Supporting glass substrate
The supporting glass substrate with a high ε/d ratio effectively addresses the challenge of suppressing deflection and reducing weight by enhancing rigidity and density through specific metal oxide compositions, achieving both objectives.
Patent Information
- Application Number
- JP2024140735
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-07-29
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-06-05
AI Technical Summary
Support glass substrates face challenges in simultaneously suppressing deflection and reducing weight, as increasing thickness to reduce deflection increases mass, while reducing thickness to reduce weight leads to deflection.
The supporting glass substrate has a Young's modulus to density ratio (ε/d) of 37.0 GPa cm³/g or higher, calculated using the composition and measured values, with specific metal oxide ratios and densities to enhance rigidity and reduce weight effectively.
The solution effectively suppresses deflection and reduces weight beyond expectations, achieving both objectives by maintaining high rigidity with reduced thickness.
Smart Images

Figure 2024160378000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a supporting glass substrate. [Background technology]
[0002] As electronic devices become smaller, there is an increasing demand for technology to package semiconductor devices used in these electronic devices at high density. In recent years, Fan Out Wafer Level Package (FOWLP) and Fan Out Panel Level Package (FOPLP) have been proposed as technologies for packaging semiconductor devices at high density. Hereinafter, FOWLP and FOPLP will be collectively referred to as FOWLP, etc.
[0003] In FOWLP and the like, a supporting glass substrate may be used to support the processed substrate on which the semiconductor devices are stacked in order to suppress bending of the processed substrate (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6443668 Summary of the Invention [Problem to be solved by the invention]
[0005] Supporting glass substrates used to support components, such as supporting glass substrates for FOWLPs, are required to suppress deflection and also to be lightweight. If the supporting glass substrate is made thicker to suppress deflection, its mass increases, and if the thickness is made thinner to reduce weight, deflection is likely to occur. Therefore, it may be difficult to suppress deflection and reduce weight at the same time.
[0006] The present invention has been made in view of the above problems, and has an object to provide a supporting glass substrate that can suppress bending and achieve a reduction in weight. [Means for solving the problem]
[0007] In order to solve the above problems and achieve the object, the supporting glass substrate according to the present disclosure has a Young's modulus ε (GPa) and a density d (g / cm 3 ) to the ratio ε / d(GPa cm 3 / g) is 37.0 (GPa cm 3 / g) or more, and the Young's modulus (GPa) calculated from the composition is 3 ) to the calculated ratio α(GPa cm 3 / g) is greater than the calculated ratio α (GPa cm 3 / g) is expressed by the following formula: α=2·Σ{(V i G i ) / M i )·X i} Here, V i is the packing parameter of the metal oxide contained in the supporting glass substrate, and G i is the dissociation energy of the metal oxide contained in the supporting glass substrate, and M i is the molecular weight of the metal oxide contained in the supporting glass substrate, and X i is the molar ratio of the metal oxide contained in the supporting glass substrate. Effect of the Invention
[0008] According to the present invention, it is possible to suppress deflection and reduce weight. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic diagram of a supporting glass substrate according to this embodiment. [Diagram 2] FIG. 2 is a graph for explaining the performance of the supporting glass substrate according to this embodiment. [Diagram 3]FIG. 3 is a schematic diagram showing a method for measuring deflection in the examples and comparative examples. [Figure 4] FIG. 4 is a graph showing the characteristics of the supporting glass substrates of the examples and the comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Note that the present invention is not limited to these embodiments, and when there are multiple embodiments, the present invention also includes combinations of the embodiments.
[0011] Fig. 1 is a schematic diagram of a supporting glass substrate according to this embodiment. As shown in Fig. 1, the supporting glass substrate 10 according to this embodiment is used as a glass substrate for manufacturing a semiconductor package, and more specifically, is a supporting glass substrate for manufacturing a FOWLP or the like. However, the use of the supporting glass substrate 10 is not limited to the use for manufacturing a FOWLP or the like, and is optional, and may be a glass substrate used to support a member. Note that the FOWLP or the like includes a FOWLP and a FOPLP, as described above.
[0012] The supporting glass substrate 10 is capable of suppressing bending and reducing weight at the same time by increasing the ratio ε / d of Young's modulus ε to density d. Specifically, the supporting glass substrate 10 has a ratio ε / d of 32.0 (GPa cm 3 / g) or more and satisfies the following formula (1). The calculated ratio α in formula (1) is a calculated ratio of the Young's modulus to the density of the supporting glass substrate 10, calculated from the composition of the supporting glass substrate 10, and will be described in detail later.
[0013] ε / d>α (1)
[0014] The ratio ε / d is a value calculated using the measured value of the Young's modulus ε of the supporting glass substrate 10 and the measured value of the density d of the supporting glass substrate 10. In this embodiment, the Young's modulus ε of the supporting glass substrate 10 is a value measured based on the propagation of ultrasonic waves using a 38DL PLUS manufactured by OLYMPUS Corporation. In addition, the density d of the supporting glass substrate 10 is a value measured using the Archimedes method in this embodiment. The ratio ε / d is calculated by dividing the thus measured Young's modulus ε by the measured density d. The unit of Young's modulus ε is GPa, and the unit of density d is g / cm 3 and the ratio ε / d is expressed in GPa cm 3 / g.
