Surface protective film
A surface protection film for optical components addresses contamination and peeling voltage issues by applying antistatic agents only to the adhesive layer surface and using a dimethylpolysiloxane-based release film, ensuring reliable protection and efficient production.
Patent Information
- Application Number
- JP2024150713
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2036-02-16
AI Technical Summary
Existing surface protection films for optical components face issues with contamination of adherends, peeling voltage, and adhesion problems, especially when used on uneven surfaces, due to the migration of antistatic agents and changes in adhesive properties over time.
A surface protection film is developed with an adhesive layer coated without antistatic agents, where an appropriate amount of antistatic agent is applied to the adhesive layer surface, and a release film with a dimethylpolysiloxane-based release agent layer containing an antistatic auxiliary agent is laminated, reducing peeling voltage and contamination.
The film maintains low peeling voltage and minimal contamination over time, ensuring reliable protection of optical components without adhesive residue, improving production efficiency and yield.
Smart Images

Figure 2024159976000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface protection film that is attached to the surface of an optical component (hereinafter, also referred to as an optical film) such as a polarizing plate, a retardation plate, a lens film for a display, etc. More specifically, the present invention provides a surface protection film that causes little contamination of an adherend, and further, a surface protection film that does not deteriorate over time and has excellent antistatic performance upon peeling, and an optical component using the same. [Background technology]
[0002] Conventionally, when optical films such as polarizing plates, retardation plates, lens films for displays, antireflection films, hard coat films, transparent conductive films for touch panels, and other optical products such as displays using the same are manufactured and transported, a surface protective film is attached to the surface of the optical film to prevent the surface from being soiled or scratched in later processes. In order to improve work efficiency by eliminating the need to peel off the surface protective film and reattach it, the appearance inspection of the optical film, which is a product, is sometimes performed with the surface protective film attached to the optical film.
[0003] Generally, a surface protection film having an adhesive layer on one side of a base film is used in the manufacturing process of optical products to prevent scratches and dirt from adhering. The surface protection film is attached to the optical film via an adhesive layer having a weak adhesive strength. The adhesive layer has a weak adhesive strength so that the used surface protection film can be easily peeled off when peeled off and removed from the surface of the optical film, and the adhesive does not adhere to and remain on the optical film of the product that is the adherend (so-called, to prevent the occurrence of adhesive residue).
[0004] In recent years, during the production process of liquid crystal display panels, there have been rare cases where the peeling charge voltage that is generated when peeling off and removing the surface protection film that has been laminated on top of the optical film has destroyed circuit components such as driver ICs that control the display screen of the liquid crystal display panel, or damaged the alignment of liquid crystal molecules. In addition, in order to reduce the power consumption of liquid crystal display panels, the driving voltage of liquid crystal materials has been lowered, and as a result, the breakdown voltage of driver ICs has also been lowered. Recently, there has been a demand for the peeling electrification voltage to be within the range of +0.7kV to -0.7kV.
[0005] In recent years, with the spread of 3D displays (stereoscopic displays), there are some in which an FPR (Film Patterned Retarder) film is laminated to the surface of an optical film such as a polarizing plate. The FPR film is laminated after peeling off the surface protective film that was laminated to the surface of the optical film such as a polarizing plate. However, if the surface of the optical film such as a polarizing plate is contaminated by the adhesive or antistatic agent used in the surface protective film, there is a problem that the FPR film is difficult to adhere. For this reason, surface protective films used for such applications are required to be ones that cause little contamination to the adherend.
[0006] In addition, some liquid crystal panel manufacturers have adopted a method for evaluating the fouling property of a surface protective film on an adherend, in which the surface protective film attached to an optical film such as a polarizing plate is once peeled off, reattached in a state in which air bubbles are mixed in, heat-treated under a specified condition, and then the surface protective film is peeled off to observe the surface of the adherend. In this evaluation method, even if the surface contamination of the adherend is small, if there is a difference in the surface contamination of the adherend between the part where the air bubbles are mixed in and the part where the adhesive of the surface protective film was in contact, the mark of the air bubbles (sometimes called air bubble stains) remains. Therefore, this is a very strict evaluation method for evaluating the fouling property on the surface of the adherend. In recent years, there has been a demand for a surface protective film that does not have any problem with fouling property on the surface of the adherend even in the results of such a strict evaluation method.
[0007] In order to prevent problems caused by high peeling electrification voltage when peeling a surface protection film from an optical film to be adhered, a surface protection film has been proposed that uses a pressure-sensitive adhesive layer containing an antistatic agent to keep the peeling electrification voltage low.
