Optical laminated body

The optical laminate addresses transportability and removability issues by optimizing the thickness and peeling forces of the surface protection film and separator, ensuring smooth handling and reduced defects during use.

JP2024159962AInactive Publication Date: 2024-11-08NITTO DENKO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024150439
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-08-21
Filing Date
2024-09-02
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure 2024159962000001_ABST
    Figure 2024159962000001_ABST
Patent Text Reader

Abstract

To provide an optical laminated body that has a thin-type polarizer, is excellent in transportability, and excellent in peelability of a surface protection film and separator.SOLUTION: An optical laminated body comprises, according to an embodiment of the present invention,: a polarizer; an adhesive layer that is provided on one side of the polarizer; a separator that is temporarily adhered peelably on a side opposite to the polarizer of the adhesive layer; and a surface protection film that is temporarily adhered peelably on a side opposite to the adhesive layer of the polarizer. A thickness of the polarizer is equal to or less than 60 μm, a thickness of the surface protection film is equal to or more than 40 μm, peeling force of the surface protection film is 0.10 N / 25 mm to 0.50 N / 25 mm, an elastic modulus of the surface protection film is equal to or more than 2.00×109 Pa, a thickness of the separator is 35 μm to 80 μm, and peeling force of the separator is less than 0.28 N / 25 mm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to an optical laminate. [Background technology]

[0002] Liquid crystal display devices, which are a typical type of image display device, have polarizers arranged on both sides of a liquid crystal cell due to their image formation method. Polarizers are typically produced by dyeing a polyvinyl alcohol (PVA)-based resin film with a dichroic substance such as iodine (see, for example, Patent Documents 1 and 2). In recent years, there has been an increasing demand for thinner image display devices. Therefore, there is also a demand for further thinner polarizers. A thin polarizer (in practice, a polarizing plate including such a polarizer) can be provided as an optical laminate in which, for example, a pressure-sensitive adhesive layer, a surface protective film, and a separator are laminated. However, such optical laminates have problems such as insufficient transportability and insufficient peelability of the surface protective film and the separator. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 5048120 [Patent Document 2] Japanese Patent Application Laid-Open No. 2013-156391 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made to solve the above-mentioned conventional problems, and its main object is to provide an optical laminate having a thin polarizing plate, a surface protective film, and a separator, which has excellent transportability and excellent peelability of the surface protective film and the separator. [Means for solving the problem]

[0005] An optical laminate according to an embodiment of the present invention includes a polarizing plate, a pressure-sensitive adhesive layer provided on one side of the polarizing plate, a separator temporarily and releasably attached to the pressure-sensitive adhesive layer on the side opposite the polarizing plate, and a surface protection film temporarily and releasably attached to the polarizing plate on the side opposite the pressure-sensitive adhesive layer. The polarizing plate has a thickness of 60 μm or less, a thickness of 40 μm to 87 μm, a peel strength of 0.10 N / 25 mm to 0.50 N / 25 mm, and a modulus of elasticity of 2.00×10 9 Pa~3.91×10 9 Pa, the thickness of the separator is 35 μm to 60 μm, and the peel strength of the separator is 0.15 N / 25 mm or less. In one embodiment, the separator has a peel force of less than 0.10 N / 25 mm. In one embodiment, the polarizing plate includes a polarizer having a thickness of 10 μm or less and made of a polyvinyl alcohol-based resin film containing iodine. In one embodiment, the polarizer has an iodine content of 10% to 25% by weight. [Effects of the Invention]

[0006] According to the present invention, in an optical laminate comprising a thin polarizing plate, a surface protective film and a separator, by optimizing the thickness, peel strength and elastic modulus of the surface protective film, and the thickness and peel strength of the separator, an optical laminate having excellent transportability and excellent peel strength of the surface protective film and separator can be realized. [Brief explanation of the drawings]

[0007] [Figure 1] 1 is a schematic cross-sectional view of an optical laminate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE INVENTION

[0008] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0009] A. Overall structure of the optical laminate 1 is a schematic cross-sectional view of an optical laminate according to one embodiment of the present invention. The optical laminate 100 of the illustrated example has a surface protection film 10, a polarizing plate 20, a pressure-sensitive adhesive layer 30, and a separator 40. The polarizing plate 20 has a thickness of 60 μm or less. Furthermore, the surface protection film 10 has a thickness of 40 μm or more, a peel strength of 0.10 N / 25 mm to 0.50 N / 25 mm, and an elastic modulus of 2.00×10 9 Pa or more. Furthermore, the thickness of the separator 40 is 35 μm to 80 μm, and the peel strength thereof is less than 0.28 N / 25 mm. The components of the optical laminate will be described in more detail below.