[0015] While the ratio ε / d is a value using measured values, the calculated ratio value α is a value calculated from the composition of the supporting glass substrate 10 without using measured values of Young's modulus ε and density d. Since it is known that the Young's modulus of glass can be calculated from its composition, the calculated ratio value α of the Young's modulus to the density of the supporting glass substrate 10 can be calculated from the composition of the supporting glass substrate 10. The composition of the supporting glass substrate 10 here refers to the composition when the composition contained in the supporting glass substrate 10 is converted into a metal oxide. More specifically, the ratio calculation value α corresponds to a value obtained by multiplying the size of the metal oxide ion by its binding strength, dividing the result by the weight of the ion, adding up the results for each metal oxide, and multiplying the total by 2. Specifically, the ratio calculation value α is calculated by the following formula (2).
[0016] α=2·Σ(P i X i )=2·Σ{(V i G i ) / M i )·X i} ···(2)
[0017] Here, P i is (V i G i / M i ) V i (cm 3 / mol) is the packing parameter of the metal oxide contained in the supporting glass substrate 10, and G i (kJ / cm 3) is the dissociation energy of the metal oxide contained in the supporting glass substrate 10, and M i (g / mol) is the molecular weight of the metal oxide contained in the supporting glass substrate 10, and X i is the molar ratio of the metal oxide contained in the supporting glass substrate 10 to the entire supporting glass substrate 10. i The unit of is dimensionless. As shown in the formula (2), the ratio calculation value α is calculated by multiplying the value {(V i G i ) / M i )·X i} for all the metal oxides contained in the supporting glass substrate 10 and multiplied by 2. The unit of the ratio calculation value α is GPa cm 3 / g.
[0018] Also, V i is calculated using the following formula (3), and G i is calculated using the following formula (4).
[0019] V i =6.02 10 23 (4 / 3)π(xr 3 M +y·r 3 O ) ···(3) G i =d i / M i ·{x·ΔHf(M gas ) + y ΔHf(O gas )-ΔHf(M x O ycrystal )-(x+y)·RT} ···(4)
[0020] Here, the metal oxide contained in the supporting glass substrate 10 is M x O y Let us assume that. M is a metal element, O is an oxygen element, x is the valence of the metal element M, and y is the valence of the oxygen element O. r M is the metal oxide M x O yis the Shannon ionic radius of the metal element M in O is the metal oxide M x O y is the Shannon ionic radius of the oxygen element O in the i is the metal oxide M x O y is the density. ΔHf(M gas ) is the standard enthalpy of formation of the gaseous metal element M, and ΔHf(O gas ) is the standard enthalpy of formation of gaseous oxygen, O, and ΔHf(M x O ycrystal ) is a metal oxide M x O y where R is the gas constant and T is the absolute temperature.
[0021] The supporting glass substrate 10 has a ratio ε / d of 32.0 (GPa cm 3 / g) or more and is greater than the ratio α calculated based on the composition. In other words, the supporting glass substrate 10 is a member in which the ratio ε / d of Young's modulus to density obtained by actual measurement is greater than the calculated ratio α, which is the ratio of Young's modulus to density calculated based on the composition. The ratio ε / d of the supporting glass substrate 10 was set to 32.0 (GPa cm 3 / g) or more, the supporting glass substrate 10 can be made thin and lightweight with high rigidity, so that it is possible to suppress deflection and to make the supporting glass substrate 10 thin and lightweight at the same time. Furthermore, the supporting glass substrate 10 has a ratio ε / d that is greater than the ratio calculation value α calculated based on the composition, in other words, the Young's modulus per unit density is greater than the value expected based on the composition. Therefore, the supporting glass substrate 10 can suppress bending and reduce weight to a greater extent than expected.
[0022] FIG. 2 is a graph for explaining the performance of the supporting glass substrate according to this embodiment. FIG. 2 is a graph showing the range of the ratio ε / d explained above, with the horizontal axis representing the calculated ratio value α and the vertical axis representing the ratio ε / d. The line segment L1a corresponds to the range where the ratio ε / d=32.0 (GPa cm 3 / g), and line segment L2a is a boundary line where the ratio ε / d=ratio calculation value α. In Fig. 2, it can be said that the ratio ε / d of the supporting glass substrate 10 is plotted above the line segments L1a and L2a in the vertical axis direction, in other words, the ratio ε / d is plotted within the shaded region in Fig. 2.
[0023] The supporting glass substrate 10 has a ratio ε / d of 37.0 (GPa cm 3 / g) or more, and 40.0 (GPa cm 3 / g) or more. The ratio ε / d is preferably 37.0 (GPa cm 3 / g) or more, it is possible to more effectively suppress deflection and reduce weight, and the ratio ε / d is 40.0 (GPa cm 3 / g) or more, it is possible to more suitably suppress the deflection and reduce the weight. In Figure 2, the line segment L1b has a ratio ε / d = 37.0 (GPa cm 3 / g), and the line segment L1c is the boundary where the ratio ε / d = 40.0 (GPa cm 3 / g).
[0024] Moreover, in the supporting glass substrate 10, it is more preferable that the ratio ε / d satisfies the following formula (5), and even more preferable that it satisfies formula (6). By satisfying formula (5), it is possible to more suitably suppress the deflection and reduce the weight, and by satisfying formula (6), it is possible to more suitably suppress the deflection and reduce the weight.
[0025] ε / d>α+2.0(GPa cm 3 / g) ···(5) ε / d>α+4.0(GPa cm 3 / g) ···(6)
[0026] In Figure 2, the line segment L2b is ε / d=α+2.0(GPa cm 3 / g), and the line segment L2c is ε / d=α+4.0(GPa cm 3 / g).