[0008] For example, Patent Document 1 discloses a surface protection film that uses a pressure-sensitive adhesive made of an alkyltrimethylammonium salt, a hydroxyl group-containing acrylic polymer, and a polyisocyanate. Furthermore, Patent Document 2 discloses a pressure-sensitive adhesive composition comprising an ionic liquid and an acrylic polymer having an acid value of 1.0 or less, and pressure-sensitive adhesive sheets using the same. Furthermore, Patent Document 3 discloses a pressure-sensitive adhesive composition comprising an acrylic polymer, a polyether polyol compound, and an alkali metal salt treated with an anion-adsorbing compound, and a surface protection film using the same. Furthermore, Patent Document 4 discloses a pressure-sensitive adhesive composition comprising an ionic liquid, an alkali metal salt, and a polymer having a glass transition temperature of 0° C. or lower, and a surface protection film using the same. Furthermore, Patent Document 5 discloses a pressure-sensitive adhesive composition and a pressure-sensitive adhesive sheet for use in a surface protection sheet for optical members, which is made of a polymer containing a liquid ionic salt. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2005-131957 A [Patent Document 2] JP 2005-330464 A [Patent Document 3] JP 2005-314476 A [Patent Document 4] JP 2006-152235 A [Patent Document 5] JP 2008-069261 A Summary of the Invention [Problem to be solved by the invention]
[0010] In the above Patent Documents 1 to 5, an antistatic agent is added to the inside of the adhesive layer. However, as the thickness of the adhesive layer increases, and as time passes after the surface protection film is attached to the adherend, the amount of the antistatic agent that migrates from the adhesive layer to the adherend increases. If the amount of the antistatic agent that migrates to the adherend increases, the appearance quality of the optical film that is the adherend may decrease, or the adhesiveness of the FPR film may decrease when the FPR film is attached.
[0011] If the thickness of the adhesive layer is reduced in order to reduce the increase over time of the antistatic agent that migrates from the adhesive layer to the adherend, other problems arise. For example, when the adhesive layer is used for an optical film having an uneven surface, such as a polarizing plate that has been antiglare-treated to prevent glare, the adhesive layer cannot conform to the unevenness of the optical film surface, causing air bubbles to be mixed in, or the adhesive area between the optical film and the adhesive layer is reduced, causing the adhesive strength to decrease, resulting in the surface protection film floating or peeling off during use.
[0012] For this reason, there is a demand for a surface protection film for use with optical films, which can be used even on optical films having uneven surfaces, which causes very little contamination of the adherend and does not increase the contamination of the adherend over time, and which has a low peeling electrification voltage when the surface protection film is peeled off from the adherend.
[0013] The present inventors have conducted extensive research into this issue. In order to reduce the staining of the adherend and to reduce the increase in staining over time, it is necessary to reduce the amount of the antistatic agent component in the adhesive layer, which is assumed to stain the adherend. However, if the amount of the antistatic agent component in the adhesive layer is reduced, the peeling electrification voltage increases when the surface protection film is peeled off from the adherend. Therefore, a method for suppressing the peeling electrification voltage when the surface protection film is peeled off from the adherend without increasing the absolute amount of the antistatic agent component in the adhesive layer was investigated. As a result, they discovered that, rather than forming an adhesive layer by coating and drying an adhesive composition containing an antistatic agent on one side of a base film, by coating and drying an adhesive composition not containing an antistatic agent to laminate an adhesive layer, and then applying an appropriate amount of an antistatic agent component only to the surface of the adhesive layer, it is possible to keep the peeling electrification voltage low when peeling the surface protection film from the optical film to be adhered, and thus completed the present invention.
[0014] The present invention has been made in consideration of the above circumstances, and has an object to provide a surface protection film that can be used on optical films having uneven surfaces, causes little contamination to adherends, and whose low contamination properties to adherends do not change over time, and that does not deteriorate over time and has excellent antistatic performance against peeling, and an optical component using the same. [Means for solving the problem]
[0015] In order to solve the above problems, the surface protection film of the present invention has the technical idea of coating and drying an adhesive composition that does not contain an antistatic agent on one side of a base film to laminate an adhesive layer, and then applying an appropriate amount of antistatic agent to the surface of the adhesive layer, thereby minimizing the contamination of the adherend and minimizing the peeling electrification voltage when peeled off from the adherend, which is the optical film.
[0016] In order to solve the above problems, the present invention provides a surface protection film comprising a base film made of a transparent resin having a pressure-sensitive adhesive layer formed on one side thereof, and a release film having a release agent layer laminated onto the pressure-sensitive adhesive layer, the release film comprising a resin film having a release agent layer laminated on one side thereof, the release agent layer containing a release agent mainly composed of dimethylpolysiloxane, an antistatic agent that does not react with the release agent, and an antistatic auxiliary, the antistatic agent component being an ionic compound having a melting point of less than 30°C, the antistatic auxiliary being a polyether-modified silicone, the antistatic agent component and the antistatic auxiliary being transferred from the release agent layer of the release film to the surface of the pressure-sensitive adhesive layer, and the peeling electrification voltage when the pressure-sensitive adhesive layer is peeled off from an adherend is reduced.
[0017] The pressure-sensitive adhesive layer is preferably formed by crosslinking a pressure-sensitive adhesive composition containing a (meth)acrylate copolymer and a crosslinking agent.
[0018] It is also preferable that the peeling force required to peel the release film from the pressure-sensitive adhesive layer is 0.2 N / 50 mm or less.