[0010] B. Polarizing plate The polarizing plate 20 typically includes a polarizer 22 and a protective layer disposed on one or both sides of the polarizer 22. Preferably, as shown in the illustrated example, in the polarizing plate 20, a protective layer 21 is disposed on one side of the polarizer 22. The thickness of the polarizing plate is 60 μm or less, preferably 40 μm or less, and more preferably 35 μm or less. The lower limit of the thickness of the polarizing plate can be, for example, 20 μm.

[0011] B-1.Polarizer The polarizer 22 is typically made of a polyvinyl alcohol (PVA) resin film containing iodine.

[0012] The upper limit of the thickness of the polarizer is 10 μm in one embodiment, and 3 μm in another embodiment, and the lower limit of the thickness is 1 μm in one embodiment.

[0013] The iodine content of the polarizer can be appropriately set so as to achieve both sufficient polarization performance and optimal single-piece transmittance. The iodine content is preferably 10% to 25% by weight, more preferably 15% to 25% by weight. The polarizer used in the embodiment of the present invention has such an extremely high iodine content, yet it can achieve extremely excellent heat resistance, which has been difficult to achieve in the past. More specifically, a polarizer having an extremely high iodine content can significantly suppress changes in optical properties in a high-temperature environment. In this specification, the "iodine content" means the amount of all iodine contained in the polarizer (PVA-based resin film). More specifically, iodine in the polarizer is iodine ions (I - ), polyiodide ion (I3 - , I5 - ), and the iodine content in this specification refers to the amount of iodine including all of these forms. The iodine content can be calculated, for example, by the calibration curve method of X-ray fluorescence analysis. Note that polyiodine ions exist in the polarizer in the form of a PVA-iodine complex. The formation of such a complex can cause absorption dichroism in the wavelength range of visible light. Specifically, a complex of PVA and triiodide ion (PVA·I3 - ) has an absorption peak around 470 nm, and the complex of PVA and pentaiodide ion (PVA·I5 - ) has an absorption peak around 600 nm. As a result, polyiodide ions can absorb light in a wide range of visible light depending on their form. On the other hand, iodide ions (I - ) has an absorption peak around 230 nm and does not substantially contribute to the absorption of visible light. Therefore, polyiodide ions present in a complex state with PVA may be primarily responsible for the absorption performance of the polarizer.

[0014] The single transmittance (Ts) of the polarizer is preferably 30.0% to 43.0%, more preferably 35.0% to 41.0%. The degree of polarization of the polarizer is preferably 99.9% or more, more preferably 99.95% or more, and even more preferably 99.98% or more. By setting the single transmittance low and increasing the degree of polarization, it is possible to increase contrast and make black display even blacker, thereby realizing an image display device with excellent image quality. The single transmittance is a value measured using a spectrophotometer with an integrating sphere. The single transmittance is a Y value measured using a 2-degree visual field (C light source) according to JIS Z8701 and corrected for luminosity, and can be measured using, for example, a spectrophotometer with an integrating sphere (manufactured by JASCO Corporation, product name: V7100).

[0015] B-2. PVA resin film Examples of PVA-based resins that form the PVA-based resin film include polyvinyl alcohol and ethylene-vinyl alcohol copolymers. Polyvinyl alcohol can be obtained by saponifying polyvinyl acetate. Ethylene-vinyl alcohol copolymers can be obtained by saponifying ethylene-vinyl acetate copolymers. The saponification degree of the PVA-based resin is usually 85 mol% or more and less than 100 mol%, preferably 95.0 mol% to 99.95 mol%, and more preferably 99.0 mol% to 99.93 mol%. The saponification degree can be determined in accordance with JIS K 6726-1994. By using a PVA-based resin with such a saponification degree, a polarizer with excellent durability can be obtained. If the saponification degree is too high, gelation may occur.

[0016] The thickness of the PVA-based resin film is not particularly limited and can be set according to the desired thickness of the polarizer, and is, for example, 10 μm to 200 μm.