[0027] The supporting glass substrate 10 has a packing density Vt of 13.8 (cm 3 / mol), and preferably less than 13.6 (cm 3 / mol), and more preferably less than 13.3 (cm 3 / mol) is more preferable. With the filling density Vt in this range, the molecules can be densely packed, and it is possible to preferably suppress bending and reduce weight. Here, the filling density Vt refers to the degree of packing of the molecules, and in this embodiment, refers to the degree of packing of the metal oxide contained in the supporting glass substrate 10. The filling density Vt is a value calculated based on the composition of the supporting glass substrate 10. The filling density Vt is calculated from the following formula (7).
[0028] Vt = Σ(V i X i ) · · · (7)
[0029] V in Equation (7) i is the packing parameter of the metal oxide contained in the supporting glass substrate 10, as described above, and X in formula (7) i As described above, is the molar ratio of the metal oxide contained in the supporting glass substrate 10 to the entire supporting glass substrate 10. In other words, the filling density Vt is the total value of all the metal oxides contained in the supporting glass substrate 10, obtained by multiplying the filling parameter calculated for each metal oxide by the molar ratio.
[0030] The supporting glass substrate 10 has a calculated ratio α of 31.6 (GPa cm 3 / g) or more, and the packing density Vt is 13.8 (cm 3 / mol). In addition, the supporting glass substrate 10 has a calculated ratio α of 32.8 (GPa cm 3 / g) or more, and the packing density Vt is more preferably less than 13.8, and the calculated ratio α is 33.1 (GPa cm 3 / g) or more, and the packing density Vt is 13.6 (cm 3 / mol), and the calculated ratio α is preferably less than 33.5 (GPa cm 3 / g) and the packing density Vt is 13.3 (cm 3 / mol) is more preferable. By using the supporting glass substrate 10 in which the calculated ratio α and the packing density Vt satisfy such a relationship, it is possible to preferably suppress bending and reduce the weight.
[0031] The ratio of the ratio ε / d to the calculated ratio value α, i.e., the ratio ε / d divided by the calculated ratio value α, is defined as the structure factor M. In other words, the structure factor M refers to the ratio of the measured value of the specific elastic modulus to the specific elastic modulus calculated from the composition. In this case, it is preferable that the structure factor M of the supporting glass substrate 10 is greater than 1, more preferably 1.1 or more, and even more preferably greater than 1.12. By setting the structure factor M within this range, it is possible to preferably achieve suppression of bending and weight reduction.
[0032] The ratio of the average molecular weight V to the density d of the supporting glass substrate 10, that is, the value obtained by dividing the average molecular weight V by the density d, is defined as the molecular volume Vm (cm 3 / mol). The average molecular weight V is a calculated value of the average molecular weight of the supporting glass substrate 10, and is calculated based on the composition of the supporting glass substrate 10. For example, a supporting glass substrate containing 50% Al2O3 by molar ratio and 50% SiO2 by molar ratio has an average molecular weight V of (101.96×0.5)+(60.08×0.5). It can be said that the molar volume Vm is the ratio of the average molecular weight calculated from the composition to the measured value of the density d. The supporting glass substrate 10 has a molar volume Vm of 24.1 (cm 3 / mol), and preferably less than 23.2 (cm 3 / mol), and more preferably less than 22.7 (cm 3When the molar volume Vm is in this range, the molecules are densely packed, and the suppression of bending can be suitably realized.
[0033] Next, a description will be given of the composition of the supporting glass substrate 10. In this embodiment, the supporting glass substrate 10 is configured with the composition described below, thereby making the ratio ε / d 32.0 (GPa cm 3 / g) and larger than the calculated ratio α, but the composition described below is an example. 3 / g) and greater than the calculated ratio α, any composition may be used.
[0034] The supporting glass substrate 10 includes a base material and an additive material. The supporting glass substrate 10 preferably includes SiO2 and Al2O3 as base materials. The supporting glass substrate 10 preferably has a total content of SiO2 and Al2O3 of 50% to 85%, and more preferably 60% to 75%, expressed in mole % on an oxide basis. Here, 50% to 85% refers to 50% or more and 85% or less when the mole % of the total amount of the supporting glass substrate 10 is taken as 100%, and the same applies hereinafter. Furthermore, the supporting glass substrate 10 may contain, as a base material, B2O3 in addition to SiO2 and Al2O3. The content of B2O3 is preferably 1% to 30%, more preferably 3% to 10%, in mole percent based on oxide. By setting the content of the base material within such a range, the ratio ε / d can be increased, and the suppression of deflection and weight reduction can be suitably achieved. Furthermore, the supporting glass substrate 10 may contain, as a base material, at least one of P2O5, Ga2O3, AlN, and Si3N4.
[0035] The additive material is a metal oxide. The supporting glass substrate 10 contains at least one of MgO, CaO, and Y2O3 as the additive material. The content of the additive material in the supporting glass substrate 10, in other words, the total content of one or more components selected from the group consisting of MgO, CaO, and Y2O3, is preferably in the range of 15% to 50%, and more preferably 20% to 45%, expressed in mole % on an oxide basis. Of the additive materials MgO, CaO, and Y2O3, the supporting glass substrate 10 preferably contains only MgO, only MgO and CaO, all of MgO, CaO, and Y2O3, or only Y2O3. The supporting glass substrate 10 preferably contains 11% to 35% MgO, and more preferably contains 20% to 30%, in terms of mole percent on an oxide basis. The supporting glass substrate 10 preferably contains 7% to 32% CaO, and more preferably contains 8% to 15%, in terms of mole percent on an oxide basis. The supporting glass substrate 10 preferably contains 2.8% to 20% Y2O3, in terms of mole percent on an oxide basis. By setting the content of the additive material within these ranges, the ratio ε / d can be increased, and the suppression of bending and weight reduction can be suitably achieved. Furthermore, the supporting glass substrate 10 may contain, as an additive material, at least one selected from the group consisting of ZrO2, TiO2, Li2O, and ZnO, in addition to at least one selected from the group consisting of MgO, CaO, and Y2O3.
