Coating material, and coated film formation method
A coating material with scaly particles of varying sizes and specific ratios addresses the issue of uneven patterns in decorative coatings, achieving a uniform and aesthetically pleasing film with reduced roughness.
Patent Information
- Application Number
- JP2024140611
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-12-02
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-12-01
AI Technical Summary
Existing decorative coating materials using small colored mica particles struggle to achieve large, uniform, and aesthetically pleasing patterns due to particle overlap or gaps, leading to unevenness and roughness.
A coating material comprising a resin component and scaly particles of varying sizes, including large, medium, and small particles, with specific weight ratios and color combinations, applied in a method that ensures balanced distribution and reduced roughness.
The solution results in a film with a large, uniform pattern and excellent aesthetics, minimizing unevenness and roughness, while maintaining good pattern balance and dispersibility.
Smart Images

Figure 2024159906000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel coating material. [Background technology]
[0002] Conventionally, decorative finishing methods that impart the aesthetic appearance of natural stone to buildings and civil engineering structures have been known. In recent years, there have been an increasing number of cases where decorative finishing with design features such as the diverse colors peculiar to natural stone is desired. For example, Patent Document 1 describes such a method in which a coating material containing colored mica and a binder resin is applied. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-224363 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the above Patent Document 1 uses relatively small colored mica with an average particle diameter of 0.3 to 2 mm, making it difficult to obtain a large pattern design. In order to obtain a large pattern design, it is possible to use large mica particles of more than 2 mm, but when a coating material containing such large particles is applied, the scale-like particles tend to partially overlap (crowded), causing a bias in the pattern, or on the other hand, there may be cases where there are areas (gaps) with few scale-like particles, resulting in the formation of an uneven pattern. In addition, the ends of the scale-like particles may jump up, causing the formed coating to have a rough feel. Under these circumstances, a coating material and a coating forming method that can form a coating with excellent aesthetics without bias in the pattern of the scale-like particles by a simple method are desired. [Means for solving the problem]
[0005] As a result of intensive research into solving the above problems, the present inventors came up with the idea of easily obtaining a coating film having a large pattern, which is less likely to be biased, has a good design with a well-balanced (arranged) pattern, and is aesthetically excellent with little roughness, by using a coating material containing scaly particles having a specific particle size in a coating material containing a resin component and scaly particles, and thus completed the present invention. That is, the present invention has the following characteristics.
[0006] That is, the present invention has the following features. 1. A coating material comprising a resin component (A) and scaly particles (B), The coating material contains 5 to 200 parts by weight of the scale-like particles (B) relative to 100 parts by weight of the solid content of the resin component (A), The scale-like particles (B) include large particles (b1) with a short diameter of more than 2 mm, medium particles (b2) with a short diameter of more than 0.7 mm and 2 mm or less, and small particles (b3) with a short diameter of 0.7 mm or less. fruit, The coating material has a mixing ratio of granular aggregate of 50 parts by weight or less per 100 parts by weight of the solid content of the aqueous resin (A). A coating material characterized by: 2. The coating material according to 1., wherein the weight ratio of the medium particles (b2) and small particles (b3) to the large particles (b1), [(b2)+(b3)] / (b1), in the scaly colored particles (B), is 1 or more and 50 or less. 3. The coating material according to 1 or 2, wherein the scale-like particles include particles of at least two colors. 4. On the substrate, 1. To A method for forming a coating, comprising applying the coating material described above to form a coating. 5. A method for forming a coating, comprising applying an undercoat material to a substrate to form a colored coating, and then applying the coating material described in 1. to form a coating. 6. The method for forming a coating according to 5., wherein the color tone of the colored coating is set to a hue similar to that of the medium particles (b2) of component (B). Effect of the Invention
[0007] According to the present invention, it is possible to obtain a coating film having a large pattern, which is less prone to uneven distribution of the scale-like particles, imparts design properties with a well-balanced (arranged) pattern, and is excellent in appearance with little roughness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present invention will be described.
[0009] <Coating material> The coating material of the present invention is characterized by containing a resin component (A) and scaly particles (B) having a specific size in combination.
