Method of manufacture of curly fibers

By stretching ethylene/α-olefin interpolymers with controlled molecular weight distribution and comonomer composition, the method enhances curling properties in polyethylene-based fibers, improving the drape and smoothness of nonwoven fabrics for consumer and medical applications.

JP2024160231AActive Publication Date: 2024-11-13DOW GLOBAL TECHNOLOGIES LLC
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
JP2024112302
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-11-20
Filing Date
2024-07-12
Publication Date
2024-11-13
Estimated Expiration
2039-11-20

AI Technical Summary

Technical Problem

Existing methods for producing polyethylene-based fibers with enhanced curling properties are inefficient and lack effective means to achieve desirable drape and smoothness in nonwoven fabrics used in consumer products and medical applications.

Method used

The method involves stretching multicomponent fibers, specifically ethylene/α-olefin interpolymers with controlled molecular weight distribution and comonomer composition, to enhance curling properties by forming fibers with distinct regions that respond differently to stretching and relaxation.

Benefits of technology

The process results in fibers with improved curling properties, allowing for the production of nonwoven fabrics with enhanced drape and smoothness, suitable for use in disposable materials and medical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160231000001_ABST
    Figure 2024160231000001_ABST
Patent Text Reader

Abstract

To provide a process for forming fibers with an enhanced curling property.SOLUTION: There is provided a process comprising forming fibers having at least a first region and a second region, wherein the first region comprises an ethylene / α-olefin interpolymer composition characterized in that: a density is in a range of 0.930 to 0.965 g / cm3; a melt index (I2) is in a range of from 10 to 60 g / 10 minutes; a molecular weight distribution is in a range of from 1.5 to 2.6; a tan delta at 1 radian / second is at least 45; a low temperature peak and a high temperature peak on an elution profile via improved comonomer composition distribution (ICCD) procedure; and a full width at half maximum of the high temperature peak is less than 6.0°C and stretching the fibers to an elongation of at least 20% thereby increasing a curling property of the fiber. The process may further include forming a non-woven fabric from the fibers.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application is a continuation of U.S. Application No. 62 / 769,618, filed November 20, 2018. The benefit of which is claimed and is incorporated herein by reference in its entirety.

[0002] The field of the invention is curled fibers and methods for producing nonwoven fabrics having such fibers. and the method includes stretching. [Background technology]

[0003] Polyethylene-based fibers are used in consumer products, especially nonwoven fabrics. Such fibers are: It is desirable for its drapeability and smoothness. Nonwovens are used in filters, medical applications, It has many uses, including as waste material, diaper stock, etc. To reduce the weight of the final product. In this paper, crimping or curling of the fibers is proposed.

[0004] The present invention provides a method for forming fibers with enhanced curl (also known as crimp) and using the same. It remains desirable to be able to do this more efficiently. Summary of the Invention

[0005] The inventors have also discovered that by selecting specific materials for use in the multicomponent fibers, They discovered that stretching these fibers enhanced the curl or crimp. Thus, disclosed herein is a method for producing a medicament comprising at least a first region and a second region. The process includes forming a fiber having a first region having a viscosity of 0.930 to 0.940 mm. .965g / cm 3 Density in the range of 10~60g / 10min. I2), wherein I2 is an ethylene / α-olefin interpolymer composition characterized by A Measured by STM D1238 at 190C, 2.16kg, and measured by GPC The ratio of the weight average molecular weight to the number average molecular weight (M w(GPC) / M n(GPC) ) The molecular weight distribution is in the range of 1.5 to 2.6, and the tan delta at 1 radian / sec is small. The elution profile is at least 45 and is determined by the improved comonomer composition distribution (ICCD) method. The low and high temperature peaks on the core and the full width at half maximum of the high temperature peak are less than 6.0°C. This stretches the fiber to at least 20% elongation, thereby increasing the curl of the fiber. The process may further include forming a nonwoven fabric from the fibers, the stretching of the fibers being Stretching can occur before or after formation of the nonwoven. [Brief description of the drawings]

[0006] [Figure 1] FIG. 1 is an ICCD elution plot of the ethylene / α-olefin composition of Sample 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] Producing fibers and / or nonwoven fabrics from fibers having first and second regions Disclosed herein is an efficient method for preventing fiber curl or deformation after drawing. are characterized by different responses to stretching and relaxation such that crimp increases. One of these areas is surprisingly good when compared to certain other ethylene-based resin systems. Includes ethylene / α-olefin interpolymer compositions that provide curl or crimp. Stretching can occur before or after formation of the nonwoven.

[0008] The fibers useful in this process are said to have at least a first region and a second region. The fibers may be bicomponent fibers, or the fibers may be made up of three or more components. The fibers may have a cross section of one region surrounded by a sheath (multicomponent fiber). In multicomponent fibers, the fibers may have a core-sheath configuration, which represents one region, the core. There may be one or more inner cores, one or more inner sheaths and an outer sheath. A section of a part of the cross section, for example, a quarter, a third, or a half of the cross section, is an area. It is possible to have a segmented pie configuration where the first region occupies the remainder of the cross section. In split fibers, the third or fourth regions may occupy a portion of the pie cross section. Alternatively, the core-sheath configuration may be combined with a segmented pie. For example, the core may be , may have two components in a segmented pie structure surrounded by a sheath. Alternatively, the third component may be included within the first or second region of the sea-island structure. The portions may form a separate region within a first region that forms a core and is surrounded by a sheath. Each region of the fiber has a center of gravity, and the fiber itself also has a center of gravity. Centricity means the arithmetic average of all points in the cross-sectional area of ​​the fiber or in a particular area of ​​the fiber. In the core-sheath case, the center of gravity of the core and the sheath is the same. The first and second regions have the same weight. The center of gravity of the first and second regions may be the same as the center of gravity of the entire fiber. Alternatively, the first and second regions may have different centers of gravity. At least one of the regions has a center of gravity that is different from the center of gravity of the fiber. can be done.

[0009] Each region has a 2% secant modulus E and a yield stress σ y Different materials with The 2% secant modulus of each region, the yield strength of each region, or both are different from each other. The difference between the yield stresses of the materials in the first and second regions divided by the yield stress of the second region is At least 0.4, or at least 0.45, or at least 0.5, or at least The first and second halves may be at least 0.55 or at least 0.6, and may be no greater than 1.0. The difference between the 2% secant modulus of the material in the second region and the 2% secant modulus of the material in the second region is At least 0.4 or at least 0.45, or at least 0.5 or at least The first yield stress may be 0.55 or may be 1.0 or less. The quotient of the second yield stress divided by the second 2% secant modulus is subtracted from the quotient of the second yield stress divided by the second 2% secant modulus The absolute value of |σ y1 / E1-σ y2 / E2| / (σ y2 / E2) must be at least 0. 01, or at least 0.02, or at least 0.05, or at least 0.0 7, or at least 0.1, and may be no greater than 1.0, or no greater than 0.8, or 0. 7 or less, or 0.5 or less, or 0.4 or less, or 0.3 or less, where E1 is the 2% secant modulus of the first region material and E2 is the 2% secant modulus of the second region material. is the linear modulus, σ y1 is the yield stress of the first region material, and σ y2 is the second domain material The 2% secant modulus and yield stress were measured according to ASTM D638. It is measured on extruded samples.

[0010] Ethylene / α-olefin interpolymer composition An interpolymer is a polymer made up of two, three or more monomers. This means that the polymer is a copolymer, terpolymer, etc. The first monomer is ethylene. The second monomer is an α-olefin. The olefin has at least 3 carbon atoms, e.g., up to 20, up to 10, or Exemplary α-olefin comonomers include propylene, propylene glycol, propylene glycol terpolymer ... 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene Examples of suitable ethylene glycol ethers include, but are not limited to, 1-decene, 1-decene, and 4-methyl-1-pentene. Optionally, the third, fourth, or more monomers can be α-olefins. The interpolymer composition is bimodal and has different molecular weights, as described in more detail below. At least two different molecular weights and / or different densities and / or ICCD elution Combining two ethylene / α-olefin interpolymers having different peaks The electrochemical cell can be easily prepared by the above method.