[0036] More specifically, the supporting glass substrate 10 preferably has, in terms of oxide-based mole %, a SiO2 content of 40% to 60%, an Al2O3 content of 20% to 30%, and an MgO content of 20% to 30%. In this case, the supporting glass substrate 10 preferably does not contain anything other than SiO2, Al2O3, and MgO, except for unavoidable impurities.
[0037] A preferred composition of the supporting glass substrate 10 will be described in more detail. The supporting glass substrate 10 is preferably one in which the parameters such as the ratio ε / d, the structure factor M, and the molecular volume Vm are within the ranges specified above, and the composition is not particularly limited. That is, various supporting glass substrates are manufactured with arbitrary compositions, and the parameters such as the ratio ε / d, the structure factor M, and the molecular volume Vm are measured and calculated for the manufactured supporting glass substrates, and the one in which the calculated parameters are within the ranges specified above may be adopted as the supporting glass substrate 10.
[0038] The supporting glass substrate 10 preferably has a SiO2 content of 20% to 66%, an Al2O3 content of 6% to 30%, and an MgO content of 25% to 30%, expressed in mole % on an oxide basis. Alternatively, the supporting glass substrate 10 preferably has a SiO2 content of 20% to 66%, an Al2O3 content of 6% to 30%, and a total content of MgO and CaO of 19% to 46%, expressed in mole % on an oxide basis. Alternatively, the supporting glass substrate 10 preferably has a SiO2 content of 20% to 66%, an Al2O3 content of 6% to 30%, and a total content of B2O3 and Y2O3 of 5.8% to 50%, and more preferably a total content of B2O3 and Y2O3 of 25% to 50%.
[0039] (1st composition) A first composition is an example of a preferable composition of the supporting glass substrate 10. The supporting glass substrate 10 of the first composition preferably has a SiO2 content of 48% to 52%, an Al2O3 content of 20% to 25%, and an MgO content of 25% to 30%, and contains no components other than SiO2, Al2O3, and MgO, except for unavoidable impurities.
[0040] (2nd composition) A second composition is an example of a preferable composition of the supporting glass substrate 10. The supporting glass substrate 10 of the second composition preferably contains SiO2 of 43% to 58%, Al2O3 of 12% to 17%, MgO of 14% to 27%, and CaO of 7% to 32%, and contains no components other than SiO2, Al2O3, MgO, and CaO, except for unavoidable impurities.
[0041] (Third composition) A third composition is an example of a preferable composition of the supporting glass substrate 10. The supporting glass substrate 10 of the third composition preferably contains SiO2 of 64% to 68%, Al2O3 of 10% to 14%, MgO of 9% to 13%, CaO of 6% to 10%, and B2O3 of 1% to 5%, and does not contain any components other than SiO2, Al2O3, MgO, CaO, and B2O3 except for unavoidable impurities.
[0042] (4th composition) A fourth composition is an example of a preferable composition of the supporting glass substrate 10. The supporting glass substrate 10 of the fourth composition preferably contains SiO2 of 55.7% to 59.7%, Al2O3 of 15% to 19%, MgO of 13% to 17%, CaO of 7% to 11%, and SrO of 0.1% to 1%, and contains no components other than SiO2, Al2O3, MgO, CaO, and SrO except for unavoidable impurities.
[0043] (5th composition) A fifth composition is an example of a preferable composition of the supporting glass substrate 10. The supporting glass substrate 10 of the fifth composition preferably contains SiO2 of 58% to 59%, Al2O3 of 13% to 14%, MgO of 17% to 19%, CaO of 7% to 8%, and TiO2 of 2% to 4%, and contains no components other than SiO2, Al2O3, MgO, CaO, and TiO2, except for unavoidable impurities.
[0044] (6th composition) A sixth composition is an example of a preferable composition of the supporting glass substrate 10. The supporting glass substrate 10 of the sixth composition preferably contains SiO2 of 58% to 62%, Al2O3 of 11% to 15%, MgO of 15% to 19%, CaO of 6% to 10%, and ZrO2 of 0.5% to 2%, and does not contain any components other than SiO2, Al2O3, MgO, CaO, and ZrO2, except for unavoidable impurities.
[0045] (7th composition) A seventh composition is an example of a preferred composition of the supporting glass substrate 10. The supporting glass substrate 10 of the seventh composition preferably contains SiO2 of 48% to 50%, Al2O3 of 6% to 10%, MgO of 12% to 16%, CaO of 7% to 11%, Y2O3 of 0.8% to 4.8%, TiO2 of 0% to 4%, ZrO2 of 0% to 3%, LiO2 of 2% to 6%, and ZnO of 4% to 8%, and does not contain any other components than SiO2, Al2O3, MgO, CaO, Y2O3, TiO2, ZrO2, LiO2, and ZnO, except for unavoidable impurities.
[0046] (8th composition) An eighth composition is an example of a preferable composition of the supporting glass substrate 10. The supporting glass substrate 10 of the eighth composition preferably contains 20% to 50% SiO2, 20% to 30% Al2O3, 5% to 30% B2O3, and 19% to 20% Y2O3, and contains no components other than SiO2, Al2O3, B2O3, and Y2O3, except for unavoidable impurities.