[0017] In one embodiment, the PVA-based resin film may be a PVA-based resin layer formed on a substrate. A laminate of a substrate and a PVA-based resin layer can be obtained, for example, by applying a coating liquid containing the PVA-based resin to the substrate, or by laminating a PVA-based resin film on the substrate. Any appropriate resin substrate can be used as the substrate, and for example, a thermoplastic resin substrate can be used.

[0018] B-3.Protective layer Any suitable resin film can be used as the protective layer. Examples of materials for forming the resin film include (meth)acrylic resins, cellulose resins such as diacetyl cellulose and triacetyl cellulose, cycloolefin resins such as norbornene resins, olefin resins such as polypropylene, ester resins such as polyethylene terephthalate resins, polyamide resins, polycarbonate resins, and copolymer resins thereof. Note that "(meth)acrylic resin" refers to acrylic resins and / or methacrylic resins.

[0019] In one embodiment, the (meth)acrylic resin is a (meth)acrylic resin having a glutarimide structure. (Meth)acrylic resins having a glutarimide structure (hereinafter also referred to as glutarimide resins) are described in, for example, JP 2006-309033 A, JP 2006-317560 A, JP 2006-328329 A, JP 2006-328334 A, JP 2006-337491 A, JP 2006-337492 A, JP 2006-337493 A, JP 2006-337569 A, JP 2007-009182 A, JP 2009-161744 A, and JP 2010-284840 A. These descriptions are incorporated herein by reference.

[0020] When a polarizer is produced using a laminate of a substrate and a PVA-based resin layer, the substrate may be used as a protective layer without being peeled off, or the substrate may be peeled off and the protective layer may be attached to the polarizer.

[0021] The thickness of the protective layer is preferably 5 mm or less, more preferably 1 mm or less, even more preferably 1 μm to 500 μm, and most preferably 5 μm to 150 μm. If a surface treatment is applied, the thickness of the protective layer includes the thickness of the surface treatment layer.

[0022] The protective layer is attached to the polarizer via any appropriate adhesive layer (adhesive layer, pressure-sensitive adhesive layer).

[0023] C. Surface protection film As shown in the illustrated example, the surface protection film 10 is temporarily and removably attached to the polarizing plate 20 on the side opposite to the adhesive layer 30. More specifically, the surface protection film 10 includes a base film and an adhesive layer, and the surface protection film 10 and the polarizing plate 20 are bonded together via the adhesive layer.

[0024] C-1. Base film The substrate film of the surface protection film may be composed of any appropriate resin film. Examples of materials for forming the resin film include ester resins such as polyethylene terephthalate resins, cycloolefin resins such as norbornene resins, olefin resins such as polypropylene, polyamide resins, polycarbonate resins, and copolymer resins thereof. Ester resins (particularly polyethylene terephthalate resins) are preferred. Such materials have the advantage of having a sufficiently high elastic modulus and being less likely to deform even when tension is applied during transportation and / or lamination.

[0025] The thickness of the substrate film is preferably 38 μm or more, more preferably 48 μm or more. The upper limit of the thickness of the substrate film may be, for example, 128 μm. Such a thickness has the advantage that deformation is unlikely to occur even when tension is applied during transportation and / or lamination.

[0026] C-2.Adhesive layer Any appropriate adhesive may be used as the adhesive forming the adhesive layer of the surface protective film. Examples of base resins for adhesives include acrylic resins, styrene resins, and silicone resins. Acrylic resins are preferred from the viewpoints of chemical resistance, adhesion to prevent penetration of treatment liquid during immersion, and flexibility to the adherend. Examples of crosslinking agents that may be contained in the adhesive include isocyanate compounds, epoxy compounds, and aziridine compounds. The adhesive may contain, for example, a silane coupling agent. The formulation of the adhesive may be appropriately set depending on the purpose.

[0027] The thickness of the pressure-sensitive adhesive layer is preferably 2 μm or more, more preferably 5 μm or more, and the upper limit of the thickness is, for example, 40 μm.

[0028] C-3. Characteristics of surface protection films The thickness of the surface protection film is 40 μm or more, preferably 50 μm or more. The upper limit of the thickness of the surface protection film can be, for example, 130 μm. The thickness of the surface protection film refers to the total thickness of the base film and the pressure-sensitive adhesive layer. When the thickness of the surface protection film is in this range, an optical laminate with excellent transportability can be obtained. If the thickness of the surface protection film is thinner than 40 μm, transportability may be insufficient.

