below C: The surface resistivity of the molded product is 1×10 15 Super.
[0093] [Table 1]
[0094] As is clear from Table 1, each Example can achieve both antistatic properties and weather resistance. That is, for antistatic properties, each Example was rated A or B. Also, for weather resistance (initial value and 2000 hours), each Example was rated A or B. In particular, the weather resistance ratings of Examples 4 to 7 and 11 to 14 are extremely good, since the ratings from the initial value to 3000 hours were A or B. It should be noted that, for weather resistance, an A or B rating at 2000 hours is considered to be at an acceptable level.
[0095] In contrast, each of the comparative examples was rated C in the antistatic property or weather resistance evaluation, indicating that both antistatic property and weather resistance could not be achieved at the same time.
Claims
1. The present invention comprises a thermoplastic resin, an antistatic agent, an ultraviolet absorber, a light resistance stabilizer, and an antioxidant, The light resistance stabilizer includes a light resistance stabilizer having a molecular weight of 500 or more. Molding material.
2. The antioxidant comprises a phosphorus-based antioxidant. The molding material according to claim 1.
3. The ultraviolet absorber includes an ultraviolet absorber having a melting point of 100° C. or more. The molding material according to claim 1 or 2.
4. The content of the antistatic agent is in the range of 5 parts by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the thermoplastic resin. The molding material according to any one of claims 1 to 3.
5. The light resistance stabilizer includes a hindered amine-based light resistance stabilizer. The molding material according to any one of claims 1 to 4.
6. A molded product of the molding material according to any one of claims 1 to 5. Molded products.
Citation Information