[0047] (9th composition) A ninth composition is an example of a preferable composition of the supporting glass substrate 10. The supporting glass substrate 10 of the ninth composition preferably has an SiO2 content of 38% to 42%, an Al2O3 content of 18% to 22%, a B2O3 content of 16% to 20%, a Y2O3 content of 18% to 22%, and a P2O5 content of 0% to 4%, and does not contain any components other than SiO2, Al2O3, B2O3, Y2O3, and P2O5, except for unavoidable impurities.
[0048] (10th composition) A tenth composition is an example of a preferable composition of the supporting glass substrate 10. The supporting glass substrate 10 of the tenth composition preferably has a SiO2 content of 38% to 42%, an Al2O3 content of 13% to 15%, a B2O3 content of 18% to 22%, a Y2O3 content of 18% to 22%, and a Ga2O5 content of 3% to 7%, and does not contain any components other than SiO2, Al2O3, B2O3, Y2O3, and Ga2O5, except for unavoidable impurities.
[0049] The supporting glass substrate 10 does not include a sintered body. In other words, the supporting glass substrate 10 is a glass that is not a sintered body. The sintered body here refers to a member in which a plurality of particles are heated at a temperature lower than the melting point to bond the particles together. A sintered body has a relatively high porosity because it contains pores, but the supporting glass substrate 10 has a low porosity, usually 0%, because it is not a sintered body. However, it is permissible to include unavoidable small pores. The porosity here refers to the so-called true porosity, which refers to the value obtained by dividing the sum of the volumes of pores (pores) that communicate with the outside and pores (pores) that do not communicate with the outside by the total volume (apparent volume). The porosity can be measured, for example, according to JIS R 1634.
[0050] The glass used for the supporting glass substrate 10 is usually amorphous glass, i.e., an amorphous solid. This glass may be crystallized glass containing crystals on the surface or inside, but amorphous glass is preferable from the viewpoint of density. Sintered bodies (ceramics) cannot be used because of their low transmittance and high density.
[0051] Next, the shape of the supporting glass substrate 10 will be described. As shown in Fig. 1, the supporting glass substrate 10 is a plate-shaped glass substrate including a first surface 12 which is one surface, a second surface 14 which is the other surface, and a side surface 16. The second surface 14 is the surface opposite to the first surface 12, and is, for example, parallel to the first surface 12. The side surface 16 is a side surface of the supporting glass substrate 10, and can also be said to be an end surface connecting the first surface 12 and the second surface 14. The supporting glass substrate 10 has a circular disk shape in a plan view, i.e., when viewed from a direction perpendicular to the first surface 12. However, the supporting glass substrate 10 is not limited to a disk shape and may have any shape, and may be a plate having a polygonal shape such as a rectangle.
[0052] Furthermore, the thickness D2 of the supporting glass substrate 10, i.e., the length between the first surface 12 and the second surface 14, is preferably 0.1 mm to 2.0 mm, and more preferably 0.1 mm to 0.5 mm. By setting the thickness D2 to 0.1 mm or more, the supporting glass substrate 10 can be prevented from becoming too thin, and damage due to bending or impact can be suppressed. By setting the thickness D2 to 2.0 mm or less, the weight can be prevented from becoming too heavy, and by setting the thickness D2 to 0.5 mm or less, the weight can be further preferably prevented from becoming too heavy.
[0053] The manufacturing method of the supported glass substrate 10 is not particularly limited and may be any method, but may be, for example, a method in which various raw materials such as silica sand and soda ash, which are raw materials for the compounds contained in the supported glass substrate 10, are charged into a continuous melting furnace, heated and melted at 1500°C to 1600°C, refined, and then supplied to a molding device, where the supplied molten glass is formed into a plate shape and slowly cooled to manufacture the supported glass substrate 10. Note that various methods can be adopted for manufacturing the supported glass substrate 10, and examples of such methods include a melt casting method, a downdraw method (e.g., an overflow downdraw method, a slot down method, and a redraw method), a float method, a roll-out method, and a press method.
[0054] Next, an example of a manufacturing process when the supporting glass substrate 10 is used for FOWLP manufacturing will be described. In FOWLP manufacturing, a plurality of semiconductor chips are bonded onto the supporting glass substrate 10, and the semiconductor chips are covered with a sealing material to form an element substrate. Then, the supporting glass substrate 10 and the element substrate are separated, and the side of the element substrate opposite to the semiconductor chips is bonded, for example, onto another supporting glass substrate 10. Then, wiring, solder bumps, and the like are formed on the semiconductor chips, and the element substrate and the supporting glass substrate 10 are separated again. Then, the element substrate is cut into individual semiconductor chips to obtain a semiconductor device.
[0055] As described above, the supporting glass substrate 10 according to this embodiment has a ratio ε / d of 32.0 (GPa cm 3 / g) or more and is a value larger than the calculated ratio α. The ratio ε / d is the ratio of the Young's modulus ε to the density d of the supporting glass substrate 10. The calculated ratio α is the ratio of the Young's modulus to the density calculated from the composition of the supporting glass substrate 10, and is expressed by the above formula (2).
[0056] There are cases where a glass substrate is required to suppress warping while being lightweight. However, in general, it is necessary to increase the thickness to suppress warping, whereas it is necessary to reduce the thickness to reduce the weight, making it difficult to suppress warping while reducing the weight. In contrast, the supporting glass substrate 10 according to this embodiment has a ratio ε / d of 32.0 (GPa cm 3 / g) or more, even if the supporting glass substrate 10 is made thin to reduce weight, it is possible to suppress deflection due to the high Young's modulus, and thus it is possible to achieve both suppression of deflection and weight reduction. Furthermore, the ratio ε / d of the supporting glass substrate 10 is greater than the ratio calculated value α calculated based on the composition, in other words, the Young's modulus per unit density is greater than the value expected based on the composition. Therefore, the supporting glass substrate 10 can suppress bending and reduce weight to a degree greater than expected.