[0019] The present invention also provides an optical component having the above-mentioned surface protection film attached thereto. Effect of the Invention
[0020] The surface protective film of the present invention causes little contamination of the adherend, and the low contamination of the adherend does not change even with time. In addition, the surface protective film of the present invention can be used even if the adherend is an optical film having an uneven surface such as an AG polarizing plate. In addition, according to the present invention, the peeling electrification voltage generated when peeling from the adherend, i.e., the optical film, can be kept low, and a surface protective film having excellent peeling antistatic performance without deterioration with time, and an optical component using the same can be provided. According to the surface protective film of the present invention, the surface of the optical film can be reliably protected, and therefore the productivity and yield can be improved. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a cross-sectional view illustrating the concept of a surface protection film of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing a state in which the release film has been peeled off from the surface protective film of the present invention. [Diagram 3] FIG. 1 is a cross-sectional view showing one embodiment of an optical component according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, the present invention will be described in detail based on the embodiments. Fig. 1 is a cross-sectional view showing the concept of the surface protection film of the present invention. This surface protection film 10 has a pressure-sensitive adhesive layer 2 formed on one surface of a transparent base film 1. A release film 5 having a release agent layer 4 formed on the surface of a resin film 3 is attached to the surface of this pressure-sensitive adhesive layer 2.
[0023] The substrate film 1 used in the surface protection film 10 according to the present invention is made of a transparent and flexible resin. This allows the appearance inspection of the optical component to be performed while the surface protection film is attached to the optical component to be adhered. The film made of a transparent resin used as the substrate film 1 is preferably a polyester film such as polyethylene terephthalate, polyethylene naphthalate, polyethylene isophthalate, or polybutylene terephthalate. In addition to polyester films, films made of other resins can also be used as long as they have the necessary strength and optical suitability. The substrate film 1 may be a non-stretched film or a uniaxially or biaxially stretched film. The stretching ratio of the stretched film and the axial orientation angle formed by the crystallization of the stretched film may be controlled to a specific value. The thickness of the substrate film 1 used in the surface protection film 10 according to the present invention is not particularly limited, but is preferably about 12 to 100 μm, and more preferably about 20 to 50 μm for ease of handling. If necessary, an antifouling layer for preventing surface staining, an antistatic layer, a hard coat layer for preventing scratches, etc. may be provided on the surface of the base film 1 opposite to the surface on which the pressure-sensitive adhesive layer 2 is formed. The surface of the base film 1 may also be subjected to an easy-adhesion treatment such as surface modification by corona discharge or application of an anchor coating agent.
[0024] Furthermore, the adhesive layer 2 used in the surface protection film 10 of the present invention is not particularly limited as long as it adheres to the surface of the adherend, can be easily peeled off after use, and is not likely to contaminate the adherend. However, taking into consideration durability after application to an optical film, it is common to use an adhesive made by crosslinking a (meth)acrylate copolymer.
[0025] Examples of the (meth)acrylate copolymer include a copolymer obtained by copolymerizing a main monomer such as n-butyl acrylate, 2-ethylhexyl acrylate, isooctyl acrylate, or isononyl acrylate with a comonomer such as acrylonitrile, vinyl acetate, methyl methacrylate, or ethyl acrylate, a functional monomer such as acrylic acid, methacrylic acid, hydroxyethyl acrylate, hydroxybutyl acrylate, glycidyl methacrylate, or N-methylol methacrylamide, or a monomer containing a polyoxyalkylene group such as methoxypolyethylene glycol methacrylate. The (meth)acrylate copolymer may contain all of the main monomer and other monomers as (meth)acrylates, or may contain one or more monomers other than (meth)acrylates as monomers other than the main monomer. The monomers other than the main monomer can be selected from the above-mentioned comonomers, functional monomers, and monomers containing a polyoxyalkylene group without any particular limitation.
[0026] Examples of the curing agent added to the adhesive layer 2 include crosslinking agents that crosslink the (meth)acrylate copolymer, such as isocyanate compounds, epoxy compounds, melamine compounds, metal chelate compounds, etc. Examples of the tackifier include rosin-based, coumarone-indene-based, terpene-based, petroleum-based, and phenol-based agents.
[0027] The thickness of the adhesive layer 2 used in the surface protection film 10 according to the present invention is not particularly limited, but is preferably about 5 to 40 μm, and more preferably about 10 to 30 μm. In addition, the adhesive layer 2 preferably has a peel strength (adhesive strength) of the surface protection film to the surface of the adherend of about 0.03 to 0.3 N / 25 mm, which is a weak adhesive strength, because this provides excellent operability when peeling the surface protection film from the adherend. In addition, in order to provide excellent operability when peeling the release film 5 from the surface protection film 10, the peel strength when peeling the release film 5 from the adhesive layer 2 is preferably 0.2 N / 50 mm or less, and more preferably 0.14 N / 50 mm or less.
[0028] Furthermore, the release film 5 used in the surface protective film 10 according to the present invention has a release agent layer 4 containing a release agent mainly composed of dimethylpolysiloxane, an antistatic agent that does not react with the release agent, and an antistatic auxiliary laminated on one side of a resin film 3. In the release film used in the surface protective film according to the present invention, it is preferable that the antistatic agent component is an ionic compound having a melting point of less than 30° C., and the antistatic auxiliary is polyether-modified silicone.