[0011] The interpolymer can be a random interpolymer. At least 50 mole percent based on the total moles of repeat units in the terpolymer or at least 60 mole percent or at least 70 mole percent ethylene-based The interpolymer may include repeat units. 99.9 or less, or 99.5 or less, or 99 or less, based on the total moles of the unit; or less than 95, or less than 90, or less than 85 mole percent ethylene repeat units The interpolymer may comprise a total mole fraction of repeat units in the interpolymer. Based on the number, at least 0.1 or at least 0.5 or at least 1 or less At least 5 or at least 10 mole percent of α-olefin repeat units (i.e. The interpolymer may include a second and optionally a third and fourth monomer. The number of moles of repeat units in the interpolymer is 50 or less, or 30 or less. 100% or less of α-olefin repeat units (i.e., second and optionally third and and a fourth monomer).

[0012] These ethylene / α-olefin interpolymer compositions, in certain embodiments, At least 0.930 g / cm 3 and 0.965 g / cm 3 Less than or equal to 0.9 60 or less, or 0.955 or less, or 0.950 or less, or 0.945 or less, or is 0.940g / cm 3 It is characterized by the following density: Density is determined according to ASTM D79 The bicomponent containing the disclosed ethylene / α-olefin interpolymer is measured according to 2. The fibers can exhibit a higher curvature. The bimodal polymer composition has a curvature of about 0.900 to about 0.940g / cm 3 and a low density fraction having a density in the range of at least about 0.950. g / cm 3の The granular material may be characterized by a high density fraction having a density.

[0013] These ethylene / α-olefin interpolymer compositions are 10 to 60 g / 10 They can be characterized by a melt index (I2) in the range of AST min. Measured at 190°C and 2.16 kg according to M D1238. 2 may be less than 6.9 or 6.8 or 6.7, where I10 is less than AS Measured at 190°C, 10kg according to TM D1238. Lower I10 / I2 The ratio may exhibit lower long chain branching resulting in better spinnability / processability.

[0014] These ethylene / α-olefin interpolymer compositions have a molecular weight of 2.6 or less. .5 or less, and at least 1.5 or at least 1.7, or at least 2.0 The ratio of weight average molecular weight to number average molecular weight (M w(GPC) / M n(GPC) ) The polymer may be characterized by its molecular weight distribution according to the method described below. The interpolymer composition having a molecular weight distribution in the range is preferably a copolymer having a higher molecular weight distribution than the interpolymer composition having a higher molecular weight distribution. It is believed to have better processability (e.g., fiber spinning) than terpolymers. The olefin / α-olefin interpolymer has an M greater than (I10 / I2)-4.63. w( GPC) / M n(GPC) It can be characterized by:

[0015] The ethylene / α-olefin interpolymer composition is 15,000 g / mol, 20 ,000 g / mol, or a lower limit of 30,000 g / mol to 100,000 g / mol, 1 With a weight average molecular weight of 20,000 g / mol, or up to an upper limit of 150,000 g / mol It is possible. z(GPC) / M w(GPC) is less than 3.0 or less than 2.0 A bimodal polymer composition has an ICCD elution ratio of 2.0 or more. The high temperature fraction may show two different peaks below 70,000 g / mol or below 50,00 The high temperature fraction may have a peak position molecular weight of at least 15.0 g / mol or less. ,000 g / mole or at least 20,000 g / mole. The low temperature fraction may be at least 30,000, or at least 40,000, or The low temperature fraction may have a peak position molecular weight of at least 50,000 g / mol. , 250,000, or 200,000, or 150,000 g / mol or less It may have a positional molecular weight.

[0016] These ethylene / α-olefin interpolymer compositions are characterized by a tan delta of at least 45 or at least 50. In addition, these ethylene / α-olefin interpolymers have a viscosity of 1 rad / s. tan delta at 100 rad / s and 190°C vs. tan delta at 100 rad / s and 190°C The ratio of the β-amyloides to the β-amyloides is at least 12. These properties are This can be measured by dynamic mechanical analysis (DMS).

[0017] These ethylene / α-olefin interpolymer compositions include improved comonomers. - At least two of the composition distribution (ICCD) elution profiles between 35℃ and 110℃ It can be characterized by distinct peaks with distinct valleys (smaller peaks) between the peaks. (at least 10% reduction compared to the peak height of the peak) and the peak position is at least Each peak must be spaced 10° apart. A vertical line must be drawn at the lowest point of the adjacent valley. are separated by.

[0018] The peak temperature of the low temperature peak may be at least 50° C. or at least 60° C. The peak temperature of the high temperature peak may be at least 90°C or at least 95°C, 110°C, or 105°C or 100°C The present inventors have found that a low-temperature peak in the range of 50 to 75° C. produces curled fibers. It has been found that this can be particularly useful in preparing

[0019] The weight fraction of the low temperature peak fraction is at least 25 or at least 30 and less than 65, or less than 60 or 55 weight percent The weight fraction of the high temperature peak fraction may be less than or equal to the total weight of the eluted polymer. , at least 35 or at least 40, or at least 45 and 75 weight percent The value can be less than 10 ...

[0020] The full width at half maximum of the high temperature peak may be less than 6.0° C. The narrow peak of the high density fraction is Very high or very low molecular weight species that can interfere with performance or produce extractables It shows a narrower composition distribution than the conventional one.

[0021] The ethylene / alpha olefin composition is less than 0.5 (i.e., less than 50%), 0.3 (3 0%), 0.25 (25%), 0.22 (22%), or 0.2 (2 0%).

[0022] The ethylene / α-olefin interpolymer composition has a molecular weight of less than 100, preferably less than 30 It may have a comonomer distribution constant (CDC) of .about.80.

[0023] The ethylene / α-olefin interpolymer composition has a molecular weight of greater than 0.20 or greater than 0. More than .25, or more than .30, or more than .35, or more than .40 or a molecular weighted comonomer distribution index greater than 0.45 or greater than 0.50 The MWCDI can be characterized by the conventional gel permeation chromatograph. is a measure of the slope of comonomer incorporation as a function of molecular weight obtained from chromatographic analysis. When MWCDI is greater than 0.25 (molecular weight range 20,000-200,000 g / mol), the resin structure has significant comonomer incorporation towards the higher molecular weight end of the distribution. It is believed to have incorporation of reverse comonomers.

[0024] The ethylene / α-olefin interpolymer compositions disclosed herein contain small amounts of long It can be characterized by the amount of chain branching (LCB), which is the zero shear viscosity ratio (ZSV R) is low. Specifically, ZSVR is less than 1.35 or less than 1.30. Possible. ZSVR is likely to be at least 1.10.

[0025] The ethylene / α-olefin interpolymer composition comprises 1 Determined by H-NMR less than 230, or less than 210, or less than 190, or less than 170, or less than 15 It can be characterized by a vinyl saturation number per 1,000,000 carbon atoms less than 0. Cut.

[0026] Ethylene / α-olefin interpolymer compositions can be prepared using any conventional polymerization process. Such a conventional polymerization process may include one or more conventional reactors. , for example, loop reactors, isothermal reactors, stirred tank reactors, parallel and series batch reactors, and / or any combination thereof, Such polymerization processes include, but are not limited to, those known in the art. Any type of reactor or reactor configuration may be used to perform gas phase, solution, or slurry polymerization. or any combination thereof.

[0027] Generally, the solution phase polymerization process is carried out at a temperature in the range of 115 to 250°C, for example, 115 to 200°C. At temperatures in the range of 300 to 1000 psi, e.g., 400 to 750 psi. , one or more well-stirred reactors, for example, one or more isothermal loop reactors or one In a double reactor, for example, the temperature in the first reactor is 1 The second reactor temperature may range from 15 to 190° C., or from 115 to 150° C. The temperature may be in the range of 50 to 200° C., or 170 to 195° C. In a single reactor, The temperature in the reactor can range from 115 to 190°C, or from 115 to 150°C. The residence time in the phase polymerization process is typically 2 to 30 minutes, for example 10 to 20 minutes. The catalyst comprises ethylene, a solvent, hydrogen, one or more catalyst systems, optionally one or more cocatalysts, and and optionally one or more comonomers are continuously fed into one or more reactors. Examples of solvents include, but are not limited to, isoparaffins. Solvents were purchased from ExxonMobil Chemical Co. (Houston, Tex.). The resulting ethylene / α-olefin copolymer is commercially available from Epson under the name ISOPAR E. The mixture of ethylene / α-olefin interpolymer and solvent is removed from the reactor. The solvent is typically recovered in a solvent recovery unit, i.e., a heat exchanger, and then the resulting copolymer is isolated. It is recovered via an exchanger and a gas-liquid separator drum and then recycled to the polymerization system.

