Heterogeneous catalyst
A heterogeneous catalyst with alumina support and strategically distributed gold addresses the inefficiencies in existing catalysts, achieving enhanced production of methyl methacrylate from methacrolein and methanol.
Patent Information
- Application Number
- JP2024125909
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-06-28
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-13
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing heterogeneous catalysts supported on silica and alumina do not offer the desired properties for efficiently converting methacrolein to methyl methacrylate, necessitating the development of a catalyst with improved performance.
A heterogeneous catalyst comprising alumina support with 0.1-5% by weight of gold, where at least 90% of the gold is distributed in the outer 60% of the catalyst volume, and catalyst particles with a diameter ranging from 200 microns to 30 mm, is used to convert methacrolein and methanol into methyl methacrylate.
The catalyst effectively produces methyl methacrylate with improved yield and efficiency by optimizing gold distribution and particle size, enhancing the catalytic process.
Smart Images

Figure 2024160280000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a heterogeneous catalyst, which is particularly useful in a process for preparing methyl methacrylate from methacrolein and methanol. [Background technology]
[0002] Heterogeneous catalysts in which precious metals are supported on silica in combination with alumina and other elements are known, see for example U.S. Pat. No. 7,326,806 (B2), however, there is a need for additional catalyst particles with improved properties. Summary of the Invention
[0003] The present invention is directed to a heterogeneous catalyst comprising a support and gold, where (i) the support comprises alumina, (ii) the catalyst comprises 0.1 to 5 weight percent gold, (iii) at least 90 weight percent of the gold is in the outer 60% of the catalyst volume, and (iv) the particles of the catalyst have an average diameter between 200 microns and 30 mm, the weight percentages being based on the weight of the catalyst.
[0004] The present invention is further directed to a catalyst bed comprising particles of this heterogeneous catalyst.
[0005] The present invention is further directed to a process for preparing methyl methacrylate from methacrolein and methanol, the process comprising contacting a mixture comprising methacrolein, methanol, and oxygen with a catalyst bed comprising particles of a heterogeneous catalyst. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0006] Unless otherwise stated, all compositional percentages are weight percent (wt%) and all temperatures are in °C. "Metal" means an element in Groups 1-12 of the Periodic Table, excluding hydrogen, aluminum, gallium, indium, thallium, tin, lead, and bismuth. "Catalyst center" is the center of gravity of the catalyst particle, i.e., the average location of all points in all coordinate directions. Diameter is any linear dimension passing through the center of the catalyst, and average diameter is the arithmetic mean of all possible diameters. Aspect ratio is the ratio of the longest diameter to the shortest diameter.
[0007] Preferably, the carrier is 10 m 2 / g, preferably 30m 2 / g, preferably 50m 2 / g, preferably 100m 2 / g, preferably 120m 2 In the portion of the catalyst containing little or no gold, the support has a surface area of more than 50 m 2 / g, preferably less than 20m 2 The catalyst particles may have a surface area of less than 1 / g. Preferably, the catalyst particles comprise at least 0.1 wt%, preferably at least 0.2 wt%, preferably at least 0.3 wt%, preferably not more than 95 wt%, preferably not more than 90 wt%, preferably not more than 80 wt%, preferably not more than 70 wt%, preferably not more than 60 wt%, preferably not more than 50 wt%, preferably not more than 40 wt%, preferably not more than 30 wt%, preferably not more than 20 wt%, preferably not more than 10 wt%, preferably not more than 5 wt% alumina. Preferably, the catalyst particles are silica particles comprising the aforementioned amounts of alumina. Preferably, the catalyst particles are alumina particles.
[0008] Preferably, the aspect ratio of the catalyst particles is 10:1 or less, preferably 5:1 or less, preferably 3:1 or less, preferably 2:1 or less, preferably 1.5:1 or less, preferably 1.1:1 or less. Preferred shapes of particles include spheres, cylinders, cuboids, rings, multi-lobed shapes (e.g., cloverleaf cross-sections), shapes with multiple holes and "wagon wheels", preferably spheres. Irregular shapes may also be used.