[0029] Examples of the resin film 3 include polyester film, polyamide film, polyethylene film, polypropylene film, and polyimide film, among which polyester film is particularly preferred due to its excellent transparency and relatively low price. The resin film may be a non-stretched film or a uniaxially or biaxially stretched film. In addition, the stretching ratio of the stretched film and the axial orientation angle formed by the crystallization of the stretched film may be controlled to a specific value. The thickness of the resin film 3 is not particularly limited, but is preferably about 12 to 100 μm, and more preferably about 16 to 50 μm for ease of handling. If necessary, the surface of the resin film 3 may be subjected to a treatment for improving adhesion, such as surface modification by corona discharge or application of an anchor coating agent.
[0030] The release agent mainly composed of dimethylpolysiloxane constituting the release agent layer 4 includes known silicone-based release agents such as addition reaction type, condensation reaction type, cationic polymerization type, and radical polymerization type. Examples of products commercially available as addition reaction type silicone-based release agents include KS-776A, KS-847T, KS-779H, KS-837, KS-778, and KS-830 (manufactured by Shin-Etsu Chemical Co., Ltd.), SRX-211, SRX-345, SRX-357, SD7333, SD7220, SD7223, LTC-300B, LTC-350G, and LTC-310 (manufactured by Dow Corning Toray Co., Ltd.). Examples of products commercially available as condensation reaction type release agents include SRX-290 and SYLOFF-23 (manufactured by Dow Corning Toray Co., Ltd.). Examples of commercially available cationic polymerization products include TPR-6501, TPR-6500, UV9300, VU9315, UV9430 (manufactured by Momentive Performance Materials, Inc.), and X62-7622 (manufactured by Shin-Etsu Chemical Co., Ltd.). Examples of commercially available radical polymerization products include X62-7205 (manufactured by Shin-Etsu Chemical Co., Ltd.).
[0031] The antistatic agent constituting the release agent layer 4 is preferably one that has good dispersibility in a release agent solution mainly composed of dimethylpolysiloxane and does not inhibit the hardening of the release agent mainly composed of dimethylpolysiloxane. In addition, since the antistatic agent is transferred from the release agent layer 4 to the surface of the adhesive layer 2 and imparts antistatic properties to the adhesive layer 2, it is preferable that the antistatic agent does not react with the release agent mainly composed of dimethylpolysiloxane. As such an antistatic agent, an ionic compound having a melting point of less than 30°C is preferable.
[0032] The ionic compound having a melting point of less than 30° C. is an ionic compound having a cation and an anion, and the cation may be a cyclic amidine ion such as an imidazolium ion, a pyridinium ion, an ammonium ion, a sulfonium ion, a phosphonium ion, or the like. The anion may be, for example, a C n H 2n+1 COO - , C n F 2n+1 COO - , NO3 - , C n F 2n+1 SO3 - , (C n F 2n+1 SO2)2N - , (C n F 2n+1 SO2)3C - , PO4 3- , AlCl4 - , Al2Cl7 - , ClO4 - , BF4 - , PF6 - , AsF6 - , SbF6 - etc. The amount of antistatic agent added to the release agent containing dimethylpolysiloxane as the main component varies depending on the type of antistatic agent and the degree of affinity with the release agent. The amount of antistatic agent added may be set in consideration of the desired peeling electrification voltage, staining property on the adherend, adhesive properties, etc. when the surface protection film is peeled off from the adherend.
[0033] The antistatic aid constituting the release agent layer 4 is used to improve the antistatic properties of the surface of the pressure-sensitive adhesive layer. Polyether-modified silicone is suitable as such an antistatic aid. The polyether chain in the polyether-modified silicone is composed of ethylene oxide, propylene oxide, etc., and by selecting the molecular weight of the polyethylene oxide used in the side chain, for example, the compatibility with the silicone release agent and physical properties such as antistatic effect can be adjusted. In addition, examples of commercially available polyether-modified silicone products include KF-351A, KF-352A, KF-353, KF-354L, KF-355A, and KF-642 (manufactured by Shin-Etsu Chemical Co., Ltd.), SH8400, SH8700, and SF8410 (manufactured by Dow Corning Toray Co., Ltd.), TSF-4440, TSF-4441, TSF-4445, TSF-4446, and TSF-4450 (manufactured by Momentive Performance Materials), BYK-300, BYK-306, BYK-307, BYK-320, BYK-325, and BYK-330 (manufactured by BYK-Chemie). The amount of polyether-modified silicone added to a release agent containing dimethylpolysiloxane as a main component varies depending on the type of polyether-modified silicone and the degree of compatibility with the release agent, but can be set taking into consideration the desired peeling electrification voltage, contamination of the adherend, and adhesive properties when the surface protection film is peeled off from the adherend.