[0029] The peel strength of the surface protection film is 0.10 N / 25 mm to 0.50 N / 25 mm, preferably 0.10 N / 25 mm to 0.35 N / 25 mm. When the peel strength of the surface protection film is within this range, an optical laminate with excellent peelability between the surface protection film and the separator can be obtained. If the peel strength of the surface protection film is less than 0.10 N / 25 mm, the surface protection film may lift off when the separator is peeled off. Furthermore, if the peel strength is greater than 0.50 N / 25 mm, delamination may occur when the surface protection film is peeled off.

[0030] The elastic modulus of the surface protection film is 2.00 x 10 9 Pa or more, preferably 2.50 × 10 9The upper limit of the elastic modulus of the surface protection film is 8.00 × 10 9 When the elastic modulus of the surface protective film is in this range, an optical laminate having excellent transportability can be obtained. 9 If it is smaller than Pa, wrinkles and creases may occur in the film during transport.

[0031] D.Adhesive layer The adhesive layer 30 may typically be made of an acrylic adhesive. As shown in the illustrated example, the adhesive layer 30 is formed on one surface of the polarizing plate 20, and is provided for the purpose of bonding the liquid crystal panel and the polarizing plate 20 together.

[0032] The thickness of the pressure-sensitive adhesive layer is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or less. The lower limit of the thickness can be, for example, 1 μm.

[0033] E. Separator As shown in the illustrated example, separator 40 can be temporarily and removably attached to the pressure-sensitive adhesive layer 30 on the side opposite to polarizing plate 20. The separator protects the pressure-sensitive adhesive layer until actual use and also enables the polarizing plate to be formed into a roll.

[0034] Examples of materials for forming the separator include ester resins such as polyethylene terephthalate resins, cycloolefin resins such as norbornene resins, olefin resins such as polypropylene, polyamide resins, polycarbonate resins, and copolymer resins thereof. Ester resins (particularly polyethylene terephthalate resins) are preferred.

[0035] The thickness of the separator is 35 μm to 80 μm, preferably 40 μm to 60 μm. By having the separator thickness in this range, an optical laminate having excellent transportability and excellent separator peelability can be obtained. If the separator thickness is thinner than 35 μm, transportability may be insufficient. Furthermore, if the separator thickness is thicker than 80 μm, poor pickup may occur when the separator is peeled off.

[0036] The peel strength of the separator is less than 0.28 N / 25 mm, preferably less than 0.10 N / 25 mm. By setting the peel strength of the separator in this range, an optical laminate with excellent separator peel strength can be obtained. If the peel strength of the separator is 0.28 N / 25 mm or more, poor pickup may occur when the separator is peeled off.

[0037] F. Method for manufacturing optical laminate F-1. Polarizer A method for producing a polarizer according to an embodiment of the present invention includes at least stretching and dyeing a PVA-based resin film. Typically, the production method includes a step of preparing a PVA-based resin film, a stretching step, a dyeing step, a crosslinking step, a washing step, and a drying step. A swelling step may be performed before the stretching step, if necessary. Each step in which a PVA-based resin film is provided can be performed in any appropriate order and at any appropriate timing. Therefore, each step may be performed in the above order or in an order different from the above. If necessary, one step may be performed multiple times. Furthermore, a step other than the above (e.g., an insolubilization step) may be performed at any appropriate timing. When the PVA-based resin film is a PVA-based resin layer formed on a substrate, a laminate of the substrate and the PVA-based resin layer is subjected to the above steps.

[0038] Each step will be described below, but as mentioned above, the steps can be performed in any suitable order and are not limited to the order described.

[0039] (Stretching process) In the stretching step, the PVA-based resin film is typically uniaxially stretched 3 to 7 times. The stretching direction may be the longitudinal direction (MD) of the film or the width direction (TD) of the film. The stretching method may be dry stretching, wet stretching, or a combination of these. The PVA-based resin film may be stretched during the crosslinking step, swelling step, dyeing step, etc. The stretching direction may correspond to the absorption axis direction of the resulting polarizer.