[0028] The ethylene / α-olefin interpolymer compositions can be produced in a dual reactor system, e.g. It can be produced by solution polymerization in a loop reactor system, where ethylene and and optionally one or more α-olefins are polymerized in the presence of one or more cocatalysts. In addition, one or more promoters may be present.

[0029] Ethylene / α-olefin interpolymers can be produced in a single reactor system, e.g., a single loop. In a reactor system, ethylene and optionally Optionally, one or more α-olefins are polymerized in the presence of one or more cocatalysts. Two different catalysts can be used in the system. One or both of the two different catalysts can be The bimodal interpolymer composition has the formula (I) as shown below. This makes it possible to manufacture

[0030] Exemplary catalysts suitable for producing the first ethylene / α-olefin interpolymer include The catalytic system may be a catalyst system comprising a precatalyst component comprising a metal-ligand complex of formula (I): [ka]

[0031] In formula (I), M is selected from titanium, zirconium, or hafnium. metal, which is in the +2, +3, or +4 formal oxidation state, and n is 0, 1 , or +2, and when n is 1, X is a monodentate or bidentate ligand, and n When is 2, each X is a monodentate ligand, the same or different, and the metal-ligand complex is , the charge is neutral overall, and each Z is -O-, -S-, -N(R N )-, or -P(R P )-, L is independently selected from (C1-C 40 ) hydrocarbylene or (C1- C 40 ) heterohydrocarbylene, R N and R P is (C1-C 30 ) Hydroca Rubir or (C1-C 30 ) heterohydrocarbyl, where (C1-C 40 ) Hydrocarbylene is a linker having 1 to 10 carbon atoms connecting the two Z groups of formula (I). or (C1-C 40 ) Heterohydrin The locarbylene has a linker skeleton of 1 to 10 atoms connecting the two Z groups of formula (I). wherein the moiety comprises: (C1-C 40 ) Heterohydrocarbylene 1 to 10 atoms Each of the 1 to 10 atoms of the linker backbone is independently a carbon atom or a heteroatom. , where each heteroatom is independently O, S, S(O), S(O)2, Si(R C )2, Ge(R C )2, P(R C ), or N(R C ) where, independently, each R C teeth, (C1-C 30 ) hydrocarbyl or (C1-C 30 ) heterohydrocarbyl; R 1 and R 8 is -H(C1-C40 ) hydrocarbyl, (C1-C 40 ) Heterohydrin Locarbyl, -Si(R C )3, -Ge(R C )3, -P(R P )2, -N(R N )2, -OR C , -SR C , -NO2, -CN, -CF3, R C S(O)-, R C S(O)2- , (R C )2C=N-, R C C(O)O-, R C OC(O)-, R C C(O)N(R N ) -, (R N )NC(O)-, a halogen, and a compound represented by formula (II), formula (III), or formula ( IV). [ka]

[0032] In formulas (II), (III), and (IV), R 31-35 , R 41-48 ,Ma Or R 51-59 Each of (C1-C 40 ) hydrocarbyl, (C1-C 40 ) Hetero Hydrocarbyl, -Si(R C )3, -Ge(R C )3, -P(R P )2, -N(R N ) 2. -N=CHR C , -OR C , -SR C , -NO2, -CN, -CF3, R C S(O) -, R C S(O)2-, (R C )2C=N-, R C C(O)O-, RC OC(O)-, R C C(O)N(R N )-, (R N )2NC(O)-, halogen, or -H independently Selected, where R 1 or R 8 At least one of the formula (II), formula (III), or or a radical having the formula (IV), C、 R N , and R P is defined above. As expected.

[0033] In formula (I), R 2-4 , R 5-7 , or R 9-16 Each of (C1 -C 40 ) hydrocarbyl, (C1-C 40 ) heterohydrocarbyl, -Si(R C )3 , -Ge(R C )3, -P(R P )2, -N(R N )2, -N=CHR C , -OR C , - S.R. C , -NO2, -CN, -CF3, R C S(O)-, R C S(O)2-, (R C )2 C=N-, R C C(O)O-, R C OC(O)-, R C C(O)N(R N )-, (R C ) 2 is independently selected from N-C(O)-, halogen, or -H, C、 R N , and BiR P is as defined above.

[0034] The catalyst system comprising the metal-ligand complex of formula (I) is useful for catalyzing the metal-based polymerization of olefins. The catalyst may be catalytically activated by any technique known in the art for activating a catalyst. For example, those containing a metal-ligand complex of formula (I) may be prepared by contacting the complex with an activating cocatalyst or The catalyst or complex may be made catalytically active by combining it with an activating cocatalyst. The activating cocatalyst used in the present invention is an alkylaluminum, a polymer or an oligomer. Alumoxanes (also known as aluminoxanes), neutral Lewis acids, and non-polymers, Non-coordinating, ion-forming compounds (including the use of such compounds under oxidizing conditions) One of the activation techniques is bulk electrolysis. Combinations of one or more of these are also contemplated. The term "aluminum alkyl" refers to Monoalkylaluminum dihydride or monoalkylaluminum dihalide, di Alkyl aluminum hydride or dialkyl aluminum halide, or trialkyl aluminum hydride Examples of polymeric or oligomeric alumoxanes include: Methylalumoxane, triisobutylaluminum modified methylalumoxane, and isobutylaluminum modified methylalumoxane Butylalumoxane is an example.

[0035] The Lewis acid activator (cocatalyst) may be one to three (C1 -C 20 ) Group 13 metal compounds containing hydrocarbyl substituents. Examples of compounds include tri((C1-C 20 )hydrocarbyl)-substituted aluminum, or Ri((C1-C 20 )hydrocarbyl)-boron compounds, tri((C1-C 20 ) Hydro Carbyl)-boron compounds, tri((C1-C 10 ) alkyl) aluminum, tri(( C6-C 18 )aryl)boron compounds, and halogenation (including perhalogenation) derivatives of Other examples of Group 13 metal compounds include tris(fluoro-substituted phenyl)borane, The activating cocatalyst is tris(pentafluorophenyl)borane. 20 ) hydrocarbyl borates (e.g., trityl tetrafluoroborate) or tri ((C1-C 20 )hydrocarbyl)ammonium tetra((C1-C 20 ) Hydrocal bis(octadecyl)methylammonium tetrakis(pentaphenyl)borane (e.g., bis(octadecyl)methylammonium tetrakis(pentaphenyl)borane) As used herein, the term "ammonium" includes The term is ((C1-C 20 ) Hydrocarbyl) 4N + , ((C1-C 20 ) Hydrocarbohydrates 3N(H) + , ((C1-C 20 )hydrocarbyl)2N(H)2 + , (C1-C2 0) Hydrocarbyl N(H)3 + , or N(H)4 + Each of the nitrogen cations is (C1-C 20 When two or more hydrocarbyls are present, they may be the same or different. It's fine.

[0036] The combination of neutral Lewis acid activators (cocatalysts) includes tri((C1-C4) alkyl) Aluminum and trihalides ((C6-C 18 )Aryl)boron compounds, especially thi Tris(pentafluorophenyl)borane or its mixture with neutral Lewis acids and polymers. and combinations with mono- or oligomeric alumoxanes, and with single neutral Lewis acids, particularly tricyclic alumoxanes. Combinations of bis(pentafluorophenyl)borane with polymeric or oligomeric alumoxanes. (Metal-ligand complex): (Tris(pentafluorophenylborane) (Group 4 metal-ligand complexes): (tris(pentafluoro) The molar ratio of (phenylborane):(alumoxane) is 1:1:1 to 1:10:3. 0, and in another embodiment, it is 1:1:1.5 to 1:5:10.

[0037] The catalyst system comprising the metal-ligand complex of formula (I) may be activated by the addition of one or more cocatalysts, e.g. cation forming cocatalyst, strong Lewis acid, or a combination thereof. Suitable activating cocatalysts include polymers, or oligomeric aluminoxanes, especially methylaluminoxane, as well as inert, compatible Examples of suitable cocatalysts include modified methyl Aluminoxane (MMAO), Bis(hydrogenated tallow alkyl)methyl, Tetrakis(penta Fluorophenyl)borate (1 - ) amines, and combinations thereof. , but not limited to these.