[0010] Resin component (A) (hereinafter referred to as "component (A)") is not particularly limited, but is preferably at least one selected from water-soluble resins and water-dispersible resins. Examples of the resin include vinyl acetate resins, polyester resins, alkyd resins, vinyl chloride resins, epoxy resins, acrylic resins, urethane resins, acrylic silicone resins, fluororesins, and composites thereof. These resins can be used alone or in combination of two or more. These components (A) may also have crosslinking reactivity. When a component (A) having crosslinking reactivity is used, the water resistance, weather resistance, chemical resistance, and other properties of the coating can be improved.
[0011] In the present invention, acrylic resin is particularly suitable as component (A). Acrylic resin is a resin skeleton in which alkyl (meth)acrylate ester is the main component, and other monomers and other polymerizable monomers are copolymerized as necessary. In the present invention, alkyl acrylate ester and alkyl methacrylate ester are collectively referred to as alkyl (meth)acrylate ester. Furthermore, monomer is a general term for compounds having a polymerizable unsaturated double bond.
[0012] Examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, cyclohexyl (meth)acrylate, and the like. One or more of these can be used.
[0013] Specific examples of other monomers include, for example, Aromatic monomers such as styrene, 2-methylstyrene, vinyltoluene, t-butylstyrene, chlorostyrene, vinylanisole, vinylnaphthalene, divinylbenzene, phenyl (meth)acrylate, and benzyl (meth)acrylate; Nitrile group-containing monomers such as (meth)acrylonitrile, vinylidene cyanide, and α-cyanoethyl (meth)acrylate; Amide group-containing monomers such as maleic acid amide, (meth)acrylamide, N-monoalkyl (meth)acrylamide, N,N-dialkyl (meth)acrylamide, 2-(dimethylamino)ethyl (methacrylate), N-[3-(dimethylamino)propyl] (meth)acrylamide, and vinylamide; Carbonyl group-containing monomers such as acrolein, diacetone (meth)acrylamide, vinyl methyl ketone, vinyl ethyl ketone, and vinyl butyl ketone;
[0014] Carboxyl group-containing monomers such as (meth)acrylic acid, crotonic acid, maleic acid, itaconic acid, fumaric acid, isocrotonic acid, and salicylic acid; Amino group-containing monomers such as aminomethyl acrylate, aminoethyl acrylate, aminopropyl (meth)acrylate, amino-n-butyl (meth)acrylate, butylvinylbenzylamine, vinylphenylamine, p-aminostyrene, N-methylaminoethyl (meth)acrylate, and Nt-butylaminoethyl (meth)acrylate; Epoxy group-containing monomers such as glycidyl (meth)acrylate, diglycidyl fumarate, 3,4-epoxycyclohexyl (meth)acrylate, 3,4-epoxyvinylcyclohexane, allyl glycidyl ether, ε-caprolactone-modified glycidyl (meth)acrylate, and β-methylglycidyl (meth)acrylate; Hydroxyl group-containing monomers such as hydroxypropyl (meth)acrylate, ethylene glycol mono(meth)acrylate, and glycerol mono(meth)acrylate; vinylidene halide monomers such as vinylidene fluoride; Alkoxysilyl group-containing monomers, such as vinyltrimethoxysilane, vinyltriethoxysilane, γ-(meth)acryloyloxypropyltrimethoxysilane, γ-(meth)acryloyloxypropyltriethoxysilane, and γ-(meth)acryloyloxypropylmethyldimethoxysilane; Examples of the vinyl ether include ethylene, propylene, isoprene, butadiene, vinyl ether, vinyl ketone, etc. These may be used alone or in combination of two or more.
[0015] The component (A) can be produced by emulsion polymerization of a monomer group obtained by appropriately mixing the above-mentioned monomers. Any known method can be used as the polymerization method, and in addition to normal emulsion polymerization, soap-free emulsion polymerization, feed emulsion polymerization, seed emulsion polymerization, etc. can also be used. During polymerization, an emulsifier, initiator, dispersant, polymerization inhibitor, polymerization retarder, buffer, chain transfer agent, etc. can be used.