[0040] (Swelling process) The swelling step is usually carried out before the dyeing step. The swelling step is carried out, for example, by immersing the PVA-based resin film in a swelling bath. Water such as distilled water or pure water is usually used as the swelling bath. The swelling bath may contain any appropriate other component other than water. Examples of the other components include solvents such as alcohol, additives such as surfactants, and iodides. Examples of iodides include potassium iodide, lithium iodide, sodium iodide, zinc iodide, aluminum iodide, lead iodide, copper iodide, barium iodide, calcium iodide, tin iodide, and titanium iodide. Potassium iodide is preferably used. The temperature of the swelling bath is, for example, 20°C to 45°C. The immersion time is, for example, 10 to 300 seconds.

[0041] (dying process) The dyeing step is a step of dyeing the PVA-based resin film with a dichroic substance. Preferably, the dyeing step is carried out by adsorbing the dichroic substance. Examples of the adsorption method include immersing the PVA-based resin film in a dyeing solution containing the dichroic substance, applying the dyeing solution to the PVA-based resin film, and spraying the dyeing solution onto the PVA-based resin film. Preferably, the method involves immersing the PVA-based resin film in the dyeing solution, as this allows for good adsorption of the dichroic substance.

[0042] Examples of the dichroic substance include iodine and dichroic dyes. Iodine is preferred. When iodine is used as the dichroic substance, an iodine aqueous solution is preferably used as the dyeing solution. The iodine content of the iodine aqueous solution is preferably 0.04 to 5.0 parts by weight per 100 parts by weight of water. In order to increase the solubility of iodine in water, it is preferable to add an iodide to the iodine aqueous solution. Potassium iodide is preferably used as the iodide. The iodide content is preferably 0.3 to 15 parts by weight per 100 parts by weight of water.

[0043] The temperature of the dye solution during dyeing can be set to any appropriate value, for example, 20° C. to 50° C. When the PVA resin film is immersed in the dye solution, the immersion time is, for example, 5 seconds to 5 minutes.

[0044] (Crosslinking process) In the crosslinking step, a boron compound is usually used as a crosslinking agent. Examples of the boron compound include boric acid and borax. Boric acid is preferred. In the crosslinking step, the boron compound is usually used in the form of an aqueous solution.

[0045] When an aqueous boric acid solution is used, the boric acid concentration of the aqueous boric acid solution is, for example, 1% by weight to 15% by weight, and preferably 1% by weight to 10% by weight. The aqueous boric acid solution may further contain an iodide such as potassium iodide, or a zinc compound such as zinc sulfate or zinc chloride.

[0046] The crosslinking step can be carried out by any appropriate method. For example, a method of immersing a PVA-based resin film in an aqueous solution containing a boron compound, a method of applying an aqueous solution containing a boron compound to a PVA-based resin film, or a method of spraying an aqueous solution containing a boron compound to a PVA-based resin film can be mentioned. Immersion in an aqueous solution containing a boron compound is preferred.

[0047] The temperature of the solution used for crosslinking is, for example, 25° C. or higher, preferably 30° C. to 85° C., and more preferably 40° C. to 70° C. The immersion time is, for example, 5 seconds to 800 seconds, and preferably 8 seconds to 500 seconds.

[0048] (Cleaning process) The washing step is typically carried out after the crosslinking step. The washing step is typically carried out by immersing the PVA resin film in a washing solution. A typical example of the washing solution is pure water. Potassium iodide may be added to the pure water.

[0049] The temperature of the cleaning liquid is, for example, 5° C. to 50° C. The immersion time is, for example, 1 second to 300 seconds.

[0050] (drying process) The drying step can be performed by any appropriate method. Examples of drying methods include natural drying, air drying, reduced-pressure drying, and heat drying. Heat drying is preferably used. When heat drying is performed, the heating temperature is, for example, 30°C to 100°C from the viewpoint of shortening the drying time. In another embodiment, the heating temperature is preferably 50°C or less, more preferably 45°C or less, and even more preferably 40°C or less. The lower limit of the heating temperature is not particularly limited, but is the lowest temperature that can be set in a heat drying device. For example, it is 30°C. By setting the heating temperature in the drying step within this range, the free boric acid content of the polarizer can be adjusted to fall within a predetermined range. The drying time is, for example, 20 seconds to 10 minutes. In one embodiment, heat drying is performed in two or more stages. In this case, the heating temperature in at least one stage is preferably within the above range. When heat drying is performed, setting the heating temperature within the above range can provide a polarizer with excellent heat resistance.