[0038] One or more of the aforementioned activating cocatalysts may be used in combination with each other. The best combination is tri((C 1- C4)hydrocarbyl)aluminum, tri((C1- C4) Hydrocarbyl) borane or ammonium borate and oligomer or polymer The total molar ratio of one or more metal-ligand complexes of formula (I) is 1:1 or 2:1 or 2:1. The ratio of the number of moles of the catalyst to the total number of moles of the one or more activating cocatalysts is 1:10,000 to 100:1. For example, the ratio may be at least 1:5000, or at least 1:1000, and The ratio of alumoxane alone to the activating cocatalyst may be 10:1 or less, or 1:1 or less. When used as a metal-catalyst, preferably the number of moles of alumoxane used is The number of moles of the ligand complex may be at least 100 times that of the tris(pentafluorophenyl) When the phenyl)borane is used alone as an activating cocatalyst, one or more metal- The moles of tris(pentafluorophenyl)borane used relative to the total moles of ligand complex. The ratio of the residuals can be 0.5:1 to 10:1, 1:1 to 6:1, or 1:1 to 5:1. The activating cocatalyst is generally present in an amount approximately equal to the total molar amount of one or more metal-ligand complexes of formula (I). They are used in equal molar amounts.

[0039] Fibers and nonwovens At least 75%, or at least 80%, or at least 8 5%, or at least 90%, or at least 95%, or at least 97%, or or at least 98%, or at least 99%, or 100% (all by weight) The remaining portion of the first component may be an ethylene / α-olefin interpolymer. may be additional components such as one or more other polymers and / or one or more additives. The other polymer may be another polyethylene (e.g., polyethylene homopolymer or ethylene / α-olefin interpolymers), propylene-based polymers (e.g., polypropylene Pyrene homopolymer, propylene-ethylene copolymer, or propylene / α-olefin The amount of other polymers may be up to 25%. Additives include antistatic agents, color enhancers, dyes, lubricants, TiO2 or CaC Fillers such as O3, opacifiers, nucleating agents, processing aids, pigments, primary antioxidants, secondary antioxidants, Processing aids, UV stabilizers, anti-blocking agents, slip agents, tackifiers, flame retardants, antibacterial agents , odor reducing agents, antifungal agents, and combinations thereof. The ethylene / α-olefin interpolymer composition does not contain such additives. Such additives are based on the weight of the ethylene / α-olefin interpolymer composition. The total weight of the mixture is about 0.01, or 0.1, or 1 to about 25, or about 20, or may comprise about 15 or about 10 weight percent in the mixture.

[0040] Other regions may include different polyolefins or polyesters. For example, Other areas include polypropylene-based polymers, polypropylene, polyethylene terephthalate The remainder of the second region may be one or more Additional components may include other polymers and / or one or more additives. The cellulose fiber is made of polypropylene or polyester (with or without the above additives). For example, another poly(ethylene terephthalate) or polybutylene terephthalate The polymer may be a polyolefin or another polyester. Possible additives include antistatic agents. , color enhancers, dyes, lubricants, fillers such as TiO2 or CaCO3, opacifiers, Nucleating agents, processing aids, pigments, primary antioxidants, secondary antioxidants, processing aids, UV stabilizers, Anti-blocking agents, slip agents, tackifiers, flame retardants, antibacterial agents, odor reducing agents, antifungal agents, and combinations thereof. The polymer composition is an ethylene / α-olefin copolymer containing such an additive. about 0.01, or about 0.1, or about 1 based on the weight of the interpolymer composition About 25, or about 20, or about 15, or about 10 weight percent of such The composition may contain a mixture of various additives.

[0041] the weight ratio of the first component or region to the second component or region is at least 5 / 95; and is at least 10 / 90, or at least 20 / 80, or at least 30 / 70, Or it may be at least 40 / 60, but not more than 95 / 5, or not more than 90 / 10, or may be 80 / 20 or less, or 70 / 30 or less, or 60 / 40 or less.

[0042] The fibers taught herein can be formed by any conventional spinning technique. The fibers disclosed herein may have one or more of the following characteristics: At least 5 micrometers, or at least 10 micrometers, and 50 micrometers The fibers may have a diameter of less than 1000 mm or less than 30 micrometers. The filament may have a denier per filament ranging from 50g / 9000 to less than 50g / 9000m. All individual values ​​and subranges less than m are included herein and disclosed herein, and are not intended to be limiting unless otherwise specified. For example, the denier per filament can be set to lower limits of 0.1, 0.5, 1, 5, 10, 15, 17, 20, 25, 30, 33, 40, or 44g / 9000m~Upper limit 0.5, 1, 5, 10, 15, 17, 20, 25, 30, 33, 40, 44, or 50g / 9000 For example, the fibers may have a filament yield of less than 40 g / 9000 m. The fibers may have a denier of less than 30 g / 9000 m or less. The fibers may have a denier per m or may have a fiber size in the range of less than 20g / 9000m. The fibers may have a denier per lament or may be in the range of less than 10 g / 9000 m. Alternatively, the fibers may have a denier per filament of 0.5 to 10 g / 9. The filament may have a denier per filament in the range of 000 to 1000 m.

[0043] Bicomponent fibers are made by pumping air through tiny orifices in a metal plate called a spinneret. or other gas, where it is cooled and solidified to form the continuous A bicomponent fiber is formed. The continuous fiber is then rotated between a set of rotating rollers having different rotational speeds. The fibers are guided into the rollers or godets and stretched between them. Between the sets, at least 20%, or at least 30%, or at least 40%, or The fibers can be stretched to an elongation of at least 50% or at least 75%. 00% or less, or 700% or less, or 600% or less, or 500% or less, or 4 00% or less, or 250% or less, or 200% or less, or 150% or less, or 1 The fibers can be stretched to an elongation of up to 0.00%. The stretching is performed on the fibers at ambient temperature. can be done.

[0044] The fibers can be chopped into short fibers, or they can be cut and then stretched. Stretching before cutting is efficient. Cut fibers have a length of at least 0.2, or At least 0.5 or at least 1 cm, and no more than 16 or 12 or 10 cm The resulting short fibers can then be processed in a carded web process, an airlaid process, or the like. It can be processed into nonwoven fabric by the bonding process, such as thermal calendaring process, adhesive bonding. The bonding process, hot air bonding process, needle punch process, hydroentanglement process, and It may be, but is not limited to, a combination of these.

[0045] Bicomponent fibers are made by pumping air through tiny orifices in a metal plate called a spinneret. or other gas, where it is cooled and solidified to form the continuous A bicomponent fiber is formed. The solidified fiber is pneumatically drawn through an air stream and then The nonwoven web may be laid on a conveyor belt to form a nonwoven web. Before or after rolling, the material is stretched by the MDO (machine direction orientation) process or the ring rolling process. The bonding process can be a hot calendar process, an adhesive bonding process, or a hot air bonding process. The processes include the joining process, the needle punch process, the hydroentanglement process, and combinations thereof. The nonwoven web may include, but is not limited to, at least 20% at least 30% or at least 40%, or at least 50% or at least 75% The nonwoven web can be stretched to an elongation of 800% according to certain embodiments. or less than 700%, or less than 600%, or less than 500%, or less than 400% or less than 250%, or less than 200%, or less than 150%, or less than 100% The fibers can be stretched to an elongation of: do.