[0009] Preferably, at least 90% by weight of the gold is in the outer 60% of the catalyst volume (i.e. the volume of the average catalyst particle), preferably the outer 50%, preferably the outer 40%, preferably the outer 30%, preferably the outer 25%. Preferably, the outer volume of any particle shape is calculated for a volume having a certain distance from its inner surface to its outer surface (the surface of the particle) measured along a line perpendicular to the outer surface. For example, for a spherical particle, the outer x% of the volume is the spherical shell, its outer surface is the surface of the particle, and its volume is x% of the volume of the entire sphere. Preferably, at least 95% by weight, preferably at least 97% by weight, preferably at least 99% by weight of the gold is in the outer volume of the catalyst. Preferably, at least 90% by weight (preferably at least 95% by weight, preferably at least 97% by weight, preferably at least 99% by weight) of the gold is within a distance from the surface that is no more than 15% of the catalyst diameter, preferably no more than 13%, preferably no more than 10%, preferably no more than 8%. The distance from the surface is measured along a line perpendicular to the surface.
[0010] Preferably, the average diameter of the catalyst particles is at least 300 microns, preferably at least 400 microns, preferably at least 500 microns, preferably at least 600 microns, preferably at least 700 microns, preferably at least 800 microns, preferably no greater than 20 mm, preferably no greater than 10 mm, preferably no greater than 5 mm. The average diameter of the support and the average diameter of the final catalyst particles do not differ significantly.
[0011] Preferably the amount of gold as a percentage of the catalyst (gold and support) is between 0.2 and 5 wt.%, preferably at least 0.3 wt.%, preferably at least 0.5 wt.%, preferably at least 0.7 wt.%, preferably at least 0.9 wt.%, preferably no more than 4 wt.%, preferably no more than 3 wt.%, preferably no more than 2.5 wt.%.
[0012] Preferably, the support is produced by precipitating an aluminum salt on silica particles. Preferably, the resulting material is then treated by calcination, reduction, or other treatment known to those skilled in the art to decompose the metal salt to metal or metal oxide. Preferably, gold is precipitated from an aqueous solution of the metal salt in the presence of the support. Preferably, the solution contains an acid such as nitric acid, sulfuric acid, hydrochloric acid, acetic acid, etc. Preferably, the solution also contains a sulfur-containing acid, such as thiomalic acid, and preferably a carboxylic acid, such as citric acid or oxalic acid. Preferably, the sulfur-containing acid is present in a concentration of 1-10% by weight (preferably 3-8%). Preferably, the carboxylic acid is present in an amount of 0.1-25% by weight (preferably 0.5-15% by weight). Preferably, the weight ratio of sulfur to acid is 0.1:1 to 5:1, preferably 0.2:1 to 3:1. Preferably, before adding the gold precursor, the support is washed with ammonium hydroxide to remove the chloride content, preferably to a level of less than 100 ppm, preferably less than 50 ppm in the bulk support. Preferably, aluminum is precipitated from an aqueous solution of metal salts in the presence of the support. Preferred aluminum salts include aluminum nitrate, aluminum sulfate, aluminum chloride, aluminum hydroxide, and aluminum oxide, preferably aluminum nitrate, aluminum sulfate, or aluminum chloride. Preferred gold salts include tetrachloroauric acid, sodium gold thiosulfate, sodium gold thiomalate, and gold hydroxide. In a preferred embodiment, the support is produced by the incipient wetness technique, in which an aqueous solution of aluminum precursor salt is added to silica particles so as to fill the pores with the solution, and then the water is removed by drying. Preferably, the resulting material is then treated by calcination, reduction, or other treatments known to those skilled in the art to decompose the metal salt to metal or metal oxide. Preferably, the gold is loaded onto an alumina or alumina modified silica support by incipient wetness, followed by drying and, preferably, calcination.
[0013] Calcination is preferably carried out at a temperature between 250° C. and 600° C., preferably at least 300° C., preferably up to 550° C. Preferably the temperature is increased in a stepwise or continuous manner up to the final calcination temperature.
[0014] In another preferred embodiment, the catalyst is produced by deposition precipitation in which porous silica, including alumina, is immersed in an aqueous solution containing a suitable gold precursor salt, which is then allowed to interact with the surface of the inorganic oxide by adjusting the pH of the solution. The resulting treated solid is then recovered (e.g., by filtration) and then converted to the finished catalyst by calcination, reduction, or other treatments known to those skilled in the art to decompose the gold salt to metal or metal oxide.