[0051] F-2. Polarizing plate A resin film serving as a protective layer is attached to the surface (the surface opposite to the resin substrate) of the polarizer obtained in F-1 above. The resin substrate is then peeled off to obtain a polarizing plate having a protective layer / polarizer configuration. If necessary, a resin film serving as another protective layer may be attached to the peeled surface.

[0052] F-3. Optical laminate A pressure-sensitive adhesive layer is formed on the polarizer side of the polarizing plate obtained in F-2 above, and a separator is temporarily and releasably attached to the surface of the pressure-sensitive adhesive layer. Furthermore, a surface protection film is temporarily and releasably attached to the surface of the polarizing plate opposite the pressure-sensitive adhesive layer, thereby obtaining an optical laminate 100. [Example]

[0053] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring each property are as follows.

[0054] (1) Transportability During the process of conveying the polarizing plate while the surface of the polarizing plate is in contact with the guide roll, the polarizing plate is visually inspected for folds, scratches, etc. The conveying speed was set to 5 m / min to 30 m / min. 〇: Can be transported without any problems. △: The film is caught in the roll during transport, but no breaks or scratches occur. ×: The product is caught in the roll during transport, causing breakage, scratches, etc. (2) Evaluation of surface protection film peeling A tape (Cellotape (registered trademark) CT-24, manufactured by Nichiban Co., Ltd.) is applied to a corner of the surface protection film, and the peeling state is visually confirmed when the surface protection film is peeled off. ◯: The surface protection film can be peeled off without any problems. △: In rare cases, the surface protection film does not adhere to the tape. The success rate is 80% to 100%. ×: The surface protection film does not adhere to the trigger tape. The success rate is less than 80%. Even if the surface protection film can be peeled off, the separator lifts and the polarizing plate delaminates. (3) Evaluation of separator peeling A tape (Cellotape (registered trademark) CT-24, manufactured by Nichiban Co., Ltd.) is applied to the corner of the separator, and the state of peeling is visually confirmed when peeling off the separator. ○: The separator can be peeled off without any problems. △: In rare cases, the separator film does not adhere to the trigger tape. The success rate is 80% to 100%. ×: The separator film does not adhere to the trigger tape. The success rate is 80% or less. Or, peeling occurs between the surface protection film and the polarizing plate. (4) Peeling strength of surface protection film The optical laminate was cut into a size of 25 mm x 150 mm, and after peeling off the separator, it was attached so that the adhesive layer surface was in contact with glass. The stress (N / 25 mm) was measured when the surface protection film was peeled off in a 90° direction at a rate of 300 mm / min using an adhesive film peeling analyzer (manufactured by Kyowa Interface Science Co., Ltd., model: VPA-2). The measurement temperature was 25°C. (5) Separator peeling force The optical laminate was cut to a size of 25 mm x 150 mm and attached to a glass sheet with double-sided tape (Nitto Denko Corporation, No. 500) so that the surface protective film and the double-sided tape were in contact. The separator was peeled in a 90° direction at a rate of 300 mm / min using an adhesive film peeling analyzer (Kyowa Interface Science Co., Ltd., Model: VPA-2) to measure the stress (N / 25 mm). The measurement temperature was 25°C.