[0016] As the emulsifier, various surfactants that can be used in emulsion polymerization can be used, and these may be reactive types (reactive surfactants) having polymerizable unsaturated double bonds. As the emulsifier, anionic surfactants and nonionic surfactants may be used alone or in combination.
[0017] The glass transition temperature (hereinafter simply referred to as "Tg") of the component (A) is preferably set to -50°C to 50°C. If Tg is within this range, the effects of the present invention can be stably obtained. In the present invention, Tg is a value calculated by Fox's formula. In addition, the average particle size of the component (A) is preferably 300 nm or less (more preferably 20 to 200 nm). If the average particle size is within this range, the water resistance, weather resistance, chemical resistance, etc. of the coating can be improved. In addition, the average particle size referred to here is a value measured by dynamic light scattering.
[0018] The scaly particles (B) (hereinafter referred to as "component (B)") impart an excellent design to the formed coating. In addition, component (B) is also advantageous in terms of thinning and weight reduction of the formed coating. The present invention is characterized in that the scaly particles (B) are contained in an amount of 5 to 200 parts by weight (preferably 10 to 100 parts by weight, more preferably 15 to 80 parts by weight) per 100 parts by weight of the solid content of resin component (A). When the above range is satisfied, a coating having a design such as a natural stone look can be obtained.
[0019] The present invention is characterized in that the (B) component contains large particles (b1) with a short diameter of more than 2 mm (hereinafter referred to as "large particles (b1)"), medium particles (b2) with a short diameter of more than 0.7 mm and 2 mm or less (hereinafter referred to as "medium particles (b2)"), and small particles (b3) with a short diameter of 0.7 mm or less (hereinafter referred to as "small particles (b3)"). By using (B) components of different sizes in this way, it is possible to form a coating film with excellent aesthetics, with a good balance (arrangement) of the pattern and little roughness, and to impart design such as a large pattern. Specifically, the large particles (b1) mainly effectively impart a large pattern design to the coating film. The medium particles (b2) are mainly visually recognized as the base pattern of the coating film. Furthermore, the small particles (b3) are a component that imparts a small design to the formed coating and also fills the gaps between the scale-like particles to impart hiding properties, etc. to the formed coating.
[0020] In the present invention, it is preferable to use the large particles (b1), the medium particles (b2), and the small particles (b3) in combination at a specific weight ratio, and it is preferable that the weight ratio [(b2)+(b3)] / (b1) of the medium particles (b2) and the small particles (b3) to the large particles (b1) is 1 or more and 50 or less (more preferably 3 or more and 40 or less, and even more preferably 5 or more and 30 or less). When such a range is satisfied, the large particles (b1) are less likely to be biased, and a coating having excellent aesthetics and a good balance (arrangement) of the large pattern by the large particles (b1) can be formed in the base pattern formed by the medium particles (b2) and the small particles (b3). Furthermore, the medium particles (b2) and the small particles (b3) can suppress the end jumping of the large particles (b1), and a flat coating with little roughness can be formed. Furthermore, the weight ratio (b2) / (b3) of the medium particles (b2) to the small particles (b3) is preferably 1 or more and 30 or less (more preferably 1.5 or more and 20 or less, and even more preferably 2 or more and 10 or less). When such a range is satisfied, the above-mentioned effects can be further enhanced.
[0021] The mechanism of action by which such an effect is obtained is not limited, but for example, the medium particles (b2) and small particles (b3) smaller than the large particles (b1) act as spacers for the large particles (b1) and contribute to the dispersibility of the large particles (b1). In addition, the small particles (b3) smaller than the medium particles (b2) act as spacers for the medium particles (b2) and contribute to the dispersibility of the medium particles (b2). It is presumed that the (B) component dispersed in the coating material can maintain good dispersibility for the large particles (b1), medium particles (b2), and small particles (b3). In particular, in a coating material containing a relatively large amount of medium particles (b2) such as the coating material of the present invention, it is presumed that the large particles (b1) and the small particles (b3) are dispersed in a well-balanced manner in the medium particles (b2). It is presumed that by applying such a coating material, the particles are less likely to be biased, a coating with a well-balanced pattern is formed, and the jumping up of the particle ends can be suppressed.