[0015] The catalyst of the present invention is useful in a process for producing methyl methacrylate (MMA), which comprises treating methacrolein with methanol in an oxidative esterification reactor (OER) containing a catalyst bed. The catalyst bed comprises catalyst particles and is located in the OER, and a fluid flow may pass through the catalyst bed. The catalyst particles in the catalyst bed are typically held in place by solid walls and screens. In some configurations, screens are at both ends of the catalyst bed and solid walls are at the side(s), while in some configurations the catalyst bed may be completely surrounded by screens. Preferred shapes of the catalyst bed include a cylinder, a rectangular parallelepiped, and a cylindrical shell, preferably a cylinder. The OER further comprises a liquid phase comprising methacrolein, methanol, and MMA, and a gas phase comprising oxygen. The liquid phase may further comprise by-products, such as methacrolein dimethyl acetal (MDA) and methyl isobutyrate (MIB). Preferably, the liquid phase is at a temperature between 40 and 120°C, preferably at least 50°C, preferably at least 60°C, preferably not more than 110°C, preferably not more than 100°C. Preferably, the catalyst bed is at a pressure between 0 and 2000 psig (101.3 and 13890.8 kPa), preferably not more than 2000 kPa, preferably not more than 1500 kPa. Preferably, the pH of the catalyst bed is between 4 and 10, preferably at least 4.5, preferably at least 5, preferably not more than 9, preferably not more than 8, preferably not more than 7.5, preferably not more than 7, preferably not more than 6.5. Preferably, the catalyst bed is in a tubular continuous reactor.
[0016] The OER typically produces MMA along with methacrylic acid and unreacted methanol. Preferably, methanol and methacrolein are fed to a reactor containing a fixed bed in a methanol:methacrolein molar ratio of 1:10 to 100:1, preferably 1:2 to 20:1, preferably 1:1 to 10:1. Preferably, the fixed bed further comprises an inert material. Preferred inert materials include, for example, alumina, clay, glass, silicon carbide, and quartz. Preferably, the inert material is below the size range of the catalyst. Preferably, the reaction product is fed to a methanol recovery distillation column providing an overhead stream rich in methanol and methacrolein, and preferably this stream is recycled back to the OER. The bottom stream from the methanol recovery distillation column comprises MMA, MDA, methacrylic acid, salts, and water. In one embodiment of the present invention, MDA is hydrolyzed in a medium comprising MMA, MDA, methacrylic acid, salts, and water. MDA may be hydrolyzed in the bottom stream from the methanol recovery distillation column, the stream containing MMA, MDA, methacrylic acid, salts, and water. In another embodiment, MDA is hydrolyzed in an organic phase separated from the methanol recovery bottom stream. Water may need to be added to the organic phase to ensure there is enough water present for MDA hydrolysis, and these amounts can be easily determined from the composition of the organic phase. The product of the MDA hydrolysis reactor is phase separated, and the organic phase passes through one or more distillation columns to produce the MMA product and light and / or heavy by-products. EXAMPLES
[0017] Example 1 Batch recycle fixed bed bubble column reactor operation: A 150 g feed solution containing 10 wt. % methacrolein, 200 ppm inhibitor, and the remainder methanol was prepared and placed in a 300 mL Parr® reactor, which served as a gas release vessel. The liquid in the vessel was maintained at a temperature of about 20° C. The liquid feed was pumped at 7 mL / min from the gas release vessel into the bottom of the vertically oriented fixed bed reactor. Air and nitrogen gas were mixed to provide 7.8 mole % oxygen and mixed with the liquid feed before entering the fixed bed reactor. The fixed bed reactor was a jacketed ¼ inch stainless steel tube maintained at 60° C. using an external heater. The reactor itself was loaded with 2 mm glass beads to fill approximately 18 inches of the tube, and then the catalyst was loaded. The remaining void at the top of the reactor was filled with 3 mm glass beads. The liquid and gas exiting the top of the reactor were sent to a condenser where the non-condensable gases were vented while the liquid was recycled back to the gas release vessel. Catalyst 1, as well as several other examples, were run in this manner.