[0057] The supporting glass substrate 10 has a ratio ε / d of 37.0 (GPa cm 3 / g) or more, the structure factor M is 1.1 or more, and the packing density Vt is 13.8 (cm 3 The supporting glass substrate 10 that satisfies these conditions can suppress bending and reduce weight to a greater extent than expected.
[0058] In addition, the supporting glass substrate 10 has a calculated ratio α of 31.6 (GPa cm 3 / g) or more, and the packing density Vt is 13.8 (cm 3 By setting the calculated ratio α and the packing density Vt in this range, it is possible to suppress deflection and reduce weight to a greater extent than expected.
[0059] In addition, the supporting glass substrate 10 has a ratio ε / d>calculated ratio α+2.0 (GPa cm 3 / g), and the relationship is preferably satisfied: ratio ε / d> calculated ratio α+4.0(GPa cm 3 / g) is more preferably satisfied. By satisfying these relationships, it is possible to more suitably suppress deflection and reduce weight.
[0060] The supporting glass substrate 10 has a ratio ε / d of 37.0 (GPa cm 3 / g) or more, and the ratio ε / d is preferably 40.0 (GPa cm 3 When the ratio ε / d is this value, it is possible to more suitably suppress the deflection and reduce the weight.
[0061] Furthermore, the supporting glass substrate 10 preferably has a total content, in mol %, of one or more components selected from the group consisting of MgO, CaO, and Y2O3 in the range of 15% to 50% with respect to the total amount of the supporting glass substrate 10. By including such materials in such amounts, the supporting glass substrate 10 can have a higher Young's modulus ε than expected, and can more suitably achieve suppression of deflection and weight reduction.
[0062] Moreover, the supporting glass substrate 10 preferably has a total content, in mol %, of SiO2 and Al2O3 in the range of 50% to 85% with respect to the total amount of the supporting glass substrate 10. With such a composition, the supporting glass substrate 10 can have a higher Young's modulus ε than expected, and can more suitably achieve suppression of deflection and weight reduction.
[0063] Moreover, it is preferable that the thickness D2 of the supporting glass substrate 10 is in the range of 0.1 mm to 0.5 mm. By setting the thickness D2 in this range, it is possible to reduce the weight while suppressing damage due to bending or impact.
[0064] The supporting glass substrate 10 is glass that is not a sintered body. Since the supporting glass substrate 10 is not a sintered body, it is possible to prevent the density from becoming too high and reduce the weight, and since light is not scattered by pores that are present in a sintered body, the light transmittance can be ensured.
[0065] Moreover, it is preferable that the supporting glass substrate 10 is made of amorphous glass. Since the supporting glass substrate 10 is made of amorphous glass, the density of the supporting glass substrate 10 can be prevented from becoming too high, thereby making the substrate lighter.
[0066] The supporting glass substrate 10 is preferably a supporting glass substrate for manufacturing FOWLP, in other words, at least one of a fan-out wafer level package and a fan-out panel level package. By using the supporting glass substrate 10 for at least one of the fan-out wafer level package manufacturing and the fan-out panel level package manufacturing, the semiconductor package can be manufactured suitably.
[0067] (Example) Next, examples will be described. Note that the embodiment may be modified as long as the effects of the invention are achieved. In the examples and comparative examples, supporting glass substrates with different compositions were prepared. Then, for each supporting glass substrate, the ratio calculation value α was calculated, and the Young's modulus ε and density d were measured to calculate the ratio ε / d. In addition, for each supporting glass substrate, the deflection amount and mass were also measured, and evaluation was performed based on the deflection amount and mass. The following is a more detailed description.
[0068] Table 1 shows the materials used in the supporting glass substrates in the examples and comparative examples. Table 1 shows the contents, in mole % on an oxide basis, of the materials used in producing the supporting glass substrates of Examples 1 to 17 and Comparative Examples 1 to 11. Table 2 shows the contents, in mole % on an oxide basis, of the materials used in producing the supporting glass substrates of Examples 18 to 26. In the examples and comparative examples, a blank plate having a diameter of 320 mm and a thickness of 6 mm was manufactured using a melt casting method with the compositions shown in Tables 1 and 2, respectively. Next, a plurality of blank plates having a diameter of 300 mm and a thickness of 3 mm were cut out from the center of the blank plate. Both sides of these blanks were polished using cerium oxide as an abrasive, and the thicknesses were adjusted to 0.4 mm, 0.7 mm, 1.3 mm, and 2.0 mm, respectively, to manufacture a supporting glass substrate. The supporting glass substrate thus produced was used as a sample and was evaluated.
[0069] [Table 1] [Table 2]
[0070] In the examples and comparative examples, for each of the supporting glass substrates prepared as samples, the ratio calculation value α was calculated based on the material composition shown in Table 1. Then, for each of the supporting glass substrates prepared as samples, the Young's modulus ε was measured using 38DL PLUS manufactured by OLYMPUS Corporation, and the density d was measured by the Archimedes method, and the ratio ε / d was calculated based on the measured Young's modulus ε and density d.