[0022] In the present invention, the "minor diameter" is calculated by sieving using a metal mesh sieve (standard sieve) specified in JIS Z8801-1:2000, and the opening (a) of the standard sieve is taken as the length of the diagonal (L = √2 a) to represent the minor diameter. Specifically, 100 g of component (B) of the present invention is weighed out and sieved for 10 minutes using a test method in accordance with JIS K 0069 (manual sieving), Large particles (b1) are those that do not pass through a 12 mesh (a=1.4 mm, L=2.0 mm) sieve. Those that pass through a 12 mesh (a=1.4mm, L=2.0mm) sieve but do not pass through a 30 mesh (a=0.5mm, L=0.7mm) sieve are called medium particles (b2), Those that pass through a 30 mesh (a=0.5mm, L=0.7mm) sieve are small particles (b3), Let us assume that. The upper limit of the large particles (b1) is preferably those that pass through a 6.5 mesh (a=2.8 mm, L=4.0 mm) sieve (particles with a minor axis of 4 mm or less), whereas the lower limit of the small particles (b3) is preferably those that do not pass through a 70 mesh (a=0.21 mm, L=0.3 mm) sieve (particles with a minor axis of more than 0.3 mm).
[0023] In addition, the ratio of the minor axis to the major axis of component (B) (minor axis / major axis) is preferably 0.3 to 1 (more preferably 0.4 to 1, and even more preferably 0.5 to 1). When the size of component (B) satisfies the above range, its shape is easily recognized by the naked eye, and is suitable for design. The "minor axis / major axis" is calculated by placing component (B) stably on a horizontal surface and observing it from above with a microscope, taking the length of the shortest part as the "minor axis" and the length of the longest part as the "major axis".
[0024] Furthermore, the thickness of component (B) is preferably 1 mm or less (more preferably 0.001 to 0.5 mm, and even more preferably 0.005 to 0.2 mm). In the present invention, component (B) preferably has an aspect ratio (ratio of "minor axis / thickness") of 1.5 or more (more preferably 2 or more, and even more preferably 3 or more). The "thickness" referred to here is the maximum height from the bottom surface when the particle is stably placed on a horizontal surface, and can be measured with an optical microscope or the like.
[0025] In the (B) component of the present invention, the thickness of each of the large particles (b1), the medium particles (b2) and the small particles (b3) is not particularly limited as long as it satisfies the above range, but in the present invention, it is particularly preferable that the thickness of each particle is approximately the same. That is, the (B) component of the present invention is preferably a mixture of particles with different aspect ratios, and preferably contains at least two or more particles with different aspect ratios (more preferably three or more). This can further enhance the effects of the present invention. Specifically, the aspect ratio of the large particles (b1) is preferably 5 or more and 2000 or less (more preferably 6 or more and 1500 or less, and even more preferably 7 or more and 1000 or less), the aspect ratio of the medium particles (b2) is preferably 3 or more and 1000 or less (more preferably 4 or more and 800 or less, and even more preferably 5 or more and 500 or less), and the aspect ratio of the small particles (b3) is preferably 1.5 or more and 500 or less (more preferably 2 or more and 300 or less, and even more preferably 2.5 or more and 200 or less). In addition, it is preferable that the aspect ratios of the large particles (b1), the medium particles (b2) and the small particles (b3) are different from each other. By using components (B) having different aspect ratios in this way, it is possible to more stably form a coating film that is less likely to cause uneven distribution of the scaly particles, has a well-balanced pattern (arrangement), is less rough and has excellent aesthetics.
[0026] Examples of such (B) components include inorganic pieces such as mica, sericite, clay, talc, plate-like kaolin, barium sulfate flakes, glass flakes, alumina flakes, shell pieces, and metal pieces, as well as rubber pieces, plastic pieces, and wood pieces. Also included are base particles colored using these (scale-like colored particles). The coloring treatment is not particularly limited, but examples include a method of coating (or adsorbing) a colorant containing a pigment or dye on the base particles, and a method of subjecting the base particles to a baking treatment, etc. In the present invention, it is preferable to use mica coated with a colorant (colored mica). The (B) component can be used alone or in combination of two or more (one color or two or more colors), and various colors can be expressed.