[0034] There is no particular limitation on the method of mixing the release agent mainly composed of dimethylpolysiloxane with the antistatic agent and the antistatic auxiliary. Any method may be used, such as a method of adding the antistatic agent and the antistatic auxiliary to the release agent mainly composed of dimethylpolysiloxane, mixing them, and then adding and mixing a catalyst for hardening the release agent, a method of diluting the release agent mainly composed of dimethylpolysiloxane with an organic solvent in advance, and then adding and mixing the antistatic agent, the antistatic auxiliary, and the catalyst for hardening the release agent, or a method of diluting the release agent mainly composed of dimethylpolysiloxane with an organic solvent in advance, adding and mixing the catalyst, and then adding and mixing the antistatic agent and the antistatic auxiliary. In addition, if necessary, a material that aids the antistatic effect, such as an adhesion improver such as a silane coupling agent or a compound containing a polyoxyalkylene group, may be added.
[0035] The mixing ratio of the release agent mainly composed of dimethylpolysiloxane to the antistatic agent and the antistatic auxiliary is not particularly limited, but the ratio of the total of the antistatic agent and the antistatic auxiliary as solids to 100 of the solids of the release agent mainly composed of dimethylpolysiloxane is preferably about 5 to 100. If the total amount of the antistatic agent and the antistatic auxiliary added in terms of solids is less than 5 to 100 of the solids of the release agent mainly composed of dimethylpolysiloxane, the amount of the antistatic agent and the antistatic auxiliary transferred to the surface of the adhesive layer is also reduced, making it difficult for the adhesive to exhibit its antistatic function. In addition, if the total amount of the antistatic agent and the antistatic auxiliary added in terms of solids exceeds 100 to 100 of the solids of the release agent mainly composed of dimethylpolysiloxane, the release agent mainly composed of dimethylpolysiloxane is also transferred to the surface of the adhesive layer together with the antistatic agent and the antistatic auxiliary, which may reduce the adhesive properties of the adhesive.
[0036] The method for forming the adhesive layer 2 on the base film 1 of the surface protection film 10 according to the present invention and the method for laminating the release film 5 may be performed by known methods and are not particularly limited. Specifically, there may be mentioned (1) a method in which a resin composition for forming the adhesive layer 2 is applied to one side of the base film 1, dried, an adhesive layer is formed, and then the release film 5 is laminated, and (2) a method in which a resin composition for forming the adhesive layer 2 is applied to the surface of the release film 5, dried, an adhesive layer is formed, and then the base film 1 is laminated, and any of these methods may be used.
[0037] The pressure-sensitive adhesive layer 2 may be formed on the surface of the base film 1 by a known method. Specifically, known coating methods such as reverse coating, comma coating, gravure coating, slot die coating, Mayer bar coating, and air knife coating can be used.
[0038] Similarly, the release agent layer 4 may be formed on the resin film 3 by a known method. Specifically, known coating methods such as gravure coating, Mayer bar coating, and air knife coating can be used.
[0039] The surface protection film 10 according to the present invention having the above-mentioned configuration preferably has a surface potential of +0.7 kV to -0.7 kV when the pressure-sensitive adhesive layer is peeled off from the adherend, i.e., the optical film. The surface potential is more preferably +0.5 kV to -0.5 kV, and particularly preferably +0.1 kV to -0.1 kV. This surface potential can be adjusted by adjusting the types and amounts of the antistatic agent and antistatic auxiliary contained in the release agent layer.
[0040] FIG. 2 is a cross-sectional view showing a state in which the release film has been peeled off from the surface protection film of the present invention. By peeling off the release film 5 from the surface protection film 10 shown in FIG. 1, a part of the antistatic agent and antistatic auxiliary (reference numeral 7) contained in the release agent layer 4 of the release film 5 is transferred (adhered) to the surface of the adhesive layer 2 of the surface protection film 10. Therefore, in FIG. 2, the antistatic agent and antistatic auxiliary transferred to the surface of the adhesive layer 2 of the surface protection film 11 in a state in which the release film has been peeled off are shown by spots of reference numeral 7. By transferring the components 7 of the antistatic agent and antistatic auxiliary from the release film 5 to the surface of the adhesive layer 2, the peeling electrification voltage when the adhesive layer 2 is peeled off from the adherend is reduced compared to the adhesive layer 2 before transfer. The peeling electrification voltage when the adhesive layer is peeled off from the adherend can be measured by a known method. For example, after a surface protection film is attached to an adherend such as a polarizing plate, the surface protection film is peeled off at a peeling speed of 40 m per minute using a high-speed peel tester (manufactured by Tester Sangyo Co., Ltd.), while the surface potential of the adherend surface is measured every 10 ms using a surface potential meter (manufactured by Keyence Corporation). The maximum absolute value of the surface potential is measured as the peeling electrification voltage (kV). In the surface protection film according to the present invention, when the surface protection film 11 from which the release film has been peeled off as shown in Fig. 2 is attached to an adherend, the antistatic agent and antistatic auxiliary transferred from the release agent layer to the surface of the pressure-sensitive adhesive layer 2 come into contact with the surface of the adherend. This makes it possible to keep the peeling electrification voltage low when the surface protection film is peeled off from the adherend again.