[0018] Preparation of catalyst 1: Catalyst 1 was prepared by the incipient wetness method using 5 g of Norpro 3.2 mm alumina spherical pellets as the starting support material to which was added a solution of 0.19 g of gold sodium thiosulfate, 0.2 g of mercaptosuccinic acid, 0.06 g of citric acid monohydrate, and about 5 g of DI water that had been stirred for 30 minutes prior to addition. The catalyst was then placed in a box oven with a constant air purge of about 50 LPH at room temperature for 1 hour, then calcined at 400° C. using a 5° C. / min temperature ramp and held at 400° C. for 4 hours.
[0019] Example 2 Batch recycle fixed bed bubble column reactor operation: A batch recycle reactor was used as described in Example 1.
[0020] Preparation of catalyst 2: Catalyst 2 was prepared by the incipient wetness method using 10 g of Norpro 3.2 mm alumina spherical pellets as the starting support material to which was added a solution of 0.39 g of gold sodium thiosulfate and 0.04 g of thiomalic acid in 10 g of DI water that was stirred for 30 minutes before addition. The catalyst was then placed in a box oven at 120° C. with a constant air purge of about 50 LPH for 1 hour, then calcined at 400° C. using a 5° C. / min temperature ramp and held at 400° C. for 4 hours.
[0021] Example 3 Single pass fixed bed bubble column reactor operation: A feed consisting of 20 wt. % methacrolein, 200 ppm inhibitor, and the remainder methanol was fed at a rate of 40 g / hr to a 3 / 8 inch stainless steel tubular reactor containing a short front of borosilicate glass beads, followed by 5 g of catalyst. Catalyst 2 was utilized. A gas containing 8% oxygen in nitrogen was also fed with 4.5% O in the vent. 2 The reactor was operated at 60° C. and 160 psig. The reactor product was sent to a gas-liquid separator, the vapor was sent to a condenser with liquid return, and the non-condensable gases went to vent. The results are set forth in the table below.
[0022] Preparation of catalyst 3: Catalyst 3 was prepared by the incipient wetness method, using 20 g of CALiACT Q-10 support manufactured by Fuji Silysia Chemical, Ltd. as the starting material and adding aluminum to the support material. Specifically, 13.8 g of aluminum nitrate nonhydrate was dissolved in 20 g of deionized water. The salt solution was added to the support in a rotating drum type apparatus in very small droplets so that the solution was uniformly distributed on the support material. The solution was at 80°C at the time of addition. The modified support material was then dried under slight vacuum at 60°C for 4 hours, and then calcined in air at ambient pressure by increasing the temperature from ambient temperature to 125°C at 5°C per minute and holding for 1 hour, then increasing the temperature to 250°C at 5°C per minute and holding for 1 hour, then increasing the temperature to 350°C at 5°C per minute and holding for 1 hour, and finally increasing the temperature to 450°C at 5°C per minute and holding for 4 hours. Gold was then added to the support by the incipient wetness method utilizing 0.83 g of sodium gold thiosulfate in 10 g of deionized water at 40°C. The resulting catalyst was dried and calcined in air using the same heating profile as above. Analysis of the catalyst using a scanning electron microscope (SEM) equipped with energy dispersive spectroscopy (EDS) clearly shows that eggshell deposits of both Al and Au are present, with Au preferentially present only where Al was deposited. The thickness of the Al and Au eggshells was found to be approximately 1 micron.
[0023] Example 4 Comparative Example Batch recycle fixed bed bubble column reactor operation: A batch recycle reactor was used as described in Example 1.
[0024] Preparation of catalyst 4: Catalyst 4 was prepared by incipient wetness where 4.1 g of gold sodium thiosulfate was dissolved in 100 g of water to form an aqueous solution, then placed on 100 g of CALiACT Q-20 silica support material from Fuji Silysia Chemical, Ltd. The sample was dried at 120° C. for 1 hour and then calcined at 400° C. for 4 hours. The gold loading was nearly uniform within the catalyst. [Table 1]
[0025] The gold contents of all catalysts were in the range of 1.1-1.5 wt%.