[0046] The nonwoven fabrics disclosed herein can be made by any known method. Such methods include the spunbond process, the meltblowing process, card Web process, airlaid process, thermal calendar process, adhesive bonding process, hot air Bonding process, needle punch process, hydroentanglement process, electrospinning pinning processes, and combinations thereof. The nonwoven fabrics disclosed herein are formed directly from constituent polymeric materials by a spunbond process. In the spunbond process, the production of nonwoven fabrics includes the following steps: (a) extruding one or more polymer compositions through a spinneret; (b) dissolving the molten spinneret in a liquid state; The polymer composition or compositions are mixed in a stream of air which is typically cooled to promote solidification of the strands. (c) pneumatically drawing the filaments in an air stream; or by winding on mechanical stretch rolls of the type commonly used in the textile fiber industry. The applied drawing tension attenuates the filaments by advancing them through a quenching section. (d) passing the drawn strands through a foraminous surface, such as a moving screen or a porous (e) collecting the web of loose strands into a nonwoven fabric. Bonding step. The bonding may be performed by a thermal calendar process, an adhesive bonding process, a hot air bonding process, etc. The processes include, but are not limited to, the needle punch process, the hydroentanglement process, and combinations thereof. This can be accomplished by a variety of means, including but not limited to:

[0047] The staple fibers are blended and "opened" in a multi-step process and then passed through a conveyor belt. Distributed evenly over the surface for wet laid, air laid or carded / cross lapped application In a wet laid operation, the fibers are typically spread into a uniform web of about 0.5 mm in length. Use 2-2cm of fiber, but if the fiber is hard or thick it may be longer. Airlaid processing typically uses fibers with lengths of about 1 to about 10 cm. Staple nonwovens are typically made with fibers 3-4 cm long. The web is bonded using resin. Bonding is achieved by resin saturation or by total thermal bonding. across the body or in separate patterns by resin printing or heat spot bonding The compatibility with staple fibers is usually seen in high-end woven insulation. This refers to the combination with melt blowing that is often used.

[0048] After the nonwoven fabric is formed, it is stretched in at least one direction. The web may be drawn using a roller or two rollers at different speeds. This can be used to stretch in the machine direction (MD) if the roller speed is adjusted to The web can be attached to a whole web roll or mechanism for stretching in the cross direction. The stretching is preferably at least 5, or at least 10, or less. Temperature at least 15°C and below 90, or below 80, or below 60, or below 50 The nonwoven fabric must be at least 20% elongation or less. At least 30%, or at least 50%, or at least 75% but not more than 800% Stretched to 700%, 500%, 400%, or 300% or less. It is.

[0049] Desirably, when the nonwoven fabric is stretched, at least a portion of the fibers are stretched by at least 20%, Or at least 30%, or at least 40%, or at least 50%, or less Stretched to at least 75% elongation, not more than 700%, or not more than 600%, or not more than 500 % or less, or 400% or less, or 300% or less, or 250% or less, or 200 % or less, or 150% or less, or 100% or less elongation.

[0050] According to certain embodiments, the fibers have a molecular weight of greater than 1, or greater than 1.5, or or greater than 2, or greater than 2.5, or greater than 3 mm -1 Greater curling ability It is characterized by:

[0051] Spunbond nonwoven fabrics can be formed into multi-layer or laminate structures. The layer structure comprises at least two or more layers, where at least one or more of the layers is a and one or more other layers are one or more melt bonded. a blown nonwoven layer, one or more wet laid nonwoven layers, one or more air laid nonwoven layers, Any nonwoven fabric or one or more webs produced by a melt spinning process, 1 One or more film layers are selected. Cast film, blown film, e.g. For example, extrusion coating, spray coating, gravure coating, printing, dipping, Derived from the coating composition via kiss rolling or blade coating Laminated structures may be bonded using any number of bonding methods, thermal bonding, adhesive layer bonding, etc. They can be bonded through layers, hydroentanglement, needle punching. The structures range from S to SX or SX X, or SXXX, or SXXXX, or SXXXXX, where S is a nonwoven fabric as disclosed herein and X is a film, coating, or may be any combination of nonwoven materials, and one or more of X may be S The additional spunbond layer may be an ethylene / α-olefin copolymer as described herein. from the terpolymer composition, and optionally one or more polymers and / or additives. It can be made in combination with.

[0052] Test Method density The density of ethylene / α-olefin interpolymers was measured according to ASTM D792, method This was carried out according to method B.

[0053] Melt index (I2) and (I10) The melt index (I2) value of the ethylene / α-olefin interpolymer is expressed as A Measured at 190°C and 2.16 kg according to STM D1238. Similarly, ethylene / The melt index (I10) values ​​of the α-olefin interpolymers were calculated according to ASTM D1 238 at 190°C and 10 kg. Values ​​are reported in g / 10 min, which is Corresponds to grams dissolved per minute.

[0054] Dynamic mechanical spectroscopy (DMS) The sample was heated at 177°C for 5 minutes under a pressure of 10 MPa in a circular tube of 3 mm thickness and 25 mm diameter. The samples are then removed from the press and placed on a counter. Under nitrogen purge, the ARES strain-controlled rheometer equipped with 25 mm parallel plates was used. A constant temperature thermostat (TA Instruments) was used to measure the temperature of the compression molded plaques. For each measurement, the rheometer is turned on for a short period before the gap is zeroed. Allow to thermally equilibrate for at least 30 minutes. Place the sample disk on the plate and heat at 190°C for 5 minutes. The plates are then closed to a gap of 2 mm and the sample is trimmed before testing. The method may be delayed for an additional 5 minutes to allow for temperature equilibration. This experiment was performed at 190°C, 5 locations at 0.1 to 100 rad / s at 10 intervals. The frequency range is 100 Hz and the distortion amplitude is constant at 10%. The stress response is analyzed, from which the storage modulus (G'), loss modulus (G''), and complex elastic modulus (G'') are calculated. Rate (G * ), dynamic viscosity (η * ), and tan δ (or tan delta). You get tan delta in radians / second and tan delta in 100 radians / second.

[0055] Improved Comonomer Composition Distribution (ICCD) Improved Comonomer Composition Distribution (ICCD) test was performed using the IR-5 detector (Spanish PolymerChar) and a two-angle light scattering detector model 2040 (Precision Crystal detector (now Agilent Technologies) ization Elution Fractionation Equipment (CEF) (Pol The ICCD column is coated with gold. Nickel particles (Bright 7GNM8-NiS, Nippon Chemica l Industrial Co.) on a 15cm (length) x 1 / 4 inch (ID) sticker Packing and conditioning of the column were performed according to the reference (Cong, R. ;Parrott,A.;Hollis,C.;Cheatham,M.WO20170 The slurry method using trichlorobenzene (TCB) slurry paste is used. The final pressure of the column is 150 bar. The column is then placed in the IR-5 detector of the detector oven. Orthodichlorobenzene (ODCB, 99% anhydrous grade or Silica gel from EMD Chemicals was used as the eluent. Obtain ODC 40 (particle size 0.2 mm to 0.5 mm, catalog number 10181-3). It can be used to dry the B solvent. The ICCD device is equipped with a nitrogen (N2) purge function. The ODCB was spatula- ted with dry N2 for 1 h before use. Sample preparation was performed by shaking at 160°C for 1 hour at 4mg / ml (unless otherwise specified). The injection volume is 300 μl. The temperature profile was crystallization from 105°C to 30°C at 3°C / min, followed by 2 min at 30°C. 30 min thermal equilibration (including 2 min soluble fraction elution time), followed by 30 to 140 °C The column is heated at 3°C / min to 30°C. The flow rate during elution is 0.50 ml / min. Data are shown for one Data points are collected per second. Column temperature calibration is performed using a linear homopolymer polyethylene standard. (Comonomer content: 0, Melt index (I2): 1.0 g / 10 min, Polydispersity: M w(GPC) / M n(GPC) By conventional gel permeation chromatography, the A mixture of eicosane (2 mg / ml) in ODCB was used. The ICCD temperature calibration consists of four steps: (1) measurement The temperature offset was calculated by subtracting 30.00°C from the peak elution temperature of eicosane. (2) calculate the temperature offset of the elution temperature by the ICCD This temperature offset should be subtracted from the raw temperature data. (3) Linear homopolymer polyethylene reference is 101 0°C and eicosane has a peak temperature of 30.0°C. A linear calibration line was constructed to convert elution temperatures over the range 0.00°C to 140.00°C. and (4) an elution temperature of less than 30.0°C for the soluble fraction measured isothermally at 30°C. In the reference (Cerk and Cong et al., U.S. Pat. No. 9,688,7 Linear extrapolation was performed using a dissolution heating rate of 3°C / min according to (No. 95). .