[0041] FIG. 3 is a cross-sectional view showing an embodiment of an optical component according to the present invention. The release film 5 is peeled off from the surface protection film 10 of the present invention, and in a state in which the pressure-sensitive adhesive layer 2 is exposed, the surface protection film 10 is attached to an optical component 8 as an adherend via the pressure-sensitive adhesive layer 2 . That is, Fig. 3 shows an optical component 20 to which a surface protective film 11 of the present invention is attached. Examples of optical components include optical films such as a polarizing plate, a retardation plate, a lens film, a polarizing plate that also serves as a retardation plate, and a polarizing plate that also serves as a lens film. Such optical components are used as components of liquid crystal display devices such as liquid crystal display panels, optical devices of various instruments, etc. In addition, examples of optical components include optical films such as anti-reflection films, hard coat films, and transparent conductive films for touch panels. According to the optical component of the present invention, when the surface protective film 11 is peeled off from the adherend, the optical component (optical film), the peeling electrification voltage can be suppressed to a sufficiently low level. Therefore, there is no risk of damaging circuit components such as driver ICs, TFT elements, and gate line driving circuits, and the production efficiency in the process of manufacturing liquid crystal display panels and the like can be improved and the reliability of the production process can be maintained. EXAMPLES
[0042] The present invention will now be further described with reference to examples. Example 1 (Preparation of surface protection film) 5 parts by weight of addition reaction type silicone (manufactured by Dow Corning Toray Co., Ltd., product name: SRX-345), 7.5 parts by weight of 10% ethyl acetate solution of tri-n-butylmethylammonium bistrifluoromethanesulfonimide (manufactured by 3M Co., Ltd., FC-4400), an ionic compound having a melting point of 27.5°C, 0.3 parts by weight of polyether modified silicone (manufactured by Dow Corning Toray Co., Ltd., product name: SH8400), 95 parts by weight of a 1:1 mixed solvent of toluene and ethyl acetate, and 0.05 parts by weight of platinum catalyst (manufactured by Dow Corning Toray Co., Ltd., product name: SRX-212) were mixed and stirred to prepare a coating material for forming the release agent layer of Example 1. The coating material for forming the release agent layer of Example 1 was applied to the surface of a polyethylene terephthalate film having a thickness of 38 μm with a Mayer bar so that the thickness after drying was 0.2 μm, and the mixture was dried in a hot air circulating oven at 120°C for 1 minute to obtain a release film of Example 1. On the other hand, 30 parts by weight of an acrylate copolymer having a weight average molecular weight of 470,000, obtained by copolymerizing 2-ethylhexyl acrylate and 2-hydroxyethyl acrylate in a weight ratio of 96:4, was dissolved in 70 parts by weight of ethyl acetate to prepare an adhesive polymer solution (ethyl acetate solution with a solid content of 30%). To this solution, 1.2 parts by weight of an HDI-based curing agent (manufactured by Tosoh Corporation, product name: Coronate (registered trademark) HX) was added and mixed to prepare the adhesive composition of Example 1. Note that "HDI-based" means "hexamethylene diisocyanate-based". The adhesive composition of Example 1 was applied to the surface of a polyethylene terephthalate film having a thickness of 38 μm so that the thickness after drying was 20 μm, and then dried for 2 minutes in a hot air circulating oven at 100° C. to form an adhesive layer. Then, the release layer (silicone-treated surface) of the release film of Example 1 prepared above was attached to the surface of this adhesive layer. The obtained adhesive film was kept warm in an environment of 40° C. for 5 days to harden the adhesive layer, and a surface protection film of Example 1 was obtained.
[0043] Comparative Example 1 5 parts by weight of addition reaction type silicone (manufactured by Dow Corning Toray Co., Ltd., product name: SRX-345), 95 parts by weight of a 1:1 mixed solvent of toluene and ethyl acetate, and 0.05 parts by weight of a platinum catalyst (manufactured by Dow Corning Toray Co., Ltd., product name: SRX-212) were mixed and stirred / mixed to prepare a coating material for forming the release agent layer of Comparative Example 1. The coating material for forming the release agent layer of Comparative Example 1 was applied to the surface of a polyethylene terephthalate film having a thickness of 38 μm with a Mayer bar so that the thickness after drying would be 0.2 μm, and the coating material was dried in a hot air circulating oven at 120° C. for 1 minute to obtain a release film of Comparative Example 1. On the other hand, 3 parts by weight of a 10% ethyl acetate solution of tri-n-butylmethylammonium bistrifluoromethanesulfonimide (FC-4400 manufactured by 3M), an ionic compound having a melting point of 27.5°C, and 1.2 parts by weight of an HDI-based curing agent (manufactured by Tosoh Corporation, product name: Coronate (registered trademark) HX) were added to and mixed with 100 parts by weight of the adhesive polymer solution of Example 1 (ethyl acetate solution with a solid content of 30%) to prepare the adhesive composition of Comparative Example 1. The adhesive composition of Comparative Example 1 was applied to the surface of a polyethylene terephthalate film having a thickness of 38 μm so that the thickness after drying was 20 μm, and then dried in a hot air circulating oven at 100° C. for 2 minutes to form an adhesive layer. Then, the release layer (silicone-treated surface) of the release film of Comparative Example 1 prepared above was attached to the surface of this adhesive layer. The obtained adhesive film was kept warm in an environment of 40° C. for 5 days to harden the adhesive layer, and a surface protection film of Comparative Example 1 was obtained.