[0071] FIG. 3 is a schematic diagram showing a method for measuring deflection in the examples and comparative examples. In the examples and comparative examples, the deflection due to its own weight was measured for each of the supported glass substrates prepared as samples. Specifically, as shown in FIG. 3, the deflection amount at the center part of the first surface 12 (the part indicated by the arrow in FIG. 3) when the second surface 14 of the sample supported glass substrate was supported at three points by the supporting part B was measured using Dyvoce manufactured by Kohzu Seiki. The diameter of the supporting part B was 1.6 mm, and the supporting part B was arranged so that the center position overlapped with a point 5.0 mm inward in the radial direction from the outer periphery of the supported glass substrate. In addition, the mass was measured for each of the supported glass substrates prepared as samples.
[0072] Table 3 shows the evaluation results of the examples and comparative examples. Fig. 4 is a graph showing the characteristics of the supporting glass substrates of the examples and comparative examples. Table 3 shows the calculated ratio α, Young's modulus ε, density d, ratio ε / d, deflection amount for each thickness D2, mass of a sample with a thickness of 2.0 mm, the evaluation results of deflection and mass, and the overall evaluation result for each sample supporting glass substrate. As shown in Table 3, in Examples 1 to 17, the ratio ε / d was 32.0 (GPa cm 3 / g) or more, and the ratio ε / d is larger than the calculated ratio value α. On the other hand, in Comparative Example 1 to Comparative Example 11, the ratio ε / d is 32.0 (GPa cm 3 / g) or greater and the ratio ε / d is greater than the calculated ratio value α. Fig. 4 is a graph plotting the relationship between the ratio ε / d and the calculated ratio value α of the sample supporting glass substrate. The black circles in Fig. 4 represent the supporting glass substrates of Examples 1 to 17, and the crosses represent the supporting glass substrates of Comparative Examples 1 to 11. Fig. 4 also shows that the supporting glass substrates of Examples 1 to 17 have a ratio ε / d of 32.0 (GPa cm 3 / g) or more, and the ratio ε / d is larger than the calculated ratio value α, which shows that the supporting glass substrates of Comparative Example 1 to Comparative Example 11 do not satisfy at least one of these conditions. According to Fig. 4, in the present examples, the ratio ε / d deviates from the calculated ratio value α, but in the comparative examples, it is seen that the ratio ε / d of the samples with particularly high ratio ε / d does not deviate from the calculated ratio value α.
[0073] [Table 3]
[0074] In addition, in determining the amount of deflection in Table 3, If the deflection is less than 0.8 mm, a double circle is displayed. If the deflection is 0.8 mm or more but less than 0.9 mm, it is marked with a circle. When the deflection is 0.9 mm or more but less than 1.0 mm, it is called a triangle. Deflection of 1.0 mm or more was marked as X. Double circles, circles, and triangles were judged as acceptable. In addition, in determining the mass in Table 3, If the mass is less than 400g, a double circle is marked. If the mass is between 400g and 430g, it will be marked as a circle. If the mass is between 430g and 500g, it is considered triangular. If the mass was 500g or more, it was marked as "X". Double circles, circles, and triangles were judged as acceptable. If both the deflection and mass are double circles, the overall judgment is double circles. If both the deflection and mass are circled or larger and at least one of them is circled, the overall judgment is circled. If both the deflection and the mass are greater than or equal to a triangle and at least one of them is a triangle, the overall judgment is a triangle. If at least one of the deflection amount and mass was judged as "no", the overall judgement was "no". In the overall evaluation, double circles, circles, and triangles were judged as passing.
[0075] As shown in Table 3, the supporting glass substrates according to Examples 1 to 17 were judged as pass in terms of the amount of deflection and the mass. On the other hand, the supporting glass substrates according to Comparative Examples 1 to 11 were judged as failing in terms of at least one of the amount of deflection and the mass. That is, the ratio ε / d was 32.0 (GPa cm 3 / g) or more and the ratio ε / d is greater than the calculated ratio value α, it can be seen that the supporting glass substrate of this embodiment can achieve both suppression of bending and weight reduction.
[0076] Table 4 shows the measurement results of the calculated ratio α and the ratio ε / d for Examples 18 to 27. As shown in Table 4, in Examples 18 to 27, the ratio ε / d was 32.0 (GPa cm 3 / g) or more, and the ratio ε / d is greater than the calculated ratio value α.
[0077] [Table 4]
[0078] Table 5 shows the ratio ε / d, structural factor M, molar volume Vm, calculated ratio value α, and packing density Vt for the supporting glass substrates of the examples and comparative examples. As shown in Table 5, in Examples 1, 3-4, 6-9, and 20-26, the ratio ε / d was 37.0 (GPa cm 3 / g) or more, which is a value larger than the calculated ratio α, the structure factor M is 1.1 or more, and the molar volume Vm is less than 24.1. Also, as shown in Table 5, in Examples 2, 4, 6-9, and 20-27, the calculated ratio α is 31.6 (GPa cm 3 / g) or more, and the packing density Vt is 13.8 (cm 3 / mol).