[0056] Calibration curve for comonomer content (mol percent of ICCD vs. comonomer at elution temperature (T) The mer content was measured using 12 reference materials (linear ethylene homopolymers and single-site metallopolymers). 11 ethylene-octene random copolymers prepared with Sen catalyst, 35000-12 8000) with known comonomer content. All of these standards were constructed at 4 mg / mL and analyzed in the same manner as previously specified. The comonomer content in mole percent and the peak temperature on the elution curve are as follows: This is the case.

number

[0057] Determination of peaks and full width at half maximum in ICCD elution profiles It begins with zero relative mass at the lowest and highest elution temperatures (typically 35°C to 119°C). A single baseline was used to generate starting and ending relative mass elution profile plots. The IR signal is subtracted from the measured IR signal. For convenience, this is taken as a normalized coefficient for the total area equal to 1. The relative mass vs. elution profile plots from the ICCD are presented as the quantified amount. At each temperature (T), the weight fraction (w T (T)) can be obtained. T ( T) vs. T) ranges from 35.0°C to 119.0°C with a stepwise increase in temperature of 0.200°C. From the ICCD:

number

[0058] w T In the (T) vs. T elution profile, a single peak has one maximum in the center. It is defined as a curve that has two minimum points on either side (the low-temperature side and the high-temperature side). The height of both lowest points must be at least 10% lower than the height of the highest point. If one or both of the following points are less than 10% lower than the highest point, i.e., If one or both of the points have a height that is more than 90% of the height of the highest point, such a curve is considered a shoulder associated with another peak, but is not a peak itself. The distinct peaks are T (T) vs. the maximum height of the peak in the elution profile plot The width at 50% of the peak height (°C) is called the full width at half maximum of the peak. .

[0059] If there are multiple peaks in the ICCD elution profile, the separation point between the peaks (T分離 ) can be defined as the lowest point between two adjacent peaks. ピークn ) The weight fraction of can be calculated according to the following formula:

number

[0060] Comonomer Distribution Constant (CDC) The comonomer distribution constant (CDC) is calculated according to the following steps, which are shown graphically in Figure 1: , ICCD T (T) vs. T calculated from the elution profile. (1) In the range of 35.0°C to 119.0°C with a stepwise temperature increase of 0.200°C From ICCD T (T) vs. T dissolution profile is obtained. The total weight fraction from 35°C to 119°C is It is normalized to 1.0 and should follow equation 2. (2) The median temperature (T median ) to calculate:

number

number

number

number

[0061] Conventional Gel Permeation Chromatography (Conventional GPC) and MWCDI The chromatographic system was a Pol 1000 with a built-in IR5 infrared detector (IR5). ymerChar GPC-IR (Valencia, Spain) High-temperature GPC chromatograph The oven compartment of the autosampler was set to 160 °C and the column was The column compartment was set at 150 °C. The columns used were four Agilent "Mixed A" is a 30 cm, 20 micron linear mixed bed column. The chromatography solvent was 1,2,4-trichlorobenzene with 200 ppm butyl The solvent source is nitrogen infused. The injection volume was 200 microliters and the flow rate was 1.0 milliliters / minute. be.

[0062] The GPC column set was calibrated for molecular weights ranging from 580 to 8,400,000 g / mol. The assay was performed using at least 20 narrow molecular weight distribution polystyrene standards having The standards were placed in six "cocktail" mixtures with at least 10 molecular weight intervals between each standard. Standards are purchased from Agilent Technologies. The ethylene standard is 50 milliliters for molecular weights above 1,000,000 g / mol. at 0.025 grams in 100 ml of solvent and at a molecular weight of less than 1,000,000 g / mol For each standard, prepare 0.05 grams in 50 milliliters of solvent. Dissolve at 37 °C for 30 min with gentle stirring. Determine the peak molecular weight of the polystyrene standards: Convert to ethylene / α-olefin interpolymer molecular weight (W) using the following equation: illiams and Ward, J. Polym. Sci., Polym. Let. ,6,621(1968)).

number

[0063] Using a fifth-order polynomial, each ethylene / α-olefin interpolymer equivalent The calibration points are fitted to the NIST standard NBS1475, which has a molecular weight of 52,000 g / mol. A small adjustment to A (approximately 0.39 to 0.44) was made to the column resolution so that and correct for band broadening effects.

[0064] The total plate count for the GPC column set was 0.0 in 50 mL of TCB. 4 g of eicosane (prepared and dissolved for 20 minutes with gentle stirring). The speed count (Equation 8) and symmetry (Equation 9) are calculated for a 200 microliter sample according to the following equations: The measurement is performed by injection of 1000 torr.

number

number

[0065] The samples were analyzed using PolymerChar's "Instrument Control" software. The sample was prepared semi-automatically using the Poloxamer software. Via the YmerChar high-temperature autosampler, with pre-nitrogen-filled septa caps Add solvent (containing 200 ppm BHT) to the vial. Shake at "slow" speed at 160°C. Dissolve the sample at RT for 3 h.

[0066] M n(GPC) , M w(GPC) , and M. z(GPC) The calculation is Polymer Char GPCOne™ software, each equally spaced data collection point i(IR i )in The baseline-subtracted IR chromatogram and the narrow standard calibration curve for point i from Eq. The ethylene / α-olefin interpolymer equivalent molecular weight (g / mol) was obtained from the M ポリエチレン、i ) to obtain the PolymerChar G according to formulas 11a-c. The results of GPC using the built-in IR5 detector (measurement channel) of the PC-IR chromatograph Based on the results, the GPC molecular weight distribution (GPC-MWD) plot (wt GPC (lg MW) vs. lgMW plot, where wt GPC (lgMW) has a molecular weight of lgMW The molecular weight is in g / mol. ri,wt GPC (lgMW) follows equation 10.

number

[0067] Number average molecular weight M n(GPC) , weight average molecular weight M w(GPC) and z-average molecular weight M z(GPC) can be calculated as follows:

number

[0068] To monitor deviations over time, a PolymerChar GPC-IR system was used. Introduce a flow marker (decane) into each sample via a stem-controlled micropump This flow marker (FM) was used to determine the respective decafluorouracil fractions in the sample (RV (FM sample)). The RV of the decane peak is aligned with the RV of the decane peak in the narrow standard calibration (RV(FM calibration)). The pump flow rate (nominal flow rate) for each sample is then linearly corrected by Any change in the time of the can marker peak will be reflected in the flow rate (Flow (effective)) throughout the experiment. This is assumed to be related to a linear shift in the RV flow marker peak. To advance the flow marker concentration chromatogram, a least-squares fitting routine was used. Then, use the first derivative of the quadratic equation to find the true After calibrating the system based on the flow marker peak, the (narrow standard For semi-calibration, the effective flow is calculated as in Equation 12. The flow marker peak is processed as P Through the Oligomeric GPCOne™ software. Volume correction is made so that the effective flow rate is within 0.5% of the nominal flow rate.

number

[0069] The IR5 detector ratio calibration ranges from homopolymer (0 SCB / 1000 total C) to approximately Range up to 50SCB / 1000 total C (where total C=carbons in main chain+carbons in branches) The known short chain branching (SCB) frequency of 13 At least eight of the 10C NMR spectra were obtained. Ethylene / α-olefin interpolymer standard (one polyethylene homopolymer and seven ethylene / octene copolymers). The weight average molecular weight of the copolymer is 36,000 g / mol to 126,000 g / mol when measured by GPC. / mol. The molecular weight distribution (M w(GPC) / M n(GPC )) is a GPC The baseline value of the IR5 methyl channel sensor is 2.0 to 2.5. Baseline-subtracted area response vs. baseline-subtracted area response for IR5 measurement channel sensor "IR5 area ratio (or "IR5 methyl channel area / IR5 measurement channel area response area ratio)" Standard filters and filters supplied by PolymerChart "Area" -Wheel: Part Number IR5_FWM01 is part of the GPC-IR device. The SCB frequency vs. "IR5" standard is calculated for each of the "SCB" standards. A linear approximation of the "area ratio" is constructed in the form of the following equation:

number

[0070] A study on the chromatograms generated by the "IR5 methyl channel sensor" The "linear baseline-subtracted chromatographic height" of each run was calculated as the column elution volume. Generate baseline-corrected chromatograms (methyl channels) as a function of A series of "linear" measurements for the chromatograms generated by the "IR5 measurement channel" "Baseline-subtracted chromatographic height" as a function of column elution volume Establish and generate a baseline-corrected chromatogram (measurement channel).