[0027] In the present invention, it is preferable that component (B) contains scaly colored particles, particularly colored mica. In particular, it is preferable that the large particles (b1) contain scaly colored particles, which makes the large pattern more visible and improves the aesthetic appearance. Furthermore, it is preferable that the large particles (b1), the medium particles (b2), and the small particles (b3) each contain scaly colored particles, which makes it possible to form a coating having a large pattern and various colors.
[0028] The hue of the component (B) of the present invention can be set according to the desired pattern (design). For example, (p) an embodiment in which the component (B) contains only monochromatic (one-color) particles; (q) an embodiment in which the component (B) contains particles of at least two or more colors (more preferably two to six colors) selected from the same color system; (r) an embodiment in which the component (B) contains particles of at least two or more different colors (more preferably two to six colors); In the above embodiments (p) and (q), a coating having a design with a sense of calm can be obtained. On the other hand, in the above embodiment (r), a coating having a colorful design (accent design) can be obtained.
[0029] In the case of the above (q) and (r), the above large particles (b1), the above medium particles (b2), and the above small particles (b3) can each contain particles of one color or two or more colors, which can enhance the design.
[0030] In particular, in the case of the above embodiment (r), it is preferable that the large particles (b1) and the medium particles (b2) contain particles of different colors. This allows the large accent design to be effectively visually recognized, and a coating with excellent aesthetics can be easily formed. It is also preferable that the small particles (b3) contain particles of the same color system as the large particles (b1) or the medium particles (b2) (more preferably the medium particles (b2)). This gives the formed coating a sense of depth, and further enhances the aesthetics.
[0031] Furthermore, when the large particles (b1) contain particles of two or more different colors, the sense of color is improved, and the aesthetic appearance can be further improved. When the medium particles (b2) contain particles of two or more different colors, it is preferable that the medium particles (b2') that will be the base pattern (base color) of the formed coating are contained in the medium particles (b2) at 50% by weight or more (more preferably 55% by weight or more). The medium particles (b2') can also contain two or more types of particles of a single color (only one color) or similar colors (close or similar colors). This makes the accent design of the large particles (b1) easier to see, and the aesthetic appearance can be improved. When the small particles (b3) contain particles of two or more different colors, it is preferable that the small particles (b3') that will be the base pattern (base color) of the formed coating of the same color system as the hollow particles (b2') are contained in the small particles (b3) at 60% by weight or more (more preferably 65% by weight or more).
[0032] In the above component (B), the term "similar colors" refers to a color difference (ΔE) of preferably less than 10 (more preferably 8 or less). Also, the term "different colors" refers to a color difference (ΔE) of preferably 10 or more (more preferably 15 or more). The color difference (ΔE) referred to here is a value measured using a color difference meter, and each L * Value, a * Value, b *It can be calculated from the value using the following formula. <Formula>△E={(L *1 -L *2 ) 2 +(a *1 -a *2 ) 2 +(b *1 -b *2 ) 2} 0.5 During the ceremony, L *1 , a *1 , b *1 are the first color of the (B) component, L * , a * , b * . L *2 , a *2 , b *2 are the second color of the (B) component, L * , a * , b * . In addition, the L of component (B) * Value, a * Value, b * The value can be calculated by placing component (B) on a glass plate until the glass surface is covered, and then measuring the surface that is covered with a PE film.
[0033] The coating material of the present invention can be produced by uniformly mixing the above-mentioned components by a known method, but if necessary, other components that can be used in coating materials can also be mixed in. Examples of such components include aggregates, color pigments, extender pigments, luster pigments, fibers, film-forming assistants, thickeners, leveling agents, plasticizers, antifreeze agents, pH adjusters, preservatives, antifungal agents, anti-algae agents, antibacterial agents, dispersants, antifoaming agents, ultraviolet absorbers, light stabilizers, antioxidants, and water.