[0026] For catalyst 2, approximately 95% of the gold was within the outer 200 microns, ie, the outer 33% of the volume, and for comparative catalyst 4, approximately 95% was within the outer 1000 microns (the outer 95% of the volume).
[0027] SEM / EDS of an example of eggshell Sample imaging and EDS cross-sectional mapping: SEM-EDS imaging was performed on a Hitachi SU-8230 equipped with a Bruker AXS XFlash 6160 FlatQUAD energy dispersive X-ray spectrometer (EDS). The microscope working distance was 15 mm, the accelerating voltage was 15 keV, and the beam current was 20 nA. The beam limiting aperture was set to either 1 or 0. Typical X-ray count rates were 100-200 kcps. Maps were collected for 5 min with a map size of 1000 × 750 pixels. Maps were generated using Au M lines at 21 keV, Al K at 1.5 keV, and S Ka at 2.4 keV.
Claims
1. 1. A heterogeneous catalyst comprising a support and gold, wherein (i) the support comprises alumina, (ii) the catalyst comprises 0.1-5 weight percent gold, (iii) at least 90 weight percent of the gold is in the outer 60% of the catalyst volume, and (iv) particles of the catalyst have an average diameter of 200 microns to 30 mm, the weight percentages being based on the weight of the catalyst, the heterogeneous catalyst being used to prepare methyl methacrylate from methacrolein and methanol, and the heterogeneous catalyst is nickel-free.
2. 10. The catalyst of claim 1, wherein the particles of the catalyst have an average diameter of from 300 microns to 20 mm.
3. 3. The catalyst of claim 2, wherein at least 95% by weight of the gold is in the outer 50% of the catalyst volume.
4. 4. The catalyst of claim 3, wherein the catalyst comprises 0.2-3 wt. % gold, 60-95 wt. % silica, and 0.1-15 wt. % alumina.
5. 1. A catalyst bed comprising: (a) a heterogeneous catalyst comprising a support and gold, (i) the support comprises alumina, (ii) the catalyst comprises 0.1 to 5 weight percent gold, (iii) at least 90 weight percent of the gold is in the outer 60% of the catalyst volume, and (iv) particles of the catalyst have an average diameter of 200 microns to 30 mm, the weight percentages being based on the weight of the catalyst; and (b) a liquid phase comprising methacrolein, methanol, and methyl methacrylate, wherein the heterogeneous catalyst does not comprise nickel.
6. 6. The catalyst bed of claim 5, wherein the catalyst has an average diameter of from 500 microns to 10 mm, and the catalyst bed further comprises a gas phase comprising oxygen.
7. 7. The catalyst bed of claim 6, wherein the catalyst comprises 0.2-3 wt. % gold, 60-95 wt. % silica, and 0.1-15 wt. % alumina.
8. 1. A process for preparing methyl methacrylate from methacrolein and methanol, the process comprising contacting a mixture comprising methacrolein, methanol, and oxygen with a catalyst bed comprising a support and a heterogeneous catalyst comprising gold, (i) the support comprises alumina, (ii) the catalyst comprises 0.1 to 5 weight percent gold, (iii) at least 90 weight percent of the gold is in the outer 60% of the catalyst volume, and (iv) particles of the catalyst have an average diameter of 200 microns to 30 mm, weight percentages being based on the weight of the catalyst, and the heterogeneous catalyst does not comprise nickel.
9. The method of claim 8, wherein the catalyst has an average diameter of from 500 microns to 10 mm.
10. 10. The method of claim 9, wherein the catalyst comprises 0.2-3 wt. % gold, 60-95 wt. % silica, and 0.1-15 wt. % alumina.
Citation Information
Patent Citations
Method for producing methacrylic ester
JP2003292473A
Gold-carrying catalyst for liquid phase reaction and method for producing carboxylic acid ester
JP2004181358A
Method for producing a shell catalyst and the shell catalyst therefor
JP2010527777A
Process for producing unsaturated esters by direct oxidative esterification starting from aldehydes
JP2017504607A
Composite particle-loaded article, method for producing the composite particle-loaded article, and method for producing compound using the composite particle-loaded article as chemical synthesis catalyst