[0071] "Baseline corrected chromatogram (methyl channel)" vs. "Baseline corrected chromatogram (methyl channel) The "IR5 height ratio" of the "IR5 matrix (measurement channel)" is the ratio of each column across the sample integration boundary. Dissolution volume index (each index is equally spaced, dissolution at 1 ml / min) The calculation is performed at 1 data point per second. The "IR5 height ratio" is multiplied by the coefficient A1. and add the coefficient A0 to this result to get the predicted SCB frequency for the sample, as shown in Equation 14 below. Convert the results to mole percent comonomer as follows: Mole percent comonomer = {SCBf / [SCBf+((1000-SCBf*comonomer (length of monomer) / 2)}*100 (Eq. 14), During the ceremony, “SCB f " is "SCB per 1000 total C" and "comonomer The "length" of the comonomer is the number of carbon atoms in the comonomer, e.g., octene is 8, hexene is 6, etc. Such is the case.

[0072] Using the method of Williams and Ward (equation 7 above), each elution volume The mole percent comonomer is calculated by converting the molecular weight index to a molecular weight value (Mwi). The slope of the plot is a function of Mwi of 20,000 to 200,000 g / s. Calculated in molar Mwi (end group corrections for chain ends are omitted for this calculation) Using linear regression, the Mwi ranges from 20,000 to 200,000 g / mol and Calculate the slope of the concentration chromatogram (wt GPC (lgMW) vs. l The slope of the gMW plot is at least 10% of the peak height in the chromatogram. is defined as the molecular weight comonomer distribution index (MWCDI).

[0073] Zero Shear Viscosity Ratio (ZSVR) The zero shear viscosity ratio is calculated by the equivalent weight average molecular weight (M w(GPC) ) Zero shear viscosity (ZSV) of branched polyethylene materials vs. linear polyethylene materials in (See ANTEC minutes below).

number

[0074] Interpolymer

number

number

[0075] Creep Test Interpolymer

number

[0076] 1 H NMR method The stock solution (3.26 g) was added to 0.133 g of polymer sample in a 10 mm NMR tube. The stock solution was a mixture of tetrachloroethane-d2 (TCE) and perchloroethylene (50:5 0 wt.) and 0.001M Cr 3+ The solution in the tube was purged with N2 for 5 min. The capped sample tubes are left at room temperature overnight to allow the polymer samples to swell. The samples were dissolved at 110°C with periodic vortex mixing. It does not contain any additives that may contribute to slippage, such as erucamide. 1 H.N.M. R analysis was performed on a Bruker AVANCE 400MHz spectrometer at 120°C for 10m. m cryoprobe.

[0077] Two experiments were performed to measure the degree of unsaturation, one as a control and the other as a duplicate In the control experiment, the data were processed with an exponential window function with a line broadening of 1 Hz. The baseline is adjusted to about 7-2 ppm. TCE residue 1 Set the signal from H to 100. In the control experiment, the integral value ( I 合計 The total number of carbon atoms in the polymer, NC, is calculated using Equation 16 as follows: NC=Itotal / 2 (Formula 16)

[0078] For the double presaturation experiments, the data were processed with an exponential window function with 1 Hz line broadening and based Correct the line to about 6.6 to 4.5 ppm. TCE Residue 1 Set the signal from H to 100. and the corresponding integral for unsaturation (I ビニレン , I トリ置換 , I ビニル , and I ビ ニリデン ) is integrated. Using NMR spectroscopy to determine polyethylene unsaturation is well known and is described, for example, in Busico, V., et al., Macromolecules, 2 See US Pat. No. 5,38,6988. Vinylene, trisubstituted, vinyl, and vinylidene The number of unsaturated units of the copolymer is calculated as follows:

number

number

[0079] 13 C NMR method The sample was prepared using tetrachloroethane-d2 / containing 0.025M Cr(AcAc)3. Approximately 3 g of a 50 / 50 mixture of orthodichlorobenzene was added to a Norell 1001- 7 Prepare by adding 0.25 g of polymer sample in a 10 mm NMR tube. Oxygen is removed from the sample by purging the tube headspace with nitrogen. Using a heating block and heat gun, heat the tube and its contents to 150 °C. Dissolve and homogenize the samples by visually inspecting each sample to ensure homogeneity. Samples should be thoroughly mixed immediately prior to analysis and allowed to cool before insertion into the heated NMR probe. This is necessary to ensure that the sample is homogenous and representative of the whole. All data was obtained using a Bruker 400 MHz spectrometer equipped with a Bruker cryolobe. Data was collected using a 6 second pulse repetition delay, 90 degree flip angle, and All measurements were collected using inverse gated decoupling with a sample temperature of 120 °C. The measurements are performed on a non-rotating sample in locked mode. The sample is allowed to thermally equilibrate for 7 min before data acquisition. 13C NMR chemical shifts are internally referenced to the EEE triad at 30 ppm. .

[0080] C13 NMR Comonomer Content: Using NMR spectroscopy to determine polymer composition It is well known that ASTM D 5017-96, JCRanda ll et al., in “NMR and Macromolecules” ACS Symposium series 247;JCRandall,Ed.,Am Chem. Soc., Washington, DC, 1984, Ch. 9; and JCRandall in “Polymer Sequence Determinition” "The Nation," Academic Press, New York (1977) A general method for polymer analysis by MR spectroscopy is presented.

[0081] Denier Measurement Fiber size is measured by optical microscopy. Denier (the diameter of such fiber per 9000 meters) The fiber density (defined as the weight of the fiber) is calculated based on the density of each polymer component and the fiber size.

[0082] 2% secant modulus (E) and yield stress (σ y ) The yield stress and 2% secant modulus are measured as follows. Using Toyo Si-90 Plastar injection molding machine, ASTMD36 41. This is done with a 1.1 inch (i.e. 28 mm) diameter screw. The temperature profile is from the throat to the nozzle. The melting temperature was set at 48℃ / 121℃ / 175℃ / 204℃ / 204℃. The injection pressure was 2000 bar and the injection time was 1.43 seconds. The holding pressure was set at 300 bar and the holding time was 25 seconds. The cooldown time was 20 seconds, and the recovery time was 12.49 seconds for PE and 9.84 seconds for PP. The screw speed was 90 rpm.

[0083] For injection molded Type I ASTM bars according to ASTM D638 test procedure The tensile test is performed at room temperature and at a tensile speed of 2 inches / min. y ) and 2 The % secant modulus (E) is obtained from the tensile stress-strain curve. The 2% secant modulus is E = The yield stress is defined as the stress at 2% strain / 2%. The yield stress is the stress at 0% strain to 5% strain on the stress-strain curve. The highest stress in the 0% strain range. Five specimens were measured and the average value was reported.

[0084] Curl property Curl is measured using an optical microscope. Curl (defined as the curvature of the fiber) is the amount of curl caused by the fiber. The radius of the helix is ​​calculated as the reciprocal of the radius of the approximate helix formed by the fiber. It is formed by projecting the approximate helix formed by the fiber onto a surface perpendicular to it. The radius of the circle is equal to the radius of the circle. Report the average of at least five samples. Working Example Materials used ASPUN(TM) 6835 is manufactured by Dow Chemical Company Unimodal (i.e., unimodal or monomodal, showing only one peak in the ICCD elution) It is an ethylene / octene copolymer of 1,2-difluoroethylene (Dal). ASPUN 6000 is manufactured by Dow Chemical Company. It is an ethylene / octene copolymer. Sample 1 is a bimodal ethylene / α-olefin copolymer, synthesized as follows: do. Sample 2 is a bimodal ethylene / α-olefin copolymer, synthesized as follows: do. · Exxon 3854 polypropylene is manufactured by Exxon Mobil. The yield stress and 2% secant modulus of these samples are summarized in Table 1. [Table 1]

[0085] Example 1 - Synthesis and Characterization of Ethylene / α-Olefin Interpolymer Compositions All raw materials (ethylene monomer, 1-octene comonomer) and and process solvents (Isopar E (trade name) from ExxonMobil Chemical). A high-purity isoparaffin solvent with a narrow boiling range (product name) is purified with molecular sieves. Hydrogen is supplied under pressure as a high purity grade and is not further purified. Reactor Ethylene The feed stream is compressed to a pressure higher than the reaction pressure via a mechanical compressor. The feed of the catalyst is pressurized via a pump to a pressure higher than the reaction pressure. , manually dilute the batch to the appropriate component concentration using purified solvents, and perform the reaction at a pressure higher than the reaction pressure. All reactor feed flows were measured by mass flow meters and controlled by a computerized automatic valve control system. The system is independently controlled.