[0034] When the coating material of the present invention contains granular aggregate, a granular accent pattern can be imparted to the flat pattern formed by the (B) component. The aggregate can be granular in shape different from the (B) component, and can be, for example, either organic aggregate or inorganic aggregate, or can be either transparent (semi-transparent) aggregate or colored aggregate. Examples of such aggregate include crushed natural stone, ceramic powder, ceramic powder, metal particles, silica sand, feldspar, silica stone, kansui stone, glass beads, rubber particles, resin beads, etc., which may be colored. Also, aggregates of the same hue as the (B) component can be used. The particle size of the colored aggregate is 0.01 mm to 5 mm (more preferably 0.03 mm to 4.5 mm). When the coating material contains aggregate, it is preferably 50 parts by weight or less (more preferably 0 to 30 parts by weight) relative to the (A) component. In such a range, a granular accent pattern can be imparted in a well-balanced manner to the flat pattern formed by the (B) component.
[0035] Furthermore, when a luster pigment is contained, a sense of brilliance can be imparted to the pattern formed by the component (B). Examples of the luster pigment include pearl pigments, aluminum pigments, metallic pigments, etc. The particle size of the luster pigment is preferably 0.5 to 100 μm (more preferably 1 to 80 μm).
[0036] As described above, the coating material of the present invention contains large particles (b1), medium particles (b2), and small particles (b3) in combination as component (B), thereby ensuring the dispersibility of component (B). As a result, compared to conventional coating materials, good dispersibility can be obtained even when a small amount of dispersant is added (preferably 0.1% by weight or less in the coating material, and more preferably no dispersant is added). As a result, excellent effects can be achieved in terms of the water resistance of the formed coating film.
[0037] <Film formation method> The coating material of the present invention is applied to a substrate to form a coating film. The substrate constitutes the surface of buildings, civil engineering structures, etc. Examples of such substrates include concrete, mortar, siding boards, extrusion molding boards, gypsum boards, perlite boards, plywood, bricks, plastic boards, metal boards, glass, and porcelain tiles. These substrates may have a coating already formed on the surface, or may have wallpaper attached thereto, etc. The substrate surface may also have an uneven pattern such as a joint pattern or a stone-like pattern.
[0038] The coating material of the present invention can be applied with a brush, trowel, roller, spray, or the like to form a coating, but it is particularly preferred to form the coating by spray coating using a spray. This makes it possible to easily form a coating that is less likely to be biased in the scaly particles (B), has a good balance (arrangement) of the pattern, and is flat and has excellent aesthetics with little roughness. In particular, it is possible to easily form a design with high aesthetics, such as a natural stone look.
[0039] The amount of the coating material of the present invention to be applied is not particularly limited, but is preferably 100 to 1000 g / m 2 (More preferably 200 to 800 g / m 2 The number of times of application can be set depending on the desired design, but is preferably 1 to 2 times (more preferably 2 times). In such a case, the effect of the present invention can be fully exhibited.
[0040] In the present invention, it is preferable to apply a primer to the surface of the substrate to form a colored coating, and then apply a coating material. As the primer for forming the colored coating, a material containing a resin and a pigment can be used. In the present invention, the color, gloss, etc. can be set by adjusting the type and mixing ratio of the pigment. The mixing ratio of the resin and the pigment is preferably 5 to 500 parts by weight (more preferably 20 to 400 parts by weight, and even more preferably 30 to 300 parts by weight) of the pigment per 100 parts by weight of the resin solid content.
[0041] In the present invention, it is preferable to set the color tone of the colored coating to a hue (common color) similar to that of the medium particles (b2) of the above-mentioned (B) component. This makes it possible to prevent unevenness in the formed coating. In addition, it is possible to give the formed coating a greater sense of depth and form a multi-layer coating with excellent aesthetics.