[0044] Comparative Example 2 The surface protection film of Comparative Example 2 was obtained in the same manner as Comparative Example 1, except that tri-n-butylmethylammonium bistrifluoromethanesulfonimide, an ionic compound having a melting point of 27.5°C, was not contained in the adhesive layer.
[0045] Comparative Example 3 A surface protection film of Comparative Example 3 was obtained in the same manner as in Example 1, except that the release agent layer did not contain polyether-modified silicone.
[0046] Example 2 The surface protection film of Example 2 was obtained in the same manner as in Example 1, except that an adhesive composition was used in place of the adhesive composition of Example 1, in which 30 parts by weight of an acrylate copolymer having a weight average molecular weight of 480,000, copolymerized with 2-ethylhexyl acrylate, butyl acrylate, and 2-hydroxyethyl acrylate in a weight ratio of 60:36:4, was dissolved in 70 parts by weight of ethyl acetate to obtain 100 parts by weight of an adhesive polymer solution (ethyl acetate solution with a solid content of 30%), to which 1.2 parts by weight of an HDI-based curing agent (manufactured by Tosoh Corporation, product name: Coronate (registered trademark) HX) was added and mixed.
[0047] Example 3 The surface protection film of Example 3 was obtained in the same manner as in Example 1, except that an adhesive composition was used in place of the adhesive composition of Example 1, in which 30 parts by weight of a (meth)acrylate copolymer having a weight average molecular weight of 380,000, copolymerized in a weight ratio of 86:10:4, was dissolved in 70 parts by weight of ethyl acetate to obtain 100 parts by weight of an adhesive polymer solution (ethyl acetate solution with a solid content of 30%), to which 1.2 parts by weight of an HDI-based curing agent (manufactured by Tosoh Corporation, product name: Coronate (registered trademark) HX) was added and mixed.
[0048] The evaluation test methods and results are shown below. <Method for measuring the peel strength of the release film> A sample of the surface protection film was cut to a width of 50 mm and a length of 150 mm. Under a test environment of 23°C x 50% RH, the strength was measured when the release film was peeled off in a 180° direction at a peeling speed of 300 mm / min using a tensile tester, and this was taken as the peel strength of the release film (N / 50 mm).
[0049] <Method for measuring adhesive strength of surface protection film> An anti-glare low reflection treated polarizing plate (AG-LR polarizing plate) was attached to the surface of the glass plate using a laminating machine with double-sided adhesive tape. After that, a surface protection film cut to a width of 25 mm was attached to the surface of the polarizing plate, and then it was stored for one day under a test environment of 23°C x 50% RH. Then, using a tensile tester, the strength was measured when the surface protection film was peeled off in the 180° direction at a peeling speed of 300 mm / min, and this was taken as the adhesive strength (N / 25 mm).
[0050] <Method for measuring the peeling electrification voltage of surface protection film> An anti-glare low reflection treated polarizing plate (AG-LR polarizing plate) was attached to the surface of a glass plate with a double-sided adhesive tape using a laminating machine. After that, a surface protection film cut to a width of 25 mm was attached to the surface of the polarizing plate, and then the polarizing plate was stored for one day under a test environment of 23°C x 50% RH. Then, the surface protection film was peeled off at a peeling speed of 40 m per minute using a high-speed peeling tester (manufactured by Tester Sangyo Co., Ltd.), and the surface potential of the polarizing plate surface was measured every 10 ms using a surface potential meter (manufactured by Keyence Corporation). The maximum absolute value of the surface potential was taken as the peeling electrification voltage (kV).
[0051] <Method for checking surface contamination of surface protection film> An anti-glare low reflection treated polarizing plate (AG-LR polarizing plate) was attached to the surface of the glass plate with a double-sided adhesive tape using a laminating machine. Then, a surface protection film cut to a width of 25 mm was attached to the surface of the polarizing plate, and the plate was stored for 3 days and 30 days under a test environment of 23°C x 50% RH. The surface protection film was then peeled off, and the presence or absence of contamination on the surface of the polarizing plate was visually observed. As the criterion for judging surface contamination, a case where no contamination was transferred to the polarizing plate was marked as (○), and a case where contamination was confirmed to be transferred to the polarizing plate was marked as (×).