[0086] Two reactor systems are used in a series configuration. Each continuous solution polymerization reactor has a separate reactor for removing heat. A liquid-filled, non-adiabatic, isothermal circulating reactor is used to simulate a continuous stirred tank reactor (CSTR). The reactor consists of a loop reactor. All fresh solvent, ethylene, hydrogen and catalyst component feeds are separated. The total fresh feed to each reactor (solvent, ethylene, 1-octene, and hydrogen) is controlled. The fresh feed stream is heated to maintain a single solution phase by passing the feed stream through a heat exchanger. The total unused feed to each polymerization reactor is controlled to a roughly equal reactor volume between each injection location. Fresh feed is injected into the reactor at two locations, with each injector receiving the total fresh feed material flow rate. The catalyst components are pumped through specially designed injection stringers. The main catalyst component feed (precatalyst) is injected into the polymerization reactor at a specific target. The reactor is computer controlled to maintain ethylene conversion. The cocatalyst components are calculated and specified. The feed is based on the molar ratio of the main catalyst (pre-catalyst) component to the feed of each reactor. Immediately after the injection point, the feed stream is mixed with the contents of the circulating polymerization reactor using a static mixing element. The contents of each reactor are passed through a heat exchanger which serves to remove most of the heat of reaction, and in particular The temperature of the coolant side is continuously circulated to maintain a constant, isothermal reaction environment. Circulation around the reactor loop is provided by a pump.

[0087] In the dual reactor series configuration, the (solvent, ethylene, 1-octene) from the first polymerization reactor , hydrogen, catalyst components, and polymer) exits the first reactor loop; Add to the second reactor loop.

[0088] The second reactor effluent is inactivated by the addition and reaction of water to the zone. Following catalyst deactivation and additive addition, the reactor effluent is mixed with the non-polymerized The polymer stream enters a devolatilization system where it is removed from the polymer stream. The isolated polymer melt is pelletized. The non-polymer stream is separated from the bulk of the ethylene that is removed from the system. The solvent and most of the unreacted 1-octene are removed through a purification system. After filtration, the solvent and 1-octene are recycled to the reactor. Do it.

[0089] To generate the examples, reactor stream feed data flow corresponding to the values ​​in Table 2 are used. The data was compiled assuming that the complexity of the solvent recycle system was taken into account and that the reaction system was run with a once-through flow diagram. The catalyst components used are shown in Table 3. Each polymer produced was tested for various properties according to the methods described above. The results are shown in Table 4. [Table 2] [Table 3] [Table 4]

[0090] Example 2 - Spun and drawn eccentric fibers Exxon3854PP core and one of the ethylene copolymers as sheath A bicomponent fiber with a highly eccentric core-sheath configuration was made using The extruder profile was set to a melt temperature of 240°C. Adjust to achieve a throughput rate of 0.6 ghm (grams / hole / minute). A Hills bicomponent die was operated with a 40 / 60 core / sheath weight ratio and one extruder. in one extruder it uses Exxon 3854 PP and in another it uses ethylene copolymers. The die configuration has a hole diameter of 0.6 mm and a length / diameter (L / D) of 4 / 1, The quench air temperature and flow rate were set at 23°C and 520 cfm (cubic meter). After the quenching section, the airflow evacuates the filament in the slot unit. A drawing tension is applied to the filaments 144 by air drawing the filaments. The air flow velocity is , controlled by the pressure of the slot aspirator, and the pressure of the slot aspirator was set to 20ps Set it to i.

[0091] The resulting fibers were stretched at room temperature at a stretch rate of 100% / min for 5 min using an Instron tensile machine. The stretched fiber was then removed from the Instron and the curvature was measured. The results are shown in Table 5. [Table 5]

[0092] Example 3 - Spun Concentric Fibers for Use as Staple Fibers It has a polypropylene core and sheath (having a concentric core-sheath configuration). The bicomponent fibers were fabricated using ASPUN™ 6835 or sample 1 as the sheath material. , sample 2. On a Hills bicomponent continuous filament fiber spinning line, 0. Fiber is spun at a throughput rate of 5ghm (grams per hole per minute). The extruder was operated at a 40 / 60 core / sheath ratio by weight and was fed Exxon 3854 in one extruder. Use PP and ethylene / α-olefin intercopolymer in a separate extruder The diameter of the hole used was 0.5 mm, and the length / diameter L / D was 4 / 1. Set the air temperature and flow rate at 25°C and 520 cfm (cubic feet per minute). The profile of the machine is adjusted to achieve a melt temperature of 240°C. After the quenching section, The 44 fibers are collected by a denier roll and then guided to two drawing rolls. The two draw rolls rotate at different speeds and draw the fiber between them. The fibers are then removed from the bobbin before being examined under a microscope for curl. The fiber spinning conditions are shown in Table 6. The curvature results are shown in Table 7. [Table 6] [Table 7]

Claims

1. forming a fiber having at least a first region and a second region, and wherein the first region has a density of 0.930 to 0.965 g / cm 3 Density in the range of Ethylene / alpha-olefin copolymers characterized by a melt index (I2) in the range of 10 to 60 g / 10 min. The I2 comprises a olefin interpolymer composition, the I2 being as defined by ASTM D1238 as follows: The weight average molecular weight and number average molecular weight were measured by GPC at 190°C and 2.16 kg. Molecular weight ratio (M w(GPC) / M n(GPC) ) is 1.5 to 2. 6 and a tan delta at 1 radian / sec of at least 45; The comonomer composition distribution (ICCD) method was used to determine the low-temperature peak and the high-temperature peak on the elution profile. and the full width at half maximum of the high temperature peak is less than 6.0° C., and the fiber is heated to at least 20 % elongation, thereby increasing the curl of said fiber.

2. The ethylene / α-olefin interpolymer composition has the following: a density of 0.930 to 0.950; 0.940 g / cm 3 The ethylene / α-olefin interpolymer composition is in the range of The composition has a peak temperature of 60 to 80°C and a weight of 25 to 65% of the low-temperature peak. fraction, peak temperature of the high temperature peak above 90° C., and weight of the high temperature peak between 35 and 75% 10. The process of claim 1, further comprising one or more of the following fractions:

3. The first region has a first 2% secant modulus E 1 and the first yield stress σ y1 Have , the second region has a second 2% secant modulus E 2 and the second yield stress σ y2 having The first 2% secant modulus E 1 is the second 2% secant modulus E 2 Is it different from or the first yield strength σ y1 is the second yield strength σ y2 Differs from, or both The process according to any one of claims 1 to 2,

4. Dividing the difference in the yield stress of the materials of the first and second regions by the yield stress of the second region 4. The process of claim 3, wherein the value obtained is at least 0.

4.

5. The difference between the 2% secant modulus of the materials of the first and second regions is the 2% secant modulus of the material of the second region.

4. The process of claim 3, wherein the value divided by the linear modulus is at least 0.

4.

6. |σ y1 / E 1 -σ y2 / E 2 | / (σ y2 / E 2 ) is at least 0.01 The process of claim 3.

7. The second region is the ethylene / α-olefin interpolymer of the first region. The composition according to any one of claims 1 to 6, comprising different polyolefins or polyesters. The process described in paragraph .

8. The process of claim 7 , wherein the second region comprises polypropylene.

9. The first region is a sheath around a core of the second region, or the second region is a sheath around a core of the second region. The second region is a sheath around a core of the first region. The process described.

10. 10. Any of claims 1 to 9, further comprising heating the fiber before or after drawing.

3. The process according to claim 1.

11. 11. The method according to claim 1, wherein the stretching is carried out at a temperature in the range of 5 to 90° C. The process described.

12. The process according to any one of claims 1 to 11, wherein the fibers are formed into a nonwoven web. Seth.

13. The process of claim 12, wherein the stretching is performed after forming the nonwoven web. vinegar.

14. Any one of claims 12 to 13, wherein the loft of the nonwoven increases after stretching by at least 10%. The method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Filament nonwoven fabric and its production

    JP1997059860A

  • Soft nonwoven fabric

    JP2001115367A

  • Method for production of latent crimpable polyester conjugated short fibers, and fiber assembly, and nonwoven fabric

    JP2004124351A

  • Conjugated fiber, method for producing the same and nonwoven fabric using the same

    JP2005060896A

  • Catalyst olefin block copolymer having a controlled block arrangement distribution and at least one low-crystallinity hard block

    JP2010533774A