[0042] It is desirable to set the color tone of the colored coating so that the color difference (ΔE) between the color tone of the medium particles (b2') that form the base pattern (base color) in the medium particles (b2) is 20 or less (preferably 15 or less, more preferably 10 or less). In such a case, a laminated coating with excellent aesthetics can be obtained. The color difference (ΔE) referred to here is a value measured using a color difference meter, and the respective L * Value, a * Value, b * It can be calculated from the value using the following formula. <Formula>△E={(L *1 -L *2 ) 2 +(a *1 -a *2 ) 2 +(b *1 -b *2 ) 2} 0.5 During the ceremony, L *1 , a *1 , b *1 are the L of the colored coating, * , a * , b * . L *2 , a *2 , b *2 are the L of the medium particle (b2'), * , a * , b * . The L*, a*, and b* of the base layer are the L values of the coating when each first coating material is applied to a standard white paper using a film applicator with a gap of 2 mm, the coated surface is placed horizontally, and dried for 48 hours under standard conditions (temperature 23°C, relative humidity 50%; the same applies below). * Value, a * Value, b *It can be calculated from the value (average value of three or more measurement points). In addition, the L of the medium particle (b2') * Value, a * Value, b * The value can be calculated by placing medium particles (b2) on a glass plate until the glass surface is covered, and then measuring the surface on which a PE film is placed.
[0043] As the resin, the same resin as the above-mentioned coating material can be used. As the pigment, known color pigments, extender pigments, etc. can be used. Among them, examples of color pigments include titanium oxide, zinc oxide, carbon black, lamp black, bone black, graphite, black iron oxide, copper chrome black, cobalt black, copper manganese iron black, red iron oxide, molybdate orange, permanent red, permanent carmine, anthraquinone red, perylene red, quinacridone red, yellow iron oxide, titanium yellow, fast yellow, benzimidazolone yellow, chrome green, cobalt green, phthalocyanine green, ultramarine blue, Prussian blue, cobalt blue, phthalocyanine blue, quinacridone violet, dioxazine violet, heat shielding pigments, aluminum flake pigments, pearl pigments, and luster pigments. By using one or more of these color pigments, it is possible to color the material to any hue.
[0044] Examples of the extender pigment include heavy calcium carbonate, kansui stone, light calcium carbonate, white carbon, kaolin, clay, china clay, diatomaceous earth, barite powder, barium sulfate, precipitated barium sulfate, silica sand, silica stone powder, quartz powder, resin beads, glass beads, hollow balloons, etc., and one or more of these can be used. By appropriately setting the type of extender pigment, the mixing ratio, etc., the coating material can be adjusted to a desired glossiness.
[0045] In addition to the above components, the undercoat material of the present invention may contain known additives, such as aggregates, dyes, thickeners, wetting agents, antifreeze agents, film-forming assistants, preservatives, antifungal agents, anti-algae agents, antibacterial agents, dispersants, antifoaming agents, ultraviolet absorbers, light stabilizers, antioxidants, catalysts, diluting solvents, etc., within the range that does not significantly impair the effects of the present invention. The undercoat material can be manufactured by uniformly mixing the above-mentioned components by a conventional method.
[0046] The undercoat material can be applied, for example, with a brush, trowel, roller, spray, etc. to form a colored coating. The amount of the undercoat material applied is not particularly limited, but is preferably 50 to 1000 g / m 2 (More preferably 100 to 800 g / m 2 ). EXAMPLES
[0047] The following examples will clarify the features of the present invention.
[0048] (Coating material 1~11) Based on the formulation shown in Table 1, the raw materials were mixed in a standard manner to produce coating materials 1 to 11.