[0079] [Table 5]
[0080] Although the embodiment of the present invention has been described above, the embodiment is not limited to the contents of this embodiment. The above-mentioned components include those that a person skilled in the art can easily imagine, those that are substantially the same, and those that are within the so-called equivalent range. Furthermore, the above-mentioned components can be appropriately combined. Furthermore, various omissions, substitutions, or modifications of the components can be made without departing from the gist of the above-mentioned embodiment. [Explanation of symbols]
[0081] 10 Support glass substrate d density Alpha ratio calculation value ε Young's modulus ε / d ratio
Claims
1. In mole percent based on oxide, SiO 2 and Al 2 O 3 The total content of Y is in the range of 50% to 85%. 2 O 3 The content of is 2.8% to 20% and B 2 O 3 The content is in the range of 1% to 30%, or SiO 2 The content of Al is 20% to 66%. 2 O 3 The content of is 6% to 30%, and B 2 O 3 and Y 2 O 3 and the total content is 25% to 50%, or SiO 2 The content of Al is 36% to 50%. 2 O 3 The content of is 20% to 25%, and B 2 O 3 The content of Y is 5% to 20%. 2 O 3 The content of is 19% to 20%, excluding unavoidable impurities, SiO 2 , Al 2 O 3 , B 2 O 3 , and Y 2 O 3 Not including anything other than, or SiO 2 The content of Al is 38% to 42%. 2 O 3 The content of is 18% to 22%, and B 2 O 3 The content of Y is 16% to 20%. 2 O 3 The content of P is 18% to 22%. 2 O 5 The content of is 0% to 4%, excluding unavoidable impurities, SiO 2 , Al 2 O 3 , B 2 O 3 , Y 2 O 3 , and P 2 O 5 Not including anything other than, or SiO 2 The content of Al is 42%. 2 O 3 The content of is 13% to 15%, and B 2 O 3 The content of Y is 18% to 22%. 2 O 3 The content of is 18% to 22%, and Ga 2 O 5 The content of is 3% to 7%, excluding unavoidable impurities, SiO 2 , Al 2 O 3 , B 2 O 3 , Y 2 O 3 , and Ga 2 O 5 Not including except, Support glass substrate.
2. Ratio ε / d (GPa cm 3 / g)>Ratio calculation value α (GPa cm 3 / g) + 2.0 (GPa cm 3 The supported glass substrate according to claim 1 , wherein the relationship of (a) is satisfied. The ratio ε / d (GPa cm 3 / g) is the Young's modulus ε (GPa) and density d (g / cm 3 ) and the calculated ratio α (GPa cm 3 / g) is the Young's modulus (GPa) density (g / cm3) calculated from the composition 3 ) and is expressed by the following formula: α = 2 Σ {(V i ・G i ) / M i ) X i} Here, V i is the filling parameter of the metal oxide contained in the supporting glass substrate, and G i is the dissociation energy of the metal oxide contained in the supporting glass substrate, and M i is the molecular weight of the metal oxide contained in the supporting glass substrate, and X i is the molar ratio of the metal oxide contained in the supporting glass substrate.
3. Ratio ε / d (GPa cm 3 / g)>Ratio calculation value α (GPa cm 3 / g) + 4.0 (GPa cm 3 The supported glass substrate according to claim 2 , wherein the relationship of (a) is satisfied.
4. Ratio ε / d (GPa cm 3 / g) is 32.0 (GPa cm 3 The supporting glass substrate according to claim 1 , wherein the surface area of the supporting glass substrate is 10 μm or more. The ratio ε / d (GPa cm 3 / g) is the Young's modulus ε (GPa) and density d (g / cm 3 ) as a ratio.
5. In mole percent based on oxide, SiO 2 and Al 2 O 3 and the total content is 50% to 85%, 2 O 3 The content of is 2.8% to 20% and B 2 O 3 The content is in the range of 1% to 30%, or S 2 O 3 The content of Al is 20% to 66%. 2 O 3 The content of is 6% to 30%, and B 2 O 3 and Y 2 O 3 and the total content is 25% to 50%, or SiO 2 The content of Al is 20% to 50%. 2 O 3 The content of is 20% to 30%, and B 2 O 3 The content of Y is 5% to 30%. 2O 3 The content of is 19% to 20%, excluding unavoidable impurities, SiO 2 , Al 2 O 3 , B 2 O 3 , and Y 2 O 3 Not including anything other than, or SiO 2 The content of Al is 38% to 42%. 2 O 3 The content of is 18% to 22%, and B 2 O 3 The content of Y is 16% to 20%. 2 O 3 The content of P is 18% to 22%. 2 O 5 The content of is 0% to 4%, excluding unavoidable impurities, SiO 2 , Al 2 O 3 , B 2 O 3 , Y 2 O 3 , and P 2 O 5 Not including anything other than, or SiO 2 The content of Al is 38% to 42%. 2 O 3 The content of is 13% to 15%, and B 2 O 3 The content of Y is 18% to 22%. 2 O 3 The content of is 18% to 22%, and Ga 2 O 5 The content of is 3% to 7%, excluding unavoidable impurities, SiO 2 , Al 2 O 3 , B 2 O 3 , Y 2 O 3 , and Ga 2 O 5 Not including except, Support glass substrate.
6. SiO 2 and Al 2 O 3 The total content of Y is in the range of 50% to 85%. 2 O 3 The content of is 2.8% to 20% and B 2 O 3 The supporting glass substrate according to claim 1 or claim 5, wherein the content of is in the range of 5% to 18%.
7. MgO, CaO, and Y 2 O 3 The supporting glass substrate according to claim 1 or claim 5, wherein the total content of one or more components selected from the group consisting of is in the range of 15% to 50% by mol% with respect to the total amount of the supporting glass substrate.
8. The supporting glass substrate according to claim 1 or claim 5, having a thickness in the range of 0.1 mm to 0.5 mm.
9. The supporting glass substrate according to claim 1 or 5, which is made of amorphous glass.
10. 6. The supporting glass substrate of claim 1 or 5, which is a supporting glass substrate for manufacturing at least one of a fan-out wafer level package and a fan-out panel level package.
Citation Information
Patent Citations
Glass for information recording medium substrate
JP2000063144A
Glass substrate for information recording medium and magnetic information recording medium using the same
JP2002358626A
Glass composition
WO2019114499A1
Method of cut-off construction of concrete wall
JP1989043668A