[0055] [Example 1] The thermoplastic resin substrate was an amorphous isophthalic acid-co-polyethylene terephthalate (IPA-co-PET) film (thickness: 100 μm) with a water absorption rate of 0.75% and a Tg of 75°C. One side of the substrate was subjected to a corona treatment, and an aqueous solution containing polyvinyl alcohol (degree of polymerization 4200, degree of saponification 99.2 mol%) and acetoacetyl-modified PVA (degree of polymerization 1200, degree of acetoacetyl-modification 4.6%, degree of saponification ≥99.0 mol%, manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIMER Z200") in a 9:1 ratio was applied to the corona-treated surface and dried at 25°C to form an 11 μm-thick PVA-based resin layer, producing a laminate. The obtained laminate was stretched in air at 140° C. by 4.5 times in a direction perpendicular to the longitudinal direction of the laminate using a tenter stretching machine (stretching treatment). Next, the laminate was immersed in a dye bath (aqueous solution with an iodine concentration of 1.4 wt % and a potassium iodide concentration of 9.8 wt %) at a liquid temperature of 25° C. for 12 seconds to be dyed (dyeing treatment). Next, the laminate was immersed in a cleaning bath (pure water) at a liquid temperature of 25° C. for 6 seconds (first cleaning treatment). Next, the substrate was immersed in a crosslinking bath (aqueous solution containing 1% by weight of boron and 1% by weight of potassium iodide) at a liquid temperature of 60° C. for 16 seconds (crosslinking treatment). Next, the laminate was immersed in a cleaning bath (aqueous solution with a potassium iodide concentration of 1% by weight) at a liquid temperature of 25° C. for 3 seconds (second cleaning treatment). The laminate was then dried in an oven at 40° C. for 8 seconds (first drying treatment). Finally, the laminate was dried in an oven at 40°C for 13 seconds (second drying treatment) to obtain a laminate (polarizing plate) having a 1.2µm-thick PVA-based resin layer (polarizer). The iodine content of the obtained polarizer was 18.6% by weight, and the single transmittance was 39.9%. A pressure-sensitive adhesive layer was formed on the polarizer-side surface of the polarizing plate obtained above, and a separator was temporarily and releasably attached to the surface of the pressure-sensitive adhesive layer. Furthermore, a surface protection film was temporarily and releasably attached to the surface of the polarizing plate opposite the pressure-sensitive adhesive layer to obtain an optical laminate. The obtained optical laminate was subjected to the above-mentioned evaluations (1) to (3). The results are shown in Table 1.

[0056] [Examples 2 to 12 and Comparative Examples 1 to 10] An optical laminate was obtained in the same manner as in Example 1, except that the thickness, peel strength, and elastic modulus of the surface protective film, and the thickness and peel strength of the separator were changed as shown in Table 1. The obtained optical laminate was subjected to the same evaluations as in Example 1. The results are shown in Table 1. [Table 1]

[0057] As is clear from Table 1, the optical laminates of the examples of the present invention (particularly Example 1) are excellent in transportability, and are also excellent in the releasability of the surface protective film and the releasability of the separator. Comparative Example 1 shows that if the thickness of the surface protection film is less than 40 μm, the conveying properties become insufficient. Comparative Examples 2 and 5 show that if the peeling force of the surface protection film exceeds 0.50 N / 25 mm, delamination occurs when the surface protection film is peeled off. Comparative Examples 3 and 4 show that if the peeling force of the surface protection film is less than 0.10 N / 25 mm, lifting of the surface protection film occurs when the separator is peeled off. Comparative Example 9 shows that if the modulus of elasticity of the surface protection film is 2.00×10 9 It can be seen that if the separator thickness is less than 35 μm, wrinkles will occur during conveyance. Furthermore, Comparative Examples 6 and 7 show that if the separator thickness is less than 35 μm, conveyance will be insufficient, and Comparative Example 10 shows that if the separator thickness exceeds 80 μm, pickup failure will occur when the separator is peeled off. Comparative Example 8 shows that if the separator peeling force exceeds 0.28 N / 25 mm, pickup failure will occur when the separator is peeled off. [Industrial Applicability]

[0058] The optical layered body of the present invention can be suitably used in image display devices. [Explanation of symbols]

[0059] 10 Surface protection film 20 Polarizing plate 21 Protective layer 22 Polarizer 30 adhesive layer 40 Separator 100 Optical laminate

Claims

[Claim 1] a polarizing plate, a pressure-sensitive adhesive layer provided on one side of the polarizing plate, a separator releasably and temporarily attached to the pressure-sensitive adhesive layer on the opposite side to the polarizing plate, and a surface protective film releasably and temporarily attached to the polarizing plate on the opposite side to the pressure-sensitive adhesive layer, The thickness of the polarizing plate is 60 μm or less, The thickness of the surface protective film is 40 μm to 87 μm, The peel strength of the surface protective film is 0.10 N / 25 mm to 0.50 N / 25 mm; The elastic modulus of the surface protection film is 2.00×10 9 Pa ~ 3.91 x 10 9 Pa, The thickness of the separator is 35 μm to 60 μm, The peel strength of the separator is 0.15 N / 25 mm or less. Optical laminate.

Citation Information

Patent Citations

  • JP1975048120A

  • Manufacturing method of roll-shaped circularly polarizing plate, organic electroluminescence display device and lateral electric field type switching mode type liquid crystal display device

    JP2013156391A