[0052] The results of the measurements of the obtained surface protection films of Examples 1 to 3 and Comparative Examples 1 to 3 are shown in Tables 1 and 2. "2EHA" means 2-ethylhexyl acrylate, "HEA" means 2-hydroxyethyl acrylate, "BA" means butyl acrylate, "#400G" means methoxypolyethylene glycol (400) methacrylate, and "FC4400" means tri-n-butylmethylammonium bistrifluoromethanesulfonimide. In Tables 1 and 2, the composition of the adhesive layer is expressed in parts by weight so that the total amount of the adhesive polymer (solid content) is about 100 parts by weight. Therefore, in the adhesive layer of Comparative Example 1, the weight ratio of the adhesive polymer (solid content) to FC4400 is 30 parts by weight:0.3 parts by weight=100 parts by weight:1.0 parts by weight.
[0053] [Table 1]
[0054] [Table 2]
[0055] The measurement results shown in Tables 1 and 2 reveal the following: The surface protection films of Examples 1 to 3 according to the present invention have an appropriate adhesive strength, do not contaminate the surface of the adherend, and have a low peeling electrification voltage when the surface protection film is peeled off from the adherend. On the other hand, the surface protection film of Comparative Example 1, which contained an antistatic agent in the adhesive layer, had a low and favorable peeling electrification voltage when the surface protection film was peeled off from the adherend, but caused a lot of contamination of the adherend after peeling. In addition, the surface protection film of Comparative Example 2, in which neither the adhesive layer of the surface protection film nor the release agent layer of the release film contained an antistatic agent, had good staining properties against the adherend, but the peeling electrification voltage was high when the surface protection film was peeled off from the adherend. In other words, it is difficult to achieve both a reduction in peeling electrification voltage and staining resistance to the adherend in the surface protection film of Comparative Example 1, in which an antistatic agent is contained in the adhesive layer of the surface protection film, and the surface protection film of Comparative Example 2, in which an antistatic agent is not contained in either the adhesive layer of the surface protection film or the release agent layer of the release film. On the other hand, in the surface protection films of Examples 1 to 3, in which an antistatic agent and an antistatic auxiliary were incorporated into the release agent layer of the release film and then the antistatic agent and antistatic auxiliary of the release agent layer were transferred only to the surface of the adhesive layer, the addition of a small amount of the antistatic auxiliary had the effect of significantly reducing the peel-off electrification voltage, so there was no contamination of the adherend and the peel-off antistatic performance was also good. In addition, the surface protection film of Comparative Example 3, in which the release agent layer contained only an antistatic agent and no antistatic auxiliary, did not stain the adherend and had good antistatic performance upon peeling. However, compared with the surface protection films of Examples 1 to 3, in which the release agent layer contained an antistatic agent and an antistatic auxiliary, the peeling electrification voltage was higher. [Industrial Applicability]
[0056] The surface protection film of the present invention can be used to protect the surface of, for example, optical films such as polarizing plates, retardation plates, lens films, and other various optical components in the production process of the optical components, etc. Furthermore, the surface protection film of the present invention can reduce the amount of static electricity generated when peeled from an adherend, and reduces the change over time in antistatic performance upon peeling and the contamination of the adherend, thereby improving the yield of the production process, and is of great industrial utility. [Explanation of symbols]
[0057] Reference Signs List 1...base film, 2...adhesive layer, 3...resin film, 4...release agent layer, 5...release film, 7...antistatic agent and antistatic auxiliary, 8...adherend (optical component), 10...surface protective film, 11...surface protective film from which the release film has been removed, 20...optical component to which the surface protective film has been attached.
Claims
1. A surface protective film comprising a base film having a pressure-sensitive adhesive layer formed on one side thereof and a release film for surface protective films capable of transferring an antistatic agent bonded to the surface of the pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer is obtained by crosslinking a pressure-sensitive adhesive composition containing a (meth)acrylate copolymer and a crosslinking agent, and does not contain an antistatic agent; the release film for surface protective film is formed by laminating, on one side of a resin film, a release agent layer containing a release agent mainly composed of dimethylpolysiloxane, an antistatic agent that does not react with the release agent, and an antistatic auxiliary; the antistatic agent component is an ionic compound (but not an alkali metal salt) having a melting point of less than 30° C., the antistatic auxiliary is a polyether-modified silicone, the ionic compound is an ionic compound having a cation and an anion, when the release film for surface protective film is attached to the surface of the pressure-sensitive adhesive layer via the release agent layer, the antistatic agent component of the release agent layer and the antistatic auxiliary are transferred to the surface of the pressure-sensitive adhesive layer, A surface protection film characterized in that after the surface protection film is attached to an adherend, the surface potential when the pressure-sensitive adhesive layer of the surface protection film is peeled off from the adherend is +0.7 kV to -0.7 kV.
2. 2. The surface protective film according to claim 1, wherein the cation is one selected from the group consisting of an imidazolium ion, a pyridinium ion, an ammonium ion, a sulfonium ion, and a phosphonium ion.
Citation Information
Patent Citations
Surface protective film and optical component to which the surface protective film is laminated
JP2015039788A
Antistatic surface protective film
JP2015131414A
Surface protecting film and optical component whereon it is stuck
JP2005131957A
Adhesive composition, adhesive sheet and surface-protective film
JP2005314476A
Pressure sensitive adhesive composition and pressure sensitive adhesive sheet
JP2005330464A