[0049] The following components were used: (A) Resin component Acrylic silicone resin emulsion (solid content 50% by weight, medium: water) (B) Scaly colored particles (b1) Large particles (b1-1) Black mica piece [minor diameter: over 2 mm and less than 4 mm, minor diameter / major diameter (average value): 0.95, minor diameter / thickness (average value): 31.4, L value = 44.2, a value = -0.4, b value = -1.5] (b1-2) White mica piece [minor diameter: over 2 mm and less than 4 mm, minor diameter / major diameter (average value): 0.88, minor diameter / thickness (average value): 30.7, L value = 91.5, a value = 0.5, b value = 4.4] (b1-3) Light cream-colored mica pieces [minor diameter: over 2 mm and less than 4 mm, minor diameter / major diameter (average): 0.92, minor diameter / thickness (average): 31.5, L value = 86.7, a value = 0.7, b value = 14.1] (b1-4) Gray mica pieces [minor diameter: over 2 mm and less than 4 mm, minor diameter / major diameter (average value): 0.98, minor diameter / thickness (average value): 32.5, L value = 70.5, a value = -0.6, b value = -0.5] (b2) Medium particles (b2-1) Gray mica piece [minor diameter: over 0.7 mm and 2 mm or less, minor diameter / major diameter (average value): 0.87, minor diameter / thickness (average value): 15.5, L value = 69.3, a value = -0.7, b value = 0.2] (b2-2) White mica piece [minor diameter: over 0.7 mm and 2 mm or less, minor diameter / major diameter (average value): 0.92, minor diameter / thickness (average value): 14.5, L value = 90.1, a value = 0.7, b value = 5.2] (b3) Small particles (b3-1) Gray mica pieces [minor diameter: over 0.3 mm and less than 0.7 mm, minor diameter / major diameter (average): 0.92, minor diameter / thickness (average): 5.4, L value = 69.3, a value = -0.7, b value = 0.2] (b3-2) White mica piece [minor diameter: over 0.3 mm and less than 0.7 mm, minor diameter / major diameter (average value): 0.94, minor diameter / thickness (average value): 4.9, L value = 90.1, a value = 0.7, b value = 5.2] (others) Additives (thickeners, defoamers, etc.)
[0050] (Examples 1 to 8, Comparative Examples 1 to 3) The coating material was applied to the substrate (slate board) with a primer [gray: colored coating formed by the primer and (b2) color difference of medium particles (△E) = 5] with a spray gun (diameter: 5.5 mm) at a coating amount of 800 g / m 2 The paint was spray-painted with a paint and then dried and hardened at 23°C for 24 hours to form a patterned coating.
[0051] <Evaluation> The following evaluations were carried out, and the results are shown in Table 1. ·Design Those with little bias in the scaly colored particles and a good balance of the pattern were given an "AA" rating, while those with a poorer pattern were given a "D", and the evaluation was on a five-level scale from AA>A>B>C>D. ·Smoothness The coating that was formed was rated on a four-point scale of A>B>C>D, with "A" being the least rough coating and "D" being the rough coating.
[0052] [Table 1]
[0053] In Examples 1 to 8, coatings excellent in design and aesthetics could be easily formed. In particular, in Examples 1 and 5, the scaly colored particles were less biased, the design was well balanced in the pattern, and coatings with little roughness were obtained. In addition, in Examples 5 and 6, the color was excellent. On the other hand, there was no large-scale pattern and the aesthetics were poor in Comparative Example 1. Moreover, in Comparative Examples 2 and 3, the scale-like particles were unevenly distributed and the pattern balance was poor.
Claims
1. A coating material comprising a resin component (A) and scaly particles (B), The coating material contains 5 to 200 parts by weight of scale-like particles (B) per 100 parts by weight of a solid content of a resin component (A), The scale-like particles (B) include large particles (b1) having a short diameter of more than 2 mm, medium particles (b2) having a short diameter of more than 0.7 mm and not more than 2 mm, and small particles (b3) having a short diameter of 0.7 mm or less, The coating material is characterized in that the mixing ratio of the granular aggregate is 50 parts by weight or less per 100 parts by weight of the solid content of the aqueous resin (A).
2. The coating material according to claim 1, characterized in that the weight ratio [(b2)+(b3)] / (b1) of the medium particles (b2) and small particles (b3) to the large particles (b1) in the scale-like particles (B) is 1 or more and 50 or less.
3. 3. The coating material according to claim 1, wherein the scale-like particles include particles of at least two colors.
4. A method for forming a coating, comprising applying the coating material according to claim 1 onto a substrate to form a coating.
Citation Information
Patent Citations
Decorative coating material and decorative building material
JP2006152231A
Coating material and coating film formation method
JP2015134912A
Coating film formation method
JP2017177099A
Coating film formation method
JP2017177100A
Multi-coating layer color golf ball
US9205304B1